Cosmetic materials

A decorative material with a thermoplastic resin and scale-like filler, combined with olefin additives, addresses the issues of differential expansion and weight in conventional materials, offering a wide, lightweight, and strong solution for construction.

JP7562982B2Active Publication Date: 2024-10-08TOPPAN HOLDINGS INC
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2020072271
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-04-14
Publication Date
2024-10-08
Estimated Expiration
2040-04-14

AI Technical Summary

Technical Problem

Conventional decorative materials face issues with warping, insect bite, corrosion due to moisture absorption, and increased construction burden due to wood-based materials, which are heavy and have differential linear expansion in the flow and width directions, making them difficult to widen and economically inefficient.

Method used

A decorative material comprising a base material with a thermoplastic resin and a scale-like filler, having a coefficient of linear expansion of at least 6.0×10^-5 in both directions, containing 50-70% scale-like filler by weight, and incorporating an olefin elastomer and strain-hardening olefin additives to enhance strength and foamability.

Benefits of technology

The solution provides a wide, lightweight decorative material with excellent mechanical strength and reduced construction burden, maintaining dimensional stability and foamability while ensuring high bending strength and elasticity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007562982000002
    Figure 0007562982000002
  • Figure 0007562982000001
    Figure 0007562982000001
Patent Text Reader

Abstract

To provide a wide and lightweight decorative material excellent in strength and less burdened in construction.SOLUTION: In a decorative material 10 comprising a base material 20 and a decorative sheet 30 laminated on the base material 20, the base material 20 contains a thermoplastic resin and a scaly filler, has a Celuka structure, and has a linear expansion coefficient of 6.0×10-5 or less in at least the width direction of the flow direction and the width direction. The filler is contained in an amount of 50-70 wt.%, and the base material 20 has a bending strength of not less than 30 MPa and a bending elasticity within the range of 2000-9000 MPa. In the decorative material 10, the base material 20 may have a width of 500 mm or more and a length of 500 mm or more, the filler may have an average aspect ratio calculated from the average diameter / thickness of the plate surface of 10 or more, and the base material 20 may contain olefinic elastomer with a melt flow rate (MFR) of 300 or more by 10-30 wt.% based on the weight of the base material 20 excluding the filler.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a wide, lightweight decorative material that is excellent in strength and imposes little strain on the construction. [Background technology]

[0002] Conventionally, decorative sheets attached to wood-based substrates such as plywood and fiberboard have been widely used for architectural interior materials, flooring materials, fittings, surface materials for home appliances, etc. However, these decorative materials have problems with physical properties such as warping, insect damage, and corrosion caused by moisture absorption and release in the wood-based substrate, and the substrate is heavy due to being made of wood, which increases the burden of construction work. As a countermeasure to the above problems, many resin moldings containing a thermoplastic resin and a filler have been developed. One of the molding methods is the Cerca process (Patent Document 1 and Patent Document 2). The Cerca process is a molding method that uses a special die to solidify the surface layer to form a low foam layer, and at the same time, forms a foam layer in the core. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] Patent No. 4206802 [Patent Document 2] Patent No. 3932883 Summary of the Invention [Problem to be solved by the invention]

[0004] However, since the above-mentioned Celca process is a profile extrusion molding process, the dimension in the width direction is shorter than the flow direction, and therefore different linear expansion properties are required in the flow direction and the width direction. For this reason, fibrous wood powder, which has a high effect of suppressing dimensional change in the flow direction, has often been used as a filler. However, it is difficult to make resin moldings with added fibrous fillers wide, which increases the workload during construction and poses economic challenges. By adding scaly filler, it is possible to suppress linear expansion in both the machine and cross directions, and this effect can be further enhanced by increasing the filler mixing ratio. However, problems such as a decrease in base material strength and deterioration of foaming properties can be encountered, particularly under mixing conditions where the filler ratio is 50% or more.

