Steel slab, continuous casting method, and method for manufacturing steel slab
The continuous casting method for Ni-containing steel slabs addresses surface cracking issues by optimizing alloy composition and process conditions, improving productivity and cost-effectiveness through reduced surface defects and lower nickel usage.
Patent Information
- Application Number
- JP2023556717
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2022-09-09
- Filing Date
- 2023-07-28
- Publication Date
- 2024-10-08
- Estimated Expiration
- 2043-07-28
AI Technical Summary
Existing continuous casting methods for Ni-containing steel slabs struggle to completely suppress surface cracks, leading to increased maintenance time and costs due to the need for surface grinding, which is exacerbated by the rising cost of nickel alloys and the demand for lower Ni content steels.
A continuous casting method involving specific alloy compositions and process conditions, including controlled mold powder viscosity and mold vibration frequency, to enhance the density of solidification nuclei on the steel slab surface, reducing the size of solidification cells and dispersing stress, thereby minimizing surface cracking.
The method effectively reduces surface cracking in Ni-containing steel slabs, enhancing productivity and reducing manufacturing costs by minimizing the need for surface treatment, while maintaining equivalent low-temperature toughness with lower Ni content.
Smart Images

Figure 0007563626000001 
Figure 0007563626000002 
Figure 0007563626000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a steel slab containing Ni (nickel), a continuous casting method, and a method for producing the steel slab. [Background technology]
[0002] It is known that adding Ni to steel improves its low-temperature toughness. Steel containing about 9 mass% Ni (hereinafter also referred to as Ni-containing steel) is also called 9% Ni steel. 9% Ni steel can withstand use at temperatures below -160°C, so it is widely used as a welded structural steel for low-temperature applications such as LNG tanks.
[0003] It is known that Ni-containing steel is prone to surface defects. For example, after casting, a slab has many cracks on the surface or in the vicinity of the surface (hereinafter also referred to as surface cracks).
[0004] It has been known that surface cracks in Ni-containing steel slabs occur along grain boundaries of coarse solidification structures. Specifically, it is believed that surface cracks occur when tensile stresses such as straightening stress, bulging stress, and thermal stress are applied to the steel slabs in the temperature range of 600 to 900°C where the ductility of Ni-containing steel decreases, i.e., in the secondary cooling zone of continuous casting.
[0005] More specifically, when tensile stress is applied to a steel slab, S (sulfur), P (phosphorus), and other elements contained in the steel slab become concentrated in a specific region. The increase in the concentration of S (sulfur) and P (phosphorus) leads to grain boundary embrittlement of the steel slab. Therefore, in the region, the embrittled grain boundaries are destroyed by the tensile stress, causing surface cracks.
[0006] In order to prevent such surface cracks, the temperature of the steel slab is controlled in the secondary cooling when the steel slab is cast. For example, Patent Document 1 discloses that the cooling rate and the surface temperature of the slab are controlled in the secondary cooling zone when molten steel containing 5 to 10 mass % of Ni is continuously cast.
[0007] Furthermore, Patent Document 2 discloses that when continuously casting Ni-containing steel containing 8 to 10 mass % Ni, the reduction in area during casting is estimated and the secondary cooling intensity is controlled so that the reduction in area becomes 50% or more. [Prior art documents] [Patent documents]
[0008] [Patent Document 1] Japanese Patent Application Publication No. 8-10919 [Patent Document 2] Japanese Patent Application Publication No. 8-33964 Summary of the Invention [Problem to be solved by the invention]
[0009] Thus, although continuous casting methods that suppress many surface cracks have been proposed, it is difficult to completely suppress the occurrence of surface cracks. When surface cracks occur in a steel slab, the surface cracks are removed by a so-called finishing process, such as grinding the surface with a grinder. Therefore, when the surface cracks increase, the area and time of the finishing process become longer, resulting in a problem of reduced productivity and increased manufacturing costs.
[0010] However, in recent years, the price of Ni alloys has been rising sharply, and efforts are being made to reduce the Ni content in steel. For example, efforts are being made to expand the range of alternative steel types to 7% Ni steel as an alternative to 9% Ni steel. In addition, 5% Ni steel is used for ethylene liquefied fuel containers. Thus, the demand for Ni-containing steels with a Ni content of less than 7.5 mass% is also increasing significantly.
[0011] Even for steel types with a relatively low Ni content, that is, less than 7.5 mass%, the occurrence of surface cracks along the grain boundaries of the coarse solidification structure described above poses a manufacturing issue.
[0012] The present invention has been made in consideration of the above problems, and has an object to provide a steel slab that contains 2.0 mass% or more and less than 7.5 mass% Ni and has few surface cracks, a continuous casting method, and a method for manufacturing a steel slab. [Means for solving the problem]
[0013] In order to solve the above problems, the present invention has the following features.
