Methods for forming topology-controlled amorphous carbon polymer films.
The method of using flowable carbon-based films and nitrogen plasma redeposition addresses the challenge of void-free, top-selective deposition in high aspect ratio trenches, ensuring precise film thickness and stability in semiconductor manufacturing.
Patent Information
- Application Number
- JP2020120476
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-07-19
- Filing Date
- 2020-07-14
- Publication Date
- 2024-10-08
- Estimated Expiration
- 2040-07-14
AI Technical Summary
Existing deposition methods struggle with void-free filling of high aspect ratio trenches in semiconductor manufacturing, particularly in applications requiring top-selective deposition of amorphous carbon films, as conventional gap-filling techniques often result in unwanted deposition on sidewalls and bottom surfaces, leading to blocked openings and difficulty in controlling film thickness on the top surface.
A method involving the use of flowable carbon-based films that are deposited in trenches until a predetermined thickness is reached, followed by exposure to a nitrogen plasma in an oxygen and hydrogen-free atmosphere to selectively redeposit the film onto the top surface, utilizing nitrogen plasma to siphon the film from the bottom to the top, achieving top-selective deposition.
This approach ensures void-free filling with precise control over the film thickness on the top surface, enhancing the deposition process by maintaining fluidity and achieving a denser, more stable film composition with improved thermal stability and selectivity.
Smart Images

Figure 0007563908000003 
Figure 0007563908000004 
Figure 0007563908000005
Abstract
Description
[Technical field]
[0001] 2. Background of the Invention The present invention relates generally to a method for forming a topology-controlled carbon-based film on a patterned recess in a substrate, and more particularly to a method for top-selective deposition using a flowable carbon-based film on the patterned recess. [Background technology]
[0002] Processes for fabricating integrated circuits, e.g., for shallow trench isolation, intermetal dielectric layers, passivation layers, etc., often require filling trenches (any recess that typically has an aspect ratio of 1 or greater) with insulating materials. However, as the interconnect pitch of large-scale integrated (LSI) devices shrinks, void-free filling of high aspect ratio spaces (e.g., AR ≥ 3) becomes increasingly difficult due to limitations of existing deposition processes.
[0003] In view of the above, the present inventors have developed a gap-fill technique for the deposition of flowable films, which provides complete gap-fill by plasma-assisted deposition using hydrocarbon precursors with substantially no void formation under conditions where nitrogen, oxygen, or hydrogen plasma is not required, and is disclosed in U.S. patent application Ser. Nos. 16 / 026,711, filed July 3, 2018, and 16 / 427,288, filed May 30, 2019, the disclosures of each of which are incorporated herein by reference in their entireties.
[0004] However, if a particular application requires deposition of only the top of the amorphous carbon using the above gap-filling techniques on a substrate without deposition in the substrate trench, e.g., at the bottom of the trench, e.g., where a sacrificial etch-stop layer or protective layer is required only on the top surface of the recess, the following problems may occur: i) The deposition by the gap-filling technique is essentially a bottom-up deposition, and therefore a certain amount of film may necessarily be deposited on the bottom of the recess; (ii) If the recess is an ultra-deep hole (e.g., having an aspect ratio of more than 10, typically 15-100) used in applications such as 3D NAND, the gap-filling technique may be a bottomless deposition (because the flowable material flows downward but cannot reach the bottom of the recess), but a certain amount of film may necessarily be deposited on the sidewall of the recess due to the material flowing along the sidewall of the recess; iii) In ii), the film is deposited on the top surface. However, because the top opening of the recess is small, the opening may be blocked, eventually causing the film to deposit and accumulate uniformly on the top surface, and iv) if the top opening of the recess is wide enough to allow the flowable material to flow into the recess, it may be difficult to deposit a thick film on the top surface, i.e., it may be difficult to control the thickness of the film deposition on the top surface. The present inventors provide an innovative solution to the above problems using gap-filling technology.
[0005] Any discussion of problems and solutions relating to the related art is included in this disclosure merely for the purpose of providing a background for the invention and should not be construed as an understanding that any or all of the discussions were known at the time the invention was made. Summary of the Invention [Means for solving the problem]
[0006] In view of the above, some embodiments provide a method of top selective deposition using a flowable carbon-based film on a substrate having a recess defined by a top surface, sidewalls, and a bottom, comprising: (i) depositing a flowable carbon-based film in a recess of the substrate in a reaction space until the thickness of the flowable carbon-based film in the recess reaches a predetermined thickness, then stopping the deposition step; and (ii) exposing the carbon-based film to a nitrogen plasma in an atmosphere substantially devoid of hydrogen and oxygen to selectively redeposit the carbon-based film on the top surface. In the above, it is quite surprising that a flowable material once accumulated in a recess, such as a fluid accumulated in a reservoir, can move upward and accumulate on the top surface as if the fluid were siphoned. In one embodiment, a combination of the flowability of the film and the nitrogen plasma allows the carbon-based film to be selectively redeposited on the top surface from the bottom of the recess. In some embodiments, the flowable film needs to accumulate at the bottom of the recess by bottom-up deposition, so the recess needs to have an aspect ratio of 2 to 30 (typically 3 to 20). Gap-filling techniques for deposition of flowable films are disclosed, for example, in U.S. patent application Ser. No. 16 / 026,711, filed July 3, 2018, and Ser. No. 16 / 427,288, filed May 30, 2019, the disclosures of each of which are incorporated by reference in their entirety herein, and such techniques may be applied to some embodiments of the present invention.
[0007] In some embodiments, the carbon-based flowable film accumulating at the bottom of the recess is exposed to a nitrogen plasma, the plasma being substantially devoid of H2 and O2, e.g., the total H2 and O2 concentration in the atmosphere of the reaction space is less than 5%, preferably less than 1%. If the concentration of H2 and O2 in the atmosphere exceeds the above, the plasma exhibits more of an ashing function rather than contributing to the redeposition of the film. Furthermore, in some embodiments, noble gases such as Ar and He may be contained in the atmosphere of the reaction space to the extent that the addition of the noble gas does not significantly affect the redeposition of the carbon-based film when the carbon-based flowable film is exposed to the bottom of the recess, e.g., the concentration of noble gases (e.g., Ar and / or He) is at least less than 50%, preferably less than 30%, more preferably less than 20%, and most preferably less than 15% in total. In some embodiments, the atmosphere consists essentially of or consists of nitrogen gas. In some embodiments, to achieve flowability or bottom-up deposition of the carbon-based film when depositing the carbon-based film, the deposition temperature is adjusted, where the flowability of the film is inversely proportional to the deposition temperature, which is adjusted depending on the type of precursor, for example, at temperatures below about 100° C., e.g., about 75° C.
