Polyol-based adhesives, polyurethane adhesives, and laminates
A polyurethane adhesive using a plant-derived polyol and pH-adjusted filler addresses environmental concerns and appearance defects in metallized film bonding, achieving excellent adhesion and uniform coating without 'yuzu skin' issues.
Patent Information
- Application Number
- JP2020215683
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-12-24
- Publication Date
- 2024-10-08
- Estimated Expiration
- 2040-12-24
AI Technical Summary
Existing solvent-based adhesives used in laminating metallized films and metal foils for applications like food packaging suffer from environmental pollution issues and cause 'yuzu peel' appearance defects, poor adhesive performance, and insufficient bonding due to high viscosity or filler settling, which are not effectively addressed by existing solvent-free solutions.
A polyurethane adhesive comprising a plant-derived polyol with a number average molecular weight of 50 to 2,500, a polyisocyanate, and a filler with a pH value over 7, such as aluminum hydroxide or zeolite, is used to achieve low viscosity and uniform dispersion, ensuring excellent coating appearance and adhesive performance without 'yuzu skin' defects.
The solution provides a solvent-free adhesive with improved coating appearance and strong adhesion to metallized films and metal foils, maintaining uniform dispersion and cohesive force, thus preventing defects and enhancing bonding performance.
Smart Images

Figure 0007563170000001 
Figure 0007563170000002 
Figure 0007563170000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a polyol base, a polyurethane adhesive, and a laminate using the same, and more specifically to a polyol base that constitutes a polyurethane adhesive useful as a packaging material for foods, medical products, cosmetics, etc., a polyurethane adhesive, and a laminate using the same. [Background technology]
[0002] Conventionally, bonding various plastic films together, or bonding plastic films to metal-deposited films or metal foils, has been carried out by the dry lamination method using a polyol / isocyanate-based solvent-based adhesive. However, because the dry lamination method uses adhesives that contain organic solvents, it has many problems, such as environmental pollution from exhaust, the risk of fire and explosion, and the impairment of hygienic working conditions. Due to demands for improving the working environment, strengthening the Fire Service Act, and restricting the release of VOCs (volatile organic compounds) into the atmosphere, there is a growing demand for adhesives that do not use organic solvents, and studies are underway to develop solvent-free adhesives.
[0003] For example, Patent Document 1 discloses a solventless laminating adhesive composition comprising an organic polymer polyol and an organic polyisocyanate compound. Patent Document 2 discloses a solventless laminating adhesive in which the ratio of hydroxyl groups in a polyol component to isocyanate groups in a polyisocyanate component is hydroxyl groups:isocyanate groups=1:1 to 1:3. However, when the adhesives described in Patent Documents 1 and 2 are used to bond metal-deposited films for applications such as food packaging that require high barrier properties, a "yellow peel" pattern occurs during application of the adhesive, resulting in poor appearance. In particular, for a lattice-like printed pattern in which the plain areas extend in both the TD and MD directions, there is a problem that a step occurs between the ink area and the plain area, and no winding pressure is applied, resulting in frequent poor appearance.
[0004] As a method for improving the appearance defect, for example, Patent Documents 3 and 4 propose a method of lowering the viscosity of the adhesive. However, the methods described in Patent Documents 3 and 4 cannot improve the coating appearance in the MD direction where the winding pressure is not applied. Furthermore, lowering the viscosity of the adhesive reduces the cohesive force of the resin and the adhesive performance. Therefore, although it can be applied to adhesion between films such as oriented polypropylene film and non-oriented polypropylene film, which are relatively easy to bond, there is a problem that the adhesive performance is insufficient for metal-deposited films, metal foils, etc.
[0005] Meanwhile, in recent years, as part of efforts to combat environmental pollution, along with growing calls for the creation of a recycling-oriented society, there is a desire to move away from fossil fuels in the materials field, just as in the energy field, and the use of biomass has been attracting attention. Biomass is an organic compound that is photosynthesized from carbon dioxide and water, and by using it, it becomes carbon dioxide and water again, making it a so-called carbon-neutral renewable energy. Recently, the practical application of biomass plastics made from these biomass materials has progressed rapidly, and attempts are being made to manufacture various resins from biomass materials.
[0006] For example, Patent Documents 5 and 6 propose an adhesive containing a filler as a method for achieving high cohesive strength. However, although the adhesives described in Patent Documents 5 and 6 can suppress the foaming of bubbles, the viscosity increases due to the addition of filler, which deteriorates the appearance in the TD direction. On the other hand, there is a problem that the filler settles when the viscosity is reduced. Furthermore, it cannot solve the problem of orange peel caused by the step between the ink area and the plain area. [Prior art documents] [Patent documents]
[0007] [Patent Document 1] Japanese Patent Application Publication No. 8-60131 [Patent Document 2] JP 2003-96428 A [Patent Document 3] Japanese Patent Application Publication No. 8-283691 [Patent Document 4] JP 2002-249745 A [Patent Document 5] JP 2001-162579 A [Patent Document 6] JP 2009-114258 A Summary of the Invention [Problem to be solved by the invention]
[0008] The object of the present invention is to provide a polyol base that constitutes a polyurethane adhesive which uses biomass raw materials, has excellent coating appearance without causing poor appearance such as "citrus peel" regardless of the printing pattern, and exhibits excellent adhesive performance even to metal vapor-deposited films and metal foils, a polyurethane adhesive, and a laminate which uses the polyol base and the polyurethane adhesive and has excellent coating appearance and adhesive performance. [Means for solving the problem]
[0009] A polyurethane adhesive according to one embodiment of the present invention is a polyurethane adhesive comprising a polyol (A), a polyisocyanate (B), and a filler (C), characterized in that the polyol (A) comprises a plant-derived polyol (a1) and a polyol (a2) comprising a structural unit derived from a polyether polyol having a number average molecular weight in the range of 50 to 2,500, and the filler (C) is a filler having a pH value of greater than 7 as measured in accordance with JIS K 5101.
[0010] A polyurethane adhesive according to one embodiment of the present invention is characterized in that the polyol (A) contains 20 to 70 mass % of structural units derived from the polyether polyol having a number average molecular weight in the range of 50 to 2,500.
[0011] In a polyurethane adhesive according to one aspect of the present invention, the plant-derived polyol (a1) has an acid value in the range of 0.1 to 15 mgKOH / g.
