Method for producing porous hollow fiber membrane

A polyolefin-based porous hollow fiber membrane with controlled shrinkage addresses the issue of performance deterioration and breakage during cleaning, enhancing durability and extending the life of water treatment elements.

JP7562983B2Active Publication Date: 2024-10-08MITSUBISHI CHEM CORP
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2020073459
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-04-16
Publication Date
2024-10-08
Estimated Expiration
2040-04-16

AI Technical Summary

Technical Problem

Porous hollow fiber membranes used in water treatment face performance deterioration and breakage due to drying and shrinkage when lifted from treatment tanks for cleaning, leading to reduced product life.

Method used

A porous hollow fiber membrane made of polyolefin resin with a shrinkage rate of 3% or less, glass transition temperature of 40°C or less, and a production method involving spinning, stretching, and thermal relaxation steps to minimize shrinkage during drying.

Benefits of technology

The membrane maintains performance and reduces breakage by minimizing shrinkage upon drying, extending the life and reducing the need for replacements.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007562983000002
    Figure 0007562983000002
  • Figure 0007562983000001
    Figure 0007562983000001
Patent Text Reader

Abstract

To provide a porous hollow fiber membrane which can extend a product life of a hollow fiber membrane element.SOLUTION: A porous hollow fiber membrane is composed of a polyolefin resin and has a contraction ratio obtained by the following measurement method of 3% or less. Measurement method: A porous hollow fiber membrane having a length of 400 mm is immersed in ethanol for 10 minutes, is immersed in pure water for 10 minutes, is dried under an atmosphere of 60°C for 30 minutes, and then is immersed at a room temperature for 5 minutes, and a length L1 (unit: mm) of the treated porous hollow fiber membrane is measured, and a contraction ratio (unit: %) is calculated by the following expression (I): Contraction ratio=(400-L1) / 400×100.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a porous hollow fiber membrane, a method for producing the same, and a hollow fiber membrane element having the porous hollow fiber membrane. [Background technology]

[0002] For example, porous hollow fiber membranes are preferably used for purification treatment of domestic wastewater, industrial wastewater, etc. Porous hollow fiber membranes are often used in the form of a hollow fiber membrane element in which a plurality of porous hollow fiber membranes are aligned in one direction and integrally held.

[0003] In water treatment using a porous hollow fiber membrane, a hollow fiber membrane element is immersed in a treatment tank that stores the water to be treated, and, for example, the water to be treated is sucked from the outside to the inside of the porous hollow fiber membrane, thereby capturing pollutants on the outer surface of the porous hollow fiber membrane. In order to prevent the porous hollow fiber membranes from becoming clogged with contaminants, the hollow fiber membrane elements are washed as necessary. Here, for example, Patent Document 1 describes a method of pulling up a hollow fiber membrane element from a treatment tank of a wastewater treatment system and washing it. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2013-31839 A Summary of the Invention [Problem to be solved by the invention]

[0005] If the hollow fiber membrane element is repeatedly removed from the treatment tank, washed, and then immersed in the treatment tank again for use, its performance may deteriorate and the porous hollow fiber membrane may break, making it necessary to replace it with a new one. According to the inventors' findings, when a hollow fiber membrane element is removed from a treatment tank and subjected to a cleaning operation in air, the porous hollow fiber membrane may dry out and shrink, and if the porous hollow fiber membrane shrinks significantly, performance degradation and fiber breakage are likely to occur. An object of the present invention is to provide a porous hollow fiber membrane capable of extending the product life of a hollow fiber membrane element, a method for producing the same, and a hollow fiber membrane element having the porous hollow fiber membrane. [Means for solving the problem]

