Use of aryl-containing organopolysiloxane gums as additives to enhance rheological behavior
The use of an organopolysiloxane gum with aryl groups in curable silicone compositions addresses the need for improved yield stress and mechanical properties in 3D printable silicone elastomers, ensuring precise and deformation-free printing with enhanced mechanical strength.
Patent Information
- Application Number
- JP2022562576
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2020-04-15
- Filing Date
- 2021-04-14
- Publication Date
- 2024-10-08
- Estimated Expiration
- 2041-04-14
AI Technical Summary
There is a need to improve both the yield stress and mechanical properties of 3D printable silicone elastomer compositions for additive manufacturing, particularly in extrusion printing, to enhance shape retention and printing precision.
The use of an organopolysiloxane gum with a consistency of 200 to 900 containing aryl groups as a rheology modifier in curable silicone compositions for 3D printing, which includes a silicone base, a curing agent, and a filler, to achieve improved rheological properties and mechanical strength.
The method provides reduced viscosity under high shear rates for extrusion, stable rheology over time, and enhanced mechanical properties in 3D printed silicone elastomer parts, enabling precise printing without deformation and improved durometer range.
Smart Images

Figure 0007564235000013 
Figure 0007564235000014 
Figure 0007564235000015
Abstract
Description
[Technical field]
[0001] CROSS-REFERENCE TO RELATED APPLICATIONS This application is an international application filed under the Patent Cooperation Treaty, claiming priority to U.S. Provisional Patent Application No. 63 / 010,510, filed April 15, 2020, the contents of which are incorporated herein by reference in their entirety. The present invention relates to curable silicone compositions and their use in processes for the additive manufacturing of three-dimensional silicone elastomeric articles. [Background technology]
[0002] The selection of materials for additive manufacturing, and especially extrusion printing, requires consideration of their rheological properties. This is because these properties determine the extrusion pressure, shape retention after extrusion, and printing resolution. It is well known that the rheological behavior of viscoelastic materials as shear thinning, or more specifically, the yield stress properties, is a key parameter for the successful use of three-dimensional (3D) deposition techniques. Thus, when the yield stress reaches a sufficiently high value, the shape of the printed object is not only retained during and after deposition, but also during the polymerization process after printing.
[0003] Shear thinning properties are particularly desirable for extrusion, allowing for a reduction in viscosity at the high shear rates involved in extrusion, and an increase in viscosity after extrusion to maintain shape. Shear thinning is typically achieved by the addition of rheology modifiers, many of which are commercially available.
[0004] To provide an additive manufacturing method for producing 3D printed parts with siloxane-based elastomer compositions, WO 2017 / 081028 and WO 2017 / 121733 disclose the use of a rheological agent containing polar groups and selected from epoxy, polyether or polyester functional compounds. Additional rheological modifiers such as caprolactone, hydroxycaproic acid and polycarbonate polyols are also mentioned.
[0005] US Patent No. 5,036,131 discloses silicone dispersions with improved toughness and thixotropic properties that cure to elastomers on exposure to air. The silicone dispersions used therein are based on hydroxyl endblocked polydiorganosiloxanes, aluminum trihydrate, and a moisture-activated cure system. To obtain the thixotropic properties of the coating, the silicone dispersion must contain a siloxane (2) with hydroxyl endblocks and phenyl or 3,3,3-trifluoropropyl radicals in combination with untreated fumed silica. Summary of the Invention [Problem to be solved by the invention]
[0006] There remains a need to improve both the yield stress and mechanical properties of 3D printable silicone elastomer compositions. [Means for solving the problem]
[0007] As a result of extensive research, the present inventors have found that the above problems can be solved by using an organopolysiloxane gum having a consistency of 200 to 900 and containing an aryl group as a rheology modifier.
