Preparation process and application of perovskite-based microcrystalline material

By controlling the combination of aluminum nitrate and terephthalic acid and adding small particle sizes to form a composite structure of frame particles, the problem of insufficient stability of perovskite-based microcrystalline materials in long-term light, high temperature and humidity environments is solved. High stability and excellent photoelectric properties of the material are achieved.

CN119018933AActive Publication Date: 2024-11-26SHANDONG ZHOULAN ENVIRONMENTAL PROTECTION TECH CO LTD
View PDF 12 Cites 0 Cited by

Patent Information

Application Number
CN202411153927.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-21
Publication Date
2024-11-26
Estimated Expiration
2044-08-21

AI Technical Summary

Technical Problem

Perovskite-based microcrystalline materials have insufficient stability in long-term light, high temperature and humidity environments, and there are problems of material decomposition and energy efficiency losses, which affects their photoelectric performance and service life.

Method used

By controlling the compounding ratio of aluminum nitrate and terephthalic acid, frame particles are formed to improve the binding force of the material, and by adding small particle sizes to add particles such as titanium dioxide and zinc oxide, a composite structure is formed to reduce defects and decomposition phenomena, and enhance the Resistance to light and moisture.

Benefits of technology

It significantly improves the stability of perovskite-based microcrystalline materials in long-term light, high temperature and humidity environments, avoids decomposition, enhances photoelectric performance and service life, and has excellent application value.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005004387980000121
    Figure BDA0005004387980000121
Patent Text Reader

Abstract

The invention relates to the field of microcrystalline materials, in particular to a perovskite-based microcrystalline material and a preparation process and application thereof. The invention discloses a preparation process of a perovskite-based microcrystalline material. The preparation process specifically comprises the following steps: S1, preparing a site material solution; s2, adding framework particle raw materials; s3, preliminary synthesis of a microcrystalline material; and S4, preparing the composite microcrystalline material. The perovskite-based microcrystalline material prepared by the invention can effectively overcome the internal defects in the material, thereby avoiding the loss of photoelectric properties, and can ensure that the perovskite material has excellent stability in long-term illumination, high-temperature and humidity environments, and still keeps good own characteristics in a high-humidity environment, thereby avoiding the decomposition phenomenon, and improving the performance of the perovskite-based microcrystalline material. Therefore, the method has very excellent application value.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of microcrystalline materials, and in particular to a perovskite-based microcrystalline material and a preparation process and application thereof. Background Art

[0002] As an emerging semiconductor material, perovskite-based microcrystalline materials have attracted widespread attention in recent years due to their excellent optoelectronic properties. As a special microcrystalline material, perovskite-based microcrystalline materials are based on perovskite structure and have unique optoelectronic properties, making them a research hotspot in many application fields. Due to their excellent performance, perovskite-based microcrystalline materials have gradually gained more and more applications in solar cells, sensors, electronic products, testing instruments and other fields.

[0003] However, as consumers' performance requirements for products in the fields of solar cells, sensors, and electronic products continue to increase, the performance of perovskite-based microcrystalline materials has also increased. Although perovskite-based microcrystalline materials have many advantages, there are still some problems that need to be solved. For example, the stability of perovskite materials under long-term light, high temperature, and humidity environments is still insufficient, which is a major challenge for practical applications; the organic components in organic-inorganic hybrid perovskite materials may cause material decomposition, affecting their stability and service life; defects in perovskite materials can lead to energy efficiency loss, affecting their optoelectronic properties, etc.

