Magnetic recording medium, magnetic recording / reproducing device, and magnetic recording medium cartridge
The magnetic recording medium with a polyester base and optimized magnetic layer properties, combined with a specialized apparatus, addresses the need for higher data density by enhancing electromagnetic conversion and signal accuracy in magnetic recording.
Patent Information
- Application Number
- JP2020202320
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-12-04
- Publication Date
- 2024-10-08
- Estimated Expiration
- 2039-10-01
AI Technical Summary
There is a demand for magnetic recording media that can achieve higher data density as the amount of data to be recorded increases.
A magnetic recording medium with a base body containing polyester, a magnetic layer with specific surface roughness and thickness, and magnetic powders with controlled coercive forces and aspect ratios, optimized for perpendicular magnetic recording, along with a magnetic recording and reproducing apparatus and cartridge designed for high-density data storage.
The solution enables high-density data recording with improved electromagnetic conversion characteristics, reduced magnetization transition width, and enhanced signal-to-noise ratio, facilitating accurate data reading and increased recording capacity.
Smart Images

Figure 0007563148000005 
Figure 0007563148000006 
Figure 0007563148000007
Abstract
Description
[Technical field]
[0001] The present disclosure relates to a magnetic recording medium, as well as a magnetic recording / reproducing device and a magnetic recording medium cartridge using the same. [Background technology]
[0002] Tape-shaped magnetic recording media having a magnetic layer are widely used for storing electronic data. The magnetic layer of the magnetic recording media is provided with a data band including a plurality of recording tracks, and data is recorded on the recording tracks. The magnetic layer is also provided with a servo band at a position adjacent to the data band in the width direction, and a servo signal is recorded on the servo band. The magnetic head is aligned with respect to the recording tracks by reading the servo signal recorded on the servo band.
[0003] Known methods of recording data on a magnetic recording medium include a horizontal magnetic recording method in which magnetic particles in a magnetic layer are magnetized in a horizontal direction to record data, and a perpendicular magnetic recording method in which magnetic particles in a magnetic layer are magnetized in a vertical direction to record data. In general, the perpendicular magnetic recording method can record data at a higher density than the horizontal magnetic recording method. The present applicant has disclosed a technology for obtaining a reproduced waveform of a servo signal having good symmetry when the magnetization direction of the servo signal includes a perpendicular component (see, for example, Patent Document 1). [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2014-199706 A Summary of the Invention [Problem to be solved by the invention]
[0005] In recent years, as the amount of data to be recorded increases, there is a demand for even higher density recording, and therefore a magnetic recording medium capable of achieving even higher density recording is desired. [Means for solving the problem]
[0006] A magnetic recording medium according to an embodiment of the present disclosure is a tape-shaped magnetic recording medium, which includes a substrate containing polyester as a main component, and a magnetic layer provided on the substrate, containing a plurality of magnetic powders, and capable of recording data signals. Here, the arithmetic mean roughness Ra of the surface of the magnetic layer is 2.5 nm or less. The PSD (Power Spectrum Density) of the magnetic layer up to a spatial wavelength of 5 μm is 2.5 μm or less. The average thickness of the magnetic layer is 90 nm or less. The average aspect ratio of the magnetic powder is 1.0 to 3.0. The magnetic recording medium has a coercive force in the perpendicular direction of 3000 Oersteds or less. The ratio of the coercive force in the longitudinal direction to the coercive force in the perpendicular direction of the magnetic recording medium is 0.8 or less. The half-width of an isolated waveform in the reproduced waveform of the data signal is 200 nm or less.
[0007] A magnetic recording and reproducing device according to one embodiment of the present disclosure includes a feed section capable of sequentially feeding out the above-mentioned magnetic recording medium, a winding section capable of winding up the magnetic recording medium fed out from the feed section, and a magnetic head capable of writing information to the magnetic recording medium and reading information from the magnetic recording medium while coming into contact with the magnetic recording medium traveling from the feed section to the winding section.
[0008] A magnetic recording medium cartridge according to an embodiment of the present disclosure includes the above-mentioned magnetic recording medium and a housing that houses the magnetic recording medium.
[0009] The magnetic recording medium, magnetic recording and reproducing device, and magnetic recording medium cartridge according to an embodiment of the present disclosure have the above-mentioned configurations, and are therefore advantageous for high-density data recording. [Brief description of the drawings]
[0010] [Figure 1] 1 is a cross-sectional view of a magnetic recording medium according to an embodiment of the present disclosure. [Diagram 2] FIG. 2 is a cross-sectional view that typically illustrates the cross-sectional structure of an ε iron oxide particle contained in the magnetic layer shown in FIG. [Diagram 3] 2 is a graph showing an example of an SFD curve of the magnetic recording medium shown in FIG. [Figure 4] 2 is a schematic explanatory diagram showing the layout of a data band and a servo band in the magnetic recording medium shown in FIG. [Diagram 5] FIG. 5 is an enlarged schematic explanatory diagram showing the data band shown in FIG. 4. [Figure 6] 5 is a schematic explanatory diagram showing an enlarged view of a servo signal recording pattern in the servo band shown in FIG. 4. [Figure 7] 2 is a schematic diagram of a recording / reproducing device that uses the magnetic recording medium shown in FIG. [Figure 8] 2 is a schematic diagram of a servo signal recording device for recording a servo signal on the magnetic recording medium shown in FIG. 1. [Figure 9] 9 is an enlarged schematic diagram showing the configuration of a main part of the servo signal recording device shown in FIG. 8. [Figure 10] 9 is a schematic diagram showing the direction of magnetization of a magnetic recording medium that is demagnetized in the servo signal recording device shown in FIG. 8. [Figure 11] 9 is an explanatory diagram showing the relationship between the magnetization direction of a magnetic recording medium written in the servo signal recording device shown in FIG. 8 and the reproduced waveform of a servo signal. [Figure 12] FIG. 13 is a diagram for explaining a half-value width in an isolated waveform. [Figure 13] FIG. 1 is a diagram for explaining the basic concept of the present technology, showing two stripes in a servo signal recording pattern. [Figure 14] FIG. 11 is a cross-sectional view that typically illustrates a cross-sectional structure of an ε-iron oxide particle as a modified example. [Figure 15] 2 is a schematic diagram showing an inner end of a magnetic recording medium attached to a reel of a magnetic recording medium cartridge. FIG. [Figure 16] 5 is a schematic diagram of a data band and a servo band for explaining a method of measuring the deviation amount of a servo track width. FIG. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0011] Hereinafter, embodiments of the present disclosure will be described in detail with reference to the drawings. The description will be made in the following order. 1. One embodiment 1-1. Structure of magnetic recording media 1-2. Manufacturing method of magnetic recording media 1-3. Configuration of recording / playback device 1-4.Effects 2. Variations
[0012] <1. One embodiment> [1-1 Configuration of magnetic recording medium 10] FIG. 1 shows an example of a cross-sectional configuration of a magnetic recording medium 10 according to an embodiment of the present disclosure. As shown in FIG. 1, the magnetic recording medium 10 has a laminated structure in which multiple layers are laminated. Specifically, the magnetic recording medium 10 includes a long tape-shaped substrate 11, an underlayer 12 provided on one main surface 11A of the substrate 11, a magnetic layer 13 provided on the underlayer 12, and a back layer 14 provided on the other main surface 11B of the substrate 11. A surface 13S of the magnetic layer 13 is the surface against which the magnetic head will run while contacting it. The underlayer 12 and the back layer 14 are provided as necessary and may not be required. The average thickness of the magnetic recording medium 10 may be, for example, 5.6 μm or less.
[0013] The magnetic recording medium 10 is in the form of a long tape, and runs along its own longitudinal direction during recording and reproducing operations. The magnetic recording medium 10 is preferably used in a recording and reproducing device equipped with a ring-type head as a recording head, for example.
[0014] (Base 11) The substrate 11 is a non-magnetic support that supports the underlayer 12 and the magnetic layer 13. The substrate 11 is in the form of a long film. The upper limit of the average thickness of the substrate 11 is preferably 4.2 μm or less, more preferably 4.0 μm or less. When the upper limit of the average thickness of the substrate 11 is 4.2 μm or less, the recording capacity that can be recorded in one data cartridge can be made higher than that of a typical magnetic recording medium. The lower limit of the average thickness of the substrate 11 is preferably 3 μm or more, more preferably 3.2 μm or more. When the lower limit of the average thickness of the substrate 11 is 3 μm or more, a decrease in the strength of the substrate 11 can be suppressed.
[0015] The average thickness of the substrate 11 is obtained as follows. First, a magnetic recording medium 10 with a width of 1 / 2 inch is prepared and cut into a length of 250 mm to prepare a sample. Next, layers other than the substrate 11 of the sample, i.e., the underlayer 12, the magnetic layer 13, and the back layer 14, are removed with a solvent such as MEK (methyl ethyl ketone) or dilute hydrochloric acid. Next, the thickness of the sample substrate 11 is measured at five or more positions using a Mitutoyo Laser Hologram (LGH-110C) as a measuring device. Then, the measured values are simply averaged (arithmetic average) to calculate the average thickness of the substrate 11. Note that the measurement positions are selected randomly from the sample.
[0016] The base 11 contains, for example, polyesters as a main component. In addition to polyesters, the base 11 may contain at least one of polyolefins, cellulose derivatives, vinyl resins, and other polymer resins. When the base 11 contains two or more of the above materials, the two or more materials may be mixed, copolymerized, or laminated.
[0017] The polyesters contained in the base 11 include, for example, at least one of PET (polyethylene terephthalate), PEN (polyethylene naphthalate), PBT (polybutylene terephthalate), PBN (polybutylene naphthalate), PCT (polycyclohexylene dimethylene terephthalate), PEB (polyethylene-p-oxybenzoate), and polyethylene bisphenoxycarboxylate.
[0018] The polyolefins contained in the base 11 include, for example, at least one of PE (polyethylene) and PP (polypropylene). The cellulose derivatives include, for example, at least one of cellulose diacetate, cellulose triacetate, CAB (cellulose acetate butyrate) and CAP (cellulose acetate propionate). The vinyl resins include, for example, at least one of PVC (polyvinyl chloride) and PVDC (polyvinylidene chloride).
[0019] Other polymer resins contained in the base 11 include, for example, at least one of PA (polyamide, nylon), aromatic PA (aromatic polyamide, aramid), PI (polyimide), aromatic PI (aromatic polyimide), PAI (polyamideimide), aromatic PAI (aromatic polyamideimide), PBO (polybenzoxazole, such as Zylon (registered trademark)), polyether, PEK (polyetherketone), polyetherester, PES (polyethersulfone), PEI (polyetherimide), PSF (polysulfone), PPS (polyphenylene sulfide), PC (polycarbonate), PAR (polyarylate), and PU (polyurethane).
[0020] (Magnetic layer 13) The magnetic layer 13 is a recording layer for recording signals. The magnetic layer 13 contains, for example, a magnetic powder, a binder, and a lubricant. The magnetic layer 13 may further contain additives such as conductive particles, an abrasive, and an anti-rust agent, as necessary.
[0021] The magnetic layer 13 has a surface 13S in which a large number of holes are provided. A lubricant is stored in these holes. It is preferable that the holes extend in a direction perpendicular to the surface of the magnetic layer 13. This is because this can improve the supply of the lubricant to the surface 13S of the magnetic layer 13. Note that some of the holes may extend in the vertical direction.
[0022] The arithmetic mean roughness Ra of the surface 13S of the magnetic layer 13 is 2.5 nm or less, preferably 2.2 nm or less, more preferably 1.9 nm or less. When the arithmetic mean roughness Ra is 2.5 nm or less, excellent electromagnetic conversion characteristics can be obtained. The lower limit of the arithmetic mean roughness Ra of the surface 13S of the magnetic layer 13 is preferably 1.0 nm or more, more preferably 1.2 nm or more, and even more preferably 1.4 nm or more. When the lower limit of the arithmetic mean roughness Ra of the surface 13S of the magnetic layer 13 is 1.0 nm or more, deterioration of running properties due to increased friction can be suppressed.
[0023] The arithmetic mean roughness Ra of the surface 13S is found as follows. First, the surface of the magnetic layer 13 is observed with an AFM (Atomic Force Microscope) to obtain an AFM image of 40 μm×40 μm. A Nano Scope IIIa D3100 manufactured by Digital Instruments is used as the AFM, a single crystal silicon cantilever is used, and measurements are performed with a tapping frequency of 200 Hz to 400 Hz tuning. For example, an "SPM Probe NCH Normal Type PointProbe L (cantilever length)=125 um" manufactured by Nano World cantilever can be used. Next, the AFM image is divided into 512 x 512 (= 262,144) measurement points, and the height Z(i) (i: measurement point number, i = 1 to 262,144) is measured at each measurement point. The heights Z(i) of each measurement point are simply averaged (arithmetic mean) to obtain the average height (average surface) Zave (= (Z(1) + Z(2) + ··· + Z(262,144)) / 262,144). Next, the deviation Z"(i) (= |Z(i)-Zave|) from the average center line at each measurement point is obtained, and the arithmetic mean roughness Ra [nm] (= (Z"(1) + Z"(2) + ··· + Z"(262,144)) / 262,144) is calculated. In this case, the data used is filtered using Flatten order 2 and planefit order 3 XY as image processing.
[0024] Furthermore, it is desirable that the PSD (Power Spectrum Density) of the magnetic layer 13 up to a spatial wavelength of 5 μm is, for example, 2.5 μm or less. By suppressing the PSD to a certain value or less, the spacing between the recording / reproducing head and the tape during recording / reproducing can be made small, making it possible to make the medium suitable for high recording density. The PSD is measured as follows. First, the surface of the magnetic tape is observed with an atomic force microscope (AFM) to obtain two-dimensional (2D) surface profile data. The AFM suitable for the measurement is shown below. Digital Instruments Dimension 3100 Cantilever: NanoWorld NCH-10T The AFM measurement conditions are as follows. Measurement area: 30μm×30μm Resolution: 512×512 AFM probe scan direction: MD direction (longitudinal direction) of magnetic tape Measurement mode: Tapping mode Scan ratio: 1Hz Next, the following filtering process is applied to the 2D surface profile data obtained by the AFM. Flatten: 3rd order Planefit: 3rd order only in MD direction Next, a Fast Fourier Transform (FFT) is applied to each of the 512 lines of the filtered 2D surface profile data in the MD direction to obtain 512 power spectrum densities (PSDs). The 512 PSDs obtained in the MD direction are then averaged for each wavelength to obtain one averaged PSD in the MD direction (hereinafter referred to as "PSDMD" or "PSD(k)MD"). The following formula (1) is used to average the PSD in the MD direction.
number
[0025] The upper limit of the average thickness of the magnetic layer 13 is preferably 90 nm or less, particularly preferably 80 nm or less, more preferably 70 nm or less, and even more preferably 50 nm or less. When the upper limit of the average thickness of the magnetic layer 13 is 90 nm or less, when a ring-type head is used as the recording head, the magnetization can be recorded uniformly in the thickness direction of the magnetic layer 13, and the electromagnetic conversion characteristics can be improved. Also, when the upper limit of the average thickness of the magnetic layer 13 is 90 nm or less, the half-width of the isolated waveform in the reproduced waveform of the data signal can be narrowed (for example, to 200 nm or less), and the peak of the reproduced waveform of the data signal can be made sharp. This improves the reading accuracy of the data signal, and the number of recording tracks can be increased to improve the recording density of the data.
[0026] The lower limit of the average thickness of the magnetic layer 13 is preferably 35 nm or more. If the upper limit of the average thickness of the magnetic layer 13 is 35 nm or more, output can be ensured when an MR head is used as the reproducing head, and therefore the electromagnetic conversion characteristics can be improved.
[0027] The average thickness of the magnetic layer 13 is determined as follows. First, a carbon film is formed by vapor deposition on the surface 13S of the magnetic layer 13 and the surface 14S of the back layer 14 of the magnetic recording medium 10, and then a tungsten thin film is further formed by vapor deposition on the carbon film covering the surface 13S of the magnetic layer 13. These carbon and tungsten films protect the sample during the thinning process described below.
[0028] Next, the magnetic recording medium 10 is processed by a FIB (Focused Ion Beam) method or the like to be sliced. When the FIB method is used, a carbon film and a tungsten thin film are formed as protective films as a pretreatment for observing a TEM image of the cross section described later. The carbon film is formed on the magnetic layer side surface and the back layer side surface of the magnetic recording medium 10 by a vapor deposition method, and the tungsten thin film is further formed on the magnetic layer side surface by a vapor deposition method or a sputtering method. The slice is performed along the length direction (longitudinal direction) of the magnetic recording medium 10. That is, the slice forms a cross section parallel to both the longitudinal direction and the thickness direction of the magnetic recording medium 10. The cross section of the obtained sliced sample is observed under the following conditions by a transmission electron microscope (TEM) to obtain a TEM image. The magnification and acceleration voltage may be appropriately adjusted depending on the type of device. Equipment: TEM (Hitachi H9000NAR) Acceleration voltage: 300 kV Magnification: 100,000x
[0029] Next, using the obtained TEM image, the thickness of the magnetic layer 13 is measured at at least 10 positions in the longitudinal direction of the magnetic recording medium 10. The obtained measurements are simply averaged (arithmetic average) to obtain the average thickness of the magnetic layer 13. The positions at which the measurement is performed are selected randomly from the test piece.
[0030] (magnetic powder) The magnetic powder includes, for example, a powder of nanoparticles containing ε-iron oxide (hereinafter referred to as "ε-iron oxide particles"). Even fine particles of ε-iron oxide particles can obtain high coercivity. It is preferable that the ε-iron oxide contained in the ε-iron oxide particles has a crystal orientation preferentially in the thickness direction (perpendicular direction) of the magnetic recording medium 10.
[0031] FIG. 2 is a cross-sectional view that shows a schematic example of the cross-sectional structure of the ε iron oxide particles 20 contained in the magnetic layer 13. As shown in FIG. 2, the ε iron oxide particles 20 are spherical or nearly spherical, or cubic or nearly cubic. Since the ε iron oxide particles 20 have the above-mentioned shapes, when the ε iron oxide particles 20 are used as the magnetic particles, the contact area between the particles in the thickness direction of the magnetic recording medium 10 can be reduced and aggregation between the particles can be suppressed, compared to when hexagonal plate-shaped barium ferrite particles are used as the magnetic particles. This improves the dispersibility of the magnetic powder and provides a better SNR (Signal-to-Noise Ratio). It is possible.
