WC-based hard alloy, mixed powder for producing WC-based hard alloy, WC-based hard alloy member, and method for producing WC-based hard alloy member
A balanced WC-based cemented carbide composition with controlled phases and element ratios addresses the trade-off between thermal conductivity and wear resistance, achieving high hardness and conductivity for applications like cutting tools and molds.
Patent Information
- Application Number
- JP2023575329
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2022-01-24
- Filing Date
- 2023-01-24
- Publication Date
- 2024-10-08
- Estimated Expiration
- 2043-01-24
AI Technical Summary
Existing WC-based cemented carbides face a trade-off between high thermal conductivity and wear resistance, with increased binder phase content improving toughness but reducing thermal conductivity, and high Cu content enhancing thermal conductivity but necessitating further hardness improvements.
A WC-based cemented carbide composition comprising 10-40% Co, 5-15% Cu, with the remainder consisting of Ti, Zr, Cr, W, B, C, and unavoidable impurities, structured into phases that balance hardness and thermal conductivity, including a first phase of Ti, W, and C, a second phase of W, B, and Co, and a third phase predominantly Co, with controlled molar ratios and area ratios for optimal properties.
The solution provides a WC-based cemented carbide with high wear resistance and thermal conductivity, suitable for applications requiring both properties, such as cutting tools and molds, by maintaining hardness above 45HRC and thermal conductivity above 10 W/(m·K).
Smart Images

Figure 0007563634000005 
Figure 0007563634000006 
Figure 0007563634000007
Abstract
Description
[Technical field]
[0001] The present disclosure relates to a WC-based cemented carbide, a mixed powder for producing a WC-based cemented carbide, a WC-based cemented carbide member, and a method for producing the WC-based cemented carbide member. [Background technology]
[0002] Hot stamping is a manufacturing method in which a workpiece heated to a high temperature is press-molded and simultaneously cooled in a die to harden it. For hot stamping dies, it is desirable to improve the thermal conductivity of the die material in order to improve hardenability and increase production efficiency. In addition, wear resistance is required to reduce damage to the die caused by scale that adheres to the workpiece heated to a high temperature.
[0003] For example, a material that combines thermal conductivity and wear resistance is a composite material in which hard WC is dispersed in a metallic bonding phase such as Co (hereinafter referred to as "WC-based cemented carbide"). WC-based cemented carbide has excellent wear resistance and is used in cutting tools and the like. On the other hand, it also has excellent thermal conductivity, and the thermal conductivity of WC-based cemented carbide is higher than that of tool steel.
[0004] Patent Document 1 discloses a WC-based cemented carbide in which tungsten carbide particles are bound by a binder phase of cobalt or a cobalt alloy, the cobalt or cobalt alloy content being 35 to 50 mass %, and fine tungsten carbide particles showing a predetermined distribution.
[0005] Patent Document 2 discloses a WC-based cemented carbide member which is an additive manufacturing body including WC particles, Cu, and a metallic bonding phase consisting of at least one of Co, Fe, and Cr, in which the WC particle content is 40 mass% or more, the content of at least one of Co, Fe, and Cr is 25 mass% or more and less than 60 mass%, and the ratio a / b of the Cu content a to the content b of at least one of Co, Fe, and Cr satisfies 0.070≦a / b≦1.000.
[0006] Non-Patent Document 1 describes that a combination of molecular dynamics and density functional theory makes it possible to simulate both covalent bond systems and metal systems.
[0007] Non-Patent Document 2 describes obtaining a stress-strain curve by predicting the ideal strength of silicon along several loading paths using density functional theory. [Prior art documents] [Patent documents]
[0008] [Patent Document 1] JP 2016-160500 A [Patent Document 2] International Publication No. 2021 / 039912 [Non-patent literature]
[0009] [Non-Patent Document 1] R. Car, M. Parrinello, Unified Approach for Molecular Dynamics and Density-Functional Theory. PHYSICAL REVIEW LETTERS VOLUME 55, NUMBER 22, 2471-2474 (1985) [Non-Patent Document 2] SM-M. Dubois et al., Ideal strength of silicon: An ab initio study. PHYSICAL REVIEW B 74, 235203 (2006) Summary of the Invention [Problem to be solved by the invention]
[0010] The WC-based cemented carbide described in Patent Document 1 has fine tungsten carbide particles distributed in the alloy structure, which allows the hardness to be increased without impairing the toughness improved by increasing the amount of cobalt. However, the decrease in thermal conductivity due to the increase in the binder phase remains an issue.
[0011] The WC-based cemented carbide member described in Patent Document 2 has a high Cu content and high thermal conductivity. However, there is a demand for further increasing the hardness.
[0012] An object of the present disclosure is to provide a WC-based cemented carbide that has high wear resistance while adopting a configuration advantageous for high thermal conductivity. [Means for solving the problem]
[0013] The WC-based cemented carbide of the present disclosure contains, by mass%, 10% to 40% Co, 5% to 15% Cu, and the balance consisting of at least one selected from the group consisting of Ti, Zr, and Cr, as well as W, B, C, and unavoidable impurities.
[0014] In addition, it is preferable that the B content is 1.5 to 3 times the Ti content, and the C content is 0.5 to 2 times the W content, in terms of molar ratio.
[0015] Furthermore, in mass%, it is preferable that the Ti content is more than 0% and less than 15%, the B content is more than 0% and less than 6.0%, the W content is more than 23% and 75.5% or less, and the C content is more than 1.5% and 5% or less.
[0016] Furthermore, in mass%, it is preferable that the Ti content is 15% or more and 35% or less, the B content is 6.0% or more and 16% or less, the W content is more than 0% and 61.5% or less, and the C content is more than 0% and 4% or less.
[0017] It is also preferable that the alloy has a first phase containing Ti, W, and C, a second phase containing W, B, and Co, and a third phase containing Co, and that the area ratio of the first phase in cross-sectional observation is more than 0% and 50% or less.
[0018] It is also preferable that the alloy has a first phase containing Ti, W, and C, a second phase containing W, B, and Co, and a third phase containing Co, and that the area ratio of the first phase in cross-sectional observation is 30% or more and 60% or less.
[0019] The present disclosure also provides a mixed powder for producing a WC-based cemented carbide, obtained by mixing a plurality of types of powders, the mixed powder having an average composition, in mass%, of 10% to 40% Co, 5% to 15% Cu, and the remainder consisting of at least one selected from the group consisting of Ti, Zr, and Cr, as well as W, B, C, and unavoidable impurities.
