Self-leveling material composition
A gypsum-based self-leveling material composition using a combination of α-type and β-type hemihydrate gypsum addresses the challenge of temperature-induced fluctuations in pot life and light walking time, ensuring efficient and high-quality construction outcomes.
Patent Information
- Application Number
- JP2021552343
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-10-15
- Filing Date
- 2020-10-07
- Publication Date
- 2024-10-08
- Estimated Expiration
- 2040-10-07
AI Technical Summary
Gypsum-based self-leveling materials face challenges in maintaining a stable pot life and light walking time under varying temperature conditions, particularly in winter, leading to reduced work efficiency and potential quality issues such as unevenness and wrinkles on the surface.
A gypsum-based self-leveling material composition comprising a combination of α-type and β-type hemihydrate gypsum, with specific ratios to maintain a stable pot life and reduce fluctuations in light walking time, ensuring efficient construction even in low temperatures.
The composition achieves a stable usable life without shortening the pot life, suppresses fluctuations in light walking time, and enhances work efficiency by allowing construction to proceed smoothly regardless of temperature fluctuations, maintaining excellent practicality and quality.
Smart Images

Figure 0007563763000001 
Figure 0007563763000002 
Figure 0007563763000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a self-leveling material composition for use as a floor finishing base material, and more particularly to a technique for providing a gypsum-based self-leveling material composition that exhibits excellent properties in terms of workability. [Background technology]
[0002] Self-leveling material compositions (hereinafter referred to as self-leveling materials or SL materials) are mixed with water to form a slurry, which flows naturally and forms a horizontal surface when simply poured onto the floor, and hardens, so they are widely used as floor finishing base materials. Currently popular self-leveling materials include gypsum-based and cement-based types, as specified in JASS 15M-103 (quality standard for self-leveling materials).
[0003] Gypsum-based self-leveling materials are products that have less change in length than cement-based self-leveling materials. Specifically, they are products with a length change of 0.05% or less, as stipulated in JASS 15M-103 (quality standard for self-leveling materials). Because the change in length is small, gypsum-based self-leveling materials have the following advantages over cement-based self-leveling materials. Specifically, they have the advantages of less cracking problems in the applied SL material, excellent slurry fluidity, and a short hardening time.
[0004] For gypsum-based self-leveling material products, the hardening time is set to 3 hours under normal conditions (temperature 20°C). SL material is a base material, and in order to complete the floor surface, a slurry of SL material is poured onto the floor, and once the slurry has hardened to a certain extent and people can walk on the hardened body without leaving footprints, people must stand on the hardened body and carry out the next work. The time from when the slurry has been poured until it is possible to carry out the next work is called the "light walkable time." Summary of the Invention [Problem to be solved by the invention]
[0005] When construction work is carried out using a gypsum-based SL material product with a set hardening time, light walking becomes possible within four hours at temperatures between 20 and 35°C from spring to autumn. However, in winter, when temperatures drop below 10°C, light walking becomes possible only after six hours or more have passed, which causes a drop in work efficiency. In other words, if the "light walking time" is extended to six hours or more, repair work on the SL material that has already been installed or removal work such as flow-stop frames cannot be carried out on the same day the SL material is installed, which means an extra day of construction time is required.
[0006] According to the study by the present inventors, in contrast, if the hardening time of a gypsum-based SL material product is adjusted so that light walking can be completed within 4 hours in winter, the working time of the slurry will be shortened, making the application of the SL material difficult. Here, the working time refers to the time during which the SL material can be made into a slurry and poured onto the floor, and the leveling work of the slurry can be carried out smoothly. In general, from the perspective of a series of work procedures, the working time needs to be secured for 20 minutes or more. In addition, if the working time is short, the basic performance required for the gypsum-based SL material is not fully exhibited, and quality problems arise such as unevenness and wrinkles on the surface of the applied SL material.
[0007] In contrast to the current situation with gypsum-based SL material products as described above, the technical objective of the present invention is to provide a gypsum-based SL material that is excellent in workability while ensuring the necessary pot life and minimizing the temperature-dependent fluctuations in the "light walkable time", which varies greatly with temperature and is particularly long when applied under low temperature conditions, thereby suppressing the problem of reduced efficiency during application caused by temperature fluctuations.As far as the inventors know, this has not yet been considered.
[0008] Therefore, the object of the present invention is to provide a gypsum-based self-leveling material that can fully exhibit the basic performance required of an SL material, by keeping the pot life stable without shortening it and suppressing fluctuations in the time during which light walking is possible that occur under low temperature conditions such as winter, and that also solves the problem of reduced work efficiency caused by temperature fluctuations with a simple configuration. [Means for solving the problem]
[0009] The above object can be achieved by the present invention, which provides a gypsum-based self-leveling material composition as described below. [1] A self-leveling material composition comprising a base material component which contains hemihydrate as an essential component and which may contain at least one of inorganic aggregate and cement as optional components, and an additive, wherein the content of the hemihydrate is 55 to 100 parts by mass when the total of the base material components is taken as 100 parts by mass, the hemihydrate contains α-type hemihydrate and β-type hemihydrate, and when the total of the α-type hemihydrate and the β-type hemihydrate is taken as 100 parts by mass, the content of the α-type hemihydrate is 70 to 95 parts by mass and the content of the β-type hemihydrate is 5 to 30 parts by mass, and further, when the total of the base material components is taken as 100 parts by mass, the content of the β-type hemihydrate is 20 parts by mass or less, and the length change as defined by JASS 15M-103 (quality standard for self-leveling materials) is 0.05% or less.
