Electrode or wiring, electrode pair, and method for manufacturing electrode or wiring

MXene-based electrodes and wiring solutions address ion migration issues in electronic components by combining MXene particles with metal particles and resin, ensuring high conductivity and preventing ion migration under humid conditions.

JP7563466B2Active Publication Date: 2024-10-08MURATA MFG CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2022550582
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2020-09-17
Filing Date
2021-09-15
Publication Date
2024-10-08
Estimated Expiration
2041-09-15

AI Technical Summary

Technical Problem

Existing electrodes and wiring in electronic components suffer from ion migration due to ionization of materials under high humidity, leading to defects such as short circuits, and previous solutions using inorganic and organic compounds compromise conductivity.

Method used

Incorporating particles of a layered material, known as MXene, with specific metal particles or sintered metal, and a resin, where the blending ratio of MXene is 0.1% to 20% by mass, to form electrodes or wiring that suppress ion migration while maintaining high conductivity.

Benefits of technology

The electrodes or wiring effectively prevent ion migration under humid conditions while retaining excellent conductivity, as demonstrated by the suppression of silver dendrite growth in electrode pairs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007563466000002
    Figure 0007563466000002
  • Figure 0007563466000003
    Figure 0007563466000003
  • Figure 0007563466000004
    Figure 0007563466000004
Patent Text Reader

Abstract

Provided are an electrode or wiring, an electrode pair, and a method for manufacturing the electrode or wiring. The electrode or wiring comprises: particles of a layered material including one or more layers; and metal particles or a sintered metal. The layers include a layer body represented by the following formula MmXn (wherein, M is at least one metal belonging to group 3, 4, 5, 6, or 7, X is a carbon atom, a nitrogen atom, or a combination thereof, n is 1-4, and m is greater than n and at most 5), and a modification or terminal T (T being at least one selected from the group consisting of a hydroxyl group, a fluorine atom, a chlorine atom, an oxygen atom, and a hydrogen atom) present on the surface of the layer body.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an electrode or wiring, an electrode pair, and a method for manufacturing an electrode or wiring. [Background technology]

[0002] In electronic components such as inductors, there is a problem that ion migration occurs due to ionization of the materials constituting the electronic components, moisture from the outside under high humidity, etc. When ion migration occurs, defects such as short circuits occur. For the purpose of suppressing defects caused by moisture from the outside, for example, Patent Document 1 discloses an inorganic anion exchanger and an epoxy resin composition for sealing electronic components using the same. In particular, it is disclosed that an inorganic anion exchanger with low hygroscopicity and excellent anion exchange performance can be obtained by treating and covering a specific hydrotalcite compound with a metal oxide. In addition, Patent Document 2 discloses that migration of electronic components and the like can be prevented by dissolving or uniformly dispersing an organic triazine compound in a specific polymer. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2005-1902 A [Patent Document 2] JP 2014-210732 A Summary of the Invention [Problem to be solved by the invention]

[0004] Incidentally, the electrodes or wiring constituting the electronic components are required to have high electrical conductivity as well as suppression of the ion migration. However, the inorganic compound shown in Patent Document 1 and the organic compound shown in Patent Document 2 are both insulating, and therefore the electrical conductivity decreases when they are incorporated into an electrode. The present invention has been made in view of the above circumstances, and its object is to provide an electrode or wiring, an electrode pair, and a method for manufacturing an electrode or wiring, which suppress ion migration under high humidity and have excellent electrical conductivity. [Means for solving the problem]

[0005] According to one aspect of the present invention, An electrode or wiring comprising particles of a layered material comprising one or more layers and metal particles or sintered metal, The layer comprises a compound having the following formula: M m X n (wherein M is at least one Group 3, 4, 5, 6, or 7 metal; X is a carbon atom, a nitrogen atom, or a combination thereof; n is 1 or more and 4 or less, m is greater than n and less than or equal to 5) and a modification or termination T (T is at least one selected from the group consisting of a hydroxyl group, a fluorine atom, a chlorine atom, an oxygen atom, and a hydrogen atom) present on the surface of the layer body.

[0006] According to another aspect of the present invention, An electrode pair having an anode and a cathode, At least one of the anode and the cathode is Particles of layered material including one or more layers and metal particles or sintered metal, The layer comprises a compound having the following formula: M m X n (wherein M is at least one Group 3, 4, 5, 6, or 7 metal; X is a carbon atom, a nitrogen atom, or a combination thereof; n is 1 to 4, m is greater than n and less than or equal to 5) and a modification or termination T (T is at least one selected from the group consisting of a hydroxyl group, a fluorine atom, a chlorine atom, an oxygen atom, and a hydrogen atom) present on the surface of the layer body.

[0007] According to another aspect of the present invention, (a1) preparing a mixture by kneading particles of a layered material comprising one or more layers, metal particles, and a resin, The layer comprises a compound having the following formula: M m X n (wherein M is at least one Group 3, 4, 5, 6, or 7 metal; X is a carbon atom, a nitrogen atom, or a combination thereof; n is 1 to 4, m is greater than n and less than or equal to 5) and a modification or termination T (T is at least one selected from the group consisting of a hydroxyl group, a fluorine atom, a chlorine atom, an oxygen atom, and a hydrogen atom) present on the surface of the layer body, A blending ratio of the layered material particles in the mixture is 0.1% by mass or more and 20% by mass or less with respect to the metal particles; and (b1) drying the mixture to obtain an electrode or wiring The present invention provides a method for manufacturing an electrode or wiring, comprising the steps of:

