Method for removing oxide scale and method for manufacturing stainless steel material
The use of a pulsed laser beam with controlled fluence and pulse width during oxide scale removal on stainless steel materials addresses uneven heat input issues, ensuring efficient and flawless surface treatment.
Patent Information
- Application Number
- JP2021005995
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2021-01-18
- Publication Date
- 2024-10-08
- Estimated Expiration
- 2041-01-18
AI Technical Summary
Existing methods for removing oxide scale from stainless steel materials using laser beams result in excessive unevenness and surface flaws due to uneven heat input during reciprocating scanning, leading to reduced production efficiency and corrosion resistance.
Using a pulsed laser beam with controlled fluence and pulse width, the method involves irradiating the stainless steel material in one direction while scanning back and forth, and moving it perpendicularly, with adjusted fluence at the folded portion and its vicinity to match the main scanning part, and optionally followed by pickling.
This approach suppresses the formation of excessive unevenness, maintains high production efficiency, and ensures a good appearance of the stainless steel material by effectively removing oxide scale without surface flaws.
Smart Images

Figure 0007563997000001 
Figure 0007563997000002 
Figure 0007563997000003
Abstract
Description
[Technical Field]
[0001] The present invention relates to a method for removing oxide scale and a method for manufacturing a stainless steel material. [Background technology]
[0002] Stainless steel materials have various excellent properties such as corrosion resistance, and are therefore used in a wide range of applications such as automobile parts, building parts, and kitchen utensils. Oxide scale may form on the surface of stainless steel materials during their manufacturing process, and therefore, the oxide scale is removed by pickling. For example, a typical stainless steel sheet is manufactured by the following process: molten steel, which is made by melting stainless steel raw materials, is continuously cast into a slab, and the slab is hot-rolled to obtain a hot-rolled sheet (thick plate material). Furthermore, a cold-rolled sheet (thin plate material) is obtained by cold-rolling the hot-rolled sheet. The hot-rolled sheet and the cold-rolled sheet are wound into a coil as needed. Furthermore, the hot-rolled sheet and the cold-rolled sheet are annealed as needed. In the manufacture of such stainless steel sheets, oxide scale forms on the hot-rolled sheet after hot rolling and the cold-rolled sheet after cold rolling, and therefore, the oxide scale is removed by pickling. In this specification, the term "stainless steel sheet" is a concept that includes both hot-rolled sheets and cold-rolled sheets. In addition, hereinafter, the removal of oxide scale formed on the surface of a stainless steel material may be referred to as "descaling."
[0003] However, pickling may not be able to sufficiently remove oxide scale. Therefore, the pickling time is prolonged or mechanical pretreatment such as using a scale breaker or shot blasting to crack the oxide scale before pickling. As a result, removing the oxide scale takes too long, which is a factor in reducing the production efficiency of stainless steel materials.
[0004] Therefore, various methods have been researched and implemented to efficiently remove oxide scale from the surface of stainless steel materials. For example, Patent Document 1 proposes a method of removing a scale layer formed when a stainless steel plate is annealed by irradiating the scale layer with a laser beam. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] Japanese Patent Application Publication No. 4-182020 Summary of the Invention [Problem to be solved by the invention]
[0006] When a method for removing oxide scale using a laser beam is actually applied to a manufacturing method for stainless steel materials, the laser beam must be irradiated while scanning back and forth across the stainless steel material by turning back the laser head halfway across the width of the stainless steel material, while the stainless steel material is moved in the length direction of the stainless steel material. In this case, in the width direction of the stainless steel material, there are turning-back portions and their vicinity where the laser beams of the forward scanning and the backward scanning overlap, and steady main scanning portions where the laser beams do not overlap. Therefore, with the back-and-forth scanning of the laser beam, the amount of heat input to the turning-back portions and their vicinity is greater than that of the main scanning portions, and the stainless steel material is likely to melt at the turning-back portions and their vicinity, resulting in the formation of excessively irregular portions. These excessively irregular portions can cause surface defects. For example, if oxide scale is removed using laser light after hot rolling and then cold rolling or other processes are performed in a subsequent step, excessively uneven portions will be crushed during the cold rolling, forming surface defects, which will significantly degrade the appearance of the stainless steel material, and rolling oil and the like may enter and remain in the excessively uneven portions, which may reduce corrosion resistance.
