Carbon-coated composite materials, their manufacture and use

A two-step vapor phase deposition process in a rotary kiln with controlled gases and speeds achieves a dense and uniform carbon coating on composite materials, addressing uniformity and conductivity issues, improving battery electrode performance.

JP7562838B2Active Publication Date: 2024-10-07BEIJING IAMETAL NEW ENERGY TECH CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2023511621
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2022-02-21
Filing Date
2022-06-30
Publication Date
2024-10-07
Estimated Expiration
2042-06-30

AI Technical Summary

Technical Problem

Existing carbon coating methods face challenges in achieving uniform and dense carbon layers, leading to issues such as particle agglomeration, incomplete coating, and low conductivity, which affect the performance of carbon-coated composite materials, particularly in silicon negative electrode materials for batteries.

Method used

A method involving two vapor phase depositions in a rotary kiln with controlled carbon-containing process gases and rotation speeds to achieve a carbon-coated composite material with a density of 1.0-2.0 g/cm³, ensuring complete and uniform carbon coverage, reducing core element elution to 100 ppm or less, and enhancing electrical conductivity and stability.

Benefits of technology

The method results in a carbon-coated composite material with improved conductivity, stability, and reduced volume changes, enhancing the performance of battery electrodes by forming a stable electric double layer and buffering volume expansion.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007562838000008
    Figure 0007562838000008
  • Figure 0007562838000009
    Figure 0007562838000009
  • Figure 0007562838000010
    Figure 0007562838000010
Patent Text Reader

Abstract

The present invention relates to a carbon-coated composite material, which comprises a core and a carbon coating layer coated on the outside of the core, and the density of the carbon coating layer is 1.0 g cm -3 ≦ρ 2 ≦2.0g cm -3 The carbon-coated composite material has a core characteristic element elution amount of 100 ppm or less, the carbon-coated target material has a D50 of 1 to 40 μm, a particle size distribution range of 0.5≦(D90-D10) / D50≦2, and a specific surface area of ​​1 to 5 m 2 ·g -1 The ratio of the specific surface area to the volume of the accumulated pores is 0.5 to 2 cm -1 and the increase in D50 of the composite material after coating is 3 μm or less. In the carbon-coated composite material according to the present invention, a carbon coating layer is coated on the outside of a core material, and the shell of the carbon-coated composite material can buffer the volume change of the core, and the complete and uniform carbon layer can effectively disperse the surface charge to form a more stable electric double layer, and form a more uniform and stable interface during lithium absorption, which is advantageous for improving the battery characteristics, especially the cycle stability.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to the field of carbon composite material manufacturing, and in particular to a composite material having a dense and uniform carbon coating, its manufacturing method and use. [Background technology]

[0002] Carbon coating is one of the common material modification methods. On the one hand, carbon coating can improve the electrical conductivity of materials, and on the other hand, it can provide a stable chemical and electrical reaction interface.

[0003] At present, carbon coating is generally carried out by solid-phase, liquid-phase and gas-phase processes. In the prior art, carbon coating can be carried out by a solid-phase process, that is, a solid carbon source is dispersed in the material to be coated by solid-solid mixing, and then the solid carbon source is softened by heating to a certain temperature to coat the surface of the particles of the material to be coated, and the temperature is further increased to dehydrogenate the carbon. However, the carbon coating process by the solid-phase method is difficult to achieve uniformity of the coating, and the problem of particle aggregation cannot be avoided. The liquid-phase method and the gas-phase method can well avoid the problem of particle aggregation. In the liquid-phase method, the solute is usually dispersed in a liquid phase with a solvent such as water or ethanol, and then carbonized at a high temperature to obtain a carbon-coated material. However, in the carbon coating by the liquid-phase method, the solvent needs to be recovered, and the process is complicated, making it difficult to be widely applied. The gas-phase method is specifically to coat the surface of the material to be coated with a carbon-containing gas by a gas-phase deposition method. The equipment and technology of gas-phase coating have been developed and it has been successfully applied to new energy-related materials, and it has a good effect on materials with large volume deformation, and can increase the conductivity, improve the interface, and reduce the volume expansion during the lithium absorption process. In addition, gas-phase coating has the characteristics of less pollution and the ability to control the coating amount. However, in the case of coating by gas-phase coating, the integrity of the coating layer is unstable, and it is often the case that the coating cannot be completely carried out, and it is difficult to achieve the effect of the coating layer having the appropriate density, and it is easy to cause leakage and elution of the inner coating material, which has a negative impact on the properties of the carbon-coated composite material. In the gas-phase coating process, the selection of the carbon source process gas and the screening of the key parameters of the raw material are important indicators, and the number of surface defects of the raw material, the optimization of the particle size, and the different powder deposition pore structure will result in different numbers of active sites, and such active sites, when combined with the process gas, will result in complex competitive reactions of diffusion and growth nucleation during the chemical vapor deposition process. Therefore, a uniform and dense carbon layer is still a challenge in the gas-phase coating process. The uniform and dense carbon layer can obviously improve the cycle and storage properties of the product, and can inhibit side reactions, especially under high temperature conditions.

[0004] In silicon anode materials, volume expansion is the most important issue. In the prior art, the volume expansion can be reduced to a certain extent by using silicon oxide technology, but the electrical conductivity is low and the initial coulombic efficiency is not high. Carbon coating can effectively solve the problem of low electrical conductivity, but in order to effectively improve the electrical conductivity of carbon-coated silicon anode materials, it is necessary to ensure the denseness and integrity of the coating layer of the carbon coating.

[0005] Therefore, there is an urgent need to develop carbon-coated composite materials with higher density and higher coating integrity so that the material to be coated can be more completely coated with a carbon layer and the properties of the carbon-coated composite materials can be maximized. Summary of the Invention

[0006] In response to the shortcomings of the prior art, a first object of the present application is to provide a carbon coating layer having a density of 1.0 to 2.0 g cm -3 The material to be carbon-coated has a D50 of 1 to 40 μm, preferably 3 to 10 μm, more preferably 4 to 7 μm, a particle size distribution range of 0.5≦(D90−D10) / D50≦2, preferably 1≦(D90−D10) / D50≦1.5, and a specific surface area of ​​1 to 5 m 2 ·g -1 , preferably 1 to 2 m 2 ·g -1 The ratio of the specific surface area to the volume of the deposited pores is 0.50 to 2.00 cm -1 , preferably 0.70 to 1.50 cm -1 and to provide a carbon-coated composite material in which the increase in D50 of the composite material after coating is 3 μm or less, preferably 1 μm or less.

[0007] The density of the carbon coating layer can be calculated by the following formula: ρ2=m2ρ1ρ3 / (m1ρ3-m3ρ1) (ρ2 is the density of the carbon coating layer, the mass of the carbon-coated composite material is m1, the density is ρ1, the mass of the carbon coating layer is m2, and the mass of the core is m3, the density is ρ3.) The carbon-coated composite material is placed in an excess amount of a solution capable of dissolving the core characteristic element, and the elution of the core characteristic element is measured. As a result, the elution amount of the core characteristic element is 100 ppm or less.

[0008] Preferably, in the carbon-coated composite material, the density of the carbon coating layer is 1.2 g cm -3 ≦ρ2≦1.5g cm -3 It is.