[0008] In order to summarize the aspects of the present invention and the advantages achieved over the related art, some objects and advantages of the present invention are described in this disclosure. Of course, it should be understood that not all of these objects or advantages may be achieved by any particular embodiment of the present invention. Thus, for example, a person skilled in the art will recognize that the present invention can be embodied or carried out in a manner that achieves or optimizes one or a group of advantages taught herein, without necessarily achieving other objects or advantages taught or suggested herein.
[0009] Further aspects, features, and advantages of the present invention will become apparent from the following detailed description.
[0010] These and other features of the present invention will now be described with reference to drawings of preferred embodiments which are intended to illustrate, rather than limit, the invention, and which have been greatly simplified for illustrative purposes and are not necessarily to scale. [Brief description of the drawings]
[0011] [Figure 1A] FIG. 1A is a schematic diagram of a PEALD (Plasma Enhanced Atomic Layer Deposition) apparatus for depositing dielectric films that can be used in one embodiment of the present invention. [Figure 1B] FIG. 1B is a schematic diagram of a precursor delivery system using a flow path system (FPS) that can be used in one embodiment of the present invention. [Diagram 2] FIG. 2 shows a schematic cross-sectional view of a trench illustrating the process of top selective deposition ((a)→(b)→(c)) according to an embodiment of the present invention. [Diagram 3] FIG. 3 shows a schematic cross-sectional view of a trench illustrating the expected mechanism of top-selective deposition ((a)→(b)→(c)→(d)) according to an embodiment of the present invention. [Figure 4] FIG. 4 is a graph showing the shrinkage of films exposed to plasmas of different gases. [Diagram 5] FIG. 5 shows STEM micrographs of cross-sections of trenches, where row (a) represents a trench subjected to complete-fill deposition of a flowable film, row (b) represents the trench shown in (a) after O2 / Ar ashing, row (c) represents the trench shown in (a) after N2 / H2 ashing, column (1) represents the trench at high magnification (scale bar represents 60 nm), and column (2) represents the trench at low magnification (scale bar represents 300 nm). [Figure 6] FIG. 6 shows (a) a STEM photograph of a cross-section of a trench subjected to flowable film deposition at 75° C. and subsequent exposure to N2 plasma in accordance with one embodiment of the present invention, and (b) a STEM photograph of a cross-section of a trench subjected to nearly non-flowable film deposition at 100° C. and subsequent exposure to N2 plasma. [Figure 7]FIG. 7 shows (a) a STEM photograph of a cross-sectional view of a trench subjected to flowable film deposition followed by exposure to N2 plasma for 10 seconds, and (b) a STEM photograph of a cross-sectional view of a trench subjected to flowable film deposition followed by exposure to N2 plasma for 60 seconds according to one embodiment of the present invention. [Figure 8] FIG. 8 shows a STEM image of a cross-sectional view of a trench subjected to top selective deposition according to an embodiment of the present invention. [Figure 9] FIG. 9 shows Fourier transform infrared (FTIR) spectra of an as-deposited flowable amorphous carbon polymer film ("STD") and a redeposited amorphous carbon polymer film with N2 plasma treatment ("N2-CK") in accordance with one embodiment of the present invention. [Figure 10] FIG. 10 illustrates a process sequence for top selective film formation according to one embodiment of the present invention, where the width of each column does not necessarily represent an actual length of time, and the bottom level of each row line represents an off state while the rising level of each row line represents an on state. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0012] In the present disclosure, a "gas" can include vaporized solids and / or liquids and may be constituted by a single gas or a mixture of gases, depending on the context. Similarly, the article "a" or "an" refers to a species or genus, including multiple species, depending on the context. In the present disclosure, the process gas introduced into the reaction chamber through the showerhead may consist of, consist essentially of, or consist of silicon-free hydrocarbon precursors and additive gases. The additive gas may include a plasma generating gas for exciting the precursors to form amorphous carbon polymers when RF power is applied to the additive gas. The additive gas may be an inert gas that may be supplied to the reaction chamber as a carrier gas and / or dilution gas. The additive gas may not include a reactive gas for oxidizing or nitriding the precursors. Alternatively, the additive gas may include a reactive gas for oxidizing or nitriding the precursors to the extent that it does not interfere with the plasma polymerization to form the amorphous carbon-based polymer. Furthermore, in some embodiments, the additive gas includes only a plasma generating gas (e.g., a noble gas). The precursors and additive gases may be introduced into the reaction space as a mixed gas or separately. The precursors may be introduced with a carrier gas, such as a noble gas. A gas other than the process gas, i.e., a gas introduced without passing through a showerhead, may be used to seal the reaction space, for example, with a seal gas, such as a noble gas. In some embodiments, the term "precursor" generally refers to a compound involved in a chemical reaction that produces another compound, particularly a compound that constitutes the membrane matrix or the backbone of the membrane, and the term "reactant" refers to a compound other than the precursor that activates the precursor, modifies the precursor, or catalyzes the reaction of the precursor, and when in an excited state, the reactant provides elements (e.g., O, C, N, etc.) to the membrane matrix that may become part of the membrane matrix. The term "plasma generating gas" refers to a compound other than the precursor and reactant that generates a plasma when exposed to electromagnetic energy, and the plasma generating gas may not provide the membrane matrix with elements (O, C, N) that become part of the membrane matrix. The term "plasma ashing gas" refers to a gas that ashes the membrane when in an excited state, either directly (direct plasma) or remotely (remote plasma).In some embodiments, the "plasma ashing gas" is a single gas or a mixture of two or more gases. The term "ashing" refers to the use of plasma to remove organic material, leaving mineral constituents as a residue (ash) that is typically removed with a vacuum pump.
[0013] In some embodiments, a "film" refers to a layer that extends continuously in a direction perpendicular to the thickness direction without substantially pinholes to cover the entire object or relevant surface, or simply a layer that covers the object or relevant surface. In some embodiments, a "layer" refers to a structure having a particular thickness formed on a surface, or a synonym of a film, or a structure that is not a film. A film or layer may be composed of a separate single film or layer, or multiple films or layers, having particular properties, and the boundaries between adjacent films or layers may be distinct or not, and may be defined based on any physical, chemical, and / or other characteristics, formation process or sequence, and / or the function or purpose of the adjacent film or layer. Furthermore, in this disclosure, any two variables may constitute a feasible range for that variable, since a feasible range may be determined based on routine operations, and any range stated may include or exclude the endpoints. In some embodiments, further, any values of the stated variables (whether they are stated as "about" or not) may refer to exact or approximate values, may include equivalents, may refer to averages, median, representative values, or majority, etc. Additionally, in this disclosure, the terms "consisting of" and "having" refer, in some embodiments, independently to "typically or broadly including," "comprising," "consisting essentially of," or "consisting of." In this disclosure, any defined meaning does not necessarily exclude the ordinary and customary meaning in some embodiments.