[0007] The present invention has been made to solve the above-mentioned problems, and aims to provide a method for removing oxide scale that can suppress the formation of excessively uneven portions due to an increase in the amount of heat input at and near the turning points during the reciprocating scanning of laser light. Another object of the present invention is to provide a method for producing a stainless steel material with high production efficiency and good appearance. [Means for solving the problem]
[0008] As a result of extensive research, the inventors have found that the above-described problems can be solved by using pulsed laser light as the laser light and controlling the fluence of the pulsed laser light at and near the turning points of the reciprocating scan to be smaller than the fluence of the pulsed laser light in the main scanning portion of the reciprocating scan, and have thus completed the present invention.
[0009] That is, the present invention provides: After hot rolling or cold rolling 1. A method for removing oxide scale formed on a surface of a stainless steel material by irradiating the surface with pulsed laser light, comprising: an irradiation step of irradiating the stainless steel material with the pulsed laser light while scanning it back and forth in an X direction and moving the stainless steel material in a Y direction perpendicular to the X direction; a pickling treatment step in which pickling treatment is performed after the irradiation step; Including, the pulse width of the pulsed laser light is 10 to 1000 ns; The fluence of the pulsed laser light at the return portion of the reciprocating scan and its vicinity is set to be smaller than the fluence of the pulsed laser light in the main scanning portion of the reciprocating scan. death , the irradiation step includes a first irradiation step of irradiating a portion A of the surface of the stainless steel material with the pulsed laser light, and a second irradiation step of irradiating a portion B of the surface of the stainless steel material with the pulsed laser light after the first irradiation step, an overlap of the irradiation areas of the pulsed laser light between the portion A and the portion B in the X direction is 1 to 50% of the scanning width in the X direction of each of the portion A and the portion B; This is a method for removing oxide scale.
[0010] The present invention also provides a method for producing a stainless steel material, which method includes the above-described method for removing oxide scale. [Effects of the Invention]
[0011] According to the present invention, it is possible to provide a method for removing oxide scale that can suppress the formation of excessively large irregularities due to an increase in the amount of heat input at and near the turning points during reciprocating scanning of laser light. Furthermore, the present invention can provide a method for producing a stainless steel material with high production efficiency and good appearance. [Brief explanation of the drawings]
[0012] [Figure 1] FIG. 1 is a flow chart showing an example of a method for manufacturing a stainless steel sheet. [Figure 2] FIG. 1 is a schematic diagram of a laser light irradiation device used for descaling by irradiating pulsed laser light. [Figure 3] 1 is a schematic diagram showing the trajectory of the center of a pulsed laser beam that scans back and forth across the surface of a stainless steel plate. FIG. [Figure 4] 1 is an optical microscope photograph of the surface of a stainless steel plate on which surface defects have been formed. [Figure 5] 1 is a schematic diagram showing the trajectory of the center of a pulsed laser beam that scans back and forth across the surface of a stainless steel plate. FIG. [Figure 6] FIG. 1 is a diagram showing optical microscope photographs and cross-sectional curve results in an example. DETAILED DESCRIPTION OF THE INVENTION
[0013] The following is a detailed description of the embodiments of the present invention. The present invention is not limited to the following embodiments, and it should be understood that modifications and improvements made to the following embodiments based on the ordinary knowledge of those skilled in the art without departing from the spirit of the present invention are also within the scope of the present invention. In this specification, the "%" designation for components means "% by mass" unless otherwise specified.
