Adhesive resin composition, cured adhesive resin, adhesive sheet, and image display device laminate

The adhesive resin composition with a (meth)acrylic acid ester copolymer and a photocurable compound addresses the issues of bending resistance and adhesive strength in image display devices, enhancing durability and visibility by preventing foaming and peeling.

JP7562946B2Active Publication Date: 2024-10-08MITSUBISHI CHEM CORP
View PDF 14 Cites 0 Cited by

Patent Information

Application Number
JP2019225307
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2018-12-14
Filing Date
2019-12-13
Publication Date
2024-10-08
Estimated Expiration
2039-12-13

AI Technical Summary

Technical Problem

Existing adhesive compositions for image display devices lack sufficient bending resistance, adhesive strength, and cohesive strength, especially at high and low temperatures, and are prone to foaming and peeling, which affects the visibility and durability of flexible displays.

Method used

A pressure-sensitive adhesive resin composition comprising a (meth)acrylic acid ester copolymer as the base polymer and a photocurable compound with a lower glass transition temperature than the base polymer, combined with a photoinitiator, to enhance adhesive strength and bending resistance while preventing foaming.

Benefits of technology

The composition provides excellent bending resistance, adhesive strength, and cohesive strength, reducing peeling and foaming, even at high and low temperatures, thereby improving the durability and visibility of flexible image display devices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007562946000005
    Figure 0007562946000005
  • Figure 0007562946000001
    Figure 0007562946000001
  • Figure 0007562946000002
    Figure 0007562946000002
Patent Text Reader

Abstract

To provide an adhesive resin composition which has excellent bending resistance after curing and improved adhesive force, and to provide an adhesive resin cured product, an adhesive sheet, and an image display device laminate obtained by using the adhesive resin composition.SOLUTION: The adhesive resin composition is used which contains a base polymer (A) comprising a (meth)acrylate copolymer, a photocurable compound (B), and a photoinitiator (C). A glass transition temperature (TgB) of the photocurable compound (B) after photocuring is lower than a glass transition temperature (TgA) of the base polymer (A).SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a pressure-sensitive adhesive resin composition, and a cured pressure-sensitive adhesive resin, a pressure-sensitive adhesive sheet, a laminate for an image display device, and the like, which are obtained by using the pressure-sensitive adhesive resin composition. [Background technology]

[0002] In recent years, in order to improve the visibility of image display devices, the gap between an image display panel such as an LCD (Liquid Crystal Display), PDP (Plasma Display Panel) or EL (Electro-Luminescence) panel and a protective panel or touch panel member placed on the front side (viewing side) of the image display panel has been filled with an adhesive sheet, adhesive or the like to suppress the diffuse reflection that occurs when the gap is not filled, i.e., the diffuse reflection of incident light and outgoing light from a displayed image at the air layer interface.

[0003] In this case, for example, if the protective panel is made of plastic, gas (called outgassing) may be generated from the protective panel. If the adhesive or sheet does not have sufficient adhesive strength and cohesive strength to withstand this gas pressure, the gas will remain in the adhesive or sheet and, when heated, the residual gas will foam, reducing the visibility of the screen.

[0004] In view of this, for example, Patent Document 1 proposes a pressure-sensitive adhesive sheet that can be applied in a high-temperature environment of about 80°C without foaming.

[0005] Furthermore, Patent Documents 2 and 3 propose a so-called post-curing adhesive sheet that combines the foaming resistance in high-temperature environments as described above with the ability to conform to the irregularities of an adherend, and that can be photo-cured after attachment to an adherend to improve cohesive strength.

[0006] Recently, flexible displays that can be bent freely have been attracting attention as the next generation of displays. Organic electroluminescence (OLED) displays are mainly used for flexible displays.

[0007] Since flexible displays use thin, flexible glass or plastic substrates, the double-sided pressure-sensitive adhesive sheets used to bond these components of the image display device must not only have the optical properties and durability required for conventional flat display panels, but also must not break, peel, or float when subjected to bending tests.

[0008] For example, Patent Document 4 proposes a pressure-sensitive adhesive for optical films that does not peel off or float even when a laminated film is held in a deformed state for a long period of time or when a bending test is performed, the pressure-sensitive adhesive for optical films containing a (meth)acrylic acid ester copolymer (A) having a glass transition temperature of -70 to -55°C and a mass average molecular weight of more than 1 million to 2.5 million, which is obtained by polymerizing (a1) 10 to 95 mass% of structural units derived from alkyl (meth)acrylic acid ester monomers, (a2) 5 to 90 mass% of structural units derived from (meth)acrylic acid ester monomers having an alkoxyalkyl group or an alkylene oxide group, and (a3) ​​0 to 20 mass% of structural units derived from a functional group-containing monomer that is a (meth)acrylic acid ester monomer not having a plurality of radically polymerizable functional groups.

[0009] Furthermore, Patent Document 5 proposes an adhesive sheet for use in a flexible optical display device, which contains a (meth)acrylic copolymer having a hydroxyl group formed from a monomer mixture including a hydroxyl group-containing (meth)acrylate and an alkyl group-containing (meth)acrylate, and has a glass transition temperature of -35°C or lower.

[0010] In addition, Patent Document 6 proposes a pressure-sensitive adhesive composition that does not peel off or lift even when subjected to bending operations under both high and low temperature conditions, the pressure-sensitive adhesive composition comprising a base agent (A) made of a curable compound, a crosslinking agent (B) and a photopolymerization initiator (C), the base agent (A) comprising at least one of a combination (a-1) of a (meth)acrylic acid ester monomer (a-1-a) and a hydroxyl group-containing (meth)acrylic monomer (a-1-b) and a copolymer (a-2) comprising a structural unit (1) derived from the (meth)acrylic acid ester monomer (a-1-a) and a structural unit (2) derived from the hydroxyl group-containing (meth)acrylic monomer (a-1-b), the crosslinking agent (B) being an acrylic polymer having a urethane acrylate in the side chain, and having a glass transition temperature after curing of -57.5°C or lower. [Prior art documents] [Patent documents]

[0011] [Patent Document 1] International Publication No. 2010 / 044229 [Patent Document 2] International Publication No. 2012 / 032995 [Patent Document 3] International Publication No. 2013 / 108565 [Patent Document 4] JP 2016-108555 A [Patent Document 5] US Patent Application Publication No. 2017 / 0306194 [Patent Document 6] International Publication No. 2017 / 116079 Summary of the Invention [Problem to be solved by the invention]

[0012] As described above, in Patent Documents 4 to 6, in order to impart sufficient flexibility to the cured product of the pressure-sensitive adhesive composition at low temperatures and to obtain folding resistance at low temperatures, a base polymer having a low glass transition temperature is used, thereby endowing the pressure-sensitive adhesive sheet with bending resistance at both high and low temperatures.

[0013] However, a base polymer having a low glass transition temperature is insufficient in adhesive strength and cohesive strength, and is also poor in resistance to whitening due to humidity and heat.

[0014] Therefore, an object of the present invention is to provide an adhesive resin composition having excellent flex resistance after curing and improved adhesive strength, as well as a cured adhesive resin, an adhesive sheet, and an image display device laminate obtained using the adhesive resin composition. [Means for solving the problem]

[0015] The present invention provides a pressure-sensitive adhesive resin composition comprising a base polymer (A) made of a (meth)acrylic acid ester copolymer, a photocurable compound (B), and a photoinitiator (C), The present invention proposes a pressure-sensitive adhesive resin composition, characterized in that the photocurable compound (B) has a glass transition temperature (TgB) after photocuring that is lower than the glass transition temperature (TgA) of the base polymer (A).

[0016] The present invention also provides a pressure-sensitive adhesive resin composition comprising a base polymer (A) made of a (meth)acrylic acid ester copolymer, a photocurable compound (B), and a photoinitiator (C), The present invention proposes a pressure-sensitive adhesive resin composition, characterized in that the photocurable compound (B) is a (meth)acrylate (b-1) having a glycol skeleton.

[0017] The present invention also provides a pressure-sensitive adhesive sheet having a pressure-sensitive adhesive layer formed from the pressure-sensitive adhesive resin composition, together with a cured pressure-sensitive adhesive resin obtained by curing the pressure-sensitive adhesive resin composition.

