Ferritic stainless steel and its manufacturing method

A ferritic stainless steel with controlled Ti and Nb solid solutions and specific manufacturing processes forms an oxide film that addresses oxidation and conductivity issues, providing enhanced high-temperature performance for conductive members.

JP7563919B2Active Publication Date: 2024-10-08NIPPON STEEL CORPORATION
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
JP2020141921
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-08-25
Publication Date
2024-10-08
Estimated Expiration
2040-08-25

AI Technical Summary

Technical Problem

Ferritic stainless steels used in high-temperature conductive members face challenges with gradual oxidation of the base material, leading to decreased high-temperature conductivity due to insulating oxide films, despite the formation of heat-resistant conductive coating layers.

Method used

A ferritic stainless steel composition with controlled Ti and Nb solid solution amounts, combined with specific manufacturing processes including hot rolling, cold rolling, and final annealing, forms an oxide film with enhanced high-temperature oxidation resistance, conductivity, and strength.

Benefits of technology

The resulting oxide film exhibits excellent high-temperature oxidation resistance, conductivity, and strength, making the steel suitable for high-temperature conductive members.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007563919000004
    Figure 0007563919000004
  • Figure 0007563919000005
    Figure 0007563919000005
  • Figure 0007563919000001
    Figure 0007563919000001
Patent Text Reader

Abstract

To provide a ferritic stainless steel capable of forming an oxide film (passive film) excellent in high temperature oxidation resistance and high temperature conductivity on the surface and high in high temperature strength.SOLUTION: Ferritic stainless steel has a composition including C:0.030 mass% or less, Si:1.0 mass% or less, Mn:0.10-0.50 mass%, Ni:0.5 mass% or less, P:0.05 mass% or less, S:0.01 mass% or less, Cr:17.0- 23.0 mass%, Mo:0.8-1.5 mass%, Cu:0.5 mass% or less, Al:0.15 mass% or less, N:0.030 mass% or less, Ti:0.10-0.25 mass%, Nb:0.12-0.25 mass% and the remainder consisting of Fe and inevitable impurities. Both a Ti solid solution amount and a Nb solid solution amount are 0.10 mass% or more; and the Ti solid solution amount and a Mo content satisfy the following formula (1), 70Ti solid solution amount+31Mo content≥40 (1).SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a ferritic stainless steel and a method for producing the same. [Background technology]

[0002] Conductive members (hereinafter referred to as "high-temperature conductive members") used in high-temperature environments, such as electrode materials for high-temperature electronic devices and current collectors for fuel cells, are required to have excellent high-temperature oxidation resistance, high-temperature strength, and high-temperature conductivity.

[0003] As materials for high-temperature conductive members, metals such as tungsten and molybdenum, which have excellent resistance to high-temperature oxidation and high-temperature strength, can be used. However, these metals have a large difference in thermal expansion coefficient from ceramic parts (e.g., ceramic electrodes and substrates). Therefore, when the temperature of the usage environment changes, cracks may occur in the ceramic parts, and the ceramic parts may peel off from the high-temperature conductive members. Therefore, in practice, materials in which a heat-resistant conductive coating layer such as Ag-Co plating is formed on the surface of ferritic stainless steel, which has a small thermal expansion coefficient, to improve conductivity are used as high-temperature conductive members.

[0004] As a ferritic stainless steel usable in a high-temperature environment, for example, Patent Document 1 proposes a ferritic stainless steel containing 1.5 to 6 mass% Al. This ferritic stainless steel has good high-temperature oxidation resistance because an Al oxide film is formed on the surface in a high-temperature environment. Patent Document 2 proposes a ferritic stainless steel with a high Cr content and with one or more of Zr and REM (rare earth elements) added. This ferritic stainless steel has good high-temperature oxidation resistance because a dense Cr oxide film is formed on the surface in a high-temperature environment. Patent Document 3 proposes a ferritic stainless steel with a high Cr content and with Ti, Mo, and Nb added. This ferritic stainless steel has a composition with good high-temperature oxidation resistance and contains Ti and Mo, which are effective in improving high-temperature electrical conductivity. Patent Document 4 proposes a ferritic stainless steel with Al, Ti, and Nb added. This ferritic stainless steel has a mixture of Nb oxide, Ti oxide, and Al oxide between the Cr oxide layer and the base material, which forms locally conductive areas and ensures high-temperature oxidation resistance without impairing electrical conductivity. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] Patent No. 5780716 [Patent Document 2] JP 2010-13727 A [Patent Document 3] Japanese Patent Application Publication No. 6-279951 [Patent Document 4] Patent No. 5576146 Summary of the Invention [Problem to be solved by the invention]

