Optical Sheet

The optical sheet design with controlled friction and surface characteristics minimizes multiple removals from a stack, improving handling and application efficiency.

JP7564170B2Active Publication Date: 2024-10-08SUMITOMO CHEM CO LTD
View PDF 14 Cites 0 Cited by

Patent Information

Application Number
JP2022172402
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2017-07-20
Filing Date
2022-10-27
Publication Date
2024-10-08
Estimated Expiration
2038-07-02

AI Technical Summary

Technical Problem

Optical sheets, particularly polarizing plates, are prone to multiple removal when taken out one by one from a stack due to their weight and friction characteristics, especially with the increasing demand for thinner designs.

Method used

The optical sheet is designed with a surface protection film, polarizing plate, and release film, where the coefficient of dynamic friction between the films is 0.4 or less, the polarizing plate thickness is 30 μm to 150 μm, and the polarizing plate surface has an arithmetic mean roughness of 0.001 μm to 0.3 μm, with a silicon atom abundance of 3% or more on the release film surface and a marking area ratio of 2% or less.

Benefits of technology

This configuration reduces the likelihood of multiple sheets being taken out simultaneously, enhancing handling and application efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007564170000003
    Figure 0007564170000003
  • Figure 0007564170000004
    Figure 0007564170000004
  • Figure 0007564170000005
    Figure 0007564170000005
Patent Text Reader

Abstract

The object of the present invention is to provide an optical sheet that is less likely to cause the problem of removing multiple optical sheets in one go (multiple removal) when removing each optical sheet one by one from a laminate containing multiple optical sheets stacked on top of each other. The display device includes a surface protection film, a polarizing plate, and a release film in this order. the coefficient of dynamic friction between the surface protection film and the release film is 0.4 or less; The thickness of the polarizing plate is 30 μm or more and 150 μm or less, The surface of the polarizing plate on the surface protection film side has an arithmetic mean roughness Ra of 0.001 μm or more and 0.3 μm or less in accordance with JIS B 0601:2013. Optical sheet.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an optical sheet. [Background technology]

[0002] Polarizing plates are widely used in image display devices such as liquid crystal display devices, and particularly in recent years in various mobile devices such as smartphones. Conventionally, polarizing plates have been used that are formed by laminating a protective film on one or both sides of a polarizer in which a dichroic dye is adsorbed and oriented on a polyvinyl alcohol-based resin film.

[0003] Polarizing plates are generally distributed on the market as optical sheets with a peelable surface protection film (also called a protect film) and a release film (also called a separate film) attached to their surface to prevent the surface from getting dirty or scratched.

[0004] When the polarizing plate is to be attached to a display element such as a liquid crystal cell, the optical sheets are taken out one by one from the laminate in which a plurality of the optical sheets are stacked, and the release film is peeled off from each optical sheet, so that the polarizing plate is attached to the display element via the exposed pressure-sensitive adhesive layer.

[0005] Patent Document 1 proposes automating the optical sheet removal process by using a machine in order to make the optical sheet removal process more efficient (Patent Document 1). When the optical sheet is removed automatically in this way, there is a problem that multiple optical sheets are removed in one removal (hereinafter sometimes referred to as multiple removal).

[0006] In addition, when the polarizing plate is thick, the optical sheet separates due to its own weight including the polarizing plate, so multiple taking is unlikely to occur. However, in recent years, there has been an increasing demand for thinner polarizing plates, and the separating effect due to the weight of the optical sheet is small, so multiple taking is likely to occur. [Prior art documents] [Patent documents]

[0007] [Patent Document 1] JP 2006-308912 A Summary of the Invention [Problem to be solved by the invention]

[0008] An object of the present invention is to provide an optical sheet which is less likely to result in multiple optical sheets being taken out one by one from a laminate in which a plurality of optical sheets are stacked. [Means for solving the problem]

[0009] [1] A surface protective film, a polarizing plate, and a release film, in that order; The coefficient of dynamic friction between the surface protective film and the release film is 0.4 or less; The thickness of the polarizing plate is 30 μm or more and 150 μm or less, The surface of the polarizing plate on the surface protective film side has an arithmetic average roughness Ra of 0.001 μm or more and 0.3 μm or less in accordance with JIS B 0601:2013. Optical sheet. [2] The optical sheet according to claim 1, wherein the surface of the release film opposite the polarizing plate has a silicon atom content of 3% or more. [3] The release film has a marking on a surface opposite to the polarizing plate, 3. The optical sheet according to claim 1, wherein the ratio of the area of ​​the marking to the area of ​​the release film is 2% or less. Effect of the Invention

[0010] It is possible to provide an optical sheet which is less likely to result in multiple optical sheets being taken out one by one from a laminate in which a plurality of optical sheets are superposed. [Brief description of the drawings]

[0011] [Figure 1] FIG. 2 is a schematic cross-sectional view showing an example of a layer structure of the optical sheet of the present invention. [Diagram 2] FIG. 1 is a schematic cross-sectional view showing an example of a laminate in which a plurality of optical sheets of the present invention are laminated. [Diagram 3] 1 is a schematic plan view of an optical sheet of the present invention as viewed from the release film side. [Figure 4] FIG. 13 is a schematic diagram showing an example of marking. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0012] <Optical sheet> Fig. 1 is a schematic cross-sectional view showing an example of the optical sheet of the present invention. The optical sheet 10 shown in Fig. 1 is a laminated film having a surface protective film 2, a polarizing plate 1, and a release film 3 in this order. In the optical sheet 10, the surface protective film 2, the polarizing plate 1, and the release film 3 are preferably laminated in this order. In the optical sheet 10, the surface protective film 2 and the release film 3 are preferably members that respectively constitute the outermost surface of the optical sheet.

[0013] The optical sheet 10 may be obtained by producing a long optical sheet using a roll-to-roll process while transporting each of the components that make up the optical sheet 10, and then cutting the sheet, or by preparing each of the components of a predetermined shape and stacking them in sequence.

