Titanium alloys for rapid solidification processing.

The Ti alloy systems TTFNZ and TIFS address rapid solidification limitations by enabling high-strength, low-density materials suitable for diverse applications with enhanced biocompatibility and corrosion resistance, supporting additive manufacturing processes.

JP7562934B2Active Publication Date: 2024-10-08OERLIKON AM GMBH
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2021560324
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-03-28
Filing Date
2020-03-27
Publication Date
2024-10-08
Estimated Expiration
2040-03-27

AI Technical Summary

Technical Problem

Rapid solidification processes in metal alloys, such as those used in powder atomization, welding, and additive manufacturing, are limited by gradient non-equilibrium phases, segregation effects, and residual stresses, restricting the selection of suitable alloys.

Method used

Development of titanium (Ti) alloy systems, specifically TTFNZ (Ti-6Ta-8Nb-4Fe-6Zr) and TIFS (Ti-5Ta-4Fe-6Sn), which exhibit remarkable rapid solidification behavior, allowing for fine-grained powders and particulate materials, and are compatible with additive manufacturing processes, with optional additions of Sn, O, C, and N to enhance properties.

Benefits of technology

The Ti alloy systems demonstrate high compatibility with additive manufacturing, reducing cracks and enabling production of high-strength, low-density materials suitable for aerospace, automotive, and medical applications, with improved biocompatibility and corrosion resistance, and facilitate cost-effective laser-based manufacturing.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007562934000003
    Figure 0007562934000003
  • Figure 0007562934000004
    Figure 0007562934000004
  • Figure 0007562934000005
    Figure 0007562934000005
Patent Text Reader

Abstract

The present invention relates to an additive manufacturing method for the production of a component, the method comprising the steps of: (a) providing and melting a metal-based powder; (b) forming a fused material by fusing the fused particles with each other and with their subsurfaces; and (c) solidifying the fused material by cooling, wherein the metal-based powder is a Ti-based powder containing at least Ta, Fe, and i) Sn and / or ii) Nb and Zr.
Need to check novelty before this filing date? Find Prior Art

Description

Summary of the Invention

[0001] Rapid solidification of molten metal (△T=10~10 10 Rapid solidification (K / s) occurs in many technological processes such as powder atomization, welding, additive manufacturing (AM), casting, arc or plasma melting. Gradients lead to non-equilibrium phases, segregation effects and residual stresses, limiting the choice of processable alloys. It is therefore an object of the present invention to disclose two alloy systems that show surprisingly remarkable and rapid solidification behavior. [Brief description of the drawings]

[0002] [Figure 1] TTFNZ Ti-6Ta-8Nb-4Fe-6Zr (thermodynamic equilibrium). [Diagram 2] TTFS (thermodynamic equilibrium) is shown. [Diagram 3] The microstructure of TTFNZ after NADFAM / AM conditions is shown. [Figure 4] The ultrastructure of TTFS after NADFAM / AM conditions is shown. [Diagram 5] The microstructure of TTFNZ after arc-melting conditions is shown. [Figure 6] The microstructure of TTFS after arc-melting conditions is shown. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0003] Some applications require fine-grain powders (<1 mm). Other applications require granular materials (particle size ≧1 mm). This may even result in bulky articles. All of these are powders within the meaning of this specification.

[0004] The metal systems which the inventors have found to exhibit the best properties in terms of rapid solidification processability are titanium (Ti) + tantalum (Ta) + iron (Fe) + niobium (Nb) + zirconium (Zr) and Ti + Ta + Fe + tin (Sn).

[0005] Hereafter, these will be abbreviated as TTFNZ and TIFS. [Table 1]

[0006] TTFNZ optionally contains only Sn. [Table 2]

[0007] The thermodynamic equilibrium of TTFNZ and TTFS is shown in Figures 1, 1b, 2, and 2b. The α / β microstructure and phase composition of TTFNZ and TTFS after a rapid solidification process (similar to 3D printing) are shown in Figures 3, 3b, 4, and 4b. The β-dominant microstructure of TTFNZ and TTFS after the arc-melted state is shown in Figures 5 and 6.

[0008] The thermodynamic equilibrium of TTFNZ is shown in Figures 1 and 1b. The α / β microstructure of the alloy was confirmed using Electron Backscatter Detector (EBSD) analysis for various conditions after rapid solidification (non-equilibrium) and / or finally with heat treatment to achieve a near-equilibrium microstructure. The various microstructures produced by these processes are shown in Figures 2 and 2b, where heat treatment achieves a microstructure closer to the thermodynamic calculation.

[0009] This alloy exhibits high compatibility with additive manufacturing processes in the investigated processed window, which is highlighted by the absence of cracks after processing.