[0014] [1] A steel slab containing Ni, the steel slab containing, by mass%, C: 0.03% or more and 0.10% or less, Si: 0.01% or more and 0.50% or less, Mn: 0.1% or more and 1.0% or less, P: 0.001% or more and 0.010% or less, S: 0.0001% or more and 0.0050% or less, Ni: 2.0% or more and less than 7.5%, Al: 0.010% or more and 0.080% or less, N: 0.0010% or more and 0.0050% or less, O: 0.0005% or more and 0.0040% or less, with the balance being Fe and unavoidable impurities, wherein the density of solidification nuclei on a surface of the steel slab is 0.35 nuclei / mm 2 This is the above steel casting. [2] The steel cast slab according to [1] further contains, by mass%, one or more selected from Cu: 0.03% or more and 1.50% or less, Cr: 0.03% or more and 1.00% or less, Mo: 0.02% or more and 1.00% or less, Nb: 0.003% or more and 0.100% or less, V: 0.003% or more and 0.100% or less, Ti: 0.005% or more and 0.020% or less, B: 0.0002% or more and 0.0025% or less, Ca: 0.0005% or more and 0.0050% or less, and Mg: 0.0005% or more and 0.0030% or less. [3] A continuous casting method for casting a steel slab according to [1] or [2], A continuous casting method including the step of adding mold powder having a viscosity of 0.5 Pa·s (5 poise) or more at 1300°C to a mold. [4] A continuous casting method for casting a steel slab according to [1] or [2], A method of continuous casting comprising the step of vibrating the mold at a frequency of at least 80 cycles per minute. [5] A continuous casting method for casting a steel slab according to [1] or [2], adding a mold powder having a viscosity of 0.5 Pa·s (5 poise) or more at 1300°C to the mold; vibrating the mold at a frequency of at least 50 cycles per minute. [6] A continuous casting method for casting a steel slab according to [1] or [2], adding a mold powder having a viscosity of 0.15 Pa·s (1.5 poise) or more at 1300°C to the mold; vibrating the mold at a frequency of at least 80 cycles per minute. [7] A conditioning process for performing conditioning treatment on a slab produced by the continuous casting method according to any one of [3] to [6]; a heating step of heating the slab in a heating furnace at a heating temperature of 1100°C or less after the conditioning step. Effect of the Invention
[0015] According to the present invention, the density of solidification nuclei on the surface of the steel slab is 0.35 nuclei / mm 2For the above reasons, the size of the solidification cells can be made smaller than the conventional size. This makes it possible to reduce the segregation of S (sulfur) and P (phosphorus) at the interfaces of the solidification cells compared to the conventional method. As a result, embrittlement at the interfaces of the solidification cells can be suppressed. In addition, the stress acting on the interfaces of the solidification cells can be dispersed. This makes it possible to suppress the occurrence of cracks at the interfaces of the solidification cells, and to reduce the occurrence of cracks on the surfaces of the steel slabs. As a result, the processing time for the maintenance process for removing cracks on the surfaces of the steel slabs can be reduced, and productivity can be improved and manufacturing costs can be reduced. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0016] The Ni-containing steel slab of the present invention (hereinafter also simply referred to as steel slab) contains Ni in an amount of 2.0 mass% or more and less than 7.5 mass%. The steel slab can be used, for example, as low-temperature steel used in a temperature range lower than room temperature.
[0017] The Ni-containing steel cast slab of the present invention contains, by mass%, C: 0.03% or more and 0.10% or less, Si: 0.01% or more and 0.50% or less, Mn: 0.10% or more and 1.00% or less, P: 0.001% or more and 0.010% or less, S: 0.0001% or more and 0.0050% or less, Ni: 2.0% or more and less than 7.5%, Al: 0.010% or more and 0.080% or less, N: 0.0010% or more and 0.0050% or less, O: 0.0005% or more and 0.0040% or less, with the balance being Fe and unavoidable impurities.
[0018] The strength of the base material can be ensured by including C (carbon) in the composition of the steel slab. In particular, the strength of the base material can be improved by making the C content of the steel slab 0.03 mass% (hereinafter simply referred to as "%)" or more. If the C content of the steel slab is excessive, the amount of cementite and island martensite, which are the starting points of brittle fracture, increases, and suitable toughness may not be obtained. By making the C content of the steel slab 0.10% or less, suitable toughness of the steel slab can be obtained.
[0019] By including silicon (Si) in the composition of steel slabs, the effect of deoxidization, which removes oxygen from the slabs, can be improved. Also, by including silicon in the composition of steel slabs, the strength of the base material can be ensured. If the amount of silicon added is high, island martensite is formed in the structure of the heat-affected zone (HAZ), and good HAZ toughness tends to be difficult to obtain.
[0020] That is, by making the Si content of the steel slab 0.50% or less, it is possible to ensure suitable toughness of the HAZ, and by making the Si content of the steel slab 0.01% or more, it is possible to obtain an excellent deoxidizing effect and to improve the strength of the base metal.
[0021] The steel slab can ensure the strength of the base metal by including Mn as a component. If the amount of Mn added is too high, good toughness of the HAZ tends not to be obtained.
[0022] In particular, by making the Mn content of the steel slab 0.10% or more, the strength of the base metal can be improved, and by making the Mn content of the steel slab 1.00% or less, suitable toughness of the HAZ can be ensured.
[0023] Steel slabs containing P (phosphorus) as a component tend to cause grain boundary embrittlement. For this reason, it is preferable that steel slabs contain as little P (phosphorus) as possible as a component. By making the P (phosphorus) content of the steel slab 0.010% or less, it is possible to suppress the promotion of surface cracking due to grain boundary embrittlement. This makes it possible to improve the toughness of the base material and HAZ.
[0024] Furthermore, by setting the P (phosphorus) content of the steel slab to 0.001% or more, an increase in the load of dephosphorization refining in the steelmaking process can be suppressed, and an increase in production costs can be suppressed.
