Silver paste for forming internal electrodes of multilayer inductors

The silver paste formulation achieves high conductivity and printability by controlling silver powder surface area and binder resin content, along with minimal copper, addressing migration issues and enhancing film density.

JP7563177B2Active Publication Date: 2024-10-08SHOEI CHEM IND CO LTD
View PDF 14 Cites 0 Cited by

Patent Information

Application Number
JP2020562962
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2018-12-26
Filing Date
2019-11-28
Publication Date
2024-10-08
Estimated Expiration
2039-11-28

AI Technical Summary

Technical Problem

Conductive pastes containing metal powder face a trade-off between achieving high conductivity and good printability, with issues like migration and reduced metal content affecting film density and resistivity.

Method used

A silver paste formulation with controlled specific surface area of silver powder, optimal binder resin content, and minimal copper addition, achieving a dry film density of 7.50 g/cm³ or more, while maintaining excellent printability and migration resistance.

Benefits of technology

The silver paste provides high conductivity, dense film formation, and effective migration resistance, ensuring good printability and reducing short circuits.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007563177000004
    Figure 0007563177000004
  • Figure 0007563177000005
    Figure 0007563177000005
  • Figure 0007563177000006
    Figure 0007563177000006
Patent Text Reader

Abstract

A silver paste containing at least silver powder, a binder resin, and an organic solvent, wherein the specific surface area of ​​the silver powder is S BET (m 2 / g), and the content ratio of the binder resin to the silver powder is C BND (mass%), C BND / S BET is 2.0 to 3.4, the copper content of the silver powder is 10 to 5000 ppm by mass, and the dry film density of the silver paste is 7.50 g / cm 3 The silver paste is characterized by the above. According to the present invention, a silver paste containing a high concentration of powder and having excellent printability can be provided, and thereby a silver conductor film having a high filling rate and film density, high conductivity, and excellent migration resistance can be provided.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a sintered silver paste that contains silver powder and is used to form internal and external electrodes in ceramic electronic components such as multilayer ceramic capacitors, inductors, and actuators. [Background technology]

[0002] Conventionally, conductive pastes containing metal powders have been widely used to form internal and external electrodes of electronic components. One of the reasons for this is that, compared with conductive inks using organometallic compounds, conductive pastes containing metal powders can be used with various printing methods such as screen printing, offset printing, gravure printing, inkjet printing, dipping, dispensing, brushing, and spin coating, and can form thick films by a single coating and printing process, making them advantageous in terms of obtaining high conductivity.

[0003] In order to obtain high conductivity, it is preferable that the conductive paste contains a high content of metal powder, and it is also desirable that the coating film obtained by printing the paste is dense and high density. By using a high content of metal powder, reliable conduction can be obtained even in the formation of finer patterns in the future.

[0004] For example, Patent Document 1 (JP Patent Publication No. 2005-174824) discloses an invention that uses metal colloid particles instead of metal powder to obtain a highly dense and conductive film, and uses an organometallic compound in combination with this to fill the gaps between the metal colloid particles with the organometallic compound, thereby increasing the density.

[0005] However, since metal colloid particles and organometallic compounds contain a large amount of organic components, when these are used as the main conductive component, the content of the metal components is lower than that of pastes using metal powders, and therefore a conductor film with low resistivity cannot be obtained. Moreover, it is difficult to deal with the above-mentioned wide variety of printing methods, and if a large amount of binder resin or viscosity modifier is added to the paste to solve this problem, the metal ratio in the coating film will be further reduced.

[0006] On the other hand, when metal powder is used as the conductive component of the paste, a conductive film with low resistivity can be obtained if the content of the metal powder is high, but the higher the content of the metal powder, the worse the printability becomes. Therefore, in the case of silver paste, for example, the highest coating density described in Patent Document 2 is 5.4 g / cm. 3 The maximum coating density described in Patent Document 3 is 5.70 g / cm 3 In addition, Patent Document 4 describes a nickel paste with a dry film density of 6.2 g / cm. 3 Examples are disclosed.

[0007] As described above, when trying to obtain a dense coating film with high conductivity in a conductive paste, printability is sacrificed, and there is a trade-off between the two. Therefore, there is a demand for a conductive paste that can simultaneously achieve dense coating film formation and good printability.