[0014] In this disclosure, "continuously" refers, in some embodiments, to the absence of breaking vacuum, of an interruption in the time sequence, of any intervening material step, of an immediate change in processing conditions as the next step, or of any intervening distinct physical or chemical structure between the two structures other than the two structures themselves.
[0015] In this disclosure, the term "filling ability" (also referred to as flowability) refers to the ability to fill gaps substantially free of voids (e.g., no voids having a size of about 5 nm or greater in diameter) and seams (e.g., no seams having a length of about 5 nm or greater), and seamless / void-free bottom-up growth of a layer is observed when the film is deposited in wide trenches having an aspect ratio of about 1 or greater.
[0016] Flowability often manifests as a concave surface of the film at the bottom of a wide trench prior to filling the trench, and also as a substantially planar top surface of the film during continued deposition after completely filling the trench (planarization). Such deposition is referred to as "bottom-up deposition."
[0017] Even if the film is flowable, when the trench is narrow and deep, the film may not reach the bottom of the trench. In that case, the flowability often appears as a nearly or substantially conformal film along the sidewalls of the trench, with the bottom of the trench being substantially free of the film, and typically the top opening of the trench is closed by the film. Because the film is flowable, the sidewall film flows and extends downward along the sidewalls, thereby forming a thin film, and the ratio of the average thickness of the substantially conformal portion of the film (excluding the top portion that closes the top opening of the trench, which is subsequently removed by ashing) to the depth of the film in the trench (the length that extends along the sidewalls to the bottom) can be in the range of 0.1% to 10% (typically 0.5% to 5%). Such a deposition is referred to as a "bottomless deposition".
[0018] In the present disclosure, the recess between the adjacent protruding structure and any other recess pattern is referred to as a "trench". That is, a trench is any recess pattern that includes a hole / via. For bottom-up deposition, in some embodiments, the trench has a width (if the trench has a length substantially the same as the width, it is referred to as a hole / via) of about 20 nm to about 100 nm (typically, about 30 nm to about 50 nm), a depth of about 30 nm to about 100 nm (typically, about 40 nm to about 60 nm), and an aspect ratio of about 2 to about 10 (typically, about 2 to about 5). The appropriate dimensions of the trench may vary depending on the process conditions, film fluidity, film composition, intended application, etc. For example, by adjusting the film fluidity, bottom-up deposition may be realized in trenches having sizes different from those described above.
[0019] In this disclosure, terms such as "substantially free of deposition," "substantially free of film," and the like refer to an amount functionally equal to zero, an insignificant or inconsequential amount, an amount that does not significantly interfere with a subsequent process (e.g., ashing), an amount less than a detectable or observable amount, and the like.
[0020] In this disclosure, any defined meaning does not necessarily exclude, in some embodiments, the ordinary and customary meaning, and in some embodiments, "the invention" or "the present invention" refers to at least one of the embodiments or aspects explicitly, necessarily, or inherently disclosed herein.
[0021] The embodiments are described in terms of preferred embodiments, however, it is not intended that the invention be limited to the preferred embodiments.
[0022] Some embodiments provide a method of top selective deposition using a flowable carbon-based film on a substrate having a recess defined by a top surface, sidewalls, and a bottom, comprising: (i) depositing a flowable carbon-based film in a recess of the substrate in a reaction space until the thickness of the flowable carbon-based film in the recess reaches a predetermined thickness, then stopping the deposition step; and (ii) exposing the carbon-based film to a nitrogen plasma in an atmosphere substantially devoid of hydrogen and oxygen to selectively redeposit the carbon-based film on the top surface. The carbon-based film may typically be an amorphous carbon polymer film that is a flowable film, but the carbon-based film may be any other suitable carbon-based film that is derived from a precursor and can be plasma polymerized and deposited in a flowable manner. The carbon-based film may contain Si (e.g., polycarbosilane polymer) or may be free of Si (e.g., cyclopentene-derived hydrocarbon polymer).
[0023] When the amorphous carbon polymer film is formed by using a plasma-assisted method, the resulting amorphous carbon polymer film is composed of hydrogenated amorphous carbon polymer. In this disclosure, hydrogenated amorphous carbon polymer may be simply referred to as amorphous carbon polymer, which may be abbreviated as "aC:H" or simply "aC". Furthermore, in this disclosure, SiC, SiCO, SiCN, SiCON, etc. are abbreviations that indicate film type (simply indicated by the major constituent elements) in a non-stoichiometric manner, unless otherwise stated.
[0024] In some embodiments, steps (i) and (ii) are repeated multiple times (e.g., 1-100 times, typically 2-20 times) until the thickness of the carbon-based film on the top surface reaches a desired final thickness (e.g., 1-100 nm, typically 2-20 nm), which may vary and differ depending on its intended use and application. When the carbon-based film reaches its final thickness and steps (i) and (ii) are stopped, the flowable carbon-based film at the bottom of the recess may be completely removed if desired, but its thickness has been reduced by step (ii). However, preferably, the final thickness of the carbon-based film on the top surface is greater than the thickness of the flowable carbon-based film at the bottom, so that plasma ashing (anisotropic) can be performed to further or completely remove the bottom carbon-based film, while some thickness of the top carbon-based film remains.
[0025] In some embodiments, the predetermined thickness in step (i) is greater than the thickness of a monolayer but is 15 nm or less (7.5 nm or less, more preferably 5 nm or less), and steps (i) and (ii) are repeated multiple times.
[0026] Deposition of flowable films is known in the art. However, conventional deposition of flowable films uses chemical vapor deposition (CVD) with constant application of RF power, since pulsed plasma assist such as PEALD is known to deposit conformal films, which are films with properties exactly opposite to those of flowable films. In some embodiments, the flowable film is a silicon-free carbon-containing film comprised of amorphous carbon polymers, and while any suitable one or more of the hydrocarbon precursors can be candidates, in some embodiments the precursor comprises an unsaturated or cyclic hydrocarbon with a vapor pressure of 1,000 Pa or more at 25° C. In some embodiments, the precursor is a C2-C8 alkyne (C n H 2n-2 ), C2-C8 alkenes (C n H 2n ), C2-C8 dienes (C n H n+2 ), C3-C8 cycloalkenes, C3-C8 annulenes (C n H n), C3-C8 cycloalkanes, and substituted hydrocarbons as above. In some embodiments, the precursor is ethylene, acetylene, propene, butadiene, pentene, cyclopentene, benzene, styrene, toluene, cyclohexene, and / or cyclohexane.
