Glass cloth, prepreg, and printed wiring boards

A low dielectric glass cloth with specific woven structures addresses waviness and impregnation issues, ensuring stable and uniform resin layers for high-density printed wiring boards.

JP7562772B2Active Publication Date: 2024-10-07ASAHI KASEI KOGYO KABUSHIKI KAISHA
View PDF 14 Cites 0 Cited by

Patent Information

Application Number
JP2023104084
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2023-06-26
Publication Date
2024-10-07
Estimated Expiration
2039-06-26

AI Technical Summary

Technical Problem

Existing glass cloths with a thickness of 16 μm or less suffer from waviness during prepreg coating, poor resin impregnation properties, and inadequate dimensional stability, which affect the manufacturing of high-density printed wiring boards.

Method used

A low dielectric glass cloth with a thickness of 8 μm to 16 μm, composed of warp and weft yarns with specific woven structures, including a mass ratio and density that enhances rigidity and uniform resin impregnation, and maintains dimensional stability.

Benefits of technology

The glass cloth exhibits reduced waviness, improved resin impregnation, and enhanced dimensional stability, enabling the production of high-quality prepregs and printed wiring boards with accurate circuitry.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007562772000003
    Figure 0007562772000003
  • Figure 0007562772000004
    Figure 0007562772000004
  • Figure 0007562772000001
    Figure 0007562772000001
Patent Text Reader

Abstract

To provide a low dielectric glass cloth with a thickness of 16 μm or less, which has little waviness during prepreg coating, has an excellent handling property, has a resin impregnating property, and can form a uniform resin layer on a front and back side of the glass cloth; a prepreg using the low dielectric glass cloth; and a substrate for a printed wiring board.SOLUTION: There is provided a glass cloth that has a thickness of 8 μm or more and 16 μm or less, and is composed of a glass thread consisting of multiple glass filaments as warp and weft threads, wherein an average mass per unit length of the warp thread is 1.40×10-6 kg / m or more and less than 1.60×10-6 kg / m, an average mass per unit length of the weft thread is 1.60×10-6 kg / m or more and 3.00×10-6 kg / m or less, a ratio of the average mass per unit length of the weft thread to the average mass per unit length of the warp thread (weft / warp ratio) is 1.20 or more and 1.50 or less, and a density of the glass is 2.2 g / cm3 or more and 2.5 g / cm3 or less.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a glass cloth, a prepreg, and a printed wiring board. [Background technology]

[0002] Most printed wiring boards are usually manufactured by a method in which a substrate such as glass cloth is impregnated with a thermosetting resin such as an epoxy resin, dried to form a prepreg, one or more sheets of the prepreg are stacked together, and copper foil is stacked as necessary, followed by heating and pressurizing to form a laminate, and then a circuit pattern made of copper foil is formed on the laminate by photolithography and etching or plating. Furthermore, a multilayer printed wiring board is manufactured by a method in which the above-mentioned printed wiring board is used as a core substrate, a prepreg is stacked on the surface layer, and copper foil is further stacked on the outside of that, which is then heated and pressurized to form a multilayer board, and then a circuit is formed on the surface of the multilayer board.

[0003] On the other hand, in order to achieve high functionality and small size and light weight in recent digital devices, the printed wiring boards used are also required to be smaller, thinner, and denser. To achieve this, efforts are being made to thin the glass cloth used as the substrate and increase the number of layers in multilayer printed wiring boards to achieve high density. Here, the thickness of the glass cloth is required to be as thin as 16 μm or less, for example, in order to achieve high functionality and small size and light weight in cutting-edge smartphones and wearable devices.

[0004] Here, examples of thin glass cloths proposed include those described in Patent Documents 1 to 6. Specifically, Patent Document 1 proposes a glass cloth having a thickness of 7 to 14 μm, Patent Document 2 proposes a glass cloth having a thickness of 14 μm or less, Patent Document 3 proposes a glass cloth having a thickness of 10 μm or more and 40 μm or less, Patent Document 4 proposes a glass cloth having a thickness of 10 μm or more and 50 μm or less, Patent Document 5 proposes a glass cloth having a thickness of 5 to 15 μm, and Patent Document 6 proposes a glass cloth having a thickness of 25 μm or less.

[0005] The glass cloth described in Patent Document 1 has an average warp and weft diameter of 3.5 to 4.4 μm, 20 to 60 filaments, and a fiber length of 0.5 × 10 -6 ~1.7×10 -6 It is a glass cloth woven with glass yarns of 1 kg / m. By making the number of filaments in the weft yarns greater than that of the warp yarns so that the ratio of the mass of the warp yarns to the mass of the weft yarns is in the range of 1.26 to 1.42, the spacing between the weft yarns is less likely to increase and the air permeability can be adjusted to a small value within a specific range. This is said to improve the problems of pinholes and warping when the glass cloth is made into a prepreg.

[0006] The glass cloth described in Patent Document 2 has an average filament diameter of 3.0 to 4.3 μm for the warp and weft, the number of filaments in the weft is greater than that in the warp, and the ratio (weft / warp ratio) is 0.9 or more, and the degree of opening of the weft is greater than that of the warp, i.e., the width of the weft bundle is wider than that of the warp bundle. It is said that by increasing the number of filaments in the weft, which is easier to open, the distance between adjacent wefts becomes smaller, thereby suppressing the occurrence of pinholes when the glass cloth is used as a substrate.

[0007] The glass cloth described in Patent Document 3 has a warp and weft of mass 1.8×10 -6 kg / m or more 14×10 -6 The glass cloth is composed of glass yarns of 0.1 kg / m or less, and has a ratio of the average filament diameter of the weft to the average filament diameter of the warp (weft / warp ratio) of 1.01 or more and less than 1.20. It is disclosed that, by adopting the above configuration, even in a glass cloth with a thickness of 40 μm or less, it is possible to keep the distortion when a tensile load is applied and the weft / warp ratio within a specific range, and it is possible to manufacture a printed wiring board with little anisotropy in dimensional change and no warping or twisting.

[0008] The glass cloth described in Patent Document 4 is a glass cloth in which the warp and weft threads are made of the same type of glass thread, the width of the weft thread is close to the width of the warp thread, the ratio thereof (weft / warp ratio) is 0.8 or more and 1.2 or less, and the ratio of the elongation rate in the warp direction to the elongation rate in the weft direction when a load of 25 N to 100 N per 25 mm width is applied (weft / warp ratio) is 0.8 or more and 1.2 or less. By using the same glass thread for the warp and weft threads and making the cross-sectional shape and waviness state equivalent, it is said that a film substrate using this glass cloth has excellent dimensional stability.

[0009] The glass cloth described in Patent Document 5 is a glass cloth composed of glass yarns in which at least one of the warp and weft has an average filament diameter of less than 4.5 μm and the number of filaments on both sides is 5 to 70. Despite the small number of glass filaments constituting the glass cloth, it is said that a glass cloth excellent in dimensional stability and mechanical properties can be obtained by spreading and widening the glass filaments under gentle conditions to a surface glass coverage rate of 50% to 100%.

[0010] The glass cloth disclosed in Patent Document 6 is a glass cloth composed of glass yarns in which at least one of the warp and weft threads has an average filament diameter of 3 to 4 μm and the number of filaments is 70 to 200, and at least one of the warp and weft threads are arranged so that adjacent threads are arranged with substantially no gaps between them, and therefore the glass cloth is said to have excellent surface smoothness and excellent small hole processability.

[0011] In addition, thin glass cloths such as 1000 (12 μm), 1010 (11 μm), 1017 (14 μm), and 1015 (15 μm) are commercially available and can be used as glass cloths registered with the ICP standard.

[0012] With the recent development of the information and communication society, data communication and / or signal processing have come to be performed at high speed with large capacity, and the dielectric constant of printed wiring boards used in electronic devices has been significantly reduced. For this reason, many low-dielectric glass cloths have been proposed as glass cloths for use in printed wiring boards. For example, the low-dielectric glass cloth disclosed in Patent Document 9 realizes a low dielectric constant by blending a large amount of B2O3 in the glass composition and adjusting the blending amount of other components such as SiO2, as compared to the E-glass cloth that has been commonly used in the past. [Prior art documents] [Patent documents]

[0013] [Patent Document 1] Publication No. 5831665 [Patent Document 2] Publication No. 5936726 [Patent Document 3] Publication No. 5027335 [Patent Document 4] Publication No. 3897789 [Patent Document 5] Publication No. 4446754 [Patent Document 6] Publication No. 3756066 [Patent Document 7] Japanese Patent Application Publication No. 10-245743 [Patent Document 8] JP 2001-269931 A [Patent Document 9] Japanese Patent Application Publication No. 11-292567 Summary of the Invention [Problem to be solved by the invention]

[0014] Patent Document 6 describes a glass cloth having a thickness of 25 μm or less, but the glass cloths specifically disclosed in Examples 1 to 5 have a thickness of 17 to 21 μm, with the thinnest being 17 μm. The glass cloth disclosed in Patent Document 6 requires the use of glass yarns having a large number of filaments in order to arrange adjacent yarns with no gaps between them, and as a result, it is difficult to reduce the thickness of the glass cloth. Specifically, in Examples 1 to 5 in Patent Document 6, glass yarns having 100 filaments were used for both the warp and weft.