[0008] According to another aspect of the present invention, (a2) kneading a compound comprising particles of a layered material comprising one or more layers and metal particles to prepare a mixture, The layer comprises a compound having the following formula: M m X n (wherein M is at least one Group 3, 4, 5, 6, or 7 metal; X is a carbon atom, a nitrogen atom, or a combination thereof; n is 1 to 4, m is greater than n and less than or equal to 5) and a modification or termination T (T is at least one selected from the group consisting of a hydroxyl group, a fluorine atom, a chlorine atom, an oxygen atom, and a hydrogen atom) present on the surface of the layer body, a blending ratio of the layered material particles in the mixture is 0.1% by mass or more and 20% by mass or less with respect to the metal particles; (b2) molding the mixture and drying it to obtain a molded product; and (c) sintering the molded product at a sinterable temperature. The present invention provides a method for manufacturing an electrode or wiring, comprising the steps of: Effect of the Invention

[0009] According to the present invention, an electrode or wiring contains particles of a specified layered material (also referred to in this specification as "MXene") and metal particles or sintered metal, thereby providing an electrode or wiring containing MXene, suppressing ion migration even under high humidity conditions, and having excellent conductivity. Also, according to the present invention, the above electrode or wiring can be manufactured by kneading particles of a specified layered material (MXene particles), metal particles, and a resin to prepare a mixture, in which the compounding ratio of the particles of the layered material in the mixture is 0.1 mass % or more and 20 mass % or less relative to the metal particles, and drying the mixture. [Brief description of the drawings]

[0010] [Figure 1] FIG. 1 is a schematic cross-sectional view showing an electrode or wiring in one embodiment of the present invention. [Diagram 2] FIG. 4 is a schematic cross-sectional view showing an electrode or wiring in another embodiment of the present invention. [Diagram 3]FIG. 1 is a schematic cross-sectional view showing MXene, a layered material that can be used in a conductive composite material in one embodiment of the present invention. [Figure 4] FIG. 1 is a schematic diagram illustrating the mechanism of Ag ion migration. [Diagram 5] 11 is a photograph showing the results of ion migration evaluation in a comparative example. [Figure 6] 1 is a photograph showing the results of ion migration evaluation in an example. [Figure 7] 13 is a photograph showing the results of an ion migration evaluation of another comparative example. [Figure 8] 13 is a photograph showing the results of an ion migration evaluation of another example. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] (Embodiment 1: Electrode or Wiring) The electrode or wiring in an embodiment of the present invention contains particles of a specified layered material and metal particles or sintered metal, thereby making it possible to realize an electrode or wiring that suppresses ion migration even under high humidity conditions and has excellent conductivity.

[0012] Hereinafter, the electrodes and wiring in the embodiments of the present invention will be described in detail, but the electrodes and wiring of the present invention are not limited to such embodiments.

[0013] Referring to Fig. 1, one electrode or wiring of this embodiment is an electrode or wiring 20A formed of a composite material containing particles 10 of a predetermined layered material, metal particles 11A, and resin 12. Referring to Fig. 2, another electrode or wiring of this embodiment is an electrode or wiring 20B formed of a sintered body containing particles 10 of a predetermined layered material and sintered metal 11B. The composite material or sintered body is a material that is easy to form an electrode or wiring.

[0014] First, the particles of a predetermined layered material contained in both the electrode or wiring 20A and the electrode or wiring 20B will be described.

[0015] In this embodiment, the particles of the predetermined layered material are MXene (particles), and are defined as follows. A particle of layered material comprising one or more layers, the layers being represented by the following formula: M m X n where M is at least one group 3, 4, 5, 6, 7 metal and may include at least one selected from the group consisting of so-called early transition metals, such as Sc, Ti, Zr, Hf, V, Nb, Ta, Cr, Mo and Mn; X is a carbon atom, a nitrogen atom, or a combination thereof; n is 1 to 4, m is greater than n and less than or equal to 5) and a modification or termination T (T is at least one selected from the group consisting of a hydroxyl group, a fluorine atom, a chlorine atom, an oxygen atom, and a hydrogen atom) present on a surface of the layer body (more specifically, on at least one of the two opposing surfaces of the layer body). m X n T x ", where x is any number, and z or s may be used instead of x in the past. Typically, n can be 1, 2, 3 or 4.

[0016] In the above formula for MXene, M is preferably at least one selected from the group consisting of Ti, Zr, Hf, V, Nb, Ta, Cr, Mo, and Mn, and more preferably at least one selected from the group consisting of Ti, V, Cr, and Mo.

[0017] In the above formula of MXene, M is more preferably Ti, and X is a carbon atom, or a carbon atom and a nitrogen atom. As the layer body, at least one selected from the group consisting of Ti3C2, Ti3CN, and Ti2C is even more preferably, and the above Ti3C2 is particularly preferable. By using MXene having such a layer body, high electrical conductivity can be ensured.

[0018] Such MXenes can be synthesized by selectively etching (removing and optionally phase-separating) the A atoms (and optionally some of the M atoms) from the MAX phase. The MAX phase has the following formula: M m AX n (wherein M, X, n and m are as defined above, and A is at least one Group 12, 13, 14, 15, 16 element, usually a Group A element, typically Group IIIA and Group IVA, and more particularly may include at least one element selected from the group consisting of Al, Ga, In, Tl, Si, Ge, Sn, Pb, P, As, S and Cd, and is preferably Al). and M m X n (each X may have a crystal lattice in which it is located in the octahedral array of M) between which a layer composed of A atoms is located. In the MAX phase, typically when m=n+1, one layer of X atoms is arranged between each of the n+1 layers of M atoms (collectively referred to as "M m X n The MAX phase has a repeating unit in which a layer of A atoms (also referred to as an "A layer") is arranged as a layer next to the n+1th layer of M atoms, but is not limited thereto. The A atoms (and sometimes a part of the M atoms) are selectively etched (removed and sometimes layer separated) from the MAX phase, thereby removing the A atom layer (and sometimes a part of the M atoms) to expose the M m X n The surface of the layer is modified with hydroxyl groups, fluorine atoms, chlorine atoms, oxygen atoms, hydrogen atoms, etc. present in the etching solution (usually, an aqueous solution of fluorine-containing acid is used, but is not limited to this) to terminate the surface.- For example, a method using a mixture of lithium fluoride and hydrochloric acid, a method using hydrofluoric acid, etc. Thereafter, layer separation of MXene (delamination, separation of multi-layer MXene into single-layer MXene) may be promoted by any appropriate post-treatment (e.g., ultrasonic treatment, hand shaking, etc.).