[0009] The carbon-coated composite material according to the present application has a dense carbon coating layer with a core element elution amount of 100 ppm or less, in other words, the carbon-coated composite material according to the present application has a complete and suitable dense carbon coating layer. A completely coated carbon-coated composite material can effectively avoid coating defects and represent the uniformity of the carbon coating layer on the outer layer of the core. On the other hand, the uniform coating of the carbon layer is very important for the stability of the properties of the carbon-coated material, which can buffer the volume change (e.g., volume expansion) of the core material on the one hand, and the complete and uniform carbon layer can effectively disperse the surface charge to form a more stable electric double layer and form a more uniform and stable interface during lithium absorption. The suitable carbon coating layer density can represent the compactness of the carbon coating layer, which is 1.0 g cm -3 ≦ρ2≦2.0g cm -3 (1.1 g cm -3 , 1.2g cm -3 , 1.3 g cm -3 , 1.4g cm -3 , 1.5g cm -3 , 1.6g cm -3 , 1.7g cm -3 , 1.8g cm -3 , 1.9g cm -3 ) the carbon coating layer has an appropriate density and can form a more stable electric double layer.

[0010] The present application is not particularly limited with respect to the core material of the carbon-coated composite material, and preferably, the core material comprises any one or a combination of at least two of inorganic particles, such as graphite particles, metal tin particles, tin oxide particles, silicon particles, silicon oxide particles, silicon nitride particles, element-doped silicon oxygen composite particles, metal germanium particles, and germanium oxide particles.

[0011] The carbon-coated composite material obtained by the present invention is placed in an excess amount of a solution capable of dissolving the core characteristic element, and the elution of the core characteristic element is measured, and the elution amount of the core characteristic element is 100 ppm or less. The core characteristic element is an element type for which ICP quantitative data can be obtained for the core material by a method such as a chemical reaction, and when the core itself cannot be dissolved, other soluble elements must be used as a reference. When the core is a graphite particle, the elution solution is aqua regia, and the core characteristic element is a trace element that is an impurity, such as iron element. When the core is a metal tin particle or a tin oxide particle, the elution solution is aqua regia, and the core characteristic element is tin element; when the core is a metal germanium particle or a germanium oxide particle, the elution solution is aqua regia, and the core characteristic element is germanium element; when the core is a silicon particle, a silicon oxide particle, a silicon nitride particle, or an element-doped silicon-oxygen composite particle, the core characteristic element is silicon, the elution solution is a sodium hydroxide or hydrofluoric acid solution, and the elution time is 24 hours or more.

[0012] When measuring the amount of dissolution of the core characteristic element, an excessive amount of solution means that the amount of solution added is greater than the amount of solution that can completely dissolve the core characteristic element. The smaller the amount of dissolution of the core characteristic element, the denser and more uniform the carbon coating is, covering the entire core material, and having no defects or weak parts. The complete coating structure is advantageous for reducing side reactions at the interface, and greatly contributes to improving the high temperature characteristics, low temperature characteristics, storage characteristics, and cycle characteristics of the battery.

[0013] For a carbon-coated composite material with mass m1 and density ρ1, if the carbon content of the carbon-coated composite material is A (for composite materials that do not contain carbon in the core, the carbon coating content can be measured using a carbon / sulfur analyzer, and for composite materials that contain carbon in the core, the carbon content can be determined by the TG-DSC method), the mass of the carbon coating layer is m2 = m1 × A.

[0014] The density ρ1 of the carbon-coated composite material and the density ρ3 of the core of the present application are both true densities of the corresponding materials, but the density ρ2 of the carbon coating layer defined in the present application should also be understood as the true density of the carbon coating layer. True density is the actual mass of a solid material per unit volume of a material in an absolutely dense state, that is, the density excluding internal pores or interparticle voids. True density is different from apparent density and tap density, where apparent density is the ratio of the mass of a material to the apparent volume, and apparent volume is the actual volume multiplied by the volume of closed pores, and does not take into account factors such as voids inside the material, and tap density is the mass per unit volume measured immediately after dust or powder is filled into a specific container, and similarly does not take into account pores or voids formed by the accumulation of materials. The density ρ1 of the carbon-coated composite material of the present invention and the density ρ3 of the core of the present invention can both be measured by a true density tester. The average particle size, particle size distribution, specific surface area, and sedimentary pore volume can all be measured by conventional techniques, an example of a test method is a specific surface area tester.

[0015] The second object of the present invention is to The average diameter of the core material is 1 to 40 μm, the particle size distribution range is 0.5≦(D90-D10) / D50≦2, and the specific surface area is 1 to 5 m 2 ·g -1 , the ratio of specific surface area to accumulated pore volume is 0.5 to 2.0 cm -1 (1) treating a core material to be coated so that (2) loading the treated raw material to be coated into a rotary kiln, and introducing a carbon-containing process gas under a protective atmosphere to perform a first carbon element vapor deposition to obtain a first intermediate product; (3) sieving the intermediate product to remove larger sized materials and crushing and deagglomerating the remaining materials to obtain a second intermediate product; and (4) a step of re-feeding the second intermediate product into a rotary kiln and conducting a second vapor-phase deposition of carbon element under a protective atmosphere by introducing a carbon-containing process gas to obtain a carbon-coated composite material having the raw material particle to be coated as a core and an outer layer coated with carbon.

[0016] The material is rotated in a rotary kiln and vapor deposition is performed twice on the surface of the dynamic raw material to form a complete carbon coating layer with less than 100 ppm of elution of core characteristic elements. In the manufacturing method according to the present application, the raw material has an appropriate void and an appropriate particle surface roughness according to the size range, particle size range, specific surface area and deposition pore volume of the raw material, so that the carbon layer is more easily deposited on the particle surface and pore wall in the chemical vapor deposition, and the particles are appropriately deagglomerated after one chemical vapor deposition to a specific size (the average diameter of the second intermediate product is 1 to 1.1 times the average diameter of the raw material to be coated), thus exposing defects in the coating layer caused by agglomeration in the first chemical vapor deposition, and the defects in the coating layer are repaired by the second chemical vapor deposition.

[0017] The treatment process in step (1) is well known in the art, for example, airflow pulverization, ball milling, high-speed pulverization, and 4-step classification. Note that the raw material to be coated has an average diameter of 1 to 40 μm, a particle size distribution range of 0.5≦(D90-D10) / D50≦2, and a specific surface area of ​​1 to 5 m. 2 ·g -1 , the ratio of specific surface area to accumulated pore volume is 0.5 to 2.0 cm -1 If the material does not meet the requirement that the material be coated, then the material can be treated by one of ordinary skill in the art, such as by crushing, classifying, or other conventional techniques, until the material meets the requirements of the material to be coated herein, and then coated with carbon.

[0018] Preferably, the material to be coated includes any one of graphite powder, metallic tin, tin oxide, silicon, silicon oxide, silicon nitride, element-doped silicon oxygen composite, metallic germanium particles, and germanium oxide particles.

[0019] Examples of the silicon oxide include silicon oxide, silicon monoxide, or any silicon oxide with a silicon-oxygen ratio of 1:1 to 1:2, and examples of the element-doped silicon-oxygen composite may be lithium-doped silicon monoxide, magnesium-doped silicon monoxide, etc.

[0020] The carbon-coated composite material of the present invention can be used as an anode material for lithium-ion batteries, and can improve the electrical conductivity of the composite material, mitigate volume change, and stabilize the interface. When the material to be coated is graphite, the composite material exhibits small volume expansion after absorbing lithium, improves rate characteristics, and stabilizes the interface. When the material to be coated is silicon monoxide, the composite material can improve the electrical conductivity of the material and the stability of the SEI film. In particular, the dense carbon layer has a good buffering effect against volume change. The protection provided by this continuous and dense carbon layer improves high-temperature characteristics and cycle characteristics.

[0021] In step (2), the carbon-containing process gas includes C1-4 alkanes (eg, methane, ethane, propane), C2-4 olefins (eg, ethylene, propylene, 1-butene, 1,3-butadiene), and C2-4 alkynes (eg, acetylene, propyne).