[0018] The present invention also provides a display device having a configuration in which two components for an image display device are laminated via a pressure-sensitive adhesive layer made of a cured pressure-sensitive adhesive resin obtained by curing the pressure-sensitive adhesive resin composition or a pressure-sensitive adhesive sheet having the pressure-sensitive adhesive layer, The present invention proposes a laminate for use in constructing an image display device, characterized in that at least one of the two components for the image display device is any member selected from the group consisting of a polarizing plate, a polarizing film, a retardation film, an image display panel, an organic EL display panel, a plasma display panel, a touch panel, a protective panel, and a touch sensor. Effect of the Invention

[0019] The pressure-sensitive adhesive resin composition proposed by the present invention comprises a base polymer (A) and a photocurable compound (B), and the glass transition temperature (TgB) of the photocurable compound (B) after photocuring is higher than that of the base polymer (A). Glass transition temperature (TgA) That is, the design is such that a photocurable compound (B) with a low glass transition temperature is added to a base polymer (A) with a high cohesive strength, and the composition can have both bending resistance and adhesiveness (cohesive strength) resistant to peeling and foaming. In this case, even when the photocurable compound (B) is a (meth)acrylate (b-1) having a glycol skeleton, the composition can have both bending resistance and adhesiveness (cohesive strength) resistant to peeling and foaming. Furthermore, since the flexibility of the adhesive resin composition proposed by the present invention can be controlled by the photocurable compound (B) having a low glass transition temperature, the base polymer (A) can relatively reduce the amount of low Tg components required to ensure flexibility (flexibility) and can contain a large amount of polarizable components (hydrophilic components), which has the advantage of improving the wet heat whitening property. Furthermore, since the base polymer (A) can exhibit resistance to wet heat whitening and adhesiveness (cohesive strength) using polar components (hydrophilic components) other than acid components, there is no need to contain acid components that cause corrosion, which has the advantage of providing corrosion resistance. [Brief description of the drawings]

[0020] [Figure 1] FIG. 1 is a diagram for explaining the evaluation test methods for ITO corrosion resistance reliability and Cu corrosion resistance reliability performed in the examples described below, in which FIG. 1(A) is a top view of an ITO pattern on an ITO glass substrate, FIG. 1(B) is a top view showing an adhesive sheet covered on an ITO glass substrate for evaluating ITO corrosion resistance reliability or a top view showing an adhesive sheet covered on a copper glass substrate for evaluating Cu corrosion resistance reliability, and FIG. 1(C) is a cross-sectional view of a sample for evaluating ITO corrosion resistance reliability. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0021] Next, the present invention will be described based on an embodiment, however, the present invention is not limited to the embodiment described below.

[0022] <<The resin composition>> An adhesive resin composition according to one embodiment of the present invention (hereinafter referred to as "the resin composition") contains a base polymer (A) made of a (meth)acrylic acid ester copolymer, a photocurable compound (B), and a photoinitiator (C).

[0023] In the present invention, "(meth)acrylic" encompasses acrylic and methacrylic, "(meth)acryloyl" encompasses acryloyl and methacryloyl, and "(meth)acrylate" encompasses acrylate and methacrylate. Furthermore, the term "base polymer" refers to the resin that is contained in the largest amount of the resin components contained in the resin composition, and preferably refers to a resin that is contained in more than 50 mass % of the resin components contained in the resin composition.

[0024] Furthermore, in the present invention, "flexibility" means durability against repeated bending (folding) tests and durability when maintaining a bent state, and specifically means durability against a bending test evaluated in accordance with the method described in the examples below. Moreover, the term "flexible" means that it is capable of being bent or curved, and the term "able to bend or curve" includes the state of being bent or curved. Therefore, specifically, the flexible member is preferably one that can be bent or curved with a radius of curvature of 10 mm or less, and more preferably one that has a radius of curvature of 3 mm or less.

[0025] <(Meth)acrylic acid ester copolymer> The (meth)acrylic acid ester copolymer preferably has a glass transition temperature (TgA) of -30°C or higher. When the glass transition temperature (TgA) of the base polymer is −30° C. or higher, the adhesive strength and cohesive strength of the present resin composition and the pressure-sensitive adhesive sheet formed therefrom can be increased. Therefore, the glass transition temperature (TgA) of the (meth)acrylic acid ester copolymer is preferably −30° C. or higher, and more preferably −20° C. or higher. The upper limit of the glass transition temperature (TgA) of the (meth)acrylic acid ester copolymer is -10°C or lower, taking practicality into consideration.

[0026] In the present invention, the glass transition temperature (Tg) refers to a glass transition temperature defined as the temperature at which the loss tangent (Tan δ) obtained by dynamic viscoelasticity measurement reaches a peak value. The glass transition temperature is measured in accordance with the method described in the Examples below.

[0027] The (meth)acrylic acid ester copolymer preferably contains 50% by mass or more of a structural unit represented by the following formula 2 (wherein R1 represents a hydrogen atom or a methyl group, and R2 represents a linear or branched alkyl group having 4 to 18 carbon atoms), i.e., monomer component (a), and more preferably contains 55% by mass or more or 95% by mass or less, and even more preferably contains 60% by mass or more or 90% by mass or less.

[0028] [ka]

[0029] Examples of the monomer (a) represented by the formula 2 include n-butyl (meth)acrylate, isobutyl (meth)acrylate, sec-butyl (meth)acrylate, t-butyl (meth)acrylate, pentyl (meth)acrylate, isopentyl (meth)acrylate, neopentyl (meth)acrylate, hexyl (meth)acrylate, cyclohexyl (meth)acrylate, heptyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, 2-ethylhexyl EO-modified (meth)acrylate, n-octyl (meth)acrylate, isooctyl (meth)acrylate, nonyl (meth)acrylate, isononyl (meth)acrylate, Examples of such acrylates include tert-butylcyclohexyl (meth)acrylate, decyl (meth)acrylate, isodecyl (meth)acrylate, undecyl (meth)acrylate, lauryl (meth)acrylate, tridecyl (meth)acrylate, tetradecyl (meth)acrylate, cetyl (meth)acrylate, stearyl (meth)acrylate, isostearyl (meth)acrylate, isobornyl (meth)acrylate, 3,5,5-trimethylcyclohexane (meth)acrylate, dicyclopentanyl (meth)acrylate, dicyclopentenyl (meth)acrylate, dicyclopentenyloxyethyl (meth)acrylate, etc. These may be used alone or in combination of two or more.

[0030] The (meth)acrylic copolymer preferably contains a structural unit derived from an "other monomer" other than the monomer (a). Here, the term "structural unit derived from a monomer" refers to a structural unit resulting from a copolymerization reaction of the monomer, that is, a unit that constitutes a copolymer. The "other monomer" is preferably contained in the (meth)acrylic copolymer (A) in a proportion of 1 to 30 mass %, more preferably 5 mass % or more or 25 mass % or less.

[0031] Examples of the "other monomer" include (i) a hydroxyl group-containing monomer (hereinafter also referred to as "monomer (a-1)"); (ii) a carboxyl group-containing monomer (hereinafter also referred to as "monomer (a-2)"); (iii) an amino group-containing monomer (hereinafter also referred to as "monomer (a-3)"); (iv) an epoxy group-containing monomer (hereinafter also referred to as "monomer (a-4)"); (v) an amide group-containing monomer (hereinafter also referred to as "monomer (a-5)"); (v Examples of such monomers include i) vinyl group-containing monomers (hereinafter also referred to as "monomer (a-6)"); (vii) (meth)acrylate monomers having 1 to 3 carbon atoms in the side chain (hereinafter also referred to as "monomer (a-7)"); (viii) macromonomers (hereinafter also referred to as "monomer (a-8)"); (ix) aromatic group-containing monomers (hereinafter also referred to as "monomer (a-9)"); and (x) other functional group-containing monomers (hereinafter also referred to as "monomer (a-10)". These monomers may be used alone or in combination of two or more.

[0032] Examples of the monomer (a-1) include hydroxyl group-containing monomers such as hydroxyalkyl (meth)acrylates, such as 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate, etc. These may be used alone or in combination of two or more.

[0033] Examples of the monomer (a-2) include carboxyl group-containing monomers such as (meth)acrylic acid, carboxyethyl (meth)acrylate, carboxypropyl (meth)acrylate, carboxybutyl (meth)acrylate, ω-carboxypolycaprolactone mono(meth)acrylate, 2-(meth)acryloyloxyethylhexahydrophthalic acid, 2-(meth)acryloyloxypropylhexahydrophthalic acid, 2-(meth)acryloyloxyethylphthalic acid, 2-(meth)acryloyloxypropylphthalic acid, 2-(meth)acryloyloxyethylmaleic acid, 2-(meth)acryloyloxypropylmaleic acid, 2-(meth)acryloyloxyethylsuccinic acid, 2-(meth)acryloyloxypropylsuccinic acid, crotonic acid, fumaric acid, maleic acid, and itaconic acid. These may be used alone or in combination of two or more.

[0034] Examples of the monomer (a-3) include amino group-containing monomers such as aminoalkyl (meth)acrylates, such as aminomethyl (meth)acrylate, aminoethyl (meth)acrylate, aminopropyl (meth)acrylate, and aminoisopropyl (meth)acrylate, and N,N-dialkylaminoalkyl (meth)acrylates, such as N,N-dimethylaminoethyl (meth)acrylate and N,N-dimethylaminopropyl (meth)acrylate. These may be used alone or in combination of two or more.

[0035] Examples of the monomer (a-4) include epoxy group-containing monomers such as glycidyl (meth)acrylate, methyl glycidyl (meth)acrylate, 3,4-epoxycyclohexylmethyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate glycidyl ether, etc. These may be used alone or in combination of two or more.

[0036] Examples of the monomer (a-5) include amide group-containing monomers such as (meth)acrylamide, N,N-dimethyl(meth)acrylamide, N-butyl(meth)acrylamide, N-methylol(meth)acrylamide, N-methylolpropane(meth)acrylamide, N-methoxymethyl(meth)acrylamide, N-butoxymethyl(meth)acrylamide, diacetone(meth)acrylamide, maleic acid amide, maleimide, etc. These may be used alone or in combination of two or more.

[0037] Examples of the monomer (a-6) include compounds having a vinyl group in the molecule. Examples of such compounds include (meth)acrylic acid alkyl esters having an alkyl group with 1 to 12 carbon atoms, functional monomers having functional groups such as a hydroxyl group, an amide group, and an alkoxyl alkyl group in the molecule, polyalkylene glycol di(meth)acrylates, vinyl acetate, N-vinyl-2-pyrrolidone, vinyl propionate, vinyl laurate, and other vinyl ester monomers, as well as styrene, chlorostyrene, chloromethylstyrene, α-methylstyrene, and other substituted styrenes, and other vinyl group-containing monomers. These may be used alone or in combination of two or more.