[0019] MXene is a compound represented by the above formula: m X n However, it is known that it can be expressed as follows: Sc2C, Ti2C, Ti2N, Zr2C, Zr2N, Hf2C, Hf2N, V2C, V2N, Nb2C, Ta2C, Cr2C, Cr2N, Mo2C, Mo 1.3 C, Cr 1.3 C, (Ti,V)2C, (Ti,Nb)2C, W2C, W 1.3 C, Mo2N, Nb 1.3 C, Mo 1.3 Y 0.6 C (in the above formula, "1.3" and "0.6" mean approximately 1.3 (= 4 / 3) and approximately 0.6 (= 2 / 3), respectively), Ti3C2, Ti3N2, Ti3(CN), Zr3C2, (Ti,V)3C2, (Ti2Nb)C2, (Ti2Ta)C2, (Ti2Mn)C2, Hf3C2, (Hf2V)C2, (Hf2Mn)C2, (V2Ti)C2, (Cr2Ti)C2, (Cr2V)C 2, (Cr2Nb)C2, (Cr2Ta)C2, (Mo2Sc)C2, (Mo2Ti)C2, (Mo2Zr)C2, (Mo2Hf)C2, (Mo2V)C2, (Mo2Nb)C2, (Mo2Ta)C2, (W2Ti)C2, (W2Zr)C2, (W2Hf)C2, Ti4N3, V4C3, Nb4C3, Ta4C3, (Ti,Nb)4C3, (Nb,Zr)4C3, (Ti2Nb2)C3, (Ti2Ta2)C3, (V2Ti2)C3, (V2Nb2)C3, (V2Ta2)C3, (Nb2Ta2)C3, (Cr2Ti2)C3, (Cr2V 2)C3, (Cr2Nb2)C3, (Cr2Ta2)C3, (Mo2Ti2)C3, (Mo2Zr2)C3, (Mo2Hf2)C3, (Mo2V2)C3, (Mo2Nb2)C3, (Mo2Ta2)C3, (W2Ti2)C3, (W2Zr2)C3, (W2Hf2)C3, (Mo 2.7 V 1.3 ) C3 (In the above formula, "2.7" and "1.3" mean approximately 2.7 (= 8 / 3) and approximately 1.3 (= 4 / 3), respectively.)

[0020] Typically, in the above formula, M can be titanium or vanadium, and X can be a carbon atom or a nitrogen atom. For example, the MAX phase is Ti3AlC2, and MXene is Ti3C2T x (In other words, M is Ti, X is C, n is 2, and m is 3).

[0021] In the present invention, MXene may contain a relatively small amount of residual A atoms, for example, 10 mass % or less of the original A atoms. The amount of residual A atoms may be preferably 8 mass % or less, more preferably 6 mass % or less. However, even if the amount of residual A atoms exceeds 10 mass %, there may be cases where there is no problem depending on the application and use conditions of the paste (and the conductive film obtained thereby).

[0022] The MXene (particle) 10 thus synthesized may be a layered material comprising one or more MXene layers 7a, 7b, as shown diagrammatically in FIG. 3 (examples of MXene (particle) 10 include, but are not limited to, one layer of MXene 10a in FIG. 3(a) and two layers of MXene 10b in FIG. 3(b)). More specifically, the MXene layers 7a, 7b may be formed of M m X n The layer body (M m Xn The MXene layers 7a and 7b have the following structures: (1) a, 1b of the layer bodies 1a and 1b; and (2) modifications or terminations T3a, 5a, 3b, 5b present on the surfaces of the layer bodies 1a and 1b (more specifically, on at least one of the two surfaces facing each other in each layer). m X n T x ", where x is any number. MXene10 may be one in which such MXene layers are individually separated and exist as one layer (single layer structure shown in FIG. 3(a), so-called single layer MXene10a), a laminate in which a plurality of MXene layers are stacked at a distance from each other (multilayer structure shown in FIG. 3(b), so-called multilayer MXene10b), or a mixture thereof. MXene10 may be particles (which may also be called powder or flakes) as an aggregate composed of single layer MXene10a and / or multilayer MXene10b. In this embodiment, MXene10 is preferably a particle (which may also be called nanosheet) the majority of which is composed of single layer MXene10a. In the case of multilayer MXene, two adjacent MXene layers (e.g. 7a and 7b) do not necessarily have to be completely separated, and may be partially in contact.

