Heat sink, manufacturing method thereof, and heat exchanger

The gyroid structure heat sink addresses thermal performance issues by optimizing fluid flow and reducing pressure loss, enhancing cooling efficiency and size reduction.

JP7563529B2Active Publication Date: 2024-10-08RICOH CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2023092054
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2021-11-15
Filing Date
2023-06-05
Publication Date
2024-10-08
Estimated Expiration
2042-03-10

AI Technical Summary

Technical Problem

Existing heat sinks do not effectively address the need for improved thermal performance in high-integration electronic components, particularly in terms of cooling capacity without increasing size.

Method used

A heat sink with a flow path featuring a gyroid structure having non-uniform thickness, manufactured using a three-dimensional modeling device, optimizing fluid flow and reducing pressure loss.

Benefits of technology

The gyroid structure heat sink significantly enhances thermal performance and reduces size, achieving uniform temperature distribution and improved cooling efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007563529000004
    Figure 0007563529000004
  • Figure 0007563529000005
    Figure 0007563529000005
  • Figure 0007563529000006
    Figure 0007563529000006
Patent Text Reader

Abstract

To provide a heat sink or the like capable of realizing the remarkable improvement of heat performance.SOLUTION: A heat sink has a flow passage, in which at least a part of the flow passage has a Gyroid structure, and the Gyroid structure has a non-uniform structure.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a heat sink, a manufacturing method thereof, and a heat exchanger. [Background technology]

[0002] There are various types of manufacturing apparatuses for forming a three-dimensional object. For example, Patent Document 1 discloses a method for forming a three-dimensional object by stacking powder layers. However, Patent Document 1 does not consider what kind of heat sink structure should be used for the three-dimensional object to improve thermal performance. Summary of the Invention [Problem to be solved by the invention]

[0003] An object of the present invention is to provide a heat sink that can achieve significantly improved thermal performance. [Means for solving the problem]

[0004] The heat sink of the present invention as a means for solving the problems of the present invention is a heat sink having a flow path, at least a portion of the flow path has a gyroid structure, and the gyroid structure has a non-uniform thickness. Effect of the Invention

[0005] According to the present invention, it is possible to provide a heat sink that can achieve a significant improvement in thermal performance. [Brief description of the drawings]

[0006] [Figure 1] FIG. 1 is a schematic perspective view showing an example of a gyroid structure. [Diagram 2] FIG. 2 is a view of the gyroid structure of FIG. [Diagram 3] FIG. 3 is a diagram showing the minimum thickness (wall thickness) of a gyroid structure. [Figure 4] FIG. 4 is a graph showing the relationship between the thickness and static pressure of the gyroid structure. [Diagram 5] FIG. 5 is a schematic perspective view showing an example of the heat sink of the present invention. [Figure 6] FIG. 6 is a schematic perspective view showing a state in which two heat sinks shown in FIG. 5 are combined into one body by a connecting part. [Figure 7] FIG. 7 is a schematic plan view illustrating an example of a three-dimensional modeling apparatus used in the method for producing a heat sink or a method for producing a gyroid structure of the present invention. [Figure 8] FIG. 8 is a schematic side view of an example of a three-dimensional modeling apparatus used in the method for producing a heat sink or a method for producing a gyroid structure of the present invention. [Figure 9] FIG. 9 is a cross-sectional explanatory view of a modeling unit of a three-dimensional modeling apparatus used in the method for producing a heat sink or a method for producing a gyroid structure of the present invention. [Figure 10] FIG. 10 is a block diagram illustrating an overview of a control unit of a three-dimensional modeling apparatus used in the method for manufacturing a heat sink or a method for manufacturing a gyroid structure according to the present invention. [Figure 11] FIG. 11 is an overall external view showing an example of a three-dimensional modeling apparatus used in the method for producing a heat sink or a method for producing a gyroid structure of the present invention. [Figure 12A] FIG. 12A is a schematic diagram showing an example of the operation of a three-dimensional modeling apparatus used in the method for manufacturing a heat sink or a method for manufacturing a gyroid structure of the present invention. [Figure 12B] FIG. 12B is a schematic diagram showing another example of the operation of a three-dimensional modeling apparatus used in the method for manufacturing a heat sink or a method for manufacturing a gyroid structure of the present invention. [Figure 12C] FIG. 12C is a schematic diagram showing another example of the operation of a three-dimensional modeling apparatus used in the method for manufacturing a heat sink or a method for manufacturing a gyroid structure of the present invention. [Figure 12D] FIG. 12D is a schematic diagram showing another example of the operation of a three-dimensional modeling apparatus used in the method for manufacturing a heat sink or a method for manufacturing a gyroid structure of the present invention. [Figure 12E] FIG. 12E is a schematic diagram showing another example of the operation of a three-dimensional modeling apparatus used in the method for manufacturing a heat sink or a method for manufacturing a gyroid structure of the present invention. [Figure 13] FIG. 13 is a schematic perspective view showing a heat sink body of the first comparative example. [Figure 14A] FIG. 14A is a diagram showing the left, center, and right cross-sectional positions of the heat sink of Comparative Example 1. [Figure 14B] FIG. 14B is a cross-sectional view of the heat sink of Comparative Example 1 at the left, center, and right cross-sectional positions. [Figure 15] FIG. 15 is a schematic perspective view showing an example of a heat sink model in which two heat sinks of Comparative Example 1 are stacked. [Figure 16] FIG. 16 is a schematic cross-sectional view of the center of the heat sink model of FIG. [Figure 17] FIG. 17 is a schematic perspective view showing a heat sink body of the first embodiment. [Figure 18] FIG. 18 is a schematic perspective view showing a heat sink body of the second embodiment. [Figure 19] FIG. 19 is a schematic perspective view showing a heat sink body of the third embodiment. [Figure 20A] FIG. 20A is a diagram showing the left, center, and right cross-sectional positions of the heat sink of Example 3. [Figure 20B] FIG. 20B is a cross-sectional view of the heat sink of Example 3 at the left, center, and right cross-sectional positions. [Figure 21] FIG. 21 is a schematic perspective view showing a heat sink body of the fourth embodiment. [Figure 22] FIG. 22 is a schematic perspective view showing a heat sink body of the fifth embodiment. [Figure 23] FIG. 23 is a schematic perspective view showing a heat sink body of Comparative Example 2. As shown in FIG. [Figure 24] FIG. 24 is an enlarged view of the thinnest and thickest parts of the cells in the gyroid structure of Examples 1 to 5. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0007] (Gyroid structure) The gyroid structure of the present invention has a predetermined surface and a non-uniform thickness. The gyroid structure preferably has a surface represented by the following formula 1. sin(X*P1)cos(Y*P2)+sin(Y*P2)cos(Z*P3)+sin(Z*P3)cos(X*P1)=0 ···Formula 1 In the above formula 1, X, Y, and Z are real numbers between -π and π, and P1, P2, and P3 are real numbers greater than 0.

[0008] As shown by the trigonometric functions in Equation 1 above, the gyroid structure is infinitely connected in the three directions of X, Y, and Z. When P1, P2, and P3 are 1, each period is 2π. On the other hand, when P1 and P2 are 1 and only P3 is 2, the period of Z is π, so compared to the X and Y directions, the Z direction will be connected with a half period. It is advisable to set the values ​​of P1, P2, and P3 appropriately depending on the flow direction in addition to the wall thickness and cell size.

[0009] In this specification, the X-axis, Y-axis, and Z-axis are perpendicular to each other. The Z-axis is defined as vertical. The X-axis and Y-axis are defined as horizontal. Note that the directions in which the X-axis, Y-axis, and Z-axis extend are not limited to this example.

[0010] The gyroid structure has a unique shape that can only be created using a three-dimensional modeling device and cannot be produced using a mold. Here, the gyroid structure has a three-dimensional periodic minimal surface. A periodic minimal surface is a minimal surface that can be infinitely connected in three different directions and divides space into two regions. The periodic minimal surface of a gyroid structure can be infinitely connected in the direction along the X-axis, the direction along the Y-axis, and the direction along the Z-axis. In other words, a gyroid structure is a shape that has maximum space-filling properties with a minimum amount of material.

[0011] Here, Fig. 1 is a schematic perspective view showing an example of a gyroid structure, and Fig. 2 is a view of the gyroid structure of Fig. 1 as seen from the direction of arrow A. As shown in Figure 1, a gyroid structure is a three-dimensional periodic minimal plane that is infinitely connected in three directions, and can be expressed by the above formula 1 using trigonometric functions. When P1, P2, and P3 are 1, each of the periods is 2π. Here, the cell size is defined as the size of the cube that constitutes one period of the gyroid structure. For example, a cell size of 10 indicates that one period of the gyroid structure is constituted in a space of 10 mm × 10 mm × 10 mm (see Figure 2). XYZ that satisfy the above formula 1 are surfaces and have no thickness. As shown in Figure 3, a gyroid structure with volume is obtained by providing faces offset by ±t / 2 on both ends of the normal direction of the face, and the area enclosed by these faces has a thickness of t.