[0027] In some embodiments, the gap-fill technique for the deposition of flowable films may be the method disclosed in U.S. Patent Application Nos. 16 / 026,711 and 16 / 427,288, the disclosures of which are incorporated herein by reference in their entirety, which provides complete gap-filling by plasma-assisted deposition using hydrocarbon precursors with substantially no void formation under conditions where no nitrogen, oxygen, or hydrogen plasma is required. The volumetric processes disclosed in the above references use ALD-like recipes (e.g., feed / purge / plasma strike / purge) in which the post-feed purge is spontaneously significantly shortened to leave a high partial pressure of precursor during plasma strike. This is clearly distinct from ALD chemistry and mechanisms. Although ALD-like recipes may be more beneficial as discussed later, the above process may be based on pulsed plasma CVD, which also imparts good filling capabilities to the resulting films. In some embodiments, step (i) is performed by ALD-like deposition using nitrogen plasma or periodic nitrogen plasma deposition such as pulsed plasma CVD.
[0028] In some embodiments, the atmosphere in step (ii) is within the reaction space used in step (i), i.e., steps (i) and (ii) are carried out sequentially in the same reaction space, or, in some embodiments, the atmosphere in step (ii) is within a separate reaction space that is different from the reaction space used in step (i).
[0029] In some embodiments, step (ii) includes supplying N2 without supplying hydrogen and oxygen, and applying RF power to the atmosphere in a manner that generates a nitrogen plasma. Applying RF power to the atmosphere may be accomplished using a conductively coupled plasma (CCP) reactor or an inductively coupled plasma (ICP) reactor, and in some embodiments, the nitrogen plasma may be generated as a remote plasma using a remote plasma unit. In some embodiments, the RF power is 0.14 W / cm per unit area of the substrate. 2 ~1.41W / cm 2 (Preferably 0.3 to 0.9 W / cm 2 ) and the duration of step (ii) is in the range of 10 seconds to 300 seconds (preferably 30 to 120 seconds).
[0030] In some embodiments, the method further comprises, after step (ii), removing the flowable carbon-based film at the bottom by O2, H2, O2 / Ar, or N2 / H2 plasma ashing, the carbon-based film being deposited primarily or substantially exclusively on the top surface of the substrate, among the top surface of the recess, the sidewalls, and the recess, such that the target topology may be fully achieved. In some embodiments, the plasma ashing is performed using direct or remote oxygen or hydrogen plasma. In some embodiments, the direct or remote oxygen or hydrogen plasma may be H2 only, a mixture of Ar and H2 (Ar / H2 flow ratio 0.005-0.995, typically 0.05-0.75), a mixture of He and H2 (He / H2 flow ratio 0.005-0.995, typically 0.05-0.75), a mixture of N2 and H2 (N2 / H2 flow ratio 0.005-0.995, typically 0.05-0.75), O2 only, a mixture of O2 and Ar (O2 / Ar flow ratio The plasma is a direct or remote plasma of a gas(es) selected from the group consisting of a mixture of O2 and He (O2 / He flow ratio 0.005-0.995, typically 0.05-0.75), a mixture of O2 and He (O2 / He flow ratio 0.005-0.995, typically 0.05-0.75), and a mixture of O2 and N2 (O2 / N2 flow ratio 0.005-0.995, typically 0.05-0.75). In some embodiments, the top surface of the substrate on which the carbon-based film is redeposited is comprised of silicon.
[0031] In some embodiments, the substrate has a plurality of recesses with an aspect ratio of 2-30 (typically 3-20), which are filled with a film in a bottom-up manner in step (i), with changes in surface topology due to loading effects. However, in some embodiments, the height of the redeposited carbon-based film on the top surface is approximately the same regardless of the width of the trench (no loading effect). This may be due to the volumetric nature of the growth, i.e., the amount of material deposited in each trench before N2 treatment is approximately the same regardless of the width of the trench (provided that the width difference is not extensive).
[0032] Embodiments will be described with reference to the drawings, but the invention is not intended to be limited to the drawings.
[0033] FIG. 2 is a diagram showing a schematic cross-sectional view of a trench illustrating a process of top-selective deposition ((a)→(b)→(c)) based on the phenomenon according to an embodiment of the present invention. First, in FIG. 2(a), bottom-up deposition is performed on a substrate having a trench, where the substrate 21 has a trench 20 with a width wide enough to allow the flowable film to flow into the trench and a depth small enough for the flowable film to reach the bottom of the trench 20. As a result, the flowable film is mainly deposited on the bottom of the trench 20 as a bottom flowable film 23 and partially deposited on the top surface of the trench 20 as a top flowable film 22. As an example, a suitable size of the trench is described in this disclosure and can be selected, for example, according to the flowability of the film. It is noted that FIG. 2 is overly simplified and not to scale.
[0034] Next, in the redeposition process of (b), the bottom flowable film 23 is exposed to a nitrogen plasma which generates gaseous species within the trench 20. The gaseous species are trapped within the trench 20, occupy the trench 20, and reach the top surface of the trench 20 (see FIG. 3 for a detailed description). In (c), the gaseous species are deposited (or redeposited) on the top surface of the trench 20, accumulating thereon as a top film 24. This is accomplished in a manner similar to molecular beam epitaxy growth. It should be noted that the above theory is a non-limiting theory of redeposition and does not necessarily impose any limitations on this redeposition process.
[0035] 3 shows a schematic cross-sectional view of a trench further illustrating the predicted mechanism of top-selective deposition ((a)→(b)→(c)→→(d)) based on the predicted mechanism according to an embodiment of the present invention. Step (a) in this figure is the same as step (a) in FIG. 2.
[0036] In (b), when the bottom flowable film 23 is exposed to nitrogen plasma (anisotropic), the etching of the bottom flowable film 23 (as well as the top film 22) and the formation of gaseous CxNyHz species (where each of x, y, and z is an integer other than 0 and forms a stoichiometric chemical form) occurs instantaneously, forming high density gaseous CxNyHz species 25 in the trench 20 above the etched bottom flowable film 23' while simultaneously forming low density gaseous CxNyHz species 25' above the top surface. The above phenomenon occurs due to the relatively weak / low quality of the untreated flowable material that makes up the flowable film.
