Ionic composite material containing lignosulfonic acid, cationic polymer and compound having aldehyde group as components

By combining lignin sulfonic acid with a compound having an aldehyde group and a cationic polymer, the composite material achieves enhanced strength, modulus, and water resistance, addressing the limitations of existing materials.

JP7563724B2Active Publication Date: 2024-10-08NATIONAL INSTITUTE OF ADVANCED INDUSTRIAL SCIENCE & TECHNOLOGY
View PDF 10 Cites 0 Cited by

Patent Information

Application Number
JP2020081024
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-06-04
Filing Date
2020-05-01
Publication Date
2024-10-08
Estimated Expiration
2040-05-01

AI Technical Summary

Technical Problem

Existing ionic composite materials containing lignin sulfonic acid and cationic polymers lack sufficient strength, Young's modulus, and water resistance.

Method used

Combining lignin sulfonic acid with a compound having an aldehyde group and a cationic polymer to form an ionic composite material, which includes specific components and manufacturing methods to enhance strength, modulus, and water resistance.

Benefits of technology

The resulting composite material exhibits improved strength, Young's modulus, and water resistance, making it suitable for various applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007563724000004
    Figure 0007563724000004
  • Figure 0007563724000005
    Figure 0007563724000005
  • Figure 0007563724000006
    Figure 0007563724000006
Patent Text Reader

Abstract

To provide a new ion composite material that has ligninsulfonic acid and a cationic polymer as components, can be molded in various shapes, and has flexibility and elasticity, and dramatically improve its strength, Young's modulus and water resistance.SOLUTION: It is found that a combination of ligninsulfonic acid and a cationic polymer with a compound having an aldehyde group gives excellent strength, Young's modulus and water resistance.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an ionic composite material comprising a combination of lignin sulfonic acid, which is an anionic polymer derived from wood, a cationic polymer, and a compound having an aldehyde group. [Background technology]

[0002] Conventionally, in order to effectively utilize plant biomass, attempts have been made widely to use lignin, one of the main components constituting plants, or its derivatives as moldable materials. For example, Patent Document 1 describes a composite of lignin and polystyrene resin, and Patent Document 2 describes a moldable ion-complex clay composition consisting of lignin sulfonic acid, which is a cation-exchange type (i.e., anionic) polymer, and an anion-exchange type (i.e., cationic) clay mineral. The inventors have discovered that an ionic composite material that can be molded into a variety of shapes, is highly elastic, and has excellent self-repairing ability can be obtained from a water-soluble or water-suspendable ionic complex formed by mixing lignin sulfonic acid, a lignin-derived compound that can be obtained during the production of pulp by the sulfite method or by the sulfuric acid treatment of lignin, with a cationic polymer in an aqueous solvent (Patent Document 3). [Prior art documents] [Patent documents]

[0003] [Patent Document 1] Japanese Patent Application Publication No. 11-152410 [Patent Document 2] JP 2006-133299 A [Patent Document 3] JP 2019-112526 A [Non-patent literature]

[0004] [Non-Patent Document 1] Green Chemistry;2016;18(20);5607-5620 [Non-Patent Document 2] Progress in Polymer Science;2014;39(7);1266-1290 Summary of the Invention [Problem to be solved by the invention]

[0005] The present invention aims to solve the problem of dramatically improving the strength, Young's modulus, and water resistance of a new ionic composite material described in Patent Document 3, which is made of lignin sulfonic acid and a cationic polymer as components and can be molded into a variety of shapes, and which has flexibility and elasticity. [Means for solving the problem]

[0006] In the course of conducting research into Patent Document 3, the present inventors discovered that a combination of lignin sulfonic acid and a compound having an aldehyde group in a cationic polymer exhibits superior strength, Young's modulus, and water resistance compared to the ionic composite material having the combination described in the examples of Patent Document 3. The present invention was made based on these findings by the present inventors.

[0007] That is, this application provides the following inventions. [1] An ionic composite material comprising lignin sulfonic acid, a derivative thereof, or a salt thereof, a cationic polymer (excluding ε-polylysine), a derivative thereof, or a salt thereof, and a compound having an aldehyde group. [2] The ionic composite material according to [1], characterized in that it has elasticity. [3] The ionic composite material according to [1] or [2], wherein the salt of lignosulfonic acid or a derivative thereof is a metal salt. [4] The ionic composite material according to [3], wherein the metal salt is selected from the group consisting of sodium salts, calcium salts, and magnesium salts. [5] The ionic composite material according to any one of [1] to [4], wherein the cationic polymer is a polymer having, in its molecule, at least one functional group selected from the group consisting of a primary, secondary or tertiary amino group, a quaternary ammonium group and an imino group. [6] The ionic composite material according to any one of [1] to [5], wherein the cationic polymer is a polymer composed of a single monomer having at least one functional group selected from the group consisting of a primary, secondary or tertiary amino group, a quaternary ammonium group, and an imino group. [7] The ionic composite material according to any one of [1] to [6], wherein the compound having an aldehyde group is a saccharide exhibiting reducing property or an aldehyde. [8] The ionic composite material according to [7], wherein the saccharide exhibiting reducing properties is fructose, arabinose, glucose, lactose, maltose, ribose, xylose, mannose or galactose. [9] The ionic composite material according to [7], wherein the aldehyde is an aliphatic dialdehyde or an aliphatic aldehyde.

[10] The ionic composite material according to [9], wherein the aliphatic dialdehyde is glutaraldehyde.

