Method for treating inorganic adsorbent having adsorbed lanthanides and / or minor actinides

By mixing a silicon-containing glass raw material with inorganic adsorbents that have adsorbed Ln or MA, the method achieves uniform vitrification, addressing segregation and bubble issues, and reduces waste liquid generation and facility scale.

JP7563697B2Active Publication Date: 2024-10-08MITSUBISHI HEAVY IND LTD +1
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2021144089
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2021-09-03
Publication Date
2024-10-08
Estimated Expiration
2041-09-03

AI Technical Summary

Technical Problem

The segregation of inorganic adsorbent components and bubbles within the vitrified body during the vitrification process of inorganic adsorbents that have adsorbed lanthanoids (Ln) or minor actinides (MA) leads to non-uniform vitrified products, posing risks of physical and chemical instability during long-term storage or geological disposal.

Method used

A treatment method involving mixing a silicon-containing glass raw material with the inorganic adsorbent that has adsorbed Ln or MA, followed by vitrification, with a silicon dioxide content of 20 to 95% by mass in the mixture, to ensure uniform vitrification.

Benefits of technology

The method effectively vitrifies the inorganic adsorbent, resulting in a uniformly stable vitrified product with reduced generation of waste liquid, lower concentration loads, and decreased facility scale requirements.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007563697000005
    Figure 0007563697000005
  • Figure 0007563697000006
    Figure 0007563697000006
  • Figure 0007563697000007
    Figure 0007563697000007
Patent Text Reader

Abstract

To provide a processing method of the inorganic adsorbent adsorbing lanthanide or / and minor actinide satisfactorily.SOLUTION: The processing method includes: a step of mixing a glass raw material containing silicon to inorganic adsorbent adsorbing lanthanide or / and minor actinide; and a step of vitrification of the mixture obtained by the step of mixing the glass raw materials. In the processing method of the inorganic adsorbent adsorbing lanthanide or / and minor actinide, the content of silicon in the mixture in terms of silicon dioxide is 20 to 95% by mass with respect to the total mass of the mixture.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to a method for treating an inorganic adsorbent that has adsorbed lanthanides and / or minor actinides. [Background technology]

[0002] In the reprocessing of spent nuclear fuel discharged from light water reactors, U (uranium) and Pu (plutonium) are recovered from the solution of spent nuclear fuel. Highly Active Liquid Waste (HALW) that remains after the recovery of U and Pu contains fission products (FP), minor actinides (MA) such as Np (neptunium), Am (americium), and Cm (curium), and lanthanides (Ln) such as La (lanthanum), Ce (cerium), and Eu (europium). HALW is planned to be vitrified through an enrichment process and disposed of in a geological repository.

[0003] MA includes nuclides with long half-lives of the order of 10,000 years, which increases the burden of HALW disposal. Therefore, the recovery of MA from HALW and burning the recovered MA in fast breeder reactors are being considered. Since Ln has similar chemical properties to MA, Ln is easily entrained when MA is recovered from HALW. Therefore, after the MA recovery process, an MA purification process is carried out to separate MA and Ln. Representative methods for the MA recovery process and MA purification process are solvent extraction and extraction chromatography, which use a solvent (extractant solution) to extract MA.

[0004] Figure 5 shows an example of the process from MA recovery to combustion. In this example, first, MA is recovered from HALW (MA recovery process). In the MA recovery process, MA is extracted from HALW using a solvent, and the MA is stripped from the extract into the aqueous phase. In the MA recovery process, some Ln is entrained with MA. Next, the stripped liquid is concentrated, and then MA and Ln are separated (MA purification process). In the MA purification process, MA is extracted from the concentrated liquid using a solvent, and the MA is stripped from the extract into the aqueous phase to obtain an MA-containing solution from which Ln has been separated. The obtained MA-containing solution is then concentrated, and the concentrated liquid is used to produce MA fuel, which is then combusted. The waste liquid (containing FP) after MA extraction from HALW is concentrated, vitrified, stored, and then disposed of in a geological formation. The waste liquid (containing Ln) after MA extraction from the concentrated liquid is concentrated, vitrified, and disposed of.

[0005] The wastewater generated from the MA recovery process is of the same level as HALW in the current reprocessing process that does not recover MA, so it can be vitrified through a concentration process similar to the current system. On the other hand, the wastewater generated from the MA purification process will also be vitrified, but in this case, the amount of water added for stripping in the MA purification process must be evaporated in a concentration process. In addition, the concentration of the target substance in the stripped solution obtained through solvent extraction and stripping is usually lower than the concentration in the original solution. Therefore, the concentration process for treating the wastewater generated from the MA purification process requires a larger facility scale than the current concentration process for treating HALW, which increases construction costs and running costs due to the large energy consumption during operation. To address such problems, Patent Document 1 proposes a method of adsorbing Ln in a radioactive solution with an adsorbent capable of being solidified into a glass and vitrifying the adsorbent with the Ln adsorbed therein. An inorganic adsorbent is described as the adsorbent capable of being solidified into a glass. [Prior art documents] [Patent documents]

[0006] [Patent Document 1] JP 2020-204518 A Summary of the Invention [Problem to be solved by the invention]

[0007] However, according to the study by the present inventors, when inorganic adsorbents adsorbing Ln or MA are vitrified, segregation of inorganic adsorbent components and bubbles occur in the vitrified body, and a uniform vitrified body may not be obtained. If the uniformity of the vitrified body is low, the physical and chemical stability may be impaired during long-term storage or geological disposal, and there is a concern that radioactive materials may leak.

[0008] The present disclosure has been made to solve the above-mentioned problems, and has an object to provide a treatment method capable of satisfactorily vitrifying an inorganic adsorbent having adsorbed Ln and / or MA. [Means for solving the problem]

[0009] In order to solve the above problems, the processing method according to the present disclosure includes a step of mixing a glass raw material containing silicon with an inorganic adsorbent having Ln and / or MA adsorbed thereon, and a step of vitrifying the mixture obtained by the step of mixing the glass raw materials, wherein the content of silicon in the mixture, calculated as silicon dioxide, is 20 to 95 mass% with respect to the total mass of the mixture. Effect of the Invention

[0010] According to the treatment method of the present disclosure, the inorganic adsorbent that has adsorbed Ln and / or MA can be satisfactorily vitrified. [Brief description of the drawings]

[0011] [Figure 1] FIG. 2 is a flow diagram illustrating a processing method according to the first embodiment of the present disclosure. [Diagram 2] FIG. 11 is a flow diagram illustrating a processing method according to a second embodiment of the present disclosure. [Diagram 3] FIG. 11 is a flow diagram illustrating a processing method according to a third embodiment of the present disclosure. [Figure 4] FIG. 11 is a flow diagram illustrating a processing method according to a fourth embodiment of the present disclosure. [Diagram 5] FIG. 11 is a flow diagram illustrating a process according to a comparative example. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0012] In this specification, “Ln (lanthanoid)” is a general term for elements with atomic numbers 57 to 71. "MA (Minor Actinides)" refers to the transuranium elements belonging to the actinide group, excluding Pu. "Actinide" is a general term for elements with atomic numbers 89 to 103.

[0013] First Embodiment Hereinafter, a processing method according to a first embodiment of the present disclosure will be described with reference to FIG. As shown in FIG. 1, the processing method according to the first embodiment of the present invention includes: Step S1-1: performing a separation process to separate MA together with Ln from the HALW to obtain a solution containing MA and Ln (hereinafter also referred to as "MA·Ln-containing solution"); Step S1-2: performing a solidification process for solidifying the MA·Ln-containing solution to obtain a solidified body containing MA and Ln; Step S1-3 of storing the solidified body obtained in step S1-2; Step S1-4 of dissolving the solidified body stored in step S1-3; Step S1-5: adsorbing Ln in the solidified solution obtained in step S1-4 onto an inorganic adsorbent, and separating the inorganic adsorbent with adsorbed Ln (hereinafter, also referred to as "waste adsorbent") from the solidified solution, thereby purifying MA (separating MA and Ln); Step S1-6: mixing the waste adsorbent separated from the solidified solution in step S1-5 with a glass raw material containing silicon; Step S1-7 of vitrifying the mixture obtained by step S1-6; has. If necessary, the processing method according to this embodiment may further include a step of performing a stabilization treatment on the solidified body after step S1-2 and before step S1-3 to remove some or all of the carbon, hydrogen, oxygen, and nitrogen components.

