Electric resistance welded steel pipe and its manufacturing method
Optimizing the steel structure and manufacturing process for ERW steel pipes and hot-rolled steel sheets addresses the challenges of coarse grains and inclusions, achieving high strength, toughness, and workability for mechanical structural applications.
Patent Information
- Application Number
- JP2023519410
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2022-05-06
- Filing Date
- 2022-12-09
- Publication Date
- 2024-10-08
- Estimated Expiration
- 2042-12-09
AI Technical Summary
Existing ERW steel pipes and hot-rolled steel sheets used in automobiles, construction machinery, and industrial machinery face challenges in achieving high strength, toughness, and workability due to the formation of coarse grains and Ti-based inclusions, which lead to reduced toughness and workability during processing.
The steel structure is optimized with a bainite volume fraction of 90% or more, average crystal grain size of 10.0 μm or less, and controlled Ti-based inclusions to enhance toughness and workability, with specific composition ranges for elements like C, Si, Mn, P, S, Al, N, and Ti, and a manufacturing process involving controlled cooling and rolling.
The solution results in ERW steel pipes with high strength, excellent workability, and improved toughness, suitable for mechanical structural applications, meeting requirements for yield stress, tensile strength, and Charpy impact values.
Smart Images

Figure 0007563585000006 
Figure 0007563585000001 
Figure 0007563585000002
Abstract
Description
[Technical field]
[0001] The present invention relates to an electric resistance welded steel pipe suitable for steel pipes for machine structures used in parts of automobiles, construction machinery, and industrial machinery, a hot rolled steel sheet which is the raw material for the electric resistance welded steel pipe, and a manufacturing method thereof. [Background technology]
[0002] In recent years, there has been a demand for stronger components in automobiles, construction machinery, and industrial machinery in order to improve fuel efficiency and reduce the size of equipment. In addition, the steel pipes for machine structures used in these applications are required to have high workability because they are subjected to processes such as bending, hydraulic bulging, and pipe end flaring according to the application. Furthermore, since the above-mentioned automobiles, construction machines, and industrial machines are sometimes used in cold climates, they also require high low-temperature toughness.
[0003] However, when the strength of a component is increased, the workability and toughness of the base material and electric resistance welded parts decrease, making it impossible to use the component for its intended purpose. Furthermore, since the workability and toughness of electric resistance welded steel pipes decrease due to work hardening during pipe making, the hot-rolled steel plate used as the raw material is required to have properties that take into account the decrease in workability and toughness during pipe making.
[0004] In order to solve the above problems, for example, Patent Document 1 proposes a steel sheet in which bainite accounts for 90 area % or more, the average equivalent circular diameter d of regions surrounded by high-angle grain boundaries with a misorientation of 15° or more is 4 μm or less, and further contains 3 to 10 area % of island martensite having an average equivalent circular diameter of 0.5 to 3 μm and a Vickers hardness Hv of 700 or more.
[0005] In addition, in Patent Document 2, the total area ratio of the martensite phase and the lower bainite structure is 85% or more, the average grain size is 20 μm or less, the area ratio of grains having an aspect ratio of 0.30 or less is 50% or less, and the {100} <011> ~{211} <011> A hot-rolled steel sheet has been proposed in which the average value of the X-ray random intensity ratio of a group of orientations is 6.0 or less and the maximum value is 8.0 or less.
[0006] Furthermore, Patent Document 3 proposes an Azuroll electric resistance welded steel pipe for torsion beams in which the area ratio of bainite is 80% or more, the average grain size of the bainite packet grains is 10 μm or less, the average aspect ratio of the packet grains is 2.0 or less, and the tensile strength in the axial direction of the pipe is 750 to 1000 MPa. [Prior art documents] [Patent documents]
[0007] [Patent Document 1] JP 2013-057105 A [Patent Document 2] JP 2017-057472 A [Patent Document 3] International Publication No. 2019 / 220577 Summary of the Invention [Problem to be solved by the invention]
[0008] However, the steel plates and electric resistance welded steel pipes described in Patent Documents 1 to 3 have improved strength, toughness, workability, fatigue properties, and the like by controlling the average crystal grain sizes of the main structures, bainite and martensite. However, no consideration has been given to the proportion of coarse grains, inclusions, or workability of electric resistance welds, and there is room for further improvement in toughness and workability.
[0009] The present invention has been made in consideration of the above circumstances, and aims to provide an electric resistance welded steel pipe that has high strength and excellent workability and toughness and is suitable for machine structural steel pipes used in parts for automobiles, construction machinery, and industrial machinery, and a hot-rolled steel sheet that is the raw material for the electric resistance welded steel pipe, as well as a manufacturing method for the same.
[0010] In the present invention, "high strength" refers to a hot-rolled steel sheet having a rolling direction yield stress of 650 MPa or more and a tensile strength of 750 MPa or more. In the hot-rolled steel sheet, the yield stress is preferably 700 MPa or more and the tensile strength is preferably 800 MPa or more. On the other hand, in the present invention, "high strength" means that, in the electric resistance welded steel pipe, the yield stress in the axial direction of the pipe is 650 MPa or more, the tensile strength is 750 MPa or more, and the Vickers hardness at the center of the wall thickness of the electric resistance weld is 200 HV or more. In the electric resistance welded steel pipe, the yield stress is preferably 700 MPa or more, the tensile strength is preferably 800 MPa or more, and the Vickers hardness is preferably 220 HV or more.
[0011] In the present invention, "excellent workability" refers to a hot-rolled steel sheet having a rolling direction yield ratio (=yield stress / tensile strength x 100) of 90.0% or less and a rolling direction total elongation of 15% or more. In the hot-rolled steel sheet, the rolling direction yield ratio is preferably 88.0% or less. In the hot-rolled steel sheet, the rolling direction total elongation is preferably 18% or more. On the other hand, "excellent workability" in the present invention means that, in the case of an electric resistance welded steel pipe, the yield ratio in the axial direction (= yield stress / tensile strength × 100) is 96.0% or less, the total elongation in the axial direction is 15% or more, and the flattening value of the electric resistance welded portion is 0.80 or less. In the case of an electric resistance welded steel pipe, the yield ratio in the axial direction is preferably 94.0% or less. In the case of an electric resistance welded steel pipe, the total elongation in the axial direction is preferably 17% or more, and the flattening value of the electric resistance welded portion is preferably 0.70 or less.
[0012] In the present invention, "excellent toughness" means that, in the case of a hot-rolled steel sheet, the Charpy impact value at -60°C is 100 J / cm 2In the case of a hot-rolled steel sheet, the Charpy impact value at -60°C is preferably 140 J / cm 2 That's all. On the other hand, in the present invention, "excellent toughness" means that, in the case of electric resistance welded steel pipe, the Charpy impact value at -20°C is 50 J / cm 2 In the electric resistance welded steel pipe, the Charpy impact value at -20°C is preferably 60 J / cm or more. 2 That's all. [Means for solving the problem]
[0013] The present inventors have conducted extensive research into the above-mentioned problems, and as a result have found that in steel mainly composed of bainite, when some crystal grains are coarse, toughness and workability decrease.
[0014] They also found that the presence of a large amount of coarse Ti-based inclusions reduces toughness. If the microstructure is coarse on average, the proportion of high-angle boundaries that act as barriers to brittle fracture decreases, and the toughness of the steel plate decreases. Even if the average grain size of the steel structure is small, if there is a certain proportion of coarse grains, these grains will become the starting points of brittle fracture, and the toughness of the steel plate will also decrease.
[0015] In other words, the strength of the coarse grains is lower than that of the surroundings, and strain is concentrated in the coarse grains. Therefore, if a certain proportion of coarse grains is present in the steel structure, the steel becomes prone to early fracture, has a reduced total elongation, and is poor in workability. Therefore, by suppressing the generation of bainite that exists as coarse grains, it is possible to improve toughness and workability.
[0016] In addition, Ti-based inclusions have a polygonal shape, and stress tends to concentrate near the corners, but these points of stress concentration tend to become the starting points of brittle fracture. Therefore, if there are a large number of coarse Ti-based inclusions, toughness decreases. Therefore, by suppressing the formation of such Ti-based inclusions, the toughness can be improved.
[0017] The present invention has been completed based on these findings and further investigations. That is, the gist of the present invention is as follows. 1. A hot-rolled steel sheet, In mass%, C: 0.020% or more and 0.200% or less, Si: 0.02% or more and 1.00% or less, Mn: 0.10% or more and 2.50% or less, P: 0.050% or less, S: 0.0200% or less, Al: 0.005% or more and 0.100% or less, N: 0.0100% or less and Ti: 0.030% or more and 0.200% or less The balance is Fe and unavoidable impurities. The volume fraction of bainite is 90% or more, and the remainder has a steel structure at the center of the plate thickness including one or more of ferrite, pearlite, martensite, and austenite, Furthermore, the steel structure at the center of the plate thickness has an average crystal grain size of 10.0 μm or less, a volume ratio of crystal grains with a grain size of 40.0 μm or more is 40% or less, and a number density of Ti-based inclusions with a major axis of 5.0 μm or more is 20 pieces / mm 2 The following is hot-rolled steel plate.
