Copper alloy powder for metal AM and manufacturing method for additive manufacturing
The copper alloy powder with CrSi-based and NiSi-based compounds addresses the instability in metal AM by improving laser absorption and uniformity, resulting in high-quality, defect-free additively manufactured products with enhanced properties.
Patent Information
- Application Number
- JP2024506145
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2022-10-24
- Filing Date
- 2023-10-24
- Publication Date
- 2024-10-08
- Estimated Expiration
- 2043-10-24
AI Technical Summary
Metal structures formed by metal AM using copper alloys often suffer from non-uniform microstructures, voids, and thermomechanical and electrical reliability issues due to unstable melting behavior caused by high reflectance and electromagnetic wave absorption characteristics, leading to poor productivity and quality.
A copper alloy powder with optimized compositions containing Cr, Si, and Ni, featuring CrSi-based and NiSi-based compounds precipitated at the grain boundaries, which enhances laser absorption and reduces impurities, resulting in a uniform microstructure and reduced voids.
The copper alloy powder ensures high-quality, high-reproducibility additively manufactured products with improved thermal, electrical, and mechanical properties, and reduced structural defects such as voids, enhancing productivity and stability.
Smart Images

Figure 0007563652000004 
Figure 0007563652000005 
Figure 0007563652000006
Abstract
Description
[Technical field]
[0001] The present invention relates to copper alloy powder for metal additive manufacturing (metal AM), which is optimal for metal AM technology, and a manufacturing method for additively manufactured objects. This application claims priority based on Japanese Patent Application No. 2022-169922, filed on October 24, 2022, the contents of which are incorporated herein by reference. [Background technology]
[0002] In recent years, metal AM technology, which mainly uses powder as the raw material to create products using a metal 3D printer, has been put to practical use as a method for manufacturing metal parts with various three-dimensional shapes. The main metal AM technologies that use metal powder include powder bed fusion (PBF) using electron beams or laser light, and the binder jet method. Copper alloys have many basic properties suitable for industrial applications, such as electrical conductivity, thermal conductivity, mechanical properties, wear resistance, and heat resistance, and are used as materials for various components. In recent years, attempts have been made to form components of various shapes by metal AM using copper alloy powder in various fields such as space and electrical component applications, and there is a growing need for copper and copper alloy parts manufactured by metal AM.
[0003] For example, Patent Document 1 proposes a technique for producing an additive manufacturing object by metal AM using a copper alloy powder containing either Cr or Si. Moreover, Patent Document 2 proposes a technique for producing an additive manufacturing object by metal AM using a copper alloy powder containing Cr and Zr. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2016-211062 A [Patent Document 2] JP 2019-070169 A [Non-patent literature]
[0005] [Non-Patent Document 1] YM Arisoy et. al., "Influence of scan strategy and process parameters on microstructure and its optimization in additively manufactured nickel alloy 625 via laser powder bed fusion", The International Journal of Advanced Manufacturing Technology, Volume 90, pp 1393-1417 (2017). Summary of the Invention [Problem to be solved by the invention]
[0006] Metal structures created by metal AM are used as structural components for a variety of applications, so if voids are present in the additively manufactured body or if the microstructure of the metal material is uneven, this can cause problems in terms of thermomechanical and electrical reliability. Currently, the most commonly used building method for metal AM is laser PBF, and attempts have also been made to use laser PBF for copper and copper alloys. Incidentally, when performing additive manufacturing using a method of irradiating a laser beam or an electron beam, a thin layer of powder is first formed (powder bed), and then this powder bed is locally irradiated with a laser or an electron beam to melt and solidify the material. However, in the case of copper and copper alloys, compared to other metal materials such as iron, titanium, and nickel, copper itself has a high reflectance in the visible and infrared ranges, which causes the melting behavior of the copper alloy powder to become unstable during the laser PBF process, and voids are likely to occur inside the additively manufactured object, resulting in a number of issues such as unstable quality of the object manufactured by laser PBF and poor productivity, and there is a demand for improvements in the productivity and quality of copper and copper alloys manufactured by laser PBF.
[0007] Currently, the most widely used form of raw material for metal AM is powder. For example, in metal AM using laser PBF, the electromagnetic wave absorption characteristics of the particles due to the coupling and interaction between the surface layer of the particles constituting the raw material powder and the electromagnetic wave affect the melting behavior of the raw material powder, and greatly affect the productivity of the parts and the quality including the defect density of the parts. For example, in a metal AM process using a powder bed, the thickness of the powder bed formed in one lamination process is, for example, about several tens of μm (Non-Patent Document 1), and the raw material powder is melted by irradiating such a relatively thin powder bed with converged electromagnetic waves, and the desired molded structure is realized by repeating numerous laminations and melting and solidification. The electromagnetic wave absorption characteristics of solids have a significant effect on the elementary process of such additive manufacturing using a powder bed. For example, since the electromagnetic wave absorption characteristics of solids are affected by the material composition, it is extremely important to increase the uniformity of the material composition and microstructure of the powder in order to achieve stable quality and high productivity in the entire additive manufacturing product.
[0008] Here, the electromagnetic wave absorption characteristics of copper and copper alloys can be improved, for example, by simply adding a substance with a high absorption rate of the target laser wavelength as a component other than copper. However, as many past metallurgical studies have shown, when copper and copper alloys are used for a certain application, the properties required for that application can only be realized by appropriately selecting the type and amount of elements added to copper. Therefore, in order to improve the productivity and quality of metal AM objects made of copper or copper alloys, in other words, to improve the laser absorption of raw powders of copper or copper alloys, a simple approach such as adding various foreign elements with high laser absorption rates to copper or copper alloys of optimized composition or increasing the amount of such elements may deteriorate the performance of copper alloys required for various applications. Therefore, it has been required to realize copper alloy powders for metal AM with improved laser absorption characteristics while maintaining a material composition that can fully ensure the performance of copper alloys required for various applications.
[0009] One important approach to improve the laser absorption properties of powders is to improve the laser absorption ability of each particle by surface modification of the particle surface that constitutes the powder. For this surface modification, it is possible to apply a coating of a substance that has a high absorption rate at the laser wavelength used in metal AM to the surface of each particle of the powder having the desired copper alloy composition. As an approach to coating the particle surface, a desired coating material can be formed on the particle surface using a wet or gas phase process. However, such a coating process is accompanied by problems such as the control of the thickness of the coating layer on each particle, as well as the reproducibility of the coating thickness and the homogeneity of the coating material throughout the powder, resulting in a number of issues in the productivity and quality of the molded object.
[0010] In addition, as a result of various past research and development efforts, copper alloy materials that achieve high mechanical strength while maintaining high electrical conductivity, as well as materials with excellent heat resistance, have already been developed, and in metal AM, there is a societal demand to use such existing high-performance copper alloy materials to create metal AM parts with desired shapes. However, controlling the amount of components in the material formed by coating while also controlling the material composition of the copper alloy of the final product not only places a significant burden on the manufacturing process, but there were concerns that it would result in a number of major problems, such as deterioration of the performance of the molded parts due to variations in composition and microstructure, deterioration of mass producibility of parts, and issues with maintaining the quality of the parts.
[0011] Furthermore, one of the factors that can cause structural defects in metal AM objects is the generation of voids due to the entrapment of gas, etc. When conventional copper alloy powder is used for additive manufacturing by the PBF method, gas is generated due to impurities contained in the copper alloy powder when the powder is melted, and the molten copper alloy or solidified copper alloy traps the gas components, which can cause voids to form inside the additive manufactured object, making it difficult to stably produce high-quality additive manufactured objects.
[0012] Furthermore, when additive manufacturing is performed by irradiating a powder bed of the raw material with laser light or an electron beam, if there is a lack of reproducibility of the microstructure of the raw material powder, including the reproducibility of the composition of the powder particles at each location irradiated with the laser light, the melting behavior of the powder will be non-uniform, which could result in the occurrence of structural defects such as voids inside the molded object or a deterioration of the mechanical properties due to non-uniformity in the metal composition of the molded object.
[0013] In addition, the reproducibility of the microstructure of the raw material powder, including the reproducibility of the powder's material composition, is a similar problem to other metal AM methods such as the binder jet method. In metal AM of copper alloys, improving productivity has been a major challenge due to the issues with the various raw materials.
[0014] The present invention has been made in consideration of the above-mentioned circumstances, and aims to provide a copper alloy powder for metal AM that can stably produce high-quality additively molded objects with high reproducibility of the microstructure of objects created by metal AM and few structural defects such as voids, and a method for manufacturing additively molded objects. [Means for solving the problem]
[0015] From the above viewpoints, the present inventors have conducted research and development to produce copper alloy powder that has the copper alloy composition required for practical applications and can be used to produce high-performance, high-quality copper alloy parts with high productivity using a metal AM process. As a result, when a high-purity copper alloy is used as a raw material and a powdering process is performed, it has been found that while the copper alloy powder as a whole has few impurities and maintains a uniform composition, when focusing on the individual particle surfaces in the copper alloy powder, a thin layer is formed on the copper alloy particle surface to be irradiated with a laser. Furthermore, it has been found that a characteristic structure in which powder constituent elements that exhibit higher laser absorption than copper are frequently present in the thin layer formed on the copper alloy particle surface compared to the inside of the bulk copper alloy particle is spontaneously generated in a direct powdering process from the copper alloy raw material without going through an individual coating process or an additional process on the powder. In addition to these structural features of the copper alloy particle surface, the copper alloy powder is derived from high-purity copper alloy raw materials, which means that it contains fewer impurities that lead to gas components, thereby suppressing gas generation during melting.This makes it possible to realize dense copper alloy bodies that have high thermal, electrical, and mechanical properties, and it has been discovered that it is possible to manufacture copper alloy powder for metal AM that can achieve high productivity and high quality of copper alloy bodies that exhibit such high performance.