[11] A method for producing an ionic composite material according to any one of [1] to

[10] , comprising: a step of mixing lignin sulfonic acid, a derivative thereof, or a salt thereof, a cationic polymer (excluding ε-polylysine), a derivative thereof, or a salt thereof, and a compound having an aldehyde group in a solvent to form an ionic composite material in the solvent; and a step of removing the solvent from the solvent or suspension containing the ionic composite material.

[12] A solution or suspension containing an ionic composite material formed from lignosulfonic acid, a derivative thereof, or a salt thereof, a cationic polymer, a derivative thereof, or a salt thereof, a compound having an aldehyde group, and a solvent.

[13] The solution or suspension according to

[12] , wherein the solvent is water.

[14] An ionic composite material formed from lignin sulfonic acid, a derivative thereof, or a salt thereof, a cationic polymer, a derivative thereof, or a salt thereof, and a compound having an aldehyde group, the material further containing an organic solvent.

[15] An adhesive comprising the ion composite material according to any one of [1] to

[10] or the material according to

[14] . Effect of the Invention

[0008] Specifically, it was confirmed that the combination of lignin sulfonic acid, a cationic polymer, and a compound having an aldehyde group exhibited excellent strength, Young's modulus, and water resistance. [Brief description of the drawings]

[0009] [Figure 1] A photograph of a test piece punched out in the shape of a dumbbell (No. 8, JIS K 6251) obtained from a composite of sodium lignosulfonate, poly(ethyleneimine) and lactose is shown. [Diagram 2] Photographs showing the results of a water resistance test of a composite consisting of sodium lignosulfonate, poly(ethyleneimine) and reducing sugar are shown. [Diagram 3] A photograph of a test piece punched out in the shape of a dumbbell (No. 8, JIS K 6251) obtained from a composite of sodium lignosulfonate, poly(allylamine) and fructose is shown. [Figure 4] Photographs showing the results of a water resistance test of a composite consisting of sodium lignosulfonate, poly(allylamine) and reducing sugar are shown. [Diagram 5] Photographs showing the results of elasticity evaluation of a composite composed of lignosulfonic acid sodium salt, poly(ethyleneimine) and fructose are shown. [Figure 6] Photographs showing the results of elasticity evaluation of a composite composed of lignosulfonic acid sodium salt, poly(allylamine) and fructose are shown. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010] Lignosulfonic acid is derived from lignin, which is one of the main components constituting plants along with polysaccharides such as cellulose, and is produced as a by-product by sulfonation of lignin when pulp is produced from plants by the sulfite method, for example. In the present invention, the lignosulfonic acid is not particularly limited, and may be the lignosulfonic acid itself produced as a by-product in this manner, or it may be modified lignosulfonic acid or partially desulfonated lignosulfonic acid, which are lignosulfonic acid that has been modified or partially desulfonated. The modified lignosulfonic acid may be, for example, lignosulfonic acid in which the content of functional groups has been changed by treating lignosulfonic acid with an acid or alkali. Partially desulfonated lignosulfonic acid is a lignosulfonic acid that has a sulfo group (-SO 3 H or -SO 3 - It is preferable that the desulfonation of the lignosulfonic acid in the entire ionic composite material is such that 1% or more of the total sulfo groups in the ionic composite material are desulfonated when it is assumed that partial desulfonation has not occurred.

[0011] In the present invention, examples of the lignin sulfonic acid derivatives include, but are not limited to, lignin sulfonic acid derivatives obtained by applying the technique of modifying the hydroxyl groups of lignin with polyethylene glycol as described in Non-Patent Document 1, lignin sulfonic acid derivatives obtained by applying the technique of modifying the carboxyl groups of lignin with an epoxy group-containing compound as described in Non-Patent Document 2, and lignin sulfonic acid derivatives obtained by applying the technique of modifying the phenolic hydroxyl groups of lignin with a fatty acid or aromatic carboxylic acid as described in Non-Patent Document 2.

[0012] In the present invention, the salt of lignosulfonic acid or a derivative thereof is preferably a metal salt, and from the viewpoint of water solubility, the metal salt is preferably selected from the group consisting of sodium salts, calcium salts, and magnesium salts.

[0013] The cationic polymer used in the present invention is not particularly limited except that it does not contain ε-polylysine, but examples thereof include polymers having at least one functional group selected from primary, secondary or tertiary amino groups, quaternary ammonium groups and imino groups in the molecule. Polymers made of a single monomer having at least one functional group selected from primary, secondary or tertiary amino groups, quaternary ammonium groups and imino groups are preferred. Specific examples of such cationic polymers include poly(ethyleneimine), poly(allylamine), poly(diallyldimethylammonium chloride), chitosan, cationic cellulose, cationic carboxymethylcellulose, cationic starch, cationic hyaluronic acid, cationic guar gum, α-polylysine, α-polyornithine, δ-polyornithine, lysine-containing proteins, poly(vinyl N-methylpyridine), poly{[3-(methacryloylamino)propyl]trimethylammonium}, poly[(3-a Examples of the cationic polymer include poly{[2-(acrylamidopropyl)trimethylammonium], poly{[2-(methacryloyloxy)ethyl]trimethylammonium}, poly{[2-(acryloyloxy)ethyl]trimethylammonium}, or cationic polymers in which the primary, secondary or tertiary amino groups have been converted to quaternary ammonium groups, and further examples include cationic polymers having imino groups, such as polyarginine, poly(hexamethylene biguanide), polyhexamethylene guanidine, cyanophycin, and arginine-containing proteins. The weight-average molecular weight of the cationic polymer is 30 It is preferably 0 to 10,000,000. Furthermore, examples of the derivatives of cationic polymers include cationic polymers that have been made to have a high molecular weight by crosslinking or condensing cationic polymers together. From the viewpoint of water solubility, the cationic polymer used in the present invention may be an inorganic acid salt such as a hydrochloride, or an organic acid salt such as an acetate, of the above-mentioned cationic polymer.

