Floor covering materials

The decorative floor material with a laminated structure and controlled moisture permeability addresses the warping and bending issues of lauan alternatives by using a moisture-proof film to stabilize dimensional changes, enhancing stability and suitability for diverse applications.

JP7563548B2Active Publication Date: 2024-10-08DAI NIPPON PRINTING CO LTD
View PDF 12 Cites 0 Cited by

Patent Information

Application Number
JP2023145862
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2009-03-11
Filing Date
2023-09-08
Publication Date
2024-10-08
Estimated Expiration
2030-03-11

AI Technical Summary

Technical Problem

Conventional wood-based decorative boards made from lauan alternatives experience significant warping and bending due to high dimensional changes with moisture, despite the use of moisture-proof sheets with insufficient permeability, which fail to prevent these issues effectively.

Method used

A decorative floor material with a laminated structure comprising a decorative sheet on the front surface and a moisture-proof film on the back surface, where both surfaces have matched moisture permeability of 7 g/m² or less within 24 hours, using specific materials and layers to control moisture flow and stabilize dimensional changes.

Benefits of technology

The solution effectively suppresses warping and bending of the decorative floor material, ensuring stability and suitability for various building applications, including floor heating, by maintaining consistent moisture permeability across surfaces.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007563548000003
    Figure 0007563548000003
  • Figure 0007563548000004
    Figure 0007563548000004
  • Figure 0007563548000005
    Figure 0007563548000005
Patent Text Reader

Abstract

To provide a laminate of a moisture-proof film and a wooden base material used for a decorative material for a floor having a reduced occurrence of curving and warping even when a decorative sheet with a low moisture permeability is laminated on a front surface of the wooden base material.SOLUTION: A laminate A of a moisture-proof film and a wooden base material used for a decorative material for a floor is formed by laminating a decorative sheet 1, a wooden base material 3 and a moisture-proof film 5 from a front surface to a rear surface, and in the laminate A, (1) the moisture-proof film has a moisture permeability equal to or less than 1 g / m2 24 hours and is a laminate B comprising a primer layer consisting of a two-part curing type urethane resin, an aluminium vapor deposition layer and a surface coat layer containing a polyvinyl alcohol resin in this order on a single surface of a thermoplastic resin film, and (2) the wooden base material has a dimension variation per 1% moisture content variation greater than 0.02% and has an average moisture content rate of 6-10 wt.%.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical Field]

[0001] The present invention relates to a decorative floor material that is suppressed from warping and bending. [Background technology]

[0002] Conventionally, wood-based decorative panels used as decorative materials for house floors have been known to have a decorative sheet with a natural wood design attached to the top surface of a wood substrate (e.g., lauan plywood made from hardwood) obtained from high-quality logs via an adhesive.

[0003] The above-mentioned broadleaf tree lauan is widely used as a wood base material, but in recent years, due to a shortage of natural resources, restrictions on timber harvesting, and other factors, it has become difficult to obtain raw wood, resulting in a growing shortage of materials. This problem is particularly serious for broadleaf trees such as lauan. For this reason, efforts are being made to develop wood base materials that can be used in place of lauan plywood. Examples of lauan alternatives include softwood plywood, wood boards made by molding and solidifying wood fibers or wood chips separated from wood waste with adhesives (e.g., medium-density wood fiberboard: MDF, high-density wood fiberboard: HDF, particleboard: PB), and fast-growing tree plywood made from fast-growing trees.

[0004] However, these lauan substitutes have the problem of greater dimensional change per 1% change in moisture content than lauan plywood, making them more susceptible to dimensional changes in response to changes in the surrounding environment. Specifically, the dimensional change per 1% moisture content of lauan plywood is 0.015 to 0.02%, while that of MDF and PB is around 0.045%, and that of softwood plywood (e.g., radiata pine) is around 0.025%. As a result, lauan substitutes are prone to warping and bending (the right angles of the floor surface becoming misaligned) due to changes in humidity.

[0005] In order to solve the above problem, it has been proposed to laminate a moisture-proof sheet on the backside of the lauan substitute material (for example, Patent Documents 1 to 3). However, the moisture-proof sheets described in Patent Documents 1 to 3 have a moisture permeability of at most 20 g / m 2The moisture permeability is about 24 hours, which is insufficient to prevent warping and bending of lauan substitute materials. In particular, in recent years, the moisture permeability of the surface of lauan substitute materials has become low (2 g / m 2 (24 hours or less) Because decorative sheets are often laminated, it is required that the moisture permeability of the back side be equal to or lower than that of the front side.

[0006] Based on the above, there is a need for the development of a flooring decorative material that suppresses warping and bending even when a lauan substitute material with a dimensional change of more than 0.02% per 1% moisture content change is used as the wood substrate and a decorative sheet with low moisture permeability is laminated on the surface. [Prior art documents] [Patent documents]

[0007] [Patent Document 1] Japanese Patent Application Laid-Open No. 2001-193267 [Patent Document 2] Japanese Patent Application Laid-Open No. 2001-260109 [Patent Document 3] Japanese Patent Application Laid-Open No. 2006-097321 Summary of the Invention [Problem to be solved by the invention]

[0008] The present invention aims to provide a decorative floor material that uses a lauan substitute material with a dimensional change of more than 0.02% per 1% moisture content change as a wood substrate, and that is suppressed from warping or buckling even when a decorative sheet with low moisture permeability is laminated on the front surface. [Means for solving the problem]

[0009] As a result of extensive research, the present inventors have found that the above object can be achieved when a specific moisture-proof film is used, and have thus completed the present invention.