[0014] The shape of the optical sheet is not particularly limited, but may be a rectangle, a polygon such as a triangle, a circle, an ellipse, or a combination thereof.

[0015] The area of ​​the optical sheet is not particularly limited, but is, for example, 18600 to 2500 mm 2 It is preferable that the thickness is 12600 to 6870 mm. 2 It is more preferable that the area of ​​the optical sheet is 18600 mm 2 When the area of ​​the optical sheet is smaller than 2500 mm, the optical sheet is difficult to separate into individual optical sheets due to its own weight, as described above, and therefore the effect of the present invention is remarkable. 2 If it is larger, it is easier to adjust the friction force as described below.

[0016] From a similar standpoint, when the optical sheet has a rectangular shape having long and short sides, the length of the long side is preferably 17.3 to 6.6 cm, and more preferably 15.5 to 11.0 cm, and the length of the short side is preferably 10.8 to 3.7 cm, and more preferably 8.7 to 6.2 cm.

[0017] In the present invention, the dynamic friction coefficient between the surface protective film and the release film is 0.40 or less, and preferably 0.30 or less. On the other hand, from the viewpoint of increasing the adhesive force between the release tape and the surface protective film when the surface protective film is peeled off using the release tape, the dynamic friction coefficient is preferably 0.10 or more, and may be 0.20 or more. The dynamic friction coefficient is measured according to the method described in the examples below.

[0018] As described later, the dynamic friction coefficient can be controlled by the proportion of silicon atoms present on the release film surface, the surface resistivity of the release film and the surface protective film, etc. When controlling the dynamic friction coefficient by the surface resistivity, it is preferable that at least one of the release film and the surface protective film has an antistatic function, and it is preferable that both have an antistatic function.

[0019] Each member of the optical sheet will be described below. <Polarizing plate> The polarizing plate 1 is a polarizing element including at least a polarizer, and usually further includes a thermoplastic resin film attached to one or both sides of the polarizer. The thermoplastic resin film can be a protective film for protecting the polarizer, another optical film having an optical function different from that of the polarizer, or the like. The thermoplastic resin film may have a resin layer (for example, at least one optical layer selected from a hard coat layer, an antistatic layer, an antiglare layer, a light diffusion layer, a retardation layer (a retardation layer having a retardation value of 1 / 4 wavelength, etc.), an antireflection layer, a low refractive index layer, an antifouling layer, etc.) laminated on the surface thereof. The thermoplastic resin film can be attached to the polarizer via an adhesive layer or a pressure-sensitive adhesive layer. The surface protective film 2 may be laminated on the surface of this resin layer.

[0020] The thickness of the polarizing plate 1 is not particularly limited, but is usually 200 μm or less. The effect of the present invention is remarkable when the thickness is 150 μm or less, or even 125 μm or less, at which multiple films are likely to be taken due to their own weight. The thickness of the polarizing plate 1 is preferably 30 μm or more, and more preferably 50 μm or more.

[0021] (1) Polarizer The polarizer constituting the polarizing plate 1 is an absorption-type polarizer that has the property of absorbing linearly polarized light having a vibration plane parallel to its absorption axis and transmitting linearly polarized light having a vibration plane perpendicular to the absorption axis (parallel to the transmission axis), and a polarizing film in which a dichroic dye is adsorbed and oriented on a uniaxially stretched polyvinyl alcohol-based resin film can be suitably used. The polarizer can be produced, for example, by a method including the steps of uniaxially stretching a polyvinyl alcohol-based resin film, dyeing the polyvinyl alcohol-based resin film with the dichroic dye to adsorb it, treating the polyvinyl alcohol-based resin film with a crosslinking liquid such as an aqueous boric acid solution, and washing with water after the treatment with the crosslinking liquid.

[0022] As the polyvinyl alcohol resin, a saponified polyvinyl acetate resin can be used. As the polyvinyl acetate resin, in addition to polyvinyl acetate, which is a homopolymer of vinyl acetate, copolymers of vinyl acetate with other monomers copolymerizable therewith can be mentioned. Examples of other monomers copolymerizable with vinyl acetate include unsaturated carboxylic acids, olefins, vinyl ethers, unsaturated sulfonic acids, and (meth)acrylamides having an ammonium group.

[0023] In this specification, "(meth)acrylic" means at least one selected from acrylic and methacrylic. The same applies to "(meth)acryloyl", "(meth)acrylate", etc.

[0024] The saponification degree of the polyvinyl alcohol resin is usually 85 to 100 mol%, preferably 98 mol% or more. The polyvinyl alcohol resin may be modified, and for example, polyvinyl formal or polyvinyl acetal modified with aldehydes can be used. The average polymerization degree of the polyvinyl alcohol resin is usually 1000 to 10000, preferably 1500 to 5000. The average polymerization degree of the polyvinyl alcohol resin can be determined in accordance with JIS K 6726.

[0025] Such a polyvinyl alcohol-based resin is used as a raw film for a polarizer (polarizing film). The method for forming the polyvinyl alcohol-based resin is not particularly limited, and a known method is used. The thickness of the polyvinyl alcohol-based raw film is not particularly limited, but it is preferable to use one having a thickness of 5 to 35 μm in order to make the thickness of the polarizer 15 μm or less. More preferably, it is 20 μm or less.

[0026] The uniaxial stretching of the polyvinyl alcohol-based resin film can be performed before, simultaneously with, or after dyeing with a dichroic dye. When the uniaxial stretching is performed after dyeing, the uniaxial stretching may be performed before or during a crosslinking treatment. The uniaxial stretching may also be performed in a plurality of these stages.

[0027] In the uniaxial stretching, the film may be stretched uniaxially between rolls having different peripheral speeds, or may be stretched uniaxially using a heated roll. The uniaxial stretching may be dry stretching in which stretching is performed in the atmosphere, or wet stretching in which stretching is performed in a state where the polyvinyl alcohol-based resin film is swollen using a solvent or water. The stretching ratio is usually 3 to 8 times.