[0005] On the other hand, narrow-width molded bodies are a heavy burden to install and have economic problems, so there is a demand for the development of wide-width molded bodies. With fibrous fillers such as wood powder, it is difficult to make them wide because there is a difference in linear expansion between the flow direction and the width direction. As a solution, the thermal expansion and contraction in the flow direction and width direction can be stabilized by incorporating a high amount of scale-like filler with a high aspect ratio, but on the other hand, there are issues with the deterioration of foaming due to a decrease in viscosity and the decrease in strength due to the deterioration of the filler's dispersibility. An object of one aspect of the present invention is to provide a wide, lightweight decorative material that is excellent in strength and imposes little strain on the user during application. [Means for solving the problem]

[0006] In order to achieve the above object, a decorative material according to one aspect of the present invention is a decorative material comprising a substrate and a decorative sheet laminated on the substrate, the substrate containing a thermoplastic resin and a scaly filler, having a celca structure, and having a linear expansion coefficient of 6.0×10 in at least the width direction out of the machine direction and the width direction. -5 The filler is contained at 50 to 70% by weight, and the base material has a bending strength of 30 MPa or more and a bending elasticity in the range of 2000 to 9000 MPa. A decorative material according to one aspect of the present invention is characterized in that the substrate has a width of 500 mm or more and a length of 500 mm or more. A decorative material according to one aspect of the present invention is characterized in that the filler has an average aspect ratio of 10 or more, calculated from the average diameter / thickness of the plate surface.

[0007] The decorative material according to one embodiment of the present invention is characterized in that the base material contains an olefin-based elastomer having a melt flow rate (MFR) of 300 or more in an amount of 10 to 30% by weight based on the weight of the base material excluding the filler. A decorative material according to one embodiment of the present invention contains, in a substrate, 3 to 10% by weight of an olefin having strain hardening properties, based on the weight of the substrate excluding the filler. A decorative material according to one embodiment of the present invention comprises a base material containing an olefin-based elastomer having a melt flow rate (MFR) of 300 or more as a first additive in an amount of 10 to 30% by weight based on the weight of the base material excluding the filler, and an olefin having strain hardening properties as a second additive in an amount of 3 to 10% by weight based on the weight of the base material excluding the filler, with the ratio of the first additive to the second additive being within the range of 5:1 to 1:1. Effect of the Invention

[0008] According to one aspect of the present invention, it is possible to provide a wide, lightweight decorative material that is excellent in strength and places little strain on the user during application. [Brief description of the drawings]

[0009] [Figure 1] FIG. 1 is a cross-sectional view of a decorative material according to an embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010] (Cosmetic materials 10) In FIG. 1, 10 is a decorative material. The decorative material 10 is broadly composed of a substrate 20 and a decorative sheet 30 laminated to the substrate 20. Located between the substrate 20 and the decorative sheet 30 is an adhesive layer 40 that bonds the substrate 20 and the decorative sheet 30 together. The thickness ratio of each layer of the decorative material 10 is not limited to that shown in FIG.

[0011] (Base material 20) The substrate 20 contains a thermoplastic resin and a scaly filler, and has a cell structure. As shown in FIG. 1, the substrate 20 is roughly composed of a foam layer 22 and surface layers 21, 21 located on both sides of the foam layer 22, respectively. Examples of the thermoplastic resin that can be used for the substrate 20 include polypropylene, polyethylene, polyvinyl chloride, ABS, polystyrene, polyester, polyamide, polyolefin, ethylene-propylene-diene rubber, ethylene vinyl acetate, and silicone rubber. However, polypropylene is preferred in terms of the mechanical strength and water resistance of the wood substrate.

[0012] (Decorative sheet 30) The decorative sheet 30 is a sheet made of the same material as the base material 20, such as polyolefin or vinyl chloride resin, on which a design such as wood grain or an abstract pattern is applied. As shown in Fig. 1, the decorative sheet 30 is broadly composed of a design layer 31, a laminate 32, and a top coat 33. The design layer 31 is a sheet base material or a sheet base material on which a design is applied by printing. The sheet base material may be colored. The thermoplastic resin for the decorative sheet 30 is not particularly limited, but in consideration of the recyclability of the decorative material 10, it is desirable to use a sheet of the same material as the base material 20 with a design such as wood grain or an abstract pattern.