[0012] A polyurethane adhesive according to one embodiment of the present invention is characterized in that the polyol (a2) is a polyether urethane polyol obtained by reacting a polyether polyol having a number average molecular weight in the range of 50 to 2,500 with a polyisocyanate.
[0013] In one embodiment of the polyurethane adhesive of the present invention, the filler (C) contains at least one selected from the group consisting of aluminum hydroxide, zeolite, magnesium oxide, and an inorganic compound treated with a basic silane coupling agent, and the average particle size of the filler is 1×10 -4 It is characterized by being in the range of 0.1 mm.
[0014] A polyurethane adhesive according to one aspect of the present invention is characterized in that it contains the filler (C) in an amount of 0.1 to 3 mass % based on the total mass of the polyol (A) and the polyisocyanate (B).
[0015] A polyurethane adhesive according to one aspect of the present invention is characterized in that it has a melt viscosity at 70° C. in the range of 50 to 3,000 mPa·s.
[0016] A polyol base according to one embodiment of the present invention is a polyol base constituting a polyurethane adhesive containing a polyol base and a polyisocyanate (B), and is characterized in that it contains a polyol (A) and a filler (C), the polyol (A) contains a plant-derived polyol (a1) and a polyol (a2) containing a structural unit derived from a polyether polyol having a number average molecular weight in the range of 50 to 2,500, and the filler (C) is a filler having a pH value of more than 7 when measured in accordance with JIS K 5101.
[0017] A polyurethane adhesive according to one embodiment of the present invention is characterized by containing the above-mentioned polyol base agent and a polyisocyanate (B).
[0018] A laminate according to one aspect of the present invention is characterized in that an adhesive layer made of the polyurethane adhesive described above is disposed between at least two substrates. Effect of the Invention
[0019] The present invention makes it possible to provide a polyol base that constitutes a polyurethane adhesive, which uses biomass raw materials, has excellent coating appearance without causing poor appearance such as ``citrus peel'' regardless of the printing pattern, and exhibits excellent adhesive performance even to metal vapor-deposited films and metal foils, a polyurethane adhesive, and a laminate that uses the polyol base and polyurethane adhesive and has excellent coating appearance and adhesive performance. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0020] The polyurethane adhesive of the present invention comprises a polyol, a polyisocyanate, and a filler, wherein the polyol comprises a plant-derived polyol and a polyol containing a structural unit derived from a polyether polyol having a number average molecular weight in the range of 50 to 2,500, and the filler has a pH value of greater than 7 as measured in accordance with JIS K 5101. By combining a plant-derived polyol, a polyol containing structural units derived from a polyether polyol of a specific number average molecular weight, and a filler with a pH value of above 7, it is possible to simultaneously achieve a coating film with low viscosity but high cohesive strength and prevention of settling due to filler cohesion, thereby obtaining a solvent-free adhesive with excellent coating appearance and adhesive performance. The present invention will be described in detail below.
[0021] <Polyol (A)> In the present invention, as the polyol (A), a plant-derived polyol (a1) and a polyol (a2) containing a structural unit derived from a polyether polyol having a number average molecular weight in the range of 50 to 2,500 are used. Moreover, the polyol (A) preferably contains structural units derived from the polyether polyol having a number average molecular weight in the range of 50 to 2,500 in an amount in the range of 20 to 70 mass %, more preferably in the range of 30 to 70 mass %.
[0022] [Plant-derived polyol (a1)] The plant-derived polyol (a1) in the present invention is a polyol using a component of a vegetable oil such as castor oil, and examples thereof include castor oil, castor oil derivatives, and vegetable oil derivatives other than castor oil.
[0023] (Castor oil) Castor oil is a glyceride of fatty acids, primarily ricinoleic acid, and includes, for example, glycerides of unsaturated fatty acids including ricinoleic acid, oleic acid, and linoleic acid, and saturated fatty acids including palmitic acid and stearic acid. The content of each component in castor oil is usually 87 to 90 mass% ricinoleic acid, 2.5 to 4 mass% oleic acid, 4 to 5 mass% linoleic acid, 0.5 to 1.5 mass% palmitic acid, and 0.5 to 1.5 mass% stearic acid. The average number of functional hydroxyl groups in castor oil is, for example, about 2 to 3.3, and preferably about 2.5 to 3. The hydroxyl value of castor oil is, for example, 150 to 175 mgKOH / g, and preferably 155 to 170 mgKOH / g. The hydroxyl value can be determined by an acetylation method or a phthalation method in accordance with JIS K 1557-1 (2007).
[0024] Castor oil can be commercially available. Examples of commercially available castor oil include deodorized refined castor oil (manufactured by Toyokuni Oil Mills), refined castor oil (manufactured by Toyokuni Oil Mills), ELA-DR (manufactured by Toyokuni Oil Mills), industrial No. 1 castor oil (manufactured by Toyokuni Oil Mills), refined castor oil special A (Marutoku A) (manufactured by Ito Oil Mills), refined castor oil special A (Kakutoku A) (manufactured by Ito Oil Mills), refined castor oil special A (Diamond) (manufactured by Ito Oil Mills), refined castor oil 1 (Kakukoichi) (manufactured by Ito Oil Mills), refined castor oil 1 (Koichi) (manufactured by Ito Oil Mills), FSG CASTOR OIL (manufactured by ROYAL CASTOR PRODUCTS), and COLD PRESS CASTOR OIL (manufactured by ROYAL CASTOR PRODUCTS).
[0025] (Castor oil derivatives, vegetable oil derivatives other than castor oil) Examples of castor oil derivatives include dehydrated castor oil, hydrogenated castor oil (hereinafter, hydrogenated castor oil) which is a hydrogenated product of castor oil, an adduct of 5 to 50 moles of ethylene oxide with castor oil, and castor oil-based polyols. Castor oil-based polyols are polyols with hydroxyl groups at both ends, which are obtained by condensing a low molecular weight diol or a polyfunctional alcohol with the fatty acid obtained by hydrolyzing castor oil with a strong base or the like. Among these, castor oil-based polyols, which combine ricinoleic acid with a low molecular weight diol, are preferred because they have two hydroxyl groups per molecule, suppress excessive crosslinking, and have an excellent pot life.