[0014] The compound having an aldehyde group used in the present invention is not particularly limited as long as it has an aldehyde group, and examples thereof include sugars and aldehydes that exhibit reducing properties.

[0015] Examples of reducing sugars include fructose, arabinose, glucose, lactose, maltose, ribose, xylose, mannose, galactose, dihydroxyacetone, ribulose, psicose, erythrose, and oligosaccharides and polysaccharides containing these sugars. Preferred are fructose, arabinose, glucose, lactose, maltose, ribose, xylose, mannose, or galactose, more preferred are fructose, arabinose, glucose, or lactose, and particularly preferred are fructose or arabinose. In the present invention, oligosaccharides refer to oligosaccharides, which are not limited to those in which 2 to 10 monosaccharides are bound by glycosidic bonds, and polysaccharides refer to those in which at least two monosaccharides are bound by glycosidic bonds. Oligosaccharides are included in polysaccharides.

[0016] Aldehydes include, for example, aliphatic dialdehydes, aliphatic aldehydes, or aromatic aldehydes. An example of the aliphatic dialdehyde is glutaraldehyde. Examples of aliphatic aldehydes include formaldehyde, acetaldehyde, propionaldehyde, butyraldehyde, pentanal, hexanal, heptanal, octanal, nonanal, decanal, undecanal, dodecanal, glyceraldehyde, isovaleric aldehyde, and crotonaldehyde. Examples of aromatic aldehydes include salicylaldehyde, cinnamaldehyde, furfural, methylfurfural, naphthaldehyde, phenylbenzaldehyde, acetoxybenzaldehyde, methoxybenzaldehyde, tolualdehyde, and syringaldehyde. The aldehyde is preferably glutaraldehyde or butyraldehyde.

[0017] "Containing lignosulfonic acid, a derivative thereof, or a salt thereof, a cationic polymer, a derivative thereof, or a salt thereof, and a compound having an aldehyde group" can further include any other components other than "lignosulfonic acid, a derivative thereof, or a salt thereof, a cationic polymer, a derivative thereof, or a salt thereof, and a compound having an aldehyde group". It is also possible for the composition to consist only of "lignosulfonic acid, a derivative thereof, or a salt thereof, a cationic polymer, a derivative thereof, or a salt thereof, and a compound having an aldehyde group".

[0018] The composition ratio of lignosulfonic acid, its derivatives, or their salts to the cationic polymer, its derivatives, or their salts in the ionic composite material is not particularly limited, but the weight ratio of the weight of lignosulfonic acid or the weight of a derivative of lignosulfonic acid, a salt of lignosulfonic acid, or a salt of a derivative of lignosulfonic acid in lignosulfonic acid equivalent to the weight of the cationic polymer or the weight of a derivative of a cationic polymer, a salt of a cationic polymer, or a salt of a derivative of a cationic polymer in cationic polymer equivalent is preferably 1:10 to 10:1, and more preferably 1:4 to 4:1. In addition, the weight of the compound having an aldehyde group in the ion composite material is lignin sulfonate. The weight of the cationic polymer is preferably 1 / 100 to 1 / 2, and more preferably 1 / 100 to 1 / 10, of the total weight of the cationic polymer, or the weight of the derivative of the cationic polymer, the salt of the cationic polymer, or the salt of the derivative of the cationic polymer in terms of cationic polymer.

[0019] The water content in the ionic composite material is 3 to 95% by weight, preferably 5 to 40% by weight, and more preferably 10 to 30% by weight of the entire ionic composite material. This water content allows the ionic composite material to have elasticity. The moisture content is adjusted by holding a solution or suspension containing an ion complex formed by lignin sulfonic acid, a derivative thereof, or a salt thereof, a cationic polymer, a derivative thereof, or a salt thereof, and a compound having an aldehyde group in the atmosphere or under controlled humidity conditions. In this case, evaporation of moisture may be promoted by heating using a thermostatic bath or a hot plate. Alternatively, the solution or suspension containing this ion complex may be dropped into an organic solvent to obtain a complex precipitation, and the obtained complex may be held in the atmosphere or under controlled humidity conditions as necessary to adjust the moisture content.

[0020] In the present invention, "having elasticity" refers to a property in which, when a dumbbell-shaped test piece (No. 8, JIS K 6251) is cut out from a material, tension is applied to the test piece, and the dumbbell-shaped test piece is deformed to a degree that does not break, or is deformed until the dumbbell-shaped test piece breaks, and then the tension is completely removed and the dumbbell-shaped test piece is left to stand for a predetermined time, the deformation amount after the test piece is left to stand is 50% or less of the maximum deformation amount when tension is applied. It is preferable that the deformation amount after the test piece is left to stand is 30% or less of the maximum deformation amount when tension is applied. The predetermined time for leaving the test piece to stand after the tension is completely removed and before the deformation amount of the test piece is measured is not particularly limited, but it is preferable to leave the test piece to stand for at least about 1 hour in order to properly evaluate the elasticity. Specifically, it may be 1 hour, 72 hours, or longer.

[0021] The ionic composite material of the present invention can be processed into, for example, a sheet. The thickness of the sheet is not particularly limited, but is preferably 1 to 10 mm.

