Manufacturing method of biaxially oriented polypropylene film
A controlled biaxial stretching process with specific polypropylene resin composition enhances film rigidity and heat resistance, addressing the limitations of existing films by maintaining shape and reducing wrinkles during heat sealing.
Patent Information
- Application Number
- JP2021549126
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2020-03-24
- Filing Date
- 2021-03-22
- Publication Date
- 2024-10-08
- Estimated Expiration
- 2041-03-22
AI Technical Summary
Existing biaxially oriented polypropylene films lack sufficient rigidity and heat resistance, particularly at high temperatures, and tend to develop wrinkles during heat sealing, limiting their suitability for packaging applications.
A manufacturing method involving specific polypropylene resin composition and controlled biaxial stretching processes, including precise temperature and stretching ratios, to enhance film rigidity and heat resistance, ensuring minimal wrinkles and shape retention.
The method produces a biaxially oriented polypropylene film with high rigidity and heat resistance up to 150°C, maintaining shape and reducing wrinkles during heat sealing, suitable for packaging applications.
Smart Images

Figure 0007563386000001 
Figure 0007563386000002 
Figure 0007563386000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for producing a biaxially oriented polypropylene film having excellent rigidity and heat resistance. More specifically, the present invention relates to a method for producing a biaxially oriented polypropylene film that is suitable for use as a packaging bag because the film easily retains its shape when made into a packaging bag and has fewer wrinkles in the sealed portion when heat sealed. [Background technology]
[0002] Biaxially oriented polypropylene films are used for packaging and industrial applications because they are moisture-proof and have the necessary rigidity and heat resistance. In recent years, as the range of applications expands, higher performance is required, and in particular, improved rigidity is expected. In addition, due to environmental considerations, there is a demand for maintaining strength even when the volume is reduced (film thickness is reduced), but to achieve this, it is essential to significantly improve rigidity. As a means of improving rigidity, it is known that the crystallinity and melting point of polypropylene resin can be improved by improving the catalyst and process technology used during polymerization of polypropylene resin. However, despite these improvements, there has been no biaxially oriented polypropylene film with sufficient rigidity.
[0003] In the manufacturing process of biaxially oriented polypropylene film, a method has been proposed in which, after stretching in the width direction, the film is subjected to a first-stage heat treatment while relaxing at a temperature equal to or lower than that during width direction stretching, and then a second-stage heat treatment is performed at a temperature between the first-stage temperature and the width direction stretching temperature (see, for example, Patent Document 1, etc.), and a method in which, after width direction stretching, further stretching is performed in the longitudinal direction (see, for example, Patent Document 2, etc.). However, although the film described in Patent Document 2 has excellent rigidity, wrinkles tend to occur in the sealed portion after heat sealing, and it has poor heat resistance. In addition, the orientation of the film described in Patent Document 1 is low, and the rigidity is insufficient. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] International Publication No. WO2016 / 182003 [Patent Document 2] JP 2013-177645 A Summary of the Invention [Problem to be solved by the invention]
[0005] The object of the present invention is to solve the above-mentioned problems. That is, the present invention relates to a biaxially oriented polypropylene film having excellent film rigidity, and further to a method for producing a biaxially oriented polypropylene film having excellent film rigidity and heat resistance at a high temperature of 150° C. More specifically, the present invention aims to provide a method for producing a biaxially oriented polypropylene film that is easy to maintain the bag shape when made into a packaging bag, and has few wrinkles at the sealed portion and around it when heat-sealed. [Means for solving the problem]
[0006] As a result of intensive research by the inventors to achieve this object, they have found that the following manufacturing method can provide a biaxially oriented polypropylene film having excellent film rigidity, and further having excellent film rigidity and heat resistance at a temperature as high as 150°C. That is, the present invention is a method for producing a biaxially oriented polypropylene film, which includes, in order, a step of extruding a polypropylene resin composition containing a polypropylene resin having a mesopentad fraction of 97.0% or more to obtain an unstretched sheet, a step of stretching the unstretched sheet in the longitudinal direction, a preheating step of heating the longitudinally stretched film to a preheating temperature in the range of Tm to Tm+25°C, a step of stretching the preheated longitudinally stretched film by 10 times or more in the width direction at a temperature of Tm-10°C or more and less than the preheating temperature, a step of cooling the film at a temperature not higher than the width direction stretching temperature and at a temperature of Tm-80°C or more and Tm-15°C or less at the end of the width direction stretching, and a heat treatment step.
[0007] In this case, it is preferable that the polypropylene resin constituting the biaxially oriented polypropylene film has a crystallization temperature of 105° C. or higher and a melting point of 160° C. or higher.
[0008] In this case, it is preferable that the polypropylene resin constituting the biaxially oriented polypropylene film has a melt flow rate of 4.0 g / 10 min or more.
[0009] Furthermore, in this case, it is preferable that the amount of components having a molecular weight of 100,000 or less in the polypropylene resin constituting the biaxially oriented polypropylene film is 35% by mass or more. Effect of the Invention
[0010] By applying the method for producing a biaxially oriented polypropylene film of the present invention, it is possible to obtain a biaxially oriented polypropylene film that is suitable for use as a packaging bag because it has high rigidity and therefore is easy to maintain the shape of the bag when made into a packaging bag. Furthermore, it is possible to obtain a biaxially oriented polypropylene film that is suitable for use as a packaging bag because it has high rigidity and excellent heat resistance at a high temperature of 150°C and therefore is easy to maintain the shape of the bag when made into a packaging bag, and further because there are few wrinkles in the sealed portion when heat sealed. Furthermore, the biaxially oriented polypropylene film has excellent rigidity, and can maintain its strength even when the thickness of the film is reduced, and can be suitably used in applications requiring higher rigidity. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0011] The method for producing the biaxially oriented polypropylene film of the present invention will be described in more detail below.
[0012] The biaxially oriented polypropylene film obtained by the present invention is made of a polypropylene resin composition mainly composed of a polypropylene resin. Here, the term "main component" means that the proportion of the polypropylene resin in the polypropylene resin composition is 90% by mass or more, more preferably 93% by mass or more, even more preferably 95% by mass or more, and particularly preferably 97% by mass or more.
[0013] (Polypropylene resin) The polypropylene resin used in the present invention may be a polypropylene homopolymer or a copolymer with ethylene and / or an α-olefin having 4 or more carbon atoms. A propylene homopolymer that does not substantially contain ethylene and / or an α-olefin having 4 or more carbon atoms is preferred, and even if it contains ethylene and / or an α-olefin having 4 or more carbon atoms, the amount of the ethylene and / or α-olefin having 4 or more carbon atoms is preferably 1 mol% or less. The upper limit of the amount of the component is more preferably 0.5 mol%, further preferably 0.3 mol%, and particularly preferably 0.1 mol%. When it is within the above range, the crystallinity is likely to be improved. Examples of the α-olefin component having 4 or more carbon atoms that constitutes such a copolymer include 1-butene, 1-pentene, 3-methylpentene-1, 3-methylbutene-1, 1-hexene, 4-methylpentene-1, 5-ethylhexene-1, 1-octene, 1-decene, 1-dodecene, 1-tetradecene, 1-hexadecene, 1-heptadecene, 1-octadecene, and 1-eicosene. The polypropylene resin may be a homopolymer of two or more different kinds of polypropylene, a copolymer with ethylene and / or an α-olefin having 4 or more carbon atoms, or a mixture of these.