[0006] [1] A porous hollow fiber membrane made of a polyolefin resin and having a shrinkage rate of 3% or less as measured by the following method. Measurement method: A porous hollow fiber membrane with a length of 400 mm is immersed in ethanol for 10 minutes, then immersed in pure water for 10 minutes, dried in an atmosphere at 60°C for 30 minutes, and then cooled at room temperature for 5 minutes. The length L1 (unit: mm) of the porous hollow fiber membrane after the treatment is measured, and the shrinkage rate (unit: %) is calculated using the following formula (I). Contraction rate = (400-L1) / 400×100 (I) [2] The porous hollow fiber membrane of [1], wherein the polyolefin resin has a glass transition temperature of 40°C or lower. [3] The porous hollow fiber membrane according to [1] or [2], wherein the polyolefin resin contains polyethylene. [4] A hollow fiber membrane element comprising a plurality of the porous hollow fiber membranes according to any one of [1] to [3] and water collection pipes connected to both ends of the plurality of porous hollow fiber membranes. [5] A method for producing a porous hollow fiber membrane according to any one of claims 1 to 3, comprising a spinning step of melt-spinning a raw material containing the polyolefin resin to obtain a hollow fiber, a stretching step of stretching the hollow fiber to obtain a hollow fiber membrane, and a heat-relaxing step of heat-relaxing the hollow fiber membrane. Effect of the Invention

[0007] The porous hollow fiber membrane of the present invention has a small shrinkage rate when immersed in water and then dried, and is therefore less susceptible to performance degradation and fiber breakage due to washing. The hollow fiber membrane element of the present invention has a small shrinkage rate of the porous hollow fiber membrane when immersed in water and then dried, and therefore is less susceptible to performance degradation and fiber breakage due to washing. According to the method for producing a porous hollow fiber membrane of the present invention, a porous hollow fiber membrane having a small shrinkage rate when immersed in water and then dried can be obtained. [Brief description of the drawings]

[0008] [Figure 1] FIG. 1 is a plan view showing an example of a hollow fiber membrane element of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0009] <Porous hollow fiber membrane> The porous hollow fiber membrane of this embodiment is made of a polyolefin resin. In this specification, a polyolefin resin is a polymer consisting of one or more types of units based on an alkene (wherein some of the hydrogen atoms may be replaced by fluorine atoms). Examples of polyolefin resins include polyethylene, polypropylene, poly-4-methylpentene-1, polyvinylidene fluoride, and polyolefin copolymer resins. The polyolefin resin constituting the porous hollow fiber membrane may be one type or a mixture of two or more types. In addition, it may be a mixture with a resin other than the polyolefin resin, an organic material, or an inorganic material. From the viewpoint of ease of melt-spinning porosity that can suppress elution from the membrane material during liquid filtration, it is preferable that the polyolefin resin constituting the porous hollow fiber membrane contains polyethylene or polypropylene, and it is more preferable that it contains polyethylene in particular.

[0010] Generally, the membrane filtration temperature in water treatment is often 40°C or lower. If the use temperature of the porous hollow fiber membrane is higher than the glass transition temperature, the polymer chains constituting the porous hollow fiber membrane are mobile, and residual stress is likely to occur. The residual stress causes the porous hollow fiber membrane to shrink. Therefore, if the glass transition temperature (hereinafter also referred to as Tg) of the polyolefin resin constituting the porous hollow fiber membrane is 40°C or lower, the effect of applying the present invention is easily obtained. Specific examples of polyolefin resins having a Tg of 40° C. or less include polyethylene (Tg: −125° C.) and polypropylene (Tg: 0° C.). When the porous hollow fiber membrane is composed of two or more types of polyolefin resins, it is preferable that the Tg of each of them is 40° C. or lower.

[0011] The porous hollow fiber membrane of the present embodiment may have a coating layer on at least a part of the surface (outer surface, inner surface, and surface inside the pores) of the hollow fiber membrane made of the polyolefin resin. For example, a hydrophilic resin, a surfactant, inorganic particles, etc. may be present on the surface of the porous hollow fiber membrane.

[0012] The average pore size of the porous hollow fiber membrane is not particularly limited, and is preferably, for example, 0.02 to 0.5 μm. In this specification, the average pore size of the porous hollow fiber membrane is the peak value in the pore size distribution obtained using a pore size distribution measuring device in accordance with JIS K 3832.