[0006] As described above, the main requirements for ferritic stainless steel used in high-temperature conductive components are high-temperature oxidation resistance, high-temperature strength, and high-temperature electrical conductivity. Regarding these properties, high-temperature conductive components using ferritic stainless steel have a heat-resistant conductive coating layer formed on the surface of a base made of ferritic stainless steel to ensure high-temperature oxidation resistance and high-temperature electrical conductivity. However, even if a heat-resistant conductive coating layer is formed on the surface, oxidation of the ferritic stainless steel at the base gradually progresses. The oxide film of the ferritic stainless steel has a higher resistance than the heat-resistant conductive coating layer, which causes a decrease in the high-temperature conductivity of the high-temperature conductive member.

[0007] The ferritic stainless steel of Patent Document 1 is not suitable for use as a high-temperature conductive member because the Al oxide formed on the surface is insulating and has low high-temperature conductivity. The ferritic stainless steel of Patent Document 2 has low high-temperature conductivity of the Cr oxide film formed on the surface. The ferritic stainless steel of Patent Document 3 has low high-temperature conductivity of the oxide film formed on the surface because the amount of Ti and Nb in solid solution is not controlled. Furthermore, the ferritic stainless steel of Patent Document 4 has high high-temperature conductivity by forming an Al oxide layer containing Nb oxide and Ti oxide between the Cr oxide layer and the base material, but does not have high high-temperature conductivity of the Cr oxide layer itself, so it cannot be said that the high-temperature conductivity is sufficient.

[0008] The present invention has been made to solve the above-mentioned problems, and has an object to provide a ferritic stainless steel that is capable of forming an oxide film (passive film) on its surface that has excellent high-temperature oxidation resistance and high-temperature electrical conductivity, and that has high high-temperature strength, and a method for manufacturing the same. [Means for solving the problem]

[0009] As a result of extensive research, the present inventors have found that the above problems can be solved by controlling the composition, the amount of Ti in solid solution, and the amount of Nb in solid solution, and have thus completed the present invention. That is, the present invention is a ferritic stainless steel having a composition containing 0.030 mass% or less C, 1.0 mass% or less Si, 0.10 to 0.50 mass% Mn, 0.5 mass% or less Ni, 0.05 mass% or less P, 0.01 mass% or less S, 17.0 to 23.0 mass% Cr, 0.8 to 1.5 mass% Mo, 0.5 mass% or less Cu, 0.15 mass% or less Al, 0.030 mass% or less N, 0.10 to 0.25 mass% Ti, 0.12 to 0.25 mass% Nb, with the balance being Fe and unavoidable impurities, wherein the amount of solid solution Ti and the amount of solid solution Nb are both 0.10 mass% or more, and the amount of solid solution Ti and the amount of Mo satisfy the following formula (1): 70Ti solid solution amount (mass%) +31Mo content (mass%) ≧40 (1)

[0010] The present invention also provides a method for producing a semiconductor device comprising the steps of: The method for producing the ferritic stainless steel comprises the steps of: A slab containing C: 0.030 mass% or less, Si: 1.0 mass% or less, Mn: 0.10 to 0.50 mass%, Ni: 0.5 mass% or less, P: 0.05 mass% or less, S: 0.01 mass% or less, Cr: 17.0 to 23.0 mass%, Mo: 0.8 to 1.5 mass%, Cu: 0.5 mass% or less, Al: 0.15 mass% or less, N: 0.030 mass% or less, Ti: 0.10 to 0.25 mass%, Nb: 0.12 to 0.25 mass%, and the balance being Fe and unavoidable impurities, is hot-rolled, cold-rolled, and finish-annealed. stomach , The final annealing is performed by heating the steel sheet to 1000°C or higher and then annealing the steel sheet under the following conditions: (A) a cooling rate of less than 20°C / sec to 900°C; or (B) A cooling rate of 20°C / sec or more up to 900°C, and a cooling rate of 50°C / sec or more from 900 to 400°C This is a method for producing ferritic stainless steel, in which the steel is cooled at 300° C. Effect of the Invention

[0011] According to the present invention, it is possible to form an oxide film (passive film) having excellent high-temperature oxidation resistance and high-temperature electrical conductivity on the surface, and it is also possible to provide a ferritic stainless steel having high high-temperature strength and a method for producing the same. [Brief description of the drawings]

[0012] [Figure 1] 1 is a GDS profile of Example 1. [Diagram 2] FIG. 2 is a schematic top view of a test piece for measuring high temperature electrical conductivity. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0013] The following is a detailed description of the embodiments of the present invention. The present invention is not limited to the following embodiments, and it should be understood that modifications and improvements to the following embodiments, which are made based on the ordinary knowledge of those skilled in the art, fall within the scope of the present invention, without departing from the spirit of the present invention.