[0015] The glass cloth disclosed in Patent Document 5 achieves a thin glass cloth thickness of 5 μm or more and less than 15 μm by reducing the average diameter of the glass filaments constituting the warp and weft and by reducing the number of filaments constituting the warp and weft. The glass cloths in Patent Documents 1 and 2 are also thin. However, the glass cloth disclosed in Patent Document 1 has a mass of 0.5×10 -6 ~1.7×10 -6 Because thin glass yarns (kg / m) are used, the rigidity of the glass cloth is low, which poses the issue of waviness occurring when the prepreg is applied. In Patent Document 2, the mass of both the warp and weft yarns is 1.65 × 10 -6 Because thin glass yarns are used, which are lighter than BC3000, BC3750, BC5000, and BC6000 (weight: kg / m or less), the rigidity of the glass cloth is low, which can cause waviness when the prepreg is coated. Furthermore, the glass cloth disclosed in Patent Document 5 is also prone to waviness because the number of filaments constituting the warp and weft is reduced.

[0016] Here, the waviness of glass cloth refers to a phenomenon in which the prepreg is deformed into a shape as shown in Fig. 1 during the process of manufacturing the prepreg by impregnating the glass cloth with a thermosetting resin and drying it. If the waviness of the prepreg is large, there are problems such as wrinkles occurring due to the waviness and positioning being difficult in the subsequent prepreg molding process, resulting in misalignment. In addition, when the prepregs are stored in a pile or wound up in a roll, the convex parts of the waviness come into contact with each other and rub against each other, which causes a problem of cracks occurring in the curable resin in the B stage, i.e., in a semi-cured state, and the resin peeling off.

[0017] The waviness of the prepreg occurs because the stress caused by the shrinkage of the thermosetting resin due to drying during the prepreg coating process is alleviated by the waviness in the weft direction, which is not restrained by the line tension. For example, Patent Document 7 states that the mass per unit area is 48 g / m 2 Patent Document 8 describes that waviness occurs when a prepreg having a thickness of 60 μm or less is used to manufacture a prepreg.

[0018] As described above, waviness occurs when the curable resin shrinks during curing, causing the glass cloth to bend due to the force of shrinking in the weft direction where tension is not maintained. Therefore, the thinner the glass cloth is and the lower its rigidity, the more likely waviness occurs. In addition, when the glass cloth becomes thinner and weaker, the line tension applied in the warp direction also becomes smaller, so that the glass cloth is more likely to flutter and / or sag during the prepreg coating process. Therefore, the thinner the glass cloth is, the more likely waviness is to occur.

[0019] The glass cloth described in Patent Document 4 is capable of making the wavy structures of the warp and weft yarns equivalent by subjecting them to fiber-opening processing under low tension conditions, and the elongation rates of the warp and weft yarns when a tensile load is applied are equivalent, resulting in excellent dimensional stability. However, since the glass cloth described in Patent Document 4 uses the same glass yarn for the warp and weft, it is difficult to make the undulation structures of the warp and weft equivalent. The glass cloth described in Patent Document 4 also stretches more in the weft direction than in the warp direction, and the dimensional stabilization effect in the weft direction during prepreg coating is insufficient, leaving room for improvement in preventing waviness.

[0020] The glass cloth described in Patent Document 3 is a glass cloth that realizes small distortion (elongation) and small anisotropy of distortion when a tensile load is applied by using glass yarns for the weft yarns having a larger filament diameter than the warp yarns and adjusting the number of filaments. The glass cloth described in Patent Document 3 is also useful for improving waviness during prepreg coating because the wavy structure of the weft yarns is reduced. However, in the glass cloth of Patent Document 3, in order to reduce distortion when a tensile force is applied, a 1.8×10 -6 Since it is necessary to use a relatively thick glass yarn having a thickness of 1 kg / m or more, as specifically disclosed in the examples of the patent document, even the thinnest glass cloth has a minimum thickness of 17 μm, and it is not possible to obtain a glass cloth having a thickness of 16 μm or less. In addition, the glass cloth of Patent Document 3, as shown in the examples of the patent document, uses thick weft yarns with a filament diameter of 4.5 μm or more and 100 filaments, thereby reducing distortion when tensile force acts in the weft direction. Therefore, there is also a problem that the interval between adjacent weft yarns becomes narrow. Usually, after impregnating a glass cloth with resin and removing excess resin, the resins on the front and back of the glass cloth penetrate each other through the non-glass parts of the glass cloth and are made uniform. However, the glass cloth of Patent Document 3 does not have sufficient resin impregnation, making it difficult to make the resin layer uniform on the front and back of the glass cloth.

[0021] In addition, glass cloths with a thickness of 16 μm or less, such as 1000 (12 μm), 1010 (11 μm), 1017 (14 μm), and 1015 (15 μm), which are registered in the ICP standard, are available commercially. However, all of these glass cloths have the problem of waviness during the above-mentioned prepreg coating, and improvement in this area is desired. Furthermore, in the manufacturing process of printed wiring boards, it is known that the heat and pressure in the lamination process and the etching out of part of the copper foil in the circuit pattern formation process cause dimensional changes, warping, and twisting of the copper-clad laminate. The above-mentioned 1000, 1010, 1017, 1015 style glass cloths with a thickness of 16 μm or less have a problem that they are highly susceptible to the above-mentioned problems of dimensional changes, warping, and twisting due to their weak mechanical strength. In particular, dimensional changes are likely to occur in the weft direction, and the variation in the amount of dimensional change is also large. The higher the density of printed wiring boards, the higher the importance of stability against dimensional changes, but on the other hand, if a thin glass cloth is used to increase density, dimensional stability will deteriorate as mentioned above.

[0022] As disclosed in Patent Document 9, low dielectric glass exhibits low dielectric properties by adjusting the glass composition, such as by increasing the amount of B2O3 in the glass composition. By controlling the glass composition to reduce the dielectric constant, the specific gravity of the glass constituting the glass yarn becomes lighter, and the rigidity of the glass yarn tends to become weaker. Therefore, compared with glass cloth composed of conventional E glass, low dielectric glass cloth tends to be more prone to waviness and less dimensionally stable.

[0023] The present invention has been made in view of the above problems, and has an object to provide a low dielectric glass cloth having a thickness of 16 μm or less which is easy to handle with minimal waviness when applied to a prepreg, has resin impregnation properties that enable uniform resin layers on both sides of the glass cloth, and has excellent dimensional stability, as well as a prepreg and a substrate for printed wiring boards which use the low dielectric glass cloth. [Means for solving the problem]

[0024] As a result of intensive research aimed at solving the above problems, the inventors have discovered that, by having a low dielectric glass cloth composed of warp and weft threads have a specific woven structure, it is possible to increase the rigidity of the glass cloth while maintaining a thickness of 16 μm or less, reduce waviness during prepreg coating and provide excellent handleability, have excellent resin impregnation properties, enable the resin layer to be uniform on both sides of the glass cloth, and provide excellent dimensional stability, thereby completing the present invention.

[0025] That is, the present invention is as follows. [1] A glass cloth having a thickness of 8 μm to 16 μm, the glass cloth being configured as warp and weft yarns each made of a plurality of glass filaments, The average mass per unit length of the warp thread is 1.40 x 10 -6 kg / m or more 1.60×10 -6 Less than kg / m The average mass per unit length of the weft is 1.60 x 10 -6 kg / m or more 3.00×10 -6 kg / m or less, The ratio of the average mass per unit length of the weft to the average mass per unit length of the warp (weft / warp ratio) is greater than 1.20 and less than or equal to 1.50; The density of glass is 2.2 g / cm 3 More than 2.5g / cm 3 Below is the Glass cloth. [2] The average filament count of the warp and weft yarns is substantially the same; and The average filament diameter of the warp yarn is 3.7 μm or more and 4.3 μm or less, The average filament diameter of the weft yarn is 4.2 μm or more and 5.3 μm or less, The ratio of the average filament diameter of the weft to the average filament diameter of the warp (weft / warp ratio) is 1.07 or more and 1.40 or less. [1] The glass cloth according to the present invention. [3] The average filament diameters of the warp and weft yarns are substantially the same, and The average number of warp filaments is 45 or more and 70 or less, The average number of filaments in the weft is 55 or more and 80 or less, The ratio of the average number of filaments in the weft to the average number of filaments in the warp (weft / warp ratio) is greater than 1.25 and less than or equal to 1.50; [1] The glass cloth according to the present invention. [4] The coefficient (Y: weft occupancy rate) indicating the ratio of the area where the weft is present in the longitudinal direction (MD direction) of the weft, calculated by the formula (1), is 76% or more and 90% or less. The glass cloth according to any one of [1] to [3]. Y = F / (25000 / G) × 100 (1) (In formula (1), F is the weft width (μm), and G is the weaving density of the weft (pieces / 25 mm).) [5] The gap width between adjacent weft yarns in the longitudinal direction (MD direction) is 40 μm or more and 80 μm or less. The glass cloth according to any one of [1] to [4]. [6] A dielectric constant of 5.0 or less at a frequency of 10 GHz. The glass cloth according to any one of [1] to [5]. [7] [1] to [6], and and a matrix resin, Prepreg. [8] The glass yarns are made of a plurality of glass filaments as warp and weft yarns, and the thickness is 8 μm or more and 16 μm or less, and the density of the glass is 2.2 g / cm 3 More than 2.5g / cm 3 A prepreg having a glass cloth and a matrix resin, 1) to 3) below); 1) The resin content is 50% or more and 83% or less by mass. 2) The ratio of the thickness of the first resin layer located on one side of the glass cloth to the thickness of the second resin layer located on the other side of the glass cloth is 0.7 or more and 1.3 or less; 3) The amount of waviness is less than 3 mm. Prepreg meets the above requirements. [9] The glass cloth is the glass cloth according to any one of [1] to [6]. [8] The prepreg according to [8].

