High-strength aluminum alloys for structural applications that can be manufactured by additive manufacturing

A powdered aluminum alloy with optimized alloying elements and production methods addresses the limitations of existing alloys, providing high strength, ductility, and thermal stability for additive manufacturing, suitable for complex structures and high-temperature environments.

JP7562695B2Active Publication Date: 2024-10-07AM METALS GMBH
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2022559311
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2020-03-30
Filing Date
2021-03-30
Publication Date
2024-10-07
Estimated Expiration
2041-03-30

AI Technical Summary

Technical Problem

Existing aluminum alloys for additive manufacturing face challenges in achieving high strength, ductility, and thermal stability while avoiding rare and costly alloying elements, and are prone to cracking and poor recyclability, limiting their application in high-temperature environments.

Method used

A powdered aluminum alloy comprising Cu, Zn, or Si/Mg as primary alloying elements, with additional metals like Mo, Nb, Zr, Fe, Ti, Ta, and lanthanides, optimized to have specific weight percentages and minimal Cr or Li content, produced through atomization or mechanical alloying, and processed via selective laser sintering or melting to create crack-free, thermally stable three-dimensional objects.

Benefits of technology

The alloy achieves high yield strength and tensile strength, with minimal cracking and improved corrosion resistance, suitable for high-temperature applications, and reduces production costs by avoiding rare elements, enabling efficient additive manufacturing of complex structures.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007562695000002
    Figure 0007562695000002
  • Figure 0007562695000003
    Figure 0007562695000003
  • Figure 0007562695000001
    Figure 0007562695000001
Patent Text Reader

Abstract

The present invention relates to powdered aluminum alloys having Cu, Zn, or Si / Mg as the most relevant alloying elements, and further having a metal selected from the group M1, which includes Mo, Nb, Zr, Fe, Ti, Ta, V, and the lanthanides, in a content of 1 to 15 wt. %. Such aluminum alloys can be used in additive manufacturing processes such as selective laser melting for high-strength products and three-dimensional objects. The present invention further relates to methods and apparatus for producing three-dimensional objects from such aluminum alloys, methods for producing such powdered aluminum alloys, three-dimensional objects also produced from such powdered aluminum alloys, and specific aluminum alloys.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to special powdered aluminium alloys having Cu, Zn or Si / Mg as most relevant alloying elements, said powdered aluminium alloys having a content of 1-15 wt.% of a metal selected from the group M1 comprising Mo, Nb, Zr, Fe, Ti, Ta, V and the lanthanide elements. The present invention further relates to methods for producing such powdered aluminium alloys, to these methods and to three-dimensional objects produced by the specific aluminium alloys, as well as to methods and apparatus for the additive manufacturing of three-dimensional objects. [Background technology]

[0002] Light metal components have been the subject of intensive research in the manufacture of vehicles, particularly automobiles, with the goal of continually improving vehicle performance and fuel efficiency. Many light metal components for today's automotive applications are made from aluminum and / or magnesium alloys. Such light metals can form load-bearing components that must be strong, rigid, and have good strength and ductility (e.g., elongation). High strength and ductility are particularly important for the safety requirements and robustness of vehicles such as automobiles. Traditional steel and titanium alloys offer high temperature resistance, but these alloys are either heavy or relatively expensive, respectively.

[0003] A cost-effective alternative to light metal alloys for forming vehicle structural components are aluminum-based alloys, which can be conventionally processed into desired components by extrusion, rolling, forging, stamping, or casting techniques such as die casting, sand casting, investment casting, gravity die casting, and other bulk forming processes.

[0004] High-strength aluminum alloys with sufficient plastic elongation to absorb energy are already known from the state of the art, mainly from the field of wrought alloys. Here, we mainly discuss materials of the aluminum 2000, 6000 and 7000 series. These materials are characterized by a relatively soft ductile aggregate state that allows forming. With the help of the energy introduced by extensive forming and subsequent heat treatment, the alloys are transformed into a high-strength, fully hardened state.

[0005] In recent years, "rapid prototyping" or "rapid tooling" has also gained importance in metal processing. These processes are also known as selective laser sintering and selective laser melting. In this process, thin layers of material in powder form are repeatedly applied and the material is selectively solidified in each layer in the areas where the future product will be placed by exposure to a laser beam, where the material is first melted and then solidified in place. In this way, complete three-dimensional objects can be built up in succession.

[0006] A method for producing a three-dimensional object by selective laser sintering or selective laser melting and an apparatus for carrying out this method are disclosed, for example, in EP 1 762 122 A1.

[0007] For processing by selective laser sintering or laser melting, alloys are required in which the precipitation mechanism operates without prior cold forming. Such alloys are known in particular in the field of 2000 series alloys (i.e. aluminum-copper alloys). However, relatively long melting intervals pose problems for these alloys, since hot cracks can occur in the structure as a result of rapid solidification due to the low-melting eutectic, which cannot tolerate unaffected shrinkage stresses during solidification of the structure. In the case of processing by selective laser sintering, usually only microcracked structures are obtained, whereby conventional high-strength wrought aluminum alloys cannot yet be processed by additive manufacturing.

[0008] Other available aluminum alloys for which processing using additive manufacturing techniques (such as those from the AlSi alloy family) are already established do not have the desired combination of high yield strength and elongation at break properties, or are very costly and disadvantaged due to rare alloying elements.