[0022] Another aspect of the present invention is a method for producing an ionic composite material, comprising the steps of mixing lignosulfonic acid, a derivative thereof, or a salt thereof, a cationic polymer, a derivative thereof, or a salt thereof, and a compound having an aldehyde group in a solvent to form an ionic composite in the solvent, and removing the solvent from a solution or suspension containing the ionic composite. The step of forming an ion complex is not particularly limited, but may be, for example, a step of forming an ion complex by mixing lignosulfonic acid, a derivative thereof, or a salt thereof, a cationic polymer, a derivative thereof, or a salt thereof, and a compound having an aldehyde group in a solvent, or a step of forming an ion complex by mixing a solution containing lignosulfonic acid, a derivative thereof, or a salt thereof, a solution containing a cationic polymer, a derivative thereof, or a salt thereof, and a solution containing a compound having an aldehyde group. In the step of forming an ion complex, the order in which the components are mixed and the mixing conditions for the components, such as temperature, humidity, and time, are not particularly limited as long as a significantly non-uniform composition is not formed. The step of removing the solvent refers to, for example, a step of removing the solvent from a solution or suspension containing the ion complex by volatilization, or, in the case where the solvent is water, a step of introducing the aqueous solution or aqueous suspension into an organic solvent to precipitate the ion complex in the organic solvent, and then removing the solvent.

[0023] The solvent used in the present invention is water, methanol, ethanol, isopropyl Preferred are organic solvents miscible with water, such as alcohol, ethylene glycol, glycerin, polyethylene glycol, formic acid, acetic acid, propionic acid, acetone, acetonitrile, tetrahydrofuran, dimethylsulfoxide, dimethylformamide, and dioxane, and particularly preferred is water.

[0024] Another aspect of the present invention is a solution or suspension containing an ionic complex formed in a solvent by mixing, in the solvent, lignosulfonic acid, a derivative thereof, or a salt thereof, a cationic polymer, a derivative thereof, or a salt thereof, and a compound having an aldehyde group. The solution or suspension containing the ion complex can be prepared, for example, by mixing aqueous solutions of lignosulfonic acid, its derivatives, or their salts, a cationic polymer, its derivatives, or their salts, and a compound having an aldehyde group, or by mixing powder of lignosulfonic acid, its derivatives, or their salts with an aqueous solution of a cationic polymer, its derivatives, or their salts, and a compound having an aldehyde group. The solution or suspension containing the ion complex thus prepared is placed on a flat plate such as a petri dish, and the solvent is then evaporated to obtain a sheet-like ion complex.

[0025] When the solvent is water, the ion complex can be recovered as a precipitate by adding an aqueous solution or aqueous suspension containing the ion complex thus prepared to an organic solvent.

[0026] The resulting ion complex can be subjected to a tensile test to measure the maximum stress and the breaking elongation. Based on the results of the tensile test, the toughness, which is expressed as the area under the stress-strain curve, can be calculated.

[0027] The water resistance level of the ionic complex can be determined by performing a water resistance test on the obtained ionic complex. That is, a test piece of a given mass is cut out from the ionic complex, and the test piece is immersed in pure water and shaken for a given time. The less coloring of the supernatant after the given time has elapsed, the less the amount of sodium lignin sulfonate eluted from the ionic complex, which means that the water resistance of the ionic complex is high.

[0028] Another aspect of the present invention is an adhesive comprising an ionic composite material comprising lignosulfonic acid, a derivative thereof, or a salt thereof, a cationic polymer, a derivative thereof, or a salt thereof, and a compound having an aldehyde group.

[0029] The water content in the adhesive is not particularly limited, but is usually 0.1 to 95% by weight, and preferably 2 to 30% by weight.

[0030] The adhesive of the present invention may be a one-part adhesive or an adhesive consisting of a single agent. By using a one-part adhesive or an adhesive consisting of a single agent, it is possible to achieve more stable and stronger adhesion with less uneven application compared to a two-part adhesive.

[0031] The adhesive of the present invention, which contains lignin sulfonic acid, its derivatives, or their salts, a cationic polymer, its derivatives, or their salts, and a compound having an aldehyde group, can be prepared by mixing these components by an appropriate method. There are no particular limitations on the order in which each component is mixed, or on the mixing conditions for the composition, such as temperature, humidity, or time, as long as the composition does not become significantly non-uniform.

[0032] The adhesive can be used, for example, by placing or applying the ionic complex prepared by the above method on the substrates to be bonded, and then sandwiching the ionic complex between the substrates to bond them. Here, the substrate is not particularly limited, but examples of the substrate that can be used include a stainless steel plate, an aluminum plate, a polypropylene plate, and a wooden plate. Preferably, bonding can be performed by applying pressure while heating using a device such as a hot press, which allows strong bonding to be achieved more quickly. In the hot press device, the heating temperature is not particularly limited, but is, for example, 50 to 110°C. The pressure is not particularly limited, but is, for example, 0.01 to 10 MPa, or 0.05 to 0.5 MPa. The heating and pressurizing time is not particularly limited, but is, for example, 30 seconds to 3 minutes. Furthermore, after sandwiching the ion complex between the substrates, or after heating and pressurizing with a hot press device, an operation for volatilizing the solvent may be performed. In the operation for volatilizing the solvent, the temperature is not particularly limited, but is, for example, 10 to 90°C or ambient temperature. The humidity is not particularly limited, but is, for example, 20 to 80%. The time for volatilizing the solvent is not particularly limited, but is, for example, 1 hour or more.