[0016] Specifically, when copper alloy powder is manufactured using a copper alloy ingot containing Cr, Ni, and Si with sufficiently reduced impurity content as a raw material, it was found that CrSi-based compounds are uniformly precipitated at the copper crystal grain boundaries of the copper alloy particles that make up the powder. It was also found that when this powder is used for additive manufacturing, it is possible to reduce the occurrence of structural defects such as voids.
[0017] The present invention has been made based on the above-mentioned findings, and a copper alloy powder for metal AM according to a first aspect of the present invention is a copper alloy powder for metal AM used in metal AM, As an alloying elementThe copper alloy powder is made of a copper alloy containing Cr, Si, and Ni, with the Cr content being within the range of 0.1% by mass to 0.8% by mass, the Si content being within the range of 0.4% by mass to 0.8% by mass, the Ni content being within the range of 1.8% by mass to 3.0% by mass, and the remainder being copper and impurities. The copper alloy powder is characterized in that either or both of a CrSi-based compound containing Cr and Si and a NiSi-based compound containing Ni and Si are precipitated at the copper crystal grain boundaries on the surfaces of the copper alloy particles constituting the copper alloy powder. Additive elements and impurity elements other than the above alloying elements are It may contain at least one element selected from the group consisting of Zr, Mg, Ti, Al, Zn, Ca, Sn, Pb, Fe, Mn, Te, Nb, P, Co, Sb, Bi, Ag, Ta, W and Mo in a total amount of 0.07 mass% or less.
[0018] The copper alloy powder for metal AM of embodiment 1 of the present invention is made of a copper alloy containing Cr, Si, and Ni, and either or both of CrSi-based compounds containing Cr and Si and NiSi-based compounds containing Ni and Si are precipitated at the copper crystal grain boundaries on the surface of the copper alloy particles that make up the copper alloy powder. This makes it possible to stably produce high-quality additive manufacturing objects with high reproducibility of the microstructure of objects produced by metal AM and with few structural defects such as voids.
[0019] In a second aspect of the present invention, in the copper alloy powder for metal AM of the first aspect, it is preferable that either one or both of the CrSi-based compound and the NiSi-based compound are precipitated on copper crystal grains on the surfaces of the copper alloy particles constituting the copper alloy powder. According to the copper alloy powder for metal AM of aspect 2 of the present invention, either one or both of the CrSi-based compounds and the NiSi-based compounds are precipitated on the copper crystal grains on the surfaces of the copper alloy particles that make up the copper alloy powder, which makes it possible to more reproducibly produce the microstructure of a molded object produced by metal AM and to more stably produce high-quality additively molded objects with fewer structural defects such as voids.
[0020] In a third aspect of the present invention, in the copper alloy powder for metal AM of the first or second aspect, it is preferable that a layer containing either one or both of the CrSi-based compound and the NiSi-based compound is formed on the particle surface of the copper alloy powder. According to the copper alloy powder for metal AM of aspect 3 of the present invention, a layer containing either or both of the CrSi-based compound and the NiSi-based compound is formed on the particle surface of the copper alloy powder, so that the microstructure of a molded object produced by metal AM is highly reproducible and has fewer structural defects such as voids, making it possible to stably produce high-quality additive manufacturing objects.
[0021] In a fourth aspect of the present invention, in the copper alloy powder for metal AM of the third aspect, it is preferable that a layer containing either one or both of the CrSi-based compound and the NiSi-based compound formed on the particle surface of the copper alloy powder contains oxygen. According to the copper alloy powder for metal AM of aspect 4 of the present invention, the layer containing either or both of the CrSi-based compound and the NiSi-based compound on the particle surface contains oxygen, which makes it possible to suppress deterioration of the powder, and enables the stable production of high-quality additive manufacturing objects with high reproducibility of the microstructure of the objects produced by metal AM and with fewer structural defects such as voids.
[0022] In a fifth aspect of the present invention, in the copper alloy powder for metal AM according to any one of the first to fourth aspects, it is preferable that, upon cross-sectional observation of copper alloy particles constituting the copper alloy powder, either one or both of the CrSi-based compound and the NiSi-based compound are distributed at the copper crystal grain boundaries. According to the copper alloy powder for metal AM of aspect 5 of the present invention, when a cross-sectional observation of a particle constituting the copper alloy powder is performed, either one or both of the CrSi-based compounds and the NiSi-based compounds are distributed at the copper crystal grain boundaries, making it possible to produce an additive manufacturing object having excellent electrical conductivity, thermal conductivity, and strength.
[0023] A sixth aspect of the present invention is a copper alloy powder for metal AM according to any one of the first to fifth aspects, wherein the copper alloy contains Cr in the range of 0.1% by mass to 0.8% by mass, Si in the range of 0.4% by mass to 0.8% by mass, Ni in the range of 1.8% by mass to 3.0% by mass, and the remainder is copper and impurities. According to the copper alloy powder for metal AM of aspect 6 of the present invention, the copper alloy constituting the copper alloy powder for metal AM has the above-mentioned composition. Therefore, by subjecting an additive manufacturing object produced using the copper alloy powder for metal AM to an appropriate heat treatment, compounds can be precipitated, making it possible to produce an additive manufacturing object with excellent electrical conductivity, thermal conductivity, and strength.
[0024] In a seventh aspect of the present invention, in the copper alloy powder for metal AM according to any one of the second to sixth aspects, the CrSi-based compound preferably contains Cr3Si. According to the copper alloy powder for metal AM of aspect 7 of the present invention, the CrSi-based compound contains Cr3Si, so that the microstructure of a structure produced by metal AM is highly reproducible, and it is possible to stably produce high-quality additively manufactured objects with fewer structural defects such as voids.
[0025] In an eighth aspect of the present invention, in the copper alloy powder for metal AM of any one of the second to seventh aspects, the NiSi-based compound preferably contains Ni5Si2. According to the copper alloy powder for metal AM of aspect 8 of the present invention, since the NiSi-based compound contains Ni5Si2, the microstructure of the object produced by metal AM is highly reproducible, and it is possible to stably produce high-quality additively manufactured objects with fewer structural defects such as voids.
[0026] In a ninth aspect of the present invention, in the copper alloy powder for metal AM according to any one of the first to eighth aspects, it is preferable that the volume-based 50% cumulative particle diameter D50 measured by a laser diffraction / scattering method is in the range of 5 μm or more and 120 μm or less. According to the copper alloy powder for metal AM of embodiment 9 of the present invention, the volume-based 50% cumulative particle diameter D50 measured by a laser diffraction / scattering method is in the range of 5 μm or more and 120 μm or less, so that it has a particle size distribution suitable for metal AM and enables the stable production of additive manufacturing objects.
[0027] In a tenth aspect of the present invention, in the copper alloy powder for metal AM according to any one of the first to ninth aspects, it is preferable that the volume-based 10% cumulative particle diameter D10 measured by a laser diffraction / scattering method is in the range of 1 μm or more and 80 μm or less. According to the copper alloy powder for metal AM of aspect 10 of the present invention, the volume-based 10% cumulative particle diameter D10 measured by a laser diffraction / scattering method is in the range of 1 μm or more and 80 μm or less, so that it has a particle size distribution suitable for metal AM and enables the stable production of additive manufacturing objects.
[0028] In an eleventh aspect of the present invention, in the copper alloy powder for metal AM according to any one of the first to tenth aspects, it is preferable that the volume-based 90% cumulative particle diameter D90 measured by a laser diffraction / scattering method is in the range of 10 μm or more and 150 μm or less. According to the copper alloy powder for metal AM of aspect 11 of the present invention, the volume-based 90% cumulative particle diameter D90 measured by a laser diffraction / scattering method is in the range of 10 μm or more and 150 μm or less, so that it has a particle size distribution suitable for metal AM and enables the stable production of additive manufacturing objects.
[0029] The manufacturing method of an additively molded object of aspect 12 of the present invention is characterized by comprising a preparation step of preparing a copper alloy powder for metal AM of any one of aspects 1 to 11, a first step of forming a powder bed containing the copper alloy powder for metal AM, and a second step of melting and solidifying the copper alloy powder for metal AM at a predetermined position in the powder bed to form a molded object, and a molding step of producing an additively molded object by sequentially repeating these steps.
[0030] According to the manufacturing method for an additive manufacturing object of aspect 12 of the present invention, since the copper alloy powder for metal AM of any one of aspects 1 to 11 is used, it is possible to stably manufacture high-quality additive manufacturing objects with high reproducibility of the microstructure of the object produced by metal AM and with few structural defects such as voids.
[0031] A thirteenth aspect of the present invention is preferably such that, in the method for manufacturing an additive manufacturing object according to the twelfth aspect, it further comprises a heat treatment step of performing a heat treatment at a temperature range of 300° C. or higher and lower than the melting point of pure copper after the manufacturing step. By carrying out an appropriate heat treatment according to the application of the produced additive manufacturing product, it is possible to control the microstructure of the molded copper alloy, and it is possible to realize the desired mechanical properties and conductive properties. By carrying out a heat treatment within the temperature range of the manufacturing method of the additive manufacturing product of the thirteenth aspect of the present invention, a copper alloy molded body with an appropriately controlled microstructure is realized.