[0009] Examples of aluminum alloys containing rare alloying elements are described, for example, in EP 3181711 A1, where aluminum is alloyed with a relatively high amount of Sc (0.6 to 3 wt.%). In alloys produced in this way, the intermetallic Al-Sc phase has a strong strength-increasing effect, whereby yield strengths of >400 MPa are achieved. However, in addition to the relatively costly metallic Sc ​​required for the alloy, the alloy described in EP 3181711 A1 has the disadvantage that it is not suitable for application temperatures >180°C, since the AlMg matrix is ​​soft and prone to creep.

[0010] Another approach for alloys to use in additive manufacturing is the conception of Al-MMC (MMC = matrix metal composites), which at room temperature have mechanical properties comparable to AlMgSc alloys. However, the problem with these materials is that they lose a great deal of strength at temperatures above 200 °C. Another problem with the conception of Al-MMC is that the material consists of a powder mixture of three components, which makes it difficult to transport, store and reuse, since changes in the mixing ratio due to physical processing cannot be excluded. Furthermore, detrimental is the negative recycling behavior of MMC metal ceramic composites and the fact that mechanical reworking of Al-MMC is more difficult and associated with high costs.

[0011] Based on the above-mentioned state of the art, there is a need for aluminum alloys that are as cheap as possible, thermally stable, have high strength properties, and can be fabricated into three-dimensional objects with high strength, stiffness and favorable corrosion properties using additive manufacturing techniques such as selective laser sintering or selective laser melting. Rare earth metals, such as scandium, that are in short supply on the market should be avoided if possible to ensure a high level of security of supply. There is also a need for additive processing methods for producing three-dimensional objects, and for high-strength three-dimensional objects produced by these methods. Summary of the Invention

[0012] This problem is solved by a powdered aluminum alloy according to claim 1, a method for producing a three-dimensional object according to claim 9, a method for producing a powdered aluminum alloy according to claim 8, a three-dimensional object according to claim 11 which is produced with the powdered aluminum alloy according to claim 1, an apparatus for carrying out the method for producing a three-dimensional object according to claim 14 and an aluminum alloy according to claim 15. Preferred embodiments of the invention are set out in the dependent claims.

[0013] The powdered aluminum alloy according to the invention is a powder for use in the manufacture of three-dimensional objects using additive manufacturing techniques. The powdered aluminum alloy according to the invention has a content of 1 to 15% by weight of metals selected from group M1, which contains Cu, Zn, or Si / Mg as the most relevant alloying elements, and furthermore contains Mo, Nb, Zr, Fe, Ti, Ta, V and lanthanide elements. This aluminum alloy is expediently free of relevant portions of Cr or Li (i.e. less than 0.3% by weight, preferably less than 0.15% by weight, even more preferably less than 0.1% by weight of the total portion of Cr and / or Li, in particular, and most preferably free of unavoidable impurities and portions exceeding Cr and / or Li). It should be noted that if the aluminum alloy contains Cr and / or Li, the total content of the metals of group M1 plus Cr and Li is within a specific range of 1 to 15% by weight, or within a corresponding more preferred range. [Brief description of the drawings]

[0014] [Figure 1] FIG. 1 is a schematic diagram illustrating an apparatus for layer-by-layer build-up of a three-dimensional object according to one embodiment of the present invention. [Diagram 2] FIG. 1 shows a comparison of yield strength between specimens made of an aluminum alloy according to Example 1 of the present invention and specimens made of other materials. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0015] The indication "aluminium alloy" should be understood in the context of this specification to mean that the alloy comprises aluminium as the most essential metallic element, the portion of which in the aluminium alloy is greater than 60% by weight, preferably greater than 70% by weight, and even more preferably greater than 80% by weight. The indication "Cu, Zn or Si / Mg as most relevant alloying elements" should be understood to mean that the portion of Cu, Zn or Si / Mg is greater than the respective portion of all other elements (except aluminium), where Si / Mg indicates the total content of Si and Mg in the alloy. In this case, the sum of the portions of Si and Mg is greater than the respective portion of all other elements (except aluminium) in the alloy. The "most relevant alloying element" refers to the aluminium alloy itself, i.e. without taking into account additional metals from group M1 contained in the composition according to the invention, but is preferred when the portion of Cu or Zn is greater than the respective portion of all other elements (except aluminium) in the alloy containing metals from group M1.

[0016] In this context, those skilled in the art will recognize that AlCu alloys (i.e., Cu is the most relevant alloying element) are also referred to as 2000 series aluminum alloys, AlZn alloys (i.e., Zn is the most relevant alloying element) are also referred to as 7000 series aluminum alloys, and AlSi / Mg alloys (i.e., "Si / Mg" is the most relevant alloying element) are also referred to as 6000 series (according to the International Alloy Designation System) aluminum alloys. For an overview of aluminum alloys classified in this category, see e.g. You can refer to “https: / / en.wikipedia.org / wiki / aluminium_alloy#alloy_designaitions”.