[0014] The waste liquid (FP-containing solution) remaining after the separation of MA and Ln in step S1-1 is concentrated, vitrified, stored, and then disposed of in a geological repository. The solidified solution after Ln is adsorbed by the inorganic adsorbent and separated from the waste adsorbent in step S1-5 is a solution containing MA (MA-containing solution). The MA-containing solution is used for fuel production after separating the highly exothermic MA as necessary. For example, the MA-containing solution is mixed with U and Pu to obtain mixed oxides, thereby producing fuel. The obtained fuel is burned in a fast breeder reactor or the like. The vitrified waste obtained in step S1-7 is, for example, stored and disposed of in a geological repository.

[0015] (HALW) HALW is a waste liquid obtained by separating U and Pu from a solution of spent nuclear fuel. HALW contains FP, MA, Ln, etc., but does not contain U or Pu. HALW typically contains at least Np, Am, and Cm as MA, and at least La and Ce as Ln.

[0016] An example of HALW is wastewater generated during reprocessing using the PUREX (Plutonium Uranium Redox Extraction) method. In the PUREX method, a nitric acid solution containing U and Pu is contacted and mixed with tributyl phosphate (TBP) and an organic solvent such as dodecane. As a result, U and Pu in the nitric acid solution form complexes with TBP and move to the organic solvent. Meanwhile, FP, MA, and Ln remain in the nitric acid solution (waste liquid).

[0017] (Step S1-1: Separation process) Examples of separation processes include a process involving extracting MA together with Ln from HALW by solvent extraction (hereinafter also referred to as "extraction process"), or a process involving adsorbing MA and Ln in HALW onto an adsorbent and eluting the MA and Ln adsorbed onto the adsorbent (hereinafter also referred to as "adsorption-elution process"). When the separation treatment includes an extraction treatment, the separation treatment may further include, after the extraction treatment, a treatment of back-extracting MA and Ln from the extract obtained by the extraction treatment (hereinafter also referred to as "back-extraction treatment").

[0018] In the extraction process, for example, the HALW is brought into contact with an organic solvent solution containing an extractant (extractant solution), and when the HALW is brought into contact with the extractant solution, MA and Ln migrate to the extractant solution. The extract obtained by the extraction process may be directly subjected to step S1-2 as a MA·Ln-containing solution, or may be subjected to a back-extraction process. In terms of reducing the number of steps and the amount of waste liquid, it is preferable to subject the extract obtained by the extraction process to step S1-2 as a MA·Ln-containing solution.

[0019] Examples of the extractant include complexing agents that form complexes with MA and Ln. Such complexing agents are preferable because they are less expensive than complexing agents that selectively form complexes with MA. Specific examples of the complexing agent include n-octyl(phenyl)-N,N'-diisobutylcarbamoylmethylphosphine oxide-tributyl phosphate mixture (CMPO-TBP mixture), diisodecyl phosphoric acid, 6,6'-bis(5,5,8,8-tetramethyl-5,6,7,8-tetrahydro-1,2,4-benzotriazin-3-yl)-2,2'-bipyridine (BTBP), N,N'-dibutyl-N,N'-dimethyltetradecylmalonamide (DMDBTDMA), and N,N,N',N'-tetraoctyl-3-oxapentanediamide (TODGA). The extractant may be used alone or in combination of two or more.

[0020] The organic solvent can be appropriately selected depending on the extractant used. It is desirable that the organic solvent is reusable, inexpensive, and resistant to radiation degradation. A specific example of the organic solvent is n-dodecane. The organic solvent may be used alone or in combination of two or more kinds.

[0021] In the back extraction process, for example, the extract is contacted with an aqueous solution containing nitric acid (stripping agent). This causes MA and Ln in the extract to migrate to the aqueous solution. Meanwhile, the organic solvent in the extract does not migrate to the aqueous solution but remains in the extract, making it possible to reuse it. The stripping solution obtained by the stripping process is typically directly used in step S1-2 as a MA·Ln-containing solution.

[0022] The adsorbent used in the adsorption-elution treatment may be any adsorbent capable of adsorbing MA and Ln. The method for adsorbing MA and Ln in HALW onto an adsorbent includes contacting HALW with an adsorbent, such as a column method or a batch method. The MA and Ln adsorbed on the adsorbent can be eluted by contacting the adsorbent with an eluent. The eluate obtained by the adsorption-elution process, i.e., the eluate after contact with the adsorbent, contains MA and Ln. Typically, this eluate is directly subjected to step S1-2 as a MA·Ln-containing solution.

[0023] (Step S1-2: Solidification process) Examples of the solidification treatment include decomposition treatment, hydrothermal treatment, and vitrification treatment. When vitrification is performed, it is preferable to carry out a concentration treatment for concentrating the MA·Ln-containing solution before the vitrification treatment.

[0024] When the MA·Ln-containing solution is an extract obtained by an extraction process, the solidification process is preferably a distillation / decomposition process. The extract is subjected to distillation and decomposition treatment to remove the organic solvent and oxidize the MA, resulting in a solidified product containing MA oxide. Examples of the distillation and decomposition treatment include distillation, thermal decomposition, and incineration. Distillation can be carried out using a known evaporation method such as a batch method or a continuous method (plate tower or packed tower).

[0025] When the MA·Ln-containing solution is a stripped solution obtained by stripping or an eluate obtained by adsorption-elution, the preferred solidification treatment is hydrothermal treatment or a treatment in which the MA·Ln-containing solution is concentrated and the resulting concentrate is vitrified (concentration-vitrification treatment). By subjecting the MA·Ln-containing solution to hydrothermal treatment, the MA contained in the solution is oxidized, and a solid containing MA oxide is precipitated. The solid is separated from the liquid medium (water) by solid-liquid separation. This results in a solid containing MA oxide. Concentration of the MA·Ln-containing solution and vitrification of the concentrated solution can be carried out by conventional methods.

[0026] (Stabilization treatment) The solidified body may contain organic matter such as the extractant or radiolysis products of the extractant. If the solidified body contains organic matter, gas may be generated during storage, impairing the containment function of the radioactive material and causing problems. The occurrence of such problems can be suppressed by carrying out a stabilization process on the solidified body to remove some or all of the carbon, hydrogen, oxygen, and nitrogen components. The stabilization treatment may be, for example, calcination or sintering.

[0027] (Step S1-3: Storage) In step S1-3, the solidified body is temporarily stored. As a method for storing the solidified bodies, any method known as a dry storage method for radioactive waste can be used, for example, a method in which the solidified bodies are stored in multiple canisters, and these multiple canisters are housed in a cask and stored in a storage facility.

[0028] The period for storing the solidified body can be set appropriately. Since highly heat-generating MA such as Cm is not suitable for fuel production, if the solidified body contains highly heat-generating MA, it is preferable to store the solidified body in step S1-4 until the highly heat-generating MA contained in the solidified body has sufficiently decayed. This makes it unnecessary to separate highly heat-generating MA such as Cm from the MA-containing solution when the MA-containing solution separated from the waste adsorbent in step S1-5 is used for MA fuel production. Note that Cm contained in HALW is mainly a substance with a relatively short half-life of approximately 18 years. 244 Cm.