[0038] Examples of the monomer (a-7) include (meth)acrylate monomers having 1 to 3 carbon atoms in the side chain, such as methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, i-propyl (meth)acrylate, etc. These may be used alone or in combination of two or more.

[0039] The macromonomer as the monomer (a-8) is a polymer monomer having a terminal functional group and a high molecular weight skeleton component, and is preferably a monomer having 20 or more carbon atoms in the side chain when polymerized into a (meth)acrylic acid ester copolymer.

[0040] By using the monomer (a-8), a macromonomer can be introduced as a branch component of the graft copolymer, and the (meth)acrylic acid ester copolymer can be made into a graft copolymer. For example, a (meth)acrylic acid ester copolymer (a) consisting of a graft copolymer having a macromonomer as a branch component can be obtained. Therefore, the properties of the main chain and side chains of the graft copolymer can be changed by selecting and mixing the monomer (a-8) and other monomers.

[0041] The backbone component of the macromonomer is preferably composed of an acrylic acid ester polymer or a vinyl polymer, for example, the linear or branched alkyl (meth)acrylate having 4 to 18 carbon atoms in the side chain, the monomer (a-1), the monomer (a-2), the monomer (a-7), etc., which may be used alone or in combination of two or more kinds.

[0042] Examples of the monomer (a-9) include aromatic-containing monomers such as benzyl (meth)acrylate, phenoxyethyl (meth)acrylate, 2-hydroxy-3-phenoxypropyl (meth)acrylate, nonylphenol EO-modified (meth)acrylate, etc. These may be used alone or in combination of two or more.

[0043] Examples of the monomer (a-10) include functional group-containing monomers such as (meth)acrylic modified silicones, 2,2,2-trifluoroethyl (meth)acrylate, 2,2,3,3-tetrafluoropropyl (meth)acrylate, 2,2,3,3-tetrafluoropropyl (meth)acrylate, 1H,1H,5H-octafluoropentyl (meth)acrylate, 1H,1H,2H,2H-tridecafluoro-n-octyl (meth)acrylate, etc. These may be used alone or in combination of two or more.

[0044] Among the above, the (meth)acrylic acid ester copolymer is preferably one containing a structural unit derived from the monomer (a-1) from the viewpoint of improving the wet heat whitening property. As described above, the term "structural unit derived from monomer (a-1)" refers to a structural unit resulting from a copolymerization reaction of said monomer (a-1), that is, a unit that constitutes a copolymer.

[0045] On the other hand, from the viewpoint of metal corrosion resistance, it is preferable that the (meth)acrylic acid ester copolymer does not contain any structural unit derived from the monomer (a-2), that is, a carboxyl group-containing monomer. In this case, "not containing any structural units derived from monomer (a-2)" means "not containing substantially any structural units," and it does not only mean that the (meth)acrylic acid ester copolymer is completely free of structural units derived from monomer (a-2), but also means that the (meth)acrylic acid ester copolymer may contain only a small amount of structural units derived from monomer (a-2), i.e., less than 0.5% by mass, preferably less than 0.1% by mass.

[0046] In view of the above, it is preferable that the (meth)acrylic acid ester copolymer contains a structural unit derived from the monomer (a) represented by the above formula 2 and a structural unit derived from the monomer (a-1), but does not contain a structural unit derived from the monomer (a-2) (referred to as "preferred form 1 of the base polymer"). In this case, the content of the structural unit derived from the monomer (a-1) in the (meth)acrylic acid ester copolymer is preferably 5 to 30 mass%, more preferably 7 mass% or more or 28 mass% or less, and even more preferably 10 mass% or more or 25 mass% or less.

[0047] In particular, it is preferred that the (meth)acrylic acid ester copolymer contains a structural unit derived from the monomer (a) represented by the above formula 2, a structural unit derived from the monomer (a-1), and a structural unit derived from the monomer (a-5), but does not contain a structural unit derived from the monomer (a-2) (referred to as "preferred form 2 of the base polymer"). Furthermore, it is preferable that the (meth)acrylic acid ester copolymer contains a structural unit derived from the monomer (a) represented by the above formula 2, a structural unit derived from the monomer (a-1), a structural unit derived from the monomer (a-5), and a structural unit derived from the monomer (a-7), but does not contain a structural unit derived from the monomer (a-2) (referred to as "preferred form 3 of the base polymer").

[0048] In each of the preferred embodiments 1 to 3 of the base polymer, the monomer (a) preferably includes at least one selected from the group consisting of 2-ethylhexyl (meth)acrylate, lauryl (meth)acrylate, isostearyl (meth)acrylate, and isobornyl (meth)acrylate.

[0049] <Photocurable compound (B)> The photocurable compound (B) is a compound that has the property of being cured by irradiation with light, and is preferably a compound whose glass transition temperature (TgB) after photocuring is lower than the glass transition temperature (TgA) of the base polymer (A). By blending a compound having a lower glass transition temperature (TgA) than the base polymer (A), the glass transition temperature of the resin composition can be lowered, and the flexibility at low temperatures (e.g., −30° C.) can be increased, thereby making the folding resistance at said temperatures excellent.

[0050] Furthermore, the photocurable compound (B) preferably has a glass transition temperature (TgB) after photocuring of -40°C or lower, more preferably -45°C or lower. When the photocurable compound (B) has a glass transition temperature in this range, the glass transition temperature (TgA) of the base polymer (A) can be set relatively high, making it possible to obtain a pressure-sensitive adhesive sheet that ensures adhesion while also imparting flexibility to withstand buckling during bending deformation and thus has bending resistance.

[0051] In the present invention, the term "photocurable" means reactivity (curability) to radiation in general. Specifically, it means having a property of being cured by light having a wavelength in the range of 200 nm to 780 nm, and is preferably used to mean having reactivity (curability) to ultraviolet light in particular.

[0052] The glass transition temperature (TgB) of the photocurable compound (B) after photocuring is determined by adding 1 part by mass of a photoinitiator to 100 parts by mass of the compound (B) to form the present resin composition, and the integrated light intensity at a wavelength of 365 nm is 3,000 mJ / cm. 2 This refers to the glass transition temperature of the photocurable compound (B) after the photocurable compound (B) is cured by irradiation with ultraviolet light so as to satisfy the following condition.

[0053] From the viewpoint of forming a crosslinked structure, the photocurable compound (B) is preferably a compound having one or more ethylenically unsaturated groups in the molecule.

[0054] Among the above, the photocurable compound (B) is preferably a (meth)acrylate (b-1) having a glycol skeleton. The (meth)acrylate (b-1) having the glycol skeleton can easily have a low glass transition temperature (TgB) after photocuring, and flexibility can be imparted by adjusting the molecular weight of the skeleton component.

[0055] Examples of the glycol skeleton include an ethylene glycol skeleton, a propylene glycol skeleton, a diethylene glycol skeleton, a butanediol skeleton, a hexanediol skeleton, a 1,4-cyclohexanedimethanol skeleton, a glycolic acid skeleton, a polyglycolic acid skeleton, etc. Among these, a polyethylene glycol skeleton and / or a polypropylene glycol skeleton is more preferable.

[0056] The (meth)acrylate (b-1) having a glycol skeleton more preferably has two or more peaks in the loss tangent (Tan δ) obtained by dynamic viscoelasticity measurement. More specifically, there can be mentioned a photocurable compound having a peak (b1) derived from the polymerization of a terminal (meth)acryloyl group and a peak (b2) derived from a glycol skeleton. In this case, the peak temperature of the peak (b1) is preferably -40°C or lower, more preferably -65°C or higher or -45°C or lower, more preferably -60°C or higher or -50°C or lower, and the peak temperature of the peak (b2) is preferably 0°C or lower, more preferably -50°C or higher or -5°C or lower, more preferably -45°C or higher or -10°C or lower. In this way, when the photocurable compound (B) has two peak temperatures of the loss tangent (Tan δ) of dynamic viscoelasticity, the TgB of the compound (B) can be lowered.

[0057] Furthermore, the (meth)acrylate (b-1) having a glycol skeleton is preferably a (meth)acrylate having a mass average molecular weight (Mw) of 5,000 or more, more preferably 7,000 or more, and even more preferably 9,000 or more. In particular, a urethane (meth)acrylate having a glycol skeleton and a mass average molecular weight of 5,000 or more, more preferably 7,000 or more, and even more preferably 9,000 or more is preferred. If the photocurable compound (B) is a urethane (meth)acrylate having such a glycol skeleton, the linear structure is bonded for a long period, and therefore, by having such a glycol skeleton, the glass transition temperature of the resin composition can be more effectively lowered and good wettability and high flexibility can be imparted to the adherend. Examples of the urethane (meth)acrylate having a glycol skeleton include urethane acrylate containing a polytetramethylene glycol skeleton, urethane acrylate containing a polypropylene glycol skeleton, and urethane acrylate containing a polyethylene glycol skeleton.

[0058] From the viewpoint of imparting high flexibility, the photocurable compound (B) is preferably a monofunctional urethane acrylate oligomer represented by the following formula 1. Among them, a monofunctional urethane acrylate oligomer having a polypropylene glycol skeleton represented by the following formula 1 is most preferable.

[0059] [ka]

[0060] In the formula 1, R1 is a hydrogen atom or a methyl group, X is a urethane bond, R2 and R3 each represent an alkylene group, and R4 represents an alkyl group. , where n is an integer of 2 or greater.