[0012] The gyroid structure of the present invention has a predetermined surface and a non-uniform thickness, and is used in various fields, but is preferably used in heat exchangers and heat sinks, as described below. The thickness is set to a value corresponding to the static pressure value calculated under a constant thickness (see FIG. 4).

[0013] (heat exchanger) The heat exchanger of the present invention has a gyroid structure part made of the gyroid structure of the present invention. A heat exchanger is a device that transfers heat (exchanges heat) from a warm fluid to a cold fluid. Water or air is used as the fluid. Examples of heat exchangers include heat sinks, radiators, and boilers.

[0014] (heat sink) The heat sink of the present invention is a heat sink having a flow passage, at least a portion of the flow passage having a gyroid structure, and the gyroid structure has a non-uniform thickness.

[0015] In recent years, the increased integration of electronic components such as semiconductors has led to increased heat generation, and there is a demand for heat sinks with high cooling capacity without increasing in size. The heat sink of the present invention has a non-uniform gyroid structure by being fabricated using a three-dimensional modeling apparatus, and the thermal performance can be significantly improved.

[0016] Fluids that flow through the flow paths of the heat sink include liquids, gases, and solids. Among these, liquids are preferred. Examples of liquids include water, ethylene glycol, and mixtures thereof. The viscosity of the liquid at 20°C is preferably 1 mPa·s to 100 mPa·s.

[0017] In the present invention, at least a portion of the flow path has a gyroid structure of non-uniform thickness. A gyroid structure of non-uniform thickness optimizes the flow in the flow path, reduces pressure loss and improves thermal performance, and enables a smaller heat sink, compared to a gyroid structure of uniform thickness. The heat sink of the present invention only needs to have a gyroid structure portion in which at least a portion of the flow path has a non-uniform thickness, and may have a gyroid structure of uniform thickness as long as the objects and effects of the present invention can be achieved.

[0018] In one aspect of the present invention, it is preferable that the gyroid structure has a flow path including a predetermined surface, and the thickness of the surface is non-uniform. With a uniform gyroid structure, for example, liquid such as water will tend to flow more to parts where it flows easily, resulting in uneven cooling. On the other hand, with a non-uniform gyroid structure, the thickness of the parts where water flows easily can be made thicker to make it more difficult to flow, and the thickness of the parts where water flows less easily can be made thinner to make it easier to flow, resulting in an effect of making the flow uniform overall and allowing uniform cooling up to the sides.

[0019] In one embodiment of the present invention, the minimum thickness (wall thickness) of at least a portion of the gyroid structure is preferably 1 mm or more, more preferably 1 mm or more and 15 mm or less, and even more preferably 3 mm or more and 10 mm or less. When the minimum thickness (wall thickness) of at least a portion of the gyroid structure is 1 mm or more, water leakage from the heat sink and damage during manufacturing can be prevented.

[0020] In one embodiment of the present invention, the cell size of the unit cell forming the gyroid structure is preferably 5 mm or more, more preferably 5 mm or more and 15 mm or less, and even more preferably 8 mm or more and 12 mm or less. When the cell size of the unit cell forming the gyroid structure is 5 mm or more, powder removal during three-dimensional modeling of the heat sink can be improved.

[0021] In one embodiment of the present invention, the ratio of the cell size of a unit cell forming the gyroid structure to the maximum thickness of at least a portion of the gyroid structure (cell size / maximum thickness) is preferably 2.5 or more, more preferably 2.5 to 10, and even more preferably 2.5 to 5. When the ratio (cell size / minimum thickness) is 2.5 or more, powder removal can be improved when three-dimensionally forming a heat sink.

[0022] In one embodiment of the present invention, the heat sink has a connecting portion. The connecting portion is a part that is attached to the water supply port and the water drain port to connect them to tube piping, and since pressure loss is large at this portion, by integrating the connecting portion with the heat sink body, it is possible to reduce the pressure loss.

[0023] The heat sink of the present invention comprises a heat sink body having a flow passage, and further comprises other members as required. A water supply port communicating with one end of the flow passage is provided at one end of the heat sink body, and a water drain port is provided at the other end. When liquid is supplied into the heat sink body through the water inlet, the liquid flows through the flow path and is discharged from the water outlet to the outside of the heat sink body. The liquid may be circulated between the water inlet and the water outlet. An example of the liquid is water. The water may contain an additive such as ethylene glycol.

[0024] Here, FIG. 5 is a schematic perspective view showing one example of the heat sink of the present invention, and FIG. 6 is a schematic perspective view showing a state in which two heat sinks of FIG. 5 are combined together with a connecting part to be integrated. Here, FIG. 5 is a schematic perspective view showing an example of the heat sink of the present invention, and FIG. 6 is a schematic perspective view showing a state in which a connecting portion is removed from the heat sink of FIG. The heat sink 100 shown in FIGS. 5 and 6 has a heat sink body 101, a water supply port 102, a flow path 103, a gyroid structure 104, and a drain port 105. The water supply port 102 is an inlet through which the fluid enters. The fluid flows in a vertical direction (the Y-axis direction in FIGS. 5 and 6) through a gyroid structure 104 provided in a flow path 103. The drain port 105 is an outlet through which the fluid that has entered through the water supply port 102 is discharged. In the heat sink 100 shown in Figures 5 and 6, as an example, the water supply port 102 is located at the top of the heat sink in the vertical direction and at the center in the horizontal direction (X-axis direction in Figures 5 and 6). The water drain port 105 is located at the bottom of the heat sink in the vertical direction and at the center in the horizontal direction. The fluid entering through the water supply port 102 flows from the center to the side portion, and at the same time, flows vertically and in the depth direction (Z-axis direction in Figures 5 and 6). In other words, the fluid flows from the upstream to the downstream of the heat sink.

[0025] When liquid is supplied from water inlet 102 into the heatsink body via flow path 103, the liquid flows through gyroid structure 104, which is provided in flow path 103 and is expressed by the above formula 1, and is discharged outside the heatsink body from drain outlet 105 (in the direction of arrow A in Figure 6). The liquid is heated by receiving heat from the heat generating element and is sent to the radiator by a pump (not shown). The heated liquid is cooled by the radiator's air-cooling fan, dissipates heat into the air, and is circulated back to the heat sink 100.

[0026] (Method of manufacturing a heat sink and a method of manufacturing a gyroid structure) The method for manufacturing a heat sink of the present invention is a method for manufacturing a heat sink of the present invention, and includes a powder layer formation process of stacking powder to form a powder layer, and a modeling liquid application process of applying a modeling liquid to the powder layer, and further includes other processes as necessary.

[0027] The method for manufacturing a gyroid structure of the present invention is a method for manufacturing a gyroid structure of the present invention, and includes a powder layer formation step of stacking powder to form a powder layer, and a modeling liquid application step of applying a modeling liquid to the powder layer, and further includes other steps as necessary.

[0028] The method for manufacturing a heat sink and a gyroid structure of the present invention are for forming a heat sink and a gyroid structure as three-dimensional objects using a three-dimensional modeling apparatus.

[0029] <Powder layer formation process> The powder layer forming step is a step of forming a powder layer by layering powder. The powder may be one that (1) has a base material, or one that (2) has a base material and an organic material. (1) In the case where a substrate is included, it is preferable that the substrate is made of the substrate. (2) In the case where a substrate and an organic material are included, it is preferable that the surface of the substrate is coated with the organic material.

[0030] -Base material- The substrate is not particularly limited as long as it has a powder or particle form and can be appropriately selected depending on the purpose. Examples of the material include metals, ceramics, carbon, polymers, wood, biocompatible materials, sand, magnetic materials, etc., but from the viewpoint of obtaining a three-dimensional object with extremely high strength, metals, ceramics, etc. that can be finally sintered are preferred.

[0031] The metal is not particularly limited as long as it contains a metal as a material, and examples thereof include magnesium (Mg), aluminum (Al), titanium (Ti), vanadium (V), chromium (Cr), manganese (Mn), iron (Fe), cobalt (Co), nickel (Ni), copper (Cu), zinc (Zn), yttrium (Y), zirconium (Zr), niobium (Nb), molybdenum (Mo), lead (Pd), silver (Ag), indium (In), tin (Sn), tantalum (Ta), tungsten (W), neodymium (Nd), and alloys thereof. Among these, stainless steel (SUS), iron (Fe), copper (Cu), silver (Ag), titanium (Ti), aluminum (Al), and alloys thereof are preferably used. Examples of aluminum alloys include AlSi 10 Mg, AlSi 12 , AlSi7Mg 0.6 , AlSi3Mg, AlSi9Cu3, Scalmalloy, ADC12, etc. These may be used alone or in combination of two or more. Among these, at least one selected from aluminum, zinc, magnesium, and alloys thereof is preferred.