[0028] As a method for dyeing a polyvinyl alcohol-based resin film with a dichroic dye, for example, a method of immersing the film in an aqueous solution containing the dichroic dye is adopted. As the dichroic dye, iodine or a dichroic organic dye is used. It is preferable that the polyvinyl alcohol-based resin film is immersed in water before the dyeing process.

[0029] As a crosslinking treatment after dyeing with a dichroic dye, a method of immersing the dyed polyvinyl alcohol resin film in an aqueous solution containing boric acid is usually adopted. When iodine is used as the dichroic dye, the aqueous solution containing boric acid preferably contains potassium iodide.

[0030] The thickness of the polarizer is usually 30 μm or less, preferably 20 μm or less, more preferably 15 μm or less, and even more preferably 10 μm or less. In particular, a thickness of 15 μm or less of the polarizer is advantageous for thinning the optical sheet. The thickness of the polarizer is usually 2 μm or more.

[0031] (2) Protective film The protective film that can be laminated on one or both sides of the polarizer can be a film made of a light-transmitting (preferably optically transparent) thermoplastic resin, for example, a polyolefin resin such as a chain polyolefin resin (such as a polypropylene resin) or a cyclic polyolefin resin (such as a norbornene resin); a cellulose resin such as triacetyl cellulose or diacetyl cellulose; a polyester resin such as polyethylene terephthalate or polybutylene terephthalate; a polycarbonate resin; a (meth)acrylic resin such as a methyl methacrylate resin; a polystyrene resin; a polyvinyl chloride resin; an acrylonitrile-butadiene-styrene resin; an acrylonitrile-styrene resin; a polyvinyl acetate resin; a polyvinylidene chloride resin; a polyamide resin; a polyacetal resin; a modified polyphenylene ether resin; a polysulfone resin; a polyethersulfone resin; a polyarylate resin; a polyamideimide resin; a polyimide resin, or the like.

[0032] Examples of linear polyolefin resins include linear olefin homopolymers such as polyethylene resins (polyethylene resins which are homopolymers of ethylene, and copolymers mainly composed of ethylene) and polypropylene resins (polypropylene resins which are homopolymers of propylene, and copolymers mainly composed of propylene), as well as copolymers composed of two or more types of linear olefins.

[0033] Cyclic polyolefin resin is a general term for resins polymerized with cyclic olefin as a polymerization unit, and examples thereof include resins described in JP-A-1-240517, JP-A-3-14882, JP-A-3-122137, etc. Specific examples of cyclic polyolefin resins include ring-opening (co)polymers of cyclic olefins, addition polymers of cyclic olefins, copolymers (typically random copolymers) of cyclic olefins and chain olefins such as ethylene and propylene, and graft polymers modified with unsaturated carboxylic acids or derivatives thereof, as well as hydrogenated products thereof. Among these, norbornene resins using norbornene monomers such as norbornene or polycyclic norbornene monomers as cyclic olefins are preferably used.

[0034] The polyester resin is a resin having an ester bond, excluding the cellulose ester resin described below, and is generally made of a polycondensate of a polyvalent carboxylic acid or its derivative and a polyhydric alcohol. As the polyvalent carboxylic acid or its derivative, a divalent dicarboxylic acid or its derivative can be used, for example, terephthalic acid, isophthalic acid, dimethyl terephthalate, and dimethyl naphthalenedicarboxylate. As the polyhydric alcohol, a divalent diol can be used, for example, ethylene glycol, propanediol, butanediol, neopentyl glycol, and cyclohexanedimethanol. A representative example of the polyester resin is polyethylene terephthalate, which is a polycondensate of terephthalic acid and ethylene glycol.

[0035] The (meth)acrylic resin is a resin whose main constituent monomer is a compound having a (meth)acryloyl group. Specific examples of the (meth)acrylic resin include poly(meth)acrylic acid ester such as polymethyl methacrylate; methyl methacrylate-(meth)acrylic acid copolymer; methyl methacrylate-(meth)acrylic acid ester copolymer; methyl methacrylate-acrylic acid ester-(meth)acrylic acid copolymer; methyl (meth)acrylate-styrene copolymer (MS resin, etc.); copolymers of methyl methacrylate and a compound having an alicyclic hydrocarbon group (e.g., methyl methacrylate-cyclohexyl methacrylate copolymer, methyl methacrylate-norbornyl (meth)acrylate copolymer, etc.). Preferably, poly(meth)acrylic acid C such as polymethyl (meth)acrylate is used. 1-6 A polymer containing an alkyl ester as a main component is used, and more preferably, a methyl methacrylate-based resin containing methyl methacrylate as a main component (50 to 100% by weight, preferably 70 to 100% by weight) is used.

[0036] The cellulose ester resin is an ester of cellulose and a fatty acid. Specific examples of the cellulose ester resin include cellulose triacetate, cellulose diacetate, cellulose tripropionate, and cellulose dipropionate. In addition, copolymers thereof and those in which a part of the hydroxyl group is modified with another substituent are also included. Among these, cellulose triacetate (triacetyl cellulose) is particularly preferred.

[0037] Polycarbonate resins are engineering plastics made of polymers in which monomer units are bonded via carbonate groups.

[0038] It is also useful to control the retardation value of the protective film to a value suitable for image display devices such as liquid crystal display devices. For example, in an in-plane switching (IPS) mode liquid crystal display device, it is preferable to use a film having a retardation value of substantially zero as the protective film. A retardation value of substantially zero means that the in-plane retardation value R0 at a wavelength of 590 nm is 10 nm or less, and the thickness direction retardation value R th The absolute value of is 10 nm or less, and the thickness direction retardation value R th The absolute value of is 15 nm or less.

[0039] For example, depending on the mode of the liquid crystal display device, the protective film may be stretched and / or shrunk to provide a suitable retardation value. For example, for the purpose of compensating for the viewing angle, a retardation layer (or film) having a single layer or multilayer structure may be used as the protective film. In this case, the polarizing plate 1 may be an elliptical or circular polarizing plate having a laminated structure of a polarizer and a retardation layer, or a polarizing plate having a viewing angle compensation function including a retardation layer.

