Aluminum member and manufacturing method thereof
The aluminum member with a porous layer and surface structure addresses quality issues in nitrocellulose filters by enhancing capillary action and visibility, making it suitable for immunochromatography and other applications.
Patent Information
- Application Number
- JP2023038925
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2018-09-19
- Filing Date
- 2023-03-13
- Publication Date
- 2024-10-08
- Estimated Expiration
- 2039-09-18
AI Technical Summary
Nitrocellulose membrane filters used in immunochromatography tests suffer from quality variations in pore sizes and thickness, leading to uneven liquid flow and affecting test results, and they also lack storage stability.
An aluminum member with a porous layer comprising a metal aluminum base material and an aluminum oxide film, featuring a surface structure with recesses and protrusions, and a tertiary rough surface structure, enhancing capillary action and visibility.
The aluminum member provides high whiteness, effective water wicking performance, and improved test result visibility, suitable for immunochromatography and other applications.
Smart Images

Figure 0007563515000002 
Figure 0007563515000003 
Figure 0007563515000004
Abstract
Description
[Technical field]
[0001] The present invention relates to an aluminum member and a manufacturing method thereof. [Background technology]
[0002] Conventionally, a test kit using immunochromatography has been known as an in vitro diagnostic drug for quickly and simply testing for infection with, for example, influenza virus, etc. In this test kit, for example, a specimen collected from a living body is dropped onto a predetermined position, and if both the test line and the control line can be visually confirmed, it indicates a positive result, and if only the control line can be visually confirmed, it indicates a negative result.
[0003] The test kit includes a nitrocellulose membrane filter as a spreading member for spreading a specimen, as shown in Patent Document 1. The collected specimen flows through the membrane filter by capillary action and spreads to the test line and the control line. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2003-344406 A Summary of the Invention
[0005] Nitrocellulose membrane filters generally have a high degree of whiteness, making it relatively easy to visually confirm the test line and control line, and are therefore used in many test kits.
[0006] However, nitrocellulose membrane filters tend to have large variations in quality, such as uneven pore size and thickness depending on the production date, production location, production lot, etc. If there is a large variation in quality, the flow rate of the liquid flowing due to capillary action is likely to be uneven, which may adversely affect the test results.
[0007] In addition, nitrocellulose membrane filters generally have poor storage stability, and therefore there is a demand for a development member that has high whiteness and storage stability and can replace the nitrocellulose membrane filter.
[0008] The present invention has been made in view of the problems inherent in the conventional techniques, and an object of the present invention is to provide an aluminum member having high whiteness and water wicking performance, and a method for manufacturing the same.
[0009] According to an aspect of the present invention For immunochromatography The aluminum member has a porous layer including a base material made of metallic aluminum and a coating containing aluminum oxide that covers the surface of the base material. The coating has a thickness of 5 nm to 1000 nm, and the coating has at least one of a plurality of recesses and a plurality of protrusions formed on the surface. The depth of each of the recesses is 10 nm to 100 nm, and the height of each of the protrusions is 10 nm to 100 nm. The porous layer has a plurality of pores, and the average pore size of the plurality of pores is 0.1 μm to 10 μm. The diameter of each recess is 10 nm to 200 nm, and may be smaller than the average pore diameter of the porous layer. The diameter of each projection may be from 10 nm to 200 nm. The aluminum component for immunochromatography may have a primary rough surface structure formed by a coating and at least one of a plurality of recesses and a plurality of protrusions, a secondary rough surface structure formed by a base material and a plurality of pores, and a tertiary rough surface structure consisting of an assembly of the primary rough surface structure and the secondary rough surface structure. The aluminum member for immunochromatography may have an arithmetic mean roughness Sa of 0.1 μm to 30 μm. Aluminum components for immunochromatography are L * a * b * L in color space * The value may be 80 or greater. The aluminum component for immunochromatography may have a water uptake height by capillary action of 3 cm or more. Aluminum components for immunochromatography may be bent 100 or more times without breaking in a bending test based on the MIT bending test method. The aluminum component for immunochromatography may further include a substrate made of metallic aluminum, and a porous layer may be provided on at least one surface of the substrate.
[0010] According to an aspect of the present invention For immunochromatography The method for manufacturing an aluminum member includes a film formation step of anodizing an aluminum plate having a porous structure to form a film containing aluminum oxide on the aluminum plate. For immunochromatography The method for manufacturing an aluminum member includes a depolarization treatment step of depolarizing an aluminum plate having a coating formed thereon and removing a part of the surface of the coating. The coating formation step and the depolarization treatment step are repeated alternately. The aluminum plate is made of metal aluminum. At least one of a plurality of recesses and a plurality of protrusions is formed on the surface of the film by the film forming step and the depolarization treatment step. The film has a thickness of 5 nm to 1000 nm. The depth of each of the recesses is 10 nm to 100 nm. The height of each of the protrusions is 10 nm to 100 nm. The aluminum component for immunochromatography has a plurality of pores, and the average pore diameter of the plurality of pores is 0.1 μm to 10 μm. The method for producing an aluminum member for immunochromatography may further include an etching step, prior to the film-forming step, of etching the aluminum plate to form a porous structure in the aluminum plate. The method for producing an aluminum component for immunochromatography may further include a hydration treatment step, prior to the film-forming step, of hydrating the aluminum plate to form a hydrated film on the aluminum plate having a porous structure. At least one of a plurality of recesses and a plurality of protrusions may be formed on the surface of the coating by the coating formation process and the depolarization treatment process, and at least one of the plurality of recesses and a plurality of protrusions may be formed by alternately repeating the coating formation process and the depolarization treatment process two or more times. At least one of the plurality of recesses and the plurality of protrusions may be formed by alternately repeating the film formation step and the depolarization treatment step five or more times. When the film forming step and the depolarization treatment step are alternately repeated, the treatment time for one depolarization treatment in the depolarization treatment step may be 20 minutes to 60 minutes. [Brief description of the drawings]
[0011] [Figure 1] FIG. 1 is a schematic cross-sectional view showing a tertiary rough surface structure of a porous layer according to the present embodiment, in which a part of the porous layer is enlarged. [Diagram 2] FIG. 2 is a schematic cross-sectional view showing the primary rough surface structure and the secondary rough surface structure of the porous layer, in which the framed portion in FIG. 1 is enlarged. [Diagram 3] FIG. 3 is a schematic cross-sectional view showing another example of the primary rough surface structure and the secondary rough surface structure of the porous layer. [Figure 4] FIG. 4 is a schematic cross-sectional view showing another example of the primary rough surface structure and the secondary rough surface structure of the porous layer. [Diagram 5] FIG. 5 is a cross-sectional view showing an example of the aluminum member according to the present embodiment. [Figure 6] FIG. 6 is a perspective view showing an example of a test kit using the aluminum member according to this embodiment. [Figure 7] FIG. 7 is a photograph of the surface of the etched aluminum plate observed with a scanning electron microscope (SEM). [Figure 8]FIG. 8 is a photograph of the surface of the aluminum member according to Example 3 observed with a scanning electron microscope. [Figure 9] FIG. 9 is a photograph of the surface of the aluminum member according to Example 10 observed with a scanning electron microscope. [Figure 10] FIG. 10 is a photograph of the surface of the aluminum member according to Comparative Example 3 observed with a scanning electron microscope. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0012] The aluminum member and the manufacturing method thereof according to the present embodiment will be described in detail below with reference to the drawings. The present invention is not limited to the following embodiment. In addition, the components in the embodiment can be combined in part or in whole as appropriate. Note that the dimensional ratios in the drawings are exaggerated for the sake of explanation and may differ from the actual ratios.
[0013] [Aluminum parts] In this embodiment, we investigated whether an aluminum member having a porous structure can be used as an alternative to a nitrocellulose membrane filter. However, it is generally considered difficult to make an aluminum member exhibit a capillary phenomenon sufficient for immunochromatography. In addition, aluminum members are generally gray in color, making it difficult to confirm the color of test lines and control lines.
[0014] However, it has been found that the aluminum member according to the present embodiment described in detail below has high whiteness and high water absorption performance. Such an aluminum member is expected to be useful not only as a replacement for nitrocellulose membrane filters, but also for various other applications.