[0010] That is, the present invention provides the following: Floor decorative materials Regarding. 1. A floor covering having a laminated structure including a decorative sheet, a wood substrate, and a moisture-proof film from the front to the back. With materials There 、 (1 The wood substrate has a dimensional change of more than 0.02% per 1% moisture content change, and an average moisture content of 6 to 10% by weight. the law of nature, (2) The decorative sheet has a pattern layer, a transparent resin layer containing a thermoplastic resin, and a surface protective layer in this order on a base sheet, (3) The moisture permeability of the decorative sheet is 5 g / m 2 - Less than 24 hours (4) The moisture permeability of the moisture-proof film is equal to or lower than that of the decorative sheet; (5) The floor decorative material is cut to a size of 150 mm length x 1840 mm width, and the amount of bending in the horizontal direction within 30 minutes after cutting is in the range of -1.0 mm to +0.7 mm. Characterized by Floor finishing material. 2. The decorative floor material according to item 1, wherein the decorative sheet has a synthetic resin layer having a thickness of 100 μm or more and 600 μm or less as the bottom layer.

[0011] The decorative floor material of the present invention will be described in detail below.

[0012] The floor decorative material of the present invention is a floor decorative material having a decorative sheet laminated on the front surface of a wood substrate and a moisture-proof film laminated on the back surface of the wood substrate, (1) The wood substrate has a dimensional change of more than 0.02% per 1% change in moisture content, and (2) the moisture-proof film has a moisture permeability of 7 g / m 2 The moisture permeability is measured in accordance with JIS Z0208 (moisture permeability test method (cup method)) under an environment of a temperature of 40°C and a humidity of 90% RH. Hereinafter, the moisture permeability in this specification refers to the value measured under these conditions.

[0013] The decorative floor material of the present invention having the above-mentioned characteristics has a moisture permeability of 7 g / m 2By providing a moisture-proof film with a moisture-proof film retention time of 24 hours or less, the moisture permeability of the backside of the wood substrate is kept low. Therefore, even when a lauan substitute with a dimensional change of more than 0.02% per 1% moisture content change is used as the wood substrate and a decorative sheet with low moisture permeability is laminated on the front side, the moisture permeability of the front and back sides of the wood substrate can be set to the same level, sufficiently suppressing the occurrence of warping or bending of the floor decorative material. This floor decorative material of the present invention is suitable as a floor decorative material to be applied to the floor surfaces of various buildings and as a floor decorative material for special uses such as floor heating.

[0014] Each component of the floor decorative material of the present invention will be described below. (wood base material) The wood substrate of the present invention uses a lauan substitute. That is, it is a material that can replace conventional lauan plywood, etc., and at least one of medium-density fiberboard (MDF), high-density fiberboard (HDF), particleboard (PB), softwood plywood, and fast-growing wood plywood is used. Fast-growing wood species include poplar, falcata, acacia, camellia, eucalyptus, and terminalia. These lauan substitutes have a dimensional change of more than 0.02% per 1% change in moisture content.

[0015] In this specification, the "dimensional change per 1% moisture content" is measured by the following procedure. This is the amount of dimensional change that occurs. (1) Prepare a test piece of wood substrate cut to 300 mm x 303 mm. (2) Measure the current dimensions (length of all four sides) of the test piece with a vernier caliper in a room temperature (25°C) environment. (3) Leave the test piece in a 40°C oven (humidity-free, dry atmosphere ≒ 0%) for one week. (4) After one week, measure the weight and dimensions (length of all four sides) of the test piece. (5) From the measurement data under both conditions, the dimensional change rate per 1% change in moisture content is calculated.

[0016] The thickness of the wood substrate is not particularly limited, but is preferably about 2 to 15 mm, and more preferably about 2 to 12 mm.

[0017] In the present invention, in preparation for the case where the floor decorative material is cut to fit the application location, it is preferable to use a wood substrate having an average moisture content of 6 to 10% by weight, with the moisture content in the center being in the range of -1% to +2% compared to the moisture content in the peripheral areas. For example, when the size of the wood substrate is approximately 150 mm long x 1840 mm wide (especially when the short side length is 200 mm or less), the moisture content difference between the center and peripheral areas of the wood substrate makes it prone to warping and bending. Therefore, by setting the moisture content characteristics of the wood substrate to the above conditions, it is possible to prevent warping and bending even when the floor decorative material is cut to fit the application location. Specifically, when the floor decorative material is cut to fit the application location, it is assumed that the floor decorative material will be applied to the corners of the room (near walls or around pillars).

[0018] The average moisture content of the wood substrate is preferably 6 to 10% by weight, more preferably 6.5 to 8% by weight. If the average moisture content is within the above range, it is easy to suppress the occurrence of bending or warping after cutting. In particular, when the floor decorative material is used for floor heating purposes, it is preferable to set the average moisture content to 6 to 9% by weight.

[0019] The moisture content of the central portion of the wood substrate is preferably within a range of -1% to +2% of the moisture content of the peripheral portion, and more preferably within a range of -0.5% to +1%. Note that the peripheral portion of the wood substrate refers to a 5 cm area around the wood substrate, and the central portion of the wood substrate refers to the interior of the wood substrate excluding the peripheral portion.

[0020] In this specification, the average moisture content and moisture content difference of the wood substrate (hereinafter, "moisture content difference" refers to the difference in moisture content between the peripheral part and the center part of the wood substrate) are values ​​measured by the following procedure. (A) As shown in Figure 3, prepare a wooden substrate measuring 303 mm in length and 1818 mm in width. (B) The area 5 cm from the periphery of the wood substrate is defined as the periphery, and the area inside is defined as the center. As shown in Figure 3, 35 5 cm x 5 cm samples are taken at equal intervals, as indicated by 1 to 35, and the moisture content is measured using the total drying method. The total drying method involves leaving each sample in an oven at 105°C for three days, after which the moisture content of each sample is measured using the following formula. The value before leaving is called "pre-treatment," and the value after leaving is called "post-treatment."