[0004] Therefore, in order to effectively solve the above problems, the present application provides a perovskite-based microcrystalline material and a preparation process thereof. The perovskite-based microcrystalline material prepared in the present application can effectively overcome the internal defects in the material, thereby avoiding the loss of photoelectric performance, and can ensure that the perovskite material has excellent stability under long-term illumination, high temperature and humidity environments, and still maintains good self-properties in high humidity environments, avoiding decomposition, and thus has very excellent application value. Summary of the invention

[0005] In order to solve the above problems, the first aspect of the present application provides a preparation process of a perovskite-based microcrystalline material, which specifically includes the following steps: S1: adding the A site material and the B site material to an organic mixed solvent respectively, then heating to 110-140°C, stirring evenly at a speed of 60-80rpm to obtain an A site material solution and a B site material solution; S2: adding a size control agent to the A site material solution and the B site material solution respectively, and adding aluminum nitrate to the A site material solution and stirring thoroughly, and adding terephthalic acid and hydrofluoric acid to the B site material solution, and then maintaining 120-130°C to dropwise add the B site material solution to the A site material solution, the dropping time is 30-40min, and then stirring at 60-80rpm to keep warm for reaction; S3: waiting for the reaction to have no color change When obvious precipitation is generated after standing, it is naturally cooled to room temperature, the product is centrifuged and filtered out, and washed with ethanol for 2 to 3 times to obtain pretreated particles; S4: the pretreated particles are mixed with the added particles, organic acid anhydride and coupling agent, added to deionized water, heated to 60 to 65°C, kept warm for reaction for 2.5 to 3 hours, and then transferred to a high-temperature reactor, the pressure is controlled to be 2 to 2.2 MPa, the temperature is raised to 190 to 210°C, and the reaction is kept warm for 16 to 19 hours at a speed of 120 to 160 rpm. After the reaction is completed, it is naturally cooled to 60 to 70°C and triethanolamine is added to adjust the pH to 9.5 to 10, and tetraethyl orthosilicate and isopropanol are added. The reaction is kept warm for 2 to 3 hours. After completion, the product is centrifuged and filtered, washed with ethanol for 2 to 3 times, and vacuum dried at 70 to 80°C to obtain.

[0006] As a preferred solution, the A site material is at least one of CsBr, RbBr, MAI, and FAI.

[0007] As a preferred solution, the A site material is CsBr or RbBr.

[0008] As a preferred solution, the A site material is CsBr.

[0009] As a preferred solution, the B site material is at least one of PbBr2, SnBr2, and GeBr4.

[0010] As a preferred solution, the B site material is PbBr2 or SnBr2.

[0011] As a preferred solution, the B site material is PbBr2.

[0012] As a preferred solution, the mass ratio of the A site material to the B site material is (2.5-4):(5-7).

[0013] As a preferred solution, the mass ratio of the A site material to the B site material is (2.5-3.5):(5.5-6.5).

[0014] As a preferred solution, the organic mixed solvent is a combination of oleylamine and n-octylamine.

[0015] As a preferred solution, the mass ratio of oleylamine to n-octylamine is (1.5-2.5):(1-1.4).

[0016] As a preferred solution, the mass ratio of oleylamine to n-octylamine is (1.6-2.2):(1.2-1.4).

[0017] As a preferred solution, the size control agent is oleic acid.

[0018] As a preferred solution, the mass ratio of the A site material to the size control agent is (2.5-4): (40-50).

[0019] As a preferred solution, the mass ratio of the B site material to the size control agent is (5-7): (40-50).

[0020] As a preferred solution, the mass ratio of the A site material to aluminum nitrate is (2.5-4): (2-2.5).

[0021] As a preferred solution, the mass ratio of the A site material to aluminum nitrate is (2.5-3.5): (2.1-2.3).

[0022] As a preferred solution, the mass ratio of terephthalic acid and hydrofluoric acid in the B-site material is (5-7): (3-3.8): (12-20).

[0023] As a preferred solution, the mass ratio of terephthalic acid and hydrofluoric acid in the B-site material is (5.5-6.5):(3.2-3.4):(14-16).

[0024] As a preferred solution, the average particle size of the pretreated particles is 120-200 nm.