[0017] The mixing of metals from the M1 group allows the production of essentially or completely crack-free three-dimensional objects by additive manufacturing techniques such as selective laser sintering or selective laser melting, but with the addition of relatively large amounts of transition metals. This is surprising, since in conventional aluminum processing techniques it is usually not possible to increase the alloy content of these transition metals beyond the prescribed limits (for example in the range of 0.1 to 0.3% by weight). Such an increase leads to a decrease in ductility, loss of processability, and the production of only very coarse structural parts. In the production of three-dimensional bodies and three-dimensional objects by the additive manufacturing techniques described here, this problem is avoided, since the shaping does not require a higher than average ductility of the material, the processing is very fine, and even nanoscale structures can be produced.

[0018] As a preferred portion of metals from group M1, a portion of at least 1.3% by weight, preferably from 2.0% to 8.0% by weight, more preferably from 2.5% to 5.0% by weight, can be given. Alternatively or in addition, the metal or metals selected from group M1 do not consist of a substantial portion of lanthanides, the acquisition of which can be costly, and the portion of lanthanides relative to the total amount of group M1 is preferably less than 10% by weight, more preferably less than 5% by weight, even more preferably less than 1% by weight. Preferred metals from group M1 are readily available and inexpensive metals such as Zr, Fe, and Ti, with Zr and / or Ti being shown to be particularly suitable. For Zr, a portion of 0.25 to 2% by weight, in particular 0.5 to 1.9% by weight, can be shown to be particularly suitable. Similarly, for Ti, a portion of 0.25 to 2% by weight, in particular 0.5 to 1.9% by weight, can be shown to be particularly suitable. It is particularly preferred if the aluminium alloy contains Zr and Ti as metals of group M1, which are each present in the aluminium alloy in a proportion of 0.25 to 2% by weight, in particular 0.5 to 1.9% by weight.

[0019] Preferably, the aluminium alloy according to the invention does not contain any relevant portion of Sc or Y, since these metals are associated with serious cost penalties. Therefore, the preferred aluminium alloy according to the invention contains up to 1.5 wt.% Sc and / or Y, preferably up to 1 wt.%, even more preferably up to 0.5 wt.%, and more preferably the amount of Sc and Y does not exceed the usual impurities.

[0020] In the context of this description, a particularly suitable powdered aluminum alloy is one having a Cu content of 4-6 wt.-%; Mg content of 0.1-1.5 wt.-%; and Ag content of 0.1-1 wt.-%. For this alloy, taking into account these elements and those from group M1, the remaining proportion up to 98 wt.-% of the alloy, preferably up to 99 wt.-% of the alloy, is accounted for by aluminum. In this case, the remaining proportion up to 100 wt.-% of the alloy is usually provided by other metals and / or nonmetals such as oxygen, which do not significantly affect the mechanical properties of the alloy.

[0021] In a particularly preferred embodiment, the above-mentioned aluminum alloy according to the invention has a Cu content of at least 4.5% and / or at most 5.8%, preferably at least 4.8% and / or at most 5.5%, Mg content of at least 0.2% and / or at most 1.5%, preferably at least 0.3% and / or at most 1.2%, and Ag content of at least 0.05% and / or at most 0.6%, preferably at least 0.2% and / or at most 0.4%. Alternatively or in addition, the above-mentioned aluminum alloy according to the invention preferably contains up to 0.2%, in particular 0.05-0.15%, by weight of oxygen, up to 0.6%, in particular 0.2-0.55%, by weight of manganese, and up to 0.3%, preferably 0.05 to 0.15%, by weight of silicon.

[0022] In a further particularly preferred embodiment, the above-mentioned aluminum alloy according to the invention has a content of at least 0.2% and / or at most 1.3% by weight, preferably at least 0.3% and / or at most 1.0% by weight, of Si, at least 0.4% and / or at most 2.2% by weight, preferably at least 0.6% and / or at most 1.8% by weight, and of at least 0.3% and / or at most 1.3% by weight, preferably at least 0.4% and / or at most 1.0% by weight of Mg. This aluminum alloy preferably has a total content of Si and Mg in the range of 0.9-2.8% by weight, in particular in the range of 1.2-2.5% by weight.

[0023] It has been found that for the above-mentioned aluminum alloys, the desired mechanical properties can be adjusted by heat treatment in products manufactured therefrom by additive manufacturing. By selecting the alloying elements, the electrochemical rest potential of the base material can also be shifted to a more noble value compared to the precipitates, resulting in a higher corrosion resistance and a significantly reduced susceptibility of the alloy to stress cracking.

[0024] With regard to the particle size, the powdered aluminum alloy according to the invention is not subject to any significant restrictions, and the particle size should be of a size suitable for additive processes for the production of three-dimensional objects. As suitable particle sizes, an average particle size d50 in the range of 0.1 to 500 μm, preferably at least 1 and / or at most 200 μm, particularly preferably at least 10 and / or at most 80 μm, can be given. An average particle size d50 in the range of 10 to 80 μm is very particularly preferred.

[0025] As will be further indicated below, the powdered aluminum alloy according to the invention may also be in the form of a wire, for example for certain processing operations, whereby the corresponding wire-shaped aluminum alloy is also the subject of the present invention.

[0026] d50 represents the size at which the amount of particles by weight with a diameter smaller than the specified size is 50% of the mass of the sample. Conventionally, and in the context of the present invention described herein, particle size distribution is determined by laser scattering or laser diffraction, for example according to ISO13320:2009. In some cases, the diameter of a single particle can be the respective maximum diameter (= the maximum of all distances between two points of the particle) or sieve diameter, or volume-equivalent sphere diameter.