[0061] The photocurable compound (B) is preferably contained in a proportion of more than 15 parts by mass and less than 75 parts by mass per 100 parts by mass of the base polymer (A). By containing the photocurable compound (B) in such a proportion, the pressure-sensitive adhesive sheet formed from the resin composition can have a good balance between adhesive strength and bending resistance. From this viewpoint, the photocurable compound (B) is preferably contained in an amount of more than 15 parts by mass and less than 75 parts by mass per 100 parts by mass of the base polymer (A), more preferably 20 parts by mass or more or 70 parts by mass or less, and even more preferably 30 parts by mass or more or 65 parts by mass or less.

[0062] <Photoinitiator (C)> A preferred example of the photoinitiator (C) is a compound that generates active radical species when irradiated with light such as ultraviolet light or visible light, more specifically, light with a wavelength of 200 nm to 780 nm. As the photoinitiator (C), either a cleavage type photoinitiator (C-1) or a hydrogen abstraction type initiator (C-2) can be used, and both can also be used in combination.

[0063] Examples of the cleavage-type photoinitiator (C-1) include 2,2-dimethoxy-1,2-diphenylethan-1-one, 1-hydroxycyclohexyl phenyl ketone, 2-hydroxy-2-methyl-1-phenyl-propan-1-one, 1-(4-(2-hydroxyethoxy)phenyl)-2-hydroxy-2-methyl-1-propan-1-one, 2-hydroxy-1-[4-{4-(2-hydroxy-2-methyl-propionyl)benzyl}phenyl]-2-methyl-propan-1-one, oligo(2-hydroxy-2-methyl-1-(4-(1-methylvinyl)phenyl)propanone), methyl phenylglyoxylate, 2-benzyl-2-dimethylamino-1-propanone, and the like. -(4-morpholinophenyl)butan-1-one, 2-methyl-1-[4-(methylthio)phenyl]-2-morpholinopropan-1-one, 2-(dimethylamino)-2-[(4-methylphenyl)methyl]-1-[4-(4-morpholinyl)phenyl]-1-butanone, bis(2,4,6-trimethylbenzoyl)-phenylphosphine oxide, 2,4,6-trimethylbenzoyldiphenylphosphine oxide, (2,4,6-trimethylbenzoyl)ethoxyphenylphosphine oxide, bis(2,6-dimethoxybenzoyl)2,4,4-trimethylpentylphosphine oxide, or derivatives thereof can be mentioned. The use of the cleavage-type photoinitiator (C-1) is preferable because the photoinitiator undergoes a structural change and becomes inactive after completion of the photoreaction, and therefore does not remain as an active species in the present resin composition after completion of the curing reaction, and there is no risk of causing unexpected photodegradation or the like in the present resin composition.

[0064] Examples of the hydrogen abstraction type photoinitiator (C-2) include benzophenone, 4-methyl-benzophenone, 2,4,6-trimethylbenzophenone, 4-phenylbenzophenone, 3,3'-dimethyl-4-methoxybenzophenone, 4-(meth)acryloyloxybenzophenone, 2-benzoylmethylbenzoate, benzoylmethylformate, bis(2-phenyl-2-oxoacetate)oxybisethylene, 4-(1,3-acryloyl-1,4,7,10,13-pentaoxotridecyl)benzophenone, thioxanthone, 2-chlorothioxanthone, 3-methylthioxanthone, 2,4-dimethylthioxanthone, 2-methylanthraquinone, 2-ethylanthraquinone, 2-tert-butylanthraquinone, 2-aminoanthraquinone, and derivatives thereof.

[0065] Use of the hydrogen abstraction type photoinitiator (C-2) is preferable because the photoinitiator can undergo a hydrogen abstraction reaction from the base polymer (A) as well, and therefore, in the cured resin composition, a network structure can be formed in which not only the photocurable compound (B) but also the base polymer (A) is incorporated into the crosslinked structure. In addition, the hydrogen abstraction type photoinitiator (C-2) can repeatedly function as an active species by irradiating light again even after it has been used once in a photocuring reaction. Therefore, when the present resin is used as a so-called post-cure type, which will be described later, it is preferable in that it can serve as the starting point of the photoreaction during post-curing.

[0066] The lower limit of the content of the initiator (C) is preferably 0.01 part by mass or more, more preferably 0.03 part by mass or more, and most preferably 0.05 part by mass or more, per 100 parts by mass of the base polymer (A). The upper limit is preferably 5 parts by mass or less, more preferably 3 parts by mass or less, and most preferably 2 parts by mass or less, per 100 parts by mass of the base polymer (A).

[0067] <Other ingredients> The resin composition may contain, in addition to the base polymer (A), the photocurable compound (B), and the photoinitiator (C), one or more of a crosslinking agent (D), a rust inhibitor (E), and a silane coupling agent (F) as necessary. In addition to the above, various additives such as a tackifier resin, an antioxidant, a light stabilizer, a metal deactivator, an anti-aging agent, a moisture absorbent, a polymerization inhibitor, an ultraviolet absorber, and inorganic particles can be appropriately contained as needed.

[0068] (Crosslinking agent (D)) In the present resin composition, the crosslinking agent (D) is an optional component that may be contained as necessary. While the present resin composition can be made to not contain the crosslinking agent (D), from the viewpoint of obtaining high foaming resistance reliability after curing, it is preferable to use the present resin composition containing the crosslinking agent (D) for curing, and among them, it is particularly preferable to use the polyfunctional (meth)acrylate (d-1) described later as the crosslinking agent (D).

[0069] Examples of the crosslinking agent (D) include, in addition to polyfunctional monomers, isocyanate compounds such as 2,4-tolylene diisocyanate, 2,6-tolylene diisocyanate, hydrogenated tolylene diisocyanate, 1,3-xylylene diisocyanate, 1,4-xylylene diisocyanate, hexamethylene diisocyanate, diphenylmethane-4,4-diisocyanate, isophorone diisocyanate, 1,3-bis(isocyanatomethyl)cyclohexane, tetramethylxylylene diisocyanate, 1,5-naphthalene diisocyanate, and triphenylmethane triisocyanate; Examples of the crosslinking agent include adducts of these isocyanate compounds with polyol compounds such as trimethylolpropane, biuret compounds and isocyanurates of these polyisocyanate compounds, epoxy crosslinking agents such as polyethylene glycol diglycidyl ether, diglycidyl ether, and trimethylolpropane triglycidyl ether, melamine resin crosslinking agents, aziridine crosslinking agents, oxazoline crosslinking agents, urea crosslinking agents, metal salt crosslinking agents, metal chelate crosslinking agents, amino resin crosslinking agents, metal alkoxide crosslinking agents, and peroxide crosslinking agents. These crosslinking agents (D) can be used alone or in combination of two or more.

[0070] Furthermore, a (meth)acrylate monomer having an organic functional group such as a glycidyl group, a hydroxyl group, or an isocyanate group may be used to allow crosslinked structures to coexist due to different crosslinkable reactive groups.

[0071] Among these, the polyfunctional monomer (d-1) is preferred. Examples of the polyfunctional monomer (d-1) include 1,4-butanediol di(meth)acrylate, glycerin di(meth)acrylate, neopentyl glycol di(meth)acrylate, glycerin glycidyl ether di(meth)acrylate, 1,6-hexanediol di(meth)acrylate, 1,9-Nonanediol di(meth)acrylate, tricyclodecane dimethacrylate, tricyclodecane dimethanol di(meth)acrylate, bisphenol A polyethoxy di(meth)acrylate, bisphenol A polypropoxy di(meth)acrylate, bisphenol F polyethoxy di(meth)acrylate, ethylene glycol di(meth)acrylate, neopentyl glycol di(meth)acrylate, trimethylolpropane trioxyethyl (meth)acrylate, ε- Caprolactone-modified tris(2-hydroxyethyl)isocyanurate tri(meth)acrylate, pentaerythritol tri(meth)acrylate, propoxylated pentaerythritol tri(meth)acrylate, ethoxylated pentaerythritol tri(meth)acrylate, pentaerythritol tetra(meth)acrylate, propoxylated pentaerythritol tetra(meth)acrylate, ethoxylated pentaerythritol tetra(meth)acrylate, dipentaerythritol Examples of the ultraviolet-curable polyfunctional (meth)acrylic monomers include xa(meth)acrylate, polyethylene glycol di(meth)acrylate, tris(acryloxyethyl)isocyanurate, dipentaerythritol hexa(meth)acrylate, dipentaerythritol penta(meth)acrylate, tripentaerythritol hexa(meth)acrylate, tripentaerythritol penta(meth)acrylate, hydroxypivalic acid neopentyl glycol di(meth)acrylate, di(meth)acrylate of an ε-caprolactone adduct of hydroxypivalic acid neopentyl glycol, trimethylolpropane tri(meth)acrylate, trimethylolpropane polyethoxy tri(meth)acrylate, and ditrimethylolpropane tetra(meth)acrylate, as well as polyfunctional (meth)acrylic oligomers such as polyester(meth)acrylate, epoxy(meth)acrylate, urethane(meth)acrylate, and polyether(meth)acrylate. These may be used alone or in combination of two or more.

[0072] The content of the crosslinking agent (D) is preferably 10 parts by mass or less per 100 parts by mass of the base polymer (A), more preferably 0.05 parts by mass or more or 5 parts by mass or less, and even more preferably 0.1 parts by mass or more or 3 parts by mass or less.