[0025] In the present application, by controlling the compounding ratio of raw materials such as aluminum nitrate and terephthalic acid, the framework particles formed in the initial stage are successfully controlled and added during the formation process of the microcrystalline material, and the bonding force therebetween is greatly improved, thereby effectively improving the stability of the microcrystalline material under illumination, high temperature and high humidity environments, and effectively reducing the formation of microcrystalline defects, and avoiding decomposition. The terephthalic acid raw material added in the present application can preferentially form framework particles with an initial structure in the microcrystalline bonding process, relying on the reactivity at the same temperature, and the formation of the framework particles can become a carrier platform for the formation of microcrystalline particles, and in the process of formation, a semi-encapsulated structure of microcrystalline and framework particles is formed by the initial liquid coating effect, thereby greatly reducing the self-defects of the microcrystalline material through the structure of the regular framework particles, and through the subsequent addition of particles, a more stable composite structure is formed, and a longer electronic path is formed, and the bandgap is reduced by the aggregation effect of electrons and holes, so as to obtain better and excellent light resistance, and the formed framework particles can form a more excellent composite particle low surface energy structure through its flat surface, so as to have excellent moisture resistance in a high humidity environment.

[0026] As a preferred solution, the mass ratio of the pretreated particles, the added particles, the organic anhydride and the coupling agent is (3-4): (0.6-1): (0.3-0.5): (0.1-0.15).

[0027] As a preferred solution, the mass ratio of the pretreated particles, the added particles, the organic anhydride and the coupling agent is (3.4-3.8): (0.8-1): (0.4-0.45): (0.12-0.14).

[0028] As a preferred solution, in the pre-treated particles, the mass ratio of tetraethyl orthosilicate and isopropyl alcohol is (3-4): (0.2-0.5): (0.05-0.1).

[0029] As a preferred solution, the mass ratio of tetraethyl orthosilicate and isopropyl alcohol in the pretreated particles is (3.4-3.8): (0.35-0.45): (0.06-0.08).

[0030] As a preferred solution, the added particles are any one of zinc oxide, titanium dioxide and antimony dioxide.

[0031] As a preferred solution, the added particles are zinc oxide or titanium dioxide.

[0032] As a preferred solution, the average particle size of the added particles is 5 to 15 nm.

[0033] As a preferred solution, the organic acid anhydride is succinic anhydride or glutaric anhydride.

[0034] As a preferred solution, the coupling agent is a titanate coupling agent or a silane coupling agent.

[0035] As a preferred solution, the average particle size of the perovskite-based microcrystalline material is 460-580 nm.

[0036] In the present application, by further selecting the added particles and controlling the particle size thereof, the comprehensive performance of the obtained perovskite-based microcrystalline material is greatly improved, and the self-stability is effectively improved and the defects are improved. The added particles of small particle size (such as titanium dioxide and zinc oxide) can be modified by carboxylation on the surface thereof, greatly increasing the coordination binding effect with the internal framework particles, thereby stabilizing the binding stability of the added particles on the surface of the framework particles, and forming an external wrapping for the framework particles to a certain extent, and this wrapping effect can further increase the binding strength of the framework particles for the microcrystalline particles, thereby maintaining excellent binding force during long-term use, and preventing the intrusion of water molecules by the framework particles, maintaining the overall composite structure for the resistance effect of water molecules, and obtaining good stability.

[0037] The second aspect of the present application provides an application of a perovskite-based microcrystalline material obtained by the above-mentioned preparation process of the perovskite-based microcrystalline material in the fields of solar cells, sensors, electronic products, and photocatalysis.

[0038] The beneficial effects of this application are:

[0039] 1. A perovskite-based microcrystalline material provided in the present application can effectively overcome the internal defects in the material, thereby avoiding the loss of photoelectric performance, and can ensure that the perovskite material has excellent stability under long-term illumination, high temperature and humidity environments, and still maintains good self-properties in high humidity environments, avoiding decomposition, and thus has very excellent application value.

[0040] 2. A perovskite-based microcrystalline material provided in the present application, in which the added terephthalic acid raw material can preferentially form framework particles with an initial structure during the microcrystalline bonding process by relying on the reaction activity at the same temperature, and the formation of the framework particles can become a carrier platform for the formation of microcrystalline particles, and in the formation process, a semi-encapsulated structure of microcrystals and framework particles is formed by the initial liquid coating effect, thereby greatly reducing the inherent defects of the microcrystalline material through the regular structure of the framework particles, and through the subsequent addition of particles, a more stable composite structure is formed, and a longer electron path is formed, and the bandgap is reduced by the aggregation effect of electrons and holes, thereby obtaining better light resistance, and the formed framework particles can form a better composite particle low surface energy structure through their flat surface, thereby having excellent moisture resistance in a high humidity environment.