[0027] As mentioned above, by including elements from group M1, the tendency of the material to form stress cracks can be significantly reduced and ideally stress cracks are completely avoided. For this purpose, it is not necessary to include ceramic materials mentioned for a similar purpose. The powdered aluminum alloy according to the invention therefore contains as little as possible additional ceramic compounds, in particular metal borides, metal nitrides and metal carbides. The portion of such materials in the aluminum alloy is therefore expediently limited to less than 0.2% by weight, in particular less than 0.1% by weight and even more preferably less than 0.05% by weight. Also, nanoparticulate metals or metal hydrides (for example Zr, Hf or ZrH2 with a particle size of up to 5 μm), described elsewhere in the prior art to avoid stress cracks, are not necessary for the purposes of the powdered aluminum alloy according to the invention, whereby their portion should be within the limits indicated for metal borides, metal nitrides and metal carbides or ceramic additives. It is particularly advantageous if no corresponding materials are added to the powdered aluminum alloy according to the invention for or during its processing.

[0028] The powdered aluminum alloy according to the invention can be produced by any method known to the skilled person for the production of powdered alloys. Particularly useful processes include, for example, atomization or mechanical alloying of liquid aluminum alloys. Thus, in a further aspect, the invention relates to a method for producing powdered aluminum alloys, comprising the step of atomizing the liquid alloy at a temperature of >850°C, preferably >950°C, more preferably >1050°C. Temperatures above 1200°C are not necessary for atomization and are undesirable due to the high energy requirements. Therefore, the range from >850 to 1200°C, preferably >950 to 1150°C, can be identified as a particularly preferred temperature range for atomization. It is necessary to ensure by sufficient superheating of the melt or by process control that the abovementioned temperatures run constantly at the nozzle to prevent undesirable primary precipitation. The production of powdered aluminum alloys by atomization is associated with the advantage that the additive metals of group M1 are dissolved in the aluminum alloy or are present as metastable phases. During the subsequent processing by laser sintering or laser melting, these phases dissolve and the metals have a grain refining effect.

[0029] The powdered aluminum alloy according to the invention can also be produced by mechanical alloying. In this method, the metal powders of the individual components of the latter alloy (or premixtures thereof) are intensively mechanically processed and homogenized to the atomic level. For particle modification, it is possible to post-treat the particles obtained after mechanical alloying, for example to change the morphology, particle size, particle size distribution or to carry out surface treatments. The post-treatment can comprise one or more steps selected from chemical modification of the particles and / or particle surfaces, sieving, crushing, rounded grinding, plasma spheroidization (i.e. processing to round particles) and additive treatment. Here, a modification of the particle morphology or particle size distribution in particular is recommended, since plates or flakes are usually obtained in mechanical alloying. This morphology is generally problematic for subsequent additive processing methods.

[0030] Furthermore, the invention relates to powdered aluminum alloys obtainable by the described process, preferably by atomization of the liquid alloy at temperatures >850° C., more preferably >1050° C., or by mechanical alloying with optional post-treatment, where reference is also made to the above explanations of the preferred embodiments of atomization, mechanical alloying and optional post-treatment.

[0031] Also disclosed below is a powdered aluminium alloy for use in the manufacture of three-dimensional objects with the aid of additive manufacturing techniques, which in addition to aluminium contains as most relevant alloying elements Cu, Zn or Si / Mg, and further has a content of 1-15% by weight of a metal selected from group M1, which contains Mo, Nb, Zr, Fe, Ti, Ta, V, the lanthanide elements and Li. The preferred embodiments disclosed above for the aluminium alloy according to the invention are likewise considered to be preferred for this powdered aluminium alloy.

[0032] Another aspect of the invention relates to a method for manufacturing a three-dimensional object by an additive manufacturing process (i.e. a process in which an object is built up layer by layer). The object is manufactured by applying build-up material layer by layer at a position in each layer that is preferably related to a cross-section of the object in that layer and selectively solidifying the build-up material, in particular by supplying radiant energy. Preferably, the position is scanned with at least one irradiation area, in particular the radiation irradiation area of ​​an energy beam, or the build-up material is introduced into the radiation impact area, melted and applied to the substrate. In the context of the invention described herein, the build-up material comprises the powdered aluminum alloy described above, but may alternatively comprise the corresponding wire-shaped aluminum alloy. Preferably, the build-up material comprises said powdered or wire-shaped aluminum alloy.

[0033] The three-dimensional object may be an object made of one material (i.e., an aluminum alloy) or may be an object made of different materials. If the three-dimensional object is an object made of different materials, the object may be produced, for example, by applying the aluminum alloy of the present invention to a substrate of another material.

[0034] In the context of this method, it is useful to preheat the powdered aluminum alloy before selective solidification, with preheating to a temperature of at least 110°C being given as preferred, with preheating to a temperature of at least 120°C, more preferably at least 130°C, more preferably at least 150°C, more preferably at least 165°C, more preferably at least 190°C. On the other hand, preheating to very high temperatures places considerable demands on the apparatus for producing the three-dimensional object, i.e. at least the container in which the three-dimensional object is formed, whereby a temperature of at most 400°C can be defined as a reasonable maximum temperature for preheating. Preferably, the maximum temperature for preheating is equal to or lower than 350°C, more preferably equal to or lower than 300°C. The temperatures indicated for preheating respectively indicate the temperatures to which the build platform on which the powdered aluminum alloy is applied and the powder bed formed by the powdered aluminum alloy are heated.