[0010] The present invention provides the following configuration as a preferred embodiment of the above-mentioned self-leveling material composition. [2] The gypsum-based self-leveling material composition according to the above [1], in which the content of the hemihydrate gypsum is 55 to 100 parts by mass, the content of the cement is 0 to 25 parts by mass, and the content of the inorganic aggregate is 0 to 30 parts by mass, when the total amount of the base components is 100 parts by mass. [3] The gypsum-based self-leveling material composition according to the above [1] or [2], wherein the cement is any one selected from the group consisting of ordinary Portland cement, high-early-strength Portland cement, blast-furnace cement and alumina cement. [4] The gypsum-based self-leveling material composition according to any one of the above [1] to [3], wherein the components of the base material are gypsum hemihydrate and cement. [5] The gypsum-based self-leveling material composition according to any one of the above [1] to [3], wherein the inorganic aggregate is calcium carbonate. [6] The gypsum-based self-leveling material composition according to any one of [1] to [5] above, wherein the content of the α-type hemihydrate is 80 to 90 parts by mass and the content of the β-type hemihydrate is 10 to 20 parts by mass, when the total amount of the hemihydrate is 100 parts by mass. [7] A gypsum-based self-leveling material composition according to the above item [1], in which the content of the hemihydrate gypsum is 100 parts by mass when the total amount of the base components is 100 parts by mass, and which does not contain the optional components. Effect of the Invention
[0011] According to the present invention, it is possible to provide a gypsum-based self-leveling material composition which, while having a simple constitution, maintains its pot life stably without shortening it, minimizes fluctuations in the time during which light walking is possible that occur under low temperature conditions such as winter, has sufficient functionality as an SL material, suppresses the problem of reduced work efficiency during construction caused by temperature fluctuations, and has excellent practicality with a remarkable improvement in work efficiency compared to conventional products. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0012] Next, the present invention will be described in more detail with reference to preferred embodiments. First, the terms will be explained. In the present invention, "light walking possible" in determining the "light walking possible time" of the SL material refers to a state in which the SL material has hardened to a certain extent, in which the SL material slurry that has been poured has hardened and the surface of the SL material can be walked on without leaving footprints. In the present invention, in order to determine the state of the hardened body that is lightly walkable in an objective numerical value, a durometer (rubber hardness meter) that is widely used to measure the hardness of various rubber and plastic products was used. Specifically, a durometer (type D, JIS K 6253) was used to measure the hardness of the surface of the hardened body, and the measured value was used as an index to objectively determine the degree to which the slurry of the poured SL material had hardened. In the present invention, the time when the surface hardness of the hardened body became 55 points or more after the SL material was poured was defined as the "light walking possible time" by the measurement of the durometer.
[0013] In the present invention, the powder state before being kneaded with water (mixing water) is called the "self-leveling material composition" or "self-leveling material (SL material)", and the material in the form of a slurry after being kneaded with water (mixing water) is called the "slurry".
[0014] The present inventors have intensively studied the problems of the conventional technology described above, and have arrived at the present invention. Conventionally, additives such as setting retarders and water reducing agents have been mixed into the materials forming the SL material as a method for adjusting the pot life of the slurry. However, according to the study by the present inventors, it was not possible to obtain a product in which the light walking time, which becomes longer when the material is applied under low temperature conditions such as winter, is adjusted to a condition suitable for application work, without shortening the pot life that affects the basic quality of the SL material, by devising the mixture of these additives. Specifically, for example, it has not been possible to obtain a product in which the light walking time is shorter than that of conventional products, within 5 hours, preferably within 4 hours, under low temperature conditions of about 10°C.
[0015] In response to the above, the present inventors have been studying whether there is a means to solve the technical problem of the present invention by improving the base material itself, rather than improving the additives. In conventional products, α-type hemihydrate gypsum is used as hemihydrate gypsum, which is the main component of the base material constituting the gypsum-based SL material. There are α-type hemihydrate gypsum and β-type hemihydrate gypsum, and they are calcined by different methods. α-type hemihydrate gypsum is manufactured by a wet method, and β-type hemihydrate gypsum is manufactured by a dry method. The standard mixed water amount of α-type hemihydrate gypsum specified in JIS R 9111 is less than that of β-type hemihydrate gypsum, and the amount of water required for hardening is less than that of β-type hemihydrate gypsum. And, although this is also thought to be the cause, the use of α-type hemihydrate gypsum has the advantage of increasing the strength when hardened. For this reason, α-type hemihydrate gypsum was used as the base material in conventional gypsum-based SL materials.