[10] The gap width between adjacent weft yarns in the longitudinal direction (MD direction) is 40 μm or more and 80 μm or less. The prepreg according to [8] or [9].

[11] A printed wiring board comprising the prepreg according to any one of [7] to

[10] . Effect of the Invention

[0026] According to the present invention, it is possible to provide a thin low dielectric glass cloth having a thickness of 16 μm or less, which has excellent handleability with little waviness during prepreg coating, excellent resin impregnation when made into prepreg, and excellent dimensional stability. [Brief description of the drawings]

[0027] [Figure 1] FIG. 1 is a schematic diagram of a prepreg having corrugations. [Diagram 2] FIG. 1 is a diagram showing a method for measuring the height of waviness. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0028] Below, we will explain in detail the embodiment of the present invention (hereinafter referred to as the "present embodiment"). However, the present invention is not limited to this embodiment, and various modifications are possible without departing from the gist of the present invention.

[0029] <Glass cloth> The glass cloth of this embodiment is a glass cloth having a thickness of 8 μm or more and 16 μm or less, which is constituted of glass yarns each consisting of a plurality of glass filaments as warp yarns and weft yarns. By setting the thickness of the glass cloth to 8 μm or more and 16 μm or less, a thin prepreg having a thickness, for example, 18 μm or more and 35 μm or less, can be obtained, and a printed wiring board that can accommodate the increased functionality and smaller, lighter weight of electronic devices can be obtained.

[0030] In the glass cloth of this embodiment, the mass per unit length of the warp yarn is 1.40 × 10 -6 kg / m or more 1.60×10 -6 kg / m. In the glass cloth of this embodiment, the mass per unit length of the weft is 1.60 × 10 -6 kg / m or more 3.00×10 -6 kg / m or less. The ratio of the average mass per unit length of the weft to the average mass per unit length of the warp, that is, the mass ratio of the warp to the weft (weft / warp ratio) is greater than 1.20 and equal to or less than 1.50.

[0031] The density of the glass constituting the glass cloth of this embodiment is 2.10 g / cm 3 More than 2.50g / cm 3 The density of the glass is preferably 2.20 g / cm 3 More than 2.45g / cm 3 Less than or equal to 2.25 g / cm 3 More than 2.45g / cm 3 The following is the result.

[0032] The density of the glass in the E-glass cloth that has been commonly used up until now is 2.54g / cm 3 In order to reduce the dielectric constant and dielectric tangent of glass cloth, it is necessary to change the composition of the glass, and low dielectric glass contains more substances with relatively low specific gravity, such as B2O3, compared to E-glass cloth. Therefore, the density of low dielectric glass is smaller than that of E-glass, and the strength of the glass threads also tends to decrease. During the manufacturing process, the glass cloth is subjected to physical stress in the process of adjusting the amount of silane agent applied after impregnation coating with a silane treatment agent, or in the fiber opening process. In addition, when the glass cloth is used for prepreg coating, the glass cloth is also subjected to physical stress in the process of adjusting the amount of resin varnish and drying after impregnation coating with resin varnish. In order to transport the glass cloth stably and continuously in the above processes without breaking it, it is necessary for the warp yarns to have a certain strength or more, and the warp yarn strength can be maintained by setting the density of the glass to 2.10 g or more. In addition, since the density of the glass is 2.10 g or more, the strength of the weft yarn can be reinforced, and waving can be prevented. The density of glass is 2.50 g / cm 3 By satisfying the following conditions, excellent low dielectric properties can be obtained.

[0033] As mentioned above, the density of glass is controlled by blending a large amount of substances with a relatively low specific gravity, such as B2O3, in other words, by controlling the composition of the components that make up the glass. 3 More than 2.50g / cm 3 It is controlled within the following range: The composition of the glass can be appropriately adjusted, and may be, for example, as long as it has the following composition. The Si content of the glass cloth, calculated as SiO2, is preferably 40 to 60 mass %, more preferably 45 to 55 mass %, further preferably 47 to 53 mass %, and even more preferably 48 to 52 mass %. The B content of the glass cloth, calculated as B2O3, is preferably 15 to 30 mass%, more preferably 17 to 28 mass%, even more preferably 20 to 27 mass%, still more preferably 21 to 25 mass%, and even more preferably 21 to 24 mass%. The Al content of the glass cloth is preferably 10 to 20 mass %, more preferably 11 to 18 mass %, and further preferably 12 to 17 mass %, calculated as Al2O3. The Ca content of the glass cloth is, in terms of CaO, preferably 4 to 12 mass %, more preferably 5 to 10 mass %, and even more preferably 6 to 9 mass %. Other compositions may include, for example, Mg, P, Na, K, Ti, Zn, etc. The composition of the glass can be adjusted according to the amount of raw material used to prepare the glass filaments.

[0034] The ranges of the mass per unit length of the warp yarn, the mass per unit length of the weft yarn, and the mass ratio of the warp yarn to the weft yarn are preferably: warp; 1.40×10 -6 kg / m or more 1.57×10 -6 kg / m or less, weft: 1.65×10 -6 kg / m or more 2.80×10 -6 kg / m or less, and the weft / warp ratio is 1.17 to 1.79, more preferably 1.40×10 -6 kg / m or more 1.55×10 -6 kg / m or less, weft: 1.70×10 -6 kg / m or more 2.50×10 -6 kg / m or less, weft / warp ratio: 1.21 or more and 1.62 or less.

[0035] During the manufacturing process, glass cloth is subjected to physical stress in the process of adjusting the amount of silane agent applied after impregnation coating with a silane treatment agent, or in the fiber opening process. In addition, when glass cloth is used for prepreg coating, the glass cloth is also subjected to physical stress in the process of adjusting the amount of resin varnish and drying after impregnation coating with resin varnish. In order to transport the glass cloth stably and continuously without breaking in the above processes, it is necessary for the warp yarns to have a certain level of strength, so the average mass per unit length of the warp yarns is 1.40 x 10 -6 On the other hand, the average mass per unit length of the warp thread must be 1.80×10 -6 By using glass yarns of less than kg / m, the thickness can be maintained at 16 μm or less, and the weaving density can be increased to, for example, 90 or more, which tends to suppress the occurrence of pinholes.

[0036] As a weft thread, the average mass per unit length is 1.60 × 10 -6 By using glass yarns of 1.0 kg / m or more, the reinforcing effect against the shrinkage of the thermosetting resin during the prepreg coating is enhanced, which is advantageous in suppressing the occurrence of waviness. The larger the mass per unit length of the glass yarns used for the weft yarns, the stronger the reinforcing effect tends to be, which is preferable. However, in order to keep the thickness of the glass cloth to 16 μm or less, the average mass per unit length of the weft yarns should be 3.00×10 -6 It must be less than or equal to kg / m.

[0037] In addition, since the mass ratio of warp to weft is greater than 1.20, the difference between the rigidity of the weft and that of the warp becomes large, so that even if the yarn used for the weft is thin and has low rigidity, the waviness of the weft during the weaving process can be suppressed to a small level. In addition, in the weaving process, the waviness of the weft inserted without any restraining force varies depending on the variation in the line tension acting on the warp, but by keeping the mass ratio of warp to weft within the above range, the variation in the waviness structure of the weft can be suppressed to a small level. Therefore, the dimensional stabilization effect can be improved against the cure shrinkage of the thermosetting resin in the prepreg coating process.

[0038] On the other hand, when the mass ratio of warp threads to weft threads is 1.50 or less, the difference in rigidity between the warp threads and weft threads is prevented from becoming extremely large, and the wavy structure of the weft threads is moderately preserved so that there is no large difference in the wavy structure between the warp threads and weft threads, thereby preventing anisotropy in dimensional stability when made into a printed wiring board. By setting the mass per unit length of the warp yarns, the mass per unit length of the weft yarns, and the mass ratio of the warp yarns to the weft yarns within the above-mentioned ranges, it is possible to increase the rigidity in the warp and weft directions while preventing anisotropy in dimensional stability when made into a printed wiring board. Therefore, a glass cloth having a thickness of 16 μm or less can be obtained, which has a strength that does not break during line transportation, can reduce waviness of the prepreg, and has excellent stability against dimensional changes. In addition, by setting the mass ratio of the warp yarns to the weft yarns to 1.50 or less, the density of the glass constituting the glass cloth can be increased to 2.10 g / cm. 3More than 2.50g / cm 3 As described below, even if a low dielectric glass cloth is used, waviness of the prepreg can be reduced and the prepreg can have excellent stability against dimensional changes. The average mass per unit length of the warp yarn and the average mass per unit length of the weft yarn can be controlled, for example, by adjusting the filament diameter and / or the average number of filaments constituting the warp yarn and the weft yarn.