[0032] The ε-iron oxide particle 20 has, for example, a core-shell structure. Specifically, as shown in Fig. 2, the ε-iron oxide particle 20 includes a core portion 21 and a two-layered shell portion 22 provided around the core portion 21. The two-layered shell portion 22 has a first shell portion 22a provided on the core portion 21 and a second shell portion 22b provided on the first shell portion 22a.
[0033] The core portion 21 of the ε-iron oxide particle 20 contains ε-iron oxide. The ε-iron oxide contained in the core portion 21 preferably has ε-Fe2O3 crystals as a main phase, and more preferably is made of single-phase ε-Fe2O3.
[0034] The first shell portion 22a covers at least a part of the periphery of the core portion 21. Specifically, the first shell portion 22a may cover a part of the periphery of the core portion 21, or may cover the entire periphery of the core portion 21. From the viewpoint of ensuring sufficient exchange coupling between the core portion 21 and the first shell portion 22a and improving magnetic characteristics, it is preferable that the entire surface of the core portion 21 is covered.
[0035] The first shell portion 22a is a so-called soft magnetic layer, and includes a soft magnetic material such as α-Fe, a Ni-Fe alloy, an Fe-Si-Al alloy, etc. The α-Fe may be obtained by reducing ε-iron oxide included in the core portion 21.
[0036] The second shell portion 22b is an oxide coating serving as an anti-oxidation layer. The second shell portion 22b includes α-iron oxide, aluminum oxide, or silicon oxide. The α-iron oxide includes at least one type of iron oxide, for example, Fe3O4, Fe2O3, and FeO. When the first shell portion 22a includes α-Fe (soft magnetic material), the α-iron oxide may be obtained by oxidizing the α-Fe included in the first shell portion 22a.
[0037] By having the first shell portion 22a as described above, the coercive force Hc of the core portion 21 alone can be kept large to ensure thermal stability, while the coercive force Hc of the entire ε-iron oxide particle (core-shell particle) 20 can be adjusted to a coercive force Hc suitable for recording. Furthermore, by having the second shell portion 22b as described above, the ε-iron oxide particle 20 can be prevented from deteriorating in the properties of the ε-iron oxide particle 20 due to rust or the like occurring on the particle surface caused by exposure of the ε-iron oxide particle 20 to air during and before the manufacturing process of the magnetic recording medium 10. Therefore, by covering the first shell portion 22a with the second shell portion 22b, deterioration in the properties of the magnetic recording medium 10 can be prevented.
[0038] The average particle size (average maximum particle size) of the magnetic powder is preferably 25 nm or less, more preferably 8 nm to 22 nm, and even more preferably 12 nm to 22 nm. In the magnetic recording medium 10, the area with a size of 1 / 2 of the recording wavelength becomes the actual magnetization area. Therefore, by setting the average particle size of the magnetic powder to half the shortest recording wavelength or less, a good S / N ratio can be obtained. Therefore, when the average particle size of the magnetic powder is 22 nm or less, good electromagnetic conversion characteristics (e.g., SNR) can be obtained in a high recording density magnetic recording medium 10 (e.g., a magnetic recording medium 10 configured to be able to record signals at the shortest recording wavelength of 50 nm or less). On the other hand, when the average particle size of the magnetic powder is 8 nm or more, the dispersibility of the magnetic powder is further improved, and better electromagnetic conversion characteristics (e.g., SNR) can be obtained.
[0039] The average aspect ratio of the magnetic powder is preferably 1.0 to 3.0, more preferably 1.0 to 2.8, and even more preferably 1.0 to 2.0. When the average aspect ratio of the magnetic powder is within the range of 1 to 3.0, aggregation of the magnetic powder can be suppressed, and the resistance applied to the magnetic powder when the magnetic powder is vertically oriented in the process of forming the magnetic layer 13 can be suppressed. Therefore, the vertical orientation of the magnetic powder can be improved.
[0040] The average particle size and average aspect ratio of the magnetic powder are obtained as follows. First, the magnetic recording medium 10 to be measured is processed and thinned by FIB (Focused Ion Beam) method or the like. The thinning is performed along the length direction (longitudinal direction) of the magnetic tape. That is, this thinning forms a cross section parallel to both the longitudinal direction and the thickness direction of the magnetic recording medium 10. The obtained thin sample is observed by a transmission electron microscope (H-9500 manufactured by Hitachi High-Technologies Corporation) at an acceleration voltage of 200 kV and a total magnification of 500,000 times so that the entire magnetic layer 13 is included in the thickness direction of the magnetic layer 13, and a TEM photograph is taken. Next, 50 particles are randomly selected from the TEM photograph, and the long axis length DL and short axis length DS of each particle are measured. Here, the long axis length DL means the maximum distance between two parallel lines drawn from all angles so as to be tangent to the contour of each particle (so-called maximum Feret diameter). On the other hand, the minor axis length DS means the maximum length of the particle in a direction perpendicular to the major axis length DL of the particle.
[0041] Next, the long axis lengths DL of the 50 measured particles are simply averaged (arithmetic mean) to determine the average long axis length DLave. The average long axis length DLave thus determined is the average particle size of the magnetic powder. The short axis lengths DS of the 50 measured particles are also simply averaged (arithmetic mean) to determine the average short axis length DSave. The average aspect ratio of the particles (DLave / DSave) is then calculated from the average long axis length DLave and the average short axis length DSave.
[0042] The average particle volume of the magnetic powder is preferably 2300 nm 3 Less than or equal to 2200 nm, preferably 3 Less than or equal to 2100 nm, preferably 3 Less than or equal to 1950 nm, more preferably 3 Less than or equal to 1600 nm, more preferably 3 Below 1300 nm, and even more preferably below 1300 nm 3 The average particle volume of the magnetic powder is 2300 nm or less. 3 If it is less than this, the half-width of the isolated waveform in the reproduced waveform of the data signal can be narrowed (200 nm or less), and the peak of the reproduced waveform of the data signal can be made sharper. This improves the accuracy of reading the data signal, so the number of recording tracks can be increased to improve the data recording density (details will be described later). The smaller the average particle volume of the magnetic powder, the better, so there is no particular restriction on the lower limit of the volume, but for example, the lower limit can be 800 nm 3 That is all.
[0043] When the ε iron oxide particles 20 are spherical or nearly spherical, the average particle volume of the magnetic powder is calculated as follows. First, the average major axis length DLave is calculated in the same manner as in the calculation method for the average particle size of the magnetic powder described above. Next, the average volume V of the magnetic powder is calculated by the following formula. V = (π / 6) × (DLave) 3
[0044] (Binding agent) As the binder, a resin having a structure in which a crosslinking reaction is given to a polyurethane resin, a vinyl chloride resin, or the like is preferable. However, the binder is not limited to these, and other resins may be appropriately blended depending on the physical properties required for the magnetic recording medium 10. There is no particular limitation on the resin to be blended, so long as it is a resin that is generally used in coating-type magnetic recording media 10.
[0045] Examples of the polymer include polyvinyl chloride, polyvinyl acetate, vinyl chloride-vinyl acetate copolymer, vinyl chloride-vinylidene chloride copolymer, vinyl chloride-acrylonitrile copolymer, acrylic acid ester-acrylonitrile copolymer, acrylic acid ester-vinyl chloride-vinylidene chloride copolymer, vinyl chloride-acrylonitrile copolymer, acrylic acid ester-acrylonitrile copolymer, acrylic acid ester-vinylidene chloride copolymer, methacrylic acid ester-vinylidene chloride copolymer, methacrylic acid ester-vinyl chloride copolymer, methacrylic acid ester-ethylene copolymer, polyvinyl fluoride, vinylidene chloride-acrylonitrile copolymer, acrylonitrile-butadiene copolymer, polyamide resin, polyvinyl butyral, cellulose derivatives (cellulose acetate butyrate, cellulose diacetate, cellulose triacetate, cellulose propionate, nitrocellulose), styrene-butadiene copolymer, polyester resin, amino resin, and synthetic rubber.
[0046] Examples of the thermosetting resin or reactive resin include phenol resin, epoxy resin, urea resin, melamine resin, alkyd resin, silicone resin, polyamine resin, and urea formaldehyde resin.
[0047] Furthermore, in order to improve the dispersibility of the magnetic powder, polar functional groups such as -SO3M, -OSO3M, -COOM, and P=O(OM)2 may be introduced into each of the above-mentioned binders. Here, M in the above chemical formula is a hydrogen atom or an alkali metal such as lithium, potassium, or sodium.
[0048] Furthermore, the polar functional groups include -NR1R2, -NR1R2R3 + X - Side chain type with terminal group of >NR1R2 + X - In the above formula, R1, R2, and R3 are hydrogen atoms or hydrocarbon groups, and X -is a halogen element ion such as fluorine, chlorine, bromine, or iodine, or an inorganic or organic ion. Examples of the polar functional group include -OH, -SH, -CN, and an epoxy group.
[0049] (Lubricant) The lubricant contained in the magnetic layer 13 contains, for example, a fatty acid and a fatty acid ester. The fatty acid contained in the lubricant is, for example, a compound represented by the following general formula: <1> and compounds represented by the general formula <2> In addition, the fatty acid ester contained in the lubricant preferably contains at least one of the compounds represented by the following general formula: <3> and compounds represented by the general formula <4> It is preferred that the lubricant contains at least one of the compounds represented by the general formula: <1> and compounds represented by the general formula <3> By including two kinds of compounds represented by the general formula <2> and compounds represented by the general formula <3> By including two kinds of compounds represented by the general formula <1> and compounds represented by the general formula <4> By including two kinds of compounds represented by the general formula <2> and compounds represented by the general formula <4> By including two kinds of compounds represented by the general formula <1> Compounds represented by the general formula <2> and compounds represented by the general formula <3> By including three kinds of compounds represented by the general formula <1> Compounds represented by the general formula <2> and compounds represented by the general formula <4> By including three kinds of compounds represented by the general formula <1> Compounds represented by the general formula <3> and compounds represented by the general formula <4> By including three kinds of compounds represented by the general formula <2> Compounds represented by the general formula <3> and compounds represented by the general formula <4> or by including three kinds of compounds represented by the general formula <1> Compounds represented by the general formula <2> Compounds represented by the general formula <3> and compounds represented by the general formula <4> By containing these four compounds, it is possible to suppress an increase in the dynamic friction coefficient due to repeated recording or reproduction on the magnetic recording medium 10. As a result, the running properties of the magnetic recording medium 10 can be further improved. CH3(CH2) k COOH... <1> (However, the general formula <1> In the formula, k is an integer selected from the range of 14 to 22, more preferably from the range of 14 to 18. CH3(CH2) n CH=CH(CH2) m COOH... <2> (However, the general formula <2> In the formula, the sum of n and m is an integer selected from the range of 12 to 20, more preferably from the range of 14 to 18. CH3(CH2) p COO(CH2) q CH3... <3> (However, the general formula <3> In the formula, p is an integer selected from the range of 14 to 22, more preferably from 14 to 18, and q is an integer selected from the range of 2 to 5, more preferably from 2 to 4. CH3(CH2) p COO-(CH2) q CH(CH3)2… <4> (However, the above general formula <4> In the formula, p is an integer selected from the range of 14 to 22, and q is an integer selected from the range of 1 to 3.
[0050] (Additives) The magnetic layer 13 may further contain non-magnetic reinforcing particles such as aluminum oxide (α, β or γ alumina), chromium oxide, silicon oxide, diamond, garnet, emery, boron nitride, titanium carbide, silicon carbide, titanium carbide, titanium oxide (rutile or anatase titanium oxide), etc.
[0051] (base layer 12) The underlayer 12 is a non-magnetic layer containing a non-magnetic powder and a binder. The underlayer 12 may further contain at least one additive selected from the group consisting of a lubricant, conductive particles, a hardener, and an anti-rust agent, as necessary. The underlayer 12 may have a multi-layer structure in which multiple layers are stacked. The average thickness of the underlayer 12 is preferably 0.4 μm or more and 1.4 μm or less, more preferably 0.6 μm or more and 1.2 μm or less.
[0052] The average thickness of the underlayer 12 can be obtained, for example, as follows. First, a magnetic recording medium 10 with a width of 1 / 2 inch is prepared, and cut into a length of 250 mm to prepare a sample. Next, the underlayer 12 and the magnetic layer 13 are peeled off from the substrate 11 for the sample magnetic recording medium 10. Next, a Mitutoyo Laser Hologram (LGH-110C) is used as a measuring device to measure the thickness of the laminate of the underlayer 12 and the magnetic layer 13 peeled off from the substrate 11 at five or more positions. After that, the measured values are simply averaged (arithmetic averaged) to calculate the average thickness of the laminate of the underlayer 12 and the magnetic layer 13. The measurement positions are selected randomly from the sample. Finally, the average thickness of the underlayer 12 is obtained by subtracting the average thickness of the magnetic layer 13 measured using the TEM as described above from the average thickness of the laminate.
[0053] The underlayer 12 may have pores, that is, the underlayer 12 may be provided with a large number of pores. The pores of the underlayer 12 may be formed, for example, by forming pores (holes) in the magnetic layer 13, and in particular, may be formed by pressing a large number of protrusions provided on the surface 14S of the back layer 14 of the magnetic recording medium 10 against the surface of the magnetic layer side. That is, pores may be formed in the magnetic layer 13 and the underlayer 12 by forming recesses corresponding to the shape of the protrusions on the surface 13S of the magnetic layer 13. In addition, the pores may be formed by volatilization of the solvent in the drying process of the paint for forming the magnetic layer. In addition, when the paint for forming the magnetic layer is applied to the surface of the underlayer 12 to form the magnetic layer 13, the solvent in the paint for forming the magnetic layer may pass through the pores of the underlayer 12 formed when the underlayer is applied and dried, and penetrate into the underlayer 12. Thereafter, when the solvent that has penetrated into the underlayer 12 volatilizes during the drying process of the magnetic layer 13, the solvent that has penetrated into the underlayer 12 may move from the underlayer 12 to the surface 13S of the magnetic layer 13, thereby forming pores. The pores thus formed may, for example, communicate with the magnetic layer 13 and the underlayer 12. The average diameter of the pores can be adjusted by changing the solid content or type of solvent of the paint for forming the magnetic layer and / or the drying conditions of the paint for forming the magnetic layer. By forming pores in both the magnetic layer 13 and the underlayer 12, a particularly suitable amount of lubricant for good running stability appears on the magnetic layer side surface, and the increase in the dynamic friction coefficient due to repeated recording or reproduction can be further suppressed.
[0054] From the viewpoint of suppressing a decrease in the dynamic friction coefficient after repeated recording or reproduction, it is preferable that the holes in the underlayer 12 are connected to the holes in the magnetic layer 13. Here, the holes in the underlayer 12 being connected to the holes in the magnetic layer 13 includes a state in which some of the many holes in the underlayer 12 are connected to some of the many holes in the magnetic layer 13.
[0055] From the viewpoint of improving the supply of lubricant to the surface 13S of the magnetic layer 13, it is preferable that the numerous holes include some extending in a direction perpendicular to the surface 13S of the magnetic layer 13. Also, from the viewpoint of improving the supply of lubricant to the surface 13S of the magnetic layer 13, it is preferable that the holes of the underlayer 12 extending in a direction perpendicular to the surface 13S of the magnetic layer 13 and the holes of the magnetic layer 13 extending in a direction perpendicular to the surface 13S of the magnetic layer 13 are connected to each other.
[0056] (Non-magnetic powder in underlayer 12) The non-magnetic powder includes at least one of inorganic particle powder and organic particle powder. The non-magnetic powder may also include carbon powder such as carbon black. One type of non-magnetic powder may be used alone, or two or more types of non-magnetic powder may be used in combination. The inorganic particles include, for example, metals, metal oxides, metal carbonates, metal sulfates, metal nitrides, metal carbides, or metal sulfides. The shape of the non-magnetic powder may be, for example, various shapes such as needle-like, spherical, cubic, and plate-like, but is not limited thereto.
[0057] (Binding agent for base layer 12) The binder in the underlayer 12 is the same as that in the magnetic layer 13 described above.
[0058] (Back layer 14) The back layer 14 contains, for example, a binder and a nonmagnetic powder. The back layer 14 may further contain at least one additive selected from the group consisting of a lubricant, a hardener, and an antistatic agent, as necessary. The binder and nonmagnetic powder in the back layer 14 are the same as those in the underlayer 12 described above.
[0059] The average particle size of the non-magnetic powder in the back layer 14 is preferably 10 nm or more and 150 nm or less, more preferably 15 nm or more and 110 nm or less. The average particle size of the non-magnetic powder in the back layer 14 is determined in the same manner as the average particle size of the magnetic powder in the magnetic layer 13. The non-magnetic powder may include powder having two or more particle size distributions.
[0060] The upper limit of the average thickness of the back layer 14 is preferably 0.6 μm or less, and particularly preferably 0.5 μm or less. If the upper limit of the average thickness of the back layer 14 is 0.6 μm or less, the thickness of the underlayer 12 and the base 11 can be kept thick even when the average thickness of the magnetic recording medium 10 is 5.6 μm or less, so that the running stability of the magnetic recording medium 10 in a recording and reproducing device can be maintained. The lower limit of the average thickness of the back layer 14 is not particularly limited, but is, for example, 0.2 μm or more, and particularly preferably 0.3 μm or more.
[0061] The average thickness of the back layer 14 is obtained as follows. First, a magnetic recording medium 10 having a width of 1 / 2 inch is prepared and cut into a length of 250 mm to prepare a sample. Next, the thickness of the sample magnetic recording medium 10 is measured at five or more points using a Mitutoyo Laser Hologram (LGH-110C) as a measuring device, and the measured values are simply averaged (arithmetic average) to obtain the average thickness t T [μm] is calculated. Note that the measurement positions are selected randomly from the sample. Next, the back layer 14 is removed from the sample magnetic recording medium 10 with a solvent such as MEK (methyl ethyl ketone) or dilute hydrochloric acid. After that, the above-mentioned laser hologram is used again to measure the thickness of the sample from which the back layer 14 has been removed from the magnetic recording medium 10 at five or more points, and these measured values are simply averaged (arithmetic average) to obtain the average thickness t B [μm] is calculated. The measurement positions are selected randomly from the sample. Finally, the average thickness t of the back layer 14 is calculated from the following formula: b Calculate [μm]. t b [μm]=t T [μm]-t B [μm]
[0062] The back layer 14 has a surface on which a large number of protrusions are provided. The large number of protrusions are intended to form a large number of holes in the surface of the magnetic layer 13 when the magnetic recording medium 10 is wound in a roll. The large number of holes are composed of, for example, a large number of non-magnetic particles protruding from the surface of the back layer 14.