[0015] FIG. 1 is a schematic cross-sectional view of a part of the porous layer 40 according to the present embodiment, in which a part surrounded by a frame in FIG. 1 is enlarged. FIGS. 2 to 4 are schematic cross-sectional views showing the primary rough surface structure 10 and the secondary rough surface structure 20 of the porous layer 40, in which a part surrounded by a frame in FIG. 1 is enlarged. As shown in FIG. 1, the aluminum member 100 according to the present embodiment includes a porous layer 40. As shown in FIGS. 2 to 4, the porous layer 40 includes a base material 11 and a coating 12. In the porous layer 40, the coating 12 is in contact with the base material 11, and is disposed on the outer surface side of the aluminum member 100. The coating 12 has at least one of a recess 13 (first recess) and a protrusion 14 (first protrusion) on its surface. The porous layer 40 has a plurality of pores 15.
[0016] <Rough surface structure> The aluminum member 100 has a rough surface structure on its surface. The rough surface structure refers to a surface structure having a plurality of irregularities on the surface, making the surface rougher than a smooth surface. Preferably, the rough surface structure refers to one in which at least one of the concave portions 13 and the convex portions 14 is distributed and arranged on the surface of the aluminum member 100. It is preferable that the rough surface structure on the surface of the aluminum member 100 does not have needle-shaped or plate-shaped irregular structures arranged thereon. The rough surface structure of the aluminum member 100 can be expressed by a primary rough surface structure 10, a secondary rough surface structure 20, and a tertiary rough surface structure 30 in order of increasing scale of surface roughness. That is, the scale of the surface roughness of the secondary rough surface structure 20 is larger than that of the primary rough surface structure 10, and the scale of the surface roughness of the tertiary rough surface structure 30 is larger than that of the secondary rough surface structure 20. As described later, it is presumed that the whiteness of the aluminum member 100 is increased by having the primary rough surface structure 10, the secondary rough surface structure 20, and the tertiary rough surface structure 30.
[0017] 2 to 4, the primary rough surface structure 10 is a fine rough surface structure formed by a coating 12 and at least one of a plurality of recesses 13 and a plurality of protrusions 14 present on the surface of the coating 12. The primary rough surface structure 10 is formed on the surface of the coating 12. The primary rough surface structure 10 has a structure in which the surface roughness scale is on the order of several nm to several hundreds of nm.
[0018] As shown in Figs. 2 to 4, the secondary rough surface structure 20 is a rough surface structure formed by the base material 11 and a plurality of pores 15 in the porous layer 40. That is, the secondary rough surface structure 20 is formed by a convex portion 21 (second convex portion, protruding portion) and a concave portion 22 (second concave portion, recessed portion). The convex portion 21 is formed by the base material 11 and the coating 12, and protrudes toward the outside of the porous layer 40. The concave portion 22 is formed by the base material 11 and the coating 12, and recesses toward the inside of the porous layer 40. The pores 15 are formed by the internal space of the porous layer 40 surrounded by the base material 11 and the coating 12 that form the concave portion 22. In other words, the secondary rough surface structure 20 is formed on the surface of the aluminum member 100 by the base material 11 and the coating 12 themselves. The secondary rough surface structure 20 is a structure in which the scale of the surface roughness is on the order of several hundreds of nm to several tens of µm.
[0019] In this way, the porous layer 40 is a porous body having pores 15 inside that communicate with the outside. At this time, the pores 15 are surrounded by the film 12. That is, the recesses 13 and the protrusions 14 of the primary rough surface structure 10 are formed in the film 12 on the surface of the porous layer 40, while the pores 15 of the secondary rough surface structure 20 are formed surrounded by the base material 11 inside the porous layer 40 and the film 12 covering the surface of the base material 11. The pores 15 forming one cell structure surrounded by the film 12 may communicate with the pores 15 forming another cell structure. Specifically, the porous layer 40 may have an open cell structure. The pores 15 may or may not penetrate from one surface to the other surface of the porous layer 40.
[0020] As shown in FIG. 1, the tertiary rough surface structure 30 is formed by the outer surface of the porous layer 40. The tertiary rough surface structure 30 is a coarse rough surface structure formed by a collection of multiple irregularities due to the primary rough surface structure 10 and the secondary rough surface structure 20. The tertiary rough surface structure 30 is an aggregate of the primary rough surface structure 10 and the secondary rough surface structure 20 on the surface of the aluminum member 100. As will be described later, the tertiary rough surface structure 30 is formed by repeating the film formation process and the depolarization treatment process after the etching process, thereby developing an irregular structure consisting of an aggregate of the primary rough surface structure 10 and the secondary rough surface structure 20. The tertiary rough surface structure 30 is a structure with a surface roughness scale on the order of several tens of μm to several hundreds of μm.
[0021] As shown in FIG. 1, a tertiary rough surface structure 30 consisting of an assembly of a primary rough surface structure 10 and a secondary rough surface structure 20 forms an uneven structure on the surface of an aluminum member 100. Specifically, the tertiary rough surface structure 30 has convex portions 31 (third convex portions, mountain portions) and concave portions 32 (third concave portions, valley portions) formed by the assembly of the primary rough surface structure 10 and the secondary rough surface structure 20. The convex portions 31 rise like mountains in the thickness direction of the surface of the aluminum member 100, and the concave portions 32 drop like valleys in the thickness direction of the surface of the aluminum member 100. These convex portions 31 and concave portions 32 appear repeatedly at intervals, so that the tertiary rough surface structure 30 has a periodic mountain-valley structure on a larger scale than the primary rough surface structure 10 and the secondary rough surface structure 20.
[0022] The period of the tertiary rough surface structure 30 is preferably 10 μm to 500 μm, and more preferably 30 μm to 200 μm. The period of the tertiary rough surface structure 30 refers to the interval between adjacent convex portions 31 that appear periodically with a concave portion 32 sandwiched therebetween in the planar direction of the aluminum member 100, or between adjacent concave portions 32 that appear periodically with a convex portion 31 sandwiched therebetween. By setting the period of the tertiary rough surface structure 30 within this range, it is possible to provide an aluminum member 100 with better whiteness. The period of the tertiary rough surface structure 30 can be measured by observing a cross section of the aluminum member 100 with an optical microscope or the like.
[0023] By having the above-mentioned tertiary rough surface structure 30, the aluminum member 100 has a reduced glossy appearance and an improved matte appearance on the surface. This suppresses the gloss on the surface of the aluminum member 100, improving the visibility of information such as colors, patterns, figures, symbols, and characters presented on the aluminum member 100. Such improved visibility is effective, for example, when the aluminum member 100 is used as a test sheet or a developing member for chromatography, and test results generated on the aluminum member 100 are visually or optically confirmed.
[0024] <Base material> The base material 11 is made of metallic aluminum. The metallic aluminum constituting the base material 11 is preferably pure aluminum having a purity of 99% or more, more preferably pure aluminum having a purity of 99.9% or more, and even more preferably pure aluminum having a purity of 99.98% or more.
[0025] The base material 11 may contain unavoidable impurities. In this embodiment, the unavoidable impurities refer to those that are present in raw materials or that are inevitably mixed in during the manufacturing process. Although the unavoidable impurities are essentially unnecessary, they are permitted because they are present in trace amounts and do not affect the properties of the aluminum. The unavoidable impurities that may be contained in the aluminum are elements other than aluminum (Al). Examples of the unavoidable impurities that may be contained in the aluminum include magnesium (Mg), iron (Fe), silicon (Si), copper (Cu), lead (Pb), manganese (Mn), chromium (Cr), zinc (Zn), titanium (Ti), gallium (Ga), boron (B), vanadium (V), zirconium (Zr), calcium (Ca), and cobalt (Co). The amount of the unavoidable impurities in the aluminum is preferably 1% by mass or less in total, more preferably 0.1% by mass or less, and even more preferably 0.02% by mass or less.
[0026] The shape of the base material 11 is not particularly limited, and may be porous, dendritic, fibrous, lumpy, spongy, or the like.
[0027] <Coating> The coating 12 covers the surface of the base material 11. Specifically, the coating 12 is in contact with the surface and pores 15 of the base material 11, and inhibits the base material 11 from corroding.
[0028] The coating 12 contains aluminum oxide. In this embodiment, the coating 12 is an anodized coating, and the anodized coating is preferably a barrier-type anodized coating. The coating 12 may also contain aluminum hydroxide. The coating 12 may have a hydrated coating containing aluminum hydroxide.