[0014] A ferritic stainless steel according to an embodiment of the present invention has a composition containing C: 0.030 mass% or less, Si: 1.0 mass% or less, Mn: 0.10 to 0.50 mass%, Ni: 0.5 mass% or less, P: 0.05 mass% or less, S: 0.01 mass% or less, Cr: 17.0 to 23.0 mass%, Mo: 0.8 to 1.5 mass%, Cu: 0.5 mass% or less, Al: 0.15 mass% or less, N: 0.030 mass% or less, Ti: 0.10 to 0.25 mass%, Nb: 0.12 to 0.25 mass%, with the balance being Fe and unavoidable impurities. In this specification, the term "unavoidable impurities" refers to components that are difficult to remove, such as O. Inevitable impurities are inevitably mixed in at the stage of melting raw materials.

[0015] Furthermore, the ferritic stainless steel according to the embodiment of the present invention may further contain at least one selected from V, W and Co in a total amount of 1.0 mass % or less, if necessary. Furthermore, the ferritic stainless steel according to the embodiment of the present invention may further contain, as necessary, 0.10 mass % or less in total of at least one selected from REM (rare earth elements) and Ca. Furthermore, the ferritic stainless steel according to the embodiment of the present invention may further contain B: 0.010 mass % or less, if necessary.

[0016] C is an element that affects the high-temperature oxidation resistance of ferritic stainless steel. If the C content is too high, abnormal oxidation is likely to occur, and the high-temperature oxidation resistance is reduced. Therefore, the C content is set to 0.030 mass% or less, more preferably 0.025 mass% or less, and even more preferably 0.020 mass% or less. On the other hand, the lower limit of the C content is not particularly limited, but the lower the C content, the longer the refining process will take, and the higher the manufacturing cost may be. Therefore, the C content is preferably set to 0.0005 mass% or more, and more preferably 0.0010 mass% or more.

[0017] Silicon is an element effective in improving the high-temperature oxidation resistance of ferritic stainless steel. However, if the silicon content is too high, the material may become hard and its toughness may decrease. Therefore, the silicon content is set to 1.0 mass% or less, preferably 0.9 mass% or less, more preferably 0.7 mass% or less, and further preferably 0.5 mass% or less. On the other hand, the lower limit of the silicon content is not particularly limited, but from the viewpoint of obtaining the above-mentioned effect of silicon, it is preferably set to 0.1 mass% or more, and more preferably 0.12 mass% or more.

[0018] Mn is an element effective in improving the high-temperature oxidation resistance of ferritic stainless steel. To obtain this effect, the Mn content is set to 0.10 mass% or more, preferably 0.12 mass% or more. On the other hand, if the Mn content is too high, properties such as workability may be degraded. Therefore, the Mn content is set to 0.50 mass% or less, preferably 0.40 mass% or less.

[0019] Ni is an element that improves the corrosion resistance of ferritic stainless steel and suppresses the deterioration of workability. However, since Ni is an austenite phase stabilizing element, if the Ni content is too high, a martensite phase is generated and the workability is deteriorated. Therefore, the Ni content is set to 0.5 mass% or less, preferably 0.4 mass% or less. On the other hand, the lower limit of the Ni content is not particularly limited, but from the viewpoint of obtaining the above-mentioned effect of Ni, it is preferably set to 0.01 mass% or more, more preferably 0.05 mass% or more.

[0020] P is an element that may reduce the high-temperature oxidation resistance and toughness of ferritic stainless steel. Therefore, the P content is set to 0.05 mass% or less, preferably 0.04 mass% or less. On the other hand, the lower limit of the P content is not particularly limited, but the lower the P content, the longer the refining process will take, and the higher the manufacturing cost may be. Therefore, the P content is preferably set to 0.001 mass% or more, more preferably 0.010 mass% or more.

[0021] S is an element that may generate sulfide-based inclusions and deteriorate the surface properties of ferritic stainless steel. Therefore, the S content is set to 0.01 mass% or less, preferably 0.008 mass% or less. On the other hand, the lower limit of the S content is not particularly limited, but the lower the S content, the longer the refining process will take, and the higher the manufacturing cost may be. Therefore, the S content is preferably set to 0.0001 mass% or more, more preferably 0.0005 mass% or more.

[0022] Cr is a major element for forming a passive film on the surface of ferritic stainless steel, and the passive film can improve properties such as high-temperature oxidation resistance, corrosion resistance, and heat resistance. In particular, from the viewpoint of forming a passive film with excellent high-temperature oxidation resistance, the Cr content is set to 17.0 mass% or more, preferably 17.5 mass% or more. On the other hand, if the Cr content is too high, properties such as toughness decrease, so the Cr content is set to 23.0 mass% or less, preferably 22.5 mass% or less.