[0025] Steel slabs containing S (sulfur) as a component tend to cause grain boundary embrittlement. For this reason, it is preferable that the steel slab contains as little S (sulfur) as possible as a component. By making the S (sulfur) content of the steel slab 0.0050% or less, grain boundary embrittlement and promotion of surface cracking can be suppressed. This makes it possible to improve the toughness of the base material and HAZ. In particular, S (sulfur) reduces the toughness of the steel slab as an inclusion such as MnS. For this reason, it is preferable that the S (sulfur) content of the steel slab is low.
[0026] Furthermore, by setting the S (sulfur) content of the steel slab to 0.0001% or more, an increase in the load of dephosphorization refining in the steelmaking process can be suppressed, and an increase in production costs can be suppressed.
[0027] As described above, the steel slab contains 2.0% or more and less than 7.5% Ni (nickel) as a composition. By containing the above-mentioned components, the steel slab can achieve physical properties equivalent to those of 9% Ni steel with a lower Ni content than 9% Ni steel. For this purpose, the Ni content of the steel slab is preferably 2.0% or more and less than 7.5%, and preferably 6.5% or more and less than 7.5%. If the Ni content is less than 2.0%, the toughness at low temperatures due to Ni tends not to be obtained.
[0028] By including aluminum (Al) in the composition of the steel slab, the effect of deoxidization, which removes oxygen from the steel slab, can be enhanced. Also, by including aluminum (Al) in the composition of the steel slab, the strength of the base material can be ensured. When the amount of aluminum (Al) added increases, the toughness of the base material and HAZ tends to decrease due to coarse AlN.
[0029] That is, by setting the Al (aluminum) content of the steel slab to 0.080% or less, it is possible to ensure suitable toughness of the HAZ. In particular, by setting the Si content of the steel slab to 0.010% or more, it is possible to obtain an excellent deoxidation effect.
[0030] When steel slabs contain nitrogen (N) as a component, coarse metal nitrides such as AlN are generated, which tends to reduce the toughness of the base material and HAZ. For this reason, it is preferable for steel slabs to contain as little nitrogen (N) as possible as a component.
[0031] By making the N (nitrogen) content of the steel slab 0.0050% or less, it is possible to ensure suitable toughness of the base material and HAZ, and by making the N (nitrogen) content of the steel slab 0.0010% or more, it is possible to suppress an increase in the load of denitrification treatment and nitrogen absorption prevention treatment in the steelmaking process, and thus to suppress an increase in production costs.
[0032] When a steel slab contains O (oxygen) as a component, it tends to form inclusions, which reduces the toughness of the base material and HAZ. For this reason, it is preferable that the steel slab contains as little O (oxygen) as possible as a component. By keeping the O (oxygen) content of the steel slab to 0.0040% or less, it is possible to ensure suitable toughness of the base material and HAZ.
[0033] Furthermore, by setting the O (oxygen) content of the steel slab to 0.0005% or more, an increase in the load of inclusion removal processing in the steelmaking process can be suppressed, and an increase in production costs can be suppressed.
[0034] Furthermore, in addition to the above alloying elements, the steel cast slab preferably contains one or more elements selected from Cu, Cr, Mo, Nb, V, Ti, B, Ca, and Mg in order to improve the strength and toughness of the base material and the joint.
[0035] The steel slab may contain copper (Cu) as a component. By containing copper (Cu) as a component, the steel slab can ensure the strength of the base material. If the amount of copper (Cu) added is high, good HAZ toughness tends not to be obtained.
[0036] That is, by making the Cu (copper) content of the steel slab 0.03% or more, good strength of the base material can be obtained, and by making the Cu (copper) content of the steel slab 1.50% or less, suitable toughness of the HAZ can be ensured.
[0037] The steel slab may contain Cr (chromium) as a component. By containing Cr (chromium) as a component, the steel slab can ensure the strength of the base material. If the amount of Cr (chromium) added is high, good HAZ toughness tends not to be obtained.
[0038] That is, by making the Cr (chromium) content of the steel slab 0.03% or more, good strength of the base metal can be obtained, and by making the Cr (chromium) content of the steel slab 1.00% or less, suitable toughness of the HAZ can be ensured.
[0039] The steel slab may contain Mo (molybdenum) as a component. By containing Mo (molybdenum) as a component, the steel slab can ensure the strength of the base material. If the amount of Mo (molybdenum) added is high, good HAZ toughness tends not to be obtained.
[0040] That is, by making the Mo (molybdenum) content of the steel slab 0.02% or more, good strength of the base metal can be obtained, and by making the Mo (molybdenum) content of the steel slab 1.00% or less, suitable toughness of the HAZ can be ensured.
[0041] The steel slab may contain Nb (niobium) as a component. By containing Nb (niobium) as a component, the strength of the base material can be ensured and the grain size can be made fine. If the amount of Nb (niobium) added is high, good HAZ toughness tends not to be obtained.
[0042] That is, by making the Nb (niobium) content of the steel slab 0.003% or more, it is possible to obtain good strength of the base material and to refine the crystal grains in the slab, and by making the Nb (niobium) content of the steel slab 0.100% or less, it is possible to ensure suitable toughness of the HAZ.
[0043] The steel slab may contain V (vanadium) as a component. By containing V (vanadium) as a component of the steel slab, the strength of the base material can be ensured and the crystal grains can be refined. If the amount of V (vanadium) added is high, good HAZ toughness tends not to be obtained.
