Vinyl polymer, curable composition, and cured product

A vinyl polymer with a terminal structure from 3-20-mer (meth)acrylic monomers addresses solvent and alkaline water solubility issues, improving workability and reducing odor, suitable for curable compositions and cured products.

JP7563491B2Active Publication Date: 2024-10-08MITSUBISHI CHEM CORP
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
JP2022574025
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2021-01-08
Filing Date
2021-12-27
Publication Date
2024-10-08
Estimated Expiration
2041-12-27

AI Technical Summary

Technical Problem

Existing polymers containing vinyl aromatic compounds and methacrylic acid face issues with solvent solubility, alkaline water solubility, and odor, making them unsuitable for applications like inks and resists due to poor workability and environmental impact.

Method used

A vinyl polymer with a terminal structure derived from 3-20-mer (meth)acrylic monomers, having an acid value of 35-300 mgKOH/g, and incorporating structural units from vinyl monomers with acid groups and aromatic rings, ensuring good solubility in solvents and alkaline water while reducing odor.

Benefits of technology

The polymer achieves improved solubility in solvents and alkaline water, reducing environmental burden and enhancing workability, with enhanced curability and stability in cured products.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007563491000001
    Figure 0007563491000001
  • Figure 0007563491000002
    Figure 0007563491000002
  • Figure 0007563491000003
    Figure 0007563491000003
Patent Text Reader

Abstract

The objective of the present invention is to provide a low odor polymer which is soluble in a solvent and can reduce a working environment load. In addition, the objective of the present invention is to provide a curable composition using said polymer and a cured product thereof. A vinyl-based polymer according to the present invention has a terminal structure derived from at least one among 3-mer to 20-mer of a (meth)acrylic-based monomer, and has an acid value of 35-300 mgKOH / g.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a vinyl polymer suitable for a photosensitive resin composition useful as an ink or a binder for a resist, a curable composition, and a cured product thereof. This application claims priority based on Japanese Patent Application No. 2021-002164, filed in Japan on January 8, 2021, the contents of which are incorporated herein by reference. [Background technology]

[0002] Polymers containing vinyl aromatic compounds and methacrylic acid are useful industrially in inks and resists, and are widely used as binders for dry film resists. In order to impart viscosity, water resistance and alkaline water solubility suitable for various applications such as inks and resists to polymers containing vinyl aromatic compounds and methacrylic acid, it is necessary to control the composition and molecular weight to an appropriate level.

[0003] Patent Document 1 describes a suspension polymerization method in which n-dodecyl mercaptan or α-methylstyrene dimer is used as a chain transfer agent to control the molecular weight of the polymer. The method of Patent Document 1 is an excellent polymerization method in that polymer particles with good handleability can be obtained, but since n-dodecyl mercaptan is used, the solubility in solvents and alkaline water is not good, and the workability is not good due to the odor derived from n-dodecyl mercaptan, and there is room for improvement in that the load on the working environment is large.

[0004] Patent Document 2 describes a terminally unsaturated methacrylic acid ester n-mer as a chain transfer agent capable of more efficiently adjusting the molecular weight of the produced polymer or copolymer, and a polymerization method using the same. The method of Patent Document 2 does not use an alkyl mercaptan chain transfer agent, and therefore can achieve a reduction in odor, but has the problem that the polymer does not have an acid group, and therefore has poor solubility when dissolved in alkaline water, and is not good in solvent solubility.

[0005] Patent Document 3 describes a method for producing an addition polymer having a polymerizable olefin end group. Since the polymer polymerized using the chain transfer agent produced by the method of Patent Document 3 does not have an acid group, the solubility of the polymer when dissolved in alkaline water is not good, and there is room for improvement in terms of solvent solubility. [Prior art documents] [Patent documents]

[0006] [Patent Document 1] Japanese Patent Publication No. 7-102004 [Patent Document 2] Japanese Patent Application Publication No. 2006-176587 [Patent Document 3] Japan Special Publication No. 2000-514845 Summary of the Invention [Problem to be solved by the invention]

[0007] An object of the present invention is to provide a polymer which can be used in a curable composition and a cured product thereof, which is soluble in a solvent and has a low odor and can reduce the burden on the working environment. [Means for solving the problem]

[0008] The present invention relates to the following items [1] to

[12] .

[0009] [1] A vinyl polymer having a terminal structure derived from one or more types of trimers to 20mers of a (meth)acrylic monomer and an acid value of 35 to 300 mgKOH / g. [2] The vinyl polymer according to [1], wherein the terminal structure is an terminal structure derived from a chain transfer agent. [3] The vinyl polymer of [1] or [2], further comprising structural units derived from two or more kinds of vinyl monomers. [4] The vinyl polymer according to [3], wherein at least one of the vinyl monomers is a vinyl monomer having an acid group. [5] The vinyl polymer according to [3] or [4], wherein at least one of the vinyl monomers has an aromatic ring. [6] The vinyl polymer according to any one of [3] to [5], wherein at least one of the vinyl monomers is a (meth)acrylic monomer. [7] The vinyl polymer according to [6], wherein the (meth)acrylic monomer in the vinyl monomer is an alkyl (meth)acrylate, and the alkyl group in the ester structure of the alkyl (meth)acrylate has 1 to 18 carbon atoms. [8] The vinyl polymer of any one of [1] to [7], having a weight average molecular weight of 5,000 to 1,000,000. [9] The vinyl polymer according to any one of [1] to [8], wherein the vinyl polymer is in a particulate form, and the particulate vinyl polymer has a mass average particle diameter of 20 to 2000 μm.

[10] A curable composition comprising the vinyl polymer according to any one of [1] to [9] and a compound having a polymerizable double bond.

[11] The curable composition according to

[10] , further comprising one or more 3-20 monomers of a (meth)acrylic monomer.

[12] A cured product of the curable composition according to

[10] or

[11] . Effect of the Invention

[0010] According to the present invention, it is possible to provide a polymer which can be used in a curable composition and a cured product thereof, which is soluble in a solvent and has a low odor and can reduce the burden on the working environment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] <Vinyl polymer> The vinyl polymer of the present invention has, as a terminal structure of the polymer, one or more structures derived from a trimer to an aryl monomer, and has an acid value of 35 to 300 mgKOH / g. In the present invention, "(meth)acrylic" is a general term for acrylic and methacrylic.