[0073] (Rust inhibitor (E)) The present resin composition may contain a rust inhibitor (E) as required in order to enhance the property of not promoting metal corrosion.

[0074] The rust inhibitor (E) is preferably a triazole-based compound, and particularly preferably one or a mixture of two or more selected from benzotriazole, 1,2,3-triazole, and 1,2,4-triazole.

[0075] The benzotriazole may be any of substituted or unsubstituted benzotriazole, and examples thereof include alkylbenzotriazoles such as 1,2,3-benzotriazole and methyl-1H-benzotriazole, carboxybenzotriazole, 1-hydroxybenzotriazole, 5-aminobenzotriazole, 5-phenylthiolbenzotriazole, 5-methoxybenzotriazole, nitrobenzotriazole, chlorobenzotriazole, bromobenzotriazole, and fluorobenzotriazole, as well as halogenobenzotriazoles such as copper benzotriazole, silver benzotriazole, and benzotriazole silane compounds. Among these, from the viewpoints of dispersibility and ease of addition in the resin composition, and metal corrosion prevention effect, one or a mixture of two or more selected from the group consisting of 1,2,3-benzotriazole, 1-[N,N-bis(2-ethylhexyl)aminomethyl]benzotriazole, 1-[N,N-bis(2-ethylhexyl)aminomethyl]methylbenzotriazole, and 2,2'-[[(methyl-1H-benzotriazol-1-yl)methyl]imino]bisethanol is preferred. Furthermore, 1,2,4-triazole is a solid with a melting point of about 120° C., whereas 1,2,3-triazole is in a nearly liquid state at room temperature with a melting point of about 20° C. Therefore, 1,2,3-triazole has excellent dispersibility when mixed into the resin composition, can be mixed uniformly, and has other excellent advantages, such as being easily made into a masterbatch.

[0076] The content of the rust inhibitor (E) is preferably 0.01 to 5 parts by mass relative to 100 parts by mass of the base polymer (A), more preferably 0.1 part by mass or more or 1 part by mass or less, and even more preferably 0.2 part by mass or more or 0.5 part by mass or less.

[0077] (Silane coupling agent (F)) The present resin composition may contain a silane coupling agent (F) as necessary from the viewpoints of improving durability and adhesion to glass. Examples of the silane coupling agent (F) include epoxy group-containing silane coupling agents such as 3-glycidoxypropyltrimethoxysilane, 3-glycidoxypropyltriethoxysilane, 3-glycidoxypropylmethyldiethoxysilane, and 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane; amino group-containing silane coupling agents such as 3-aminopropyltrimethoxysilane, N-2-(aminoethyl)-3-aminopropylmethyldimethoxysilane, 3-triethoxysilyl-N-(1,3-dimethylbutylidene)propylamine, and N-phenyl-γ-aminopropyltrimethoxysilane; (meth)acrylic group-containing silane coupling agents such as 3-acryloxypropyltrimethoxysilane and 3-methacryloxypropyltriethoxysilane; and isocyanate group-containing silane coupling agents such as 3-isocyanatepropyltriethoxysilane. Commercially available silane coupling agents (F) include, for example, KBM-303, KBM-403, KBE-402, KBE-403, KBE-502, KBE-503, KBM-5103, KBM-573, KBM-802, KBM-803, KBE-846, and KBE-9007 (manufactured by Shin-Etsu Chemical Co., Ltd.). These may be used alone or in combination of two or more.

[0078] The content of the silane coupling agent (F) is preferably 0.001 parts by mass or more and 5 parts by mass or less, more preferably 0.01 parts by mass or more or 1 part by mass or less, and most preferably 0.02 parts by mass or more or 1 part by mass or less, relative to 100 parts by mass of the base polymer (A).

[0079] <Method for preparing the present resin composition> The resin composition can be obtained by mixing the base polymer (A), the photocurable compound (B), the photoinitiator (C), optionally a crosslinking agent (D), optionally a rust inhibitor (E), optionally a silane coupling agent (F), and optionally other components in predetermined amounts. The method for mixing these components is not particularly limited, and the order in which the components are mixed is also not particularly limited. A heat treatment step may be added during the production of the present resin composition. In this case, it is preferable to mix the components of the resin composition in advance and then carry out the heat treatment. A master batch made by concentrating various mixed components may also be used.

[0080] The mixing device is not particularly limited, and for example, a universal kneader, a planetary mixer, a Banbury mixer, a kneader, a gate mixer, a pressure kneader, a three-roll mill, or a two-roll mill may be used. If necessary, a solvent may be used for mixing. The present resin composition can be used as a solventless system that does not contain a solvent. By using it as a solvent-free system, no solvent remains, and there are advantages in that heat resistance and light resistance are improved.

[0081] <<This cured product>> A pressure-sensitive adhesive resin cured product according to one embodiment of the present invention (hereinafter referred to as the "cured product") is obtained by photocuring the above-mentioned resin composition. The fully cured product can also be used as a so-called post-cure type product, in which the fully cured product is further irradiated with light after lamination of an adherend and then fully cured. In addition, it can be used as a so-called non-cure type, which is used without irradiating light after lamination of the member. By using it as a non-cure type, there are advantages in that it does not require the trouble of post-curing after lamination of the adherend member, and it can be applied to a configuration in which light-impermeable members or members that cannot be irradiated with light due to photodegradation are laminated.

[0082] The cured product preferably has a loss tangent (Tan δ) at a temperature of -40°C of 0.1 or more and less than 0.6, more preferably 0.11 or more or 0.55 or less, and even more preferably 0.15 or more or 0.5 or less. At the same time, the cured product preferably has a loss tangent (Tan δ) at 100° C. of 0.3 or more and less than 1, more preferably 0.35 or more or 0.95 or less, and even more preferably 0.38 or more or 0.92 or less. The present cured product has such properties, which provide advantages such as excellent flex resistance. In order for the present cured product to have the above-mentioned properties, it is only necessary to use and cure the present resin composition.

[0083] The glass transition temperature (Tg A ) and photocurable compounds (B) The glass transition temperature (TgB) of the polymer can be calculated using the following FOX formula. FOX formula: 1 / Tg = W1 / T1 + W2 / T2 + ··· Wn / Tn In the formula, Tg is the theoretical glass transition temperature (K), W1, W2...Wn are the mass fractions of each monomer, and T1, T2...Tn are the measured glass transition temperatures (K) of each monomer.

[0084] In the present resin composition and the present cured product, the crosslinking agent (D) is an optional component. The present cured product can be prepared using the present resin composition that does not contain a crosslinking agent (D). However, from the viewpoint of obtaining high foaming resistance reliability after curing, it is preferable to cure the present resin composition that contains a crosslinking agent (D). Among these, it is particularly preferable to use a polyfunctional (meth)acrylate (d-1) as the crosslinking agent (D).

[0085] The cured product may be in any form, such as a sheet, layer, film, or block.

[0086] <<This adhesive sheet>> An adhesive sheet according to one embodiment of the present invention (hereinafter referred to as "the adhesive sheet") has an adhesive layer (hereinafter referred to as "the adhesive layer") formed from the above-mentioned resin composition.

[0087] The pressure-sensitive adhesive layer in the pressure-sensitive adhesive sheet may be a single layer or multiple layers. In the case of a multiple layer, another layer such as a so-called base layer may be interposed therebetween. When the pressure-sensitive adhesive layer has a multi-layer structure having other layers, it is preferable that the surface layer of the pressure-sensitive adhesive sheet is the pressure-sensitive adhesive layer formed from the resin composition. The pressure-sensitive adhesive layer can also be used as a so-called post-cure type, in which the pressure-sensitive adhesive layer is further irradiated with light after attachment to an adherend to fully cure the pressure-sensitive adhesive layer. In addition, the composition can be used as a so-called non-cured type, which means that it is used without irradiating light after lamination of the member. By using the composition as a non-cured type, there is an advantage that post-curing after lamination of the adherend member is not required.

[0088] The pressure-sensitive adhesive sheet preferably has a loss tangent (Tan δ) value at a temperature of -40°C of 0.1 or more and less than 0.6, more preferably 0.11 or more or 0.55 or less, and even more preferably 0.15 or more or 0.5 or less. At the same time, the pressure-sensitive adhesive sheet preferably has a loss tangent (Tan δ) value at a temperature of 100° C. of 0.3 or more and less than 1, more preferably 0.35 or more or 0.95 or less, and even more preferably 0.38 or more or 0.92 or less. The pressure-sensitive adhesive sheet has such properties, which provide advantages such as excellent flex resistance. In order for the present pressure-sensitive adhesive sheet to have the above-mentioned properties, it is necessary to use and cure the present resin composition.

[0089] In the present invention, in order for the present pressure-sensitive adhesive sheet to have the above-mentioned properties, the present pressure-sensitive adhesive layer may be formed using the present resin composition. As described above, in the present resin composition, the crosslinking agent (D) is an optional component, and the present cured product can be made using the present resin composition that does not contain the crosslinking agent (D). However, from the viewpoint of obtaining high foaming resistance reliability after curing, it is preferable to form the present pressure-sensitive adhesive layer using the present resin composition that contains the crosslinking agent (D), and among these, it is particularly preferable to use a polyfunctional (meth)acrylate (d-1) as the crosslinking agent (D).

[0090] The thickness of the present pressure-sensitive adhesive sheet is preferably 10 μm to 500 μm, more preferably 15 μm or more or 400 μm or less, and even more preferably 20 μm or more or 350 μm or less.