[0029] For example, the coating 12 may be a laminate of an anodized film and a hydrated film in this order from the base material 11 side, but it is preferable that the hydrated film is provided on a part of the surface side of the anodized film that covers the surface of the base material 11. Alternatively, the coating 12 may be a laminate of an anodized film and a hydrated film distributed in a sea-island shape on the surface of the base material 11, but it is preferable that the anodized film is distributed in a sea-like shape and the hydrated film is distributed in an island-like shape on the surface of the base material 11. Specifically, the ratio of the hydrated film to the entire outer surface of the coating 12 is preferably 5% to 50%, more preferably 10% to 40%, and even more preferably 15% to 30%. Note that when the coating 12 contains aluminum hydroxide and aluminum hydroxide is present in a part of the outermost surface of the base material 11 and the porous layer 40, it is preferable that the aluminum hydroxide forms the protrusions 14.
[0030] It is preferable that the porous layer 40 according to this embodiment does not include a hydration film covering the base material 11 and the porous layer 40 over the entire outermost surface. When the porous layer 40 does not include a hydration film over the entire outermost surface, diffuse reflection becomes dominant, and the whiteness of the aluminum member 100 can be further improved. Aluminum hydroxide is represented by the general formula Al(OH)3.
[0031] When the outermost surface of the coating 12 is covered with a needle-shaped or plate-shaped hydrated coating, the aluminum member 100 may be observed to be black or gray. This is thought to be because such a hydrated coating has a sharp tip near the surface, and although this tip contributes to the diffuse reflection of incident light, the part that can diffusely reflect light is limited to the tip, and the area is small. In addition, such a coating has an internal shape in which the space between adjacent needle-shaped or plate-shaped hydrated coatings gradually narrows from the tip to the base. Therefore, incident light that penetrates the inside is absorbed by the hydrated coating as it is repeatedly reflected, and the light is difficult to emit to the outside, which is also thought to affect the aluminum member 100 being observed to be black or gray.
[0032] Furthermore, when a hydrated film is present, the primary rough surface structure 10 and the secondary rough surface structure 20 are often clogged, so that the aluminum member 100 tends to have a black or gray appearance. Therefore, it is preferable that the film 12 made of an anodized film is provided on the surface of the porous layer 40, and the recesses 13 and pores 15 are present on the outermost surface of the film 12. On the other hand, when aluminum hydroxide does not cover the entire outermost surface of the porous layer 40 to form a hydrated film, but exists in a granular or lumpy form on a part of the outermost surface of the porous layer 40 to form protrusions 14, the whiteness can be improved by the protrusions 14. Furthermore, the whiteness can be improved by the protrusions 14 and the recesses 13 exposed on the outermost surface of the porous layer 40 without being covered by the hydrated film. When aluminum hydroxide covers the entire outermost surface of the porous layer 40 to form a hydrated film and exists in a granular or lumpy form on the outermost surface of the porous layer 40 to form protrusions 14, the whiteness can be improved by the protrusions 14.
[0033] The coating 12 usually has a thickness of 5 nm to 1000 nm. The thickness of the coating 12 is preferably 20 nm to 800 nm, more preferably 30 nm to 500 nm, and further preferably 50 nm to 300 nm. By setting the thickness of the coating 12 in such a range, it becomes easier to ensure a sufficient thickness to diffusely reflect the light incident on the porous layer 40, and it is possible to provide an aluminum member 100 with a better whiteness. Furthermore, it is possible to provide an aluminum member 100 with sufficiently high corrosion resistance. The thickness of the coating 12 can be measured, for example, by observing a cross section of the coating 12 with a scanning electron microscope or the like. In this specification, the thickness of the coating 12 means a thickness excluding the recesses 13 and the protrusions 14.
[0034] The coating 12 has at least one of a plurality of recesses 13 and a plurality of protrusions 14 formed on the surface. Specifically, as shown in FIG. 2, the coating 12 may have a plurality of recesses 13 on the surface of the coating 12. Alternatively, as shown in FIG. 3, the coating 12 may have a plurality of protrusions 14 on the surface of the coating 12. Alternatively, as shown in FIG. 4, the coating 12 may have recesses 13 and protrusions 14 on the surface of the coating 12. That is, the coating 12 may have either the recesses 13 or the protrusions 14, or may have both the recesses 13 and the protrusions 14. The presence or absence of the recesses 13 or the protrusions 14 can be determined by observing the surface of the coating 12 with a scanning electron microscope or the like.
[0035] The recesses 13 and the protrusions 14 contribute to the whiteness of the aluminum member 100. The reason why the whiteness of the aluminum member 100 is improved by forming at least one of the recesses 13 and the protrusions 14 on the surface of the coating 12 is not necessarily clear, but is presumed to be as follows. First, when light is incident on the aluminum member, the incident light is reflected by the surface of the aluminum member. At this time, if the surface of the aluminum member is smooth, it will exhibit a mirror-like luster. Here, if the surface of the aluminum member has fine irregularities, the unevenness causes diffuse reflection of the incident light, but usually there are no irregularities that are visible as white.
[0036] In contrast, the aluminum member 100 according to this embodiment can increase the diffuse reflection on the surface of the coating 12 by the recesses 13 and the protrusions 14. That is, when the coating 12 has recesses 13, the area that can diffusely reflect incident light is increased by the recesses 13, and the aluminum member 100 is observed to have a white color. Similarly, when the coating 12 has protrusions 14, the area that can diffusely reflect incident light is increased by the protrusions 14, and the aluminum member 100 is observed to have a white color.
[0037] The recess 13 is preferably formed by being recessed from the exposed surface of the coating 12 toward the base material 11. The bottom of the recess 13 does not penetrate to the base material 11, and the coating 12 is preferably formed between the recess 13 and the base material 11. The shape of the recess 13 is not particularly limited, but is preferably approximately U-shaped or approximately V-shaped in cross section in the lamination direction of the base material 11 and the coating 12 (thickness direction of the coating 12). As described later, the etched aluminum plate is anodized and depolarized to generate the coating 12 made of an anodized coating on the surface of the base material 11. The recess 13 is formed in this anodized coating. The protrusion 14 is preferably formed by protruding outward from the exposed surface of the coating 12. The shape of the protrusion 14 is not particularly limited, but is preferably granular or lumpy.
[0038] The diameter of each of the recesses 13 included in the plurality of recesses is preferably 10 nm to 200 nm, more preferably 20 nm to 150 nm, and even more preferably 50 nm to 100 nm. The diameter of each of the protrusions 14 included in the plurality of protrusions is preferably 10 nm to 200 nm, more preferably 20 nm to 150 nm, and even more preferably 50 nm to 100 nm. By setting the diameters of the recesses 13 and the protrusions 14 in such ranges, the light incident on the porous layer 40 is easily diffused and reflected by the recesses 13 and the protrusions 14, and an aluminum member 100 with better whiteness can be provided. The diameter of the recesses 13 can be obtained by observing the surface of the coating 12 with a scanning electron microscope or the like and measuring the diameter of the inlet portion of the recesses 13. The diameter of the protrusions 14 can be obtained by observing the surface of the coating 12 with a scanning electron microscope or the like and measuring the diameter of the portion where the diameter of the protrusions 14 is the largest.
[0039] Here, the determination of the recess 13 and its diameter when multiple recesses 13 are close to each other will be described. First, the position of the recess 13 is determined by the deepest position (peak position on the bottom side) of the recess 13. The interval between adjacent recesses 13 can be determined by the distance between the peak positions on the bottom side of each recess 13. When a certain recess 13 exists at an interval of 50 nm or more from the surrounding recesses 13, this recess 13 is considered to be an independent recess 13. On the other hand, when a group of multiple recesses 13 is gathered at an interval of less than 50 nm and forms a group that exists at an interval of 50 nm or more from the surrounding recesses 13 that are not included in the group, this group is considered to be one recess 13. Then, the diameter of the entire group is measured as the diameter of the recess 13. Note that when multiple recesses 13 share the periphery of a depression and the bottom side peak positions of these multiple recesses 13 are 50 nm or more apart, these multiple recesses 13 are considered to be separate and independent recesses 13. At this time, for the depressions sharing the same periphery, a Voronoi division is performed using the peak positions on the bottom side of the multiple recesses 13 as generating points, thereby making it possible to define the regions belonging to each recess 13.