[0029] (Step S1-4: Dissolving solidified body) To dissolve the solidified body, for example, if the solidified body contains MA oxides, an aqueous solution of nitric acid may be added. If the solidified body is a vitrified body, the solidified body is dissolved with an acid solution or the like, and the glass component is then separated from the resulting solution. The solution obtained by dissolving the solidified body contains MA and Ln.

[0030] (Step S1-5: MA purification (adsorption treatment)) In step S1-5, an inorganic adsorbent is used. Since the inorganic adsorbent does not contain organic matter, the waste adsorbent can be directly subjected to step S1-6. The inorganic adsorbents will be described in more detail below.

[0031] As a method for adsorbing Ln in the solidified solution (radioactive solution containing MA and Ln) obtained in step S1-4 onto an inorganic adsorbent, a method of contacting the solidified solution with an inorganic adsorbent may be mentioned. The method for contacting the solidified body solution with the inorganic adsorbent includes a column method, a batch method, etc. The column method is preferred because it allows adsorption and separation to be carried out continuously. In the column type, the solidified solution is passed through a column filled with an inorganic adsorbent. The conditions for passing the solidified solution through the column are, for example, a space velocity SV of 0.1 to 20 h -1 It is. In the case of the batch type, the contact time between the solidified body solution and the inorganic adsorbent is, for example, 8 to 24 hours. The temperature when the solidified solution is brought into contact with the Ln adsorbent is, for example, 10 to 40°C.

[0032] The method for separating the waste adsorbent from the solidified solution is not particularly limited, and any known solid-liquid separation method can be used. When the solidified solution is contacted with the inorganic adsorbent in a column, the solidified solution is passed through a column packed with the inorganic adsorbent, and the solidified solution (MA-containing solution) that has come into contact with the inorganic adsorbent in the column flows out of the column, while the waste adsorbent remains in the column. This allows the waste adsorbent and the solidified solution to be separated.

[0033] <Inorganic adsorbents> Typically, the inorganic adsorbent adsorbs Ln of MA and Ln due to the difference in ionic radius, that is, due to the molecular sieve effect. It is known that the ionic radius of Ln decreases as the atomic number increases, due to a phenomenon known as "lanthanide contraction." The hydrated ionic radius (values ​​ignoring the size of hydrogen atoms) of Ln and MA is shown in Table 1. In Table 1, all elements other than Am and Cm are Ln.

[0034] [Table 1]

[0035] Therefore, in step S1-5, typically, an inorganic adsorbent is selected that is difficult to adsorb the MA to be separated from Ln and is easy to adsorb Ln having a smaller ionic radius than the MA. For example, when attempting to separate Cm as MA and MA (such as Am) having a larger ionic radius than Cm from Ln, an adsorbent is selected that is difficult to adsorb ions having a hydrated ionic radius of 4.91 Å or more and is easy to adsorb Ln having a hydrated ionic radius of less than 4.91 Å (for example, 4.85 Å or less).

[0036] Examples of inorganic adsorbents include aluminosilicates (such as zeolites), borosilicates, silicotitanates, silicon dioxide, aluminum oxide, and zirconium oxide. Examples of cations that form salts in aluminosilicates, borosilicates, and silicotitanates include alkali metal ions such as sodium ions and potassium ions.

[0037] The inorganic adsorbent preferably contains silicon. Since glass generally contains silicon, when the inorganic adsorbent contains silicon, it has excellent affinity with the glass raw material, and tends to easily produce a uniform vitrified body. Examples of the silicon-containing inorganic adsorbents include aluminosilicates, borosilicates, silicotitanates, and silicon dioxide.

[0038] The content of silicon in the inorganic adsorbent in terms of silicon dioxide (SiO2) is preferably 20 to 90 mass% and more preferably 20 to 50 mass% based on the total mass of the inorganic adsorbent. If the silicon content in the inorganic adsorbent is 20 to 90 mass%, the affinity between the glass raw material and the inorganic adsorbent becomes good, and the uniformity of the obtained vitrified body becomes more excellent. The preferred range of the silicon content in the waste adsorbent calculated as silicon dioxide is the same as above.

[0039] The inorganic adsorbent may contain an alkali metal, which makes it easier to vitrify the inorganic adsorbent. Examples of inorganic adsorbents containing alkali metals include aluminosilicates, borosilicates, and silicotitanates, in which at least a portion of the cations forming the salt are alkali metal ions.

[0040] The inorganic adsorbent may contain titanium. The inorganic adsorbent containing titanium can be easily produced in pellet form by the method for producing an inorganic adsorbent described below, and separation of waste adsorbent in the adsorption treatment is easy. An example of an inorganic adsorbent containing titanium is silicotitanate.

[0041] A preferred example of the inorganic adsorbent is a crystalline metal oxide containing silicon (hereinafter, also referred to as "Si-based crystalline metal oxide"). The term "crystalline metal oxide" refers to a metal oxide that exhibits a peak intensity in X-ray diffraction (hereinafter also referred to as "XRD") method. Silicon typically constitutes the crystalline framework of Si-based crystalline metal oxides together with oxygen. The Si-based crystalline metal oxide may further contain one or more elements other than silicon and oxygen. Examples of the Si-based crystalline metal oxide include crystalline silicotitanate, zeolite, borosilicate, and silicon dioxide.

[0042] The Si-based crystalline metal oxide may contain an alkali metal. In the Si-based crystalline metal oxide containing an alkali metal, the alkali metal typically exists in the form of ions between the crystal skeleton of the Si-based crystalline metal oxide, and is ion-exchanged with Ln during Ln adsorption. The alkali metal is preferably sodium. Examples of the Si-based crystalline metal oxide containing an alkali metal include crystalline silicotitanate, zeolite, and borosilicate, in which at least a part of the cations forming a salt is an alkali metal ion.

[0043] The Si-based crystalline metal oxide may contain titanium. In the titanium-containing Si-based crystalline metal oxide, titanium typically constitutes the crystal skeleton of the Si-based crystalline metal oxide together with silicon and oxygen. The titanium-containing Si-based crystalline metal oxide may further contain elements other than silicon, titanium, and oxygen.

[0044] In the titanium-containing Si-based crystalline metal oxide, the silicon / titanium atomic ratio is preferably 0.5 or more. If the silicon / titanium atomic ratio is 0.5 or more, the titanium-containing Si-based crystalline metal oxide is easily formed. The silicon / titanium atomic ratio is preferably 50 or less, particularly preferably 2 or less.

[0045] In the titanium-containing Si-based crystalline metal oxide, a portion of silicon may be substituted with boron. When a portion of silicon is replaced by boron, the content of boron calculated as boron oxide (B2O3) is preferably 50 mass% or less based on the total mass of the titanium-containing Si-based crystalline metal oxide in terms of affinity with the glass raw materials. The preferred range of the (silicon+boron) / titanium atomic ratio is the same as the preferred range of the silicon / titanium atomic ratio described above.

[0046] The titanium-containing Si-based crystalline metal oxide preferably contains an alkali metal. When the titanium-containing Si-based crystalline metal oxide contains an alkali metal, the content of the alkali metal, calculated as an oxide, is preferably 5 to 30 mass%, and more preferably 5 to 15 mass%, based on the total mass of the titanium-containing Si-based crystalline metal oxide, from the viewpoint of ease of vitrification. The atomic ratio of alkali metal / titanium is preferably at least 1. When the atomic ratio of alkali metal / titanium is at least 1, the adsorption capacity is superior.

[0047] Examples of the Si-based crystalline metal oxides containing titanium include crystalline silicotitanates. Examples of the crystalline silicotitanates include Natisite [Na2TiSiO5] (tetragonal), ETS-4 [Na9Ti5Si 12 O 38 (OH)·12H2O](orthorhombic), AM-1(JDF-L1)[Na4Ti2Si8O 22 ·4H2O] (tetragonal crystal), etc. Here, ETS-4 is a name derived from Engelhard Corporation in the United States, and is also called Engelhard TitanoSilicate-4. AM-1 is a name derived from Aveiro University in Portugal and Manchester University in the UK, and is also called Aveiro-Manchester material number 1. JDF-L1 is a name derived from Jilin University in China and the Davy-Faraday Laboratory of the Royal Institution in the UK, and is also called Jilin-Davy-Faraday, Layered solid no.1.