[0020] In addition, the WC-based cemented carbide preferably has a B content of 1.5 to 3 times the Ti content, and a C content of 0.5 to 2 times the W content, in molar ratio.
[0021] Furthermore, in the WC-based cemented carbide, it is preferable that the Ti content is more than 0% and less than 15%, the B content is more than 0% and less than 6.0%, the W content is more than 23% and 75.5% or less, and the C content is more than 1.5% and 5% or less, in mass percent.
[0022] In addition, the WC-based cemented carbide preferably has, in mass%, a Ti content of 15% or more and 35% or less, a B content of 6.0% or more and 16% or less, a W content of more than 0% and 61.5% or less, and a C content of more than 0% and 4% or less.
[0023] The present disclosure also provides a member formed of a WC-based cemented carbide, the WC-based cemented carbide containing, by mass%, 10% to 40% Co, 5% to 15% Cu, and the remainder being at least one selected from the group consisting of Ti, Zr, and Cr, as well as W, B, C, and unavoidable impurities.
[0024] In addition, the WC-based cemented carbide preferably has a B content of 1.5 to 3 times the Ti content, and a C content of 0.5 to 2 times the W content, in molar ratio.
[0025] Furthermore, in the WC-based cemented carbide, it is preferable that the Ti content is more than 0% and less than 15%, the B content is more than 0% and less than 6.0%, the W content is more than 23% and 75.5% or less, and the C content is more than 1.5% and 5% or less, in mass percent.
[0026] In addition, the WC-based cemented carbide preferably has, in mass%, a Ti content of 15% or more and 35% or less, a B content of 6.0% or more and 16% or less, a W content of more than 0% and 61.5% or less, and a C content of more than 0% and 4% or less.
[0027] In addition, it is preferable that the hardness is 45HRC or more and the thermal conductivity is 10W / (m·K) or more.
[0028] The present disclosure also provides a WC-based cemented carbide member including a substrate and a cemented carbide portion formed on a surface of the substrate, the cemented carbide portion being formed of a WC-based cemented carbide containing, by mass%, 10% to 40% Co, 5% to 15% Cu, and the balance being at least one selected from the group consisting of Ti, Zr, and Cr, as well as W, B, C, and unavoidable impurities.
[0029] In addition, the WC-based cemented carbide preferably has a B content of 1.5 to 3 times the Ti content, and a C content of 0.5 to 2 times the W content, in molar ratio.
[0030] Furthermore, in the WC-based cemented carbide, it is preferable that the Ti content is more than 0% and less than 15%, the B content is more than 0% and less than 6.0%, the W content is more than 23% and 75.5% or less, and the C content is more than 1.5% and 5% or less, in mass percent.
[0031] In addition, the WC-based cemented carbide preferably has, in mass%, a Ti content of 15% or more and 35% or less, a B content of 6.0% or more and 16% or less, a W content of more than 0% and 61.5% or less, and a C content of more than 0% and 4% or less.
[0032] The cemented carbide portion preferably has a hardness of 45HRC or more and a thermal conductivity of 10W / (m·K) or more.
[0033] The present disclosure also provides a method for producing a WC-based cemented carbide member, which includes a melting and solidifying process in which a mixed powder is irradiated with a heat source beam to melt the mixed powder and then solidify it, and the average composition of the components constituting the mixed powder includes, by mass%, 10% to 40% Co and 5% to 15% Cu, with the balance being at least one selected from the group consisting of Ti, Zr, and Cr, as well as W, B, C, and unavoidable impurities.
[0034] It is preferable that the method further includes a powder mixing step of individually pumping and mixing a plurality of types of powder together with a carrier gas to form a mixed powder, and a mixed powder supplying step of supplying the mixed powder.
[0035] The present disclosure also relates to an apparatus for manufacturing a mixed powder for producing WC-based cemented carbide, the apparatus having a mixing section in a truncated cone shape and a plurality of pipes connected to the mixing section, the diameter of an upper bottom surface of the mixing section being larger than the diameter of a lower bottom surface of the mixing section, the mixing section being composed of an outer wall section that is externally recognized as a slant portion of the truncated cone and an inserted section that corresponds to the slant portion of the truncated cone inserted inside the outer wall section, the space formed between the outer wall section and the inserted section being a flow path for a plurality of types of powder supplied from the plurality of pipes, the plurality of pipes being connected to the outer edge of the upper bottom surface of the mixing section, the plurality of types of powder being raw materials for the WC-based cemented carbide and being components of the mixed powder, and the mixed powder being configured to flow out from a lower portion of the mixing section.
[0036] In addition, it is preferable that the average composition of the components constituting the mixed powder contains, in mass%, 10% to 40% Co, 5% to 15% Cu, and the remainder consisting of at least one selected from the group consisting of Ti, Zr, and Cr, as well as W, B, C, and unavoidable impurities.
[0037] In addition, the cross-sectional area of the upper part of the space is preferably larger than the total cross-sectional area of the multiple pipes.
[0038] The present disclosure also provides an apparatus for manufacturing a WC-based cemented carbide member, the apparatus having a head unit that irradiates a mixed powder with a heat source beam and a mixed powder supply unit that supplies the mixed powder, the mixed powder having an average composition, by mass%, of 10% to 40% Co and 5% to 15% Cu, with the remainder being at least one selected from the group consisting of Ti, Zr and Cr, as well as W, B, C and unavoidable impurities.
[0039] Moreover, the head portion preferably has a mixed powder supply portion and is configured to cause the mixed powder to flow outward from the heat source beam.
[0040] It is also preferable that the apparatus further comprises a mixing section having a truncated cone shape for mixing a plurality of types of powders pumped together with the carrier gas to produce a mixed powder. Effect of the Invention
[0041] According to the present disclosure, it is possible to provide a WC-based cemented carbide having high wear resistance while adopting a configuration advantageous for high thermal conductivity. [Brief description of the drawings]
[0042] [Figure 1] FIG. 2 is a perspective view showing an example of a main part of an apparatus for mixing powders used to produce a WC-based cemented carbide. [Diagram 2] FIG. 1 is an overall configuration diagram showing an example of a manufacturing apparatus for a WC-based cemented carbide member. [Diagram 3] FIG. 2 is a side view showing an example of a WC-based cemented carbide member. [Figure 4] FIG. 1 is a diagram showing the results of elemental mapping analysis by EPMA and a backscattered electron image of Test Piece No. 1 of the example. [Diagram 5] FIG. 13 is a diagram showing the results of elemental mapping analysis by EPMA and a backscattered electron image of Test Piece No. 2 of the example. [Figure 6] FIG. 13 is a diagram showing the results of elemental mapping analysis by EPMA and a backscattered electron image of Test Piece No. 3 of the example. [Figure 7] 1 is a graph showing the relationship between shear fracture energy and Cu concentration. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0043] The present disclosure relates to a WC-based cemented carbide having a boride added thereto, a mixed powder for producing a WC-based cemented carbide, a WC-based cemented carbide member, a method for producing a WC-based cemented carbide member, an apparatus for producing a mixed powder for producing a WC-based cemented carbide, and an apparatus for producing a WC-based cemented carbide member.