[0063] Here, a case has been described in which a large number of protrusions provided on the surface of the back layer 14 are transferred to the surface of the magnetic layer 13 to form a large number of holes in the surface of the magnetic layer 13, but the method of forming a large number of holes is not limited to this. For example, a large number of holes may be formed in the surface of the magnetic layer 13 by adjusting the type of solvent contained in the paint for forming the magnetic layer and the drying conditions of the paint for forming the magnetic layer.
[0064] [Average thickness of magnetic recording media] The upper limit of the average thickness (average total thickness) of the magnetic recording medium 10 is preferably 5.6 μm or less, more preferably 5.0 μm or less, particularly preferably 4.6 μm or less, and even more preferably 4.4 μm or less. When the average thickness of the magnetic recording medium 10 is 5.6 μm or less, the recording capacity that can be recorded in one data cartridge can be increased compared to that of a general magnetic recording medium. The lower limit of the average thickness of the magnetic recording medium 10 is not particularly limited, but is, for example, 3.5 μm or more.
[0065] The average thickness tT of the magnetic recording medium 10 is found as follows. First, a magnetic recording medium 10 with a width of 1 / 2 inch is prepared, and then cut into a length of 250 mm to prepare a sample. Next, using a Mitutoyo Laser Hologram (LGH-110C) as a measuring device, the thickness of the sample is measured at five or more positions, and the measured values are simply averaged (arithmetic mean) to calculate the average value tT [μm]. Note that the measurement positions are selected randomly from the sample.
[0066] (Coercive force Hc1 in the perpendicular direction) The upper limit of the coercive force Hc1 in the perpendicular direction is 3000 Oe or less, more preferably 2900 Oe or less, and even more preferably 2850 Oe or less. A large coercive force Hc1 is preferable because it is less susceptible to thermal disturbance and demagnetizing fields. However, if the coercive force Hc1 exceeds 3000 Oe, it becomes difficult to perform saturation recording with the recording head, which may result in some areas that cannot be recorded and increased noise, which may result in a deterioration of the electromagnetic conversion characteristics (e.g., C / N).
[0067] The lower limit of the coercive force Hc1 in the perpendicular direction is preferably 2200 Oe or more, more preferably 2400 Oe or more, and even more preferably 2600 Oe or more. If the coercive force Hc1 is 2200 Oe or more, it is possible to suppress the deterioration of the electromagnetic conversion characteristics (e.g., C / N) in a high-temperature environment due to the influence of thermal disturbance and the influence of a demagnetizing field.
[0068] The coercive force Hc1 is obtained as follows. Three magnetic recording media 10 are stacked and bonded with double-sided tape, and then punched out with a φ6.39 mm punch to create a measurement sample. At this time, marking is performed with any non-magnetic ink so that the longitudinal direction (running direction) of the magnetic recording medium can be identified. Then, the MH loop of the measurement sample (whole magnetic recording medium 10) corresponding to the longitudinal direction (running direction of magnetic recording medium 10) of the magnetic recording medium 10 is measured using a vibrating sample magnetometer (VSM). Next, the coating film (underlayer 12, magnetic layer 13, back layer 14, etc.) is wiped off with acetone or ethanol, etc., leaving only the substrate 11. Then, three obtained substrates 11 are stacked and bonded with double-sided tape, and then punched out with a φ6.39 mm punch to obtain a sample for background correction (hereinafter simply referred to as a correction sample). Thereafter, the MH loop of the correction sample (substrate 11) corresponding to the perpendicular direction of the substrate 11 (thickness direction of the magnetic recording medium 10) is measured using the VSM.
[0069] The MH loop of the measurement sample (whole magnetic recording medium 10) and the MH loop of the correction sample (substrate 11) are measured using, for example, a high-sensitivity vibration sample magnetometer "VSM-P7-15 type" manufactured by Toei Kogyo Co., Ltd. The measurement conditions are as follows: measurement mode: full loop, maximum magnetic field: 15 kOe, magnetic field step: 40 bits, time constant of locking amp: 0.3 sec, waiting time: 1 sec, number of MH averages: 20.
[0070] After obtaining the two MH loops, background correction is performed by subtracting the MH loop of the correction sample (substrate 11) from the MH loop of the measurement sample (whole magnetic recording medium 10), and the MH loop after background correction is obtained. For the calculation of this background correction, a measurement and analysis program attached to the "VSMP7-15 type" is used.
[0071] The coercive force Hc1 is obtained from the obtained MH loop after background correction. For this calculation, a measurement and analysis program attached to the "VSM-P7-15 type" is used. All of the above MH loop measurements are performed at 25°C. Furthermore, no "demagnetizing field correction" is performed when measuring the MH loop in the perpendicular direction to the magnetic recording medium 10.
[0072] (Coercive force Hc2 in the longitudinal direction) The upper limit of the coercive force Hc2 in the longitudinal direction of the magnetic recording medium 10 is preferably 2000 Oe or less, more preferably 1900 Oe or less, and even more preferably 1800 Oe or less. When the coercive force Hc2 in the longitudinal direction is 2000 Oe or less, the magnetization reacts sensitively to the perpendicular magnetic field from the recording head, and therefore a good recording pattern can be formed.
[0073] The lower limit of the coercivity Hc2 measured in the longitudinal direction of the magnetic recording medium 10 is preferably 1000 Oe or more. If the lower limit of the coercivity Hc in the longitudinal direction is 1000 Oe or more, demagnetization due to leakage flux from the recording head can be suppressed.
[0074] The above coercive force Hc2 is determined in the same manner as the coercive force Hc1 in the perpendicular direction, except that the MH loops of the entire measurement sample and the sample for background correction are measured in the direction corresponding to the longitudinal direction (running direction) of the magnetic recording medium 10.
[0075] (Hc2 / Hc1) The ratio Hc2 / Hc1 of the coercive force Hc1 in the perpendicular direction to the coercive force Hc2 in the longitudinal direction satisfies the relationship Hc2 / Hc1≦0.8, preferably Hc2 / Hc1≦0.75, more preferably Hc2 / Hc1≦0.7, even more preferably Hc2 / Hc1≦0.65, and particularly preferably Hc2 / Hc1≦0.6. When the coercive forces Hc1 and Hc2 satisfy the relationship Hc2 / Hc1≦0.8, the degree of perpendicular orientation of the magnetic powder can be increased. Therefore, the magnetization transition width can be reduced and a high-output signal can be obtained during signal reproduction, thereby improving the electromagnetic conversion characteristics (e.g., C / N). As described above, when Hc2 is small, the magnetization reacts sensitively to the magnetic field in the perpendicular direction from the recording head, so that a good recording pattern can be formed.
[0076] When the ratio Hc2 / Hc1 is Hc2 / Hc1≦0.8, it is particularly effective that the average thickness of the magnetic layer 13 is 90 nm or less. If the average thickness of the magnetic layer 13 exceeds 90 nm, when a ring-type head is used as a recording head, the lower region of the magnetic layer 13 (the region on the underlayer 12 side) may be magnetized in the longitudinal direction, and the magnetic layer 13 may not be uniformly magnetized in the thickness direction. Therefore, even if the ratio Hc2 / Hc1 is Hc2 / Hc1≦0.8 (i.e., even if the degree of vertical orientation of the magnetic powder is increased), it may not be possible to improve the electromagnetic conversion characteristics (e.g., C / N).
[0077] The lower limit of Hc2 / Hc1 is not particularly limited, but is, for example, 0.5≦Hc2 / Hc1.
[0078] In addition, Hc2 / Hc1 represents the degree of vertical orientation of the magnetic powder, and the smaller Hc2 / Hc1, the higher the degree of vertical orientation of the magnetic powder. Below, the reason for using Hc2 / Hc1 as an index showing the degree of vertical orientation of the magnetic powder in this embodiment will be explained.
[0079] Conventionally, the squareness ratio SQ (=(Mr / Ms)×100, where Mr(emu): residual magnetization, Ms(emu): saturation magnetization) has generally been used as an index (parameter) indicating the degree of vertical orientation of magnetic powder. However, according to the findings of the present inventors, the squareness ratio SQ is not an appropriate index to indicate the degree of vertical orientation of magnetic powder for the following reasons. (1) The squareness ratio SQ varies depending on the value of the coercive force Hc of the magnetic powder. For example, as shown in Figure 5, when the coercive force Hc of the magnetic powder increases, the squareness ratio SQ also appears to increase. (2) The squareness ratio SQ is affected by the distortion of the MH loop due to overdispersion.
[0080] Therefore, in this embodiment, Hc2 / Hc1 is used as an index that more appropriately indicates the degree of orientation of the magnetic powder. Since the coercive forces Hc1 and Hc2 simply change depending on the orientation direction of the magnetic powder, Hc2 / Hc1 is a more appropriate index that more appropriately indicates the degree of orientation of the magnetic powder.
[0081] (Square ratio) The squareness ratio S1 in the perpendicular direction (thickness direction) of the magnetic recording medium 10 is, for example, 65% or more, preferably 70% or more, more preferably 75% or more, even more preferably 80% or more, and particularly preferably 85% or more. When the squareness ratio S1 is 65% or more, the perpendicular orientation of the magnetic powder is sufficiently high, and therefore a better SNR can be obtained.
[0082] The squareness ratio S1 is obtained as follows. Three magnetic recording media 10 are stacked and bonded with double-sided tape, and then punched out with a φ6.39 mm punch to create a measurement sample. At this time, marking is performed with any non-magnetic ink so that the longitudinal direction (running direction) of the magnetic recording medium can be identified. Then, the MH loop of the measurement sample (whole magnetic recording medium 10) corresponding to the longitudinal direction (running direction of magnetic recording medium 10) of the magnetic recording medium 10 is measured using a vibrating sample magnetometer (VSM). Next, the coating film (underlayer 12, magnetic layer 13, back layer 14, etc.) is wiped off with acetone or ethanol, etc., leaving only the substrate 11. Then, three obtained substrates 11 are stacked and bonded with double-sided tape, and then punched out with a φ6.39 mm punch to obtain a sample for background correction (hereinafter simply referred to as a correction sample). Thereafter, the MH loop of the correction sample (substrate 11) corresponding to the longitudinal direction of the substrate 11 (the running direction of the magnetic recording medium 10) is measured using the VSM.
[0083] The MH loop of the measurement sample (whole magnetic recording medium 10) and the MH loop of the correction sample (substrate 11) are measured using, for example, a high-sensitivity vibration sample magnetometer "VSM-P7-15 type" manufactured by Toei Kogyo Co., Ltd. The measurement conditions are as follows: measurement mode: full loop, maximum magnetic field: 15 kOe, magnetic field step: 40 bits, time constant of locking amp: 0.3 sec, waiting time: 1 sec, number of MH averages: 20.
[0084] After obtaining the two MH loops, background correction is performed by subtracting the MH loop of the correction sample (substrate 11) from the MH loop of the measurement sample (whole magnetic recording medium 10), and the MH loop after background correction is obtained. For the calculation of this background correction, a measurement and analysis program attached to the "VSMP7-15 type" is used.
[0085] The saturation magnetization Ms (emu) and residual magnetization Mr (emu) of the obtained MH loop after background correction are substituted into the following equation to calculate the squareness ratio S1 (%). Squareness ratio S1(%)=(Mr / Ms)×100 It should be noted that all of the above MH loop measurements are performed at 25° C. Furthermore, when measuring the MH loop in the perpendicular direction to the magnetic recording medium 10, no “demagnetizing field correction” is performed.
[0086] The squareness ratio S2 in the longitudinal direction (running direction) of the magnetic recording medium 10 is preferably 35% or less, more preferably 30% or less, even more preferably 25% or less, particularly preferably 20% or less, and most preferably 15% or less. When the squareness ratio S2 is 35% or less, the magnetic powder has a sufficiently high vertical orientation, so that a better SNR can be obtained.
[0087] The squareness ratio S2 is determined in the same manner as the squareness ratio S1, except that the MH loop is measured in the longitudinal direction (traveling direction) of the magnetic recording medium 10 and the substrate 11.
[0088] (SFD) In the SFD (Switching Field Distribution) curve of the magnetic recording medium 10, the peak ratio X / Y between the main peak height X and the sub-peak height Y near zero magnetic field is preferably 3.0 or more, more preferably 5.0 or more, even more preferably 7.0 or more, particularly preferably 10.0 or more, and most preferably 20.0 or more (see FIG. 3). When the peak ratio X / Y is 3.0 or more, it is possible to suppress the inclusion of a large amount of low coercive force components specific to ε-iron oxide (e.g., soft magnetic particles and superparamagnetic particles) in the magnetic powder in addition to the ε-iron oxide particles 20 that contribute to actual recording. Therefore, it is possible to suppress the deterioration of the magnetization signal recorded on the adjacent track due to the leakage magnetic field from the recording head, and therefore a better SNR can be obtained. The upper limit of the peak ratio X / Y is not particularly limited, but is, for example, 100 or less.
[0089] The peak ratio X / Y is obtained as follows. First, an MH loop after background correction is obtained in the same manner as in the above-mentioned method for measuring the coercive force Hc. Next, an SFD curve is calculated from the obtained MH loop. A program attached to the measuring device or other programs may be used to calculate the SFD curve. The absolute value of the point where the calculated SFD curve crosses the Y axis (dM / dH) is taken as "Y" and the height of the main peak observed in the vicinity of the coercive force Hc in the MH loop is taken as "X" to calculate the peak ratio X / Y. The measurement of the MH loop is performed at 25°C in the same manner as in the above-mentioned method for measuring the coercive force Hc. In addition, "demagnetization field correction" is not performed when measuring the MH loop in the thickness direction (perpendicular direction) of the magnetic recording medium 10. In addition, the MH loop may be measured by stacking multiple samples to be measured according to the sensitivity of the VSM used.
[0090] (Activation volume Vact) The activation volume Vact is preferably 8000 nm 3 Less than 6000 nm, more preferably 3 Less than or equal to 5000 nm, and even more preferably less than 5000 nm 3 Below 4000 nm, particularly preferably 3 Below 3000 nm, most preferably 3 The activation volume Vact is 8000 nm 3 If the magnetic powder is dispersed in a good state, the bit inversion region can be made steeper, and the magnetic signal recorded on the adjacent track can be prevented from being deteriorated by the leakage magnetic field from the recording head, resulting in a better SNR.
[0091] The activation volume Vact is calculated by the following formula derived by Street & Woolley. Vact(nm 3 )=kB×T×Χirr / (μ0×Ms×S) (where kB is the Boltzmann constant (1.38×10 -23 J / K), T: temperature (K), Χirr: irreversible magnetic susceptibility, μ0: vacuum permeability, S: magnetorheological coefficient, Ms: saturation magnetization (emu / cm3 ))
[0092] The irreversible magnetic susceptibility Χirr, saturation magnetization Ms, and magnetic viscosity coefficient S substituted in the above formula are obtained using VSM as follows. The measurement sample used in VSM is prepared by punching out three magnetic recording media 10 stacked with double-sided tape using a φ6.39 mm punch. At this time, marking is performed with any non-magnetic ink so that the longitudinal direction (running direction) of the magnetic recording medium 10 can be identified. The measurement direction by VSM is the thickness direction (vertical direction) of the magnetic recording medium 10. Furthermore, the measurement by VSM is performed at 25°C on a measurement sample cut out from a long magnetic recording medium 10. Furthermore, "demagnetization field correction" is not performed when measuring the MH loop in the thickness direction (vertical direction) of the magnetic recording medium 10. Furthermore, a high-sensitivity vibration sample magnetometer "VSM-P7-15 type" manufactured by Toei Kogyo Co., Ltd. is used to measure the MH loop of the measurement sample (the entire magnetic recording medium 10) and the MH loop of the correction sample (substrate 11). The measurement conditions were as follows: measurement mode: full loop, maximum magnetic field: 15 kOe, magnetic field step: 40 bits, time constant of locking amp: 0.3 sec, waiting time: 1 sec, number of MH averages: 20.
[0093] (irreversible magnetic susceptibility Χirr) The irreversible magnetic susceptibility Χirr is defined as the slope of the remanent magnetization curve (DCD curve) near the remanent coercivity Hr. First, a magnetic field of -1193 kA / m (15 kOe) is applied to the entire magnetic recording medium 10, and the magnetic field is returned to zero to create a remanent magnetization state. Then, a magnetic field of about 15.9 kA / m (200 Oe) is applied in the opposite direction, and the magnetic field is returned to zero again to measure the amount of remanent magnetization. After that, a magnetic field 15.9 kA / m larger than the previous applied magnetic field is applied, and the measurement is repeated to return the magnetic field to zero. The remanent magnetization is plotted against the applied magnetic field to measure the DCD curve. From the obtained DCD curve, the point where the magnetization amount is zero is taken as the remanent coercivity Hr, and the DCD curve is differentiated to determine the slope of the DCD curve for each magnetic field. The slope of this DCD curve near the remanent coercivity Hr is the slope of the DCD curve.
[0094] (Saturation magnetization Ms) First, a background-corrected MH loop is obtained in the same manner as in the above-mentioned method for measuring the coercive force Hc. Next, the value of the saturation magnetization Ms(emu) of the obtained MH loop and the volume (cm 3 ) to Ms(emu / cm 3 ) is calculated. The volume of the magnetic layer 13 is found by multiplying the area of the measurement sample by the average thickness of the magnetic layer 13. The method for calculating the average thickness of the magnetic layer 13, which is necessary for calculating the volume of the magnetic layer 13, is as described above.
[0095] (Magnetic viscosity coefficient S) First, a magnetic field of -1193 kA / m (15 kOe) is applied to the entire magnetic recording medium 10 (measurement sample), and the magnetic field is returned to zero to create a state of residual magnetization. After that, a magnetic field equivalent to the value of the residual coercivity Hr obtained from the DCD curve is applied in the opposite direction. With the magnetic field applied, the amount of magnetization is continuously measured at regular time intervals for 1000 seconds. The magnetic viscosity coefficient S is calculated by referring to the relationship between time t and amount of magnetization M(t) obtained in this way according to the following formula. M(t) = M0 + S × ln(t) (where M(t) is the amount of magnetization at time t, M0 is the initial amount of magnetization, S is the magnetic viscosity coefficient, and ln(t) is the natural logarithm of time.)