[0018] 2. The composition further includes, in mass%, Cu: 0.50% or less, Ni: 0.50% or less, Cr: 0.50% or less, Mo: 0.50% or less Nb: 0.050% or less, V: 0.050% or less, Ca: 0.0050% or less and B: 0.0050% or less The hot-rolled steel sheet according to claim 1, further comprising one or more of the following:
[0019] 3. A method for producing a hot-rolled steel sheet according to 1 or 2, A casting process in which molten steel is cast from the solidification point of the molten steel to 1200°C at an average cooling rate of 0.30°C / s or more to produce a steel material; A hot rolling process in which the steel material is heated to a heating temperature in the range of 1150°C to 1300°C, and then hot-rolled at a rough rolling end temperature of 950°C to 1180°C, a finish rolling end temperature of 850°C to 1000°C, and a total reduction ratio in the finish rolling of 50% to 80%; After the hot rolling step, a cooling step is performed in which cooling is performed at an average cooling rate at the center of the thickness of 10°C / s or more and 60°C / s or less, and a cooling stop temperature at the center of the thickness of 400°C or more and 580°C or less. a winding step of winding the sheet at a temperature of 400° C. or more and 580° C. or less after the cooling step; A method for producing a hot-rolled steel sheet, comprising:
[0020] 4. An electric resistance welded steel pipe having a base metal portion, a welded portion, and a welded heat affected portion, The base material portion comprises, in mass%, C: 0.020% or more and 0.200% or less, Si: 0.02% or more and 1.00% or less, Mn: 0.10% or more and 2.50% or less, P: 0.050% or less, S: 0.0200% or less, Al: 0.005% or more and 0.100% or less, N: 0.0100% or less and Ti: 0.030% or more and 0.200% or less The balance is Fe and unavoidable impurities. The base metal portion has a steel structure in a center of a wall thickness, the volume fraction of which is 90% or more of bainite, and the remainder is one or more of ferrite, pearlite, martensite, and austenite, Furthermore, the steel structure at the center of the thickness of the base material portion has an average crystal grain size of 10.0 μm or less, a volume fraction of crystal grains with a grain size of 40.0 μm or more is 40% or less, and a number density of Ti-based inclusions with a major axis of 5.0 μm or more is 20 pieces / mm 2 is as follows: the weld has a steel structure in a center of a wall thickness, the volume fraction of ferrite being 10% or more, the total volume fraction of ferrite and bainite being 60% or more and 98% or less, and the remainder including one or more of pearlite, martensite, and austenite; Furthermore, in the electric resistance welded steel pipe, the steel structure at the center of the wall thickness of the weld has an average crystal grain size of 15.0 μm or less.
[0021] 5. The composition of the base material portion is further, in mass%, Cu: 0.50% or less, Ni: 0.50% or less, Cr: 0.50% or less, Mo: 0.50% or less Nb: 0.050% or less, V: 0.050% or less, Ca: 0.0050% or less and B: 0.0050% or less 5. The electric resistance welded steel pipe according to claim 4, comprising one or more of the following:
[0022] 6. A method for producing an electric resistance welded steel pipe according to claim 4 or 5, a pipe-making process in which the hot-rolled steel sheet is formed into a cylindrical shape by cold rolling, and both circumferential ends of the cylindrical shape are butted together and electric resistance welded; After the pipe making process, the portion subjected to the electric resistance welding is heated to 850°C or more and 1050°C or less, and then air-cooled for 5 s or more and 50 s or less, and then water-cooled to 200°C or less. a sizing step of adjusting the outer diameter of the pipe by a sizing roll after the weld heat treatment step; A method for producing an electric resistance welded steel pipe, comprising: Effect of the Invention
[0023] According to the present invention, it is possible to provide an electric resistance welded steel pipe having high strength and excellent workability and toughness, which is suitable for steel pipes for machine structures used in parts for automobiles, construction machinery, and industrial machinery, a hot-rolled steel sheet which is the raw material for the electric resistance welded steel pipe, and a method for manufacturing the same. [Brief description of the drawings]
[0024] [Figure 1] 1 is a schematic diagram of a circumferential cross section (cross section perpendicular to the axial direction) of an electric resistance welded portion of an electric resistance welded steel pipe. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0025] Hereinafter, the hot-rolled steel sheet and the electric resistance welded steel pipe using the hot-rolled steel sheet as a base material according to the present invention, as well as the manufacturing method thereof, will be described. Note that the present invention is not limited to the following embodiments.
[0026] Here, in the present invention, when the circumferential center of the electric welded portion (also referred to as the electric welded portion in the present invention) in a cross section perpendicular to the axis of an electric welded steel pipe is defined as 0°, the chemical composition and steel structure of the base material portion 90° away from the circumferential center of the pipe are defined as the chemical composition and steel structure of the base material portion of the electric welded steel pipe in the present invention. Although the position 90° away from the electric resistance weld is specified, the chemical composition and steel structure are the same even at a position 180° away from the electric resistance weld, for example.
[0027] First, the reasons for limiting the steel structure of the base material of the hot-rolled steel sheet and electric resistance welded steel pipe of the present invention will be explained. In the steel structure of the hot-rolled steel sheet and electric resistance welded steel pipe of the present invention, the steel structure at the center of thickness of the hot-rolled steel sheet and the center of thickness of the base material part of the electric resistance welded steel pipe has a volume fraction of bainite of 90% or more, with the remainder including one or more of ferrite, pearlite, martensite and austenite. Moreover, this steel structure has an average crystal grain size of 10.0 μm or less, and the volume fraction of crystal grains with a grain size of 40.0 μm or more is 40% or less. Furthermore, this steel structure has a number density of Ti-based inclusions with a major axis of 5.0 μm or more of 20 pieces / mm 2 The following is the result. In the present invention, it is essential that the above-mentioned steel structure is defined at least at the center of thickness of the hot-rolled steel sheet and the center of thickness of the base material of the electric resistance welded steel pipe. This is because these are the final solidification positions in the casting process, and therefore the cooling rate is the slowest and the inclusions become the coarsest. Also, in the cooling process of hot rolling, the cooling rate is the slowest and the crystal grains become the coarsest.
[0028] Here, ferrite is a soft structure, and bainite is harder than ferrite and softer than pearlite, martensite, and austenite.
[0029] [Bainite volume fraction] If the volume fraction of bainite at the center of thickness of the hot-rolled steel plate and the base material of the electric resistance welded steel pipe is less than 90%, the desired yield stress or tensile strength cannot be obtained. Or, the desired toughness cannot be obtained. Therefore, the volume fraction of bainite at the center of thickness of the hot-rolled steel plate and the base material of the electric resistance welded steel pipe is set to 90% or more. The volume fraction of bainite at the center of thickness of the hot-rolled steel plate and the base material of the electric resistance welded steel pipe is preferably 93% or more, and more preferably 96% or more. Although there is no particular upper limit for the volume fraction of bainite at the center of thickness of a hot-rolled steel plate and at the center of thickness of the base material of an electric resistance welded steel pipe, it is preferable to set it to 99% or less from the viewpoint of ductility. In the present invention, the volume fraction of each structure such as bainite is a value that occupies the entire steel structure in the same field of view at the target position.
[0030] [Remainder: one or more of austenite, ferrite, pearlite and martensite] The center of thickness of the hot-rolled steel plate and the remainder of the base material of the electric resistance welded steel pipe contain one or more of austenite, ferrite, pearlite, and martensite. Each of these structures has a hardness difference from bainite, and stress is concentrated at the interface with bainite. If the total volume fraction of these structures exceeds 10%, the area of the interface with bainite increases, and fracture is likely to occur due to stress concentration, resulting in a decrease in toughness. Therefore, the total volume fraction of these structures is set to 10% or less, preferably 7% or less, and more preferably 4% or less. Since it is difficult to completely suppress the formation of these structures in the cooling process in hot rolling, a lower limit of about 1% is allowed for the total volume fraction.
[0031] Among the above steel structures, the various structures except for austenite have austenite grain boundaries or deformation bands within austenite grains as nucleation sites. That is, in hot rolling, by increasing the reduction at a low temperature where austenite recrystallization is difficult to occur, a large number of dislocations can be introduced into the austenite to refine the austenite and a large number of deformation bands can be introduced into the grains. As a result, in the present invention, the area of the nucleation sites increases, the frequency of nucleation increases, and the steel structure can be refined.
[0032] In the present invention, the steel structure can be observed by the method described below or in the examples described later. That is, first, test pieces for microstructural observation are taken so that the observation surface is a cross-section parallel to both the rolling direction and the plate thickness direction of a hot-rolled steel plate and at the center of the plate thickness, and a cross-section parallel to both the axial direction and the thickness direction of an electric-resistance welded steel pipe and at the center of the plate thickness. The observation surface is polished and then etched with nital to prepare the specimens. For the microstructural observation, an optical microscope (magnification: 1000 times) or a scanning electron microscope (SEM, magnification: 1000 times) is used to observe and photograph the microstructural structure at the center of the plate thickness (or wall thickness). Next, the area ratios of bainite and the remainder (ferrite, pearlite, martensite, and austenite) are determined from the obtained optical microscope images and SEM images. The area ratios of each structure are determined by observing five or more fields in the center of the plate thickness (or wall thickness) and averaging the values obtained in each field. In the present invention, the area ratio obtained by observing the structure is regarded as the volume ratio of each structure. In the present invention, the center of the plate thickness (or wall thickness) is defined as the center position in the plate thickness direction (1 / 2 position of the plate thickness) or the center position in the wall thickness direction (1 / 2 position of the wall thickness). However, as long as at least the above-mentioned steel structure exists within a range of ±0.20 mm in the plate thickness (or wall thickness) direction from the plate thickness (or wall thickness) center, the effect of the present invention can be obtained in the same manner. Therefore, in the present invention, the "steel structure in the plate thickness (or wall thickness) center" refers to a predetermined area (0.10 mm) that exists within a range of ±0.20 mm in the plate thickness (or wall thickness) direction from the plate thickness (or wall thickness) center. 2 The steel structure referred to is preferably such that the above mentioned conditions are met.