[0044] That is, by making the V (vanadium) content of the steel slab 0.003% or more, it is possible to obtain good strength of the base metal and to refine the crystal grains in the slab, and by making the V (vanadium) content of the steel slab 0.100% or less, it is possible to ensure suitable toughness of the HAZ.
[0045] The steel slab may contain Ti (titanium) as a component. By containing Ti (titanium) as a component, the strength of the base material can be ensured and the grain size of the crystals in the slab can be made fine. If the amount of Ti (titanium) added is large, the HAZ toughness tends to decrease due to coarse TiN.
[0046] That is, by making the Ti (titanium) content of the steel slab 0.005% or more, it is possible to obtain good strength of the base material and to achieve fine grains, and by making the Ti (titanium) content of the steel slab 0.020% or less, it is possible to ensure suitable toughness of the HAZ.
[0047] The steel slab may contain boron (B) as a component. By containing a trace amount of boron (B) as a component, the steel slab can improve hardenability. As a result, when controlled cooling and quenching heat treatment are performed, a significant increase in strength can be achieved. When the amount of boron (B) added is high, coarse boron nitrides and boron carbohydrates are precipitated, which tends to reduce HAZ toughness.
[0048] That is, by making the B (boron) content of the steel slab 0.0002% or more, good strength can be obtained, and by making the B (boron) content of the steel slab 0.0025% or less, suitable toughness of the HAZ can be ensured.
[0049] The steel slab may contain Ca (calcium) as a component. By containing Ca (calcium), the steel slab can control the shape of inclusions and improve toughness. Ca (calcium) combines with S to become CaS. CaS can suppress ductility-dip cracking at grain boundaries and reduce surface cracking. When the amount of Ca (calcium) added is high, coarse Ca-containing inclusions are generated, which tends to reduce HAZ toughness.
[0050] That is, by making the Ca (calcium) content of the steel slab 0.0005% or more, good strength can be obtained, and by making the Ca (calcium) content of the steel slab 0.0050% or less, suitable toughness of the HAZ can be ensured.
[0051] The steel slab may contain magnesium (Mg) as a component. By containing magnesium (Mg), the steel slab can control the shape of inclusions and improve toughness. Mg combines with S to form MgS. MgS can suppress ductility-dip cracking at grain boundaries.
[0052] In addition, MgS has a great effect of refining the austenite grain size, and can reduce surface cracks during continuous casting and rolling. When the amount of Mg (magnesium) added is high, coarse Mg-containing inclusions are generated, which tends to reduce the HAZ toughness.
[0053] That is, by making the Mg (magnesium) content of the steel slab 0.0005% or more, good strength can be obtained, and by making the Mg (magnesium) content of the steel slab 0.0030% or less, suitable toughness of the HAZ can be ensured.
[0054] The density of solidification nuclei on the surface of the steel slab is 0.35 / mm 2 The density of solidification nuclei on the surface is 0.35 / mm 2 More than 5.00 pieces / mm 2Preferably, it is less than 0.50 pieces / mm 2 More than 5.00 pieces / mm 2 It is even more preferable that it is less than 1000 .mu.m.
[0055] The density of solidification nuclei is 5.00 pieces / mm 2 Above this level, it is undesirable because it is necessary to use a mold powder with stronger cooling and to set the mold vibration frequency to a very high value. In other words, if the mold cooling is too strong, the occurrence of vertical cracks due to uneven cooling of the steel slab in the mold tends to become more pronounced. In addition, operational problems such as breakouts due to insufficient mold powder inflow are likely to occur. As a result, the density of solidification nuclei is extremely high (5.00 nuclei / mm 2 The above cannot be considered valid.
[0056] The density of solidification nuclei on the surface of a steel slab can be measured by the following method. For example, on the surface of a steel slab, agglomerates (solidification cells, or dendritic cells) whose dendrite branches face in almost the same direction can be considered to have grown from one solidification nucleus. In other words, the density of solidification nuclei can be calculated by calculating the number of such agglomerates per given area.
[0057] A detailed investigation of actual Ni-containing steel slabs revealed that the more solidification nuclei there are, the more desirable it is for surface cracks to be suppressed. Specifically, when the density of solidification nuclei on the surface of the steel slab is 0.35 nuclei / mm 2 If it is equal to or greater than this, surface cracks can be effectively suppressed.
[0058] The above-described continuous casting method for casting a steel slab will now be described. One method for increasing the density of solidification nuclei on the surface of a steel slab during continuous casting is to strengthen the cooling during the initial solidification stage of continuous casting, that is, to strengthen the cooling within the mold.
[0059] In general, continuous casting of Ni-containing steel slabs involves the step of adding mold powder from above the surface of the molten steel in the mold. The mold powder functions as an antioxidant, a heat retainer, a lubricant between the mold and the solidified shell, etc.
[0060] Since this mold powder flows into the gap between the solidified shell and the mold, the molten steel does not come into direct contact with the mold, and the molten steel is indirectly cooled by the mold through the mold powder flow layer.
[0061] Therefore, by adjusting the viscosity of the molding powder, the thickness of the inflow layer can be made thin, and the heat removal capacity of the mold can be increased, thereby increasing the density of the solidification nuclei.
[0062] For example, mold powder is made of CaO, SiO 2、 Na 2 O, CaF 2、 Al 2 O 3 The thermal conductivity of mold powder is significantly lower than that of molten steel, which is a metal, and copper, which constitutes the continuous casting mold.