[0032] Aspect 14 of the present invention is preferably such that, in the manufacturing method of an additive manufacturing method of aspect 12, it further comprises a first heat treatment step in which heat treatment is performed after the molding step in a temperature range of 800°C or higher and lower than the melting point of pure copper, and a second heat treatment step in which heat treatment is performed after the first heat treatment in a temperature range of 300°C or higher and lower than 800°C. By carrying out a two-step heat treatment under such temperature conditions, it is possible to realize a copper alloy having a desired microstructure. Effect of the Invention
[0033] According to the present invention, it is possible to provide a copper alloy powder for metal AM that can stably produce high-quality additively molded objects with high reproducibility of the microstructure of objects produced by metal AM and few structural defects such as voids, and a method for manufacturing additively molded objects. [Brief description of the drawings]
[0034] [Figure 1] FIG. 1 is a schematic explanatory diagram of a copper alloy particle that constitutes the copper alloy powder for metal AM of the present embodiment. [Figure 2A]This is a secondary electron image, which is the result of an Auger electron spectroscopy analysis of the particle surface of a copper alloy particle constituting the copper alloy powder for metal AM of this embodiment, after etching for 15 minutes from the outermost surface of the particle. [Figure 2B] This is the result of an Auger electron spectroscopy analysis of the particle surface of a copper alloy particle constituting the copper alloy powder for metal AM of this embodiment, after etching for 15 minutes from the outermost surface of the particle, and is a Cr mapping image. [Figure 2C] FIG. 1 shows the results of an Auger electron spectroscopy analysis of the particle surface of a copper alloy particle constituting the copper alloy powder for metal AM of this embodiment, after etching for 15 minutes from the outermost surface of the particle, and is a Si mapping image. [Figure 2D] This is an Auger electron spectroscopy analysis of the particle surface of a copper alloy particle constituting the copper alloy powder for metal AM of this embodiment, after etching for 15 minutes from the outermost surface of the particle, and is a Ni mapping image. [Figure 2E] This is the result of Auger electron spectroscopy analysis of the particle surface of a copper alloy particle constituting the copper alloy powder for metal AM of this embodiment, after 15 minutes of etching from the outermost surface of the particle, and is a composite element mapping image. [Figure 3A] This is the result of an Auger electron spectroscopy analysis of the particle surface of a copper alloy particle constituting the copper alloy powder for metal AM of this embodiment, and is a secondary electron image of the outermost particle surface before etching. [Figure 3B] This is an Auger electron spectroscopy analysis of the particle surface of the copper alloy particles constituting the copper alloy powder for metal AM according to the present embodiment, and is a Cr mapping image of the outermost particle surface before etching. The arrows indicate the presence of Cr-based precipitates on the copper crystal particles. [Figure 3C] This is an Auger electron spectroscopy analysis of the particle surface of the copper alloy particles constituting the copper alloy powder for metal AM according to the present embodiment, and is a Cr mapping image of the particle surface after etching for 5 minutes from the outermost particle surface. The arrows indicate the presence of Cr-based precipitates on the copper crystal particles. [Figure 3D]This is an Auger electron spectroscopy analysis of the particle surface of the copper alloy particles constituting the copper alloy powder for metal AM according to the present embodiment, and is a Cr mapping image of the particle surface after etching for 15 minutes from the outermost particle surface. The arrows indicate the presence of Cr-based precipitates on the copper crystal particles. [Figure 3E] This is the result of an Auger electron spectroscopy analysis of the particle surface of a copper alloy particle constituting the copper alloy powder for metal AM of this embodiment, and is a Cr mapping image of the particle surface after etching for 30 minutes from the outermost particle surface. [Figure 3F] This is the result of an Auger electron spectroscopy analysis of the particle surface of a copper alloy particle constituting the copper alloy powder for metal AM of this embodiment, and is a Cr mapping image of the particle surface after etching for 50 minutes from the outermost particle surface. [Figure 4] 1 is an example of intensity depth profiles of oxygen, copper, chromium, and silicon by Auger electron spectroscopy analysis of the particle surface of a copper alloy powder for metal AM according to this embodiment. [Figure 5A] 1 is a secondary electron image showing the results of Auger electron spectroscopy analysis of a particle cross-section of the copper alloy powder for metal AM according to the present embodiment. [Figure 5B] 1 is a result of Auger electron spectroscopy analysis of a particle cross-section of the copper alloy powder for metal AM of this embodiment, and is an element mapping image of Cr. [Figure 5C] 1 is a result of Auger electron spectroscopy analysis of a particle cross section of the copper alloy powder for metal AM according to the present embodiment, and is an element mapping image of Ni (the arrow indicates the position of Ni). [Figure 5D] 1 is a result of Auger electron spectroscopy analysis of a particle cross-section of the copper alloy powder for metal AM of this embodiment, and is an element mapping image of Si. [Figure 6] FIG. 1 is a flow diagram of a method for producing a copper alloy powder for metal AM according to the present embodiment. [Figure 7] FIG. 1 is a schematic explanatory diagram of a continuous casting device used when producing the copper alloy powder for metal AM according to the present embodiment. [Figure 8] FIG. 2 is a flow diagram of a method for manufacturing a layered object according to the present embodiment. [Figure 9]FIG. 2 is a schematic explanatory diagram of another continuous casting device used when producing a copper alloy powder for metal AM according to an embodiment. [Figure 10] FIG. 1 shows an example of an analysis result of the particle surface of the copper alloy powder for metal AM according to the present embodiment, using high-angle annular dark field scanning transmission electron microscopy (HAADF-STEM), in which (A) shows a HAADF image, (B) shows Cu mapping, (C) shows Si mapping, and (D) shows Cr mapping. [Figure 11] These are the results of electron diffraction analysis using a transmission electron microscope of the particle surface of the copper alloy powder for metal AM of this embodiment, in which (A) is a bright-field image, (B) is the electron diffraction pattern of the Cu portion (Cu[1-10]), and (C) is the electron diffraction pattern of the CrSi-based compound derived from the CrSi-based precipitates (Cr3Si[01-2]). DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0035] Hereinafter, a copper alloy powder for metal AM according to one embodiment of the present invention will be described with reference to the attached drawings. The copper alloy powder for metal AM of this embodiment is a copper alloy powder used for metal AM. Note that the copper alloy powder for metal AM of this embodiment is particularly suitable for the PBF method using a laser.
[0036] The copper alloy powder for metal AM of this embodiment is an aggregate of particles composed of a copper alloy containing Cr, Si, and Ni, and either or both of a CrSi-based compound containing Cr and Si and a NiSi-based compound containing Ni and Si are precipitated at the copper crystal grain boundaries on the surface of the copper alloy particles that constitute the copper alloy powder for metal AM. In the copper alloy powder for metal AM according to the present embodiment, it is preferable that either or both of a CrSi-based compound containing Cr and Si and a NiSi-based compound containing Ni and Si are precipitated on the copper crystal grains on the surfaces of the copper alloy particles constituting the copper alloy powder. In this embodiment, the surface (particle surface) (or surface layer) of the copper alloy particle of the copper alloy powder for metal AM refers to a region from the outermost surface of the particle to a depth of 100 nm.
[0037] In addition, in the copper alloy particle 50 of the copper alloy powder for metal AM of this embodiment, a CrSiNi-containing layer 52 containing either or both of a CrSi-based compound and a NiSi-based compound is formed on the particle surface. That is, in the copper alloy particle 50 of the copper alloy powder for metal AM of this embodiment, as shown in FIG. 1, it is preferable that the particle body 51 is made of a copper alloy containing Cr, Ni, and Si, and the outer surface (or surface layer) of the particle body 51 is provided with a CrSiNi-containing layer 52 containing either or both of a CrSi-based compound containing Cr and Si and a NiSi-based compound containing Ni and Si.
[0038] Specific examples of CrSi-based compounds contained in the CrSiNi-containing layer 52 include Cr3Si, etc. Specific examples of NiSi-based compounds contained in the CrSiNi-containing layer 52 include Ni5Si2, etc. Thus, the CrSiNi-containing layer 52 can contain either or both of Cr3Si and Ni5Si2.
[0039] The CrSiNi-containing layer 52 may contain a copper alloy containing Cr, Si, and Ni and an oxide of the copper alloy, in addition to the CrSi-based compound and the NiSi-based compound. The oxide may be an oxide of Cr, Si, or Ni. The oxide may be formed when the copper alloy powder for metal AM is exposed to an oxygen-containing atmosphere or a moisture-containing atmosphere.
[0040] In addition, the thickness of the CrSiNi-containing layer 52 on the particle surface of the copper alloy powder for metal AM is preferably 1 nm or more and 100 nm or less. More specifically, the thickness of the CrSiNi-containing layer 52 is preferably 1 nm or more, and may be 5 nm or more, 10 nm or more, 20 nm or more, 30 nm or more, or 50 nm or more. Also, the thickness of the CrSiNi-containing layer 52 is preferably 100 nm or less, and may be 95 nm or less, 90 nm or less, 80 nm or less, or 70 nm or less.
[0041] The CrSiNi-containing layer 52 is preferably a layer disposed on the outer circumferential surface (or surface layer) of the particle body 51, and contains either or both of a CrSi-based compound containing Cr and Si and a NiSi-based compound containing Ni and Si. In the CrSiNi-containing layer 52, the CrSi-based compound and / or the NiSi-based compound may be contained in the CrSiNi-containing layer 52 as dot-shaped precipitates uniformly or non-uniformly dispersed in the CrSiNi-containing layer 52. In the CrSiNi-containing layer 52, the CrSi-based compound and / or the NiSi-based compound may be contained in the CrSiNi-containing layer 52 as aggregated precipitates forming a plurality of amorphous island shapes (amorphous aggregates) uniformly or non-uniformly dispersed in the CrSiNi-containing layer 52. The CrSi-based compound and / or NiSi-based compound may be precipitated along the copper crystal grain boundaries on the surface of the particle body 51 .