[0091] <How this adhesive sheet is used> The present pressure-sensitive adhesive sheet can be used as a single pressure-sensitive adhesive sheet. For example, the present resin composition can be directly applied to an adherend to form a sheet, or the present resin composition can be directly extruded or injected into a mold to use the present pressure-sensitive adhesive sheet. Furthermore, the pressure-sensitive adhesive sheet can also be used by directly filling the gaps between members such as conductive members with the resin composition.

[0092] On the other hand, the present pressure-sensitive adhesive sheet can also be used as a pressure-sensitive adhesive sheet having a pressure-sensitive adhesive layer formed from the present resin composition. For example, the present resin composition can be formed into a single-layer or multi-layer sheet on a release film to form a pressure-sensitive adhesive sheet with a release film.

[0093] Examples of the material for the release film include polyester film, polyolefin film, polycarbonate film, polystyrene film, acrylic film, triacetyl cellulose film, fluororesin film, etc. Among these, polyester film and polyolefin film are particularly preferred.

[0094] The thickness of the release film is not particularly limited. For example, from the viewpoint of processability and handling, the thickness of the release film is preferably 25 μm to 500 μm, more preferably 38 μm or more or 250 μm or less, and even more preferably 50 μm or more or 200 μm or less.

[0095] <<This laminate>> A laminate for constituting an image display device according to one embodiment of the present invention (hereinafter referred to as "the laminate") has a configuration in which either an adhesive layer made of the present cured product described above or the present adhesive sheet (hereinafter these are collectively referred to as "the present adhesive sheets") is interposed between two constituent members for an image display device. In this case, at least one of the two image display device components can be any one selected from the group consisting of a polarizing plate, a polarizing film, a retardation film, an image display panel, an organic EL display panel, a plasma display panel, a touch panel, a protective panel, and a touch sensor.

[0096] Specific examples of the present laminate include those having configurations such as release film / the present adhesive sheets / touch panel, image display panel / the present adhesive sheets / touch panel, image display panel / the present adhesive sheets / touch panel / the present adhesive sheets / protective panel, polarizing film / the present adhesive sheets / touch panel, and polarizing film / the present adhesive sheets / touch panel / the present adhesive sheets / protective panel.

[0097] The touch panel includes a structure in which a touch panel function is incorporated in a protection panel, and a structure in which a touch panel function is incorporated in an image display panel. Thus, the present laminate may have a configuration such as release film / the present pressure-sensitive adhesive sheets / protective panel, release film / the present pressure-sensitive adhesive sheets / image display panel, or image display panel / the present pressure-sensitive adhesive sheets / protective panel. In addition, in the above-mentioned configuration, all configurations in which the conductive layer is interposed between the pressure-sensitive adhesive sheet and an adjacent member such as a touch panel, a protective panel, an image display panel, a polarizing film, etc. can be mentioned, but the present invention is not limited to these lamination examples.

[0098] The touch panel may be of a resistive film type, a capacitive type, an electromagnetic induction type, etc. Among these, the capacitive type is preferable.

[0099] The material of the protective panel may be glass, or may be plastic such as an acrylic resin, a polycarbonate resin, an alicyclic polyolefin resin such as a cycloolefin polymer, a styrene resin, a polyvinyl chloride resin, a phenol resin, a melamine resin, or an epoxy resin.

[0100] The image display panel is composed of a polarizing film and other optical films such as other retardation films, a liquid crystal material, and a backlight system (usually, the surface of the adhesive resin composition or adhesive article that is adhered to the image display panel is an optical film), and depending on the control method of the liquid crystal material, there are STN method, VA method, IPS method, etc., and any of these methods may be used.

[0101] The present laminate can be used as a component of image display devices such as liquid crystal displays, organic EL displays, inorganic EL displays, electronic paper, plasma displays, and microelectromechanical system (MEMS) displays.

[0102] Since the present pressure-sensitive adhesive sheets have bending resistance, the above-mentioned two constituent members for an image display device are preferably flexible members that can be bent or curved.

[0103] <Method of manufacturing the present laminate> The present laminate can be produced by bonding the present pressure-sensitive adhesive sheet to any one of the components of an image display device selected from the group consisting of a polarizing plate, a polarizing film, a retardation film, an image display panel, an organic EL display panel, a plasma display panel, a touch panel, a protective panel, and a touch sensor.

[0104] The pressure-sensitive adhesive sheets in the laminate may further have photocuring properties (post-curing properties). When the above-mentioned adhesive sheets have the photocuring properties (post-curing properties), the adhesive sheets can be bonded to the image display device component, and then light can be irradiated from the outside of the image display device component through the image display device component to fully cure the adhesive sheets, and the two image display device components can be bonded together to produce the laminate, which also has excellent foaming resistance reliability. As described above, the above-mentioned pressure-sensitive adhesive sheets can be used in a non-cure type form in which no further post-curing by light irradiation is performed after attachment of the adherend, and using them in this form has the advantage that curing after attachment of the adherend is not required.

[0105] In order to obtain excellent flex resistance, it is preferable that the pressure-sensitive adhesive sheets used in the laminate have a loss tangent (Tan δ) value at a temperature of -40°C of 0.1 or more and less than 0.6, and a loss tangent (Tan δ) value at a temperature of 100°C of 0.3 or more and less than 1.

[0106] <<This display device>> An image display device according to one embodiment of the present invention (hereinafter referred to as "the present display device") includes the present laminate described above. Specific examples of the present image display device include liquid crystal displays, organic EL (electroluminescence) displays, inorganic EL displays, electronic paper, plasma displays, and microelectromechanical system (MEMS) displays, all of which include the present laminate.

[0107] <<Explanation of terms>> In the present invention, when expressed as "X to Y" (X and Y are any numbers), unless otherwise specified, it includes the meaning of "X or more and Y or less", as well as "preferably larger than X" or "preferably smaller than Y". In addition, when it is expressed as "X or more" (X is any number) or "Y or less" (Y is any number), it also includes the intention that "greater than X is preferable" or "less than Y is preferable." EXAMPLES

[0108] The present invention will be described in more detail below with reference to examples and comparative examples, but the present invention is not limited to these examples.

[0109] [Example 1] To 1 kg of an acrylic graft copolymer (A-1, mass average molecular weight: 440,000) as a (meth)acrylic copolymer obtained by randomly copolymerizing 64 parts by mass of 2-ethylhexyl acrylate, 19 parts by mass of methyl acrylate, and 17 parts by mass of hydroxyethyl acrylate, 300 g of a monofunctional urethane acrylate containing a propylene glycol skeleton (B-1, "PEM-X264" manufactured by AGC, mass average molecular weight (Mw): 10,000) as a photocurable compound and 10 g of a mixture of 2,4,6-trimethylbenzophenone and 4-methylbenzophenone (C-1, "Esacure TZT" manufactured by IGM) as a photoinitiator were added and mixed uniformly to obtain a pressure-sensitive adhesive resin composition 1. The photocurable compound (B-1) is a compound having two or more peaks of loss tangent (Tan δ) obtained by dynamic viscoelasticity measurement of the cured product, and the peak (b1) derived from the polymerization of the terminal acryloyl group was at -53°C, and the peak (b2) derived from the glycol skeleton was at -24°C.

[0110] Next, the pressure-sensitive adhesive resin composition 1 was sandwiched between two polyethylene terephthalate films ("Diafoil MRV (V03)" manufactured by Mitsubishi Chemical Corporation, thickness 100 μm, and "Diafoil MRQ" manufactured by Mitsubishi Chemical Corporation, thickness 75 μm) whose surfaces had been subjected to a release treatment, i.e., two release films, and hot-melt molded into a sheet having a thickness of 100 μm. Then, using a high-pressure mercury lamp, an integrated light amount of 3000 mJ / cm at a wavelength of 365 nm was projected through the release film. 2 The pressure-sensitive adhesive resin composition 1 was cured by irradiating with ultraviolet light so as to obtain a double-sided pressure-sensitive adhesive sheet laminate 1 consisting of a release film / pressure-sensitive adhesive sheet / release film.

[0111] [Example 2] To 1 kg of the acrylic graft copolymer (A-1), 300 g of a urethane acrylate containing a propylene glycol skeleton (B-1) as a photocurable compound and 10 g of a mixture of 2,4,6-trimethylbenzophenone and 4-methylbenzophenone (C-1, "Esacure TZT" manufactured by IGM) as a photoinitiator were added, and 5 g of a silane coupling agent ("KBM-403" manufactured by Shin-Etsu Silicones) was further mixed uniformly to obtain a pressure-sensitive adhesive resin composition 2.

[0112] Next, the pressure-sensitive adhesive resin composition 2 was sandwiched between two polyethylene terephthalate films ("Diafoil MRV (V03)" manufactured by Mitsubishi Chemical Corporation, thickness 100 μm, and "Diafoil MRQ" manufactured by Mitsubishi Chemical Corporation, thickness 75 μm) whose surfaces had been subjected to a release treatment, i.e., two release films, and hot-melt molded into a sheet having a thickness of 100 μm. Then, using a high-pressure mercury lamp, an integrated light amount of 3000 mJ / cm at a wavelength of 365 nm was projected through the release film. 2The adhesive resin composition 2 was cured by irradiating with ultraviolet light so as to obtain a double-sided adhesive sheet laminate 2 consisting of a release film / adhesive sheet / release film.

[0113] [Example 3] A pressure-sensitive adhesive resin composition 3 and a double-sided pressure-sensitive adhesive sheet laminate 3 were obtained in the same manner as in Example 1, except that 500 g of propylene glycol skeleton-containing urethane acrylate (B-1) was added as the photocurable compound.