[0014] (stereoregularity) The mesopentad fraction ([mmmm]%), which is an index of stereoregularity of the polypropylene resin used in the present invention, is preferably within the range of 97.0 to 99.9%, more preferably within the range of 97.5 to 99.7%, even more preferably within the range of 98.0 to 99.5%, and particularly preferably within the range of 98.5 to 99.3%. If it is 97.0% or more, the crystallinity of the polypropylene resin is increased, and the melting point, crystallinity, and crystal orientation of the crystals in the film are improved, making it easier to obtain rigidity and heat resistance at high temperatures. If it is 99.9% or less, it is easier to reduce costs in terms of polypropylene production, and the film is less likely to break during film formation. It is more preferable that it is 99.5% or less. The mesopentad fraction is measured by the nuclear magnetic resonance method (the so-called NMR method). In order to set the mesopentad fraction of the polypropylene resin within the above-mentioned range, a method of washing the obtained polypropylene resin powder with a solvent such as n-heptane, a method of appropriately selecting a catalyst and / or a co-catalyst, and a method of appropriately selecting the components of the polypropylene resin composition are preferably adopted.
[0015] (Melting temperature) The lower limit of the melting temperature (Tm) measured by DSC of the polypropylene resin constituting the biaxially oriented polypropylene film of the present invention is preferably 160° C., more preferably 161° C., even more preferably 162° C., and still more preferably 163° C. When Tm is 160° C. or higher, rigidity and heat resistance at high temperatures are easily obtained. The upper limit of Tm is preferably 170° C., more preferably 169° C., even more preferably 168° C., still more preferably 167° C., and particularly preferably 166° C. If Tm is 170° C. or less, it is easy to suppress an increase in cost in terms of polypropylene production, and breakage during film formation is difficult. The melting temperature can also be further increased by blending a crystal nucleating agent with the above-mentioned polypropylene resin. Tm is the main endothermic peak temperature associated with melting, which is observed when 1 to 10 mg of a sample is packed into an aluminum pan and set in a differential scanning calorimeter (DSC), melted at 230°C for 5 minutes in a nitrogen atmosphere, cooled to 30°C at a scanning rate of -10°C / min, held for 5 minutes, and then heated again at a scanning rate of 10°C / min.
[0016] (crystallization temperature) The lower limit of the crystallization temperature (Tc) of the polypropylene resin constituting the biaxially oriented polypropylene film of the present invention, as measured by DSC, is 105° C., preferably 108° C., and more preferably 110° C. When Tc is 105° C. or higher, crystallization is likely to proceed during width direction stretching and the subsequent cooling step, and rigidity and heat resistance at high temperatures are likely to be obtained. The upper limit of Tc is preferably 135° C., more preferably 133° C., even more preferably 132° C., still more preferably 130° C., particularly preferably 128° C., and most preferably 127° C. If Tc is 135° C. or lower, it is difficult to increase the cost of polypropylene production, and the film is difficult to break during film formation. Tc is the main exothermic peak temperature observed when 1 to 10 mg of a sample is packed into an aluminum pan, set in a DSC, melted at 230°C for 5 minutes in a nitrogen atmosphere, and cooled to 30°C at a scanning rate of -10°C / min. The crystallization temperature can be further increased by adding a crystal nucleating agent to the polypropylene resin.
[0017] (Melt Flow Rate) The melt flow rate (MFR) of the polypropylene resin constituting the biaxially oriented polypropylene film of the present invention, when measured in accordance with JIS K 7210 (1995), condition M (230°C, 2.16 kgf), is preferably 4.0 to 30 g / 10 min, more preferably 4.5 to 25 g / 10 min, even more preferably 4.8 to 22 g / 10 min, particularly preferably 5.0 to 20 g / 10 min, and most preferably 6.0 to 20 g / 10 min. When the melt flow rate (MFR) of the polypropylene resin is 4.0 g / 10 min or more, a biaxially oriented polypropylene film having a low thermal shrinkage rate is easily obtained. Furthermore, when the melt flow rate (MFR) of the polypropylene resin is 30 g / 10 min or less, the film formability is easily maintained.
[0018] From the viewpoint of film properties, the lower limit of the melt flow rate (MFR) (230°C, 2.16 kgf) of the polypropylene resin constituting the film is preferably 5.0 g / 10 min, more preferably 5.5 g / 10 min, even more preferably 6.0 g / 10 min, particularly preferably 6.3 g / 10 min, and most preferably 6.5 g / 10 min. When the melt flow rate (MFR) of the polypropylene resin is 5.0 g / 10 min or more, the amount of low molecular weight components in the polypropylene resin constituting the film is large. Therefore, by adopting a width direction stretching process in the film production process described below, the oriented crystallization of the polypropylene resin is further promoted and the crystallinity of the film is more likely to be increased. In addition, the entanglement of polypropylene molecular chains in the amorphous portion is reduced, making it easier to increase heat resistance. In order to set the melt flow rate (MFR) of the polypropylene resin within the above range, a method of controlling the average molecular weight or molecular weight distribution of the polypropylene resin is preferably adopted.
[0019] That is, the lower limit of the amount of components having a molecular weight of 100,000 or less in the GPC cumulative curve of the polypropylene resin constituting the film of the present invention is preferably 35 mass%, more preferably 38 mass%, even more preferably 40 mass%, particularly preferably 41 mass%, and most preferably 42 mass%. The upper limit of the amount of components having a molecular weight of 100,000 or less in the GPC cumulative curve is preferably 65% by mass, more preferably 60% by mass, and even more preferably 58% by mass. When the amount of components having a molecular weight of 100,000 or less in the GPC cumulative curve is 65% by mass or less, the film strength is unlikely to decrease. In this case, if the polypropylene resin contains high molecular weight components with long relaxation times or long-chain branched components, the amount of components with a molecular weight of 100,000 or less contained in the polypropylene resin can be easily adjusted without significantly changing the overall viscosity, making it easier to improve film formability without significantly affecting rigidity or thermal shrinkage.
[0020] (molecular weight distribution) The polypropylene resin used in the present invention has a lower limit of mass average molecular weight (Mw) / number average molecular weight (Mn), which is an index of the breadth of the molecular weight distribution, of preferably 3.5, more preferably 4.0, even more preferably 4.5, and particularly preferably 5.0. The upper limit of Mw / Mn is preferably 30, more preferably 25, even more preferably 23, particularly preferably 21, and most preferably 20. Mw / Mn can be obtained by gel permeation chromatography (GPC). When Mw / Mn is within the above range, it is easy to increase the amount of components having a molecular weight of 100,000 or less.
[0021] The molecular weight distribution of polypropylene resin can be adjusted by polymerizing components of different molecular weights in a series of plants in multiple stages, blending components of different molecular weights offline in a kneader, polymerizing by blending catalysts with different performance, or using a catalyst that can achieve a desired molecular weight distribution. The shape of the molecular weight distribution obtained by GPC may be a gentle molecular weight distribution with a single peak in a GPC chart with the logarithm (logM) of molecular weight (M) on the horizontal axis and the differential distribution value (weight fraction per logM) on the vertical axis, or a molecular weight distribution with multiple peaks or shoulders.
[0022] (Method for producing biaxially oriented polypropylene film) The method for producing the biaxially oriented polypropylene film of the present invention is preferably to prepare an unstretched sheet made of a polypropylene resin composition containing the above-mentioned polypropylene resin as a main component, and to biaxially stretch the sheet. The biaxial stretching method may be any of the inflation simultaneous biaxial stretching method, the tenter simultaneous biaxial stretching method, and the tenter sequential biaxial stretching method, but it is preferable to adopt the tenter sequential biaxial stretching method from the viewpoint of film formation stability and thickness uniformity. It is particularly preferable to stretch in the longitudinal direction and then in the width direction, but a method in which stretching in the width direction and then in the longitudinal direction may also be used.
[0023] Next, the method for producing the biaxially oriented polypropylene film of the present invention will be described below, but is not necessarily limited thereto. The biaxially oriented polypropylene film obtained by the present invention may have a layer having another function laminated on at least one side. Lamination may be performed on one or both sides. In that case, the resin composition of the other layer or the central layer may be the polypropylene resin composition described above. It may also be different from the polypropylene resin composition described above. The number of layers to be laminated may be one, two, or three or more layers per side, but one or two layers are preferred from the viewpoint of production. As a lamination method, for example, coextrusion by a feed block method or a multi-manifold method is preferred. In particular, for the purpose of improving the processability of the biaxially oriented polypropylene film, a resin layer having heat sealability can be laminated within a range that does not deteriorate the properties. In addition, in order to impart printability, corona treatment can be performed on one or both sides.