[0042] In the CrSiNi-containing layer 52, the CrSi-based compound and / or NiSi-based compound may be precipitated so as to continuously cover the outer peripheral surface (or surface layer) of the particle body 51. In this case, the entire outer peripheral surface of the particle body 51 may be covered with the CrSi-based compound and / or NiSi-based compound, or a part of the outer peripheral surface (or surface layer) (e.g., 50% or more of the outer peripheral surface) may be continuously covered. Note that a part of the outer peripheral surface (or surface layer) of the particle body 51 (e.g., 50% or more of the outer peripheral surface) may be discontinuously (or in an island shape) covered.
[0043] The thickness of the CrSiNi-containing layer 52 can be calculated from the time until the intensity (cps) of chromium (Cr) and / or silicon (Si) stops decreasing or becomes equal to or less than a predetermined value by etching the surface of the copper alloy particle 50 of the copper alloy powder for metal AM under the standard etching conditions of an ion etching method at an etching rate of 1.08 nm / min, and analyzing the surface of the copper alloy particle 50 of the copper alloy powder for metal AM by Auger electron spectroscopy using a scanning Auger electron spectrometer PHI700xi manufactured by ULVAC-PHI, Inc. to obtain a Cr mapping image showing CrSi-based compounds and a Si mapping image showing NiSi-based compounds. Intensity depth profiles of chromium (Cr) and / or silicon (Si) (graph showing the relationship between intensity and etching time shown in FIG. 4) are obtained, and the intensity (cps) of chromium (Cr) and / or silicon (Si) stops decreasing or becomes equal to or less than a predetermined value. That is, it can be calculated as follows: time (min) until the chromium (Cr) and silicon (Si) intensities (cps) no longer decrease or become equal to or below a predetermined value × etching rate under standard conditions 1.08 nm / min = thickness of the CrSiNi-containing layer 52.
[0044] 2A to 2E, as an example, a particle body 51 of a copper alloy particle 50 of the copper alloy powder for metal AM according to this embodiment is polycrystalline, and it is confirmed that either or both of a CrSi-based compound containing Cr and Si and a NiSi-based compound containing Ni and Si are dispersed on the surface of the particle body 51. Note that either or both of a CrSi-based compound containing Cr and Si and a NiSi-based compound containing Ni and Si are dispersed both at the copper crystal grain boundaries and on the copper crystal grains (copper crystal grain surfaces).
[0045] In this embodiment, it is preferable that the diameter or major axis along the particle surface of the CrSi-based compound derived from the Cr-based precipitates and / or the NiSi-based compound derived from the Ni-based precipitates present in the CrSiNi-containing layer 52 is within the range of 1 nm or more and 1000 nm or less. The upper limit of the diameter or major axis along the particle surface of the CrSi-based compound and / or NiSi-based compound may be 800 nm or less, 500 nm or less, 300 nm or less, 100 nm or less, or 80 nm or less. The lower limit of the diameter or major axis along the particle surface of the CrSi-based compound and / or NiSi-based compound may be 5 nm or more, or 10 nm or more, and the upper limit may be 90 nm or less, or 80 nm or less.
[0046] Moreover, as shown in Figures 2A to 2E and 11, the particle body 51 of the copper alloy particle 50 of the copper alloy powder for metal AM of this embodiment is polycrystalline, and it is confirmed that Cr3Si containing Cr and Si is formed on the surface of the particle body 51. In this embodiment, it is preferable that the diameter or major axis along the particle surface of Cr3Si originating from the Cr-based precipitates present in the CrSiNi-containing layer 52 is within the range of 1 nm or more and 1000 nm or less. The upper limit of the diameter or major axis of Cr3Si derived from Cr-based precipitates along the particle surface may be 800 nm or less, 500 nm or less, 300 nm or less, 100 nm or less, or 80 nm or less. The lower limit of the diameter or major axis of Cr3Si derived from Cr-based precipitates along the particle surface may be 5 nm or more, or 10 nm or more, and the upper limit may be 90 nm or less, or 80 nm or less.
[0047] In detail, the diameter or major axis along the particle surface of the CrSi-based compound and / or NiSi-based compound is the diameter or major axis of each aggregate of precipitates of the CrSi-based compound and / or NiSi-based compound along the outer peripheral surface of the particle body 51 when the CrSi-based compound and / or NiSi-based compound are dispersed in dot shapes or amorphous island shapes (island shapes) on the outer peripheral surface of the particle body 51, and can be measured from an image obtained by analyzing the outer peripheral surface of the particle body 51 by Auger electron spectroscopy using a scanning Auger electron spectrometer PHI700xi manufactured by ULVAC-PHI, Inc.
[0048] Furthermore, when precipitates derived from CrSi-based compounds and / or NiSi-based compounds are dispersed on the surface of the particle body 51 of the copper alloy particle 50 of the copper alloy powder for metal AM of this embodiment, the density of the precipitates derived from the CrSi-based compounds and / or each NiSi-based compound in the CrSiNi-containing layer 52 is preferably such that an area ratio of 15% or more can be observed at any point on the outermost surface of the CrSiNi-containing layer 52, and an area ratio of 20% or more can be observed at any point.
[0049] The density of precipitates derived from CrSi-based compounds and / or each NiSi-based compound in the CrSiNi-containing layer 52 was measured by analyzing the outermost surface of the CrSiNi-containing layer 52 by Auger electron spectroscopy using a scanning Auger electron spectrometer PHI700xi manufactured by ULVAC-PHI, Inc., and measuring the density of precipitates derived from CrSi-based compounds and / or each NiSi-based compound in the CrSiNi-containing layer 52 by measuring the density of precipitates derived from each NiSi-based compound within a range of 1 μm. 2 The area occupancy of the CrSi-based compound and / or each NiSi-based compound can be calculated from the size and number of precipitates of the CrSi-based compound and / or each NiSi-based compound per one piece.
[0050] When the precipitates derived from the CrSi-based compound and / or each NiSi-based compound in the CrSiNi-containing layer 52 are precipitated along the copper grain boundaries on the surface of the particle body 51, and when the surface of the particle body 51 is observed using Auger electron spectroscopy, the copper grain boundaries can be seen as lines. In this case, the density (linear density) of the precipitates derived from the CrSi-based compound and / or each NiSi-based compound per unit length of the copper grain boundaries can be obtained. The outermost surface of the CrSiNi-containing layer 52 may be analyzed by Auger electron spectroscopy using a scanning Auger electron spectrometer PHI700xi manufactured by ULVAC-PHI, Inc., and the copper crystal grain boundaries may be observed in an image, and the linear density per 1 μm of grain boundary length may be calculated from the proportion of precipitates of CrSi-based compounds and / or NiSi-based compounds per 1 μm of grain boundary length. In this case, it is preferable to observe a portion where the linear density is 30% or more.
[0051] In addition, in the copper alloy particles 50 of the copper alloy powder for metal AM of this embodiment, it is preferable that the CrSiNi-containing layer 52 on the particle surface of the copper alloy powder for metal AM contains oxygen. That is, in the copper alloy particle 50 of the copper alloy powder for metal AM of this embodiment, as shown in FIG. 1, it comprises a particle body 51 made of a copper alloy containing Cr, Si, and Ni, and a CrSiNi-containing layer 52 formed on the outer peripheral surface of the particle body 51, and it is preferable that the CrSiNi-containing layer 52 contains oxygen.
[0052] In addition, the copper alloy constituting the copper alloy particles 50 of the copper alloy powder for metal AM of this embodiment preferably contains, as alloy elements, Cr in the range of 0.1 mass% to 0.8 mass%, Si in the range of 0.4 mass% to 0.8 mass%, Ni in the range of 1.8 mass% to 3.0 mass%, and the rest is copper and impurities. That is, the copper alloy constituting the copper alloy particles 50 of the copper alloy powder for metal AM of this embodiment has a composition equivalent to C18000. In this embodiment, the alloy elements refer to Cr, Si, and Ni. The impurities referred to here are components including impurity elements described below as well as O, H, S, and N. In addition, in the composition of the copper alloy constituting the copper alloy particles 50 of the copper alloy powder for metal AM, the numerical accuracy error is ±10% (excluding O, H, S, and N).
[0053] The lower limit of the Cr content is more preferably 0.2 mass% or more, and even more preferably 0.3 mass% or more.The upper limit of the Cr content is more preferably 0.8 mass% or less, and even more preferably 0.7 mass% or less. The lower limit of the Si content is more preferably 0.45 mass% or more, and even more preferably 0.5 mass% or more.The upper limit of the Si content is more preferably 0.7 mass% or less, and even more preferably 0.6 mass% or less. The lower limit of the Ni content is more preferably 1.9 mass% or more, and even more preferably 2.0 mass% or more.The upper limit of the Ni content is more preferably 2.9 mass% or less, and even more preferably 2.8 mass% or less.