[0039] The glass cloth of this embodiment is preferably a glass cloth (hereinafter also referred to as glass cloth X) in which the average filament numbers of the warp and weft are substantially the same, the average filament diameter of the warp is 3.7 μm or more and 4.3 μm or less, the average filament diameter of the weft is 4.2 μm or more and 5.3 μm or less, and the ratio of the average filament diameter of the weft to the average filament diameter of the warp (weft / warp ratio) is 1.07 or more and 1.40 or less. By setting the number of warp and weft filaments and the filament diameter within the above-mentioned ranges, it is possible to maintain the thickness of the glass cloth at 16 μm or less, while preventing anisotropy in the dimensional stability of the printed wiring board and providing a glass cloth with high rigidity in the weft direction.

[0040] The ranges of the average filament diameters of the warp and weft threads and the weft / warp ratio are more preferably, respectively, warp: 3.8 μm or more and 4.2 μm or less, weft: 4.3 μm or more and 5.2 μm or less, and the weft / warp ratio of the average filament diameter: 1.08 or more and 1.25 or less, and even more preferably, warp: 3.9 μm or more and 4.1 μm or less, weft: 4.4 μm or more and 5.1 μm or less, and the weft / warp ratio of the average filament diameter: 1.09 or more and 1.20 or less.

[0041] The average filament counts of the warp and weft yarns being substantially the same means that the ratio of the number of filaments in the warp yarn to the number of filaments in the weft yarn (weft / warp ratio) is in the range of 0.94 to 1.06. A weft / warp ratio of the average filament counts of 0.94 to 1.06 is preferable because it provides the effect of a large filament diameter of the weft yarn, i.e., rigidity in the weft direction. In addition, in this embodiment, when the average filament numbers of the warp and weft are substantially the same, the filament numbers of the warp and weft are preferably 60 or less. When the filament numbers of the warp and weft are 60 or less, the filaments are easily diffused by physical processing in the glass cloth manufacturing process, and the filament distribution in the Z direction of the glass yarn bundle can be reduced, so that the thickness of the glass cloth can be easily reduced. In order to reduce the thickness of the glass cloth, it is preferable to have a smaller number of filaments, but from the viewpoint of the strength and handleability of the glass cloth, when the average filament numbers of the warp and weft are substantially the same, the lower limit of the average filament numbers of the warp and weft is preferably 44 or more, more preferably 46 or more, and even more preferably 48 or more.

[0042] In addition, the glass cloth of this embodiment is preferably a glass cloth (hereinafter also referred to as glass cloth Y) in which the average filament diameters of the warp and weft are substantially the same, the average number of filaments of the warp is 45 to 70, the average number of filaments of the weft is 55 to 80, and the ratio of the average number of filaments of the weft to the average number of filaments of the warp (weft / warp ratio) is greater than 1.25 and less than 1.50. By setting the number of warp and weft filaments and the filament diameter within the above-mentioned ranges, it is possible to obtain a glass cloth with high rigidity in the weft direction without impairing the dimensional stability of the printed wiring board while maintaining the thickness of the glass cloth at 16 μm or less.

[0043] The ranges of the average number of filaments in the warp and weft threads and the ratio thereof (weft / warp ratio) are more preferably, respectively, 43 or more and 65 or less in the warp thread, 57 or more and 75 or less in the weft thread, and the weft / warp ratio of the average number of filaments is 1.27 or more and 1.45 or less, and even more preferably, 45 or more and 60 or less in the warp thread, 60 or more and 70 or less in the weft thread, and the weft / warp ratio of the average number of filaments is 1.30 or more and 1.40 or less, respectively.

[0044] The average filament diameters of the warp and weft yarns being substantially the same means that the ratio of the warp filament diameter to the weft filament diameter (weft / warp ratio) is in the range of 0.95 to 1.05. When the weft / warp ratio of the average filament diameter is in the range of 0.95 to 1.05, the effect of increasing the number of filaments in the weft yarn, that is, the rigidity in the weft direction, is exhibited, which is preferable. In the present embodiment, when the average filament diameters of the warp and weft are substantially the same, the filament diameters of the warp and weft are preferably 3.8 μm or more. When the average filament diameters of the warp and weft are 3.8 μm or more, the rigidity of the glass cloth can be increased. In order to increase the rigidity of the glass cloth, a larger filament diameter is preferable, but from the viewpoint of the thickness of the glass cloth, when the average filament diameters of the warp and weft are substantially the same, the upper limit of the filament diameters of the warp and weft is preferably 4.4 μm or less, more preferably 4.3 μm or less, and even more preferably 4.2 μm or less.

[0045] Of the above-mentioned glass cloth X and glass cloth Y, the glass cloth of this embodiment is preferably glass cloth X because it has superior dimensional stability.

[0046] In the glass cloth of the present embodiment, the coefficient (Y: weft occupancy) indicating the proportion of the area in the longitudinal direction (MD) of the weft, calculated by the formula (1), is preferably 76% or more and 90% or less. Here, the weft occupancy rate Y is a value obtained by dividing the weft width by the sum of the weft width and the width of the gap between the wefts, and is calculated using formula (1). Y = F / (25000 / G) × 100 (1) (In formula (1), F is the weft width (μm), and G is the weaving density of the weft (pieces / 25 mm).) The weft width is the average value of the widths of all the wefts obtained by observing the surface of a glass cloth sample having a size of 100 mm x 100 mm under a microscope. The weft occupancy ratio Y is more preferably 78% or more and less than 89%, and further preferably 79% or more and 88% or less.

[0047] In the glass cloth of this embodiment, the weft is made of glass yarns having a larger mass than the warp, so the width of the weft is wider than the width of the warp, and the gap between the weft and the weft tends to be wider than the gap between the warp and the warp. Here, by ensuring an appropriate amount of gap between the weft and the weft and allowing the presence of a portion where no glass is present, when the glass cloth is impregnated with resin, the resin on one side and the other side penetrate each other through the portion where no glass is present of the glass cloth after removing excess resin to adjust the amount of resin. This results in a prepreg in which the thickness of the resin relative to the glass cloth is the same as the thickness of the resin. From the above viewpoint, the weft occupancy rate Y is preferably 90% or less. In addition, by making the weft occupancy rate Y 76% or more, the glass yarns are uniformly distributed throughout the glass cloth, and the areas where no glass yarns exist, called basket holes, which are formed by gaps between warp yarns and gaps between weft yarns, can be made smaller, thereby suppressing the occurrence of pinholes.

[0048] Furthermore, in the glass cloth of this embodiment, the gap width between adjacent wefts in the longitudinal direction (MD) of the wefts, i.e., the distance between the wefts, is preferably 40 μm or more and 80 μm or less, more preferably 45 μm or more and 75 μm or less, and even more preferably 50 μm or more and 70 μm or less. By setting the spacing between weft yarns to 40 μm or more and 80 μm or less, a proper balance between the distribution of the glass cloth and the impregnation of the resin is achieved, thereby simultaneously suppressing the occurrence of pinholes and ensuring that the resin is applied symmetrically to the glass cloth. The spacing between the weft yarns can be controlled, for example, by adjusting the weft width and / or the weave density of the weft yarns. The interval between the wefts can also be adjusted by carrying out a flattening process of the yarns constituting the glass cloth through, for example, opening the yarns to adjust the yarn width. Examples of the opening treatment include opening by water flow pressure, opening by high-frequency vibration using a liquid as a medium, processing by pressure of a fluid having a surface pressure, and processing by applying pressure with a roll. Among these opening treatment methods, from the viewpoint of uniformity of the yarn width, opening by water flow pressure and / or opening by high-frequency vibration using a liquid as a medium are preferred. From the viewpoint of enhancing the effect of the flattening treatment, it is preferred to carry out the opening treatment etc. in a state where the tension applied to the glass cloth for transportation is reduced. Furthermore, the adjustment of the spacing between the weft yarns can also be carried out by flattening the glass cloth in a state where an organic substance exhibiting lubricant properties is attached to the glass yarn, or the glass cloth in a state where a binder, a glue agent, etc. used in weaving a normal glass cloth is attached, or by carrying out a surface treatment with a silane coupling agent after the opening treatment and then carrying out the opening treatment.

[0049] The glass yarn constituting the glass cloth of the present embodiment is not particularly limited, and low dielectric constant glass such as D glass, L glass, NE glass, silica glass (Q glass), etc. can be used.

[0050] The weave structure of the glass cloth is not particularly limited, but examples thereof include plain weave, sash weave, satin weave, twill weave, etc. Furthermore, a mixed weave structure using different types of glass yarns may be used. Among these, the plain weave structure is preferred.

[0051] Furthermore, the glass cloth constituting the laminate used in the printed wiring board, etc. may be subjected to a surface treatment with a treatment liquid containing a silane coupling agent. As the silane coupling agent, a commonly used silane coupling agent may be used, and an acid, a dye, a pigment, a surfactant, etc. may be added as necessary.