[0048] The Si-based crystalline metal oxide preferably satisfies either or both of the following: (i) the crystallite size is 500 nm or less; and (ii) the aspect ratio of the crystal face in which ion exchange is performed to other crystal faces is 1 or more. The Si-based crystalline metal oxide that satisfies either or both of (i) and (ii) has a high adsorption capacity. By using an adsorbent with a high adsorption capacity, it is possible to reduce the scale of the device. In addition to using a Si-based crystalline metal oxide that satisfies either or both of the above (i) and (ii), the adsorption capacity can also be increased by increasing the surface area of ​​the inorganic adsorbent by etching treatment with H2O2 water or the like.

[0049] The crystallite size of (i) is preferably 200 nm or less. The lower limit of the crystallite size is, for example, 10 nm. The crystallite size is measured, for example, by the XRD method. When a Si-based crystalline metal oxide is produced using the dry gel conversion method described below, the crystallite size tends to be smaller than when it is produced using the hydrothermal synthesis method. The crystallite size can also be adjusted by adjusting the silicon / titanium atomic ratio or the sodium / titanium atomic ratio.

[0050] The aspect ratio (ratio of ab planes to ac planes and bc planes) of (ii) is preferably 1.5 or more. The aspect ratio is measured, for example, by the XRD method. The crystal growth direction can be controlled by adding a crystal habit modifier (in the presence of anions such as fluoride ions) during the production of Si-based crystalline metal oxides. For example, in the case of Natisite, the aspect ratio of the ab plane, which is the crystal plane where ion exchange takes place, to the other crystal planes (ac plane, bc plane) can be increased by using a crystal habit modifier to grow in the ab axis direction or suppress growth in the c axis direction.

[0051] The shape of the inorganic adsorbent is not particularly limited, but is preferably in the form of pellets. If the inorganic adsorbent is in the form of pellets, it can be used by filling it into a column. In addition, compared with the case of a powder, it has good handling properties. The size of the pellets is not particularly limited, but for example, in the case of a circle, it is preferable that the diameter is about 5 to 50 mm and the thickness is about 1 to 10 mm.

[0052] The inorganic adsorbent to be used may be a commercially available one or a prepared one. A preferred example of the production method of the titanium-containing Si-based crystalline metal oxide (hereinafter also referred to as "Si-Ti-based crystalline metal oxide") includes the following steps S5-1 to S5-3. Step S5-1: A step of dry mixing two or more kinds of raw materials including at least a first crystalline substance containing silicon and a second crystalline substance containing titanium. Step S5-2: A step of molding the mixture obtained by mixing the two or more raw materials in step S5-1. Step S5-3: A step of treating the mixture formed in step S5-2 (hereinafter also referred to as "formed body") by a dry gel conversion method.

[0053] "Step S5-1" The first crystalline substance is a silicon source for the Si-Ti crystalline metal oxide and may contain elements other than silicon. Examples of the first crystalline substance include crystalline sodium silicate (e.g., [δ-Na2Si2O5]). Two or more of these may be used in combination. The second crystalline material is a titanium source for the Si-Ti-based crystalline metal oxide and may contain elements other than titanium. For example, the second crystalline material may be crystalline sodium titanate (e.g., [Na8Ti5O 14 These may be used in combination of two or more kinds.

[0054] The mixing ratio of the first crystalline material and the second crystalline material is preferably set so that the mixture obtained in step S5-1 has an atomic ratio of silicon / titanium of 0.5 to 50. If the atomic ratio of silicon / titanium is 0.5 or more, Si-based crystalline metal oxide is easily formed, and if it is 50 or less, localized formation of silicon dioxide can be suppressed. The silicon / titanium atomic ratio is more preferably 0.5-2. In addition, since the excess silicon locally forms a silicon dioxide structure in the excess area, it is considered that the adsorption performance is not hindered.

[0055] If necessary, other raw materials may be mixed together with the first crystalline substance and the second crystalline substance. Examples of the other raw materials include a crystal habit modifier. Examples of the crystal habit modifier include alkali metal halides such as sodium fluoride, alkaline earth metal halides such as barium chloride, sodium sulfite, and sodium nitrate.

[0056] Two or more kinds of raw materials are mixed dry, that is, without adding a liquid medium such as water. This eliminates the need to evaporate and dry the liquid medium in the process of obtaining the Si-Ti-based crystalline metal oxide, and shortens the time required to produce the inorganic adsorbent. The mixing method may be a known dry mixing method. For example, when the first crystalline substance and the second crystalline substance are each in a powder form, they may be powder-mixed.

[0057] "Step S5-2" The mixture obtained in step S5-1 can be molded, for example, by press molding. The pressure in the press molding is, for example, 20 to 50 MPa. The temperature during press molding is, for example, 10 to 40°C.

[0058] The shape of the compact obtained by molding the mixture is not particularly limited, but is preferably pellet-like. If the compact is pellet-like, a pellet-like inorganic adsorbent is obtained. If the inorganic adsorbent is pellet-like, it can be used by filling it into a column. In addition, compared with the case of a powder, it has good handling properties. The size of the pellet is not particularly limited, but for example, in the case of a circle, it is preferably about 5 to 50 mm in diameter and 1 to 10 mm in thickness.

[0059] "Step S5-3" The dry gel conversion method refers to a method in which water vapor, for example pressurized water vapor, is used to promote crystallization in the gas phase. When the compact is treated by the dry gel conversion method, a Si-Ti crystalline metal oxide is produced. To treat the molded body by the dry gel conversion method, for example, water and the molded body are placed in a pressure-resistant container so as not to come into contact with each other, and then heated. The pressure vessel may be, for example, a vessel for hydrothermal synthesis. The pressure vessel is preferably made of polytetrafluoroethylene (PTFE) because of its excellent heat resistance. In order to prevent the molded body from coming into contact with water, for example, a pedestal is placed in a pressure-resistant container so that its upper surface protrudes above the water surface, and the molded body is placed on the upper surface of the pedestal. The pedestal is preferably made of PTFE because of its excellent heat resistance. The heating temperature is preferably 150° C. or higher and equal to or lower than the heat-resistant temperature of the pressure-resistant container, which is, for example, about 260° C. when made of PTFE. The heating time varies depending on the heating temperature, but is preferably 12 hours or more.

[0060] After step S5-3, if necessary, the obtained Si-Ti-based crystalline metal oxide may be washed with water and dried.

[0061] In this manner, an inorganic adsorbent containing a Si-Ti-based crystalline metal oxide and having a shape similar to that of the molded product molded in step S5-2 is obtained. The atomic ratio of silicon / titanium in the Si-Ti-based crystalline metal oxide is the same as the atomic ratio of silicon / titanium in the mixture obtained in step S5-1.

[0062] (Step S1-6: Mixing) The glass raw material mixed with the waste adsorbent in step S1-6 contains silicon. The silicon-containing glass frit usually contains an oxide containing silicon. The glass raw material may further contain elements other than silicon and oxygen, such as boron, alkali metals (lithium, sodium, potassium, etc.), alkaline earth metals (magnesium, calcium, barium, etc.), and other metal elements (aluminum, zinc, lead, etc.). The glass raw material preferably contains boron. By containing boron in the glass raw material, boron can be contained in the mixture, and in the vitrified body. In the vitrified body, boron functions as a neutron absorber. The glass raw materials can be appropriately selected from known glass raw materials and used. The glass raw materials can be used alone or in combination of two or more. The composition of the glass raw material is set taking into consideration the composition of the inorganic adsorbent and the composition of the mixture to be obtained in step S1-6.