[0032] Examples of ceramics include oxides, carbides, nitrides, and hydroxides. Examples of oxides include metal oxides. Examples of metal oxides include silica (SiO2), alumina (Al2O3), zirconia (ZrO2), and titania (TiO2). However, these are only examples and are not limited to these. These may be used alone or in combination of two or more.

[0033] The substrate may be a commercially available product, such as pure Al (A1070-30BB, manufactured by Toyo Aluminum Co., Ltd.), pure Ti (Osaka Titanium Technologies Co., Ltd.), SUS316L (PSS316L, manufactured by Sanyo Special Steel Co., Ltd.), AlSI10Mg (Si10MgBB, manufactured by Toyo Aluminum Co., Ltd.), SiO2 (Excelica SE-15K, manufactured by Tokuyama Corporation), AlO2 (Taimei Chemical Industry Co., Ltd., product name: Taimicron TM-5D), ZrO2 (TOSOH Corporation, product name: TZ-B53), etc. The substrate may be subjected to a known surface treatment (surface modification treatment) for the purpose of improving adhesion to organic materials and improving coating properties.

[0034] The volume average particle diameter of the base material is not particularly limited and can be appropriately selected depending on the purpose, but is preferably, for example, from 2 μm to 100 μm, and more preferably from 8 μm to 50 μm. When the volume average particle diameter of the base material is 2 μm or more, the effect of aggregation is prevented from increasing, resin coating of the base material is facilitated, and a decrease in yield, a decrease in the production efficiency of the three-dimensional object, and a decrease in the handleability and handling properties of the base material can be prevented. In addition, when the average particle diameter is 100 μm or less, a decrease in the contact points between particles and an increase in voids can be prevented, and a decrease in the strength of the three-dimensional object and its sintered product can be prevented. The particle size distribution of the base material is not particularly limited and can be appropriately selected depending on the purpose, but a sharper particle size distribution is preferable. The volume average particle size and particle size distribution of the base material can be measured using a known particle size measuring device, for example, a particle size distribution measuring device Microtrac MT3000II series (manufactured by Microtrac Bell Co., Ltd.).

[0035] The outer shape, surface area, circularity, flowability, wettability, etc. of the substrate can be appropriately selected depending on the purpose.

[0036] The substrate can be manufactured by a conventionally known method. Examples of methods for manufacturing a powder or particulate substrate include a pulverization method in which a solid is compressed, impacted, or rubbed to be finely divided, an atomization method in which a molten metal is sprayed to obtain a quenched powder, a precipitation method in which a component dissolved in a liquid is precipitated, and a gas-phase reaction method in which a component is vaporized and crystallized. The manufacturing method of the substrate is not limited, but a more preferred method is, for example, atomization, which can obtain a spherical shape and has little variation in particle size. Examples of atomization methods include water atomization, gas atomization, centrifugal atomization, and plasma atomization, and any of them can be suitably used.

[0037] -Organic materials- The organic material may be any material that is used in the above case (1), has a reactive functional group, dissolves in the modeling liquid, and reacts with the cross-linking agent contained in the modeling liquid to form a cross-linked structure by a covalent bond. The term "soluble" means that, for example, when 1 g of resin is mixed and stirred in 100 g of the solvent constituting the modeling liquid at 30° C., 90% by mass or more of the resin dissolves. It is preferable that the organic material has low reactivity with the highly active metal (highly active metal) powder as the base material, is soluble in an organic solvent before shaping (before solidification), and is insoluble in an organic solvent after shaping (after solidification, crosslinking). In particular, it is more preferable that the organic material is soluble in an organic solvent that has low solubility in water. By covering the substrate surface with an organic material, it is possible to suppress dust explosions that occur when the substrate particles are small. In addition, if the organic material has low reactivity with the highly active metal (active metal) powder used as the substrate, and the organic material is soluble in an organic solvent before the application of the modeling liquid, and is insoluble in an organic solvent after the application of the modeling liquid (after crosslinking), the method can be applied even if the substrate is a highly active metal, i.e., a water-restricted material (e.g., aluminum, titanium, etc.), and the produced solidified object (three-dimensional object) can be prevented from collapsing even when immersed in a solvent-based solution.

[0038] The reactive functional group is not particularly limited as long as it can react with a crosslinking agent to form a covalent bond, and can be appropriately selected depending on the purpose. Examples of the reactive functional group include a hydroxyl group, a carboxyl group, an amide group, a phosphate group, a thiol group, an acetoacetyl group, and an ether bond. Among these, it is preferable that the resin as the organic material has a hydroxyl group in terms of improving adhesion to the substrate and reactivity with the crosslinking agent.

[0039] Furthermore, in order to prevent the organic material from remaining in the three-dimensional object during sintering and inhibiting sintering, it is preferable that the organic material is one that is thermally decomposed in an amount of 95% by mass or more when the resin alone is heated at 450°C.

[0040] As the organic material, a resin having a hydroxyl group is preferable. Examples of the resin include polyvinyl acetal (glass transition temperature: 107°C), polyvinyl butyral (glass transition temperature: 67°C), polyacrylic polyol (glass transition temperature: 80°C), polyester polyol (glass transition temperature: 133°C), polybutadiene polyol (glass transition temperature: -17°C), ethyl cellulose (glass transition temperature: 145°C), and nitrocellulose (glass transition temperature: 50°C). Other examples include partially saponified vinyl acetate copolymers (vinyl chloride-vinyl acetate, ethylene-vinyl acetate, etc.), polyether polyols, and phenol-based polyols. These may be used alone or in combination of two or more. Among these, polyacrylic polyols are preferable.

[0041] Among organic materials, those having many hydroxyl groups within the molecule, not at the molecular terminals, and having a weight average molecular weight and a hydroxyl value of at least a certain level are preferred. The weight average molecular weight is preferably 100,000 or less, more preferably from 2,000 to 100,000, and it is preferable that the weight average molecular weight is 100,000 or less and the polymer is a solid at room temperature. The hydroxyl value is preferably 50 mgKOH / g or more, and more preferably 100 mgKOH / g or more.

[0042] The organic material may be a commercially available product. Examples of commercially available products include polyacrylic polyol (ACRYDIC WFU-580, etc., manufactured by DIC Corporation), polyester polyol (POLYLITE OD-X-668, etc., manufactured by DIC Corporation, ADEKA NEW ACE YG-108, etc., manufactured by ADEKA Corporation), polybutadiene polyol (GQ-1000, etc., manufactured by Nippon Soda Co., Ltd.), polyvinyl butyral (MOBITAL B20H, etc., manufactured by Kuraray Co., Ltd.), polyvinyl acetal (S-LEC BM-2, KS-1, etc., manufactured by Sekisui Chemical Co., Ltd.), ethyl cellulose (ETHOCEL, etc., manufactured by Nisshin Seiki Co., Ltd.), and polyacrylic (ORICOX KC-3000, etc., manufactured by Kyoeisha Chemical Co., Ltd.).

[0043] The powder is preferably one in which the surface of the base material is coated with an organic material. The coating thickness of the substrate with the organic material is preferably 5 nm to 1,000 nm, more preferably 5 nm to 500 nm, even more preferably 50 nm to 300 nm, and particularly preferably 100 nm to 200 nm. In the present invention, since the crosslinking reaction caused by the crosslinking agent is utilized, it is possible to make the coating thickness thinner than in the conventional case, and it is possible to achieve both strength and precision even with a thin film. If the average coating thickness is 5 nm or more, the strength of the solidified powder (layer) formed by applying the modeling liquid to the powder is improved, and problems such as deformation during subsequent processing such as sintering or handling will not occur. If the average coating thickness is 1,000 nm or less, the dimensional accuracy of the solidified powder (layer) formed by applying the modeling liquid to the powder is improved. The average thickness can be obtained, for example, by embedding the powder in acrylic resin or the like, exposing the surface of the base material by etching or the like, and then measuring the thickness at any ten points using a scanning tunneling microscope (STM), an atomic force microscope (AFM), a scanning electron microscope (SEM), or the like, and calculating the average value.

[0044] The ratio of the organic material covering the surface of the substrate to the surface area of ​​the substrate (surface coverage rate) is not particularly limited as long as the organic material covers the surface of the substrate to an extent that the effects of the present invention can be achieved. For example, the surface coverage rate is preferably 15% or more, more preferably 50% or more, and particularly preferably 80% or more. When the surface coverage rate is 15% or more, the strength of the solidified product made of the powder (layer) formed by applying the molding liquid to the powder is sufficient, and problems such as deformation during subsequent processing such as sintering or handling do not occur, and the dimensional accuracy of the solidified product made of the powder (layer) formed by applying the molding liquid to the powder is improved. The surface coverage can be measured, for example, by observing a photograph of the powder, measuring the percentage (%) of the area of ​​the part coated with the organic material relative to the total surface area of ​​the powder particles for any 10 particles of the powder shown in the two-dimensional photograph, and calculating the average value to determine the surface coverage. Alternatively, the part coated with the organic material can be measured by performing elemental mapping using energy dispersive X-ray spectroscopy such as SEM-EDS.

