Method for Providing Structural and / or Compositional Modifications of Molecular Semiconductor Target Films - Patent application

The use of a semi-permeable temporary interlayer with thermal, solvent vapor, or optical stimulation addresses the limitations of existing methods by enabling precise structural and compositional modifications in molecular semiconductor films, enhancing their properties for electronic and photonic devices.

JP7562710B2Active Publication Date: 2024-10-07CONSEJO SUPERIOR DE INVESTIGACIONES CIENTIFICAS (CSIC)
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
JP2022577159
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2020-06-15
Filing Date
2021-06-14
Publication Date
2024-10-07
Estimated Expiration
2041-06-14

AI Technical Summary

Technical Problem

Existing methods for local modification of molecular semiconductor films, such as shadow masks, photolithography, dip-pen nanolithography, and mechanical rubbing, suffer from limitations in spatial resolution, throughput, mechanical damage, and complexity, making them unsuitable for efficient production of devices with precise electronic and optical properties.

Method used

A method involving a semi-permeable temporary interlayer is used to deposit a donor layer on a molecular semiconductor film, followed by thermal, solvent vapor, or optical stimulation to activate the diffusion of functional molecules, allowing for precise structural and compositional modifications with spatial resolution below 5 μm, using solvents and stimuli to control the diffusion of functional additives.

Benefits of technology

This method enables controllable and localized modification of molecular semiconductor films with improved properties like electrical conductivity, optical absorption, and chain structure, suitable for various electronic and photonic devices, while maintaining the integrity of the target film.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007562710000002
    Figure 0007562710000002
  • Figure 0007562710000003
    Figure 0007562710000003
  • Figure 0007562710000004
    Figure 0007562710000004
Patent Text Reader

Abstract

The present invention relates to a method for providing structural and / or compositional modification of molecular semiconductor target films by thermal, solvent vapor, or light stimulation that locally activates the diffusion of functional molecules of a solution-deposited donor layer into the molecular semiconductor target film through a semipermeable temporary intermediate layer. Thus, the present invention can be included in the fields of fabrication of electronic, optoelectronic, and photonic devices, and structures based on molecular semiconductor materials.
Need to check novelty before this filing date? Find Prior Art

Description

Detailed Description of the Invention

[0001] The present invention relates to a method for providing structural and / or compositional modification of a molecular semiconductor target film by thermal, solvent vapor or light stimulation that locally activates diffusion of functional molecules of a solvent-deposited donor layer through a semi-permeable temporary intermediate layer into the molecular semiconductor target film.

[0002] Thus, the present invention may be included in the fields of fabrication of electronic, optoelectronic, photonic devices and structures based on molecular semiconductor materials.

[0003] [Background technology] Molecular semiconductors exhibit electronic and optical properties that stem from their specific chemical structure, which may, for example, in the case of organic (polymeric) molecular semiconductors, contain π-conjugated (hetero)aromatic moieties. In a wide range of existing and new applications, molecular semiconductors are generally used in the form of thin solid films with thicknesses ranging from a few nanometers to a few micrometers (see, for example, M. Eslamian, Nano-Micro Lett. 9, 3 (2017)). A wide range of solution-based processing schemes, performed vacuum-free, are highly desirable to enable energy- and cost-efficient manufacturing and are actively developed in this field.

[0004] Besides the deposition of the molecular semiconductor layer, local modification of the molecular material is often required at critical points in the fabrication as part of the fabrication process for a wide range of devices in order to achieve specific device functionality. For example: Local modification of material composition is required, for example, to define highly electrically conductive film regions of electrodes and wiring in thin film transistors (TFTs) by local doping or to structure light-emitting elements in light-emitting diodes (LEDs).

[0005] Local modifications are required in terms of crystallinity and, in the case of polymeric materials, chain-like structures, short-range molecular alignment, for example with the aim of defining film regions exhibiting different charge carrier mobilities or refractive indices.

[0006] · Localized manipulation of long-range molecular alignment through (hyper)molecular orientation is required to define film regions that exhibit anisotropic optical, electronic, thermal and mechanical properties.

[0007] The most recent methods of solvent-enhanced dye diffusion in polymer films use shadow masks, whose spatial resolution is determined by the shadow mask (see F. Pschenitzka et al Materials Research Society Symposium Proceedings vol. 665. 31 December 2001 (2001-12-31) and F. Pschenitzka and JC Sturm, Appl. Phys. Lett., Vol. 74, No. 13, 29 March 1999). Hence, the drawback of using a shadow mask is that the spatial resolution is only a few hundred microns. Furthermore, the method using the mask provides only two possible compositions for the target film: one for the covered areas and a given composition for the parts with holes.

[0008] The state-of-the-art technique for localized modification of material compositions is photolithography (see GM Wallraff et al., Chem. Rev. 99, 1801 (1999)). Typical process steps may include (i) spin-coating a photosensitive resist onto the molecular semiconductor film of interest, (ii) baking the photoresist, (iii) exposing the desired spatial pattern onto the photoresist, (iv) developing the photoresist, (v) performing the desired treatment on the layer of interest, and (vi) removing the residual photoresist. Although photolithography offers spatial resolution down to the micrometer scale, the disadvantages of photolithography include the complex multi-step process mentioned above, which reduces throughput and therefore increases costs. Further disadvantages are related to the additive or subtractive modifications in nature, which often require subsequent backfilling to restore the format of the planar film for integration into devices, as well as the property of delamination of adjacent layers upon aging or bending. In most cases, photoresists and target layers of a similar nature are not necessarily indifferent to the solvents used, i.e., a typical photoresist deposition can at least partially dissolve or swell the underlying target layer modifying its properties.

[0009] The state-of-the-art technique for localized modification of short-range molecular alignment is dip-pen nanolithography (see A. Perevedentsev et al., Nat. Commun. 6, 5977 (2015)). The typical process involves the localized deposition of a solvent ink onto a target molecular semiconductor film via an atomic force microscope (AFM) tip. Although dip-pen nanolithography offers spatial resolution down to the micrometer scale, drawbacks of dip-pen nanolithography include slow typical writing speeds of micrometers per second, as well as the need for careful control of the tip-film separation to allow ink deposition without simultaneous mechanical damage of the target film.

[0010] The state-of-the-art technique for local modification of long-range molecular alignment is mechanical rubbing (see L. Hartmann et al., Adv. Funct. Mater. 21, 4047 (2011)). A typical process involves directional rubbing of a molecular semiconductor film of interest using a spinning wheel coated with a microfiber cloth. Although mechanical rubbing offers rapid process speeds, the drawbacks of mechanical rubbing include the tendency to mechanically damage the film of interest, low spatial resolution (typically on the scale of a few millimeters) and the inability to form complex patterns.

[0011] It is therefore necessary to develop new methods for structurally and / or compositionally modifying molecular semiconductor layers.

[0012] Summary of the Invention The problem to be solved by the process of the present invention is to provide a versatile method for the fabrication of a wide range of devices and structures based on molecular materials, in particular molecular semiconductors. In particular, the process of the present invention aims to provide a method for structurally and / or compositionally modifying (with a spatial resolution of less than 5 μm) molecular semiconductor target films in order to modify properties / characteristics in the molecular semiconductor target films, such as material composition, molecular orientation, chain structure and crystallinity, for example with respect to optical and electronic properties such as light absorption / emission, refractive index, electrical conductivity, etc.

[0013] The method is directed to the fabrication of electronic devices and structures in the field of molecular electronics, such as, for example, waveguides, diffraction gratings, LEDs, TFTs, security elements for banknotes and personal IDs, photodetectors, thermoelectric generators, wearable electronics, and photonic devices and structures. The modified molecular semiconductor target films are suitable for use as part of electronic and / or photonic devices.

[0014] A first aspect of the invention relates to a method for providing structural and / or compositional modifications to a molecular semiconductor target film disposed on a substrate, said method being characterized in that it comprises the following steps: a) depositing a semi-permeable temporary intermediate layer on a surface of said molecular semiconductor film of interest located on a substrate by a solution-based deposition technique; b) depositing a solid donor layer comprising a plurality of functional molecular additives on the semi-permeable temporary intermediate layer obtained in step (a) by a solution-based deposition technique; c) exposing the structure obtained in step (b) to a thermal, solvent vapor, or light stimulus, thereby activating diffusion through the non-perforated, semi-permeable temporary intermediate layer; and d) Chemically or physically removing said solid donor layer and said semi-permeable temporary intermediate layer.

[0015] The term "molecular semiconductor target film" in the present invention refers to a target film to be structurally and / or compositionally modified by the method of the present invention. In the case of organic (polymeric) molecular semiconductors, there are two subclasses: low molecular weight materials and polymers. Both have sp 2 Hybrid orbital p of C atom z They have a conjugated π-electron system formed by orbitals. Compared with the σ-bonds that make up the backbone of the molecule, the π-bonds are significantly weaker. Thus, the lowest electronic excitation of conjugated molecules is generally a π-π transition with an energy gap of 1.5-3 eV, resulting in light absorption or emission in the visible and near-infrared spectral range. Molecular semiconductors, such as polymers, can conduct electricity when they are doped or injected with charge carriers. Molecular semiconductors, which have the electrical and optical properties of semiconductors and the mechanical properties of plastics, are good candidates for developing low-cost, flexible, electronic, optoelectronic, and photonic devices, such as transistors, LEDs, and photodetectors.