[0016] As a result of intensive research by the present inventors in response to the above-mentioned current situation, the main component of the substrate constituting the gypsum-based SL material is hemihydrate gypsum, which is the same as that of conventional products, but surprisingly, it was found that the above-mentioned technical problem of the present invention can be solved by a very simple means of using α-type hemihydrate gypsum in combination with β-type hemihydrate gypsum as the substrate. Then, as a result of further research, when the total of α-type hemihydrate gypsum and β-type hemihydrate gypsum is 100 parts by mass, α-type hemihydrate gypsum is used in the range of 70 to 95 parts by mass, and β-type hemihydrate gypsum is configured to be in the range of 5 to 30 parts by mass, and further, when the total of the substrate components is 100 parts by mass, the content of β-type hemihydrate gypsum is 20 parts by mass or less, and the present invention was achieved by finding that the remarkable effect aimed at by the present invention can be obtained stably and reliably.
[0017] Specifically, when considering construction in winter, it was found that by configuring the hemihydrate gypsum used as described above, it is possible to ensure pot life while significantly reducing the temperature-dependent fluctuations in the light walking time compared to conventional products. In this way, the SL material product obtained by the present invention does not have a large fluctuation in the light walking time depending on the temperature, so the construction work of the SL material can always be stable and efficient regardless of temperature fluctuations. The ripple effect of this on improving work efficiency and the like is extremely large. It was also found that even if β-type hemihydrate gypsum is used within the above range, it is not inferior in strength after hardening compared to conventional SL material products that are composed entirely of α-type hemihydrate gypsum.
[0018] The present inventors first investigated the case where the base material components were all composed of hemihydrate gypsum without using any other materials. As a result, it was found that by using α-type hemihydrate gypsum in combination with β-type hemihydrate gypsum, the light walking time when applied under low temperature conditions of, for example, 10°C can be shortened without affecting the pot life. In addition, it was found that in this case, the viscosity of the slurry increases by using β-type hemihydrate gypsum in combination, but the degree of thickening can be suppressed within a practical range by adjusting the amount of β-type hemihydrate gypsum used in combination. Specifically, as described below, when the total amount of hemihydrate gypsum is 100 parts by mass, the content of α-type hemihydrate gypsum is 70 to 95 parts by mass, and the content of β-type hemihydrate gypsum used in combination is 5 to 30 parts by mass, it was found that the light walking time, which was caused by the reduction in work efficiency in winter due to the increase in time due to temperature fluctuations, can be shortened to the 4-hour range even under low temperature conditions while ensuring the pot life that affects the basic quality of the SL material.
[0019] In addition, it was confirmed that in order to shorten the light walking time to within 4 hours regardless of temperature fluctuations, it is effective to make the content of β-type hemihydrate gypsum 10 parts by mass or more. Furthermore, considering the increase in viscosity of the composition caused by the use of β-type hemihydrate gypsum, it was found that it is necessary to adjust the content of β-type hemihydrate gypsum to 20 parts by mass or less when the total amount of the base material components is 100 parts by mass. The above means that if the composition of the base material components is made entirely of hemihydrate gypsum without using other materials, and the amount of β-type hemihydrate gypsum used in combination with α-type hemihydrate gypsum is adjusted as specified in the present invention, the effect aimed at by the present invention can be obtained, and a gypsum-based SL material composition suitable for practical use can be obtained.
[0020] Next, the inventors conducted a detailed study on the effect of shortening the light walkable time in low temperature environments described above when a base material configuration is used in which hemihydrate gypsum is used in combination with cement or inorganic aggregate that are commonly used in addition to hemihydrate gypsum, as well as the effect on thickening that occurs when β-type hemihydrate gypsum is used in combination to achieve this effect.
[0021] Cement and inorganic aggregates are used in building materials for the purpose of improving strength and reducing costs. Usually, in a gypsum-based SL material, when the total of the base material components is 100 parts by mass, 55 parts by mass or more of hemihydrate gypsum is used as the main component, and other components such as cement and inorganic aggregates such as calcium carbonate are mixed to form the base material. Therefore, the present inventors prepared SL material compositions having a base material configuration in which 100 parts by mass of the base material components are mixed in stages with 65 parts by mass of hemihydrate gypsum, with a mixture of α-type hemihydrate gypsum and β-type hemihydrate gypsum in a ratio of 90:10, with 5 to 30 parts by mass of cement and 10 to 35 parts by mass of calcium carbonate, which is an inorganic aggregate, and used these slurries to examine the effects on viscosity, pot life, and light walkable time. As a result, as described below, it was found that the same effects as described above can be obtained even when a base material containing 5 to 25 parts by mass of cement and 10 to 30 parts by mass of inorganic aggregate is used. In other words, it has been found that even when cement or an inorganic aggregate is used as an optional component of the base material, as long as hemihydrate gypsum is used as the main component of the base material and the composition of the hemihydrate gypsum satisfies the blending requirements of α-type hemihydrate gypsum and β-type hemihydrate gypsum specified in the present invention, a remarkable effect can be obtained, for example, that the time during which light walking is possible under low-temperature conditions of about 10° C. can be shortened to within 5 hours, preferably within 4 hours, without causing any problems in viscosity and pot life.