[0026] Examples of the low molecular weight diol include bifunctional alcohols such as ethylene glycol, triethylene glycol, propylene glycol, diethylene glycol, 1,3-propanediol, 1,4-butanediol, 1,3-butanediol, bishydroxyethoxybenzene, 1,6-hexanediol, 1,8-octanediol, 1,9-nonanediol, neopentyl glycol, 3-methyl-1,5-pentanediol, 2-methyl-1,3-propanediol, 3,3,5-trimethylpentanediol, 1,12-octadecanediol, 1,2-alkanediol, 1,3-alkanediol, dimer diol, hydrogenated dimer diol, 3,3'-dimethylolheptane, polyoxyethylene glycol, polyoxypropylene glycol, and polytetramethylene ether glycol, or mixtures thereof.
[0027] Examples of the polyfunctional alcohol include trifunctional or higher polyfunctional alcohols such as glycerin, trimethylolpropane, pentaerythritol, sorbitol, trimethylolethane, 1,2,6-hexatriol, and 1,2,4-butanetriol, and mixtures thereof.
[0028] An example of a vegetable oil derivative other than castor oil is a reaction product of epoxidized soybean oil with a low molecular weight diol. As the low molecular weight diol, the above-mentioned low molecular weight diols can be used.
[0029] A preferred plant-derived polyol is castor oil-based polyol, since it has two hydroxyl groups per molecule, which can suppress excessive crosslinking and reduce the viscosity of the adhesive, and it has an acid value, which gives it excellent adhesive strength.
[0030] The plant-derived polyol (a1) usually has an acid value, which is preferably in the range of 0.1 to 30 mgKOH / g, more preferably in the range of 0.1 to 15 mgKOH / g. An acid value in the range of 0.1 to 15 mgKOH / g is particularly preferred because it provides excellent adhesion performance and pot life.
[0031] [Polyol (a2) containing a structural unit derived from a polyether polyol having a number average molecular weight in the range of 50 to 2,500] There are no particular limitations on the polyol (a2) so long as it contains, in the molecule, a structural unit derived from a polyether polyol having a number average molecular weight in the range of 50 to 2,500 and two or more hydroxyl groups. Such polyol (a2) may be a polyether polyol having a number average molecular weight in the range of 50 to 2,500, which is used as it is, or may be a polyether urethane polyol obtained by reacting a polyol containing a polyether polyol having a number average molecular weight in the range of 50 to 2,500 with a polyisocyanate, or may be a polyether ester polyol obtained by reacting a polyol containing a polyether polyol having a number average molecular weight in the range of 50 to 2,500 with a polyvalent carboxylic acid. The polyols including polyether polyols, polyisocyanates, and polyvalent carboxylic acids constituting the polyol (a2) may be used alone or in combination of two or more.
[0032] (Polyether polyol with a number average molecular weight in the range of 50 to 2,500) Examples of the polyether polyol having a number average molecular weight in the range of 50 to 2,500 include polyether polyols obtained by polymerizing an oxirane compound such as ethylene oxide, propylene oxide, butylene oxide, or tetrahydrofuran using a low molecular weight polyol such as water, ethylene glycol, propylene glycol, trimethylolpropane, or glycerin as an initiator. The number average molecular weight of the polyether polyol is preferably in the range of 200 to 2,500.
[0033] When the polyol (a2) is a polyether urethane polyol, the polyol constituting the polyol (a2) may contain other polyols other than the polyether polyol having a number average molecular weight in the range of 50 to 2500. Examples of such other polyols include polyester polyols, polyether polyols having a number average molecular weight of more than 2500, polyurethane polyols, polyesteramide polyols, acrylic polyols, polycarbonate polyols, polycaprolactone polyols, polyvalerolactone polyols, polyolefin polyols, and polyhydroxyalkanes.
[0034] (Polyisocyanate) When the polyol (a2) is a polyether urethane polyol, the polyisocyanate constituting the polyol (a2) is not particularly limited. Examples of such polyisocyanates include aliphatic diisocyanates such as trimethylene diisocyanate, tetramethylene diisocyanate, hexamethylene diisocyanate, 1,2-propylene diisocyanate, 1,2-butylene diisocyanate, 2,3-butylene diisocyanate, 1,3-butylene diisocyanate, 2,4,4- or 2,2,4-trimethylhexamethylene diisocyanate, and 2,6-diisocyanate methyl caproate; 1,4-cyclohexane diisocyanate; Alicyclic diisocyanates such as 1,3-cyclohexane diisocyanate, 3-isocyanatomethyl-3,5,5-trimethylcyclohexyl isocyanate, 4,4'-methylenebis(cyclohexyl isocyanate), methyl 2,4-cyclohexane diisocyanate, methyl 2,6-cyclohexane diisocyanate, 1,4-bis(isocyanatomethyl)cyclohexane, 1,3-bis(isocyanatomethyl)cyclohexane; m-phenylene diisocyanate, p-phenylene diisocyanate, Aromatic diisocyanates such as 1,5-naphthalene diisocyanate, 4,4'-diphenyl diisocyanate, 1,5-naphthalene diisocyanate, 4,4'-diphenylmethane diisocyanate, 2,4- or 2,6-tolylene diisocyanate or mixtures thereof, 4,4'-toluidine diisocyanate, dianisidine diisocyanate, 4,4'-diphenylether diisocyanate; 1,3- or 1,4-xylylene diisocyanate or mixtures thereof, ω,ω'-diisocyanate-1, Aromatic aliphatic diisocyanates such as 4-diethylbenzene, 1,3- or 1,4-bis(1-isocyanato-1-methylethyl)benzene or mixtures thereof; polyisocyanate monomers such as organic triisocyanates such as triphenylmethane-4,4',4"-triisocyanate, 1,3,5-triisocyanatobenzene, 2,4,6-triisocyanatotoluene, and organic tetraisocyanates such as 4,4'-diphenyldimethylmethane-2,2'-5,5'-tetraisocyanate;Examples of the polyisocyanate include dimers, trimers, biurets, and allophanates derived from the above polyisocyanate monomers, and polyisocyanates having a 2,4,6-oxadiazinetrione ring obtained from carbon dioxide gas and the above polyisocyanate monomers. The polyisocyanates may be used alone or in combination of two or more kinds.
[0035] (Polycarboxylic Acid) When the polyol (a2) is a polyether ester polyol, the polyvalent carboxylic acid constituting the polyol (a2) is not particularly limited. Examples of such polyvalent carboxylic acids include dibasic acids such as terephthalic acid, isophthalic acid, naphthalenedicarboxylic acid, phthalic anhydride, adipic acid, azelaic acid, sebacic acid, succinic acid, glutaric acid, tetrahydrophthalic anhydride, hexahydrophthalic anhydride, maleic anhydride, and itaconic anhydride, dialkyl esters thereof, and mixtures thereof.