[0114] [Comparative Example 1] To 1 kg of the acrylic graft copolymer (A-1), 45 g of a mixture of 2,4,6-trimethylbenzophenone and 4-methylbenzophenone (C-1, “Esacure TZT” manufactured by IGM) was added as a photoinitiator, and mixed uniformly to obtain a pressure-sensitive adhesive resin composition 4.

[0115] Next, the pressure-sensitive adhesive resin composition 4 was sandwiched between two polyethylene terephthalate films ("Diafoil MRV (V03)" manufactured by Mitsubishi Chemical Corporation, thickness 100 μm, and "Diafoil MRQ" manufactured by Mitsubishi Chemical Corporation, thickness 75 μm) whose surfaces had been subjected to a release treatment, i.e., two release films, and hot-melt molded into a sheet having a thickness of 100 μm. Then, using a high-pressure mercury lamp, an integrated light amount of 3000 mJ / cm at a wavelength of 365 nm was projected through the release film. 2 The adhesive resin composition 5 was cured by irradiating with ultraviolet light so as to obtain a double-sided adhesive sheet laminate 4 consisting of a release film / adhesive sheet / release film.

[0116] [Comparative Example 2] To 1 kg of an acrylic graft copolymer (A-2, mass average molecular weight: 470,000) as a (meth)acrylic copolymer obtained by randomly copolymerizing 71 parts by mass of butyl acrylate, 26.2 parts by mass of 2-ethylhexyl acrylate, and 2.8 parts by mass of acrylamide, 60 g of nonanediol diacrylate (B-2, "Viscoat 260" manufactured by Osaka Organic Chemical Industry Co., Ltd., mass average molecular weight (Mw): 268) as a photocurable compound and 15 g of a mixture of 2,4,6-trimethylbenzophenone and 4-methylbenzophenone (C-1, "Esacure TZT" manufactured by IGM) as a photoinitiator were added and mixed uniformly to obtain a pressure-sensitive adhesive resin composition 5.

[0117] Next, the pressure-sensitive adhesive resin composition 5 was sandwiched between two polyethylene terephthalate films ("Diafoil MRV (V03)" manufactured by Mitsubishi Chemical Corporation, thickness 100 μm, and "Diafoil MRQ" manufactured by Mitsubishi Chemical Corporation, thickness 75 μm) whose surfaces had been subjected to a release treatment, i.e., two release films, and hot-melt molded into a sheet having a thickness of 100 μm. Then, using a high-pressure mercury lamp, an integrated light amount of 1000 mJ / cm at a wavelength of 365 nm was projected through the release film. 2 The adhesive resin composition 6 was cured by irradiating with ultraviolet light so as to obtain a double-sided adhesive sheet laminate 5 consisting of a release film / adhesive sheet / release film.

[0118] [Comparative Example 3] An adhesive resin composition 6 and a double-sided adhesive sheet laminate 6 were obtained in the same manner as in Comparative Example 2, except that an acrylic graft copolymer (A-3, mass average molecular weight: 420,000) was used as the (meth)acrylic copolymer, which was obtained by randomly copolymerizing 72 parts by mass of butyl acrylate, 26 parts by mass of 2-ethylhexyl acrylate, and 2 parts by mass of acrylic acid.

[0119] [Comparative Example 4] To 1 kg of propylene glycol skeleton-containing urethane acrylate (B-1) as a photocurable compound, 10 g of a mixture of 2,4,6-trimethylbenzophenone and 4-methylbenzophenone (C-1, "Esacure TZT" manufactured by IGM) as a photoinitiator was added and mixed uniformly to obtain adhesive resin composition 7.

[0120] Next, the pressure-sensitive adhesive resin composition 7 was applied to a polyethylene terephthalate film ("Diafoil MRV (V03)" manufactured by Mitsubishi Chemical Corporation, thickness 100 μm) whose surface had been treated for release, i.e., a release film, in the form of a sheet having a thickness of 100 μm, and then the applied surface was covered with a polyethylene terephthalate film ("Diafoil MRQ" manufactured by Mitsubishi Chemical Corporation, thickness 75 μm) whose surface had been treated for release, i.e., a release film. Using a high-pressure mercury lamp, an integrated light quantity of 365 nm wavelength was 3000 mJ / cm2 through the release film. 2 The adhesive resin composition 7 was cured by irradiating with ultraviolet light so as to obtain a double-sided adhesive sheet laminate 7 consisting of a release film / adhesive sheet / release film.

[0121] [evaluation] The double-sided pressure-sensitive adhesive sheet laminates produced in the above Examples and Comparative Examples were subjected to the following various measurements and evaluations. The evaluation results are summarized in Table 1.

[0122] <Viscoelasticity measurement> The release films of the adhesive sheet laminates 1 to 7 prepared in the examples and comparative examples were peeled off, and the adhesive sheets were stacked to a thickness of 1 mm or more. Next, dynamic viscoelasticity measurements were performed using a rheometer ("MARS" manufactured by Eiko Seiki Co., Ltd.) under the following conditions: adhesive tool: Φ20 mm parallel plate, strain: 0.5%, frequency: 1 Hz, heating rate: 3°C / min, measurement temperature: -70°C to 130°C. From the obtained viscoelasticity curve, the peak temperature of Tan δ was read and determined as the glass transition temperature (Tg). In addition, the values ​​of Tan δ were read at −40° C. and 100° C. The results are shown in the table.

[0123] The glass transition temperature of the photocurable compound after photocuring was measured as follows. To 100 g of the photocurable compound, 1 g of a mixture of 2,4,6-trimethylbenzophenone and 4-methylbenzophenone (IGM's "Esacure TZT") was added as a photoinitiator, and the mixture was uniformly mixed and applied onto a polyethylene terephthalate film with a release-treated surface (Mitsubishi Chemical's "Diafoil MRV (V03)", i.e., a release film), and then the applied surface was covered with a polyethylene terephthalate film with a release-treated surface (Mitsubishi Chemical's "Diafoil MRQ", thickness 75 μm). Using a high-pressure mercury lamp, the integrated light quantity of 365 nm wavelength was 3000 mJ / cm through the release film. 2 The photocurable compound was photocured by irradiating it with ultraviolet light so that the photocurable compound was photocured. The cured photocurable compound was then layered to a thickness of 1 mm or more. Next, dynamic viscoelasticity measurements were performed using a rheometer ("MARS" manufactured by Eiko Seiki Co., Ltd.) under the following conditions: adhesion jig: Φ20 mm parallel plate, strain: 0.5%, frequency: 1 Hz, heating rate: 3°C / min, measurement temperature: -70°C to 100°C. The peak temperature of Tan δ was read from the obtained viscoelastic curve and determined as the glass transition temperature of the photocurable compound. The glass transition temperature of each photocurable compound after photocuring is shown in the table below.

[0124] <Glass adhesion> For the adhesive sheet laminates 1 to 7 produced in the examples and comparative examples, one of the release films was peeled off, and a polyethylene terephthalate film (Toyobo Co., Ltd., "Cosmoshine A4300", thickness 100 μm) was roll-pressed as a backing film using a hand roller. This was cut into a 10 mm wide x 150 mm long rectangular shape, and the remaining release film was peeled off to expose the adhesive surface, which was roll-attached to soda lime glass using a hand roller to produce a laminate consisting of a release film / adhesive sheet / backing film, and this laminate was autoclaved (60°C, gauge pressure 0.2 MPa, 20 minutes) for finish attachment to produce a glass adhesion measurement sample. The backing film was peeled off from the glass while being pulled at an angle of 180° at a peeling speed of 60 mm / min, and the tensile strength was measured with a load cell to determine the 180° peel strength (N / cm) of the adhesive sheet to the glass before photocuring.

[0125] <Heat and humidity haze> For each of the adhesive sheet laminates 1 to 7 produced in the examples and comparative examples, one of the release films was peeled off, and a COP film (Zeon Corporation, "ZF-14", thickness 100 μm) was pressed onto the exposed adhesive surface with a hand roller. The remaining release film was peeled off, and a piece of soda lime glass measuring 82 mm x 53 mm and 0.55 mm thick was attached to the exposed adhesive surface with a hand roller, and then autoclaved at 60°C, 0.2 MPa, and 20 minutes to obtain a sample for evaluating moist heat haze consisting of glass / adhesive sheet / COP film. The sample for evaluating wet heat haze was stored in an environment of 65°C and 90% RH for 300 hours, and then the haze value of the sample for evaluating wet heat haze was measured using a haze meter ("NDH5000" manufactured by Nippon Denshoku Industries Co., Ltd.) in accordance with JIS K7136.

[0126] <Corrosion resistance> (1) Corrosion resistance to ITO substrate An ITO glass substrate for evaluating corrosion resistance was prepared by forming a round-trip line of indium oxide (ITO) on a glass substrate (60 mm × 45 mm) with a thickness of 150 to 200 Å, a line width of 70 μm, a line length of 46 mm, and a line spacing of 30 μm, making 10.5 round trips, and forming 2 mm squares made of ITO on both ends of the round-trip line to form an ITO pattern (approximately 97 cm long) (see FIG. 1(A)).