[0040] Similarly, the determination of the convex portion 14 and its diameter when multiple convex portions 14 are close to each other will be described. First, the position of the convex portion 14 is determined by the highest position (peak position on the top side) of the convex portion 14. The interval between adjacent convex portions 14 can be determined by the distance between the peak positions on the top side of each convex portion 14. When a certain convex portion 14 exists at an interval of 50 nm or more from the surrounding convex portions 14, this convex portion 14 is considered to be an independent convex portion 14. On the other hand, when a group of multiple convex portions 14 is gathered at an interval of less than 50 nm and forms a group that exists at an interval of 50 nm or more from the surrounding convex portions 14 that are not included in the group, this group is considered to be one convex portion 14. Then, the diameter of the entire group is measured as the diameter of the convex portion 14. Note that when multiple convex portions 14 share the peripheral portion of the overhang and the peak positions on the top side of these multiple convex portions 14 are 50 nm or more apart, these multiple convex portions 14 are considered to be separate and independent convex portions 14. In this case, for the protrusions that share a common peripheral portion, a Voronoi division is performed using the peak positions on the top sides of the multiple protrusions 14 as generating points, thereby making it possible to define the areas belonging to each protrusion 14.
[0041] The depth of each of the recesses 13 included in the plurality of recesses is typically 10 nm to 100 nm, preferably 20 nm to 80 nm, and more preferably 30 nm to 50 nm, in a cross-sectional view in the stacking direction of the base material 11 and the coating 12. The depth of the recesses 13 can be obtained by observing the cross-section of the coating 12 with a scanning electron microscope or the like and calculating the average value of the distances measured from the entrances to the bottoms of the recesses 13.
[0042] The height of each of the protrusions 14 included in the multiple protrusions is typically 10 nm to 100 nm, preferably 20 nm to 80 nm, and more preferably 30 nm to 50 nm, in a cross-sectional view in the lamination direction of the base material 11 and the coating 12. The height of the protrusions 14 can be obtained by observing the cross-section of the coating 12 with a scanning electron microscope or the like and calculating the average value of the distances measured from the surface of the flat part of the coating 12 to the tops of the protrusions 14.
[0043] When the depth of the recess 13 and the height of the protrusion 14 exceed the lower limit of the above range, the area that can diffusely reflect the incident light by the recess 13 and the protrusion 14 increases, and the diffuse reflection is likely to increase. When the depth of the recess 13 and the height of the protrusion 14 are below the upper limit of the above range, the decrease in diffuse reflection caused by the recess 13 and the protrusion 14 becoming, for example, a needle-like or plate-like uneven structure can be suppressed. The decrease in diffuse reflection is considered to be due to the decrease in the area that can diffusely reflect the incident light and the absorption of the incident light caused by the needle-like or plate-like uneven structure. In this way, when the depth of the recess 13 and the height of the protrusion 14 are within the above range, the aluminum member 100 tends to be observed to show a white color.
[0044] The density of the recesses 13 and the protrusions 14 in the coating 12 is 3 / μm 2 ~500 pieces / μm 2 It is preferable that the number of particles is 5 / μm. 2 ~200 pieces / μm 2 It is more preferable that the number of particles is 10 / μm. 2 ~100 pieces / μm 2 It is even more preferable that the density of the recesses 13 and the protrusions 14 is within such a range. By setting the density of the recesses 13 and the protrusions 14 in this range, light incident on the porous layer 40 can be easily diffused and reflected by the recesses 13 and the protrusions 14, making it possible to provide an aluminum member 100 with better whiteness. The density of the recesses 13 and the protrusions 14 can be obtained by counting the total number of recesses 13 and protrusions 14 per unit area on the surface of the coating 12 using a scanning electron microscope or the like.
[0045] The area ratio of the recesses 13 and the protrusions 14 in the coating 12 is preferably 5% to 80%, more preferably 20% to 70%, and further preferably 30% to 60%. By setting the area ratio of the recesses 13 and the protrusions 14 in such a range, the light incident on the porous layer 40 is easily diffused and reflected by the recesses 13 and the protrusions 14, and an aluminum member 100 having a better whiteness can be provided. The area ratio of the recesses 13 and the protrusions 14 is expressed as a percentage of the area occupied by the recesses 13 and the protrusions 14 on the surface of the porous layer 40 relative to the surface area of the coating 12. The area ratio of the recesses 13 and the protrusions 14 can be obtained by calculating the total area occupied by the recesses 13 and the protrusions 14 per unit area on the surface of the coating 12 using a scanning electron microscope or the like.
[0046] The porous layer 40 has a plurality of pores, and the average pore diameter of the plurality of pores is 0.1 μm to 10 μm. The average pore diameter of the pores 15 in the porous layer 40 is preferably 0.5 μm to 8 μm, and more preferably 1 μm to 5 μm. When the time required for the aluminum member 100 to absorb 4 cm of water is t seconds, the average pore diameter d (μm) in the porous layer 40 is preferably within the range represented by the following formula: Average pore diameter d=k / t Here, k is a constant, and specifically, k is preferably 200 to 2000, and more preferably 500 to 1500. Such pores 15 can easily ensure an appropriate diameter for sucking up water by capillary action, and can improve the water sucking performance of the aluminum member 100. The average pore diameter of the pores 15 can be measured by, for example, mercury intrusion porosimetry. The diameter of the recesses 13 or the protrusions 14 is preferably within the above-mentioned predetermined range and smaller than the average pore diameter in the porous layer 40. Specifically, the diameter of the recesses 13 is preferably 10 nm to 200 nm and smaller than the average pore diameter in the porous layer 40. The diameter of the protrusions 14 is preferably 10 nm to 200 nm and smaller than the average pore diameter in the porous layer 40.
[0047] The thickness of the porous layer 40 is preferably 30 μm to 10 cm. By setting the thickness of the porous layer 40 in this range, it becomes easier to ensure a sufficient thickness for absorbing water by capillary action, and it is possible to provide an aluminum member 100 with better whiteness and water absorbing performance. The thickness of the porous layer 40 is preferably 40 μm or more, and more preferably 50 μm or more. The thickness of the porous layer 40 is more preferably 1000 μm or less, further preferably 200 μm or less, and particularly preferably 150 μm or less.
[0048] <Substrate> 5, the aluminum member 100 may further include a substrate 50. The substrate 50 can support the porous layer 40 and can improve the rigidity of the aluminum member 100. The substrate 50 may have a layered shape.
[0049] The porous layer 40 may be provided on at least one surface of the substrate 50. Specifically, the porous layer 40 may be provided on only one surface of the substrate 50, or on both surfaces of the substrate 50. The porous layer 40 is preferably disposed on the outermost surface of the aluminum member 100.
[0050] The aluminum member 100 does not necessarily have to include the substrate 50, and therefore the thickness of the substrate 50 is greater than 0 μm. The thickness of the substrate 50 depends on the application, and may be, for example, 1 mm or less, 100 μm or less, 10 μm or less, or 1 μm or less.
[0051] The material constituting the substrate 50 may be substantially the same as the material of the base material 11. When the substrate 50 and the base material 11 are made of the same material, the substrate 50 and the base material 11 may be formed as one piece. In this case, the substrate 50 and the base material 11 of the porous layer 40 may be formed continuously. The substrate 50 may be made of metallic aluminum. The metallic aluminum constituting the substrate 50 is preferably pure aluminum having a purity of 99% or more, more preferably pure aluminum having a purity of 99.9% or more, and even more preferably pure aluminum having a purity of 99.98% or more.
[0052] The thickness of the aluminum member 100 depends on the application, but may be, for example, 50 μm or more, 100 μm or more, or 150 μm or more. The thickness of the aluminum member 100 may be 300 μm or less, 250 μm or less, or 200 μm or less. By setting the thickness of the aluminum member 100 within such a range, it is possible to provide an aluminum member 100 with good bending strength.
[0053] The arithmetic mean roughness Sa of the aluminum member 100 is preferably 0.1 μm to 30 μm, more preferably 0.6 μm to 20 μm, and further preferably 1 μm to 10 μm. By setting the arithmetic mean roughness Sa in such a range, L * The value tends to increase, making it easier to provide an aluminum member 100 with better whiteness. The arithmetic mean roughness Sa can be obtained by measuring the surface of the aluminum member 100 on the porous layer 40 side in accordance with ISO25178. Note that in this specification, the arithmetic mean roughness Sa of the aluminum member 100 mainly reflects the roughness due to the secondary rough surface structure 20.