[0037] In (c), the nitrogen plasma causes ion beam-like deposition because the nitrogen plasma is highly directional at certain pressure methods, e.g., in the range of 100-1000 Pa, preferably 200-800 Pa, more preferably 300-700 Pa. The ion beam-like deposition occurs instantaneously, whereby the top film 24' is redeposited on the top surface, leaving a bottom flowable film 23''. Presumably, the top selective redeposition occurs because (a) there is little or no deposition layer left on the top surface, and thus the sticking coefficient of the CxNyHz species is higher for the pattern material (silicon in this case) than for the original flowable film, and (b) the density of the gas species is high in the trench 20, and therefore not enough ions can pass through the cloud of gas species in the trench to the extent that they are involved in the ion beam-like deposition at the bottom. Note that the above theory is a non-limiting theory of redeposition and does not necessarily impose any limitations on this redeposition process.
[0038] By repeating steps (a)-(c), the final structure shown in (d) is obtained, where a final top film 24 ("redeposited film") is redeposited on the top surface while substantially no or little film is left at the bottom of the trench. The redeposited film 24 has a different composition and properties than the top flowable film 22 or the bottom flowable film 23 before the nitrogen plasma treatment, and in some embodiments, the redeposited film 24 has a higher density (or higher RI), a lower contact angle, a higher compressive stress, a lower thermal shrinkage, a lower carbon content, a higher nitrogen content, etc., compared to that of the flowable films 22 or 23. Thus, in some embodiments, the redeposited film is comprised of a nitrocarbon-based film compared to a flowable film comprised of a hydrocarbon-based film.
[0039] FIG. 10 illustrates a process sequence for top selective film formation according to one embodiment of the present invention, where the width of each column does not necessarily represent an actual length of time, and the bottom level of each row line represents an off state while the rising level of each row line represents an on state.
[0040] The process sequence includes a deposition process, "ax (aC deposition)" ("FEED" → "PURGE 1" → "RF" (plasma polymerization) → "PURGE 2", performed a times, i.e., repeated (a-1) times), a redeposition process, "N2 treatment" ("N2-In" (stabilization) → "N2 treatment" (redeposition) → "PURGE 3"), and an optional plasma ashing process, "O2 / Ar or N2 / H2 descum" ("N2 / H2-In") → "Trim / descum" (plasma ashing) → "PURGE 4"). The thickness of the redeposited film on the top surface in a single exposure to nitrogen plasma is limited because the amount of gas species generated from the flowable film in a single exposure to nitrogen plasma is limited by the limited depth of the flowable film reached by the nitrogen plasma containing ions passing through the cloud of gas species in the trench (e.g., 15 nm, 7.5 nm, or 5 nm or less) and / or by the nature of the redeposition to generate gas species. The flowable film does not need to maintain its flowability when exposed to nitrogen plasma, since the flowability is lost relatively quickly when continuously exposed to plasma for deposition and / or redeposition (although in some embodiments, the flowability may be maintained). The ability of redeposition may belong to the nature of the flowable film, for example, the film is an oligomeric product, which is a soft / low density material compared to typical carbon-based films, the nature of which makes it susceptible to reaction with nitrogen plasma and enables the redeposition process. In some embodiments, the thickness of the redeposited film in one exposure to nitrogen plasma ranges from 2 to 20 nm, typically 5 to 15 nm, but the range varies greatly depending on the area of the top surface between adjacent trenches, the size of the reservoir, i.e., the opening size and depth of the flowable film in the trench, the degree of gas species attachment, and other conditions / parameters. Thus, steps (a) to (c) shown in FIG. 3 may be repeated to obtain a final film with the desired thickness shown in step (d) of FIG. 3. In FIG. 10, where the deposition process, nitrogen plasma treatment process, and optional plasma ashing process constitute one cycle of redeposition (full cycle), the cycle may be performed b times (i.e., repeated (b-1) times, where b is an integer between 1 and 100, typically between 2 and 15).The ashing process does not have to be performed every time the entire cycle is repeated, but can be performed intermittently as needed with respect to the desired topology of the final film.
[0041] In some embodiments, the plasma polymerization process includes depositing an amorphous carbon polymer film on a substrate having a trench by PEALD-like deposition using a Si- and metal-free C-containing precursor and a plasma generating gas that generates a plasma by applying RF power between two electrodes (between which the substrate is placed parallel to the two electrodes), where RF power is applied in each sublayer deposition cycle of the PEALD-like deposition, and the plasma generating gas and the carrier gas flow continuously and also serve as purge gas during "purge 1" and "purge 2". The above process is a PEALD-like process, where one cycle of the process for forming a sublayer (typically thicker than a monolayer) is performed a times (e.g., a is an integer between 1 and 30, typically between 2 and 15) until the thickness of the film reaches a thickness greater than the thickness of a monolayer but not greater than 15 nm (e.g., 1 nm to 7.5 nm).
[0042] In some embodiments, the feed time is in the range of 0.3-10 seconds (typically 0.6-2 seconds), the post-feed purge time is in the range of 0-0.1 seconds (typically 0-0.5 seconds), the RF time is in the range of 0.5-4 seconds (typically 0.8-2 seconds), the post-RF purge time is in the range of 0-0.5 seconds (typically 0-0.1 seconds), the carrier gas flow rate is in the range of 0-0.8 slm (typically 0.1-0.3 slm), the plasma generating gas flow rate is in the range of 0-0.5 slm (typically 0.1-0.3 slm), and the RF power is in the range of 50-400 W (typically 75-200 W) for a 300 mm wafer (for different size wafers, the above wattages are calculated based on the unit area (cm) of each wafer). 2 ) is applied as W per kW.
[0043] Film fluidity is obtained temporarily, for example, when a volatile hydrocarbon precursor is polymerized by the plasma and deposited on the surface of a substrate, where the gaseous monomer (precursor) is activated or fragmented by the energy provided by the plasma gas discharge to initiate polymerization, and the resulting polymeric material is deposited on the surface of the substrate, where the material exhibits temporary fluid behavior. Once the deposition step is complete, the fluid film is no longer fluid and solidifies, and therefore no separate solidification process is required.