[0044] Hereinafter, the embodiments of the present disclosure will be described in detail with reference to the drawings. In this specification, the numerical range of "to" is a range including the numerical values before and after it by "greater than" and "less than". In addition, when "greater than" or "less than" is added to a numerical value, the numerical value is not included. In the drawings, the same or similar parts are given the same reference symbols, and the description thereof will not be repeated.
[0045] (WC type cemented carbide) The WC-based cemented carbide according to an embodiment of the present disclosure is characterized in that it contains, by mass%, 10% to 40% Co, 5% to 15% Cu, and the balance consisting of at least one selected from the group consisting of Ti, Zr, and Cr, as well as W, B, C, and unavoidable impurities.
[0046] [Co: 10% by mass to 40% by mass] Co (cobalt) constitutes the metallic bonding phase. Therefore, by increasing the Co content, the toughness of the WC-based cemented carbide member is improved. For example, in the WC-based cemented carbide used for manufacturing the WC-based cemented carbide member, the content of the metallic bonding phase, in mass%, of 10% to 40% can be set to prevent the hardness of the WC-based cemented carbide from decreasing. In addition, Fe or Cr may be added in addition to Co to prevent the hardness from decreasing.
[0047] [Cu: 5% to 15% by mass] Cu (copper) disperses in the metal bonding phase and plays a role in increasing the thermal conductivity of the WC cemented carbide member. If the WC cemented carbide member contains Cu, the thermal conductivity can be increased. In addition to Cu, Al, etc. may be added to increase the thermal conductivity.
[0048] Also, B forms borides of W and Ti. All of these borides contribute to improving hardness and thermal conductivity. On the other hand, W and Ti borides have lower toughness compared to carbides. Therefore, if added in excess, toughness decreases. The content of B (boron) is appropriate to be about twice that of Ti in order to make it exist in the form of TiB2, and is preferably 1.5 to 3 times the content of Ti in molar ratio. On the other hand, if there is too much TiB2, it is likely to become brittle, so it is more preferable that the ratio of TiB2 is 5 to 20 mass% of the total. In that case, the amount of boron added contained in TiB2 is about 1.6 to 6.0 mass%. Also, the content of C is appropriate to be about 1 time that of W in order to make it exist in the form of WC, and is preferably 0.5 to 2 times the content of W in molar ratio.
[0049] [Structure of WC-based cemented carbide] WC-based cemented carbide has a structure as a composite material in which particles of hard WC (tungsten carbide), a carbide of W (tungsten) and C (carbon), are integrated with a metal bonding phase. The greater the amount of WC in a WC-based cemented carbide member, the higher the hardness. For example, it is preferable for the WC content to be 40% by mass or more.
[0050] In addition to the above elements, the WC cemented carbide of this embodiment may be allowed to contain elements such as Na, Mg, Al, Si, P, S, Ca, Ti, Mn, Ni, Zn, Ga, As, Se, Br, Cd, Sn, Sb, and Te that are brought in due to the conditions of raw materials, materials, and manufacturing equipment. The lower the content of these elements, the more preferable, and the total of these elements is allowed to be 200 ppm or less. In addition to these elements, O, N, and Ar may be included. It is preferable that the O, N, and Ar contents are 0.5% or less by mass, 0.5% or less by mass, and 0.5% or less by mass, respectively.
[0051] The above elements may be mixed in within permissible limits, but may be unavoidable depending on the factors, and are therefore included in unavoidable impurities.
[0052] In the WC-based cemented carbide, the contents of the constituent elements other than the above Co and Cu are preferably set to the contents shown in the following alloy composition I or alloy composition II. When priority is given to thermal conductivity, alloy composition I can be selected, and when priority is given to hardness, alloy composition II can be selected.
[0053] <Alloy composition I> [Ti: over 0 mass% and less than 15 mass%] When WC-based cemented carbide contains Ti, it forms thermodynamically stable TiC, which increases its hardness. In addition, WC dissolves in TiC to form a (W,Ti)C solid solution carbide (β phase), which improves oxidation resistance.
[0054] TiC has a rock-salt structure, and as a structural body, it has both strength and toughness. TiC has a non-stoichiometric composition, and maintains a stable crystal structure over a wide composition range. In addition, since its specific gravity is small compared to its strength, it contributes to improving the specific strength. On the other hand, Ti carbide has a low thermal conductivity compared to W carbide. Therefore, if it is added in excess, the thermal conductivity decreases. Therefore, the Ti content, in mass%, is preferably more than 0 mass% and less than 15 mass%, and more preferably 3.4 mass% to 14 mass%.
[0055] [Zr: more than 0 mass% and 17.0 mass% or less] When Zr is added to WC-based cemented carbide, a small amount of Zr dissolves in Co, contributing to improved high-temperature strength. In addition, by dispersing ZrB2 in the WC-based cemented carbide, it is expected to improve thermal conductivity.
[0056] On the other hand, Zr has a strong bond with oxygen and is prone to producing ZrO2, which leads to a decrease in toughness. Therefore, the Zr content is preferably more than 0 mass% and not more than 17.0 mass%, and more preferably 4.0 mass% to 17.0 mass%.
[0057] [Cr: more than 0 mass% and 15.0 mass% or less] When Cr is added to WC-based cemented carbide, most of the Cr dissolves in the binder phase, which contributes to improving corrosion resistance and oxidation resistance. In addition, when rapid solidification is performed, such as in additive manufacturing, a large amount of Cr dissolves in Co. Furthermore, when such rapid solidification is performed, the grain size of the carbides and borides dispersed in the WC-based cemented carbide becomes fine, so that the flexural strength increases from low to high temperatures, and the decrease in strength can be suppressed.