[0023] Mo is an element effective in improving the high-temperature oxidation resistance of ferritic stainless steel. Mo is also an element that improves the high-temperature electrical conductivity of the passive film formed on the surface of ferritic stainless steel. Usually, the passive film is a dense Cr oxide and has low high-temperature electrical conductivity, but by making Mo exist as an oxide in the passive film, the high-temperature electrical conductivity of the passive film can be improved. In order to obtain these effects, the Mo content is 0.8 mass% or more, preferably 0.9 mass% or more. On the other hand, if the Mo content is too high, it becomes difficult to form a uniform passive film. Therefore, the Mo content is 1.5 mass% or less, preferably 1.4 mass% or less, more preferably 1.3 mass% or less, and even more preferably 1.2 mass% or less.

[0024] Cu is an element that improves the corrosion resistance, especially the pitting corrosion resistance, of ferritic stainless steel. However, if the Cu content is too high, the ferrite phase becomes unstable and the cost increases. Therefore, the Cu content is set to 0.5 mass% or less, preferably 0.3 mass% or less. On the other hand, the lower limit of the Cu content is not particularly limited, but from the viewpoint of obtaining the above-mentioned effects of Cu, it is preferably set to 0.01 mass% or more, more preferably 0.03 mass% or more.

[0025] Al is an element effective in improving the high-temperature oxidation resistance of ferritic stainless steel. However, if the Al content is too high, the high-temperature electrical conductivity of the passive film formed on the surface of the ferritic stainless steel may decrease. Therefore, the Al content is set to 0.15 mass% or less, preferably 0.13 mass% or less. On the other hand, the lower limit of the Al content is not particularly limited, but from the viewpoint of obtaining the above-mentioned effect of Al, it is preferably set to 0.01 mass% or more, more preferably 0.02 mass% or more.

[0026] N is an element that may combine with Al to generate AlN, which is the starting point of abnormal oxidation, and may reduce the toughness of the ferritic stainless steel sheet. Therefore, the N content is set to 0.030 mass% or less, preferably 0.025 mass% or less. On the other hand, the lower limit of the N content is not particularly limited, but the lower the N content, the longer the refining process will take, and the higher the manufacturing cost may be. Therefore, the N content is preferably set to 0.001 mass% or more, more preferably 0.010 mass% or more.

[0027] Like Mo, Ti is an element that improves the high-temperature electrical conductivity of a passive film formed on the surface of a ferritic stainless steel by being present as an oxide in the passive film. Ti also preferentially bonds with C and N to form Ti carbonitrides, and is therefore an element that suppresses the deterioration of corrosion resistance due to the formation of Cr carbonitrides. In order to allow Ti to exist sufficiently as an oxide in the passive film, it is necessary to increase the amount of solute Ti that is not consumed in the formation of Ti carbonitrides. Therefore, the Ti content is set to 0.10% by mass or more, preferably 0.11% by mass or more. On the other hand, if the Ti content is too high, the Ti carbonitrides will become coarse and the high-temperature strength will decrease. Therefore, the Ti content is set to 0.25% by mass or less, preferably 0.24% by mass or less.

[0028] Nb is an element effective in improving the high-temperature strength of ferritic stainless steel. In addition, like Ti, Nb preferentially bonds with C and N to form Nb carbonitrides, and is therefore also an element that suppresses the deterioration of corrosion resistance due to the formation of Cr carbonitrides. From the viewpoint of obtaining these effects, the Nb content is set to 0.12 mass% or more, preferably 0.14 mass% or more. On the other hand, if the Nb content is too high, the amount of solid-solubilized Nb that is not consumed in the formation of Nb carbonitrides increases. As a result, the oxidation of Ti is hindered, and it becomes difficult for Ti to exist as an oxide in the passive film. Therefore, the Nb content is set to 0.25 mass% or less, preferably 0.24 mass% or less.

[0029] V, W, and Co are elements that improve high-temperature strength without impairing the toughness of ferritic stainless steel. However, if the content of these elements is too high, there is a risk of reducing workability and toughness, and the cost increases. Therefore, the total content of at least one selected from V, W, and Co is preferably 1.0 mass% or less, more preferably 0.8 mass% or less. On the other hand, the lower limit of the total content of these elements is not particularly limited, but from the viewpoint of obtaining the effects of these elements, it is preferably 0.01 mass% or more, more preferably 0.05 mass% or more.