[0035] The layer-by-layer application or deposition layer is advantageously carried out with a layer thickness suitable for processing by additive manufacturing, for example a layer thickness in the range of 20-60 μm, preferably at least 25 and / or at most 50 μm thick, further preferably at least 30 and / or at most 40 μm thick.

[0036] As mentioned above, the method according to the invention can also be configured in such a way that the build-up material is introduced into the radiation exposure area of ​​an energy source, e.g. a laser, and melted by the laser and applied to the substrate. In such a method, also called laser cladding in the mode of powder build-up welding, the powder is spot sprayed onto the substrate through one or more nozzles, and the laser is simultaneously aligned to the application point of the laser. Due to the radiant energy, the substrate is partially melted and the applied alloy powder melts, whereby the applied alloy can be bonded to the molten substrate. In this way, a layer of granular material is applied to the workpiece and bonded to the surface layer of the workpiece. By successively "spraying" molten layers of granular material, larger workpieces can thus be produced.

[0037] Alternatively, the laser coating process can also be carried out in the mode of a wire build-up welding method, where a wire is used instead of the powder. The method according to the invention therefore also includes an embodiment in which a wire made of an aluminium alloy is used, as described above.

[0038] It has further been found, with regard to the method according to the invention, that the heat treatment of the produced three-dimensional object can significantly improve its physical properties, for example in particular tensile, strength and / or yield strength. Presumably, this effect is due to a microstructural rearrangement of the alloy of the initially formed three-dimensional object. To this end, it is therefore preferred that the method according to the invention further comprises a step of subjecting the initially formed three-dimensional object to a heat treatment, preferably at a temperature between 400°C and 500°C and / or for a time between 20 and 200 minutes. Particularly preferred temperature ranges can be mentioned in the range between 420°C and 470°C, in particular at least 430°C and / or up to 450°C. Particularly preferred time frames for the heat treatment are between 30 and 120 minutes, in particular at least 40 minutes and / or up to 80 minutes. Furthermore, it has been found that such heat treatment provides particularly advantageous results if, after such heat treatment at a relatively high temperature, the three-dimensional object is cooled rapidly (i.e. within 10 minutes, preferably within 5 minutes, for example by water quenching) to about ambient temperature and then aged at a temperature between 90°C and 150°C, in particular at least 110°C and / or up to 140°C, for at least 12 hours, preferably 18 hours.

[0039] Another aspect of the invention relates to a three-dimensional object manufactured using a powdered aluminum alloy, in particular manufactured according to the method described above. The powdered aluminum alloy is an aluminum alloy as described above, and the three-dimensional object comprises or consists of such an aluminum alloy. The use of the alloy described above in the manufacture of such objects results in a very good "as-built" surface, whereby subsequent post-treatment of the surface (e.g. smoothing) can be minimized.

[0040] The three-dimensional object according to the invention has advantageously adapted mechanical properties, such as in particular a yield strength of at least 400 MPa and / or at most 550 MPa, preferably at least 440 MPa to 550 MPa, particularly preferably 460 to 480 MPa, and / or a tensile strength of 450 MPa and / or at most 550 MPa, preferably at least 470 MPa, particularly preferably in the range of 500 to 550 MPa. These respective yield strengths and strengths should be determined in accordance with EN ISO 6892.1 (2011) within the scope of the invention described herein. Alternatively or additionally, the three-dimensional object according to the invention preferably has a yield strength of at least 330 MPa, more preferably at least 350 MPa, even more preferably in the range of 360 MPa to 420 MPa, preferably at 200 ° C.

[0041] Another aspect of the invention relates to a manufacturing apparatus for carrying out the method for manufacturing a three-dimensional object as described above, the apparatus comprising a laser sintering or melting apparatus, a process chamber configured as an open container having a container wall, a support disposed within the process chamber, a storage container, and a horizontally movable coater, where the process chamber and the support are vertically movable relative to one another, and where the storage container is at least partially filled with a powdered aluminum alloy as described above.

[0042] The invention likewise relates to a manufacturing apparatus for carrying out a method for manufacturing a three-dimensional object, said manufacturing apparatus comprising a device for laser coating, a processing chamber, a supply device for supplying granular material or a wire to the irradiation area of ​​the laser, and a storage container at least partially filled with the above-mentioned powdered aluminum alloy or a wire of such an aluminum alloy.

[0043] Additive manufacturing apparatus and related methods for producing three-dimensional objects are generally characterized by the fact that the object is produced layer by layer by solidification of shapeless (or wire-shaped) build-up material. Solidification can be brought about by, for example, selective laser sintering ("SLS" or "DMLS"), or laser melting, or electron beam melting, by supplying thermal energy to the build-up material, for example by irradiating it with electromagnetic or particle radiation.

[0044] For example, in laser sintering or laser melting, the irradiated area of ​​a laser beam on a layer of build-up material ("laser spot") moves over those points of the layer that correspond to the object cross-section of the object to be produced in the layer. Instead of the application of energy, selective solidification of the applied build-up material can also be performed by 3D printing, for example by applying an adhesive or binder. In general, the invention relates to the production of objects by layer-by-layer application and selective solidification of build-up material, regardless of the way in which the build-up material is solidified.