[0045] -Other ingredients- The other components are not particularly limited and may be appropriately selected depending on the purpose. Examples of the other components include a fluidizing agent, a filler, a leveling agent, a sintering aid, and polymeric resin particles. A fluidizing agent is preferred because it allows the formation of a powder layer and the like easily and efficiently. Fillers are effective materials for adhering to the surface of powder particles and for filling gaps between powder particles, and have the effect of improving the flowability of powder particles, increasing the number of contact points between powder particles, and reducing the number of gaps, thereby improving the strength and dimensional accuracy of the three-dimensional object. The leveling agent is a material that is effective mainly for controlling the wettability of the powder surface, and has the effect of, for example, increasing the permeability of the modeling liquid into the powder, increasing the strength and speed of the three-dimensional object, and maintaining the shape stably. The sintering aid is an effective material for increasing the sintering efficiency when sintering the obtained three-dimensional object, and has the effects of, for example, improving the strength of the three-dimensional object, lowering the sintering temperature, and shortening the sintering time.

[0046] There are no particular limitations on the method for disposing powder on a support (on a modeling stage) to form a powder layer, and the method can be appropriately selected depending on the purpose. For example, suitable methods for disposing the powder in a thin layer include a method using a known counter rotation mechanism (flattening roller) used in the selective laser sintering method described in Japanese Patent No. 3607300, a method of spreading the powder into a thin layer using a member such as a brush, roller, or blade, a method of pressing the surface of the powder using a pressing member to spread it into a thin layer, and a method using a known powder additive manufacturing device.

[0047] In addition, the powder can be placed in a thin layer on the support by using a known three-dimensional object manufacturing device, which can be performed automatically and simply. The three-dimensional object manufacturing device generally includes a recoater (flattening roller) for stacking the powder, a movable supply tank for supplying the powder onto the support, and a movable modeling tank for placing and stacking the powder in a thin layer. In the powder layer modeling device, the surface of the supply tank can always be slightly higher than the surface of the modeling tank by raising the supply tank, lowering the modeling tank, or both, and the powder can be arranged in a thin layer using the recoater from the supply tank side, and the powder can be stacked in a thin layer by repeatedly moving the recoater.

[0048] The thickness of the powder layer is not particularly limited and can be appropriately selected depending on the purpose, but for example, the average thickness per layer is preferably 30 μm to 500 μm, more preferably 60 μm to 300 μm. If the average thickness is 30 μm or more, the strength of the solidified product (sintered precursor) made from the powder (layer) formed by applying the molding liquid to the powder will be sufficient, and problems such as deformation will not occur during subsequent processing or handling such as sintering.If the average thickness is 500 μm or less, the dimensional accuracy of the solidified product made from the powder (layer) formed by applying the molding liquid to the powder will be improved. The average thickness is not particularly limited and can be measured according to a known method.

[0049] In order to deposit a thin layer of powder on a support using a counter rotating mechanism, a brush or a blade, a pressing member or the like as a powder layer forming means, the following procedure can be used, for example. That is, the powder is placed on a support arranged within an outer frame (sometimes called a "modeling tank," "mold," "hollow cylinder," "cylindrical structure," etc.) that can be raised and lowered while sliding against the inner wall of the outer frame, using a counter-rotating mechanism or the like. At this time, when a support that can be raised and lowered within the outer frame is used, the support is positioned slightly below the upper opening of the outer frame, that is, positioned below by the thickness of the powder layer, and the powder is placed on the support. In this manner, the powder can be placed in a thin layer on the support.

[0050] <Modeling liquid application process> The modeling liquid application process is a process of applying a modeling liquid to the powder layer. The modeling liquid used in the present invention is applied to a powder to solidify the particles of the powder together, and (1) when the powder contains a base material and an organic material, the modeling liquid preferably contains a crosslinker, an organic solvent, and a surfactant, and further contains other components as necessary. (2) When the powder contains a base material, the modeling liquid contains an organic material, and preferably contains a crosslinker, an organic solvent, and a surfactant, and further contains other components as necessary.

[0051] In the above (1), when the modeling liquid is applied to the organic material contained in the powder, the organic material is dissolved by the organic solvent contained in the modeling liquid and is crosslinked by the action of the crosslinking agent contained in the modeling liquid. In the above (2), when the modeling liquid is applied to the powder, the organic material contained in the modeling liquid precipitates due to the volatilization of the organic solvent, and the powder solidifies.

[0052] -Organic materials- In the above case (2), the organic material contained in the modeling liquid is preferably a resin having a hydroxyl group, from the viewpoint of adhesion at the interface between the metal substrate and the organic material. Examples of resins having a hydroxyl group include polyvinyl acetal, polyvinyl butyral, polyacrylic polyol, polyester polyol, polybutadiene polyol, ethyl cellulose, nitrocellulose, polyvinylpyrrolidone, partially saponified vinyl acetate copolymers (vinyl chloride-vinyl acetate, ethylene-vinyl acetate, etc.), polyether polyols, phenolic polyols, etc. These may be used alone or in combination of two or more. The content of the organic material is preferably from 1% by mass to 20% by mass, and more preferably from 1% by mass to 10% by mass, based on the total amount of the modeling liquid.

[0053] Examples of organic solvents include aliphatic or aromatic hydrocarbons such as n-octane, m-xylene, and solvent naphtha, ketones such as diisobutyl ketone, 3-heptanone, and 2-octanone, butyl acetate, amyl acetate, n-hexyl acetate, n-octyl acetate, ethyl butyrate, ethyl valerate, ethyl caprylate, ethyl octylate, ethyl acetoacetate, ethyl 3-ethoxypropionate, diethyl oxalate, diethyl malonate, diethyl succinate, diethyl adipate, bis-2-ethylhexyl maleate, triacetin, tributyrin, and ethylene glycol monobutyl ether acetate, ethers such as dibutyl ether, 1,2-dimethoxybenzene, and 1,4-dimethoxybenzene, dimethyl sulfoxide, and dihydroterpinyl acetate. These may be used alone or in combination of two or more. Compounds not listed here may also be used as long as they have a vapor pressure of 2,000 Pa or less at 25° C. and are insoluble or slightly soluble in water, and are not subject to any particular limitations, and may be appropriately selected depending on the purpose.

[0054] The content of the organic solvent is preferably 30% by mass or more and 90% by mass or less, and more preferably 50% by mass or more and 80% by mass or less, based on the total amount of the modeling liquid. When the content of the organic solvent is 30% by mass or more and 90% by mass or less, the solubility of the resin can be improved, and the strength of the three-dimensional model can be improved. In addition, the nozzle can be prevented from drying out when the device is not in operation (standby), and clogging and nozzle dropping can be suppressed.

[0055] -Crosslinking agent- In the case of (1) above, the crosslinking agent forms a crosslinked structure by forming a covalent bond with the reactive functional group of the powdered organic material (resin), thereby further increasing the strength of the resulting solidified product and improving its solvent resistance. In the case of (2) above, after the modeling liquid is applied to the powder, the crosslinking agent can be crosslinked by heat or ultraviolet light, thereby further increasing the strength of the resulting solidified product and improving its solvent resistance. In the present invention, the term "crosslinking agent" is synonymous with the term "curing agent."

[0056] The crosslinking agent is not particularly limited and may be appropriately selected from isocyanate, acid anhydride, epoxy, and phenol aldehyde. It is preferable that the crosslinking agent has two or more of any of the above in the molecule or at the molecular terminal, and more preferably has three or more of any of the above.

[0057] Examples of the isocyanate include diisocyanates and polyisocyanates. Examples of diisocyanates include aromatic or aromatic-derived polyisocyanates such as tolylene diisocyanate (TDI), diphenylmethane diisocyanate (MDI), polymeric MDI (MDI), tolidine diisocyanate (TODI), naphthalene diisocyanate (NDI), xylylene diisocyanate (XDI), and paraphenylene diisocyanate; aliphatic isocyanates such as isophorone diisocyanate (IPDI) and hexamethylene diisocyanate (HMDI); lysine diisocyanate (LDI), tetramethylxylene diisocyanate (TMXDI), etc. These may be used alone or in combination of two or more. Examples of polyisocyanates include adducts, isocyanurates, and allophanates of diisocyanates.