[0024] In the following, an example of a single layer will be described in which a tenter sequential biaxial stretching method is adopted. First, a resin composition containing a polypropylene resin is heated and melted in a single-screw or twin-screw extruder, extruded into a sheet from a T-die, and cooled and solidified by being placed on a cooling roll. In order to promote solidification, it is preferable to further cool the sheet cooled by the cooling roll by immersing it in a water tank.
[0025] The sheet is then stretched in the longitudinal direction between two pairs of heated stretching rolls by increasing the rotation speed of the rear stretching roll, to obtain a uniaxially stretched film.
[0026] The uniaxially stretched film is then preheated, and stretched in the width direction at a specific temperature while holding the film ends in a tenter-type stretching machine to obtain a biaxially stretched film. This width direction stretching step will be described in detail later.
[0027] After the width direction stretching step is completed, the biaxially stretched film is heat-treated at a specific temperature to obtain a biaxially oriented film. In the heat treatment step, the film may be relaxed in the width direction.
[0028] The biaxially oriented polypropylene film thus obtained can be subjected to a corona discharge treatment on at least one side, if necessary, and then wound up on a winder to obtain a film roll.
[0029] Each step will be described in detail below. (Extrusion process) First, a polypropylene resin composition mainly composed of polypropylene resin is heated and melted in a range of 200°C to 300°C using a single-screw or twin-screw extruder, and the sheet-shaped molten polypropylene resin composition is extruded from a T-die and cooled and solidified by contacting it with a metal cooling roll. The obtained unstretched sheet is preferably further placed in a water tank. The temperature of the cooling roll, or the cooling roll and water bath, is preferably in the range of 10° C. to Tc, and when it is desired to increase the transparency of the film, it is preferable to cool and solidify the film with a cooling roll having a temperature in the range of 10 to 50° C. If the cooling temperature is 50° C. or less, the transparency of the unstretched sheet is likely to increase, and it is preferably 40° C. or less, and more preferably 30° C. or less. In order to increase the degree of crystal orientation after sequential biaxial stretching, it may be preferable to set the cooling temperature to 40° C. or more, but when a propylene homopolymer having a mesopent fraction of 97.0% or more is used as described above, it is preferable to set the cooling temperature to 40° C. or less in order to easily perform the stretching in the next step and to reduce thickness unevenness, and it is more preferable to set the cooling temperature to 30° C. or less. The thickness of the unstretched sheet is preferably 3500 μm or less in terms of cooling efficiency, more preferably 3000 μm or less, and can be appropriately adjusted depending on the film thickness after sequential biaxial stretching. The thickness of the unstretched sheet can be controlled by the extrusion speed of the polypropylene resin composition and the lip width of the T-die, etc.
[0030] (Longitudinal stretching process) The lower limit of the longitudinal stretching ratio is preferably 3 times, more preferably 3.5 times, and particularly preferably 3.8 times. Within the above range, strength is easily increased and thickness unevenness is reduced. The upper limit of the longitudinal stretching ratio is preferably 8 times, more preferably 7.5 times, and particularly preferably 7 times. Within the above range, width direction stretching is easily performed in the width direction stretching step, and productivity is improved. The lower limit of the longitudinal stretching temperature is preferably Tm-40°C, more preferably Tm-37°C, and even more preferably Tm-35°C. Within the above range, the subsequent width direction stretching becomes easy and thickness unevenness is reduced. The upper limit of the longitudinal stretching temperature is preferably Tm-7°C, more preferably Tm-10°C, and even more preferably Tm-12°C. Within the above range, the heat shrinkage rate is easily reduced, and there is little deterioration in quality due to adhesion to the stretching rolls making stretching difficult or increased surface roughness. The longitudinal stretching may be performed in two or more stages using three or more pairs of stretching rolls.
[0031] (Preheating process) Prior to the width direction stretching step, the uniaxially stretched film after the longitudinal stretching is heated in the range of Tm to Tm+25°C to soften the polypropylene resin composition. By setting the temperature at or above Tm, softening proceeds and width direction stretching becomes easier. By setting the temperature at or below Tm+25°C, orientation proceeds during transverse stretching and rigidity is easily developed. The temperature is more preferably Tm+2 to Tm+22°C, and particularly preferably Tm+3 to Tm+20°C. Here, the maximum temperature in the preheating step is defined as the preheating temperature.
[0032] (Width direction stretching process) In the transverse stretching step after the preheating step, a preferred method is as follows.
[0033] In the width direction stretching step, stretching is preferably performed at a temperature of Tm-10° C. or more and the preheating temperature or less. In this case, the start of width direction stretching may be when the preheating temperature is reached, or when the temperature is lowered after reaching the preheating temperature to a temperature lower than the preheating temperature. The lower limit of the temperature in the width direction stretching step is more preferably Tm-9° C., further preferably Tm-7° C., and particularly preferably Tm-5° C. When the width direction stretching temperature is within this range, the rigidity of the obtained biaxially oriented film is easily improved. The upper limit of the temperature in the width direction stretching step is preferably Tm+10° C., more preferably Tm+7° C., and particularly preferably Tm+5° C. When the width direction stretching temperature is within this range, stretching unevenness is unlikely to occur. Upon completion of the transverse stretching, i.e., immediately after the final transverse stretching ratio is reached, the film is cooled. The cooling temperature is preferably equal to or lower than the transverse stretching temperature, and is from Tm-80° C. to Tm-15° C., more preferably from Tm-80° C. to Tm-20° C., even more preferably from Tm-80° C. to Tm-30° C., and particularly preferably from Tm-70° C. to Tm-40° C. The temperature can be gradually lowered from the temperature at the end of the transverse stretching to the temperature at the time of cooling, or can be lowered stepwise or in one step. Lowering the temperature stepwise or in one step is preferred because it facilitates increasing the crystal orientation in the film.
[0034] The lower limit of the final width direction stretching ratio in the width direction stretching step is preferably 10 times, more preferably 11 times. If it is 10 times or more, the rigidity is easily increased and the film thickness unevenness is easily reduced. The upper limit of the width direction stretching ratio is preferably 20 times, more preferably 17 times, and even more preferably 15 times. If it is 20 times or less, the heat shrinkage rate is easily reduced and the film is less likely to break during stretching.
[0035] In this way, by using a highly crystalline polypropylene resin with high stereoregularity and a high melting point and adopting the above-mentioned width direction stretching process, the molecules of the polypropylene resin are highly aligned in the main orientation direction (which corresponds to the width direction in the above-mentioned width direction stretching process), and therefore, the crystal orientation in the obtained biaxially oriented film is strong and it is easy to produce more crystals with a high melting point. In addition, the orientation of the amorphous parts between the crystals is also increased in the main orientation direction (corresponding to the width direction in the width direction stretching process described above), resulting in high rigidity. In addition, since there are many crystals with high melting points around the amorphous parts, the stretched polypropylene molecules in the amorphous parts are less likely to relax at temperatures lower than the melting point of the crystals, and are more likely to maintain their tensed state. Therefore, the entire biaxially oriented film can maintain high rigidity even at high temperatures. It should also be noted that by adopting such a width direction stretching process, the heat shrinkage rate at a high temperature of 150° C. is also likely to be reduced. The reason for this is that since there is strong crystal orientation around the amorphous portion and there are more crystals with high melting points, the elongated polypropylene resin molecules in the amorphous portion are less likely to relax at a temperature lower than the melting point of the crystals. Furthermore, it is noteworthy that the orientation of the amorphous portion between the crystals is also increased in the main orientation direction (which corresponds to the width direction in the width direction stretching process described above), but since the orientation is not under extreme tension, the tensile breaking elongation is improved.