[0030] REM (rare earth elements) and Ca preferentially bond with S and P to form compounds, and therefore can suppress the deterioration of properties (for example, deterioration of toughness and surface properties) caused by S and P. However, if the content of these elements is too high, the ferritic stainless steel may become hard and the workability may decrease. Therefore, the total content of at least one selected from REM (rare earth elements) and Ca is preferably 0.10 mass% or less, more preferably 0.08 mass% or less. On the other hand, the lower limit of the total content of these elements is not particularly limited, but from the viewpoint of obtaining the effects of these elements, it is preferably 0.01 mass% or more, more preferably 0.02 mass% or more.

[0031] B is an element that is effective in improving secondary workability by preferentially precipitating at grain boundaries. However, if the B content is excessive, the boride (precipitates) at the grain boundaries become coarse, thereby reducing fatigue strength. Therefore, the B content is preferably 0.010 mass% or less, and more preferably 0.008 mass% or less. On the other hand, the lower limit of the B content is not particularly limited, but from the viewpoint of obtaining the effects of B, it is preferably 0.0005 mass% or more, and more preferably 0.001 mass% or more.

[0032] In the ferritic stainless steel according to the embodiment of the present invention, both the amount of Ti in solid solution and the amount of Nb in solid solution are 0.10% by mass or more. By making the amount of Ti in solid solution 0.10% by mass or more, it is possible to make Ti exist as an oxide in a sufficient amount in the passive film formed on the surface of the ferritic stainless steel, and therefore the high-temperature electrical conductivity of the passive film is improved. In addition, by making the amount of Nb in solid solution 0.10% by mass or more, the high-temperature strength is also improved. The upper limits of the amount of Ti and Nb in solid solution are not particularly limited, but are preferably 0.30 mass % or less, and more preferably 0.25 mass % or less.

[0033] In the ferritic stainless steel according to the embodiment of the present invention, the amount of dissolved Ti and the amount of Mo satisfy the following formula (1). 70Ti solid solution amount+31Mo content≧40 (1) By satisfying the condition of the above formula (1), it is possible to allow sufficient amounts of Ti and Mo to be present as oxides in the passive film formed on the surface of the ferritic stainless steel, thereby improving the high-temperature electrical conductivity of the passive film.

[0034] The ferritic stainless steel having the above-mentioned composition, Ti solid solution amount, and Nb solid solution amount can be produced by hot rolling a slab having the above-mentioned composition, followed by cold rolling and finish annealing. At this time, by controlling the finish annealing conditions, the type of inclusions (carbides) that precipitate can be controlled, and the Ti solid solution amount and Nb solid solution amount can be adjusted to the desired amount.

[0035] Finish annealing is performed by heating to 1000°C or higher and then cooling. By setting the heating temperature to 1000°C or higher, the solid solution of TiC can be promoted, so that the amount of Ti and the amount of Nb in the solid solution can be adjusted in the subsequent cooling process. The upper limit of the heating temperature is not particularly limited, but is preferably 1100°C or lower.

[0036] In the cooling process, at about 900°C, the solute C and Nb combine to precipitate NbC, and at about 800°C, the solute C that was not able to combine with Nb combines with Ti to precipitate TiC. Therefore, in order to suppress the decrease in the amount of solute Ti due to the precipitation of TiC, the cooling process is performed under the following conditions: (A) a cooling rate of less than 20°C / sec to 900°C; or (B) A cooling rate of 20°C / sec or more up to 900°C, and a cooling rate of 50°C / sec or more from 900 to 400°C It is held.

[0037] Condition (A) is achieved by slowing down the cooling rate to 900°C, which ensures sufficient time for Nb to combine with solute C and precipitate NbC, thereby increasing the amount of NbC precipitated. As a result, the amount of solute C that cannot be combined with Nb can be reduced, making it possible to suppress the decrease in the amount of solute Ti due to the precipitation of TiC. On the other hand, in the condition (B), the cooling rate to 900°C is fast, so the time for NbC precipitation is not sufficiently secured, and TiC is likely to precipitate at about 800°C. Therefore, when the cooling rate to 900°C is increased, the cooling rate at temperatures below 900°C is further increased to 50°C / sec or more. This makes it possible to reduce the precipitation of TiC at about 800°C. In addition, at around 600°C, Cr 23 C 6 Since this precipitates, the cooling rate must be 50°C / sec or faster up to 400°C.

[0038] In the above manufacturing method, the conditions other than the final annealing are not particularly limited. Hot rolling and cold rolling can be performed according to a method known in the art. After hot rolling, known processes such as annealing and pickling may be performed. Also, after the final annealing, known processes such as pickling may be performed.