[0036] The polyol (a2) is preferably a polyetherurethane polyol obtained by reacting a polyether polyol having a number average molecular weight in the range of 50 to 2,500 with a polyisocyanate, and more preferably a polyetherurethane polyol obtained by reacting a polyether polyol having a number average molecular weight in the range of 50 to 2,500 with an aromatic polyisocyanate. The number average molecular weight of the polyol (a2) is preferably in the range of 1,000 to 10,000, and more preferably in the range of 1,500 to 5,000. These polyols (a2) may be used alone or in combination of two or more.
[0037] [Other polyols] The polyol (A) in the present invention may be used in combination with other polyols than the plant-derived polyol (a1) and the polyol (a2) as long as the effects of the present invention are not impaired. Examples of such other polyols include polyester polyols, polyether polyols, polyurethane polyols, polyesteramide polyols, acrylic polyols, polycarbonate polyols, polycaprolactone polyols, polyvalerolactone polyols, polyolefin polyols, and polyhydroxyalkanes. These may be used alone or in combination of two or more.
[0038] <Polyisocyanate (B)> The polyisocyanate (B) in the present invention is not particularly limited as long as it is a compound having two or more isocyanate groups in the molecule. Examples of such polyisocyanates (B) include aliphatic diisocyanates such as trimethylene diisocyanate, tetramethylene diisocyanate, hexamethylene diisocyanate, 1,2-propylene diisocyanate, 1,2-butylene diisocyanate, 2,3-butylene diisocyanate, 1,3-butylene diisocyanate, 2,4,4- or 2,2,4-trimethylhexamethylene diisocyanate, and 2,6-diisocyanate methyl caproate; 1,4-cyclohexane diisocyanate; Isocyanates, alicyclic diisocyanates such as 1,3-cyclohexane diisocyanate, 3-isocyanatomethyl-3,5,5-trimethylcyclohexyl isocyanate, 4,4'-methylenebis(cyclohexyl isocyanate), methyl 2,4-cyclohexane diisocyanate, methyl 2,6-cyclohexane diisocyanate, 1,4-bis(isocyanatomethyl)cyclohexane, 1,3-bis(isocyanatomethyl)cyclohexane; m-phenylene diisocyanate, p- Aromatic diisocyanates such as phenylene diisocyanate, 4,4'-diphenyl diisocyanate, 1,5-naphthalene diisocyanate, 4,4'-diphenylmethane diisocyanate, 2,4- or 2,6-tolylene diisocyanate or mixtures thereof, 4,4'-toluidine diisocyanate, dianisidine diisocyanate, 4,4'-diphenylether diisocyanate; 1,3- or 1,4-xylylene diisocyanate or mixtures thereof, ω,ω'-diisocyanate-1, Aromatic aliphatic diisocyanates such as 4-diethylbenzene, 1,3- or 1,4-bis(1-isocyanato-1-methylethyl)benzene or mixtures thereof; polyisocyanate monomers such as organic triisocyanates such as triphenylmethane-4,4',4"-triisocyanate, 1,3,5-triisocyanatobenzene, 2,4,6-triisocyanatotoluene, and organic tetraisocyanates such as 4,4'-diphenyldimethylmethane-2,2'-5,5'-tetraisocyanate;Examples of the polyisocyanate include dimers, trimers, biurets, and allophanates derived from the above polyisocyanate monomers, and polyisocyanates having a 2,4,6-oxadiazinetrione ring obtained from carbon dioxide gas and the above polyisocyanate monomers.
[0039] Among these, a mixture of 4,4'-diphenylmethane diisocyanate and 2,4-diphenylmethane diisocyanate or a mixture of biuret of 4,4'-diphenylmethane diisocyanate and hexamethylene diisocyanate is preferably used from the viewpoints of pot life and coating appearance, since it does not cause rapid thickening.
[0040] The polyisocyanate (B) may be an adduct (hereinafter referred to as polyurethane polyisocyanate) in which a glycol is added to the above-mentioned diisocyanate or polyisocyanate monomer. Examples of the glycol include low molecular weight polyols having a molecular weight of less than 200, such as ethylene glycol, propylene glycol, butylene glycol, hexylene glycol, neopentyl glycol, 1,6-hexanediol, 3-methyl-1,5-pentanediol, 3,3'-dimethylolpropane, cyclohexanedimethanol, diethylene glycol, triethylene glycol, dipropylene glycol, glycerol, trimethylolpropane, pentaerythritol, and sorbitol; and polypropylene glycol, polyester polyols, polyether ester polyols, polyester amide polyols, polycaprolactone polyols, polyvalerolactone polyols, acrylic polyols, polycarbonate polyols, polyhydroxy alkanes, castor oil, and polyurethane polyols. The glycols may be used alone or in combination of two or more.
[0041] The polyisocyanate (B) is preferably a polyurethane polyisocyanate, more preferably a reaction product of an aromatic polyisocyanate with a polyol, and even more preferably a reaction product of an aromatic polyisocyanate with a polyol including polypropylene glycol and a polyester polyol. The polyisocyanate (B) contains an aromatic skeleton, which improves heat resistance and suppresses lifting caused by folding of the heat-sealed portion. The structure derived from the polyester polyol improves adhesive strength to metal-deposited films, metal foils, etc. The number-average molecular weight of the polypropylene glycol is preferably 200 to 3,000. The polyisocyanate (B) may be used alone or in combination of two or more kinds.
[0042] <Filler (C)> It is important that the filler (C) used in the present invention has a pH value, measured in accordance with JIS K 5101, exceeding 7. If the surface pH value is 7 or less, the interaction with the plant-derived polyol (a1) having an acid value is small, the filler cannot maintain a uniformly dispersed state, and the filler aggregates. On the other hand, by using a filler (C) having a pH value of more than 7, the filler can maintain a uniformly dispersed state by interacting with the plant-derived polyol (a1) having an acid value. In particular, when used as a solvent-free adhesive, it exhibits excellent coating appearance and good adhesive performance. The adhesive containing the filler (C) exhibits thixotropic flow characteristics, and when subjected to strong shearing force on the coating roll during coating, it becomes low in viscosity and is transferred from the roll to the substrate. The adhesive transferred to the substrate rapidly exhibits structural viscosity and quickly adheres to the substrate. This allows a good appearance to be obtained.