[0096] (Data band and servo band) Fig. 4 is a schematic diagram of the magnetic recording medium 10 as viewed from above. As shown in Fig. 4, the magnetic layer 13 has a plurality of data bands DB (data bands DB0 to DB3 are shown in Fig. 4) extending in the longitudinal direction (X-axis direction) of the magnetic recording medium 10, and a plurality of servo bands SB (servo bands SB0 to SB4 are shown in Fig. 4) extending in the longitudinal direction (X-axis direction) of the magnetic recording medium 10. A data signal is written in each of the plurality of data bands DB, and a servo signal for tracking control of the magnetic head is written in each of the plurality of servo bands SB. In addition, each data band DB is arranged so as to be sandwiched between a plurality of adjacent servo bands SB in the width direction (Y-axis direction).
[0097] The total area S of the servo bands S relative to the area S of the surface 13S of the magnetic layer 13 SB The ratio of R S (=(S SB From the viewpoint of ensuring a high recording capacity, the upper limit of the ratio of the total area S of the servo bands SB to the surface area S of the magnetic layer 13 is preferably 4.0% or less, more preferably 3.0% or less, and even more preferably 2.0% or less. SB The ratio of R S The lower limit is preferably 0.8% or more, from the viewpoint of ensuring five or more servo tracks.
[0098] The total area S of the servo bands SB relative to the area S of the surface 13S of the magnetic layer 13 SB The ratio of R S For example, the servo bandwidth W can be measured by developing the magnetic recording medium 10 using a ferricolloid developer (Sigma Car Q, manufactured by Sigma High Chemical Co., Ltd.) and then observing the developed magnetic recording medium 10 with an optical microscope. SB and the number of servo bands SB. Next, calculate the ratio R from the following formula: S Request. Ratio R S[%]=(((Servo bandwidth W SB )×(number of servo bands) / (magnetic recording medium Body width 10)) x 100
[0099] The number of servo bands SB is preferably 5 or more, and more preferably 5+4n or more (where n is a positive integer). If the number of servo bands SB is 5 or more, the effect on the servo signal due to dimensional changes in the width direction of the magnetic recording medium 10 can be suppressed, and stable recording and reproducing characteristics with little off-track can be ensured.
[0100] Servo Bandwidth W SB From the viewpoint of ensuring a high recording capacity, the upper limit of the servo band width W is preferably 95 μm or less, more preferably 60 μm or less, and even more preferably 30 μm or less. SB From the viewpoint of recording head manufacturing, the lower limit of the servo band width W is preferably 10 μm or more. SB The width of the servo band width W is obtained as follows. First, the magnetic recording medium 10 is developed using a ferricolloid developer (Sigma Car Q, manufactured by Sigma High Chemical Co., Ltd.). Next, the developed magnetic recording medium 10 is observed with an optical microscope to determine the servo band width W SB The width can be measured.
[0101] As shown in Fig. 4, the data band DB can form a plurality of recording tracks 5 each extending along the X-axis direction and aligned adjacent to each other in the Y-axis direction. Data signals are recorded in the recording tracks 5 along the recording tracks 5. In this technology, the length of one bit in the longitudinal direction of the data signal recorded in the data band DB (the distance between magnetization reversals) is typically 48 nm or less. The servo band SB includes a predetermined servo signal recording pattern 6 in which a servo signal is recorded by a servo signal recording device (not shown).
[0102] 5 is an enlarged view showing the recording tracks 5 in the data band DB. As shown in FIG. 5, each recording track 5 has a predetermined recording track width Wd in the Y-axis direction. The recording track width Wd is typically 3.0 μm or less. Note that such a recording track width Wd can be measured, for example, by developing the magnetic recording medium 10 using a developer such as a ferricolloid developer, and then observing the developed magnetic recording medium 10 with an optical microscope.
[0103] The number of recording tracks 5 included in one data band DB is, for example, about 1000 to 2000.
[0104] 6 is an enlarged view showing a servo signal recording pattern 6 in a servo band SB. As shown in FIG. 6, the servo signal recording pattern 6 includes a plurality of stripes 7 inclined at a predetermined azimuth angle α with respect to the width direction (Y-axis direction). The plurality of stripes 7 are classified into a first stripe group 8 inclined clockwise with respect to the width direction (Y-axis direction) and a second stripe group 9 inclined counterclockwise with respect to the width direction. The shape of such stripes 7 can be measured, for example, by developing the magnetic recording medium 10 with a developer such as a ferricolloid developer, and then observing the developed magnetic recording medium 10 with an optical microscope.
[0105] 6, the servo trace lines T, which are lines traced by a servo read head on the servo signal recording pattern 6, are shown by dashed lines. The servo trace lines T are set along the longitudinal direction (X-axis direction) and are set at a predetermined interval Ps in the width direction.
[0106] The number of servo trace lines T per servo band SB is, for example, about 30 to 60.
[0107] The interval Ps between two adjacent servo trace lines T is the same as the recording track width Wd, and is, for example, 2.0 μm or less. Here, the interval Ps between two adjacent servo trace lines T is a value that determines the recording track width Wd. In other words, when the interval Ps between the servo trace lines T is narrowed, the recording track width Wd is narrowed and the number of recording tracks 5 included in one data band DB increases. As a result, the data recording capacity increases (and vice versa when the interval Ps is widened). Therefore, in order to increase the recording capacity, it is necessary to reduce the recording track width Wd, but as a result of the interval Ps between the servo trace lines T also being narrowed, it becomes difficult to accurately trace the adjacent servo trace lines. Therefore, in this embodiment, as described later, the reproduction signal width, i.e., the half-width of the isolated waveform in the reproduction waveform of the data signal is narrowed, thereby making it possible to cope with the narrowing of the recording track width Wd.
[0108] The half-width PW50 of an isolated waveform in the reproduced waveform of a data signal recorded on the recording track 5 of the magnetic recording medium 10 is, for example, 200 nm or less, preferably 175 nm or less, more preferably 170 nm or less, and even more preferably 165 nm or less.
[0109] The half-width PW50 of the isolated waveform can be found, for example, as follows. First, a digital storage oscilloscope is used to average (synchronous averaging) a number of isolated waveforms under conditions of, for example, sampling: 500Ms / s (2nsec / point) and sampling number: 50,000 points. Then, the half-width of the isolated waveform is calculated from the obtained isolated reproduced waveform. Note that the synchronous averaging is performed by aligning at the peak position of the waveform.
[0110] A TMR head including a TMR element (TMR: Tunnel Magneto Resistive) is used as a servo read head for reading the servo signal. The reproducing track width of the servo signal in this TMR head (Y-axis direction: width direction of the magnetic recording medium 10) is 48 nm. The spacing between the two shields in the TMR head used here (X-axis direction: conveying direction of the magnetic recording medium 10) is 40 nm, and the bias current in the TMR head is less than 2 mA. The conveying speed of the magnetic recording medium 10 is 2 m / s.
[0111] [1-2 Manufacturing method of magnetic recording medium 10] Next, a method for manufacturing the magnetic recording medium 10 having the above-mentioned configuration will be described. First, a paint for forming the undercoat layer is prepared by kneading and dispersing non-magnetic powder, binder, lubricant, etc. in a solvent. Next, a paint for forming the magnetic layer is prepared by kneading and dispersing magnetic powder, binder, lubricant, etc. in a solvent. Next, a paint for forming the back layer is prepared by kneading and dispersing binder, non-magnetic powder, etc. in a solvent. For example, the following solvents, dispersing devices, and kneading devices can be used to prepare the paint for forming the magnetic layer, the paint for forming the undercoat layer, and the paint for forming the back layer.
[0112] Examples of the solvent used in preparing the coating material include ketone-based solvents such as acetone, methyl ethyl ketone, methyl isobutyl ketone, and cyclohexanone, alcohol-based solvents such as methanol, ethanol, and propanol, ester-based solvents such as methyl acetate, ethyl acetate, butyl acetate, propyl acetate, ethyl lactate, and ethylene glycol acetate, ether-based solvents such as diethylene glycol dimethyl ether, 2-ethoxyethanol, tetrahydrofuran, and dioxane, aromatic hydrocarbon-based solvents such as benzene, toluene, and xylene, and halogenated hydrocarbon-based solvents such as methylene chloride, ethylene chloride, carbon tetrachloride, chloroform, and chlorobenzene. These may be used alone or in appropriate mixture.
[0113] Examples of the kneading device used in the preparation of the above-mentioned coating material include, but are not limited to, a continuous twin-screw kneader, a continuous twin-screw kneader capable of diluting in multiple stages, a kneader, a pressure kneader, a roll kneader, etc. Examples of the dispersing device used in the preparation of the above-mentioned coating material include, but are not limited to, a roll mill, a ball mill, a horizontal sand mill, a vertical sand mill, a spike mill, a pin mill, a tower mill, a pearl mill (for example, "DCP Mill" manufactured by Eirich Co., Ltd.), a homogenizer, an ultrasonic dispersing machine, etc.
[0114] Next, the underlayer forming paint is applied to one main surface 11A of the substrate 11 and dried to form the underlayer 12. Next, the magnetic layer forming paint is applied to the underlayer 12 and dried to form the magnetic layer 13 on the underlayer 12. During drying, it is preferable to magnetically orient the magnetic powder in the thickness direction of the substrate 11, for example, by a solenoid coil. Also, during drying, the magnetic powder may be magnetically oriented in the running direction (longitudinal direction) of the substrate 11, and then magnetically oriented in the thickness direction of the substrate 11, for example, by a solenoid coil. By performing such magnetic field orientation treatment, the degree of vertical orientation (i.e., squareness ratio S1) of the magnetic powder can be improved. After the magnetic layer 13 is formed, the back layer forming paint is applied to the other main surface 11B of the substrate 11 and dried to form the back layer 14. This results in a magnetic recording medium 10.
[0115] The squareness ratios S1, S2 and the ratio Hc2 / Hc1 are set to desired values by, for example, adjusting the strength of the magnetic field applied to the coating film of the paint for forming the magnetic layer, the concentration of the solid content in the paint for forming the magnetic layer, and the drying conditions (drying temperature and drying time) of the coating film of the paint for forming the magnetic layer. The strength of the magnetic field applied to the coating film is preferably at least twice the coercive force of the magnetic powder. In order to further increase the squareness ratio S1 (i.e., to further reduce the squareness ratio S2), it is preferable to improve the dispersion state of the magnetic powder in the paint for forming the magnetic layer. In addition, in order to further increase the squareness ratio S1, it is also effective to magnetize the magnetic powder before the paint for forming the magnetic layer enters an orientation device for magnetic field orientation of the magnetic powder. The above-mentioned methods for adjusting the squareness ratios S1 and S2 may be used alone or in combination of two or more.
[0116] The obtained magnetic recording medium 10 is then subjected to a calendaring process to smooth the surface 13S of the magnetic layer 13. Next, the calendared magnetic recording medium 10 is wound into a roll, and in this state, the magnetic recording medium 10 is subjected to a heat treatment to transfer the numerous protrusions on the surface 14S of the back layer 14 to the surface 13S of the magnetic layer 13. As a result, numerous pores are formed in the surface 13S of the magnetic layer 13.
[0117] The heat treatment temperature is preferably 50° C. or higher and 80° C. or lower. When the heat treatment temperature is 50° C. or higher, good transferability can be obtained. On the other hand, when the heat treatment temperature is 80° C. or lower, the amount of pores becomes too large, and there is a risk of an excess of lubricant on the surface 13S of the magnetic layer 13. Here, the heat treatment temperature is the temperature of the atmosphere in which the magnetic recording medium 10 is held.
[0118] The heat treatment time is preferably 15 hours or more and 40 hours or less. When the heat treatment time is 15 hours or more, good transferability can be obtained. On the other hand, when the heat treatment time is 40 hours or less, a decrease in productivity can be suppressed.
[0119] The pressure applied to the magnetic recording medium 10 during the heat treatment should preferably be in the range of 150 kg / cm to 400 kg / cm.
[0120] Finally, the magnetic recording medium 10 is cut to a predetermined width (for example, 1 / 2 inch width). In this manner, the desired magnetic recording medium 10 is obtained.
[0121] [1-3 Configuration of recording / playback device 30] Next, with reference to FIG. 7, a configuration of a recording / reproducing device 30 that records information on the above-mentioned magnetic recording medium 10 and reproduces information from the above-mentioned magnetic recording medium 10 will be described.
[0122] The recording and reproducing device 30 has a configuration capable of adjusting the tension applied to the magnetic recording medium 10 in the longitudinal direction. The recording and reproducing device 30 has a configuration capable of loading a magnetic recording medium cartridge 10A. Here, for ease of explanation, a case will be described in which the recording and reproducing device 30 has a configuration capable of loading one magnetic recording medium cartridge 10A. However, in the present disclosure, the recording and reproducing device 30 may have a configuration capable of loading a plurality of magnetic recording medium cartridges 10A. As described above, the magnetic recording medium 10 is in the form of a tape, and may be, for example, a long magnetic recording tape. The magnetic recording medium 10 may be housed in a housing in a state in which it is wound around a reel inside the magnetic recording medium cartridge 10A. The magnetic recording medium 10 is adapted to run in the longitudinal direction during recording and reproducing. The magnetic recording medium 10 may be configured to record signals at a shortest recording wavelength of preferably 100 nm or less, more preferably 75 nm or less, even more preferably 60 nm or less, and particularly preferably 50 nm or less, and may be used in a recording and reproducing device 30 in which the shortest recording wavelength is within the above range, for example. The recording track width can be, for example, 2 μm or less.
[0123] The recording / playback device 30 is connected to information processing devices such as a server 41 and a personal computer (hereinafter referred to as "PC") 42, for example, via a network 43, and is configured to be able to record data supplied from these information processing devices onto the magnetic recording medium cartridge 10A.
[0124] As shown in FIG. 7, the recording / playback device 30 includes a spindle 31, a reel 32, a drive unit 33, a drive unit 34, a plurality of guide rollers 35, a head unit 36, a communication interface (hereinafter referred to as I / F) 37, and a control device 38.
[0125] The spindle 31 is configured to be able to mount the magnetic recording medium cartridge 10A. The magnetic recording medium cartridge 10A is compliant with the LTO (Linear Tape Open) standard, and a single reel 10C around which the magnetic recording medium 10 is wound is rotatably housed in a cartridge case 10B. A V-shaped servo pattern is recorded in advance as a servo signal on the magnetic recording medium 10. The reel 32 is configured to be able to fix the tip of the magnetic recording medium 10 pulled out from the magnetic recording medium cartridge 10A.
[0126] The driving device 33 is a device that rotates the spindle 31. The driving device 34 is a device that rotates the reel 32. When recording or reproducing data on the magnetic recording medium 10, the driving devices 33 and 34 rotate the spindle 31 and the reel 32, respectively, to run the magnetic recording medium 10. The guide roller 35 is a roller for guiding the running of the magnetic recording medium 10.
[0127] The head unit 36 includes a plurality of recording heads for recording data signals on the magnetic recording medium 10, and a plurality of reproducing heads for reproducing the data signals recorded on the magnetic recording medium 10. As the recording heads, for example, a ring-type head can be used, and as the reproducing heads, for example, a magnetoresistive effect magnetic head can be used, but the types of the recording heads and reproducing heads are not limited to these.
[0128] The I / F 37 is for communicating with information processing devices such as a server 41 and a PC 42 , and is connected to a network 43 .
[0129] The control device 38 controls the entire recording / reproducing device 30. For example, in response to a request from the information processing device, such as the server 41 or the PC 42, the control device 38 records a data signal supplied from the information processing device on the magnetic recording medium 10 by the head unit 36. In addition, in response to a request from the information processing device, such as the server 41 or the PC 42, the control device 38 reproduces the data signal recorded on the magnetic recording medium 10 by the head unit 36, and supplies it to the information processing device.
[0130] FIG. 8 is a front view showing the overall configuration of the servo signal recording device 100. FIG. 9 is a schematic diagram showing an enlarged configuration of the main parts of the servo signal recording device 100. As shown in FIG. 8, the servo signal recording device 100 includes, from upstream to downstream in the transport direction of the magnetic recording medium 10, a feed roller 51, a pre-processing unit 52, a servo signal recording head 53, a servo signal reproducing head 54, and a take-up roller 55. Note that the back layer 14 of the magnetic recording medium 10 is omitted in FIG. 8. The servo signal recording device 100 may also include a control unit that comprehensively controls each part of the servo signal recording device 100, a recording unit in which various programs and data required for processing by the control unit are stored, and a display unit that displays data.
[0131] The feed roller 51 is capable of rotatably supporting the magnetic recording medium 10 (before the servo signal recording pattern 6 is recorded) which is a roll-shaped magnetic tape. The feed roller 51 is rotated in response to the driving of a driving source such as a motor, and feeds out the magnetic recording medium 10 downstream in response to the rotation.
[0132] The winding roller 55 is capable of rotatably supporting the magnetic recording medium 10 after the servo signal recording pattern 6 is recorded. The winding roller 55 rotates in synchronization with the delivery roller 51 in response to the drive of a driving source such as a motor, and takes up the magnetic recording medium 10 on which the servo signal recording pattern 6 is recorded in response to the rotation. The delivery roller 51 and the winding roller 55 are capable of moving the magnetic recording medium 10 at a constant speed on the transport path.
[0133] The pre-processing unit 52 is disposed, for example, upstream of the servo signal recording head 53 and below the magnetic recording medium 10 (at a position opposite to the surface of the magnetic layer 13). However, the pre-processing unit 52 may be disposed above the magnetic recording medium 10 (at a position facing the surface of the magnetic layer 13). The pre-processing unit 52 includes a permanent magnet 52A that can rotate about a rotation axis along the Y-axis direction, i.e., the width direction of the magnetic recording medium 10. The shape of the permanent magnet 52A is, for example, a cylindrical shape or a polygonal prism shape, but is not limited thereto.
[0134] Before the servo signal recording head 53 records the servo signal recording pattern 6, the permanent magnet 52A applies a magnetic field to the entire magnetic layer 13 by a DC magnetic field, thereby demagnetizing the entire magnetic layer 13. This allows the permanent magnet 52A to magnetize the magnetic layer 13 in advance in a second direction opposite to the magnetization direction of the servo signal recording pattern 6 (see the white arrow in FIG. 9). By thus setting the two magnetization directions in opposite directions, the reproduced waveform of the servo signal recording pattern 6 when it is read can be made symmetrical in the up-down direction (±) (see FIG. 11 described later).