[0022] Preferably, in the first carbon element vapor deposition, the carbon-containing process gas is a mixture of propylene and methane in a volume ratio of 1-2:1-2, and the introduction flow rate of the process gas satisfies the condition h=V / s, where V is the total volume of the rotary kiln chamber (unit L), s is the introduction rate of the process gas (unit L / min), and the flow rate of the process gas satisfies h=20-60 min. As an example, when the total volume of the furnace body is 100 L, the flow rate is 1.667-5.000 L / min, and when the total volume of the furnace body is 1200 L, the flow rate is 20-60 L / min.

[0023] More preferably, in the first carbon element vapor deposition, the carbon-containing process gas is a mixture of methane and propylene, and propylene is introduced from a position from the throat of the rotary kiln to 1 / 5 of the total length of the furnace body (i.e., a position close to the throat), and methane is introduced from a position from 1 / 3 to 2 / 3 of the total length of the furnace body of the rotary kiln (i.e., the central position of the rotary kiln). How to introduce the carbon-containing process gas from various positions of the rotary kiln is known to those skilled in the art, for example, gas introduction pipes of various lengths can be used, or gas introduction pipes can be provided at various positions of the rotary kiln. The present inventors have found that introducing propylene as the carbon-containing process gas from a position close to the throat and methane as the carbon-containing process gas from the central position of the rotary kiln is more advantageous for the denseness and uniformity of the carbon coating layer. Carbon formation in chemical vapor deposition is closely related to the carbon / hydrogen ratio of the carbon source gas. When the carbon / hydrogen ratio is large, layered deposition is likely to occur, while when the carbon / hydrogen ratio is small, an isotropic carbon structure is likely to be deposited. In addition, the content of polycyclic aromatic hydrocarbons, which are by-products of the deposition of the carbon source gas, also changes with the adjustment of the carbon / hydrogen ratio, and the higher the by-product content, the more likely carbon blocks are formed and particles are aggregated. For this reason, the ratio and concentration of the carbon source gas are very important in this process. In the present invention, the second carbon coating can repair defective or weak areas that are not coated or are insufficiently coated, but the flow rate of the process gas in the second coating must be lower than that in the first coating. The gas of the protective atmosphere is nitrogen gas or argon gas, and the protective atmosphere may be introduced into the rotary kiln alone or may be premixed with a carbon-containing gas before being introduced. The volume ratio of the protective gas to the carbon-containing gas is 1-3:1-3.

[0024] Preferably, in step (2), the rotation speed of the rotary kiln is 0.1 to 2 rpm (e.g., 0.2 rpm, 0.5 rpm, 0.8 rpm, 1.2 rpm, 1.5 rpm, 1.8 rpm, etc.). When the rotation speed of the rotary kiln is within the range of 0.1 to 2 rpm, both the completeness and denseness of the carbon coating layer are excellent.

[0025] The first carbon element vapor phase deposition is performed at a temperature of 600 to 1200° C. for 0.5 to 10 hours, or the first carbon element vapor phase deposition is plasma vapor phase deposition at 100 to 500° C. for 0.5 to 10 hours.

[0026] Preferably, the introduction flow rate of the carbon-containing process gas in the second carbon element vapor phase deposition is 1 / 4 to 4 / 5, preferably 1 / 2 to 4 / 5, of the flow rate of the carbon-containing process gas in the first carbon element vapor phase deposition.

[0027] The second carbon element vapor deposition is intended to repair defects in the carbon coating layer produced by the first carbon element vapor deposition and completely coat the carbon layer. After the first carbon element vapor deposition is performed on the core particles, the cut surface of the carbon coating layer is deagglomerated, and the cut surface of the cut layer is uneven. In the second carbon element vapor deposition, the introduction flow rate of the carbon-containing process gas is reduced to 1 / 4 to 4 / 5 of the introduction flow rate of the carbon-containing process gas in the first carbon element vapor deposition, so that a carbon layer can be further generated and coated well on the cut surface of the carbon coating layer produced by the first carbon element vapor deposition.

[0028] Preferably, in step (3), the large particle size material is a material having a particle size of more than 50 μm, and the crushing and deagglomeration is carried out by a method such as mechanical crushing or airflow crushing, whereby agglomerated particles are collided and dispersed.

[0029] Preferably, in step (4), the rotation speed of the rotary kiln is 0.1 to 2 rpm (e.g., 0.2 rpm, 0.5 rpm, 0.8 rpm, 1.2 rpm, 1.5 rpm, 1.8 rpm, etc.). Note that in steps (2) and (4), the rotation speed of the rotary kiln is independently selected from the range of 0.1 to 2 rpm, and preferably, in step (2), the rotation speed of the rotary kiln is 2 to 3 times the rotation speed of the rotary kiln in step (4).

[0030] Preferably, the second carbon element vapor deposition is performed at a temperature of 600-1200°C for 0.5-10h, or the second carbon element vapor deposition is plasma vapor deposition at 100-500°C for 0.5-10h. As a preferred technical solution, in the method for producing a carbon-coated composite material of the present invention, the process gases of the first carbon element vapor deposition and the second carbon element vapor deposition are each independently selected from propylene and methane.

[0031] A third object of the present invention is to provide a use of the carbon coated composite material as an electrode material for any of lithium batteries, sodium batteries, potassium batteries, etc. Compared with the prior art, the present application has the following beneficial effects:

[0032] (1) This application provides a carbon coating with an appropriate density (the density of the carbon coating layer is 1.0 g cm -3 The present invention provides a carbon-coated composite material with high integrity (the amount of elution of core characteristic elements is 100 ppm or less), in which a carbon coating layer is coated on the outside of the core material, and this carbon material shell can buffer the volume change of the core material. In addition, the complete and uniform carbon layer can effectively disperse the surface charge to form a more stable electric double layer, and form a more uniform and stable interface during lithium absorption.

[0033] (2) In the preferred technical solution, the core material of the carbon-coated composite material is silicon monoxide, which can improve the electrical conductivity of the material and the stability of the SEI film. In particular, the dense carbon layer has a good buffer effect against volume change. The protection provided by this continuous and dense carbon layer can improve the high-temperature properties and cycle properties.

[0034] (3) The present invention also provides a method for producing a carbon-coated composite material having the appropriate density and high coating integrity, which is simple and suitable for mass production.

[0035] (4) In the present invention, the coating is performed twice, and different coating gases and different gas flow rates are used for the two coatings, so that the resulting carbon-coated composite material is more densely and uniformly coated, and has better electrochemical properties as an electrode material. Preferably, in the present invention, a carbon-containing process gas containing a mixture of propylene and methane is used in the first carbon coating, and the introduction positions are different, which further improves the uniformity and density of the carbon coating. [Brief description of the drawings]

[0036] [Figure 1] 1 is an SEM image of the carbon-coated composite material produced in Example 1. [Diagram 2] 1 is a TEM image of the carbon-coated composite material produced in Example 1. [Diagram 3] 1 is an SEM image of the carbon-coated composite material produced in Example 3. [Figure 4] 1 is an SEM image of the carbon-coated composite material produced in Example 4. [Diagram 5] 1 is a TEM image of the carbon-coated composite material produced in Comparative Example 1. [Figure 6] FIG. 29 is a schematic diagram of the gas supply and material supply of the rotary kiln of Example 29. [Figure 7] 1 is a TEM image of the carbon-coated composite material obtained in Example 29. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0037] The technical solution of the present invention will be described in more detail with reference to specific examples below. The following examples are merely for illustrative purposes and are not to be construed as limiting the scope of the present invention. Any technology realized based on the above content of the present invention shall be included within the scope of the present invention.