[0013] (adhesive layer 40) The adhesive layer 40 bonds the surface layer 21 of the substrate 20 and the design layer 31 of the decorative sheet 30 . The adhesive material used for the adhesive layer 40 is not particularly limited, but a two-liquid urethane resin adhesive or the like can be used. The adhesive layer 40 may be omitted if sufficient adhesive strength is obtained between the surface layer 21 of the substrate 20 and the design layer 31 of the decorative sheet 30.

[0014] (Selkie structure) A Cerca structure is a structure obtained by the Cerca process (Cerca method) or an equivalent structure. The Cerca process (Cerca method) is a foam extrusion molding method in which an extrusion die having outlet dimensions approximately the same as or slightly smaller than the inlet dimensions of a cooling sizing die is used, and a foamable resin composition is extruded from the extrusion die with the outlet of the extrusion die and the inlet of the cooling sizing die being brought into close contact with each other, thereby introducing the foamable resin composition into the cooling sizing die in a state in which foaming has hardly progressed, and foaming occurs mainly inside the cooling sizing die. The Celca structure is not limited to structures produced by the above-mentioned methods, and is characterized in that at least a portion of the surface is non-foamed or low-foamed, the core is highly foamed, the non-foamed or low-foamed surface and the core are made of thermoplastic resin of the same composition, and the core and the surface have a continuous structure. In this embodiment, the Cerca structure is adopted because the resin molded body formed by the Cerca process has excellent workability for cutting and nailing, and because a surface layer is formed, the surface is smooth and highly scratch-resistant.In addition, because it is a foam, it is lightweight, requires little construction effort, and has high thermal insulation properties.

[0015] (Characteristics of the substrate 20) The base material 20 is required to be a wide and lightweight flooring material that has excellent mechanical strength such as bending elasticity and bending strength, and that reduces the burden of construction. For this reason, the base material 20 is desirably 500 mm or more in width and 500 mm or more in length. If the base material 20 is less than 500 mm in width or less than 500 mm in length, the burden of construction increases. The linear expansion coefficient of the substrate 20 is 6.0×10 in at least the transverse direction (TD) out of the machine direction (MD) and the transverse direction (TD). -5 It is desirable that the following: This allows the substrate 20 to have a large width. The linear expansion coefficient is 6.0×10 in both the machine direction (MD) and transverse direction (TD). -5 It may be the following.

[0016] (Material composition of base material 20) The material composition of the base material 20 is required to contain 50 to 70% by weight of a flaky filler. This is because if the filler is less than 50%, the linear expansion coefficient of the resin will affect it, reducing dimensional stability, and if it exceeds 70%, the filler will not disperse well, reducing bending strength and melt viscosity, resulting in poor foaming properties. In this embodiment, the material composition of the base material 20 contains 50 to 70% by weight of a scaly filler, thereby providing a decorative material 10 with high dimensional stability without compromising foamability and strength. As the flaky filler, it is preferable to use talc, mica, clay, bentonite, silica, hexagonal boron nitride, etc.

[0017] (Aspect ratio of scale-like filler) The aspect ratio of the scaly filler is desirably 10 or more, preferably 30 or more. The aspect ratio is a value calculated from the average diameter / thickness of the plate surface of the scaly filler. To suppress linear expansion, it is preferable to use a filler with a high aspect ratio.

[0018] (Additives for Base Material 20) The base material 20 contains a thermoplastic resin and a scaly filler, as well as one or more types of additives. In this embodiment, the following additives are added. The additives are not limited to the following (1) and (2). (1) First additive (hereinafter also referred to as "additive 1") Additive 1 contains an olefin-based elastomer having a melt flow rate (MFR) of 300 or more, preferably 1000 or more, in an amount of 10 to 30% by weight based on the weight of the base material excluding the scaly additives. Here, the melt flow rate (MFR) is one of the methods for evaluating the fluidity of a resin.