[0008] There are known examples of using two types of silver powder with different particle sizes, large and small, to obtain a dense coating film (Patent Document 5 and Patent Document 6). However, a phenomenon called migration is known to occur, particularly in the case of silver paste that uses silver powder, and the more small-diameter silver powder (e.g., less than 0.5 μm) contained in the silver paste, the more likely migration is to occur.

[0009] Conventionally, various measures have been attempted to suppress migration, such as adding a migration inhibitor containing fluorine to silver paste (Patent Document 7) or adding a mixed powder, alloy powder, or compound powder containing the three elements of copper, tin, and manganese to silver powder (Patent Document 8). [Prior art documents] [Patent documents]

[0010] [Patent Document 1] JP 2005-174824 A [Patent Document 2] JP 2007-131950 A [Patent Document 3] JP 2008-192565 A [Patent Document 4] JP 2004-220807 A [Patent Document 5] JP 2003-280179 A [Patent Document 6] JP 2005-203304 A [Patent Document 7] JP 2014-197483 A [Patent Document 8] International Publication No. 2014 / 061765 DISCLOSURE OF THEINVENTION [Problem to be solved by the invention]

[0011] However, adding a large amount of components other than the silver powder as described above to the paste for the purpose of preventing migration is not preferable in terms of obtaining high electrical conductivity.

[0012] Therefore, the object of the present invention is to solve these problems. That is, the object of the present invention is to provide a silver paste containing a high concentration of silver powder and having excellent printability, and thereby to provide a silver conductor film having a high filling rate and film density, high conductivity, and excellent migration resistance. [Means for solving the problem]

[0013] As a result of intensive research to solve the above problems, the present inventors have discovered that even when a paste contains a high concentration of silver powder, a dense dry film can be obtained without sacrificing printability by controlling the specific surface area of ​​the silver powder and the solid component of the binder resin within a specific range, and that migration can be effectively suppressed by simply adding the minimum necessary amount of copper component to the silver powder, thereby completing the present invention. That is, the present invention (1) contains at least silver powder, a binder resin, and an organic solvent. For forming internal electrodes of multilayer inductors A silver paste comprising: The specific surface area of ​​the silver powder is S BET (m 2 / g), the content ratio of the binder resin to the silver powder is C BND (mass%), C BND / S BET The value of is 2.00 to 3.40, The copper content of the silver powder is 10 to 5000 ppm by mass, The dry film density of the silver paste is 7.50 g / cm 3 That is all, Characterized by For forming internal electrodes of multilayer inductors A silver paste is provided.

[0014] In the present invention (2), the dry film density is 7.60 g / cm 3 The above-mentioned (1) For forming internal electrodes of multilayer inductors A silver paste is provided.

[0015] The present invention (3) also relates to the C BND / S BET Either (1) or (2) above, characterized in that the value of For forming internal electrodes of multilayer inductors A silver paste is provided.

[0016] The present invention (4) provides the silver powder according to any one of (1) to (3), characterized in that the silver powder contains 30 to 500 ppm by mass of copper. For forming internal electrodes of multilayer inductorsA silver paste is provided.

[0017] In addition, the present invention (5) provides a silver powder content C relative to the silver paste. AG Any one of (1) to (4) is characterized in that For forming internal electrodes of multilayer inductors A silver paste is provided.

[0018] In addition, the present invention (6) provides a silver powder content C relative to the silver paste. AG The content of the composition (5) is 92.00 to 96.00 mass%. For forming internal electrodes of multilayer inductors A silver paste is provided.

[0019] In addition, the present invention (7) provides a method for producing a silver powder having a specific surface area S BET 0.10~0.30m 2 Any one of (1) to (6) is a powder having a molecular weight of 1 / g. For forming internal electrodes of multilayer inductors A silver paste is provided.

[0020] The present invention (8) is any one of (1) to (7), characterized in that, when the 10% value and the 50% value in the volume-based cumulative fraction of the silver powder in the laser diffraction particle size distribution measurement are D10 and D50, respectively, D10 is 1.00 to 3.00 μm and D50 is 3.00 to 7.00 μm. For forming internal electrodes of multilayer inductors A silver paste is provided.

[0021] The present invention (9) further comprises the method according to (8), wherein the D10 is 1.20 to 2.00 μm. For forming internal electrodes of multilayer inductors A silver paste is provided.