[0036] In addition, by increasing the low molecular weight component of the polypropylene resin, the crystallinity of the film is increased, and the entanglement of the polypropylene resin molecular chains in the amorphous portion is reduced, weakening the heat shrinkage stress and further reducing the heat shrinkage rate. Considering that in conventional technology, if either the strength or the heat shrinkage rate is improved, the other property tends to decrease, this is a groundbreaking development.
[0037] (Heat treatment process) If necessary, the biaxially stretched film can be heat-treated to further reduce the heat shrinkage. The upper limit of the heat treatment temperature is preferably Tm+10°C, more preferably Tm+7°C, and particularly preferably Tm+5°C. By setting the temperature at Tm+10°C or less, the rigidity is easily developed, the film surface does not become too rough, and the film is less likely to whiten. The lower limit of the heat treatment temperature is preferably Tm-5°C, more preferably Tm-2°C, and particularly preferably Tm°C. If it is less than Tm-5°C, the heat shrinkage may be high. By adopting the above-mentioned width direction stretching process, even if heat treatment is performed at a temperature between Tm-5°C and Tm+10, the highly oriented crystals generated in the stretching process are unlikely to melt, and the heat shrinkage rate can be reduced without decreasing the rigidity of the obtained film. In order to adjust the heat shrinkage rate, the film may be relaxed (relaxed) in the width direction during heat treatment, but the upper limit of the relaxation rate is preferably 4%. Within the above range, the film strength is unlikely to decrease and the film thickness fluctuation is likely to be small. It is more preferably 3%, even more preferably 2%, even more preferably 1%, and particularly preferably 0%.
[0038] (film thickness) The thickness of the biaxially oriented polypropylene film obtained by the present invention is set according to each application, but in order to obtain the strength of the film, the lower limit of the film thickness is preferably 2 μm, more preferably 3 μm, even more preferably 4 μm, particularly preferably 8 μm, and most preferably 10 μm. When the film thickness is 2 μm or more, the film is easily rigid. The upper limit of the film thickness is preferably 100 μm, more preferably 80 μm, even more preferably 60 μm, particularly preferably 50 μm, and most preferably 40 μm. When the film thickness is 100 μm or less, the cooling rate of the unstretched sheet during the extrusion process is unlikely to be reduced. The biaxially oriented polypropylene film obtained by the present invention is usually formed into a roll having a width of about 2000 to 12000 mm and a length of about 1000 to 50000 m, and wound into a film roll. It is further slit according to each application and provided as a slit roll having a width of about 300 to 2000 mm and a length of about 500 to 5000 m. The biaxially oriented polypropylene film of the present invention can be used to obtain a longer film roll.
[0039] (Thickness uniformity) The lower limit of the thickness uniformity of the biaxially oriented polypropylene film obtained by the present invention is preferably 0%, more preferably 0.1%, even more preferably 0.5%, and particularly preferably 1%. The upper limit of the thickness uniformity is preferably 20%, more preferably 17%, even more preferably 15%, particularly preferably 12%, and most preferably 10%. Within the above range, defects are unlikely to occur during post-processing such as coating and printing, and the film is easily used in applications requiring precision. The measurement method was as follows: A test piece 40 mm wide was cut out from a steady region where the film properties were stable in the length direction of the film, and the film thickness was measured continuously over 20,000 mm using a film feeder manufactured by Micron Measurement Instruments Co., Ltd. (product number: A90172) and a continuous film thickness measuring instrument manufactured by Anritsu Corporation (product name: K-313A wide-range high-sensitivity electronic micrometer), and the thickness uniformity was calculated using the following formula. Thickness uniformity (%) = [(maximum thickness value - minimum thickness value) / average thickness value] x 100
[0040] (Film characteristics) The biaxially oriented polypropylene film of the present invention is characterized by the following properties. Here, the "longitudinal direction" of the biaxially oriented polypropylene film of the present invention is the direction corresponding to the flow direction in the film manufacturing process, and the "width direction" is the direction perpendicular to the flow direction in the film manufacturing process. For polypropylene films whose flow direction in the film manufacturing process is unknown, wide-angle X-rays are incident perpendicularly to the film surface, and the scattering peaks originating from the (110) plane of the α-type crystals are scanned in the circumferential direction, and the direction with the largest diffraction intensity in the obtained diffraction intensity distribution is defined as the "longitudinal direction" and the direction perpendicular to that is defined as the "width direction."
[0041] (Heat shrinkage rate at 150℃) The upper limit of the heat shrinkage rate in the longitudinal direction of the biaxially oriented polypropylene film of the present invention at 150° C. is 10%, preferably 7.0%, more preferably 6.0%, even more preferably 5.0%, and particularly preferably 4.0% or less. The upper limit of the heat shrinkage rate in the transverse direction at 150° C. is preferably 30%, more preferably 24%, even more preferably 21%, and particularly preferably 18% or less. When the heat shrinkage rate in the longitudinal direction is 10% or less and the heat shrinkage rate in the transverse direction is 30% or less, wrinkles are unlikely to occur during heat sealing, and in particular, when the heat shrinkage rate in the longitudinal direction is 8.0% or less and the heat shrinkage rate in the transverse direction is 20% or less at 150°C, distortion when the zipper part is fused to the opening part is small, which is preferable. In order to reduce the heat shrinkage rate at 150°C, it is effective to set the lower limit of the amount of components with a molecular weight of 100,000 or less when measuring the gel permeation chromatography (GPC) integrated curve of the polypropylene resin constituting the film to 35% by mass, and to adjust the stretch ratio, stretching temperature, and heat setting temperature.
[0042] (23℃ tensile breaking strength) It is necessary that the heat shrinkage rate (%) in the width direction at 150° C. and the tensile breaking strength (MPa) in the width direction at 23° C. of the biaxially oriented polypropylene film of the present invention satisfy the following formulae. By satisfying the following formula, the rigidity is higher and the thermal shrinkage rate at high temperatures is smaller, so that when made into a packaging bag, the bag shape is more easily maintained and the film is less likely to deform during processing such as printing. Tensile strength (MPa) in the width direction at 23°C ≥ Heat shrinkage (%) in the width direction at 150°C x 6.2 + 300
[0043] The lower limit of the longitudinal tensile breaking strength of the biaxially oriented polypropylene film of the present invention at 23°C is preferably 90 MPa, more preferably 100 MPa, even more preferably 110 MPa, and particularly preferably 120 MPa. If it is 90 MPa or more, printing pitch deviation is unlikely to occur when transferring printing ink, and the durability of the packaging bag is likely to be excellent. The upper limit of the longitudinal tensile breaking strength is preferably 200 MPa as a practical value, more preferably 180 MPa, and even more preferably 160 MPa. If it is 200 MPa or less, film breakage and packaging bag breakage are likely to be reduced. The lower limit of the tensile breaking strength in the width direction of the biaxially oriented polypropylene film of the present invention at 23°C is preferably 380 MPa, more preferably 400 MPa, even more preferably 430 MPa, and particularly preferably 450 MPa. If it is 380 MPa or more, the printing pitch deviation is unlikely to occur when transferring the printing ink, and the durability of the packaging bag is likely to be excellent. The upper limit of the tensile breaking strength in the width direction is preferably 550 MPa as a practical value, more preferably 520 MPa, and even more preferably 500 MPa. If it is 550 MPa or less, the film breakage and the packaging bag breakage are likely to be reduced. In order to increase the tensile breaking strength, it is effective to set the lower limit of the amount of components with a molecular weight of 100,000 or less when measuring the gel permeation chromatography (GPC) cumulative curve of the polypropylene resin constituting the film to 35 mass%, and to adjust the stretching ratio, stretching temperature, and heat setting temperature.