[0054] The aluminum member 100 is L * a * b * L in color space *The value is preferably 80 or more, more preferably 85 or more, even more preferably 90 or more, and particularly preferably 95 or more. * a * b * L in color space * The value can be calculated according to JIS Z8722:2009 (Method of measuring color - Reflection and transmission object color). * The value can be measured using a color difference meter or the like under conditions such as diffuse lighting, perpendicular light receiving method (D / 0), viewing angle 2°, and C light source.
[0055] The aluminum member 100 preferably has a water wicking height of 3 cm or more, more preferably 4 cm or more, and even more preferably 5 cm or more. In this way, it is possible to provide an aluminum member 100 suitable for, for example, chromatography. The wicking height can be obtained, for example, by immersing the aluminum member 100 in pure water so that the planar direction of the aluminum member 100 is perpendicular to the liquid surface, leaving it for 10 minutes, and then measuring the height to which water has been wicked up by capillary action. The pure water has a resistivity of 10 kΩm measured at 30° C.
[0056] It is preferable that the aluminum member 100 does not break even when folded 100 times or more in a folding test based on the MIT folding test method. If the aluminum member 100 satisfies such requirements, the aluminum member 100 can be easily stored and transported in a rolled form. The MIT folding test method is specified in EIAJ RC-2364A, and the MIT folding test device used can be one specified in JIS P8115 (Paper and cardboard--Folding endurance test method--MIT testing machine method).
[0057] As described above, the aluminum member 100 according to this embodiment includes a porous layer 40 including a base material 11 made of metallic aluminum and a coating 12 containing aluminum oxide that coats the surface of the base material 11. The coating 12 has a thickness of 5 nm to 1000 nm, and the coating 12 has at least one of a plurality of recesses 13 and a plurality of protrusions 14 formed on the surface. The depth of each of the recesses 13 included in the plurality of recesses 13 is 10 nm to 100 nm, and the height of each of the protrusions 14 included in the plurality of protrusions 14 is 10 nm to 100 nm. The porous layer 40 has a plurality of pores 15, and the average pore diameter of the plurality of pores 15 is 0.1 μm to 10 μm.
[0058] Moreover, the aluminum member 100 may further include a substrate 50 made of metallic aluminum, and a porous layer 40 may be provided on at least one surface side of the substrate 50.
[0059] The aluminum member 100 of this embodiment has high whiteness and water wicking performance, but it can be used not only in applications where both of these characteristics are required, but also in applications where only one of the characteristics is required.
[0060] Examples of useful applications of the aluminum member 100 according to this embodiment include, for example, separation membranes for gas or liquid; moisture absorbing materials; water absorbing materials; adsorption materials for adsorbing foreign matter such as pollen, particulate matter, bacteria, odor components, and heavy metals; wiping sheets; test sheets for drugs such as concentrated sulfuric acid, urinalysis, and pH tests; development members for chromatography such as thin layer chromatography; materials for sterilization and disinfection; reflective materials: standard white plates; separators for batteries and electric double layer capacitors; catalyst carriers; reaction fields for synthesis reactions; heat insulating materials; and the like. Examples of the separation membranes include reverse osmosis membranes, ion exchange membranes, and gas separation membranes. Examples of the adsorption materials include masks, filtration membranes, and filters.
[0061] Since the aluminum member 100 has a high whiteness, it is preferable to use it as a test sheet, a developing member for chromatography, a reflecting material, and a standard white plate. Also, since the aluminum member 100 is porous, it is preferable to use it as a separation membrane, a moisture absorbing material, a water absorbing material, an adsorbing material, a developing member for chromatography, a separator, a catalyst carrier, a reaction field, and a heat insulating material.
[0062] Among these, the aluminum member 100 is more preferably used for chromatography because of its high whiteness and water wicking performance. Among chromatography, it is even more preferably used for lateral flow type chromatography. Moreover, the chromatography is preferably immunochromatography. Among immunochromatography, it is more preferably used for lateral flow immunoassay. Therefore, the aluminum member 100 may be a developing member for chromatography. The developing member for chromatography may be a test strip for chromatography. Moreover, the aluminum member 100 is also preferably used for in vitro diagnostic medicines such as a test kit using immunochromatography. Note that the test kit may also be called a diagnostic kit.
[0063] [Test kit] Next, an example of a test kit 200 using the aluminum member 100 will be described. As shown in Fig. 6, the test kit 200 includes the aluminum member 100. Specifically, the test kit 200 includes the aluminum member 100, a specimen supplying section 110, a determining section 120, and an absorbing section 130.
[0064] The specimen supplying section 110 may contain a labeled antibody that specifically binds to a detection target such as an influenza virus. A specimen collected from a living body or the like is supplied to the specimen supplying section 110 and mixed with the labeled antibody to form a mixed liquid. The mixed liquid is developed to the determination section 120 by capillary action of the aluminum member 100, and excess specimen is absorbed by the absorption section 130.
[0065] The determination unit 120 has, for example, a test line and a control line. For example, an antibody that specifically binds to the target to be detected is fixed to the test line. When the target to be detected is contained in the sample, the labeled antibody is fixed to the antibody on the test line via the target to be detected. For example, an antibody that specifically binds to the labeled antibody is fixed to the control line. When the mixture containing the sample and the labeled antibody is developed to the control line, the labeled antibody binds to the antibody fixed to the control line.
[0066] A labeled antibody generally contains a label such as a colored particle or a gold colloid particle, and an antibody that binds to the label to form a complex and specifically binds to the target. Therefore, if there is a location where the concentration or density of the labeled antibody is high, the label will be concentrated, allowing this location to be visually confirmed. Therefore, the test kit 200 can be used to test for a positive result when both the test line and the control line can be visually confirmed, and for a negative result when only the control line can be visually confirmed.
[0067] The test kit 200 can be used, for example, for infectious disease testing; genetic analysis; pregnancy testing; livestock testing; and allergen testing for foods, animals, plants, metals, house dust, etc.
[0068] The test kit 200 can be used to test, for example, amino acids, peptides, proteins, genes, sugars, lipids, cells, or complexes thereof. More specifically, peptides such as PCT (procalcitonin); proteins such as urinary albumin; hormones such as HCG (human chorionic gonadotropin) and LH (luteinizing hormone); HBs antigen, rotavirus antigen, adenovirus antigen, RSV (respiratory syncytial virus), etc. Antigens or antibodies of viral infections such as HBs antibody, HCV (Hepatitis C virus) antibody, HIV antibody, EBV antibody, RSV antibody, rubella virus antibody, measles virus antibody, enterovirus antibody, dengue virus antibody, and SARS antibody; antigens or antibodies of bacterial infections such as pneumococcus antigen, mycoplasma antigen, group A hemolytic streptococcus antigen, legionella antigen, tuberculosis antigen, gonococcus antigen, tetanus antigen, mycoplasma antibody, Helicobacter pylori antibody, and tuberculosis antibody; antigens or antibodies of chlamydia infections such as chlamydia antigen; antigens or antibodies of spirochete infections such as Treponema pallidum antibody; antigens or antibodies of protozoal diseases such as malaria antibody and toxoplasma antibody.
[0069] [Method of manufacturing aluminum components] Next, a method for manufacturing the aluminum member 100 according to this embodiment will be described. The method for manufacturing the aluminum member 100 according to this embodiment is not particularly limited, but may include, for example, an etching step, a film forming step, and a depolarization treatment step. Furthermore, the method for manufacturing the aluminum member 100 may include a hydration treatment step as necessary. Each step will be described in detail below.
[0070] (Etching process) In the etching step, prior to the film forming step, the aluminum plate is etched to form a porous structure in the aluminum plate. The etching step can form an aluminum plate having a porous structure with a plurality of pits. In the etching step, the aluminum plate is etched to form the base material 11. The aluminum plate can be made of the same material as the substrate 50 described above. That is, the aluminum plate may be made of metallic aluminum.
[0071] In the etching process, pits are formed in the aluminum plate to make the aluminum plate porous. This makes the aluminum plate porous, thereby expanding its surface area. The etching process can be performed by, for example, electrolytic etching, chemical etching, etc. Examples of electrolytic etching include direct current electrolytic etching and alternating current electrolytic etching. Examples of chemical etching include chemical etching using an acidic solution and chemical etching using an alkaline solution. These etching methods may be performed alone or in combination.