[0021] Moisture content (%) = {(weight before treatment - weight after treatment) / weight after treatment} x 100 (C) The average value of the 35 samples is taken as the "average moisture content." (D) The "moisture content difference" is calculated by subtracting the average value of the samples (20 samples) from the average value of the samples (15 samples) in the center. (decorative sheet) A decorative sheet is laminated on the front surface of the wood substrate. The decorative sheet has a moisture permeability of 7g / m at a temperature of 40°C and a humidity of 90%. 2 24 hours or less is preferable, 5g / m 2 A life of 24 hours or less is even more preferable. The structure of the decorative sheet is not limited, but for example, a decorative sheet having a picture layer (solid ink layer / pattern ink layer), a transparent resin layer, and a surface protection layer in this order on a base sheet is preferred. This decorative sheet will be described below as an example.

[0022] Examples of base sheets include laminates of one or more of the following: 1) paper such as tissue paper, high-quality paper, kraft paper, Japanese paper, titanium paper, resin-impregnated paper, and reinforced paper; 2) woven or nonwoven fabrics made of wood fiber, glass fiber, asbestos, polyester fiber, vinylon fiber, rayon fiber, and the like; and 3) synthetic resin sheets such as polyolefin, polyester, polyacrylic, polyamide, polyurethane, and polystyrene.

[0023] The thickness of the substrate sheet is preferably about 20 to 300 μm. The substrate sheet may be colored as needed. The surface may be subjected to a surface treatment such as corona discharge treatment, plasma treatment, or ozone treatment.

[0024] The design layer is composed of a design ink layer and / or a solid ink layer. The design layer can be formed by a printing method such as gravure printing, offset printing, or silk screen printing. Examples of patterns in the design ink layer include wood grain patterns, pebble patterns, fabric patterns, leather patterns, geometric patterns, letters, symbols, line drawings, and various abstract patterns. The solid ink layer is obtained by solid printing of colored inks. The design layer is composed of one or both of a design ink layer and a solid ink layer.

[0025] The ink used for the design layer may be a mixture of one or more of the following vehicles: chlorinated polyolefins such as chlorinated polyethylene and chlorinated polypropylene, polyester, polyurethanes made from isocyanates and polyols, polyacrylics, polyvinyl acetate, polyvinyl chloride, vinyl chloride-vinyl acetate copolymers, cellulose-based resins, polyamide-based resins, etc., to which pigments, solvents, various auxiliary agents, etc. are added to form an ink. Among these, from the viewpoints of environmental issues, adhesion to the printed surface, etc., a mixture of one or more of polyesters, polyurethanes made from isocyanates and polyols, polyacrylics, polyamide-based resins, etc. is preferred.

[0026] The transparent resin layer is not particularly limited as long as it is a transparent resin layer, and can be suitably formed from, for example, a transparent thermoplastic resin.

[0027] Specific examples include soft, semi-rigid, or rigid polyvinyl chloride, polyethylene terephthalate, polybutylene terephthalate, polyamide, polyethylene, polypropylene, ethylene-vinyl acetate copolymer, ethylene-acrylic acid copolymer, ethylene-acrylic acid ester copolymer, ionomer, acrylic acid ester, methacrylic acid ester, etc. Among the above, polyolefin resins such as polypropylene are preferred.

[0028] The transparent resin layer may be colored by adding a colorant to the thermoplastic resin. The colorant may be the same pigment or dye as that used in the design layer.

[0029] The transparent resin layer may contain various additives such as fillers, matting agents, foaming agents, flame retardants, lubricants, antistatic agents, antioxidants, ultraviolet absorbers, light stabilizers, radical scavengers, and soft components (e.g., rubber).

[0030] The surface protective layer (transparent surface protective layer) is provided to impart surface properties required of the decorative sheet, such as scratch resistance, abrasion resistance, water resistance, and contamination resistance. The resin forming this surface protective layer is preferably a curable resin such as a thermosetting resin or an ionizing radiation curable resin. In particular, ionizing radiation curable resins are preferred from the viewpoints of high surface hardness, productivity, etc.

[0031] Examples of thermosetting resins include unsaturated polyester resins, polyurethane resins (including two-component curing polyurethanes), epoxy resins, aminoalkyd resins, phenolic resins, urea resins, diallyl phthalate resins, melamine resins, guanamine resins, melamine-urea co-condensation resins, silicon resins, and polysiloxane resins.

[0032] The resin may contain a curing agent such as a crosslinking agent or a polymerization initiator, or a polymerization accelerator. For example, curing agents such as isocyanate and organic sulfonate may be added to unsaturated polyester resins and polyurethane resins, organic amines may be added to epoxy resins, and peroxides such as methyl ethyl ketone peroxide and radical initiators such as azoisobutylnitrile may be added to unsaturated polyester resins.

[0033] Examples of methods for forming a surface protective layer using a thermosetting resin include applying a solution of the thermosetting resin by a coating method such as roll coating or gravure coating, followed by drying and curing. The amount of solution applied is approximately 5 to 30 μm, preferably 5 to 20 μm, in terms of solid content.

[0034] The ionizing radiation-curable resin is not limited as long as it undergoes a crosslinking polymerization reaction upon irradiation with ionizing radiation and changes into a three-dimensional polymer structure. For example, one or more prepolymers, oligomers, and monomers having a polymerizable unsaturated bond or epoxy group in the molecule that can be crosslinked upon irradiation with ionizing radiation can be used. Examples include acrylate resins such as urethane acrylate, polyester acrylate, and epoxy acrylate; silicon resins such as siloxane; polyester resins; and epoxy resins.

[0035] Ionizing radiation includes visible light, ultraviolet light (near ultraviolet light, vacuum ultraviolet light, etc.), X-rays, electron beams, ion beams, etc., and among these, ultraviolet light and electron beams are preferred.