[0022] Hereinafter, each material that can constitute the self-leveling material composition of the present invention will be described. (Base material component) The base material component constituting the self-leveling material composition of the present invention must be composed mainly of hemihydrate gypsum, which is a hydraulic material, and can be composed of an optional component such as cement or calcium carbonate. What is important about the self-leveling material composition of the present invention is that hemihydrate gypsum is used as the main component of the base material, and in that case, β-type hemihydrate gypsum is used in combination with α-type hemihydrate gypsum in a specific blending ratio as specified in the present invention. First, in the present invention, it is essential that 100 parts by mass of the base material component contains 55 parts by mass or more of hemihydrate gypsum, and if necessary, inorganic aggregate such as cement or calcium carbonate used as an extender may be used in the base material material, and the amount of hemihydrate gypsum contained in the base material is gypsum-based, which is greater than the total amount of other materials. The SL material of the present invention is gypsum-based as described above, and the gypsum-based SL material has the advantage that the drying shrinkage of the hardened body of the mixture (slurry) with water is less and cracks are less than that of a cement-based SL material in which the base material contains a large amount of cement. For this reason, in the SL material of the present invention, it is essential that the base material is configured so that the content of hemihydrate gypsum is 55 parts by mass or more when the total of the base material components is 100 parts by mass. According to the studies of the present inventors, other base material materials (components) that can be arbitrarily mixed as necessary without impairing the effects of the present invention are at least one of inorganic aggregate and cement. The range of the amount of these optional components to be mixed is preferably about 0 to 25 parts by mass for the cement content and about 0 to 30 parts by mass for the inorganic aggregate content.
[0023] <Gypsum hemihydrate> The hemihydrate gypsum, which is an essential component of the base material constituting the SL material of the present invention, is characterized by being composed of α-type hemihydrate gypsum in combination with β-type hemihydrate gypsum. The calcination methods of α-type hemihydrate gypsum and β-type hemihydrate gypsum are different. α-type hemihydrate gypsum is manufactured by a wet method and is obtained by calcining dihydrate gypsum in water (including in steam). β-type hemihydrate gypsum is manufactured by a dry method and is obtained by calcining dihydrate gypsum in air. As mentioned above, in conventional gypsum-based SL materials, α-type hemihydrate gypsum has been used because it has the advantage that the amount of water required for hardening is small and the strength is high when hardened. In contrast, in the SL material of the present invention, β-type hemihydrate gypsum is used in combination with the hemihydrate gypsum constituting the base material, and the content of α-type hemihydrate gypsum is used in a ratio of 70 to 95 parts by mass and 5 to 30 parts by mass when the total of α-type hemihydrate gypsum and β-type hemihydrate gypsum is 100 parts by mass. Preferably, the content of α-type hemihydrate gypsum is 80 to 90 parts by mass, and the content of β-type hemihydrate gypsum is 10 to 20 parts by mass. Furthermore, in the SL material of the present invention, the amount of β-type hemihydrate gypsum constituting the substrate is configured so that the content of β-type hemihydrate gypsum is in the range of 20 parts by mass or less when the total of the hemihydrate gypsum substrates is 100 parts by mass. By adopting the above configuration, the SL material of the present invention can realize excellent workability that could not be obtained by conventional SL materials, and at the same time, compared with conventional products that are entirely composed of α-type hemihydrate gypsum, there is no deterioration in strength after construction. The lower limit of the amount of β-type hemihydrate gypsum used in the substrate is not particularly limited, but may be, for example, 3 parts by mass or more.
[0024] <Cement> Cement can be used as necessary for the base material component constituting the SL material of the present invention. Examples of cement that can be used for the base material material include the following. For example, various cements such as ordinary Portland cement, high-early-strength Portland cement, moderate-heat Portland cement, blast-furnace cement, silica cement, fly ash cement, alumina cement, and jet cement can be mentioned. A cement material selected from these can be appropriately used as an optional component of the base material constituting the SL material of the present invention. The above cement is appropriately blended into the base material for the purpose of, for example, improving the water resistance of the floor finishing base material formed by the SL material. The amount of cement blended when used as an optional component of the base material may be, for example, about 5 to 25 parts by mass in 100 parts by mass of the base material component.
[0025] <Inorganic aggregate> Inorganic aggregates can be used as necessary for the base material constituting the SL material of the present invention. For example, calcium carbonate, which is widely used as a filler, can be used as an inorganic aggregate for the base material. Calcium carbonate is inexpensive, and by using it as a filler, it is possible to provide the desired SL material at a low cost. When inorganic aggregates are used as optional components of the base material, the blending amount is preferably about 10 to 30 parts by mass in 100 parts by mass of the base material component.
[0026] (Additives) In the gypsum-based SL material of the present invention, as in conventional products, additives such as water-reducing agents (plasticizers or dispersants), antifoaming agents, thickeners, and setting retarders are appropriately selected and blended as necessary within the range that does not contradict the intended purpose of the present invention. It is preferable to blend these additives in a total amount of 5% or less of the base material.
[0027] The water-reducing agent (fluidizing agent or dispersing agent) is not particularly limited as long as it is commercially available. Usually, polycarboxylic acid-based, naphthalene-based and lignin-based water-reducing agents can be used. In the case of SL materials, it is necessary to obtain excellent fluidity with as little water as possible, so water-reducing agents are usually used. In this case, if the amount used is too small, the effect cannot be obtained, and conversely, if it is too large, it may cause separation of inorganic aggregates used as optional components, which may cause a decrease in the strength of the horizontal surface formed, so care must be taken.