[0033] The adhesive strength test is not particularly limited, but can be carried out, for example, by the following method. A complex of lignosulfonic acid sodium salt, a cationic polymer, and a compound having an aldehyde group (9 mg) was placed on a substrate with an overlapping area of ​​1 cm 2The substrate is sandwiched between two substrates (5 cm long, 1 cm wide, 2 mm thick) so that the substrate is sandwiched between two substrates. The substrate is heated in a hot press at 80°C and 0.2 MPa for 2 minutes. After the substrate is cooled in the air, the solvent is evaporated in a constant temperature and humidity chamber at 30°C and 50% humidity for more than 24 hours. The resulting bonded substrate is subjected to a tensile test to measure the tensile shear adhesive strength (maximum stress), which can be used as an index of adhesive strength. EXAMPLES

[0034] Next, the present invention will be described more specifically with reference to examples, but the present invention is not limited to these examples.

[0035] Example 1 Preparation of a Complex of Lignosulfonic Acid Sodium Salt, Poly(ethyleneimine) and Lactose 7.68 mL of a 25 wt% aqueous solution of Pearlex NP (high-purity, high-molecular-weight lignosulfonic acid sodium salt, manufactured by Nippon Paper Industries Co., Ltd.) and 253 mg of lactose monohydrate (Wako Pure Chemical Industries, special grade) were mixed and stirred until the lactose was completely dissolved. 7.2 mL of a 40 wt% aqueous solution of poly(ethyleneimine) (Wako Pure Chemical Industries, molecular weight 10,000) was added to this solution and mixed uniformly. This mixture was transferred to a fluororesin petri dish (size: 6 cm x 6 cm) and the solvent was evaporated to obtain a sheet-like composite with a thickness of 1 mm or more. Figure 1 shows a photograph of a test piece punched into the shape of a dumbbell-shaped test piece (No. 8, JIS K 6251) from the obtained sheet-like composite.

[0036] Example 2 Preparation of a complex consisting of lignosulfonic acid sodium salt, poly(ethyleneimine) and glucose A composite was prepared in the same manner as in Example 1 using 7.68 mL of a 25 wt% aqueous solution of Pearlex NP used in Example 1, 7.2 mL of a 40 wt% aqueous solution of poly(ethyleneimine) (Wako Pure Chemical Industries, Ltd., molecular weight 10,000) and 240 mg of D-glucose (Wako Pure Chemical Industries, Ltd., special grade), to obtain a sheet-like composite. The appearance of the obtained composite was almost the same as that of the composite obtained in Example 1.

[0037] Example 3 Preparation of a complex consisting of lignosulfonic acid sodium salt, poly(ethyleneimine) and arabinose 7.68 mL of a 25% by weight aqueous solution of Pearlex NP used in Example 1, 7.2 mL of a 40% by weight aqueous solution of poly(ethyleneimine) (Wako Pure Chemical Industries, Ltd., molecular weight 10,000), and D-(-)-arabinose A composite in the form of a sheet was obtained by using 240 mg of cellulose acetate (Tokyo Chemical Industry Co., Ltd.) in the same manner as in Example 1. The appearance of the obtained composite was almost the same as that of the composite obtained in Example 1.

[0038] Example 4 Preparation of a complex consisting of lignosulfonic acid sodium salt, poly(ethyleneimine) and fructose A composite was prepared in the same manner as in Example 1 using 7.68 mL of a 25 wt% aqueous solution of Pearlex NP used in Example 1, 7.2 mL of a 40 wt% aqueous solution of poly(ethyleneimine) (Wako Pure Chemical Industries, Ltd., molecular weight 10,000) and 240 mg of D-(-)-fructose (Wako Pure Chemical Industries, Ltd., special grade), to obtain a sheet-like composite. The appearance of the composite obtained was almost the same as that of the composite obtained in Example 1.

[0039] Example 5 Preparation of a complex consisting of lignosulfonic acid sodium salt, poly(ethyleneimine) and glutaraldehyde 7.68 mL of the 25 wt% aqueous solution of Pearlex NP used in Example 1 and 192 μL of an aqueous solution of glutaraldehyde (50% solution, Polysciences) were mixed uniformly. 11.52 mL of a 25 wt% aqueous solution of poly(ethyleneimine) (Wako Pure Chemical Industries, Ltd., molecular weight 10,000) was added to this solution and mixed uniformly. This mixture was transferred to a fluororesin petri dish (size: 6 cm x 6 cm) and the solvent was volatilized to obtain a sheet-like composite with a thickness of 1 mm or more. The appearance of the obtained composite was almost the same as that of the composite obtained in Example 1.

[0040] Example 6 Preparation of a composite of lignosulfonic acid sodium salt, poly(ethyleneimine) and butyraldehyde Using the Pearlex NP used in Example 1, 7.68 mL of a 25 wt% aqueous solution of Pearlex NP was newly prepared, and 240 μL of butylaldehyde (Wako Pure Chemical Industries, Ltd., special grade) was mixed uniformly. 11.52 mL of a 25 wt% aqueous solution of poly(ethyleneimine) newly prepared using the poly(ethyleneimine) (Wako Pure Chemical Industries, Ltd., molecular weight 10,000) used in Example 1 was added to this solution and mixed uniformly. This mixture was transferred to a fluororesin petri dish (size: 6 cm x 6 cm) and the solvent was volatilized to obtain a sheet-like composite with a thickness of 1 mm or more. The appearance of the obtained composite was almost the same as that of the composite obtained in Example 1.