[0040] The thickness of the protective film is usually 1 to 100 μm, but is preferably 5 to 60 μm and more preferably 5 to 50 μm from the viewpoints of strength, handleability, etc. If the thickness is within this range, the polarizer is mechanically protected, and the polarizer does not shrink even when exposed to a moist and hot environment, and stable optical properties can be maintained.

[0041] When protective films are attached to both sides of a polarizer, these protective films may be made of the same type of thermoplastic resin or different types of thermoplastic resin. In addition, the thicknesses may be the same or different. Furthermore, the retardation properties may be the same or different.

[0042] As described above, at least one of the protective films may have a surface treatment layer (coating layer) on its outer surface (the surface opposite to the polarizer), such as a hard coat layer, an antiglare layer, a light diffusion layer, a retardation layer (e.g., a retardation layer having a ¼ wavelength retardation value), an antireflection layer, a low refractive index layer, an antistatic layer, or an antifouling layer.

[0043] From the viewpoint of suppressing the intrusion of air bubbles between the surface protective film and the polarizing plate, the surface of the polarizing plate 1 on the surface protective film 2 side (the surface to which the surface protective film 2 is attached) preferably has a small arithmetic average roughness Ra according to JIS B 0601:2013. Specifically, the Ra of the above surface is preferably 0.3 μm or less, more preferably 0.2 μm or less, and even more preferably 0.15 μm or less. The Ra of the above surface is usually 0.001 μm or more, for example 0.005 μm or more.

[0044] The protective film can be attached to the polarizer via, for example, an adhesive layer. As the adhesive for forming the adhesive layer, a water-based adhesive, an active energy ray-curable adhesive, or a thermosetting adhesive can be used, and a water-based adhesive or an active energy ray-curable adhesive is preferable.

[0045] Examples of the aqueous adhesive include an adhesive made of an aqueous polyvinyl alcohol resin solution, an aqueous two-liquid urethane emulsion adhesive, and the like. Among them, an aqueous adhesive made of an aqueous polyvinyl alcohol resin solution is preferably used. Examples of the polyvinyl alcohol resin include a vinyl alcohol homopolymer obtained by saponifying polyvinyl acetate, which is a homopolymer of vinyl acetate, a polyvinyl alcohol copolymer obtained by saponifying a copolymer of vinyl acetate and another monomer copolymerizable therewith, and a modified polyvinyl alcohol polymer in which the hydroxyl groups of these are partially modified. The aqueous adhesive may contain a crosslinking agent such as an aldehyde compound (such as glyoxal), an epoxy compound, a melamine compound, a methylol compound, an isocyanate compound, an amine compound, or a polyvalent metal salt.

[0046] When a water-based adhesive is used, it is preferable to carry out a drying step for removing water contained in the water-based adhesive after laminating the polarizer and the protective film. After the drying step, a curing step may be carried out, for example, at a temperature of 20 to 45° C.

[0047] The active energy ray-curable adhesive is an adhesive containing a curable compound that is cured by irradiation with active energy rays such as ultraviolet rays, visible light, electron beams, and X-rays, and is preferably an ultraviolet ray-curable adhesive.

[0048] The curable compound may be a cationic polymerizable curable compound or a radical polymerizable curable compound. Examples of the cationic polymerizable curable compound include an epoxy compound (a compound having one or more epoxy groups in the molecule), an oxetane compound (a compound having one or more oxetane rings in the molecule), or a combination thereof. Examples of the radical polymerizable curable compound include a (meth)acrylic compound (a compound having one or more (meth)acryloyloxy groups in the molecule), other vinyl compounds having a radical polymerizable double bond, or a combination thereof. A cationic polymerizable curable compound and a radical polymerizable curable compound may be used in combination. An active energy ray curable adhesive usually further includes a cationic polymerization initiator and / or a radical polymerization initiator for initiating the curing reaction of the curable compound.

[0049] When laminating the polarizer and the protective film, at least one of the laminating surfaces may be subjected to a surface activation treatment in order to enhance adhesion. Examples of the surface activation treatment include dry treatments such as corona treatment, plasma treatment, discharge treatment (glow discharge treatment, etc.), flame treatment, ozone treatment, UV ozone treatment, and ionizing active ray treatment (ultraviolet ray treatment, electron beam treatment, etc.); and wet treatments such as ultrasonic treatment using a solvent such as water or acetone, saponification treatment, and anchor coat treatment. These surface activation treatments may be performed alone or in combination of two or more.

[0050] When protective films are attached to both sides of the polarizer, the adhesive for attaching these protective films may be the same kind of adhesive or different kinds of adhesives.

[0051] (3) Other optical films The polarizing plate 1 may include other optical films in addition to the polarizer and the protective film, typical examples of which are a brightness enhancement film and a retardation film. When the polarizing plate 1 includes other optical films, the surface protective film 2 may be laminated on the surface of the optical film or on the surface of a resin layer laminated on the optical film.

[0052] The brightness enhancement film is also called a reflective polarizing film, and a polarization conversion element having a function of separating light emitted from a light source (backlight) into transmitted polarized light and reflected polarized light or scattered polarized light is used. By disposing the brightness enhancement film on a polarizer, the output efficiency of the linearly polarized light output from the polarizer can be improved by utilizing the retroreflected light, which is reflected polarized light or scattered polarized light. The brightness enhancement film can be laminated on the polarizer via an adhesive layer. Another film such as a protective film may be interposed between the polarizer and the brightness enhancement film.

[0053] The brightness enhancement film can be, for example, an anisotropic reflective polarizer. One example of an anisotropic reflective polarizer is an anisotropic multi-layer thin film that transmits linearly polarized light in one vibration direction and reflects linearly polarized light in the other vibration direction, a specific example of which is "DBEF" manufactured by 3M (see JP-A-4-268505, etc.). Another example of an anisotropic reflective polarizer is a complex of a cholesteric liquid crystal layer and a λ / 4 plate, a specific example of which is "PCF" manufactured by Nitto Denko Corporation (see JP-A-11-231130, etc.). Yet another example of an anisotropic reflective polarizer is a reflective grid polarizer, a specific example of which is a metal grid reflective polarizer that emits reflected polarized light even in the visible light region by microfabricating a metal (see U.S. Pat. No. 6,288,840, etc.), and a film obtained by adding metal fine particles to a polymer matrix and stretching the polymer matrix (see JP-A-8-184701, etc.).