[0008] A method for additively manufacturing a silicone elastomeric article is provided, the method comprising the steps of: 1) printing a first curable silicone composition onto a substrate using a 3D printer selected from an extrusion 3D printer or a material jetting 3D printer to form a first layer; 2) printing a second curable silicone composition onto the first layer or a previous layer with the 3D printer to form a subsequent layer; 3) optionally repeating step 2) for any additional layers desired, using independently selected curable silicone compositions; 4) Crosslinking the first and subsequent layers, optionally by heating, to obtain a cured silicone elastomeric article. Includes; At least one layer of the curable silicone composition is a curable silicone composition X, the curable silicone composition X comprising: (A) a silicone base containing an organosilicon component that cures via an addition cure, condensation cure, or peroxide cure reaction, respectively; (D) a curing agent capable of curing the silicone base, which is an addition catalyst, a condensation catalyst, or a peroxide curing compound, respectively; (C) at least one organopolysiloxane gum C having a consistency of 200 to 900 at 25° C., and at least one silicon-bonded C6-C 12 Organopolysiloxane gum C containing aryl groups and containing at least one functional group per molecule selected from the group consisting of silicon-bonded C2 to C 20 alkenyl groups, silicon-bonded hydrogen atoms, silicon-bonded hydroxyl groups, silicon-bonded alkoxy groups, silicon-bonded oxime groups, silicon-bonded amino groups, silicon-bonded amido groups, silicon-bonded aminoxy groups, silicon-bonded acyloxy groups, silicon-bonded ketiminoxy groups, and silicon-bonded enoxy groups; and (E) at least one filler E Includes.
[0009] In some embodiments, a method for additively manufacturing a silicone elastomeric article is provided, wherein the curable silicone composition X is an addition-curable liquid silicone composition X, the addition-curable liquid silicone composition X comprising: (A) At least two silicon bonds C2 to C per molecule 20 at least one organopolysiloxane A containing alkenyl groups; (B) at least one organosilicon crosslinker B containing at least two silicon-bonded hydrogen atoms per molecule; (C) at least one organopolysiloxane gum C having a consistency of 200 to 900 at 25 ° C., and at least one silicon bond C2 to C3 per molecule 20 Alkenyl group and at least one silicon bond C6-C per molecule 12at least one organopolysiloxane gum C containing aryl groups; (D) at least one addition reaction catalyst D; (E) at least one filler E; (F) optionally, at least one diorganohydrogensiloxy-terminated diorganopolysiloxane chain extender F; (G) optionally, at least one cure rate modifier G; (H) optionally, at least one silicone resin H; and (I) Optionally, at least one additive I.
[0010] In some embodiments, a method for additively manufacturing a silicone elastomeric article is provided, wherein the 3D printer is an extrusion 3D printer.
[0011] Silicone elastomeric articles made by the methods of the present invention are also provided.
[0012] Also provided is an addition-curable liquid silicone composition X for additively manufacturing silicone elastomeric articles, said addition-curable liquid silicone composition X comprising: (A) At least two silicon bonds C2 to C per molecule 20 at least one organopolysiloxane A containing alkenyl groups; (B) at least one organosilicon crosslinker B containing at least two silicon-bonded hydrogen atoms per molecule; (C) at least one organopolysiloxane gum C having a consistency of 200 to 900 at 25 ° C., and at least one silicon bond C2 to C3 per molecule 20 Alkenyl group and at least one silicon bond C6-C per molecule 12 at least one organopolysiloxane gum C containing aryl groups; (D) at least one addition reaction catalyst D; (E) at least one filler E; (F) optionally, at least one diorganohydrogensiloxy-terminated diorganopolysiloxane chain extender F; (G) optionally, at least one cure rate modifier G; (H) optionally, at least one silicone resin H; and (I) Optionally, at least one additive I.