[0058] On the other hand, Cr has a lower thermal conductivity than W carbide and Co. Therefore, adding an excessive amount of Cr causes a decrease in thermal conductivity. Therefore, the Cr content is preferably more than 0 mass% and not more than 15.0 mass%, and more preferably 3.5 mass% to 14.5 mass%.
[0059] [B: More than 0% by mass and less than 6.0% by mass] B forms borides of W and Ti. All of these borides contribute to improving hardness and thermal conductivity. On the other hand, borides of W and Ti have lower toughness than carbides. Therefore, if added in excess, the toughness decreases. Therefore, the content of B is preferably more than 0 mass% and less than 6.0 mass%, and more preferably 1.6 mass% to 6.0 mass%.
[0060] [W: More than 23 mass% and 75.5 mass% or less] W forms carbides and borides. WC has both hardness and toughness. It is also characterized by its high Young's modulus, and is less likely to bend when used as a structural material. WB has similar properties to WC, so materials based on these materials are suitable for tools such as dies and cutting tools. Therefore, W is preferably more than 23 mass% and not more than 75.5 mass%, and more preferably 42 mass% to 57 mass%.
[0061] [C: More than 1.5% by mass and 5% by mass or less] C is an element that forms carbides. There is an appropriate amount of C in each composition, and if there is not enough C, an embrittled layer such as the η phase will occur, while if there is too much C, it will lead to the generation of free carbon. Both of these are likely to become the starting point for the destruction of the component, so it is preferable to suppress them. Therefore, C is preferably more than 1.5 mass% and not more than 5 mass%, and more preferably 2.7 mass% to 3.7 mass%.
[0062] <Alloy composition II> Alloy composition II has improved hardness and specific strength compared to alloy composition I. The effects of each element are as described above.
[0063] [Ti: 15% by mass or more and 35% by mass or less] From the viewpoints of hardness and specific strength, the TiC content is made larger than that of alloy composition I. Therefore, the Ti content is made 15 mass % to 35 mass %.
[0064] [B: 6.0% by mass or more and 16% by mass or less] B forms borides of W and Ti. Both of these borides contribute to improving hardness and thermal conductivity. On the other hand, W and Ti borides have lower toughness compared to carbides. Therefore, if added in excess, toughness decreases. From the viewpoint of hardness and specific strength, the content is made larger than that of alloy composition I. Therefore, B is set to 6.0 mass% to 16 mass%.
[0065] [W: More than 0 mass% and 61.5 mass% or less] W has the property of providing both hardness and toughness by forming WC and WB, so the W content is set to more than 0 mass% and not more than 61.5 mass%.
[0066] [C: More than 0 mass% and 4 mass% or less] WC-Co cemented carbide is a two-phase alloy (WC+Co bonded phase) if the amount of alloy carbon is equal to or close to the amount of bonded carbon in WC. However, if the amount of alloy carbon is slightly more than that, it becomes a three-phase alloy with the addition of free carbon (C), and if the amount of alloy carbon is slightly less than that, it becomes a three-phase alloy with the addition of η-phase (Co3W3C). These phases are called harmful phases and reduce the mechanical properties. Therefore, the C content is set to more than 0 mass% and 4 mass% or less.
[0067] The amounts of the above elements can be analyzed by, for example, ICP-OES or ICP-MS, or quantitatively analyzed by surface analysis techniques such as XRF, EPMA, and EDX.
[0068] [Alloy structure] The WC-based cemented carbide of this embodiment has a first phase containing Ti, W, and C, a second phase containing W, B, and Co, and a third phase containing Co. The first phase, the second phase, and the third phase can be evaluated using, for example, an electron probe micro analyzer (EPMA).
[0069] The first phase can be referred to as a hard phase containing Ti, W, and C (also referred to as a "WTiC phase"). The second phase can be referred to as a hard phase containing W, B, and Co (also referred to as a "WBCo phase"). The third phase can also be called a metal phase that is composed of a metal phase containing the most Co by mass percent (Co-rich phase). In the first phase, the top three elements with the highest content are Ti, W, and C.
[0070] In the case of alloy composition I, the area ratio of the first phase is preferably more than 0% and not more than 50%, and in the case of alloy composition II, the area ratio of the first phase is preferably 30% or more and 60% or less.
[0071] [Area ratio] The area ratio in this specification may be calculated by observing the cross section of the alloy and calculating the area ratio in the observed region from image processing based on element mapping using an EPMA, etc. For example, the area ratio may be calculated by regarding the phase in which W, Ti, and C are detected as concentrated as the first phase, the phase in which W, B, and Co are detected as concentrated as the second phase, and the phase in which Co is mainly detected as the third phase.
[0072] When using an EPMA (e.g., EPMA-1610, manufactured by Shimadzu Corporation), the observation conditions can be, for example, accelerating voltage: 15 kV, irradiation current: 100 nA, data point X: 400, Y: 400, step size X: 0.300 μm, Y: 0.300 μm, beam diameter: 1 μm, and counting time: 20 msec.
[0073] (WC type cemented carbide powder) The WC-based cemented carbide powder can be a powder that is an aggregate of particles having the composition of the above-mentioned WC-based cemented carbide, that is, a pre-alloyed alloy powder. As a method for producing pre-alloyed alloy powder, it is preferable to increase the sphericity and improve the fluidity by thermal plasma droplet smelting, which is a refining method in which alloy granulated powder is passed through a high-temperature region such as plasma. In addition to granulated powder, powder produced by gas atomization or water atomization may be used. For example, in order to improve the molding accuracy, the fluidity of the powder (a value measured in accordance with JIS Z2502) is preferably 10 to 40 sec / 50 g, more preferably 10 to 30 sec / 50 g, and even more preferably 10 to 25 sec / 50 g.
[0074] Also, WC-Co powder containing WC and Co, WC powder, Cu powder, and at least one boride powder selected from WB4, TiB2, ZrB2, and CrB2 can be used. As the WC-Co powder, WC-Co powder having a Co ratio of 10 to 40% can be used. Also, only WC powder and Co powder may be used, or W powder, Co powder, and C powder may be added separately. Furthermore, WC powder and Co powder can be used after using WC-Co powder.
[0075] For example, the powder for WC-based cemented carbide may be a powder in which each powder of W, Co, Cu, Ti, B and C is mixed to have a desired composition range, or an alloy powder containing two or more of the above elements may be mixed with a powder of the remaining element. Of course, alloy powders containing two or more of the above elements may be mixed together.
[0076] FIG. 1 is a perspective view showing an example of a main part of an apparatus for mixing powders used to produce a WC-based cemented carbide.