[0036] Usable ultraviolet light sources include ultra-high pressure mercury lamps, high pressure mercury lamps, low pressure mercury lamps, carbon arc lamps, black light fluorescent lamps, and metal halide lamps. The wavelength of ultraviolet light is approximately 190 to 380 nm.

[0037] As the electron beam source, various electron beam accelerators can be used, such as Cockcroft-Waldt type, Van de Graaf type, resonant transformer type, insulating core transformer type, linear type, dynamitron type, and high frequency type. The energy of the electron beam is preferably about 100 to 1000 keV, more preferably about 100 to 300 keV. The dose of the electron beam is preferably about 2 to 15 Mrad.

[0038] Ionizing radiation curable resins are sufficiently cured by irradiation with electron beams, but when curing is performed by irradiation with ultraviolet rays, it is preferable to add a photopolymerization initiator (sensitizer).

[0039] For resin systems having radically polymerizable unsaturated groups, the photopolymerization initiator may be at least one of acetophenones, benzophenones, thioxanthones, benzoin, benzoin methyl ether, Michler's benzoyl benzoate, Michler's ketone, diphenyl sulfide, dibenzyl disulfide, diethyl oxide, triphenyl biimidazole, isopropyl-N,N-dimethylaminobenzoate, etc. For resin systems having cationically polymerizable functional groups, the photopolymerization initiator may be at least one of aromatic diazonium salts, aromatic sulfonium salts, metallocene compounds, benzoin sulfonate esters, furyloxysulfoxonium diallyliodosyl salts, etc.

[0040] The amount of the photopolymerization initiator added is not particularly limited, but is generally about 0.1 to 10 parts by weight per 100 parts by weight of the ionizing radiation curable resin.

[0041] The protective layer can be formed from an ionizing radiation curable resin by, for example, applying a solution of the ionizing radiation curable resin by a coating method such as gravure coating or roll coating. The amount of the solution to be applied is generally 5 to 30 μm, preferably about 5 to 20 μm, in terms of solid content.

[0042] To further impart scratch resistance and abrasion resistance to a surface protective layer formed from an ionizing radiation curable resin, an inorganic filler may be blended in. Examples of inorganic fillers include powdered aluminum oxide, silicon carbide, silicon dioxide, calcium titanate, barium titanate, magnesium pyroborate, zinc oxide, silicon nitride, zirconium oxide, chromium oxide, iron oxide, boron nitride, diamond, emery sand, and glass fiber.

[0043] The amount of inorganic filler added is about 1 to 80 parts by weight per 100 parts by weight of the ionizing radiation curable resin.

[0044] The lamination of each layer can be carried out, for example, by forming a pattern layer (solid ink layer, pattern ink layer) in that order by printing on one side of a base sheet, and then laminating a transparent resin layer on the pattern layer using a dry lamination method, a T-die extrusion method, or the like, via a known dry lamination adhesive such as a two-component curing urethane resin, and then forming a surface protective layer.

[0045] A concave-convex pattern may be formed by embossing the surface protective layer side. The concave-convex pattern can be formed by hot pressing, hairline processing, etc. Examples of the concave-convex pattern include vessel grooves, stone slab surface irregularities, cloth surface texture, matte finish, sand grain, hairline, and linear grooves.

[0046] The decorative sheet may have a synthetic resin layer (so-called backer layer) with a thickness of 100 μm or more as the bottom layer (the layer that adheres to the wood substrate). The backer layer refers to a buffer layer in floor decorative materials intended for shock absorption, etc. Examples of materials that can be used to form the backer layer include polypropylene, ethylene-vinyl alcohol copolymer, polymethylene, polymethylpentene, polyethylene terephthalate, highly heat-resistant polyalkylene terephthalate (e.g., polyethylene terephthalate in which part of the ethylene glycol is replaced with 1,4-cyclohexanedimethanol or diethylene glycol, known as PET-G (manufactured by Eastman Chemical Company)), polybutylene terephthalate, polyethylene naphthalate, polyethylene naphthalate-isophthalate copolymer, polycarbonate, polyarylate, polyimide, polystyrene, polyamide, and ABS. These resins can be used alone or in combination. The upper limit of the backer layer thickness is not limited, but 600 μm is appropriate.

[0047] When laminating the decorative sheet to the wood substrate, known adhesives can be used. Examples of adhesives include those containing polyvinyl acetate, polyvinyl chloride, vinyl chloride-vinyl acetate copolymer, ethylene-acrylic acid copolymer, ionomer, butadiene-acrylonitrile rubber, neoprene rubber, natural rubber, etc. as active ingredients. The thickness of the adhesive layer is not limited, but is preferably about 0.1 to 50 μm. (moisture-proof film) The moisture-proof film is provided on the back surface of the wood substrate. In the present invention, the moisture-proof film has a moisture permeability of 7 g / m at a temperature of 40°C and a humidity of 90%. 2 Use materials with a moisture permeability of 5g / m or less. 2 - Preferably less than 24 hours.

[0048] The moisture-proof film is not limited as long as it satisfies the above moisture permeability requirements, and examples of films that can be used include synthetic resin films such as olefin-based thermoplastic resins such as polyethylene and polypropylene, and ester-based thermoplastic resins such as polyethylene terephthalate, polybutylene terephthalate, and polyethylene naphthalate. Among these, films having at least a synthetic resin substrate layer and a vapor-deposited layer are particularly preferred. This embodiment will be described below by way of example.

[0049] The synthetic resin base layer may be an olefin-based thermoplastic such as polyethylene, polypropylene, ethylene-propylene copolymer, ethylene-vinyl alcohol copolymer, or a mixture thereof. thermoplastic resins; ester-based thermoplastic resins such as polyethylene terephthalate, polybutylene terephthalate, polyethylene naphthalate, polyethylene naphthalate-isophthalate copolymer, polycarbonate, and polyarylate; acrylic-based thermoplastic resins such as polymethyl methacrylate, polyethyl methacrylate, and polybutyl acrylate; and non-halogen-based thermoplastic resins such as polyimide, polyurethane, polystyrene, and acrylonitrile-butadiene-styrene resin.