[0052] As the silane coupling agent, for example, a silane coupling agent represented by the formula (2) is preferably used. X(R) 3-n SiY n (2) In formula (2), X is an organic functional group having at least one of an amino group and an unsaturated double bond group, each Y is independently an alkoxy group, n is an integer of 1 to 3, and each R is independently a group selected from the group consisting of a methyl group, an ethyl group, and a phenyl group.

[0053] X is preferably an organic functional group having at least three or more of amino groups and unsaturated double bond groups, and more preferably an organic functional group having at least four or more of amino groups and unsaturated double bond groups. The alkoxy group may be in any form, but from the viewpoint of stabilizing the treatment of the glass cloth, an alkoxy group having 5 or less carbon atoms is preferred.

[0054] Specific examples of the silane coupling agent include N-β-(N-vinylbenzylaminoethyl)-γ-aminopropyltrimethoxysilane and its hydrochloride, N-β-(N-vinylbenzylaminoethyl)-γ-aminopropylmethyldimethoxysilane and its hydrochloride, N-β-(N-di(vinylbenzyl)aminoethyl)-γ-aminopropyltrimethoxysilane and its hydrochloride, N-β-(N-di(vinylbenzyl)aminoethyl)-N-γ-(N-vinylbenzyl)-γ-aminopropyltrimethoxysilane and its hydrochloride, N-β Examples of known simple substances include -(N-benzylaminoethyl)-γ-aminopropyltrimethoxysilane and its hydrochloride, N-β-(N-benzylaminoethyl)-γ-aminopropyltriisoethoxysilane and its hydrochloride, γ-(2-aminoethyl)aminopropyltrimethoxysilane, γ-(2-aminoethyl)aminopropyltriethoxysilane, aminopropyltrimethoxysilane, vinyltrimethoxysilane, methacryloxypropyltrimethoxysilane, acryloxypropyltrimethoxysilane, and the like, or mixtures thereof.

[0055] The molecular weight of the silane coupling agent is preferably 100 to 600, more preferably 150 to 500, and further preferably 200 to 450. Among these, it is preferable to use two or more silane coupling agents having different molecular weights. By treating the glass fiber surface with two or more silane coupling agents having different molecular weights, the density of the treatment agent on the glass surface tends to increase, and the reactivity with the matrix resin tends to be further improved.

[0056] The ignition loss value of the glass cloth is preferably 0.10% by mass or more and 1.20% by mass or less, more preferably 0.11% by mass or more and 1.10% by mass or less, and even more preferably 0.12% by mass or more and 1.00% by mass or less. By making the ignition loss value 0.10% by mass or more and 1.2% by mass or less, the transportability, i.e., the handleability, of the prepreg can be improved more than before. In addition, the deterioration of the insulation reliability of the board caused by the resin and the glass cloth easily peeling off at the interface can be suppressed, and the deterioration of the insulation reliability of the board caused by the plating solution soaking into the glass cloth tends to be suppressed. The "ignition loss value" referred to here can be measured according to the method described in JIS R 3420. That is, first, the glass cloth is placed in a dryer at 110°C and dried for 60 minutes. After drying, the glass cloth is transferred to a desiccator, left for 20 minutes, and allowed to cool to room temperature. After cooling, the glass cloth is weighed to the nearest 0.1 mg. Next, the glass cloth is heated in a muffle furnace at 625°C for 20 minutes. After heating in the muffle furnace, the glass cloth is transferred to a desiccator, left for 20 minutes, and allowed to cool to room temperature. After cooling, the glass cloth is weighed to the nearest 0.1 mg. The ignition loss value obtained by the above measurement method defines the amount of silane coupling agent treatment of the glass cloth.

[0057] <Glass cloth manufacturing method> The method for producing the glass cloth of the present embodiment is not particularly limited, but a suitable example is a method having a coating process in which the surfaces of the glass filaments are almost completely covered with a silane coupling agent using a treatment liquid having a silane coupling agent concentration of 0.1 to 3.0 wt %, a fixing process in which the silane coupling agent is fixed to the surfaces of the glass filaments by heating and drying, and a fiber-opening process in which the glass yarns of the glass cloth are opened.

[0058] As the solvent for dissolving or dispersing silane coupling agent, water or organic solvent can be used, but from the viewpoint of safety and global environmental protection, it is preferable to use water as the main solvent.As the method for obtaining the treatment liquid with water as the main solvent, it is preferable to directly put silane coupling agent into water, or to dissolve silane coupling agent in a water-soluble organic solvent to make an organic solvent solution, and then put the organic solvent solution into water.In order to improve the water dispersibility and stability of silane coupling agent in the treatment liquid, it is also possible to use surfactant in combination.

[0059] Methods for applying the treatment liquid to the glass cloth include (a) a method in which the treatment liquid is stored in a bath and the glass cloth is immersed and passed through the treatment liquid (hereinafter referred to as the "immersion method"), and (b) a method in which the treatment liquid is directly applied to the glass cloth using a roll coater, a die coater, a gravure coater, etc. When applying the treatment liquid by the immersion method (a) above, it is preferable to immerse the glass cloth in the treatment liquid for 0.5 seconds or more and 1 minute or less.

[0060] As a method for heating and drying the solvent after applying the treatment liquid to the glass cloth, known methods such as hot air and electromagnetic waves can be used. The heating and drying temperature is preferably 90° C. or higher, more preferably 100° C. or higher, so that the reaction between the silane coupling agent and the glass is sufficiently carried out. The heating and drying temperature is preferably 300° C. or lower, more preferably 200° C. or lower, so as to prevent deterioration of the organic functional group of the silane coupling agent.

[0061] The method for opening the fibers in the opening step is not particularly limited, but examples thereof include a method for opening the glass cloth with spray water (high pressure water opening), a vibro washer, ultrasonic water, a mangle, etc. In order to keep the total area of ​​the basket holes within a certain range, it is preferable to carry out the opening step with spray water. When the fibers are spread using spray water, the water pressure may be appropriately set, and it is preferable to keep the water pressure constant in order to adjust the total area of ​​the basket holes present in the glass cloth. Keeping the water pressure constant here means reducing the difference between the spray water pressure set for spreading and the maximum and minimum values ​​of the actual water pressure. A heat drying step may also be included before or after the spreading step.

[0062] <Prepreg> One of the present embodiments is a prepreg (hereinafter referred to as prepreg A) that is composed of the glass cloth of the present embodiment and a matrix resin. The matrix resin is impregnated into the glass cloth.

[0063] One of the present embodiments is a prepreg (hereinafter referred to as prepreg B) that is composed of a glass cloth having a thickness of 8 μm to 16 μm and that is made of glass yarns consisting of a plurality of glass filaments as warp and weft yarns, and a matrix resin. The matrix resin is impregnated into the glass cloth. Prepreg B is the following 1) to 3); 1) Resin content is 50% or more and 83% or less by mass. 2) The ratio of the thickness of the first resin layer located on one side of the glass cloth to the thickness of the second resin layer located on the other side of the glass cloth is 0.7 or more and 1.3 or less; 3) The amount of waviness is less than 3 mm. Meet the following.

[0064] The glass cloth constituting the prepreg B in this embodiment is a low dielectric glass cloth, and the density of the glass constituting the glass cloth is 2.2 g / cm 3 More than 2.5g / cm 3 The following is the result.

[0065] The glass cloth constituting the prepreg of the present embodiment is preferably the glass cloth of the present embodiment. By using the glass cloth of the present embodiment, waviness during coating of the prepreg is reduced, and a prepreg having excellent stability in dimensional change can be obtained.

[0066] The resin content in prepreg B of this embodiment is 50% by mass or more and 83% by mass or less, preferably 52% by mass or more and 80% by mass or less, and more preferably 54% by mass or more and 76% by mass or less, when the total amount of prepreg B is taken as 100% by mass. By having a resin content of 50% by mass or more and 83% by mass, it is possible to respond to high performance of electronic devices.

[0067] In the prepreg B of this embodiment, the ratio of the thickness of the first resin layer located on one side of the glass cloth to the thickness of the second resin layer located on the other side of the glass cloth is 0.70 or more and 1.30 or less, preferably 0.80 or more and 1.20 or less, and more preferably 0.85 or more and 1.15 or less. By making the ratio of the thickness of the first resin layer to the thickness of the second resin layer 0.70 or more and 1.30 or less, waviness of the prepreg can be suppressed even in a thin glass cloth having a thickness of 16 μm or less.

[0068] Moreover, the amount of waviness in the prepreg B of this embodiment is 3 mm or less, preferably 2 mm or less, and more preferably 1 mm or less. It is presumed that the waviness of the prepreg of 3 mm or less can suppress the occurrence of distortion such as bending of the glass yarns forming the glass cloth when the prepreg is heated and pressure molded, and is also preferable because it provides excellent stability against dimensional change. Here, the waviness of the prepreg is a value determined as follows. The prepreg is cut to a size of 340 mm x 510 mm to prepare a test piece for measuring the amount of waviness. As shown in Figure 2, it is placed on a flat surface measuring table 1, and the height 3 of the waviness generated in the prepreg 2 is measured, and the maximum value is defined as the "amount of waviness."