[0077] In this figure, the mixed powder manufacturing apparatus 100 (mixed powder manufacturing apparatus) has a configuration in which a plurality of pipes 120 are connected to a mixing section 110 in the shape of a truncated cone. The diameter of the upper bottom surface of the mixing section 110 is larger than the diameter of the lower bottom surface. The mixing section 110 is composed of a large diameter section 112 (outer wall section) that is externally recognized as the inclined surface part of the truncated cone, and a small diameter section 114 (internal insertion section) that corresponds to the inclined surface part of the truncated cone inserted inside the large diameter section 112. A space 116 formed between the large diameter section 112 and the small diameter section 114 is a flow path for the powders 132 and 134 supplied from the pipe 120. The pipe 120 is connected to the outer edge of the upper bottom surface of the mixing section 110. The powders 132 and 134 are raw materials for WC-based cemented carbide.
[0078] The multiple types of powders 132, 134 flow into the space 116 together with the carrier gas through different pipes 120, are mixed while passing through the space 116 as indicated by the dashed arrow 136, and flow out from the bottom of the space 116. Although the arrow 136 is simply shown pointing downward, the powders 132, 134 actually flow down the space 116 while swirling. Therefore, the multiple types of powders 132, 134 are naturally mixed together to become a mixed powder 138. The mixed powder 138 flows out from the bottom of the mixing section 110. The carrier gas is preferably an inert gas or compressed air.
[0079] The method for producing the mixed powder 138 using the mixed powder production apparatus 100 shown in this figure includes the following steps.
[0080] The multiple types of powders 132, 134 are individually pumped together with a carrier gas through the pipes 120 into the space 116 (first step). The pumped multiple types of powders 132, 134 and the carrier gas are ejected into the space 116 and mixed together to obtain a mixed powder 138 (second step). Here, the cross-sectional area of the upper part of the space 116 is larger than the sum of the cross-sectional areas of the multiple pipes 120.
[0081] The mixed powder 138 is discharged from a discharge port provided in the lower part of the space 116 (third step).
[0082] The first step and the second step, or the first step, the second step and the third step may be collectively referred to as a "powder mixing step."
[0083] There are no particular limitations on the type of powders 132 and 134. The particle size of the powders 132 and 134 is preferably an average particle size (D50) of about 0.1 to 300 μm. For example, in the metal deposition method, the average particle size (D50) is preferably 30 to 250 μm, and more preferably about 60 μm to 150 μm, in an integrated distribution curve of particle size on a volume basis determined by a laser diffraction method.
[0084] FIG. 2 is a diagram showing an overall configuration of an example of a manufacturing apparatus for a WC-based cemented carbide member.
[0085] In this figure, an additive manufacturing apparatus 200 (a manufacturing apparatus for a WC-based cemented carbide member) includes a mixed powder manufacturing apparatus 100 (a mixed powder manufacturing section), a plurality of powder supply sections 210, and a head section 240. The mixed powder manufacturing apparatus 100 and the powder supply sections 210 are connected by a pipe 120 (a powder supply path). In addition, the mixed powder manufacturing apparatus 100 and the head section 240 are connected by a pipe 230 (a mixed powder supply path).
[0086] From each powder supply section 210, powders that are components of the mixed powder are pressure-fed by a carrier gas 220 (indicated by the dashed arrow in the figure).
[0087] In the mixed powder manufacturing apparatus 100, a plurality of types of powder sent from each powder supply unit 210 are mixed as shown in FIG. 1 to produce a mixed powder.
[0088] From the head unit 240, a heat source beam 250 is irradiated toward the substrate 320, and mixed powder sent to the head unit 240 via the piping 230 is supplied. In the figure, the mixed powder is indicated by a dotted line outside the heat source beam 250. The heat source beam 250 is a laser, an electron beam, a plasma, an arc, or the like. In particular, a laser is preferable because it can make the irradiation spot relatively small and can perform the work under atmospheric pressure.
[0089] The mixed powder is heated by the heat source beam 250 on the surface of the substrate 320 , melted, and laminated to form the cemented carbide portion 310 .
[0090] When the cemented carbide part 310 is formed, a part of the base material 320 may also be heated by the heat source beam 250 and melt. In this case, the cemented carbide part 310 contains a mixture of the mixed powder and the components of the base material 320. Even in such a case, if the cemented carbide part 310 is laminated to a predetermined thickness or more by further supplying the mixed powder, that part becomes a region in which the components of the base material 320 do not melt. By forming the cemented carbide part 310 in this manner, the exposed part of the cemented carbide part 310 can be made of a cemented carbide having the desired hardness and thermal conductivity.
[0091] (WC-based cemented carbide materials) An example of the WC-based cemented carbide member includes a substrate and a cemented carbide part formed on the surface of the substrate, as described above. The cemented carbide part is formed of a WC-based cemented carbide and contains, by mass%, 10% to 40% Co, 5% to 15% Cu, and the balance is at least one selected from the group consisting of Ti, Zr, and Cr, as well as W, B, C, and inevitable impurities. The cemented carbide part may be formed in the form of a film.
[0092] FIG. 3 shows an example of a WC-based cemented carbide member.
[0093] In this figure, the WC-based cemented carbide member 300 has a configuration in which a part of the surface of a base material 320 is covered with a cemented carbide portion 310 .
[0094] The WC-based cemented carbide member may be a member obtained by separating the cemented carbide portion from the member integral with the substrate as described above. The method of separation is not particularly limited. In this case, the WC-based cemented carbide member does not include the substrate and is made of only the WC-based cemented carbide.
[0095] [hardness] The hardness of the cemented carbide member is, for example, 45HRC or more in Rockwell hardness, preferably 50HRC or more, more preferably 60HRC or more, and particularly preferably 70HRC or more.
[0096] [Hardness measurement method] The hardness can be measured by the Rockwell hardness test method.
[0097] The cemented carbide part is cut, and the cut surface is polished to a mirror finish using emery paper and diamond abrasives to prepare a test piece. Then, at room temperature, the hardness is measured using a Rockwell hardness tester with an initial load of 10 kgf for 2 seconds, followed by a load of 60 kgf and a holding time of 4 seconds. The measurement is carried out three times, and the average value of the three measurements is taken as the hardness.
[0098] [Thermal Conductivity] The thermal conductivity is 10 W / (m·K) or more, preferably 20 W / (m·K) or more, more preferably 30 W / (m·K) or more, and particularly preferably 40 W / (m·K) or more.