[0023] Without being limiting to this embodiment, the thickness of each MXene layer (corresponding to the above-mentioned MXene layers 7a and 7b) is, for example, 0.8 nm to 5 nm, particularly 0.8 nm to 3 nm (which may vary mainly depending on the number of M atomic layers contained in each layer), and the maximum dimension in a plane parallel to the layer (two-dimensional sheet surface) is, for example, 0.1 μm to 200 μm, particularly 1 μm to 40 μm. When the MXene is a laminate (multilayer MXene), for each laminate, the interlayer distance (or gap dimension, shown as Δd in Figure 3(b)) is, for example, 0.8 nm or more and 10 nm or less, particularly 0.8 nm or more and 5 nm or less, more particularly about 1 nm; the total number of layers may be 2 or more, but is, for example, 50 to 100,000, particularly 1,000 to 20,000; the thickness in the stacking direction is, for example, 0.1 μm or more and 200 μm or less, particularly 1 μm or more and 40 μm or less; and the maximum dimension in a plane perpendicular to the stacking direction (two-dimensional sheet surface) is, for example, 0.1 μm or more and 100 μm or less, particularly 1 μm or more and 20 μm or less. These dimensions are determined as number-average dimensions (e.g., number-average of at least 40 particles) based on scanning electron microscope (SEM), transmission electron microscope (TEM) or atomic force microscope (AFM) photographs, or as distances in real space calculated from the position in reciprocal space of the (002) plane measured by X-ray diffraction (XRD).

[0024] The type of metal constituting the metal particles 11A or the sintered metal 11B is not particularly limited. The electrode or wiring of this embodiment may contain one or more elements selected from the group consisting of Ag, Sn, Pt, Ni, Cu, Au and Zn as the metal particles 11A or the sintered metal 11B. These elements are elements that may cause ion migration. When these elements are contained, especially when Ag is contained, the ion migration suppression effect is fully exerted. When the metal particles 11A or the sintered metal 11B are formed of one or more elements selected from the group consisting of Ag, Sn, Pt, Ni, Cu, Au and Zn, especially when formed of Ag, the ion migration suppression effect is fully exerted.

[0025] The size of the metal particles 11A is not particularly limited, but it is preferable that the average particle size (D50) measured by a laser diffraction / scattering method is in the range of 0.1 μm or more and 100 μm or less.

[0026] The particle content of the layered material containing one or more layers is preferably 0.1% by mass or more and 20% by mass or less with respect to the metal particles or sintered metal. By setting the particle content of the layered material to 0.1% by mass or more with respect to the metal particles or sintered metal, the ion migration suppression effect is more effectively exhibited, which is preferable. The above content is more preferably 1% by mass or more, and even more preferably 3% by mass or more. On the other hand, from the viewpoint of ease of processing into electrodes or wiring and ensuring conductivity, the above content is preferably 20% by mass or less, more preferably 15% by mass or less, and even more preferably 10% by mass or less.

[0027] The resin 12 in the electrode or wiring 20A is not limited, and may be a thermosetting resin or a thermoplastic resin, for example, an acrylic resin, a fluororesin such as polytetrafluoroethylene, a vinyl resin such as polyvinyl chloride, an epoxy resin, a polyurethane, a melamine resin, a phenolic resin, a polyester such as polyethylene terephthalate, a polyamide, a polyether, etc.

[0028] The proportion of resin in the composite material constituting the electrode or wiring 20A is preferably greater than 0 mass%, and more preferably 2 mass% or more, in order to function as a binder, while from the viewpoint of ensuring electrical conductivity, it is preferably 25 mass% or less, and more preferably 12 mass% or less.

[0029] The "electrodes" include internal electrodes, external electrodes, pad electrodes, wiring-like electrodes, ground (reference potential) electrodes, shield patterns, etc. in electronic components and circuit boards, which may cause the above-mentioned ion migration failure. The "wiring" includes signal lines, coil patterns, interlayer connection conductors (via conductors), etc. that form circuit patterns.

[0030] The above-mentioned ion migration may occur, depending on the atmosphere such as humidity, when the distance between the electrodes is more than 0 mm, for example, 6 mm or less, and when the distance between the wires is more than 0 mm, for example, 1 mm or less. Liquid may be present between these electrodes and wires. That is, the above-mentioned electrodes and wires may be present in liquid, or in the atmosphere where a small amount of liquid is present. Examples of the atmosphere where a small amount of liquid is present include a case where the humidity in the atmosphere is high, and a case where liquid sweat is present on the surface of a person's skin. The electrodes or wires of this embodiment can more effectively suppress ion migration in the atmosphere where a small amount of liquid is present.

[0031] (Embodiment 2: Electrode Pair) The electrode pair in the embodiment of the present invention uses an electrode according to the embodiment of the present invention as at least one of the anode and cathode, thereby making it possible to effectively suppress ion migration even under high humidity conditions and to realize an electrode pair with excellent conductivity.

[0032] In particular, the electrode pair in the embodiment of the present invention is An electrode pair having an anode and a cathode, At least one of the anode and the cathode is Particles of layered material including one or more layers and metal particles or sintered metal, The layer comprises a compound having the following formula: M m X n (wherein M is at least one Group 3, 4, 5, 6, or 7 metal; X is a carbon atom, a nitrogen atom, or a combination thereof; n is 1 or more and 4 or less, m is greater than n and less than or equal to 5) and a modification or termination T (T is at least one selected from the group consisting of a hydroxyl group, a fluorine atom, a chlorine atom, an oxygen atom and a hydrogen atom) present on the surface of the layer body.

[0033] At least one of the anode and the cathode may contain one or more elements selected from the group consisting of Ag, Sn, Pt, Ni, Cu, Au and Zn. These elements are elements that may cause ion migration. When these elements are contained, especially when Ag is contained, the ion migration suppression effect is fully exerted. When at least one of the anode and the cathode is formed of one or more elements selected from the group consisting of Ag, Sn, Pt, Ni, Cu, Au and Zn, especially when it is formed of Ag, the ion migration suppression effect is fully exerted. When at least one of the anode and the cathode contains MXene particles, the metal particles or sintered metal contained therein is not particularly limited. Therefore, the metal particles or sintered metal that can be contained in the anode and the cathode may be the same or different.