[0013] The outer and inner diameters of the porous hollow fiber membrane are not particularly limited. They can be selected as desired depending on the intended use, element shape, etc. In general, the outer diameter is often selected in the range of about 300 to 1000 μm.

[0014] The porous hollow fiber membrane of the present embodiment has a shrinkage rate of 3% or less, measured by the following measurement method. The lower the shrinkage rate, the more excellent the dimensional stability. The shrinkage rate is preferably 2% or less, and more preferably 1.5% or less.

[0015] Shrinkage rate measurement method: A porous hollow fiber membrane with a length of 400 mm is immersed in ethanol for 10 minutes, then immersed in pure water for 10 minutes, dried in an atmosphere at 60°C for 30 minutes, and then cooled at room temperature for 5 minutes. The length L1 (unit: mm) of the porous hollow fiber membrane after the treatment is measured, and the shrinkage rate (unit: %) is calculated according to the following formula (I). Contraction rate = (400-L1) / 400×100 (I)

[0016] The shrinkage rate is specifically measured by the following method. (1) First, cut a porous hollow fiber membrane (one filament) to a length of 500 mm to prepare a test specimen. Fix one end of the test specimen and allow the other end to hang down under its own weight. With a load of 50 mg / dtex applied to the tip of the other end, a mark is made on a 400 mm long section (measurement section) excluding both ends. (2) Next, an immersion treatment is performed: the test specimen is immersed in ethanol (room temperature) for 10 minutes, then removed, and then immersed in pure water (room temperature) for 10 minutes, then removed. With one end of the test specimen fixed and the other end hanging down under its own weight, it is dried in a dryer at an ambient temperature of 60°C for 30 minutes, and then cooled at room temperature for 5 minutes. (3) Next, in the same manner as in (1) above, a load of 50 mg / dtex is applied to the tip of the other end of the test specimen, and the length L1 (unit: mm) of the measurement portion marked in (1) above is measured. (4) The shrinkage rate is calculated according to the above formula (I). In this specification, "room temperature" means a temperature within the range of 23°C ± 2°C unless otherwise specified.

[0017] The porous hollow fiber membrane of this embodiment may or may not be provided with a support (for example, a fibrous material such as a knitted cord or braided cord) for reinforcing the hollow fiber membrane. A porous hollow fiber membrane without a support is preferable because the effects of the present invention are predominant.

[0018] <Method for producing porous hollow fiber membrane> The porous hollow fiber membrane of the present embodiment is produced by a method including a spinning step of melt-spinning a raw material containing a polyolefin resin to obtain a hollow fiber, a stretching step of stretching the hollow fiber to obtain a hollow fiber membrane, and a heat-relaxing step of heat-relaxing the hollow fiber membrane. An optional step may be provided between the spinning step and the stretching step. An optional step may be provided between the stretching step and the heat-relaxing step. After the heat-relaxing step, an optional step not involving stretching may be performed.

[0019] [Spinning process to drawing process] From the spinning step to the drawing step, known methods can be used. For example, a raw material containing a polyolefin resin is melt-spun, cooled and solidified to obtain hollow fibers, and the hollow fibers are stretched to form a porous hollow fiber membrane having interconnected slit-shaped micropores from the inner surface to the outer surface. For example, the method described in paragraphs 0033 to 0049 of Japanese Patent Application No. 2017-081783 can be used.

[0020] In the stretching step, the hollow fibers are heated and stretched while being transported to form hollow fiber membranes. The ambient temperature during stretching (stretching temperature t) is preferably equal to or lower than the Vicat softening point of the polyolefin resin constituting the hollow fiber. If the stretching temperature t is equal to or lower than the Vicat softening point, the pore size of the porous hollow fiber membrane is easily enlarged. If the stretching temperature t exceeds the Vicat softening point, the pores may be blocked.