[0135] The servo signal recording head 53 is disposed, for example, above the magnetic recording medium 10 (at a position facing the surface of the magnetic layer 13). The servo signal recording head 53 may also be disposed below the magnetic recording medium 10 (opposite the surface of the magnetic layer 13). The servo signal recording head 53 generates a magnetic field at a predetermined timing in response to a square wave pulse signal, and applies the magnetic field to a part of the magnetic layer 13 (after pretreatment) of the magnetic recording medium 10.
[0136] As a result, the servo signal recording head 53 magnetizes a part of the magnetic layer 13 in the first direction to record the servo signal recording pattern 6 on the magnetic layer 13 (see the black arrow in FIG. 9). When the magnetic layer 13 passes below the servo signal recording head 53, the servo signal recording head 53 is capable of recording the servo signal recording pattern 6 on each of the five servo bands SB0 to SB4.
[0137] The first direction, which is the magnetization direction of the servo signal recording pattern 6, includes a perpendicular component perpendicular to the top surface of the magnetic layer 13. That is, in this embodiment, since the magnetic layer 13 contains perpendicularly oriented or non-oriented magnetic powder, the servo signal recording pattern 6 recorded in the magnetic layer 13 includes a perpendicular magnetization component.
[0138] Fig. 10 is a diagram showing the magnetization direction of the magnetic recording medium 10. As shown in Fig. 10, in this specification, the angle (0°) when the magnetization direction faces the transport direction of the magnetic recording medium 10 is taken as the reference, and the clockwise direction is taken as the direction in which the angle increases. Fig. 10 shows the magnetization direction of the servo signal recording pattern 6, but the same applies to the magnetization direction of the magnetization after preprocessing by the preprocessing unit 52 and the magnetization direction of the entire magnetic layer 13.
[0139] The magnetization direction (first direction) of the servo signal recording pattern 6 differs depending on the squareness ratio of the magnetic layer 13. For example, perpendicularly oriented barium ferrite, non-oriented barium ferrite, and perpendicularly oriented acicular metal typically have different squareness ratios. In such cases, even if a magnetic field is applied under the same conditions in the servo signal recording section 13, the magnetization direction (first direction) of the servo signal recording pattern 6 differs. In other words, if the squareness ratio is the same and the conditions of the servo signal recording head 53 are the same, the first direction is the same even if the type of magnetic recording medium 10 is different.
[0140] The magnetization direction (first direction) of the servo signal recording pattern 6 differs depending on the squareness ratio of the magnetic layer 13. Therefore, in order to match the magnetization direction of the servo signal recording pattern 6, the magnetization direction (second direction) of the pre-processing in the pre-processing unit 52 also needs to be made different.
[0141] In this embodiment, the permanent magnet 52A is rotatable about the rotation axis along the Y-axis direction, which allows the magnetization direction (second direction) by the pre-processing to be appropriately adjusted according to the type of the magnetic recording medium 10.
[0142] There is an appropriate angle range for the angle of the permanent magnet 52A depending on the type of magnetic recording medium 10. In this specification, the angle of the permanent magnet 52A is defined as the reference angle (0°) when the N pole of the permanent magnet 52A faces the transport direction of the magnetic recording medium 10, and the angle increases in the clockwise direction.
[0143] Here, the servo signal recording head 53 overwrites the servo signal recording pattern 6 on the magnetic layer 13 magnetized in the second direction by the permanent magnet 52A. However, the first direction, which is the magnetization direction of the servo signal recording pattern 6, is constant regardless of the second direction as long as the squareness ratio of the magnetic layer 13 is the same.
[0144] The servo signal reproducing head 54 is disposed downstream of the servo signal recording head 53 and above the magnetic recording medium 10 (at a position facing the magnetic layer 13). The servo signal reproducing head 54 reads the servo signal recording pattern 6 from the magnetic layer 13 of the magnetic recording medium 10 that has been preprocessed by the preprocessing unit 52 and on which the servo signal recording pattern 6 has been recorded by the servo signal recording head 53. The reproduced waveform of the servo signal recording pattern 6 read by the servo signal reproducing head 54 is displayed on the screen of the display unit.
[0145] Typically, the servo signal reproducing head 54 detects magnetic flux generated from the surface of the servo band SB when the magnetic layer 13 passes under the servo signal reproducing head 54. The magnetic flux detected at this time becomes the reproduced waveform of the servo signal recording pattern 6.
[0146] FIG. 11 is a diagram showing the relationship between the magnetization direction and the reproduced waveform of the servo signal recording pattern 6. As shown in FIG.
[0147] 11, in this embodiment, the magnetization direction of the servo signal recording pattern 6 and the magnetization direction by the pre-processing are opposite to each other, so that the reproduced waveform of the servo signal recording pattern 6 when the servo signal recording pattern 6 is read can be made symmetrical in the up-down direction (±). Note that if the servo signal recording pattern 6 is recorded without pre-processing, the servo signal recording pattern 6 contains a magnetization component in the vertical direction, so the reproduced waveform becomes asymmetrical in the up-down direction (±).
[0148] Furthermore, in this embodiment, the amount of magnetic flux generated near the surface of the magnetic layer 13 can be increased compared to when the servo signal recording pattern 6 is recorded without pre-processing. This makes it possible to obtain a high-output reproduced waveform even when the magnetic layer 13 is thin.
[0149] Here, the magnetization direction (first direction) of the servo signal recording pattern 6 and the magnetization direction (second direction) by the pre-processing do not need to be strictly opposite directions, but may be substantially opposite directions. This is related to the symmetry of the reproduced waveform of the servo signal recording pattern 6.
[0150] Let us assume that the magnetization direction of the servo signal recording pattern 6 and the magnetization direction by the pre-processing are not exactly opposite to each other, but slightly shifted. For example, suppose that the magnetization direction of the servo signal recording pattern 6 is -120°, and the magnetization direction by the pre-processing is 50° (see FIG. 10). Even in such a case, it is sufficient that the reproduced waveform of the servo signal recording pattern 6 has symmetry to the extent that the servo signal recording pattern 6 can be properly read. The fact that the reproduced waveform of the servo signal recording pattern 6 has symmetry means that the magnetization direction of the servo signal recording pattern 6 (first direction) and the magnetization direction by the pre-processing (second direction) are opposite to each other.
[0151] The following describes how to determine whether the reproduced waveform of the servo signal recording pattern 6 is symmetric or asymmetric. For example, if the difference between the maximum voltage value Vmax and the minimum voltage value Vmin (absolute value) of the reproduced waveform is within the allowable range (approximately 5% to 10%) for the amplitude of the reproduced waveform, the reproduced waveform is determined to be symmetric.
[0152] [1-4 Effects] As described above, the magnetic recording medium 10 of the present embodiment is a tape-shaped member in which the substrate 11, the underlayer 12, and the magnetic layer 13 are laminated in this order, and is designed to satisfy each of the following constituent requirements (1) to (9). (1) The substrate 11 contains polyester as a main component. (2) The magnetic layer 13 is provided on the substrate 11, contains a plurality of magnetic powder particles, and is capable of recording data signals. (3) The arithmetic mean roughness Ra of the surface of the magnetic layer is 2.5 nm or less. (4) The PSD up to a spatial wavelength of 5 μm is 2.5 μm or less. (5) The average thickness of the magnetic layer 13 is 90 nm or less. (6) The average aspect ratio of the magnetic powder in the magnetic layer 13 is equal to or greater than 1.0 and equal to or less than 3.0. (7) The coercive force Hc1 in the perpendicular direction is equal to or less than 3000 Oersted. (8) The ratio Hc2 / Hc1 of the coercive force Hc2 in the longitudinal direction to the coercive force Hc1 in the perpendicular direction is 0.8 or less. (9) The half-width PW50 of an isolated waveform in the reproduced waveform of a data signal is 200 nm or less.
[0153] The magnetic recording medium 10 of the present embodiment has such a configuration, and while making the magnetization transition width steep, it is possible to ensure good electromagnetic conversion characteristics (e.g., C / N), and therefore it is possible to realize a configuration that is advantageous for high density recording.
[0154] (Basic concept of this technology) Here, the basic concept of the present technology will be described. In the present technology, attention is paid to the half-value width PW50 of an isolated waveform in a reproduced waveform of a data signal. Therefore, the half-value width PW50 of this isolated waveform will be described.
[0155] As shown in Figure 11 above, the reproduced waveform when the data signal is read out protrudes on both the positive and negative sides. An isolated waveform basically refers to either of these waveforms.
[0156] Fig. 12 is a diagram for explaining the half-width PW50 of an isolated waveform. In Fig. 12, the vertical axis is intensity (arbitrary unit) and the horizontal axis is length along the running direction. As shown in Fig. 12, the half-width PW50 is the width of the waveform at a height that is half (50%) of the maximum value (100%) in the reproduced waveform of the data signal.
[0157] This half-value width PW50 is a value that indicates the sharpness of the peak in the reproduced waveform of the data signal. In other words, the narrower the half-value width PW50, the sharper the peak in the reproduced waveform, and conversely, the wider the half-value width PW50, the duller the peak in the reproduced waveform.
[0158] FIG. 13 is a diagram for explaining the basic concept of the present technology, showing two stripes 7 in a servo signal recording pattern 6. In FIG.
[0159] 13, of the multiple stripes 7 included in the first stripe group 8 of the servo signal recording pattern 6, an arbitrary stripe 7 is designated as a first stripe 7a. Furthermore, of the multiple stripes 7 included in the second stripe group 9 of the servo signal recording pattern 6, an arbitrary stripe 7 is designated as a second stripe 7b. Furthermore, of the multiple servo trace lines T, an arbitrary servo trace line T is designated as a first servo trace line T1. Furthermore, the servo trace line T adjacent to the first servo trace line T1 is designated as a second servo trace line T2.
[0160] Also, the intersection point between the first stripe 7a and the first servo trace line T1 is defined as P1. Note that, regarding this P1, any point on the first stripe 7a may be defined as P1.
[0161] Also, the intersection point between the first stripe 7a and the second servo trace line T2 is defined as P2. Alternatively, P2 may be a point on the first stripe 7a that is spaced apart from P1 by an interval Ps (i.e., the recording track width Wd) in the width direction (Y-axis direction).
[0162] The distance between P1 and P2 in the longitudinal direction (X-axis direction) is defined as distance D. Distance D corresponds to the longitudinal deviation between adjacent tracks. The intersection of second stripe 7b and first servo trace line T1 is defined as P3, and the intersection of second stripe 7b and second servo trace line T2 is defined as P4.
[0163] When the first servo trace line T1 is being traced, it is necessary to determine the difference between the time when the reproduced waveform is detected at P1 and the time when the reproduced waveform is detected at P3. This difference is defined as a first period. Similarly, when the second trace line T is being traced, it is necessary to determine the difference between the time when the reproduced waveform is detected at P2 and the time when the reproduced waveform is detected at P4. This difference is defined as a second period.
[0164] Next, consider the difference between the first period and the second period. Here, assume that the interval Ps of the servo trace lines T and the recording track width Wd are both 1.56 μm, and the azimuth angle α is 12 degrees. In this case, the distance D is 1.56×tan12°, or 0.33 μm. The difference between the distance between P1 and P3 and the distance between P2 and P4 is twice the distance D, or 0.66 μm.
[0165] At this time, if the running speed of the magnetic recording medium 1 is 5 m / s, then 0.66 / 5000000 is 0.13 μs, which is the difference between the first period and the second period.
[0166] In other words, in order to accurately trace the first servo trace line T1 and the second servo trace line T2, it is necessary to accurately determine the minute difference of 0.13 μs. If this cannot be done, the data signal will be recorded on the adjacent recording track 5.
[0167] However, if the peaks in the reproduced waveform of the data signal (FIG. 11) are not sharp, such a small difference cannot be accurately determined. In particular, if the recording track width Wd is reduced and the interval Ps of the servo trace lines T is reduced in order to increase the number of recording tracks 5, the distance D becomes narrower and the difference between the first and second periods becomes smaller.
[0168] Therefore, in the present technology, the degree of perpendicular orientation of the magnetic layer 13 is set to a certain value or more, so that the half-width of the isolated waveform in the reproduced waveform of the data signal is set to a certain value or less, thereby making the peak of the reproduced waveform of the data signal sharper.
[0169] More specifically, the half-width of the isolated waveform can be made 200 nm or less by setting the ratio Hc2 / Hc1, which is an index of the degree of perpendicular orientation of the magnetic powder in the magnetic layer 13, to 0.8 or less. This makes it possible to make the peaks in the reproduced waveform of the data signal sharp enough to distinguish the above-mentioned minute differences (e.g., 0.13 μs) (see each embodiment described later).
[0170] Furthermore, in this technology, the PSD for spatial wavelengths up to 5 μm is set to a certain value or less, for example, 2.5 μm or less, in the magnetic layer 13. By suppressing the PSD to a certain value or less, the spacing between the recording / reproducing head and the tape during recording / reproducing can be reduced, making the medium more suitable for high recording density.
[0171] (Stretchability and tension control of magnetic recording medium 10) Next, the elasticity of the magnetic recording medium 10 and tension control of the magnetic recording medium 10 by the recording and reproducing device 30 will be described. In the LTO standard, the number of recording tracks is rapidly increasing due to the demand for high density data recording. In such a case, the recording track width becomes narrow, and even a slight variation in the width (Y-axis direction) of the magnetic recording medium 10 may become a problem.
[0172] For example, suppose that predetermined data is stored in the magnetic recording medium 10 by the recording and reproducing device 30, and then (for example, after a certain period of storage), the data recorded on the magnetic recording medium 10 is reproduced by the recording and reproducing device 30. In such a case, if the width of the magnetic recording medium 10 during data reproduction varies even slightly compared to the width of the magnetic recording medium 10 during data recording, off-track (the data reproduction head of the head unit 36 is positioned on the wrong recording track 5) may occur. As a result, the data recorded on the magnetic recording medium 10 may not be reproduced accurately, and an error may occur.
[0173] Causes of the width fluctuation of the magnetic recording medium 10 include, for example, temperature fluctuation, humidity fluctuation, etc. Generally, a method is used in which the magnetic recording medium 10 is designed so that it does not expand or contract, thereby dealing with the width fluctuation of the magnetic recording medium 10. However, it is practically impossible to completely prevent the magnetic recording medium 10 from expanding or contracting.
[0174] Therefore, in this embodiment, rather than making the magnetic recording medium 10 difficult to expand and contract, a method is used in which the magnetic recording medium 10 is made somewhat easier to expand and contract, and the tension of the magnetic recording medium 10 (X-axis direction: tension in the transport direction of the magnetic recording medium 10) is controlled (increased or decreased) in the recording and reproduction device 30.
[0175] Specifically, when reproducing a data signal, the recording and reproducing device 30 increases the tension in the longitudinal direction (X-axis direction) of the magnetic recording medium 10 as necessary (when the width of the magnetic recording medium 10 is widened), thereby reducing the width (Y-axis direction) of the magnetic recording medium 10. Also, when reproducing a data signal, the recording and reproducing device 30 increases the width of the magnetic recording medium 10 as necessary (when the width of the magnetic recording medium 10 is narrowed), thereby reducing the tension in the longitudinal direction of the magnetic recording medium 10. Note that the recording and reproducing device 30 may control the tension in the longitudinal direction of the magnetic recording medium 10 not only when reproducing a data signal, but also when recording a data signal.
[0176] According to this method, when the width of the magnetic recording medium 10 fluctuates due to temperature or the like, it is possible to adjust the width of the magnetic recording medium 10 as necessary to make the width of the magnetic recording medium 10 constant. Therefore, it is believed that off-track can be prevented and data recorded on the magnetic recording medium 10 can be accurately reproduced.
[0177] <2. Modifications> (Variation 1) In the above embodiment, the ε-iron oxide particles 20 ( FIG. 2 ) having the shell portion 22 with a two-layer structure have been described as an example, but the magnetic recording medium of the present technology may include the ε-iron oxide particles 20A having the shell portion 23 with a single-layer structure, as shown in, for example, FIG. 14 . The shell portion 23 in the ε-iron oxide particles 20A has a similar configuration to the first shell portion 22a, for example. However, from the viewpoint of suppressing deterioration of characteristics, the ε-iron oxide particles 20 having the shell portion 22 with a two-layer structure described in the above embodiment are more preferable than the ε-iron oxide particles 20A of Modification 1.
[0178] (Variation 2) In the magnetic recording medium 10 according to the embodiment described above, the ε iron oxide particles 20 having a core-shell structure have been described as an example, but the ε iron oxide particles may contain an additive instead of the core-shell structure, or may have a core-shell structure and contain an additive. In this case, a part of Fe in the ε iron oxide particles is replaced with the additive. By containing an additive in the ε iron oxide particles, the coercive force Hc of the ε iron oxide particles as a whole can be adjusted to a coercive force Hc suitable for recording, thereby improving ease of recording. The additive is a metal element other than iron, preferably a trivalent metal element, more preferably at least one of Al (aluminum), Ga (gallium) and In (indium), and even more preferably at least one of Al and Ga.
[0179] Specifically, the ε-iron oxide containing the additive is an ε-Fe2-xMxO3 crystal (wherein M is a metal element other than iron, preferably a trivalent metal element, more preferably at least one of Al, Ga, and In, and even more preferably at least one of Al and Ga. x is, for example, 0 <x<1である。)である。
[0180] (Variation 3) The magnetic powder of the present disclosure may contain a powder of nanoparticles containing hexagonal ferrite (hereinafter referred to as "hexagonal ferrite particles") instead of a powder of ε iron oxide particles. The hexagonal ferrite particles have, for example, a hexagonal plate shape or a nearly hexagonal plate shape. The hexagonal ferrite preferably contains at least one of Ba (barium), Sr (strontium), Pb (lead) and Ca (calcium), more preferably at least one of Ba and Sr. The hexagonal ferrite may specifically be, for example, barium ferrite or strontium ferrite. The barium ferrite may further contain at least one of Sr, Pb and Ca in addition to Ba. The strontium ferrite may further contain at least one of Ba, Pb and Ca in addition to Sr.
[0181] More specifically, hexagonal ferrite has the general formula MFe 12 O 19 The average composition is represented by the formula: where M is, for example, at least one metal selected from Ba, Sr, Pb, and Ca, and preferably at least one metal selected from Ba and Sr. M may be a combination of Ba and at least one metal selected from the group consisting of Sr, Pb, and Ca. M may also be a combination of Sr and at least one metal selected from the group consisting of Ba, Pb, and Ca. In the above general formula, a part of Fe may be substituted with another metal element.