[0016] The term "compositional modification" refers to a change in the composition of a molecular semiconductor film of interest.

[0017] As used herein, the term "structural modification" refers to a change in the conformation, crystal structure, crystallinity, or molecular orientation of a molecular semiconductor film of interest.

[0018] In the present invention, structural and / or compositional modification is achieved by introducing functional molecular additives into the molecular semiconductor target film. The term "functional" refers to the ability of said functional molecular additives to induce desired structural and / or compositional modification by specific physicochemical interactions with the target molecular material. Said functional molecular additives should be soluble and have a melting point above 40°C and a molecular weight below about 1500 g / mol to form a solid donor layer.

[0019] Examples of the functional molecular additives include solvents, dyes, luminescent dyes, nucleating agents, crosslinking agents, reactive monomers and catalysts. Preferably, the additives have a molecular weight of less than about 1500 g / mol.

[0020] Examples of said "bio" functional molecular additives are antigens, antibiotics, amino acids and oligopeptides. Preferably, said additives have a molecular weight of less than about 1500 g / mol.

[0021] Other functional molecular additives are electron compounds such as fullerene or non-fullerene electron acceptors, and molecular dopants.

[0022] The term "additive" means that it is added to the target layer, but is not necessarily permanently retained. Depending on the particular structural and / or compositional modification desired, the functional molecular additive may or may not be retained in the resulting modified molecular semiconductor target film. For example, in the case of building chain structures and orientation, the functional molecular additive is then removed by chemical means or sublimation.

[0023] As used herein, the term "donor layer" refers to a layer containing multiple functional molecular additives that are used to induce desired structural and / or compositional modifications in a molecular semiconductor. Preferably, the functional molecular additives of the donor layer are selected from solvents, dyes, luminescent dyes, nucleating agents, crosslinkers, reactive monomers, catalysts, antigens, antibiotics, amino acids, oligopeptides, molecular electron acceptors, molecular electron donors, molecular electrical dopants, or combinations thereof.

[0024] In the present specification, the term "semipermeable temporary intermediate layer" refers to a layer disposed between a molecular semiconductor target film and a donor layer. The semipermeable temporary intermediate layer prevents the functional molecular additive from diffusing into the target layer during deposition of the donor layer containing said functional molecular additive. Thus, the semipermeable temporary intermediate layer should be sufficiently impermeable under the conditions used to deposit the donor layer (temperature and kinetics of solidification of the donor layer) to sufficiently retain the main structural and / or compositional properties of the target layer. On the other hand, the semipermeable temporary intermediate layer allows the multiple functional molecular additives comprising the donor layer to diffuse through the intermediate layer into the molecular semiconductor target film under application of a suitable stimulus. Thus, the semipermeable temporary intermediate layer should be sufficiently permeable under application of the stimulus. Diffusion only occurs under application of the stimulus.

[0025] Therefore, in order for a desired proportion of the functional molecular additive to diffuse through the semipermeable temporary intermediate layer within a time period of less than about 1 minute, the functional molecular additive preferably has a molecular weight of less than about 1500 g / mol.

[0026] The composition of the semi-permeable temporary intermediate layer is preferably selected from a group of polymers that are selectively insoluble in the solvents used in the solution-based deposition of the target molecular semiconductor layer and the donor layer. Thus, for common molecular semiconductors and functional molecular additives that are selectively soluble in aromatic solvents (e.g., toluene or chlorobenzene) and polar aprotic solvents (e.g., acetone or acetonitrile), the semi-permeable temporary intermediate layer should be selected from a group of polymers that are selectively soluble in polar protic solvents such as water or methanol. Examples of semi-permeable temporary intermediate layers include poly(sodium 4-styrenesulfonate), polyvinyl butyral, and polyvinyl alcohol.

[0027] One advantage of the process of the present invention is that due to the presence of the semipermeable temporary intermediate layer, the main characteristics of the molecular semiconductor target film (e.g., photoluminescence spectrum or electrical conductivity) are not modified after solution-based deposition of the temporary intermediate layer and the donor layer. This allows for controllable / localized modification under the application of a subsequent stimulus. The presence of the semipermeable temporary intermediate layer prevents the possibility of subsequent localized modification, since in the absence of the semipermeable temporary intermediate layer, the structural and / or compositional characteristics of the molecular semiconductor target film are modified simultaneously with the deposition of the donor layer.

[0028] The function of the thermal, solvent vapor or light stimulation is to melt and / or dissolve the multiple functional molecular additives in the donor layer and activate the diffusion of a sufficient proportion of the functional additives through the semi-permeable temporary intermediate layer into the molecular semiconductor target film. Not all of the functional molecular additives diffuse into the target layer, only a small portion.

[0029] Step (a) of the present invention refers to depositing a semi-permeable temporary intermediate layer onto a molecular semiconductor film of interest located on a substrate by a solution-based deposition technique. Preferably, the molecular semiconductor film of interest is deposited on the substrate by a solution-based deposition technique, more preferably by spin, blade, spray, or slot-die coating technique.

[0030] The molecular semiconductor target film precursor solution and the substrate may be preheated prior to deposition in step (a).

[0031] Step (b) of the present invention refers to depositing a solid donor layer onto the semi-permeable temporary intermediate layer obtained in step (a) by a solution-based deposition technique. Preferably, step (b) is carried out by spin, blade, spray, or slot-die coating techniques.

[0032] The deposition of the solid donor layer on the semi-permeable temporary intermediate layer in step b) does not change the main characteristics of the molecular semiconductor film of interest. Preferably, if said characteristic is the light emission or material composition, the spectral position of the maximum photoluminescence intensity does not change by more than 10 nm. Preferably, if said characteristic is the electrical conductivity, its value does not change by more than a factor of 100.

[0033] Step (c) of the present invention refers to exposing the structure obtained in step (b) to a thermal, solvent vapor or light stimulus, thereby inducing structural and / or compositional modifications in the molecular semiconductor target film, the stimulus being applied in a rastering mode, scanning the stimulus over the structure obtained in step (b).

[0034] As described above, the function of the thermal, solvent vapor or light stimulation is to melt and / or dissolve the multiple functional molecular additives in the donor layer and activate the diffusion of a sufficient proportion of said functional additives through the semi-permeable temporary intermediate layer into the molecular semiconductor target film.

[0035] In a preferred embodiment of step (c), the structure obtained in step (b) is patternwise exposed to a thermal, solvent vapor or light stimulus, for example, the patternwise scanning (exposure) creates a directional thermal gradient that creates molecular orientation.

[0036] In a more preferred embodiment of step (c), the structure obtained in step (b) is exposed to a thermal stimulus, preferably by means of a hot plate, a hot tip, a hot stamp or hot gas.

[0037] In another more preferred embodiment of step (c), the structure obtained in step (b) is exposed to a solvent vapor stimulus, preferably by a nozzle or a slot die, said solvent being selected from the group of solvents such as acetone or toluene that selectively dissolve or swell materials comprising the donor layer.

[0038] In another more preferred embodiment of step (c), the structure obtained in step (b) is exposed to a light stimulus. The presence of a light absorbing layer is essential for converting the light stimulus into heat. Therefore, in this latter preferred embodiment of step (c), at least the substrate, the molecular semiconductor target film, the semi-permeable temporary intermediate layer or donor layer are light absorbing layers or the substrate on which the molecular semiconductor target film is arranged contains a light absorbing layer. The preferred wavelength of the light stimulus is a wavelength in the ultraviolet to near infrared spectral range that substantially matches the absorption of the given light absorbing layer to enable light-to-heat conversion. Furthermore, the structure obtained in step (b) is exposed to a light stimulus, preferably by a laser or a flash lamp. Pulsed or continuous wave lasers can be used. Furthermore, a shadow mask can be used to modify localized areas of the molecular semiconductor target film. Furthermore, it is also possible to scan the localized areas in a pattern using a laser.

[0039] Step (d) of the present invention refers to chemically or physically removing the solid donor layer and the semipermeable temporary intermediate layer, which is performed without significantly impairing the structural and / or compositional modifications induced in the target molecular semiconductor layer.

[0040] Chemical removal of the solid donor layer and the semi-permeable temporary intermediate layer may be performed by exposure to a solvent selected from the group of solvents that selectively dissolve the materials comprising the donor layer (e.g., acetone or acetonitrile) and the temporary intermediate layer (e.g., water or methanol), which can be selected to be the same as those used for the solution-based deposition of the temporary intermediate layer and the donor layer in steps (a) and (b), respectively.

[0041] Physical removal of the solid donor layer and the semi-permeable temporary intermediate layer may be accomplished by imprinting and lift-off, for example, with a stamp of polydimethylsiloxane (PDMS) elastomer that forms conformal contact.