[0019] The melt flow rate is measured by loading resin test material (pellets) into a test device called a melt flow indexer, heating it to melt a specified weight of resin, and measuring the amount of resin that flows out, and the test method is stipulated by JIS and ISO. The higher the melt flow rate, the better the resin is evaluated to have fluidity, and the lower the melt flow rate, the worse the flow. When the filler content exceeds 50%, the bending strength decreases, so the dispersibility of the filler in the resin becomes important. To improve dispersibility, it is desirable to use a material with a high MFR as an additive. (2) The second additive (hereinafter also referred to as "additive 2") Additive 2 contains an olefin having strain hardening properties in an amount of 3 to 10% by weight based on the weight of the base material excluding the filler. As the compounding ratio of the scaly filler increases, the melt viscosity decreases and the foaming property of the base material 20 deteriorates, so it is advisable to add a resin having strain hardening properties.

[0020] (Ratio of Additive 1 to Additive 2) The ratio of additive 1 to additive 2 is preferably 5:1 to 1:1. This is because a high ratio of additive 1 deteriorates the foaming property, and a high ratio of additive 2 deteriorates the dispersibility due to an increase in melt viscosity.

[0021] (Other characteristics of the substrate 20) Other characteristics of the substrate 20 include the following: (1) Flexural modulus The flexural modulus of the substrate 20 is 2000 to 9000 MPa. If the flexural modulus is less than 2000 MPa, the rigidity and surface hardness are insufficient, and scratch resistance and indentation resistance deteriorate.If the flexural modulus exceeds 9000 MPa, the substrate becomes hard, resulting in poor walking feel and reduced flexural strength. (2) Bending strength The bending strength of the substrate 20 is 30 MPa or more. (3) Foaming method The substrate 20 is preferably foamed by chemical foaming, physical foaming, supercritical foaming, or the like. (4) Foam structure The foam structure of the base material 20 is preferably such that it is foamed in a closed cell type, a continuous cell type, or the like.

[0022] (Features of this embodiment) The decorative material 10 according to this embodiment has an object to provide a wide, lightweight flooring material that has excellent mechanical strength such as bending elasticity and bending strength, and that places a small burden on construction. In order to increase the width of the substrate 20, it is necessary to increase the suppression of linear expansion in the width direction. In order to improve the suppression of linear expansion in the width direction, it is necessary to pack a large amount of filler with a high aspect ratio (scale-like filler). On the other hand, the substrate 20 becomes heavy, and therefore needs to be foamed. As a solution to this problem, it is effective to add a high melt tension resin (olefin having strain hardening properties) to impart foamability. In addition, the strength of the substrate 20 is reduced, making it necessary to add an interfacial modifier. As a solution, for example, it is effective to add an olefin-based elastomer to improve dispersibility and suppress the reduction in bending elasticity and bending strength. EXAMPLES

[0023] With reference to this embodiment, the decorative materials of Examples 1 to 10 and Comparative Examples 1 to 9 will be described below. (Example 1: Base) In Example 1, the following materials were mixed and pelletized in a twin-screw kneader. The pellets were expanded 1.4 times by chemical foaming using a sodium bicarbonate-citric acid foaming agent, and molded into a rectangular parallelepiped shape with a thickness of 5 mm by the Celca process. (1) Thermoplastic resin: Polypropylene 30 parts by weight (wt%) (2) Scaly filler: Filler (mica) 60 parts by weight (wt%) The aspect ratio is 80. (3) Additive 1: Olefin-based elastomer (hereinafter also referred to as "elastomer") 7 parts by weight (wt%) (4) Additive 2: Branched olefin 2 parts by weight (wt%) In this case, the elastomer / branched olefin ratio is 3.5. (5) Others: Maleic acid modified polypropylene 1 part by weight (wt%)

[0024] (Example 2: Low aspect ratio) Example 2 is the same as Example 1, except that the aspect ratio of the filler in Example 1 is reduced from "80" to "10".