[0041] 3. A perovskite-based microcrystalline material provided in the present application greatly improves the comprehensive performance of the perovskite-based microcrystalline material obtained by selecting added particles and controlling their particle size, and effectively improves its own stability and improves defects; the added small-size added particles (such as titanium dioxide and zinc oxide) can greatly increase their coordination and binding effect with the internal framework particles through carboxyl modification of their surfaces, thereby stabilizing the binding stability of the added particles on the surface of the framework particles, and forming an external wrapping of the framework particles to a certain extent. This wrapping effect can further increase the bonding strength of the framework particles to the microcrystalline particles, thereby maintaining excellent bonding strength during long-term use, and blocking the invasion of water molecules through the framework particles, maintaining the overall composite structure's resistance to water molecules, and obtaining good stability. DETAILED DESCRIPTION

[0042] The following will further explain and demonstrate the technical solutions in the above invention content of this application in the form of specific implementation schemes. The following embodiments are only practical examples used to illustrate and explain the contents of the technical solutions in the specification, and should not limit the scope of the claims to be protected by this application. All technical products based on the technical solutions described in the invention content of this application should be included in the scope to be protected by this application.

[0043] In the following examples, unless otherwise specified, the raw materials are all commercially available products, or can be prepared by methods well known to those skilled in the art.

[0044] Example 1

[0045] Example 1 The first aspect provides a preparation process for a perovskite-based microcrystalline material, which specifically includes the following steps, measured in parts by mass: S1: 2.92 parts of A site material and 6.15 parts of B site material are respectively added to 320 parts of an organic mixed solvent, and then the temperature is raised to 125°C, and stirred evenly at a speed of 80rpm to obtain an A site material solution and a B site material solution; S2: 42.5 parts and 44.8 parts of size control agents are added to the A site material solution and the B site material solution, respectively, and 2.2 parts of aluminum nitrate are added to the A site material solution and stirred completely, and 3.4 parts of terephthalic acid and 14.8 parts of hydrofluoric acid are added to the B site material solution, and then the B site material solution is added dropwise to the A site material solution at 130°C, and the dropping time is 40min, and then the reaction is stirred at 80rpm for insulation; S3 : When there is no color change in the reaction and obvious precipitation is generated after standing, it is naturally cooled to room temperature, the product is centrifuged and filtered out, and washed with ethanol for 3 times to obtain pretreated particles; S4: 3.6 parts of pretreated particles, 0.82 parts of added particles, 0.44 parts of organic acid anhydride and 0.12 parts of coupling agent are mixed and added to 150 parts of deionized water, the temperature is raised to 65°C, and the reaction is kept warm for 3 hours. Then, the mixture is transferred to a high-temperature reactor, the pressure is controlled to be 2.1MPa, the temperature is raised to 200°C, and the reaction is kept warm for 18 hours at a speed of 140rpm. After the reaction is completed, it is naturally cooled to 65°C and triethanolamine is added to adjust the pH to 9.8. 0.38 parts of tetraethyl orthosilicate and 0.08 parts of isopropanol are added, and the reaction is kept warm for 2 hours. After completion, the product is centrifuged and filtered, washed with ethanol for 3 times, and vacuum dried at 70-80°C to obtain.

[0046] The A site material is CsBr; the B site material is PbBr2.

[0047] The organic mixed solvent is a composition of oleylamine and n-octylamine, and the mass ratio of the two is 1.8:1.2.

[0048] The size control agent is oleic acid.

[0049] The average particle size of the pretreated particles was 148 nm.

[0050] The added particles are titanium dioxide, and the average particle size is 10 nm.

[0051] The organic acid anhydride is succinic anhydride, and the silane coupling agent is 3-aminopropyltriethoxysilane.

[0052] The average particle size of the perovskite-based microcrystalline material is 527 nm.