[0021] After the spinning step, the hollow fibers are preferably subjected to an annealing treatment (fixed length heat treatment) prior to the drawing step. In the annealing treatment, it is preferable to heat the hollow fiber in a wound state. The heating temperature (ambient temperature) during the annealing treatment is set to be equal to or lower than the melting point of the polyolefin resin constituting the hollow fiber. For example, when polyethylene is used as the polyolefin resin, it is preferable to heat the hollow fibers at an atmospheric temperature of 105 to 130° C. for 8 to 16 hours.

[0022] When the annealing treatment is performed, it is preferable to perform cold stretching after the annealing treatment, and then perform stretching (hot stretching) at the stretching temperature t. Cold stretching is a stretching method that breaks down the membrane structure at a relatively low temperature and generates micro cracks. The atmospheric temperature during cold stretching is preferably at least 20°C lower than the Vicat softening point of the polyolefin resin that constitutes the hollow fiber (Vicat softening point -20°C or lower). The lower limit is preferably 0°C or higher. The stretching ratio in cold stretching is preferably 1.2 to 1.8 times. The stretching process when annealing and cold stretching are performed may be a two-stage stretching in which cold stretching is followed by hot stretching, or a multi-stage stretching in which cold stretching is followed by hot stretching divided into two or more stages.

[0023] The total stretching ratio of the porous hollow fiber membrane to the hollow fiber is preferably 2 to 5. If the total stretching ratio is 2 or more, the porosity tends to be high, and if it is 5 or less, the breaking elongation tends to be high.

[0024] [Thermal relaxation process] In the heat-relaxing step, the hollow fiber membrane is heated (heat-relaxing treatment) at a temperature at which the residual stress generated in the stretching step can be relaxed, and then cooled. It is preferable to heat the hollow fiber membrane while transporting it. It is preferable to heat the hollow fiber membrane in a relaxed state by making the winding speed slower than the delivery speed. The atmospheric temperature in the heat-relaxing treatment (heat-relaxing temperature T) is set to be equal to or lower than the melting point of the polyolefin resin constituting the hollow fiber membrane. The difference between the heat-relaxing temperature T and the melting point is preferably 5 to 35°C. In the heat-relaxing treatment, the relaxation rate (unit: %) expressed by (1-winding speed / delivering speed) x 100 is 0% or more, preferably 0 to 35%, and more preferably 10 to 20%. A relaxation rate within the above range is preferable in terms of achieving both production stability and shrinkage rate and film performance.

[0025] In the heat-relaxing step, the heat-relaxing treatment may be performed multiple times. The conditions for the multiple heat-relaxing treatments may be the same or different, and from the viewpoints of production and quality stability, it is preferable to carry out the heat-relaxing treatment two or more times.

[0026] In one heat-relaxing treatment, the time (heating time) during which the hollow fiber membrane is in an atmosphere at the heat-relaxing temperature T is preferably 5 seconds to 10 minutes, and more preferably 10 seconds to 5 minutes. Within the above range, the residual stress can be sufficiently reduced and the membrane can be produced with good productivity.

[0027] In the heat-relaxing step, the shrinkage rate of the porous hollow fiber membrane can be adjusted by changing one or more of the heat-relaxing temperature T, the relaxation rate, the heating time, and the number of heat-relaxing treatments. For example, increasing the heat relaxation temperature T tends to decrease the shrinkage rate. Increasing the heat relaxation rate tends to decrease the shrinkage rate. Increasing the heating time tends to decrease the shrinkage rate. Increasing the number of heat relaxation treatments tends to decrease the shrinkage rate.

[0028] [Hydrophilization process] If necessary, the hollow fiber membrane can be subjected to a hydrophilization treatment to impart hydrophilicity to the porous hollow fiber membrane. The hydrophilization treatment can be carried out by a known method. For example, at least a part of the surface of the hollow fiber membrane (the outer surface, the inner surface, and the surface inside the pores) can be hydrophilized by coating with a hydrophilic resin. Specifically, the method described in paragraph 0029 of Japanese Patent No. 3628446 can be used.