[0072] Here, electrolytic etching is taken as an example for explanation. In the etching process, direct current electrolytic etching is performed to form pits on the surface of the aluminum plate, and the pits grow in a tunnel-like shape in the depth direction perpendicular to the surface of the aluminum plate, while the diameter of the pits increases. In addition, alternating current electrolytic etching is performed to form pits in three dimensions, growing in a spongy shape, while the diameter of the pits increases. When the pits grow to the center of the aluminum plate, an aluminum member 100 made of a porous layer 40 is formed. When the pits do not grow to the center of the aluminum plate, and the aluminum plate has a center where the porous layer 40 is not formed, an aluminum member 100 made of a porous layer 40 and a substrate 50 is formed.
[0073] In this embodiment, the etching of the substrate 50 is preferably AC electrochemical etching. The etching conditions are not particularly limited, but for example, the etching time is 1 minute to 60 minutes, and the etching temperature is 20° C. to 80° C. In the case of electrochemical etching, for example, the current density is 50 mA / cm 2 ~500mA / cm 2 It is.
[0074] The etching solution used for etching is preferably an aqueous solution containing hydrochloric acid. The concentration of the aqueous hydrochloric acid solution is preferably 6% by mass to 25% by mass. The aqueous hydrochloric acid solution may contain aluminum ions derived from aluminum chloride or the like in order to suppress excessive dissolution of aluminum. The concentration of aluminum chloride is preferably 0.1% by mass to 10% by mass.
[0075] The etching process may be performed in a single step or in multiple separate steps, for example, the etching process may include multiple etching steps with different chemical species contained in the etching solution, different concentrations of the etching solution, different etching times, different etching temperatures, different current densities, etc.
[0076] (Film formation process) In the film formation process, an aluminum plate having a porous structure is anodized to form a film 12 containing aluminum oxide on the surface of the aluminum plate. In the film formation process, a film 12 is formed by anodization on the surface of a base material 11 that has been made porous by the etching process. At this time, the film 12 is formed on the surface of the base material 11 exposed to the outside of the aluminum plate and on the surface of the base material 11 that forms internal pits. In the film formation process, for example, an anode on which a substrate 50 is placed and a cathode on which stainless steel (SUS) is placed are immersed in an electrolytic solution to perform electrolytic treatment.
[0077] The electrolyte used for film formation is not particularly limited. For example, an aqueous solution of boric acid, ammonium borate, phosphoric acid, pyrophosphoric acid, ammonium phosphate, ammonium adipate, sulfuric acid, or oxalic acid can be used. The conditions for film formation are not particularly limited, but for example, the voltage is 5V to 500V. Film formation may be performed in a single step or may be performed in a plurality of different steps.
[0078] (Depolarization process) In the depolarization process, the aluminum plate on which the coating 12 is formed is depolarized to remove a portion of the surface of the coating 12. In the depolarization process, a portion of the coating 12 formed in the coating formation process is removed, exposing voids and cracks remaining in the coating 12. In the depolarization process, the surface of the coating 12 is roughened by removing (eroding) the coating 12, and recesses 13 can be formed in the surface of the coating 12. The depolarization process is carried out, for example, by immersing the aluminum plate, which is the member on which the coating 12 is formed in the coating formation process, in a depolarization solution.
[0079] The depolarization treatment solution is not particularly limited as long as it can remove (erode) the surface of the aluminum oxide film, but is preferably a solution in which at least one selected from the group consisting of phosphoric acids, metal salts of phosphoric acids, tartaric acid, hydrochloric acid, and metal salts of hydrochloric acid is dissolved, or at least one of a sodium hydroxide solution and an aqueous ammonia solution. Phosphoric acids include, for example, orthophosphoric acid, phosphorous acid, hypophosphorous acid, and mixtures thereof. Metals that form metal salts include, for example, aluminum, sodium, magnesium, calcium, and zinc.
[0080] When phosphoric acids and metal salts of phosphoric acids are used as the depolarization treatment solution, the content of the phosphoric acids and metal salts of phosphoric acids is preferably, for example, 0.1 g / L to 50 g / L. The treatment temperature of the phosphating treatment is preferably, for example, 50° C. to 80° C. The treatment time of the phosphating treatment is preferably 1 minute to 60 minutes.
[0081] In the manufacturing method of the aluminum member 100 according to this embodiment, at least one of a plurality of recesses 13 and a plurality of protrusions 14 is formed on the surface of the film by the film forming step and the depolarization treatment step. That is, in the manufacturing method of the aluminum member 100 according to this embodiment, the etching step, the film forming step, and the depolarization treatment step can be performed in this order at least once. The number of times each step is performed is not particularly limited, but it is preferable to alternately repeat the film forming step and the depolarization treatment step after the etching step. As a result, the erosion of the film 12 and the repair of the eroded film 12 are repeated, so that a good porous layer 40 is formed. At least one of the plurality of recesses 13 and the plurality of protrusions 14 is preferably formed by alternately repeating the film forming step and the depolarization treatment step two or more times. The number of times the film forming step and the depolarization treatment step are repeated is not particularly limited, but may be, for example, 20 times or less, or may be 15 times or less. The number of times that the film formation step and the depolarization treatment step are repeated is preferably 2 to 10 times, and more preferably 3 to 8 times. The number of times that the film formation step and the depolarization treatment step are repeated is further preferably 5 or more times. By repeating the film formation step and the depolarization treatment step, a plurality of recesses 13 can be formed in the film 12, and therefore the whiteness of the aluminum member 100 can be improved.
[0082] (Hydration process) The manufacturing method of the aluminum member 100 according to the present embodiment may include a hydration step, but when the hydration step is performed, it is preferable to repeat the film forming step and the depolarization step thereafter. The manufacturing method of the aluminum member 100 may further include a hydration step of hydrating the aluminum plate before the film forming step to form a hydrated film on the aluminum plate having a porous structure. The hydration step is generally a step of forming a hydrated film of aluminum hydroxide on the surface of metal aluminum after the etching step, and is a step of heat treating the aluminum whose surface has been made porous with hot water such as boiling water. When the fine irregularities on the surface are covered with aluminum hydroxide, the diffuse reflection of light is inhibited, and the whiteness of the aluminum member may decrease. Furthermore, the porous portion of the aluminum member is easily clogged with aluminum hydroxide, which inhibits the diffuse reflection of light and decreases the whiteness of the aluminum member.
[0083] By omitting the hydration treatment step, the whiteness of the aluminum member 100 can be further improved. Furthermore, when a hydrated film is formed by the hydration treatment step, the hydrated film can be dissolved by further performing anodization and depolarization. This reduces or eliminates the hydrated film, and allows the formation of protrusions 14 on the surface of the film 12. The whiteness can be improved by these protrusions 14. At this time, it is considered that the protrusions 14 can be formed by the remaining hydrated film or anodized film.
[0084] Specifically, by performing anodization and depolarization, the hydrated film is incorporated into the anodized film in order from the inner layer side, and a film 12 consisting of the anodized film and the remainder of the hydrated film is formed on the surface of the base material 11. In other words, a layered structure is formed in which the base material 11, the anodized film, and the remainder of the hydrated film are laminated in this order. By further performing anodization and depolarization on this layered structure, protrusions 14 are formed in the film 12.
[0085] Depending on the conditions of the anodizing treatment and the depolarization treatment, recesses 13 can be formed in addition to protrusions 14 in the film 12. By performing the anodizing treatment and the depolarization treatment to such an extent that no hydrated film remains, recesses 13 can be formed on the surface of the film 12. The protrusions 14 are formed by (the remainder of) the hydrated film or the anodized film.
[0086] As described above, the etching step creates porosity by generating pits in the base material 11, and the film formation step and depolarization step form and remove the anodized film, resulting in the generation of voids 15 in the porous layer 40, forming a secondary rough surface structure 20. The film formation step and depolarization step also create recesses 13 on the surface of the film 12, forming a primary rough surface structure 10. The film formation step and depolarization step after the hydration step also create protrusions 14 on the surface of the film 12, forming the primary rough surface structure 10. The film formation step and depolarization step are repeated after the etching step to develop an uneven structure consisting of an aggregate of the primary rough surface structure 10 and the secondary rough surface structure 20, forming a tertiary rough surface structure 30.