[0053] Example 2

[0054] Example 2 The first aspect provides a preparation process for a perovskite-based microcrystalline material, which specifically includes the following steps, measured in parts by mass: S1: 3.14 parts of A site material and 5.76 parts of B site material are respectively added to 330 parts of an organic mixed solvent, and then the temperature is raised to 125°C, and stirred evenly at a speed of 80rpm to obtain an A site material solution and a B site material solution; S2: 44.2 parts and 43.5 parts of a size control agent are added to the A site material solution and the B site material solution, respectively, and 2.3 parts of aluminum nitrate are added to the A site material solution and stirred completely, and 3.4 parts of terephthalic acid and 15.5 parts of hydrofluoric acid are added to the B site material solution, and then the B site material solution is added dropwise to the A site material solution at 130°C, and the dropping time is 40min, and then the reaction is stirred at 80rpm for insulation; S3 : When there is no color change in the reaction and obvious precipitation is generated after standing, it is naturally cooled to room temperature, the product is centrifuged and filtered out, and washed with ethanol for 3 times to obtain pretreated particles; S4: 3.6 parts of pretreated particles, 0.82 parts of added particles, 0.44 parts of organic acid anhydride and 0.12 parts of coupling agent are mixed and added to 150 parts of deionized water, the temperature is raised to 65°C, and the reaction is kept warm for 3 hours. Then, the mixture is transferred to a high-temperature reactor, the pressure is controlled to be 2.1MPa, the temperature is raised to 200°C, and the reaction is kept warm for 18 hours at a speed of 140rpm. After the reaction is completed, it is naturally cooled to 65°C and triethanolamine is added to adjust the pH to 9.8. 0.38 parts of tetraethyl orthosilicate and 0.08 parts of isopropanol are added, and the reaction is kept warm for 2 hours. After completion, the product is centrifuged and filtered, washed with ethanol for 3 times, and vacuum dried at 70-80°C to obtain.

[0055] The A site material is RbBr; the B site material is SnBr2.

[0056] The organic mixed solvent is a composition of oleylamine and n-octylamine, and the mass ratio of the two is 1.8:1.2.

[0057] The size control agent is oleic acid.

[0058] The average particle size of the pretreated particles was 166 nm.

[0059] The added particles are titanium dioxide, and the average particle size is 10 nm.

[0060] The organic acid anhydride is succinic anhydride, and the silane coupling agent is 3-aminopropyltriethoxysilane.

[0061] The average particle size of the perovskite-based microcrystalline material is 561 nm.

[0062] Comparative Example 1

[0063] The specific implementation method of this comparative example is basically the same as that of Example 1, except that: S1: 1.55 parts of site A material and 8.55 parts of site B material are respectively added to 320 parts of an organic mixed solvent, then heated to 125°C, and stirred evenly at 80 rpm to obtain site A material solution and site B material solution.

[0064] The average particle size of the perovskite-based microcrystalline material is 322 nm.

[0065] Comparative Example 2

[0066] The specific implementation method of this comparative example is basically the same as that of Example 1, except that: S1: 5.8 parts of site A material and 3.55 parts of site B material are respectively added to 320 parts of an organic mixed solvent, then heated to 125°C and stirred evenly at 80 rpm to obtain site A material solution and site B material solution.

[0067] The average particle size of the perovskite-based microcrystalline material is 351 nm.

[0068] Comparative Example 3

[0069] The specific implementation method of this comparative example is basically the same as that of Example 1, with the only difference being: S2: 22.5 parts and 15.5 parts of size control agents are added to the A site material solution and the B site material solution, respectively, and 4.5 parts of aluminum nitrate are added to the A site material solution and stirred thoroughly, and 6.8 parts of terephthalic acid and 25 parts of hydrofluoric acid are added to the B site material solution, and then the B site material solution is added dropwise to the A site material solution at 130°C for 50 minutes, and then the reaction is stirred at 80rpm for insulation.

[0070] The average particle size of the perovskite-based microcrystalline material is 687 nm.