[0013] In some embodiments, at least two silicon bonds C2-C 20 The at least one organopolysiloxane A containing alkenyl groups has the following formula (1): [ka] During the ceremony, -n is an integer in the range of 1 to 1000, -R is independently C1-C such as methyl, ethyl, propyl, etc. 20 C6-C alkyl groups, such as xylyl, tolyl, or phenyl groups 12 C2-C such as aryl groups, vinyl, allyl, hexenyl, decenyl, or tetradecenyl groups 20 alkenyl groups, preferably methyl groups; -R' is independently a C2-C alkyl group such as vinyl, allyl, hexenyl, decenyl, or tetradecenyl group. 20 alkenyl groups, preferably vinyl groups; -R" is independently a C1-C alkyl group such as methyl, ethyl, or propyl. 20 C6-C alkyl groups, such as xylyl, tolyl, or phenyl groups 12 It is independently selected from aryl groups, and is preferably a methyl group.
[0014] In some embodiments, the at least one organosilicon crosslinker B, which contains at least two silicon-bonded hydrogen atoms per molecule, is (i) at least two, preferably 3 to 60, siloxy units of the same or different formula (XL-1): (H)(Z)e SiO (3-e) / 2 (XL-1) During the ceremony, - The symbol H represents a hydrogen atom, the symbol Z represents an alkyl group containing 1 to 8 carbon atoms; the symbol e is equal to 0, 1 or 2; and (ii) at least one, preferably 1 to 550, more preferably 1 to 250, siloxy units of formula (XL-2): (Z) g SiO (4-g) / 2 (XL-2) During the ceremony, - the symbol Z is an alkyl group having 1 to 8 carbon atoms, or a C6 to C6 alkyl group such as a xylyl, tolyl or phenyl group; 12 represents an aryl group, - the symbol g is equal to 0, 1, 2 or 3; Including, Z in XL-1 and XL-2 may be the same or different.
[0015] In some embodiments, at least one silicon bond C2-C 20 Alkenyl group and at least one silicon bond C6-C per molecule 12 Said at least one organopolysiloxane gum C containing aryl groups comprises: at least one siloxy unit of formula (A-3): (Alk)(R) h SiO (3-h) / 2 (A-3) In the formula, the symbol "Alk" represents a C2-C alkyl group such as vinyl, allyl, hexenyl, decenyl, or tetradecenyl. 20 Represents an alkenyl group, and the symbol R is a C1-C alkyl group such as methyl, ethyl, propyl, or the like. 20 C6-C alkyl, xylyl, tolyl, or phenyl groups 12 represents an aryl group, in which "Alk" and R in each case may be the same or different, h=1 or 2; at least one siloxy unit of formula (A-4): (Ar) k (R 1 ) h SiO (4-h-k) / 2 (A-4) In the formula, the symbol "Ar" is C6-C 12 Aryl groups (optionally C2-C such as xylyl, tolyl, xylene, or phenyl groups) 20 substituted by an alkylene group), or C1-C 20 Aralkyl (optionally C2 to C 20 alkylene group), or naphthyl group (optionally C1-C 20 Alkyl group and / or C2-C 20 alkylene group), or anthracenyl group (optionally C1-C 20 Alkyl group and / or C2-C 20 substituted with an alkylene group), preferably a phenyl group, and the symbol R 1 is a C1-C group such as a methyl, ethyl, or propyl group. 20 C2-C alkyl groups, such as vinyl, allyl, hexenyl, decenyl, or tetradecenyl groups 20 In each case, "Ar" and R represent an alkenyl group. 1 may be the same or different, h=0, 1 or 2; k=1 or 2 and h+k=1, 2, or 3; Other siloxy units of formula (A-2): (L) g SiO (4-g) / 2 (A-2) In the formula, the symbol L is a C1-C aryl such as methyl, ethyl, or propyl. 20 where the symbol g is equal to 0, 1, 2, or 3, and in each occurrence L may be the same or different.
[0016] In some embodiments, the at least one organopolysiloxane gum C is a diphenylsiloxane-dimethylsiloxane-vinylmethylsiloxane copolymer gum.
[0017] In some embodiments, the at least one organopolysiloxane gum C is vinyl terminated.
[0018] In some embodiments, the at least one organopolysiloxane gum C comprises less than 30 mol % of aryl groups. For example, the at least one organopolysiloxane gum C may comprise from about 10 mol % to about 20 mol % of aryl groups.