[0010] The graphs of the simulated thermodynamic equilibrium phases of the TTFS are shown in Figures 2 and 2b. The simulations were performed in 1 K increments. The alloy is in the liquid state at TS = 1922 K (matrix formation temperature) and transforms to a 100% phase mole fraction of the solid cubic BCC_B2 phase at TS = 1821 K. This results in an equilibrium solidification interval of approximately TLS = 101 K. After cooling to 1027 K, the hexagonal HCP phase aggregates (β-α transition temperature) and stabilizes to a 92.88% phase mole fraction at the simulation temperature of 300 K. At this temperature, the remaining phases are the rhombohedral μ phase (Fe7Ta6) with a phase mole fraction of 4.3% and the intermetallic compound FeTi (BCC_B2#2, cubic B2 type) with a solution of Ta. The precipitation of intermetallic phases such as μ phase or secondary phases such as HCP_A3 (α phase) leads to an increase in the electrical resistivity of the material. This increases the absorption of laser radiation, which can reduce production costs for laser-based manufacturing processes.

[0011] The α / β microstructure of the alloy was confirmed using electron backscatter detector (EBSD) analysis for various conditions after rapid solidification (non-equilibrium) and / or finally with heat treatment to achieve a near-equilibrium microstructure. The various microstructures produced by these processes are shown in Figure 6, where the heat treatment achieves a microstructure that is closer to the thermodynamic calculation.

[0012] This alloy exhibits high compatibility with additive manufacturing processes in the investigated processed window, which is highlighted by the absence of cracks after processing.

[0013] According to another aspect of the invention, the new material may be attractive for aerospace, automotive, tooling, or medical applications due to its high specific strength >200 kN·m / kg.

[0014] According to another aspect of the invention, the new materials may be attractive for aerospace, automotive, tooling, or medical applications due to their low density, high toughness, excellent corrosion properties, and resistance to hot or cold cracking.

[0015] The metallic systems TTFNZ and TTFS are particularly suitable for medical applications. The most common implant materials (Ti64, CoCr, 316L) [1] have a relatively low corrosion resistance, but in human body fluids they are exposed to a very aggressive environment of dissolved oxygen, chlorides and proteins that promote the release of Al-, Co-, Cr-, Ni- and V-ions into the human body. The dissolved ions can interfere with cell metabolism and cause lethal tumor diseases in minute excesses. Optimal properties in terms of wear resistance and biocompatibility are achieved for Ti, Ta, Nb, Zr and their alloys. A further important parameter of the alloys currently used in medical applications is the mismatch of elastic properties between the implant material and the hard tissue. In this regard, the presented metallic systems TTFNZ and TTFS exhibit better biocompatibility than the off-the-shelf ISO [1] and ASTM standardized alloys. In particular, due to the biocompatible alloying elements and the relatively low elastic modulus (E<100 GPa, preferably <120 GPa), the presented metal-based TTF NZ should be more suitable for clinical use than the pre-existing ISO [1] and ASTM standardized alloys. In particular, due to the biocompatible alloying elements and the relatively low elastic modulus (E<115 GPa, preferably <120 GPa), the presented metal-based TTFS should be more suitable for clinical use than the pre-existing ISO [1] and ASTM standardized alloys.

[0016] Furthermore, the general AM rapid setting process of TTFNZ and TTFS can enable a tissue engineered open porous bone mimetic lattice structure (scaffold) that is receptive to oxygenation and nutrition of bone cells, facilitating osseointegration and strong implant fixation.

[0017] According to another aspect of the present invention, for TTFS, it is considered to add tin (Sn; preferably 0.01-10 wt%) to all existing titanium alloys to improve additive (AM) processability in general, and weldability or printability (AM) in particular. Sn can reduce the high surface tension and high melting viscosity, which can cause the balling effect during rapid solidification. Specifically, Sn can simultaneously enhance the absorption of laser radiation, leading to more cost-effective titanium alloy processing.

[0018] In this case, Sn can be added to the pre-alloy powder mixture as an elemental powder, or Sn can be directly alloyed into the pre-alloy powder.

[0019] This specification has been described with a focus on powders, however, those skilled in the art will appreciate that additive manufacturing methods exist that are not based on powders but on wires or, for example, mixtures of metal powders in liquid polymers, and the materials presented herein may also be used in such methods, which are also an aspect of the present invention.

[0020] According to another aspect of the invention, it is contemplated that oxygen, O, and / or carbon, C, and / or nitrogen may be added to the TTFNZ and / or TTFS to produce a hard, wear resistant material.