[0042] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by those skilled in the art to which the present invention belongs. Methods and materials similar or equivalent to those described herein can be used in the practice of the present invention. Throughout the present specification and claims, the term "comprises" and its variations are not intended to exclude other technical features, additives, ingredients, or steps. Additional objects, advantages, and features of the present invention may become apparent to those skilled in the art upon reading the description herein or may be learned by practicing the present invention. The following examples and figures are provided for illustration purposes and are not intended to limit the present invention.

[0043] BRIEF DESCRIPTION OF THE DRAWINGS 1(A)-(E) are schematic cross-sectional diagrams of the main steps for modifying a target layer using thermal stimulation, with corresponding fluorescence micrographs of exemplary target films whose chain structure and luminescence properties have been modified using thermal stimulation.

[0044] 2(A)-(E) are schematic cross-sectional diagrams of the main steps for modifying a target layer using solvent vapor, with corresponding fluorescence micrographs of exemplary target films whose chain structure and luminescence properties have been modified using solvent vapor.

[0045] 3(A)-(B) are schematic cross-sectional views and corresponding fluorescent photographs illustrating modification of the composition and luminescence properties of a subject semiconducting polymer film having modified composition and luminescence properties using solvent vapor stimulation.

[0046] Figure 4(A)-(C) are schematic cross-sectional diagrams of target semiconducting polymer films with spatially varying modifications of composition and emission properties using solvent vapor stimulation, as well as the corresponding fluorescence photographs and photoluminescence spectra.

[0047] 5(A)-(C) are plots of electrical conductivity, optical micrographs, and absorbance spectra of subject semiconducting polymer films whose composition and electrical conductivity were modified using a thermal stimulus.

[0048] 6(A)-(C) are electrical conductivity plots and optical micrographs of target semiconducting polymer films whose composition and electrical conductivity were modified using a co-solvent-assisted thermal stimulus.

[0049] 7(A)-(B) are schematic cross-sectional views showing various means for exposing a sample to a light stimulus.

[0050] Figure 8(A)-(D) are confocal photoluminescence micrographs and Raman intensity ratio images; photoluminescence spectra and plots of pattern characteristics as a function of process parameters for a target semiconducting polymer film whose chain structure has been locally modified by optical stimulation.

[0051] 9(A)-(F) show polarized optical micrographs, polarized Raman spectra, details of an exemplary Raman anisotropy analysis, and plots of Raman anisotropy as a function of process parameters for a target semiconducting polymer film in which chain orientation has been locally modified using photostimulation.

[0052] 10(A)-(B) are polarized optical micrographs of a large area of ​​a target semiconducting polymer film in which chain orientation has been locally modified using photostimulation.

[0053] FIG. 11(A)-(C) are atomic force microscope images and topography analysis of target semiconducting polymer films in which chain orientation was locally modified using light stimulation.

[0054] FIG. 12 is an optical micrograph of a subject semiconducting polymer film in which chain orientation was locally modified using light-based stimulation without the use of a semipermeable temporary intermediate layer.

[0055] 13(A)-(D) are optical micrographs and plots of electrical conductivity as a function of process parameters of target semiconducting polymer films whose composition and electrical conductivity have been modified using optical stimulation; and reference Raman spectroscopy data as a function of electrical conductivity for target films of the same polymer whose composition and electrical conductivity have been modified using thermal stimulation.

[0056] 14(A)-(C) are optical micrographs, Raman intensity ratio images, and plots of electrical conductivity as a function of position of target semiconducting polymer films whose composition and electrical conductivity were modified using photostimulation.

[0057] 15(A)-(B) are optical micrographs and schematic cross-sectional views of an exemplary donor layer where the solution is deposited onto a temporary intermediate layer and an exemplary donor layer where the solution is deposited directly onto a target membrane.

[0058] 16(A)-(B) are cross-sectional views and optical micrographs illustrating the removal of the temporary interlayer by chemical and physical means.

[0059] [Example] (material) The following compounds were purchased from Sigma-Aldrich: "pNaSS": Poly(sodium 4-styrenesulfonate); MW approximately 1,000,000 g / mol "PFO": poly(9,9-dioctylfluorene); MW≧20,000g / mol "P3HT": Poly(3-hexylthiophene); MW approximately 100,000 g / mol, regioregular "PMMA": Poly(methyl methacrylate); MW approximately 15,000 g / mol "Coumarin 334": 10-acetyl-2,3,6,7-tetra-hydro-1H,5H,11H-1-benzo-pyrano[6,7,8-ij]quinolizin-11-one (99%) "Triton X-100": 4-(1,1,3,3-tetramethylbutyl)phenyl-polyethylene glycol The following compounds were purchased from TCI Chemicals:

[0060] Lauric acid (>98%) "BT": 2,1,3-benzothiadiazole (>99%) "BCF": Tris(pentafluorophenyl)borane (>98%) Biphenyl (>99.5%) "DCM": 4-(dicyanomethylene)-2-methyl-6-(4-dimethylaminostyryl)-4H-pyran (>95%) L-(+)-Mandelic acid (>99%) The following compounds were purchased from 1-Material:

[0061] PBTTT-C14: Poly(2,5-bis(3-tetradecylthiophen-2-yl)thieno-[3,2-b]thiophene); molecular weight approximately 50,000g / mol Standard laboratory grade solvents (>99% purity) were used throughout.

[0062] [Table 1]

[0063] (Technology used for characterization) The film thickness was measured using a DektakXT profilometer (Bruker).

[0064] Electrical conductivity was measured using an Ecopia HMS-5000 instrument using the four-point probe van der Pauw technique on a 6×6 mm2 area with silver paste contacts at each corner.2 The measurements were performed on a rectangular membrane having an area of ​​.

[0065] Vis-NIR absorption spectra were recorded using a Bruker Vertex 70 FTIR spectrophotometer coupled to a Bruker Hyperion optical microscope.

[0066] Photoluminescence and Raman scattering spectroscopy was performed using a WITec Alpha 300RA instrument (reflection geometry; continuous wave excitation was used throughout). PL spectra were recorded with excitation at 355 nm or 365 nm (as indicated herein). Raman spectra were recorded with excitation at 488 nm (PBTTT-C14 film), 633 nm (PFO film) and 785 nm (P3HT film). Polarized Raman analysis was performed by synchronously tuning both the excitation and detection polarizations.

[0067] Atomic force microscopy was performed in tapping mode using a Keysight 5500 instrument (Agilent).

[0068] All characterizations were performed at room temperature in air.

[0069] Example 1: Modification of the chain structure and luminescence properties of the target film (2) of PFO by thermal stimulation.

[0070] A schematic diagram of each treatment step and the corresponding optical micrographs recorded under UV irradiation at a wavelength of 365 nm are shown in FIG.

[0071] (1) Base material (2) Molecular semiconductor film (3) A semi-permeable temporary intermediate layer (4) Donor base (5) Hot plate

[0072] A glassy, ​​in-plane isotropic, target film (2) (approximately 85 nm thick) of PFO was spin-coated from a 2 wt % solution in toluene onto a glass substrate (1) at 2000 rpm, with both the solution and the substrate (1) preheated to 70° C. prior to deposition. See FIG. 1(A).

[0073] A semipermeable temporary intermediate layer (3) of pNaSS was then spin-coated at 3000 rpm (thickness approximately 200 nm) from a 4 wt % aqueous solution further containing approximately 1 wt % Triton X-100 surfactant added relative to the amount of solvent.

[0074] FIG. 1(B) shows that the semi-permeable temporary intermediate layer (3) can be easily removed by immersion in water without changing the luminescent color of the PFO target membrane (2).

[0075] The lauric acid donor layer (4) was then spin coated at 8000 rpm from a 20 wt % solution in acetone.

[0076] FIG. 1C shows that in areas without the semipermeable temporary intermediate layer (3), lauric acid diffuses into the target membrane of the PFO layer (2) during deposition, which leads to the formation of the so-called “β-phase” structure in the target membrane of PFO (2), resulting in a change in the emission color.

[0077] On the other hand, as shown in FIG. 1(C), the target membrane of PFO (2) retains its original chain structure and luminescence properties in the region where the semipermeable temporary intermediate layer of pNaSS (3) is present.

[0078] The sample was then placed on a hotplate (5) at 50 °C (melting point of lauric acid = 44 °C) for 1 min to activate the diffusion of lauric acid into the target film of PFO (2), resulting in a concomitant emission color change from purple / dark blue ("glassy" PFO; shown in dark gray in Figures 1(A)-(C)) to light blue ("β-phase" PFO; shown in light gray in Figures 1(C)-(E)). PFO deposited from heated solution (as in this example) is characterized by a series of chains in a disordered "worm-like" structure - collectively "glassy". Subsequent exposure of the glassy PFO to solvent results in some of the chain segments adopting a "β-phase" structure, a well-defined chain-extended molecular structure in which adjacent repeat units are oriented in the same plane. The presence of a flattened β-phase structure is evident in the infrared absorption and photoluminescence (PL) spectra; specifically, the maximum PL intensity for β-phase PFO is 438 nm (light blue) compared to 423 nm (purple / dark blue) for glassy PFO.