[0043] The filler (C) is not particularly limited, and any inorganic or organic compound can be used as long as it has a pH value exceeding 7. These fillers (C) may be used alone or in combination of two or more kinds.
[0044] Examples of inorganic compound fillers include aluminum oxide, aluminum silicate, aluminum hydroxide, alumina white, potassium sulfate, zinc oxide, zinc carbonate, magnesium aluminometasilicate, magnesium silicate, magnesium oxide, magnesium carbonate, magnesium hydroxide, barium titanate, barium sulfate, barium carbonate, calcium carbonate, calcium hydroxide, calcium oxide, calcium silicate, calcium sulfite, calcium sulfate, titanium oxide, silica, zeolite, activated carbon, kaolin, talc, rosewood clay, silica stone, mica, graphite, sericite, montmorillonite, sericite, sepiolite, bentonite, perlite, zeolite, wollastonite, fluorite, and dolomite. In addition, the inorganic compounds may be treated with a basic silane coupling agent. Among them, aluminum hydroxide, zeolite, and magnesium oxide are preferred from the viewpoint of pH.
[0045] Examples of organic compound fillers include benzoguanamine resin, silicone resin, styrene resin, crosslinked polystyrene, epoxy resin, phenol resin, fluororesin, polyethylene resin, polyester resin, polyimide resin, polyamide resin, polyacetal resin, polyurethane resin, vinyl acetate copolymer resin, polyphenylene oxide resin, nylon 6, nylon 12, cellulose, acrylic resin, and methacrylic resin.
[0046] The filler (C) is preferably an inorganic compound, and more preferably contains at least one selected from the group consisting of alumina, zeolite, magnesium oxide, and inorganic compounds treated with a basic silane coupling agent.
[0047] The average particle size of the filler (C) is usually 1×10 -5 ~0.2 mm, preferably 1×10 -4 When the average particle size is 0.2 mm or less, the appearance of the coating film after coating is excellent. -5When the particle size is 1 mm or more, the adhesive has excellent flow characteristics and the coating appearance has excellent transparency, which is preferable. The average particle size in this specification is the average volume diameter, and is a value determined by a laser light scattering method.
[0048] The content of the filler (C) in the adhesive of the present invention is appropriately selected depending on the required performance, adhesion method, etc., but is preferably in the range of 0.1 to 3 mass %, more preferably 0.5 to 2 mass %, based on the total mass of the polyol (A) and the polyisocyanate (B). If the content of the filler (C) is 0.1% by mass or more, the adhesive has excellent flow properties, and if it is 3% by mass or less, the adhesive has excellent transparency in its coating appearance, which is preferable.
[0049] The filler (C) may be mixed with the polyol (A) to form a polyol base. The polyurethane adhesive of the present invention can be obtained by further mixing the polyol base with the polyisocyanate (B). The filler (C) may be mixed with the polyisocyanate (B) and used as a polyol curing agent. The polyurethane adhesive of the present invention can be obtained by further mixing the polyisocyanate curing agent with the polyol (A). The filler (C) may be blended in both the polyol (A) and the polyisocyanate (C), or may be blended when the polyol (A) and the polyisocyanate (B) are mixed together.
[0050] The polyurethane adhesive of the present invention has an initial melt viscosity at 70°C after mixing the polyol (A), polyisocyanate (B), and filler (C) in the range of preferably 50 to 3,000 mPa s, and more preferably 100 to 1,000 mPa s. In this specification, the term "initial" in the initial mixed viscosity refers to within 5 minutes after mixing, and the melt viscosity is a value determined using a Brookfield viscometer. If the melt viscosity at 70°C is 3,000 mPa·s or less, the coating property at temperatures below 100°C is good, and there is no pitch shift of the printed pattern due to the film stretching, resulting in excellent workability. If the melt viscosity is 50 mPa·s or more, sufficient initial cohesive strength is expressed, resulting in excellent adhesive performance. In addition, the thickness when coated is uniform, which is preferable as it is less likely to cause poor appearance or warping.
[0051] <Other ingredients> The polyurethane adhesive of the present invention may further contain additives such as antioxidants, ultraviolet absorbers, hydrolysis inhibitors, antifungals, thickeners, plasticizers, defoamers, pigments, and fillers as necessary. In order to further improve the adhesive performance, the polyurethane adhesive may also contain adhesion aids such as silane coupling agents, phosphoric acid, phosphoric acid derivatives, acid anhydrides, and adhesive resins. In order to adjust the curing reaction, the polyurethane adhesive may also contain known catalysts, additives, and the like. These other components may be used alone or in combination of two or more.
[0052] <Laminate> The laminate of the present invention is one in which an adhesive layer made of a polyurethane adhesive obtained by mixing a polyol (A), a polyisocyanate (B) and a filler (C) is laminated between at least two substrates. The laminate can be formed, for example, by applying the polyurethane adhesive to a first substrate, laminating a second substrate thereon, and curing the adhesive layer located between both substrates at room temperature or under heating, but is not limited to this structure. The laminate of the present invention may further include another layer disposed thereon via an adhesive layer or the like. The amount of adhesive to be applied is appropriately selected depending on the type of substrate and coating conditions, but is usually 1.0 to 5.0 g / m 2 and preferably 1.5 to 4.5 g / m 2 It is. Moreover, the thickness of the laminate is preferably 10 μm or more from the viewpoint of strength and durability as a packaging material.
[0053] [Base material] The substrate is not particularly limited and examples thereof include plastic films, papers, gas barrier substrates, sealants, etc., which are commonly used for packaging applications, and the two substrates may be the same or different. Examples of plastic films that can be used include polyester resin films such as polyethylene terephthalate, polyethylene naphthalate (PEN), and polylactic acid (PLA); polyolefin resin films such as polyethylene (PE) and polypropylene (PP); polystyrene resin films; polyamide resin films such as nylon 6 and poly-p-xylylene adipamide (MXD6 nylon); polycarbonate resin films; polyacrylonitrile resin films; polyimide resin films; laminates thereof (e.g., nylon 6 / MXD6 / nylon 6, nylon 6 / ethylene-vinyl alcohol copolymer / nylon 6), and mixtures thereof. Among these, those having mechanical strength and dimensional stability are preferred. The plastic film preferably has a thickness of 5 to 50 μm, more preferably 10 to 30 μm.