[0045] Further features and embodiments of the invention can be found in the description of exemplary embodiments using the attached drawings.

[0046] FIG. 1 shows a schematic, partially reproduced in cross section, view of an apparatus for the layer-by-layer construction of a three-dimensional object according to one embodiment of the present invention.

[0047] The device shown in FIG. 1 is a laser sintering or laser melting device a1 known per se. It comprises a process chamber a3 with a chamber wall a4 for the construction of the object a2. In the process chamber a3 an upwardly open build vessel a5 with a wall a6 is arranged. A working surface a7 is defined by the upper opening of the build vessel a5, the area of ​​the working surface a7 lying within the opening which can be used for the construction of the object a2 is called the construction area a8. In the vessel a5 a support a10 movable in a vertical direction V is arranged, to which a substrate a11 is attached, which closes the build vessel a5 at the bottom and thus forms its bottom. The substrate a11 can be a plate formed separately from the support a10, which is attached to the support a10, or it can be formed integrally with the support a10. Depending on the powder and the process used, a build platform a12 on which the object a2 is constructed can also be attached to the substrate a11. However, the object a2 can also be built on the substrate a11 itself, which serves as the build platform. In Fig. 1, the object a2 to be formed in a build container a5 on a build platform a12 is shown below a working surface a7 in an intermediate state with several solidified layers surrounded by build-up material a13 that remains unsolidified. The laser sintering apparatus a1 further comprises a storage container a14 for a powdered build-up material a15 that can be solidified by electromagnetic radiation, and a coater a16 movable in a horizontal direction H to apply the build-up material a15 to a build area a8. The laser sintering apparatus a1 further comprises an irradiation device a20 having a laser a21 that generates a laser beam a22 as an energy beam, which is deflected via a deflection device a23 and focused by a focusing device a24 on the working surface a7 through a coupling window a25 attached to the upper side of the wall a4 of the process chamber a3.

[0048] The laser sintering apparatus a1 also comprises a control unit a29, which controls the individual components of the apparatus a1 in a coordinated manner to carry out the build process. The control unit a29 may include a CPU, whose operation is controlled by a computer program (software). The computer program can be stored separately from the apparatus on a storage medium and loaded from there into the apparatus, in particular into the control unit. In operation, to apply the powder layer, the support a10 is first lowered by a height corresponding to the desired thickness. By moving the coater a16 on the working plane a7, a layer of powder build-up material a15 is then applied. For safety, the coater a16 extrudes in front of it a slightly larger amount of build-up material a15 than is necessary to build up the layer. The coater a16 extrudes the planned excess build-up material a15 into an overflow container a18, which is arranged on both sides of the build container a5. The application of the powder build-up material a15 is performed at least over the entire cross section of the object a2 to be produced, preferably over the entire build area a8, i.e. over the area of ​​the working surface a7 that can be lowered by the vertical movement of the support a10. The cross section of the object a2 to be produced is then scanned in a beam emission area (not shown) by the laser beam a22, which represents diagrammatically the intersection of the energy beam with the working plane a7. Thereby, the powder build-up material a15 is solidified at points corresponding to the cross section of the object a2 to be produced. These steps are repeated until the object a2 is completed and can be removed from the build vessel a5. The laser sintering apparatus a1 further comprises a gas supply channel a32, a gas inlet nozzle a30, a gas outlet opening a31 and a gas exhaust channel a33, preferably for generating a laminar process gas flow a34 in the process chamber a3. The process gas flow a34 moves horizontally across the build area a8. The gas supply and exhaust may also be controlled by a control unit a29 (not shown). The gas extracted from the processing chamber a3 is sent to a filter device (not shown), and the filtered gas is returned to the processing chamber a3 via the gas supply channel a32, thereby forming a recirculation system with a closed gas circuit.Instead of only one gas inlet nozzle a30 and one gas outlet opening a31, several nozzles or openings can be provided in each case.

[0049] In the device according to the invention, the reservoir a14 is at least partially filled with powdered aluminum alloy a15 as described above.

[0050] Finally, another embodiment of the invention relates to an aluminium alloy having 4-6% by weight Cu, 0.1-1.5% by weight Mg and 0.1-1% by weight Ag, and a metal selected from the group M1 comprising Mo, Nb, Zr, Fe, Ti, Ta, V and the lanthanides in a content of 1.3-15% by weight, preferably with the remainder up to 99% by weight of the alloy being made up by aluminium, more preferably with the remainder up to 100% by weight of the alloy being made up by aluminium, manganese, silicon and oxygen.

[0051] The present invention is further illustrated by a number of examples, which should not be construed as determining the scope of protection of the present application.

[0052] Example 1: Various aluminium alloys having the compositions shown in Table 1 were processed into specimens by direct metal laser sintering (DMLS). The specimens produced in this way were investigated with regard to their hardness, yield strength and tensile strength at 23°C. The results of these tests are also shown in Table 1.

[0053] [Table 1]

[0054] The specimens produced to determine the hardness were subjected to the Brinell method according to the standard DIN EN ISO 6506-1:2015 "Metallic materials - Brinell hardness test - Part 1: Test method". Density cube specimens were used for the determination. The test was performed three times for each specimen and the measured values ​​are given with an accuracy of 1 HBW.