[0039] The ferritic stainless steel produced as described above has a passive film formed on its surface in an oxygen-containing atmosphere (e.g., air atmosphere). This passive film has excellent high-temperature oxidation resistance and high-temperature electrical conductivity, and the ferritic stainless steel also has high high-temperature strength. Therefore, this ferritic stainless steel is suitable for use in high-temperature electrical conductive members.

[0040] A high temperature conductive member according to an embodiment of the present invention includes a base and a heat-resistant conductive coating layer formed on a surface of the base. The base is formed from the above-mentioned ferritic stainless steel. The ferritic stainless steel may be modified (roughened) to improve adhesion to the heat-resistant conductive coating layer. For example, the modification (roughening) of the passive film can be performed by a known method such as immersing the ferritic stainless steel in a hydrofluoric / nitric acid solution.

[0041] The heat-resistant conductive coating layer is not particularly limited and can be formed from a material known in the art. For example, the heat-resistant conductive coating layer can be formed using a metal with excellent conductivity, such as Ag or Co. The heat-resistant conductive coating layer can be a single metal layer or an alloy layer, and can have a single-layer structure or a multilayer structure.

[0042] The high-temperature electrical conductor according to the embodiment of the present invention has a base portion formed from the above-mentioned ferritic stainless steel, and therefore has excellent high-temperature oxidation resistance, high-temperature electrical conductivity, and high-temperature strength. EXAMPLES

[0043] The present invention will be described in detail below with reference to examples, but the present invention should not be construed as being limited to these.

[0044] A slab having the composition shown in Table 1 was melted and hot rolled to a hot rolled sheet having a thickness of 3.0 mm, which was then annealed at 1,050°C and pickled to obtain a hot rolled annealed sheet. The hot rolled annealed sheet was then cold rolled to a cold rolled sheet having a thickness of 1.0 mm, which was then finish annealed and pickled under the conditions shown in Table 2 to obtain a ferritic stainless steel sheet.

[0045] [Table 1]

[0046] Next, the amounts of Ti and Nb in solid solution were measured for the obtained ferritic stainless steel sheets. The measurements were performed as follows. First, a square test piece with a side length of 20 mm was cut out from a ferritic stainless steel plate by cutting, and the entire surface was wet-polished with a #600 abrasive, after which electrolytic etching was performed by the SPEED method. In the SPEED method, a 10 mass% acetylacetone solution was used, and electrolysis was performed at a constant potential of 400 mV until the potential reached 5 kCoulombs, and the solution after electrolysis was filtered through a filter with a lattice diameter of 0.05 μm to collect inclusions. The amount of dissolved inclusions and the amount of collected inclusions were then determined by mass measurement. Next, the collected inclusions were analyzed by an X-ray diffractometer (XRD). The sums of the peak intensities of Ti-based and Nb-based carbonitrides (hereinafter referred to as Ti carbonitride peak intensity and Nb carbonitride peak intensity) were calculated from the profiles obtained by XRD. The positions of the peaks (diffraction angle 2θ) used in the calculations are as follows: Ti-based: TiC: 48.838°, TiN: 49.895° Nb series: NbC: 40.557°, NbN: 41.307°, CrNbN: 42.919°

[0047] Next, the amount of Ti (amount of consumed Ti) and the amount of Nb (amount of consumed Nb) used in the formation of carbonitrides were calculated by the following formulas. Amount of Ti consumed (mass%) = (0.8 × amount of inclusions collected (g) × Ti carbonitride peak intensity / (Ti carbonitride peak intensity + Nb carbonitride peak intensity)) / amount dissolved (g) Amount of Nb consumed (mass%) = (0.8 × amount of inclusions collected (g) × Nb carbonitride peak intensity / (Ti carbonitride peak intensity + Nb carbonitride peak intensity)) / amount dissolved (g) Next, the amount of Ti solid solution (mass%) was calculated by subtracting the amount of Ti consumed (mass%) from the Ti content (mass%). Similarly, the amount of Nb solid solution (mass%) was calculated by subtracting the amount of Nb consumed (mass%) from the Nb content (mass%). The calculated amounts of Ti solid solution and Nb solid solution are shown in Table 2.

[0048] [Table 2]

[0049] Next, the ferritic stainless steel sheet obtained above was immersed in an aqueous solution (liquid temperature 60°C) containing 5.0 mass% hydrofluoric acid and 15 mass% nitric acid for 1 to 5 minutes to modify the surface, and then a coating process was performed to form a heat-resistant conductive coating layer. In the coating process, Co plating was adjusted to 2 to 5 μm on the surface of the surface-modified ferritic stainless steel sheet.