[0063] The silicon content in the glass raw materials, calculated as silicon dioxide, is preferably 20 to 95 mass% relative to the total mass of the glass raw materials, and more preferably 50 to 70 mass%. If the silicon content in the glass raw materials is 20 to 95 mass%, the silicon content in the mixture, calculated as silicon dioxide, is easily set to 20 to 95 mass%.

[0064] The content of boron in the glass raw materials in terms of boron oxide is preferably 5 to 60 mass% and more preferably 10 to 30 mass% based on the total mass of the glass raw materials. If the content of boron in the glass raw materials is 5 to 60 mass%, the content of boron in the mixture in terms of boron oxide is easily set to 5 to 60 mass%.

[0065] An example of a preferred composition of the glass raw materials is shown below. The content of each component is the ratio to the total mass of the glass raw materials (total mass of two or more glass raw materials when two or more types are combined). However, the composition of the glass raw materials used in the present invention is not limited to this. SiO2: 20 to 95 mass% (further 50 to 70 mass%), B2O3: 5 to 60 mass% (further 10 to 30 mass%), Na2O: 0 to 20 mass% (further 0 to 10 mass%), TiO2: 0% by mass, Other oxides: 0 to 25 mass% (or even 0 to 20 mass%).

[0066] The amount of glass frit mixed into the waste adsorbent is set in consideration of the composition of the inorganic adsorbent and the composition of the mixture to be obtained in step S1-6, and is not particularly limited, but for example, the mass ratio represented by glass frit / waste adsorbent is preferably 0.1 / 1 to 3 / 1, more preferably 0.5 / 1 to 2 / 1. The more the amount of glass frit mixed, the more uniform the vitrified body tends to be, and the less the amount of glass frit mixed, the more the waste volume reduction tends to be.

[0067] The silicon content in the mixture obtained in step S1-6, calculated as silicon dioxide, is 20 to 95 mass % relative to the total mass of the mixture, preferably 30 to 60 mass %, and more preferably 40 to 55 mass %. If the silicon content in the mixture is 20 to 95 mass %, the mixture can be satisfactorily vitrified, and the obtained vitrified body has excellent uniformity.

[0068] The content of boron in the mixture calculated as boron oxide (B2O3) is preferably 5 to 60 mass% based on the total mass of the mixture, more preferably 10 to 30 mass%, and even more preferably 10 to 20 mass%. If the content of boron in the mixture is 5 mass% or more, the function as a neutron absorber is fully exhibited, and if it is 60 mass% or less, the affinity for vitrification is good and the uniformity of the obtained vitrified body is superior.

[0069] The content of the alkali metal in the mixture, calculated as alkali metal oxide, is preferably 40 mass % or less, more preferably 20 mass % or less, based on the total mass of the mixture. If the content of the alkali metal in the mixture is 40 mass % or less, the affinity for vitrification is good, and the uniformity of the obtained vitrified body is excellent.

[0070] The titanium content in the mixture, calculated as titanium dioxide (TiO2), is preferably 50 mass% or less, more preferably 20 mass% based on the total mass of the mixture. If the titanium content in the mixture is 50 mass% or less, the affinity for vitrification is good, and the uniformity of the obtained vitrified body is excellent.

[0071] An example of a preferred composition of the mixture is shown below. The content of each component is the ratio to the total mass of the mixture. SiO2: 20 to 95 mass% (further, 30 to 60 mass%, further, 40 to 55 mass%), B2O3: 5 to 60 mass% (further, 10 to 30 mass%, further, 10 to 20 mass%), Na2O: 0 to 40 mass% (further 0 to 20 mass%), TiO2: 0 to 50 mass% (further 0 to 20 mass%), Other oxides: 0 to 35 mass% (or even 0 to 20 mass%).

[0072] (Step S1-7: Vitrification) The mixture can be vitrified, for example, by melting the mixture in a melting furnace and then cooling and solidifying the molten mixture.

[0073] (Action and effect) In the treatment method having the above-described configuration, a glass raw material containing silicon is mixed with the waste adsorbent, and the silicon content in the resulting mixture, calculated as silicon dioxide, is set to 20 to 95 mass %, so that the waste adsorbent can be satisfactorily vitrified, and the resulting vitrified body has excellent uniformity.

[0074] Furthermore, in the treatment method having the above-described configuration, the waste adsorbent is vitrified without eluting Ln. Therefore, compared with the process according to the comparative example shown in FIG. 5, the amount of waste liquid generated in the MA purification step can be reduced, and the load of concentrating the waste liquid and the scale of the equipment required for the concentration can be reduced. In the process of the comparative example shown in Figure 5, solvent extraction and stripping are performed in the MA purification step, so the MA concentration in the MA-containing solution is low and it is necessary to concentrate it. However, in the treatment method configured as described above, the MA-containing solution separated from the waste adsorbent contains MA at a high concentration, so it can be used to produce MA fuel without concentrating it, and even if it is concentrated, the concentration load is small. In addition, in the process of the comparative example shown in Figure 5, solvent extraction and stripping are performed in the MA purification step, so that a low-concentration Ln-containing solution is generated, which needs to be concentrated. However, in the treatment method configured as described above, a low-concentration Ln-containing solution is not generated, and the burden of concentrating the waste liquid can be further reduced.

[0075] In addition, in the processing method configured as described above, a solution containing Ln and MA is obtained by dissolving the solidified body, so that a radioactive solution containing high concentrations of MA and Ln can be obtained without performing a concentration step as in the process of the comparative example shown in Figure 5.

[0076] In addition, the treatment method configured as above separates MA from HALW, thereby reducing the disposal burden of HALW. The solidified wastewater obtained by vitrifying the wastewater after separating MA from HALW is smaller in volume and has a shorter containment period than the solidified wastewater obtained by vitrifying the entire amount of HALW, so the burden of geological disposal is less. In addition, since the separated MA is stored as a solidified body, the storage burden is less than when it is stored in solution form. By storing the solidified body until the highly heat-generating MA contained in the solidified body has sufficiently decayed, it is also possible to eliminate the need to separate the highly heat-generating MA from the MA-containing solution.

[0077] Second Embodiment Hereinafter, a processing method according to a second embodiment of the present disclosure will be described with reference to FIG. As shown in FIG. 2, the processing method according to the second embodiment of the present invention includes: Step S2-1: A solution containing MA and Ln is obtained by separating MA together with Ln from the HALW; Step S2-2: performing a solidification process for solidifying the MA·Ln-containing solution to obtain a solidified body containing MA and Ln; Step S2-3 of storing the solidified body obtained in step S2-2; Step S2-4 of dissolving the solidified body stored in step S2-3; Step S2-5: adding a ligand that selectively coordinates with MA to the solidified solution obtained in step S1-4 to make the apparent ionic radius of MA larger than the ionic radius of Ln; Step S2-6: adsorbing Ln in the solidified solution, the apparent ionic radius of which has been increased in step S2-5, onto an inorganic adsorbent, and separating the inorganic adsorbent (waste adsorbent) with adsorbed Ln from the solidified solution, thereby purifying MA (separating MA from Ln); Step S2-7: mixing the waste adsorbent separated from the solidified solution in step S2-6 with a glass raw material containing silicon; Step S2-8 of vitrifying the mixture obtained by step S2-7; has. The processing method according to this embodiment may further include, as necessary, a step of performing the above-mentioned stabilization treatment on the solidified body after step S2-2 and before step S2-3.