[0044] The biaxially oriented polypropylene film of the present invention preferably has the following characteristics and structure. (Stress at 23℃ 5% elongation) The lower limit of the stress (F5) of the biaxially oriented polypropylene film of the present invention at 5% elongation in the longitudinal direction at 23° C. is preferably 40 MPa, more preferably 42 MPa, even more preferably 44 MPa, still more preferably 46 MPa, and particularly preferably 48 MPa. At 40 MPa or more, the film has high rigidity, so that the shape of the bag when made into a packaging bag is easily maintained, and deformation of the film is unlikely to occur during processing such as printing. The upper limit of F5 in the longitudinal direction is preferably 70 MPa, more preferably 65 MPa, further preferably 62 MPa, and particularly preferably 60 MPa. At 70 MPa or less, practical production becomes easy and the longitudinal-width balance tends to be improved. The lower limit of F5 in the width direction of the biaxially oriented polypropylene film of the present invention at 23° C. is preferably 160 MPa, more preferably 170 MPa, even more preferably 180 MPa, and particularly preferably 190 MPa. At 160 MPa or more, the film has high rigidity, so that the shape of the bag formed into a packaging bag is easily maintained, and deformation of the film is unlikely to occur during processing such as printing. The upper limit of F5 in the width direction is preferably 250 MPa, more preferably 230 MPa, and further preferably 220 MPa. If it is 250 MPa or less, practical production is easy and the longitudinal-width balance is easily improved. F5 can be kept within the range by adjusting the stretch ratio and relaxation rate, or by adjusting the temperature during film formation.
[0045] (23℃ tensile elongation at break) The lower limit of the longitudinal tensile elongation at break of the biaxially oriented polypropylene film of the present invention at 23°C is preferably 195%, more preferably 200%, more preferably 210%, and particularly preferably 220% or more. If it is 195% or more, film breakage and packaging bag breakage tend to be reduced. The upper limit of the longitudinal tensile elongation at break is preferably 300% as a practical value, and more preferably 280%.
[0046] The lower limit of the tensile elongation at break in the width direction of the biaxially oriented polypropylene film of the present invention at 23°C is preferably 25%, more preferably 30%, even more preferably 32%, and particularly preferably 35% or more. If it is 25% or more, film breakage and packaging bag breakage are likely to be reduced. The upper limit of the tensile elongation at break in the width direction is preferably 60%, more preferably 55%, and even more preferably 50%. If it is 60% or less, printing pitch deviation is unlikely to occur when transferring printing ink, and the durability of the packaging bag is likely to be excellent. The tensile elongation at break can be controlled within the range by adjusting the stretch ratio, stretching temperature, and heat setting temperature.
[0047] (Heat shrinkage rate at 120℃) The upper limit of the heat shrinkage rate in the longitudinal direction of the biaxially oriented polypropylene film of the present invention at 120°C is preferably 2.0%, more preferably 1.5%, even more preferably 1.2%, and particularly preferably 1.0%. If it is 2.0% or less, printing pitch deviation is unlikely to occur when transferring printing ink. The upper limit of the heat shrinkage rate in the transverse direction at 120°C is 5.0%, preferably 4.0%, more preferably 3.5%, and particularly preferably 2.5%. If it is 5.0% or less, wrinkles are unlikely to occur during heat sealing. If the longitudinal heat shrinkage rate at 120°C is smaller than the transverse heat shrinkage rate at 120°C, printing pitch deviation is less likely to occur when transferring printing ink. The thermal shrinkage rate at 120°C and the balance of the thermal shrinkage rates in the longitudinal and transverse directions can be kept within the range by adjusting the stretch ratio, stretching temperature, and heat setting temperature.
[0048] (Refractive Index) The lower limit of the refractive index (Nx) in the longitudinal direction of the biaxially oriented polypropylene film of the present invention is preferably 1.4950, more preferably 1.4970, and even more preferably 1.4980. If it is 1.4950 or more, the rigidity of the film is easily increased. The upper limit of the refractive index (Nx) in the longitudinal direction is preferably 1.5100, more preferably 1.5070, and even more preferably 1.5050. If it is 1.5100 or less, the film is likely to have an excellent balance of properties in the longitudinal direction and the width direction.
[0049] The lower limit of the refractive index (Ny) in the width direction of the biaxially oriented polypropylene film of the present invention is 1.5230, preferably 1.5235, and more preferably 1.5240. If it is 1.5230 or more, the rigidity of the film is easily increased. The upper limit of the refractive index (Ny) in the width direction is preferably 1.5280, more preferably 1.5275, and even more preferably 1.5270. If it is 1.5280 or less, the film is likely to have an excellent balance of properties in the longitudinal direction and the width direction.
[0050] The lower limit of the refractive index (Nz) in the thickness direction of the biaxially oriented polypropylene film of the present invention is preferably 1.4960, more preferably 14965, and even more preferably 1.4970. If it is 1.4960 or more, the rigidity of the film is easily increased. The upper limit of the refractive index (Nz) in the thickness direction is preferably 1.5020, more preferably 1.5015, and even more preferably 1.5010. If it is 1.5020 or less, the heat resistance of the film is easily increased. The refractive index can be adjusted within the range by adjusting the stretch ratio, stretching temperature, and heat setting temperature.
[0051] (△Ny) The lower limit of ΔNy of the biaxially oriented polypropylene film of the present invention is 0.0220, preferably 0.0225, more preferably 0.0228, and even more preferably 0.0230. If it is 0.0220 or more, the rigidity of the film tends to be high. The upper limit of ΔNy is preferably 0.0270 as a practical value, more preferably 0.0265, even more preferably 0.0262, and particularly preferably 0.0260. If it is 0.0270 or less, the thickness unevenness tends to be good. ΔNy can be kept within the range by adjusting the stretch ratio, stretching temperature, and heat setting temperature of the film. ΔNy is calculated by the following formula, where Nx, Ny, and Nz are the refractive indices along the length, width, and thickness directions of the film, respectively, and it means the degree of orientation in the width direction in the overall orientation of the film in the length, width, and thickness directions. △Ny=Ny-[(Nx+Nz) / 2]
[0052] (Face orientation coefficient) The lower limit of the plane orientation coefficient (ΔP) of the biaxially oriented polypropylene film of the present invention is preferably 0.0135, more preferably 0.0138, and even more preferably 0.0140. If it is 0.0135 or more, the balance in the plane direction of the film is good, and the thickness unevenness is also good. The upper limit of the plane orientation coefficient (ΔP) is preferably 0.0155 as a practical value, more preferably 0.0152, and even more preferably 0.0150. If it is 0.0155 or less, it is likely to have excellent heat resistance at high temperatures. The plane orientation coefficient (ΔP) can be within the range by adjusting the stretch ratio, stretching temperature, and heat setting temperature. The plane orientation coefficient (ΔP) was calculated using the formula: [(Nx+Ny) / 2]-Nz.
[0053] (Hayes) The upper limit of the haze of the biaxially oriented polypropylene film of the present invention is preferably 5.0%, more preferably 4.5%, even more preferably 4.0%, particularly preferably 3.5%, and most preferably 3.0%. If it is 5.0% or less, it is easy to use in applications where transparency is required. The lower limit of the haze is preferably 0.1% as a practical value, more preferably 0.2%, even more preferably 0.3%, and particularly preferably 0.4%. If it is 0.1% or more, it is easy to manufacture. The haze can be kept within the range by adjusting the cooling roll (CR) temperature, the width direction stretching temperature, the tenter preheating temperature before width direction stretching, the width direction stretching temperature, or the heat setting temperature, or the amount of the component having a molecular weight of 100,000 or less of the polypropylene resin, but it may become large by adding an antiblocking agent or providing a seal layer.
[0054] (Half-width of diffraction peak due to oriented crystals) In the azimuth angle dependence of the scattering peak of the (110) plane of the polypropylene α-type crystals obtained by wide-angle X-ray measurement perpendicular to the film surface of the biaxially oriented polypropylene film of the present invention, the upper limit of the half-width (Wh) of the diffraction peak derived from the oriented crystals in the width direction of the film is preferably 25°, more preferably 24°, more preferably 23°, and particularly preferably 22°. If the half-width (Wh) is 25° or less, the rigidity of the film is easily increased. The lower limit of Wh is preferably 16°, more preferably 17°, and even more preferably 18°.