[0054] Furthermore, the copper alloy constituting the copper alloy particles 50 of the copper alloy powder for metal AM may contain additive elements and impurity elements (excluding O, H, S, and N) other than the alloy elements. In this embodiment, the additive elements are elements that are intentionally added to the copper alloy powder for metal AM of this embodiment. On the other hand, the impurity elements (excluding O, H, S, and N) are elements that are unintentionally mixed into the copper alloy powder for metal AM of this embodiment, and originate from contamination during the manufacturing process or impurities contained in trace amounts in the raw materials. The impurity elements may be unavoidable impurities. In the alloy corresponding to C18000 constituting the copper alloy particles 50 of the copper alloy powder for metal AM, examples of additive elements and impurity elements (excluding O, H, S, and N) other than alloy elements include Zr, Mg, Ti, Al, Zn, Ca, Sn, Pb, Fe, Mn, Te, Nb, P, Co, Sb, Bi, Ag, Ta, W, Mo, etc. Here, the additive elements and impurity elements (excluding O, H, S, and N) other than alloy elements may include at least one element selected from the group including Zr, Mg, Ti, Al, Zn, Ca, Sn, Pb, Fe, Mn, Te, Nb, P, Co, Sb, Bi, Ag, Ta, W, and Mo. In the alloy corresponding to C18000 constituting the copper alloy particles 50 of the copper alloy powder for metal AM, the total amount of additive elements and impurity elements (excluding O, H, S, and N) other than alloy elements may be 0.07 mass% or less, may be 0.06 mass% or less, may be 0.05 mass% or less, is preferably 0.04 mass% or less, is more preferably 0.03 mass% or less, is even more preferably 0.02 mass% or less, and is even more preferably 0.01 mass% or less. In addition, in the alloy corresponding to C18000 constituting the copper alloy particles 50 of the copper alloy powder for metal AM, the upper limit of the content of each of the additive elements other than the alloy elements and the impurity elements (excluding O, H, S, and N) is preferably 30 massppm or less, more preferably 20 massppm or less, and even more preferably 15 massppm or less.
[0055] In the copper alloy powder for metal AM of this embodiment, it is preferable that the volume-based 50% cumulative particle diameter D50 measured by a laser diffraction / scattering method is in the range of 5 μm or more and 120 μm or less, the 10% cumulative particle diameter D10 is in the range of 1 μm or more and 80 μm or less, and the 90% cumulative particle diameter D90 is in the range of 10 μm or more and 150 μm or less.
[0056] The lower limit of the 50% cumulative particle size D50 is more preferably 10 μm or more, and even more preferably 15 μm or more.The upper limit of the 50% cumulative particle size D50 is more preferably 100 μm or less, and even more preferably 90 μm or less. The lower limit of the 10% cumulative particle size D10 is more preferably 5 μm or more, and even more preferably 10 μm or more. The upper limit of the 10% cumulative particle size D10 is more preferably 70 μm or less, and even more preferably 60 μm or less. Furthermore, the lower limit of the 90% cumulative particle size D90 is more preferably 20 μm or more, and even more preferably 30 μm or more.The upper limit of the 90% cumulative particle size D90 is more preferably 140 μm or less, and even more preferably 120 μm or less.
[0057] An example of a method for producing copper alloy powder for metal AM according to the present embodiment will be described with reference to the flow diagram of Fig. 6. Note that, in this embodiment, copper alloy powder suitable for the laser PBF method is produced. The manufacturing method of copper alloy powder for metal AM according to this embodiment includes a melting and casting step S01 for obtaining a copper alloy ingot, a copper alloy raw material preparation step S02 for processing the obtained copper alloy ingot into a wire rod to obtain a copper alloy raw material, and a powder processing step S03 for processing the copper alloy raw material into powder.
[0058] (Melting and casting process S01) First, a copper alloy ingot 1 having a predetermined composition is manufactured. In this embodiment, a copper alloy ingot 1 is manufactured using a continuous casting apparatus 10 shown in FIG. This continuous casting apparatus 10 includes a melting furnace 11, a tundish 12 arranged downstream of the melting furnace 11, a connecting trough 13 connecting the melting furnace 11 and the tundish 12, an addition section 14 for adding alloy elements in the tundish 12, a continuous casting mold 15 arranged downstream of the tundish 12, and a pouring nozzle 16 for pouring molten copper alloy from the tundish 12 into the continuous casting mold 15.
[0059] In the melting furnace 11, the copper raw material is melted in a non-oxidizing atmosphere (an inert gas atmosphere or a reducing atmosphere) to obtain the molten copper 3. Here, the copper raw material melted in the melting furnace 11 is high-purity copper with a purity of 99.99 mass% or more (e.g., high-purity electrolytic copper or oxygen-free copper). The copper raw material to be melted is high-purity copper of 4N (99.99 mass%) or more, more preferably high-purity copper of 5N (99.999 mass%) or more, and even more preferably high-purity copper of 6N (99.9999 mass%) or more. The obtained molten copper 3 is preferably oxygen-free molten copper.
[0060] In the connecting trough 13, the obtained molten copper 3 is supplied to the tundish 12 while a non-oxidizing atmosphere (an inert gas atmosphere or a reducing atmosphere) is maintained. In addition, in the tundish 12, the molten copper 3 is held in a non-oxidizing atmosphere (an inert gas atmosphere or a reducing atmosphere). In addition, since the melting furnace 11, the connecting trough 13, and the tundish 12 are in a non-oxidizing atmosphere (an inert gas atmosphere or a reducing atmosphere), the gas components (O, H) in the molten copper 3 are reduced.
[0061] In the tundish 12, alloy elements (Cr, Si, Ni, etc.) are appropriately added to the held molten copper 3 using the addition section 14. Also, additive elements may be appropriately added here. By adding alloying elements to the molten copper 3 in which the gas components (O, H) have been sufficiently reduced, the yield of the alloying elements added is good, so that the amount of the alloying elements used can be reduced, and the manufacturing cost of the copper alloy can be reduced. Furthermore, by adding alloying elements to the molten copper 3 flowing inside the tundish 12, the alloying elements can be uniformly dissolved, and a molten copper alloy having stable component values can be continuously produced.
[0062] The obtained molten copper alloy is poured into a continuous casting mold 15 through a pouring nozzle 16, and a copper alloy ingot 1 is continuously produced. In this embodiment, a copper alloy ingot having a circular cross section is produced.
[0063] In this embodiment, the obtained copper alloy ingot 1 has an O concentration of 10 massppm or less and an H concentration of 5 massppm or less. In the obtained copper alloy ingot 1, the S concentration is preferably 15 massppm or less. Furthermore, in the obtained copper alloy ingot 1, the total content of impurity elements other than Cu is preferably 0.04 mass% or less.
[0064] (Copper alloy raw material preparation process S02) Next, the copper alloy ingot obtained in the melting and casting step S01 is processed into a wire rod to produce a copper alloy raw material. The copper alloy raw material preparation step S02 includes an extrusion step, a drawing step, and a cutting step. In this copper alloy raw material preparation step S02, first, a copper alloy ingot having a circular cross section is heated and processed by hot extrusion into a rod having a predetermined diameter (extrusion step). In this embodiment, the heating temperature during the hot extrusion process is preferably set within a range of 700°C or more and 1000°C or less.
[0065] Next, the obtained rod is drawn to produce a wire having a predetermined diameter (drawing step). The temperature for the drawing is not particularly limited, but is preferably within the range of -200°C to 200°C, which corresponds to cold or warm rolling, and particularly preferably at room temperature.
[0066] The obtained wire is then cut to a predetermined length to provide a copper alloy raw material (cutting step). Here, it is preferable that the O concentration in the obtained copper alloy raw material is 10 massppm or less, and the H concentration is 5 massppm or less. In addition, it is preferable that the S concentration in the obtained copper alloy raw material is 15 massppm or less. Furthermore, the total content of impurity elements (excluding O, H, and S) other than Cu and alloying elements in the obtained copper alloy raw material is preferably 0.04 mass% or less.
[0067] (Powder processing process S03) Next, the copper alloy raw material obtained in the copper alloy raw material preparation step S02 is subjected to an atomization process to produce copper alloy powder for metal AM. This powder processing step S03 includes a melting step, an atomizing step, and a classification step. In the melting step, the copper alloy raw material is heated and melted to obtain a molten alloy. In this embodiment, the melting atmosphere is preferably a non-oxidizing atmosphere. In the atomization process, for example, a powder is obtained by a gas atomization method. That is, the molten alloy obtained in the melting process is sprayed with a high-pressure gas to rapidly cool the droplets of the molten alloy, thereby producing a powder having a spherical or similar shape. In the classification process, the obtained powder is classified to obtain a copper alloy powder having a predetermined particle size distribution. Inert gases such as argon and nitrogen can be used as the gas used in the gas atomization process. The melting temperature of the copper alloy raw material in the gas atomization process (the melting temperature during the gas atomization process) is preferably equal to or higher than the melting point of copper and equal to or lower than 1500°C. The melting temperature during the gas atomization process may be equal to or higher than 1085°C and equal to or lower than 1500°C.
[0068] Here, in this embodiment, as described above, the atomization process is performed using a molten alloy derived from a copper alloy raw material in which the content of impurity elements (excluding O, H, S, and N) has been sufficiently reduced, so that Cr and Si are prevented from reacting with and being consumed by impurity elements (excluding O, H, S, and N), and it becomes possible to precipitate CrSi-based compounds containing Cr and Si and NiSi-based compounds containing Ni and Si at least at the copper crystal grain boundaries on the particle surfaces of the copper alloy powder for metal AM. Furthermore, in this embodiment, the atomization process is performed using a molten alloy derived from a copper alloy raw material in which the content of impurities (components including impurity elements and O, H, S, and N) has been sufficiently reduced. This prevents Cr and Si from reacting with and being consumed by the impurities (components including impurity elements and O, H, S, and N), and makes it possible to precipitate CrSi-based compounds containing Cr and Si and NiSi-based compounds containing Ni and Si at least at the copper crystal grain boundaries on the particle surfaces of the copper alloy powder for metal AM.