[0014] The method for removing oxide scale according to an embodiment of the present invention is carried out by irradiating the surface of a stainless steel material with pulsed laser light to remove the oxide scale formed thereon. Also, the method for manufacturing a stainless steel material according to an embodiment of the present invention includes this method for removing oxide scale. The stainless steel material is not particularly limited, but is preferably a stainless steel sheet. In this specification, the term "steel sheet" includes a steel strip. The stainless steel sheet may be a hot-rolled sheet after hot rolling or a cold-rolled sheet after cold rolling, or an annealed sheet after annealing these. Here, a method for manufacturing a stainless steel plate will be taken as an example of a method for manufacturing a stainless steel material and explained using the flow diagram in FIG.
[0015] (Method of manufacturing stainless steel sheets) Fig. 1 shows an example of a manufacturing method for a hot-rolled annealed stainless steel sheet. As shown in Fig. 1, this manufacturing method includes a steelmaking step (S1), a continuous casting step (S2), a hot rolling step (S3), a continuous annealing step (S4), and an oxide scale removal step (S5). The type of stainless steel used to make the stainless steel sheet is not particularly limited, and various stainless steels can be used as the material, including, for example, pickling-resistant steel containing 2.5 to 5.0% Si, 18 to 20% Cr, and 12 to 20% Ni, and general-purpose steels such as SUS304, SUS430, and SUS316.
[0016] First, in the steelmaking process (S1), scrap containing Fe, Cr, Ni, etc. as its main components is melted in an electric furnace, and then the components are adjusted in a refining furnace to produce molten steel. Next, in the continuous casting process (S2), the molten steel produced in the refining furnace is poured into a ladle, and then continuously poured from the ladle into a mold where it is cooled. The cooled and solidified stainless steel is then cut into specified lengths to produce multiple slabs.
[0017] Next, in the hot rolling step (S3), the slab produced in the continuous casting step (S2) is heated to a predetermined temperature, and the slab that has reached the predetermined temperature is hot rolled in a hot rolling mill. Specifically, the slab is subjected to multiple stages of rough rolling and finish rolling to hot roll the slab until it reaches a predetermined thickness, thereby producing a hot-rolled sheet.
[0018] Next, in the continuous annealing step (S4), the hot-rolled sheet produced in the hot rolling step (S3) is continuously annealed in an annealing furnace to produce a hot-rolled annealed sheet. By continuously annealing the hot-rolled sheet, the hot-rolled sheet, which has hardened and lost its ductility, is softened and the ductility of the hot-rolled sheet is restored. Next, in the oxide scale removal step (S5), the oxide scale formed on the surface of the hot-rolled annealed steel sheet is descaled by irradiating it with a pulsed laser beam (hereinafter referred to as "laser descaling"). This laser descaling is a technique that utilizes laser ablation. Laser ablation can vaporize the irradiated material by irradiating it with laser beam. Furthermore, in the oxide scale removal step (S5), after laser descaling, descaling by pickling may be performed as needed.
[0019] The above manufacturing method is merely an example, and is not limited to the above-described content and order of each step, the equipment used, etc. Furthermore, when the stainless steel sheet is a cold-rolled annealed sheet, a cold rolling step and a continuous annealing step may be performed between the continuous annealing step (S4) and the oxide scale removing step (S5), or the cold rolling step and the continuous annealing step may be performed in this order after the oxide scale removing step (S5), and then the oxide scale removing step (S5) may be performed again.
[0020] Next, the oxide scale removing step (S5) will be described in detail. Laser descaling includes an irradiation step in which a pulsed laser beam is irradiated while scanning back and forth in the X direction, while the stainless steel sheet is moved in the Y direction perpendicular to the X direction. This irradiation step can be performed using a laser beam irradiation device 10 as shown in FIG. 2. The laser beam irradiation device 10 includes a laser oscillator 11, a laser head 12, a drive unit (not shown), and a control unit (not shown). In this laser beam irradiation device 10, a pulsed laser beam 13 generated by the laser oscillator 11 is irradiated from the laser head 12 while scanning back and forth in the X direction (the width direction of the stainless steel sheet 1 in FIG. 2), while the stainless steel sheet 1 is moved in the Y direction perpendicular to the X direction (the conveying direction of the stainless steel sheet 1 in FIG. 2). This irradiation step allows the pulsed laser beam 13 to be continuously irradiated onto the oxide scale, thereby efficiently vaporizing the oxide scale.