[0029] The hydrophilization treatment may be carried out after the stretching step and before the heat-relaxing step, after the stretching step and the heat-relaxing step, or during the heat-relaxing step. In other words, when the heat-relaxing step includes a plurality of heat-relaxing treatments, the hydrophilization treatment may be carried out between the heat-relaxing treatments.

[0030] <Hollow fiber membrane element> The hollow fiber membrane element of this embodiment has a plurality of porous hollow fiber membranes and water collection pipes connected to both ends of the plurality of porous hollow fiber membranes. FIG. 1 is a plan view showing one embodiment of the hollow fiber membrane element of the present embodiment. The hollow fiber membrane element of this embodiment comprises a sheet material 2 in which a plurality of porous hollow fiber membranes 1 are aligned in one direction, and water collection pipes 3 and 4 respectively provided at both ends of the sheet material 2 in the longitudinal direction of the porous hollow fiber membranes 1. Both ends in the longitudinal direction of the porous hollow fiber membrane 1 are open, and the porous hollow fiber membrane 1 communicates with the water collection pipes 3 and 4. Specifically, a linear slit (not shown) is provided in the pipe wall of the water collection pipes 3 and 4 along the longitudinal direction of the water collection pipes 3 and 4. An end of the sheet-like material 2 is inserted into this slit, and while the opening of the porous hollow fiber membrane 1 is maintained, the end of the sheet-like material 2 and the water collection pipe 3 (4) are fixed with a potting material such as a cured resin. In this embodiment, the filtrate that has passed from the outside to the inside of the porous hollow fiber membrane 1 passes through water collection pipes 3 and 4 and is discharged to the outside of the hollow fiber membrane element.

[0031] The hollow fiber membrane element of this embodiment is suitable for use as a component of a water treatment device, for example, a component of a water treatment device used for purifying domestic wastewater, industrial wastewater, and the like. The hollow fiber membrane element of this embodiment is preferably used in the form of a hollow fiber membrane module configured so that a plurality of hollow fiber membrane elements can be handled as an integrated unit. For example, a hollow fiber membrane module includes a plurality of hollow fiber membrane elements and a support member that integrally supports the plurality of hollow fiber membrane elements. The support member may also serve as a water collection pipe (main pipe) that communicates with the water collection pipes (branch pipes) of each hollow fiber membrane element. The hollow fiber membrane module and the water treatment device may have a known configuration.

[0032] The porous hollow fiber membrane constituting the hollow fiber membrane element of this embodiment has a small shrinkage rate when immersed in water and then dried, so performance degradation and fiber breakage due to cleaning are unlikely to occur, and the hollow fiber membrane element can have a longer life and require fewer replacements. EXAMPLES

[0033] The present invention will be described in more detail below using examples, but the present invention is not limited to these examples.

[0034] (Reference example) Polyethylene (density 0.965g / cm 3 The raw material was a polyester fiber (polyethylene glycol terephthalate, MFR: 0.7 g / 10 min, Tg: -125°C, Vicat softening point: 128°C), which was melt-spun using a nozzle for producing hollow fiber membranes and then cooled and solidified to obtain hollow fibers with an inner diameter of 609 μm and a membrane thickness of 161 μm. The hollow fiber was wound on a bobbin and annealed at 115°C for 16 hours. The annealed hollow fiber was cold-stretched at room temperature to a stretch ratio of 1.8, then hot-stretched at a stretching temperature of 114°C, and hydrophilized to obtain a porous hollow fiber membrane. The stretch ratio of the hot stretching was set so that the total stretch ratio including the cold stretching was 6.6. The outer diameter, inner diameter, and average pore size of the obtained porous hollow fiber membrane are shown in Table 1. In addition, the shrinkage rate of the obtained porous hollow fiber membrane was measured by the above-mentioned method. The results are shown in Table 1 (the same applies below).