[0022] The present invention (10) is the method according to any one of (8) and (9), characterized in that the D50 is 3.90 to 5.00 μm. For forming internal electrodes of multilayer inductors A silver paste is provided.

[0023] In addition, the present invention ( 11) is used to form a conductor film by a heat treatment of 700° C. or less, For forming internal electrodes of multilayer inductors A silver paste is provided. Effect of the Invention

[0024] According to the present invention, it is possible to provide a silver paste that contains a high concentration of silver powder and has excellent printability, and thereby to provide a silver conductor film that has a high filling rate and film density, exhibits high conductivity, and has excellent migration resistance. [Brief description of the drawings]

[0025] [Figure 1] FIG. 2 is an external view of a laminated inductor. [Diagram 2] FIG. 2 is an exploded view of an element part of the laminated inductor. [Diagram 3] FIG. 2 is a simplified cross-sectional view taken along axis XX in FIG. 1. [Figure 4] FIG. 4 is a simplified enlarged view of a part of FIG. 3. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0026] The silver paste of the present invention contains at least silver powder, a binder resin, and an organic solvent, The specific surface area of ​​the silver powder is S BET (m 2 / g), the content ratio of the binder resin to the silver powder is C BND (mass%), C BND / S BET The value of is 2.00 to 3.40, The copper content of the silver powder is 10 to 5000 ppm by mass, The dry film density of the silver paste is 7.50 g / cm 3 That is all, This is a silver paste characterized by the above.

[0027] The silver paste of the present invention contains at least silver powder, a binder resin, and an organic solvent.

[0028] The silver powder according to the silver paste of the present invention, that is, the silver powder contained in the silver paste of the present invention, is not particularly limited in shape, particle size, production method, etc. as long as it can satisfy the requirements described below.

[0029] The copper content of the silver powder according to the silver paste of the present invention is 10 to 5000 mass ppm, preferably 30 to 500 mass ppm. When the copper content of the silver powder is in the above range, migration is unlikely to occur. On the other hand, if the copper content of the silver powder is less than the above range, migration is likely to occur. From the viewpoint of migration resistance, there is no upper limit to the copper content, but if it exceeds the above range, the resistivity increases. Therefore, in the present invention, the copper content of the silver powder is in the range of 10 to 5000 mass ppm. In this specification, the symbol "~" indicating a numerical range indicates a range including the numerical values ​​written before and after the symbol "~", unless otherwise specified. That is, for example, the expression "10 to 5000" is synonymous with "10 to 5000" unless otherwise specified.

[0030] The binder resin in the silver paste of the present invention is not particularly limited, and examples of the binder resin include those used in ordinary silver pastes. Examples of the binder resin include cellulose, acrylic resin, phenolic resin, epoxy resin, urethane resin, polyester resin, and polyethylene resin.

[0031] The organic solvent for the silver paste of the present invention is not particularly limited, and may be any organic solvent used in ordinary silver pastes. Examples of the organic solvent include alcohol-based, ether-based, ester-based, and hydrocarbon-based organic solvents, water, and mixed solvents thereof.

[0032] The specific surface area of ​​the silver powder is S BET (m 2 / g), and the content ratio of binder resin to silver powder is C BND (mass%) of the silver paste of the present invention. BND / S BETThe value of " is 2.00 to 3.40, preferably 2.50 to 3.10. BND / S BET When the value of C is in the above range, the silver content in the silver paste can be increased while maintaining good printability, and as a result, a conductive film having a high dry film density, denseness, and high conductivity can be obtained. BND / S BET If the value of C is less than the above range, the amount of binder resin covering the silver surface will be insufficient, which will impair the dispersibility of silver particles in the silver paste and reduce the strength of the dried film. For example, in the case of screen printing, this will result in poor screen removal and difficulty in maintaining the shape of the coating film after printing and drying. BND / S BET If the value of S exceeds the above range, a large amount of organic solvent will be used to maintain appropriate printability, and the silver content in the silver paste will decrease, resulting in a low dry film density and poor compactness and conductivity. BET (m 2 / g) is the specific surface area determined by the BET method in which helium gas is adsorbed on the surface of silver powder. BND (% by mass) is the content ratio (% by mass) of the binder resin relative to the silver powder obtained by the formula "(content of binder resin in silver paste / content of silver powder in silver paste) x 100".