[0127] The release film on one side of the adhesive sheet laminates 1 to 7 produced in the above Examples and Comparative Examples was peeled off, and a PET film (manufactured by Toyobo Co., Ltd., product name "Cosmoshine A4100", 125 μm) was pressed onto the exposed surface with a hand roller. Next, the adhesive sheet with the PET film was cut into a size of 52 mm × 45 mm, and the remaining release film was peeled off. As shown in Figure 1 (B), the adhesive sheet was attached to an ITO glass substrate for corrosion resistance evaluation with a hand roller so as to cover the ITO reciprocating lines, to produce a sample for corrosion resistance evaluation (ITO wiring with adhesive sheet) (see Figure 1 (C)).

[0128] The resistance value (Ω0) of the ITO wiring in this corrosion resistance evaluation sample (ITO wiring with adhesive sheet) at room temperature was measured in advance. On the other hand, the corrosion resistance evaluation sample (ITO wiring with adhesive sheet) was stored in an environment of 65°C and 90% RH for 500 hours, and the resistance value (Ω) of the ITO wiring in the corrosion resistance evaluation sample (ITO wiring with adhesive sheet) was measured after storage. Then, the rate of change (%) of the ITO resistance, i.e., the end-to-end resistance of the line, [(Ω / Ω0)-1)×100] was calculated and shown in the table as “change in resistance”.

[0129] <Bending test> (1) Dynamic bending test The release films were peeled off from the adhesive sheet laminates 1 to 7 prepared in the examples and comparative examples, and a PET film (Mitsubishi Chemical Corporation's "Diafoil S-100", thickness 38 μm, Toyobo Co., Ltd.'s "Cosmoshine A4300", thickness 100 μm) was roll-laminated to the exposed adhesive surface to create a release film / adhesive sheet / PET film laminate, which was then cut to 50 mm x 100 mm to prepare an evaluation sample for dynamic bending tests. The evaluation sample thus prepared was set in a bending tester (Yuasa Systems' "DLDMLH-FS") with the 38 μm PET laminated surface facing inward, and a bending test was performed under the following test conditions in test environments of 24°C (room temperature) and -20°C (low temperature). Test temperature: 24℃ (normal temperature), -20℃ (low temperature) ·Curvature radius r:3mm Test speed: 60 rpm Test count: 300,000 times

[0130] The evaluation samples were visually observed after testing in the test environments of 24°C (room temperature) and -20°C (low temperature). Those that had fold marks on the adhesive sheet or peeling at the interface between the adherend and the adhesive sheet were rated as "X (no good)", and those that showed no change upon visual observation were rated as "O (good)".

[0131] (2)Static bending test The release films were peeled off from the adhesive sheet laminates 1 to 7 prepared in the examples and comparative examples, and a PET film (Mitsubishi Chemical Corporation's "Diafoil S-100", thickness 38 μm, Toyobo Co., Ltd.'s "Cosmoshine A4300", thickness 100 μm) was roll-laminated to the exposed adhesive surface to create a release film / adhesive sheet / PET film laminate, which was then cut to 40 mm x 100 mm to prepare an evaluation sample for static bending tests. The evaluation sample thus prepared was folded with a curvature radius r of 3 mm so that the 38 μm PET laminated surface was on the inside, and then stored in an environment of 65° C. and 90% RH for 48 hours. After the test, the evaluation samples were visually observed. Those that had fold marks on the adhesive sheet or peeling at the interface between the adherend and the adhesive sheet were rated as "X (no good)", and those that showed no change upon visual observation were rated as "O (good)".

[0132] <Overall rating> The overall evaluation was based on the following criteria. Specimens with a glass adhesion strength of 2 N / cm or more and no visible changes in any of the bending tests (dynamic bending test: 300,000 times at 24°C, 300,000 times at -20°C, and static bending test: 48 hours at 65°C, 90%) were rated as "very good." Specimens with a glass adhesion strength of less than 2 N / cm and / or those that showed creases or peeling in the dynamic bending test at room temperature or the static bending test at high temperature were rated as "poor."

[0133] [Table 1]

[0134] (Evaluation Results) The pressure-sensitive adhesive sheets obtained in Examples 1 to 3 were found to be pressure-sensitive adhesive resin compositions comprising a base polymer (A) made of a (meth)acrylic acid ester copolymer having a glass transition temperature (TgA) of -30°C or higher, a photoinitiator (C), and a photocurable compound (B) having a lower glass transition temperature than that of the base polymer (A), and containing a predetermined amount of compound (B) in the composition, and thus had excellent adhesive properties, optical properties, and flex resistance.

[0135] It was found that Comparative Example 1, which does not contain a photocurable compound, exhibited poor bending resistance in the static bending test and at low temperatures.

[0136] It was found that Comparative Examples 2 and 3 used a photocurable compound having a higher glass transition temperature than the base polymer (A), and therefore had poor bending resistance in the static bending test. It was found that Comparative Example 4, which does not contain the base polymer (A) made of a (meth)acrylic acid ester, did not adhere to the adherend and peeled off in the bending test. [Industrial Applicability]

[0137] The adhesive resin composition of the present invention has excellent adhesive properties and flexural resistance properties, and the adhesive resin cured product, adhesive sheet, and image display device laminate formed from the composition can be used as a gap filling layer to improve the visibility of an image display device, and can be particularly suitably used in image display devices having flexible members.

Claims

1. A pressure-sensitive adhesive resin composition comprising a base polymer (A) made of a (meth)acrylic acid ester copolymer, a photocurable compound (B), and a photoinitiator (C), The photocurable compound (B) is a (meth)acrylate (b-1) having a glycol skeleton, The photocurable compound (B) has a glass transition temperature (TgB) after photocuring of -45°C or lower, and the glass transition temperature (TgB) after photocuring of the photocurable compound (B) is lower than the glass transition temperature (TgA) of the base polymer (A).

2. 2. The pressure-sensitive adhesive resin composition according to claim 1, wherein the photocurable compound (B) is a (meth)acrylate (b-1) having a glycol skeleton.

3. 3. The pressure-sensitive adhesive resin composition according to claim 1, wherein the (meth)acrylate (b-1) is a urethane (meth)acrylate having a mass average molecular weight (Mw) of 5,000 or more.

4. The pressure-sensitive adhesive resin composition according to claim 3 , wherein the urethane (meth)acrylate is a monofunctional urethane acrylate oligomer represented by the following formula 1: 【Chemistry 1】 (In formula 1, R1 represents a hydrogen atom or a methyl group, X represents a urethane bond, R2 and R3 each represent an alkylene group, R4 represents an alkyl group, and n is an integer of 2 or more.)

5. The photocurable compound (B) is contained in an amount of more than 15 parts by mass and less than 75 parts by mass per 100 parts by mass of the base polymer. The pressure-sensitive adhesive resin composition according to any one of claims 1 to 4.

6. The pressure-sensitive adhesive resin composition according to any one of claims 1 to 5, wherein the base polymer (A) has a glass transition temperature (TgA) of -30°C or higher.

7. The pressure-sensitive adhesive resin composition according to any one of claims 1 to 6, wherein the base polymer (A) is a copolymer that contains at least a structural unit derived from a hydroxyl group-containing monomer (a-1) and does not contain a structural unit derived from a carboxyl group-containing monomer (a-2), and the content of the structural unit derived from the hydroxyl group-containing monomer (a-1) in the copolymer is 5 to 30 mass%.

8. A cured adhesive resin obtained by curing the adhesive resin composition according to any one of claims 1 to 7.

9. The pressure-sensitive adhesive resin cured product according to claim 8, having a loss tangent (Tan δ) value of 0.1 or more and less than 0.6 at a temperature of -40°C, and a loss tangent (Tan δ) value of 0.3 or more and less than 1 at a temperature of 100°C.

10. A pressure-sensitive adhesive sheet having a pressure-sensitive adhesive layer formed from the pressure-sensitive adhesive resin composition according to any one of claims 1 to 7.

11. The pressure-sensitive adhesive sheet according to claim 10, having a loss tangent (Tan δ) value at a temperature of -40°C of 0.1 or more and less than 0.6, and a loss tangent (Tan δ) value at a temperature of 100°C of 0.3 or more and less than 1.

12. A structure in which two components for an image display device are laminated via a pressure-sensitive adhesive layer made of the cured pressure-sensitive adhesive resin according to claim 8 or a pressure-sensitive adhesive sheet according to claim 10 having the pressure-sensitive adhesive layer, A laminate for constituting an image display device, characterized in that at least one of the two constituent members for the image display device is any member selected from the group consisting of a polarizing plate, a polarizing film, a retardation film, an image display panel, an organic EL display panel, a plasma display panel, a touch panel, a protective panel, and a touch sensor.

13. The pressure-sensitive adhesive layer or the pressure-sensitive adhesive sheet has a loss tangent (Tan δ) value of 0.1 or more and less than 0.6 at a temperature of -40 ° C., and a loss tangent (Tan δ) value of 0.3 or more and less than 1 at a temperature of 100 ° C. The laminate for constituting an image display device according to claim 12.

14. 14. The laminate for constituting an image display device according to claim 12, wherein both of said two constituent members for the image display device are flexible members that can be bent or curved.

Citation Information

Patent Citations

  • The indigo produced by microorganisms

    JP1984501972A

  • Adhesive composition

    JP2006225443A

  • Adhesive sheet for fixing electronic parts and method of manufacturing electronic parts using the same

    JP2008013692A

  • Resin composition for optical use and resin material for optical use using the same

    JP2009024160A

  • Adhesive, and adhesive sheet using the same, temporarily surface-protecting adhesive, and temporarily surface-protecting adhesive sheet using the same, method of using the temporarily surface-protecting sheet, and active energy ray-curable resin composition

    JP2009287016A