[0055] (X-ray orientation degree) The lower limit of the degree of X-ray orientation of the biaxially oriented polypropylene film of the present invention calculated from Wh by the following formula is preferably 0.860, more preferably 0.867, and even more preferably 0.872. By making it 0.860 or more, it is easy to increase the rigidity. X-ray orientation = (180-Wh) / 180 The upper limit of the degree of X-ray orientation is preferably 0.911, more preferably 0.906, and further preferably 0.900. By setting it to 0.911 or less, film formation is likely to be stable.
[0056] (Practical properties of film) The practical properties of the biaxially oriented polypropylene film of the present invention will now be described.
[0057] (Wrinkles during heat sealing) To form a bag for packaging food, the contents are filled into a bag that has already been made, and the film is heated to melt and fuse and seal it. In addition, the same process is often used when making a bag while filling it with food. Usually, a sealant film made of polyethylene or polypropylene is laminated on the base film, and the sealant film surfaces are fused together. The heating method is to apply pressure from the base film side with a heating plate to hold down the film and seal it, and the seal width is often about 10 mm. At this time, the base film is also heated, and the shrinkage at that time causes wrinkles. In terms of bag durability, it is better to have fewer wrinkles, and it is also better to have fewer wrinkles to increase purchasing desire. The sealing temperature may be around 120°C, but a higher sealing temperature is required to increase the bag making processing speed, and even in that case, it is preferable that the shrinkage is small. When a zipper is fused to the opening of the bag, it is required to seal at an even higher temperature.
[0058] (Print pitch deviation) Packaging films are often basically made up of a laminated film of a printed base film and a sealant film. Bag making machines are used to manufacture bags, and various types of bags are used, including three-sided bags, standing bags, and gusset bags. Print pitch deviation is thought to occur because tension and heat are applied to the film during the printing process, causing the film base material to expand and contract. Eliminating defective products due to print pitch deviation is important in terms of efficient use of resources and increasing purchasing motivation.
[0059] (Film processing) Printing on the biaxially oriented polypropylene film of the present invention can be carried out by letterpress printing, lithographic printing, intaglio printing, stencil printing or transfer printing, depending on the application. Also, it can be used as a laminate with heat sealability by laminating an unstretched sheet, uniaxially stretched film, or biaxially stretched film made of low density polyethylene, linear low density polyethylene, ethylene-vinyl acetate copolymer, polypropylene, or polyester as a sealant film. When gas barrier properties or heat resistance is to be improved, an unstretched sheet, uniaxially stretched film, or biaxially stretched film made of aluminum foil, polyvinylidene chloride, nylon, ethylene-vinyl alcohol copolymer, or polyvinyl alcohol can be provided as an intermediate layer between the biaxially oriented polypropylene film and the sealant film. An adhesive applied by dry lamination or hot melt lamination can be used to laminate the sealant film. To improve the gas barrier properties, aluminum or inorganic oxides can be vapor-deposited onto the biaxially oriented polypropylene film, the intermediate layer film, or the sealant film. Vacuum deposition, sputtering, and ion plating can be used as the vapor deposition method, but vacuum deposition of silica, alumina, or a mixture thereof is particularly preferred.
[0060] The biaxially oriented polypropylene film of the present invention can be made suitable for packaging fresh produce such as vegetables, fruits, flowers, and other plants that require high freshness by containing an anti-fog agent, such as fatty acid esters of polyhydric alcohols, amines of higher fatty acids, amides of higher fatty acids, or ethylene oxide adducts of amines or amides of higher fatty acids, in an amount of 0.2 to 5 mass %.
[0061] In addition, various additives for improving qualities such as slipperiness and antistatic properties, for example, lubricants such as wax and metal soaps for improving productivity, plasticizers, processing aids, heat stabilizers, antioxidants, antistatic agents, ultraviolet absorbers, etc. can also be blended within a range that does not impair the effects of the present invention.
[0062] (Industrial Applicability) Since the biaxially oriented polypropylene film of the present invention has the above-mentioned excellent properties not available in the prior art, it can be preferably used for packaging bags, and the thickness of the film can be made thinner than in the prior art.
[0063] Furthermore, it is also suitable for applications that require high temperatures, such as insulating films for capacitors and motors, backsheets for solar cells, barrier films for inorganic oxides, and base films for transparent conductive films such as ITO, as well as applications that require rigidity, such as separate films. In addition, it is now possible to use coating agents, inks, and laminating adhesives that were previously difficult to use, enabling coating and printing processes at high temperatures, which is expected to improve production efficiency. EXAMPLES
[0064] The present invention will be described in detail below with reference to examples. The properties were measured and evaluated by the following methods. (1) Melt flow rate The melt flow rate (MFR) was measured in accordance with JIS K7210 at a temperature of 230° C. and a load of 2.16 kgf.
[0065] (2) Meso-pentad fraction The mesopentad fraction ([mmmm]%) of polypropylene resin was measured using 13C-NMR. The mesopentad fraction was calculated according to the method described in Zambelli et al., Macromolecules, Vol. 6, p. 925 (1973). 13C-NMR measurement was performed using AVANCE500 manufactured by BRUKER, by dissolving 200 mg of a sample in a mixture of o-dichlorobenzene and heavy benzene in a ratio of 8:2 at 135°C, and at 110°C.
[0066] (3) Number average molecular weight, weight average molecular weight, amount of components with molecular weights of 100,000 or less, and molecular weight distribution of polypropylene resin The molecular weight was determined by gel permeation chromatography (GPC) using monodisperse polystyrene as the standard in terms of PP. When the baseline was unclear, the baseline was set to the lowest point of the high molecular weight tail of the elution peak closest to the elution peak of the standard substance. The GPC measurement conditions are as follows. Equipment: HLC-8321PC / HT (Tosoh Corporation) Detector: RI Solvent: 1,2,4-trichlorobenzene + dibutylhydroxytoluene (0.05%) Column: TSK gelguard column HHR(30)HT(7.5mmI.D.×7.5cm)×1 + TSK gel GMHHR-H(20)HT(7.8mmI.D.×30cm)×3 Flow rate: 1.0mL / min Injection volume: 0.3mL Measurement temperature: 140℃ The number average molecular weight (Mn) and the mass average molecular weight (Mw) are respectively defined by the number of molecules (Ni) of the molecular weight (Mi) at each elution position of the GPC curve obtained via the molecular weight calibration curve, as follows: Number average molecular weight: Mn=Σ(Ni·Mi) / ΣNi Mass average molecular weight: Mw=Σ(Ni·Mi 2 ) / Σ(Ni·Mi) Here, the molecular weight distribution can be obtained by Mw / Mn. In addition, the proportion of components having a molecular weight of 100,000 or less was determined from the integral curve of the molecular weight distribution obtained by GPC.
[0067] (4) Crystallization temperature (Tc), melting temperature (Tm) Heat measurements were performed under nitrogen atmosphere using a TA Instruments Q1000 differential scanning calorimeter. Approximately 5 mg was cut out from the polypropylene resin pellets and sealed in an aluminum pan for measurement. The temperature was raised to 230°C and held for 5 minutes, then cooled to 30°C at a rate of -10°C / min, and the exothermic peak temperature was taken as the crystallization temperature (Tc). The heat of crystallization (△Hc) was calculated by setting a baseline so that the area of the exothermic peak was smoothly connected from the start of the peak to the end of the peak. The temperature was held at 30°C for 5 minutes, and then raised to 230°C at 10°C / min, and the main endothermic peak temperature was taken as the melting temperature (Tm).
[0068] (5) Film thickness The thickness of the films was measured using a Seiko EM Millitron 1202D.
[0069] (6) Hayes Measurement was performed at 23° C. in accordance with JIS K 7105 using NDH5000 manufactured by Nippon Denshoku Industries Co., Ltd.