[0063] The heat transfer from the molten steel to the mold depends on the thickness of the mold powder layer. If the thickness of the mold powder layer is thin, the cooling efficiency by the mold increases. If the thickness is thick, the cooling efficiency decreases.
[0064] The thickness of the mold powder inflow layer can be estimated from the consumption amount of mold powder. The thickness of the mold powder inflow layer is usually about 0.1 to 0.3 mm.
[0065] To form a thin layer of mold powder, it is advisable to use mold powder with a high viscosity. Therefore, it is preferable to continuously cast steel slabs by adding mold powder with a viscosity of 0.5 Pa·s (5 poise) or more at 1300°C to the mold.
[0066] The viscosity of the molding powder at 1300°C is preferably 0.5 Pa·s (5 poise) or more and 5.0 Pa·s (50 poise) or less, and more preferably 1.0 Pa·s (10 poise) or more and 5.0 Pa·s (50 poise) or less.
[0067] By setting the viscosity of the mold powder at 1300°C to 0.5 Pa·s (5 poise) or more, it is possible to make it difficult for the mold powder to flow into the gap between the solidified shell and the mold. This makes it possible to reduce the thickness of the mold powder inflow layer, and to increase the amount of heat removed from the molten steel to the mold. This increases the density of solidification nuclei, i.e., 0.35 nuclei / mm 2 or more, and the occurrence of surface cracks can be suppressed.
[0068] The density of solidification nuclei can also be controlled by vibrating the mold at a certain frequency (oscillation cycle). For example, when the mold is vibrated, some of the dendrites in the process of solidification dissociate and adhere to the surface of the mold powder inflow layer. When the dendrites adhere to the surface of the mold powder inflow layer, solidification nuclei are generated from that point. This increases the density of solidification nuclei.
[0069] The continuous casting preferably includes, for example, a step of vibrating the mold at a frequency of 80 cycles per minute or more. The frequency of the vibration of the mold is preferably 80 to 400 cycles, and more preferably 100 to 400 cycles.
[0070] If the frequency of vibration of the mold is less than 80 cycles, there is a risk that a sufficient density of solidification nuclei cannot be secured, and if the frequency of vibration of the mold is more than 400 cycles, the mold tends to resonate, making casting unstable.
[0071] The viscosity of the mold powder can be changed according to the mold vibration frequency (oscillation cycle). For example, if the mold vibration frequency (oscillation cycle) is set to 50 cycles per minute, it is recommended to use a mold powder with a viscosity of 0.5 Pa·s (5 poise) or more at 1300°C. Even in this case, it is possible to keep the density of solidification nuclei on the surface of a Ni-containing steel slab to 0.35 nuclei / mm 2 It can be more than that.
[0072] For example, if the mold vibration frequency (oscillation cycle) is set to 80 cycles per minute, it is recommended to use a mold powder with a viscosity of 0.15 Pa·s (1.5 poise) or more at 1300°C. Even in this case, the density of solidification nuclei on the surface of a Ni-containing steel slab is reduced to 0.35 nuclei / mm 2 It can be more than that.
[0073] In particular, it is preferable to set the mold oscillation frequency (oscillation cycle) to 80 cycles per minute or more and to use mold powder with a viscosity of 0.5 Pa·s (5 poise) or more at 1300°C. Under these conditions, surface cracks in steel slabs can be significantly reduced.
[0074] The surface of a Ni-containing steel slab includes a surface that includes fine dimples and an extremely flat surface. The surface that includes dimples is believed to be formed by the destruction of grain boundaries in the ductility-reducing temperature range of 600 to 900°C.
[0075] Judging from its shape, the flat surface is thought to have been formed by a type of solidification crack. More specifically, when molten steel solidifies, the final solidification part becomes concentrated with C, S, P, etc., lowering its melting point. The flat surface is formed when the surrounding area that has already completed solidification shrinks while the final solidification part contains a low-melting point liquid phase.
[0076] More specifically, surface cracks occur when solute elements such as C, S, and P are concentrated at the boundary between two solidification cells that compose the solidification shell as the shell grows in the mold. As a result, a liquid phase with a low melting point is generated, causing solidification cracks. It is believed that this solidification crack is the starting point for further cracking due to thermal stress in the secondary cooling zone and stress caused by bending straightening.
[0077] Therefore, surface cracks cannot be sufficiently suppressed by simply reducing the thermal stress or bending stress in the secondary cooling zone, which has been conventionally performed. In order to suppress surface cracks, it is important and necessary to suppress solidification cracks during the initial solidification in the mold.
[0078] Solidification cracking is less likely to occur the less concentrated the solute elements are in the final solidified portion and the smaller the thermal stress acting on the final solidified portion. For example, when the size of the solidified cells is reduced, the cooling rate increases and the concentration of solute elements is suppressed. In addition, when the size of the solidified cells is reduced, the thermal stress is dispersed and the thermal stress acting on the interface between each solidified cell is reduced. Reducing the size of the solidified cells is effective in preventing solidification cracking.
[0079] It is generally known that there is a correlation between the number of solidification cells and the number of solidification nuclei, and the size of the solidification cells decreases as the density of the solidification nuclei increases, so that the size of the solidification cells can be reduced by increasing the density of the solidification nuclei in the area where the molten steel contacts the mold.