[0021] The present invention provides an additive manufacturing method for the production of a component, comprising: (a) providing and melting a metal-based powder; (b) forming a fused material by fusing the molten particles with each other and with their subsurface; (c) solidifying the fusion material by cooling; Including, A process is claimed, wherein the metal based powder is a Ti based powder containing at least Ta, Fe, and i) Sn and / or ii) Nb and Zr.

[0022] Preferably, the method is characterized in that the Ti-based powder also contains Si.

[0023] Preferably, the method is characterized in that the Ti-based powder contains C and / or N and / or O.

[0024] The present invention provides a Ti-based powder for additive manufacturing, the powder comprising: Ta in the range of 0.01% to 15% by weight, preferably in the range of 3% to 10% by weight, most preferably 6% by weight; - in the range of 0.01% to 25% by weight, preferably in the range of 4% to 12% by weight, most preferably 8% by weight of Nb; Fe in the range of 0.01% to 15% by weight, preferably in the range of 2% to 6% by weight, most preferably 4% by weight, Ti-based powders containing Zr in the range of -0.01% to 25% by weight, preferably in the range of 3% to 9% by weight, and most preferably 6% by weight, are claimed.

[0025] The present invention provides a Ti-based powder for additive manufacturing, comprising: Ta in the range of 0.01% to 20% by weight, preferably in the range of 3% to 10% by weight, most preferably 7% by weight; Fe in the range of 0.01% to 15% by weight, preferably in the range of 2% to 10% by weight, most preferably 5% by weight, Sn in the range of 0.01% to 10% by weight, preferably in the range of 0.1% to 9% by weight, most preferably 3% by weight; Ti-based powders containing Si in the range of -0.001 wt.% to 3 wt.% are claimed.

[0026] Preferably, the Ti-based powder is - oxygen, preferably in the range of 0.001% to 0.3% by weight, and / or - nitrogen, preferably in the range of 0.001% to 0.2% by weight, and / or Preferably, the carbon content is in the range of 0.001% by weight to 0.9% by weight.

[0027] For some of the Ti-based powders, such as those mentioned above, the metal added to Ti leads to a more rapid solidification of the fused material compared to the solidification of Ti-based powders containing only Ti as the metallic element. In some of these cases, this can be explained by an increase in the melting point of the fused material compared to pure Ti. The higher the melting point, the greater the temperature gradient between the solidified melt and the surrounding medium during cooling, resulting in a faster solidification. In this context, faster means that the solidification is at least 1 K / s faster.

[0028] Main literature [1] ISO 5832, Surgical implants - Metallic materials

Claims

1. 1. An additive manufacturing method for the production of a component, comprising: (a) providing and melting a metal-based powder; (b) forming a fused material by fusing the molten particles with each other and with their subsurface; (c) solidifying the fusion material by cooling; Including, The metal-based powder is a Ti-based powder containing at least Ta, Fe, and i) Sn or ii) Nb and Zr; In case i), the powder comprises: Ta in the range of 3% to 10% by weight, Fe in the range of 2% to 10% by weight, Sn in the range of 0.1% to 9% by weight, and % Si in the range of 0.001 wt. % to 3 wt. %; Including, Ti is used as the balance of the composition; In case ii), the powder comprises: Ta in the range of 3% to 10% by weight, Fe in the range of 2% to 10% by weight, Nb in the range of 4% to 12% by weight, and Zr in the range of 3% to 9% by weight, Including, The method wherein Ti is used as the balance of the composition.

2. A Ti-based powder for additive manufacturing, said powder comprising: Ta in the range of 3% to 10% by weight, Nb in the range of 4% to 12% by weight, Fe in the range of 2% to 10% by weight, and Zr in the range of 3% to 9% by weight, Including, Ti-based powder, with Ti being used as the balance of the composition.

3. A Ti-based powder for additive manufacturing, said powder comprising: Ta in the range of 3% to 10% by weight, Fe in the range of 2% to 10% by weight, Sn in the range of 0.1% to 9% by weight, and % Si in the range of 0.001 wt. % to 3 wt. %; Including, Ti-based powder, with Ti being used as the balance of the composition.

4. The powder is Oxygen in the range of 0.001% to 0.3% by weight; Nitrogen in the range of 0.001% to 0.2% by weight, or Carbon in the range of 0.001% to 0.9% by weight; The Ti-based powder according to claim 2 or 3, comprising:

Citation Information

Patent Citations

  • Low-elastic-modulus beta type titanium alloy for dental filling and production method thereof

    CN108486408A

  • Heat resistant material of ti-al system

    JP1991257130A

  • Powdered titanium alloy composition and article formed therefrom

    JP2018115386A

  • Titanium alloys

    WO2018162919A1