[0069] The copper alloy powder for metal AM of this embodiment is produced by the above-mentioned steps. In the copper alloy powder for metal AM of this embodiment, it is preferable that the O concentration is 1000 massppm or less and the H concentration is 5 massppm or less. Specifically, the O concentration may be about 2700 massppm or less, preferably 1000 massppm or less, and more preferably 900 massppm or less. The lower limit of the O concentration is not particularly limited, but may be a value that does not include 0 (or a value that exceeds 0). If the O concentration is high, foreign matter such as oxygen or oxides may remain in the molded product, which may deteriorate various properties of the molded product. The H concentration may be 90 massppm or less, 60 massppm or less, and preferably 5 massppm or less. The lower limit of the H concentration is not particularly limited, but may be a value that does not include 0 (or a value that exceeds 0). The S concentration in the copper alloy powder for metal AM may be 90 massppm or less, may be 60 massppm or less, and is preferably 30 massppm or less. Furthermore, the S concentration in the copper alloy powder for metal AM is more preferably 10 massppm or less. The lower limit of the S concentration is not particularly limited, but may be a value that does not include 0 (or a value that exceeds 0). In addition, in a process carried out under a finite pressure, such as atomization, atmospheric components contained in the atmosphere or during the process may cause atmospheric components to be contained in the powder. For example, nitrogen derived from atmospheric components may be contained in the powder. In the copper alloy powder for metal AM, the nitrogen concentration (N concentration) is preferably 30 massppm, more preferably 20 massppm, and even more preferably 10 massppm or less. In the copper alloy powder for metal AM of this embodiment, the nitrogen concentration (N concentration) is preferably 30 massppm, more preferably 20 massppm, and may be 10 massppm or less, and even more preferably 5 massppm or less. In addition, the lower limit of the N concentration is not particularly limited, but may be a value that does not include 0 (or a value that exceeds 0).
[0070] In addition, copper alloy powder for metal AM may contain additive elements and impurity elements other than alloy elements as long as they do not affect the characteristics. Here, the total amount of additive elements and impurity elements (excluding O, H, S, and N) may be 0.07 mass% or less, may be 0.06 mass% or less, may be 0.05 mass% or less, is preferably 0.04 mass% or less, is more preferably 0.03 mass% or less, is further preferably 0.02 mass% or less, and is further preferably 0.01 mass% or less. In addition, the upper limit of each of the contents of additive elements and impurity elements (excluding O, H, S, and N) is preferably 30 massppm or less, more preferably 20 massppm or less, and even more preferably 15 massppm or less.
[0071] Next, the method for producing a layered object according to this embodiment will be described with reference to the flow chart of FIG. The manufacturing method of this embodiment of an additive manufacturing object includes a preparation process S101 of preparing the above-mentioned copper alloy powder for metal AM, a first process S121 of forming a powder bed containing the copper alloy powder for metal AM, and a second process S122 of solidifying the copper alloy powder for metal AM at a predetermined position in the powder bed to form a modeling bed, in order to produce an additive manufacturing object. Through these steps, an additive manufacturing process is performed to produce an additive manufacturing product having a predetermined shape. Since the additive manufacturing product uses the copper alloy powder for metal AM according to the present embodiment, the additive manufacturing product has few structural defects such as voids and has excellent mechanical properties.
[0072] The copper alloy powder for metal AM of this embodiment, configured as described above, is composed of copper alloy particles containing Cr, Si, and Ni, and either or both of CrSi-based compounds containing Cr and Si and NiSi-based compounds containing Ni and Si are precipitated at the copper crystal grain boundaries on the particle surfaces of the copper alloy powder for metal AM. This makes it possible to stably produce high-quality additive manufacturing objects with high reproducibility of the microstructure of the objects produced by metal AM and few structural defects such as voids.
[0073] In the copper alloy powder for metal AM of this embodiment, if either or both of CrSi-based compounds containing Cr and Si and NiSi-based compounds containing Ni and Si are precipitated on the copper crystal grains on the surface of the copper alloy particles that make up the copper alloy powder for metal AM, the reproducibility of the microstructure of the object produced by metal AM will be even higher, and it will be possible to more stably produce high-quality additively manufactured objects with fewer structural defects such as voids.
[0074] In the copper alloy powder for metal AM of this embodiment, a CrSiNi-containing layer 52 containing either or both of CrSi-based compounds and NiSi-based compounds is formed on the particle surface of the copper alloy powder for metal AM, which makes it possible to more reproducibly produce the microstructure of a molded object produced by metal AM and to more stably produce high-quality additively molded objects with fewer structural defects such as voids.
[0075] Furthermore, in the copper alloy powder for metal AM of this embodiment, when the CrSiNi-containing layer 52 formed on the particle surface of the copper alloy powder for metal AM contains oxygen, deterioration of the copper alloy powder for metal AM can be suppressed, and it is possible to stably produce even higher quality additively molded objects with high reproducibility of the microstructure of the object produced by metal AM and fewer structural defects such as voids.
[0076] Furthermore, in the copper alloy powder for metal AM of this embodiment, when the copper alloy constituting the copper alloy powder for metal AM contains Cr in the range of 0.1 mass% or more and 0.8 mass% or less, Si in the range of 0.4 mass% or more and 0.8 mass% or less, Ni in the range of 1.8 mass% or more and 3.0 mass% or less, and the remainder is composed of copper and impurities, by subjecting an additive manufacturing object produced using this copper alloy powder for metal AM to an appropriate heat treatment, compounds can be precipitated, and it is possible to produce an additive manufacturing object with excellent electrical conductivity, thermal conductivity, and strength.
[0077] Furthermore, in the copper alloy powder for metal AM of this embodiment, when the volume-based 50% cumulative particle diameter D50 measured by a laser diffraction / scattering method is within the range of 5 μm or more and 120 μm or less, it has a particle size distribution suitable for metal AM, and it becomes possible to stably manufacture additive manufacturing objects.
[0078] Furthermore, in the copper alloy powder for metal AM of this embodiment, when the volume-based 10% cumulative particle diameter D10 measured by a laser diffraction / scattering method is within the range of 1 μm or more and 80 μm or less, it has a particle size distribution suitable for metal AM, and it becomes possible to stably manufacture additive manufacturing objects.
[0079] In addition, in the copper alloy powder for metal AM according to this embodiment, when the volume-based 90% cumulative particle diameter D90 measured by a laser diffraction / scattering method is within the range of 10 μm or more and 150 μm or less, the powder has a particle size distribution suitable for metal AM, and it becomes possible to stably manufacture additive manufacturing objects.
[0080] In the manufacturing method for additive manufacturing of this embodiment, the copper alloy powder for metal AM of this embodiment is used, so it is possible to consistently produce high-quality additive manufacturing objects with high reproducibility of the microstructure of the object produced by metal AM and with few structural defects such as voids.
[0081] The copper alloy powder for metal AM and the method for manufacturing an additive manufacturing object according to the embodiment of the present invention have been described above. However, the present invention is not limited thereto and can be modified as appropriate without departing from the technical concept of the invention. For example, in the above-described embodiment, the copper alloy powder for metal AM is produced by gas atomization, but this is not limited to this, and the copper alloy powder for metal AM may be produced by water atomization, centrifugal atomization, plasma atomization, or the like.
[0082] In addition, the copper alloy powder for metal AM obtained as described above may be appropriately heat-treated in a controlled atmosphere to stabilize the structure. Furthermore, in this embodiment, the copper alloy powder for metal AM suitable for the PBF method using a laser has been described as being produced, but this is not limited to this, and the copper alloy powder for metal AM may be applied to other metal AM.
[0083] Furthermore, after the shaping step S102, a heat treatment step may be performed in which heat treatment is performed at a temperature of 300° C. or more and the melting point of pure copper or less. Also, after the shaping step S102, a first heat treatment step may be performed in which heat treatment is performed at a temperature range of 800° C. or more and the melting point of pure copper or less, and after this first heat treatment step, a second heat treatment step may be performed in which heat treatment is performed at a temperature range of 300° C. or more and 800° C. or less. In addition, in the present embodiment, the continuous casting apparatus shown in FIG. 7 is used to produce a copper alloy ingot, but the present invention is not limited to this, and other casting apparatuses may be used.
[0084] For example, a continuous casting apparatus 101 shown in Fig. 9 may be used. This continuous casting apparatus 101 includes an oxygen-free copper supply means 102 disposed at the most upstream portion, a heating furnace 103 disposed downstream thereof, a tundish 104 disposed downstream of the heating furnace 103, molten metal supply paths 105a, 105b, and 105c connecting the oxygen-free supply means 102 to the heating furnace 103, a trough 106 connecting the heating furnace 103 and the tundish 104, addition means 107 and 108 for adding alloy elements, and a continuous casting mold 142.
[0085] The oxygen-free copper supply means 102 is composed of a melting furnace 121 for melting the copper raw material, a holding furnace 122 for temporarily holding the molten copper obtained by melting in the melting furnace 121, a degassing treatment device 124 for removing oxygen and hydrogen from the molten copper, and molten metal supply paths 105a, 105b, and 105c connecting these.
[0086] The degassing treatment device 124 has a gas bubbling device as stirring means for stirring the molten copper therein, and removes oxygen and hydrogen from the molten copper by bubbling with an inert gas, for example. The molten metal supply passages 105a, 105b, and 105c have a non-oxidizing atmosphere therein to prevent the molten copper and the oxygen-free copper molten metal from being oxidized. The non-oxidizing atmosphere is formed by blowing an inert gas such as a mixture of nitrogen and carbon monoxide or argon into the molten metal supply passages.
[0087] As adding means for adding alloy elements, a first adding means 107 disposed in the heating furnace 103 and a second adding means 108 disposed in the tundish 104 are provided. When alloying elements are continuously or intermittently charged from first adding means 107 provided in heating furnace 103, the alloying elements are added to the oxygen-free copper molten metal stored in heating furnace 103. Here, the oxygen-free copper molten metal stored in the storage section is heated by a high-frequency induction coil, which promotes the melting of the added alloying elements. Furthermore, when alloying elements are continuously or intermittently charged from the second adding means 108 provided in the tundish 104, the alloying elements are added to the molten oxygen-free copper flowing in the tundish 104. Here, the molten oxygen-free copper flowing in the tundish 104 is heated in the heating furnace 103 and has a high temperature, and also flows within the tundish 104, which promotes the dissolution of the added alloying elements. EXAMPLES
[0088] The results of experiments carried out to confirm the effects of the present invention will be described below.