[0182] When the magnetic powder contains a powder of hexagonal ferrite particles, the average particle size of the magnetic powder is preferably 50 nm or less, more preferably 40 nm or less, and even more preferably 30 nm or less. The average particle size of the magnetic powder is preferably 25 nm or less, 22 nm or less, 21 nm or less, or even more preferably 20 nm or less. The average particle size of the magnetic powder is, for example, 10 nm or more, preferably 12 nm or more, and more preferably 15 nm or more. Therefore, the average particle size of the magnetic powder containing the powder of hexagonal ferrite particles can be, for example, 10 nm or more to 50 nm or less, 10 nm or more to 40 nm or less, 12 nm or more to 30 nm or less, 12 nm or more to 25 nm or less, or 15 nm or more to 22 nm or less. When the average particle size of the magnetic powder is the above upper limit or less (for example, 50 nm or less, particularly 30 nm or less), good electromagnetic conversion characteristics (for example, SNR) can be obtained in the high recording density magnetic recording medium 10. When the average particle size of the magnetic powder is equal to or greater than the lower limit (eg, 10 nm or greater, preferably 12 nm or greater), the dispersibility of the magnetic powder is improved, and better electromagnetic conversion characteristics (eg, SNR) can be obtained.
[0183] When the magnetic powder contains a powder of hexagonal ferrite particles, the average aspect ratio of the magnetic powder may be preferably 1 or more and 3.5 or less, more preferably 1 or more and 3.1 or less, or 2 or more and 3.1 or less, and even more preferably 2 or more and 3 or less. By having the average aspect ratio of the magnetic powder within the above numerical range, aggregation of the magnetic powder can be suppressed, and further, the resistance applied to the magnetic powder when the magnetic powder is vertically oriented in the process of forming the magnetic layer 13 can be suppressed. This can lead to an improvement in the vertical orientation of the magnetic powder.
[0184] The average particle size and average aspect ratio of the magnetic powder containing the powder of hexagonal ferrite particles are obtained as follows. First, the magnetic recording medium 10 to be measured is processed and thinned by the FIB (Focused Ion Beam) method or the like. The thinning is performed along the length direction (longitudinal direction) of the magnetic tape. The obtained thin sample is observed in cross section in the thickness direction of the recording layer at an acceleration voltage of 200 kV and a total magnification of 500,000 times using a transmission electron microscope (H-9500 manufactured by Hitachi High-Technologies). Next, 50 particles that face the side toward the observation surface are selected from the TEM photograph taken, and the maximum plate thickness DA of each particle is measured. The maximum plate thicknesses DA thus obtained are simply averaged (arithmetic average) to obtain the average maximum plate thickness DAave. Next, the plate diameter DB of each magnetic powder is measured. Here, the plate diameter DB means the maximum distance between two parallel lines drawn from all angles so as to be tangent to the contour of the magnetic powder (so-called maximum Feret diameter). Next, the average plate diameter DBave is calculated by simply averaging (arithmetic mean) the measured plate diameters DB. Then, the average aspect ratio of the particles (DBave / DAave) is calculated from the average maximum plate thickness DAave and the average plate diameter DBave.
[0185] When the magnetic powder comprises a powder of hexagonal ferrite particles, the average particle volume of the magnetic powder is preferably 5900 nm 3 Less than or equal to 500 nm, preferably 3 More than 3400nm 3 Less than or equal to 1000 nm, and even more preferably less than 1000 nm 3 More than 2500nm 3 The average particle volume of the magnetic powder is 5900 nm or less. 3 If the average particle size of the magnetic powder is 30 nm or less, the same effect as when the average particle volume of the magnetic powder is 500 nm or less can be obtained. 3 If the average particle size of the magnetic powder is 12 nm or more, the same effect as in the case where the average particle size of the magnetic powder is 12 nm or more can be obtained.
[0186] The average particle volume of the magnetic powder is calculated as follows. First, the average maximum plate thickness DAave and the average maximum plate diameter DBave are calculated using the above-mentioned method for calculating the average particle size of the magnetic powder. Next, the average volume V of the ε iron oxide particles is calculated using the following formula (2).
number
[0187] According to a particularly preferred embodiment of the present technology, the magnetic powder may be barium ferrite magnetic powder or strontium ferrite magnetic powder, more preferably barium ferrite magnetic powder. The barium ferrite magnetic powder includes magnetic particles of iron oxide having barium ferrite as a main phase (hereinafter referred to as "barium ferrite particles"). The barium ferrite magnetic powder has high reliability in data recording, for example, the coercive force does not decrease even in a high temperature and high humidity environment. From this viewpoint, the barium ferrite magnetic powder is preferable as the magnetic powder.
[0188] The average particle size of the barium ferrite magnetic powder is 50 nm or less, more preferably 10 nm or more and 40 nm or less, and even more preferably 12 nm or more and 25 nm or less.
[0189] When the magnetic layer 13 contains barium ferrite magnetic powder as the magnetic powder, the average thickness tm [nm] of the magnetic layer 13 is preferably 35 nm≦tm≦100 nm, and particularly preferably 80 nm or less. In addition, the coercive force Hc measured in the thickness direction (perpendicular direction) of the magnetic recording medium 10 is preferably 160 kA / m or more and 280 kA / m or less, more preferably 165 kA / m or more and 275 kA / m or less, and even more preferably 170 kA / m or more and 270 kA / m or less.
[0190] (Variation 4) The magnetic powder may contain a powder of nanoparticles containing Co-containing spinel ferrite (hereinafter referred to as "cobalt ferrite particles") instead of the powder of ε iron oxide particles. The cobalt ferrite particles preferably have uniaxial anisotropy. The cobalt ferrite particles have, for example, a cubic or nearly cubic shape. The Co-containing spinel ferrite may further contain at least one of Ni, Mn, Al, Cu, and Zn in addition to Co.
[0191] The Co-containing spinel ferrite has, for example, an average composition represented by the following formula. Co x M y FeO Z (In formula (1), M is, for example, at least one metal selected from the group consisting of Ni, Mn, Al, Cu, and Zn. x is a value within the range of 0.4≦x≦1.0. y is a value within the range of 0≦y≦0.3. However, x and y satisfy the relationship of (x+y)≦1.0. z is a value within the range of 3≦z≦4. A part of Fe may be substituted with another metal element.)
[0192] When the magnetic powder contains cobalt ferrite particles, the average particle size of the magnetic powder is preferably 25 nm or less, more preferably 10 nm or more and 23 nm or less. When the average particle size of the magnetic powder is 25 nm or less, good electromagnetic conversion characteristics (e.g., SNR) can be obtained in a high recording density magnetic recording medium 10. On the other hand, when the average particle size of the magnetic powder is 10 nm or more, the dispersibility of the magnetic powder is further improved, and better electromagnetic conversion characteristics (e.g., SNR) can be obtained. When the magnetic powder contains cobalt ferrite particles, the average aspect ratio of the magnetic powder is the same as that of the above-mentioned embodiment. The average particle size and average aspect ratio of the magnetic powder are also calculated in the same manner as that of the above-mentioned embodiment.
[0193] The average particle volume of the magnetic powder is preferably 15,000 nm 3 Less than 1000 nm, more preferably 3 More than 12000nm 3The average particle volume of the magnetic powder is 15,000 nm or less. 3 When the average particle size of the magnetic powder is 25 nm or less, the same effect as when the average particle volume of the magnetic powder is 1000 nm or less can be obtained. 3 With this or more, the same effect as when the average particle size of the magnetic powder is 10 nm or more can be obtained. Note that the average particle volume of the magnetic powder is calculated in the same manner as in the above-mentioned embodiment (the method for calculating the average particle volume when the ε iron oxide particles are cubic or nearly cubic).
[0194] The coercive force Hc of the cobalt ferrite magnetic powder is preferably 2500 Oe or more, and more preferably 2600 Oe or more and 3500 Oe or less.
[0195] (Variation 5) The magnetic recording medium 10 may further include a barrier layer provided on at least one surface of the substrate 11. This barrier layer is a layer for suppressing dimensional changes of the substrate 11 according to the environment. For example, one example of a cause of the dimensional changes is the hygroscopicity of the substrate 11, and the provision of a barrier layer can reduce the rate at which moisture penetrates into the substrate 11. The barrier layer includes, for example, a metal or a metal oxide. As the metal, for example, at least one of Al, Cu, Co, Mg, Si, Ti, V, Cr, Mn, Fe, Ni, Zn, Ga, Ge, Y, Zr, Mo, Ru, Pd, Ag, Ba, Pt, Au, and Ta can be used. As the metal oxide, for example, a metal oxide containing one or more of the above metals can be used. More specifically, for example, at least one of Al2O3, CuO, CoO, SiO2, Cr2O3, TiO2, Ta2O5, and ZrO2 can be used. The barrier layer 15 may also contain diamond-like carbon (DLC) or diamond.
[0196] The average thickness of the barrier layer 15 is preferably 20 nm or more and 1000 nm or less, more preferably 50 nm or more and 1000 nm or less. The average thickness of the barrier layer 15 is determined in the same manner as the average thickness of the magnetic layer 13. However, the magnification of the TEM image is appropriately adjusted according to the thickness of the barrier layer 15.
[0197] (Variation 6) In the above embodiment, a case has been described in which a large number of protrusions 14A provided on the surface 14S of the back layer 14 are transferred to the surface 13S of the magnetic layer 13 to form a large number of holes in the surface 13S of the magnetic layer 13, but the method of forming a large number of holes is not limited to this. For example, a large number of holes may be formed in the surface 13S of the magnetic layer 13 by adjusting the type of solvent contained in the paint for forming the magnetic layer and the drying conditions of the paint for forming the magnetic layer.
[0198] (Variation 7) The magnetic recording medium 10 according to the embodiment described above may be used in a library device. In this case, the library device may include a plurality of recording / reproducing devices 30 according to the embodiment described above.
[0199] (Variation 8) As described above, the magnetic recording medium of the present disclosure is housed in a state of being wound around a reel 32 in a magnetic recording medium cartridge 10A in a recording and reproducing device 30 shown in FIG. 7, for example. In this case, it is preferable that (servo track width on the inner side of the magnetic recording medium)-(servo track width on the outer side of the magnetic recording medium)>0 μm. In this modification, (servo track width on the inner side of the magnetic recording medium)-(servo track width on the outer side of the magnetic recording medium) is also referred to as "difference between servo track widths on the inner side and the outer side of the magnetic recording medium". The difference between the servo track widths on the inner side and the outer side of the magnetic recording medium is preferably 0.01 μm or more, more preferably 0.02 μm or more, and even more preferably 0.05 μm or more. The difference between the servo track widths on the inner side and the outer side of the magnetic recording medium may be, for example, 0.10 μm or more, 0.15 μm or more, or 0.20 μm or more. By having the difference between the servo track widths on the inside and outside of the winding within the above-mentioned numerical range, it is possible to prevent wrinkles from occurring in the magnetic recording medium wound on the reel in the cartridge (particularly in the portion of the magnetic recording medium closer to the reel). The wrinkles may cause, for example, winding misalignment or track misalignment during running, and the occurrence of these phenomena caused by the wrinkles can also be prevented by the present technology. The difference between the servo track widths on the inside and outside of the winding may be, for example, 2.5 μm or less, preferably 1.8 μm or less, more preferably 1.5 μm or less, 1.0 μm or less, 0.8 or less, or 0.5 μm or less. By having the difference between the servo track widths on the inside and outside of the winding be equal to or less than the above-mentioned upper limit value, it is easier to keep the width of the magnetic recording medium constant by adjusting the tension. A method for measuring the difference and a method for measuring the deviation amount of the servo track width used to calculate the difference will be described below.
[0200] ((servo track width on the inside of the reel) - (servo track width on the outside of the reel) The difference in servo track width between the inside and outside of the winding is more than 0 μm, preferably 0.0 m or more, more preferably 0.02 μm or more, and even more preferably 0.05 μm or more. The difference in servo track width between the inside and outside of the winding may be, for example, 0.10 μm or more, 0. μm or more, or 0.20 μm or more. This can prevent wrinkles from occurring in the magnetic recording medium wound on the reel in the cartridge. The difference in servo track width between the inside and outside of the winding may be, for example, 2.5 μm or less, preferably 1.8 μm or less, more preferably 1.5 μm or less, 1.0 μm or less, 0.8 or less, or 0.5 μm or less.
[0201] In order to obtain the difference between the servo track widths on the inside and outside of the reel, the deviation amount TinW of the servo track width on the inside of the reel and the deviation amount ToutW of the servo track width on the outside of the reel are measured. The measurement is performed in an environment with a temperature of 23±3° C. and a relative humidity of 50%±5%. Each of these deviation amounts indicates how large or small the servo track width is relative to the standard servo track width. The measurement method for these deviation amounts will be described separately below. In this specification, the inside of the reel refers to an area starting from a position 50 m from the end (hereinafter also referred to as the "inside end") attached to a reel (a reel on which the magnetic recording medium is wound) in a magnetic recording cartridge, and proceeding from this position to a position 10 m in the direction of the end opposite to the inside end (hereinafter also referred to as the "outside end"). In this specification, the outside of the reel refers to an area starting from a position 50 m from the outside end, and proceeding from this position to a position 10 m in the direction of the inside end.
[0202] The inside and outside of the winding will be described in more detail with reference to FIG. 15. FIG. 15 shows the state in which the inside end E1 of the magnetic recording medium 10 is attached to the reel 32 of the magnetic recording medium cartridge 10A mounted on the recording and reproducing device 30. The area between position A 50 m from the inside end E1 and position B 10 m from position A to the outside end E2 is the inside of the winding. The area between position C 50 m from the outside end E2 to the inside end E1 and position D 10 m from position C to the inside end E1 is the outside of the winding. The deviation amount TinW of the servo track width on the inside of the winding is measured while the magnetic recording medium 10 housed in the magnetic recording medium cartridge 10A is run so as to be wound into the recording and reproducing device 30 (running in the so-called forward direction). In this measurement, the tension applied to the magnetic recording medium 10 is 0.55 N, and the running speed is 3 to 6 m / s. The average value of the deviation of the servo track width measured over a 10 m region on the inside of the turn is used as the deviation inW of the servo track width on the inside of the turn for determining the difference. The average value is calculated by simple averaging.
[0203] The servo track width deviation ToutW on the outer side of the reel is measured while the reel is running in the forward direction, similar to the inner side of the reel. The average value of the servo track width deviations measured over a 10 m area on the outer side of the reel is used as the servo track width deviation ToutW on the outer side of the reel for determining the difference. This average value is also calculated by simple averaging.
[0204] By subtracting the deviation amount ToutW of the servo track width on the outside of the winding from the deviation amount TinW of the servo track width on the inside of the winding obtained as described above, the difference (TinW-ToutW) is obtained, and this difference is (servo track width on the inside of the winding)-(servo track width on the outside of the winding).
[0205] (Servo track width deviation) A method for measuring the deviation of the servo track width will be described with reference to FIG. 16. FIG. 16(a) is a schematic diagram of a data band and a servo band formed on a magnetic layer of a magnetic recording medium. As shown in FIG. 16(a), the magnetic layer has four data bands d0 to d3. The magnetic layer has a total of five servo bands S0 to S4, with each data band sandwiched between two servo bands. As shown in FIG. 16(b), each servo band has a repeating frame unit consisting of five servo signals S5a inclined at a predetermined angle θ1, five servo signals S5b inclined at the same angle in the opposite direction to the signals, four servo signals S4a inclined at the predetermined angle θ1, and four servo signals S4b inclined at the same angle in the opposite direction to the signals. The angle θ1 can be, for example, 5° to 25°, and particularly 11° to 20°.
[0206] The deviation of the servo track width measured by the above measurement method is the deviation of the servo track width between the two servo tracks S1 and S2 sandwiching the second data band d1 from the top in FIG. 16(a) from the standard servo track width. When the two servo tracks S1 and S2 sandwiching the data band d1 are reproduced during drive running, a waveform as shown in FIG. 16(c) is obtained for each servo track by a digital oscilloscope (Lecroy WAVEPRO 960). The time between the timing signals is obtained from the waveform obtained by reproducing the servo track S1, and the distance between the leading magnetic stripe of the A burst and the leading magnetic stripe of the B burst in the servo track S1 is calculated from the time and the tape running speed. For example, as shown in FIG. 16(b), the distance L1 between the leading magnetic stripe of the A burst S5a-1 (the leftmost magnetic stripe of the five magnetic stripes) and the leading magnetic stripe of the B burst S5b-1 (the leftmost magnetic stripe of the five magnetic stripes) is calculated. Similarly, the time between timing signals is obtained from the waveform obtained by reproducing the servo track S2, and the distance between the leading magnetic stripe of the A burst and the leading magnetic stripe of the B burst in the servo track S2 is calculated from the time and the tape running speed. For example, as shown in FIG. 16(b), the distance L2 between the leading magnetic stripe of the A burst S5a-2 and the leading magnetic stripe of the B burst S5b-2 is calculated. For example, when the magnetic recording tape expands in the width direction, the time between the timing signals obtained by reproducing the servo track S1 becomes longer, and as a result, the calculated distance L1 may also become larger. When the magnetic recording tape shrinks in the width direction, the calculated distance L1 may become smaller. Therefore, the deviation amount of the servo track width can be obtained by using the distance L1, the distance L2, and the azimuth angle. The deviation amount of the servo track width can be obtained from the following formula. (Servo track width deviation)={(L1-L2) / 2}×tan(90°-θ1) In this formula, L1 and L2 are the distances L1 and L2 described above, and θ1 is the inclination angle θ1 described above, also called the azimuth angle. θ1 is determined by developing the magnetic recording medium removed from the cartridge with a ferricolloid developer, and using a universal tool microscope (TOPCON TUM-220ES) and a data processing device (TOPCON CA-1B). The deviation of the servo track width is the amount of change from the standard servo track width. The standard servo track width may be the same as the servo read head width of the magnetic recording and reproducing device, and may be determined according to the type of the magnetic recording medium 10, such as the standard to which the magnetic recording medium 10 complies.
[0207] The servo track width can be adjusted, for example, as follows. In order to alleviate distortion caused in the magnetic recording medium 10, the winding tension may be lowered in the drying process and / or calendaring process (heating area) of the magnetic recording medium 10. Also, in order to alleviate distortion in the pancake state and / or cartridge state after cutting, the magnetic recording medium 10 may be stored for a long period of time at a temperature of 55° C. or higher. By alleviating distortion in this manner, the servo track width can be adjusted.
[0208] As in this modified example, by satisfying (servo track width on the inner side of the magnetic recording medium)-(servo track width on the outer side of the magnetic recording medium)>0, it is possible to suppress the occurrence of wrinkles on the inner side of the roll inside the cartridge. EXAMPLES
[0209] The present disclosure will be specifically described below using examples, but the present disclosure is not limited to these examples.