[0054] As described above, the outer surface of the brightness enhancement film may be provided with a surface treatment layer (coating layer) such as a hard coat layer, an antiglare layer, a light diffusion layer, a retardation layer (such as a retardation layer having a ¼ wavelength retardation value), an antireflection layer, a low refractive index layer, an antistatic layer, or an antifouling layer. The formation of such layers can improve adhesion to the backlight tape and uniformity of the displayed image. The thickness of the brightness enhancement film 50 is usually 10 to 100 μm, but from the viewpoint of making the polarizing plate 1 thinner, it is preferably 10 to 50 μm, and more preferably 10 to 30 μm.

[0055] (4) Adhesive layer The polarizing plate 1 preferably has an adhesive layer on its outermost surface. This adhesive layer can be used to attach the polarizing plate 1 to a display element (such as a liquid crystal cell) or other optical members. It is preferable that a release film 3 is laminated on this adhesive layer. The adhesive layer can also be used to laminate a polarizer with a protective film or a brightness-enhancing film. The adhesive layer can be composed of an adhesive composition containing a resin such as a (meth)acrylic, rubber, urethane, ester, silicone, or polyvinyl ether resin as a main component. Among them, an adhesive composition containing a (meth)acrylic resin as a base polymer, which is excellent in transparency, weather resistance, heat resistance, etc., is preferable. The adhesive composition may be an active energy ray curable type or a heat curable type.

[0056] As the (meth)acrylic resin (base polymer) used in the pressure-sensitive adhesive composition, for example, a polymer or copolymer containing one or more (meth)acrylic acid esters as monomers, such as butyl (meth)acrylate, ethyl (meth)acrylate, isooctyl (meth)acrylate, and 2-ethylhexyl (meth)acrylate, is preferably used. It is preferable to copolymerize a polar monomer into the base polymer. Examples of the polar monomer include monomers having a carboxyl group, a hydroxyl group, an amide group, an amino group, an epoxy group, and the like, such as (meth)acrylic acid, 2-hydroxypropyl (meth)acrylate, hydroxyethyl (meth)acrylate, (meth)acrylamide, N,N-dimethylaminoethyl (meth)acrylate, and glycidyl (meth)acrylate.

[0057] The adhesive composition may contain only the base polymer, but usually further contains a crosslinking agent. Examples of the crosslinking agent include divalent or higher metal ions that form a carboxylate metal salt with a carboxyl group; polyamine compounds that form an amide bond with a carboxyl group; polyepoxy compounds or polyols that form an ester bond with a carboxyl group; and polyisocyanate compounds that form an amide bond with a carboxyl group. Among them, polyisocyanate compounds are preferred.

[0058] The active energy ray curable adhesive composition has a property of being cured by irradiation with active energy rays such as ultraviolet rays and electron beams, and has adhesiveness even before irradiation with active energy rays, can be adhered to an adherend such as a film, and can be cured by irradiation with active energy rays to adjust the adhesive strength. The active energy ray curable adhesive composition is preferably an ultraviolet ray curable type. The active energy ray curable adhesive composition further contains an active energy ray polymerizable compound in addition to a base polymer and a crosslinking agent. If necessary, a photopolymerization initiator, a photosensitizer, etc. can also be contained.

[0059] The pressure-sensitive adhesive composition can contain additives such as microparticles for imparting light scattering properties, beads (e.g., resin beads, glass beads), glass fibers, resins other than the base polymer, antistatic agents, tackifiers, fillers (e.g., metal powders and other inorganic powders), antioxidants, UV absorbers, dyes, pigments, colorants, defoamers, corrosion inhibitors, and photopolymerization initiators.

[0060] The pressure-sensitive adhesive layer can be formed by applying an organic solvent dilution of the pressure-sensitive adhesive composition onto a substrate and drying it. The substrate can be a polarizer, a protective film, another optical film such as a brightness-improving film, a release film (e.g., release film 3), etc. When an active energy ray-curable pressure-sensitive adhesive composition is used, the formed pressure-sensitive adhesive layer can be irradiated with active energy rays to form a cured product having a desired degree of cure.

[0061] The thickness of the adhesive layer is usually 1 to 40 μm, but from the viewpoint of making the optical sheet thinner and suppressing dimensional changes in the polarizing plate 1 while maintaining good processability, it is preferably 3 to 25 μm (for example, 3 to 20 μm, or even 3 to 15 μm).

[0062] <Surface protection film> The surface protection film 2 can include a base film and a pressure-sensitive adhesive layer laminated thereon. The surface protection film 2 is a film for protecting the surface of the polarizing plate 1, and is usually peeled off and removed together with the pressure-sensitive adhesive layer thereof after the optical sheet is attached to, for example, a display element or other optical members.

[0063] The substrate film is preferably a thermoplastic resin film. Examples of the thermoplastic resin constituting the thermoplastic resin film include polyolefin resins such as polyethylene resins and polypropylene resins; cyclic polyolefin resins; polyester resins such as polyethylene terephthalate and polyethylene naphthalate; polycarbonate resins; (meth)acrylic resins, etc. The substrate film may have a single-layer structure or a multi-layer structure.

[0064] The thickness of the substrate film may be 20 to 150 μm (e.g., 30 to 80 μm, preferably 30 to 60 μm), and the thickness of the surface protective film 2 may be 40 to 200 μm (e.g., 50 to 160 μm). The configuration of the pressure-sensitive adhesive layer is basically the same as that described above for the pressure-sensitive adhesive layer of the polarizing plate.