[0071] Comparative Example 4

[0072] The specific implementation method of this comparative example is basically the same as that of Example 1, with the only difference being: S2: 44.2 parts and 43.5 parts of size control agents are added to the A site material solution and the B site material solution respectively, and 0.9 parts of aluminum nitrate is added to the A site material solution and stirred thoroughly, and 1.9 parts of terephthalic acid and 6.5 parts of hydrofluoric acid are added to the B site material solution, and then the B site material solution is added dropwise to the A site material solution at 130°C for 40 minutes, and then the reaction is stirred at 80rpm for insulation.

[0073] The average particle size of the perovskite-based microcrystalline material is 359 nm.

[0074] Comparative Example 5

[0075] The specific implementation of this comparative example is basically the same as that of Example 1, except that: S4: 3.6 parts of pretreated particles, 0.35 parts of added particles, 0.25 parts of organic anhydride and 0.04 parts of coupling agent are mixed and added to 120 parts of deionized water, the temperature is raised to 65°C, and the mixture is kept warm for 3 hours. The mixture is then transferred to a high-temperature reactor, the pressure is controlled to be 2.1 MPa, the temperature is raised to 200°C, and the mixture is stirred and kept warm for 18 hours at a speed of 140 rpm. After the reaction is completed, the mixture is naturally cooled to 65°C, triethanolamine is added to adjust the pH to 9.8, 0.38 parts of tetraethyl orthosilicate and 0.08 parts of isopropanol are added, and the mixture is kept warm for 2 hours. After completion, the product is centrifuged and filtered, washed with ethanol for 3 times, and dried in a vacuum oven at 70-80°C.

[0076] The average particle size of the perovskite-based microcrystalline material is 405 nm.

[0077] Comparative Example 6

[0078] The specific implementation of this comparative example is basically the same as that of Example 1, except that the average particle size of titanium dioxide is 25 nm.

[0079] The average particle size of the perovskite-based microcrystalline material is 677 nm.

[0080] Performance Evaluation

[0081] High temperature and high humidity stability: Samples of the microcrystalline materials prepared in the examples and comparative examples were placed in a constant temperature and humidity chamber at 85±3°C and 75±3% relative humidity and stably stored for 6 months. After 6 months, the samples were taken out and observed to see if there were any cracking, pulverization, hydrolysis and oxidation phenomena. If there were any, it was recorded as unqualified, otherwise it was qualified. 50 samples were tested in each group, and the qualified rate was recorded in Table 1.

[0082] Light stability: Samples of the microcrystalline materials prepared in the examples and comparative examples were placed in a light box to simulate constant sunlight, ensuring a relative humidity of 50±3%, and stably stored for 3 months. After 6 months, the samples were taken out and observed to see if there was any etching, yellowing, or oxidation. If there was any, it was recorded as unqualified, otherwise it was qualified. 50 samples were tested in each group, and the qualified rate was recorded in Table 1.

[0083] Excitation light test: The microcrystalline materials prepared in the examples and comparative examples were excited by 365 nm light, and the emitted light was green light. The peak value of the emission (nm) was detected and determined. The test value was the average value of 10 tests and recorded in Table 1.

[0084] Table 1 Performance test results

[0085]

[0086] It can be seen from the embodiments and comparative examples of the present application and the data results in Table 1 that embodiments 1 and 2 of the present application have obvious advantages over comparative examples 1 to 6 in terms of high temperature and high humidity stability, light resistance stability, and photoelectric performance. This is mainly due to the combined effect of the framework particle structure and added particles as specified in the present application and other matching schemes. Comparative examples 1 to 6 did not adopt the technical scheme specified in the present application, resulting in obvious disadvantages in the above-mentioned performance tests. This further proves the necessity of the technical scheme specified in the present application for the technical effect of the present application and solving technical problems.