[0025] (Example 3: Low filler) Examples 3 to 10 are the same as Example 1 except that the material composition in Example 1 is changed. First, in Example 3, the amount of the filler in Example 1 was reduced from "60 parts by weight" to "50 parts by weight." In this case, the amount of elastomer in Example 1 was increased from "7 parts by weight" to "9 parts by weight", and the amount of branched olefin was increased from "2 parts by weight" to "2.5 parts by weight". As a result, the "elastomer / branched olefin" ratio increased from "3.5" to "3.6".

[0026] (Example 4: Filler High) In Example 4, contrary to Example 3, the amount of the filler in Example 1 was increased from "60 parts by weight" to "70 parts by weight." At this time, the amount of elastomer in Example 1 was reduced from "7 parts by weight" to "5 parts by weight", and the amount of branched olefin was reduced from "2 parts by weight" to "1.5 parts by weight". As a result, the "elastomer / branched olefin" ratio was reduced from "3.5" to "3.3".

[0027] (Example 5: Elastomer Low) In Example 5, the amount of the elastomer blended in Example 1 was reduced from "7 parts by weight" to "4 parts by weight." At this time, the blending amount of the branched olefin in Example 1 was increased from "2 parts by weight" to "2.5 parts by weight", and as a result, the "elastomer / branched olefin" was decreased from "3.5" to "1.6". (Example 6: High Elastomer) In Example 6, contrary to Example 5, the amount of the elastomer in Example 1 was increased from "7 parts by weight" to "12 parts by weight." At this time, the blending amount of the branched olefin in Example 1 was increased from "2 parts by weight" to "2.5 parts by weight", and as a result, the "elastomer / branched olefin" increased from "3.5" to "4.8".

[0028] (Example 7: Low branched olefin) In Example 7, the amount of the branched olefin in Example 1 was reduced from "2 parts by weight" to "1.2 parts by weight." At this time, the amount of the elastomer in Example 1 was reduced from "7 parts by weight" to "5 parts by weight", and as a result, the "elastomer / branched olefin" increased from "3.5" to "4.2". (Example 8: High branched olefins) In Example 8, contrary to Example 7, the blending amount of the branched olefin in Example 1 was increased from "2 parts by weight" to "4 parts by weight." At this time, the blending amount of the elastomer in Example 1 was reduced from "7 parts by weight" to "5 parts by weight", and as a result, the "elastomer / branched olefin" was reduced from "3.5" to "1.3".

[0029] (Example 9: Elastomer / Low Branched Olefin) Example 9 reduced the "Elastomer / Branched Olefins" in Example 1 from "3.5" to "1.0". At this time, the blending amount of the elastomer in Example 1 was decreased from "7 parts by weight" to "4 parts by weight", and the blending amount of the branched olefin was increased from "2 parts by weight" to "4 parts by weight". (Example 10: Elastomer / High Branched Olefin) In Example 10, unlike Example 9, the "Elastomer / branched olefin" in Example 1 was increased from "3.5" to "5.0". At this time, the blending amount of the elastomer in Example 1 was increased from "7 parts by weight" to "8 parts by weight", and the blending amount of the branched olefin was decreased from "2 parts by weight" to "1.6 parts by weight".

[0030] (Comparative Example 1: Low aspect ratio) Comparative Example 1 is the same as Example 1, except that the aspect ratio of the filler in Example 1 was reduced from "80" to "9". (Comparative Example 2: Low filler) Comparative Examples 2 to 9 are the same as Comparative Example 1 except that the material composition in Comparative Example 1 was changed. The changes in other parameters when the setting is changed are as shown in Table 1 below, and so a description thereof will be omitted. First, in Comparative Example 2, the amount of the filler in Comparative Example 1 was reduced from "60 parts by weight" to "40 parts by weight." (Comparative Example 3: High Filler) In Comparative Example 3, contrary to Comparative Example 2, the blending amount of the filler in Comparative Example 1 was increased from "60 parts by weight" to "80 parts by weight."