[0069] The prepreg of the present embodiment can be produced by a conventional method, for example, by impregnating a glass cloth with a varnish in which a matrix resin is diluted with an organic solvent, volatilizing the organic solvent in a drying furnace, and curing the thermosetting resin to a B-stage state, i.e., a semi-cured state, to produce a resin-impregnated prepreg.

[0070] As the matrix resin, either a thermosetting resin or a thermoplastic resin can be used. The thermosetting resin is not particularly limited, but examples thereof include: a) epoxy resins obtained by reacting a compound having an epoxy group with a compound having at least one of an amino group, a phenol group, an acid anhydride group, a hydrazide group, an isocyanate group, a cyanate group, and a hydroxyl group that reacts with the epoxy group, without a catalyst or by adding a catalyst having a reaction catalytic ability, such as an imidazole compound, a tertiary amine compound, a urea compound, or a phosphorus compound, to harden the compound; b) radical polymerization type hardening resins obtained by hardening a compound having at least one of an allyl group, a methacryl group, and an acrylic group, using a thermal decomposition type catalyst or a photodecomposition type catalyst as a reaction initiator; c) maleimide triazine resins obtained by hardening a compound having a cyanate group with a compound having a maleimide group; d) thermosetting polyimide resins obtained by hardening a maleimide compound with an amine compound; and e) benzoxazine resins obtained by crosslinking and hardening a compound having a benzoxazine ring by thermal polymerization. The thermoplastic resin is not particularly limited, but examples thereof include polyphenylene ether, modified polyphenylene ether, polyphenylene sulfide, polysulfone, polyether sulfone, polyarylate, aromatic polyamide, polyether ether ketone, thermoplastic polyimide, insoluble polyimide, polyamide imide, and fluororesin. A thermosetting resin and a thermoplastic resin may be used in combination.

[0071] <Printed wiring board> One of the present embodiments is a printed wiring board manufactured using the prepreg of the present embodiment, that is, a printed wiring board produced using the prepreg of the present embodiment. By manufacturing a printed wiring board using the prepreg of the present embodiment, it is possible to provide a high-quality printed wiring board with an accurate wiring circuit. EXAMPLES

[0072] The present invention will now be described in detail with reference to examples. In the examples and comparative examples, the physical properties were measured by the following methods.

[0073] (1) Physical properties of glass cloth The physical properties of the glass cloth, specifically, the thickness of the glass cloth, the mass of the glass cloth, the mass of the warp and weft, the diameter of the filaments constituting the warp and weft, the number of filaments, and the weaving density of the warp were measured in accordance with JIS R 3420. The warp width, weft width, and the gap width between adjacent wefts in the longitudinal direction (MD) were determined by observing a portion of 100 mm × 100 mm or more at any position on the glass cloth.

[0074] (2) Evaluation of waviness of prepreg The prepregs obtained in the examples and comparative examples were cut to a size of 340 mm × 510 mm to obtain test pieces. These test pieces were placed on a flat surface measuring table 1 as shown in Figure 2, and the height 3 of the waviness generated in the prepreg 2 was measured, and the maximum value was taken as the "amount of waviness."

[0075] (3) Pinhole The prepregs obtained in the examples and comparative examples were cut to a size of 500 mm x 500 mm to obtain test pieces. The test pieces were observed with a 20x magnifying glass to determine the number of pinholes.

[0076] (4) Evaluation of dimensional stability in the weft direction The prepregs obtained in the examples and comparative examples were cut to a size of 340 mm x 340 mm, and two sheets of the prepregs were laminated together. Then, copper foils having a thickness of 12 μm were placed on both surfaces of the prepregs, and the laminated sheets were then heated at 195° C. and 40 kgf / cm 2The test substrate was compression molded at 100°C to obtain a test substrate. The test substrate thus obtained was marked with 9 gauge marks, 3 in the vertical direction and 3 in the horizontal direction, at intervals of 125 mm. Then, the gauge marks between two adjacent gauge marks were measured at 6 points in each of the vertical and horizontal directions (measured value a). Next, the steel foil was removed by etching, and the gauge marks were heated at 170°C for 30 minutes, after which the gauge marks were measured again (measured value b). In the weft direction, the ratio of the difference between the measured values ​​a and b to the measured value a was calculated, and the dimensional change rate between each reference point in the weft direction was obtained (6 points in total). The above test was performed three times. The average value of the dimensional change rate between each reference point for the three times (6 points x 3 times = 18 dimensional change rate values) was calculated as the dimensional change rate in the weft direction. In addition, the standard deviation of all 18 dimensional change rate values ​​was calculated as the variation in the dimensional change rate in the weft direction.

[0077] <Example 1> The warp yarn has an average filament diameter of 4.0 μm, 50 filaments, 1.0Z twist, and a mass per unit length of 1.46 × 10 -6 kg / m of L glass yarn, as weft yarn, average filament diameter 4.5 μm, number of filaments 50, twist number 1.0Z, mass per unit length 1.83 × 10 -6 Using L-glass yarn of kg / m, glass cloth was woven using an air jet loom at a weaving density of 93.5 warp threads / 25 mm and 60 weft threads / 25 mm. The density of the L-glass (composition: SiO2: 51%, Al2O3: 13%, CaO: 8%, B2O3: 23%) constituting the glass cloth was 2.30 g / cm 3 The obtained grey fabric was heat-treated at 400°C for 24 hours to remove the size. Next, the glass cloth was immersed in a treatment solution containing a silane coupling agent, N-β-(N-vinylbenzylaminoethyl)-γ-aminopropyltrimethoxysilane; SZ6032 (manufactured by Dow Corning Toray Co., Ltd.), and after squeezing out the liquid, it was dried at 120°C for 1 minute and further opened by a high-pressure water spray to a mass of 10.1 g / m 2 Glass cloth A having a thickness of 12 μm was obtained. The yarn widths of the warp and weft of glass cloth A were 136 μm and 269 μm, respectively, the weft occupancy was 65%, and the weft gap was 148 μm. Glass cloth A was processed to a width of 650 mm for the coating test, and a prepreg coating test was performed using epoxy resin varnish. The epoxy resin varnish was prepared by mixing 80 parts by mass of low-brominated bisphenol A type epoxy resin, 20 parts by mass of cresol novolac type epoxy resin, 2 parts by mass of dicyandiamide, 0.2 parts by mass of 2-ethyl-4-methylimidazole, and 100 parts by mass of 2-methoxy-ethanol. The glass cloth was conveyed at a speed of 3 m / min, and the glass cloth A was immersed in the epoxy resin varnish. The excess varnish was scraped off through a slit whose gap was adjusted so that the resin content was 68% by mass, and then the glass cloth was dried under the conditions of a drying temperature of 170°C and a drying time of 1 minute and 30 seconds, and the epoxy resin was semi-cured (B-staged) to obtain prepreg A.

[0078] <Example 2> The glass cloth was woven and subsequently processed in the same manner as in Example 1, except that the weaving density of the weft yarn was 70 threads / 25 mm, and the mass was 10.7 g / m 2 Thus, a glass cloth B having a thickness of 13 μm was obtained. The warp and weft widths of the glass cloth B were 141 μm and 288 μm, respectively, the weft occupancy was 81%, and the weft gap was 69 μm. Prepreg B was obtained in the same manner as in Example 1, except that glass cloth B was used.

[0079] <Example 3> The glass cloth was woven and subsequently processed in the same manner as in Example 1, except that the weaving density of the weft yarn was 75 threads / 25 mm, and the mass was 11.1 g / m 2 Thus, a glass cloth C having a thickness of 14 μm was obtained. The warp and weft widths of the glass cloth C were 139 μm and 279 μm, respectively, the weft occupancy was 84%, and the weft gap was 54 μm. Prepreg C was obtained in the same manner as in Example 1, except that glass cloth C was used.

[0080] <Example 4> The glass cloth was woven and subsequently processed in the same manner as in Example 1, except that the weaving density of the weft yarn was 78 threads / 25 mm, and the mass was 11.3 g / m2 Thus, a glass cloth D having a thickness of 14 μm was obtained. The warp and weft widths of the glass cloth D were 138 μm and 277 μm, respectively, the weft occupancy rate was 86%, and the weft gap was 44 μm. Prepreg D was obtained in the same manner as in Example 1, except that glass cloth D was used.

[0081] <Example 5> The glass cloth was woven and subsequently processed in the same manner as in Example 1, except that the weaving density of the weft yarn was 81 threads / 25 mm, and the mass was 11.5 g / m 2 Thus, a glass cloth E having a thickness of 15 μm was obtained. The warp and weft widths of the glass cloth E were 136 μm and 272 μm, respectively, the weft occupancy was 88%, and the weft gap was 37 μm. A prepreg E was obtained in the same manner as in Example 1, except that the glass cloth E was used.

[0082] <Example 6> The glass cloth was woven and subsequently processed in the same manner as in Example 1, except that the weaving density of the weft yarn was 85 threads / 25 mm, and the mass was 11.8 g / m 2 Thus, a glass cloth F having a thickness of 16 μm was obtained. The warp and weft widths of the glass cloth F were 133 μm and 268 μm, respectively, the weft occupancy was 91%, and the weft gap was 26 μm. Prepreg F was obtained in the same manner as in Example 1, except that glass cloth F was used.