[0034] For example, Ag ion migration is considered to occur as shown in FIG. 4. That is, as shown in FIG. 4A, Ag ions, which are metal ions, migrate from the anode 31 to the anode 31. + As shown in Figure 4B, Ag + moves between the electrodes from the anode (positive electrode) 31 to the cathode (negative electrode) 33. The arrow 35 indicates the direction of the electric field. Then, as shown in C in FIG. 4, the metal ions Ag + arrives at the cathode 33 and precipitates as metallic Ag 37. During precipitation, the shielding effect makes it easier for precipitation to occur at the tips of the branches, as shown in D in Fig. 4. As electrons are supplied from the cathode, the crystals grow into branches, as shown in E in Fig. 4, and as the branches grow, precipitation may also occur midway along the branches, as shown in F in Fig. 4.

[0035] In the electrode pair of this embodiment, as shown in A in Fig. 4, MXene prevents the metal at the anode (positive electrode) from losing electrons and changing into the above-mentioned metal ions, so metal ions that cause ion migration are not generated and ion migration is suppressed. This is thought to be because electrons are removed from MXene instead of the metal, that is, MXene functions as a reducing agent.

[0036] In the electrode pair of this embodiment, as shown in C in Fig. 4, MXene prevents metal ions that have migrated to the cathode (negative electrode) 33 from receiving electrons, so that metal (metal Ag 37 in Fig. 4) does not precipitate at the cathode 33, and ion migration is suppressed. This is thought to be because MXene receives electrons instead of metal ions, i.e., functions as an oxidizing agent.

[0037] The reason why ion migration is suppressed in the electrode pair of this embodiment is not limited to the above, and other mechanisms, such as preventing metal ions from migrating from the anode to the cathode, may also be considered.

[0038] MXene, a two-dimensional layered compound, is characterized by high electrical conductivity and also has redox activity (donation and receipt of electrons). This redox activity is thought to be effective in suppressing ion migration.

[0039] Therefore, it is preferable that at least one of the electrodes constituting the anode and the cathode of an electrode pair having an anode and a cathode contains the above-mentioned MXene.

[0040] The distance between the anode and the cathode may be more than 0 μm, for example, 6 mm or less, depending on the atmosphere such as humidity, as a mode in which the ion migration may occur. The anode and the cathode may be present in a liquid or in the atmosphere where a small amount of liquid is present. Examples of the atmosphere where a small amount of liquid is present include a case where the humidity in the atmosphere is high and a case where sweat, which is liquid, is present on the surface of a person's skin. The electrode or wiring of this embodiment can more effectively suppress ion migration in the atmosphere where a small amount of liquid is present.

[0041] (Embodiment 3: Method for manufacturing electrodes or wiring) Hereinafter, a method for producing an electrode or wiring according to an embodiment of the present invention will be described in detail, but the present invention is not limited to such an embodiment.

[0042] The manufacturing method (first manufacturing method) of one electrode or wiring of this embodiment is as follows: (a1) preparing a mixture by kneading particles of a predetermined layered material, metal particles, and a resin, the blending ratio of the particles of the layered material in the mixture being 0.1% by mass or more and 20% by mass or less with respect to the metal particles; and (b1) drying the mixture to obtain an electrode or wiring Includes.

[0043] Another method for manufacturing an electrode or wiring (second manufacturing method) of this embodiment is as follows: (a2) preparing a mixture by kneading a compound containing particles of a predetermined layered material and metal particles, wherein the compounding ratio of the particles of the layered material in the mixture is 0.1% by mass or more and 20% by mass or less with respect to the metal particles; (b2) molding the mixture and drying it to obtain a molded product; and (c) sintering the molded product at a sinterable temperature. Each step of the first and second production methods will be described in detail below.

[0044] Step (a1) of the first manufacturing method The particles of a predetermined layered material, i.e., the particles of a layered material including one or more layers, are the particles described in the above embodiment 1. The metal particles and resin can also be the materials described in the above embodiment 1. A metal paste in which the metal particles and resin are mixed in advance can be used as the metal particles and resin.

[0045] The blending ratio of the layered material particles in the mixture is set to 0.1% by mass or more and 20% by mass or less with respect to the metal particles. The reasons for setting the upper and lower limit values ​​and the preferred upper and lower limit values ​​are as described in the first embodiment.

[0046] The kneading method is not particularly limited, and examples thereof include stirring with a centrifugal stirrer, kneading with a three-roll mill, and dispersion treatment. If the fluidity is reduced during the kneading, an organic solvent that can be removed in a subsequent drying step, such as diethylene glycol monobutyl ether acetate used in the examples, may be added.

[0047] Step (b1) of the first manufacturing method The mixture is dried to obtain an electrode or wiring. The mixture can be molded into a molded product having the shape of an electrode or wiring before drying, but the molding method is not particularly limited. For example, the mixture may be applied to an object to be coated such as a substrate. The application method is not limited, and examples thereof include a method of spray coating using a nozzle such as a one-fluid nozzle, a two-fluid nozzle, or an airbrush, a method of slit coating using a table coater, a comma coater, or a bar coater, a screen printing method, a metal mask printing method, a spin coating method, a dip coating method, and a drip coating method. The above-mentioned object to be coated may be appropriately selected from a printed circuit board, a metal substrate, a resin substrate, a laminated electronic component, a metal pin, a metal wire, or the like, depending on the application.

[0048] The drying conditions vary depending on the shape and size of the molded mixture, but may be, for example, at a temperature of 60° C. to 200° C. for 10 minutes to 120 minutes.