[0079] Thus, in this example, exposure of a target membrane of PFO (2) to a lauric acid donor compound (4) by thermally activated diffusion through a semipermeable temporary intermediate layer (3) modifies the chain structure of some of the chain segments of PFO from the glassy to the β-phase, resulting in the change in the luminescence properties described above.

[0080] The residual lauric acid donor layer (4) and the semipermeable temporary intermediate layer of pNaSS (3) were then removed from the sample by spinning the sample at 5000 rpm and sequentially depositing 50 μL of acetone, 50 μL of water, and another 50 μL of acetone. The properties induced in the PFO target membrane (2) are not affected by this chemical process. The uniformity of the emission color of the PFO target membrane (2) obtained in the area where the semipermeable temporary intermediate layer of pNaSS (3) is present is shown in Figure 1(E). On the other hand, in the area where no intermediate layer is present, the uniformity of the emission color is clearly very poor.

[0081] Example 2: Modification of the chain structure and luminescence properties of the target film (2) of PFO by solvent vapor stimulation.

[0082] A schematic diagram of each processing step and the corresponding optical micrographs recorded under UV irradiation with a wavelength of 365 nm are shown in FIG.

[0083] (1) Base material (2) Molecular semiconductor film (3) A semi-permeable temporary intermediate layer (4) Donor base (6) Nozzle

[0084] On a glass substrate (1), a target membrane of PFO (2), a semipermeable temporary intermediate layer of pNaSS (3) and a lauric acid donor layer (4) were deposited as described in Example 1; see Figures 2(A)-(C).

[0085] Then, a solvent vapor of 1:1 volume / volume acetone:water was generated by bubbling nitrogen carrier gas through a two-necked vessel containing the solution and directed to the sample via a 2 mm diameter nozzle (6) positioned approximately 5 mm above the sample surface. Solvent vapor-activated diffusion of the lauric acid donor compound (4) into the target film of PFO (2) reforms the corresponding chain structure from glassy to β-phase, thereby inducing a change in the luminescence properties (Figure 2(D)).

[0086] The residual lauric acid donor layer (4) and the semipermeable temporary intermediate layer of pNaSS (3) were then removed from the sample by spinning the sample at 5000 rpm and sequentially depositing 50 μL of acetone, 50 μL of water, and another 50 μL of acetone. The properties induced in the PFO target membrane (2) are unaffected by this chemical process. Figure 2(E) shows that the resulting PFO target membrane (2) contains localized β-phase PFO regions surrounded by glassy PFO.

[0087] Example 3: Modification of the composition and luminescence properties of PFO film (2) by solvent vapor stimulation.

[0088] As shown in FIG. 3(A), a target membrane of PFO (2) and a semi-permeable temporary intermediate layer of pNaSS (3) were deposited on a glass substrate (1) as described in Example 1.

[0089] (1) Base material (2) Molecular semiconductor film (3) A semi-permeable temporary intermediate layer (4) Donor base (6) Nozzle

[0090] The donor layer (4) was then spin-coated at 6000 rpm from the following solution: 2% Coumarin 334 (C) in 1:2 wt / wt acetone:methylene chloride 17 H 17 NO3; Cyan luminescent dye 1) solution The solution was prepared by adding 1wt% DCM (C 19 H 17 Further containing N3O; orange emitting dye 2), mandelic acid (solid solvent; melting temperature = 135°C) and 4 wt% PMMA.

[0091] The resulting solid donor layer (4) comprises a solid solution of coumarin 334, DCM and mandelic acid embedded in an inert PMMA matrix.

[0092] The resulting emission of the sample, observed under irradiation with 365 nm light through the substrate (1), is dark blue, consistent with the emission of the essentially glassy PFO target film (2) (see the 0 second image in Figure 3(B)). The emission of the dye containing donor layer (4) is not evident here, as it is quenched by the induced concentration.

[0093] A solvent vapor of 1:1 volume / volume acetone:water was then generated by bubbling nitrogen carrier gas through a two-necked vessel containing the solution and directed at the sample via an 8 mm diameter nozzle (6) positioned approximately 20 mm above the sample surface.

[0094] The smaller molar mass Coumarin 334 dye (dye 1) diffuses faster into the target membrane of PFO (2) than the larger molar mass DCM dye (dye 2).

[0095] Thus, for images recorded 10 to 15 seconds after application of the solvent vapor, the presence of dye 1 in the PFO target film (2) changes the emission from dark blue to cyan, as shown in gray in Figure 3(B).

[0096] With continued exposure to the solvent vapor, the higher molar mass DCM dye (dye 2) diffuses into the PFO target film (2). Thus, for images recorded 25-30 seconds after application of the solvent vapor, the presence of dye 2 in the PFO target film (2) changes the emission from cyan to orange, as shown by gray and white in Figure 3(B) and orange in Figure 3(B).

[0097] Example 4: Spatially varying modification of the composition and luminescence properties of a PFO target film (2) by solvent vapor stimulation.

[0098] As shown in FIG. 4(A), on a glass substrate (1), a target membrane of PFO (2), a semipermeable temporary intermediate layer of pNaSS (3), and a donor layer (4) comprising a solid solution of coumarin 334 (dye 1), DCM (dye 2), and mandelic acid embedded in an inert PMMA matrix were deposited by spin coating as described in Example 3.

[0099] (1) Base material (2) Molecular semiconductor film (3) A semi-permeable temporary intermediate layer (4) Donor base (7) Slot die

[0100] A solvent vapor of 1:1 volume / volume acetone:water was then generated by bubbling nitrogen carrier gas through a two-necked vessel containing the solution and directed at the sample via a slot die (7) positioned at the lower end of the substrate (1).

[0101] FIG. 4(B) shows an image recorded under irradiation with light of wavelength 365 nm of the sample after removal of the residual donor layer (4) by spinning the sample at 5000 rpm and depositing 50 μL of methylene chloride.

[0102] The relative solvent vapor pressure P, as determined by the configuration of the slot die (7), vap The solvent vapor pressure (i.e., the ratio of the solvent vapor pressure at a given location on the sample to that of the saturating stream) changes across the sample, increasing from top to bottom. Thus, the emission of the sample changes from dark blue to cyan and orange from top to bottom. This is further confirmed by photoluminescence (PL) spectra recorded at spatial positions across the sample length from top to bottom (Figure 4(C)).

[0103] Example 5: Modification of the composition and electrical conductivity of PBTTT-C14 target membrane (2) by thermal stimulation.

[0104] A film of PBTTT-C14 (2) (approximately 43 nm thick) was spin-coated from a 1.5 wt % solution in chlorobenzene onto a glass substrate (1) at 4000 rpm, with both the solution and the substrate (1) preheated to 110° C. prior to deposition.

[0105] To avoid temperature-dependent changes in polymer crystallinity following the application of a subsequent thermal stimulus, the resulting film (2) was then crystallized by annealing at 180° C. under a nitrogen atmosphere, followed by slow cooling to room temperature.

[0106] A semipermeable temporary intermediate layer (3) of pNaSS was then spin-coated at 6000 rpm (thickness about 80 nm) from a 2 wt % aqueous solution, further containing about 1 wt % Triton X-100 surfactant added relative to the amount of solvent.

[0107] A donor layer (4) comprising the electrical p-type dopant BCF (B(C6F5)3) was then spin coated at 6000 rpm from a 60 wt % BCF solution in 10:1 wt / wt diethyl ether:methanol.

[0108] Thermal stimulation: The sample was then thermally annealed in air at a selected temperature in the range of 50°C to 120°C for 1 min to activate the diffusion of the dopant BCF from the donor layer (4) into the PBTTT-C14 target film (2).

[0109] The residual BCF donor layer (4) and the semi-permeable temporary intermediate layer of pNaSS (3) were then removed by spinning the sample at 5000 rpm and sequentially depositing 100 μL of acetonitrile and 100 μL of water.

[0110] Electrical conductivity is induced in the PBTTT-C14 target film (2). FIG. 5(A) shows the electrical conductivity induced in the PBTTT-C14 target film (2) versus the annealing temperature used as the thermal stimulus, where the conductivity is plotted on a semi-logarithmic scale, follows a sigmoidal profile, and reaches a high value of 62 S / cm. Note that without the thermal stimulus, the PBTTT-C14 target film (2) has a conductivity of about 4×10 -5 Note also that the conductivity remains low at 23° C. / cm (data point “23° C.” in FIG. 5(A)).

[0111] FIG. 5(B) shows transmitted light micrographs of the obtained PBTTT-C14 target film (2) after applying a thermal stimulus by annealing at various temperatures T, highlighting the improved doping uniformity at higher annealing temperatures. It should be noted that using annealing temperatures T higher than the melting temperature of the BCF dopant in the donor layer (4) (126-131 °C) can lead to dedoping of the PBTTT-C14 target film (2) due to evaporation of the dopant BCF in the donor layer (4), with an associated decrease in the electrical conductivity obtained.