[0044] The redeposition process is then initiated, which includes, for example, stopping the diluent He supply and starting the nitrogen gas supply ("N2-In") while continuously supplying carrier He (in some embodiments, Ar and / or N2 may alternatively or additionally be used as a carrier gas), which should be limited to less than 50%, preferably less than 30%, more preferably less than 20%, typically less than 15% of the gas mixture in the reaction space for effective redeposition. In some embodiments, the nitrogen gas flow rate is in the range of 0.5-20 slm (typically 1-3 slm). Then, RF power is applied to the reaction space to generate nitrogen plasma and expose the flowable amorphous carbon polymer film thereto ("N2 treatment"), the RF power being in the range of 100-1,000 W (preferably 200-800 W, more preferably 300-700 W) for a 300 mm wafer, for a duration of 5-300 seconds (preferably 20-120 seconds, more preferably 30-90 seconds) under a pressure of 100-1,000 Pa (preferably 600 Pa or less, more preferably 400 Pa or less) (for wafers of different sizes, the above wattages are calculated per unit area (cm) of each wafer). 2 )). A purge is then initiated ("Purge 3"), with the purge time after the nitrogen plasma treatment ranging from 0 to 60 seconds (preferably 10 to 30 seconds). During the redeposition process, only H2 addition to the N2 plasma results in ashing (which does not contribute to redeposition and top selectivity), so the gas mixture during the redeposition treatment should be substantially devoid of H2 and O2, e.g., preferably less than 5%, more preferably less than 1%, or substantially 0%.
[0045] Next, depending on the target topology of the final carbon-based film, an optional plasma ashing process is initiated, which involves supplying an ashing gas (H2 or O2, or a mixture of the above with N2, Ar, and / or He) to the reaction space excited by RF power ("N2 / H2-In") to generate a plasma and ash the amorphous carbon polymer film ("Trim / Descum"), followed by purging ("Purge 4"), in which a supply of dilute He is disclosed while a carrier gas is continuously supplied to the reaction space. In some embodiments, the RF power for plasma ashing is in the range of 5-200 W (typically 50-200 W) for a duration of 200 seconds (typically 10-100 seconds) under a pressure of 100 Pa-1000 Pa (typically 200-600 Pa), the stabilization time is in the range of 5-60 seconds (typically 10-30 seconds), the post-RF purge time is in the range of 5-60 seconds (typically 10-30 seconds), and the ashing gas flow rate is in the range of 0.1-10 slm (typically 0.5-2 slm).
[0046] In some embodiments, the carrier gas is continuously supplied to the reaction space throughout the process, and the temperature of the process is adjusted, for example, in the range of −50° C. to 175° C. (preferably 35° C. to 150° C.) to achieve flowability of the amorphous carbon polymer film and enable redeposition of the nitrogen-doped hydrocarbon polymer film.
[0047] A continuous flow of carrier gas can be achieved using a flow path system (FPS), in which a carrier gas line is provided with a bypass line with a precursor reservoir (bottle), and the main line and the bypass line are switched, and when only carrier gas is intended to be supplied to the reaction chamber, the bypass line is closed, while when both carrier gas and precursor gas are intended to be supplied to the reaction chamber, the main line is closed, and the carrier gas flows through the bypass line and flows out of the bottle together with the precursor gas. In this way, the carrier gas can flow continuously into the reaction chamber, and the precursor gas can be delivered in pulses by switching between the main line and the bypass line. FIG. 1B illustrates a precursor supply system using a flow path system (FPS) according to an embodiment of the present invention (black valve indicates that the valve is closed). As shown in FIG. 1B (a), when a precursor is supplied to a reaction chamber (not shown), first, a carrier gas such as Ar (or He) flows through a gas line with valves b and c, and then enters a bottle (reservoir) 26. The carrier gas flows out of the bottle 26 carrying an amount of precursor gas according to the vapor pressure in the bottle 26, flows through a gas line having valves f and e, and is then supplied to the reaction chamber together with the precursor. In the above, valves a and d are closed. When only the carrier gas (noble gas) is supplied to the reaction chamber, the carrier gas flows through the gas line having valve a while bypassing the bottle 26, as shown in (b) of FIG. 1B. In the above, valves b, c, d, e, and f are closed.
[0048] The process cycle may be carried out using any suitable apparatus, including, for example, the apparatus shown in FIG. 1A. FIG. 1A is a schematic diagram of a PEALD apparatus usable in some embodiments of the present invention, preferably integrated with a controller programmed to carry out the sequence described below. In this figure, a pair of conductive plate electrodes 4, 2 are provided in parallel facing each other in the interior 11 (reaction region) of a reaction chamber 3, and a plasma is excited between the electrodes by applying HRF power (13.56 MHz to 2000 MHz) 25 to one side and electrically grounding the other side 12. A temperature regulator is provided on the lower stage 2 (lower electrode), and the temperature of a substrate 1 placed thereon is kept constant at a predetermined temperature. The upper electrode 4 also functions as a shower plate, and reaction gases and / or dilution gases, if any, and precursor gases are introduced into the reaction chamber 3 through gas lines 27 and 28, respectively, and through the shower plate 4. In addition, a circular duct 13 having an exhaust line 7 is provided in the reaction chamber 3, through which gases in the interior 11 of the reaction chamber 3 are exhausted. In addition, the transfer chamber 5 disposed below the reaction chamber 3 is provided with a seal gas line 29 for introducing a seal gas into the interior 11 of the reaction chamber 3 through the interior 16 (transfer zone) of the transfer chamber 5, and is provided with a separation plate 14 for separating the reaction zone from the transfer zone (the gate valve through which the wafer is transferred in and out of the transfer chamber 5 is omitted from this figure). The transfer chamber is also provided with an exhaust line 6. In some embodiments, the deposition of the multi-element film and the surface treatment are performed in the same reaction space, so that all steps can be performed consecutively without exposing the substrate to air or other oxygen-containing atmospheres.
[0049] In some embodiments, in the apparatus shown in FIG. 1A, a system for switching between inert gas flow and precursor gas flow as illustrated in FIG. 1B (discussed above) may be used to introduce pulses of precursor gas without substantially fluctuating the pressure in the reaction chamber.
[0050] Those skilled in the art will appreciate that the apparatus includes one or more controllers (not shown) programmed or otherwise configured to cause the deposition and reactor cleaning processes described elsewhere herein. As will be appreciated by those skilled in the art, the controller(s) are in communication with the various power sources, heating systems, pumps, robotics, and gas flow controllers or valves of the reactor.
[0051] In some embodiments, a dual chamber reactor (two sections or compartments for processing wafers placed close to each other) may be used, in which reactant and noble gases may be supplied through shared lines, while precursor gases are supplied through non-shared lines.
[0052] Films with filling capabilities can be applied in various semiconductor devices, including but not limited to cell isolation in 3D cross-point memory devices, self-aligned vias, dummy gates (replacing current poly-Si), reverse tone patterning, PC RAM isolation, cut hard mask, and DRAM storage node contact (SNC) isolation.
[0053] [Example] In the following examples where conditions and / or structures are not specified, one of skill in the art can readily provide such conditions and / or structures in light of the present disclosure as a matter of routine experimentation. One of skill in the art will understand that the apparatus used in the examples included one or more controllers (not shown) programmed or otherwise configured to effect the deposition and reactor cleaning processes described elsewhere herein. As will be appreciated by one of skill in the art, the controllers were in communication with various power sources, heating systems, pumps, robots, and gas flow controllers or valves of the reactor.