[0021] There are no particular limitations on the type of laser oscillator 11 as long as it is capable of oscillating pulsed laser light. From the viewpoint of shortening the descaling time, it is preferable that the laser oscillator 11 be a solid-state laser with a large laser output per unit area. The laser head 12 focuses the pulsed laser light 13 oscillated from the laser oscillator 11 and irradiates the oxide scale formed on the surface of the stainless steel plate 1 with the light.
[0022] The drive unit is connected to the laser head 12 and drives the laser head 12 to move the irradiation position of the pulsed laser beam 13. The control unit is connected to the laser oscillator 11 and the laser head 12 and controls the irradiation conditions of the pulsed laser beam 13. Examples of the irradiation conditions of the pulsed laser beam 13 include the fluence, pulse width, oscillation period, laser output, irradiation speed, irradiation width, and beam diameter.
[0023] The oscillation period of the pulsed laser beam 13 is not particularly limited, but is preferably 60 to 120 kHz. By controlling the oscillation period of the pulsed laser beam 13 within this range, it is possible to irradiate the oxide scale formed on the surface of the stainless steel sheet 1 with the pulsed laser beam 13 at an optimized fluence. If the oscillation period of the pulsed laser beam 13 is less than 60 kHz, the number of times the stainless steel sheet 1 is irradiated per unit time will be too small. As a result, it may be impossible to irradiate the stainless steel sheet 1 with the pulsed laser beam 13 having a fluence sufficient for descaling. Furthermore, if the oscillation period of the pulsed laser beam 13 is greater than 120 kHz, the fluence per pulse of the pulsed laser beam 13 will be small. As a result, it may be impossible to irradiate the stainless steel sheet 1 with the pulsed laser beam 13 having a fluence sufficient for descaling.
[0024] Here, a schematic diagram showing the trajectory of the center of pulsed laser beam 13 that scans back and forth across the surface of stainless steel sheet 1 is shown in Figure 3. When pulsed laser beam 13 is irradiated while scanning back and forth in the X direction (e.g., the width direction of stainless steel sheet 1) and stainless steel sheet 1 is moved in the Y direction (e.g., the conveyance direction of stainless steel sheet 1) perpendicular to the X direction, the center of pulsed laser beam 13 follows trajectory 15 as shown in Figure 3. The energy of the pulsed laser beam 13 is concentrated at the turning portion 21 and its vicinity 22 compared to the main scanning portion 20, resulting in a greater heat input to these areas. Therefore, if the pulsed laser beam 13 is irradiated at the turning portion 21 and its vicinity 22 in the same manner while maintaining the fluence of the pulsed laser beam 13 required for descaling in the main scanning portion 20, the surface of the stainless steel sheet 1 will melt, resulting in the formation of excessively irregularities. These excessively irregularities can cause surface defects. For example, if oxide scale is removed using a laser beam after hot rolling and then cold rolling is performed in a subsequent process, the excessively irregularities will be crushed during the cold rolling, resulting in the formation of surface defects. An optical microscope photograph of the surface of the stainless steel sheet 1 on which surface defects have been formed is shown in Figure 4. In Figure 4, (a) is an optical microscope photograph, and (b) is an enlarged photograph of the area within the rectangular frame in (a). When surface defects are formed in this way, the appearance of the stainless steel sheet 1 is significantly deteriorated, and there is also the risk that rolling oil and the like will penetrate and remain in the excessively uneven parts, thereby reducing corrosion resistance. Excessively large unevenness that can cause surface defects has an arithmetic mean height Ra exceeding 5.0 μm and a maximum height Rz exceeding 20.0 μm. In this specification, the arithmetic mean height Ra and maximum height Rz are measured in accordance with JIS B0601:2013.