[0112] The absorbance spectra of the target film of PBTTT-C14 (2) without application of a thermal stimulus and with application of a thermal stimulus by annealing at 80° C. and 120° C., respectively, are shown in FIG. 5(C). Doping is confirmed by the expected attenuation of the neutral polymer absorption (centered at about 550 nm) and the simultaneous presence of a broad band corresponding to ionic species (centered at about 780 nm) when thermal annealing is performed at 80° C. and 120° C., respectively.

[0113] Example 6: Modification of the composition and electrical conductivity of the target membrane (2) of PBTTT-C14 by thermal stimulation.

[0114] A film of interest (2) of PBTTT-C14 was deposited on a glass substrate (1) as described in Example 5.

[0115] To avoid temperature-dependent changes in polymer crystallinity following the application of a subsequent thermal stimulus, the resulting film (2) was then crystallized by annealing at 180° C. under a nitrogen atmosphere, followed by slow cooling to room temperature.

[0116] A semipermeable temporary intermediate layer of pNaSS (3) was then deposited as described in Example 5.

[0117] The donor layer (4) comprises BCF:biphenyl; spin-coated at 6000 rpm from a 60 wt% BCF solution in 10:1 wt / w diethyl ether:methanol, further containing 5 wt% biphenyl added relative to the amount of solvent. Biphenyl ("BP"; melting temperature = 69°C) is used as a co-solvent for BCF to reduce the annealing temperature or annealing time required to obtain the desired electrical conductivity.

[0118] Thermal Stimulation: The samples were then thermally annealed in air (as described below) to activate the diffusion of BCF into the PBTTT-C14 target membrane (2).

[0119] The residual BCF:biphenyl donor layer (4) and the semi-permeable temporary intermediate layer of pNaSS (3) were removed by spinning the sample at 5000 rpm and sequentially depositing 100 μL of acetonitrile and 100 μL of water.

[0120] The electrical conductivity of the samples obtained after applying a thermal stimulus by thermal annealing for 1 min in the temperature range of 50-120 °C is shown in Figure 6 (A). At annealing temperatures equal to or slightly above the melting temperature of biphenyl (BP), the presence of biphenyl (BP) in the donor layer (4) can increase the electrical conductivity by about two orders of magnitude compared to samples in which the donor layer (4) contains only BCF. The corresponding transmitted light micrographs (Figure 6 (B)) show a simultaneous improvement in the doping uniformity at a given temperature (see data for the "80 °C" and "90 °C" samples).

[0121] The electrical conductivity of the samples obtained after applying a thermal stimulus by thermal annealing at 100 °C for annealing times ranging from 2 to 30 seconds is shown in Figure 6 (C). For an annealing time of 2 seconds, the presence of biphenyl (BP) in the donor layer (4) can increase the electrical conductivity by more than an order of magnitude relative to a sample in which the donor layer (4) is only BCF.

[0122] Example 7: Modification of the chain structure of PFO target membrane (2) by light stimulation.

[0123] Onto the ITO layer (9) / glass substrate (1), a target membrane of PFO (2), a semipermeable temporary intermediate layer of pNaSS (3) and a lauric acid donor layer (4) were deposited as described in Example 1; see FIG. 7(A).

[0124] (1) Base material (2) Molecular semiconductor film (3) A semi-permeable temporary intermediate layer (4) Donor base (8) Laser (wavelength = 785 nm) (9) Light absorbing layer

[0125] The output of a 785 nm laser (8) was then guided through the substrate (1) to the sample and focused on the target film (2) of the PFO layer, as shown in FIG. 7(B). Here, the absorption of the laser light mainly occurs in the ITO layer (9), with the main heat being generated at the interface between the substrate (1) and the target film (2). It should be noted that the target film (2), the semi-permeable temporary intermediate layer (3) and the donor film (4) do not absorb the light beam of 785 nm wavelength to any significant extent. The laser power P was adjusted in the range of 10-50 mW. The sample was scanned continuously at a speed ν in the range of 0.1-10 μm / s in the focal plane of the laser (8). The role of the laser irradiation here is to provide localized heat by light absorption in the ITO, activating the local diffusion of the lauric acid solvent from the lauric acid donor layer (4) into the PFO target layer (2) and modifying its chain structure.

[0126] The residual lauric acid donor layer (4) and the semipermeable temporary intermediate layer of pNaSS (3) were then removed from the sample by spinning the sample at 5000 rpm and sequentially depositing 50 μL of acetone, 50 μL of water, and another 50 μL of acetone.

[0127] In the obtained samples, a modification of the chain structure is induced. Confocal PL microscopy images recorded with excitation at 355 nm for the indicated laser powers (P = 10-50 mW) and continuous lines drawn at a constant speed ν = 5 μm / s are shown in the left panel of Figure 8(A) and selectively selected the maximum of the PFO PL emission of the β-phase using spectral filtering at 438 nm as shown in Figure 8(B). Thus, the bright areas in Figure 8(A) correspond to areas of the sample where the structure of some of the chain segments has been modified from glassy to β-phase.

[0128] The PL spectrum recorded at the center of the drawn line (solid line in Figure 8(B)) confirms the formation of β-phase structure showing characteristic vibrational peaks at 438 nm, 467 nm and 498 nm. Meanwhile, the reference PL spectrum recorded outside the laser-exposed sample area corresponds to that of pristine glassy PFO (dashed line in Figure 8(B)) and shows vibrational peaks at 423 nm and 449 nm. Furthermore, the above spectrum shows that the above-mentioned laser-based process does not induce any significant photooxidative degradation of the target film of PFO (2), which can be corroborated by the prominent PL appearing at wavelengths above 500 nm.

[0129] The size of the regions with modified chain-like structures was estimated as the full width at half maximum (FWHM) of the PL intensity profile at 438 nm across the drawn line. The contrast of the modified regions (i.e., the maximum induced volume fraction of chain segments in the β phase) was calculated as the Raman intensity ratio to the β phase fraction, r R (1257cm -1 :1606cm -1 ) was estimated by calibration. Spectroscopic Raman mapping of the modified area with excitation at 633 nm determined R and the corresponding β phase fraction were determined, and an exemplary r R The image is shown in the right panel of Figure 8(A).

[0130] The size and contrast of the regions of the sample with modified chain-like structures show an evolution that correlates with the incident laser power (Figure 8(C)) and writing speed (Figure 8(D)), allowing a simple means to obtain the desired properties of the modified regions. For example, at a constant ν = 5 μm / s, tuning P from 50 to 10 mW allows a 10-fold and 6-fold reduction in the size and contrast of the modified regions, respectively.

[0131] Example 8: Modification of chain orientation of a symmetric film of P3HT (2) by light stimulation.

[0132] A film of P3HT (2) (approximately 90 nm thick) was spin-coated at 4000 rpm from a 2 wt % solution in chlorobenzene onto the ITO layer (9) / glass substrate (1), both of which were preheated to 50° C. prior to deposition; see FIG. 7(A).

[0133] A semipermeable temporary intermediate layer (3) of pNaSS was then spin-coated at 7000 rpm (thickness approximately 130 nm) from a 4 wt % aqueous solution further containing approximately 1 wt % Triton X-100 surfactant added relative to the amount of solvent.

[0134] A 2,1,3-benzothiadiazole (BT) donor layer (4) was then deposited by spin-coating at 700 rpm from a 40 wt % solution in methylene chloride, followed by about 60 s of solvent evaporation and placing a glass coverslip (0.17 mm thick) on the still liquid BT donor layer (4). Concomitant nucleation and crystallization of BT results in the desired solid BT donor layer (4) beneath the glass coverslip. Although not essential to the process, the use of a glass coverslip prevents excessive and rapid sublimation of BT during subsequent laser-based modification and improves the uniformity of the resulting donor layer (4) in terms of film thickness.

[0135] BT has a periodicity, c, of crystalline BT along its fast growth axis that is comparable to that of crystalline P3HT (c BT = 3.85 Å; C p3HT BT is selected as the donor layer (4) because of its low melting temperature (44° C. / 2≈3.8 Å), which allows for the orientation of P3HT by epitaxial crystallization. A further condition for the orientation of P3HT is that the crystallization of BT occurs before that of P3HT, which is easily achieved for the hypoeutectic BT:P3HT composition. Here, BT is further selected as the donor layer (4) because of its low melting temperature (44° C.), which reduces the required processing temperature.

[0136] The output of a 785 nm laser (8) was then guided through the substrate (1) to the sample and focused on the P3HT target film (2), as shown in FIG. 7(B). Here, absorption of the laser light occurs mainly in the ITO layer (9), with the main heating occurring at the interface between the substrate (1) and the target film (2). In this example, the target film (2), the semi-permeable temporary intermediate layer (3) and the donor layer (4) do not absorb light of a wavelength of 785 nm to any significant extent. A constant laser power P=55 mW was used. The sample was scanned continuously in the focal plane of the laser (8) at a speed ν ranging from 0.1 to 3 mm / s.

[0137] The glass cover slip used in this example was then removed, allowing for rapid removal of the residual BT donor layer (4) by sublimation in ambient conditions. The semi-permeable temporary intermediate layer of pNaSS (3) was then removed from the sample by spinning the sample at 5000 rpm and depositing 50 μL of water.