[0033] The dry film density of the silver paste of the present invention is 7.50 g / cm 3 The lower limit of the dry film density of the silver paste of the present invention is preferably 7.60 g / cm. 3 , particularly preferably 7.80 g / cm 3 In addition, the upper limit of the dry film density of the silver paste of the present invention is preferably as high as possible as long as the printability is good. 3 ), and taking into consideration workability and productivity, a realistic limit is 8.50 g / cm 3The upper limit is about 15 mm. In addition, the method for controlling the dry film density can be controlled by a widely known general method, and examples of the method include adjusting the particle size distribution of the silver powder and its surface condition (smoothness, presence or absence of surface treatment, etc.), changing the binder resin or organic solvent used, or changing the type and amount of a dispersant added to the paste. In the present invention, the dry film density refers to the density of a dry film obtained by drying a coating film of the silver paste as it is without applying pressure. In the example described below, the silver paste to be measured is applied to a PET film with a thickness of about 150 μm, and then temporarily dried at 80 ° C. for 10 minutes, and then punched out with the PET film into a circular shape with a diameter of 15 mm. The PET film is further dried at 150 ° C. for 1 hour, and the PET film is peeled off. The mass W and volume V of the obtained dry film are measured to calculate W / V.

[0034] In the silver paste of the present invention, BND / S BET When the value of and the copper content in the silver powder satisfy the above-mentioned ranges, and the dry film density is within the above-mentioned range, a dense and highly conductive film can be obtained. As a result, the silver paste of the present invention can form a dense conductor film with low resistivity, while also providing a conductor film with excellent printability and coating film shape, and furthermore, excellent migration resistance and reduced occurrence of short circuits between conductor films. In the experimental examples described below, after the silver paste of the present invention is screen-printed on a substrate to be printed, the closer the contact angle (rectangularity) between the substrate and the coating film is to 90°, the more preferable the coating film shape (printing pattern) and the better the printability.

[0035] The higher the silver content in the silver paste, the more conductive the film can be obtained, but if the silver content is too high, the printability is reduced. AGis preferably 80.00 to 97.00 mass%, and particularly preferably 92.00 to 96.00 mass%, in that both electrical conductivity and printability can be increased. The silver content (mass%) in the silver paste is the content ratio of silver powder to the silver paste calculated by the formula "(silver powder content / silver paste mass)×100".

[0036] The specific surface area S of the silver powder in the silver paste of the present invention BET is 0.10~0.30m 2 / g. The specific surface area S BET 0.10~0.30m 2 / g, the content of small-diameter silver powder, which is prone to migration, is low, so short circuits between conductor films are more effectively suppressed. BET is particularly preferably 0.12 to 0.20 m 2 / g. The shape of the silver powder may be granular, flaky, or irregular, but is preferably spherical. In the present invention, the term "spherical" refers to a particle having an aspect ratio of 50 particles in a field of view observed with a SEM (scanning electron microscope) within the range of 1.0 to 1.5. In the present invention, it is particularly preferable that the aspect ratio is within the range of 1.0 to 1.3.

[0037] In addition, the silver powder in the silver paste of the present invention is preferably a silver powder having a D10 of 1.00 to 3.00 μm and a D50 of 3.00 to 7.00 μm, more preferably a silver powder having a D10 of 1.20 to 2.00 μm, and particularly preferably a silver powder having a D50 of 3.90 to 5.00 μm. When the D10 and D50 of the silver powder satisfy the above requirements, the dry film density is increased and the content of small-diameter silver powder that is prone to migration is reduced, so that short circuits between conductor films are more effectively suppressed.

[0038] In addition, the silver powder in the silver paste of the present invention is preferably a mixed powder in which two or more types of silver powders having different average particle sizes (D50) are mixed. By using a mixed powder made of two or more types of silver powders having different average particle sizes (D50), it becomes easier to obtain a conductor film with a high dry film density and a dense and highly conductive film.