[0033] Ferrite is a product of diffusion transformation and has a low dislocation density and a nearly restored structure. This includes polygonal ferrite and pseudo-polygonal ferrite. Bainite is a complex phase structure of lath-shaped ferrite and cementite with high dislocation density. Pearlite is a eutectoid structure of iron and iron carbide (ferrite + cementite) and exhibits a lamellar structure in which linear ferrite and cementite are arranged alternately. Martensite is a lath-shaped low-temperature transformed structure with an extremely high dislocation density. In SEM images, it shows brighter contrast than ferrite and bainite.
[0034] In addition, since it is difficult to distinguish martensite from austenite in the optical microscope image and the SEM image, the total area ratio of the structure observed as martensite or austenite in the obtained SEM image is calculated, and the volume ratio of austenite measured by the following method is subtracted from the total value to obtain the volume ratio of martensite. That is, by utilizing the fact that austenite is an fcc phase, the volume fraction of austenite is determined by X-ray diffraction. The volume fraction of austenite can be calculated from the integrated intensities of the (200), (220), and (311) planes of fcc iron and the (200) and (211) planes of bcc iron obtained by such X-ray diffraction.
[0035] Furthermore, the steel structure at the center of thickness of the hot-rolled steel plate and the base material of the electric resistance welded steel pipe has an average crystal grain size of 10.0 μm or less, and the volume fraction of crystal grains with a grain size of 40.0 μm or more is 40% or less. Furthermore, the steel structure has a number density of Ti-based inclusions with a major axis of 5.0 μm or more of 20 pieces / mm 2 The following applies.
[0036] In the present invention, the term "average crystal grain size" refers to the average value of the equivalent circle diameters of crystal grains, where the crystal grains are regions surrounded by a boundary where the misorientation between adjacent crystals is 15° or more. Moreover, the "circle equivalent diameter (crystal grain size)" refers to the diameter of a circle having the same area as the target crystal grain. Moreover, "Ti-based inclusions" refer to inclusions with a Ti ratio of 50% or more by mass. However, since there is a large measurement error for elements with atomic numbers 1 to 10 (H to Ne in the periodic table) and they may be dirt attached to the surface, the Ti ratio refers to the ratio of elements with atomic numbers 11 or higher (Na and higher in the periodic table).
[0037] [Average grain size] When the average grain size of the grains at the center of thickness of the hot-rolled steel sheet and the center of thickness of the base material of the electric resistance welded steel pipe exceeds 10.0 μm, the steel structure is not fine enough, and the yield stress or tensile strength targeted in the present invention cannot be obtained. In addition, the toughness is also reduced. Therefore, the average grain size of the grains at the center of thickness of the hot-rolled steel sheet and the center of thickness of the base material of the electric resistance welded steel pipe is set to 10.0 μm or less. The average grain size of the grains is preferably 8.0 μm or less. If the average grain size is too small, the yield ratio is likely to increase, so the average grain size is preferably 3.0 μm or more.
[0038] [Grain size: Volume ratio of crystal grains 40.0 μm or larger] If the volume fraction of crystal grains with a grain size of 40.0 μm or more at the center of thickness of a hot-rolled steel sheet and at the center of thickness of a base material of an electric resistance welded steel pipe exceeds 40%, the proportion of coarse crystal grains is high, and the toughness and / or workability is reduced. Therefore, the volume fraction of crystal grains with a grain size of 40.0 μm or more at the center of thickness of a hot-rolled steel sheet and at the center of thickness of a base material of an electric resistance welded steel pipe is set to 40% or less. The volume fraction of crystal grains with a grain size of 40.0 μm or more at the center of thickness of a hot-rolled steel sheet and at the center of thickness of a base material of an electric resistance welded steel pipe is preferably 30% or less.
[0039] [Number density of Ti-based inclusions with major axis of 5.0 μm or more] The number density of Ti-based inclusions with major diameters of 5.0 μm or more at the center of thickness of hot-rolled steel sheets and the center of thickness of the base metal of electric resistance welded steel pipes is 20 pieces / mm 2 In the case of 0.15 or more, the toughness is reduced due to the large number of coarse polygonal inclusions. Therefore, the number density of Ti-based inclusions with a major axis of 5.0 μm or more at the center of thickness of the hot-rolled steel plate and the base material of the electric resistance welded steel pipe is 20 pieces / mm 2 The number density of Ti-based inclusions with a major diameter of 5.0 μm or more at the center of thickness of the hot-rolled steel plate and the base metal of the electric resistance welded steel pipe is preferably 10 pieces / mm 2 The following is the result.
[0040] Although details will be described later in the Examples, the average crystal grain size of the steel structure, the volume fraction of crystal grains having a grain size of 40.0 μm or more, and the number density of Ti-based inclusions having a major axis of 5.0 μm or more can be measured by the following methods.
[0041] The average grain size is measured by mirror-polishing cross sections parallel to both the rolling direction and the plate thickness direction of the hot-rolled steel plate, and cross sections parallel to both the pipe axis direction and the thickness direction of the base material of the electric-resistance welded steel pipe, and using the SEM / EBSD method, calculating histograms of the grain size distribution (horizontal axis: grain size, vertical axis: the proportion of each grain size) at the center of thickness of the hot-rolled steel plate and the center of thickness of the base material of the electric-resistance welded steel pipe, and determining the arithmetic mean of the grain size. The measurement conditions are accelerating voltage: 15 kV, measurement area: 300 μm × 300 μm, measurement step size (measurement resolution): 0.5 μm, and the measured values of 5 or more fields of view are averaged. In the analysis of crystal grain size, crystal grains with a grain size of less than 2.0 μm are excluded from the analysis as measurement noise.
[0042] The volume fraction of crystal grains having a grain size of 40.0 μm or more can be obtained by calculating the sum of the area fractions of crystal grains having a grain size of 40.0 μm or more from the histogram of the crystal grain size distribution and regarding the sum of these area fractions as the volume fraction.
[0043] The number density of Ti-based inclusions with a major axis of 5.0 μm or more is determined by mirror-polishing cross sections parallel to both the rolling direction and the plate thickness direction of hot-rolled steel plate, and cross sections parallel to both the axial direction and the wall thickness direction of the base material of electric resistance welded steel pipe, and combining the measurement of the major axis of the inclusions by SEM and elemental analysis by SEM / EDS method in the same field of view. The number density is measured at the centre of thickness for hot-rolled steel plate and at the centre of thickness for the base material of electric resistance welded steel pipe, in an area of 4 mm x 10 mm, and by averaging the measured values from five or more visual fields.
[0044] The steel structure at the center of the wall thickness of the electric welded part of the electric welded steel pipe in the present invention has a ferrite volume fraction of 10% or more, a total volume fraction of ferrite and bainite of 60% or more and 98% or less, and the remainder containing one or more of pearlite, martensite and austenite, and further has an average crystal grain size of 15.0 μm or less.
[0045] [Ferrite volume fraction] If the volume fraction of ferrite at the center of the wall thickness of the electric welded part of the electric welded steel pipe is less than 10%, the ductility of the electric welded part decreases, and the flattening value of the electric welded part targeted in the present invention cannot be obtained. Therefore, the volume fraction of ferrite at the center of the wall thickness of the electric welded part of the electric welded steel pipe is set to 10% or more. The volume fraction of ferrite at the center of the wall thickness of the electric welded part of the electric welded steel pipe is preferably 20% or more, and more preferably 30% or more. The upper limit of the volume fraction of ferrite is not particularly limited, but from an industrial perspective, it is preferably about 90%.
[0046] [Total volume fraction of ferrite and bainite] If the total volume fraction of ferrite and bainite at the center of the wall thickness of the electric welded part of the electric welded steel pipe is less than 60%, the ductility of the electric welded part is reduced, and the flattening value of the electric welded part targeted by the present invention cannot be obtained. Therefore, the total volume fraction of ferrite and bainite at the center of the wall thickness of the electric welded part of the electric welded steel pipe is set to be 60% or more. On the other hand, if the total volume fraction of ferrite and bainite at the center of the wall thickness of the electric welded part of the electric welded steel pipe is more than 98%, the strength of the electric welded part is reduced, and the desired Vickers hardness cannot be obtained. In addition, strain is concentrated in the electric welded part during the flattening test, and the desired flattening value of the electric welded part cannot be obtained. Therefore, the total volume fraction of ferrite and bainite at the center of the wall thickness of the electric welded part of the electric welded steel pipe is set to 60% or more and 98% or less. The total volume fraction of ferrite and bainite at the center of the wall thickness of the electric welded part of the electric welded steel pipe is preferably 70% or more, and more preferably 80% or more. On the other hand, the total volume fraction of ferrite and bainite at the center of the wall thickness of the electric welded part of the electric welded steel pipe is preferably 96% or less, and more preferably 94% or less.