[0138] Optical anisotropy was induced in the resulting samples. Polarized transmitted light micrographs (Figure 9(A)) show that the lines drawn at ν ≥ 0.5 mm / s exhibit optical anisotropy, i.e., they appear darker or lighter for transmitted light polarized parallel or perpendicular to the laser scanning direction, respectively (left and right sides of Figure 10(A) respectively; polarization directions are indicated by arrows). More extensive polarized transmitted light micrographs shown in Figure 10(A)-(B) (transmitted light polarized parallel and perpendicular to the laser scanning direction, respectively, indicated by arrows) highlight the uniformity of the modified regions. The dependence of the absorbance on the direction of light polarization indicates a preferred orientation of the P3HT chain segments parallel to the laser scanning direction. The latter is further supported by cross-polarized light micrographs for the same sample area (Figure 9(B); polarization directions are indicated), which show that the birefringence of the modified regions is only visible for light polarized at an angle to the laser scanning direction (Figure 9(B), right panel).

[0139] The role of the laser irradiation here is therefore to activate the local diffusion of the BT solvent from the BT donor layer (4) into the P3HT target layer (2), resulting in localized heating and subsequent melting due to light absorption inside the ITO. Subsequent removal of the light-induced heat (i.e. by scanning the laser away from the predefined sample area) results in the crystallization of BT in the P3HT:BT layer (2) and with it the directional crystallization of P3HT. A local modification of the chain orientation of the P3HT target layer (2) is thus obtained.

[0140] Polarized Raman spectroscopy is used to quantify the degree of molecular anisotropy (i.e., chain orientation) in the modified regions. An exemplary polarized Raman spectrum recorded with excitation at 785 nm at the center of the line drawn with ν=2.5 mm / s and P=55 mW (solid line; Figure 9(C)) shows an approximate peak at 1450 cm for polarization parallel to the laser scan direction. -1 Figure 9(C) shows a stronger intensity of the symmetric C=C stretching mode of P3HT at 1000 nm, indicating a preferred orientation of the P3HT chain segments parallel to the laser scanning direction. Also shown is a reference spectrum recorded outside the modified region (dotted line; Figure 9(C)).

[0141] Therefore, the Raman anisotropy A R was defined as the ratio of the maximum intensities for the vibrational modes of P3HT recorded with polarization parallel and perpendicular to the laser scanning direction. Polarized spectroscopic Raman mapping was used to quantify the molecular anisotropy and its spatial distribution in the modified regions. A for a line drawn with ν=2 mm / s and P=55 mW R An example image of the average Raman anisotropy is shown in FIG. R The corresponding profile of is along the laser scanning direction. R > The image was obtained by averaging the images. R Example images obtained R The profile is shown in Figure 9(E), where R > increases to about 2.6, indicating a preferred orientation of the P3HT chain segments in the symmetric film (2) parallel to the laser scanning direction in the laser irradiated areas. <A​​​​R >The FWHM size of the regions with modified chain orientation estimated from the profiles is 4.6 ± 0.3 μm for lines drawn with ν in the range of 0.5–3 mm / s.

[0142] FIG. 9(E) shows the results for the sample area not exposed to the light stimulus. R >=1, indicating that the chain orientation retains in-plane isotropy similar to that of the original P3HT target film (2) (consistent with the polarized optical micrographs shown in Figures 9(A)-(B)). This confirms that in the absence of an applied stimulus, such as laser irradiation, the semipermeable temporary intermediate layer (3) prevents the diffusion of BT containing donor layer (4) into the P3HT target film (2), thereby preserving its original microstructure.

[0143] FIG. 9(F) shows the maximum R > value (shown in Figure 9(E) R > max ), which indicates that rapid modification of chain orientation can be achieved with laser scanning speeds in the mm / s range. R > max increases with ν, reaching a value of about 3 for ν = 2.5 mm / s. At lower speeds (e.g., 0.1 mm / s, see FIG. 9(F)), laser-induced overheating causes the depletion of BT from the exposed area and hence R > max At higher speeds (e.g., 3 mm / s, see FIG. 9(F)), insufficient heating and / or diffusion of insufficient amounts of BT through the semi-permeable temporary intermediate layer (3) into the target membrane of P3HT (2) can result in R > max Higher writing speeds can be used without compromising the degree of chain orientation after optimization of the multilayer structure, for example with regard to the thickness of the semi-permeable temporary intermediate layer (3) as well as using higher laser powers.

[0144] ​​​​​​An exemplary analysis of the film topography by atomic force microscopy (AFM) of a line drawn using ν=2.5 mm / s and P=55 mW is shown in FIG. 11(A). The corresponding film thickness profile (FIG. 11(B)) reveals only a 2% reduction in film thickness in the modified regions, which are shown in a magnified view in FIG. 11(C). This indicates that the planarity of the resulting film of interest of P3HT (2) with regions of modified chain orientation is preserved due to containment by the semipermeable temporary interlayer (3). Retaining the planarity of the film offers a great advantage for the integration of such samples in electronic, optoelectronic, and photonic devices. In comparison, films of P3HT macroscopically oriented using crystalline small molecule compounds similar to BT without the use of a temporary interlayer typically exhibit root-mean-square (RMS) surface roughness of up to 30 nm, and in some cases exceeding 100 nm.

[0145] Comparative example: modification of the chain orientation of a symmetric membrane of P3HT (2) by light stimulation without a semipermeable temporary intermediate layer (3).

[0146] In this comparative example, laser-based modification of chain orientation of a P3HT target film (2) was performed without the use of a semi-permeable temporary intermediate layer. On an ITO (9) / glass substrate (1), a P3HT target film (2) was deposited as described in Example 8. A BT donor layer (4) was then deposited as described in Example 8.

[0147] The output of a 532 nm laser (8) was then guided through the substrate (1) to the sample and focused on approximately 25 μm above the target film (2) of P3HT to increase the synthesis width of the modified area. Here, the absorption of the laser light occurs mainly in the target layer (2), assuming that the laser excitation at 532 nm closely matches the spectral position of the absorption maximum of P3HT. Thus, heat is generated mainly in the target film (2) of P3HT. A constant laser power P = 10 mW was used. The sample was scanned continuously in the focal plane of the laser (8) at a speed ν = 3 mm / s.

[0148] The BT donor layer (4) was then removed by sublimation as described in Example 8.

[0149] Polarized transmitted light micrographs (Figure 12; polarization direction indicated by arrows) highlight some drawbacks of modifying chain orientation without the use of a semipermeable temporary intermediate layer. First, although some degree of chain orientation is induced relative to the line, as shown by the polarization-dependent difference in brightness (i.e., absorbance) in the modified areas, the direction of orientation does not clearly correlate with the laser scanning direction, with the average angle between the two being about 70°. This is due to the BT donor layer (4) being in direct contact with the P3HT target film (2). Thus, although the laser-induced heat stimulates the required diffusion of BT into the P3HT target film (2) and dissolution of the latter, upon removal of the heat, the direction of crystallization of BT within the P3HT:BT layer (2) is instead determined by the orientation of the crystalline BT in the donor layer (4) outside the laser-irradiated sample area. Given that it is extremely difficult to precisely control the crystalline orientation of a BT donor layer (4) deposited from solution, in the absence of a semipermeable temporary intermediate layer (3), a controllable and reproducible modification of the chain orientation of the target membrane (2) parallel to the laser scanning direction is prevented in the absence of a semipermeable temporary intermediate layer (3).

[0150] Secondly, the resulting P3HT target film (2) shows a pronounced fibrous texture outside the laser irradiated areas (Figure 12; see the sample area between the lines). This indicates that the original P3HT target film (2) has been irreversibly modified by the direct deposition of the BT donor layer (4) onto the P3HT target layer (2), accompanied by a (partial) dissolution and directional crystallization of the latter. Further inspection of the polarized optical micrograph in Figure 12 shows that the polarization-dependent brightness (i.e., absorbance) is different in the sample areas not exposed to the light stimulus. This confirms that the P3HT target film (2) before the application of any stimulus is (partially) oriented. The use of a temporary intermediate layer therefore offers a clear advantage to allow the modification of the chain orientation of the polymer target film (2) in selected areas determined, for example, by laser irradiation.

[0151] Example 9: Modification of the composition and electrical conductivity of the target membrane (2) of PBTTT-C14 by light stimulation.

[0152] A film of PBTTT-C14 (2) (approximately 43 nm thick) was spin-coated from a 1.5 wt % solution in chlorobenzene onto a glass substrate (1) at 4000 rpm, with both the solution and the substrate (1) preheated to 110° C. prior to deposition.

[0153] To avoid temperature-dependent changes in polymer crystallinity following the application of a subsequent thermal stimulus, the resulting film (2) was then crystallized by annealing at 180° C. under a nitrogen atmosphere, followed by slow cooling to room temperature.

[0154] A semipermeable temporary intermediate layer (3) of pNaSS was then spin-coated at 6000 rpm (thickness about 80 nm) from a 2 wt % aqueous solution further containing about 1 wt % Triton X-100 surfactant added relative to the amount of solvent.