[0080] That is, since the Ni-containing steel slab of the present invention has a high density of solidification nuclei, the size of the solidification cells can be reduced, and as a result, a Ni-containing steel slab with few surface cracks can be provided.
[0081] According to the continuous casting method of the present invention, it is possible to control the initial solidification on the surface of the steel slab. This generates a large number of solidification nuclei, and reduces the concentration of impurity elements such as P (phosphorus) and S (sulfur) and C (carbon) at the interface of the solidification cells. This makes it possible to suppress solidification cracks at the interface of the solidification cells. Therefore, it is possible to suppress so-called surface cracks that occur on the surface of the steel slab.
[0082] As described above, the Ni-containing steel slab according to the present invention has a solidification nucleus density of 0.35 nuclei / mm on the slab surface. 2 That is all. For this reason, the size of the solidification cells can be reduced. This reduces the concentration of S and P at the solidification cell interfaces, making it possible to suppress embrittlement at the solidification cell interfaces. In addition, the stress acting on the solidification cell interfaces is also dispersed, making it possible to suppress solidification cracking at the solidification cell interfaces. As a result, it is possible to reduce the occurrence of cracks on the surface of the steel slab.
[0083] In addition, the present invention will describe a method for producing a steel slab using the slab produced by the above-mentioned continuous casting. The method for producing a steel slab containing Ni includes a shaping step for shaping the slab produced by the continuous casting method, and a heating step for heating the slab in a heating furnace at a heating temperature of 1100°C or less after the shaping step.
[0084] In a method for manufacturing steel slabs, a slab is produced by continuously casting molten steel. Conventionally, the produced slab is heated at 1000 to 1200°C (first heat treatment). The slab that has been subjected to the first heat treatment is then subjected to preliminary rolling (light blooming) to reduce its thickness to about 60 to 90%. The preliminary rolled slab is then ground until it is free of defects, and a finishing process is performed to remove the defects. The slab that has been subjected to the finishing process is then heated at 1000 to 1200°C (second heat treatment). The slab that has been subjected to the second heat treatment is then rolled (main rolling).
[0085] It has been confirmed that steel slabs produced by conventional manufacturing methods have cracks with scale at the austenite grain boundaries. The composition of this scale is Fe 2SiO 4 One of the causes of cracking with scale is Fe. 2 SiO 4 The presence of Firelight has been cited.
[0086] Fe 2 SiO 4 Scale is formed in steel containing 0.05% or more silicon (Si), and is 2 SiO 4 It is produced in conjunction with the formation of Fe 2 SiO 4 The eutectic temperature with wustite (FeO) is 1170℃. 2 SiO 4 is a liquid phase oxide above the eutectic temperature.
[0087] Fe 2 SiO 4 When scale is formed, the grain boundaries become weak. Fe 2 SiO 4 Since scale is in a liquid phase at high temperatures, it easily diffuses into grain boundaries and deep within the matrix.
[0088] Fe 2 SiO 4 After the scale is formed, thermal stress and strain during rolling cause grain boundary cracking. Therefore, even if the occurrence of surface defects is suppressed during continuous casting, Fe 2 SiO 4 The presence of fayalite causes defects on the surface of the finished steel slab.
[0089] Therefore, when producing steel slabs, Fe is added during the manufacturing process. 2 SiO 4 In other words, the heating temperature of the heating furnace is preferably set to be equal to or lower than the eutectic temperature of Fe 2 SiO 4 It is preferable that the temperature is equal to or lower than the eutectic temperature.
[0090] In addition, Fe at the grain boundaries 2 SiO 4The formation of scale is also related to the segregation of elements such as P and S in the region. For this reason, even if the manufacturing process is carried out at a temperature below the eutectic temperature of about 1100°C, the liquid phase Fe may exist in part of the region. 2 SiO 4 Scale may form.
[0091] For this reason, Fe 2 SiO 4 In order to prevent the occurrence of cracks accompanied by scale, the heating step is preferably performed at 1100° C. or less, and more preferably at 1050° C. or less. In addition, it is preferable that the rolling step is performed after the slab is heated in the heating step under such conditions.
[0092] Incidentally, when a slab is produced by controlling the density of solidification nuclei according to the continuous casting method of the present invention, the slab has superior toughness to conventional slabs, and therefore a steel slab can be produced without preliminary rolling such as light blooming.
[0093] Therefore, when a slab is produced by controlling the density of solidification nuclei by the continuous casting method of the present invention, a steel slab can be produced by carrying out the following steps (1) to (3).
[0094] (1) The generated slab is subjected to a finishing process in which the surface is ground away for about 3 to 6 mm until all defects are removed (finishing process). (2) The treated slab is heated to a temperature of 1100°C or less (heating process). (3) The slab that has undergone the heating process is rolled (final rolling).
[0095] In this way, by performing the heat treatment at a slab temperature of 1100°C or less, it is possible to suppress surface defects of the steel slab (product) to a level that does not cause problems as a product. 2 SiO 4 It is possible to suppress the formation of scale, and to manufacture steel slabs (products) with suppressed defects in a single rolling process. EXAMPLES
[0096] Molten steels were prepared by melting 3.5%Ni steel with a Ni content of 3.5 mass%, 5%Ni steel with a Ni content of 5.0 mass%, and 5%Ni steel with a Ni content of 7.0 mass%. A converter and an RH vacuum degassing device were used to prepare the molten steels.