[0078] The waste liquid (FP-containing solution) remaining after the separation of MA and Ln in step S2-1 is concentrated, vitrified, stored, and then disposed of in a geological repository. The solidified solution after Ln is adsorbed by the inorganic adsorbent and separated from the waste adsorbent in step S2-6 is a solution containing MA (MA-containing solution). The MA-containing solution is used for fuel production after separating the highly exothermic MA as necessary. For example, the MA-containing solution is mixed with U and Pu to obtain mixed oxides, thereby producing fuel. The obtained fuel is burned in a fast breeder reactor or the like. The vitrified waste obtained in step S2-8 is, for example, stored and disposed of in a geological repository.

[0079] (Step S2-1: Separation process) Step S2-1 is similar to step S1-1.

[0080] (Step S2-2: Solidification process) Step S2-2 is similar to step S1-2.

[0081] (Step S2-3: Storage) Step S2-3 is similar to step S1-3.

[0082] (Step S2-4: Dissolving solidified body) Step S2-4 is similar to step S1-4.

[0083] (Step S2-5: Ligand addition) As shown in Table 1, some Ln have a larger ionic radius than MA. In the first embodiment, such Ln is difficult to adsorb to the Ln adsorbent and tends to remain in the MA-containing solution. Therefore, by adding a ligand that selectively coordinates to MA to the solidified solution and making the apparent ionic radius of MA larger than the ionic radius of Ln, Ln with a larger ionic radius than MA can also be adsorbed by the Ln adsorbent.

[0084] In the HASB (Hard and Soft Acids and Bases) theory, the cation of MA easily forms a complex with a soft base such as N or S, and the cation of Ln easily forms a complex with a hard base such as O. Therefore, a soft base is used as a ligand that selectively coordinates to MA. Specific examples of ligands that selectively coordinate to MA include C2-BTP (2,6-bis(5,6-dietyl-1,2,4-triazin-3-yl)) and ADAAM (alkyldiamide amine).

[0085] The apparent ionic radius of MA is preferably 5.5 Å or more, and more preferably 10 Å or more, in terms of ease of separation from Ln shown in Table 1. The apparent ionic radius of MA can be adjusted by the ligand used.

[0086] (Step S2-6: MA purification (adsorption treatment)) Step S2-6 is similar to step S1-5. However, in step S2-6, an inorganic adsorbent is selected that is less likely to adsorb MA whose apparent ionic radius has been increased in step S2-5, and is more likely to adsorb Ln whose ionic radius is smaller than that of MA. For example, when the apparent hydrated ionic radius of MA is 10 Å or more, an adsorbent is selected that is less likely to adsorb ions whose hydrated ionic radius is 10 Å or more, and is more likely to adsorb Ln whose hydrated ionic radius is less than 10 Å (for example, 5.20 Å or less).

[0087] (Step S2-7: Mixing) Step S2-7 is similar to step S1-6.

[0088] (Step S2-8: Vitrification) Step S2-8 is similar to step S1-7.

[0089] (Action and effect) In the treatment method having the above configuration, as in the first embodiment, a glass raw material containing silicon is mixed with the waste adsorbent, and the silicon content in the resulting mixture is set to 20 to 95 mass % in terms of silicon dioxide, so that the waste adsorbent can be satisfactorily vitrified and the resulting vitrified body has excellent uniformity.

[0090] Furthermore, in the treatment method having the above configuration, the waste adsorbent is vitrified without eluting Ln, as in the first embodiment. Therefore, compared with the process according to the comparative example shown in FIG. 5, the amount of waste liquid generated in the MA purification step can be reduced, and the load of concentrating the waste liquid and the scale of the equipment required for concentration can be reduced. In addition, in the processing method configured as described above, as in the first embodiment, a solution containing Ln and MA is obtained by dissolving the solidified body, so that a radioactive solution containing high concentrations of MA and Ln can be obtained without performing a concentration step as in the process related to the comparative example shown in Figure 5. Furthermore, in the processing method configured as above, similarly to the first embodiment, the MA is separated from the HALW, so that the disposal load of the HALW can be reduced.

[0091] In addition, in the treatment method having the above-mentioned configuration, before Ln in the MA·Ln-containing solution is adsorbed by the adsorbent, the apparent ionic radius of MA is made larger than the ionic radius of Ln. Therefore, Ln, which has a larger ionic radius than MA, can also be adsorbed by the Ln adsorbent, and MA can be separated more selectively.

[0092] <Third embodiment> Hereinafter, a processing method according to a third embodiment of the present disclosure will be described with reference to FIG. As shown in FIG. 3, the processing method according to the third embodiment of the present invention includes: Step S3-1: A separation process is performed to separate MA and Ln from the HALW to obtain an MA·Ln-containing solution; Step S3-2: performing a solidification process for solidifying the MA·Ln-containing solution to obtain a solidified body containing MA and Ln; Step S3-3 of storing the solidified body obtained in step S3-2; Step S3-4 of dissolving the solidified body stored in step S3-3; Step S3-5: performing extraction treatment (solvent extraction and stripping) on ​​the solidified solution obtained in step S3-4 to purify MA (separate MA and Ln); Step S3-6: adsorbing Ln from the solution containing Ln (Ln-containing solution) separated from MA in step S3-5 onto an inorganic adsorbent, and separating the inorganic adsorbent (waste adsorbent) with the Ln adsorbed thereon from the solution; Step S3-7: mixing the waste adsorbent separated from the solution in step S3-6 with a glass raw material containing silicon; Step S3-8 of vitrifying the mixture obtained by step S3-7; has. The processing method according to this embodiment may further include, as necessary, a step of performing the above-mentioned stabilization treatment on the solidified body after step S3-2 and before step S3-3.

[0093] The waste liquid (FP-containing solution) remaining after the separation of MA and Ln in step S3-1 is concentrated, vitrified, stored, and then disposed of in a geological repository. The solution containing MA separated from Ln in step S3-5 (MA-containing solution) is used for fuel production after separating the highly exothermic MA as necessary. For example, the MA-containing solution is mixed with U and Pu to obtain a mixed oxide, which is then used to produce fuel. The obtained fuel is burned in a fast breeder reactor or the like. The vitrified waste obtained in step S3-8 is, for example, stored and disposed of in a geological repository.

[0094] (Step S3-1: Separation process) Step S3-1 is similar to step S1-1.

[0095] (Step S3-2: Solidification process) Step S3-2 is similar to step S1-2.

[0096] (Step S3-3: Storage) Step S3-3 is similar to step S1-3.

[0097] (Step S3-4: Dissolving solidified body) Step S3-4 is similar to step S1-4. When steps S3-4 to S3-6 are repeated multiple times, the solvent remaining after separating the waste adsorbent in step S3-6 can be recovered and used as the solvent for dissolving the solidified body in step S3-4. Similarly, the waste liquid remaining after the solvent extraction of MA and Ln in step S3-5 can be collected and used as a solvent for dissolving the solidified body in step S3-4.

[0098] (Step S3-5: MA purification (extraction treatment)) In step S3-4, first, solvent extraction is performed. When the solution obtained in step S3-4 is contacted with an organic solvent solution containing an extractant (extractant solution), MA and Ln migrate to the extractant solution. Then, the obtained extract is subjected to back extraction so that MA and Ln are separated, and an Ln-containing solution and an MA-containing solution are obtained.

[0099] For the solvent extraction, an extractant capable of extracting Ln and MA is used, such as the extractants listed in step S1-1. In addition, an extractant that selectively extracts MA from among Ln and MA may be used for the solvent extraction. Examples of such extractants include complexing agents that selectively form complexes with MA, and specific examples include phosphorus-containing extractants such as DIDPA and CMPO, DGA (diglycolamide) extractants such as TDDGA (tetradecyl DGA) and TDdDGA (tetradodecyl DGA), HONTA (hexaoctylnitrilotriacetamide), and ADAAM (EH) (alkyldiamide amine). The extractant may be used alone or in combination of two or more kinds.

[0100] The organic solvent can be appropriately selected depending on the extractant used. It is desirable that the organic solvent is reusable, inexpensive, and resistant to radiation degradation. A specific example of the organic solvent is n-dodecane. The organic solvent may be used alone or in combination of two or more kinds.