[0012] The vinyl polymer of the present invention has one or more types of trimers to 20-mers of a (meth)acrylic monomer as a terminal structure of the polymer. The terminal structure which is a trimer to 20-mer of a (meth)acrylic monomer is preferably a trimer to 10-mer of a (meth)acrylic monomer, and more preferably a trimer to 5-mer of a (meth)acrylic monomer. The terminal structure is preferably an terminal structure derived from a chain transfer agent, and the terminal structure preferably further has a polymerizable double bond. When the end structure of the polymer is a chain transfer agent-derived end structure, the solubility in the solvent is good. In addition, when the end structure of the polymer has a polymerizable double bond, the curability of the curable composition containing the vinyl polymer is good, which is preferable. When the end structure of the polymer is a chain transfer agent-derived end structure and has a polymerizable double bond, the solubility of the polymer in the solvent is good, and the curability of the curable composition containing the vinyl polymer is good, which is more preferable.

[0013] Examples of the (meth)acrylic monomer in the trimer to 20-mer of a (meth)acrylic monomer include acrylic acid esters such as methyl acrylate, ethyl acrylate, n-butyl acrylate, i-butyl acrylate, t-butyl acrylate, 2-ethylhexyl acrylate, lauryl acrylate, dodecyl acrylate, stearyl acrylate, glycidyl acrylate, 2-hydroxyethyl acrylate, 2-hydroxypropyl acrylate, 2-methoxyethyl acrylate, and 2-ethoxyethyl acrylate; Methacrylic acid esters such as methyl methacrylate, ethyl methacrylate, n-butyl methacrylate, i-butyl methacrylate, t-butyl methacrylate, 2-ethylhexyl methacrylate, cyclohexyl methacrylate, lauryl methacrylate, dodecyl methacrylate, stearyl methacrylate, behenyl methacrylate, isobornyl methacrylate, phenyl methacrylate, benzyl methacrylate, glycidyl methacrylate, 2-hydroxyethyl methacrylate, 2-hydroxypropyl methacrylate, 2-methoxyethyl methacrylate, 2-ethoxyethyl methacrylate, phenoxyethyl methacrylate, 2-methacryloyloxyethyl hexahydrophthalate, and 2-methacryloyloxyethyl phthalate; Polymerizable amides such as acrylamide and methacrylamide; Dialkylaminoethyl (meth)acrylates such as dimethylaminoethyl acrylate, diethylaminoethyl acrylate, dimethylaminoethyl methacrylate, and diethylaminoethyl methacrylate; Examples include:

[0014] From the viewpoint of miscibility with the monomer during polymerization, acrylic acid esters and methacrylic acid esters are preferred, and from the viewpoint of good solubility in alkaline water and solvent of the resulting resin, methyl acrylate, ethyl acrylate, n-butyl acrylate, i-butyl acrylate, t-butyl acrylate, 2-ethylhexyl acrylate, cyclohexyl acrylate, phenyl acrylate, methyl methacrylate, ethyl methacrylate, n-butyl methacrylate, i-butyl methacrylate, t-butyl methacrylate, 2-ethylhexyl methacrylate, cyclohexyl methacrylate, and phenyl methacrylate are more preferred, and methyl methacrylate, ethyl methacrylate, and phenyl methacrylate are even more preferred. These may be used alone or in combination of two or more.

[0015] The term "end structure derived from a chain transfer agent" refers to a chemical structure portion derived from a chain transfer agent used to adjust the molecular weight of various polymers or copolymers produced from polymerizable monomers or mixtures thereof.

[0016] The vinyl polymer in the present invention preferably further has structural units derived from two or more types of vinyl monomers in addition to the terminal structures. Vinyl monomers include maleimides such as N-phenylmaleimide and N-cyclohexylmaleimide; Monobasic acids such as acrylic acid, methacrylic acid, crotonic acid; Dibasic acids such as fumaric acid, maleic acid, itaconic acid, and partial esters of these dibasic acids; Vinyl compounds having a sulfonic acid group, such as vinyl sulfonic acid and 2-acrylamido-2-methylpropanesulfonic acid; Vinyl compounds having an aromatic ring, such as styrene, o-methylstyrene, m-methylstyrene, p-methylstyrene, α-methylstyrene, o-methoxystyrene, m-methoxystyrene, p-methoxystyrene, pt-butylstyrene, pt-butoxystyrene, 1-vinylnaphthalene, 2-vinylnaphthalene, phenyl acrylate, benzyl acrylate, and phenoxyethyl acrylate; Examples include:

[0017] In view of improving the solubility of the polymer in alkaline water, it is preferred that at least one of the vinyl monomers is a vinyl monomer having an acid group.

[0018] Examples of the vinyl monomer having an acid group include monobasic acids such as acrylic acid, methacrylic acid, and crotonic acid; Dibasic acids such as fumaric acid, maleic acid, itaconic acid, and partial esters of these dibasic acids; Vinyl compounds having a sulfonic acid group, such as vinyl sulfonic acid and 2-acrylamido-2-methylpropanesulfonic acid; Examples include: These may be used alone or in combination of two or more.

[0019] In view of improving the solvent solubility of the polymer, it is preferred that at least one of the vinyl monomers is a vinyl monomer having an aromatic ring.

[0020] Examples of vinyl monomers having an aromatic ring include styrene, o-methylstyrene, m-methylstyrene, p-methylstyrene, α-methylstyrene, o-methoxystyrene, m-methoxystyrene, p-methoxystyrene, pt-butylstyrene, pt-butoxystyrene, 1-vinylnaphthalene, 2-vinylnaphthalene, phenylacrylate, benzyl methacrylate, benzyl acrylate, phenoxyethyl methacrylate, and phenoxyethyl acrylate. Styrene, p-methylstyrene, p-methoxystyrene, and pt-butylstyrene are preferred from the viewpoints of excellent solubility of the resulting vinyl polymer in a solvent and ease of availability. These may be used alone or in combination of two or more.