[0097] A test was conducted to cast this molten steel using a vertical bending type slab continuous casting machine. The vertical bending type slab continuous casting machine had a thickness of 250 mm and a width of 2100 mm. A total of 20 heats were tested (Test Nos. 1 to 20). Table 1 shows the chemical compositions of Test Nos. 1 to 20. Table 2 shows the casting conditions for the continuous casting machine for Test Nos. 1 to 20.
[0098] [Table 1]
[0099] [Table 2]
[0100] For tests No. 1, 4, 6, 9, 11, 14, and 16, the casting speed was 0.8 m / min. The amplitude of the mold oscillation was 8 mm. The frequency of the oscillation was 60 cycles per minute. The viscosity of the mold powder at 1300°C was 0.20 Pa s.
[0101] For Test Nos. 2, 3, 5, 7, 8, 10, 12, 13, 15, 17, and 18, the casting speed was 0.8 m / min. The amplitude of the mold oscillation was 8 mm. The frequency of the oscillation was 60 cycles per minute. The mold powder used had a viscosity of 0.06 to 2.00 Pa s at 1300°C.
[0102] For Test No. 19, the casting speed was 0.8 m / min. The amplitude of the mold oscillation was 8 mm. The frequency of the oscillation was 80 cycles per minute. The mold powder used had a viscosity of 0.20 Pa·s at 1300°C.
[0103] For test No. 20, the casting speed was 0.8 m / min. The amplitude of the mold oscillation was 8 mm. The frequency of the oscillation was 80 cycles per minute. The mold powder used had a viscosity of 0.5 Pa·s at 1300°C.
[0104] After casting, the steel slab was cut into a length of 300 mm. The cut samples were subjected to the following treatment, and then evaluated for surface cracks. The surface of each sample was shot blasted to remove the oxide film on the surface. Then, surface cracks were identified by penetrant testing. The length and number of surface cracks identified were measured.
[0105] To check the depth of surface cracks, the specimen was ground at positions 3 mm, 6 mm, and 9 mm from the surface. Surface cracks were identified on each ground surface by penetrant testing. The length and number of surface cracks identified were measured.
[0106] The density of solidification nuclei on the slab surface was measured by the following method. A sample was taken from the surface of the steel slab, and the oxide film on the surface was removed by shot blasting. The surface of the steel slab from which the oxide film had been removed was mirror-ground and etched with picric acid to reveal the solidification structure.
[0107] The exposed solidification structure was photographed. In the photograph, a mass (solidification cell, or dendritic cell) whose dendrite branches were oriented in almost the same direction was considered to have grown from one solidification nucleus. The density of the solidification nuclei was calculated by calculating the number of such masses per given area.
[0108] Specifically, the number of solidification cells in the solidification structure photograph was counted, and the density of solidification nuclei was calculated by dividing the number by the area occupied by the solidification cells. The size of the solidification cells tends to be small near the oscillation marks and large away from the oscillation marks. For this reason, the range for counting the solidification cells was set to be from one adjacent oscillation mark to another, and the average value was calculated.
[0109] Table 3 shows the results of investigation of the density of solidification nuclei and the total crack length (crack length x number of cracks) for Test Nos. 1 to 20.
[0110] [Table 3]
[0111] In tests No. 1, 6, 11, and 16, the density of solidification nuclei was 0.35 / mm 2 In Test Nos. 1, 5, 9, and 13, many surface cracks occurred. In Test Nos. 1, 6, 11, and 16, cracks occurred at positions 3 mm or 6 mm away from the surface.
[0112] In contrast, in Tests Nos. 2-5, 7-10, 12-15, and 17-20, the density of solidification nuclei was 0.35 / mm 2 Looking at the results of Test Nos. 2 to 5, 7 to 10, 12 to 15, and 17 to 20, the occurrence of surface cracks decreased as the density of solidification nuclei increased.
[0113] In particular, the density of solidification nuclei is 1.50 / mm 2 A significant reduction in surface cracking was confirmed in Test Nos. 5, 10, 15, and 20, which exceeded 100%. In the remarks column of Table 3, tests within the scope of the present invention are indicated as "Examples of the present invention", and other tests are indicated as "Comparative Examples".
[0114] (Steel billet manufacturing test) The slabs of Test Nos. 1 to 20 were subjected to the heating process and rolling process by the following methods to produce steel slabs (hereinafter also referred to as products). The products were produced using "Method A" corresponding to the conventional manufacturing method and "Method B" corresponding to the manufacturing method of the present invention.
[0115] (Method A) The resulting slab is subjected to a finishing process in which approximately 3 to 6 mm from the surface is ground to remove defects until the slab is free of defects. The slab that has been subjected to the finishing process is heated at 1050°C or 1200°C (first heat treatment). The slab that has been subjected to the first heat treatment is pre-rolled (light bloom rolling) to reduce the thickness from 250 mm to 190 mm. The slab that has been pre-rolled is subjected to a finishing process in which approximately 3 to 6 mm from the surface is ground to remove defects until the slab is free of defects. The slab that has been subjected to the finishing process is heated at 1050°C or 1200°C (second heat treatment). The slab that has been subjected to the second heat treatment is rolled to reduce the thickness from 190 mm to 25 mm. Thereafter, the surfaces at a distance of 3 mm, 6 mm, and 9 mm from the surface are inspected for defects (hereinafter also referred to as product inspection).