[0054] The paper includes natural paper and synthetic paper. As the gas barrier substrate, aluminum foil and plastic films having a vapor-deposited layer of aluminum, silica, alumina, etc. are preferable. For example, in the case of aluminum foil, a thickness in the range of 3 to 50 μm is preferable from an economical point of view.
[0055] Examples of the sealant include polyethylenes such as low-density polyethylene (LDPE), linear low-density polyethylene (LLDPE) and high-density polyethylene (HDPE), acid-modified polyethylene, polypropylene (PP), acid-modified polypropylene, copolymerized polypropylene, ethylene-vinyl acetate copolymer, ethylene-(meth)acrylic acid ester copolymer, ethylene-(meth)acrylic acid copolymer, polyolefin resins such as ionomers, etc. Among these, polypropylene-based resins are preferred from the viewpoint of heat resistance during retort, and unstretched polypropylene is particularly preferred from the viewpoint of heat sealability. The thickness of the sealant is not particularly limited, but is preferably in the range of 10 to 60 μm, more preferably 15 to 40 μm, taking into consideration processability into packaging, heat sealing properties, etc. Also, by providing the sealant with unevenness with a height difference of 5 to 20 μm, it is possible to impart slipperiness to the sealant and tearability of the packaging. Furthermore, the various sealants may have a vapor-deposited layer of aluminum, silica, alumina, or the like in addition to the aluminum foil.
[0056] The substrate may have a printed layer on the substrate. The printed layer is a layer on which any desired printed pattern such as letters, numbers, pictures, figures, symbols, patterns, etc. is formed for decoration, display of contents, display of expiration date, display of manufacturer, seller, etc., and for imparting aesthetics, and includes a solid printed layer. The printed layer can be formed using a conventionally known pigment or dye, and the method of forming the printed layer is not particularly limited. Generally, the printing layer is formed using a printing ink containing a colorant such as a pigment or dye. The method for applying the printing ink is not particularly limited, and the printing ink can be applied by a method such as gravure coating, flexo coating, roll coating, bar coating, die coating, curtain coating, spin coating, inkjet, etc. The printing layer can be formed by leaving the ink alone or, if necessary, blowing air, heating, drying under reduced pressure, irradiating with ultraviolet light, etc. The printing layer preferably has a thickness of 0.1 to 10 μm, more preferably 1 to 5 μm, and even more preferably 1 to 3 μm. EXAMPLES
[0057] The present invention will be described in more detail below with reference to examples and comparative examples. In the examples and comparative examples, "parts" and "%" mean "parts by mass" and "% by mass" unless otherwise specified.
[0058] The number average molecular weight (Mn) of the polyol was calculated using gel permeation chromatography (GPC) and converted into a value using standard polystyrene. The melt viscosity at 70° C. was measured using a B-type viscometer.
[0059] <Production of plant-derived polyols> (Castor oil-based polyol B) 85 parts of castor oil-based polyol A (manufactured by Toyokuni Oil Mills, product name: HS 2G-270B, acid value 0.4 mgKOH / g), 3 parts of dimethylolbutanoic acid, and 12 parts of 4,4'-diphenylmethane diisocyanate were charged into a reaction vessel. The mixture was heated at 100°C for 3 hours while stirring under a nitrogen gas flow to carry out a urethane reaction, thereby obtaining castor oil-based polyol B with a number average molecular weight of 1,000. The acid value of castor oil-based polyol B was 13 mgKOH / g.
[0060] (Castor oil-based polyol C) 84 parts of castor oil-based polyol A (manufactured by Toyokuni Oil Mills, product name: HS 2G-270B), 5 parts of dimethylolbutanoic acid, and 11 parts of 4,4'-diphenylmethane diisocyanate were charged into a reaction vessel. The mixture was heated at 100°C for 3 hours while stirring under a nitrogen gas flow to carry out a urethane reaction, thereby obtaining castor oil-based polyol C with a number average molecular weight of 800. The acid value of castor oil-based polyol C was 18 mgKOH / g.
[0061] <Production of polyol (a2) containing structural units derived from polyether polyol having a number average molecular weight in the range of 50 to 2,500> (Synthesis Example 1) Polyol (a2-1) A reaction vessel was charged with 20 parts of a triol having a molecular weight of about 400, which was obtained by adding polypropylene glycol to glycerin, 38 parts of polypropylene glycol having a molecular weight of about 2,000, 5 parts of 4,4'-diphenylmethane diisocyanate, and 5 parts of 2,4-diphenylmethane diisocyanate. The mixture was heated at 80°C to 90°C for 3 hours while stirring under a nitrogen gas stream to carry out a urethane reaction, thereby obtaining polyol (a2-1), which is a polyether urethane polyol having a number average molecular weight of 3,000 and hydroxyl groups at both ends.
[0062] (Synthesis Examples 2 to 8) Polyols (a2-2 to a2-8) Polyols (a2-2) to (a2-6) were obtained in the same manner as in Synthesis Example 1, except that the blending recipe was changed to that shown in Table 1. The Mn values of the obtained resins are shown in Table 1.
[0063] [Table 1]
[0064] The abbreviations in Table 1 are as follows: PPG400 (3f): A triol with a molecular weight of approximately 400, in which polypropylene glycol is added to glycerin (manufactured by ADEKA Corporation, product name: ADEKA Polyether G-400) PPG2000: Polypropylene glycol with a molecular weight of approximately 2,000 (manufactured by ADEKA Corporation, product name: ADEKA Polyether P-2000) Polyester resin 1: Polyester polyol with a molecular weight of approximately 2000, mainly composed of adipic acid and propylene glycol (manufactured by ADEKA CORPORATION, product name: ADEKA New Ace F7-67) Polyester resin 2: Polyester polyol with a molecular weight of approximately 1,000, mainly composed of adipic acid and butanediol (manufactured by Showa Denko K.K., product name: Teslac 2464) 4,4′-MDI: 4,4′-diphenylmethane diisocyanate 2,4-MDI: 2,4-diphenylmethane diisocyanate
[0065] <Production of polyol base material> (Example 1) Polyol base (S1) 68 parts of the polyether polyol (a2-1) obtained in Synthesis Example 1 was stirred at 70° C. under a nitrogen gas stream to obtain a 1.0×10 sintered polyether polyol having an average particle size of 2.0×10 -3 Two parts of zeolite filler (manufactured by Mizusawa Chemical Industry Co., Ltd., product name: Silton JC-20) of 1 mm and 30 parts of castor oil polyol A (manufactured by Toyokuni Oil Mills Co., Ltd., product name: HS 2G-270B) were added and stirred for 1 hour to obtain a polyol base material (S1) containing polyol (A) and filler (C).