[0087] As described above, the method for producing the aluminum member 100 includes a film forming step of anodizing an aluminum plate having a porous structure to form the film 12 containing aluminum oxide on the aluminum plate. The method for producing the aluminum member 100 includes a depolarization step of depolarizing the aluminum plate on which the film 12 has been formed, and removing a part of the surface of the film 12. The film forming step and the depolarization step are alternately repeated. The aluminum plate is made of metal aluminum. Furthermore, the method for producing the aluminum member 100 includes forming at least one of a plurality of recesses 13 and a plurality of protrusions 14 on the surface of the film 12 by the film forming step and the depolarization step. The film 12 has a thickness of 5 nm to 1000 nm. The depth of each of the recesses 13 included in the plurality of recesses 13 is 10 nm to 100 nm, and the height of each of the protrusions 14 included in the plurality of protrusions 14 is 10 nm to 100 nm. The aluminum member 100 has a plurality of pores 15, and the average pore diameter of the plurality of pores 15 is 0.1 μm to 10 μm.
[0088] In this embodiment, a method for manufacturing the aluminum member 100 having the porous layer 40 by electrochemical etching or the like has been described. However, the method for manufacturing the aluminum member 100 is not limited to the above embodiment, and the porous layer 40 may be formed by, for example, sintering aluminum powder. EXAMPLES
[0089] Hereinafter, the present embodiment will be described in more detail with reference to examples and comparative examples, but the present embodiment is not limited thereto.
[0090] [Example 1] An aluminum foil having a thickness of 150 μm was electrolytically etched with AC in an aqueous solution containing 3 mol / L hydrochloric acid and 0.2 mol / L sulfuric acid to make the surface of the aluminum foil porous, and then thoroughly washed with water. The aluminum foil used was high-purity aluminum with a purity of 99.98%.
[0091] Fig. 7 is a photograph showing the surface of the aluminum plate after etching, observed with a scanning electron microscope. As shown in Fig. 7, the etched aluminum plate has a porous structure having a plurality of pits extending inward, each pit having a diameter of about 0.1 µm to 1 µm. In addition, a plurality of pits having a diameter of about 0.1 µm to 1 µm are formed on the surface of the aluminum plate and exposed to the outside, resulting in a roughened surface of the aluminum plate.
[0092] Next, the electrolytically etched aluminum foil was anodized to form a coating on the surface of the base material made of pure aluminum. Specifically, the aluminum foil placed on the anode and stainless steel (SUS) placed on the cathode were immersed in a boric acid electrolyte with a concentration of 80 g / L and an electrolyte temperature of 70°C. Then, anodization was performed at a voltage of 200 V for 10 minutes.
[0093] Next, the aluminum foil on which the film was formed was thoroughly washed with water, and then immersed in an aqueous phosphoric acid solution having a concentration of 50 g / L and a temperature of 60° C. for 20 minutes for depolarization treatment.
[0094] The above-mentioned anodization and depolarization treatment were then repeated five times in this order under the same conditions as above to produce an aluminum member.
[0095] [Example 2] An aluminum member was produced in the same manner as in Example 1, except that the boric acid electrolyte used in the anodizing treatment was changed to a 1 g / L aqueous solution of ammonium dihydrogen phosphate and the anodizing treatment voltage was changed to 50V.
[0096] [Example 3] An aluminum member was produced in the same manner as in Example 1, except that the boric acid electrolyte used in the anodizing treatment was changed to a 100 g / L aqueous solution of ammonium adipate and the anodizing treatment voltage was changed to 150V.
[0097] [Example 4] An aluminum member was produced in the same manner as in Example 1, except that the boric acid electrolyte used in the anodizing treatment was changed to a 50 g / L aqueous solution of oxalic acid, the anodizing treatment temperature was changed to 30°C, and the anodizing treatment voltage was changed to 20V.
[0098] [Example 5] An aluminum member was produced in the same manner as in Example 1, except that before anodizing, a depolarization treatment was performed by immersing the aluminum member in a phosphoric acid aqueous solution with a concentration of 50 g / L and a temperature of 60° C. for 10 minutes as a pretreatment, and the voltage for the anodizing treatment was changed to 150 V.
[0099] [Example 6] An aluminum member was produced in the same manner as in Example 1, except that a hydrophilic coating agent was applied to the sample after the repeated depolarization treatment as a post-treatment.
[0100] [Example 7] An aluminum member was produced in the same manner as in Example 1, except that one surface of the sample after the repeated depolarization treatment was covered with a 20 μm-thick nylon resin as a post-treatment.
[0101] [Example 8] Except for changing one of the depolarization treatments using the phosphoric acid aqueous solution to a heat treatment, an aluminum member was produced in the same manner as in Example 1. The heat treatment was carried out in air at 500° C. for 5 minutes.
[0102] [Example 9] An aluminum member was produced in the same manner as in Example 1, except that the phosphoric acid aqueous solution used in the depolarization treatment was changed to a 5 g / L aqueous solution of sodium hydroxide, and the depolarization treatment temperature was changed to 40°C.
[0103] [Example 10] Before the anodizing treatment, the electrolytically etched aluminum foil was immersed in boiling pure water for 10 minutes for hydration treatment, and then the anodizing treatment and the depolarization treatment were performed, and the number of repetitions of the anodizing treatment and the depolarization treatment was changed to 7. Except for the above, the aluminum member was produced in the same manner as in Example 1.
[0104] [Comparative Example 1] An aluminum member was produced in the same manner as in Example 1, except that the electrolytically etched aluminum foil was subjected to anodizing treatment only once and was not subjected to depolarization treatment.
[0105] [Comparative Example 2] An aluminum member was produced in the same manner as in Example 1, except that anodizing treatment and depolarization treatment were carried out without carrying out electrolytic etching.
[0106] [Comparative Example 3] An aluminum member was produced in the same manner as in Example 10, except that the number of repetitions of the anodizing treatment and the depolarization treatment was changed to one.
[0107] [evaluation] The surfaces of the aluminum members according to Example 3, Example 10, and Comparative Example 3 were observed by a scanning electron microscope. The electron microscope photographs are shown in Fig. 8, Fig. 9, and Fig. 10, respectively.
[0108] For the aluminum members obtained in each example, the coating thickness, the diameter of the concave or convex part of the primary structure, the depth of the concave or the height of the convex part, the average pore diameter of the pores, the bending test, the arithmetic mean roughness Sa, the period of the tertiary rough surface structure, L * The value and water uptake height were evaluated as follows:
[0109] (Coating thickness) After cutting the aluminum member, the cut surface was mirror-finished with a Cross Section Polisher (registered trademark) manufactured by JEOL Ltd. to obtain a sample for measuring the coating thickness. The cross section of the sample for measuring the coating thickness was observed with a scanning electron microscope ULTRA plus manufactured by Carl Zeiss K.K. to measure the thickness of the coating.
[0110] (Diameter of recess in primary structure) The surface of the coating was observed with a scanning electron microscope ULTRA plus manufactured by Carl Zeiss KK, and the diameter of the recesses was calculated by averaging the diameters of the entrances of the recesses.
[0111] (Diameter of the convex part of the primary structure) The surface of the coating was observed under a scanning electron microscope ULTRA plus manufactured by Carl Zeiss KK, and the diameter of the projections was calculated by averaging the diameters of the largest projections.
[0112] (depth of recess) The cross section of the film was observed by a scanning electron microscope, and the depth of the recess was determined by calculating the average value of the distances measured from the entrance to the bottom of the recess.
[0113] (Height of convex part) The cross section of the film was observed under a scanning electron microscope, and the height of the projections was determined by measuring the distance from the surface of the flat part of the film to the top of the projections and calculating the average value.
[0114] (average pore size) The average pore size of the pores was measured by mercury intrusion porosimetry.
[0115] (Bending test) The bending test was carried out in accordance with the MIT type bending test method (EIAJ RC-2364A) specified by the Electronic Industries Association of Japan. The MIT type bending test device used was the one specified in JIS P8115 (Paper and cardboard - Folding endurance test method - MIT testing machine method). In the bending test, the process of bending the aluminum part 90 degrees and returning it to its original shape was counted as one bending, and the aluminum part was bent 100 times. If the aluminum part did not break, it was evaluated as "good", and if it broke, it was evaluated as "bad".
[0116] (Arithmetic mean roughness Sa) The arithmetic mean roughness Sa of the surface on the porous layer side of the aluminum member was measured in accordance with ISO 25178. The measurement conditions for the arithmetic mean roughness Sa were as follows.