[0025] Therefore, in the oxide scale removal method according to the embodiment of the present invention, the fluence of the pulsed laser beam 13 at the turning portion 21 of the reciprocating scan and its vicinity 22 is set smaller than the fluence of the pulsed laser beam 13 at the main scanning portion 20 of the reciprocating scan. By controlling in this manner, it is possible to prevent an excessive increase in the amount of heat input at the turning portion 21 and its vicinity 22, where the energy of the pulsed laser beam 13 is likely to concentrate. As a result, it is possible to prevent the formation of excessively large uneven portions at the turning portion 21 and its vicinity 22, while maintaining the descaling effect.
[0026] After laser descaling, the surfaces of the folded portion 21 and its vicinity 22 preferably have an arithmetic mean height Ra of 5.0 μm or less and a maximum height Rz of 20.0 μm or less. By controlling the surface roughness to such a level, surface defects are less likely to occur even if cold rolling or other processes are performed in later steps.
[0027] The method for controlling the fluence of the pulsed laser light 13 is not particularly limited, and any method known in the art can be used. For example, the fluence can be adjusted by electronically controlling the laser oscillator 11. Alternatively, the fluence can be adjusted by controlling the pulse width using an Fθ lens disposed at the tip of the laser head 12. The fluence of the pulsed laser light 13 at the return portion 21 of the reciprocating scan and its vicinity 22 may be controlled to be gradually reduced to a predetermined value, or may be controlled to be suddenly reduced to a predetermined value.
[0028] The area of the turn-back portion 21 and its vicinity 22 may be set appropriately depending on the pulse width, but is preferably an area of 1% or less of the scan width in the X direction from each end of the scan width, and more preferably an area of 0.5 to 1%. For example, if the scan width in the width direction (X direction) of the stainless steel plate 1 is 200 mm, the area of the turn-back portion 21 and its vicinity 22 can be an area of 1 to 2 mm from each end of the scan width. With an area in this range, an excessive increase in the amount of heat input to the turn-back portion 21 and its vicinity 22 can be stably suppressed.
[0029] The fluence of the pulsed laser beam 13 in the main scanning unit 20 is not particularly limited, but it is preferable to determine an appropriate range depending on the pulse width. Specifically, the fluence of the pulsed laser beam 13 in the main scanning unit 20 is set to F [J / cm 2 ] and the pulse width is τ [ns], it is preferable that the following formula (1) is satisfied. 1×(τ / 100) 1 / 2 ≦F≦15×(τ / 100) 1 / 2 ···(1) The descaling effect can be ensured by setting the fluence of the pulsed laser beam 13 in the main scanning unit 20 within the range of formula (1). The lower limit of formula (1) is preferably 2×(τ / 100) 1 / 2 , more preferably 3×(τ / 100) 1 / 2 The upper limit of the formula (1) is preferably 13×(τ / 100). 1 / 2 , more preferably 10×(τ / 100) 1 / 2 is. For example, when the pulse width is 100 ns, the fluence of the pulsed laser light 13 in the main scanning unit 20 is preferably 1 to 15 J / cm. 2 , more preferably 2 to 13 J / cm 2 , and more preferably 3 to 10 J / cm 2 The pulse width can be set in the range of 10 to 1000 ns, and is preferably set in the range of 30 to 500 ns, and more preferably 50 to 300 ns.
[0030] The pulse width is the time per pulse that the pulsed laser beam 13 exerts a thermal effect on the irradiated object. The fluence is the energy density per unit area of the pulsed laser beam 13. In this specification, the fluence is the value obtained by dividing the energy per pulse of the pulsed laser beam 13 by the irradiated area of the pulsed laser beam 13. Therefore, if other conditions are the same, the longer the pulse width of the pulsed laser beam 13, the greater the fluence of the pulsed laser beam 13.
[0031] The fluence of the pulsed laser beam 13 at the turning portion 21 and its vicinity 22 is not particularly limited as long as it is smaller than the fluence of the pulsed laser beam 13 at the main scanning portion 20, but is preferably 20 to 90%, and more preferably 20 to 60%, of the fluence of the pulsed laser beam 13 at the main scanning portion 20. By controlling it within such a range, an excessive increase in the amount of heat input at the turning portion 21 and its vicinity 22 can be stably suppressed.