[0101] In the back extraction process, for example, the extract is contacted with an aqueous solution containing nitric acid (stripping agent). This causes MA and Ln in the extract to migrate to the aqueous solution. At this time, MA and Ln can be transferred separately to the aqueous solution by changing the nitric acid concentration or adding an additive such as diethylenetriaminepentaacetic acid (DTPA). On the other hand, the organic solvent in the extract does not migrate to the aqueous solution but remains in the extract, so it can be reused.

[0102] In step S3-5, as described above, the waste liquid remaining after extracting MA and Ln from the solution obtained in step S3-4 is recovered and can be used in step S3-4.

[0103] (Step S3-6: Adsorption process) Step S3-6 is similar to step S1-5, except that the Ln-containing solution obtained in step S3-5 is used instead of the solidified solution.

[0104] In this embodiment, since MA and Ln have already been separated in step S2-5, the inorganic adsorbent used in step S2-6 may be one that non-selectively adsorbs Ln and MA. Such an inorganic adsorbent is less expensive than one that selectively adsorbs Ln because it requires fewer functions.

[0105] In step S3-6, as described above, the solvent remaining after separating Ln from the Ln-containing solution is recovered and can be used in step S3-4.

[0106] (Step S3-7: Mixing) Step S3-7 is similar to step S1-6.

[0107] (Step S3-8: Vitrification) Step S3-8 is similar to step S1-7.

[0108] (Action and effect) In the treatment method having the above configuration, as in the first embodiment, a glass raw material containing silicon is mixed with the waste adsorbent, and the silicon content in the resulting mixture is set to 20 to 95 mass % in terms of silicon dioxide, so that the waste adsorbent can be satisfactorily vitrified and the resulting vitrified body has excellent uniformity.

[0109] In the process of solvent extraction and stripping in the MA purification step, a low-concentration Ln-containing solution is generated, which needs to be concentrated before vitrification in the process according to the comparative example shown in Fig. 5. In the treatment method having the above configuration, since Ln can be separated as a solid (waste adsorbent) from the Ln-containing solution, there is no need to concentrate the low-concentration Ln-containing solution. In addition, the waste liquid after the solvent extraction and the adsorption treatment can be reused in step S3-4. Therefore, the load of concentrating the waste liquid and the scale of the equipment for concentrating the waste liquid can be reduced compared to the process according to the comparative example shown in FIG. 5. Furthermore, in the treatment method having the above configuration, the waste adsorbent is vitrified without eluting Ln, as in the first embodiment. Therefore, compared with the process according to the comparative example shown in FIG. 5, the amount of waste liquid generated in the MA purification step can be reduced, and the load of concentrating the waste liquid and the scale of the equipment required for concentration can be reduced. In addition, in the processing method configured as described above, as in the first embodiment, a solution containing Ln and MA is obtained by dissolving the solidified body, so that a radioactive solution containing high concentrations of MA and Ln can be obtained without performing a concentration step as in the process related to the comparative example shown in Figure 5. Furthermore, in the processing method configured as above, similarly to the first embodiment, the MA is separated from the HALW, so that the disposal load of the HALW can be reduced.

[0110] <Fourth embodiment> Hereinafter, a processing method according to the fourth embodiment of the present disclosure will be described with reference to FIG. As shown in FIG. 4, the processing method according to the fourth embodiment of the present invention includes: Step S4-1: A separation process is performed to separate MA and Ln from the HALW to obtain an MA·Ln-containing solution; Step S4-2 of concentrating the MA·Ln-containing solution obtained in step S4-1; Step S4-3: adsorbing Ln in the concentrated solution obtained in step S4-2 onto an inorganic adsorbent, and separating the inorganic adsorbent (waste adsorbent) with adsorbed Ln from the concentrated solution, thereby purifying MA (separating MA from Ln); Step S4-4 of mixing the waste adsorbent separated from the concentrated liquid in step S4-3 with a glass raw material containing silicon; Step S4-5 of vitrifying the mixture obtained by step S4-4; has.

[0111] The waste liquid (FP-containing solution) remaining after the separation of MA and Ln in step S4-1 is concentrated, vitrified, stored, and then disposed of in a geological repository. The solution containing MA separated from Ln in step S4-3 (MA-containing solution) is further concentrated, and the highly exothermic MA is separated as necessary, and then used for fuel production. For example, the MA-containing solution is mixed with U and Pu to obtain a mixed oxide, thereby producing fuel. The obtained fuel is burned in a fast breeder reactor or the like. The vitrified waste obtained in step S4-5 is, for example, stored and disposed of in a geological repository.

[0112] (Step S4-1: Separation process) Step S4-1 is similar to step S1-1.

[0113] (Step S4-2: Concentration) As the concentration method, a known concentration method such as evaporation concentration can be used. In step S4-2, the MA·Ln-containing solution is concentrated so that the concentration of the MA·Ln-containing solution after concentration in step S4-2 is similar to that of the HALW. The same applies to the concentration of the MA-containing solution.

[0114] (Step S4-3: MA purification (adsorption treatment)) Step S4-3 is similar to step S1-5.

[0115] (Step S4-4: Mixing) Step S4-4 is similar to step S1-6.

[0116] (Step S4-6: Vitrification) Step S4-6 is similar to step S1-7.

[0117] (Action and effect) In the treatment method having the above configuration, as in the first embodiment, a glass raw material containing silicon is mixed with the waste adsorbent, and the silicon content in the resulting mixture is set to 20 to 95 mass % in terms of silicon dioxide, so that the waste adsorbent can be satisfactorily vitrified and the resulting vitrified body has excellent uniformity.

[0118] Furthermore, in the treatment method having the above configuration, the waste adsorbent is vitrified without eluting Ln, as in the first embodiment. Therefore, compared with the process according to the comparative example shown in FIG. 5, the amount of waste liquid generated in the MA purification step can be reduced, and the load of concentrating the waste liquid and the scale of the equipment required for concentration can be reduced. Furthermore, in the processing method configured as above, similarly to the first embodiment, the MA is separated from the HALW, so that the disposal load of the HALW can be reduced.

[0119] <Other embodiments> The above describes in detail an embodiment of the processing method of the present disclosure with reference to the drawings. However, the specific configuration is not limited to this embodiment, and design changes and the like that do not deviate from the gist of the present invention are also included.

[0120] In each of the above first, second and third embodiments, the MA·Ln-containing solution obtained by the HALW separation treatment may be concentrated and then subjected to a solidification treatment. In the fourth embodiment, step S4-2 may be omitted, and the MA·Ln-containing solution may be subjected to step S4-3 without being concentrated.

[0121] In the above third embodiment, before step S3-6, a step of adding a ligand that selectively coordinates to MA to the Ln-containing solution obtained by step S3-5 to make the apparent ionic radius of MA larger than the ionic radius of Ln may be included. In the above fourth embodiment, before step S4-3, a step may be included in which a ligand that selectively coordinates to MA is added to the concentrated solution obtained in step S4-2 to make the apparent ionic radius of MA larger than the ionic radius of Ln.

[0122] The waste adsorbent treated by the treatment method of the present disclosure may have adsorbed only Ln, only MA, or both Ln and MA. In each of the above first, second and third embodiments, Ln and MA in the MA·Ln-containing solution obtained by the separation treatment of the HALW may be adsorbed onto an inorganic adsorbent, and the inorganic adsorbent with adsorbed Ln and MA may be separated from the MA·Ln-containing solution and vitrified.