[0050] The synthetic resin substrate layer may be a uniaxially or biaxially stretched sheet, or may be unstretched. It is preferable that a vapor deposition layer is further laminated on the synthetic resin substrate layer. Since the synthetic resin substrate layer functions as a substrate on which the vapor deposition layer is formed, a biaxially stretched sheet is preferred for reasons such as high mechanical strength and excellent dimensional stability. The thickness of the synthetic resin substrate layer is generally 9 to 25 μm.

[0051] Examples of the vapor-deposited layer include a vapor-deposited layer of an inorganic material made of a thin metal film, such as aluminum, and an inorganic oxide vapor-deposited layer made of a thin inorganic oxide film, such as silicon oxide, magnesium oxide, or aluminum oxide. The vapor-deposited layer is formed on the synthetic resin substrate layer by a well-known vapor deposition method, such as vacuum vapor deposition or plasma-activated chemical reaction vapor deposition. A transparent inorganic oxide vapor-deposited layer is more preferred.

[0052] In order to further improve the gas barrier properties of the vapor deposition layer, a surface coating layer may be provided on the vapor deposition layer. Examples of the surface coating layer include polyvinyl alcohol-based resins. 1 n M(OR 2 ) m (wherein, R 1 , R 2 These compositions include those prepared by polycondensation of at least one alkoxide represented by the formula (where n represents an organic group having 1 to 8 carbon atoms, M represents a metal atom, n represents an integer of 0 or greater, m represents an integer of 1 or greater, and n + m represents the valence of M) with a polyvinyl alcohol resin and / or an ethylene-vinyl alcohol copolymer by a sol-gel process in the presence of a sol-gel catalyst, acid, water, and an organic solvent. Furthermore, the combination of polyvinyl alcohol and an ethylene-vinyl alcohol copolymer significantly improves gas barrier properties, water resistance, weather resistance, and other properties. Silane coupling agents may also be added to the compositions. A surface coating layer can be obtained by applying these resins or compositions to a vapor-deposited layer using well-known coating methods such as roll coating or gravure coating. The surface coating layer also functions as a protective layer for the vapor-deposited layer, and its thickness is approximately 1 to 10 μm.

[0053] The synthetic resin substrate layer and / or the surface coating layer may be subjected to a surface treatment such as a corona treatment, if necessary, which can further increase the adhesive strength with adjacent layers.

[0054] In the present invention, a primer layer may be further provided between the synthetic resin substrate layer and the vapor-deposited layer, and on one or both sides of the moisture-proof film. Thus, a suitable embodiment of the moisture-proof film is, for example, a "synthetic resin substrate layer / primer layer / vapor-deposited layer / surface coating layer" embodiment, and further, the moisture-proof film may have a primer layer provided on one or both sides.

[0055] These primer layers are provided to improve the adhesion between the synthetic resin substrate layer and the vapor-deposited layer, and to improve the adhesion when the moisture-proof film is laminated to other layers.

[0056] Examples of resins used for such a primer layer include ester resins, urethane resins, acrylic resins, polycarbonate resins, vinyl chloride-vinyl acetate copolymers, polyvinyl butyral resins, and nitrocellulose resins, and these resins can be used alone or in combination. The primer layer can be formed using an appropriate coating method such as roll coating or gravure printing.

[0057] Among these, the primer layer is made of (i) a copolymer of an acrylic resin and a urethane resin and (ii) ) isocyanate. That is, (i) acrylic resin and urethane The copolymer with the resin is obtained by blending and reacting an acrylic polymer component (component A) having hydroxyl groups at its terminals, a polyester polyol component (component B) having hydroxyl groups at both terminals, and a diisocyanate component (component C) to form a prepolymer, and then adding a chain extender (component D) such as a diamine to the prepolymer to extend the chain. This reaction forms a polyester urethane and introduces the acrylic polymer component into the molecule, forming an acrylic-polyester urethane copolymer having hydroxyl groups at its terminals. The hydroxyl groups at the terminals of this acrylic-polyester urethane copolymer are then reacted with the isocyanate (ii) to harden the copolymer.

[0058] A linear acrylic ester polymer having terminal hydroxyl groups is used as the component A. Specifically, linear polymethyl methacrylate (PMMA) having terminal hydroxyl groups is preferred because it has excellent weather resistance (particularly resistance to light degradation) and is easy to copolymerize with urethane. The component A becomes the acrylic resin component in the copolymer, and is preferably used with a molecular weight of 5,000 to 7,000 (weight-average molecular weight) because it has particularly good weather resistance and adhesive properties. Furthermore, the component A may be one having hydroxyl groups at both ends alone, or one having a conjugated double bond remaining at one end may be mixed with the above-mentioned one having hydroxyl groups at both ends.

[0059] Component B reacts with diisocyanate to form a polyester urethane, constituting the urethane resin component of the copolymer. Component B is a polyester diol having hydroxyl groups at both ends. Examples of this polyester diol include an addition reaction product of a diol compound having an aromatic or spiro ring skeleton with a lactone compound or its derivative, or an epoxy compound, a condensation product of a dibasic acid with a diol, and a polyester compound derived from a cyclic ester compound. Examples of the diol include short-chain diols such as ethylene glycol, propylene glycol, diethylene glycol, butanediol, hexanediol, and methylpentenediol; and alicyclic short-chain diols such as 1,4-cyclohexanedimethanol. Examples of dibasic acids include adipic acid, phthalic acid, isophthalic acid, and terephthalic acid. A preferred polyester polyol is an adipate polyester using adipic acid or a mixture of adipic acid and terephthalic acid, particularly adipic acid, as the acid component and 3-methylpentenediol and 1,4-cyclohexanedimethanol as the diol component.