[0083] <Example 7> The average weft filament diameter is 4.0 μm, the number of filaments is 67, the number of twists is 1.0Z, and the mass per unit length is 1.95 × 10 -6 The same method as in Example 1 was used to weave a glass cloth and then process it, except that a L-glass yarn of 10.5 g / m2 was used and the weaving density of the weft yarn was 65 threads / 25 mm. 2 Thus, a glass cloth G having a thickness of 13 μm was obtained. The warp and weft widths of the glass cloth G were 153 μm and 288 μm, respectively, the weft occupancy was 75%, and the weft gap was 97 μm. Prepreg G was obtained in the same manner as in Example 1, except that glass cloth G was used.

[0084] <Example 8> A glass cloth was woven and subsequently processed in the same manner as in Example 7, except that the weaving density of the weft yarn was 72 threads / 25 mm, and the mass was 11.1 g / m 2 Thus, a glass cloth H having a thickness of 14 μm was obtained. The warp and weft widths of the glass cloth H were 150 μm and 282 μm, respectively, the weft occupancy was 81%, and the weft gap was 65 μm. Prepreg H was obtained in the same manner as in Example 1, except that glass cloth H was used.

[0085] <Example 9> A glass cloth was woven and subsequently processed in the same manner as in Example 7, except that the weaving density of the weft yarn was 75 threads / 25 mm, and the mass was 11.3 g / m 2 Glass cloth I having a thickness of 14 μm was obtained. The warp and weft widths of glass cloth I were 147 μm and 278 μm, respectively, the weft occupancy was 83%, and the weft gap was 55 μm. Prepreg I was obtained in the same manner as in Example 1, except that Glass Cloth I was used.

[0086] <Example 10> The warp yarn has an average filament diameter of 4.0 μm, 50 filaments, 1.0Z twist, and a mass per unit length of 1.41 × 10 -6 kg / m of low dielectric glass yarn, as weft yarn, average filament diameter 4.5μm, number of filaments 50, twist number 1.0Z, mass per unit length 1.78×10 -6 Using low dielectric glass yarn of 1.0 kg / m, glass cloth was woven using an air jet loom at a weaving density of 93.5 warp threads / 25 mm and 75 weft threads / 25 mm. The density of the low dielectric glass (composition: SiO2: 51%, Al2O3: 17%, CaO: 3%, B2O3: 24%) that constitutes the glass cloth is 2.23 g / cm 3 It was. Then, the same treatment as in Example 1 was carried out to obtain a mass of 10.8 g / m 2 Thus, a glass cloth J having a thickness of 13 μm was obtained. The warp and weft widths of the glass cloth J were 142 μm and 283 μm, respectively, the weft occupancy was 85%, and the weft gap was 50 μm. A prepreg J was obtained in the same manner as in Example 1, except that the glass cloth J was used.

[0087] <Comparative Example 1> The weft has an average filament diameter of 4.0 μm, 50 filaments, 1.0Z twist, and a mass per unit length of 1.46 × 10 -6 The same method as in Example 1 was used to weave a glass cloth and then process it, except that the L glass yarn of 1.0 kg / m2 was used and the weaving density of the weft yarn was 93.5 threads / 25 mm. The glass cloth had a mass of 11.1 g / m2. 2 Thus, a glass cloth K having a thickness of 14 μm was obtained. The warp and weft widths of the glass cloth K were 134 μm and 223 μm, respectively, the weft occupancy was 83%, and the weft gap was 44 μm. Prepreg K was obtained in the same manner as in Example 1, except that glass cloth K was used.

[0088] <Comparative Example 2> The weft and warp have an average filament diameter of 4.0 μm, 40 filaments, 1.0Z twist, and a mass per unit length of 1.17 × 10 -6 The same method as in Example 1 was used to weave a glass cloth and then process it, except that L glass yarn of 9.0 kg / m was used and the weaving density of the warp and weft yarns was 95 threads / 25 mm. 2 Thus, a glass cloth L having a thickness of 11 μm was obtained. The warp and weft widths of the glass cloth L were 156 μm and 177 μm, respectively, the weft occupancy was 67%, and the weft gap was 86 μm. A prepreg L was obtained in the same manner as in Example 1, except that the glass cloth L was used.

[0089] <Comparative Example 3> The warp yarn has an average filament diameter of 4.0 μm, 40 filaments, 1.0Z twist, and a mass per unit length of 1.17 × 10 -6 kg / mL glass thread, average filament diameter of weft thread 4.0 μm, number of filaments 50, twist number 1.0Z, mass per unit length 1.46 × 10 -6 The glass cloth was woven and subsequently processed in the same manner as in Example 1, except that L glass yarn of 1.0 kg / m was used, the warp yarn density was 95 threads / 25 mm, and the weft yarn density was 95 threads / m. The glass cloth was woven and processed in the same manner as in Example 1, and the mass was 8.2 g / m. 2 Thus, a glass cloth M having a thickness of 13 μm was obtained. The warp and weft widths of the glass cloth M were 157 μm and 213 μm, respectively, the weft occupancy rate was 81%, and the weft gap was 50 μm. A prepreg M was obtained in the same manner as in Example 1, except that a glass cloth M was used.

[0090] <Comparative Example 4> A glass cloth was woven and subsequently processed in the same manner as in Comparative Example 3, except that the weaving density of the weft yarn was 76 threads / 25 mm, and the mass was 6.3 g / m 2 Thus, a glass cloth N having a thickness of 12 μm was obtained. The warp and weft widths of the glass cloth N were 162 μm and 232 μm, respectively, the weft occupancy was 71%, and the weft gap was 97 μm. Prepreg N was obtained in the same manner as in Example 1, except that glass cloth N was used.

[0091] <Comparative Example 5> Glass cloth was woven in the same manner as in Comparative Example 1. The obtained greige fabric was subjected to a fiber-opening process using a high-pressure water spray under a tension of 4.9 N / m (processing pressure: 196 N / cm 2 ) method was applied. It was then heated at 400°C for 24 hours to remove the glue. Next, the glass cloth was immersed in a treatment solution using a silane coupling agent, N-β-(N-vinylbenzylaminoethyl)-γ-aminopropyltrimethoxysilane; SZ6032 (Toray, Dow Corning), squeezed out, and dried at 120°C for 1 minute to obtain a mass of 12.5 g / m2. 2Thus, a glass cloth O having a thickness of 14 μm was obtained. The chemical and physical treatment of the glass cloth was performed in accordance with the method of Example 2 of Patent Document 4: Japanese Patent No. 3897789. The yarn widths of the warp and weft of the glass cloth O were 150 μm and 166 μm, respectively, the weft occupancy rate was 62%, and the weft gap was 101 μm. A prepreg O was obtained in the same manner as in Example 1, except that a glass cloth O was used.

[0092] <Comparative Example 6> Both warp and weft yarns have an average filament diameter of 4.0 μm, 100 filaments, 1.0Z twist, and 2.93×10 mass per unit length. -6 The glass cloth was woven and subsequently processed in the same manner as in Example 1, except that L glass yarn of 100 kg / m was used and the weaving density of both the warp and weft yarns was 100 threads / 25 mm. The glass cloth was woven and processed in the same manner as in Example 1, and the mass was 19.5 g / m. 2 Thus, a glass cloth P having a thickness of 20 μm was obtained. A prepreg P ​​was obtained in the same manner as in Example 1, except that a glass cloth P was used.

[0093] <Comparative Example 7> The warp yarn has an average filament diameter of 4.0 μm, 100 filaments, 1.0Z twist, and a mass per unit length of 2.93 × 10 -6 kg / m of L glass yarn, average filament diameter 4.5 μm in weft, 100 filaments, twist number 1.0Z, mass per unit length 3.65 × 10 -6 The glass cloth was woven and subsequently processed in the same manner as in Example 1, except that L glass yarn of 17.7 kg / m was used, the warp density was 75 threads / 25 mm, and the weft density was 60 threads / 25 mm. The glass cloth was woven and processed in the same manner as in Example 1, and the mass was 17.7 g / m. 2 Thus, a glass cloth Q having a thickness of 19 μm was obtained. A prepreg Q was obtained in the same manner as in Example 1, except that a glass cloth Q was used.

[0094] <Comparative Example 8> The weft has an average filament diameter of 5.0 μm, 50 filaments, 1.0Z twist, and a mass per unit length of 2.44 × 10-6 The same method as in Example 1 was used to weave a glass cloth and then process it, except that the L glass yarn of 1.2 kg / m2 was used and the weaving density of the weft yarn was 57 threads / 25 mm. The glass cloth had a mass of 11.2 g / m2. 2 Thus, a glass cloth R having a thickness of 15 μm was obtained. The warp and weft widths of the glass cloth R were 162 μm and 273 μm, respectively, the weft occupancy was 62%, and the weft gap was 166 μm. A prepreg R was obtained in the same manner as in Example 1, except that a glass cloth R was used.