[0117] Measurement conditions for arithmetic mean roughness Sa Equipment: Bruker AXS 3D white light interference microscope ContourGT-I Measurement range: 60μm×79μm Objective lens: 115x Internal lens: 1x
[0118] (Periodicity of tertiary rough surface structure) The cross section of the resulting aluminum member was observed with an optical microscope, and the period of the tertiary rough surface structure was measured.
[0119] (L * value) In accordance with JIS Z8722, the surface of the aluminum component is measured with a color difference meter, and the L * The color measurement conditions were as follows:
[0120] L * Value measurement conditions Colorimeter: Konica Minolta Japan CR400 Illumination and light receiving optical system: Diffuse illumination and vertical light receiving system (D / 0) Observation conditions: CIE 2° viewing angle color matching function approximation Light source: C light source Color system: L* a * b *
[0121] (Water suction height) The aluminum member was immersed in pure water so that the plane direction of the aluminum member was perpendicular to the liquid surface, and after leaving it for 10 minutes, the height to which the water was sucked up by capillary action was recorded as the water suction height.
[0122] 8, 9, and 10 are photographs of the surfaces of the aluminum members according to Example 3, Example 10, and Comparative Example 3, respectively, observed by a scanning electron microscope. The aluminum member according to Example 3 does not include a hydration film because it has not been hydrated, and a primary rough surface structure with recesses having a diameter of 10 nm to 200 nm was formed on the surface of the aluminum member, as indicated by the arrows. The aluminum member according to Example 10 was repeatedly subjected to anodizing and depolarization after forming a hydration film by boiling pure water. Therefore, as indicated by the arrows, a primary rough surface structure with protrusions having a diameter of 10 nm to 200 nm was formed on the surface of the aluminum member. It is presumed that these recesses and protrusions contribute to the whiteness of the aluminum member. In contrast, in the aluminum member of Comparative Example 3, the anodizing and depolarization after the hydration were insufficient, so that no recesses or protrusions were formed, and the surface of the porous aluminum plate was covered with aluminum hydroxide having a needle-like or plate-like structure. This is presumably why the whiteness of the aluminum member in Comparative Example 3 is reduced.
[0123] Next, Table 1 shows the evaluation results of the aluminum members obtained in each example.
[0124] [Table 1]
[0125] As shown in Table 1, the aluminum members of Examples 1 to 10 have a higher whiteness (L *The value) and water wicking performance were good. On the other hand, in Comparative Example 1, since depolarization treatment was not performed after anodization treatment, no concave or convex parts were formed, and the whiteness was low. In Comparative Example 2, since electrolytic etching was not performed, no pores were formed, and the water wicking performance was insufficient. In Comparative Example 3, since the number of repetitions of anodization treatment and depolarization treatment after hydration treatment was small, the entire surface was covered with a hydration film, and the whiteness was low.
[0126] The arithmetic mean roughness Sa of the aluminum plate before etching (not shown) is 0.37 μm, and L * The arithmetic mean roughness Sa of the aluminum plate after etching shown in FIG. 7 is 0.336 μm, and the L * The value is 71.4. Therefore, the whiteness of the aluminum plate does not increase simply by etching the aluminum plate.
[0127] The entire contents of Patent Application No. 2018-174947 (filing date: September 19, 2018) are incorporated herein by reference.
[0128] Although the present embodiment has been described above with reference to examples and comparative examples, the present embodiment is not limited to these, and various modifications are possible within the scope of the gist of the present embodiment. [Industrial Applicability]
[0129] According to the present invention, it is possible to provide an aluminum member having high whiteness and water wicking performance, and a method for manufacturing the same. [Explanation of symbols]
[0130] 10 Primary rough surface structure 11 Base material 12. Membrane 13 Recess 14 Convex part 15 Vacancies 20 Secondary rough surface structure 30 Tertiary rough surface structure 40 Porous Layer 50 Substrates 100 Aluminum components
Claims
1. A porous layer including a base material made of metallic aluminum and a coating including aluminum oxide that covers a surface of the base material, The coating has a thickness of 5 nm to 1000 nm; the coating has at least one of a plurality of recesses and a plurality of protrusions formed on a surface thereof, a depth of each of the recesses included in the plurality of recesses is 10 nm to 100 nm; the height of each of the plurality of protrusions is 10 nm to 100 nm; The aluminum component for immunochromatography, wherein the porous layer has a plurality of pores, and the average pore size of the plurality of pores is 0.1 μm to 10 μm.
2. 2. The aluminum component for immunochromatography according to claim 1, wherein the diameter of each of the recesses is 10 nm to 200 nm and is smaller than the average pore size of the porous layer.
3. 3. The aluminum member for immunochromatography according to claim 1, wherein the diameter of each of the protrusions is 10 nm to 200 nm.
4. a primary rough surface structure formed by the coating and at least one of the plurality of recesses and the plurality of protrusions; a secondary rough surface structure formed by the base material and the plurality of pores; a tertiary rough surface structure consisting of a set of the primary rough surface structure and the secondary rough surface structure; The aluminum component for immunochromatography according to any one of claims 1 to 3, comprising:
5. The aluminum member for immunochromatography according to any one of claims 1 to 4, having an arithmetic mean roughness Sa of 0.1 µm to 30 µm.
6. L * a * b * L in color system * The aluminum component for immunochromatography according to any one of claims 1 to 5, wherein the value is 80 or more.
7. The aluminum component for immunochromatography according to any one of claims 1 to 6, wherein the height of water uptake by capillary action is 3 cm or more.
8. 8. The aluminum component for immunochromatography according to claim 1, which does not break even when bent 100 times or more in a bending test based on the MIT type bending test method.
9. Further comprising a substrate made of metallic aluminum; The aluminum member for immunochromatography according to any one of claims 1 to 8, wherein the porous layer is provided on at least one surface side of the substrate.
10. a film forming step of anodizing an aluminum plate having a porous structure to form a film containing aluminum oxide on the aluminum plate; A method for producing an aluminum member for immunochromatography, comprising: a depolarization treatment step of depolarizing the aluminum plate on which the coating is formed and removing a part of the surface of the coating, The film forming step and the depolarization treatment step are alternately repeated, The aluminum plate is made of metal aluminum, forming at least one of a plurality of recesses and a plurality of protrusions on a surface of the coating by the coating formation step and the depolarization treatment step; The coating has a thickness of 5 nm to 1000 nm; a depth of each of the recesses included in the plurality of recesses is 10 nm to 100 nm; the height of each of the plurality of protrusions is 10 nm to 100 nm; The method for producing an aluminum member for immunochromatography, wherein the aluminum member for immunochromatography has a plurality of pores, and the average pore size of the plurality of pores is 0.1 μm to 10 μm.
11. The method for producing an aluminum member for immunochromatography according to claim 10, further comprising an etching step of etching the aluminum plate to form the porous structure in the aluminum plate prior to the film forming step.
12. The method for producing an aluminum component for immunochromatography according to claim 10 or 11, further comprising a hydration treatment step, prior to the film formation step, of hydrating the aluminum plate to form a hydrated film on the aluminum plate having the porous structure.
13. forming at least one of a plurality of recesses and a plurality of protrusions on a surface of the coating by the coating formation step and the depolarization treatment step; The method for producing an aluminum member for immunochromatography according to any one of claims 10 to 12, wherein at least one of the plurality of recesses and the plurality of protrusions is formed by alternately repeating the film formation process and the depolarization treatment process two or more times.
14. A method for manufacturing an aluminum component for immunochromatography described in any one of claims 10 to 13, wherein at least one of the plurality of recesses and the plurality of protrusions is formed by alternately repeating the coating formation process and the depolarization treatment process five or more times.
15. A method for manufacturing an aluminum component for immunochromatography described in any one of claims 10 to 14, wherein when the film formation process and the depolarization treatment process are repeated alternately, the treatment time for one depolarization treatment in the depolarization treatment process is 20 minutes to 60 minutes.
Citation Information
Patent Citations
Method for manufacturing substrate for lithographic printing plate, substrate for lithographic printing plate, and original plate for lithographic printing plate
JP2002293055A
Developing solvent for immuno-chromatography, measuring method and kit
JP2003344406A
Method for manufacturing aluminium electrolytic capacitor electrode
JP2018080373A
Water repellent aluminum base, method for producing water repellent aluminum base, heat exchanger and power transmission line
WO2015146681A1