[0099] [Method of measuring thermal conductivity] The thermal conductivity of an alloy member can be measured by measuring the thermal diffusivity α, density ρ, and specific heat c, and calculating the thermal conductivity λ from the following formula (1).
[0100] λ=α·ρ·c …Equation (1) The thermal diffusivity can be measured using a Xe flash method thermal diffusivity measuring device (manufactured by Bruker-axs, model: Nanoflash LFA447 NETZSCH). For example, the sample (test piece) used to measure thermal diffusivity may be 9.5 mm × 9.5 mm × 1.5 mm in size, polished to #600 with waterproof Emily paper, and blackened by spraying with fine graphite powder to be used as the specimen.
[0101] The specific heat can be measured, for example, by using a differential scanning calorimeter (DSC).
[0102] [Evaluation of wear resistance] Wear resistance can be evaluated using friction and wear testers, such as ball-on-disk, pin-on-disk, block-on-ring, and reciprocating sliding tests.
[0103] A lathe can also be used in these wear resistance evaluation tests. By using a lathe, the rotating steel piece is brought into contact with the test piece and slid against it using the rotational force of the lathe, and the wear depth can be measured and evaluated after a certain number of slides. In this case, it is preferable to rotate the steel piece eccentrically with respect to the rotation axis of the lathe.
[0104] <Application> The WC-based cemented carbide and WC-based cemented carbide member of the present embodiment have both high thermal conductivity and high wear resistance. Therefore, they can be applied to tools such as cutting tools and dies, bearings, guides for sliding surfaces, gears, and other wear-resistant members. In particular, when applied to a die for hot stamping to form ultra-high tensile steel, the cooling time is greatly shortened due to the improved thermal conductivity of the die, which is optimal for contributing to improved productivity.
[0105] (Method of manufacturing WC-based cemented carbide members) One method for manufacturing WC-based cemented carbide parts is the additive manufacturing method. This will be explained below with reference to Fig. 2. In the following explanation, the steps other than the preheating step may be collectively referred to as the "additive manufacturing step."
[0106] As shown in this figure, a base material 320 is prepared, and is preheated as necessary (preheating step).
[0107] Next, raw material powders are fed under pressure from the powder feeder 210 to the mixed powder manufacturing apparatus 100 (raw powder feeding step). The fed powders are mixed in the mixed powder manufacturing apparatus 100 to prepare a mixed powder (mixed powder preparation step).
[0108] Then, the heat source beam 250 is irradiated from the head unit 240 toward the substrate 320, and the mixed powder sent to the head unit 240 via the piping 230 is supplied (mixed powder supplying step). The mixed powder melts on the surface of the substrate 320, and then the melted portion solidifies by adjusting the amount of irradiation energy of the heat source beam 250 or by moving the head unit 240 (melting and solidifying step).
[0109] By repeating the mixed powder supplying step and the melting and solidifying step, a cemented carbide member (reference numeral 310) having a desired shape can be produced.
[0110] The mixed powder may be placed on the surface of the base material 320 or the like in advance, and may be melted by irradiating the heat source beam 250, and then solidified. The mixed powder may be supplied from a discharge unit (mixed powder supply unit) provided separately from the head unit 240 that irradiates the heat source beam 250. In this case, the process of supplying the mixed powder from the discharge unit may be called a "mixed powder supply process" separately from the process of irradiating the heat source beam 250.
[0111] The mixed powder is a mixture of multiple types of raw material powders, and in order to manufacture the WC-based cemented carbide member according to the present disclosure, the average composition of the components constituting the mixed powder contains, in mass%, 10% to 40% Co, 5% to 15% Cu, and the remainder is at least one selected from the group consisting of Ti, Zr, and Cr, as well as W, B, C, and unavoidable impurities. The mixed powder is also called "mixed powder for manufacturing WC-based cemented carbide."
[0112] In the case of a component that does not require base material 320, cemented carbide portion 310 is separated from base material 320 by cutting or the like to produce a component made only of WC-based cemented carbide.
[0113] The raw material powder supplying step and the mixed powder preparation step may be performed in advance to prepare an appropriate mixed powder. By preparing the mixed powder in this manner, the manufacturing time of the cemented carbide portion 310 can be shortened.
[0114] The above is an example of a method for additively manufacturing the entire object using WC-based cemented carbide powder.
[0115] The process of repeating the mixed powder supplying process and the melting and solidifying process may be called a model stacking formation process.
[0116] The additive manufacturing method described above is preferable compared to conventional liquid phase sintering methods because it creates shapes instantly and locally through melting and solidification, which can suppress deformation due to the material's own weight during creation.
[0117] The additive manufacturing method according to the present disclosure is not limited to the method using a heat source beam as described above, but may use, for example, directed energy deposition methods such as laser metal deposition, powder bed fusion, plasma powder deposition, etc.
[0118] According to the additive manufacturing method described above, additive manufacturing can be performed while accurately and quickly mixing multiple types of powder in a desired mixing ratio.
[0119] The preheating step is a step of preheating the substrate to a temperature of 350°C or higher, and is carried out as necessary. Preheating can be carried out, for example, by using high-frequency induction heating, a gas burner, an infrared electric heater, a heating furnace, or irradiation with an electron beam or laser. In the preheating step, it is more preferable to preheat the substrate to a temperature of 500°C or higher, and particularly preferable to preheat to a temperature of 700°C or higher. In addition, in the preheating step, from the viewpoint of preventing deformation due to its own weight, it is preferable to set the temperature of the substrate to 1300°C or lower, and more preferably 1000°C or lower.
[0120] In the preheating step, by preheating the substrate to a temperature of 350°C or higher, it is possible to suppress the occurrence of cracks and peeling between the WC-based cemented carbide shaped body and the substrate, the occurrence of microcracks in the shaped part (the cemented carbide part 310), and the like, in the subsequent additive manufacturing step. Specifically, by preheating the substrate to a certain temperature or higher in the preheating step, the temperature gradient of the WC-based cemented carbide shaped body and the substrate during additive manufacturing becomes gentle, making it possible to suppress deformation due to thermal stress and alleviate residual stress. In addition, by preheating the substrate to a temperature of 500°C or higher in the preheating step, the thermal stress is further alleviated, and it is possible to further suppress the occurrence of cracks, peeling, cracks, and the like, in the additive manufacturing step.