[0039] The silver powder in the silver paste of the present invention is (a) a first silver powder having a D50 in the range of 3.50 to 7.50 μm, preferably 3.70 to 7.50 μm, and particularly preferably 4.00 to 6.00 μm; (b) a second silver powder having a D50 of 0.80 to 2.70 μm, which may be 0.80 to 2.00 μm, and preferably in the range of 0.80 to 1.80 μm; In this case, the specific surface area S BET The various physical quantities such as D50, D10, copper content, etc., of the mixed powder after mixing two or more types of silver powders may be within the above-mentioned numerical ranges. Note that, since the D10 value of the entire mixed powder is likely to decrease due to the second silver powder, it is preferable to use the second silver powder whose D10 is adjusted to 0.70 μm or more.

[0040] In the present invention, the method for producing silver powder is not particularly limited, but for example, the conventionally known atomization method, wet reduction method, CVD method, PVD method as described in Japanese Patent No. 3541939, spray pyrolysis method as described in Japanese Patent Publication No. 63-31522, and "method of pyrolyzing a pyrolytic metal-containing compound in a gas phase" as described in Japanese Patent No. 3812359 can be used to produce silver powder. Among them, the above-mentioned PVD method, spray pyrolysis method, or "method of pyrolyzing a pyrolytic metal-containing compound in a gas phase" is preferable in that it is easy to obtain silver powder that is spherical, highly crystalline, and has a uniform particle size.

[0041] In the silver paste of the present invention, the content ratio C of the binder resin to the silver powder is BDN is preferably 0.430 to 0.750 mass %, and particularly preferably 0.440 to 0.600 mass %.

[0042] The silver paste of the present invention can appropriately contain, as necessary, glass frit, inorganic compounds such as metal oxides, and additives that are typically used in silver pastes, such as plasticizers, viscosity adjusters, surfactants, dispersants, and oxidizers.

[0043] The silver paste of the present invention is produced in a conventional manner by kneading together silver powder, a binder resin, an organic solvent, and, where necessary, an inorganic oxide, an additive, and the like, and uniformly dispersing them to prepare a paste having a rheology suitable for screen printing and other printing methods.

[0044] The silver paste of the present invention is used for forming internal electrodes, external electrodes, and thick-film conductor circuits in electronic components such as multilayer ceramic capacitors, inductors, actuators, etc. In particular, the silver paste of the present invention is suitably used for forming internal electrodes of powder magnetic core materials, particularly multilayer inductors in which soft magnetic metal particles are used as the magnetic material.

[0045] In order to facilitate understanding of the "printability" in the present invention, a laminated inductor will be taken as an example for explanation below. Typically, a multilayer inductor 10 is composed of an element body 11, and a first external electrode 12 and a second external electrode 13 covering a pair of end faces of the element body 11, as shown in FIG.

[0046] As shown in FIG. 2, the element 11 is constructed by laminating magnetic layers A1 to A20 and internal electrode layers B1 to B17. The magnetic layers A1 to A20 are obtained by kneading core-shell type composite particles, in which the surfaces of soft magnetic iron alloy particles mainly composed of iron are covered with an insulating film made of resin or oxide film, together with an appropriate binder resin and organic solvent to prepare a magnetic paste, which is then formed into a sheet and dried. On the surfaces of the magnetic layers A3 to A19, the internal electrode layers B1 to B17 are formed in a predetermined pattern by a screen printing method. The silver paste of the present invention is used to form these internal electrode layers. One end of the internal electrode layer B1 is exposed on the end face of the magnetic layer A3 and is electrically connected to the external electrode 12, and one end of the internal electrode layer B17 is similarly electrically connected to the external electrode 13. The internal electrode layers B1 to B17 are electrically connected via through-hole electrodes C1 to C16 formed in the thickness direction of the magnetic layers A3 to A19, and the internal electrode layers B1 to B17 are configured in a coil shape in the lamination direction as a whole. When the internal electrode layers B1 to B17 are formed on the magnetic layers A3 to A19, it is preferable that a magnetic layer (not shown) having a shape capable of filling the step caused by the film thickness of the internal electrode layers B1 to B17 is further laminated on the magnetic layers A3 to A19. Then, the element body 11 in which the magnetic layers A1 to A20 and the internal electrode layers B1 to B17 are laminated is subjected to a thermocompression bonding process and sintered at about 700°C, and then external electrodes 11 and 12 are formed on a pair of ends thereof to form a laminated inductor. Here, the external electrodes may be formed using the silver paste of the present invention, or may be formed using a conductive paste mainly composed of nickel or copper.