[0089] First, by the manufacturing method described in the embodiment, a copper alloy ingot of C18000 having the composition shown in Table 1 was produced using a copper raw material made of high purity copper of 4N grade. Next, the copper alloy powder for metal AM with the C18000 composition shown in Table 2 was produced using the produced copper alloy ingot with the C18000 composition as the raw material by gas atomization with argon gas, and classified to a particle size suitable for the powder bed of laser PBF. The melting temperature during the gas atomization process was 1300°C.
[0090] The obtained copper alloy powder for metal AM with a C18000 composition was evaluated for the presence or absence of CrSi-based compounds at the copper crystal grain boundaries and on the copper crystal grains on the particle surfaces of the copper alloy particles that make up the copper alloy powder, the presence or absence of NiSi compounds at the copper crystal grain boundaries and on the copper crystals on the surface of the copper particles that make up the powder, the presence or absence of oxygen on the particle surfaces of the copper alloy particles that make up the copper alloy powder, the volume-based 10% cumulative particle diameter D10, 50% cumulative particle diameter D50, 90% cumulative particle diameter D90, and composition.
[0091] (Presence or absence of CrSi-based compounds on the copper grain boundaries and copper grains of copper alloy particles) Auger electron spectroscopy was used to confirm the presence or absence of CrSi-based compounds at the copper grain boundaries and on the copper grains on the surface of the copper alloy particles constituting the powder, and at the copper grain boundaries and on the copper grains inside the copper alloy particles, in the copper alloy powder for metal AM of the present invention. The observation results are shown in Figures 2A to 2E.
[0092] (Presence or absence of NiSi-based compounds on the copper grain boundaries and copper grains of copper alloy particles) Auger electron spectroscopy was used to confirm the presence or absence of NiSi-based compounds at the copper grain boundaries and on the copper grains (copper grain surfaces) on the surfaces of the copper alloy particles constituting the powder, as well as at the copper grain boundaries and on the copper grains inside the powder, in the copper alloy powder for metal AM of the present invention. The observation results are shown in Figures 2A to 2E.
[0093] (Presence or absence of oxygen on the surface of the copper alloy particles that make up the powder) The presence or absence of oxygen on the particle surface was confirmed by Auger electron spectroscopy.
[0094] (Presence or absence of CrSi-based compounds and NiSi-based compounds on the surface of copper alloy particles) The presence or absence of CrSi-based compounds and NiSi-based compounds on the surfaces of the copper alloy particles constituting the copper alloy powder for metal AM of the present invention was confirmed by high-angle annular dark-field scanning transmission microscopy. The analysis results are shown in Figures 10 and 11.
[0095] (Volume average particle size of copper alloy powder) Using a Microtrac MT3300EXII, wet particle size distribution measurements were performed, and the volume-based 10% cumulative particle size D10, 50% cumulative particle size D50, and 90% cumulative particle size D90 were calculated from the results. The particle size distribution measurements performed on the copper alloy powder for metal AM after classification of the present invention using this method resulted in a volume-based D10 of 15 μm, D50 of 27 μm, and D90 of 45 μm.
[0096] (Composition of copper alloy powder for ingot and metal AM) The O concentration in the ingots and the copper alloy powder for metal AM of the present invention shown in Table 1 was determined by inert gas fusion-infrared absorption method, the H concentration by inert gas fusion-thermal conductivity method, and the S concentration by combustion-infrared absorption method. In addition, the concentrations of components other than these substances, except for copper, were determined by a combination of X-ray fluorescence analysis, glow discharge mass spectrometry, and inductively coupled plasma mass spectrometry.
[0097] (Additive Manufacturing) The copper alloy powder for metal AM of the present invention was used, and the energy density was set to 13 J / mm using a commercially available laser PBF device. 2 A small piece of the layered object was produced under the above conditions. The density of the layered object was then measured. In addition, the obtained laminated object was subjected to a heat treatment under the conditions shown in Table 3, and the mechanical and electrical properties of the laminated object after the heat treatment were evaluated.
[0098] (model density) The density of the layered object was evaluated from the cross section of the layered object and the area occupied by voids observed in the cross section of the layered object. In this specification, this density is defined as the density of the object. The density of the molded object was evaluated by first defining the cross-sectional area of the object to be measured (this is called the evaluation cross-sectional area, 3.4 mm square), then checking for voids within this measurement cross-sectional area, and calculating the area occupied by voids in the evaluation cross-sectional area. The density of the molded object was then defined as (evaluation cross-sectional area - void area) / evaluation cross-sectional area. The evaluation results of the density of the molded object are shown in Table 2.
[0099] (Evaluation of mechanical properties and electrical conductivity of the object) As a mechanical property of the fabricated additive manufacturing object, the Vickers hardness (HV unit) was measured at room temperature according to JIS Z 2244: 2009. The Vickers hardness measurement load was 10 kgf. The electrical conductivity (%IACS unit) of the fabricated additive manufacturing object was measured at room temperature using an eddy current electrical conductivity measurement.
[0100] [Table 1] (The impurities shown in Table 1 exclude O, H, and S.)
[0101] [Table 2] (The impurities shown in Table 2 exclude O, H, S, and N.)
[0102] [Table 3]
[0103] 2A to 2E show the results of Auger electron spectroscopy after 15 minutes of ion etching of the particle surface of the copper alloy powder for metal AM of the present invention. The etching rate of each element alone or compounds generated by each element on the particle surface of the copper alloy powder of the present invention in the experimental system of this Auger electron spectroscopy analysis is not clear, but since the etching rate of SiO2 in the experimental system of this Auger electron spectroscopy analysis is 1.08 nm / min, it is considered that 15 minutes of ion etching is the structure after etching a thickness of approximately 15 nm.
[0104] As shown in Figures 2A to 2E, in addition to copper crystal grains and copper crystal grain boundaries, numerous island-like fine structures appeared on the particle surface after ion etching. First, the secondary electron image in Figure 2A confirmed the grain boundaries of the copper crystal grains and the surfaces of the copper crystal grains (above the copper crystal grains) on the surface of the copper alloy particles of the copper alloy powder for metal AM of the present invention. Furthermore, Figure 2B confirmed that the island-like fine structures present on the grain boundaries of the copper crystal grains and on the surfaces of the copper crystal grains are derived from Cr-based precipitates. From the results shown in Figures 2B to 2E, it was confirmed that CrSi-based compounds and NiSi-based compounds were precipitated at the copper grain boundaries on the particle surface. In addition, from the results shown in Figures 2B to 2E, it was confirmed that the substances precipitated on the particle surface of the copper alloy powder for metal AM of the present invention were predominantly CrSi-based compounds, and were widely distributed on the copper grain boundaries and copper grains. It is believed that the Cr-based precipitates widely distributed on the particle surfaces of the copper alloy powder for metal AM of the present invention contribute to improving the laser absorption of the particle surface in the metal AM modeling process. In addition, by applying the copper alloy powder for metal AM of the present invention having such a microstructure to metal AM, it is possible to manufacture an additive manufacturing object of a copper alloy with excellent electrical conductivity, thermal conductivity, and strength.
[0105] The density of precipitates derived from CrSi compounds and / or each NiSi compound in the CrSiNi-containing layer 52 of the particles of the copper alloy powder for metal AM of the present invention was measured using an image of the outermost surface of the CrSiNi-containing layer 52 analyzed by Auger electron spectroscopy using a scanning Auger electron spectrometer PHI700xi manufactured by ULVAC-PHI, Inc. 2 The area occupancy of the CrSi-based compound and / or each NiSi-based compound was calculated from the size and number of precipitates of the CrSi-based compound and / or each NiSi-based compound per one piece. On the outermost surface of the CrSiNi-containing layer 52 of the particles of the copper alloy powder for metal AM of the present invention, there were areas where the density of precipitates was 17% by area and areas where the density was 21% by area (see Figures 2A and 2B).
[0106] In addition, the outermost surface of the CrSiNi-containing layer 52 of the particles of the copper alloy powder for metal AM of the present invention was analyzed by Auger electron spectroscopy using a scanning Auger electron spectrometer PHI700xi manufactured by ULVAC-PHI, Inc., and the copper crystal grain boundaries were observed in an image, and the linear density per μm of grain boundary length was calculated from the proportion of precipitates of CrSi-based compounds and / or each NiSi-based compound per μm of grain boundary length. In the CrSiNi-containing layer 52 of the particles of the copper alloy powder for metal AM of the present invention, there were places where the linear density was 31% and places where the linear density was 60%.
[0107] As shown in Figure 10, the results of analysis of the copper alloy particle surfaces of the copper alloy powder for metal AM of the present invention using a high-angle scattering annular dark-field scanning transmission microscope confirmed that the CrSi-based compounds formed on the surfaces of the copper alloy particles of the copper alloy powder for metal AM of the present invention contain Cr3Si. Furthermore, as shown in Figure 11, analysis of the electron diffraction pattern confirmed that in the case of Figure 10, Cr3Si is formed in lattice matching with Cu crystals.