[0058] Examples of the acid anhydride include acid dianhydrides. Examples of the acid dianhydride include pyromellitic anhydride, 3,4'-oxydiphthalic anhydride, 4,4'-oxydiphthalic anhydride, 4,4-carbonyldiphthalic anhydride, bicyclo[2.2.2]oct-7-ene-2,3,5,6-tetracarboxylic dianhydride, diphenyl-3,3',4,4'-tetracarboxylic dianhydride, diphenyl-2,3,3',4'-tetracarboxylic dianhydride, meso-butane-1,2, 3,4-Tetracarboxylic dianhydride, 1,2,3,4-cyclobutanetetracarboxylic dianhydride, 1,2,3,4-cyclopentanetetracarboxylic dianhydride, 1,2,4,5-cyclohexanetetracarboxylic dianhydride, 5-(2,5-dioxotetrahydrofuryl)-3-methyl-3-cyclohexene-1,2-dicarboxylic anhydride, 4-(2,5-dioxotetrahydrofuran-3-yl)-tetralin-1,2- Dicarboxylic acid anhydride, 5,5'-(ethyne-1,2-diyl)bis(isobenzofuran-1,3-dione), 5,5'-(9H-fluorene-9,9-diyl)bis(2-benzofuran-1,3-dione), naphthalene-1,4,5,8-tetracarboxylic dianhydride, 4,4'-(4,4'-isopropylidenediphenoxy)bis(phthalic anhydride), 1,2,3,4-tetramethyl-1,2,3,4-cyclobutanetetraacetate Examples of the dianhydride include tetracarboxylic dianhydride, octahydrobiphenylene-4a,8b:4b,8a-tetracarboxylic dianhydride, bis(1,3-dioxo-1,3-dihydroisobenzofuran-5-carboxylic acid)1,4-phenylene, 3,4,9,10-perylenetetracarboxylic dianhydride, 4,4'-ethylenebis(2,6-morpholinedione), N,N-bis[2-(2,6-dioxomorpholino)ethyl]glycine, etc. These may be used alone or in combination of two or more.

[0059] Examples of the epoxy include diepoxides and polyepoxides. Examples of the diepoxides include aliphatic epoxy monomers such as 1,3-butadiene diepoxide, 1,5-hexadiene diepoxide, and 1,7-octadiene diepoxide, epoxy monomers such as bisphenol A diglycidyl ether, and polyfunctional epoxy monomers such as triglycidyl isocyanurate and 4,4'-methylenebis(N,N-diglycidylaniline). These may be used alone or in combination of two or more.

[0060] The content of the crosslinking agent is preferably 1.0% by mass or more and 50% by mass or less, and more preferably 10% by mass or more and 30% by mass or less, based on the total amount of the modeling liquid. When the content of the crosslinking agent is 1.0% by mass or more and 50% by mass or less, it is possible to prevent a shortage of strength of the obtained three-dimensional object, to prevent an increase in the viscosity of the modeling liquid or gelation, and to prevent a decrease in the liquid storage stability and viscosity stability.

[0061] -Surfactants- The surfactant is preferably added for the purpose of adjusting the surface tension of the modeling liquid. Examples of the surfactant include anionic surfactants, nonionic surfactants, amphoteric surfactants, acetylene glycol surfactants, fluorine-based surfactants, and silicone-based surfactants.

[0062] -Physical properties of modeling liquid- The viscosity of the modeling liquid is preferably 3 mPa·s or more and 20 mPa·s or less, and more preferably 5 mPa·s or more and 10 mPa·s or less, at 25° C. If the viscosity is 3 mPa·s or more or 20 mPa·s or less, the ejection from the inkjet nozzle is stabilized, and the strength of the solidified object formed by applying the modeling liquid to the powder layer is sufficient, and the dimensional accuracy is good. The viscosity can be measured, for example, in accordance with JIS K7117.

[0063] In the powder layer forming process, when the molding liquid is applied to the powder placed in a thin layer, the layer solidifies. On the solidified thin layer obtained here, powder is placed in a thin layer in the same manner as described above, and when the modeling liquid is applied to the powder (layer) placed in the thin layer, the powder solidifies. The solidification occurs not only in the powder (layer) placed in the thin layer, but also between the powder (layer) placed in the thin layer and the previously solidified thin layer present below it. As a result, a solidified material having a thickness of about twice the thickness of the powder (layer) placed in the thin layer is obtained.

[0064] The method of applying the modeling liquid to the powder (layer) is not particularly limited and can be appropriately selected depending on the purpose, and examples thereof include a dispenser method, a spray method, an inkjet method, etc. In addition, when carrying out these methods, a known device can be suitably used as a solidification forming means. Among these, the dispenser method is excellent in the quantity of droplets, but the coating area is narrow, while the spray method can easily form fine discharged material, has a wide coating area, and is excellent in coating ability, but the quantity of droplets is poor and powder scattering occurs due to the spray flow. For this reason, the inkjet method is particularly preferred in the present invention. The inkjet method has the advantages of being better in the quantity of droplets than the spray method, being able to coat a wider area than the dispenser method, and being preferred in that it can form complex three-dimensional shapes with high precision and efficiency.

[0065] In the case of the inkjet method, the solidified material forming means has a nozzle capable of applying the modeling liquid to the powder layer by the inkjet method. As the nozzle, a nozzle (ejection head) in a known inkjet printer can be suitably used, and an inkjet printer can be suitably used as the solidified material forming means. As an inkjet printer, for example, SG7100 manufactured by Ricoh Co., Ltd. can be suitably mentioned. An inkjet printer is preferable in that a large amount of modeling liquid can be dropped from the head part at one time and the application area is large, so that the application can be speeded up.

[0066] In the present invention, even when an inkjet printer capable of applying the modeling liquid with high precision and efficiency is used, the modeling liquid does not contain solid matter such as particles or highly viscous polymeric materials such as resin, so clogging does not occur in the nozzle or its head, and no corrosion or other problems occur. Furthermore, when the modeling liquid is applied (discharged) to the powder layer, it can efficiently penetrate the organic material in the powder, resulting in excellent efficiency in the production of three-dimensional objects. Moreover, since no polymeric components such as resin are applied, there is no unexpected increase in volume, and solidified objects with good dimensional precision can be obtained easily and efficiently in a short period of time.

[0067] <Other processes> Examples of other steps include a powder removal step, a sintering step, a surface protection treatment step, and a painting step.

[0068] -Powder removal process- The powder removing step is a step of removing the powder adhering to the solidified material from the solidified material. A preferred method of removing the powder adhering to the solidified material from the solidified material is to immerse the solidified material in a powder removing liquid. By immersing the solidified material in a powder removing liquid that does not dissolve (soften) the solidified material and dissolves the organic material in the powder, the excess powder adhering to the surface and inside of the solidified material can be removed. In other words, by immersing the solidified object in the powder removal liquid, the modeling portion that was solidified when the modeling liquid was applied to the powder is not dissolved (softened), but the non-modeling portion, which is the area of ​​the powder where the modeling liquid was not applied, can be dissolved.

[0069] A three-dimensional model (green body) made of laminated solidified materials exists in a state where it is embedded in non-modeled parts (unsolidified powder) to which no modeling liquid has been applied. When the green body is removed from this embedded state, the excess (unsolidified) powder around the green body adheres to its surface and inside the structure, making it difficult to remove easily. This is even more difficult when the green body has a complex surface irregularity or an interior that resembles a flow path. With the general binder jetting method, the strength of the green body is not high, so there is a risk that the green body will collapse if the air blow pressure is increased (0.3 MPa or more). A three-dimensional object (green body) formed by layering solidified materials formed using the powder and modeling liquid used in the present invention has the strength to withstand the pressure of air blowing because the organic material covering the base material is further dissolved and solidified by the compounds contained in the modeling liquid that can develop reactive groups when heated.

[0070] The powder removing liquid contains an organic solvent and, if necessary, further contains other components. The organic solvent contained in the powder removal liquid is not particularly limited as long as it is an organic solvent that does not dissolve the solidified material and dissolves the organic material in the powder, and can be appropriately selected depending on the purpose. At least one selected from ketones, halogens, alcohols, esters, ethers, hydrocarbons, glycols, glycol ethers, glycol esters, pyrrolidones, amides, amines, and carbonates can be used.

[0071] As other components, additives such as surfactants, antifoaming agents, antiseptics and antifungals, pH adjusters, chelating agents, and rust inhibitors may be further added as necessary.

[0072] -Drying process- The drying step is a step of drying the three-dimensional object (green body) formed by stacking the solidified materials obtained in the modeling liquid application step. In the drying step, not only the moisture contained in the green body but also organic matter may be removed (degreased). Examples of drying means include a known dryer and a thermo-hygrostat.

[0073] -Sintering process- The sintering step is a step of sintering the three-dimensional object (green body) formed by stacking the solidified materials obtained in the modeling liquid application step. By carrying out the sintering step, the green body can be made into a densified and integrated metal or ceramic model (sintered three-dimensional object). As a sintering means, for example, a known sintering furnace can be used.

[0074] -Surface protection treatment process- The surface protection treatment step is a step of forming a protective layer on the three-dimensional object (green body) formed by stacking the solidified materials obtained in the modeling liquid application step. By carrying out this surface protection treatment step, it is possible to impart durability to the surface of the solidified material, which allows the solidified material to be used as is. Specific examples of protective layers include a water-resistant layer, a weather-resistant layer, a light-resistant layer, a heat-insulating layer, and a glossy layer. Examples of surface protection treatment means include known surface protection treatment devices, such as a spray device and a coating device.