[0155] A donor layer (4) comprising BCF was then spin coated at 9000 rpm from a 60 wt % BCF solution in 10:1 wt / wt diethyl ether:methanol.

[0156] Then, as shown in FIG. 7(A), the output of the 532 nm laser (8) was guided to the sample through the donor layer (4) and focused on about 20 μm above the PBTTT-C14 target film (2) to expand the synthetic width of the modified region. Here, assuming that the laser excitation at 532 nm closely matches the spectral position of the absorption maximum of the PBTTT-C14 target film (2), the absorption of the laser light occurs mainly in the target layer (2). Therefore, the role of the laser irradiation here is to provide local heat by light absorption in the PBTTT-C14 target film (2) and activate the local diffusion of the BCF dopant from the donor layer (4) to the PBTTT-C14 target film (2) and dope the latter. The laser power P was adjusted in the range of 5 to 10 mW. The sample was continuously scanned in the focal plane of the laser (8) at a speed ν in the range of 5 μm / s to 3 mm / s.

[0157] The sample was then spun at 5000 rpm and the residual BCF donor layer (4) and the semi-permeable temporary intermediate layer of pNaSS (3) were removed by sequentially depositing 100 μL of acetonitrile and 100 μL of water.

[0158] The transmitted light micrograph (FIG. 13(A)) shows that the traced lines have a brighter appearance compared to the original film given the decay of absorption of neutral PBTTT-C14 upon doping described above, indicating that electrical conductivity has been induced in the modified regions. Thus, FIG. 13(A) shows that the use of optical stimulation can locally modify the electrical conductivity of the target film (2) of PBTTT-C14 on the micrometer scale, compared to the larger millimeter-scale similar modifications obtained with thermal stimulation in Examples 5 and 6. Localized micrometer-scale modification of electrical conductivity is required for a variety of electronic devices, including thin film transistors and other optoelectronic devices.

[0159] A quantitative analysis of the maximum electrical conductivity induced by photostimulation as a function of writing speed ν and laser power P is shown in Fig. 13(B), where the local conductivity value is calculated as a function of the experimentally obtained Raman intensity ratio r R (1393cm -1 :1417cm -1 r as a function of electrical conductivity σ) versus the calibration data of PBTTT-C14 control film macroscopically doped with BCF by thermal stimulation (see Example 5). R Calibration data for is shown in Figure 13(C) and an exemplary Raman spectrum is shown in Figure 13(D) (spectral positions of relevant peaks are indicated with asterisks). Thus, the electrical conductivity maxima within the modified regions were determined by the spectroscopic mapping of Example 7. R It was decided by.

[0160] As shown in Figure 13(B), a maximum electrical conductivity of about 7 S / cm is obtained at v = 10 μm / s and P = 7 mW. The data also show that, at sufficiently high laser power, high values ​​of conductivity can be obtained up to v reaching about 3 mm / s, as required for optimal high throughput manufacturing. Further improvement can be achieved by using a pulsed rather than continuous wave laser source to minimize the concomitant occurrence of overheating induced dedoping.

[0161] Example 10: Modification of the composition and electrical conductivity of a target film (2) of PBTTT-C14 by light stimulation to provide an RFID antenna type structure.

[0162] Onto a glass substrate (1), a target film (2) of PBTTT-C14 was deposited as described in Example 9.

[0163] To avoid temperature-dependent changes in polymer crystallinity following the application of a subsequent thermal stimulus, the resulting film (2) was then crystallized by annealing at 180° C. under a nitrogen atmosphere, followed by slow cooling to room temperature.

[0164] A semipermeable temporary intermediate layer of pNaSS (3) and a donor layer containing BCF (4) were then deposited as described in Example 9.

[0165] The output of a 532 nm laser (8) was then directed through the donor layer to the sample, as shown in Figure 7(A), and focused approximately 20 μm onto a target film (2) of PBTTT-C14, as described in Example 9. A constant laser power P = 7 mW was used. The sample was continuously scanned in the focal plane of the laser (8) at a speed v = 3 μm / s.

[0166] The remaining BCF donor layer (4) and the semipermeable temporary intermediate layer of pNaSS (3) were then removed as described in Example 9.

[0167] The transmission optical microscope photograph (FIG. 14(A)) of the obtained PBTTT-C14 target film (2) shows a 280×280 μm 2 It is shown that electrical conductivity is increased in the shape of a spiral having a contour size of 100 nm. Thus, here, exposure of the sample to scanning laser irradiation at selected locations provides a continuous and uniform structure comprising conductive lines embedded in an otherwise semiconductor target film (2). Such a structure can be used as an antenna for a radio frequency identification (RFID) tag. The r obtained at selected sample areas as described in Example 9. R (1393cm -1 :1417cm -1 The image of (recorded with 488 nm excitation) is shown in FIG. R The average profile of and electrical conductivity σ (Fig. 14(C)) of the maximum r R , and the associated σ values ​​show close agreement with the maximum conductivity of about 3 S / cm, highlighting the uniformity of the modified electrical properties. Also, from FIG. 14(C), it can be seen that the obtained PBTTT-C14 target film (2) has a conductivity of about 1.5 S / cm, which is higher than that of undoped PBTTT-C14 (σ ≈ 4 × 10 -5 It can be seen that the original conductivity of 1.0 S / cm (shown by the dashed line in FIG. 14(C)) is maintained.

[0168] Example 11: Effect of a temporary interlayer on the uniformity of the deposited donor layer.

[0169] A film of PBTTT-C14 (2) (approximately 43 nm thick) was spin-coated from a 1.5 wt % solution in chlorobenzene onto a glass substrate (1) at 4000 rpm, with both the solution and the substrate (1) preheated to 110° C. prior to deposition.

[0170] The resulting film was then crystallized by annealing at 180° C. under a nitrogen atmosphere, followed by slow cooling to room temperature.

[0171] Here, four samples were prepared.

[0172] For two samples, a semi-permeable temporary intermediate layer (3) of pNaSS was then spin-coated at 6000 rpm (thickness about 80 nm) from a 2 wt % aqueous solution further containing about 1 wt % Triton X-100 surfactant added relative to the amount of solvent.

[0173] - The other two samples were left uncoated, ie without the semipermeable temporary intermediate layer of pNaSS (3).

[0174] Afterwards, two different donor layers (4) were deposited: ·BCF: spin-coated at 6000 rpm from a 40 wt% solution in 10:1 wt / wt diethyl ether:methanol; · 2:1 wt / wt BCF:biphenyl (BP): spin-coated at 6000 rpm from a 50 wt% solution in 10:1 wt / wt diethyl ether:methanol.

[0175] Transmitted light micrographs of the obtained samples are shown in Figure 15. The presence of a semipermeable temporary intermediate layer of hydrophilic pNaSS (3) allows optimal wettability of the solutions used to deposit the BCF and BCF+BP donor layers (4), resulting in a donor layer (4) with uniform crystals deposited thereon (Figure 15(A)).

[0176] In contrast, BCF and BCF+BP donor layer solutions deposited directly onto the hydrophobic PBTTT-C14 target membrane (2) did not form a uniform layer, but instead yielded single regions (Figure 15(B)).

[0177] Example 12: Stability of the thermally modified target layer (2) after chemical removal of the donor layer (4) and the semipermeable temporary intermediate layer (3).

[0178] A film of PBTTT-C14 (2) (approximately 43 nm thick) was spin-coated from a 1.5 wt % solution in chlorobenzene onto a glass substrate (1) at 4000 rpm, with both the solution and the substrate (1) preheated to 110° C. prior to deposition.

[0179] To avoid temperature-dependent changes in polymer crystallinity following the application of a subsequent thermal stimulus, the resulting film (2) was then crystallized by annealing at 180° C. under a nitrogen atmosphere, followed by slow cooling to room temperature.

[0180] A semipermeable temporary intermediate layer (3) of pNaSS was then spin-coated at 6000 rpm (thickness about 80 nm) from a 2 wt % aqueous solution further containing about 1 wt % Triton X-100 surfactant added relative to the amount of solvent.

[0181] A donor layer (4) comprising BCF was then spin coated at 8000 rpm from a 57 wt % BCF solution in 9:1 wt / wt diethyl ether:methanol.

[0182] The sample was then thermally annealed at 120° C. for 30 seconds in air to dope the target film (2) of PBTTT-C14.

[0183] The composition and electrical conductivity modification of the target membrane (2) is desirably not substantially affected by the subsequent chemical removal of the donor layer (4) and the semi-permeable temporary intermediate layer (3), where the electrical conductivity of the resulting sample was measured by depositing a selected volume of a given solvent by spinning the sample at 5000 rpm after successive exposure to the liquid solvent used to remove the remaining donor layer and temporary intermediate layer.

[0184] The BCF donor layer (4) can be removed by any BCF solvent, including those used to deposit the donor layer (4) (i.e., diethyl ether and methanol), as well as other organic solvents such as acetonitrile. The electrical conductivity of the thermally modified target layer (2) remains essentially constant at 24 S / cm after deposition of 100 μL of acetonitrile, with the donor layer (4) being completely removed. This indicates that the electrical conductivity of the modified target layer (2) is retained after this process.