[0095] <Comparative Example 9> The warp yarn has an average filament diameter of 4.0 μm, 50 filaments, 1.0Z twist, and a mass per unit length of 1.40 × 10 -6 kg / m of low dielectric glass yarn, as weft yarn, average filament diameter 4.5μm, number of filaments 50, twist number 1.0Z, mass per unit length 1.76×10 -6 Using low dielectric glass yarn of 1.0 kg / m, glass cloth was woven using an air jet loom at a weaving density of 93.5 warp threads / 25 mm and 75 weft threads / 25 mm. The density of the low dielectric glass (composition: SiO2: 51%, Al2O3: 12%, CaO: 4%, B2O3: 29%) that constitutes the glass cloth is 2.19 g / cm 3 It was. Then, the same treatment as in Example 1 was carried out to obtain a mass of 10.7 g / m 2 Thus, a glass cloth S having a thickness of 13 μm was obtained. The warp and weft widths of the glass cloth S were 142 μm and 284 μm, respectively, the weft occupancy was 85%, and the weft gap was 50 μm. A prepreg S was obtained in the same manner as in Example 1, except that the glass cloth S was used.

[0096] [Performance test] Various evaluations were carried out on the prepregs A to S obtained in Examples 1 to 10 and Comparative Examples 1 to 9. The results are shown in Tables 1 and 2.

[0097] [Table 1]

[0098] [Table 2]

[0099] As can be seen from the results in Table 1, all of the prepregs A to J obtained in Examples 1 to 10 had little waviness, and the amount of dimensional change in the weft direction and the variation therein were small. Prepregs K, L, and P of Comparative Examples 1, 2, and 6 are prepregs obtained from low dielectric glass cloth adjusted to have the same volume occupied by the warp and weft threads and the same weaving density as the IPC-registered 1017, 1010, and 1027 style E-glass cloth that is available on the market. The prepregs of the Examples had less waviness and were superior in terms of the amount of dimensional change in the weft direction and its variation compared to the prepregs of Comparative Examples 1, 2, and 6.

[0100] Prepreg M of Comparative Example 3 is a prepreg obtained from a low dielectric glass cloth adjusted so that the volume occupied by the warp and weft and the weaving density are equivalent to those of the E-glass cloths of Example 1 of Patent Document 1 and Example 1 of Patent Document 2. Compared with glass cloth L (IPC registered 1010) of Comparative Example 2, which has the same warp configuration, prepreg M of Comparative Example 3 showed a reduced amount of dimensional change in the weft, but the variation was large.

[0101] Comparative Example 5 corresponds to a glass cloth that has been opened under low tension conditions to make the weft and warp widths equal, i.e., a weft / warp ratio in the range of 0.8 to 1.2, as disclosed in Patent Document 4, and is a prepreg obtained from said glass cloth. Patent Document 4 describes the glass cloth as having excellent dimensional stability, but Prepreg O had significant waviness and large variation in dimensional change.

[0102] Prepreg Q of Comparative Example 7 is a prepreg obtained from a low dielectric glass cloth adjusted so that the volume occupied by the warp and weft yarns and the weaving density are equivalent to those of Example 3 of Patent Document 3. The thickness of the glass cloth Q was 19 μm, and it was not a thin glass cloth either. In addition, the thickness of the resin layer on both sides of the glass cloth of Prepreg Q was not uniform, and some waviness occurred. The variation in dimensional change was also large compared to Examples 1 to 9.

[0103] Prepreg R of Comparative Example 8 is a prepreg obtained from a low dielectric glass cloth in which the average mass per unit length of the weft yarn is significantly greater than that of the warp yarn. Prepreg R had relatively small waviness and dimensional change in the weft yarn, but the variation in dimensional change was large.

[0104] Prepreg S of Comparative Example 9 is a prepreg obtained from a low dielectric glass cloth produced using low dielectric glass cloth yarn containing a large amount of B2O3 to improve the dielectric properties of the glass cloth and using yarns similar to those used in Example 3. Prepreg S was significantly wavier than Example 3, and had significantly poorer variation in dimensional change. [Industrial Applicability]

[0105] The glass cloth and prepreg of the present invention have industrial applicability as substrates for printed wiring boards used in the electronic and electrical fields. [Explanation of symbols]

[0106] 1: Measuring table 2: Prepreg 3: Height of the waves

Claims

1. The glass yarns are made of a plurality of glass filaments and are used as warp and weft yarns. The thickness is 8 μm or more and 16 μm or less. The density of the glass is 2.1 g / cm 3 2.5g / cm or more 3 A prepreg having a glass cloth and a matrix resin, The following 1) to 3); 1) The resin content is 50% or more and 83% or less by mass; 2) The ratio of the thickness of the first resin layer located on one side of the glass cloth to the thickness of the second resin layer located on the other side of the glass cloth is 0.7 or more and 1.3 or less; 3) The amount of waviness is less than 3 mm; Fulfilling The glass cloth is A glass cloth having a thickness of 8 μm to 16 μm, the glass cloth being configured as warp and weft yarns each made of a plurality of glass filaments, The average mass per unit length of the warp yarn is 1.40×10 −6 kg / m or more and less than 1.60×10 −6 kg / m; The average mass per unit length of the weft yarn is 1.60×10 −6 kg / m or more and 3.00×10 −6 kg / m or less, a ratio of the average mass per unit length of the weft to the average mass per unit length of the warp (weft / warp ratio) is greater than 1.20 and less than or equal to 1.50; The density of the glass is 2.1 g / cm 3 or more and 2.5 g / cm 3 or less. Prepreg.

2. A prepreg comprising: a glass cloth, the warp and weft being made of glass yarns consisting of a plurality of glass filaments, the thickness of which is 8 μm or more and 16 μm or less, and the density of the glass being 2.1 g / cm 3 or more and 2.5 g / cm 3 or less; and a matrix resin, The following 1) to 3); 1) The resin content is 50% or more and 83% or less by mass; 2) The ratio of the thickness of the first resin layer located on one side of the glass cloth to the thickness of the second resin layer located on the other side of the glass cloth is 0.7 or more and 1.3 or less; 3) The amount of waviness is less than 3 mm; Fulfilling The gap width between adjacent weft yarns in the longitudinal direction (MD direction) is 40 μm or more and 80 μm or less. Prepreg.

3. The glass cloth, A glass cloth having a thickness of 8 μm to 16 μm, the glass cloth being configured as warp and weft yarns each made of a plurality of glass filaments, The average mass per unit length of the warp yarn is 1.40×10 −6 kg / m or more and less than 1.60×10 −6 kg / m; The average mass per unit length of the weft yarn is 1.60×10 −6 kg / m or more and 3.00×10 −6 kg / m or less, a ratio of the average mass per unit length of the weft to the average mass per unit length of the warp (weft / warp ratio) is greater than 1.20 and less than or equal to 1.50; The density of the glass is 2.1 g / cm 3 or more and 2.5 g / cm 3 or less. The prepreg according to claim 2.

4. The average filament count of the warp yarns and the weft yarns is substantially the same; and The average filament diameter of the warp yarn is 3.7 μm or more and 4.3 μm or less, The average filament diameter of the weft is 4.2 μm or more and 5.3 μm or less, The ratio of the average filament diameter of the weft to the average filament diameter of the warp (weft / warp ratio) is 1.07 or more and 1.40 or less. The prepreg according to any one of claims 1 to 3.

5. The average filament diameters of the warp and weft yarns are substantially the same, and The average number of filaments in the warp yarn is 45 or more and 70 or less, The average number of filaments of the weft yarn is 55 or more and 80 or less, The ratio of the average number of filaments of the weft to the average number of filaments of the warp (weft / warp ratio) is greater than 1.25 and less than or equal to 1.50; The prepreg according to any one of claims 1 to 3.

6. A prepreg comprising: a glass cloth, the warp and weft being made of glass yarns consisting of a plurality of glass filaments, the thickness of which is 8 μm or more and 16 μm or less, and the density of the glass being 2.1 g / cm 3 or more and 2.5 g / cm 3 or less; and a matrix resin, The following 1) to 3); 1) The resin content is 50% or more and 83% or less by mass; 2) The ratio of the thickness of the first resin layer located on one side of the glass cloth to the thickness of the second resin layer located on the other side of the glass cloth is 0.7 or more and 1.3 or less; 3) The amount of waviness is less than 3 mm; Fulfilling The average filament diameters of the warp and weft yarns are substantially the same, and The average number of filaments in the warp yarn is 45 or more and 70 or less, The average number of filaments of the weft yarn is 55 or more and 80 or less, The ratio of the average number of filaments of the weft to the average number of filaments of the warp (weft / warp ratio) is greater than 1.25 and less than or equal to 1.50; Prepreg.

7. A coefficient (Y: weft occupancy rate) indicating a ratio of a portion where the weft is present in the longitudinal direction (MD direction) of the weft, calculated by the formula (1), is 76% or more and 90% or less. The prepreg according to any one of claims 1 to 6. Y=F / (25000 / G)×100...(1) (In formula (1), F is the weft width (μm), and G is the weaving density of the weft (pieces / 25 mm).)

8. having a dielectric constant of 5.0 or less at a frequency of 10 GHz; The prepreg according to any one of claims 1 to 7.

9. A printed wiring board comprising the prepreg according to any one of claims 1 to 8.

Citation Information

Patent Citations

  • JP1975027335A

  • Television receiver

    JP1983031665A

  • Precursor pitch fiber for carbon fiber

    JP1984036726A

  • Glass fiber woven fabric for printed circuit board

    JP1998245743A

  • Low dielectric constant glass fiber

    JP1999292567A