[0055] The specimens produced with comparative sample 1 showed a large amount of hot cracks. In comparative sample 2, the hot cracks were significantly reduced compared to comparative sample 1, but were still visible; the heat treatment of the specimens did not lead to an improvement in the hardness of the material. The material according to the invention showed no hot cracks and significantly improved mechanical properties compared to these immediately produced comparative samples. Heat treatment (485°C / 40 min, followed by water quenching and ageing at 25°C) made it possible to significantly improve these properties.

[0056] Example 2: Specimens made of aluminum alloy according to Example 1 (-●-) were compared with corresponding specimens made of other materials with regard to their yield strength properties. As comparison materials, specimens made of Skalmalloy (DMLS processed, -◇-), aluminum alloy AW2618 (forged, T6, -□-), aluminum alloy 7075 (T6, -▲-), aluminum alloy 2024 (T6, -×-) and Adaloy (DMLS processed, -○-) were used. Data for the comparison materials are taken from the literature or from the corresponding data sheets. The yield strengths of the test specimens made of these materials are shown in Figure 2.

[0057] From FIG. 2 it is clear that the aluminum alloy according to the invention already had the highest yield strength of all the tested materials at 23° C., whereas only Skarmalloy and aluminum alloy 7075 had yield strengths in a similarly high range. In comparison with the high-temperature forging alloy AW-2618A, the difference was about 27%. Above a temperature of about 100-120° C., the yield strength of aluminum alloy 7075 drops sharply, while the yield strength of Skarmalloy drops even more significantly, even at these temperatures. In contrast, the yield strength of the aluminum alloy according to the invention drops only slightly at these temperatures. At about 200° C., the aluminum alloy according to the invention has a yield strength about 42% better than the second best alloy AW2618A. The invention as originally claimed in the present application is set forth below. [1] A powdered aluminum alloy having Cu, Zn, or Si / Mg as the most relevant alloying elements, characterized in that it further has a content of 1 to 15% by weight of a metal selected from the group M1 comprising Mo, Nb, Zr, Fe, Ti, Ta, V and the lanthanide elements. [2] 1. Powdered aluminum alloy according to claim 1, characterized in that it has a content of at least 1.3% by weight, preferably 2.0% by weight, up to 8.0% by weight, further preferably 2.5% by weight, up to 5.0% by weight of metals from group M1, preferably Zr and / or Ti. [3] 1. A powdered aluminum alloy according to claim 1 or 2, characterized in that the alloy contains 4-6 wt. % Cu, 0.1-1.5 wt. % Mg, and 0.1-1 wt. % Ag, with the remaining proportion up to 99 wt. % of the alloy being aluminum. [4] % and / or at most 5.8% by weight, preferably at least 4.8% and / or at most 5.5% by weight of Cu, at least 0.2% and / or at most 1.5% by weight, preferably at least 0.3% and / or at most 1.2% by weight of Mg, and at least 0.05% and / or at most 0.6% by weight, preferably at least 0.2% and / or at most 0.4% by weight of Ag [3]. [5] % by weight, preferably 0.05 to 0.15% by weight of oxygen; up to 0.6% by weight, preferably 0.2 to 0.55% by weight of manganese; and up to 0.3% by weight, preferably 0.05 to 0.15% by weight of silicon. [6] Powdered aluminum alloy according to any one of [1] to [5], characterized in that it has an average particle size d50 in the range of 0.1 to 500 μm, preferably at least 1 and / or at most 200 μm, particularly preferably at least 10 and / or at most 80 μm. [7] A powdered aluminum alloy according to any one of [1] to [5], characterized in that it has a content of metal borides, metal nitrides and metal carbides of less than 0.2% by weight, preferably less than 0.1% by weight, and more preferably 0.05% by weight. [8] A method for producing any one of the powdered aluminum alloys described above, comprising the steps of: A method for the production of powdered aluminium alloys, characterized in that it comprises a step of atomisation of a liquid alloy at a temperature of >850°C, preferably >1050°C, or a step of mechanical alloying and optionally a post-treatment. [9] A method for producing a three-dimensional object, the object being produced by applying build-up material layers layer by layer and selectively solidifying the build-up material, in particular at a location within each layer related to a cross-section of the object within that layer, by supplying radiation energy, preferably by scanning the location with at least one irradiation area, in particular a radiation exposure area of ​​an energy beam, or by introducing the build-up material into the radiation exposure area, melting it and applying it to a substrate, A method for producing a three-dimensional object, wherein the build-up material comprises, or preferably consists of, any one of powdered aluminum alloys [1] to [7] or a corresponding wire-shaped aluminum alloy.

[10] The method of [9], wherein the powdered aluminium alloy is preheated to a temperature of preferably at least 100°C, more preferably at most 400°C.

[11] The method according to [9] or

[10] , wherein the three-dimensional object produced is subjected to a heat treatment, preferably at a temperature of at least 400-500 °C and / or for a duration of 20-200 minutes.

[12] A three-dimensional object produced using a powdered aluminum alloy, in particular produced by the method of [8], wherein the powdered aluminum alloy is any one of the aluminum alloys of [1] to [7], and the three-dimensional object comprises or consists of such an aluminum alloy.

[13] The three-dimensional object according to

[12] , characterized in that it has a yield strength of at least 400 MPa and / or at most 550 MPa, preferably at least 440 MPa, particularly preferably in the range of 460 to 500 MPa, and / or a tensile strength of 450 MPa, preferably at least 470 MPa and / or at most 550 MPa, particularly preferably in the range of 500 to 550 MPa.