[0210] In the following examples and comparative examples, the average aspect ratio of the magnetic powder in the vertical direction, the average particle size of the magnetic powder, the average particle volume of the magnetic powder, the average thickness of the underlayer, the overall average thickness of the magnetic recording medium (average tape thickness), the average thickness of the magnetic layer, the coercive force Hc1, the coercive force Hc2, the ratio Hc2 / Hc1, the arithmetic mean roughness of the surface of the magnetic layer (magnetic layer Ra), the magnetic layer PSD (≦0.5 μm), and the half-width PW50 of the isolated waveform are values obtained by the measurement method described in the above-mentioned embodiment.
[0211] [Example 1] The magnetic recording medium of Example 1 was obtained as follows.
[0212] <Preparation process of paint for forming magnetic layer> The magnetic layer-forming paint was prepared as follows. First, the first composition having the following composition was mixed with an extruder. Next, the mixed first composition and the second composition having the following composition were added to a stirring tank equipped with a disperser and premixed. Then, further mixing was performed with a sand mill and filtering was performed to prepare the magnetic layer-forming paint.
[0213] (First composition) The components and their weights in the first composition are as follows: Barium ferrite (BaFe 12 O 19 ) particle powder (hexagonal plate shape, average aspect ratio 2.8, average particle size 20.3 nm, average particle volume 1950 nm 3 ):100 parts by mass Vinyl chloride resin (cyclohexanone solution 30% by weight): 40 parts by weight (including cyclohexanone solution) (Degree of polymerization: 300, Mn=10,000, contains polar groups OSO3K=0.07mmol / g and secondary OH=0.3mmol / g.) ·Aluminum oxide powder (α-Al2O3, average particle size 0.2μm): 5 parts by mass Carbon black (manufactured by Tokai Carbon Co., Ltd., product name: Seast TA): 2 parts by weight
[0214] (Second composition) The components and their weights in the second composition are as follows: Vinyl chloride resin: 20 parts by weight (including cyclohexanone solution) (Resin solution: resin 30% by mass, cyclohexanone 70% by mass) n-Butyl stearate as fatty acid ester: 2 parts by weight Methyl ethyl ketone: 121.3 parts by weight Toluene: 121.3 parts by weight Cyclohexanone: 60.7 parts by weight
[0215] To the magnetic layer-forming coating material prepared as described above, 4 parts by mass of polyisocyanate (product name: Coronate L, manufactured by Nippon Polyurethane Co., Ltd.) as a curing agent and 2 parts by mass of stearic acid as a fatty acid were added.
[0216] <Preparation process of paint for forming base layer> The paint for forming the undercoat layer was prepared as follows. First, the third composition having the following composition was mixed with an extruder. Next, the mixed third composition and the fourth composition having the following composition were added to a stirring tank equipped with a disperser and premixed. Then, further mixing was performed with a sand mill and filtering was performed to prepare the paint for forming the undercoat layer.
[0217] (Third composition) The components and their weights in the third composition are as follows: ·Acicular iron oxide powder (α-Fe2O3, average major axis length 0.15μm): 100 parts by mass Vinyl chloride resin (resin solution: resin content 30% by mass, cyclohexanone 70% by mass): 55.6 parts by mass Carbon black (average particle size 20 nm): 10 parts by weight
[0218] (4th composition) The components and their weights in the fourth composition are as follows. Polyurethane resin UR8200 (manufactured by Toyobo): 18.5 parts by weight n-Butyl stearate as fatty acid ester: 2 parts by weight Methyl ethyl ketone: 108.2 parts by weight Toluene: 108.2 parts by mass Cyclohexanone: 18.5 parts by weight
[0219] To the coating material for forming an undercoat layer prepared as described above, 4 parts by mass of polyisocyanate (product name: Coronate L, manufactured by Nippon Polyurethane Co., Ltd.) as a curing agent and 2 parts by mass of stearic acid as a fatty acid were added.
[0220] <Preparation process of paint for forming back layer> The paint for forming the back layer was prepared as follows: The following raw materials were mixed in a stirring tank equipped with a disperser, and the mixture was filtered to prepare the paint for forming the back layer. Small particle size carbon black powder (average particle size (D50) 20 nm): 90 parts by weight Large particle size carbon black powder (average particle size (D50) 270 nm): 10 parts by weight Polyester polyurethane (Nippon Polyurethane Co., Ltd., product name: N-2304): 100 parts by weight Methyl ethyl ketone: 500 parts by weight Toluene: 400 parts by weight Cyclohexanone: 100 parts by weight
[0221] <Coating process> Using the magnetic layer forming paint and the undercoat layer forming paint prepared as described above, an undercoat layer with an average thickness of 1.1 μm and a magnetic layer with an average thickness of 80 nm were formed on one main surface of a long polyester film with an average thickness of 4.0 μm, which is a non-magnetic support, as follows. First, the undercoat layer forming paint was applied to one main surface of the polyester film and dried to form an undercoat layer. Next, the magnetic layer was formed by applying the magnetic layer forming paint on the undercoat layer and drying it. During drying of the magnetic layer forming paint, the magnetic powder was magnetically oriented in the thickness direction of the film by a solenoid coil. In addition, the drying conditions (drying temperature and drying time) of the magnetic layer forming paint were adjusted to set the coercive force Hc1 in the thickness direction (perpendicular direction) of the magnetic recording medium and the coercive force Hc2 in the longitudinal direction to the values shown in Table 1 below. Next, the back layer forming paint was applied to the other main surface of the polyester film and dried to form a back layer with an average thickness of 0.3 μm.
[0222] <Calendar process and transfer process> Then, a calendaring process was performed to smooth the surface of the magnetic layer. Next, the magnetic recording medium with the smoothed surface of the magnetic layer was wound into a roll, and then the magnetic recording medium was heat-treated at 60°C for 10 hours in this state. Then, the magnetic recording medium was rewound into a roll so that the end located on the inner circumference side was reversely positioned on the outer circumference side, and then the magnetic recording medium was heat-treated again at 60°C for 10 hours in this state. As a result, many protrusions on the surface of the back layer were transferred to the surface of the magnetic layer, and many holes were formed on the surface of the magnetic layer.
[0223] <Cutting process> The magnetic recording medium obtained as described above was cut into a width of 1 / 2 inch (12.65 mm). As a result, the desired long magnetic recording medium (average thickness 5.6 μm) was obtained. This magnetic recording medium has a four-layer structure as shown in Table 2 below, with an overall average thickness (average tape thickness) of 5.6 μm, five servo tracks, and an average thickness of the substrate (base film) of 4.0 μm. W is 2.9 μm and L is 0.052 μm. The above configuration is referred to as media configuration 1. W represents the recording track width, and L represents the distance between magnetization reversals (bit length) in the part recorded with the shortest wavelength. The magnetic layer Ra of the obtained magnetic recording medium was 1.9 nm, the magnetic layer PSD was 2.1 μm, and the half-value width PW50 of the isolated waveform in the reproduced waveform was 175 nm.
[0224] [Example 2] In the preparation process of the coating material for forming the magnetic layer, the barium ferrite (BaFe 12 O 19 ) particles, the powder average aspect ratio is 2.6, the average particle size is 18.6 nm, and the average particle volume is 1600 nm 3 In the coating process, the average thickness of the magnetic layer was 60 nm, the coercive force Hc1 was 2920 Oe, and the coercive force Hc2 was 1920 Oe. Except for the above points, a magnetic recording medium was obtained as Example 2 in the same manner as in Example 1. The magnetic layer Ra of the obtained magnetic recording medium was 1.85 nm, the magnetic layer PSD was 2.0 μm, and the half-width PW50 of the isolated waveform in the reproduced waveform was 170 nm.
[0225] [Example 3] In the preparation process of the coating material for forming the magnetic layer, the barium ferrite (BaFe 12 O 19 ) particles, the powder average aspect ratio is 3.0, the average particle size is 21.3 nm, and the average particle volume is 2100 nm 3Except for the above points, a magnetic recording medium was obtained as Example 3 in the same manner as in Example 1. The magnetic layer Ra of the obtained magnetic recording medium was 1.9 nm, the magnetic layer PSD was 2.1 μm, and the half-value width PW50 of the isolated waveform in the reproduced waveform was 177 nm.
[0226] [Example 4] Except for the fact that the average thickness of the magnetic layer was set to 90 nm in the coating process, a magnetic recording medium was obtained as Example 4 in the same manner as in Example 1. The magnetic layer Ra of the obtained magnetic recording medium was 1.9 nm, the magnetic layer PSD was 2.1 μm, and the half-value width PW50 of the isolated waveform in the reproduced waveform was 175 nm.
[0227] [Example 5] In the preparation process of the coating material for forming the magnetic layer, the barium ferrite (BaFe 12 O 19 ) particles, the powder average aspect ratio is 2.9, the average particle size is 20.9 nm, and the average particle volume is 2050 nm 3 In the coating process, the coercive force Hc1 was set to 2980 Oe. Except for the above points, a magnetic recording medium was obtained as Example 5 in the same manner as in Example 1. The magnetic layer Ra of the obtained magnetic recording medium was 1.9 nm, the magnetic layer PSD was 2.1 μm, and the half-value width PW50 of the isolated waveform in the reproduced waveform was 177 nm.
[0228] [Example 6] In the preparation process of the paint for forming the magnetic layer, a powder of ε iron oxide particles (spherical, average aspect ratio 1.3, average particle size 15.7 nm, particle volume 2050 nm) was used as the magnetic powder. 3 ) was used. In the coating process, the coercive force Hc1 was set to 2850 Oe, and the coercive force Hc2 was set to 2020 Oe. Except for the above points, a magnetic recording medium was obtained as Example 6 in the same manner as in Example 1. The magnetic layer Ra of the obtained magnetic recording medium was 2 nm, the magnetic layer PSD was 2.1 μm, and the half-width PW50 of the isolated waveform in the reproduced waveform was 177 nm.
[0229] [Example 7] In the preparation process of the paint for forming the magnetic layer, cobalt ferrite powder (cubic, average aspect ratio 1.1, average particle size 12.6 nm, particle volume 2030 nm) was used as the magnetic powder. 3 ) was used. In the coating process, the coercive force Hc1 was set to 2800 Oe, and the coercive force Hc2 was set to 2020 Oe. Except for the above points, a magnetic recording medium was obtained as Example 7 in the same manner as in Example 1. The magnetic layer Ra of the obtained magnetic recording medium was 2 nm, the magnetic layer PSD was 2.1 μm, and the half-value width PW50 of the isolated waveform in the reproduced waveform was 177 nm.
[0230] [Example 8] In the preparation process of the coating material for forming the magnetic layer, the barium ferrite (BaFe 12 O 19 ) particles, the powder average aspect ratio is 2.3, the average particle size is 17 nm, and the average particle volume is 1400 nm 3 In the coating process, the average thickness of the magnetic layer was 60 nm, the coercive force Hc1 was 2550 Oe, and the coercive force Hc2 was 1820 Oe. Except for the above points, a magnetic recording medium was obtained as Example 8 in the same manner as in Example 1. The magnetic layer Ra of the obtained magnetic recording medium was 1.8 nm, the magnetic layer PSD was 1.9 μm, and the half-width PW50 of the isolated waveform in the reproduced waveform was 170 nm.
[0231] [Example 9] In the preparation process of the coating material for forming the magnetic layer, the barium ferrite (BaFe 12 O 19 ) particles, the powder average aspect ratio is 2.0, the average particle size is 15 nm, and the average particle volume is 1100 nm 3 In the coating process, the average thickness of the magnetic layer was 60 nm, the coercive force Hc1 was 2500 Oe, and the coercive force Hc2 was 1840 Oe. Except for the above points, a magnetic recording medium was obtained as Example 9 in the same manner as in Example 1. The magnetic layer Ra of the obtained magnetic recording medium was 1.75 nm, the magnetic layer PSD was 1.8 μm, and the half-width PW50 of the isolated waveform in the reproduced waveform was 160 nm.
[0232] [Example 10] Except for the media configuration being 2 (Table 2), a magnetic recording medium was obtained as Example 10 in the same manner as in Example 1. The magnetic layer Ra of the obtained magnetic recording medium was 1.9 nm, the magnetic layer PSD was 2.1 μm, and the half-value width PW50 of the isolated waveform in the reproduced waveform was 175 nm.
[0233] [Example 11] The media composition was set to 3 (Table 2). In the process of preparing the coating material for forming the magnetic layer, the barium ferrite (BaFe 12 O 19 ) particles, the powder average aspect ratio is 2.6, the average particle size is 18.6 nm, and the average particle volume is 1600 nm 3 In the coating process, the average thickness of the magnetic layer was 60 nm, the coercive force Hc1 was 2920 Oe, and the coercive force Hc2 was 1920 Oe. Furthermore, the average tape thickness was 5.2 μm. Except for the above points, the magnetic recording medium was obtained as Example 11 in the same manner as in Example 1. The magnetic layer Ra of the obtained magnetic recording medium was 1.85 nm, the magnetic layer PSD was 2.0 μm, and the half-width PW50 of the isolated waveform in the reproduced waveform was 168 nm.
[0234] [Example 12] The media composition was set to 4 (Table 2). In the preparation process of the coating material for forming the magnetic layer, the barium ferrite (BaFe 12 O 19 ) particles, the powder average aspect ratio is 2.3, the average particle size is 17 nm, and the average particle volume is 1400 nm 3 In the coating process, the average thickness of the magnetic layer was 60 nm, the coercive force Hc1 was 2550 Oe, and the coercive force Hc2 was 1820 Oe. Furthermore, the average tape thickness was 5.2 μm. Except for the above points, a magnetic recording medium was obtained as Example 12 in the same manner as in Example 1. The magnetic layer Ra of the obtained magnetic recording medium was 1.8 nm, the magnetic layer PSD was 1.9 μm, and the half-width PW50 of the isolated waveform in the reproduced waveform was 166 nm.
[0235] [Example 13] The media composition was set to 5 (Table 2). In the preparation process of the coating material for forming the magnetic layer, the barium ferrite (BaFe 12 O 19 ) particles, the powder average aspect ratio is 2.3, the average particle size is 17 nm, and the average particle volume is 1400 nm 3 In the coating process, the average thickness of the magnetic layer was 60 nm, the coercive force Hc1 was 2550 Oe, and the coercive force Hc2 was 1820 Oe. Furthermore, the average tape thickness was 4.5 μm. Except for the above points, the magnetic recording medium was obtained as Example 13 in the same manner as in Example 1. The magnetic layer Ra of the obtained magnetic recording medium was 1.8 nm, the magnetic layer PSD was 1.9 μm, and the half-width PW50 of the isolated waveform in the reproduced waveform was 166 nm.
[0236] [Example 14] The media composition was set to 6 (Table 2). In the preparation process of the coating material for forming the magnetic layer, the barium ferrite (BaFe 12 O 19 ) particles, the powder average aspect ratio is 2.0, the average particle size is 15 nm, and the average particle volume is 1100 nm 3 In the coating process, the average thickness of the magnetic layer was 60 nm, the coercive force Hc1 was 2500 Oe, and the coercive force Hc2 was 1840 Oe. Furthermore, the average tape thickness was 4.5 μm. Except for the above points, the magnetic recording medium was obtained as Example 14 in the same manner as in Example 1. The magnetic layer Ra of the obtained magnetic recording medium was 1.75 nm, the magnetic layer PSD was 1.8 μm, and the half-width PW50 of the isolated waveform in the reproduced waveform was 155 nm.
[0237] [Example 15] In the coating process, the average thickness of the magnetic layer was 90 nm, the coercive force Hc1 was 2990 Oe, and the coercive force Hc2 was 1500 Oe. Except for the above points, a magnetic recording medium was obtained as Example 15 in the same manner as in Example 1. The magnetic layer Ra of the obtained magnetic recording medium was 1.85 nm, the magnetic layer PSD was 2.0 μm, and the half-width PW50 of the isolated waveform in the reproduced waveform was 175 nm.
[0238] [Example 16] In the coating process, the coercive force Hc1 was set to 2690 Oe, and the coercive force Hc2 was set to 2150 Oe. Except for the above points, the magnetic recording medium was obtained as Example 16 in the same manner as in Example 1. The magnetic layer Ra of the obtained magnetic recording medium was 1.85 nm, the magnetic layer PSD was 2.0 μm, and the half-width PW50 of the isolated waveform in the reproduced waveform was 180 nm.
[0239] [Example 17] In the preparation process of the paint for forming the magnetic layer, a powder of ε iron oxide particles (spherical, average aspect ratio 1.3, average particle size 15.7 nm, particle volume 2050 nm) was used as the magnetic powder. 3 ) was used. In the coating process, the average thickness of the magnetic layer was 90 nm, the coercive force Hc1 was 2900 Oe, and the coercive force Hc2 was 1950 Oe. Except for the above points, a magnetic recording medium was obtained as Example 17 in the same manner as in Example 1. The magnetic layer Ra of the obtained magnetic recording medium was 2 nm, the magnetic layer PSD was 2.1 μm, and the half-width PW50 of the isolated waveform in the reproduced waveform was 175 nm.
[0240] [Example 18] By changing the conditions of the calendaring, the magnetic layer of the obtained magnetic recording medium had a Ra of 1.6 nm and a PSD of 1.7 μm.The half-width PW50 of the isolated waveform in the reproduced waveform was 175 nm.
[0241] [Example 19] By changing the conditions of the calendaring process, the magnetic layer of the obtained magnetic recording medium had a Ra of 2.4 nm and a PSD of 2.5 μm.The half-width PW50 of the isolated waveform in the reproduced waveform was 175 nm.
[0242] [Comparative Example 1] In the preparation process of the coating material for forming the magnetic layer, the barium ferrite (BaFe 12 O 19) particles, the powder average aspect ratio is 3.5, the average particle size is 23.6 nm, and the average particle volume is 2450 nm 3 In the coating process, the average thickness of the magnetic layer was 85 nm, and the coercive force Hc1 was 2820 Oe. Except for the above points, a magnetic recording medium was obtained as Comparative Example 1 in the same manner as in Example 1. The magnetic layer Ra of the obtained magnetic recording medium was 1.9 nm, the magnetic layer PSD was 2.1 μm, and the half-width PW50 of the isolated waveform in the reproduced waveform was 205 nm.