[0038] The test methods in the following examples are conventional methods unless otherwise specified, and the reagents and materials are commercially available unless otherwise specified.

[0039] <Example 1> The method for producing carbon coated silicon monoxide includes the following steps. (1) 500 kg of silicon monoxide was crushed by airflow pulverization, with a D50 of 5 μm, (D90-D10) / D50 of 1.0, and a specific surface area of ​​1.1 m 3 ·g -1 , A / V (ratio of specific surface area to volume of accumulated pores) is 0.8 cm -1 Thus, the raw material to be coated was obtained. (2) The raw material to be coated was fed into a rotary kiln at a rate of 5 kg / h, a rotation speed of 0.5 rpm, a total volume of 1,200 L, and a high furnace temperature of 850°C. Nitrogen gas and propylene gas were continuously introduced at 50 L / min from a position close to the head of the rotary kiln (a position approximately 1 / 10 of the total length of the rotary kiln from the head of the furnace). The material was rotated in the kiln for 3 hours, at which point the first carbon element gas phase deposition was completed and the first intermediate product was obtained. (3) The first intermediate product of step (2) was sieved through a minimum 325 mesh sieve, and the sieved material was deagglomerated by mechanical deagglomeration to obtain a second intermediate product having a D50 of 5.1 μm. (4) The material from step (3) was fed into a rotary kiln at a speed of 5 kg / h, a rotation speed of 1.5 rpm, and a high furnace temperature of 850°C. Nitrogen gas at 50 L / min and propylene process gas at 25 L / min were continuously introduced into the rotary kiln from a position close to the furnace head (a position approximately 1 / 10 of the total length of the rotary kiln from the furnace head) to carry out a second carbon element vapor deposition. The residence time of the material in the furnace was controlled to 2 hours, and a crude carbon-coated composite material with a silicon monoxide core and carbon coated on the outer layer was obtained. (5) The crude carbon-coated composite material from step (4) was sieved to obtain a carbon-coated composite material having a uniform and dense carbon coating. The carbon-coated composite material produced in Example 1 had a D50 of 5.2 μm, a (D90-D10) / D50 of 1.1, and a specific surface area of ​​1.3 m 3 ·g -1 , A / V (ratio of specific surface area to volume of accumulated pores) is 1.09 cm -1 It is. Figure 1 shows an SEM image of the carbon-coated composite material produced in Example 1. Figure 2 shows a TEM image of the carbon-coated composite material produced in Example 1. From these figures, it can be seen that there are obvious lattice stripes on the surface of the carbon-coated composite material produced in Example 1, and there is a complete carbon coating layer.

[0040] <Example 2> A method for producing carbon-coated tin oxide, which is different from Example 1 in that 500 kg of silicon monoxide is changed to 500 kg of tin oxide, and in step (1), 500 kg of tin oxide is crushed by air flow to obtain a carbon-coated tin oxide powder with a D50 of 4.9 μm, a (D90-D10) / D50 of 1.0, and a specific surface area of ​​1.2 m. 3 ·g -1 , A / V (ratio of specific surface area to volume of accumulated pores) is 1.0 cm -1 The only difference is that the raw material to be coated is obtained by treating the raw material as described above. The carbon-coated composite material produced in Example 2 had a D50 of 5.0 μm, a (D90-D10) / D50 of 1.2, and a specific surface area of ​​1.4 m 3 ·g -1 , A / V (ratio of specific surface area to volume of accumulated pores) is 1.17 cm -1 It is.

[0041] <Example 3> A method for producing carbon-coated silicon, which, compared to Example 1, changes 500 kg of silicon monoxide to 500 kg of silicon; in step (1), 500 kg of silicon is crushed by airflow pulverization to obtain a carbon-coated silicon powder with a D50 of 5.3 μm, a (D90-D10) / D50 of 1.0, and a specific surface area of ​​1.3 m. 3 ·g -1 , A / V (ratio of specific surface area to volume of accumulated pores) is 1.15 cm -1 The only difference is that the raw material to be coated is obtained by treating the raw material as described above. The carbon-coated composite material produced in Example 3 had a D50 of 5.5 μm, a (D90-D10) / D50 of 1.0, and a specific surface area of ​​1.5 m 3 ·g -1 , A / V (ratio of specific surface area to volume of accumulated pores) is 1.39 cm -1 It is. FIG. 3 shows an SEM image of the carbon-coated composite material produced in Example 3. As can be seen from FIG. 3, a carbon-coated silicon material was produced in Example 3.

[0042] <Example 4> A method for producing carbon-coated graphite, in which, compared to Example 1, 500 kg of silicon monoxide was changed to 500 kg of natural graphite, and in step (1), 500 kg of natural graphite was crushed by air flow to obtain a graphite having a D50 of 4.9 μm, a (D90-D10) / D50 of 1.0, and a specific surface area of ​​1.3 m. 3 ·g -1 , A / V (ratio of specific surface area to volume of accumulated pores) is 1.25 cm -1 The only difference is that the raw material to be coated is obtained by treating the raw material as described above. The carbon-coated composite material produced in Example 4 had a D50 of 5 μm, a (D90-D10) / D50 of 1.0, and a specific surface area of ​​1.6 m 3 ·g -1 , A / V (ratio of specific surface area to volume of accumulated pores) is 1.49 cm -1 It is. FIG. 4 shows an SEM image of the carbon-coated composite material produced in Example 4. As can be seen from FIG. 4, a carbon-coated graphite material was produced in Example 4.

[0043] <Example 5> A method for producing carbon-coated silicon oxide, which is different from Example 1 in that 500 kg of silicon monoxide is changed to 500 kg of silicon oxide, and in step (1), 500 kg of silicon oxide is crushed by air flow pulverization to obtain a carbon-coated silicon oxide having a D50 of 4.9 μm, a (D90-D10) / D50 of 1.0, and a specific surface area of ​​1.3 m. 3 ·g -1 , A / V (ratio of specific surface area to volume of accumulated pores) is 1.25 cm -1 The only difference is that the raw material to be coated is obtained by treating the raw material as described above. The carbon-coated composite material produced in Example 5 had a D50 of 5 μm, a (D90-D10) / D50 of 1.0, and a specific surface area of ​​1.3 m 3 ·g -1 , A / V (ratio of specific surface area to volume of accumulated pores) is 1.1 cm -1 It is.

[0044] <Example 6> A method for producing carbon-coated magnesium-doped silicon monoxide, in which, compared to Example 1, 500 kg of silicon monoxide was changed to 500 kg of magnesium-doped silicon monoxide; in step (1), 500 kg of magnesium-doped silicon monoxide was crushed by airflow pulverization to obtain a carbon-coated magnesium-doped silicon monoxide having a D50 of 5.2 μm, a (D90-D10) / D50 of 1.0, and a specific surface area of ​​1.5 m. 3 ·g -1 , A / V (ratio of specific surface area to volume of accumulated pores) is 1.28 cm -1 The only difference is that the raw material to be coated is obtained by treating the raw material as described above. The carbon-coated composite material produced in Example 6 had a D50 of 5.5 μm, a (D90-D10) / D50 of 1.1, and a specific surface area of ​​1.8 m 3 ·g -1 , A / V (ratio of specific surface area to volume of accumulated pores) is 1.51 cm -1 It is.