[0021] The vinyl polymer of the present invention may further contain one or more constituent units derived from other monomers having a polymerizable double bond other than the constituent units derived from the vinyl monomer having an acid group and the constituent units derived from the vinyl monomer having an aromatic ring.

[0022] The other monomer having a polymerizable double bond is not particularly limited as long as it is copolymerizable with the vinyl monomer having an acid group and the vinyl monomer having an aromatic ring. Examples of other monomers having a polymerizable double bond include acrylic acid esters such as methyl acrylate, ethyl acrylate, n-butyl acrylate, i-butyl acrylate, t-butyl acrylate, 2-ethylhexyl acrylate, lauryl acrylate, dodecyl acrylate, stearyl acrylate, glycidyl acrylate, 2-hydroxyethyl acrylate, 2-hydroxypropyl acrylate, 2-methoxyethyl acrylate, and 2-ethoxyethyl acrylate; Methacrylic acid esters such as methyl methacrylate, ethyl methacrylate, n-butyl methacrylate, i-butyl methacrylate, t-butyl methacrylate, 2-ethylhexyl methacrylate, cyclohexyl methacrylate, lauryl methacrylate, dodecyl methacrylate, stearyl methacrylate, behenyl methacrylate, isobornyl methacrylate, phenyl methacrylate, glycidyl methacrylate, 2-hydroxyethyl methacrylate, 2-hydroxypropyl methacrylate, 2-methoxyethyl methacrylate, 2-ethoxyethyl methacrylate, 2-methacryloyloxyethyl hexahydrophthalate, and 2-methacryloyloxyethyl phthalate; Polymerizable amides such as acrylamide and methacrylamide; Examples of the dialkylaminoethyl (meth)acrylates include dimethylaminoethyl acrylate, diethylaminoethyl acrylate, dimethylaminoethyl methacrylate, diethylaminoethyl methacrylate, and other dialkylaminoethyl (meth)acrylates. These may be used alone or in combination of two or more.

[0023] In the vinyl polymer of the present invention, from the viewpoint of imparting hardness and flexibility to a cured product of a curable composition containing the vinyl polymer, it is preferable that one or more of the vinyl monomers is a (meth)acrylic monomer. From the viewpoint of imparting hardness and flexibility to a cured product of a curable composition containing a vinyl polymer, the (meth)acrylic monomer is preferably a (meth)acrylic acid alkyl ester, more preferably an alkyl group in the ester structure of the (meth)acrylic acid alkyl ester having 1 to 18 carbon atoms, and further preferably ethyl acrylate, n-butyl acrylate, 2-ethylhexyl acrylate, methyl methacrylate, n-butyl methacrylate, or 2-ethylhexyl methacrylate.

[0024] When the vinyl polymer of the present invention contains a constituent unit derived from a vinyl monomer having an acid group, the mass ratio of the constituent unit derived from the vinyl monomer having an acid group to the constituent units derived from all monomers of the vinyl polymer is preferably 5 to 60%, more preferably 10 to 45%, and even more preferably 15 to 40%. When the mass ratio is equal to or greater than the lower limit, the curable composition containing the vinyl polymer has excellent solubility in alkaline water. When the mass ratio is equal to or less than the upper limit, the curable composition has excellent solubility in solvents.

[0025] When the vinyl polymer of the present invention contains a constituent unit derived from a vinyl monomer having an aromatic ring, the mass ratio of the constituent unit derived from the vinyl monomer having an aromatic ring to the constituent units derived from all monomers of the vinyl polymer is preferably 5 to 80%, more preferably 10 to 70%, and even more preferably 25 to 60%. Within the above range, the water resistance and strength of the curable composition containing the vinyl polymer when cured into a cured product are good.

[0026] The mass ratio of the structure derived from the (meth)acrylic monomer (a trimer to 20-mer of the (meth)acrylic monomer) in the terminal structure to the total monomer-derived structural units of the vinyl polymer of the present invention is preferably 1 ppm to 10%, more preferably 100 ppm to 7%, and even more preferably 2000 ppm to 4%. When it is equal to or more than the lower limit, the solvent solubility of the curable composition containing the vinyl polymer tends to be good. When it is equal to or less than the upper limit, the purity of the vinyl polymer is improved.

[0027] The mass ratio of the constituent units derived from other monomers having a polymerizable double bond to the constituent units derived from all monomers of the vinyl polymer of the present invention is preferably 0 to 90%, more preferably 5 to 80%, and even more preferably 10 to 70%. If it is within the above range, the compatibility of the vinyl polymer with all monomers when made into a curable composition is good.

[0028] The mass proportion of the structural units derived from each monomer of the vinyl polymer and the structure derived from the (meth)acrylic monomer (a trimer to 20-mer of the (meth)acrylic monomer) in the terminal structure can be determined from the mass percentage calculated from the mass ratio of each monomer used in the polymerization raw material to the trimer to 20-mer of the (meth)acrylic monomer.

[0029] The acid value of the vinyl polymer of the present invention is 35 to 300 mgKOH / g, preferably 60 to 300 mgKOH / g, more preferably 70 to 240 mgKOH / g, and even more preferably 120 to 200 mgKOH / g. If it is equal to or more than the lower limit, the solubility of the vinyl polymer in alkaline water is good. If it is equal to or less than the upper limit, the water resistance of the cured product of the curable composition containing the vinyl polymer is good. The acid value of a vinyl polymer can be determined by dissolving the polymer in a 1:1 toluene-ethanol solution, adding dropwise KOH dissolved in ethanol, and titrating the polymer to measure the number of milligrams of KOH required to neutralize 1 g of the polymer, based on the discoloration point of phenolphthalein.