[0047] [Remainder: one or more of pearlite, martensite and austenite] The remainder at the center of the wall thickness of the electric resistance welded steel pipe contains one or more of pearlite, martensite, and austenite. This is because the remainder needs to be a structure harder than ferrite and bainite to ensure the strength of the electric resistance welded part. If the total volume ratio of these structures exceeds 40%, the desired flattening value of the electric resistance welded part cannot be obtained. Therefore, the total volume ratio of these structures is set to 40% or less, preferably 30% or less, and more preferably 20% or less.
[0048] [Average grain size is 15.0 μm or less] When the average grain size of the grains at the center of the wall thickness of the electric welded part of the electric welded steel pipe exceeds 15.0 μm, the strength of the electric welded part decreases and the desired Vickers hardness cannot be obtained. In addition, since strain is concentrated in the electric welded part during the flattening test, the desired flattening value of the electric welded part cannot be obtained. Therefore, the average grain size of the grains at the center of the wall thickness of the electric welded part of the electric welded steel pipe is set to 15.0 μm or less. The average grain size of the grains is preferably 10.0 μm or less. If the average grain size is too small, the ductility is likely to decrease, and the flattening value is likely to increase. Therefore, the average grain size is preferably 3.0 μm or more.
[0049] [Component composition] Next, from the viewpoint of ensuring the above-mentioned characteristics and steel structure, the ranges of the composition of the electric resistance welded steel pipe of the present invention and the hot-rolled steel sheet that is the raw material for the electric resistance welded steel pipe and the reasons for limiting the ranges will be explained. In this specification, unless otherwise specified, "%" indicating the composition of the steel (including the steel sheet and steel pipe) is mass %.
[0050] C: 0.020% or more and 0.200% or less C is an element that increases the strength of steel by solid solution strengthening. In order to ensure the strength targeted in the present invention, 0.020% or more of C is contained. On the other hand, if the C content exceeds 0.200%, the hardenability increases and hard pearlite, martensite, and austenite are excessively generated, so the C content is set to 0.200% or less. The C content is preferably 0.030% or more and preferably 0.180% or less. Moreover, the C content is more preferably 0.040% or more and more preferably 0.170% or less.
[0051] Si: 0.02% or more and 1.00% or less Silicon is an element that increases the strength of steel by solid solution strengthening. To obtain such an effect, 0.02% or more of silicon is contained. On the other hand, if the silicon content exceeds 1.00%, the ductility and toughness decrease. In addition, the melting point of oxides containing silicon increases, and oxides tend to remain in the electric resistance welded portion, so that the ductility of the electric resistance welded portion decreases. For this reason, the silicon content is set to 1.00% or less. The silicon content is preferably 0.05% or more and preferably 0.90% or less. In addition, the silicon content is more preferably 0.10% or more and more preferably 0.80% or less.
[0052] Mn: 0.10% or more and 2.50% or less Mn is an element that increases the strength of steel by solid solution strengthening. In addition, Mn is an element that contributes to microstructural refinement by lowering the transformation start temperature. In order to secure the strength and steel structure targeted in the present invention, 0.10% or more of Mn is contained. On the other hand, if the Mn content exceeds 2.50%, the hardenability increases and hard pearlite, martensite, and austenite are excessively generated, so the Mn content is set to 2.50% or less. The Mn content is preferably 0.40% or more and preferably 2.30% or less. In addition, the Mn content is more preferably 0.50% or more and more preferably 2.00% or less.
[0053] P:0.050% or less Since P segregates at grain boundaries and causes inhomogeneity in the material, it is necessary to reduce it as much as possible, and the P content is set to be within the range of 0.050% or less. The P content is preferably 0.040% or less, and more preferably 0.030% or less. Although there is no particular lower limit for P, excessive reduction leads to high smelting costs, so P is preferably set to 0.001% or more.
[0054] S: 0.0200% or less S is usually present in steel as MnS, but MnS is thinly drawn in the hot rolling process and has a negative effect on ductility and toughness. For this reason, in the present invention, it is necessary to reduce S as much as possible, and the S content is set to 0.0200% or less. The S content is preferably 0.0100% or less, and more preferably 0.0050% or less. There is no particular lower limit for S, but since excessive reduction leads to an increase in smelting costs, it is preferable that S be 0.0001% or more.
[0055] Al: 0.005% or more and 0.100% or less Al is an element that acts as a strong deoxidizer. In order to obtain such an effect, it is necessary to contain 0.005% or more of Al. On the other hand, if the Al content exceeds 0.100%, the weldability deteriorates, and the amount of alumina-based inclusions increases, deteriorating the surface properties. Furthermore, the toughness also decreases. For this reason, the Al content is set to 0.100% or less. The Al content is preferably 0.010% or more and preferably 0.080% or less. Moreover, the Al content is more preferably 0.015% or more and more preferably 0.070% or less.
[0056] N: 0.0100% or less N is an impurity that may be unavoidably contained, and is an element that has the effect of reducing ductility and toughness by firmly fixing the movement of dislocations. In the present invention, it is desirable to reduce N as an impurity as much as possible, but the N content can be tolerated up to 0.0100%. For this reason, the N content is set to 0.0100% or less. The N content is preferably 0.0080% or less. There is no particular lower limit for the N content, but since excessive reduction leads to high refining costs, it is preferable that N be 0.0010% or more.
[0057] Ti: 0.030% or more and 0.200% or less Ti is an element that contributes to improving the strength of steel by forming fine carbides and nitrides in steel, and also contributes to reducing the amount of dissolved N in steel due to its high affinity with N. In order to obtain the above-mentioned effects, it is necessary to contain 0.030% or more of Ti. On the other hand, if the Ti content exceeds 0.200%, coarse Ti-based inclusions are formed in the casting process, making it difficult to ensure the number density of Ti-based inclusions with a major axis of 5.0 μm or more, which is the objective of the present invention, and toughness is reduced. In addition, ductility is also reduced. For this reason, the Ti content is set to 0.200% or less. The Ti content is preferably 0.040% or more and preferably 0.180% or less. The Ti content is more preferably 0.050% or more and more preferably 0.150% or less.
[0058] The above composition may further include the following elements: One or more of the following: Cu: 0.50% or less, Ni: 0.50% or less, Cr: 0.50% or less, Mo: 0.50% or less, Nb: 0.050% or less, V: 0.050% or less, Ca: 0.0050% or less, and B: 0.0050% or less
[0059] Cu: 0.50% or less, Ni: 0.50% or less, Cr: 0.50% or less, Mo: 0.50% or less Cu, Ni, Cr, and Mo are elements that improve the hardenability of steel and increase its strength, and can be contained as necessary. In order to obtain the above effects, when Cu, Ni, Cr, and Mo are contained, it is preferable that the Cu content is 0.01% or more, Ni content is 0.01% or more, Cr content is 0.01% or more, and Mo content is 0.01% or more. On the other hand, excessive content of Cu, Ni, Cr, and Mo may cause excessive generation of hard pearlite, martensite, and austenite. In addition, defects are likely to occur in electric resistance welded parts, and the flattening value increases (deteriorates). Therefore, when Cu, Ni, Cr, and Mo are contained, it is preferable that the Cu content be 0.50% or less, Ni content be 0.50% or less, Cr content be 0.50% or less, and Mo content be 0.50% or less, respectively.
[0060] That is, when Cu, Ni, Cr, and Mo are contained, it is preferable that the Cu content be 0.01% or more and 0.50% or less, Ni content be 0.01% or more and 0.50% or less, Cr content be 0.01% or more and 0.50% or less, and Mo content be 0.01% or more and 0.50% or less, respectively. More preferably, Cu: 0.05% or more and Cu: 0.40% or less, Ni: 0.05% or more and Ni: 0.40% or less, Cr: 0.05% or more and Cr: 0.40% or less, Mo: 0.05% or more and Mo: 0.40% or less, and even more preferably, Cu: 0.10% or more and Cu: 0.30% or less, Ni: 0.10% or more and Ni: 0.30% or less, Cr: 0.10% or more and Cr: 0.30% or less, and Mo: 0.10% or more and Mo: 0.30% or less.
[0061] Nb: 0.050% or less Nb is an element that contributes to improving the strength of steel by forming fine carbides and nitrides in the steel, and also contributes to refining the structure by suppressing the coarsening of austenite during hot rolling. In order to obtain the above-mentioned effects, it is desirable to contain 0.002% or more of Nb. On the other hand, if the Nb content exceeds 0.050%, the ductility and toughness decrease. For this reason, the Nb content is preferably 0.050% or less. The Nb content is more preferably 0.005% or more, and more preferably 0.040% or less. The Nb content is further preferably 0.010% or more, and further preferably 0.030% or less.
[0062] V:0.050% or less V is an element that contributes to improving the strength of steel by forming fine carbides and nitrides in the steel. In order to obtain the above-mentioned effects, it is desirable to include 0.002% or more of V. On the other hand, if the V content exceeds 0.050%, the ductility and toughness decrease. For this reason, the V content is preferably 0.050% or less. The V content is more preferably 0.005% or more, and more preferably 0.040% or less. Furthermore, the V content is further preferably 0.010% or more, and further preferably 0.030% or less.
[0063] Ca: 0.0050% or less Ca is an element that contributes to improving the toughness of steel by spheroidizing sulfides such as MnS that are thinly drawn in the hot rolling process, and can be contained as necessary. In order to obtain the above-mentioned effects, when Ca is contained, it is preferable that Ca is contained in an amount of 0.0005% or more. On the other hand, when the Ca content exceeds 0.0050%, Ca oxide clusters are formed in the steel, and the toughness deteriorates. For this reason, when Ca is contained, it is preferable that the Ca content is 0.0050% or less. The Ca content is more preferably 0.0008% or more, and more preferably 0.0045% or less. Moreover, the Ca content is further preferably 0.0010% or more, and further preferably 0.0040% or less.