[0047] The cross section of the laminated inductor of FIG. 1 manufactured in this manner along the XX axis is shown in FIG. 3, and a part of it is enlarged and shown in FIG. 4. Note that both FIG. 3 and FIG. 4 are simplified diagrams and do not necessarily match the contents and structure shown in FIG. 2, including the number of layers. As shown in FIG. 3, the cross section of the internal electrode layer is ideally desired to be rectangular. However, in reality, when the silver paste is applied and printed on the substrate, the viscosity and fluidity of the paste affect the cross section, so that the actual cross section of the internal electrode layer is usually approximately trapezoidal as shown in FIG. 4. To make this shape closer to a rectangle, it is necessary to obtain a paste with high fluidity when printing the paste and high viscosity immediately after printing. However, there are a great number of parameters that must be controlled in the paste, and they affect each other in a complex manner, so it is no exaggeration to say that there are no cases in which the expected results or characteristics are obtained.

[0048] As described above, in this specification, "printability" means not only that the composition exhibits appropriate fluidity when printed by screen printing, gravure printing or the like, but also that the composition quickly exhibits high viscosity after printing, resulting in a coating film (conductor film) that is closer to a rectangular shape.

[0049] The silver paste of the present invention is suitably used as a fired silver paste used to form internal electrodes and external electrodes in ceramic electronic components such as multilayer ceramic capacitors, inductors, actuators, etc. For example, the silver paste of the present invention is used to form a conductor film by heat treatment at 700° C. or less.

[0050] The present invention will be described below based on specific experimental examples, but the present invention is not limited to these. EXAMPLES

[0051] <Manufacturing of silver powder> First, silver powders 1 to 21 listed in Table 1 were prepared based on the spray pyrolysis method described in JP-B-63-31522. That is, for silver powders 6, 8, 13 to 17, and 19 to 21, the copper content in the obtained silver powder was the value listed in the silver powder overall column in Table 1, and the D10 and D50 values ​​were adjusted by spray pyrolysis of an aqueous solution in which silver salt and copper salt were weighed and dissolved, and the collected silver powder was classified. For silver powders 1 to 5, 7, 9 to 12, and 18, the copper content in the obtained silver powder was the value listed in the first silver powder or second silver powder column in Table 1, and the D10 and D50 values ​​were adjusted by spray pyrolysis of an aqueous solution in which silver salt and copper salt were weighed and dissolved, and the collected silver powder was classified. Then, the obtained first silver powder and second silver powder were mixed to obtain a mixed powder as a silver powder. For each silver powder, the 10% value (D10) and 50% value (D50) in the cumulative volume fraction were determined using a laser diffraction particle size distribution analyzer. In addition, the specific surface area (S BET The aspect ratios of 50 randomly selected silver powder particles were measured by SEM (scanning electron microscope) image observation, and the average value was calculated. The results are shown in Table 1.

[0052] [Table 1]

[0053] (Examples 1 to 13 and Comparative Examples 1 to 9) The silver powder shown in Table 1 is mixed with the silver powder shown in Table 2 at the content C AG and ethyl cellulose was added at the content C shown in Table 2. BND The remainder was terpineol (TPO), and these were kneaded to prepare silver paste samples a to u. Next, each of the silver paste samples a to u was applied to a PET film in an area of ​​20 mm x 20 mm x 151 μm, dried at 80°C for 10 minutes, punched out using a 15 mm diameter punch, and further dried at 150°C for 1 hour. Next, the mass W and volume V of the resulting dried film were measured, and the dry film density was calculated using the formula W / V. The results are shown in Table 2. The acceptable standard for dry film density was 7.50 g / cm. 3 That's all. Next, the silver paste sample was applied and printed onto a ceramic substrate in the shape of a rectangular parallelepiped measuring 60 mm x 0.6 mm x 40 μm, and fired at 650°C in an oxidizing atmosphere (air) to form a conductive film, after which the electrical resistance was measured using a four-terminal method to calculate the resistivity. The results are shown in Table 2. The pass standard for resistivity was set to 2.00 μΩ·cm or less, and preferably 1.90 μΩ·cm or less.