[0028] The water reducing agent can be added during the construction to prepare the slurry and used to adjust the flow value. According to the study by the present inventors, the flow value can be increased by increasing the amount of α-type hemihydrate gypsum constituting the base material, but compared to β-type hemihydrate gypsum, it tends to cause delay in setting at low temperatures and increase the light walkable time. In contrast, when the amount of α-type hemihydrate gypsum constituting the base material is decreased, the flow value decreases, and the amount of water reducing agent used increases. On the other hand, when the amount of water reducing agent used increases, setting delay occurs and the light walkable time that the present invention aims to shorten increases, so from this point of view, excessive use of the water reducing agent is not preferable. Furthermore, economic issues such as high chemical costs arise.
[0029] As the defoaming agent, for example, polyether-based, silicone-based, alcohol-based, mineral oil-based, vegetable oil-based and nonionic surfactants and other commonly used defoaming agents can be appropriately used.
[0030] Examples of the setting retarder that can be used include citrates such as sodium citrate, succinates, acetates, malates, borates such as borax, sucrose, hexametaphosphates, ethylenediaminetetraacetate, diethylenetriaminepentaacetate, starch, and protein hydrolysates. The amount of setting retarder to be added may be set to an extent that the required setting retardation function can be achieved.
[0031] In order to prevent separation of the aggregate, the SL material of the present invention may contain a thickener so that the slurry (kneaded material) has a certain level of viscosity when kneaded with water. As the thickener, cellulose ether or the like can be used.
[0032] (Construction location) The SL material of the present invention is made into a floor finishing base material by adding water, thoroughly mixing and kneading it to form a slurry (kneaded material), pouring it onto the subfloor surface, spreading it, leaving it, hardening, and drying it. Examples of the subfloor surface include mortar, cement, wood, plastic tiles or sheets, ceramics, and metals such as stainless steel. In this respect, it is no different from conventional SL materials.
[0033] As described above, when the SL material of the present invention is used for construction, it is necessary to knead it with water to make a slurry. The amount of water used is preferably about 35 to 70 parts by mass per 100 parts by mass of the substrate. If the amount of water is small, sufficient fluidity cannot be obtained, spreading becomes difficult, and workability may decrease. On the other hand, if the amount of water is too large, it causes deterioration of the surface condition and strength reduction due to unevenness of the surface of the hardened body, which are both undesirable. The SL material of the present invention is preferably one that is adjusted so that the flow value required when the slurry (sludge) is poured is 190 mm or more, for example, 210 mm or more and 260 mm or less. EXAMPLES
[0034] Next, the present invention will be described in more detail with reference to examples and comparative examples. However, the present invention is not limited to these examples. In the text, "parts" are based on mass unless otherwise specified.
[0035] [Examples 1-1 to 1-5, Comparative Examples 1 and 2] As the base material, 65 parts of hemihydrate gypsum, 15 parts of ordinary Portland cement, and 20 parts of calcium carbonate as inorganic aggregate were prepared. In this case, in Examples 1-1 to 1-5 and Comparative Examples 1 and 2, the contents of 65 parts of hemihydrate gypsum constituting the base material were as shown in Table 1. First, in Comparative Example 1, all of the hemihydrate gypsum used in the base material was α-type hemihydrate gypsum. On the other hand, in Examples 1-1 to 1-5 and Comparative Example 2, the hemihydrate gypsum was set to 100 parts by mass, and the blending ratio (α and β ratio) of α-type hemihydrate gypsum and β-type hemihydrate gypsum was adjusted so that the relative amount of β-type hemihydrate gypsum increased stepwise between 5 and 40 parts, as shown in Table 1. Then, in the results of the investigation described later, the viscosity of the slurry increased, and the functionality as a SL material and the workability of construction were poor, so an example of a blending ratio of α-type hemihydrate gypsum = 60 parts and β-type hemihydrate gypsum = 40 parts was set as Comparative Example 2.
[0036] As described above, seven types of SL materials with different compositions were obtained according to a conventional method by adding equal amounts of the same setting retarder, expansion inhibitor, thickener, and defoamer to seven types of base materials with different amounts of β-type hemihydrate gypsum (Comparative Example 1, which used only α-type hemihydrate gypsum, and Examples 1-1 to 1-5 and Comparative Example 2, which used hemihydrate gypsum with different blends of α-type hemihydrate gypsum and β-type hemihydrate gypsum).
[0037] Using 100 parts of each of the obtained SL materials, evaluation was performed in the following manner. First, 35 parts of water were added to 100 parts of the SL material to prepare a slurry for evaluation. In order to perform the evaluation under the same conditions, when preparing the slurry, a water reducing agent was added to adjust the fluidity so that the flow value measured in accordance with JASS15 M103 in an environment of 20°C was 230±2 mm in all cases.
[0038] (evaluation) The physical properties of each slurry prepared using the SL material obtained as described above and the time until light walking was possible when the slurry was applied were measured. Each measurement was performed under the following conditions. It was confirmed that in all tests, the length change specified in JASS 15M-103 (quality standard for self-leveling materials) was 0.05% or less. The evaluation results are summarized in Table 1. In addition, in Table 1, the evaluation results that can be judged to have achieved the goals of the present invention are listed as "achievement target value."