[0032] Fluence Fm [J / cm 2 ] of the pulsed laser light 13 at the turning portion 21 and its vicinity 22 2] can be expressed by equation (2) under the condition that it is smaller than the fluence of the pulsed laser beam 13 in the main scanning unit 20. 0.5×(τ / 100) 1 / 2 ≦Fm≦10×(τ / 100) 1 / 2 ···(2) In the formula, τ is the pulse width [ns]. Fluence Fm = 10 × (τ / 100) 1 / 2 By setting the fluence Fm to 0.5 × (τ / 100) or less, even if surface defects occur, they can be removed by pickling or the like. 1 / 2 By doing so, it is possible to obtain a sufficient descaling effect. The lower limit of the formula (2) is preferably 1×(τ / 100) 1 / 2 , more preferably 2×(τ / 100) 1 / 2 The upper limit of the formula (2) is preferably 8×(τ / 100). 1 / 2 , more preferably 7×(τ / 100) 1 / 2 is. For example, when the pulse width is 100 ns, the fluence of the pulsed laser light 13 at the turning portion 21 and its vicinity 22 is preferably 0.5 to 10 J / cm. 2 , more preferably 1 to 8 J / cm 2 , more preferably 2 to 7 J / cm 2 is.
[0033] If the reciprocating scanning width of the pulsed laser beam 13 is smaller than the length of the stainless steel plate 1 in the X direction (e.g., width direction), it is preferable to divide the region in the X direction into multiple regions and repeatedly perform reciprocating scanning of the pulsed laser beam 13 in each of the multiple regions. As an example, FIG. 5 shows a schematic diagram illustrating the trajectory of the center of pulsed laser beam 13 when the region in the X direction is divided into two and reciprocating scanning of pulsed laser beam 13 is repeated in each of the two regions. As shown in FIG. 5 , the pulsed laser beam 13 irradiation process includes a first irradiation process in which a portion A on the surface of the stainless steel sheet 1 is irradiated with the pulsed laser beam 13, and a second irradiation process in which a portion B on the surface of the stainless steel sheet 1 is irradiated with the pulsed laser beam 13 after the first irradiation process. In the first irradiation process, the center of the pulsed laser beam 13 follows a locus 16, and in the second irradiation process, the center of the pulsed laser beam 13 follows a locus 17. Here, the overlap D of the irradiation areas of the pulsed laser beam 13 in the X direction between the portions A and B is preferably 1 to 50%, more preferably 2 to 30%, of the scanning width in the X direction of each of the portions A and B. Setting the overlap D of the irradiation areas to 1% or more can enhance the descaling effect. Furthermore, setting the overlap D of the irradiation areas to 50% or less can enable efficient descaling even when the reciprocating scanning width of the pulsed laser beam 13 is smaller than the length of the stainless steel sheet 1 in the X direction (e.g., the width direction).
[0034] After the irradiation step (laser descaling), a pickling step can be further included as needed. By carrying out the pickling step, oxide scale can be stably removed. The method of pickling is not particularly limited, but may involve immersing the stainless steel sheet 1 in a pickling bath, which may contain, for example, HNO3 (nitric acid), H2SO4 (sulfuric acid), FeCl3 (ferric chloride solution), or a mixture of HNO3 and HF (hydrofluoric acid).
[0035] As a pretreatment for the pickling treatment, the surface of the stainless steel sheet 1 may be subjected to neutral salt electrolysis between the irradiation step and the pickling treatment step. The neutral salt electrolysis can be performed by immersing the stainless steel sheet 1 in a neutral salt aqueous solution containing neutral salts such as Na2SO4, K2SO4, or NaNO3 as the main component. By performing the neutral salt electrolysis, the stainless steel sheet 1 after the irradiation step is electrolyzed in the neutral salt aqueous solution. Therefore, even if the oxide scale is a chemically stable oxide with a dense structure, such as a Cr-based oxide, the oxide scale can be reliably removed by the pickling treatment after the neutral salt electrolysis.