[0045] <Example 7> A method for producing carbon-coated lithium-doped silicon monoxide, which is different from Example 1 in that 500 kg of silicon monoxide is replaced with 500 kg of lithium-doped silicon monoxide; in step (1), 500 kg of lithium-doped silicon monoxide is crushed by airflow pulverization to obtain a carbon-coated silicon monoxide having a D50 of 5.2 μm, a (D90-D10) / D50 of 1.0, and a specific surface area of ​​1.4 m. 3 ·g -1 , A / V (ratio of specific surface area to volume of accumulated pores) is 1.24 cm -1 The only difference is that the raw material to be coated is obtained by treating the raw material as described above. The carbon-coated composite material produced in Example 7 had a D50 of 5.4 μm, a (D90-D10) / D50 of 1.1, and a specific surface area of ​​1.6 m 3 ·g -1 , A / V (ratio of specific surface area to volume of accumulated pores) is 1.49 cm -1 It is. The carbon coated composite materials provided in Examples 1-7 were tested as follows. (1) Carbon content: The carbon content of the carbon-coated composite material was measured using a LECO carbon-sulfur analyzer and was designated as A. (2) Carbon layer density: The measurement method was as follows: the true density ρ1 and mass m1 of the carbon-coated composite material, and the mass m3 and density ρ3 of the material to be coated (core) were measured using a JWGB true density meter; as in (1), the carbon content (A) of the carbon-coated composite material was measured using a carbon-sulfur analyzer; the mass of the carbon coating layer was defined as m2 = m1 × A; and then ρ2 was calculated by ρ2 = m2ρ1ρ3 / (m1ρ3-m3ρ1). (3) Core element elution amount: As a measurement method, the carbon-coated composite material was placed in an excess amount of a solution capable of dissolving the core characteristic elements, and left to stand for 48 hours, and the content of the core elements in the solution was measured and designated as X1. The test results are shown in Table 1. JPEG0007562838000001.jpg41170JPEG0007562838000002.jpg36170As can be seen from Table 1, when propylene is used as the carbon-containing process gas, under the condition of 850 °C, propylene is introduced at 50 L / min in the first carbon element vapor phase deposition, and propylene is introduced at 25 L / min in the second carbon element vapor phase deposition, and the density of the carbon layer is 1.30 g cm regardless of the inorganic particles in the core. -3 In particular, in the case of silicon monoxide, the density of the carbon layer can be controlled to 1.40 g cm -3 It is possible to control the above.

[0046] <Examples 8 to 11> Compared to Example 1, the only difference is that the temperatures of the first carbon element vapor deposition and the second vapor deposition are 830°C (Example 8), 920°C (Example 9), 800°C (Example 10), and 1000°C (Example 11). The carbon-coated composite material produced in Example 8 had a D50 of 5.1 μm, a (D90-D10) / D50 of 1.1, and a specific surface area of ​​1.3 m 3 ·g -1 , A / V (ratio of specific surface area to volume of accumulated pores) is 1.03 cm -1 The carbon-coated composite material produced in Example 9 had a D50 of 5.2 μm, a (D90-D10) / D50 of 1.1, and a specific surface area of ​​1.4 m 3 ·g -1 , A / V (ratio of specific surface area to volume of accumulated pores) is 1.19 cm -1 The carbon-coated composite material produced in Example 10 had a D50 of 5 μm, a (D90-D10) / D50 of 1.1, and a specific surface area of ​​1.3 m 3 ·g -1 , A / V (ratio of specific surface area to volume of accumulated pores) is 1.27 cm -1 The carbon-coated composite material produced in Example 11 had a D50 of 5.3 μm, a (D90-D10) / D50 of 1.1, and a specific surface area of ​​1.5 m 3 ·g -1 , A / V (ratio of specific surface area to volume of accumulated pores) is 1.49 cm -1 It is.

[0047] <Examples 12 to 15> Compared to Example 1, the only difference is that the flow rate of the propylene process gas in the second vapor deposition was 13 L / min (Example 12), 40 L / min (Example 13), 50 L / min (Example 14), and 7 L / min (Example 15). The carbon-coated composite material produced in Example 12 had a D50 of 5.1 μm, a (D90-D10) / D50 of 1.1, and a specific surface area of ​​1.3 m 3 ·g -1 , A / V (ratio of specific surface area to volume of accumulated pores) is 1.27 cm -1 The carbon-coated composite material produced in Example 13 had a D50 of 5.6 μm, a (D90-D10) / D50 of 1.1, and a specific surface area of ​​1.4 m 3 ·g -1 , A / V (ratio of specific surface area to volume of accumulated pores) is 1.29 cm -1 The carbon-coated composite material produced in Example 14 had a D50 of 6.4 μm, a (D90-D10) / D50 of 1.1, and a specific surface area of ​​1.7 m 3 ·g -1 , A / V (ratio of specific surface area to volume of accumulated pores) is 1.68 cm -1 The carbon-coated composite material produced in Example 15 had a D50 of 5.3 μm, a (D90-D10) / D50 of 1.1, and a specific surface area of ​​1.6 m 3 ·g -1 , A / V (ratio of specific surface area to volume of accumulated pores) is 1.55 cm -1 It is.

[0048] <Example 16> The only difference from Example 1 is that the rotation speed of the high-temperature rotary kiln is 0.5 rpm in both steps (2) and (4). <Example 17> The only difference from Example 1 is that the rotation speed of the high-temperature rotary kiln is 1.5 rpm in both steps (2) and (4).

[0049] <Comparative Example 1> The method for producing carbon coated silicon monoxide includes the following steps. (1) 500 kg of silicon monoxide was crushed by airflow pulverization, with a D50 of 5 μm, (D90-D10) / D50 of 1.0, and a specific surface area of ​​1.1 m 3 ·g -1 , A / V (ratio of specific surface area to volume of accumulated pores) is 0.8 cm -1 Thus, the raw material to be coated was obtained. (2) The raw material to be coated was fed into a rotary kiln at a rate of 200 kg / h and a high furnace temperature of 850°C. Nitrogen gas was continuously introduced at 200 L / min and propylene gas at 50 L / min. The material was rotated in the kiln for 6 hours, at which point the first carbon element vapor deposition was completed and a crude carbon-coated composite material with a carbon-coated outer layer was obtained. (3) The crude carbon-coated composite material from step (2) was sieved to obtain a carbon-coated composite material coated with carbon. FIG. 5 shows a TEM image of the carbon-coated composite material produced in Comparative Example 1. As can be seen from FIG. 5, there are exposed areas on the surface of the carbon-coated composite material produced in Comparative Example 1 that are not covered with the carbon layer, suggesting that the carbon layer is not completely covered. The carbon-coated composite material produced in Example 16 had a D50 of 5.6 μm, a (D90-D10) / D50 of 1.0, and a specific surface area of ​​1.3 m 3 ·g -1 , A / V (ratio of specific surface area to volume of accumulated pores) is 1.19 cm -1 The carbon-coated composite material produced in Example 17 had a D50 of 5.3 μm, a (D90-D10) / D50 of 1.0, and a specific surface area of ​​1.4 m 3 ·g -1 , A / V (ratio of specific surface area to volume of accumulated pores) is 1.28 cm -1 The carbon-coated silicon monoxide obtained in Examples 8 to 17 was tested for the carbon layer density and the amount of silicon element eluted by the same test method as in Example 1, and the results of the carbon layer density and the amount of core characteristic element eluted for each Example are shown in Table 2. As can be seen from the comparison between Comparative Example 1 and Examples, when carbon element vapor deposition is performed only once, the integrity of the carbon coating and the density of the carbon layer cannot be ensured even if the deposition time is extended. As can be seen from Examples 8 to 11, when the vapor deposition temperature is 830 to 920°C, the carbon coating layer has a density of 1.3 g cm -3 ≦ρ2≦1.45g cm -3 The elution rate is 60 ppm or less, and if the temperature is too high or too low, the elution rate increases. As can be seen from Examples 12 to 15, when the gas flow rate of the second coating is 1 / 4 to 4 / 5 of the gas flow rate of the first coating, the carbon coating layer has a density of 1.4 g cm -3 ≦ρ2≦1.45g cm -3 When the gas flow rate of the second coating is too low, the integrity of the carbon coating layer is reduced and the leaching rate is improved, but it can be ensured to be below 100 ppm. When the gas flow rate of the second coating is too high, the leaching rate is reduced, but the reduction is not obvious. When propylene is used as the carbon-containing process gas, the conditions are 830-920 °C, and the rotation speed is 0.5-1.5 rpm. Propylene is introduced at 50 L / min in the first carbon element vapor deposition, and 25 L / min in the second carbon element vapor deposition. In both cases, the carbon layer density is 1.38-1.43 g cm -3 As a result, the amount of elution of the core elements can be controlled to less than 100 ppm.