[0039] <Viscosity> The viscosity was measured using a viscosity measuring device (product name: Viscotester "VT-06", manufactured by Rion Co., Ltd.) in an environment at a temperature of 20°C. The results are summarized in Table 1. In the present invention, the target viscosity of the slurry was set to 10 to 20 dPa s from the viewpoint of workability when preparing the slurry.
[0040] <Pot life> The pot life means the longest time during which the slurry can be poured after preparation. Specifically, as explained above, the slurry was prepared so that the flow value measured in accordance with JASS15 M103 in an environment of 20°C was 230±2 mm, and the pot life was determined as the longest time during which the flow value of the slurry was 90% or more of the flow value of the slurry when it was prepared. The results obtained are summarized in Table 1. Here, taking into consideration the procedure for starting construction work, the target pot life was set to 20 minutes or more. If the pot life is 20 minutes or more, the worker can start construction work sufficiently, smoothly and stably.
[0041] <Light walking time> The light walking time means the time when a person can get on and perform subsequent work after the application of the slurry. In order to investigate the effect of differences in temperature conditions after application on the light walking time for each slurry of different configurations, tests were conducted under two conditions, one where the room temperature was kept at 10°C and the other where the room temperature was kept at 20°C. Specifically, after the application of the slurry, the surface hardness of the application surface was measured using a durometer (type D, JIS K 6253), and the measured value was used as an index to measure the time from the time of application of the slurry until the measured surface hardness reached 55 points or more, thereby objectively evaluating and confirming the "light walking time". In the present invention, the goal was to make the light walking time measured as described above within 5 hours even under low temperature conditions of 10°C, taking into consideration the work procedures that can be smoothly performed in one day, including the preparation of the slurry, application of the slurry, and the subsequent process.
[0042] TIFF0007563763000001.tif89170
[0043] As shown in Table 1, the following was found as a result of the investigation of Examples 1-1 to 1-5 and Comparative Examples 1 and 2. It was confirmed that the slurry using the conventional SL material of Comparative Example 1, in which all the hemihydrate gypsum used in the base material was α-type hemihydrate gypsum, had a light walking time of about 3 hours when the room temperature was set at 20°C, but exceeded 5 hours when the room temperature was set at 10°C. This shows that although the composition of Comparative Example 1 has no problem with viscosity or pot life, the light walking time differs greatly with a difference of about 10°C in room temperature conditions, greatly affecting workability. In response to this fact, considering the large temperature differences depending on the season and region in which it is used, and the temperature differences that occur throughout the day, it is clear that there is an urgent need to improve this point and develop a composition that suppresses the impact of differences in room temperature conditions (temperature fluctuations) on the light walking time.
[0044] As shown in Table 1, in the above Comparative Example 1, the slurries prepared using the compositions of Examples 1-1 to 1-5 and Comparative Example 2 all had a shorter light walkable time than the slurry of Comparative Example 1, and it was confirmed that the light walkable time could be shortened without exceeding 5 hours even under a low temperature condition of 10 ° C. Furthermore, in the composition of hemihydrate gypsum, which is an essential component of the base material, by adjusting the blending ratio (α and β ratio) of β-type hemihydrate gypsum used in combination with α-type hemihydrate gypsum, the difference between the light walkable time under the condition of 10 ° C. and the light walkable time under the condition of 20 ° C. can be reduced. Specifically, it was found that the difference was as much as 2 hours and 30 minutes in the slurry of Comparative Example 1, whereas the slurries of Examples 1-3 to 1-5 and Comparative Example 2 could be shortened to 45 minutes to 30 minutes. This means that, unlike conventional compositions, the SL material composition of the present invention, which is composed of the essential components of the base material in combination with α-type hemihydrate gypsum and β-type hemihydrate gypsum, has little effect on the light walkable time due to temperature differences, and the next work can be started stably and efficiently after the slurry is applied.
[0045] More specifically, as shown in Table 1, it was found that the influence of temperature conditions on the light walking time can be reduced by using 100 parts of hemihydrate gypsum constituting the base material of the SL material in a ratio of 60 to 95 parts of α-type hemihydrate gypsum and 5 to 40 parts of β-type hemihydrate gypsum. The composition of Comparative Example 2, which contains 60 parts of α-type hemihydrate gypsum and 40 parts of β-type hemihydrate gypsum, has an improved light walking time and no problem with the pot life compared to the composition of Comparative Example 1, but it was confirmed that there is another problem in that the viscosity becomes too high when made into a slurry. For this reason, in the present invention, it is essential that the content of α-type hemihydrate gypsum is 70 to 95 parts and the content of β-type hemihydrate gypsum is 5 to 30 parts when the total of α-type hemihydrate gypsum and β-type hemihydrate gypsum is 100 parts as the hemihydrate gypsum constituting the base material. Also, as can be seen from the results of Table 1, in the present invention, the composition of 100 parts of hemihydrate gypsum is such that the amount of α-type hemihydrate gypsum is 70 to 90 parts and the amount of β-type hemihydrate gypsum is 10 to 30 parts, and further, in terms of viscosity, it is more preferable to set the amount of α-type hemihydrate gypsum to 80 to 90 parts and the amount of β-type hemihydrate gypsum to 10 to 20 parts. Also, as shown in Examples 1-5, when the total amount of the base material is 100 parts by mass, if the content of β-type hemihydrate gypsum is 20 parts by mass or less, there is no problem of the viscosity becoming too high due to the combined use of β-type hemihydrate gypsum. On the other hand, as shown in Comparative Example 2, if the content of β-type hemihydrate gypsum is more than 20 parts by mass, the viscosity becomes too high and is not suitable for practical use.