[0065] In particular, the pressure-sensitive adhesive layer preferably has a storage modulus of 0.15 MPa or less, more preferably 0.14 MPa or less, and even more preferably 0.10 MPa or less at 80° C. Usually, the storage modulus of the pressure-sensitive adhesive layer at 80° C. is 0.01 MPa or more. In this specification, the storage modulus of the pressure-sensitive adhesive layer can be measured using a commercially available viscoelasticity measuring device, for example, a viscoelasticity measuring device "DYNAMIC ANALYZER RDA II" manufactured by REOMETRIC.

[0066] The surface of the surface protection film 2 opposite to the polarizing plate 1 has a surface resistivity of 1×10 7 ~1×10 12 It is preferable that the surface resistivity is 1×10 Ω / □. A surface protective film having such a surface resistivity can be said to have an antistatic function. A surface protective film having such a surface resistivity is difficult to be charged, and the dynamic friction coefficient is easily controlled to 0.40 or less. 12 If it exceeds Ω / □, the surface protection film becomes easily charged. The surface resistivity is measured by the method described in the examples below.

[0067] The surface protective film 2 may contain an antistatic agent. The antistatic agent may be contained in the pressure-sensitive adhesive layer, for example. Instead of or in addition to containing an antistatic agent in the pressure-sensitive adhesive layer, an antistatic layer containing an antistatic agent may be provided on the surface of the base film opposite to the surface on which the pressure-sensitive adhesive layer is laminated.

[0068] The antistatic agent may be an ionic compound, which is a compound having an inorganic or organic cation and an inorganic or organic anion. Two or more ionic compounds may be used.

[0069] <Release film> The release film 3 is a film that is temporarily attached to protect the surface of the adhesive layer until it is attached to a display element (e.g., a liquid crystal cell) or other optical components. The release film 3 is usually made of a thermoplastic resin film with one side subjected to a release treatment using a silicone-based, fluorine-based or other release agent, and the release-treated surface is attached to the adhesive layer. It is preferable that an antistatic layer is formed on the surface of the release film 3 opposite to the polarizing plate 1.

[0070] When an optical sheet manufactured by roll-to-roll is cut to obtain the optical sheet 10, the release film may be provided as a rolled body in which the release film is rolled up in the manufacture of a long optical sheet. In the rolled body of the release film, the surface to be bonded to the adhesive layer (the release-treated surface) is in contact with the surface that will become the outermost surface of the optical sheet 10, so that the components of the release-treated surface may be transferred to the surface that will become the outermost surface of the optical sheet 10. As a result of the inventor's investigation, it was found that the use of transfer makes it easier to prevent multiple taking. On the other hand, the surface of the release film 3 is beautified to remove any excess of the adhesive layer, etc. The beautification cleans the surface, removing the transferred silicon atoms, and the proportion of silicon atoms is often low. Therefore, moderate beautification is effective in preventing multiple take-up.

[0071] From the viewpoint of preventing multiple filming, the surface of the release film 3 opposite to the polarizing plate 1 preferably has a silicon atom content of 2% or more, more preferably 4% or more, and may be 6% or more. On the other hand, since it is necessary to perform moderate cosmetic treatment, the silicon atom content is usually 10% or less, preferably 8% or less. In the present invention, the silicon atom content is a value determined by X-ray photoelectron spectroscopy, and the details are as described in the examples below.

[0072] Of course, the proportion of silicon atoms present may be adjusted by applying silicone to the surface of the release film 3.

[0073] Furthermore, the proportion of silicon atoms present on one surface and the other surface of release film 3 may be the same or different.

[0074] The surface of the release film 3 opposite to the polarizing plate 1 has a surface resistivity of 1×10 7 ~1×10 12 It is preferable that the surface resistivity is 1×10 Ω / □. A release film having such a surface resistivity can be said to have an antistatic function. A release film having such a surface resistivity is difficult to be charged, and the dynamic friction coefficient is easily controlled to 0.40 or less. 12 If it exceeds Ω / □, the release film is likely to be charged. The surface resistivity is measured by the method described in the Examples below.

[0075] The surface resistivity of the release film can be controlled by forming an antistatic layer on the surface of the release film. The antistatic layer can be formed, for example, by applying an antistatic spray to the release film or by applying and curing a resin composition containing an antistatic agent. An example of the static electricity removal spray is static electricity removal liquid "SB-8" manufactured by Showa Kako Co., Ltd. The above-mentioned examples can be used as the antistatic agent.

[0076] The thermoplastic resin constituting the release film 3 can be, for example, a polyethylene-based resin such as polyethylene, a polypropylene-based resin such as polypropylene, a polyester-based resin such as polyethylene terephthalate or polyethylene naphthalate, etc. The thickness of the release film 3 is, for example, 10 to 50 μm.

[0077] <Marking> The optical sheet 10 may have a marking 4 on at least one of the surface protective film 2 and the release film 3, and it is preferable that the release film has the marking 4. The surface protective film 2 or the release film 3 preferably has the marking 4 on the surface opposite to the polarizing plate 1. When the optical sheet 10 is obtained by cutting an optical sheet produced by roll-to-roll production, the marking may be applied before or after cutting the long optical sheet.

[0078] By providing the markings, for example, the absorption axis direction or transmission axis direction of the polarizing plate 1 can be easily identified, and alignment can be easily performed, for example, when the polarizing plate is attached to a liquid crystal cell. On the other hand, the inventors have found that the presence of markings on the optical sheet makes it easier for multiple take-up to occur. Although this is not intended to limit the present invention, it is believed that this is because the markings cause the coating film to bulge on the surface of the optical sheet 10, increasing the dynamic friction coefficient.

[0079] In order to prevent multiple taking, the ratio of the area of ​​the marking to the area of ​​the release film is preferably 10% or less, more preferably 5% or less, and even more preferably 2% or less.

[0080] From the same viewpoint, the height of the marking (coating) from the film surface is preferably 0.1 to 0.2 μm, and may be 0.3 to 0.5 μm.