[0064] B: 0.0050% or less B is an element that contributes to the refinement of the structure by lowering the transformation start temperature, and can be included as necessary. In order to obtain the above-mentioned effects, when B is included, it is preferable to include 0.0003% or more of B. On the other hand, if the B content exceeds 0.0050%, the ductility and toughness deteriorate. For this reason, when B is included, the B content is preferably 0.0050% or less. The B content is more preferably 0.0005% or more, and more preferably 0.0040% or less. Moreover, the B content is further preferably 0.0008% or more, and further preferably 0.0030% or less.
[0065] In the above composition, the balance is Fe and unavoidable impurities, however, as an unavoidable impurity, it is permissible to contain 0.0050% or less of O (oxygen) as long as the effect of the present invention is not impaired.
[0066] The above-mentioned composition is the composition of the base material of the hot-rolled steel sheet and electric resistance welded steel pipe of the present invention. By satisfying this composition, the properties targeted by the present invention can be obtained. Moreover, the composition of the hot-rolled steel sheet substantially corresponds to the composition of the steel material and molten steel used in the production thereof.
[0067] In the present invention, furthermore, in order to reduce the flattening value of the electric resistance welded steel pipe, it is preferable that the Mn / Si value is set to 2.0 or more and 100.0 or less. If the Mn / Si ratio is less than 2.0 or exceeds 100.0, the melting point of the Si-Mn oxides becomes high, and they do not melt during electric resistance welding and remain as inclusions in the electric resistance welded part. As a result, the flattening value may increase (deteriorate). The Mn / Si ratio is more preferably 2.1 or more and more preferably 90.0 or less. Furthermore, the Mn / Si ratio is further preferably 2.2 or more and more preferably 80.0 or less.
[0068] [Methods of manufacturing hot-rolled steel sheets and electric resistance welded steel pipes] Next, a method for producing a hot-rolled steel sheet and an electric resistance welded steel pipe according to an embodiment of the present invention will be described. The hot-rolled steel sheet of the present invention is produced by casting molten steel having the above-mentioned composition at an average cooling rate of 0.30 ° C. / s or more from the solidification point of the molten steel to 1200 ° C. (casting process), heating the steel material to a heating temperature of 1150 ° C. or more and 1300 ° C. or less, hot rolling the steel material at a rough rolling end temperature of 950 ° C. or more and 1180 ° C. or less, a finish rolling end temperature of 850 ° C. or more and 1000 ° C. or less, and a total reduction rate in finish rolling of 50% or more and 80% or less (hot rolling process), and then cooling at an average cooling rate of 10 ° C. / s or more and 60 ° C. / s or less at the center of the thickness and a cooling end temperature of 400 ° C. or more and 580 ° C. or less at the center of the thickness (cooling process), and then winding the steel material into a coil at 400 ° C. or more and 580 ° C. or less (winding process).
[0069] Furthermore, the electric welded steel pipe of the present invention can be produced by forming the hot-rolled steel sheet produced as described above into a cylindrical shape by cold roll forming, butting both circumferential ends of the cylindrical shape together and electric welding them to form a pipe into an electric welded steel pipe (pipe-making process), then heating the area where the electric welded steel pipe is formed (electric welded part) to 850°C or higher and 1050°C or lower, further air-cooling for 5 s or higher and 50 s or lower, and then water-cooling to 200°C or lower (welded part heat treatment process), and then adjusting the outer diameter of the pipe using a sizing roll (sizing process).
[0070] In the following description of the manufacturing method, the temperature indicated in "°C" refers to the surface temperature of the steel material or steel plate (hot-rolled plate) unless otherwise specified. These surface temperatures can be measured with a radiation thermometer or the like. The temperature at the center of the thickness of the steel plate can be obtained by calculating the temperature distribution in the cross section of the steel plate by heat transfer analysis and correcting the result by the surface temperature of the steel plate. Furthermore, "hot-rolled steel plate" includes hot-rolled plate and hot-rolled steel strip.
[0071] First, the method for producing a hot-rolled steel sheet according to the present invention will be described. In the present invention, the method of smelting the steel material (steel slab) is not particularly limited. For example, any of the known smelting methods such as converter, electric furnace, vacuum melting furnace, etc. are suitable. The casting method is also not particularly limited. For example, a steel material of the desired dimensions is produced by a known casting method such as continuous casting. However, there is no problem even if an ingot casting-blooming rolling method is applied instead of the continuous casting method. The molten steel may further be subjected to secondary refining such as ladle refining.
[0072] [Average cooling rate from solidification point to 1200℃ in the casting process: 0.30℃ / s or more] In the casting process, if the average cooling rate from the solidification point of the molten steel after melting to 1200°C is less than 0.30°C / s, the Ti-based inclusions become coarse, making it difficult to ensure the number density of Ti-based inclusions with a major axis of 5.0 μm or more, which is the objective of the present invention, and toughness decreases. For this reason, the average cooling rate from the solidification point to 1200°C is set to 0.30°C / s or more. The average cooling rate is preferably 0.35°C / s or more, more preferably 0.40°C / s or more. There is no particular upper limit to the average cooling rate. If the average cooling rate exceeds 100°C / s, the effect of improving toughness with increasing cooling rate becomes small, and the equipment load only increases. For this reason, the average cooling rate from the solidification point to 1200°C is preferably 100°C / s or less. The average cooling rate is more preferably 80°C / s or less. The above-mentioned freezing point can be calculated by the following formula (1). Freezing point (℃)=1539-(70[C]+8[Si]+5[Mn]+30[P]+25[S]+5[Cu]+4[Ni]+1.5[Cr])...(1) In formula (1), the element symbols represent the content (mass%) of each element in the steel. Elements that are not contained are regarded as 0%.
[0073] In the present invention, the steel material (steel slab) obtained through the casting is heated (reheated) to a heating temperature in the range of 1150°C to 1300°C, and then the heated steel material is hot rolled (hot rolling process) to form a hot-rolled sheet, which is then cooled (cooling process). The cooled hot-rolled sheet is then wound into a coil (winding process) to form a hot-rolled steel sheet.
[0074] [Heating temperature in hot rolling process: 1150℃ to 1300℃] In the hot rolling process, if the heating temperature (reheating temperature) is less than 1150°C, the deformation resistance of the rolled material increases, making rolling difficult. On the other hand, if the heating temperature exceeds 1300°C, the austenite grains become coarse, and fine austenite grains cannot be obtained in the subsequent rolling (rough rolling, finish rolling), making it difficult to ensure the average crystal grain size targeted in the present invention. Therefore, the heating temperature in the hot rolling process is set to 1150°C or higher and 1300°C or lower. The heating temperature is preferably 1170°C or higher and preferably 1280°C or lower.
[0075] In addition to the conventional method of producing a steel slab, cooling it to room temperature and then reheating it, the present invention can also easily apply energy-saving direct rolling processes in which the slab is not cooled to room temperature, but is instead charged into a heating furnace as a hot slab, or is immediately rolled after a short period of heat retention.
[0076] [Rough rolling end temperature: 950℃ to 1180℃] In the hot rolling process, if the rough rolling end temperature is less than 950°C, the surface temperature of the steel sheet during the subsequent finish rolling will be equal to or lower than the ferrite transformation start temperature, resulting in the formation of a large amount of ferrite, making it difficult to ensure the volume fraction of bainite targeted in the present invention, and reducing the yield stress or tensile strength. On the other hand, if the rough rolling end temperature exceeds 1180°C, the austenite grains will become coarse, making it difficult to ensure the average crystal grain size targeted in the present invention, and reducing the toughness. For this reason, the rough rolling end temperature in the hot rolling step is set to 950° C. or higher and 1180° C. or lower. The rough rolling end temperature is more preferably 970° C. or higher and more preferably 1150° C. or lower.
[0077] [Finish rolling temperature: 850℃ to 1000℃] In the hot rolling process, if the finish rolling end temperature is less than 850°C, the surface temperature of the steel sheet during the finish rolling will be equal to or lower than the ferrite transformation start temperature, resulting in the formation of a large amount of ferrite, making it difficult to secure the bainite volume fraction targeted in the present invention, and decreasing the yield stress or tensile strength. On the other hand, if the finish rolling end temperature exceeds 1000°C, the austenite grains will become coarse, making it difficult to secure the average crystal grain size targeted in the present invention, and decreasing the toughness. For this reason, the finish rolling end temperature in the hot rolling step is set to 850° C. or higher and 1000° C. or lower. The finish rolling end temperature is more preferably 870° C. or higher and more preferably 980° C. or lower.