[0046] [Examples 2-1 to 2-6, Comparative Example 3] From the results of Example 1 described above, a mixture of 90 parts of α-type hemihydrate gypsum and 10 parts of β-type hemihydrate gypsum (α:β=90:10) was used as the hemihydrate gypsum constituting the base material. As shown in Table 2, the amount of hemihydrate gypsum of the above composition, which is an essential component, was gradually changed in the range of 50 to 80 parts, and a constant amount of 20 parts of inorganic aggregate (calcium carbonate) was added as a base material component, and cement (ordinary Portland cement) was added in a gradually changed amount in the range of 0 to 30 parts to prepare compositions of Examples 2-1 to 2-6 and Comparative Example 3. Specifically, the SL materials were obtained by adding predetermined amounts of setting retarder, expansion inhibitor, thickener, and defoamer to the seven types of base materials having different compositions described above in the same manner as in Example 1.
[0047] Using 100 parts of each SL material obtained above, evaluation was performed using the following method. First, 35 parts of water were added to 100 parts of the SL material to prepare a slurry for evaluation. In order to perform the evaluation under the same conditions, when preparing the slurry, a water reducing agent was added to adjust the fluidity so that the flow value of each was 230±2 mm.
[0048] (evaluation) The physical properties of each SL material slurry obtained as described above and the light walking time when the slurry was applied were measured in the same manner as described above. In all tests, it was confirmed that the length change specified in JASS 15M-103 (quality standard for self-leveling materials) was 0.05% or less. The test results are summarized in Table 2.
[0049] TIFF0007563763000002.tif88170
[0050] As shown in Table 2, when cement is used as a constituent of the base material, it was confirmed that the light walkable time tends to be longer when the amount of cement is increased, presumably because the amount of β-type hemihydrate gypsum in the base material is relatively reduced. Furthermore, as shown in Comparative Example 3, it was found that when the total amount of base material materials other than hemihydrate gypsum is increased, the viscosity of the slurry increases, resulting in poor workability.
[0051] [Examples 3-1 to 3-4, Comparative Example 4] From the results of Example 1, a mixture of 90 parts of α-type hemihydrate gypsum and 10 parts of β-type hemihydrate gypsum (α:β=90:10) was used as the hemihydrate gypsum constituting the base material. As shown in Table 3, the composition of the base material was changed stepwise in the range of 45 to 85 parts by adding a constant amount of 15 parts of cement (ordinary Portland cement), and further, the amount of inorganic aggregate (calcium carbonate) was changed stepwise in the range of 0 to 40 parts to prepare the SL materials of Examples 3-1 to 3-4 and Comparative Example 4. Specifically, the SL materials were obtained by adding predetermined amounts of a setting retarder, an expansion inhibitor, a thickener, and an antifoaming agent to the five types of base materials having different compositions described above in the same manner as in Example 1.
[0052] Using 100 parts of each SL material obtained above, evaluation was performed using the following method. First, 35 parts of water were added to 100 parts of the SL material to prepare a slurry for evaluation. In order to perform the evaluation under the same conditions, when preparing the slurry, a water reducing agent was added to adjust the fluidity so that the flow value of each was 230±2 mm.
[0053] (evaluation) The physical properties of each SL material slurry obtained as described above and the light walking time when the slurry was applied were measured in the same manner as described above. In all tests, it was confirmed that the length change specified in JASS 15M-103 (quality standard for self-leveling materials) was 0.05% or less. The test results are summarized in Table 3.
[0054] TIFF0007563763000003.tif83170
[0055] As shown in Table 3, it is believed that as the amount of inorganic aggregate increases, the amount of β-type hemihydrate gypsum in the base material decreases relatively, but it was found that the effect of shortening the light walkable time obtained by devising the composition of the hemihydrate gypsum is lost and the light walkable time tends to increase. Also, as in the case of Example 2, when the amount of base material materials other than hemihydrate gypsum is more than half the total amount of the base material, it was found that the effect of shortening the light walkable time under low temperature conditions is almost lost, as shown in Comparative Example 4.
[0056] [Examples 4-1 to 4-4, Comparative Examples 5 and 6] In this example, a constant amount of 15 parts of cement was added to the base material, and the blending ratio (α and β ratio) of α-type hemihydrate gypsum to β-type hemihydrate gypsum was changed stepwise as shown in Table 4, and an SL material was prepared in the same manner as in Example 1. The SL material obtained was evaluated in the same manner as in Example 1. In all tests, it was confirmed that the length change specified by JASS 15M-103 (quality standard for self-leveling materials) was 0.05% or less. The obtained evaluation results are summarized in Table 4.