[0049] The above coating and drying steps may be repeated multiple times as necessary until a film of the desired thickness is obtained.

[0050] Step (a2) of the second manufacturing method The particles of the predetermined layered material, i.e., the particles of the layered material containing one or more layers, are the particles described in the first embodiment. The metal particles may also be the materials described in the first embodiment. The metal particles may be metal particles having an average particle size (D50) of 1 nm or more and 200 μm or less, as measured by a laser diffraction / scattering method, for example. The mixture may contain a binder that can be removed by firing in a later step, so as to facilitate kneading.

[0051] The blending ratio of the layered material particles in the mixture is set to 0.1% by mass or more and 20% by mass or less with respect to the metal particles. The reasons for setting the upper and lower limit values ​​of the blending ratio and the preferred upper and lower limit values ​​are as described in the first embodiment.

[0052] The method of kneading is not particularly limited, and for example, a method of mixing and dispersing using a three-roll mill can be mentioned.

[0053] Step (b2) of the second manufacturing method The mixture is molded and dried to obtain a molded product. The molding method is not particularly limited, and molding may be performed by applying the mixture to an object to be coated such as a substrate. The coating method is not limited, and examples thereof include a method of spray coating using a nozzle such as a one-fluid nozzle, a two-fluid nozzle, or an airbrush, a method of slit coating using a table coater, a comma coater, or a bar coater, a screen printing method, a metal mask printing method, a spin coating method, a dip coating method, and a drip coating method. The above-mentioned object to be coated may be appropriately selected from a printed circuit board, a metal substrate, a resin substrate, a laminated electronic component, a metal pin, a metal wire, or the like, depending on the application.

[0054] The drying conditions vary depending on the shape and size of the molded product, but may be, for example, within the range of 60° C. to 200° C., and for 10 minutes to 120 minutes.

[0055] Step (c) of the second manufacturing method The molded product is sintered at a sinterable temperature. The sinterable temperature may be determined according to the metal type, for example, within a range of approximately 150°C or higher and 800°C or lower. The sintering time may be determined according to the shape and size of the molded product. The atmosphere during sintering is not particularly limited. For the purpose of removing the binder, etc., the atmosphere during sintering may be appropriately adjusted to an inert atmosphere, an oxidizing atmosphere, or a reducing atmosphere.

[0056] Although the electrodes or wiring, electrode pairs, and methods for manufacturing the electrodes or wiring in the embodiments of the present invention have been described in detail above, various modifications are possible. Note that the electrodes or wiring of the present invention may be manufactured by a method different from the manufacturing method in the above-mentioned embodiments. EXAMPLES

[0057] [Example 1] Preparation of MAX particles TiC powder, Ti powder, and Al powder (all manufactured by Kojundo Chemical Laboratory Co., Ltd.) were mixed in a 2:1:1 molar ratio in a ball mill containing zirconia balls for 24 hours. The mixed powder was sintered at 1350°C for 2 hours in an Ar atmosphere. The sintered body (block-shaped MAX phase) obtained in this way was pulverized with an end mill to a maximum dimension of 40 μm or less. As a result, Ti3AlC2 particles were obtained as MAX particles.

[0058] Preparation of MXene clay and MXene powder 1 g of Ti3AlC2 particles (powder) prepared by the above method was weighed out, and added to 10 mL of 9 mol / L hydrochloric acid together with 1 g of LiF, and stirred with a stirrer at 35°C for 24 hours to obtain a solid-liquid mixture (suspension) containing solid components derived from Ti3AlC2 powder. This was washed with pure water and the supernatant was separated and removed by decantation using a centrifuge (the remaining sediment after removing the supernatant was washed again) about 10 times, and a clay-like substance (clay) was obtained as the sediment. As a result, Ti3C2T was obtained as MXene clay. x A water-dispersed clay was obtained. The water-dispersed clay was freeze-dried and pulverized using an IKA mill to obtain MXene powder.

[0059] The above MXene powder was mixed with Ag paste (manufactured by Taiyo Ink, product name: ELEPASTE TR70901, containing 10% to 20% copolymer resin as resin) at 7% by mass (when dry) relative to the metal particles, and stirred for 90 seconds at 9000 rpm using a centrifugal stirrer. If the viscosity became too high and the fluidity was lost, a solvent (diethylene glycol monobutyl ether acetate) was added as appropriate.

[0060] The Ag paste containing MXene was then dispersed using a three-roll mill at a rotation speed of 230 rpm. The dispersion conditions were to pass the mixture through rolls with a gap of 50 μm twice, then through rolls with a gap of 20 μm twice, and finally through rolls with a gap of 10 μm twice to obtain a paste of the mixture.

[0061] Using a metal mask and a rubber squeegee, the paste of the mixture was hand-printed on two substrates, respectively, to obtain a pair of opposing electrodes, an anode and a cathode, spaced 1 mm apart. The molded product was dried at 140°C for 30 minutes to obtain a pair of opposing electrodes, an anode and a cathode, as a sample for ion migration evaluation. A total of two samples for ion migration evaluation were prepared by the same manufacturing method. In this example, the paste of the mixture containing MXene was printed on both the anode and the cathode, but the same effect can be obtained even if the paste of the mixture containing MXene was printed on one of the anode and the cathode.

[0062] As a comparative example, a pair of counter electrodes, an anode and a cathode, was prepared in the same manner as above, except that MXene was not added, to obtain a sample for evaluating ion migration. A total of two pairs of counter electrodes were prepared by the same manufacturing method.