[0078] [Total reduction in finish rolling: 50% to 80%] In the present invention, by refining the subgrains in the austenite in the hot rolling process, the structure of the bainite and the remaining parts formed in the subsequent cooling and coiling processes is refined, and a steel structure having the yield strength targeted in the present invention is obtained. Therefore, in order to refine the subgrains in the austenite in the hot rolling process, it is necessary to increase the reduction in the austenite non-recrystallization temperature range and introduce sufficient processing strain. To achieve this objective, in the present invention, the total reduction in the finish rolling is set to 50% or more. If the total reduction in the finish rolling is less than 50%, sufficient processing strain cannot be introduced in the hot rolling process. Therefore, a steel structure having a desired average crystal grain size and a volume fraction of crystal grains having a grain size of 40.0 μm or more, which are the objectives of the present invention, cannot be obtained. The total reduction in the finish rolling is preferably 55% or more. On the other hand, if the total reduction exceeds 80%, ferrite is easily generated, making it difficult to secure the bainite volume fraction, which is the objective of the present invention, and the yield stress or tensile strength decreases. Therefore, the total reduction in the finish rolling is set to 80% or less. The total reduction is preferably 75% or less. The total reduction in the above-mentioned finish rolling refers to the sum of the reductions in each rolling pass in the finish rolling. In addition, in the present invention, no upper or lower limit is particularly specified for the finished plate thickness. However, from the viewpoint of ensuring the necessary rolling reduction rate and controlling the steel plate temperature, it is preferable that the finished plate thickness (the plate thickness of the steel plate after finish rolling) be in the range of 2 mm or more and 25 mm or less.
[0079] [Average cooling rate at the center of plate thickness during cooling process: 10℃ / s to 60℃ / s] After the hot rolling step, a cooling step is carried out to cool the hot-rolled sheet. If the average cooling rate in the cooling step is less than 10°C / s, the ferrite volume fraction of the steel structure increases, and therefore a steel structure having the bainite volume fraction targeted in the present invention cannot be obtained. In addition, the frequency of bainite nucleation decreases and the nuclei become coarse, and therefore a steel structure having the average grain size targeted in the present invention cannot be obtained. On the other hand, if the average cooling rate exceeds 60°C / s, a large amount of martensite is formed, and workability and toughness decrease. Therefore, the average cooling rate at the center of the thickness of the hot-rolled sheet is set to be in the range of 10°C / s to 60°C / s. The average cooling rate is preferably 15° C. / s or more and preferably 55° C. / s or less. In the present invention, from the viewpoint of suppressing the formation of ferrite on the steel sheet surface before the cooling step, it is preferable to start the cooling step immediately after the end of finish rolling in the hot rolling step.
[0080] [Cooling stop temperature at the center of plate thickness in the cooling process: 400℃ to 580℃] If the cooling stop temperature at the center of the thickness of the hot-rolled sheet in the cooling step is less than 400°C, a large amount of martensite is generated, resulting in reduced workability and toughness. On the other hand, if the cooling stop temperature exceeds 580°C, the ferrite volume fraction increases, making it impossible to obtain a steel structure having the bainite volume fraction targeted in the present invention. In addition, the frequency of bainite nucleation decreases and these become coarse, making it impossible to obtain a structure having the average grain size targeted in the present invention. Therefore, the cooling stop temperature is set to a range of 400°C to 580°C. The cooling stop temperature is preferably 420°C or higher and preferably 550°C or lower. In the present invention, the average cooling rate is a value calculated by ((temperature at the center of thickness of the hot-rolled sheet before cooling−temperature at the center of thickness of the hot-rolled sheet after cooling) / cooling time).
[0081] The cooling method in the cooling step of the present invention may be water cooling such as spraying water from a nozzle, or cooling by spraying cooling gas, etc. In the present invention, it is preferable to perform the cooling operation (treatment) on both sides of the hot-rolled sheet so that both sides of the hot-rolled sheet are cooled under the same conditions.
[0082] [Temperature at the center of plate thickness during winding process (winding temperature): 400℃ to 580℃] After the cooling step, a coiling step is performed in which the hot-rolled sheet is coiled. After the coiling step, the sheet can be allowed to cool naturally. If the coiling temperature is less than 400°C, a large amount of martensite is generated, resulting in reduced workability and toughness. On the other hand, if the coiling temperature exceeds 580°C, the ferrite volume fraction increases, making it impossible to obtain a steel structure having the bainite volume fraction targeted in the present invention. In addition, the frequency of bainite nucleation decreases and these nuclei become coarse, making it impossible to obtain a structure having the average crystal grain size targeted in the present invention. Therefore, the coiling temperature is set to a range of 400°C to 580°C. The coiling temperature is preferably 420°C or higher and preferably 550°C or lower.
[0083] Next, a method for producing an electric resistance welded steel pipe will be described. The hot-rolled steel sheet (the hot-rolled steel sheet of the present invention) obtained by the above-mentioned coiling process is subjected to a pipe-making process. In this pipe-making process, the hot-rolled steel sheet is formed into a cylindrical open pipe (round steel pipe) by cold rolling, and both circumferential ends (butt joints) of the cylindrical open pipe are butted together and melted by high-frequency electric resistance heating, while being pressure-welded by upsetting with a squeeze roll and then electric resistance welded to produce an electric-resistance welded steel pipe.
[0084] The electric welded steel pipe manufactured in this manner has a base material portion which is the above-mentioned hot-rolled steel plate, an electric welded portion (also called a bond portion or simply a welded portion) which is the portion where electric welding has been applied, and a weld heat-affected portion which is generated in the base material by the heat during the electric welding. After the pipe-making process, the electric resistance welded steel pipe is subjected to a weld heat treatment process. The electric resistance welded part after the pipe-making process is heated and then rapidly cooled in the pipe-making process, and therefore has lower ductility than the base material part. Therefore, in the weld heat treatment process, the electric resistance welded part is heated and then appropriately cooled, thereby simultaneously satisfying the strength, workability, and toughness of the electric resistance welded part.
[0085] Here, the upset amount during electric resistance welding (electric resistance welding process) is preferably 20% or more of the thickness of the hot-rolled steel sheet so that inclusions such as oxides and nitrides that cause a decrease in toughness can be discharged together with the molten steel during welding. However, if the upset amount exceeds 100% of the thickness, the load on the squeeze roll increases. Therefore, the upset amount is preferably 20% or more and 100% or less of the thickness. The upset amount is more preferably 40% or more, and more preferably 80% or less. In the present invention, the amount of upset can be calculated by ((circumference of open pipe immediately before electric resistance welding)-(circumference of electric resistance welded steel pipe immediately after electric resistance welding)) / (plate thickness)×100(%).
[0086] [Heating temperature in the heat treatment process for welded parts: 850℃ to 1050℃] If the heating temperature in the weld heat treatment process is less than 850°C, the electric resistance weld is not completely austenitized, and the quenched structure formed in the pipe making process remains, resulting in reduced ductility. As a result, the desired flattening value of the electric resistance weld is not obtained. On the other hand, if the heating temperature exceeds 1050°C, the austenite grains become coarse, the number of nucleation sites for ferrite and bainite decreases, and the volume fraction of ferrite and the total volume fraction of ferrite and bainite targeted in the present invention cannot be obtained at the center of the thickness of the electric resistance weld, and the desired flattening value of the electric resistance weld is not obtained. Or, the average grain size targeted in the present invention is not obtained.
[0087] [Air cooling time in heat treatment process for welded parts: 5s to 50s] Ferrite and bainite are generated by air cooling after heating at the above heating temperature. If the air cooling time is less than 5 s, the desired ferrite volume fraction and the total volume fraction of ferrite and bainite are not obtained at the center of the thickness of the electric resistance weld, and the flattening value of the electric resistance weld as intended in the present invention is not obtained. On the other hand, if the air cooling time exceeds 50 s, the average grain size of the electric resistance weld as intended in the present invention is not obtained at the center of the thickness of the electric resistance weld. Or, since the temperature falls below the Ms point during air cooling, the ferrite volume fraction and the total volume fraction of ferrite and bainite are not obtained, and the flattening value of the electric resistance weld as intended in the present invention is not obtained.
[0088] [Temperature after water cooling in the heat treatment process of the welded parts: 200℃ or less] The ferrite transformation and bainite transformation are completed by water cooling after the air cooling. If the temperature after water cooling exceeds 200° C., the ferrite and bainite become coarse, and a structure having the average grain size targeted in the present invention cannot be obtained.
[0089] After the weld heat treatment process, a sizing process is carried out in which the outer diameter of the electric resistance welded steel pipe is adjusted using sizing rolls. In the sizing process, the electric resistance welded steel pipe is reduced in diameter using rolls arranged above, below, left and right of the electric resistance welded steel pipe, and the outer diameter and roundness are adjusted to desired values.
[0090] The sizing process is carried out to improve the outer diameter accuracy and roundness. In order to improve the outer diameter accuracy and roundness, it is preferable to reduce the diameter of the steel pipe so that the steel pipe circumference is reduced by a total of 0.5% or more. On the other hand, if the steel pipe circumference is reduced by a total of more than 4.0%, the amount of bending in the axial direction of the pipe when passing through the rolls increases, and the residual stress of the steel pipe, the dislocation density on the inner surface of the pipe, and the maximum low-angle grain boundary density all increase. As a result, the SSC resistance of the steel pipe decreases. For this reason, it is preferable to reduce the diameter so that the steel pipe circumference is reduced by a ratio of 0.5% to 4.0%. The reduction ratio of the steel pipe circumference is more preferably 1.0% or more, and more preferably 3.0% or less. In this sizing process, it is preferable to carry out multiple-stage diameter reduction using multiple stands in order to minimize the amount of bending in the tube axis direction when passing through the rolls and to suppress the occurrence of residual stress in the tube axis direction. It is also preferable that the diameter reduction in each stand is carried out so that the tube circumference is reduced by 1.0% or less.