[0060] In the primer layer, the urethane resin component formed by the reaction of Component B and Component C imparts flexibility to the primer layer and contributes to improved adhesion. Furthermore, the acrylic resin component composed of an acrylic polymer contributes to weather resistance and blocking resistance in the primer layer. The molecular weight of Component B in the urethane resin may be within a range that allows the urethane resin to exhibit sufficient flexibility in the primer layer. In the case of a polyester diol composed of adipic acid or a mixture of adipic acid and terephthalic acid, 3-methylpentanediol, and 1,4-cyclohexanedimethanol, a molecular weight of 500 to 5,000 (weight average molecular weight) is preferred.

[0061] As the component C, an aliphatic or alicyclic diisocyanate compound having two isocyanate groups per molecule is used. Examples of this diisocyanate include tetramethylene diisocyanate, 2,2,4(2,4,4)-1,6-hexamethylene diisocyanate, isophorone diisocyanate, 4,4'-dicyclohexylmethane diisocyanate, and 1,4'-cyclohexyl diisocyanate. As the diisocyanate component, isophorone diisocyanate is preferred in terms of physical properties and cost. When reacting components A to C, the equivalent ratio of the total hydroxyl groups (or amino groups) of the acrylic polymer, polyester polyol, and chain extender described below to the isocyanate groups is set so that the isocyanate groups are in excess.

[0062] When the three components A, B, and C are reacted at 60 to 120°C for about 2 to 10 hours, the isocyanate groups of the diisocyanate react with the hydroxyl groups at the terminals of the polyester polyol to form a polyester urethane resin component, and a compound in which diisocyanate is added to the hydroxyl groups at the terminals of the acrylic polymer is also mixed in, forming a prepolymer in which excess isocyanate groups and hydroxyl groups remain. A diamine such as isophorone diamine or hexamethylene diamine is added to this prepolymer as a chain extender to react the isocyanate groups with the chain extender, thereby introducing the acrylic polymer component into the polyester urethane molecule and obtaining an acrylic-polyester urethane copolymer (i) having hydroxyl groups at the terminals. can be done.

[0063] (i) Acrylic-polyester urethane copolymer is added with (ii) isocyanate. The primer layer can be formed by preparing a coating solution having a required viscosity, taking into consideration the coating method and the amount of coating after drying, and applying the solution by a known coating method such as gravure coating or roll coating. Any isocyanate may be used as long as it can react with the hydroxyl groups of the olefin-polyesterurethane copolymer to crosslink and harden it, for example, a divalent or higher aliphatic or aromatic isocyanate can be used, and aliphatic isocyanates are particularly desirable from the viewpoints of preventing thermal discoloration and weather resistance. Specific examples include polyisocyanates such as monomers of tolylene diisocyanate, xylylene diisocyanate, 4,4'-dicyclohexylmethane diisocyanate, hexamethylene diisocyanate, and lysine diisocyanate, as well as multimers such as dimers and trimers of these, and derivatives (adducts) of these isocyanates added to polyols.

[0064] The amount of the primer layer applied after drying is 1 to 20 g / m 2 and preferably 1 to 5 g / m 2 The primer layer may contain additives such as a filler such as silica powder, a light stabilizer, and a colorant, if necessary.

[0065] When laminating the moisture-proof sheet to the wood substrate, known adhesives can be used. Examples of adhesives include those containing polyvinyl acetate, polyvinyl chloride, vinyl chloride-vinyl acetate copolymer, ethylene-acrylic acid copolymer, ionomer, butadiene-acrylonitrile rubber, neoprene rubber, and natural rubber as active ingredients. The thickness of the adhesive layer is not limited, but is preferably about 0.1 to 50 μm. [Effects of the Invention]

[0066] The floor decorative material of the present invention has a moisture permeability of 7 g / m 2By providing a moisture-proof film with a moisture-proof film retention time of 24 hours or less, the moisture permeability of the backside of the wood substrate is kept low. Therefore, even when a lauan substitute with a dimensional change of more than 0.02% per 1% moisture content change is used as the wood substrate and a decorative sheet with low moisture permeability is laminated on the front side, the moisture permeability of the front and back sides of the wood substrate can be set to the same level, sufficiently suppressing the occurrence of warping or bending of the floor decorative material. This floor decorative material of the present invention is suitable as a floor decorative material to be applied to the floor surfaces of various buildings and as a floor decorative material for special uses such as floor heating. [Brief explanation of the drawings]

[0067] [Figure 1] 1 is a schematic diagram (one example) of a floor decorative material of the present invention. [Figure 2] 1 is a schematic diagram showing warping and bending of a floor decorative material. FIG. [Figure 3] FIG. 1 is a diagram showing samples used to measure the average moisture content and moisture content difference of wood substrates. [Figure 4] This is a schematic diagram of floor heating system test standard II. [Explanation of symbols]

[0068] 1. Decorative sheet 2.Adhesive layer 3. Wood-based materials (lauan substitute materials) 4.Adhesive layer 5. Moisture-proof film DETAILED DESCRIPTION OF THE INVENTION

[0069] The present invention will be described in more detail below with reference to examples and comparative examples, but the present invention is not limited to these examples.

[0070] Example 1 (1) A decorative sheet (0.4 mm) containing a synthetic resin layer was attached to the front surface of a 5.5 mm thick MDF (wood substrate) using a Chuo Rika Kogyo adhesive (BA-10L / BA-11B, 9 g / square shaku). The dimensional change rate per 1% moisture content change of the MDF was 0.05%. Note that square shaku refers to the area of ​​a plane measured 303 mm long x 303 mm wide (the same applies below). (2) Apply moisture-proof adhesive (BA-10L / BA-11B, 9g / square foot) to the back of the MDF. The laminate in this state is called a decorative board. (3) The decorative panel was cut to a size of 313 mm long x 1840 mm wide using a gang saw. (4) In addition, a Tenon processing machine was used to perform tongue processing, edge chamfering, and V-groove processing (V-groove processing width: 1.5 mm). (5) Furthermore, in the painting line, paint was applied to the tongue-processed areas, the chamfered end areas, and the V-groove processed areas (paint: paint containing two-component curing urethane resin).