[0030] The vinyl polymer of the present invention may be neutralized before use. Examples of bases that can be used to neutralize the vinyl polymer of the present invention include metal hydroxides, ammonia, and amine compounds. Examples of metal hydroxides include lithium hydroxide, sodium hydroxide, and potassium hydroxide. Examples of the amine compound include morpholine, thiomorpholine, triethylamine, propylamine, diethylamine, tripropylamine, dibutylamine, amylamine, 1-aminooctane, 2-dimethylaminoethanol, ethylaminoethanol, 2-diethylaminoethanol, 1-amino-2-propanol, 2-amino-1-propanol, 3-amino-1-propanol, 1-dimethylamino-2-propanol, 3-dimethylamino-1-propanol, 2-propylaminoethanol, ethoxypropylamine, aminobenzyl alcohol, pyrrolidine, and piperidine.

[0031] The weight average molecular weight (Mw) of the vinyl polymer of the present invention is preferably 5000 to 1000000, more preferably 5000 to 200000, further preferably 6000 to 120000, and particularly preferably 7000 to 80000. If it is equal to or more than the lower limit, the water resistance and coating strength of the cured product of the curable composition containing the vinyl polymer tend to be good. If it is equal to or less than the upper limit, the viscosity of the curable composition containing the vinyl polymer can be reduced, and the workability tends to be good.

[0032] The vinyl polymer of the present invention preferably has a ratio (Mw / Mn) of weight average molecular weight (Mw) to number average molecular weight (Mn) of 1.0 to 5.0, more preferably 1.0 to 3.5. By setting Mw / Mn within the above range, the viscosity of the curable composition containing the vinyl polymer can be reduced, and the workability becomes better. In addition, when the cured product of the curable composition is developed, the resolution becomes good.

[0033] The weight average molecular weight (Mw) and number average molecular weight (Mn) can be measured by gel permeation chromatography (GPC) and converted using a calibration curve of standard polystyrene.

[0034] The GPC measurement conditions are as follows. Equipment: Tosoh HLC-8220GPC (manufactured by Tosoh Corporation) Column: Tosoh TSKgel G5000HXL*GMHXL-L (7.8mmφ×300mm) Solvent: Tetrahydrofuran Sample concentration: 0.4% by weight Measurement temperature: 40℃ Injection volume: 100μL Flow rate: 1.0mL / min Detector: RI (built-in device), UV (Tosoh UV-8220)

[0035] The vinyl polymer of the present invention may be in the form of, for example, particles, blocks, or a solution, and is preferably in the form of particles from the viewpoint of ease of handling when dissolved in a solvent or alkaline water.

[0036] When the vinyl polymer is particulate, the mass average particle diameter of the particulate vinyl polymer is preferably 20 to 2000 μm, more preferably 50 to 800 μm, and even more preferably 100 to 600 μm. If it is equal to or greater than the lower limit, the risk of dust explosion is suppressed and the blending operation is facilitated. If it is equal to or less than the upper limit, the solvent solubility of the polymer is improved and the time required for dissolving in the solvent is shortened. The mass-average particle size can be calculated by using a standard sieve to shake and classify 20 g of granular resin for 5 minutes.

[0037] When the vinyl polymer is in the form of particles or lumps, the water content of the vinyl polymer is preferably 0.1 to 5.0% by weight, more preferably 0.5 to 4.5% by weight. When the water content is within the above range, the polymer obtained has good handleability. The moisture content can be calculated from the loss on drying of the vinyl polymer before and after drying at 105°C for 2 hours, assuming that the moisture content when the vinyl polymer is dried at 105°C for 2 hours is 0%.

[0038] <Method of producing vinyl polymer> The vinyl polymer of the present invention can be produced by a commonly known polymerization method such as bulk polymerization, solution polymerization, suspension polymerization, etc. Suspension polymerization is preferred since it gives a particulate polymer which is easy to handle.

[0039] For example, the vinyl polymer of the present invention can be produced by a process having a polymerization step using a suspension polymerization method, a first dehydration step, a washing step, a second dehydration step, and a drying step.

[0040] (Polymerization process) The polymerization step is a step of suspension polymerizing a vinyl monomer having an acid group, a vinyl monomer having an aromatic ring, and, if necessary, other monomers having a polymerizable double bond to obtain a vinyl polymer. As the suspension polymerization method, a known method can be adopted, and an example thereof includes a method in which a vinyl-based monomer having an acid group, a vinyl-based monomer having an aromatic ring, and, if necessary, other monomers having a polymerizable double bond are polymerized in water in the presence of a polymerization auxiliary in a vessel having a polymerization temperature control function and a stirring function.

[0041] Examples of the polymerization aid include a polymerization initiator, a chain transfer agent, a dispersant, and a dispersion aid. Examples of the polymerization initiator include 2,2'-azobisisobutyronitrile, 2,2'-azobis(2-methylbutyronitrile), benzoyl peroxide, and lauroyl peroxide. As the chain transfer agent, one or more trimers to 20-mers of (meth)acrylic monomers are used. t-dodecyl mercaptan, n-dodecyl mercaptan, octyl thioglycolate, α-methylstyrene dimer may be used in combination with one or more trimers to 20-mers of (meth)acrylic monomers. Examples of dispersants include surfactants that stably disperse monomers in water. Specific examples of such dispersants include copolymers of 2-sodium sulfoethyl methacrylate, potassium methacrylate, and methyl methacrylate, copolymers of 3-sodium sulfopropyl methacrylate, and methyl methacrylate, copolymers of sodium methacrylate and methacrylic acid, polyvinyl alcohol, polyvinylpyrrolidone, hydroxyethyl cellulose, and hydroxypropyl cellulose. Examples of the dispersion aid include sodium sulfate, sodium carbonate, sodium dihydrogen phosphate, disodium hydrogen phosphate, potassium chloride, calcium acetate, magnesium sulfate, and manganese sulfate.

[0042] The vinyl polymer obtained by suspension polymerization is obtained in the form of a slurry, and by dehydrating the slurry, vinyl polymer particles that are generally nearly spherical are obtained.