[0070] (7) Tensile test The tensile strength of the film in the longitudinal and transverse directions was measured at 23°C according to JIS K 7127. Samples were cut out from the film to a size of 15 mm x 200 mm, and the chuck width was set to 100 mm in a tensile tester (Instron 5965 dual column tabletop tester manufactured by Instron Japan Co., Ltd.). The tensile test was performed at a tensile speed of 200 mm / min. From the obtained strain-stress curve, the stress at 5% elongation was defined as F5. The tensile breaking strength and tensile breaking elongation were defined as the strength and elongation, respectively, at the time when the sample broke.
[0071] (8) Heat shrinkage rate The measurement was performed according to the following method in accordance with JIS Z 1712. The film was cut into pieces of 20 mm width and 200 mm length in both the longitudinal and transverse directions of the film, and was heated for 5 minutes by hanging them in a hot air oven at 120°C or 150°C. The length after heating was measured, and the thermal shrinkage rate was calculated as the ratio of the shrunken length to the original length.
[0072] (9) Refractive index, △Ny, and plane orientation coefficient Measurements were made at a wavelength of 589.3 nm and a temperature of 23°C using an Abbe refractometer manufactured by Atago Co., Ltd. The refractive indices along the longitudinal and width directions of the film were designated Nx and Ny, respectively, and the refractive index along the thickness direction was designated Nz. ΔNy was calculated using Nx, Ny, and Nz using the formula Ny-[(Nx+Nz) / 2]. The plane orientation coefficient (ΔP) was calculated using the formula [(Nx+Ny) / 2]-Nz.
[0073] (10) X-ray half-width, degree of orientation The measurements were made using an X-ray diffractometer (Rigaku Corporation, RINT2500) by the transmission method. X-rays with a wavelength of 1.5418 Å were used, and a scintillation counter was used as the detector. The film was stacked to a thickness of 500 μm to prepare a sample. The sample stage was placed at the diffraction peak position (diffraction angle 2θ = 14.1°) of the (110) plane of the α-crystal of polypropylene resin, and the sample was rotated 360° around the axis in the thickness direction of the film to obtain the azimuth angle dependence of the diffraction intensity of the (110) plane. From this azimuth angle dependence, the half-width Wh of the diffraction peak resulting from the oriented crystals in the width direction of the film was obtained. In addition, the degree of X-ray orientation was calculated using Wh according to the following formula. X-ray orientation degree=(180-Wh) / 180
[0074] Example 1 The polypropylene resin used was a blend of 80 parts by weight of a propylene homopolymer PP-1 (Sumitomo Chemical Co., Ltd., Sumitomo Noblen FLX80E4) having an MFR of 7.5 g / 10 min, [mmmm] of 98.9%, Tc of 116.2°C, and Tm of 162.5°C, and 20 parts by weight of a propylene homopolymer PP-2 (Sumitomo Chemical Co., Ltd., EL80F5) having an MFR of 11 g / 10 min, [mmmm] of 98.8%, Tc of 116.5°C, and Tm of 161.5°C. The sheet was extruded from a T-die at 250°C into a sheet, brought into contact with a cooling roll at 20°C, and then placed in a water bath at 20°C. The sheet was then stretched 4.5 times in the longitudinal direction with two pairs of rolls at 142°C, then both ends were clamped with clips, introduced into a hot air oven, preheated at 170°C, and stretched 12 times in the width direction at 167°C as the first stage. Immediately after stretching in the width direction, the sheet was cooled at 100°C while still being held by the clips, and then heat-treated at 165°C without relaxation in the width direction. The thickness of the film thus obtained was 20.3 μm. The structure of the polypropylene resin is shown in Table 1, and the film-forming conditions are shown in Table 2. As for the physical properties, as shown in Table 3, a film with high rigidity and low thermal shrinkage at high temperatures was obtained.
[0075] Example 2 The same procedure as in Example 1 was carried out, except that the film was stretched in the width direction at 162°C and heat-treated at 170°C. The thickness of the obtained film was 20.8 μm. Table 1 shows the structure of the polypropylene resin, and Table 2 shows the film-forming conditions. As for the physical properties, as shown in Table 3, a film having high rigidity and low thermal shrinkage at high temperatures was obtained.
[0076] Example 3 The same procedure as in Example 1 was carried out, except that the stretching in the width direction was carried out at 162° C. The thickness of the obtained film was 20.7 μm. The structure of the polypropylene resin is shown in Table 1, and the film-forming conditions are shown in Table 2. As for the physical properties, as shown in Table 3, a film with high rigidity and low thermal shrinkage at high temperatures was obtained.
[0077] Example 4 The same procedure as in Example 1 was carried out, except that the film was stretched in the width direction at 162° C. and cooled to 140° C. The thickness of the obtained film was 20.6 μm. The structure of the polypropylene resin is shown in Table 1, and the film-forming conditions are shown in Table 2. As for the physical properties, as shown in Table 3, a film with high rigidity and low thermal shrinkage at high temperatures was obtained.
[0078] Comparative Example 1 As the polypropylene resin, propylene homopolymer PP-1 (Sumitomo Chemical Co., Ltd., Sumitomo Noblen FLX80E4) with MFR = 7.5g / 10min, [mmmm] = 98.9%, Tc = 116.2 ° C, Tm = 162.5 ° C was used. It was extruded into a sheet from a T-die at 250 ° C, brought into contact with a cooling roll at 20 ° C, and then put into a water bath at 20 ° C. as it is. Thereafter, it was stretched 4.5 times in the longitudinal direction with two pairs of rolls at 145 ° C, then both ends were clamped with clips, introduced into a hot air oven, preheated at 170 ° C, and then stretched 6 times in the width direction at 160 ° C as the first stage, and then stretched 1.36 times at 145 ° C as the second stage, for a total stretching of 8.2 times. Immediately after the width direction stretching, it was cooled at 100 ° C while being held by the clip, and then heat-set at 163 ° C. The thickness of the film thus obtained was 18.7 μm. The structure of the polypropylene resin is shown in Table 1, and the film-forming conditions are shown in Table 2. The first stage of the transverse stretching process was the early stage, and the second stage of the transverse stretching process was the late stage. As shown in Table 3, the physical properties of the film were poor, including the thermal shrinkage at 150°C.
[0079] Comparative Example 2 As the polypropylene resin, 80 parts by weight of PP-1 and 20 parts by weight of propylene homopolymer PP-2 (manufactured by Sumitomo Chemical Co., Ltd., EL80F5) having MFR=11g / 10min, [mmmm]=98.8%, Tc=116.5°C, and Tm=161.5°C were blended and used. The same procedure was followed as in Comparative Example 1, except that the longitudinal stretching temperature was 142°C, the first-stage widthwise stretching temperature was 162°C, and the heat setting temperature was 165°C. The thickness of the obtained film was 21.3 μm. The structure of the polypropylene resin is shown in Table 1, and the film-forming conditions are shown in Table 2. As for the physical properties, as shown in Table 3, the tensile breaking strength was poor.
[0080] Comparative Example 3 Except for providing 3% relaxation during heat setting, the same procedure as in Comparative Example 2 was carried out. The thickness of the obtained film was 21.1 μm. The structure of the polypropylene resin is shown in Table 1, and the film-forming conditions are shown in Table 2. As for the physical properties, as shown in Table 3, the tensile breaking strength was poor.
[0081] Comparative Example 4 The same procedure as in Comparative Example 2 was carried out, except that the stretching temperature in the longitudinal direction was 145° C., and the cooling temperature immediately after the stretching in the transverse direction was 140° C. The thickness of the obtained film was 18.9 μm. The structure of the polypropylene resin is shown in Table 1, and the film-forming conditions are shown in Table 2. As for the physical properties, as shown in Table 3, the tensile breaking strength was poor.
[0082] Comparative Example 5 The same procedure as in Comparative Example 2 was carried out except that after the width direction stretching, the film was not cooled but was heat-set at 165° C. while still being held by the clips. The thickness of the obtained film was 19.5 μm. The structure of the polypropylene resin is shown in Table 1, and the film-forming conditions are shown in Table 2. As for the physical properties, as shown in Table 3, the heat shrinkage rate at 150°C was poor.