[0041] Comparative Example 1 Preparation of a composite of lignosulfonic acid sodium salt and poly(ethyleneimine) 7.68 mL of the 25 wt% aqueous solution of Pearlex NP used in Example 1 and 7.2 mL of a 40 wt% aqueous solution of poly(ethyleneimine) (Wako Pure Chemical Industries, Ltd., molecular weight 10,000) were uniformly mixed. This mixture was transferred to a fluororesin petri dish (size: 6 cm x 6 cm) and the solvent was evaporated to obtain a sheet-like composite with a thickness of 1 mm or more. The appearance of the obtained composite was almost the same as the composite obtained in Example 1.

[0042] Comparative Example 2 Preparation of a Complex Consisting of Lignosulfonic Acid Sodium Salt, Poly(ethyleneimine) and Sucrose (Non-reducing Sugar) A composite was prepared in the same manner as in Example 1 using 7.68 mL of a 25 wt% aqueous solution of Pearlex NP used in Example 1, 7.2 mL of a 40 wt% aqueous solution of poly(ethyleneimine) (Wako Pure Chemical Industries, Ltd., molecular weight 10,000) and 240 mg of sucrose (Wako Pure Chemical Industries, Ltd., special grade), to obtain a sheet-like composite. The appearance of the obtained composite was almost the same as that of the composite obtained in Example 1.

[0043] Comparative Example 3 Preparation of a Complex Consisting of Lignosulfonic Acid Sodium Salt, Poly(ethyleneimine) and Trehalose (Non-reducing Sugar) 7.68 mL of a 25% by weight aqueous solution of Pearlex NP used in Example 1, poly(ethyleneimine) ( A complex was prepared in the same manner as in Example 1 using 7.2 mL of a 40% by weight aqueous solution of trehalose (Wako Pure Chemical Industries, Ltd., molecular weight 10,000) and 265 mg of trehalose dihydrate (Wako Pure Chemical Industries, Ltd., special grade), to obtain a sheet-like complex. The appearance of the obtained complex was almost the same as that of the complex obtained in Example 1.

[0044] Comparative Example 4 Preparation of a Complex of Lignosulfonic Acid Sodium Salt and Poly(ethyleneimine) 7.68 mL of the 25 wt% aqueous solution of Pearlex NP used in Example 6 and 7.2 mL of a 40 wt% aqueous solution of poly(ethyleneimine) (Wako Pure Chemical Industries, Ltd., molecular weight 10,000) were mixed uniformly. This mixture was transferred to a fluororesin petri dish (size: 6 cm x 6 cm) and the solvent was evaporated to obtain a sheet-like composite with a thickness of 1 mm or more. The appearance of the obtained composite was almost the same as the composite obtained in Example 1.

[0045] Example 7 Tensile test of a composite consisting of lignosulfonic acid sodium salt, poly(ethyleneimine) and a compound having an aldehyde group The sheet-like composites prepared in Examples 1 to 5 and Comparative Examples 1 to 3 were left to stand for 5 days in a thermohygrostat at 30°C and a relative humidity of 50%, and then punched out into the shape of dumbbell-shaped test pieces (No. 8, JIS K 6251) to prepare test pieces for evaluation. The test pieces were used to carry out tensile tests (in air, tensile speed 50 mm / min), and the results are shown in Table 1 (average value of 3 to 5 tests). As shown in Table 1, it was confirmed that the maximum stress of the test pieces of Examples 1 to 5 was improved by 1.1 to 2.1 times compared to the test piece of Comparative Example 1. In other words, it was shown that the ion complex mixed with the compound having an aldehyde group has a significantly improved breaking strength. Moreover, it was confirmed that the Young's modulus of the test pieces of Examples 1 to 5 was improved by 1.4 to 2.9 times compared to the test piece of Comparative Example 1. In other words, it was shown that the Young's modulus of the ionic complex mixed with a compound having an aldehyde group is significantly improved. On the other hand, in Comparative Examples 2 and 3, although a slight improvement in Young's modulus (1.2 times) was confirmed compared to the test piece in Comparative Example 1, no improvement in maximum stress was confirmed. In other words, it was confirmed that the ionic complex mixed with non-reducing sugar does not have a significant improvement effect on physical properties such as breaking strength or Young's modulus, unlike the ionic complex mixed with reducing sugars or aldehydes.

[0046] [Table 1]

[0047] Example 8 Tensile Test of a Composite of Lignosulfonic Acid Sodium Salt, Poly(ethyleneimine) and Butyraldehyde The sheet-like composites prepared in Example 6 and Comparative Example 4 were left to stand for 5 days in a thermohygrostat at 30°C and a relative humidity of 50%, and then dumbbell-shaped test pieces were prepared in the same manner as in Example 7 and subjected to a tensile test (in air, tensile speed of 50 mm / min). The results of the tensile test are shown in Table 2 (average value of 3 to 5 tests). As shown in Table 2, it was confirmed that the maximum stress of the test piece of Example 6 was 1.4 times higher than that of the test piece of Comparative Example 4. In other words, it was shown that the ion complex mixed with butylaldehyde had a significantly improved breaking strength. Moreover, it was confirmed that the Young's modulus of the test piece of Example 6 was 1.4 times higher than that of the test piece of Comparative Example 4. In other words, it was shown that the Young's modulus of the ion complex mixed with butylaldehyde is significantly improved.