[0071] Through the above steps, a floor decorative material was produced.

[0072] The moisture-proof film was fabricated as follows: a 12 μm-thick biaxially oriented polyethylene terephthalate film was prepared, and a primer layer made of a two-component curing urethane resin was applied to one side. An aluminum vapor-deposited layer was then applied on top of the primer layer. The resulting film is called a "vapor-deposited PET film."

[0073] A surface coating layer made of PVA / silicate was applied to the vapor-deposited PET film at a rate of 0.2 g / m. 2 A laminate (synthetic resin substrate layer (PET) / vapor deposition layer / surface coating layer) was prepared by forming a laminate (dry state). After corona discharge treatment on both sides of the laminate, a two-component curing resin, in which a curing agent (isocyanate) was added to a base resin (a mixture of urethane resin and soluble nitrocellulose resin), was applied by gravure printing at a solid content of 5 g / m2 each. 2 The adhesive primer layer was formed on both sides of the film. This resulted in a moisture-proof film (moisture permeability 1 g / m 2·24 hours).

[0074] Example 2 A floor decorative material was produced in the same manner as in Example 1, except that a 9 mm thick particle board (the dimensional change rate per 1% change in moisture content was 0.049%) was used as the wood substrate.

[0075] Example 3 A floor decorative material was produced in the same manner as in Example 1, except that a 12 mm thick softwood plywood (Radiata pine, dimensional change rate per 1% moisture content change: 0.026%) was used as the wood substrate.

[0076] Example 4 PE (polyethylene sheet) as a moisture-proof film. Moisture permeability 7g / m 2 A floor decorative material was prepared in the same manner as in Example 1, except that a floor decorative material was used (for 24 hours).

[0077] Comparative Example 1 A floor decorative material was produced in the same manner as in Example 1, except that no moisture-proof film was used.

[0078] Comparative Example 2 A floor decorative material was produced in the same manner as in Example 2, except that no moisture-proof film was used.

[0079] Comparative Example 3 A floor decorative material was produced in the same manner as in Example 3, except that no moisture-proof film was used.

[0080] Comparative Example 4 Moisture-proof paper (polyethylene core layer, paper laminated on both sides) is used as a moisture-proof film. Moisture permeability 10g / m 2 A floor decorative material was prepared in the same manner as in Example 1, except that a floor decorative material was used (for 24 hours).

[0081] Conventional example 1 A floor decorative material was produced in the same manner as in Example 1, except that 12 mm thick lauan plywood (the dimensional change rate per 1% moisture content change was 0.016%) was used as the wood substrate and no moisture-proof film was used.

[0082] Test example 1 (warping and bending in a 40°C atmosphere) The floor decorative materials prepared in Examples 1 to 4, Comparative Examples 1 to 4, and Conventional Example 1 were placed in a 40°C atmosphere (dry The floor decorative material was left in the same atmosphere for 7 days, and the amount of warping and the amount of bending were measured.

[0083] A schematic diagram of the amount of warping and the amount of bending is shown in Figure 2. The amount of warping and the amount of bending were measured using a feeler gauge. A warping amount of 20 mm / 1840 mm (amount of warping relative to the horizontal length) or less is acceptable (suitable for practical use). Also, a bending amount of 0.3 mm / 1840 mm (amount of bending relative to the horizontal length) or less is unacceptable ( The results are shown in Table 1.

[0084] Test example 2 (warping and bending in a 40°C, 90% RH atmosphere) The floor decorative materials produced in the examples and comparative examples were left to stand (for 7 days) in an atmosphere of 40°C and 90% RH, and the amount of warping and the amount of bending of the floor decorative materials were measured in the same manner as in Test Example 1. The results are shown in Table 1.

[0085] [Table 1]

[0086] As is clear from the results in Table 1 above, the moisture permeability is 7 g / m 2 The decorative floor material of the present invention, which is provided with a moisture-proof film with a shelf life of 24 hours or less, effectively suppresses dimensional changes in the wood substrate due to humidity due to the presence of the moisture-proof film. As a result, warping and bending of the decorative floor material are prevented, and the test results are closer to those of Conventional Example 1 (using lauan plywood).

[0087] Example 5 (1) Floor decorative sheet (0.16 mm thick, moisture permeability: 3 g / m 224 hours) with Chuo Rika Kogyo Co., Ltd. Using adhesive (BA-10L / BA-11B, 9g / shaku square), 12mm thick particle board (PB) (wood The dimensional change rate per 1% moisture content change of the PB was 0.045%, and the average moisture content was 6.5% by weight. (2) Apply a moisture-proof film to the back of the PB using Chuo Rika Kogyo adhesive (BA-10L / BA-11B, 9g / square meter). Film (PET film + vapor deposition layer, moisture permeability: 3g / m 2 (24 hours) was stuck together. The laminate is called a decorative board. (3) The decorative panel was cut to a size of 313 mm long x 1840 mm wide using a gang saw. (4) In addition, a Tenon processing machine was used to perform tongue processing, edge chamfering, and V-groove processing (V-groove processing width: 1.5 mm). (5) Furthermore, in the painting line, paint was applied to the tongue-processed areas, the chamfered end areas, and the V-groove processed areas (paint: paint containing two-component curing urethane resin).

[0088] A floor decorative material was produced through the above steps. Between each step, the decorative board was wrapped in PP film (30 μm thick, moisture permeability 15 g) for moisture protection.