[0075] -Painting process- The coating process is a process of coating the three-dimensional object (green body) formed by stacking the solidified materials obtained in the modeling liquid application process. By carrying out the coating process, the green body can be colored in a desired color. Examples of coating means include known coating devices, such as coating devices using a spray, roller, brush, etc.

[0076] Hereinafter, an embodiment of the present invention will be described with reference to the drawings. Fig. 7 is a schematic plan view of an example of a three-dimensional modeling apparatus used in the method for manufacturing a heat sink or a gyroid structure of the present invention, Fig. 8 is a schematic side view of an example of a three-dimensional modeling apparatus used in the method for manufacturing a heat sink or a gyroid structure, Fig. 9 is a cross-sectional view of a modeling unit of the three-dimensional modeling apparatus used in the method for manufacturing a heat sink or a gyroid structure, Fig. 10 is a block diagram providing an overview of a control unit of the three-dimensional modeling apparatus used in the method for manufacturing a heat sink or a gyroid structure, and Fig. 11 is an overall external view of an example of a three-dimensional modeling apparatus used in the method for manufacturing a heat sink or a gyroid structure.

[0077] The three-dimensional modeling apparatus used in the heat sink manufacturing method or gyroid structure manufacturing method of the present invention includes a modeling section 1 in which a modeling layer 30, which is a layered object formed by bonding powder, is formed, and a modeling unit 5 that ejects modeling liquid 10 onto the layered powder layer 31 in the modeling section 1 to form a three-dimensional object (heat sink or gyroid structure).

[0078] The modeling section 1 includes a powder tank 11 and a flattening roller 12 serving as a rotating body which is flattening means. Note that the flattening means may be, for example, a plate-like member (blade) instead of the rotating body.

[0079] The powder tank 11 has a supply tank 21 that holds powder 20 to be supplied to a modeling tank 22, and the modeling tank 22 in which modeling layers 30 are stacked to form a three-dimensional object.

[0080] The bottom of the supply tank 21 is capable of moving up and down in the vertical direction (height direction) as a supply stage 23. Similarly, the bottom of the modeling tank 22 is capable of moving up and down in the vertical direction (height direction) as a modeling stage 24. A three-dimensional object is formed on the modeling stage 24 by stacking modeling layers 30.

[0081] The supply stage 23 is raised and lowered in the direction of the arrow Z (height direction) by a motor 27 as shown in FIG. 11, and the modeling stage 24 is similarly raised and lowered in the direction of the arrow Z by a motor .

[0082] The flattening roller 12 transfers and supplies the powder 20 supplied onto the supply stage 23 of the supply tank 21 to the modeling tank 22. The flattening roller 12, which is a flattening means, flattens the surface of the powder 20 supplied to the modeling tank 22 to form a powder layer 31.

[0083] The flattening roller 12 is disposed so as to be movable reciprocally relative to the stage surface (the surface on which the powder 20 is loaded) of the modeling stage 24 in the direction of the arrow Y, and is moved by a reciprocating mechanism 25. In addition, the flattening roller 12 is rotationally driven by a motor 26.

[0084] On the other hand, the modeling unit 5 is equipped with a liquid ejection unit 50 that ejects (applies) modeling liquid 10 that bonds the powder 20 to the powder layer 31 on the modeling stage 24, thereby forming a modeling layer 30 as a layered object in which the powder 20 is bonded.

[0085] The liquid ejection unit 50 includes a carriage 51 and two (or one or three or more) liquid ejection heads (hereinafter simply referred to as "heads") 52a and 52b mounted on the carriage 51.

[0086] The carriage 51 is movably held by guide members 54 and 55. The guide members 54 and 55 are held by side plates 70, 70 on both sides so as to be able to move up and down.

[0087] This carriage 51 is reciprocated in the main scanning direction, that is, the arrow X direction (hereinafter simply referred to as the “X direction”. The same applies to the other Y and Z directions.) via pulleys and a belt by an X-direction scanning motor that constitutes an X-direction scanning mechanism 550 described later.

[0088] Each of the two heads 52a, 52b (hereinafter, referred to as "head 52" when there is no need to distinguish between them) has two nozzle rows in which a plurality of nozzles that eject the modeling liquid are arranged. The two nozzle rows of one head 52a eject the cyan modeling liquid and the magenta modeling liquid. The two nozzle rows of the other head 52b eject the yellow modeling liquid and the black modeling liquid, respectively. Note that the head configuration is not limited to this.

[0089] A plurality of tanks 60 containing the cyan, magenta, yellow, and black forming liquids are attached to the tank mounting portion 56, and the liquids are supplied to the heads 52a and 52b via supply tubes or the like.

[0090] Further, on one side in the X direction, a maintenance mechanism 61 for maintaining and recovering the head 52 of the liquid ejection unit 50 is disposed.

[0091] The maintenance mechanism 61 mainly consists of a cap 62 and a wiper 63. The cap 62 is brought into close contact with the nozzle surface (surface on which the nozzles are formed) of the head 52, and the modeling liquid is sucked from the nozzle. This is to expel powder that has clogged the nozzle and to expel modeling liquid that has become highly viscous. After that, the nozzle surface is wiped (wiped) by the wiper 63 to form a meniscus of the nozzle (the inside of the nozzle is in a negative pressure state). In addition, when the modeling liquid is not being ejected, the maintenance mechanism 61 covers the nozzle surface of the head with the cap 62 to prevent the powder 20 from entering the nozzle and the modeling liquid 10 from drying out.

[0092] The modeling unit 5 has a slider part 72 movably held by a guide member 71 disposed on the base member 7, and the entire modeling unit 5 can move back and forth in a Y direction (sub-scanning direction) perpendicular to the X direction. The entire modeling unit 5 is moved back and forth in the Y direction by a Y-direction scanning mechanism 552, which will be described later.

[0093] The liquid discharge unit 50 is arranged so as to be able to rise and fall in the direction of the arrow Z together with the guide members 54 and 55, and is raised and lowered in the Z direction by a Z-direction lifting mechanism 551 which will be described later.

[0094] Here, the details of the modeling unit 1 will be described.

[0095] The powder tank 11 has a box shape and includes three tanks with open tops: a supply tank 21, a modeling tank 22, and an excess powder receiving tank 29. A supply stage 23 is arranged inside the supply tank 21, and a modeling stage 24 is arranged inside the modeling tank 22, both of which can be raised and lowered.

[0096] The side surface of the supply stage 23 is disposed so as to contact the inner surface of the supply tank 21. The side surface of the modeling stage 24 is disposed so as to contact the inner surface of the modeling tank 22. The upper surfaces of the supply stage 23 and the modeling stage 24 are kept horizontal.

[0097] A powder supplying device 554, which will be described later, is disposed above the supply tank 21. At the initial stage of modeling or when the amount of powder in the supply tank 21 decreases, powder in a tank constituting the powder supplying device 554 is supplied to the supply tank 21. Examples of a powder transport method for supplying powder include a screw conveyor method using a screw and a pneumatic transport method using air.

[0098] The flattening roller 12 transfers and supplies the powder 20 from the supply tank 21 to the modeling tank 22, and flattens the surface to form a powder layer 31 that is a layer of powder with a predetermined thickness.

[0099] This flattening roller 12 is a rod-shaped member that is longer than the inner dimensions of the modeling tank 22 and the supply tank 21 (i.e., the width of the part where the powder is supplied or loaded), and is moved back and forth in the Y direction (sub-scanning direction) over the supply tank 21 and the modeling tank 22 along the stage surface by a reciprocating mechanism 25.

[0100] The flattening roller 12, while being rotated by a motor 26, reciprocates horizontally so as to pass above the supply tank 21 and the modeling tank 22. As a result, the powder 20 is transferred and supplied onto the modeling tank 22, and the flattening roller 12 passes over the modeling tank 22 and flattens the powder 20, thereby forming a powder layer 31.

[0101] Next, an overview of a control unit of a 3D modeling apparatus used in the method for manufacturing a heat sink or a method for manufacturing a gyroid structure of the present invention will be described with reference to Fig. 10. Fig. 10 is a block diagram of the control unit of the 3D modeling apparatus.

[0102] The control unit 500 is equipped with a main control unit 500A including a CPU 501 that is responsible for controlling the entire 3D modeling apparatus, a ROM 502 that stores programs including programs for causing the CPU 501 to execute control of 3D modeling operations including control related to the present invention, and other fixed data, and a RAM 503 that temporarily stores modeling data, etc.

[0103] The control unit 500 includes a non-volatile memory (NVRAM) 504 for holding data even when the power supply to the device is cut off. The control unit 500 also includes an ASIC 505 for image processing that performs various signal processing on image data and for processing input / output signals for controlling the entire device.

[0104] The control unit 500 includes an I / F 506 for transmitting and receiving data and signals used when receiving modeling data from an external modeling data creation device 600. The modeling data creation device 600 is a device that creates modeling data in which a final model is sliced ​​into each modeling layer, and is configured with an information processing device such as a personal computer.