[0048] [Table 2]

[0049] Example 9 Water resistance test of a complex consisting of sodium lignosulfonate, poly(ethyleneimine) and a reducing saccharide A 60 mg test piece was cut out from the sheet-like complex prepared in Examples 3 and 4 and Comparative Examples 1 to 3. The test piece was immersed in 1.2 mL of pure water and shaken at room temperature for 30 minutes or 24 hours to carry out a water resistance test. The less colored the supernatant was, the less the amount of sodium lignosulfonate dissolved from the ionic complex was, which means that the ionic complex had high water resistance. is shown. The results of the water resistance test are shown in Figure 2. When the ion complex was shaken in pure water for 30 minutes, none of the supernatants were colored, indicating that almost no ion complex was dissolved. In addition, when the ionic complexes were shaken in pure water for 24 hours, the supernatants in which the ionic complexes of Comparative Examples 1 to 3 were immersed were colored dark brown, whereas the supernatants in which the ionic complexes of Examples 3 and 4 were immersed were colored only slightly brown. In other words, it was found that the use of fructose or arabinose, which are reducing sugars, showed a remarkable effect in terms of the water resistance of the ionic complexes.

[0050] Example 10 Preparation of a complex consisting of lignosulfonic acid sodium salt, poly(allylamine) and fructose 6 mL of the 25 wt% aqueous solution of Pearlex NP used in Example 1 and 225 mg of D-(-)-fructose (Wako Pure Chemical Industries, Ltd., special grade) were mixed and stirred until the fructose was completely dissolved. 20 mL of a 15 wt% aqueous solution of poly(allylamine) (Polysciences, weight average molecular weight 15,000) was added to this solution and mixed uniformly. This mixture was transferred to a fluororesin petri dish (size: 6 cm x 6 cm) and the solvent was volatilized to obtain a sheet-like composite with a thickness of 1 mm or more. A photograph of the test piece obtained by punching the obtained sheet-like composite into the shape of a dumbbell-shaped test piece (No. 8, JIS K 6251) is shown in FIG. 3.

[0051] Comparative Example 5 Preparation of a composite of lignosulfonic acid sodium salt and poly(allylamine) 6 mL of the 25 wt% aqueous solution of Pearlex NP used in Example 1 and 20 mL of the 15 wt% aqueous solution of poly(allylamine) (Polysciences, weight average molecular weight 15,000) used in Example 10 were added and mixed uniformly. This mixture was transferred to a fluororesin petri dish (size: 6 cm x 6 cm) and the solvent was evaporated to obtain a sheet-like composite with a thickness of 1 mm or more. The appearance of the obtained composite was almost the same as the composite obtained in Example 10.

[0052] Example 11 Tensile Test of a Composite of Lignosulfonic Acid Sodium Salt, Poly(allylamine) and Fructose The sheet-like composites prepared in Example 10 and Comparative Example 5 were left to stand in a thermohygrostat at 30°C and a relative humidity of 50% for 5 days, and then subjected to a tensile test (in air, tensile speed of 50 mm / min) in the same manner as in Example 7. The results of the tensile test are shown in Table 3 (average value of 3 to 5 tests). As shown in Table 3, the maximum stress of the test piece of Example 10 was 2. In other words, the ionic complex mixed with a compound having an aldehyde group exhibited a significant improvement in breaking strength. In addition, it was confirmed that the Young's modulus of the test piece of Example 10 was 13.5 times higher than that of the test piece of Comparative Example 5. In other words, it was shown that the Young's modulus of the ion complex composed of lignosulfonic acid sodium salt mixed with fructose and poly(allylamine) was significantly improved.

[0053] [Table 3]

[0054] Example 12 Water resistance test of a composite consisting of lignosulfonic acid sodium salt, poly(allylamine) and fructose A 60 mg test piece was cut out from the sheet-like composite prepared in Example 10 and Comparative Example 5. The test piece was immersed in 1.2 mL of pure water and shaken at room temperature for 24 hours to carry out a water resistance test. The less colored the supernatant, the less the amount of sodium lignosulfonate dissolved from the ionic complex, i.e., the higher the water resistance of the ionic complex. The results of the water resistance test are shown in Figure 4. The supernatant in which the ionic complex of Comparative Example 5 was soaked was colored brown, whereas the supernatant in which the ionic complex of Example 10 was soaked was hardly colored. In other words, it was found that the addition of fructose improved the water resistance of the ionic complex.

[0055] Example 13 Elasticity evaluation of a composite consisting of lignosulfonic acid sodium salt, poly(ethyleneimine) and fructose FIG. 5 shows a photograph of the composite sample of lignin sulfonate sodium salt, poly(ethyleneimine) and fructose that broke in the tensile test in Example 7 and was left to stand for 72 hours or more, and then compared with the shape of a sample that was not subjected to a tensile test. In the tensile test, the sample was deformed by a strain of 30% or more (distance between jigs 35 mm x 30% = 11.2 mm) applied to the portion between the jigs before it broke, but the deformation of the portion between the jigs of the sample after being left to stand was 10% (3.5 mm) or less of the distance between the jigs of the sample before the tensile test. In other words, the length of the sample left to stand after the tensile test spontaneously recovered to the same length as the sample before the tensile test, indicating that this composite has elasticity.

[0056] Example 14 Elasticity evaluation of a composite consisting of lignosulfonic acid sodium salt, poly(allylamine) and fructose FIG. 6 shows a photograph of the morphology of a composite sample of lignosulfonic acid sodium salt, poly(allylamine) and fructose that broke in the tensile test in Example 11 and was left to stand for 72 hours or more, compared with that of a sample that was not subjected to a tensile test. In the tensile test, the sample was deformed by a strain of 30% (distance between jigs 35 mm × 30% = 11.2 mm) applied to the portion between the jigs before it broke, but the deformation of the portion between the jigs of the sample after being left to stand was 10% (3.5 mm) or less of the distance between the jigs of the sample before the tensile test. In other words, the length of the sample left to stand after the tensile test spontaneously recovered to the same length as the sample before the tensile test, indicating that this composite has elasticity.