[0121] The obtained WC-based cemented carbide member may be subjected to a heat treatment. For example, it is preferable to perform a heat treatment at 1200°C or higher for about 0.5 to 10 hours. When the temperature is 1300°C or higher, it is preferable to perform the heat treatment in an inert gas atmosphere or in a vacuum. When the temperature is 1200°C or higher, it is preferable to perform the heat treatment using a pressurizing treatment, for example, hot isostatic pressing (HIP).
[0122] By carrying out the heat treatment, it is possible to dissolve C in W, Ti and Co contained in the WC-based cemented carbide member, and to suppress free carbon. This is expected to improve the specific strength. In addition, aging treatment may be carried out at 600°C to 900°C for 1 to 24 hours. Of course, the above heat treatment may be carried out on the WC-based cemented carbide.
[0123] The present disclosure will be described in more detail below using examples, but the present disclosure is not limited to these examples. EXAMPLES
[0124] [Preparation of WC-based cemented carbide members (No. 1-3)] The raw material powders were mixed, melted and solidified to produce a WC-based cemented carbide piece member.
[0125] The raw material powders used were WC-Co powder, WC powder, and TiB2 powder manufactured by Japan New Metals Co., Ltd., and Cu powder manufactured by Hikari Materials Industry Co., Ltd.
[0126] Table 1 shows the ratio of the raw material powders used to produce the WC-based cemented carbide members (test pieces). The numbers in the table are dimensionless.
[0127] The compositions of the WC-based cemented carbide members (test pieces) produced are shown in Table 2. The numbers in the table are in mass %.
[0128] [Table 1]
[0129] [Table 2]
[0130] [Modeling conditions] The additive manufacturing method used was directed energy deposition. The modeling conditions were an output of 1800 W and a scanning speed of 800 mm / min. The substrate used was YAG300 (manufactured by Hitachi Metals, Ltd.; YAG is a registered trademark of Hitachi Metals, Ltd.).
[0131] The structure of test specimens No. 1 to 3 of the examples shown in Tables 1 and 2 was analyzed using an EPMA. All of test specimens No. 1 to 3 correspond to alloy composition I.
[0132] The analytical conditions for each test piece are as follows: Device name: EPMA-1610 (manufactured by Shimadzu Corporation) Acceleration voltage: 15kV ·Irradiation current: 100nA Data point (X: 400, Y: 400) Beam diameter: 1μm Counting time: 20msec [result] 4 to 6 show the results of element mapping analysis by EPMA and backscattered electron images. In the figures showing the results of element mapping analysis by EPMA, areas where the concentration of an element observed in the same field of view is relatively high are shown in color, and areas where the concentration is low are shown in black.
[0133] FIG. 4 is a diagram showing the element mapping analysis results by EPMA and a backscattered electron image of the test piece No. 1 of the example.
[0134] In this figure, the distribution of boron 404 (B), carbon 406 (C), cobalt 408 (Co), copper 410 (Cu), titanium 412 (Ti), and tungsten 414 (W) is shown together with a backscattered electron image 402 (BEI). Here, the color bars shown in the lower left (next to W) of Figures 4 to 6 indicate that the concentration of the element observed in the same field of view becomes relatively higher the further up the bar.
[0135] As shown in FIG. 4, in the test piece No. 1, there are many overlapping areas where W, Ti, and C are distributed, and these overlapping areas are considered to constitute the first phase (WTiC phase), and the first phase is considered to contribute to the improvement of hardness and oxidation resistance. In addition, there are overlapping areas where B, Co, and W are distributed, and B, Co, and W form compounds and are distributed in a mass, that is, they form the second phase (WBCo phase). In addition, as a result of the element mapping analysis of Co, it was found that the coloring was dark and the Co was concentrated, that is, the third phase (Co-rich phase) was formed. In addition, it was found that Cu was distributed in a large amount in the area where the concentration of B was low. It is considered that these Cu contribute to the improvement of the thermal conductivity. In addition, there was an area where C was distributed in an area that did not overlap with the distribution of W, Ti, and Co, and it is considered that C (also called free carbon) that is not solid-dissolved is present. Regarding free carbon, for example, by performing heat treatment at 1250°C for 5 hours, C can be dissolved in W, Ti, or Co, suppressing the free carbon. This is expected to improve the specific strength of the member.
[0136] FIG. 5 is a diagram showing the element mapping analysis results by EPMA and a backscattered electron image of the test piece No. 2 of the example.
[0137] In this figure, the distribution of boron 504 (B), carbon 506 (C), cobalt 508 (Co), copper 510 (Cu), titanium 512 (Ti), and tungsten 514 (W) is shown along with a backscattered electron image 502 (BEI).
[0138] FIG. 6 is a diagram showing the element mapping analysis results by EPMA and a backscattered electron image of the test piece No. 3 of the example.
[0139] In this figure, the distribution of boron 604 (B), carbon 606 (C), cobalt 608 (Co), copper 610 (Cu), titanium 612 (Ti), and tungsten 614 (W) is shown together with a backscattered electron image 602 (BEI).
[0140] 5 and 6, as in FIG. 4, there are many overlapping areas where W, Ti, and C are distributed, and these overlapping areas are considered to constitute the first phase (WTiC phase), and the formation of the first phase is considered to contribute to the improvement of hardness and oxidation resistance. In addition, there are overlapping areas where B, Co, and W are distributed, and B, Co, and W form compounds and are distributed in clumps, that is, they form the second phase (WBCo phase). In addition, as a result of the element mapping analysis of Co, the results showed that the coloring was dark and the Co was concentrated, that is, the third phase (Co-rich phase) was formed. In addition, it was found that Cu was distributed in large amounts in the areas where the concentration of B was low. It is considered that these Cus contribute to the improvement of the thermal conductivity. In addition, there were areas where C was distributed in areas that did not overlap with the distribution of W, Ti, and Co, and it is considered that C (also called free carbon) that was not dissolved in solid solution was present. Regarding free carbon, for example, by performing heat treatment at 1250°C for 5 hours, C can be dissolved in W, Ti, or Co, suppressing the free carbon. This is expected to improve the specific strength of the member.
[0141] Table 3 shows the average value of the area ratio of the first phase for each of test pieces No. 1 to 3.
[0142] As shown in this table, the area ratio of the first phase (phase containing W, Ti, and C) is greater in No. 2 than in No. 1, and in No. 3 than in No. 2. In other words, it was confirmed that the area ratio of the first phase increases as the Ti content increases. The average area ratio was calculated by measuring three times in a measurement field of 120 μm × 120 μm.
[0143] [Table 3]
[0144] Table 4 shows the results of measuring the hardness of each of test pieces No. 1 to 3 using a Rockwell hardness tester.