Claims

1. A process for preparing a perovskite-based microcrystalline material, characterized in that: The specific steps include: S1: Add the A site material and the B site material to an organic mixed solvent respectively, then heat it to 110-140°C, stir it evenly at 60-80rpm to obtain the A site material solution and the B site material solution; S2: Add a size control agent to the A site material solution and the B site material solution respectively, add aluminum nitrate to the A site material solution and stir it completely, and add terephthalic acid and hydrofluoric acid to the B site material solution, then keep 120-130°C and add the B site material solution dropwise to the A site material solution, the dropping time is 30-40min, and then stir at 60-80rpm to keep the reaction warm; S3: When there is no color change in the reaction and obvious precipitation is generated after standing, cool it naturally to room temperature, centrifuge and filter the product out, and wash it with ethanol for 2-3 times to obtain pretreated particles; S4: Mix the pretreated particles with the added particles, organic anhydride and coupling agent and add them to deionized water, raise the temperature to 60-65°C, keep the temperature for reaction for 2.5-3h, then transfer to a high-temperature reactor, control the pressure to 2-2.2MPa, raise the temperature to 190-210°C, stir at 120-160rpm and keep the temperature for reaction for 16-19h, naturally cool to 60-70°C after the reaction is completed, add triethanolamine to adjust the pH to 9.5-10, add tetraethyl orthosilicate and isopropanol, keep the temperature for reaction for 2-3h, after completion, centrifuge and filter the product, wash with ethanol for 2-3 times, and dry under vacuum at 70-80°C to obtain the product; The A-site material is at least one of CsBr, RbBr, MAI, and FAI; The B site material is at least one of PbBr2, SnBr2, and GeBr4; The mass ratio of the A site material to the B site material is (2.5-4):(5-7); The organic mixed solvent is a composition of oleylamine and n-octylamine.

2. The process for preparing the perovskite-based microcrystalline material according to claim 1, characterized in that: The mass ratio of oleylamine to n-octylamine is (1.5-2.5):(1-1.4).

3. The process for preparing the perovskite-based microcrystalline material according to claim 2, characterized in that: The size control agent is oleic acid.

4. The process for preparing the perovskite-based microcrystalline material according to claim 3, characterized in that: The mass ratio of the A site material to the size control agent is (2.5-4): (40-50); the mass ratio of the B site material to the size control agent is (5-7): (40-50).

5. The process for preparing the perovskite-based microcrystalline material according to claim 4, characterized in that: The mass ratio of the A site material to aluminum nitrate is (2.5-4):(2-2.5); the mass ratio of the B site material, terephthalic acid and hydrofluoric acid is (5-7):(3-3.8):(12-20).

6. The process for preparing the perovskite-based microcrystalline material according to claim 5, characterized in that: The average particle size of the pretreated particles is 120-200 nm.

7. The process for preparing the perovskite-based microcrystalline material according to claim 6, characterized in that: The mass ratio of the pretreated particles, the added particles, the organic anhydride and the coupling agent is (3-4): (0.6-1): (0.3-0.5): (0.1-0.15).

8. The process for preparing the perovskite-based microcrystalline material according to claim 7, characterized in that: The mass ratio of tetraethyl orthosilicate to isopropyl alcohol in the pretreated particles is (3-4): (0.2-0.5): (0.05-0.1).

9. The process for preparing the perovskite-based microcrystalline material according to claim 8, characterized in that: The added particles are any one of zinc oxide, titanium dioxide and antimony dioxide; and the average particle size of the added particles is 5 to 15 nm.

10. Application of a perovskite-based microcrystalline material obtained by the preparation process of a perovskite-based microcrystalline material according to any one of claims 1 to 9 in the fields of solar cells, sensors, electronic products, and photocatalysis.

Citation Information

Patent Citations

  • Visible light response type efficient and stable nano-CsPbBr3 / TiO2 composite photocatalyst and preparation method thereof

    CN110975894A

  • Preparation method of CsPbBr3 perovskite quantum dots

    CN111534301A

  • Super-hydrophobic perovskite / silicon dioxide composite light-emitting film and preparation method and application thereof

    CN112457841A

  • Preparation and application of perovskite quantum dot MOF composite luminescent material

    CN113563869A

  • Lead halide cesium perovskite quantum dot and metal organic framework compounded shaped ultrafast scintillator and preparation method thereof

    CN113621368A