[0054] [Table 2] 1) Content of silver powder in silver paste: (silver powder / silver paste) x 100 2) Ethyl cellulose content relative to silver powder: (Ethyl cellulose / silver powder) x 100

[0055] (Examples 14 to 26, Comparative Examples 10 to 18) A rectangular parallelepiped pattern was formed by screen printing using the silver paste samples a to u obtained above on a magnetic layer with a thickness of 30 μm that had been prepared in advance, and a magnetic layer was printed to fill in the steps due to the thickness of the pattern. Three sets of these were stacked, and magnetic layers for covers were stacked on the top and bottom. Next, the stack was thermocompressed, degreased in an oxidizing atmosphere, and then fired at 650°C to obtain a laminate. Next, the printability was evaluated using the obtained laminate. Specifically, the laminate was cut as shown in Figure 4, the rectangularity of the cross section of the conductive film was observed, and the average value of the angle corresponding to θ in Figure 4 was measured. The results are shown in Table 3. The acceptable standard for printability was 55° or more, and preferably 65° or more. Further, 25 laminates were prepared in the same manner as above, and the short-circuit rate of the laminates was measured. Specifically, electrical resistance was measured between the top and middle layers and between the middle and bottom layers of the three conductive films in the laminate, and this was repeated for the 25 laminates prepared. The ratio of the number of times that electrical continuity occurred to the total number of measurements was taken as the short-circuit rate. The results are shown in Table 3. The pass standard for the short-circuit rate was set to 5% or less, and preferably 3% or less.

[0056] [Table 3]

Claims

1. A silver paste for forming an internal electrode of a laminated inductor, comprising at least silver powder, a binder resin, and an organic solvent, The specific surface area of ​​the silver powder is S BET (m 2 / g), and the content ratio of the binder resin to the silver powder is C BND (mass%), C BND / S BET is between 2.00 and 3.40; The copper content of the silver powder is 10 to 5000 ppm by mass, The dry film density of the silver paste is 7.50 g / cm 3 That is all, A silver paste for forming internal electrodes of multilayer inductors, characterized by:

2. The dry film density is 7.60 g / cm 3 2. The silver paste for forming an internal electrode of a laminated inductor according to claim 1,

3. Said C BND / S BET 3. The silver paste for forming an internal electrode of a laminated inductor according to claim 1, wherein the value of is 2.50 to 3.

10.

4. The silver paste for forming an internal electrode of a laminated inductor according to any one of claims 1 to 3, characterized in that the silver powder contains 30 to 500 ppm by mass of copper.

5. Content C of the silver powder relative to the silver paste AG The silver paste for forming an internal electrode of a laminated inductor according to any one of claims 1 to 4, characterized in that the content of the silver in the silver paste is 80.00 to 97.00 mass %.

6. Content C of the silver powder relative to the silver paste AG The silver paste for forming internal electrodes of a laminated inductor according to claim 5, characterized in that the content of the silver in the silver paste is 92.00 to 96.00 mass %.

7. The specific surface area S of the silver powder BET 0.10 to 0.30 m 2 7. The silver paste for forming an internal electrode of a laminated inductor according to claim 1, wherein the silver paste has a viscosity of 1000:1 or more.

8. When the 10% value and the 50% value in the volume-based cumulative fraction of the laser diffraction particle size distribution measurement of the silver powder are D10 and D50, respectively, D10 is 1.00 to 3.00 μm, and D50 is 3.00 to 7.00 μm. The silver paste for forming an internal electrode of the laminated inductor according to any one of claims 1 to 7.

9. The silver paste for forming an internal electrode of a laminated inductor according to claim 8, characterized in that the D10 is 1.20 to 2.00 μm.

10. The silver paste for forming an internal electrode of a laminated inductor according to claim 8 or 9, characterized in that the D50 is 3.90 to 5.00 μm.

11. The silver paste for forming an internal electrode of a laminated inductor according to any one of claims 1 to 10, which is used to form a conductor film by a heat treatment of 700°C or less.

Citation Information

Patent Citations

  • Manufacture of metallic powder

    JP1998102108A

  • Photosensitive silver paste and image display unit using the same

    JP2003280179A

  • Conductive paste composition and laminated ceramic capacitor using it

    JP2004220807A

  • Metal paste, and film forming method using same

    JP2005174824A

  • Mixed conductive powder

    JP2005203304A