[0031] (Comparative Example 4: Low Elastomer) In Comparative Example 4, the amount of the elastomer in Comparative Example 1 was reduced from "7 parts by weight" to "3 parts by weight." (Comparative Example 5: High Elastomer) In Comparative Example 5, unlike Comparative Example 4, the blending amount of the elastomer in Comparative Example 1 was increased from "7 parts by weight" to "13 parts by weight." (Comparative Example 6: Low branched olefin) In Comparative Example 6, the amount of the branched olefin in Comparative Example 1 was reduced from "2 parts by weight" to "1 part by weight." (Comparative Example 7: High Branched Olefins) In Comparative Example 7, contrary to Comparative Example 6, the blending amount of the branched olefin in Comparative Example 1 was increased from "2 parts by weight" to "4 parts by weight." (Comparative Example 8: Elastomer / Low Branched Olefin) In Comparative Example 8, the "Elastomer / branched olefin" in Comparative Example 1 was reduced from "3.5" to "0.8". (Comparative Example 9: Elastomer / High Branched Olefin) In Comparative Example 9, unlike Comparative Example 8, the "elastomer / branched olefin" in Comparative Example 1 was increased from "3.5" to "5.2".

[0032] (Evaluation method) The above-mentioned Examples 1 to 10 and Comparative Examples 1 to 9 were evaluated for four items: (1) bending strength, (2) bending elasticity, (3) MD (machine direction) linear expansion coefficient, and (4) TD (transverse direction) linear expansion coefficient. (Thermal expansion measurement) The linear expansion coefficient was evaluated for the above-mentioned Examples 1 to 10 and Comparative Examples 1 to 9. The linear expansion coefficient was evaluated by calculating the linear expansion coefficient in the temperature range of 10°C to 70°C using a thermomechanical analyzer TMA (product name).

[0033] (Criteria and Results) As described in the embodiment, a bending strength of 30 MPa or more was considered to be acceptable, and a bending strength of less than 30 MPa was considered to be unacceptable. As explained in the embodiment, the flexural modulus was considered to be acceptable in the range of 2000 to 9000 MPa, and was considered to be unacceptable in the cases of less than 2000 MPa and more than 9000 MPa. The linear expansion coefficient is divided into MD (machine direction) and TD (transverse direction), and is at least 6.0×10 -5 The following cases are considered to be acceptable: 6.0 x 10 -5 If it exceeded this, it was considered a failure. The evaluation results are shown in Table 1.

[0034] [Table 1]

[0035] (About bending strength) As for the bending strength, as shown in Table 1, all of the bending strengths of Examples 1 to 10 were 30 MPa or more, which was acceptable. In contrast, among Comparative Examples 1 to 9, the three pieces of Comparative Example 1, Comparative Example 2 and Comparative Example 9 had bending strengths of 30 MPa or more and passed the test. However, the remaining Comparative Examples 3 to 8 had bending strengths of less than 30 MPa, failing the test and showing insufficient bending strength. In Comparative Example 3, it can be assumed that the filler content was too high at "80 parts by weight". In Comparative Example 4, it can be assumed that the elastomer content was too low at "3 parts by weight". In Comparative Example 6, it can be assumed that the branched olefin content was too low at "1 part by weight". In Comparative Example 7, it can be assumed that the elastomer content was too low at "8 parts by weight". In Comparative Example 8, it can be assumed that the "elastomer / branched olefin" was too low at "0.8".