[0066] (Examples 2 to 16, Comparative Examples 1 to 5) Polyol base (S2 to S21) Except for changing the blending formulation as shown in Table 2, the same procedure as in Example 1 was carried out to obtain polyol base materials (S2 to S21).
[0067] [Table 2]
[0068] The abbreviations in Table 2 are as follows: Castor oil: Manufactured by Toyokuni Oil Co., Ltd. Product name: Industrial No. 1 castor oil Castor oil-based polyol A: Toyokuni Oil Co., Ltd., product name: HS 2G-270B Acidic resin: Toyochem Co., Ltd., product name: NS-5 PPG2000: Polypropylene glycol with a molecular weight of approximately 2,000 (manufactured by ADEKA Corporation, product name: ADEKA Polyether P-2000) PPG4000 (3f): A triol having a molecular weight of about 4000, obtained by adding polypropylene glycol to a trifunctional alcohol (manufactured by Mitsui Chemicals, Inc., product name: Actocol T-4000) Zeolite: pH value 9, average particle size 2.0 x 10 -3 mm zeolite filler (manufactured by Mizusawa Chemical Industry Co., Ltd., product name: Shilton JC-20) Alumina 1: Alumina filler with a pH value of 8 and an average particle size of 0.105 mm (manufactured by Nippon Light Metal Co., Ltd., product name: SA11) Alumina 2: pH value 8, average particle size 3.4 x 10 -5 mm alumina filler (manufactured by CIK Nanotech Co., Ltd., product name: Nanotech Powder) Alumina 3: pH value 8, average particle size 2.0 x 10 -4 mm alumina filler (Showa Denko K.K., product name: Alnabeads CB-02P) Magnesium oxide: pH value 10, average particle size 5.4 x 10 -4 mm magnesium oxide filler (Kyowa Chemical Industry Co., Ltd., product name: Kyowamag MF30) Treated silica: pH value 11, silica (Mizukasil P-707) treated with aminosilane coupling agent (manufactured by Evonik Japan Co., Ltd., product name: DYNASYLAN AMMO) using the integral blend method. Talc: pH value 9, average particle size 5.0 x 10 -3 mm talc filler (product name: Microace L-1, manufactured by Nippon Talc Co., Ltd.) Silica: pH value 6, average particle size 4.0 x 10 -3 mm silica filler (Mizusawa Chemical Industry Co., Ltd., product name: Mizukasil P-707)
[0069] <Production of Polyisocyanate (B)> (Polyisocyanate (B1)) 50 parts of polypropylene glycol with a molecular weight of about 2,000, 10 parts of polyester polyol with a molecular weight of about 2,000 composed mainly of adipic acid and propylene glycol (manufactured by ADEKA CORPORATION, product name: ADEKA NEW ACE F7-67), 20 parts of 4,4'-diphenylmethane diisocyanate, and 20 parts of 2,4-diphenylmethane diisocyanate were charged into a reaction vessel. The mixture was heated at 80°C to 90°C for 3 hours while stirring under a nitrogen gas stream to carry out a urethane reaction, and polyisocyanate (B1), which is a polyurethane polyisocyanate resin with a number average molecular weight of 2,500 and isocyanato groups at both ends, was obtained.
[0070] (Polyisocyanate (B2)) 40 parts of polypropylene glycol with a molecular weight of about 2,000, 10 parts of polyester polyol with a molecular weight of about 2,000 mainly composed of adipic acid and propylene glycol (manufactured by Adeka Corporation, product name: Adeka New Ace F7-67), 20 parts of 4,4'-diphenylmethane diisocyanate, 20 parts of 2,4-diphenylmethane diisocyanate, and 10 parts of biuret of hexamethylene diisocyanate were charged into a reaction vessel. The mixture was heated at 80°C to 90°C for 3 hours while stirring under a nitrogen gas flow to carry out a urethane reaction, and polyisocyanate (B2), which is a polyurethane polyisocyanate resin with isocyanato groups at both ends and a number average molecular weight of 3,000, was obtained.
[0071] (Polyisocyanate (B3)) 50 parts of 4,4'-diphenylmethane diisocyanate and 50 parts of a biuret of hexamethylene diisocyanate were charged into a reaction vessel. The mixture was stirred under a nitrogen gas flow to obtain polyisocyanate (B3).
[0072] <Production of polyurethane adhesive> (Example 17) 100 parts of the polyol base (S1) was placed in a reaction vessel and dissolved by heating at 50°C to 70°C for 50 minutes while stirring under a nitrogen gas flow. Next, 100 parts of the polyisocyanate (B1) was mixed at 80°C to obtain a solvent-free polyurethane adhesive.
[0073] (Examples 18 to 34, Comparative Examples 6 to 10) Except for changing the blending composition of the polyol base resin and the polyisocyanate (B) to the contents shown in Table 3, the same procedure as in Example 17 was carried out to obtain a solvent-free polyurethane adhesive.
[0074] <Evaluation of polyol-based and polyurethane adhesives> The resulting polyol base and polyurethane adhesive were subjected to the following evaluations. The results are shown in Table 3.
[0075] [Confirmation of filler aggregates in polyol base] The obtained polyol base was placed in a transparent glass bottle with a diameter of 60 mm so that the liquid level was 70 mm, sealed, and then left to stand at room temperature for one month. After storage, the supernatant and the sediment at the bottom of the bottle were observed, and the degree of change in the supernatant and sediment compared to the state before storage was evaluated according to the following criteria. ◎: No supernatant or precipitate was observed (very good) ○: The thickness of the supernatant is less than 1 mm and the thickness of the sediment is less than 1 mm (good) △: The thickness of the supernatant is less than 3 mm and the thickness of the sediment is less than 3 mm (usable) ×: Either the thickness of the supernatant or the thickness of the sediment is 3 mm or more (not usable)
[0076] [Initial melt viscosity] Two minutes after mixing the polyurethane adhesive, the melt viscosity at 70°C was immediately measured using a Brookfield viscometer.