[0116] (Method B) The resulting slabs are ground to remove imperfections by grinding approximately 3 to 6 mm from the surface until they are free of imperfections (conditioning process). The conditioned slabs are then heated to 1050°C or 1200°C (heating process). The slabs that had undergone the heating process were then rolled to reduce their thickness from 250 mm to 25 mm. After that, product inspection was carried out on the surfaces 3 mm, 6 mm, and 9 mm away from the surface.
[0117] The product inspection was evaluated on the following three levels: ○: No defects △: Few defects on the product (can be used as a product with proper care) ×: Large amount of defects in the product (Defects remain even after maintenance treatment, making it unusable as a product)
[0118] Table 4 shows the occurrence of surface defects after rolling for each product.
[0119] [Table 4]
[0120] When manufacturing using method A with the slab heating temperature at 1200°C, some defects remained in the product, but the defects were within a range that did not cause production disruption.
[0121] In test Nos. 1, 6, and 11 of 5-7% Ni steel, the amount of finishing was 9 mm. In contrast, the amount of finishing in the other tests of 5-7% Ni steel was 3-6 mm. In test No. 16 of 3.5% Ni steel, the amount of finishing was 6 mm. In contrast, the amount of finishing in the other tests of 3.5% Ni steel was 3 mm. That is, the examples of the present invention were able to reduce the amount of finishing significantly more than the comparative examples.
[0122] Tests No. 2-5, 7-10, 12-15, and 17-20 in which the slab heating temperature was 1050°C were rated as "○: no product defects" even though light blooming was not performed. Therefore, these tests can significantly reduce process costs and stably improve product quality.
[0123] The results of investigating the defects in the products using an EPMA (Electron Probe MicroAnalyzer) showed that in the test example where the slab was heated to 1200°C, Fe was present in the defects. 2 SiO 4 It was found that the slab contained a large amount of oxide scale, and that the effect of oxide scale during heating of the slab contributed greatly to the formation of defects.
Claims
1. 1. A Ni-containing steel slab containing, by mass%, C: 0.03% or more and 0.10% or less, Si: 0.01% or more and 0.50% or less, Mn: 0.10% or more and 1.00% or less, P: 0.001% or more and 0.010% or less, S: 0.0001% or more and 0.0050% or less, Ni: 2.0% or more and less than 7.5%, Al: 0.010% or more and 0.080% or less, N: 0.0010% or more and 0.0050% or less, O: 0.0005% or more and 0.0040% or less, with the balance being Fe and unavoidable impurities, wherein the density of solidification nuclei on a surface of the steel slab is 0.35 nuclei / mm 2 or more and less than 0.60 pieces / mm 2 .
2. The steel cast slab according to claim 1, further comprising, in mass%, one or more selected from Cu: 0.03% or more and 1.50% or less, Cr: 0.03% or more and 1.00% or less, Mo: 0.02% or more and 1.00% or less, Nb: 0.003% or more and 0.100% or less, V: 0.003% or more and 0.100% or less, Ti: 0.005% or more and 0.020% or less, B: 0.0002% or more and 0.0025% or less, Ca: 0.0005% or more and 0.0050% or less, and Mg: 0.0005% or more and 0.0030% or less.
3. A continuous casting method for casting the steel slab according to claim 1 or 2, comprising the steps of: A continuous casting method comprising the step of adding a mold powder having a viscosity of 0.5 Pa·s (5 poise) or more at 1300°C into a mold.
4. A continuous casting method for casting the steel slab according to claim 1 or 2, comprising the steps of: A method of continuous casting comprising the step of vibrating the mold at a frequency of at least 80 cycles per minute.
5. A continuous casting method for casting the steel slab according to claim 1 or 2, comprising the steps of: adding a mold powder having a viscosity of 0.5 Pa·s (5 poise) or more at 1300° C. to the mold; vibrating the mold at a frequency of at least 50 cycles per minute.
6. A continuous casting method for casting the steel slab according to claim 1 or 2, comprising the steps of: adding a mold powder having a viscosity of 0.15 Pa·s (1.5 poise) or more at 1300° C. to the mold; vibrating the mold at a frequency of at least 80 cycles per minute.
7. a conditioning step for performing conditioning treatment on the slab produced by the continuous casting method according to claim 3; a heating step of heating the slab in a heating furnace at a heating temperature of 1100° C. or less after the conditioning step.
8. a conditioning step for performing conditioning treatment on the slab produced by the continuous casting method according to claim 4; a heating step of heating the slab in a heating furnace at a heating temperature of 1100°C or less after the conditioning step.
9. a conditioning step for performing conditioning treatment on the slab produced by the continuous casting method according to claim 5; a heating step of heating the slab in a heating furnace at a heating temperature of 1100°C or less after the conditioning step.
10. a conditioning step for performing conditioning treatment on the slab produced by the continuous casting method according to claim 6; a heating step of heating the slab in a heating furnace at a heating temperature of 1100°C or less after the conditioning step.
Citation Information
Patent Citations
Preventing method for surface flaw in continuous casting of ni-containing steel for low temperature use
JP1982026141A
Method for preventing surface crack on ni-contained steel in continuous casting
JP1989228644A
Production of steel for large heat input welding excellent in toughness at low temperature
JP1990250917A
Method for continuously casting nickel-containing steel
JP1996010919A
Continuous casting method of high ni steel
JP1996033964A