[0185] The semipermeable temporary intermediate layer (3) can be removed by any solvent of the material comprising said layer. Here, the semipermeable temporary intermediate layer (3) of pNaSS can be removed by water, which is a good solvent of pNaSS. The electrical conductivity of the target membrane (2) modified by thermal stimulation shows a slight decrease to 20 S / cm after 100 μL of water is dropped, and the semipermeable temporary intermediate layer (3) is completely removed. This indicates that the electrical conductivity of the modified target layer (2) is well retained after this process.

[0186] It is therefore shown that removal of the residual donor layer (4) and the semi-permeable temporary intermediate layer (3) by wet chemical means can be performed without significant loss of the induced modification.

[0187] Example 13: Stability of a target membrane (2) after physical and chemical removal of a semipermeable temporary intermediate layer (3)

[0188] As shown in Figure 16(A), a film of P3HT (2) was spin-coated from a 2 wt% solution in chlorobenzene at 4000 rpm (thickness approximately 90 nm) onto a glass substrate (1), with both the solution and the substrate (1) preheated to 55°C prior to deposition.

[0189] A semipermeable temporary intermediate layer (3) of pNaSS was then spin-coated at 6000 rpm (thickness about 80 nm) from a 2 wt % aqueous solution further containing about 1 wt % Triton X-100 surfactant added relative to the amount of solvent.

[0190] In some applications in electronic and photovoltaic devices, it may be advantageous to minimize exposure of the target membrane (2) to the solvent (e.g., water) used to remove the semipermeable temporary intermediate layer (3). It may therefore be desirable to remove the semipermeable temporary intermediate layer (3) by physical means rather than the chemical means used in the above examples.

[0191] Then, to demonstrate that both methods can be used to remove the semipermeable temporary intermediate layer (3), a portion of the semipermeable temporary intermediate layer (3) on the left side of the sample was removed by partially immersing the sample in water (see FIG. 16(A)).

[0192] Then, another portion of the semi-permeable temporary intermediate layer (3) on the right side of the sample was removed by imprinting and lift-off using a conformal contact forming stamp of polydimethylsiloxane (PDMS) elastomer.

[0193] In both cases, reflected light micrographs shown in FIG. 16(B) confirm complete and equivalent removal of the semipermeable temporary intermediate layer of pNaSS (3), further highlighting that no damage is caused to the target layer (2) by using a solvent-free physical process. [Brief description of the drawings]

[0194] [Figure 1] 1(A)-(E) are schematic cross-sectional diagrams of the main steps for modifying a target layer using thermal stimulation, with corresponding fluorescence micrographs of exemplary target films whose chain structure and luminescence properties have been modified using thermal stimulation. [Diagram 2] 2(A)-(E) are schematic cross-sectional diagrams of the main steps for modifying a target layer using solvent vapor, with corresponding fluorescence micrographs of exemplary target films whose chain structure and luminescence properties have been modified using solvent vapor. [Diagram 3] 3(A)-(B) are schematic cross-sectional views and corresponding fluorescent photographs illustrating modification of the composition and luminescence properties of a subject semiconducting polymer film having modified composition and luminescence properties using solvent vapor stimulation. [Figure 4] Figure 4(A)-(C) are schematic cross-sectional diagrams of target semiconducting polymer films with spatially varying modifications of composition and emission properties using solvent vapor stimulation, as well as the corresponding fluorescence photographs and photoluminescence spectra. [Diagram 5]5(A)-(C) are plots of electrical conductivity, optical micrographs, and absorbance spectra of subject semiconducting polymer films whose composition and electrical conductivity were modified using a thermal stimulus. [Figure 6] 6(A)-(C) are electrical conductivity plots and optical micrographs of target semiconducting polymer films whose composition and electrical conductivity were modified using a co-solvent-assisted thermal stimulus. [Figure 7] 7(A)-(B) are schematic cross-sectional views showing various means for exposing a sample to a light stimulus. [Figure 8] Figure 8(A)-(D) are confocal photoluminescence micrographs and Raman intensity ratio images; photoluminescence spectra and plots of pattern characteristics as a function of process parameters for a target semiconducting polymer film whose chain structure has been locally modified by optical stimulation. [Figure 9] 9(A)-(F) show polarized optical micrographs, polarized Raman spectra, details of an exemplary Raman anisotropy analysis, and plots of Raman anisotropy as a function of process parameters for a target semiconducting polymer film in which chain orientation has been locally modified using photostimulation. [Figure 10] 10(A)-(B) are polarized optical micrographs of a large area of ​​a target semiconducting polymer film in which chain orientation has been locally modified using photostimulation. [Figure 11] FIG. 11(A)-(C) are atomic force microscope images and topography analysis of target semiconducting polymer films in which chain orientation was locally modified using light stimulation. [Figure 12] FIG. 12 is an optical micrograph of a subject semiconducting polymer film in which chain orientation was locally modified using light-based stimulation without the use of a semipermeable temporary intermediate layer. [Figure 13] 13(A)-(D) are optical micrographs and plots of electrical conductivity as a function of process parameters of target semiconducting polymer films whose composition and electrical conductivity have been modified using optical stimulation; and reference Raman spectroscopy data as a function of electrical conductivity for target films of the same polymer whose composition and electrical conductivity have been modified using thermal stimulation. [Figure 14] 14(A)-(C) are optical micrographs, Raman intensity ratio images, and plots of electrical conductivity as a function of position of target semiconducting polymer films whose composition and electrical conductivity were modified using photostimulation. [Figure 15] 15(A)-(B) are optical micrographs and schematic cross-sectional views of an exemplary donor layer where the solution is deposited onto a temporary intermediate layer and an exemplary donor layer where the solution is deposited directly onto a target membrane. [Figure 16] 16(A)-(B) are cross-sectional views and optical micrographs illustrating the removal of the temporary interlayer by chemical and physical means.

Claims

1. A method for providing structural and / or compositional modifications to a molecular semiconductor target film (2) located on a substrate (1), characterized in that it comprises the following steps: a) depositing a semi-permeable temporary intermediate layer (3) on the surface of said molecular semiconductor film of interest (2) located on a substrate (1) by a solution-based deposition technique; b) depositing a solid donor layer (4) comprising a plurality of functional molecular additives on said semi-permeable temporary intermediate layer (3) obtained in step (a) by a solution-based deposition technique; c) exposing the structure obtained in step (b) to a thermal, solvent vapor, or light stimulus, thereby activating diffusion through said semipermeable temporary intermediate layer (3); and d) Chemical or physical removal of said solid donor layer (4) and said semi-permeable temporary intermediate layer (3).

2. The method of claim 1 , wherein the molecular semiconductor film of interest (2) is deposited on the substrate (1) by a solution-based deposition technique.

3. 3. The method according to claim 1 or 2, wherein the molecular semiconductor target film (2) is deposited on the substrate (1) by a technique selected from spin coating, blade coating, spray coating, slot-die coating, and combinations thereof.

4. The method according to any one of claims 1 to 3, wherein steps (a) and (b) are carried out by a technique selected from spin coating, blade coating, spray coating, slot-die coating, and combinations thereof.

5. The method according to any one of claims 1 to 4, wherein the plurality of functional molecular additives of the donor layer (4) are selected from solvents, dyes, luminescent dyes, nucleating agents, crosslinkers, reactive monomers, catalysts, antigens, antibiotics, amino acids, oligopeptides, molecular electron acceptors, molecular electron donors, molecular electric dopants, and combinations thereof.

6. The method according to any one of claims 1 to 5, wherein the structure obtained in step (b) is patternwise exposed to a thermal, solvent vapor or light stimulus.

7. The method according to any one of claims 1 to 6, wherein the structure obtained in step (b) is exposed in step (c) to a thermal stimulus by a hot plate (5), a hot tip, a hot stamp or hot gas.

8. The method according to any one of claims 1 to 6, wherein the structure obtained in step (b) is exposed in step (c) to a solvent vapor stimulus by a nozzle (6) or a slot die (7).

9. The method according to any one of claims 1 to 6, wherein at least the substrate (1), the molecular semiconductor target film (2), the semi-permeable temporary intermediate layer (3) or the donor layer (4) is a light absorbing layer.

10. The method according to any one of the preceding claims, wherein the substrate (1) comprises a light absorbing layer (9).

11. 11. The method according to claim 9 or 10, wherein the structure obtained in step (b) is exposed to light stimulation by a laser (8) or a flash lamp.

Citation Information

Patent Citations

  • Organic electroluminescence device and manufacturing method of the same

    JP2001223075A

  • Organic electroluminescent display

    JP2003217864A

  • Diffusion method and electroluminescence material

    JP2005158357A

  • Fabrication of light-emitting layers for multicolor OLEDs

    JP2012533852A

  • Manufacturing method of transparent electrode substrate, manufacturing method of device and manufacturing method of touch panel sensor

    JP2014135010A