[0043] (Dehydration process) The dehydration step includes a first dehydration step in which the slurry after suspension polymerization is dehydrated with a dehydrator or the like to separate the vinyl polymer particles from the reaction liquid, and a second dehydration step in which the vinyl polymer particles after the washing step are dehydrated with a dehydrator or the like to separate the vinyl polymer particles from the washing liquid. Various dehydrators can be used in each dehydration step, and for example, a centrifugal dehydrator or a device with a mechanism for sucking and removing water on a porous belt can be appropriately selected and used. One dehydrator may be used, or two of the same model may be prepared and used in each dehydration step, or multiple different models of dehydrators may be used. A model that suits the purpose can be appropriately selected from the perspectives of product quality, capital investment cost, productivity, operating cost, etc. When the balance between product quality and production speed is important, it is preferable to use a dedicated dehydrator for each dehydration step.

[0044] (Cleaning process) The washing step increases the purity of the vinyl polymer. Examples of the washing method include a method in which a washing liquid is added to the vinyl polymer particles dehydrated in the first dehydration step to reslurry the vinyl polymer and stir and mix it, and a method in which a dehydration step is performed in a dehydrator having a washing function, and then a washing liquid is added to wash the particles. Washing may be performed by combining these washing methods.

[0045] The type and amount of the cleaning solution may be selected so as to achieve the purpose of the cleaning step. Examples of cleaning agents include water (ion-exchanged water, distilled water, purified water, etc.), an aqueous solution of a sodium salt, and methanol.

[0046] (drying process) The drying step is a step of drying the vinyl polymer particles after the second dehydration step. After the second dehydration step, water remains on the surface of the vinyl polymer particles, and the inside of the vinyl polymer is in a state close to saturated water absorption. Therefore, it is preferable to dry the vinyl polymer in order to further reduce the water content. Various types of dryers can be used for drying, and examples of such dryers include a dryer that dries by heating under reduced pressure, a dryer that dries vinyl polymer particles while air-transporting them through a pipe using heated air, and a dryer that dries vinyl polymer particles above a porous plate by blowing heated air from below, causing the particles to flow. The drying step is preferably carried out so that the water content of the vinyl polymer after the drying step is 0.1 to 5.0% by weight. The chemical structure of the obtained vinyl polymer is 1 H-NMR and 13 This can be confirmed by known analytical methods such as C-NMR.

[0047] <Action and effect> The vinyl polymer of the present invention has good solubility in various solvents and alkaline water and has low odor, and therefore has excellent workability. The curable composition containing the vinyl polymer of the present invention has excellent compositional uniformity and is therefore less likely to develop lumps or cloudiness.

[0048] <Application> The vinyl polymer of the present invention can be used as a raw material for, for example, inks, paints, binders for ceramic firing, adhesives, and dry film resists, and is particularly suitable as a raw material for dry film resists.

[0049] <Curable composition> The curable composition of the present invention contains the vinyl polymer of the present invention and a compound having a polymerizable double bond. If necessary, it may contain any optional component. The curable composition of the present invention preferably further contains one or more kinds of trimers to 20mers of (meth)acrylic monomers, in terms of improving the curability of the curable composition. In terms of obtaining good curability of the curable composition, the trimer to 20-mer of the (meth)acrylic monomer is more preferably a trimer to 10-mer of the (meth)acrylic monomer, and further preferably a trimer to 5-mer of the (meth)acrylic monomer.

[0050] Examples of the compound having a polymerizable double bond include trimers to 20-mers of (meth)acrylic monomers, monomers that can be used in the production of the above-mentioned vinyl polymers, 1,4-butanediol di(meth)acrylate, 1,6-hexanediol di(meth)acrylate, neopentyl glycol di(meth)acrylate, polyethylene glycol di(meth)acrylate, neopentyl glycol adipate di(meth)acrylate, neopentyl glycol di(meth)acrylate hydroxypivalate, and dicyclopentadienyl di(meth)acrylate. Examples of the acrylates include caprolactone-modified dicyclopentadienyl di(meth)acrylate, allylated cyclohexyl di(meth)acrylate, isocyanurate di(meth)acrylate, trimethylolpropane tri(meth)acrylate, dipentaerythritol tri(meth)acrylate, pentaerythritol tri(meth)acrylate, methyl trimethyl tri(meth)acrylate, tris(acryloxyethyl)isocyanurate, dipentaerythritol penta(meth)acrylate, and dipentaerythritol hexa(meth)acrylate. In view of the balance between curability and releasability, the following monomers that can be used in the production of the above-mentioned vinyl polymers: 1,4-butanediol di(meth)acrylate, 1,6-hexanediol di(meth)acrylate, neopentyl glycol di(meth)acrylate, polyethylene glycol di(meth)acrylate, neopentyl glycol adipate di(meth)acrylate, neopentyl glycol di(meth)acrylate hydroxypivalate, dicyclopentadienyl di(meth)acrylate, caprolactone-modified dicyclopentadienyl di(meth)acrylate, allylated cyclohexyl di(meth)acrylate, and isocyanurate di(meth)acrylate are preferred.

[0051] The optional components include various known additives, such as a solvent, a photopolymerization initiator, a dye, and a stabilizer. Various known additives can be appropriately selected depending on the desired physical properties and characteristics of the curable composition.

[0052] The curable composition of the present invention can be produced, for example, by a method in which the vinyl polymer of the present invention, a compound having a polymerizable double bond, and, if necessary, any optional components are mixed together using a conventional stirrer.

[0053] The curable composition of the present invention can be used, for example, as a resist for semiconductor production, a dry film resist, or a solder resist.

[0054] When the curable composition of the present invention is used for a dry film resist, a composition obtained by mixing the vinyl polymer of the present invention, a compound having a polymerizable double bond, a solvent, a photopolymerization initiator, and, if necessary, optional components is suitably used.

[0055] Examples of the compound having a polymerizable double bond include compounds having a polymerizable double bond that can be used in the above-mentioned curable composition. The content of the compound having a polymerizable double bond in the curable composition is preferably 5 to 90 parts by mass per 100 parts by mass of the total amount of the vinyl polymer of the present invention, in view of the balance between curability and coatability.