[0063] [Evaluation of electrical conductivity] The resistance value of the counter electrodes was measured with a tester. Specifically, the tester terminal was kept at a constant interval and contacted with each counter electrode to measure the resistance between two points. Since the resistance value changes depending on the interval distance, the interval was made constant for all measurements. Table 1 shows the electrode resistance values ​​of the two counter electrodes of the embodiment and the two counter electrodes of the comparative example.

[0064] [Table 1]

[0065] From Table 1 above, it can be seen that the resistance value of the electrode of the embodiment formed using a mixture containing Ag paste and MXene was the same as the resistance value of the electrode of the comparative example formed using only Ag paste, and maintained the same conductivity as that of Ag alone.

[0066] [Evaluation of ion migration suppression effect] An evaluation circuit was formed by clamping the positive and negative poles of a DC power supply with alligator clips to the above-mentioned counter electrodes. After dropping ion-exchanged water for an accelerated test on the 1 mm interval of the counter electrodes, 3 V was applied to the evaluation circuit, and the state after 7 minutes was photographed. The results are shown in Figures 5 and 6. Figure 5 is a photograph of the case of Ag paste only (without MXene, comparative example), and Figure 6 is a photograph of the case of Ag paste + MXene. As shown in Figure 5, in the case of Ag paste only (without MXene), silver dendrites were generated on the cathode (negative electrode), and ion migration occurred. On the other hand, as shown in Figure 6, in the case of Ag paste + MXene, no dendrites were observed, and ion migration did not occur. In addition, the tip of the anode (positive electrode) in Figure 6 was black, and when it was confirmed separately, this black substance was silver oxide. From this, it was found that the silver contained in the anode (positive electrode) was eluted as silver ions. Although these silver ions migrate to the negative electrode, it is believed that the presence of MXene at the cathode prevents ion migration failure.

[0067] [Example 2] As in Example 1, Ti3C2Tx The MXene powder obtained by freeze-drying the water-dispersed clay and pulverizing it using an IKA mill, Ag powder (size: 1 μm), and acrylic resin varnish were mixed in a mortar to a ratio of 1.9 mass%, 55.7 mass%, and 42.4 mass%, respectively. Then, they were kneaded in a three-roll mill. The conditions for kneading in the three-roll mill were a gap between the rolls of 10 μm and a peripheral speed of the rolls of 230 rpm. The obtained paste was printed on a substrate through a metal mask that matched the electrode shape, heated in an oven at 80 ° C for 30 minutes, and dried. Then, it was heated to 750 ° C at a heating rate of 10 ° C / min in a furnace in an Ar atmosphere. After keeping at 750 ° C for 1 hour, it was cooled to obtain the electrode of the present invention. In addition, the atmosphere in the above furnace was changed from an Ar atmosphere to an oxidizing atmosphere or a reducing atmosphere during heating in order to sufficiently remove the resin component.

[0068] The electrode obtained in this embodiment, like the electrode in Example 1, contains a specified MXene, and is therefore considered to have high conductivity and to be able to prevent ion migration failures.

[0069] [Example 3] Preparation of MAX particles and preparation of MXene powder The preparation of MAX particles and the preparation of MXene powder were carried out in the same manner as in Example 1.

[0070] The above MXene powder was mixed into a Cu paste (manufactured by NOF Corp., product name: CP-100D, containing 10% to 20% thermosetting resin as the resin) at 0.75 mass% (on a dry basis) relative to the metal particles, and the mixture was stirred manually to obtain a paste.

[0071] Using a metal mask and a rubber squeegee, the mixture paste was hand-printed onto two PET films that had been annealed at 150°C for 30 minutes, to obtain a pair of opposing electrodes, an anode and a cathode, spaced 1 mm apart. The formed product was dried at 150°C for 30 minutes to obtain a pair of opposing electrodes, an anode and a cathode, as a sample for evaluating ion migration.

[0072] As a comparative example for Example 3, a pair of opposing electrodes consisting of an anode and a cathode was prepared in the same manner as above, except that MXene was not added, to obtain a sample for evaluating ion migration.

[0073] [Evaluation of electrical conductivity] The resistance value of the counter electrodes was measured with a tester. Specifically, the tester terminal was kept at a constant interval and contacted with each counter electrode to measure the resistance between two points. Since the resistance value changes depending on the interval distance, the interval was kept constant for all measurements. The electrode resistance value results for both the example and the comparative example were 0.000Ω.

[0074] From the results of the above conductivity evaluation, the resistance value of the electrode of the embodiment formed using a mixture containing Cu paste and MXene was the same as the resistance value of the electrode of the comparative example formed using only Cu paste, and maintained the same conductivity as in the case of only Cu.

[0075] [Evaluation of ion migration suppression effect] An evaluation circuit was formed by clamping the positive and negative poles of a DC power supply with alligator clips to the above-mentioned counter electrodes. After dropping ion-exchanged water for an accelerated test on the 1 mm interval of the counter electrodes, 3 V was applied to the evaluation circuit, and the state after 8 minutes was photographed. The results are shown in Figures 7 and 8. Figure 7 is a photograph of the case of only Cu paste (without MXene, comparative example), and Figure 8 is a photograph of the case of Cu paste + MXene. As shown in Figure 7, in the case of only Cu paste (without MXene), black dendrites were generated on the cathode (negative electrode), and after 8 minutes they reached the anode (positive electrode) and short-circuited. On the other hand, as shown in Figure 8, in the case of Cu paste + MXene, dendrites were generated but the growth rate was suppressed, indicating the effect of suppressing the progress of ion migration. The time it took to reach the anode was 24 minutes and 45 seconds. [Industrial Applicability]

[0076] The electrode or wiring of the present invention may be used for any suitable purpose, and may be particularly preferably used as one or more of an anode and a cathode in an electrode pair of an electronic component, for example.