[0077] [Pot life] The polyurethane adhesive was mixed and then left at 40°C for 30 minutes, after which the melt viscosity at 70°C was measured in the same manner as above, and evaluated according to the following criteria. ◎: Melt viscosity is less than 4000 mPa·s (very good) ○: Melt viscosity is 4000 mPa·s or more and less than 6000 mPa·s (good) △: Melt viscosity is 6000 mPa·s or more and less than 8000 mPa·s (usable) ×: Melt viscosity is 8000 mPa s or more (not suitable for use)
[0078] [Laminated body production] A grid pattern of 10 cm x 10 cm squares arranged with blank areas of 2.5 cm width in between was printed on a 12 μm thick polyethylene terephthalate film (product name: E5100, manufactured by Toyobo Co., Ltd.) using printing ink (Rio Alpha R631 white, manufactured by Toyo Ink Co., Ltd.). The thickness of the printed layer was 1 μm. The adhesive thus obtained was then adjusted to 70°C and applied onto the printed layer of the laminate using a solventless test coater. The amount of adhesive applied was 2.0 g / m 2 It was decided. Next, a 25 μm thick aluminum-deposited non-oriented polypropylene (VMCPP) film was attached to the adhesive-coated surface. The obtained laminate was placed in a thermostatic chamber at 40° C. for 2 days to cure the adhesive. The obtained laminate was evaluated for coating appearance and adhesive strength as follows.
[0079] [Coating appearance (MD, TD)] The coating appearance of the obtained laminate was visually observed from the PET film side and evaluated according to the following criteria: The plain part extending parallel to the flow of the film (MD) and the plain part extending perpendicular to the flow of the film (TD). ◎: No orange peel pattern or small speckle pattern was observed in the 10cm x 2.5cm plain area in the MD direction and the 10cm x 2.5cm plain area in the TD direction (very good) ○: In the plain area of 10cm x 2.5cm in the MD direction and in the plain area of 10cm x 2.5cm in the TD direction, the number of orange peel patterns or small spot patterns is 1 or more but less than 10 (good) △: In the plain area of 10cm x 2.5cm in the MD direction and in the plain area of 10cm x 2.5cm in the TD direction, the number of orange peel patterns or small dot patterns is between 10 and 30 (usable). ×: In at least one of the 10cm x 2.5cm plain area in the MD direction and the 10cm x 2.5cm plain area in the TD direction, the number of orange peel patterns or small dot patterns is 30 or more (unusable)
[0080] [Adhesive strength] A test piece was cut from the laminate in the MD direction to a length of 300 mm and a width of 15 mm. Using an Instron tensile tester, the test piece was pulled at a peel rate of 300 mm / min to measure the T-type peel strength (N / 15 mm) between the PET and VMCPP. This test was carried out five times, and the average value was calculated and evaluated according to the following criteria. ◎: Peel strength is 1.3N / 15mm or more (very good) ○: Peel strength is 1.0N / 15mm or more, less than 1.3N / 15mm (good) △: Peel strength is 0.7N / 15mm or more and less than 1.0N / 15mm (usable) ×: Peel strength is less than 0.7N / 15mm (not suitable for use)
[0081] [Table 3]
[0082] As shown in Table 3, the polyurethane adhesive of the present invention had excellent stability and a good pot life, as the filler did not aggregate. Furthermore, the coated product using the polyurethane adhesive of the present invention had a good appearance with a plain pattern extending in the TD and MD, and had excellent laminate strength. This is due to the dispersion stabilization and high cohesive strength achieved by the interaction between the plant-derived polyol and the filler, as well as the improved wetting and spreading of the coating film due to the low viscosity achieved by the polyether polyol having a number average molecular weight in the range of 50 to 2,500.
Claims
1. A polyurethane adhesive comprising a polyol (A), a polyisocyanate (B), and a filler (C), the polyol (A) comprises a plant-derived polyol (a1) and a polyol (a2) including a structural unit derived from a polyether polyol having a number average molecular weight in the range of 50 to 2,500, the polyol (a2) being a polyether urethane polyol obtained by reacting a polyether polyol having a number average molecular weight in the range of 50 to 2,500 with a polyisocyanate; A polyurethane adhesive, wherein the filler (C) is a filler having a pH value of greater than 7 as measured in accordance with JIS K 5101.
2. The polyurethane adhesive according to claim 1, wherein the polyol (A) contains 20 to 70 mass% of structural units derived from the polyether polyol having a number average molecular weight in the range of 50 to 2,500.
3. The polyurethane adhesive according to claim 1 or 2, wherein the plant-derived polyol (a1) has an acid value in the range of 0.1 to 15 mg KOH / g.
4. the filler (C) contains at least one selected from the group consisting of aluminum hydroxide, zeolite, magnesium oxide, and an inorganic compound treated with a basic silane coupling agent; The average particle size of the filler is 1×10 -4 The polyurethane adhesive of any one of claims 1 to 3, which has a thickness in the range of 0.1 mm.
5. The polyurethane adhesive according to any one of claims 1 to 4, comprising the filler (C) in an amount of 0.1 to 3 mass% based on the total mass of the polyol (A) and the polyisocyanate (B).
6. The polyurethane adhesive according to any one of claims 1 to 5, having a melt viscosity at 70°C in the range of 50 to 3,000 mPa·s.
7. A polyurethane adhesive comprising a polyol base and a polyisocyanate (B), Contains a polyol (A) and a filler (C), the polyol (A) comprises a plant-derived polyol (a1) and a polyol (a2) including a structural unit derived from a polyether polyol having a number average molecular weight in the range of 50 to 2,500; the polyol (a2) is a polyether urethane polyol obtained by reacting a polyether polyol having a number average molecular weight in the range of 50 to 2,500 with a polyisocyanate; The polyol base, wherein the filler (C) is a filler having a pH value of more than 7 as measured in accordance with JIS K 5101.
8. A polyurethane adhesive comprising the polyol base agent according to claim 7 and a polyisocyanate (B).
9. A laminate comprising an adhesive layer of the polyurethane adhesive according to any one of claims 1 to 6 and claim 8 disposed between at least two substrates.
Citation Information
Patent Citations
High-strength two-component polyurethane corner glue and preparation method thereof
CN105255436A
Two-pack curable laminating adhesive composition and method for laminating
JP1996060131A
Reactive hot-melt adhesive composition
JP1996283691A
Roll cutter
JP2001162579A
Two-part curable solventless adhesive composition
JP2002249745A