[0056] The solvent is not particularly limited and can be appropriately selected depending on the purpose. Examples of the solvent include propylene glycol monomethyl ether, acetone, methyl ethyl ketone, methyl isobutyl ketone, toluene, xylene, methanol, ethanol, isopropyl alcohol, and ethyl acetate, as well as an aqueous solution of a base that can be used to neutralize the vinyl polymer of the present invention when the vinyl polymer of the present invention is neutralized for use. These solvents may be used alone or in combination of two or more.

[0057] Examples of the photopolymerization initiator include benzoin, benzoin alkyl ethers, ketals, acetophenones, benzophenone, 4,4'-dimethyl-amino-benzophenone, 4,4'-diethyl-amino-benzophenone, thioxanthones, morpholino-propanone compounds, 2,4,5-triarylimidazole dimer, 2,2'-bis(2-chlorophenyl)-4,4',5,5'-tetraphenyl-1,2'-biimidazole, oxime esters, and thioxanthones. These photopolymerization initiators may be used alone or in combination of two or more. The content of the photopolymerization initiator in the curable composition is preferably 0.01 part by mass or more and 1 part by mass or less based on 100 parts by mass of the total amount of the compound having a polymerizable double bond.

[0058] Examples of the stabilizer include p-methoxyphenol, hydroquinone, pyrogallol, naphthylamine, and t-methylcatechol. Examples of dyes include malachite green, Victoria Pure Blue, brilliant green, methyl violet, leuco crystal violet, diphenylamine, and benzylamine. In addition, a defoaming agent and a leveling agent may be used as optional components.

[0059] <Cured Product of Curable Composition> The photosensitive element can be formed by applying the curable composition to a support such as a polyester film such as polyethylene terephthalate, polyethylene, polypropylene, etc., so that the thickness after drying is 1 μm to 100 μm, and removing the volatile components. The photosensitive element can be exposed to ultraviolet light with a wavelength of 250 nm to 420 nm to form a cured product of the curable composition, thereby forming a circuit pattern. EXAMPLES

[0060] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these. In the following description, "parts" means parts by mass. Each vinyl polymer in the examples and comparative examples was synthesized according to the raw material composition ratio shown in Table 1. The dispersants used in the examples and comparative examples were produced by the method described below. In the examples and comparative examples, the physical properties were measured and evaluated by the following methods.

[0061] [Measurement and Evaluation] <Evaluation of Solubility of Vinyl Polymer Particles in Solvents> 70 g of propylene glycol monomethyl ether was placed in a flask as a solvent, and 30 g of vinyl polymer particles were added in small portions while stirring with a stirrer at room temperature. After stirring at 50°C for 2 hours, the solution was cooled to room temperature and the solubility was visually confirmed based on the transparency of the solution and evaluated according to the following criteria.

[0062] (Solvent solubility evaluation criteria) A: The solution is clear and the solubility is excellent. B: Although it takes more than 2 hours to dissolve, the solution is transparent, so the solubility is excellent. C: The solution is slightly cloudy and the solubility is poor. D: The solution is cloudy and has poor solubility.

[0063] <Evaluation of solubility of vinyl polymer particles in alkaline water> 50 mL of 0.5 M potassium hydroxide aqueous solution was placed in a flask, and 5 g of vinyl polymer particles were added in small portions while stirring at room temperature with a stirrer. After stirring at 50°C for 2 hours, the solution was cooled to room temperature and the solubility was visually confirmed to see whether any vinyl polymer particles remained dissolved. The turbidity was measured with a turbidity meter (EUTECH, portable turbidity meter TN100IR) and evaluated according to the following criteria.

[0064] (Alkaline water solubility evaluation standard) A: The turbidity of the potassium hydroxide aqueous solution after dissolving the vinyl polymer particles is less than 15 NTU. B: The turbidity of the potassium hydroxide aqueous solution after dissolving the vinyl polymer particles is 15 NTU or more. C: Undissolved vinyl polymer particles remain, and the solubility is poor.

[0065] <Measurement of Moisture Content of Vinyl Polymer Particles> The water content of the vinyl polymer particles dried at 105° C. for 2 hours was defined as 0%, and the water content was calculated from the loss in the mass of the vinyl polymer before and after drying.

[0066] <Odor evaluation> The coating solution obtained by dissolving vinyl polymer / acetone / ethylene oxide-modified bisphenol A diacrylate in a mass ratio of 30 / 45 / 25 was applied onto a PET film (Diafoil R310-16, polyethylene terephthalate, manufactured by Mitsubishi Chemical Corporation) with an applicator. After that, it was dried at room temperature for 5 minutes, and then placed in a dryer at 40°C for 15 minutes. It was then pressed onto a copper plate with a laminator (upper and lower roll temperatures: 100°C, roll speed: 1m / min, pressure setting: 0.3MPa) and cooled to room temperature. After that, seven panelists performed a sensory evaluation of the odor when peeling off the PET film using the following odor evaluation criteria, and the odor was evaluated by the majority of the panelists.

[0067] (Odor evaluation criteria) A: There is no unpleasant odor at all. B: There is a slightly unpleasant odor. C: A strong and unpleasant odor.

[0068] [Production of Dispersant (1)] In a polymerization apparatus equipped with a stirrer, a cooling tube, and a thermometer, 1230 g of deionized water, 60 g of 2-sulfoethyl sodium methacrylate, 10 g of potassium methacrylate, and 12 g of methyl methacrylate were added and stirred, and the polymerization temperature was raised to 50°C while replacing the atmosphere in the polymerization apparatus with nitrogen, and 0.08 g of 2,2'-azobis(2-methylpropionamidine) dihydrochloride was added as a polymerization initiator, and the polymerization temperature was further raised to 60°C. Simultaneously with the addition of the polymerization initiator, methyl methacrylate was continuously dropped at a rate of 0.24 g / min using a dropping pump for 75 minutes, and the polymerization temperature was maintained at 60°C for 6 hours, and then cooled to room temperature to obtain dispersant (1). The solid content of dispersant (1) was 7.5% by weight.