[0243] [Comparative Example 2] In the coating process, the average thickness of the magnetic layer was 100 nm. Except for the above points, a magnetic recording medium was obtained as Comparative Example 2 in the same manner as in Example 1. The magnetic layer Ra of the obtained magnetic recording medium was 1.9 nm, the magnetic layer PSD was 2.1 μm, and the half-value width PW50 of the isolated waveform in the reproduced waveform was 202 nm.
[0244] [Comparative Example 3] In the coating process, the average thickness of the magnetic layer was 85 nm, the coercive force Hc1 was 2500 Oe, and the coercive force Hc2 was 2100 Oe. Except for the above points, a magnetic recording medium was obtained as Comparative Example 3 in the same manner as in Example 1. The magnetic layer Ra of the obtained magnetic recording medium was 1.9 nm, the magnetic layer PSD was 2.1 μm, and the half-width PW50 of the isolated waveform in the reproduced waveform was 180 nm.
[0245] [Comparative Example 4] In the preparation process of the coating material for forming the magnetic layer, the barium ferrite (BaFe 12 O 19 ) particles, the powder average aspect ratio is 3.0, the average particle size is 21.3 nm, and the average particle volume is 2090 nm 3 In the coating process, the coercive force Hc1 was set to 3100 Oe. Except for the above points, a magnetic recording medium was obtained as Comparative Example 4 in the same manner as in Example 1. The magnetic layer Ra of the obtained magnetic recording medium was 1.9 nm, the magnetic layer PSD was 2.1 μm, and the half-width PW50 of the isolated waveform in the reproduced waveform was 190 nm.
[0246] [Comparative Example 5] In the preparation process of the paint for forming the magnetic layer, a powder of ε iron oxide particles (spherical, average aspect ratio 1.3, average particle size 15.7 nm, particle volume 2050 nm) was used as the magnetic powder. 3 ) was used. In the coating process, the coercive force Hc1 was set to 2550 Oe, and the coercive force Hc2 was set to 2080 Oe. Except for the above points, a magnetic recording medium was obtained as Comparative Example 5 in the same manner as in Example 1. The magnetic layer Ra of the obtained magnetic recording medium was 1.9 nm, the magnetic layer PSD was 2.1 μm, and the half-width PW50 of the isolated waveform in the reproduced waveform was 180 nm.
[0247] [Comparative Example 6] In the preparation process of the paint for forming the magnetic layer, cobalt ferrite powder (cubic, average aspect ratio 1.1, average particle size 12.6 nm, particle volume 2030 nm) was used as the magnetic powder. 3 ) was used. In the coating process, the coercive force Hc1 was set to 2450 Oe, and the coercive force Hc2 was set to 2080 Oe. Except for the above points, a magnetic recording medium was obtained as Comparative Example 6 in the same manner as in Example 1. The magnetic layer Ra of the obtained magnetic recording medium was 1.9 nm, the magnetic layer PSD was 2.1 μm, and the half-value width PW50 of the isolated waveform in the reproduced waveform was 179 nm.
[0248] [Comparative Example 7] By adjusting the additives in the magnetic layer, the magnetic layer Ra of the obtained magnetic recording medium was set to 2.55 nm and the magnetic layer PSD was set to 3.2 μm. The half-width PW50 of the isolated waveform in the reproduced waveform was 205 nm.
[0249] [Comparative Example 8] By adjusting the additives in the magnetic layer, the magnetic layer Ra of the obtained magnetic recording medium was set to 1.66 nm, and the magnetic layer PSD was set to 1.7 μm. The half-width PW50 of the isolated waveform in the reproduced waveform was 173 nm.
[0250] [evaluation] The magnetic recording media of Examples 1 to 19 and Comparative Examples 1 to 8 obtained as described above were evaluated as follows.
[0251] (C / N) First, a loop tester (manufactured by Microphysics) was used to obtain a reproduction signal from the magnetic recording medium. The conditions for obtaining the reproduction signal are as follows: Head: GMR head Speed: 2m / s Reproduction signal: Single recording frequency (10MHz) Recording current: Optimum recording current
[0252] Next, the playback signal was captured by a spectrum analyzer, and the playback output value of 10 MHz and the average noise value of 10 MHz ± 1 MHz were measured, and the difference between them was taken as the C / N. The results are shown in Table 1 as relative values with the C / N of Comparative Example 1 taken as 0 dB. Note that if the C / N is 1.5 dB or higher, it is possible to realize a media that can withstand short wavelengths and narrow track densities.
[0253] [Table 1]
[0254] Table 1 shows the magnetic characteristics and evaluation results of each of the magnetic recording media in Examples 1-19 and Comparative Examples 1-8.
[0255] [Table 2]
[0256] Table 2 shows the media configurations employed in the magnetic recording media of Examples 1-19 and Comparative Examples 1-8.
[0257] As shown in Tables 1 and 2, in Examples 1 to 19, the arithmetic mean roughness Ra of the surface of the magnetic layer is 2.5 nm or less, the PSD up to a spatial wavelength of 5 μm is 2.5 μm or less, the average thickness of the magnetic layer is 90 nm or less, the average aspect ratio of the magnetic powder is 1.0 to 3.0, the coercive force Hc1 in the perpendicular direction is 3000 Oe or less, Hc2 / Hc1 is 0.8 or less, and the half-width PW50 of the isolated waveform in the reproduced waveform of the data signal is 200 nm or less. Therefore, it is possible to ensure good electromagnetic conversion characteristics (C / N) while making the magnetization transition width steep. Therefore, it is possible to realize a configuration that is advantageous for high-density recording.
[0258] In addition, in Examples 1, 2, 4, 8-15, and 17-19, the half-value width PW50 was 175 nm or less, and therefore excellent electromagnetic conversion characteristics (C / N) were obtained.
[0259] In particular, in Examples 2, 8, 9, and 11-14, the half-value width PW50 was 170 nm or less, and therefore more excellent electromagnetic conversion characteristics (C / N) were obtained.
[0260] In Comparative Example 1, since the average aspect ratio of the magnetic powder exceeded 3.0, stacking of the magnetic tape occurred and the electromagnetic conversion characteristics deteriorated.
[0261] In Comparative Example 2, the average thickness of the magnetic layer was large, and the electromagnetic conversion characteristics at short wavelengths were deteriorated.
[0262] In Comparative Example 3, the degree of vertical orientation was low, and the electromagnetic conversion characteristics were deteriorated.
[0263] In Comparative Example 4, the coercive force Hc1 in the perpendicular direction was too large, so that an unsaturated region occurred and the electromagnetic conversion characteristics were deteriorated.
[0264] In Comparative Examples 5 and 6, the degree of vertical orientation was low, and the electromagnetic conversion characteristics were deteriorated.
[0265] In Comparative Example 7, the surface roughness Ra of the magnetic layer was too large, deteriorating the electromagnetic conversion characteristics. Furthermore, the deterioration of the surface properties caused a gap between the magnetic layer surface and the magnetic head, and the half-value width PW50 also deteriorated.
[0266] In Comparative Example 8, the electromagnetic conversion characteristics were improved, but the frictional force on the surface of the magnetic layer increased, making it impossible for the magnetic recording medium to run.
[0267] While the present disclosure has been specifically described above by giving embodiments and modifications thereof, the present disclosure is not limited to the above-described embodiments, and various modifications are possible.
[0268] For example, the configurations, methods, steps, shapes, materials, and values given in the above-mentioned embodiments and their modified examples are merely examples, and different configurations, methods, steps, shapes, materials, and values may be used as necessary. Specifically, the magnetic recording medium of the present disclosure may include components other than the substrate, underlayer, magnetic layer, back layer, and barrier layer. In addition, the chemical formulas of compounds, etc. are representative, and are not limited to the valences, etc. given as long as they are general names of the same compounds.
[0269] Furthermore, the configurations, methods, steps, shapes, materials, numerical values, and the like of the above-described embodiments and their modified examples can be combined with each other without departing from the spirit of this disclosure.
[0270] In addition, in the numerical ranges described in stages in this specification, the upper limit or lower limit of a certain numerical range may be replaced with the upper limit or lower limit of another numerical range. Unless otherwise specified, the materials exemplified in this specification may be used alone or in combination of two or more.
[0271] As described above, according to the magnetic recording medium according to an embodiment of the present disclosure, even higher density recording can be achieved. Note that the effects of the present disclosure are not limited to the above, and may be any of the effects described in this specification. In addition, the present technology may have the following configurations. (1) A tape-shaped magnetic recording medium, A substrate containing polyester as a main component; a magnetic layer provided on the substrate, the magnetic layer including a plurality of magnetic particles and capable of recording a data signal; having The arithmetic mean roughness Ra of the surface of the magnetic layer is 2.5 nm or less; The PSD (Power Spectrum Density) up to a spatial wavelength of 5 μm is 2.5 μm or less. The average thickness of the magnetic layer is 90 nm or less, The average aspect ratio of the magnetic powder is 1.0 or more and 3.0 or less, The coercivity in the perpendicular direction is 3000 oersted or less. The ratio of the coercive force in the longitudinal direction to the coercive force in the perpendicular direction is 0.8 or less; The half-width of an isolated waveform in the reproduced waveform of the data signal is 200 nm or less. Magnetic recording media. (2) The half-width of an isolated waveform in the reproduced waveform of the data signal is 175 nm or less. The magnetic recording medium according to (1) above. (3) The half-width of an isolated waveform in the reproduced waveform of the data signal is 170 nm or less. The magnetic recording medium according to (1) above. (4) The half-width of an isolated waveform in the reproduced waveform of the data signal is 165 nm or less. The magnetic recording medium according to (1) above. (5) The average particle size of the magnetic powder is 8 nm or more and 22 nm or less. The magnetic recording medium according to any one of (1) to (4) above. (6) The average particle volume of the magnetic powder is 2300 nm 3 is less than or equal to The magnetic recording medium according to any one of (1) to (5) above. (7) the magnetic layer has a plurality of servo bands capable of recording a plurality of servo signals, The ratio of the total area of the plurality of servo bands to the surface area of the magnetic layer is 4.0% or less. The magnetic recording medium according to any one of (1) to (6) above. (8) The number of the plurality of servo bands is 5 or more. The magnetic recording medium according to any one of (1) to (7) above. (9) The width of the servo band is 95 nm or less. The magnetic recording medium according to any one of (1) to (8) above. (10) the magnetic layer is capable of forming a plurality of recording tracks; The width of the recording track is 3.0 μm or less. The magnetic recording medium according to any one of (1) to (9) above. (11) The magnetic layer is configured to be capable of recording data such that the minimum distance between magnetization reversals is 48 nm or less. The magnetic recording medium according to any one of (1) to (10) above. (12) The coercive force in the longitudinal direction is 2000 Oe or less. The magnetic recording medium according to any one of (1) to (11) above. (13) Average thickness of 5.6μm or less The magnetic recording medium according to any one of (1) to (12) above. (14) The substrate has an average thickness of 4.2 μm or less. The magnetic recording medium according to any one of (1) to (13) above. (15) The magnetic powder contains hexagonal ferrite containing at least one of Ba (barium) and Sr (strontium), ε iron oxide containing at least one of Al (aluminum) and Ga (gallium), or Co (cobalt)-containing spinel ferrite. The magnetic recording medium according to any one of (1) to (14) above. (16) The average thickness of the magnetic layer is 80 nm or less. The magnetic recording medium according to any one of (1) to (15) above. (17) The average thickness of the magnetic layer is 70 nm or less. The magnetic recording medium according to any one of (1) to (16) above. (18) When the coercive force in the perpendicular direction is Hc1 and the coercive force in the longitudinal direction is Hc2, the following conditional expression is satisfied: <1> Fulfill Hc2 / Hc1≦0.7…… <1> The magnetic recording medium according to any one of (1) to (17) above. (19) The coercive force in the perpendicular direction is 2900 Oe or more. The magnetic recording medium according to any one of (1) to (18) above. (20) a feeding section capable of sequentially feeding out tape-shaped magnetic recording media; a winding section capable of winding up the magnetic recording medium fed from the feeding section; a magnetic head capable of writing information to the magnetic recording medium and reading information from the magnetic recording medium while contacting the magnetic recording medium traveling from the delivery section to the take-up section; Equipped with The magnetic recording medium is A substrate containing polyester as a main component; a magnetic layer provided on the substrate, the magnetic layer including a plurality of magnetic particles and capable of recording a data signal; having The arithmetic mean roughness Ra of the surface of the magnetic layer is 2.5 nm or less; The PSD (Power Spectrum Density) up to a spatial wavelength of 5 μm is 2.5 μm or less. The average thickness of the magnetic layer is 90 nm or less, The average aspect ratio of the magnetic powder is 1.0 or more and 3.0 or less, The coercivity in the perpendicular direction is 3000 oersted or less. The ratio of the coercive force in the longitudinal direction to the coercive force in the perpendicular direction is 0.8 or less; The half-width of an isolated waveform in the reproduced waveform of the data signal is 200 nm or less. Magnetic recording and playback device. (twenty one) A tape-shaped magnetic recording medium; a housing for accommodating the magnetic recording medium; Equipped with The magnetic recording medium is A substrate containing polyester as a main component; a magnetic layer provided on the substrate, the magnetic layer including a plurality of magnetic particles and capable of recording a data signal; having The arithmetic mean roughness Ra of the surface of the magnetic layer is 2.5 nm or less; The PSD (Power Spectrum Density) up to a spatial wavelength of 5 μm is 2.5 μm or less. The average thickness of the magnetic layer is 90 nm or less, The average aspect ratio of the magnetic powder is 1.0 or more and 3.0 or less, The coercivity in the perpendicular direction is 3000 oersted or less. The ratio of the coercive force in the longitudinal direction to the coercive force in the perpendicular direction is 0.8 or less; The half-width of an isolated waveform in the reproduced waveform of the data signal is 200 nm or less. Magnetic recording medium cartridge. [Explanation of symbols]
[0272] 5...recording track, 6...servo signal recording pattern, 7...stripe, 8...first stripe group, 9...second stripe group, 10...magnetic recording medium, 11...substrate, 11A, 11B...main surface, 12...underlayer, 13...magnetic layer, 14...back layer, 20, 20A...ε iron oxide particles, 21...core portion, 22...shell portion, 22a...first shell portion, 22b...second shell portion, 30...recording and reproducing device, 31...spindle, 32...reel, 33, 34...driving device, 35...guide roller, 36...head unit, 37...communication interface, 38...control device, 41...server, 42...personal computer, 43...network, 51...feed roller, 52...preprocessing portion, 53...servo signal recording head, 54...servo signal reproducing head, 55...take-up roller, 100...servo signal recording device.
Claims
1. A tape-shaped magnetic recording medium, A substrate containing polyester as a main component; a base layer including a binder provided on one main surface of the substrate; a magnetic layer provided on the underlayer; having the magnetic layer includes a plurality of magnetic powders and the binder, and is capable of recording a data signal having a half-width of an isolated waveform in a reproduced waveform of the data signal of 180 nm or less; The arithmetic mean roughness Ra of the surface of the magnetic layer is 2.4 nm or less; The average thickness of the magnetic layer is 90 nm or less, The average aspect ratio of the magnetic powder is 1.0 or more and 3.0 or less, The magnetic recording medium has a coercive force in a perpendicular direction of 3000 Oersted or less, a ratio of the coercive force in the longitudinal direction to the coercive force in the perpendicular direction of the magnetic recording medium is 0.75 or less; The average thickness of the magnetic recording medium is 5.6 μm or less, The magnetic powder includes hexagonal ferrite containing at least one of Ba (barium) and Sr (strontium), ε iron oxide containing at least one of Al (aluminum) and Ga (gallium), or spinel ferrite containing Co (cobalt). Magnetic recording media.
2. The average thickness of the magnetic recording medium is 5.2 μm or less.
2. The magnetic recording medium according to claim 1.
3. The average thickness of the magnetic recording medium is 5.0 μm or less.
2. The magnetic recording medium according to claim 1.
4. The half-width of an isolated waveform in the reproduced waveform of the data signal is 175 nm or less. The magnetic recording medium according to any one of claims 1 to 3.
5. The half-width of an isolated waveform in the reproduced waveform of the data signal is 170 nm or less. The magnetic recording medium according to any one of claims 1 to 3.
6. The half-width of an isolated waveform in the reproduced waveform of the data signal is 165 nm or less. The magnetic recording medium according to any one of claims 1 to 3.
7. The average particle size of the plurality of magnetic powders is 8 nm or more and 22 nm or less. The magnetic recording medium according to any one of claims 1 to 3.
8. The average particle volume of the magnetic powder is 1950 nm 3 is less than or equal to The magnetic recording medium according to any one of claims 1 to 3.
9. The average particle volume of the magnetic powder is 1600 nm 3 is less than or equal to The magnetic recording medium according to any one of claims 1 to 3.
10. The average particle volume of the magnetic powder is 1300 nm 3 is less than or equal to The magnetic recording medium according to any one of claims 1 to 3.
11. The average aspect ratio of the magnetic powder is 1.0 or more and 2.8 or less. The magnetic recording medium according to any one of claims 1 to 3.
12. The average aspect ratio of the magnetic powder is 1.0 or more and 2.6 or less. The magnetic recording medium according to any one of claims 1 to 3.
13. The substrate has an average thickness of 4.2 μm or less. The magnetic recording medium according to any one of claims 1 to 3.
14. The substrate has an average thickness of 4.0 μm or less. The magnetic recording medium according to any one of claims 1 to 3.
15. The average thickness of the magnetic layer is 80 nm or less. The magnetic recording medium according to any one of claims 1 to 3.
16. The average thickness of the magnetic layer is 70 nm or less. The magnetic recording medium according to any one of claims 1 to 3.
17. The average thickness of the magnetic layer is 60 nm or less. The magnetic recording medium according to any one of claims 1 to 3.
18. When the coercive force in the perpendicular direction is Hc1 and the coercive force in the longitudinal direction is Hc2, the following conditional formula (1) is satisfied: Hc2 / Hc1≦0.7...(1) The magnetic recording medium according to any one of claims 1 to 3.
19. The magnetic recording medium has a coercive force in the perpendicular direction of 2900 Oe or more. The magnetic recording medium according to any one of claims 1 to 3.
20. A magnetic recording medium according to any one of claims 1 to 19, a housing for accommodating the magnetic recording medium; Equipped with Magnetic recording medium cartridge.
Citation Information
Patent Citations
Magnetic recording medium
JP1984127224A
Magnetic recording medium
JP1997320031A
Magnetic recording medium and magnetic recording method
JP1998228619A
Magnetic recording medium
JP2001067639A
Slave medium for magnetic transfer
JP2004241030A