[0091] Here, whether or not a steel pipe is an electric resistance welded steel pipe can be determined by cutting the electric resistance welded steel pipe perpendicular to the pipe axis direction, polishing and corroding the cut surface including the welded part (electric resistance welded part), and observing it with an optical microscope. Specifically, if the width in the pipe circumferential direction of the bond part of the welded part (electric resistance welded part) is 1.0 μm or more and 1000 μm or less over the entire pipe thickness, it is an electric resistance welded steel pipe.
[0092] The etching solution used for the post-polishing etching may be appropriately selected depending on the steel components and the type of steel pipe. FIG. 1 shows a schematic diagram of a portion of the cross section (near the welded part of the electric resistance welded steel pipe) after corrosion. As shown in FIG. 1, the bond part (welded part) can be visually recognized as a region (bond part 3) having a different structure and contrast from the base metal part 1 and the weld heat affected zone 2. For example, the bond part 3 of electric resistance welded steel pipes of carbon steel and low alloy steel can be identified as a region observed as white under an optical microscope in the cross section corroded with nital. Also, the bond part 3 of UOE steel pipes of carbon steel and low alloy steel can be identified as a region containing a cellular or dendritic solidification structure under an optical microscope in the cross section corroded with nital.
[0093] As for the manufacturing conditions for the steel plate and steel pipe not described above, they can all be made according to conventional methods. EXAMPLES
[0094] The present invention will be further described below based on examples, but the present invention is not limited to the following examples.
[0095] (Hot-rolled steel sheet manufacturing) Molten steel having the chemical composition shown in Table 1 was produced.
[0096] [Table 1]
[0097] The molten steel was subjected to a casting process under the conditions shown in Table 2 to produce a slab (steel material). The slab was then subjected to a hot rolling process, a cooling process, and a coiling process under the conditions shown in Table 2 to produce a hot-rolled steel sheet.
[0098] [Table 2]
[0099] Various test pieces were taken from the hot-rolled steel sheet, and microstructure observation, average crystal grain size measurement, volume fraction measurement of crystal grains with a grain size of 40.0 μm or more, number density measurement of Ti-based inclusions with a major axis of 5.0 μm or more, tensile tests, and Charpy impact tests were performed using the methods described below. Various test pieces were taken from the center in the width direction of the hot-rolled steel sheet. The results are shown in Table 3.
[0100] [Table 3]
[0101] (Manufacture of electric resistance welded steel pipes) The hot-rolled steel sheet thus obtained was then formed into a cylindrical open pipe (round steel pipe) by cold roll forming, and the butt joints of the open pipes were electric resistance welded to obtain steel pipe materials (pipe making process). The weld heat treatment process was then carried out under the conditions shown in Table 4. The steel pipe materials after the weld heat treatment process were reduced in diameter by rolls arranged above, below, left and right of the steel pipe materials (sizing process), and electric resistance welded steel pipes with the outer diameter D (mm) and wall thickness t (mm) shown in Table 4 were obtained.
[0102] [Table 4]
[0103] Various test pieces were taken from the electric resistance welded steel pipe, and the following methods were used to observe the structure, measure the average crystal grain size, measure the volume fraction of crystal grains with a grain size of 40.0 μm or more, measure the number density of Ti-based inclusions with a major axis of 5.0 μm or more, and perform tensile tests, Charpy impact tests, Vickers hardness tests, and flattening tests. The various test pieces were taken from the electric resistance welds of the electric resistance welded steel pipe and from the base material part 90° away from the electric resistance welds in the circumferential direction of the pipe when the electric resistance welds are set at 0°. The results are shown in Table 5.
[0104] [Table 5]
[0105] The specific methods for various observations, measurements, and tests are as follows:
[0106] [Textural Observation] Test pieces for microstructural observation were prepared by taking specimens from the hot-rolled steel plate and the electric-resistance welded steel pipe so that, for the hot-rolled steel plate, the observation surface was a cross section parallel to both the rolling direction and the plate thickness direction of the hot-rolled steel plate; for the base material of the electric-resistance welded steel pipe, the observation surface was a cross section parallel to both the pipe axis direction and the wall thickness direction of the electric-resistance welded steel pipe; and for the electric-resistance welded part of the electric-resistance welded steel pipe, the observation surface was a cross section parallel to both the pipe circumferential direction and the wall thickness direction of the electric-resistance welded steel pipe, and then mirror polishing.
[0107] The observation surface of the above test piece was etched with nital, and then the microstructure observation was performed using an optical microscope (magnification: 1000 times) or a scanning electron microscope (SEM, magnification: 1000 times) at the center of the plate thickness for the hot-rolled steel plate, and at the center of the wall thickness for the base material part of the electric resistance welded steel pipe and the electric resistance welded part of the electric resistance welded steel pipe. From the optical microscope images and SEM images obtained in this way, the area ratios of bainite, ferrite, and the remainder (pearlite, martensite, austenite) were obtained. The area ratios of each structure were observed in five fields of view, and the values obtained in each field of view were averaged to obtain the average value. In this example, the area ratios obtained by the microstructure observation were used as the volume ratios of each structure. Here, ferrite is a product of diffusion transformation, and has a low dislocation density and a nearly restored structure. This includes polygonal ferrite and pseudo-polygonal ferrite.
[0108] Bainite is a complex phase structure of lath-shaped ferrite and cementite with high dislocation density. Pearlite is a eutectoid structure of iron and iron carbide (ferrite + cementite), and exhibits a lamellar structure in which linear ferrite and cementite are arranged alternately.
[0109] Martensite is a lath-shaped low-temperature transformed structure with an extremely high dislocation density. In SEM images, it shows brighter contrast than ferrite and bainite.
[0110] Since it is difficult to distinguish between martensite and austenite in optical microscope images and SEM images, the area fraction of structures observed as martensite or austenite in the obtained SEM images was measured, and the volume fraction of martensite was determined by subtracting this value from the volume fraction of austenite measured by the following method. The austenite volume fraction was measured by X-ray diffraction. The test pieces for measuring the center of thickness of the hot-rolled steel sheet and the center of thickness of the base metal of the electric resistance welded steel pipe were prepared by grinding so that the diffraction surface was the center of thickness of the hot-rolled steel sheet and the center of thickness of the base metal of the electric resistance welded steel pipe, respectively, and then chemically polishing to remove the surface treatment layer. For the measurement, Mo Kα radiation was used to determine the integrated intensities of the (200), (220), and (311) planes of fcc iron and the (200) and (211) planes of bcc iron, respectively, and the normalized integrated intensities obtained by dividing each value by the theoretical strength value were calculated as proportional to the volume fraction of each phase, and the volume fraction of austenite was calculated by calculating the ratio of the normalized integrated intensity of austenite.
[0111] [Measurement of average crystal grain size] In measuring the average crystal grain size, first, a histogram of the grain size distribution (horizontal axis: grain size, vertical axis: proportion of each grain size) was calculated using the SEM / EBSD method, and the arithmetic mean of the grain size was calculated. Specifically, the crystal grain size was calculated by determining the orientation difference between adjacent crystal grains, and the boundary with an orientation difference of 15° or more was regarded as a crystal grain (grain boundary), measuring the circle-equivalent diameter of the crystal grains, and the average circle-equivalent diameter was taken as the average crystal grain size. In this case, the circle-equivalent diameter was the diameter of a circle with the same area as the target crystal grain.
[0112] [Grain size: Measurement of volume ratio of crystal grains of 40.0 μm or more] The volume ratio of crystal grains having a grain size of 40.0 μm or more was measured by calculating the total area ratio of crystal grains having a grain size of 40.0 μm or more from the above-mentioned histogram of crystal grain size distribution. The measurement conditions were as follows: acceleration voltage 15 kV, measurement area 500 μm × 500 μm, measurement step size 0.5 μm. In the crystal grain size analysis, crystal grains with grain sizes of 2.0 μm or less were excluded from the analysis as measurement noise, and the obtained area ratio was considered to be equal to the volume ratio.
[0113] [Measurement of the number density of Ti-based inclusions with major axis of 5.0 μm or more] The number density of Ti-based inclusions with major axis of 5.0μm or more was measured by combining SEM major axis measurement of the inclusions and elemental analysis by SEM / EDS method in the same field of view in cross sections parallel to both the rolling direction and the plate thickness direction of the hot-rolled steel sheet, and in cross sections parallel to both the tube axis direction and the wall thickness direction of the base material of the electric resistance welded steel pipe. The measurement positions were the center of the plate thickness of the hot-rolled steel sheet and the center of the wall thickness of the base material of the electric resistance welded steel pipe, the measurement area was 4mm x 10mm, and the measured values of five fields of view were averaged.
[0114] [Tensile test] For the hot-rolled steel sheets, JIS No. 5 tensile test specimens were taken so that the tensile direction was parallel to the rolling direction. On the other hand, for the electric resistance welded steel pipes, JIS No. 11 tensile test specimens were taken so that the tensile direction was parallel to the pipe axis direction. The tensile tests were carried out in accordance with the provisions of JIS Z 2241. The yield stress YS (MPa), tensile strength TS (MPa), and total elongation EL (%) were measured, and the yield ratio YR (%), defined as (YS / TS) x 100, was calculated.