[0050] <Example 18> Compared with Example 1, the only difference is that in the first carbon element vapor deposition, the carbon-containing process gas is methane, and the temperature is adaptively adjusted, specifically: In step (2), the raw material to be coated was fed into a high-temperature rotary kiln with an internal temperature of 1000°C at a feed rate of 5 kg / h, and nitrogen gas and methane gas were continuously introduced at 50 L / min and 50 L / min, respectively. The material was rotated in the kiln for 3 h, after which the first carbon element vapor deposition was completed and the first intermediate product was obtained. The carbon-coated composite material produced in Example 18 had a D50 of 5.3 μm, a (D90-D10) / D50 of 1.1, and a specific surface area of ​​4.5 m 3 ·g -1 , A / V (ratio of specific surface area to volume of accumulated pores) is 3.78 cm -1 Since methane is used as the process gas, a non-ordered carbon layer is coated, and thus the specific surface area is greatly increased.

[0051] <Example 19> Compared with Example 1, the only difference is that in the second carbon element vapor deposition, the carbon-containing process gas is methane, and the temperature is adaptively adjusted, specifically: In step (4), the furnace temperature was adjusted to 1000°C. The material from step (3) was fed into a high-temperature rotary kiln at a speed of 5 kg / h, a rotation speed of 1.5 rpm, and a furnace temperature of 1000°C. Nitrogen gas was continuously introduced at 50 L / min and methane at 25 L / min to carry out a second carbon element vapor deposition. The residence time of the material in the kiln was controlled to 2 hours, and a crude carbon-coated composite material with silicon monoxide as the core and carbon as the outer layer was obtained. The carbon-coated composite material produced in Example 19 had a D50 of 5.3 μm, a (D90-D10) / D50 of 1.1, and a specific surface area of ​​3.5 m 3 ·g -1 , A / V (ratio of specific surface area to volume of accumulated pores) is 2.94 cm -1 It is.

[0052] <Example 20> Compared with Example 1, the only difference is that the carbon-containing process gas is methane in both the first carbon element vapor phase deposition and the second carbon element vapor phase deposition, and the temperature is adaptively adjusted. Specifically, In step (2), the raw material to be coated is fed into a high-temperature rotary kiln at a rotation speed of 0.5 rpm and a furnace temperature of 1000°C at a feed rate of 5 kg / h. Nitrogen gas and methane are continuously introduced at 50 L / min and 50 L / min, respectively, and the material is rotated in the kiln for 3 hours, completing the first carbon element vapor deposition and obtaining the first intermediate product. In step (4), the material from step (3) is fed into a high-temperature rotary kiln at a speed of 5 kg / h, a rotation speed of 1.5 rpm, and a furnace temperature of 1000°C. Nitrogen gas of 50 L / min and methane of 25 L / min are continuously introduced to carry out a second carbon element vapor deposition. The residence time of the material in the kiln is controlled to 2 hours, and adjusted to obtain a crude carbon-coated composite material with silicon monoxide as the core and carbon as the outer layer. The carbon-coated composite material produced in Example 20 had a D50 of 5.4 μm, a (D90-D10) / D50 of 1.1, and a specific surface area of ​​5.5 m 3 ·g -1 , A / V (ratio of specific surface area to volume of accumulated pores) is 4.62 cm -1 It is.

[0053] <Example 21> Compared with Example 1, the only difference is that in the first carbon element vapor deposition, the carbon-containing process gas is acetylene, and the temperature is adaptively adjusted. Specifically, In step (2), the raw material to be coated is fed into a high-temperature rotary kiln at a rotation speed of 0.5 rpm and a furnace temperature of 900°C at a feed rate of 5 kg / h. Nitrogen gas and acetylene gas are continuously introduced at 50 L / min and 50 L / min, respectively. The material is rotated in the kiln for 3 hours, at which point the first carbon element vapor deposition is completed and the first intermediate product is obtained. The carbon-coated composite material produced in Example 21 had a D50 of 5.1 μm, a (D90-D10) / D50 of 1.1, and a specific surface area of ​​1.5 m 3 ·g -1 , A / V (ratio of specific surface area to volume of accumulated pores) is 1.38 cm -1 It is.

[0054] <Example 22> Compared with Example 1, the only difference is that the carbon-containing process gas in the second carbon element vapor deposition is acetylene, and the temperature is adaptively adjusted, specifically: In step (4), the material from step (3) is fed into a high-temperature rotary kiln at a speed of 5 kg / h, a rotation speed of 1.5 rpm, and a furnace temperature of 900°C. Nitrogen gas at 50 L / min and acetylene gas at 25 L / min are continuously introduced to carry out a second carbon element vapor deposition. The residence time of the material in the kiln is controlled to 2 hours, and adjusted to obtain a crude carbon-coated composite material with silicon monoxide as the core and carbon as the outer layer. The carbon-coated composite material produced in Example 22 had a D50 of 5.2 μm, a (D90-D10) / D50 of 1.1, and a specific surface area of ​​1.6 m 3 ·g -1 , A / V (ratio of specific surface area to volume of accumulated pores) is 1.51 cm -1 It is.

[0055] <Example 23> Compared with Example 1, the only difference is that the carbon-containing process gas in the first carbon element vapor phase deposition and the second carbon element vapor phase deposition is acetylene, and the temperature is adaptively adjusted. Specifically, In step (2), the raw material to be coated is fed into a high-temperature rotary kiln at a rotation speed of 0.5 rpm and a furnace temperature of 900°C at a feed rate of 5 kg / h. Nitrogen gas and acetylene gas are continuously introduced at 50 L / min and 50 L / min, respectively. The material is rotated in the kiln for 3 hours, at which point the first carbon element vapor deposition is completed and the first intermediate product is obtained. In step (4), the material from step (3) is fed into a high-temperature rotary kiln at a speed of 5 kg / h, a rotation speed of 1.5 rpm, and a furnace temperature of 900°C. Nitrogen gas at 50 L / min and acetylene gas at 25 L / min are continuously introduced to carry out a second carbon element vapor deposition. The residence time of the material in the kiln is controlled to 2 hours, and adjusted to obtain a crude carbon-coated composite material with silicon monoxide as the core and carbon as the outer layer. The carbon-coated composite material produced in Example 23 had a D50 of 5.5 μm, a (D90-D10) / D50 of 1.1, and a specific surface area of ​​1.7 m 3 ·g -1 , A / V (ratio of specific surface area to volume of accumulated pores) is 1.67 cm -1 It is. The above examples were tested for carbon layer density and elution of core characteristic elements by the same test method as in Example 1, and Table 3 shows the test results of the above examples. JPEG0007562838000004.jpg35170JPEG0007562838000005.jpg23170As can be seen from Table 3, regardless of whether methane or acetylene is used, the carbon layer density and the uniformity of the carbon coating can be improved by performing deagglomeration after the first carbon elemental vapor deposition and then performing a second carbon elemental vapor deposition. Of course, even if other carbon-containing process gases are used, the carbon layer density and the uniformity of the carbon coating can be improved by performing deagglomeration after the first carbon elemental vapor deposition and then performing a second carbon elemental vapor deposition.