[0036] (About bending elasticity) Concerning the flexural modulus, all of Examples 1 to 10 had a flexural modulus within the range of 2000 to 9000 MPa, which was acceptable. In contrast, among Comparative Examples 1 to 9, the bending elasticity of Comparative Example 1, Comparative Example 2, Comparative Example 4, and Comparative Examples 6 to 8 was within the range of 2000 to 9000 MPa, and therefore passed the test. However, the remaining Comparative Examples 3, 5, and 9 were less than 2000 MPa or more than 9000 MPa, failing the test. In Comparative Example 3, it is presumed that the filler content was too high at "80 parts by weight." In Comparative Example 9, it is presumed that the "elastomer / branched olefin" was too high at "5.2."

[0037] (MD / TD linear expansion coefficient) The linear expansion coefficients in the MD and TD directions are all 6.0×10 -5 The following was a passing grade. In contrast, in Comparative Examples 1 to 9, the linear expansion coefficients of Comparative Examples 3 to 9 were 6.0 × 10 -5 The following was a passing grade. However, the remaining Comparative Examples 1 and 2 were 6.0×10 -5 and failed. In Comparative Example 1, it can be assumed that the aspect ratio of the filler was too low at "9". In Comparative Example 2, it can be assumed that the blending amount of the filler was too low at "40 parts by weight".

[0038] (comprehensive evaluation) Among Examples 1 to 10, Example 6 has an elastomer content of "12 parts by weight," which is within the range of 10 to 30% by weight that is preferred in the embodiment described above. As a result, the linear expansion coefficient is 6.0 × 10 -5 It was below that level and remained at a low level. In addition, among Examples 1 to 10, Examples 8 and 6 both had a branched olefin blend ratio of "4 parts by weight," which is within the range of 3 to 10% by weight that is preferred in the embodiment. As a result, the linear expansion coefficient was 6.0 × 10 -5 It was below that level and remained at a low level. In summary, only Examples 1 to 10 satisfied all four of the conditions (1) to (4). [Explanation of symbols]

[0039] 10 Cosmetic materials 20 Base material 21 Surface layer 22 Foam layer 30 Decorative Sheet 31 Design Layer 32 Lamination 33 Top Coat 40 Adhesive layer

Claims

1. A decorative material comprising a substrate and a decorative sheet laminated on the substrate, The substrate includes a thermoplastic resin and a scaly filler and has a cell structure; The linear expansion coefficient is 6.0×10 in at least the width direction among the machine direction and the width direction. -5 is as follows: The filler is contained in an amount of 50 to 70% by weight, The substrate has a bending strength of 30 MPa or more and a bending elasticity in the range of 2000 to 9000 MPa, The base material contains an olefin-based elastomer having a melt flow rate (MFR) of 300 or more as a first additive, in an amount of 10 to 18% by weight based on the weight of the base material excluding the filler, a branched olefin as a second additive, the second additive being present in an amount of 3 to 6.3 wt. % based on the weight of the base material excluding the filler; the ratio of the first additive to the second additive is in the range of 5:1 to 3.3:1, alternatively in the range of 1.6:1 to 1:1; A decorative material, characterized in that the thermoplastic resin of the substrate is ABS resin, ethylene propylene diene rubber, ethylene vinyl acetate, or silicone rubber.

2. 2. The decorative material according to claim 1, wherein the substrate has a width of 500 mm or more and a length of 500 mm or more.

3. 3. The decorative material according to claim 1, wherein the filler has an average aspect ratio of 10 or more, calculated from the average diameter / thickness of the plate surface.

4. 4. The decorative material according to claim 1, wherein the substrate has a bending strength of 42 MPa or more.

5. 5. The decorative material according to claim 4, wherein the substrate has a bending strength of 52 MPa or less.

6. The decorative material according to any one of claims 1 to 5, characterized in that the substrate has a flexural modulus in the range of 4360 to 9000 MPa.

Citation Information

Patent Citations

  • Floor material for exterior

    JP2006299734A

  • Foam molded body and its manufacturing process

    JP2008105342A

  • Polylactic acid-based foam molding composition and polylactic acid-based foam molded product obtained therefrom

    JP2008231184A

  • Multi-layer surface coating

    JP2015516320A

  • flooring

    JP3932883B2