[0115] [Charpy impact test] For the hot-rolled steel plate, a V-notch test specimen was taken from the center of the plate thickness so that the longitudinal direction of the test specimen was parallel to the rolling direction, and the Charpy impact test was performed at -60°C in accordance with the provisions of JIS Z 2242 to determine the absorbed energy. On the other hand, for the electric resistance welded steel pipe, a V-notch test specimen was taken from the center of the wall thickness of the base material so that the longitudinal direction of the test specimen was parallel to the pipe axis direction, and the test was performed at -20°C in accordance with the provisions of JIS Z 2242 to determine the absorbed energy. The impact value was determined by dividing the absorbed energy by the cross-sectional area of the fracture surface before the test. The number of test pieces for each of the above Charpy impact tests was three, and the average of the obtained impact values was calculated as the Charpy impact value (vE -60 ) and the Charpy impact value of the base metal of the electric resistance welded steel pipe (vE -20 ) was decided.
[0116] [Vickers hardness test] The Vickers hardness test was carried out by taking a test piece from the electric resistance weld of the electric resistance welded steel pipe so that the measurement surface was a cross section parallel to both the pipe circumferential direction and the wall thickness direction, in accordance with the provisions of JIS Z 2244. The load was 0.1 kgf, and the measurement position was the center of the wall thickness of the weld.
[0117] [Flattening test] The flattening test was carried out in accordance with the method described in JIS G 3441 by taking an annular test piece 100 mm long in the axial direction from the obtained electric resistance welded steel pipe, polishing the outer surface of the pipe at the welded part to a metallic luster, and carrying out the test in accordance with the method described in JIS G 3441. The compression speed was 10 mm / min, and compression was stopped when cracks occurred and the height H of the test piece at that point was measured. The flattening value was calculated by the formula H / D, where D is the outer diameter of the steel pipe.
[0118] In Table 3, hot-rolled steel sheets Nos. 1 to 5 and Nos. 14 and 15 are examples of the present invention, and hot-rolled steel sheets Nos. 6 to 13 are comparative examples. In Table 5, electric resistance welded steel pipes Nos. 1 to 5 are examples of the present invention, and electric resistance welded steel pipes Nos. 6 to 15 are comparative examples.
[0119] In the hot-rolled steel sheets of the present invention shown in Table 3, the steel structure at the center of the sheet thickness has a volume fraction of bainite of 90% or more, and the remainder contains one or more of ferrite, pearlite, martensite, and austenite. The average crystal grain size is 10.0 μm or less, the volume fraction of crystal grains with a grain size of 40.0 μm or more is 40% or less, and the number density of Ti-based inclusions with a major axis of 5.0 μm or more is 20 pieces / mm 2 The results were as follows.
[0120] On the other hand, for the electric resistance welded steel pipes of the present invention shown in Table 5, the steel structure at the center of the wall thickness of the base material portion has a volume fraction of bainite of 90% or more, with the remainder containing one or more of ferrite, pearlite, martensite and austenite, an average crystal grain size of 10.0 μm or less, a volume fraction of crystal grains with a grain size of 40.0 μm or more of 40% or less, and a number density of Ti-based inclusions with a major axis of 5.0 μm or more of 20 pieces / mm 2The steel structure at the center of the thickness of the electric resistance weld had a ferrite volume fraction of 10% or more, a total volume fraction of ferrite and bainite of 60% or more and 98% or less, with the remainder including one or more of pearlite, martensite and austenite, and an average crystal grain size of 15.0 μm or less.
[0121] The hot-rolled steel sheets of the examples of the present invention shown in Table 3 all have a yield stress YS of 650 MPa or more, a tensile strength TS of 750 MPa or more, a yield ratio YR of 90.0% or less, a total elongation EL of 15% or more, and a Charpy impact value at -60°C of 100 J / cm 2 That was all.
[0122] On the other hand, the electric resistance welded steel pipe of the present invention shown in Table 5 has a base metal portion with a yield stress YS of 650 MPa or more, a tensile strength TS of 750 MPa or more, a yield ratio YR of 96.0% or less, a total elongation EL of 15% or more, and a Charpy impact value of 50 J / cm at -20°C. 2 In the electric resistance welded portion, the Vickers hardness at the center of the wall thickness was 200 HV or more, and the flattening value was 0.80 or less.
[0123] In contrast, the comparative hot-rolled steel plate and electric resistance welded steel pipe of No. 6 had a high C content, and therefore the volume fraction of bainite was below the range of the present invention, and the Charpy impact value did not reach the desired value.
[0124] The hot-rolled steel plate and electric resistance welded steel pipe of Comparative Example No. 7 had a high Si content, and therefore the total elongation, Charpy impact value and flattening value of the electric resistance welded steel pipe did not reach the desired values.
[0125] The comparative hot-rolled steel plate and electric resistance welded steel pipe of No. 8 had a high Mn content, and therefore the volume fraction of bainite was below the range of the present invention, and the Charpy impact value did not reach the desired value.
[0126] The comparative example, the hot-rolled steel plate and electric resistance welded steel pipe of No. 9, had a low Ti content, and therefore the yield stress or tensile strength did not reach the desired value.
[0127] The comparative example No. 10 hot-rolled steel plate and electric-resistance welded steel pipe had a high Ti content, so the number density of Ti-based inclusions with a major axis of 5.0 μm or more exceeded the range of the present invention, and the Charpy impact value did not reach the desired value.
[0128] In the comparative example, the hot-rolled steel plate and electric-resistance welded steel pipe of No. 11 had a low average cooling rate in the casting process, so the number density of Ti-based inclusions with a major axis of 5.0 μm or more exceeded the range of the present invention, and the Charpy impact value did not reach the desired value.
[0129] In the comparative example No. 12 hot-rolled steel plate and electric-resistance welded steel pipe, the reheating temperature, the rough rolling end temperature and the finish rolling end temperature in the hot rolling process were high, so that the average crystal grain size exceeded the range of the present invention, and the yield stress and / or tensile strength, and the Charpy impact value did not reach the desired values.
[0130] In the comparative example, the hot-rolled steel plate and electric-resistance welded steel pipe of No. 13 had a low total reduction in finish rolling, so the volume fraction of crystal grains with a grain size of 40.0 μm or more exceeded the range of the present invention, and the Charpy impact value did not reach the desired value.
[0131] In the comparative example, electric welded steel pipe No. 14, the air cooling time in the weld heat treatment process was long, so the average crystal grain size of the electric weld exceeded the range of the present invention, and the Vickers hardness and flattening value did not reach the desired values.
[0132] In the comparative example, electric welded steel pipe No. 15, the heating temperature in the weld heat treatment process was high, so the volume fraction of ferrite and the combined volume fraction of ferrite and bainite were below the range of the present invention, and the flattening value did not reach the desired value. [Explanation of symbols]
[0133] 1 Base metal part 2. Welding heat affected zone 3 Bonding section
Claims
1. An electric resistance welded steel pipe having a base metal portion, a welded portion, and a welded heat affected zone, The base material portion comprises, in mass%, C: 0.020% or more and 0.200% or less, Si: 0.02% or more and 1.00% or less, Mn: 0.10% or more and 2.50% or less, P: 0.050% or less, S: 0.0200% or less, Al: 0.005% or more and 0.100% or less, N: 0.0100% or less; Ti: 0.030% or more and 0.200% or less The balance is Fe and unavoidable impurities, the base material portion has a steel structure in a center of a wall thickness, the volume fraction of which is 90% or more of bainite, and the remainder of which contains one or more of ferrite, pearlite, martensite, and austenite; Furthermore, the steel structure at the center of the thickness of the base material portion has an average crystal grain size of 10.0 μm or less, a volume ratio of crystal grains having a grain size of 40.0 μm or more is 40% or less, and a number density of Ti-based inclusions having a major axis of 5.0 μm or more is 20 pieces / mm 2 is as follows: the weld has a steel structure in a center of a wall thickness, the volume fraction of ferrite being 10% or more, the total volume fraction of ferrite and bainite being 60% or more and 98% or less, and the remainder including one or more of pearlite, martensite, and austenite; Furthermore, in the electric resistance welded steel pipe, the steel structure at the center of the wall thickness of the weld has an average crystal grain size of 15.0 μm or less.
2. The composition of the base material portion is further, in mass%, Cu: 0.50% or less, Ni: 0.50% or less, Cr: 0.50% or less, Mo: 0.50% or less, Nb: 0.050% or less, V: 0.050% or less, Ca: 0.0050% or less; B: 0.0050% or less The electric resistance welded steel pipe according to claim 1, comprising one or more of the following:
3. A method for producing an electric resistance welded steel pipe according to claim 1 or 2, a pipe-making process in which the hot-rolled steel sheet is formed into a cylindrical shape by cold rolling, and both circumferential ends of the cylindrical shape are butted together and electric resistance welded; After the pipe making process, a heat treatment process is performed in which the electric resistance welded portion is heated to 850°C or more and 1050°C or less, and then air-cooled for 5 seconds or more and 50 seconds or less, and then water-cooled to 200°C or less. a sizing step of adjusting the outer diameter of the pipe by a sizing roll after the weld heat treatment step; A method for producing an electric resistance welded steel pipe, comprising:
Citation Information
Patent Citations
High strength steel member, and production method therefor
JP2004131802A
Steel plate for low yield ratio thick-walled circular steel pipe having tensile strength of 780 mpa or more, method for manufacturing the same, and low yield ratio thick-walled circular steel pipe having tensile strength of 780 mpa or more
JP2013057105A
Hot rolled steel sheet and production method of the same
JP2015101781A
Hot rolled steel sheet and production method therefor
JP2017057472A
HIGH-STRENGTH HOT ROLLED STEEL SHEET HAVING TENSILE STRENGTH OF 780 MPa OR MORE
WO2014148001A1