[0054] Reference example 1 (Figure 4) A flowable amorphous carbon polymer film (aC blanket layer) was deposited on a Si substrate (having a diameter of 300 mm and a thickness of 0.7 mm) using cyclopentene to a thickness of 100-150 nm by a PEALD-like process defined in US patent application Ser. Nos. 16 / 026,711 and 16 / 427,288, followed by a deposition process shown in Fig. 10 under the conditions shown in Table 1 below, using the apparatus shown in Fig. 1A and the gas delivery system (FPS) shown in Fig. 1B. A post-deposition plasma treatment was performed on the flowable amorphous carbon polymer film under the conditions shown in Table 1 below, in the same reaction chamber as the deposition process, to evaluate the film shrinkage effect of each post-deposition treatment.
[0055] [Table 1]
[0056] Furthermore, all data reported in FIG. 10 regarding ashing was performed on layers that did not receive a nitrogen plasma treatment cycle.
[0057] Figure 4 is a graph showing the results of shrinkage of films exposed to plasmas of different gases. As shown in Figure 4, the effect of post-deposition plasma treatment on a blanket layer of flowable a-C varies depending on the gas type as follows:
[0058] Ar: Small thickness reduction (if the treatment is prolonged this effect saturates) → densification.
[0059] H2: Large thickness loss (if the treatment is prolonged this effect does not saturate but will ash all the film) → "normal" ash / dry etch effect.
[0060] N2 / H2: Large thickness loss (if the treatment is prolonged this effect does not saturate but will ash all the film, see also Figure 5) → "normal" ash / dry etch effect.
[0061] O2 / Ar: Large thickness loss (if the process is prolonged, this effect does not saturate, but will ash all the film, see also Figure 5) → "normal" ash / dry etch effect; and N2: Increased thickness → opposite of the "normal" ashing / dry etching effect.
[0062] Surprisingly, nitrogen plasma treatment performed on the flowable aC film caused redeposition (attachment) of the plasma-generated gas species.
[0063] Reference Example 2 (Figure 5) Flowable amorphous carbon polymer films (aC films) were deposited on Si substrates (having a diameter of 300 mm and a thickness of 0.7 mm) having trenches with openings of about 25-100 nm having depths of about 85 nm (aspect ratios were about 3.4-0.85) by a bottom-up PEALD-like process under the same conditions and in the same manner as in Reference Example 1, except that deposition was continued until the trenches were completely filled and the top surface of the aC film was planar. A post-deposition plasma treatment was then performed under the same conditions and in the same manner as in Reference Example 1 using O2 / Ar and N2 / H2, except that the plasma treatment was continued until all of the film was removed.
[0064] FIG. 5 shows STEM pictures of cross-sections of trenches, where row (a) represents a trench subjected to full-fill deposition of a flowable film, row (b) represents the trench shown in (a) after O2 / Ar ashing, row (c) represents the trench shown in (a) after N2 / H2 ashing, column (1) represents the trench at high magnification (scale bar represents 60 nm), and column (2) represents the trench at low magnification (scale bar represents 300 nm). It is confirmed that both O2 / Ar ashing and N2 / H2 ashing result in complete removal of the film.
[0065] Example 1 and Comparative Example 1 (FIG. 6) In Example 1, flowable amorphous carbon polymer films (aC films) were deposited by a bottom-up PEALD-like process on a Si substrate (having a diameter of 300 mm and a thickness of 0.7 mm) having trenches with openings of about 70-100 nm having a depth of about 85 nm (aspect ratios were about 1.2-0.85) under the same conditions and in the same manner as in Reference Example 1, except that 36 deposition cycles (3 x 12 deposition cycles + N2 plasma treatment) were performed. In Comparative Example 1, amorphous carbon polymer films were deposited in the same manner as in Example 1, except that the deposition temperature (susceptor and wall temperature) was 100°C compared to 75°C in Example 1. Periodic nitrogen plasma treatments were then performed on each film under the same conditions and in the same manner as in Reference Example 1 using N2 as the post-treatment gas, except that the nitrogen plasma treatment was performed for 60 seconds.
[0066] FIG. 6 shows (a) a STEM photograph of a cross section of a trench subjected to film deposition at 75° C. and subsequently exposed to N2 plasma in Example 1, and (b) a STEM photograph of a cross section of a trench subjected to film deposition at 100° C. and subsequently exposed to N2 plasma in Comparative Example 1. It can be seen from FIG. 6 that the nitrogen plasma treatment is not the only parameter responsible for the top selectivity, i.e., both films were subjected to the same cyclical process of deposition and the same nitrogen plasma treatment, but one (Example 1) was deposited at 75° C. and the other (Comparative Example 1) was deposited at 100° C., resulting in a large difference in topology in the final film. Considering that the fluidity of the deposited film is inversely proportional to the deposition temperature, and the film deposited at 75° C. is fluid while the film deposited at 100° C. is hardly fluid, the difference in topology is expected to be attributed to the fact that only the fluid (weak, fragile, low quality) layer when subjected to N2 plasma can form gas species, which leads to redeposition and top selectivity. By adjusting the deposition temperature as well as other process parameters, films can be deposited while maintaining flowability and obtaining top-preferential topologies in the final film when exposed to nitrogen plasma. One skilled in the art can readily suggest such conditions and / or structures with the present disclosure in view of routine experimentation.
[0067] Example 2 and Comparative Example 2 (Figure 7) In Example 2, a flowable amorphous carbon polymer film (aC film) was deposited by a bottom-up PEALD-like process under the same conditions and in the same manner as Example 1 on a Si substrate (having a diameter of 300 mm and a thickness of 0.7 mm) having a trench with an opening of about 70-100 nm having a depth of about 85 nm (aspect ratio was about 1.2-0.85). A post-deposition nitrogen plasma treatment was then performed on the film under the same conditions and in the same manner as Example 1. In Comparative Example 2, the same process was performed under the same conditions as Example 2, except that the nitrogen plasma treatment was performed for 10 seconds compared to 60 seconds in Example 2.
[0068] FIG. 7 shows (a) a STEM photograph of a cross-section of a trench subjected to flowable film deposition in Comparative Example 2 followed by exposure to N2 plasma for 10 seconds, and (b) a STEM photograph of a cross-section of a trench subjected to flowable film deposition in Example 2 followed by exposure to N2 plasma for 60 seconds. It can be seen from FIG. 7 that a longer N2 plasma treatment is beneficial for top topology selectivity. By adjusting the duration of the nitrogen plasma treatment, the film can be deposited in a top-selective manner. Those skilled in the art can easily suggest such conditions and / or structures in view of the present disclosure as routine experimentation.