[0069] [Production Example 1: Production of MMA trimmer] In a flask equipped with a condenser, 0.114 mmol of cobalt (II) acetate tetrahydrate and 0.228 mmol of dimethylglyoxime were charged per mol of monomer, and 0.01 mol of pyridine and 166 ml of methyl ethyl ketone (MEK) were added with a syringe. The resulting mixture was freeze-degassed three times under a nitrogen stream, and then heated and stirred at 80°C for 30 minutes to obtain a catalyst mixture. Separately, a 1 mol methyl methacrylate (MMA) solution of 1 wt% AIBN was freeze-degassed three times under a nitrogen stream to prepare an AIBN mixture, which was then added dropwise to the catalyst mixture over a period of 5 hours while maintaining the temperature at 80°C. After the dropwise addition, the mixture was maintained at 80°C for another hour to obtain a polymerization mixture. The resulting polymerization mixture was cooled to room temperature, and MEK was distilled off with an evaporator. The residue was dissolved in toluene, and MMA trimer was obtained by silica gel column chromatography using toluene as a developing solvent. 1 The purity was confirmed by H-NMR.

[0070] [Production Example 2: Production of MMA dimer to tridecamer] The polymerization mixture obtained in Production Example 1 was cooled to room temperature, and then MEK was removed by distillation using an evaporator. 1 The purity was confirmed by H-NMR.

[0071] [Production Example 3: Production of MMA octamer] The polymerization mixture obtained in Production Example 1 was cooled to room temperature, and then MEK was removed by an evaporator. The residue was dissolved in toluene, and subjected to silica gel column chromatography using toluene as a developing solvent to obtain an MMA octamer. 1 The purity was confirmed by H-NMR.

[0072] [Production Example 4: Production of BMA trimmer] A BMA trimer was obtained in the same manner as in Production Example 1, except that n-butyl methacrylate (BMA) was used as the monomer. The purity was 1 This was confirmed by H-NMR.

[0073] [Example 1] In a polymerization apparatus equipped with a stirrer, a cooling tube, and a thermometer, a monomer mixture in which 60 parts by mass of styrene, 10 parts by mass of methyl methacrylate, and 30 parts by mass of methacrylic acid were uniformly dissolved; 0.25 parts by mass of 2,2'-azobis(2-methylbutyronitrile) as a polymerization initiator; 4 parts by mass of MMA trimer as a chain transfer agent; 200 parts by mass of pure water in which 0.8 parts by mass of dispersant (1) and 0.3 parts by mass of sodium sulfate as a dispersion aid were uniformly dissolved; and nitrogen substitution was performed while stirring. Then, suspension polymerization was started at 75°C, and after the peak of polymerization heat was detected, polymerization was further performed at 85°C for 30 minutes (polymerization process). After the polymerization, the inside of the vessel was cooled to room temperature, and the resulting slurry was dehydrated by a centrifugal dehydrator (first dehydration step). The obtained vinyl polymer and pure water as a washing liquid were charged into a washing tank so that the mass ratio (vinyl polymer particles:washing liquid) was 1:2, and the mixture was stirred and mixed for 20 minutes to wash (washing step), and then dehydrated using a centrifugal dehydrator (second dehydration step). After dehydration, the dehydrated vinyl polymer particles were placed in a fluidized-tank dryer with an internal temperature set at 50° C., and dried until the moisture content reached 5% or less (drying step). The obtained powdery vinyl polymer particles were evaluated for solubility in solvents and solubility in alkaline water. The results are shown in Table 1.

[0074] [Examples 2 to 23, Comparative Examples 1 to 3] Powdered vinyl polymers were produced in the same manner as in Example 1 except that the raw material composition ratios shown in Tables 1 to 3 were used, and various measurements and evaluations were carried out. The results are shown in Tables 1 to 3.

[0075] [Table 1]

[0076] [Table 2]

[0077] [Table 3]

[0078] The abbreviations used in Tables 1 to 3 are as follows. St: styrene MAA: Methacrylic acid MMA: Methyl methacrylate BzMA: benzyl methacrylate BA: n-butyl acrylate iBMA: i-Butyl methacrylate PGM: Propylene glycol monomethyl ether tDM: t-dodecyl mercaptan nDM: n-dodecyl mercaptan OTG: 2-ethylhexyl thioglycolate MMA trimer (MMA dimer: MMA trimer: MMA tetramer: MMA pentamer = 1.9: 97.1: 0.7: 0.3 (mass ratio)) MMA octamer (MMA hexamer: MMA heptamer: MMA octamer: MMA nonamer = 0.5:17.1:70.5:11.9 (mass ratio)) MMA2-13mer (MMA dimer: MMA trimer: MMA tetramer: MMA pentamer: MMA hexamer: MMA heptamer: MMA octamer: MMA nonamer: MMA decamer: MM A11-mer: MMA12-mer: MMA13-mer = 1.9:95.2:0.7:0.4:0.5:0.3:0.1:0.1:0.3:0.2:0.2:0.1 (mass ratio)) BMA trimer (BMA dimer:BMA trimer:BMA tetramer = 15.9:83.8:0.3 (mass ratio))

[0079] As is clear from the results in Tables 1 to 3, the vinyl polymers obtained in Examples 1 to 23 were excellent in solubility in solvents and alkaline water, and had low odor.

[0080] The vinyl polymer obtained in Comparative Example 1 had a strong and unpleasant odor since it did not have a structure derived from one or more of the trimers to 20mers of a (meth)acrylic monomer as the terminal structure of the polymer. The vinyl polymers obtained in Comparative Examples 2 and 3 had acid values ​​outside the range specified in the present application, and therefore had poor solubility in alkaline water.

[0081] [Example 24, Comparative Examples 2 to 3] The vinyl polymers (a) and (z), the compound having a polymerizable double bond (b), the photopolymerization initiator (c) and the dye (d) were dissolved in an organic solvent (e) in the composition shown in Table 2 to prepare a coating liquid which is a curable composition. The compatibility was evaluated according to the following criteria.

[0082] (Combination Appropriateness Evaluation Criteria) A: The coating solution is neither cloudy nor has any lumps, and is in good condition. B: The coating solution is slightly cloudy. C: The coating solution is very cloudy and some of the coating material remains undissolved.