[0081] The marking 4 can be made by an inkjet or contact pen using oil-based or water-based ink, and the marking can be a coating of these. The color of the marking can be red, yellow, green, cyan, blue, magenta, white, black, or a mixture of these colors, and the marking can be made in one color or multiple colors.

[0082] Fig. 3 shows an example of a case where a release film 3 has a marking 4, where a linear marking 4 is formed between two opposing sides of an optical sheet 10. The shape of the marking is not limited to this, and may be a straight line, a dotted line, a dashed line, a curved line, or a combination thereof, or may be a figure such as a circle, a polygon, or a combination thereof, or may be a letter or a number, as shown in Figs. 4(a) to (d).

[0083] <Optical sheet laminate> By stacking a plurality of optical sheets, a laminate of optical sheets can be obtained, which can be fed to an optical sheet supplying device. As shown in Fig. 2, the laminate 100 of optical sheets is preferably stacked such that the release film 3 of one optical sheet 10 and the surface protective film 2 of another optical sheet 10 are in contact with each other.

[0084] The optical sheets 10 constituting the optical sheet laminate 100 may all be the same optical sheets, or some of the optical sheets may be different. The number of optical sheets constituting the optical sheet laminate 100 is not particularly limited, but may be, for example, 100 to 500.

[0085] The optical sheet 10 taken out from the optical sheet laminate 100 can be attached to a display element (e.g., a liquid crystal cell) by peeling off the release film 3. Furthermore, the surface protective film 2 can be peeled off and the optical sheet 10 can be incorporated into a display device (e.g., a liquid crystal display device). In constructing a display device, the optical sheet 10 according to the present invention may be used in a polarizing plate arranged on the viewer side, may be used in a polarizing plate arranged on the backlight side, or may be used in polarizing plates on both the viewer side and the backlight side. EXAMPLES

[0086] The present invention will be described in more detail below with reference to examples and comparative examples, but the present invention is not limited to these examples.

[0087] (1) Measurement method for dynamic friction coefficient The dynamic friction coefficient between the surface protection film and the release film was measured using a surface property measuring instrument TYPE:14FW manufactured by Shinto Scientific Co., Ltd. Specifically, an optical sheet was first cut to a size of 11 cm x 6.3 cm, and was attached to a fixture connected to the movable stage and load cell of the measuring instrument. The two optical sheets were arranged so that the release film and the surface protection film faced each other. Next, a load of 500 g was applied from above the overlapping films, and the films were moved back and forth 100 times at a speed of 5000 mm / min over a moving distance of 15.0 mm, and the average dynamic friction coefficient was calculated from the magnitude of the force detected by the load cell at that time. Note that the dynamic friction coefficient did not change depending on the direction of the marking provided in the examples and the moving direction of the movable stage, but in the case of anisotropy, the dynamic friction coefficient in the direction in which the dynamic friction coefficient is maximum is adopted.

[0088] (2) Method for measuring the proportion of silicon atoms The proportion of silicon atoms present on the film surface was measured by X-ray photoelectron spectroscopy (XPS) using K-Alpha (Thermo Fisher Scientific). The measurement surface was the back surface of the release film (the surface opposite to the surface in contact with the adhesive layer). The photoelectron take-off angle was set to 90°, and after measuring the carbon atoms, oxygen atoms, and silicon atoms, the amount of detected silicon atoms was calculated.

[0089] (3) Film thickness measurement method Measurements were made using a Nikon digital micrometer, "MH-15M."

[0090] (4) Evaluation method for multiple capture Two optical sheets were placed so that the surface protection film side and the release film side overlapped, and were rubbed together 10 times while being pressed by hand. The overlapping films were then shifted 1 cm, and one of the sheets was lifted up by holding it. If the two sheets were stuck together, they were shook three times to check whether one of the sheets would fall off. If one of the sheets did not fall off after this operation, it was deemed that multiple sheets had been taken.

[0091] (5) Measurement method of surface resistivity The surface resistivity (Ω / □) of the release film surface (the surface of the release film opposite the polarizing plate) and the surface protection film surface (the surface of the surface protection film opposite the polarizing plate) was measured using MCP-HT450 manufactured by Mitsubishi Chemical Analytech Co., Ltd. "Over" in the table indicates a surface resistivity of 1×10 12 This means that it is greater than Ω / □.

[0092] <Preparation of Optical Sheet 1> A polarizing plate having the following layer structure was prepared. Protective film 1 / Polarizer / Protective film 2 Protective film 1 was a cyclic olefin resin film and had a thickness of 23 μm. Protective film 2 was a cyclic olefin resin film having a hard coat layer on its surface, and had a thickness of 30 μm. The polarizer was a PVA resin film on which iodine was adsorbed and aligned, and had a thickness of 8 μm.

[0093] A release film having a pressure-sensitive adhesive layer was laminated on the surface of protective film 1 in the polarizing plate, and a surface protective film was laminated on the surface of protective film 2 in the polarizing plate to prepare optical sheet 1. For the surface protection film, a polyethylene terephthalate film (thickness 38 μm) with a 20 μm thick adhesive layer was used. The thickness of the surface protection film was 58 μm. An antistatic layer was formed on the surface of the polyethylene terephthalate film opposite to the surface in contact with the adhesive layer, and the surface resistivity of the surface of the surface protection film was 1×10 9 The resistivity was Ω / □. A polyethylene terephthalate film was used as the release film. The thickness of the release film was 38 μm. A 20 μm thick adhesive layer was formed on the release film. This adhesive layer on the release film is a component that will ultimately be included in the polarizing plate. Thereafter, the optical sheet 1 was cut into a rectangular shape with a long side of 110 mm and a short side of 63 mm.

[0094] <Optical sheet 2> Except for using a surface protection film without an antistatic layer, the optical sheet 2 was produced in the same manner as in the optical sheet production 1. The optical sheet 2 was cut into a rectangular shape with a long side of 110 mm and a short side of 63 mm.

[0095] <Example 1> Silicone was applied to the surface of the release film of the obtained optical sheet 1 (the surface of the release film opposite the polarizing plate) to prepare an optical sheet for evaluation. The proportion of silicon atoms was 7%. No marking was applied to the surface of the release film.