[0036] Furthermore, when cold rolling is performed, a pretreatment such as molten salt immersion (salt bath) treatment may be performed on the surface of the stainless steel sheet 1 between the irradiation step (S51) and the pickling treatment step. The salt bath treatment can be performed by immersing the stainless steel sheet 1 in a mixed alkali molten salt bath containing caustic soda (NaOH) as the main agent and maintained at 400 to 500°C.
[0037] In the oxide scale removal step (S5), it is not essential to subject the surface of the stainless steel sheet 1 after the laser light irradiation step to pickling. Although this depends on the type of stainless steel sheet 1 to be treated and the conditions for laser irradiation, if the oxide scale can be sufficiently removed by the laser light irradiation step alone, the pickling step may be omitted. In other words, in the oxide scale removal step (S5), it is sufficient that at least the laser light irradiation step is performed. Furthermore, although the above description has been given in detail using stainless steel plate 1 as an example, it should be noted that the oxide scale removal method according to the embodiment of the present invention can also be applied to stainless steel materials other than stainless steel plate 1. [Example]
[0038] The present invention will be described in detail below with reference to examples, but the present invention should not be construed as being limited to these examples. A hot-rolled and annealed sheet (stainless steel sheet) of SUS316 steel type was produced by carrying out the steelmaking process (S1), continuous casting process (S2), hot rolling process (S3), and continuous annealing process (S4) described above. Next, the hot-rolled annealed sheet was subjected to laser descaling as an oxide scale removal step (S5). Laser descaling was performed using a commercially available device (LaserClear50A manufactured by IHI Inspection & Measurement Co., Ltd.). The hot-rolled annealed sheet was placed on the movable stage of this device, and a pulsed laser beam was irradiated from above the hot-rolled annealed sheet while scanning back and forth at a constant speed in the sheet width direction (X direction), and the hot-rolled annealed sheet was moved at 0.5 m / min along the rolling direction (Y direction). The reciprocating scanning width was 25 mm, and the pulsed laser beam irradiation conditions were as follows:
[0039] (Irradiation condition A) Wavelength: 1085nm Pulse width: 100ns Oscillation frequency: 120kHz Irradiation speed: 100Hz Laser beam diameter: 90 μm Fluence: 6.55J / cm 2
[0040] (Irradiation condition B) Wavelength: 1085nm Pulse width: 100ns Oscillation frequency: 120kHz Irradiation speed: 100Hz Laser beam diameter: 90 μm Fluence: 3.93J / cm 2
[0041] The surface of the hot-rolled and annealed sheet after laser descaling was observed using an optical microscope, and the results (optical microscope photograph at 150 magnifications) are shown in Figure 6. The observed optical microscope photographs were binarized using the difference in brightness between the areas where oxide scale remained and the areas where the oxide scale had been removed, and the scale removal rate was calculated by dividing the area of the area where the oxide scale had been removed by the area of the observation range. As a result, when laser descaling was performed under irradiation condition A, the scale removal rate at the turn-back portion and its vicinity was 75%, and the scale removal rate at the main scanning portion was 72%. When laser descaling was performed under irradiation condition B, the scale removal rate at the turn-back portion and its vicinity was 55%, and the scale removal rate at the main scanning portion was 52%. Note that if the scale removal rate is 50% or higher, the remaining scale can be easily removed by pickling or other methods, and therefore the scale removal effect can be determined to be good.
[0042] In addition, the cross-sectional curves were measured in the main scanning portion (P1) of the reciprocating scan and near the turning portion (P2) in the optical microscope photograph, and the arithmetic mean height Ra and maximum height Rz were calculated. P1 was located 700 μm from the end, and P2 was located 100 μm from the end. The cross-sectional curves were measured using a laser microscope (OLS4100, manufactured by Olympus Corporation). The results of the measured cross-sectional curves are shown in Figure 6.