[0057] Example 15 Adhesion of stainless steel plates using a composite of sodium lignosulfonate, poly(allylamine) and fructose 0.45 mL of the 25 wt% aqueous solution of Pearlex NP used in Example 10, 1.75 mL of a 15 wt% aqueous solution of poly(allylamine), and 37.5 mg of D-(-)-fructose were mixed. This mixture was transferred to a fluororesin petri dish and heated on a hot plate at 150°C to remove moisture, yielding a viscous complex. Approximately 9 mg of the resulting complex was placed in a 1 cm2 overlapping area. 2 The stainless steel plates were sandwiched between two stainless steel plates (length 5 cm, width 1 cm, thickness 2 mm) so that the adhesive bond was uniform. The stainless steel plates were heated in a hot press at 80°C and 0.2 MPa for 2 minutes. After cooling in the air, the stainless steel plates were placed in a thermo-hygrostat at 30°C and 50% humidity for 24 hours or more to evaporate the solvent, thereby bonding the stainless steel plates together. A tensile test (in air, tensile speed 10 mm / min) was performed using the bonded stainless steel plates to measure the tensile shear adhesive strength, which was 7.67 ± 0.15 MPa (average of three tests).

[0058] Comparative Example 6 Adhesion of stainless steel plates using a composite of sodium lignin sulfonate and poly(allylamine) 0.45 mL of the 25 wt % aqueous solution of Pearlex NP used in Example 10 and 1.75 mL of the 15 wt % aqueous solution of poly(allylamine) were mixed, and the mixture was heated on a hot plate at 150° C. in the same manner as in Example 15. A viscous composite was obtained by heating. Approximately 9 mg of the composite obtained was used to bond a stainless steel plate in the same manner as in Example 15. A tensile test (in air, tensile speed 10 mm / min) was performed using the bonded stainless steel plate to measure the tensile shear adhesive strength, which was 6.98±0.37 MPa (average value of three tests).

[0059] From the results of Example 15 and Comparative Example 6, it was confirmed that the test piece of Example 15 had an improvement of about 1.1 times in tensile shear adhesive strength compared to the test piece of Comparative Example 6. In other words, it was shown that the composite obtained by mixing lignosulfonic acid sodium salt and poly(allylamine) with fructose had improved tensile shear adhesive strength compared to the composite made of lignosulfonic acid sodium salt and poly(allylamine). [Industrial Applicability]

[0060] The ionic composite material of the present invention can be molded into a variety of shapes, is highly elastic, and has excellent strength and water resistance, and can therefore be used as a material for molded products for a variety of applications where such properties are required.

Claims

1. (1) lignosulfonic acid, its derivative, or a salt thereof; (2) a cationic polymer (excluding ε-polylysine), its derivative, or a salt thereof; and (3) a reducing agent. An elastic ionic composite material comprising a sugar or aldehyde represented by the formula: the cationic polymer comprises poly(ethyleneimine) or poly(allylamine); An ion complex material, wherein the reducing saccharide is fructose, arabinose, glucose, or lactose.

2. The ion complex according to claim 1, wherein the salt of lignosulfonic acid or a derivative thereof is a metal salt. Composite material.

3. 3. The ionic composite material of claim 2, wherein the metal salt is selected from the group consisting of sodium salts, calcium salts, and magnesium salts.

4. The cationic polymer further has at least one functional group selected from the group consisting of a primary, secondary or tertiary amino group, a quaternary ammonium group and an imino group in its molecule. The ionic composite material according to any one of claims 1 to 3, comprising

5. The ionic composite material according to any one of claims 1 to 3, wherein the cationic polymer is poly(ethyleneimine) or poly(allylamine).

6. The ionic composite material according to any one of claims 1 to 5, wherein the aldehyde is an aliphatic dialdehyde or an aliphatic aldehyde.

7. 7. The ionic complex of claim 6, wherein the aliphatic dialdehyde is glutaraldehyde. Fee.

8. A method for producing the ionic composite material according to any one of claims 1 to 7, comprising the steps of: (1) mixing lignin sulfonic acid, a derivative thereof, or a salt thereof, (2) a cationic polymer, a derivative thereof, or a salt thereof, and (3) a sugar or an aldehyde exhibiting reducing properties in a solvent to form an ionic composite material in the solvent; and Or removing the solvent from the suspension.

9. (1) lignosulfonic acid, its derivative, or a salt thereof; (2) a cationic polymer (excluding ε-polylysine), its derivative, or a salt thereof; and (3) a reducing agent. and (4) an organic solvent, the cationic polymer comprises poly(ethyleneimine) or poly(allylamine); The material, wherein the reducing sugar is fructose, arabinose, glucose, or lactose.

10. Consisting of an ionic composite material according to any one of claims 1 to 7 or a material according to claim 9 glue.

Citation Information

Patent Citations

  • Dry strength-reinforcing agent for paper-making

    JP1990251696A

  • Improvement in strength of paper manufactured from pulp containing surface-active carboxyl compound

    JP1996232191A

  • Treatment of porous article and composition for treating porous article

    JP1998265508A

  • Resin composition including lignin

    JP1999152410A

  • Ion compound type clay composition and solidified matter thereof

    JP2006133299A