[0145] As shown in this table, No. 2 is harder than No. 1, and No. 3 is harder than No. 2. In other words, it can be seen that the more Ti and B are included, the higher the hardness becomes.
[0146] [Table 4]
[0147] Hereinafter, regarding Cu, which contributes to improving thermal conductivity, the extent to which the wear resistance, which is another effect of the WC-based cemented carbide according to the present disclosure, changes due to changes in its concentration will be described.
[0148] To demonstrate this, the molecular dynamics simulation described in Non-Patent Document 1 was applied to the WC-based cemented carbide according to the present disclosure to create a stress-strain curve as shown in Figure 2 of Non-Patent Document 2. Then, the shear fracture energy was calculated from the area enclosed by the curve of the graph up to the point where the stress on the vertical axis becomes maximum, the horizontal axis, and the straight line drawn from the maximum point of the graph to the horizontal axis.
[0149] Fig. 7 is a graph showing the relationship between the shear fracture energy calculated by the above method and the Cu concentration (mass basis). In the figure, No. 1 is represented by a ● mark, No. 2 by a ■ mark, and No. 3 by a ▲ mark.
[0150] In addition, the ratios of other elements contained in the alloy when the Cu concentration is changed are set as the change in the concentration of other elements by proportional distribution of the change in Cu concentration based on the composition of each of Nos. 1 to 3. In addition, for each of Nos. 1 to 3, the shear fracture energy was normalized to be 1 when the Cu concentration was zero.
[0151] From this figure, it can be seen that when the Cu concentration is between 5% and 15%, the shear fracture energy is significantly higher than in the range where the Cu concentration is less than 5% or more than 15%, and that it is effective to have the concentration in this range. When the Cu concentration is less than 5%, although the hardness is high, it cannot be stretched as shear deformation progresses, and it shows brittle fracture, resulting in low shear fracture energy. Also, when the Cu concentration exceeds 15%, it easily deforms with low stress, so even if there is elongation, the shear fracture energy does not increase.
[0152] From the above, it can be said that the Cu concentration must be 5% or more and 15% or less.
[0153] As described above, the present disclosure has been shown to be able to provide a WC-based cemented carbide powder capable of producing a WC-based cemented carbide member having excellent thermal conductivity and wear resistance, a WC-based cemented carbide member, and a method for producing a WC-based cemented carbide member.
[0154] In addition, the present disclosure is not limited to the above-mentioned embodiment, and other forms conceivable within the scope of the technical ideas of the present disclosure are also included in the scope of the present disclosure as long as they do not deviate from the gist of the present disclosure. For example, the configurations and processes exemplified in the above-mentioned embodiment may be appropriately integrated or separated depending on the implementation form and processing efficiency. In addition, for example, the above-mentioned embodiment and modified examples may be combined in part or in whole as long as they are not inconsistent. [Explanation of symbols]
[0155] 100: mixed powder manufacturing apparatus, 110: mixing section, 112: large diameter section, 114: small diameter section, 116: space, 120, 230: piping, 132, 134: powder, 138: mixed powder, 200: additive manufacturing apparatus, 210: powder supply section, 220: carrier gas, 240: head section, 250: heat source beam, 300: WC-based cemented carbide member, 310: cemented carbide section, 320: substrate.
Claims
1. In mass percent, 10% or more and 40% or less of Co; Cu, 5% or more and 15% or less; The balance of the WC-based cemented carbide is at least one selected from the group consisting of Ti, Zr and Cr, as well as W, B, C and unavoidable impurities.
2. In molar ratio, The content of B is 1.5 to 3 times the content of Ti, 2. The WC-based cemented carbide according to claim 1, wherein the C content is 0.5 to 2 times the W content.
3. In mass percent, The Ti content is more than 0% and less than 15%; The B content is more than 0% and less than 6.0%, The W content is more than 23% and not more than 75.5%; The WC-based cemented carbide according to claim 1 or 2, wherein the C content is more than 1.5% and not more than 5%.
4. a first phase including Ti, W, and C; a second phase comprising W, B and Co; and a third phase comprising Co, The WC-based cemented carbide according to claim 3, wherein an area ratio of the first phase in cross-sectional observation is more than 0% and not more than 50%.
5. A mixed powder obtained by mixing a plurality of types of powders to produce a WC-based cemented carbide, The mixed powder for producing WC-based cemented carbide has an average composition, in mass%, of 10% to 40% Co, 5% to 15% Cu, and the remainder being at least one element selected from the group consisting of Ti, Zr, and Cr, as well as W, B, C, and unavoidable impurities.
6. A member formed of a WC-based cemented carbide, The WC-based cemented carbide member contains, by mass%, 10% to 40% Co, 5% to 15% Cu, and the balance consisting of at least one element selected from the group consisting of Ti, Zr, and Cr, as well as W, B, C, and unavoidable impurities.
7. 7. The WC-based cemented carbide member according to claim 6, having a hardness of 45 HRC or more and a thermal conductivity of 10 W / (m·K) or more.
8. A substrate; A cemented carbide portion formed on a surface of the substrate, The cemented carbide portion is formed of a WC-based cemented carbide, The WC-based cemented carbide member contains, by mass%, 10% to 40% Co, 5% to 15% Cu, and the balance consisting of at least one element selected from the group consisting of Ti, Zr, and Cr, as well as W, B, C, and unavoidable impurities.
9. A melting and solidifying step of irradiating the mixed powder with a heat source beam to melt the mixed powder and then solidifying the melted and solidified powder, a WC-based cemented carbide member having an average composition, in mass%, of components constituting the mixed powder containing, 10% to 40% Co, 5% to 15% Cu, and the remainder being at least one element selected from the group consisting of Ti, Zr, and Cr, as well as W, B, C, and unavoidable impurities.
10. a powder mixing step of individually pumping and mixing a plurality of types of powder together with a carrier gas to obtain the mixed powder; The method for producing a WC-based cemented carbide member according to claim 9, further comprising a mixed powder supplying step of supplying the mixed powder.
Citation Information
Patent Citations
Surface-coated cutting tool made of WC-based cemented carbide excellent in thermal plastic deformation resistance
JP2011156645A
WC-based cemented carbide and production method therefor
JP2016160500A
Super hard alloy and manufacturing method therefor
JP2019151873A
WC-based super-hard alloy powder, WC-based super-hard alloy member, and method for producing WC-based super-hard alloy member
WO2021039912A1