[0043] As shown in Figure 6, when laser descaling was performed under irradiation condition A (top row of Figure 6), excessively large irregularities were observed in and around the folded portion. These irregularities had an arithmetic mean height Ra of 4.7 μm and a maximum height Rz of 30.0 μm. Therefore, these irregularities can cause surface defects. On the other hand, no excessively large irregularities were observed in the main scanning area, where the arithmetic mean height Ra was 1.1 μm and the maximum height Rz was 7.4 μm. Furthermore, when laser descaling was performed under irradiation condition B (lower row in Figure 6), small irregularities were observed in and around the folded portion. These small irregularities had an arithmetic mean height Ra of 2.1 μm and a maximum height Rz of 14.9 μm. Therefore, these small irregularities are unlikely to cause surface defects. Furthermore, no small irregularities were observed in the main scanning area, where the arithmetic mean height Ra was 0.9 μm and the maximum height Rz was 6.5 μm. Therefore, when irradiating the pulsed laser light while scanning back and forth, it is presumed that by irradiating the pulsed laser light in the main scanning area under irradiation condition A and irradiating the turning area and its vicinity under irradiation condition B, descaling can be performed without forming excessively large unevenness in the turning area and its vicinity.
[0044] As can be seen from the above results, the present invention provides a method for removing oxide scale that can suppress the formation of excessively large irregularities due to an increase in the amount of heat input at and near the turning points during reciprocating scanning of the laser light. Furthermore, the present invention provides a method for producing stainless steel materials with high production efficiency and good appearance. [Explanation of symbols]
[0045] 1 Stainless steel plate 10 Laser light irradiation device 11 Laser oscillator 12 Laser head 13 Pulsed laser light 15,16,17 Trajectory of the central part of the pulsed laser beam 20 Main scanning section 21 Folded section 22 Near the turning point
Claims
1. A method for removing oxide scale formed on a surface of a stainless steel material after hot rolling or cold rolling by irradiating the material with a pulsed laser beam, comprising the steps of: an irradiation step of irradiating the stainless steel material with the pulsed laser light while scanning it back and forth in an X direction and moving the stainless steel material in a Y direction perpendicular to the X direction; a pickling process step of performing pickling process after the irradiation process; Including, The pulse width of the pulsed laser light is 10 to 1000 ns, a fluence of the pulsed laser light in a return portion of the reciprocating scan and in the vicinity thereof is made smaller than a fluence of the pulsed laser light in a main scanning portion of the reciprocating scan; The irradiation step includes a first irradiation step of irradiating a portion A of the surface of the stainless steel material with the pulsed laser light, and a second irradiation step of irradiating a portion B of the surface of the stainless steel material with the pulsed laser light after the first irradiation step, an overlap of an irradiation area of the pulsed laser light between the part A and the part B in the X direction is 1 to 50% of a scanning width in the X direction of each of the part A and the part B.
2. The method for removing oxide scale according to claim 1 , wherein the folded portion and its vicinity are an area that is 1% or less of the scanning width in the X direction.
3. The pulsed laser light in the main scanning portion has a fluence of F [J / cm 2 3. The method for removing oxide scale according to claim 1 or 2, wherein the following formula (1) is satisfied, where m is the pulse width and τ is a pulse width [ns]. 1×(t / 100) 1 / 2 ≦F≦15×(τ / 100) 1 / 2 ・・・(1)
4. The method for removing oxide scale according to any one of claims 1 to 3, wherein a fluence of the pulsed laser light in the turning-back portion and its vicinity is 20 to 90% of a fluence of the pulsed laser light in the main scanning portion.
5. The method for removing oxide scale according to any one of claims 1 to 4, wherein the stainless steel material is a stainless steel plate.
6. A method for producing a stainless steel material, comprising the method for removing oxide scale according to any one of claims 1 to 5.
Citation Information
Patent Citations
Irradiating method of laser light
JP1984089476A
Laser hardening device
JP1986079714A
Method for descaling stainless steel sheet
JP1992182020A
Method for treating metal surface
JP1995171689A
Method and apparatus for removing oxide from metal surface
JP1999269683A