[0056] <Example 24> Compared with Example 1, the coating material had a D50 of 5 μm, (D90-D10) / D50 of 1.2, and a specific surface area of ​​1.5 m 3 ·g -1 , A / V (ratio of specific surface area to volume of accumulated pores) is 1.1 cm -1 The only difference is that it has been changed to the following: (1) 500 kg of silicon monoxide was crushed by airflow pulverization to obtain a D50 of 5 μm, (D90-D10) / D50 of 1.2, and a specific surface area of ​​1.5 m 3 ·g -1 , A / V (ratio of specific surface area to volume of accumulated pores) is 1.1 cm -1 Thus, the raw material to be coated was obtained. The carbon-coated composite material produced in Example 24 had a D50 of 5.3 μm, a (D90-D10) / D50 of 1.2, and a specific surface area of ​​1.6 m 3 ·g -1 , A / V (ratio of specific surface area to volume of accumulated pores) is 1.58 cm -1 It is.

[0057] <Example 25> Compared with Example 1, in step (1), 500 kg of silicon monoxide was crushed by airflow pulverization to obtain a powder with a D50 of 5 μm, a (D90-D10) / D50 of 1.2, and a specific surface area of ​​2.5 m 3 ·g -1, A / V (ratio of specific surface area to volume of accumulated pores) is 1.5 cm -1 The only difference is that the raw material to be coated is obtained by treating the raw material as described above. The carbon-coated composite material produced in Example 25 had a D50 of 5.5 μm, a (D90-D10) / D50 of 1.2, and a specific surface area of ​​1.9 m 3 ·g -1 , A / V (ratio of specific surface area to volume of accumulated pores) is 2.44 cm -1 It is.

[0058] <Example 26> Compared with Example 1, in step (1), 500 kg of silicon monoxide was crushed by airflow pulverization to obtain a powder with a D50 of 10 μm, a (D90-D10) / D50 of 1.0, and a specific surface area of ​​1.1 m 3 ·g -1 , A / V (ratio of specific surface area to volume of accumulated pores) is 0.8 cm -1 The only difference is that the raw material to be coated is obtained by treating the raw material as described above. The carbon-coated composite material produced in Example 26 had a D50 of 10.3 μm, a (D90-D10) / D50 of 1.0, and a specific surface area of ​​1.4 m 3 ·g -1 , A / V (ratio of specific surface area to volume of accumulated pores) is 1.48 cm -1 It is.

[0059] <Example 27> (1) In Example 27, compared with Example 1, in step (1), 500 kg of silicon monoxide was crushed by airflow pulverization to obtain a powder with a D50 of 30 μm, a (D90-D10) / D50 of 1.0, and a specific surface area of ​​1.1 m 3 ·g -1 , A / V (ratio of specific surface area to volume of accumulated pores) is 0.8 cm -1 The only difference is that the raw material to be coated is obtained by treating the raw material as described above. The carbon-coated composite material produced in Example 27 had a D50 of 30.5 μm, a (D90-D10) / D50 of 1.1, and a specific surface area of ​​1.3 m 3 ·g -1 , A / V (ratio of specific surface area to volume of accumulated pores) is 1.41 cm -1 It is.

[0060] <Example 28> Compared with Example 1, the coating material had a D50 of 5 μm, (D90-D10) / D50 of 1.8, and a specific surface area of ​​2.0 m 3 ·g -1 , A / V (ratio of specific surface area to volume of accumulated pores) is 0.8 cm -1 The only difference is that it has been changed to the above. The carbon-coated composite material produced in Example 28 had a D50 of 5.5 μm, a (D90-D10) / D50 of 1.9, and a specific surface area of ​​1.4 m 3 ·g -1 , A / V (ratio of specific surface area to volume of accumulated pores) is 0.92 cm -1 It is.

[0061] <Comparative Example 2> Compared with Example 1, the coating material had a D50 of 5 μm, (D90-D10) / D50 of 1.2, and a specific surface area of ​​1.1 m 3 ·g -1 , A / V (ratio of specific surface area to volume of accumulated pores) is 0.4 cm -1 The only difference is that it has been changed to the following: The carbon-coated composite material produced in Comparative Example 2 had a D50 of 5.5 μm, a (D90-D10) / D50 of 1.2, and a specific surface area of ​​1.5 m 3 ·g -1 , A / V (ratio of specific surface area to volume of accumulated pores) is 0.8 cm -1 It is.

[0062] <Comparative Example 3> Compared with Example 1, the coating material had a D50 of 2.5 μm, (D90-D10) / D50 of 0.6, and a specific surface area of ​​5.0 m 3 ·g -1 , A / V (ratio of specific surface area to volume of accumulated pores) is 7.0 cm -1 The only difference is that it has been changed to The carbon-coated composite material produced in Comparative Example 3 had a D50 of 3.1 μm, a (D90-D10) / D50 of 0.7, and a specific surface area of ​​2.5 m 3 ·g -1 , A / V (ratio of specific surface area to volume of accumulated pores) is 2.3 cm -1 It is. The carbon layer density and the elution of the core characteristic elements were tested for the above examples and comparative examples, and the test results are shown in Table 4. As can be seen from Table 4, the specific raw material (the raw material to be coated has an average diameter of 1 to 40 μm, a particle size distribution range of 0.5≦(D90-D10) / D50≦2, and a specific surface area of ​​1 to 50 m 2 ·g -1 , the ratio of specific surface area to volume of accumulated pores is 0.5 to 5 cm -1 The raw material is rotated in a rotary kiln, and vapor deposition is performed twice on the surface of the raw material during the rotation, resulting in a complete and dense carbon coating (density ρ2 is 1.0-2.0 g cm -3 and the elution rate of the core element is 100 ppm or less) to form a carbon coating layer.

[0063] <Example 29> In step (2), the raw material to be coated is fed into the rotary kiln at a rate of 5 kg / h, a rotation speed of 0.5 rpm, a total volume of 1200 L in the furnace, and a high temperature of 850 ° C., and 50 L / min nitrogen gas, 25 L / min propylene gas, and 25 L / min methane gas are continuously introduced. Figure 6 is a schematic diagram of the gas supply and material supply to the rotary kiln. A mixed gas of propylene gas and nitrogen gas is introduced at a position close to the head of the rotary kiln (about 1 / 10 of the total length of the rotary kiln from the head of the furnace) which is the gas supply port 1, and a mixture of methane gas and nitrogen gas is introduced from a position close to the center of the rotary kiln (about 2 / 5 of the total length of the rotary kiln from the head of the furnace) through a long gas introduction pipe. The material is rotated in the furnace for 3 hours, and the first carbon element vapor deposition is completed. The remaining conditions are the same as those in Example 1, except that the first intermediate product is obtained. Finally, a carbon-coated composite with a uniform and dense carbon coating was obtained. Figure 7 shows a TEM image of the carbon-coated composite obtained in Example 29. The change in contrast between the core and shell and the distinction of the lattice fringes on the surface indicate that the thickness and completeness of the surface-coated carbon are superior to those of the carbon-coated composite in Example 1, and the coating is more complete. Tests were performed on the carbon-coated composite obtained in Example 29, and the carbon layer density was found to be 1.44 g cm. -3 The amount of silicon eluted, which is a core characteristic element, is 29 ppm.