[14] A manufacturing apparatus for carrying out the method of [9], comprising a laser sintering apparatus or a laser melting apparatus, a treatment chamber designed as an open container having a container wall, a support body installed in the treatment chamber, a storage container, and a coater movable in a horizontal direction, the treatment chamber and the support body being movable relative to each other in a vertical direction, and the storage container being at least partially filled with a powdered aluminum alloy of any one of [1] to [7].

[15] An aluminium alloy having 4-6 wt% Cu, 0.1-1.5 wt% Mg, 0.1-1 wt% Ag and 1.3-15 wt% of a metal selected from group M1 comprising Mo, Nb, Zr, Fe, Ti, Ta, V and the lanthanides, preferably up to 99 wt% of the alloy being aluminium, more preferably the remaining proportions of aluminium, manganese, silicon and oxygen being 100 wt% of the alloy.

Claims

1. 1. A powdered aluminum alloy of the 2000, 6000 or 7000 series having Cu, Zn or Si / Mg as the most relevant alloying element, further comprising a metal selected from the group M1 comprising Mo, Nb, Zr, Fe, Ti, Ta, V and the lanthanide elements in a content of 1 to 15% by weight, said aluminum alloy containing less than 0.2% by weight of metal borides, metal nitrides and metal carbides.

2. 2. Powdered aluminum alloy according to claim 1, characterized in that it has a content of metals from group M1 between 2.0% and 8.0% by weight.

3. The powdered aluminum alloy according to claim 2, characterized in having a Zr and / or Ti content of 2.0% to 8.0% by weight.

4. 3. The powdered aluminum alloy according to claim 1, characterized in that the aluminum alloy has a Cu content of 4-6 wt.%, a Mg content of 0.1-1.5 wt.%, and an Ag content of 0.1-1 wt.%.

5. A powdered aluminum alloy as described in claim 4, wherein the Cu content is at least 4.5 wt.% and at most 5.8 wt.%, the Mg content is at least 0.2 wt.% and at most 1.5 wt.%, and the Ag content is at least 0.1 wt.% and at most 0.6 wt.%.

6. A powdered aluminum alloy as claimed in claim 4, having an oxygen content of up to 0.2% by weight, a manganese content of up to 0.6% by weight, and a silicon content of up to 0.3% by weight.

7. Powdered aluminium alloy according to any one of the preceding claims, characterized in that it has a mean particle size d50 in the range of 0.1 to 500 μm.

8. A powdered aluminum alloy as claimed in any one of claims 1 to 6, characterized in that the metal borides, metal nitrides and metal carbides are contained in an amount of less than 0.1% by weight.

9. A method for producing a powdered aluminum alloy according to any one of claims 1 to 8, 1. A method for producing a powdered aluminium alloy comprising the steps of atomising a liquid alloy at a temperature >850°C or mechanical alloying.

10. A method for producing a three-dimensional object, the object being produced by applying build-up material layers layer by layer and selectively solidifying the build-up material, in particular at a location within each layer related to a cross-section of the object within that layer, by supplying radiation energy, by scanning at a location with at least one irradiated area or by introducing the build-up material into the radiation irradiated area, melting it and applying it to a substrate, A method for producing a three-dimensional object, wherein the build-up material comprises a powdered aluminium alloy according to any one of claims 1 to 8, or a corresponding wire-form aluminium alloy.

11. 11. The method of claim 10, wherein the powdered aluminum alloy is preheated to a temperature of at least 100°C.

12. Method according to claim 10 or 11, in which the three-dimensional object produced is subjected to a heat treatment at a temperature of at least 400-500°C.

13. A three-dimensional object manufactured using a powdered aluminium alloy according to the method of any one of claims 10 to 12, wherein the powdered aluminium alloy is an aluminium alloy according to any one of claims 2 to 8 containing 2.0 to 8.0 wt. % of a metal of group M1, and the three-dimensional object comprises or consists of such an aluminium alloy.

14. A manufacturing apparatus for carrying out the method according to claim 10, comprising a laser sintering or melting apparatus, a treatment chamber designed as an open vessel with a vessel wall, a support placed in the treatment chamber, a storage vessel and a coater which is horizontally movable, the treatment chamber and the support being vertically movable relative to one another, the storage vessel being at least partially filled with the powdered aluminium alloy according to any one of claims 1 to 8.

15. 1. An aluminum alloy having a content of 4-6 wt.% Cu, 0.1-1.5 wt.% Mg, 0.1-1 wt.% Ag, and a content of 1.3-15 wt.% of a metal selected from the group M1 comprising Mo, Nb, Zr, Fe, Ti, Ta, V and the lanthanide elements, the remaining proportions up to 100 wt.% of the alloy being aluminum, manganese, silicon and oxygen.

Citation Information

Patent Citations

  • Aluminum-based blade material for automobile air-condition compressor and preparation method thereof

    CN106676342A

  • Aluminum particle group and manufacturing method thereof

    JP2017066432A

  • Aluminum alloy product and manufacturing method thereof

    JP2019532176A

  • Production of half-stages of monobloc stator guides by additive manufacturing

    WO2016142631A1

  • Process for manufacturing an aluminum alloy part

    WO2018189458A1