[0105] The control unit 500 includes an I / O 507 for receiving detection signals from various sensors.

[0106] The control unit 500 includes a head drive control unit 508 that controls the driving of the head 52 of the liquid ejection unit 50 .

[0107] The control unit 500 includes a motor driving unit 510 that drives a motor that constitutes an X-direction scanning mechanism 550 that moves the carriage 51 of the liquid ejection unit 50 in the X-direction (main scanning direction), and a motor driving unit 512 that drives a motor that constitutes a Y-direction scanning mechanism 552 that moves the modeling unit 5 in the Y-direction (sub-scanning direction).

[0108] The control unit 500 includes a motor drive unit 511 that drives a motor constituting a Z-direction lifting mechanism 551 that moves (lifts) the carriage 51 of the liquid discharge unit 50 in the Z direction. Note that the lifting in the Z direction may be configured to lift the entire modeling unit 5.

[0109] The control unit 500 includes a motor driving unit 513 that drives the motor 27 that raises and lowers the supply stage 23 , and a motor driving unit 514 that drives the motor 28 that raises and lowers the modeling stage 24 .

[0110] The control unit 500 includes a motor drive unit 515 that drives the motor 553 of the reciprocating mechanism 25 that moves the flattening roller 12 , and a motor drive unit 516 that drives the motor 26 that drives the flattening roller 12 to rotate.

[0111] The control unit 500 includes a supply system drive unit 517 that drives a powder supplying device 554 that supplies the powder 20 to the supply tank 21 , and a maintenance drive unit 518 that drives a maintenance mechanism 61 of the liquid discharge unit 50 .

[0112] The control unit 500 includes a post-supply drive unit 519 that causes the powder post-supply unit 80 to supply the powder 20 .

[0113] Detection signals from a temperature and humidity sensor 560 that detects temperature and humidity as environmental conditions of the apparatus, and other sensors are input to the I / O 507 of the control unit 500.

[0114] An operation panel 522 is connected to the control unit 500 for inputting and displaying information required for this device.

[0115] The modeling data creation device 600 and the three-dimensional modeling device (powder additive manufacturing device) 601 configure a modeling system.

[0116] Next, the operation of the three-dimensional modeling apparatus used in the method for manufacturing a heat sink or a method for manufacturing a gyroid structure of the present invention will be described with reference to FIGS. 12A to 12E. 12A to 12E are schematic explanatory diagrams for explaining the flow of modeling. Here, the description will start from a state where the first modeling layer 30 is formed on the modeling stage 24 of the modeling tank 22. When forming the next modeling layer on the first modeling layer 30, as shown in FIG. 12A, the supply stage 23 of the supply tank 21 is raised, and the modeling stage 24 of the modeling tank 22 is lowered. At this time, the lowering distance of the modeling stage 24 is set so that the interval (layer pitch) between the upper surface of the surface (powder surface) of the powder layer 31 in the modeling tank 22 and the lower part (lower tangent part) of the flattening roller 12 is Δt1. The interval Δt1 is not particularly limited, but is preferably about several tens to 100 μm.

[0117] Next, as shown in Figure 12B, the powder 20 located above the top surface level of the supply tank 21 is moved toward the modeling tank 22 while rotating the flattening roller 12 in the reverse direction (arrow direction), thereby transporting and supplying the powder 20 to the modeling tank 22 (powder supply).

[0118] 12C, the flattening roller 12 is moved parallel to the stage surface of the modeling stage 24 of the modeling tank 22 to form a powder layer 31 having a predetermined thickness Δt1 on the modeling tank 22 of the modeling stage 24 (flattening). At this time, the surplus powder 20 not used to form the powder layer 31 falls into the surplus powder receiving tank 29. After forming the powder layer 31, the flattening roller 12 is moved toward the supply tank 21 and returned (returned) to the initial position (origin position) as shown in FIG. 12D.

[0119] Thereafter, as shown in FIG. 12E, droplets 10 of the modeling liquid are discharged from the head 52 of the liquid discharge unit 50 to form a modeling layer 30 having a desired shape on the next powder layer 31.

[0120] Next, the above-mentioned powder layer formation and modeling liquid ejection are repeated to form a new modeling layer 30. At this time, the new modeling layer 30 and the modeling layer 30 below it are integrated to form a part of the solidified object. Thereafter, the powder layer formation and modeling liquid ejection are repeated to complete the modeling of the solidified object (green body). EXAMPLES

[0121] Examples of the present invention will be described below, but the present invention is not limited to these examples.

[0122] Comparative Example 1 <Making a heat sink> Fig. 13 is a schematic perspective view showing a heat sink body of Comparative Example 1. Fig. 14A is a view showing the left, center, and right cross-sectional positions of the heat sink of Comparative Example 1. Fig. 14B is a cross-sectional view of the heat sink of Comparative Example 1 at the left, center, and right cross-sectional positions. The heat sink of Comparative Example 1 in FIG. 13 has the following dimensions, is a gyroid structure 104a represented by the following formula 1, and has a uniform thickness. sin(X*P1)cos(Y*P2)+sin(Y*P2)cos(Z*P3)+sin(Z*P3)cos(X*P1)=0 ···Formula 1 In the above formula 1, X, Y, and Z are real numbers between -π and π, and P1, P2, and P3 are real numbers greater than 0. As shown in Figures 14A and 14B, the gyroid structure 104a expressed by the above formula 1 has a uniform thickness from left to right and from top to bottom (from the water inlet 103 to the water outlet 105), and is therefore of uniform thickness overall.

[0123] -Heat sink dimensions- ·External size: 100mm x 60mm x 18mm Gyroid structure: 60mm x 54mm x 12mm Coolant inlet and outlet hole diameter: φ6mm

[0124] <Creating a heat sink model> As shown in FIG. 15, two heat sinks of Comparative Example 1 (a first heat sink 110a and a second heat sink 110b) were stacked, and a connecting portion 112 between them was formed as a flow path with a diameter of 6 mm. Next, as shown in Fig. 16, a heat source 111 was placed between the first heat sink 110a and the second heat sink 110b. The size of the heat source 111 was 50 mm x 44 mm x 3 mm. In this manner, a heat sink model 120 of Comparative Example 1 was produced.

[0125] Next, a simulation was performed on the heat sink model 120 of Comparative Example 1 under the following simulation conditions to determine the ratio (cell size / maximum thickness), and the thermal resistance and pressure loss were calculated as follows. The results are shown in Table 1.

[0126] <Simulation conditions> -software- Thermal fluid analysis system STREAM (Software Cradle Co., Ltd.) -Mesh conditions- Mesh type: Unstructured -Physical model- Turbulence (k-ε model) Heat transfer flow steady state -Material properties- Heat sink: Aluminum (A6063) ·Heat source: Copper (pure copper) Coolant: Ethylene glycol solution -Boundary conditions- ·Cooling water temperature: 20℃ ·Flow rate: 10L / min Heat output: 600W

[0127] <Thermal resistance> Based on the following formula, thermal resistance R hs asked for.

number

[0128] <Pressure loss> Based on the following formula, pressure loss ΔP hs asked for.

number

[0129] (Examples 1 to 5 and Comparative Example 2) Using the static pressure distribution obtained from the simulation result of Comparative Example 1, heat sink models of Examples 1 to 5 and Comparative Example 2 were fabricated, and simulations were performed in the same manner as in Comparative Example 1 to determine the ratio (cell size / maximum thickness), thermal resistance, and pressure loss. The results are shown in Table 1. A schematic perspective view of the heat sink body of Example 1 is shown in Fig. 17. A schematic perspective view of the heat sink body of Example 2 is shown in Fig. 18. A schematic perspective view of the heat sink body of Example 3 is shown in Fig. 19. A schematic perspective view of the heat sink body of Example 4 is shown in Fig. 21. A schematic perspective view of the heat sink body of Example 5 is shown in Fig. 22. A schematic perspective view of the heat sink body of Comparative Example 2 is shown in Fig. 23. In Examples 1 to 3, the minimum thickness (wall thickness) of at least a part of the gyroid structure was changed as shown in Table 1. In Examples 4 and 5, the cell size of the unit cell forming the gyroid structure was changed as shown in Table 1. The gyroid structure of Examples 1 to 5 has a surface represented by the following formula 1 and has a non-uniform thickness. sin(X*P1)cos(Y*P2)+sin(Y*P2)cos(Z*P3)+sin(Z*P3)cos(X*P1)=0 ···Formula 1 In the above formula 1, X, Y, and Z are real numbers between -π and π, and P1, P2, and P3 are real numbers greater than 0.