[0089] Example 6 A floor decorative material was produced in the same manner as in Example 5, except that moisture-proofing treatment using PP film was not performed between each process. This resulted in the moisture content of the peripheral part of the wood substrate being higher than that of the central part.

[0090] Example 7 A floor decorative material was produced in the same manner as in Example 5, except that a PB substrate was used in which the moisture content of the central part of the wood substrate was 2% higher than that of the peripheral part.

[0091] Example 8 A floor decorative material was produced in the same manner as in Example 5, except that softwood plywood in which the moisture content in the center of the wood substrate was 1.7% higher than in the periphery was used.

[0092] Comparative Example 5 A floor decorative material was produced in the same manner as in Example 6, except that PB with an average moisture content of 5.5% was used as the wood substrate.

[0093] Comparative Example 6 A floor decorative material was produced in the same manner as in Example 6, except that after Tenona processing, the material was left for one week without being subjected to moisture-proofing treatment.

[0094] Comparative Example 7 A floor decorative material was produced in the same manner as in Example 5, except that a PB base material was used in which the moisture content of the central part of the wood was 2.5% higher than that of the peripheral part.

[0095] Comparative Example 8 A floor decorative material was produced in the same manner as in Example 5, except that the average moisture content was adjusted to 10.5% and a PB base material was used in which the moisture content in the center of the wood was 1.3% lower than in the peripheral areas.

[0096] Test Example 3 (evaluation of bending and application suitability after cutting floor decorative material) <Evaluation of bending amount after cutting> The floor decorative materials (length 313 mm × width 1840 mm) produced in Examples 5 to 8 and Comparative Examples 5 to 8 were placed in the center It was cut into approximately half (150mm long x 1840mm wide) at the end.

[0097] The cut flooring was measured for the amount of lateral bending using a straight ruler and gap gauge. Measurements were taken within 30 minutes of cutting. The amount of bending was indicated as + when each tongue side (male tongue, female tongue) was convex.

[0098] The amount of bending after cutting is acceptable if it is within the range of "-1.0mm / 1840mm width to +0.7mm / 1840mm width". <Construction suitability evaluation> The floor decorative materials (length 313 mm × width 1840 mm) produced in Examples 5 to 8 and Comparative Examples 5 to 8 were First, it was installed in its original size. Then, it was cut in half in the center (150mm long x 1840mm wide). The floor decorative material was applied within 30 minutes after cutting, and the application suitability after cutting was evaluated. The evaluation criteria were as follows:

[0099] ○: Installation was carried out without any problems, just like before cutting, and no gaps were observed at the joints.

[0100] △: With some effort, it can be installed and no gaps can be seen at the joints.

[0101] ×: Construction is difficult and gaps exceeding 0.3 mm are observed at the joints.

[0102] Test example 4 (floor heating system test) The floor decorative materials (length 313 mm × width 1840 mm) produced in Examples 5 to 8 and Comparative Examples 5 to 8 were placed in a floor heating system. The floor heating system was tested in a room system test. Floor heating systems are generally not installed in the corners of a room (near walls or around pillars), but in the center of the room excluding the corners. Therefore, in Test Example 4, a floor heating system test was conducted on a floor decorative material (length 313 mm x width 1840 mm).

[0103] Specifically, test specimens were made of tongue-and-groove floor decorative materials and subjected to the floor heating system test shown in Figure 4 (finishing materials and undercoating materials, "II. Durability performance, heat endurance test" 80°C hot water x 1100 hours of continuous hot water supply, gas company unified standard method).

[0104] Regarding the test pieces after the test, (1) If the gap displacement of the tongue and groove part (fitting part) is 0.5 mm or less, it passes. (2) If the step displacement of the tongue and groove part (fitting part) is 0.5 mm or less, it passes. (3) If the warpage in the horizontal direction (1840 mm) (= width warpage) is less than 1 mm, it passes. The evaluation was carried out according to the following criteria. A product that passed all the requirements was marked with a circle, and a product that did not meet even one of the requirements was marked with an X.

[0105] The evaluation and test results are shown in Table 2 below.

[0106] [Table 2]

[0107] As is clear from the results in Table 2 above, bending after cutting can be effectively suppressed by using a wood substrate in which the average moisture content is 6 to 10% by weight and the moisture content in the center is in the range of -1% to +2% compared to the moisture content in the peripheral area. In addition, the floor decorative material of the present invention has a moisture-proof film with a moisture permeability of 7 g / m 2 -Because it lasts for 24 hours or less, it can also be used as a flooring material for underfloor heating.

Claims

1. A floor decorative material having a laminated structure including a decorative sheet, a wood base material, and a moisture-proof film from the front surface to the back surface, (1) The wood base material has a dimensional change of more than 0.02% per 1% moisture content change and an average moisture content of 6 to 10% by weight; (2) The decorative sheet has a pattern layer, a transparent resin layer containing a thermoplastic resin, and a surface protective layer on a base sheet in this order; (3) The decorative sheet has a moisture permeability of 5 g / m 2 ·24 hours or less; (4) The moisture permeability of the moisture-proof film is equal to or lower than that of the decorative sheet; (5) The floor decorative material is cut to a size of 150 mm length x 1840 mm width, and the amount of bending in the horizontal direction within 30 minutes after cutting is in the range of -1.0 mm to +0.7 mm. A decorative floor material characterized by the above-mentioned.

2. A floor decorative material as described in claim 1, wherein the decorative sheet has a synthetic resin layer having a thickness of 100 μm or more and 600 μm or less as its bottom layer.

Citation Information

Patent Citations

  • Floor material for floor heating

    JP1995023141U

  • Dehymidifying decorative sheet and fitting such as dehumidifying decorative board and door

    JP1997174767A

  • Barrier film

    JP1997277425A

  • Manufacture of ligneous board

    JP1998044113A

  • Panel for floor heating

    JP1999264556A