[0083] Comparative Example 6 The same procedure as in Comparative Example 2 was carried out, except that the second-stage stretching temperature in the width direction was 155° C. The thickness of the film thus obtained was 20.3 μm. The structure of the polypropylene resin is shown in Table 1, and the film-forming conditions are shown in Table 2. As for the physical properties, as shown in Table 3, the tensile breaking strength was poor.
[0084] Comparative Example 7 Except for changing the longitudinal stretching ratio to 4.8 times, the same procedure as in Comparative Example 2 was carried out. The thickness of the obtained film was 19.1 μm. The structure of the polypropylene resin is shown in Table 1, and the film-forming conditions are shown in Table 2. As for the physical properties, as shown in Table 3, the tensile breaking strength was poor.
[0085] Comparative Example 8 The width direction stretching was performed in the same manner as in Comparative Example 2, except that the first-stage stretching ratio was 6.6 times and the second-stage stretching ratio was 1.5 times, resulting in a total stretching ratio of 9.9 times. The thickness of the obtained film was 20.1 μm. The structure of the polypropylene resin is shown in Table 1, and the film-forming conditions are shown in Table 2. As for the physical properties, as shown in Table 3, the tensile breaking strength was poor.
[0086] Comparative Example 9 PP-1 was used as the polypropylene resin, and the extrusion was performed at 250°C from a T-die into a sheet, contacted with a cooling roll at 20°C, and then directly put into a water tank at 20°C. The film was then stretched 4.5 times in the longitudinal direction at 143°C, and stretched 8.2 times in the transverse direction in a tenter with a preheating temperature of 170°C and a stretching temperature of 158°C, followed by heat setting at 168°C. The thickness of the obtained film was 18.6 μm. Table 1 shows the structure of the polypropylene resin, Table 2 shows the film-forming conditions, and Table 3 shows the physical properties. As shown in Table 3, the physical properties were poor in tensile breaking strength.
[0087] Comparative Example 10 The same procedure as in Comparative Example 9 was repeated, except that a blend of 80 parts by weight of PP-1 and 20 parts by weight of PP-2 was used as the polypropylene resin. The thickness of the obtained film was 20.0 μm. Table 1 shows the structure of the polypropylene resin, Table 2 shows the film-forming conditions, and Table 3 shows the physical properties. As shown in Table 3, the physical properties were poor in tensile breaking strength.
[0088] Comparative Example 11 As the polypropylene resin, PP-3 (manufactured by Japan Polypropylene Corporation, FL203D) with MFR=3g / 10min, [mmmm]=94.8%, Tc=117.2°C, and Tm=160.6°C was used. The sheet was extruded from a T-die at 250°C into a sheet, brought into contact with a cooling roll at 20°C, and then placed in a water tank at 20°C. The sheet was then stretched 4.5 times in the longitudinal direction at 135°C, and in the width direction stretching with a tenter, the preheating temperature was set to 166°C, and 6 times stretching was performed at 155°C as the first stage of stretching. The second stage stretching was performed at 139°C for a total of 8.2 times stretching. Immediately after the width direction stretching, the sheet was cooled at 95°C while being held by the clip, and then heat-treated at 158°C without relaxation in the width direction. The thickness of the obtained film was 19.2 μm. The structure of the polypropylene resin is shown in Table 1, the film-forming conditions are shown in Table 2, and the physical properties are shown in Table 3. As shown in Table 3, the physical properties were poor in terms of the heat shrinkage rate at 150°C.
[0089] Comparative Example 12 As a polypropylene raw material, PP-4 (Sumitomo Chemical Co., Ltd., FS2012) with MFR = 2.7g / 10min, [mmmm] = 98.7%, Tc = 114.7 ° C, Tm = 163.0 ° C was used. It was extruded into a sheet from a T-die at 250 ° C, brought into contact with a cooling roll at 20 ° C, and then put into a water tank at 20 ° C. as it is. Then, in the longitudinal direction, it was stretched 4.5 times at 145 ° C., and in the width direction stretching with a tenter, the preheating temperature was set to 170 ° C., and 6 times stretching was performed at 160 ° C. as the first stage of stretching. As the second stage stretching, it was stretched 1.36 times at 145 ° C., and a total of 8.2 times stretching was performed. Immediately after the width direction stretching, it was cooled at 100 ° C. while being held by the clip, and then heat treatment was performed at 163 ° C. without relaxation in the width direction. The thickness of the obtained film was 21.2 μm. The structure of the polypropylene resin is shown in Table 1, the film-forming conditions are shown in Table 2, and the physical properties are shown in Table 3. As shown in Table 3, the physical properties were poor in terms of the heat shrinkage rate at 150°C.
[0090] Comparative Example 13 PP-4 was used as the polypropylene resin. The polypropylene resin was extruded into a sheet from a T-die at 250°C, brought into contact with a cooling roll at 20°C, and then directly put into a water tank at 20°C. After that, the film was stretched 5.8 times in the longitudinal direction at 130°C, heated in a tenter at a preheating temperature of 167°C, and then stretched 8.6 times in the transverse direction at a stretching temperature of 161°C, and then heat-set at 130°C while applying 10% relaxation, and then heat-set in the second stage at 140°C. The thickness of the obtained film was 13.4 μm. Table 1 shows the structure of the polypropylene resin, Table 2 shows the film-forming conditions, and Table 3 shows the physical properties. As shown in Table 3, the physical properties were poor in terms of the heat shrinkage rate at 150°C.
[0091] (Comparative Example 14) The same procedure as in Example 1 was carried out, except that the film was stretched 8 times in the width direction at 162° C. and cooled to 140° C. The thickness of the obtained film was 19.7 μm. The structure of the polypropylene resin is shown in Table 1, and the film-forming conditions are shown in Table 2. As for the physical properties, as shown in Table 3, the tensile breaking strength was poor.
[0092] Comparative Example 15 The same procedure as in Example 1 was repeated, except that the film was stretched 8 times in the width direction at 162°C. The thickness of the obtained film was 20.1 µm. Table 1 shows the structure of the polypropylene resin, and Table 2 shows the film-forming conditions. As for the physical properties, as shown in Table 3, the tensile breaking strength was poor.
[0093] [Table 1]
[0094] [Table 2A]
[0095] [Table 2B]
[0096] [Table 3A]
[0097] [Table 3B]
Claims
1. The method for producing a biaxially oriented polypropylene film includes, in order, a step of obtaining an unstretched sheet by extruding a polypropylene resin composition containing a polypropylene resin having a mesopentad fraction of 97.0% or more and a melt flow rate of 4.0 g / 10 min or more, a step of stretching the unstretched sheet in the longitudinal direction, a step of preheating the longitudinally stretched film to a preheating temperature in the range of Tm to Tm+25°C, a step of stretching the preheated longitudinally stretched film by 10 times or more in the width direction at a temperature of Tm-10°C or more and not exceeding the preheating temperature, a step of cooling the film at a temperature not exceeding the width direction stretching temperature and at a temperature of Tm-80°C or more and not exceeding Tm-15°C, and a step of heat treatment.
2. 2. The method for producing a biaxially oriented polypropylene film according to claim 1, wherein the polypropylene resin constituting the biaxially oriented polypropylene film has a crystallization temperature of 105° C. or higher and a melting point of 160° C. or higher.
3. The method for producing a biaxially oriented polypropylene film according to any one of claims 1 to 3, wherein the amount of components of the polypropylene resin constituting the biaxially oriented polypropylene film having a molecular weight of 100,000 or less is 35% by mass or more.
Citation Information
Patent Citations
Biaxially oriented polypropylene film and method for producing the same
JP2013177645A
Biaxially oriented polypropylene film
JP2018141122A
Polypropylene film
WO2014024969A1
Biaxially oriented polypropylene film and method for producing same
WO2015072291A1
Polypropylene film, metal membrane layered film, and film capacitor, and method for manufacturing same
WO2016182003A1