[0130] Fig. 20A is a diagram showing the left, center, and right cross-sectional positions of the heat sink of Example 3. Fig. 20B is a cross-sectional view of the heat sink of Example 3 at the left, center, and right cross-sectional positions. As shown in Figures 20A and 20B, the gyroid structure 104 represented by the above formula 1 in Example 3 becomes thicker from top to bottom (from the water supply port 102 to the water drain port 105), and it is found that the thickness is non-uniform overall. FIG. 24 shows an enlarged view of the thinnest and thickest parts of the cells in the gyroid structure of Examples 1 to 5. The thickness of the gyroid structure 104 of the heat sink is calculated by calculating the pressure in the flow path when the thickness is uniform using a fluid simulation, and the thickness is made thin in the part where the pressure is high and made thick in the part where the pressure is low. As a result, in the heat sinks of Examples 1 to 5, the thinnest cell is the upstream side part. In other words, the thinnest cell is the cell in the side part at the upper part in the vertical direction. A plurality of cells are arranged in the horizontal direction upstream. For the cells arranged upstream, the thickness of the cell is thinner in the side part than in the center part. The thickest cell is the downstream side. In other words, the thickest cell is the side cell at the lower part in the vertical direction. A number of cells are arranged in the horizontal direction downstream. For the cells arranged downstream, the side cells are thicker than the center cells.

[0131] [Table 1] “*1” in Table 1: The pressure loss and heat resistance of Examples 2 to 5 were at the same level as that of Example 1. From the results in Table 1, it can be seen that Comparative Example 1 (uniform thickness) and Examples 1 to 5 (non-uniform thickness) have approximately the same level of pressure loss, but the thermal resistance of Examples 1 to 5 (non-uniform thickness) is smaller than the thermal resistance of Comparative Example 1 (uniform thickness), and thus the thermal performance is superior.

[0132] For example, aspects of the present invention are as follows. <1> 1. A heat sink having a flow passage, At least a portion of the flow passage has a gyroid structure, the gyroid structure having a non-uniform thickness. <2> The gyroid structure is represented by the following formula 1: <1> 2 is a heat sink according to the first embodiment. sin(X*P1)cos(Y*P2)+sin(Y*P2)cos(Z*P3)+sin(Z*P3)cos(X*P1)=0 ···Formula 1 In the above formula 1, X, Y, and Z are real numbers between -π and π, and P1, P2, and P3 are real numbers greater than 0. <3> The gyroid structure has a flow path including a predetermined surface, and the thickness of the surface is non-uniform. <1> from <2> 13. The heat sink according to claim 12, wherein <4> The minimum thickness (wall thickness) of at least a part of the gyroid structure is 1 mm or more. <1> from <3> 13. The heat sink according to claim 12, wherein <5> The cell size of a unit cell forming the gyroid structure is 5 mm or more. <1> from <4> 13. The heat sink according to claim 12, wherein <6> the ratio (cell size / maximum thickness) of the cell size of a unit cell forming the gyroid structure to the maximum thickness of at least a part of the gyroid structure is 2.5 or more; <5> 2 is a heat sink according to the first embodiment. <7> The said having a connecting portion <1> from <6> 13. The heat sink according to claim 12, wherein <8> The above <1> from <7> A method for manufacturing a heat sink according to any one of the preceding claims, comprising the steps of: a powder layer forming step of laminating powder to form a powder layer; A modeling liquid application process of applying a modeling liquid to the powder layer; The method for manufacturing a heat sink includes the steps of: <9> The powder is at least one selected from aluminum, zinc, magnesium, and alloys thereof. <8> This is a method for manufacturing the heat sink described above. <10> The viscosity of the modeling liquid at 25°C is 5 mPa·s or more and 50 mPa·s or less. <9> This is a method for manufacturing the heat sink described above. <11> A gyroid structure is characterized by having a predetermined surface and a non-uniform thickness. <12> The surface having the following formula 1: <11> It is a gyroid structure described in sin(X*P1)cos(Y*P2)+sin(Y*P2)cos(Z*P3)+sin(Z*P3)cos(X*P1)=0 ···Formula 1 In the above formula 1, X, Y, and Z are real numbers between -π and π, and P1, P2, and P3 are real numbers greater than 0. <13> The above <11> from <12> The present invention is a heat exchanger having a gyroid structure part comprising the gyroid structure according to any one of claims 1 to 5. <14> The above <11> from <12> A method for producing a gyroid structure according to any one of the above, a powder layer forming step of laminating powder to form a powder layer; A modeling liquid applying step of applying a modeling liquid to the powder layer; The present invention relates to a method for producing a gyroid structure, the method comprising the steps of:

[0133] The above <1> from <7> The heat sink according to any one of the preceding claims. <8> from <10> The method for manufacturing a heat sink according to any one of the above <11> from <12> The gyroid structure according to <13> The heat exchanger according to claim 1, <14> According to the method for manufacturing a gyroid structure described above, the conventional problems can be solved and the object of the present invention can be achieved. [Explanation of symbols]

[0134] 1 Modeling Department 5 Modeling Unit 10 Modeling fluid 12 Flattening roller (flattening means, rotating body) 20 powder 21, 21A, 21B supply tank 22 Modeling tank 23 Supply Stage 24 Modeling Stage 30 Modeling layer (layered modeling) 31 Powder bed (layered powder) 50 Liquid discharge unit 51 Carriage 52 Liquid ejection head (for modeling liquid) 100 Heatsink 101 Heat sink body 102 Water inlet 103 Flow Path 104 Gyroid structure 105 Drain port 107 Assembly holes 108 Gyroid Structure [Prior art documents] [Patent documents]

[0135] [Patent Document 1] JP 2020-108975 A

Claims

1. 1. A heat sink having a fluid flow path, comprising: the flow path includes an inlet for the fluid, an outlet for the fluid, and a gyroid structure having a three-dimensional periodic minimal curved surface with a non-uniform thickness in at least a part of the flow path, A heat sink, characterized in that a thickness of the three-dimensional periodic minimal surface at the outlet side is greater than a thickness of the three-dimensional periodic minimal surface at the inlet side.

2. A heat sink as described in claim 1, wherein the thickness of the three-dimensional periodic minimal curved surface at the central portion of the inlet side is greater than the thickness of the three-dimensional periodic minimal curved surface at the side portion of the inlet side.

3. A heat sink having a fluid flow path, The flow path is a fluid inlet at a vertical upper portion of the heat sink; a fluid outlet at a vertical lower portion of the heat sink; a gyroid structure having a three-dimensional periodic minimal curved surface with a non-uniform thickness in at least a part of the flow channel; Including, A heat sink, characterized in that a thickness of the three-dimensional periodic minimal curved surface at a side portion on the outlet side is greater than a thickness of the three-dimensional periodic minimal curved surface at a central portion on the outlet side.

4. The heat sink according to claim 1 , wherein the fluid is a liquid.

5. The heat sink according to claim 4 , wherein the gyroid structure has a large thickness at a portion where the liquid easily flows and a small thickness at a portion where the liquid does not easily flow.

6. The heat sink according to claim 1 , wherein the cell having the smallest thickness in the gyroid structure is a cell in a side portion at an upper portion in a vertical direction of the heat sink.

7. The heat sink according to claim 1 , wherein the cell having the greatest thickness in the gyroid structure is a cell in a side portion at a lower portion in a vertical direction of the heat sink.

8. A heat sink having a fluid flow path, comprising: the flow path includes an inlet for the fluid, an outlet for the fluid, and a gyroid structure having a three-dimensional periodic minimal curved surface with a non-uniform thickness in at least a part of the flow path, A heat sink, wherein a thickness of the three-dimensional periodic minimal curved surface on the inlet side decreases with increasing distance from the inlet in a direction perpendicular to a straight line connecting the inlet and the outlet.

9. The heat sink of claim 8, wherein the heat sink has only one inlet.

10. The heat sink of claim 1 , wherein the gyroid structure comprises a metal.

11. A heat sink described in any one of claims 1 to 10, wherein the three-dimensional periodic minimal surface is expressed by the following mathematical formula 1. sin(X*P1)cos(Y*P2)+sin(Y*P2)cos(Z*P3)+sin(Z*P3)cos(X*P1)=0...Formula 1 12. A method for manufacturing a heat sink as claimed in claim 1, comprising the steps of: a powder layer forming step of laminating powder to form a powder layer; A method for manufacturing a heat sink, comprising: a modeling liquid application process for applying a modeling liquid to the powder layer.

13. 1. A heat exchanger having a fluid flow path, the flow path includes an inlet for the fluid, an outlet for the fluid, and a gyroid structure having a three-dimensional periodic minimal curved surface with a non-uniform thickness in at least a part of the flow path, A heat exchanger comprising: a first portion of said first and second heat exchangers; a first portion of said first and second heat exchangers having a first diameter greater than a first diameter;

Citation Information

Patent Citations

  • Cooler

    JP2020035998A

  • Apparatus for three-dimensional fabrication

    JP2020108975A

  • Heat exchanger

    JP2021103060A

  • Minimal surface heat exchanger

    US20200033070A1

  • Sound suppressor

    US20210333061A1