[0108] 3A to 3F are Auger electron spectroscopy analysis results of the particle surface of the copper alloy particles constituting the copper alloy powder for metal AM according to the present embodiment, showing Cr mapping images before ion etching the particle surface, and after ion etching for 5 minutes, 15 minutes, 30 minutes, and 50 minutes. First, as shown in FIG. 3A and FIG. 3B, it can be seen that Cr-based precipitates are distributed in an island shape on the copper grain boundaries and on the copper grains (copper grain surfaces) on the outermost particle surface before ion etching. This result coincides with the tendency of the results of FIG. 2B to FIG. 2E shown above. From the results of FIG. 2B to FIG. 2E and FIG. 3A and FIG. 3B, it is considered that the distribution of Cr confirmed in FIG. 3A and FIG. 3B is derived from CrSi-based compounds. That is, from the results of Figs. 2B to 2E and Figs. 3A and 3B, it is confirmed that CrSi-based compounds are distributed on the particle surfaces of the copper alloy powder for metal AM of the present invention.
[0109] In addition, as shown in Figures 3B to 3F, the structure of the island-like microstructure on the particle surface changes with the ion etching time. As shown in Figure 3F, the distribution of Cr-based precipitates is confirmed even after 50 minutes of ion etching, but compared with Figures 3C and 3D, the distribution points of Cr tend to decrease. From the results of Figures 2B to 2E and Figures 3B to 3F, it was confirmed that a CrSiNi-containing layer 52 containing either or both of a CrSi-based compound and a NiSi-based compound is formed on the particle surface of the copper alloy powder for metal AM of the present invention. In addition, from the etching rate of SiO2 in the experimental system of this Auger electron spectroscopy analysis and the state of the structural change of the particle surface with the etching time in Figures 3B to 3F, the thickness of the CrSiNi-containing layer 52 is considered to be in the range of approximately 1 nm to 100 nm.
[0110] From the oxygen intensity depth profile of the particle surface of the copper alloy powder for metal AM of the present invention shown in Figure 4, it was confirmed that the oxygen concentration is high on the outermost surface side of the particle and decreases toward the inside of the particle. Since the copper alloy powder for metal AM of the present invention essentially contains oxygen as a copper alloy, a certain amount of oxygen exists in the particle body, and this is thought to constitute the background concentration of oxygen concentration in the particle body. On the other hand, the oxygen concentration gradient observed on the particle surface is mainly generated during the powdering process, and further, from the results of Figure 4, it is thought to exist in the range of approximately 1 nm to 100 nm, and it is thought that an oxygen concentration gradient can occur on the order of the thickness of the surface layer containing the above-mentioned Cr-based precipitates.
[0111] From the results of Figures 2B to 2E, 3B to 3F and 4, it was confirmed that the CrSiNi-containing layer on the particle surface of the copper alloy powder for metal AM of the present invention is a layer containing oxygen. The presence of such an oxygen-containing layer in the copper alloy powder for metal AM of the present invention is considered to have the effect of suppressing surface deterioration of the copper alloy powder. In addition, as shown in Figures 2B to 2E, 3B to 3F and 4, since the copper alloy powder for metal AM of the present invention is mainly composed of Cu, which is the parent phase, it is presumed that such oxygen is mainly derived from copper oxide, and further, it is presumed to exist as a constituent element of the oxide of alloy elements and other impurity elements. That is, it is presumed that the CrSiNi-containing layer on the surface of the copper alloy powder for metal AM of the present invention forms a composite layer composed of Cu, copper oxide, Cr, Si, Ni oxide, etc., while containing a compound composed of Cr, Si, and Ni.
[0112] 5A to 5D show the results of Auger electron spectroscopy of the particle cross section of the copper alloy powder for metal AM of the present invention as a cross-sectional observation of the copper alloy particle. As shown in these figures, the presence of CrSi-based precipitates and NiSi-based precipitates was confirmed at the copper grain boundaries inside the particle, while the results of this Auger electron spectroscopy analysis did not confirm Cr-based precipitates inside the copper grains. This was predicted to be either because there were almost no Cr-based precipitates inside the copper grains, or because the Cr-based precipitates inside the copper grains were very small (or the amount was small) and difficult to observe. Therefore, from a comparison of Figures 2B to 2E and Figures 5A to 5D, that is, from a comparison of the particle surface and the particle cross section, it was thought that the proportion of precipitates on a certain surface of the particle would be greater on the outermost surface (or surface layer) of the particle than on the inside of the particle. On the other hand, the presence of either or both of CrSi-based precipitates and NiSi-based precipitates was confirmed at the grain boundaries inside the particles of copper alloy powder for metal AM, as typically shown in Figure 5. This result indicates that either or both of CrSi-based precipitates and NiSi-based precipitates are present at the grain boundaries inside the CrNiSi-containing layer on the particle surface of the particles of copper alloy powder for metal AM. The particle surface of the copper alloy powder for metal AM of the present invention has such a characteristic structure compared to the interior of the particle, which promotes laser absorption, resulting in higher density of the molded body and improved productivity of the molded body.
[0113] When a product was manufactured using the copper alloy powder for metal AM with the C18000 composition of the present invention, in which either or both of CrSi-based compounds containing Cr and Si and NiSi-based compounds containing Ni and Si were precipitated at the copper crystal grain boundaries, the density of the product was 99.3% as shown in Table 2. Furthermore, as shown in Table 3, by subjecting the additive manufacturing product with the C18000 composition to an appropriate heat treatment, a practical Vickers hardness and electrical conductivity were confirmed. These results demonstrate that the copper alloy powder for metal AM of the present invention can be used to produce additively molded objects with few voids, which is important for practical use, and that the powder has sufficient mechanical properties and electrical conductivity for practical use, making it possible to realize practical copper alloy additively molded objects. [Explanation of symbols]
[0114] 50 copper alloy particles 51 Particle body 52 CrSiNi-containing layer
Claims
1. A copper alloy powder for metal AM used in metal AM, The copper alloy contains Cr, Si, and Ni as alloying elements, and has a composition in which the Cr content is within a range of 0.1 mass% or more and 0.8 mass% or less, the Si content is within a range of 0.4 mass% or more and 0.8 mass% or less, the Ni content is within a range of 1.8 mass% or more and 3.0 mass% or less, and the remainder is copper and impurities, A copper alloy powder for metal AM, characterized in that either or both of a CrSi-based compound containing Cr and Si and a NiSi-based compound containing Ni and Si are precipitated at the copper crystal grain boundaries on the surfaces of the copper alloy particles constituting the copper alloy powder.
2. A copper alloy powder for metal AM as described in claim 1, characterized in that it contains at least one element selected from the group consisting of Zr, Mg, Ti, Al, Zn, Ca, Sn, Pb, Fe, Mn, Te, Nb, P, Co, Sb, Bi, Ag, Ta, W and Mo as additive elements and impurity elements other than the alloy elements in a total amount of 0.07 mass% or less.
3. 2. The copper alloy powder for metal AM according to claim 1, characterized in that either one or both of the CrSi-based compound and the NiSi-based compound are precipitated on copper crystal grains on the surfaces of the copper alloy particles constituting the copper alloy powder.
4. 2. The copper alloy powder for metal AM according to claim 1, characterized in that a layer containing either one or both of the CrSi-based compound and the NiSi-based compound is formed on the surface of the copper alloy particle.
5. 5. The copper alloy powder for metal AM according to claim 4, wherein the layer containing either one or both of the CrSi-based compound and the NiSi-based compound contains oxygen.
6. 2. The copper alloy powder for metal AM according to claim 1, characterized in that, in a cross-sectional observation of a copper alloy particle constituting the copper alloy powder, either one or both of a CrSi-based compound and a NiSi-based compound are distributed at copper crystal grain boundaries.
7. The CrSi-based compound is Cr 3 4. The copper alloy powder for metal AM according to claim 3, further comprising Si.
8. The NiSi-based compound is Ni 5 S 2 The copper alloy powder for metal AM according to claim 3, characterized in that it contains
9. 2. The copper alloy powder for metal AM according to claim 1, characterized in that the volume-based 50% cumulative particle diameter D50 measured by a laser diffraction / scattering method is in the range of 5 μm or more and 120 μm or less.
10. 2. The copper alloy powder for metal AM according to claim 1, characterized in that the volume-based 10% cumulative particle diameter D10 measured by a laser diffraction / scattering method is in the range of 1 μm or more and 80 μm or less.
11. The copper alloy powder for metal AM according to claim 1, characterized in that the volume-based 90% cumulative particle diameter D90 measured by a laser diffraction / scattering method is in the range of 10 μm or more and 150 μm or less.
12. A preparation step of preparing the copper alloy powder for metal AM according to any one of claims 1 to 11; a molding process for producing an additive object by sequentially repeating a first process for forming a powder bed containing the copper alloy powder for metal AM and a second process for solidifying the copper alloy powder for metal AM at a predetermined position in the powder bed to form a molding bed; A method for manufacturing a layered object, comprising:
13. The method for manufacturing a layered object according to claim 12, further comprising a heat treatment step of performing a heat treatment at a temperature range of 300° C. or higher and lower than the melting point of pure copper after the shaping step.
14. The method for manufacturing an additively molded object according to claim 12, characterized in that it comprises a first heat treatment process in which heat treatment is performed in a temperature range of 800°C or higher and lower than the melting point of pure copper after the molding process, and a second heat treatment process in which heat treatment is performed in a temperature range of 300°C or higher and lower than 800°C after the first heat treatment.
Citation Information
Patent Citations
Manufacturing method of alloy structure
JP2016023366A
Copper alloy powder, manufacturing method of laminate molded article and laminate molded article
JP2016211062A
Copper alloy powder, heat treatment method for multilayer shaped structure, method for producing copper alloy shaped structure, and copper alloy shaped structure
JP2019070169A
Copper powder having excellent laser light absorbency
JP2020186429A
Cu-ni-si-based alloy for electronic material
WO2008123433A1