[0083] The obtained coating solution was applied onto a 20 μm thick PET film (Mitsubishi Chemical Corporation, Diafoil R310-16, polyethylene terephthalate) using an applicator. The PET film coated with the coating solution was left at room temperature for 30 minutes, and then dried in a 50° C. dryer for 30 minutes to form a 30 μm photosensitive layer, thereby obtaining a photosensitive film. The photosensitive film was heat-laminated onto a copper-clad laminate so that the PET film was on the outside, to obtain a test plate. The lamination conditions were a roll temperature of 100° C., a roll speed of 1 m / min, and a pressure of 0.3 MPa. The photosensitive film of the test plate was exposed to light using a parallel exposure machine with a high-pressure mercury lamp as the light source, with a photomask of a specified shape attached to it. The exposure energy was 30 mJ / cm. 2 After the exposure, the PET film was peeled off, and the unexposed parts were dissolved and removed by developing with a developer of 1% by mass of sodium carbonate aqueous solution, to obtain a circuit pattern made of a cured product of the curable composition. The development was performed by spraying the developer at a developer temperature of 30°C. The resolution and developability were evaluated according to the following criteria.

[0084] (Resolution Evaluation Criteria) A: A circuit pattern remains when a photomask with a line width (L) / space width (S) (hereafter abbreviated as L / S) of 30 μm / 30 μm is used and the development time is 1.5 times the minimum time required to develop the unexposed areas. B: When a photomask with an L / S of 30 μm / 30 μm is used and development is performed for 1.5 times the minimum time required to develop the unexposed areas, no circuit pattern remains. C: The cured product was not soluble in alkaline water, so it could not be developed and therefore could not be evaluated.

[0085] (Developability Evaluation Criteria) A: The minimum time required for development of the unexposed areas is less than 60 seconds. B: The minimum time required for development of the unexposed areas is 60 seconds or more. C: The cured product was not soluble in alkaline water and therefore could not be developed and could not be evaluated.

[0086] [Table 4]

[0087] The abbreviations used in Table 4 are as follows: (a)-1: Vinyl polymer obtained in Example 2 (z)-1: Vinyl polymer obtained in Comparative Example 2 (z)-2: Vinyl polymer obtained in Comparative Example 3 (b)-1: Bisphenol A dimethacrylate with 10 moles of ethylene oxide added (manufactured by Shin-Nakamura Chemical Co., Ltd., product name: NK Ester BPE500) (b)-2: Trimethylolpropane EO modified triacrylate (Toyo Chemicals Co., Ltd., product name: Miramer M3130) (c)-1: 2,2'-bis(2-chlorophenyl)-4,4',5,5'-tetraphenyl-1,2'-biimidazole (c)-2: 4,4'-bis(diethylamino)benzophenone (d)-1: Leuco Crystal Violet (d)-2: Malachite Green (e)-1: Methyl ethyl ketone (e)-2: Methanol

[0088] As is clear from the results in Table 4, Example 24 was excellent in blending suitability, resolution and developability.

[0089] In Comparative Examples 2 and 3, the cured products were not soluble in alkaline water, and therefore development was not possible, and the resolution and developability could not be evaluated. [Industrial Applicability]

[0090] According to the present invention, it is possible to provide a polymer which can be used in a curable composition and a cured product thereof, which is soluble in a solvent and has a low odor and can reduce the burden on the working environment.

Claims

1. Methyl acrylate, ethyl acrylate, n-butyl acrylate, i-butyl acrylate, t-butyl acrylate, 2-ethylhexyl acrylate, lauryl acrylate, dodecyl acrylate, stearyl acrylate, 2-methoxyethyl acrylate, 2-ethoxyethyl acrylate, methyl methacrylate, ethyl methacrylate, n-butyl methacrylate, i-butyl methacrylate, t-butyl methacrylate, 2-ethylhexyl methacrylate, cyclohexyl methacrylate, lauryl methacrylate the terminal structure being derived from one or more of a trimer to a decamer of a (meth)acrylic monomer selected from the group consisting of 2-methyl-3-propanediol, dodecyl methacrylate, stearyl methacrylate, behenyl methacrylate, 2-methoxyethyl methacrylate, 2-ethoxyethyl methacrylate, phenoxyethyl methacrylate, 2-methacryloyloxyethyl hexahydrophthalate, and 2-methacryloyloxyethyl phthalate; the acid value being 35 to 300 mgKOH / g, the mass average particle size being 20 to 2000 μm, and the water content being 5.0% by weight or less; A vinyl polymer that does not contain an epoxy group-containing vinyl monomer.

2. The vinyl polymer according to claim 1 , wherein the terminal structure is derived from a chain transfer agent.

3. 3. The vinyl polymer according to claim 1, further comprising structural units derived from two or more types of vinyl monomers.

4. The vinyl polymer according to claim 3, wherein at least one of the vinyl monomers is a vinyl monomer having an acid group.

5. 5. The vinyl polymer according to claim 3, wherein at least one of the vinyl monomers has an aromatic ring.

6. The vinyl polymer according to any one of claims 3 to 5, wherein at least one of the vinyl monomers is a (meth)acrylic monomer.

7. The vinyl polymer according to claim 6, wherein the (meth)acrylic monomer in the vinyl monomer is a (meth)acrylic acid alkyl ester, and the alkyl group in the ester structure of the (meth)acrylic acid alkyl ester has 1 to 18 carbon atoms.

8. The vinyl polymer according to any one of claims 1 to 7, having a weight average molecular weight of 5,000 to 1,000,000.

9. A curable composition comprising the vinyl polymer according to any one of claims 1 to 8 and a compound having a polymerizable double bond.

10. The curable composition according to claim 9, further comprising at least one 3-20-mer of a (meth)acrylic monomer.

Citation Information

Patent Citations

  • Granular vinyl polymer

    JP1995102004A

  • Chain transfer agent

    JP1999124402A

  • Branched polymer synthesis

    JP2000514845A

  • Chain transfer agent and polymerization method using the same

    JP2006176587A

  • Particulate vinyl polymer and thermosetting resin composition

    JP2006282935A