[0064] <Example 30> The remaining conditions were the same as in Example 29, except that both propylene gas and methane gas were fed through gas supply port 1. The carbon-coated composite material obtained in Example 30 was tested, and the carbon layer density was 1.44 g cm -3 The amount of silicon eluted, which is a core characteristic element, is 36 ppm. Although the cause is unclear, a comparison between Example 29 and Example 30 suggests that introducing propylene gas from a position close to the furnace head and introducing methane from a position close to the center of the furnace body is more advantageous for forming a complete, uniform and dense carbon coating layer.

[0065] <Application Examples> Characterization of the electrochemical properties of the carbon-coated composite anode material: The carbon-coated composite anode material prepared in the above example, Super P, and polyacrylic acid (adhesive) were mixed in a mass ratio of 80:10:10 to prepare a slurry, which was then uniformly applied to a copper foil current collector to obtain an electrode sheet. A metal lithium plate was used as the counter electrode, a polypropylene microporous membrane (Celgard 2400) was used as the separator, and 1 mol / L LiPF6 (the solvent is a mixture of vinyl carbonate and dimethyl carbonate in a volume ratio of 1:1, with 5% vinylidene carbonate fluoride and 2% vinylidene carbonate added) was used as the electrolyte. The battery was assembled in a glove box protected by argon gas to prepare a button battery, and a charge-discharge test was performed. The test program was 100 mAg -1The charge / discharge voltage range was 0.01 to 1.5 V, and the battery test results are shown in Table 5. Application Examples 1 to 30 and Comparative Application Examples 1 to 3 used the carbon-coated negative electrode materials of Examples 1 to 30 and Comparative Examples 1 to 3, respectively. The test results of the battery characteristics of some of the application examples are shown in Table 5 below. JPEG0007562838000007.jpg92170

Claims

1. A carbon-coated composite material comprising a core material and a carbon coating layer coated on the core material, The carbon coating layer has a density of 1.0 to 2.0 g cm -3 The core material, which is the target material for carbon coating, has a D50 of 1 to 40 μm, a particle size distribution range that satisfies 0.5≦(D90−D10) / D50≦2, and a specific surface area of ​​1 to 5 m 2 ・g -1 and the ratio of the specific surface area to the volume of the deposited pores is 0.50 to 2.00 cm -1 an increase in D50 of the composite material after coating is 3 μm or less; when the carbon-coated composite material is placed in an elution solution, the amount of elution of a core characteristic element, which is a predetermined element eluted, is measured, and the amount of elution of the core characteristic element is 100 ppm or less; the core characteristic element is an element for which ICP quantitative data can be obtained by a chemical reaction in the carbon-coated target material; the core material is any one or a combination of at least two selected from the group consisting of graphite particles, metal tin particles, tin oxide particles, silicon particles, silicon oxide particles, silicon nitride particles, element-doped silicon-oxygen composite particles, metal germanium particles, and germanium oxide particles; When the core material is a graphite particle, the eluent is aqua regia and the core characteristic element is iron element; When the core material is a metal tin particle or a tin oxide particle, the eluent is aqua regia and the core characteristic element is tin element; When the core material is a metallic germanium particle or a germanium oxide particle, the eluate is aqua regia and the core characteristic element is germanium element; A carbon-coated composite material for lithium-ion batteries, characterized in that when the core material is silicon particles, silicon oxide particles, silicon nitride particles, or element-doped silicon-oxygen composite particles, the eluent is a sodium hydroxide or hydrofluoric acid solution, and the core characteristic element is silicon.

2. The carbon coating layer has a density of 1.2 g cm -3 ≦ρ 2 ≦1.5g cm -3 The material to be carbon-coated has a D50 of 3 to 10 μm, a particle size distribution range of 1≦(D90−D10) / D50≦1.5, and a specific surface area of ​​1 to 2 m 2 ・g -1 and the ratio of the specific surface area to the volume of the deposited pores is 0.70 to 1.50 cm -1 and an increase in D50 of the composite material after coating is 1 μm or less.

3. The carbon-coated composite material according to claim 1, characterized in that the silicon oxide particles are any silicon oxide having a silicon to oxygen ratio of 1:1 to 1:2, and the element-doped silicon oxygen composite particles include lithium-doped silicon monoxide and magnesium-doped silicon monoxide.

4. The average diameter of the core material is 1 to 40 μm, the particle size distribution range is 0.5≦(D90-D10) / D50≦2, and the specific surface area is 1 to 5 m 2 ・g -1 , the ratio of the specific surface area to the volume of the accumulated pores is 0.5 to 2.0 cm -1 (1) treating a core material to be coated so that (2) loading the treated raw material to be coated into a rotary kiln, and introducing a carbon-containing process gas under a protective atmosphere to perform a first carbon element vapor deposition to obtain a first intermediate product; (3) sieving the first intermediate product to remove large sized materials and crushing and deagglomerating the remaining materials to obtain a second intermediate product; and (4) a step of feeding the second intermediate product back into a rotary kiln, and conducting a second carbon element vapor deposition by introducing a carbon-containing process gas under a protective atmosphere, thereby obtaining a carbon-coated composite material having a core of raw material particles to be coated and an outer layer of carbon coated thereon.

5. In steps (2) and (4), the carbon-containing process gas comprises C1-4 alkanes, C2-4 olefins, and C2-4 alkynes; the rotation speed of the rotary kiln is 0.1-2 rpm; The first carbon element vapor deposition is performed at a temperature of 600 to 1200° C. for 0.5 to 10 h, or the first carbon element vapor deposition is a plasma vapor deposition at 100 to 500° C. for 0.5 to 10 h; The manufacturing method according to claim 4, characterized in that the second carbon element vapor deposition is a plasma vapor deposition at a temperature of 600 to 1200 ° C and a time of 0.5 to 10 h, or the second carbon element vapor deposition is a plasma vapor deposition at a temperature of 100 to 500 ° C and a time of 0.5 to 10 h.

6. In the first carbon element vapor deposition, the carbon-containing process gas is a mixture of propylene and methane in a volume ratio of 1-2:1-2, and the introduction flow rate of the process gas satisfies the condition of h=V / s, where V is the total volume of the chamber of the rotary kiln (unit: L), s is the introduction rate of the gas (unit: L / min), and the flow rate of the process gas satisfies the condition of h=20-60 min; 5. The method of claim 4, wherein the introduction flow rate of the carbon-containing process gas in the second carbon element vapor phase deposition is 1 / 4 to 4 / 5 of the flow rate of the carbon-containing process gas in the first carbon element vapor phase deposition.

7. The method according to claim 6, characterized in that propylene is introduced from a position 1 / 5 of the total length of the furnace body from the position of the furnace mouth of the rotary kiln, and methane is introduced from a position 1 / 3 to 2 / 3 of the total length of the furnace body of the rotary kiln.

8. Use of the carbon-coated composite material according to any one of claims 1 to 3 as an electrode material for a lithium-ion battery.

Citation Information

Patent Citations

  • Electrode material carbon coating method

    CN111048784A

  • High-temperature device for preparing lithium ion battery negative electrode material and preparation method of material

    CN112209390A

  • Method for manufacturing negative electrode material for nonaqueous electrolyte secondary battery, negative electrode material for nonaqueous electrolyte secondary battery, negative electrode for nonaqueous electrolyte secondary battery, and lithium ion secondary battery

    JP2016100047A

  • Method for producing carbon-coated silicon particles

    JP2023524933A