[0077] This application claims priority from Japanese Patent Application No. 2020-156698, which is incorporated herein by reference. [Explanation of symbols]

[0078] 1a, 1b layer body (M m X n layer) 3a, 5a, 3b, 5b Modified or terminal T 7a, 7b MXene layers 10, 10a, 10b MXene particles (particles of layered materials) 11A Metal particles 11B Sintered metal 12 Resin 20A, 20B Electrodes or wiring 31 Anode 33 Cathode 35 Electric field direction 37 Metal Ag

Claims

1. An electrode or wiring comprising particles of a layered material comprising one or more layers and metal particles or sintered metal, The layer comprises a compound having the following formula: M m X n wherein M is at least one Group 3, 4, 5, 6, or 7 metal; X is a carbon atom, a nitrogen atom, or a combination thereof; n is 1 or more and 4 or less, m is greater than n and is equal to or less than 5. and a modification or termination T (T is at least one selected from the group consisting of a hydroxyl group, a fluorine atom, a chlorine atom, an oxygen atom and a hydrogen atom) present on the surface of the layer body, wherein the distance between the electrodes is more than 0 mm and 6 mm or less, or the distance between the wirings is more than 0 mm and 1 mm or less.

2. The electrode or wiring according to claim 1 , formed of a composite material comprising particles of layered material comprising said one or more layers, said metal particles, and a resin.

3. The electrode or wiring according to claim 1 , which is formed of a sintered body containing particles of a layered material comprising the one or more layers and the sintered metal.

4. 4. The electrode or wiring according to claim 1, wherein the M is at least one selected from the group consisting of Ti, Zr, Hf, V, Nb, Ta, Cr, Mo and Mn.

5. The layer body is Ti 3 C 2 , Ti 3 CN, and Ti 2 The electrode or wiring according to any one of claims 1 to 4, comprising at least one selected from the group consisting of C.

6. The electrode or wiring according to any one of claims 1 to 5, wherein the content of particles of the layered material comprising the one or more layers is 0.1% by mass or more and 20% by mass or less with respect to metal particles or sintered metal.

7. The electrode or wiring according to any one of claims 1 to 6, wherein the metal particles or sintered metal contain one or more elements selected from the group consisting of Ag, Sn, Pt, Ni, Cu, Au and Zn.

8. An electrode pair having an anode and a cathode, At least one of the anode and the cathode is particles of layered material comprising one or more layers and metal particles or sintered metal, The layer comprises a compound having the following formula: M m X n wherein M is at least one Group 3, 4, 5, 6, or 7 metal; X is a carbon atom, a nitrogen atom, or a combination thereof; n is 1 or more and 4 or less, m is greater than n and is equal to or less than 5. and a modification or termination T (T is at least one selected from the group consisting of a hydroxyl group, a fluorine atom, a chlorine atom, an oxygen atom, and a hydrogen atom) present on the surface of the layer body.

9. 9. The electrode pair of claim 8, wherein the distance between the anode and cathode is greater than 0 mm and less than or equal to 6 mm.

10. 10. The electrode pair according to claim 8, wherein at least one of the anode and the cathode contains one or more elements selected from the group consisting of Ag, Sn, Pt, Ni, Cu, Au, and Zn.

11. (a1) preparing a mixture by kneading particles of a layered material comprising one or more layers, metal particles, and a resin, The layer comprises a compound having the following formula: M m X n wherein M is at least one Group 3, 4, 5, 6, or 7 metal; X is a carbon atom, a nitrogen atom, or a combination thereof; n is 1 or more and 4 or less, m is greater than n and is equal to or less than 5. and a modification or terminal T (T is at least one selected from the group consisting of a hydroxyl group, a fluorine atom, a chlorine atom, an oxygen atom, and a hydrogen atom) present on the surface of the layer body, A blending ratio of the layered material particles in the mixture is 0.1% by mass or more and 20% by mass or less with respect to the metal particles; and (b1) Drying the mixture to obtain an electrode or wiring. wherein the distance between the electrodes is greater than 0 mm and not greater than 6 mm, or the distance between the wires is greater than 0 mm and not greater than 1 mm.

12. (a2) kneading a compound comprising particles of a layered material comprising one or more layers and metal particles to prepare a mixture, The layer comprises a compound having the following formula: M m X n wherein M is at least one Group 3, 4, 5, 6, or 7 metal; X is a carbon atom, a nitrogen atom, or a combination thereof; n is 1 or more and 4 or less, m is greater than n and is equal to or less than 5. and a modification or terminal T (T is at least one selected from the group consisting of a hydroxyl group, a fluorine atom, a chlorine atom, an oxygen atom, and a hydrogen atom) present on the surface of the layer body, a blending ratio of the layered material particles in the mixture is 0.1% by mass or more and 20% by mass or less with respect to the metal particles; (b2) molding the mixture and drying it to obtain a molded product; and (c) sintering the molded product at a sinterable temperature. A method for producing electrodes or wiring of an electronic component or a circuit board, comprising:

13. The method for producing an electrode according to claim 12, wherein the distance between the electrodes is greater than 0 mm and is equal to or less than 6 mm.

14. The method for manufacturing wiring according to claim 12, wherein the distance between the wirings is more than 0 mm and 1 mm or less.

Citation Information

Patent Citations

  • Wearable flexible stress sensor and preparation method and application thereof

    CN109238522A

  • Implantable devices using 2d metal carbides and nitrides (mxenes)

    CN111447968A

  • Inorganic anion exchanger and epoxy resin composition for sealing electronic component using the same

    JP2005001902A

  • Triazine compound

    JP2014210732A

  • Method for manufacturing electrode material for electrochemical capacitor including layer compound