[0057] TIFF0007563763000004.tif82170
[0058] As shown in Table 4, it was found that the use of cement as the base material effectively prevented the viscosity of the slurry from becoming too high, which would be caused by increasing the amount of β-type hemihydrate gypsum blended. However, as shown in Comparative Example 6, it was found that when the amount of β-type hemihydrate gypsum exceeds 20 parts per 100 parts of the total base material, the viscosity of the slurry becomes high and workability becomes poor, even if cement is used as the base material.
[0059] [Examples 5-1 to 5-4, Comparative Examples 7 and 8] Unlike the other examples, in this example, the SL material was prepared using only hemihydrate gypsum without using cement or inorganic aggregate as the base material. Specifically, α-type hemihydrate gypsum and β-type hemihydrate gypsum were used as the hemihydrate gypsum constituting the base material, with the mixing ratio gradually changed as shown in Table 5, and the SL material was prepared in the same manner as in Example 1. The obtained SL material was evaluated in the same manner as in Example 1. In addition, in all tests, it was confirmed that the length change specified by JASS 15M-103 (quality standard for self-leveling materials) was 0.05% or less. The obtained evaluation results are summarized in Table 5.
[0060] TIFF0007563763000005.tif73170
[0061] As shown in Table 5, in comparison with Comparative Example 7 in which α-type hemihydrate gypsum was used at 100 parts, it was found that by mixing 100 parts of hemihydrate gypsum constituting the base material with 75 to 95 parts of α-type hemihydrate gypsum and 5 to 25 parts of β-type hemihydrate gypsum in combination, the effect on the extension of the light walkable time that occurs under low temperature conditions can be reduced. However, in the composition of Comparative Example 8 in which 75 parts of α-type hemihydrate gypsum and 25 parts of β-type hemihydrate gypsum were mixed, the light walkable time was improved and there was no problem with the pot life, but since the content of β-type hemihydrate gypsum exceeded 20 parts by mass when the total of the base material was 100 parts by mass, another problem was found to be that, compared with the composition of Comparative Example 7 in which β-type hemihydrate gypsum was not used in combination, the viscosity of the slurry was more than twice as high. For such practical reasons, it was determined that the SL material of the present invention requires that the content of β-type hemihydrate gypsum be 20 parts by mass or less when the total of the base material was 100 parts by mass. From the results of Table 5, it was found that when the base material constituting the SL material of the present invention is composed only of gypsum hemihydrate, it is effective to set the content of α-type hemihydrate to 80 to 95 parts and the content of β-type hemihydrate to 5 to 20 parts, and more preferably the content of α-type hemihydrate to 80 to 90 parts and the content of β-type hemihydrate to 10 to 20 parts, relative to 100 parts in total of α-type hemihydrate and the β-type hemihydrate.
Claims
1. A self-leveling material composition comprising a base material component containing hemihydrate gypsum as an essential component and optionally containing at least one of inorganic aggregate and cement, and an additive, When the total amount of the base components is 100 parts by mass, the content of the hemihydrate gypsum is 55 to 100 parts by mass, the content of the cement is 0 to 25 parts by mass, and the content of the inorganic aggregate is 0 to 30 parts by mass, The hemihydrate gypsum contains α-type hemihydrate gypsum and β-type hemihydrate gypsum, and when the total of the α-type hemihydrate gypsum and the β-type hemihydrate gypsum is 100 parts by mass, the content of the α-type hemihydrate gypsum is 70 to 95 parts by mass and the content of the β-type hemihydrate gypsum is 5 to 30 parts by mass, and further, when the total of the base components is 100 parts by mass, the content of the β-type hemihydrate gypsum is 20 parts by mass or less. A gypsum-based self-leveling material composition characterized in that the length change as defined by JASS 15M-103 (quality standard for self-leveling materials) is 0.05% or less, and that when an evaluation slurry prepared by adding water is applied under conditions of room temperature maintained at 10°C, the light walkable time on the application surface is within 5 hours.
2. 2. The gypsum-based self-leveling material composition according to claim 1, wherein the light walkable time is on the order of four hours.
3. 3. The gypsum-based self-leveling material composition according to claim 1, wherein the cement is any one selected from the group consisting of ordinary Portland cement, high-early-strength Portland cement, blast-furnace cement and alumina cement.
4. The gypsum-based self-leveling material composition according to any one of claims 1 to 3, wherein the components of the base material are hemihydrate gypsum and cement.
5. The gypsum-based self-leveling material composition according to any one of claims 1 to 3, wherein the inorganic aggregate is calcium carbonate.
6. 6. The gypsum-based self-leveling material composition according to any one of claims 1 to 5, wherein the content of the α-type hemihydrate gypsum is 80 to 90 parts by mass and the content of the β-type hemihydrate gypsum is 10 to 20 parts by mass, when the total amount of the hemihydrate gypsum is 100 parts by mass.
7. 2. The gypsum-based self-leveling material composition according to claim 1, wherein the content of the hemihydrate gypsum is 100 parts by mass when the total amount of the base components is 100 parts by mass, and the optional components are not included.
Citation Information
Patent Citations
Gypsum composition having good swelling control effect for floor
JP1980126559A
Fluid gypsum composition
JP1980154365A
High strength flooring composition
JP2005521622A