[0050] The ferritic stainless steel sheets having the heat-resistant conductive coating layer were evaluated for high-temperature oxidation resistance and high-temperature electrical conductivity. The ferritic stainless steel sheets having no heat-resistant conductive coating layer were also evaluated for high-temperature strength. The evaluation methods are as follows. (1) High temperature oxidation resistance The above ferritic stainless steel sheet having a heat-resistant conductive coating layer formed thereon was thermally exposed to 700°C in an air atmosphere for 500 hours, after which a GDS (glow discharge optical emission spectroscopy) analysis was performed to analyze the structure of the oxide film on the ferritic stainless steel sheet. In the GDS analysis, the point where the Co peak intensity was half of the maximum value was defined as the surface layer of the oxide film, and the thickness of the oxide film was defined as the point where the O (oxygen) peak intensity was half of this point. As an example, the GDS profile of Example 1 is shown in Figure 1. In the GDS analysis, an oxide film thickness of 10 μm or less was judged as A (excellent resistance to high-temperature oxidation), an oxide film thickness of more than 10 μm but less than 20 μm was judged as B (good resistance to high-temperature oxidation), and an oxide film thickness of more than 20 μm was judged as C (inadequate resistance to high-temperature oxidation).

[0051] (2) High temperature conductivity Two of the above ferritic stainless steel sheets with a heat-resistant conductive coating layer formed thereon (hereinafter referred to as "ferritic stainless steel sheets with a heat-resistant conductive coating layer") were thermally exposed in the air at 700°C for 500 hours, and then these two ferritic stainless steel sheets with a heat-resistant conductive coating layer were used to prepare a test piece for measurement as shown in Figure 2, and measurements were performed by the four-terminal method using a potentiostat. Specifically, the measurements were performed as follows. First, a conductive paste (Ag paste) was applied in a square shape (10 mm on one side, 10 μm thick) to the center of two ferritic stainless steel plates 10 with a heat-resistant conductive coating layer, and dried to form a conductive part 20. Next, the conductive parts 20 of the two ferritic stainless steel plates 10 with a heat-resistant conductive coating layer were stacked and arranged in a cross shape, then sandwiched between alumina plates, a weight (200 g) was placed on top, and the conductive part 20 was baked in an electric furnace (850 ° C × 2 hours). Next, the surface was scraped using a minitor until the metal base material was exposed, and the wiring attachment part 30 shown in FIG. 2 was formed. Next, a silver wire 40 (φ 0.3 mm) was wound around the wiring attachment part 30, a conductive paste was applied, and the test piece was obtained by drying at 150 ° C for 30 minutes. Next, this test piece was placed in a high-temperature electrochemical measurement device, and a voltage-current curve was obtained by a four-terminal method using a potentiostat. In this measurement, the measurement temperature was set to 700°C, and the voltage was swept up to 10 mV. The resistance value was calculated from the slope of the voltage-current curve. In this evaluation, the resistance value was 20 mΩ cm 2 If the resistance is less than 20mΩ cm, it is classified as A (excellent high temperature conductivity). 2 When the value was exceeded, it was judged as C (insufficient high temperature conductivity).

[0052] (3) High temperature strength JIS No. 13B test pieces were cut out by cutting from the ferritic stainless steel plate obtained above (without the heat-resistant conductive coating layer). The test pieces were tensile in the rolling direction. Next, a high-temperature tensile test was performed at 700°C using a tensile tester. In this evaluation, a tensile strength of 50 MPa or more was judged to be A (high high-temperature strength), and a tensile strength of less than 50 MPa was judged to be C (low high-temperature strength). The results of each of the above evaluations are shown in Table 3.

[0053] [Table 3]

[0054] As shown in Table 3, the ferritic stainless steel sheets of Examples 1 to 6 had composition, Ti solid solution amount, and Nb solid solution amount controlled within appropriate ranges, and therefore showed good results in high-temperature oxidation resistance, high-temperature electrical conductivity, and high-temperature strength. In contrast, the ferritic stainless steel sheet of Comparative Example 1 had an inappropriate cooling rate in the finish annealing, resulting in a small amount of Ti in solid solution and insufficient high-temperature electrical conductivity. The ferritic stainless steel sheet of Comparative Example 2 had an excessively low Nb content, and therefore had a small amount of Nb in solid solution, resulting in insufficient high-temperature strength. The ferritic stainless steel sheet of Comparative Example 3 had too little Ti content and too much Nb content, so the amount of dissolved Ti was small, did not satisfy formula (1), and had insufficient high-temperature electrical conductivity. The ferritic stainless steel sheet of Comparative Example 4 had too much Ti and too little Nb, and the heating temperature in the finish annealing was too low, so that the amount of Nb in solid solution was small and the high-temperature strength was insufficient.