[0123] <Additional Notes> The processing method described in each embodiment can be understood, for example, as follows. (1) The treatment methods according to the above-mentioned first to fourth embodiments include steps (S1-6, S2-7, S3-7, S4-4) of mixing a glass raw material containing silicon with a waste adsorbent (an inorganic adsorbent having adsorbed Ln and / or MA), and steps (S1-7, S2-8, S3-8, S4-5) of vitrifying the mixture obtained by the step of mixing the glass raw materials, in which the content of silicon in the mixture in terms of silicon dioxide is 20 to 95 mass% with respect to the total mass of the mixture.

[0124] In this processing method, the waste adsorbent is mixed with a glass raw material containing silicon, and the silicon content, calculated as silicon dioxide, is set to 20 to 95 mass %, so that the waste adsorbent can be vitrified well and the obtained vitrified body has excellent uniformity.

[0125] (2) In the treatment methods according to the above first to fourth embodiments, the content of silicon in the glass raw material, calculated as silicon dioxide, is preferably 20 to 95 mass % based on the total mass of the glass raw material. By using such a glass raw material, the silicon content in the mixture, calculated as silicon dioxide, can be easily adjusted to 20 to 95 mass % relative to the total mass of the mixture.

[0126] (3) In the processing methods according to the above first to fourth embodiments, it is preferable that the glass raw material contains boron, and the content of boron in the mixture, calculated as boron oxide, is 5 to 60 mass% with respect to the total mass of the mixture. By including boron in the glass raw material, boron can be incorporated into the vitrified waste, where boron functions as a neutron absorber. When the boron content in the mixture is 5 mass % or more, the function as a neutron absorber is fully exhibited, and when the content is 60 mass % or less, the homogeneity of the obtained vitrified body is superior.

[0127] (4) In the treatment methods according to the first to fourth embodiments, it is preferable that the waste adsorbent contains silicon, and the content of silicon in the waste adsorbent, calculated as silicon dioxide, is 20 to 90 mass% relative to the total mass of the waste adsorbent. Such a waste adsorbent has a good affinity with glass raw materials, and the uniformity of the obtained vitrified body is excellent.

[0128] (5) In the treatment methods according to the first to fourth embodiments, the content of alkali metals in the mixture, calculated as alkali metal oxide, is preferably 40 mass % or less based on the total mass of the mixture. When the content of the alkali metal in the mixture is 40 mass % or less, the compatibility with vitrification is good, and the homogeneity of the obtained vitrified body is superior. When the mixture contains an alkali metal, the alkali metal may come from the spent adsorbent, from the glass frit, or from both.

[0129] (6) In the treatment methods according to the first to fourth embodiments, the waste adsorbent preferably contains an alkali metal. The presence of an alkali metal in the waste adsorbent makes the mixture easier to vitrify.

[0130] (7) In the treatment methods according to the first to fourth embodiments, the titanium content in the mixture, calculated as titanium dioxide, is preferably 50 mass % or less based on the total mass of the mixture. When the titanium content in the mixture is 50 mass % or less, the affinity with vitrification is good, and the homogeneity of the obtained vitrified body is superior. When the mixture contains titanium, the titanium may come from the spent adsorbent, from the glass frit, or from both, but typically comes from the spent adsorbent.

[0131] (8) In the treatment methods according to the first to fourth embodiments, the waste adsorbent preferably contains titanium. The inorganic adsorbent containing titanium can be easily produced in pellet form by the above-mentioned dry gel conversion method, and waste adsorbent can be easily separated in the adsorption treatment. EXAMPLES

[0132] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples.

[0133] [Test Example 1] (Manufacture of inorganic adsorbents) Crystalline sodium titanate ([Na8Ti5O 14 ]) and crystalline sodium silicate ([δ-Na2Si2O5]) were weighed and mixed so that the silicon / titanium atomic ratio was 1. The resulting mixture was placed in a molding machine and compressed under a pressure of 400 kgf / cm 2 The mixture was pressed into a circular molded body having a diameter of 20 mm and a thickness of 5 mm. Water was poured into a PTFE container for hydrothermal synthesis. A PTFE pedestal was placed in the container so that the molded body would not come into contact with water, and the molded body was set on the pedestal. The molded body was then heated at 200°C for 20 hours. The molded body was then removed from the container, washed with water, and dried at 80°C for 5 hours to obtain an inorganic adsorbent.

[0134] The inorganic adsorbent produced in Production Example 1 and Natisite produced by hydrothermal synthesis were analyzed and compared by XRD. As a result, it was observed that the inorganic adsorbent obtained in Production Example 1 and Natisite produced by the conventional method had similar peaks in the XRD spectrum chart. From this, it was confirmed that the inorganic adsorbent produced in Production Example 1 contains Natisite [Na2TiSiO5]. The composition of the obtained inorganic adsorbent is shown in Table 2.

[0135] [Table 2]

[0136] (Preparation of glass raw materials) Various oxides were mixed to prepare glass raw material powders having the compositions shown in Table 3. Other oxides included Al2O3, CaO, ZnO, and Li2O.

[0137] [Table 3]

[0138] (Mixing glass raw materials and inorganic adsorbents) The above-mentioned glass frit powder and the above-mentioned inorganic adsorbent were mixed in a mass ratio of glass frit / inorganic adsorbent = 2 / 1. The composition of the obtained mixture is shown in Table 4.

[0139] [Table 4]

[0140] (Visiting the mixture) The mixture was placed in a crucible (inner diameter φ: 30-40 mm, height: 30 mm, material: Inconel), and the crucible was placed in a tubular furnace and heat-treated at 1200° C. for 2-3 hours. After that, it was rapidly air-cooled to obtain a vitrified body.

[0141] (evaluation) The surface and cross-section of the vitrified bodies were evaluated for the presence or absence of bubbles and segregation by visual observation. As a result, no significant bubbles were observed, the color of the bodies was uniform, and no segregation was observed. In addition, the element distribution in the cross section of the vitrified body was analyzed by EPMA (Electron Probe Microanalyzer). As a result, it was confirmed that the main components of the glass raw material, Si and B, and the main components of the inorganic adsorbent, Ti and Na, were uniformly distributed.

Claims

1. A step of mixing a glass raw material containing silicon with an inorganic adsorbent having lanthanides and / or minor actinides adsorbed thereon; vitrifying the mixture obtained by the step of mixing the glass raw materials; having The inorganic adsorbent contains silicon, and the content of silicon in the inorganic adsorbent in terms of silicon dioxide is 20 to 90 mass% based on the total mass of the inorganic adsorbent; A method for treating an inorganic adsorbent having a lanthanide and / or a minor actinide adsorbed thereon, wherein the content of silicon in the mixture, calculated as silicon dioxide, is 20 to 95 mass% based on the total mass of the mixture.

2. 2. The method according to claim 1, wherein the content of silicon in the glass frit is 20 to 95 mass% based on the total mass of the glass frit, calculated as silicon dioxide.

3. The glass frit contains boron, The method according to claim 1 or 2, wherein the content of boron in the mixture, calculated as boron oxide, is 5 to 60 mass% based on the total mass of the mixture.

4. The method according to any one of claims 1 to 3, wherein the content of the alkali metal in the mixture, calculated as alkali metal oxide, is 40 mass % or less based on the total mass of the mixture.

5. The method according to any one of claims 1 to 4, wherein the inorganic adsorbent contains an alkali metal.

6. The method according to any one of claims 1 to 5, wherein the content of titanium in the mixture, calculated as titanium dioxide, is 50 mass % or less based on the total mass of the mixture.

7. The method according to any one of claims 1 to 6, wherein the inorganic adsorbent comprises titanium.

Citation Information

Patent Citations

  • Method of processing radioactive waste

    JP1984099399A

  • Solidified body of radioactive condensed waste substance and manufacture of the same

    JP2001027694A

  • Radioactive substance adsorbent, method of manufacturing the same, and apparatus of manufacturing the same

    JP2015064252A

  • Method for producing radioactive waste solidified body

    JP2019174482A

  • Method for separating lanthanoid from radioactive solution

    JP2020204518A