[0035] (Example 1) A hollow fiber was produced, annealed, cold-stretched, hot-stretched, and hydrophilized in the same manner as in Reference Example 1. The resulting hollow fiber membrane was subjected to a heat-relaxation treatment under conditions of a heat-relaxation temperature of 118°C and a relaxation rate of 0%, to obtain a porous hollow fiber membrane.

[0036] (Example 2) A porous hollow fiber membrane was obtained in the same manner as in Example 1, except that the relaxation rate of the heat-relaxing treatment was changed to 15%.

[0037] (Example 3) A hollow fiber was produced, annealed, cold stretched, and hot stretched in the same manner as in Reference Example 1. The obtained hollow fiber membrane was subjected to a first heat relaxation treatment under conditions of a heat relaxation temperature of 118°C and a relaxation rate of 20%, and then to a hydrophilization treatment in the same manner as in Reference Example 1. The hollow fiber membrane after the hydrophilization treatment was subjected to a second heat relaxation treatment under conditions of a heat relaxation temperature of 90°C and a relaxation rate of 0%, to obtain a porous hollow fiber membrane.

[0038] (Example 4) A porous hollow fiber membrane was obtained in the same manner as in Example 3, except that the heat-relaxing temperature in the second heat-relaxing treatment was changed to 110°C.

[0039] (Example 5) A porous hollow fiber membrane was obtained in the same manner as in Example 4, except that the relaxation rate in the second heat-relaxing treatment was changed to 3%.

[0040] [Table 1]

[0041] As shown in Table 1, the shrinkage rate of the porous hollow fiber membrane could be adjusted to 3% or less by changing the conditions of the heat relaxation treatment. [Explanation of symbols]

[0042] 1. Porous hollow fiber membrane 2. Sheet-like object 3, 4 Water collection pipe

Claims

1. A spinning process for melt-spinning a raw material containing a polyolefin resin to obtain a hollow fiber; a stretching step of stretching the hollow fiber to obtain a hollow fiber membrane; a first heat-relaxing step of heat-relaxing the hollow fiber membrane after the stretching step; a hydrophilization step of hydrophilizing the hollow fiber membrane after the first heat relaxation step; A method for producing a porous hollow fiber membrane having a shrinkage rate of 3% or less as measured by the following measurement method, the method comprising: a second heat-relaxing step of heat-relaxing the hollow fiber membrane after the hydrophilization step, A method for producing a porous hollow fiber membrane, wherein a relaxation rate in the first heat-relaxing step is higher than a relaxation rate in the second heat-relaxing step. Measurement method: A porous hollow fiber membrane having a length of 400 mm is immersed in ethanol for 10 minutes, then immersed in pure water for 10 minutes, dried in an atmosphere at 60°C for 30 minutes, and then cooled at room temperature for 5 minutes. The length L1 (unit: mm) of the porous hollow fiber membrane after the treatment is measured, and the shrinkage rate (unit: %) is calculated by the following formula (I). Shrinkage rate = (400 - L1) / 400 x 100 ... (I)

2. 2. The method for producing a porous hollow fiber membrane according to claim 1, wherein the heat-relaxing treatment is a treatment of heating the hollow fiber membrane in an atmosphere having a heat-relaxing temperature T, the heat-relaxing temperature T being equal to or lower than a melting point of a polyolefin resin constituting the hollow fiber membrane, and a difference between the heat-relaxing temperature T and the melting point is 5 to 35° C.

Citation Information

Patent Citations

  • Porous hollow yarn made of polyethylene

    JP1987221401A

  • Heat resistant polyethylene porous membrane and its preparation

    JP1989051101A

  • Manufacture of hollow-fiber membrane module, hollow- fiber membrane module, and hollow-fiber membrane module unit using the same

    JP2000288357A

  • Filtration membrane washing agent and method for washing filtration membrane

    JP2013031839A

  • Filtration module and filtration device

    WO2018092342A1