[0096] <Example 2> An optical sheet for evaluation was produced in the same manner as in Example 1, except that a marking was formed by drawing a straight line, as shown in Figure 3, along the absorption axis direction between two opposing sides of the optical sheet using Drysave 1 (blue, oil-based ink) manufactured by Terani Chemical Industry Co., Ltd. The ratio of the area of ​​the marking to the area of ​​the release film was 1%. The height of the marking was 0.3 μm from the surface of the release film.

[0097] <Example 3> An optical sheet for evaluation was produced in the same manner as in Example 2, except that three lines were drawn. The ratio of the area of ​​the marking to the area of ​​the release film was 3%.

[0098] <Examples 4 to 6> Optical sheets for evaluation were produced in the same manner as in Examples 1 to 3, except that the amount of silicone applied was adjusted so that the proportion of silicon atoms was 3%.

[0099] <Examples 7 to 9> Instead of applying silicone to the release film surface of the obtained optical sheet 1 (the surface of the release film opposite the polarizing plate), static electricity removal liquid "SB-8" manufactured by Showa Kako Co., Ltd. was applied to the release film surface of the obtained optical sheet 1 to increase the surface resistivity to 1×10 9The resistivity was set to Ω / □. Except for that, the optical sheets for evaluation were produced in the same manner as in Examples 1 to 3.

[0100] <Examples 10 to 12> Adjust the amount of static electricity removal liquid applied to reduce the surface resistivity to 1×10 12 Except for changing the resistivity to Ω / □, the same procedures as in Examples 7 to 9 were carried out to prepare optical sheets for evaluation.

[0101] <Example 13> The surface of the release film of the obtained optical sheet 2 (the surface of the release film opposite the polarizing plate) was coated with static electricity removing liquid "SB-8" manufactured by Showa Kako Co., Ltd. to set the surface resistivity of the release film to 1×10 12 The surface resistivity of the surface protection film was set to 1×10 Ω / □. The static electricity removal liquid "SB-8" also manufactured by Showa Kako Co., Ltd. was applied to the surface of the surface protection film (the surface of the surface protection film opposite the polarizing plate) to set the surface resistivity of the surface protection film to 1×10 12 In this manner, an optical sheet for evaluation was produced.

[0102] <Examples 14 to 16> Each optical sheet for evaluation was prepared in the same manner as in Example 13, except that the amount of static electricity removal liquid applied was adjusted to control the surface resistivity of the surfaces of the release film and surface protection film to the values ​​shown in Table 2.

[0103] <Comparative Examples 1 to 3> In Examples 1 to 3, optical sheets for evaluation were prepared in the same manner, except that the release film surface of each optical sheet was wiped several times with a cloth soaked in IP solvent (an ethanol-based solvent obtained from Showa Kako Co., Ltd.).

[0104] <Comparative Example 4> An optical sheet for evaluation was prepared in the same manner as in Example 1, except that silicone was not applied to the surface of the release film and the release film surface of the optical sheet was wiped several times with a cloth soaked in IP solvent (an ethanol-based solvent obtained from Showa Kako Co., Ltd.).

[0105] <Comparative Example 5> Optical sheets for evaluation were produced in the same manner as in Example 13, except that the amount of static electricity removing liquid applied was adjusted to control the surface resistivity of the surfaces of the release film and the surface protective film to the values ​​shown in Table 2. Note that the static electricity removing liquid was not applied to the surface protective film.

[0106] An evaluation of multiple production was carried out for the optical sheets for evaluation produced in the above-mentioned Examples 1 to 16 and Comparative Examples 1 to 5. The results are shown in Tables 1 and 2.

[0107] [Table 1]

[0108] [Table 2] [Industrial Applicability]

[0109] The present invention is useful because it can provide an optical sheet that is less likely to result in multiple optical sheets being taken out one by one from a laminate in which a plurality of optical sheets are stacked. [Explanation of symbols]

[0110] 1 Polarizing plate 2 Surface protection film 3 Release film 4. Marking 10 Optical Sheet 100 Optical sheet laminate

Claims

1. An optical sheet having a surface protective film, a polarizing plate, and a release film in this order, The coefficient of dynamic friction between the surface protective film and the release film is 0.4 or less; the release film has a marking on a surface opposite to the polarizing plate, The marking has a height of 0.5 μm or less from the film surface, The dynamic friction coefficient was measured by preparing a cut optical sheet to a size of 11 cm x 6.3 cm so as to include the portion having the marking, attaching each to a fixed jig connected to the movable stage and load cell of a measuring machine, arranging the two optical sheets so that the release film and the surface protection film face each other, applying a load of 500 g from above the overlapping films, and moving the optical sheets back and forth 100 times at a speed of 5,000 mm / min over a moving distance of 15.0 mm, and calculating the average dynamic friction coefficient from the magnitude of the force detected by the load cell during this process.

2. 2. The optical sheet according to claim 1, wherein the ratio of the area of ​​the marking to the area of ​​the release film is 5% or less.

3. 3. The optical sheet according to claim 1, wherein the surface of the polarizing plate facing the surface protective film has an arithmetic mean roughness Ra of 0.001 μm or more and 0.3 μm or less in accordance with JIS B 0601:2013.

4. 4. The optical sheet according to claim 1, wherein the surface of the release film opposite to the polarizing plate has a silicon atom content of 2% or more.

5. The surface of the surface protection film opposite to the polarizing plate has a surface resistivity of 1×10 7 ~1×10 12 Ω / □, The surface of the release film opposite to the polarizing plate has a surface resistivity of 1×10 7 ~1×10 12The optical sheet according to any one of claims 1 to 4, wherein the resistance is Ω / □.

Citation Information

Patent Citations

  • Antidazzle material and polarizing film using that

    JP1997127312A

  • Liquid crystal optical film and liquid crystal display element

    JP1998221685A

  • Polarizing plate

    JP2000081515A

  • Optical member

    JP2000321422A

  • Surface protective film

    JP2001305346A