[0055] The ferritic stainless steel sheet of Comparative Example 5 had too high Ni, Cr and Ti contents and too low Mo content, and therefore did not satisfy formula (1) and had insufficient high-temperature electrical conductivity. In the ferritic stainless steel sheet of Comparative Example 6, the cooling rate in the finish annealing was inappropriate, so that the amount of Ti in solid solution was small and the high-temperature electrical conductivity was insufficient. The ferritic stainless steel sheet of Comparative Example 7 had too little Mo and Nb content and too much Ti content, and the heating temperature in the finish annealing was too low, so that the amount of Nb in solid solution was small and formula (1) was not satisfied, and the high-temperature oxidation resistance, high-temperature electrical conductivity, and high-temperature strength were all insufficient. The ferritic stainless steel sheet of Comparative Example 8 had too little Nb content and too much Ti content, and the heating temperature in the finish annealing was too low, so that the amount of Nb in solid solution was small and the high-temperature strength was insufficient. The ferritic stainless steel sheet of Comparative Example 9 had too much Cr content and too little Mo, Ti and Nb contents, and the heating temperature in the finish annealing was too low, so it did not satisfy formula (1) and had insufficient high-temperature electrical conductivity.

[0056] As can be seen from the above results, according to the present invention, it is possible to form an oxide film (passive film) having excellent high-temperature oxidation resistance and high-temperature electrical conductivity on the surface, and it is also possible to provide a ferritic stainless steel having high high-temperature strength and a method for manufacturing the same. [Explanation of symbols]

[0057] 10. Ferritic stainless steel sheet with heat-resistant conductive coating layer 20 Conductive part 30 Wiring attachment part 40 silver wire

Claims

1. % or less, the balance consisting of Fe and unavoidable impurities, wherein the amount of dissolved Ti and the amount of dissolved Nb are both 0.10% or more by mass, and the amount of dissolved Ti and the amount of dissolved Nb satisfy the following formula (1): 70Ti solid solution amount (mass%) + 31Mo content (mass%) ≧ 40 (1)

2. The ferritic stainless steel according to claim 1, further comprising at least one selected from the group consisting of V, W and Co in a total amount of 1.0 mass% or less.

3. The ferritic stainless steel according to claim 1 or 2, further containing 0.10 mass% or less in total of at least one selected from REM and Ca.

4. The ferritic stainless steel according to any one of claims 1 to 3, further containing B: 0.010 mass% or less.

5. A method for producing the ferritic stainless steel according to claim 1, comprising the steps of: A slab containing C: 0.030 mass% or less, Si: 1.0 mass% or less, Mn: 0.10 to 0.50 mass%, Ni: 0.5 mass% or less, P: 0.05 mass% or less, S: 0.01 mass% or less, Cr: 17.0 to 23.0 mass%, Mo: 0.8 to 1.5 mass%, Cu: 0.5 mass% or less, Al: 0.15 mass% or less, N: 0.030 mass% or less, Ti: 0.10 to 0.25 mass%, Nb: 0.12 to 0.25 mass%, with the balance being Fe and unavoidable impurities, is hot-rolled, then cold-rolled and finish-annealed; The final annealing is performed by heating the steel sheet to 1000° C. or higher and then annealing the steel sheet under the following conditions: (A) a cooling rate of less than 20° C. / sec to 900° C.; or (B) A cooling rate of 20°C / sec or more down to 900°C, and a cooling rate of 50°C / sec or more from 900 to 400°C This is a method for producing ferritic stainless steel by cooling at 400K.

6. A method for producing the ferritic stainless steel according to claim 2, comprising the steps of: The method for producing a ferritic stainless steel according to claim 5, wherein the slab further contains at least one selected from the group consisting of V, W and Co in a total amount of 1.0 mass% or less.

7. A method for producing the ferritic stainless steel according to claim 3, comprising the steps of: The method for producing a ferritic stainless steel according to claim 5 or 6, wherein the slab further contains 0.10 mass% or less in total of at least one selected from REM and Ca.

8. A method for producing the ferritic stainless steel according to claim 4, comprising the steps of: The method for producing a ferritic stainless steel according to any one of claims 5 to 7, wherein the slab further contains B: 0.010 mass% or less.

Citation Information

Patent Citations

  • Hand knitting machine

    JP1980076146A

  • Manufacture of semiconductor crystal

    JP1982080716A

  • Ferritic stainless steel for water heater

    JP1994279951A

  • Ferritic stainless steel for fuel battery separator, and production method therefor

    JP2004232074A

  • Ferritic-austenitic stainless steel with excellent corrosion resistance and workability, and its manufacturing method

    JP2009035782A