[0069] Example 3 (Table 2, Figure 9) In Example 3, an amorphous carbon polymer film was formed under the same conditions and in the same manner as in Example 1, and then a nitrogen plasma treatment was performed on the film under the same conditions and in the same manner as in Example 1 to obtain an amorphous carbon polymer film redeposited on the top surface of the trench. The properties of the resulting amorphous carbon polymer film were evaluated. The results are shown in Table 2 below and FIG. 9.
[0070] [Table 2]
[0071] As shown in Table 2, the thermal shrinkage of the amorphous carbon polymer film with nitrogen plasma treatment ("redeposited film") was significantly lower than that of the amorphous carbon polymer film without plasma treatment ("STD film", standard film), indicating that the thermal stability of the redeposited film was improved. Furthermore, compositional analysis shows that the redeposited film was a nitrogen-doped hydrocarbon film, while the standard film was a hydrocarbon film. Furthermore, the redeposited film had a higher RI (higher density), lower contact angle, and higher compressive stress than that of the standard film. In addition, the Fourier transform infrared (FTIR) spectra of the deposited amorphous carbon polymer film ("STD") and the redeposited amorphous carbon polymer film with N2 plasma treatment ("N2-CK") are shown. As shown in Figure 9, the redeposited films gave rise to -NH and -RNC bonds, and considering the results shown in Table 2, it was likely that the redeposited films promoted further polymerization of the film matrix and were doped with nitrogen, thereby reducing thermally labile hydrogen-related fractions such as methyl and / or methylene fractions from the amorphous carbon polymer films. Note that oxygen atoms were detected in each film, which may be due to the films being exposed to air after the substrate was removed from the reaction chamber.
[0072] In some embodiments, the standard film is a hydrogenated amorphous carbon polymer having a composition made up of more than 50% carbon atoms and more than 35% but less than 50% hydrogen atoms (e.g., as measured using Rutherford backscattering spectroscopy (RBS)), while the redeposited film is a nitrogen-doped hydrogenated amorphous carbon polymer having a composition made up of more than 35% but less than 50% carbon atoms, and more than 35% but less than 50% hydrogen atoms, and more than 10% but less than 20% nitrogen atoms.
[0073] Example 4 (Figure 8) In Example 4, a flowable amorphous carbon polymer film (aC film) was deposited by a bottom-up PEALD-like process under the same conditions and in the same manner as in Example 1 on a Si substrate (having a diameter of 300 mm and a thickness of 0.7 mm) having trenches with openings of about 70-100 nm having a depth of about 85 nm (aspect ratios were about 1.2-0.85). A post-deposition nitrogen plasma treatment was then performed on the film under the same conditions and in the same manner as in Example 1. However, in Example 4, a total of 25 cycles (12 deposition cycles + N2 plasma treatment) were performed.
[0074] FIG. 8 shows a STEM photograph of a cross-section of a trench subjected to top-selective deposition in Example 4. As shown in FIG. 8, a remarkable top-selective topology of the film was achieved, with the thickness of the redeposited film on the top surface being about 145 nm, while the thickness of the film at the bottom of the trench was about 1-3 nm. The bottom film can be substantially or completely removed by plasma ashing (although the deposited film is also ashed to about the same extent as the bottom film, since the thickness difference between the top and bottom films is too large to cause negligible reduction in the thickness of the top film).
[0075] It will be apparent to those skilled in the art that many and various modifications can be made without departing from the spirit and scope of the present invention. Therefore, it should be clearly understood that the forms of the present invention are illustrative only and are not intended to limit the scope of the present invention. [Explanation of symbols]
[0076] 2, 4 Conductive plate electrode 3. Reaction chamber 5. Transfer chamber 7 Exhaust Line 11 Inside the reaction chamber 13 Circular Duct 14 Separation plate 16 Inside the transfer chamber 25 HRF Power 27, 28 Gas lines 29 Seal gas line
Claims
1. 1. A method of top-selective deposition using a flowable carbon-based film on a substrate having a recess defined by a top surface, sidewalls, and a bottom, comprising: (i) depositing a flowable carbon-based film in the recess of the substrate in a reaction space until the thickness of the flowable carbon-based film in the recess reaches a predetermined thickness, and then stopping the depositing step; (ii) exposing the flowable carbon-based film to a nitrogen plasma in an atmosphere substantially devoid of hydrogen and oxygen to etch the flowable carbon-based film and selectively redeposit a top carbon-based film on the top surface.
2. 2. The method of claim 1, wherein steps (i) and (ii) are repeated multiple times until the thickness of the top carbon-based film on the top surface reaches a desired final thickness.
3. 2. The method of claim 1, wherein the predetermined thickness in step (i) is greater than the thickness of a monolayer but not greater than 15 nm.
4. 2. The method of claim 1, wherein the atmosphere in step (ii) is within the reaction space used in step (i).
5. 2. The method of claim 1, wherein the atmosphere in step (ii) is in a separate reaction space that is different from the reaction space used in step (i).
6. Step (ii) is Without supplying hydrogen and oxygen, N 2 to the atmosphere; and applying RF power to the atmosphere in a manner to generate the nitrogen plasma.
7. The RF power is 0.14 W / cm per unit area of the substrate. 2 ~1.41 W / cm 2 and the duration of step (ii) is in the range of 10 seconds to 300 seconds.
8. The method of claim 1 , wherein step (i) is performed by cyclic nitrogen plasma deposition.
9. The method of claim 1 , wherein the top surface of the substrate onto which the top carbon-based film is redeposited is comprised of silicon.
10. After step (ii), the flowable carbon-based film at the bottom is O 2 , H 2 , O 2 / Ar, or N 2 / H 2 The method of claim 1 further comprising removing by plasma ashing.
11. The method of claim 1 , wherein the top carbon-based film is an amorphous carbon film.
12. The method of claim 1, wherein the deposited flowable carbon-based film is composed of a hydrogenated amorphous carbon polymer, while the top carbon-based film is composed of a nitrogen-doped hydrogenated amorphous carbon polymer.
Citation Information
Patent Citations
Hardening method for amorphous carbon film
JP1994333916A
Fluidable carbon for semiconductor processing
JP2015530742A
Method for forming film bottom-up in recessed feature
JP2017208534A
Flowable carbon film with fcvd hardware using remote plasma pecvd
JP2017505548A
Processing apparatus and embedding method
JP2019192733A