[0019] In some embodiments, the catalyst D is a platinum group metal-containing catalyst.
[0020] In some embodiments, the at least one filler E is a fumed silica that has been treated with at least one compatibilizer in the presence of at least a portion of the at least one organopolysiloxane A having alkenyl groups.
[0021] There is also provided the use of the addition-curable liquid silicone composition X in a 3D printer, such as an extrusion 3D printer or a material-jetting 3D printer. [Brief description of the drawings]
[0022] [Figure 1] 1A-1F provide representative photographs of 3D printed silicone elastomers. FIG. 1A is a photograph of a 3D printed comparative silicone elastomer without organopolysiloxane gum. FIG. 1B-1F show the effect of reducing the amount of aryl group-containing organopolysiloxane gum in the curable liquid silicone composition on 3D printability. FIG. 1B-1F are photographs of 3D printed silicone elastomers with 20% (FIG. 1B), 15% (FIG. 1C), 10% (FIG. 1D), 5% (FIG. 1E), and 0% (FIG. 1F) aryl group-containing organopolysiloxane gum. [Diagram 2] FIG. 2 shows a graph depicting the rheological properties of addition-curable liquid silicone compositions containing various organopolysiloxane gums. [Diagram 3]FIG. 3 shows a graph depicting the rheological properties of addition-curable liquid silicone compositions containing various concentrations of aryl-containing organopolysiloxane gum. [Figure 4] FIG. 4 shows a graph depicting the rheological properties of addition-curable liquid silicone compositions containing various types of aryl-containing organopolysiloxanes. [Diagram 5] Figures 5A-5C provide representative photographs of 3D printed silicone elastomers. Figure 5A is a photograph of a comparative 3D printed silicone elastomer containing an aryl group-containing low viscosity organopolysiloxane oil. Figures 5B and 5C are photographs of exemplary 3D printed silicone elastomers containing an aryl group-containing organopolysiloxane gum. [Figure 6] 6A and 6B show graphs illustrating the thixotropic properties of organopolysiloxane gums on both linear (FIG. 6A) and logarithmic (FIG. 6B) scales. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0023] Before the present disclosure is further described, it should be understood that the present disclosure is not limited to the specific embodiments of the present disclosure described below. Variations of the specific embodiments may be made and still fall within the scope of the appended claims. It should also be understood that the terms used are for the purpose of describing the specific embodiments and are not intended to be limiting. Instead, the scope of the present disclosure is established by the appended claims.
[0024] As used in this specification and the appended claims, the singular forms "a," "an," and "the" include plural references unless the context clearly dictates otherwise. Unless defined otherwise, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which this disclosure belongs.
[0025] As used herein, the term "silicone rubber" includes the crosslinked product of any crosslinkable silicone composition. The terms "silicone rubber" and "silicone elastomer" can be used interchangeably.
[0026] As used herein, the terms "crosslinked" and "cured" may be used interchangeably and refer to the reaction that occurs when the components of the curable silicone composition are combined and reacted to result in a cured silicone elastomer.
[0027] The term "alkenyl" as used herein is understood to mean a substituted or unsubstituted, unsaturated, linear or branched hydrocarbon chain having at least one olefinic double bond, more preferably a single double bond. Preferably, the "alkenyl" group has 2 to 10 carbon atoms, more preferably 2 to 6 carbon atoms. This hydrocarbon chain optionally contains at least one heteroatom, such as O, N, S. Preferred examples of "alkenyl" groups are vinyl, allyl and homoallyl groups, with vinyl being particularly preferred.
[0028] As used herein, "alkyl" refers to a saturated, straight or branched, optionally substituted (e.g., with one or more alkyl) hydrocarbon chain, preferably having 1 to 10 carbon atoms, such as 1 to 8 carbon atoms, more preferably 1 to 4 carbon atoms. Examples of alkyl groups are methyl, ethyl, isopropyl, n-propyl, tert-butyl, isobutyl, n-butyl, n-pentyl, isoamyl, and 1,1-dimethylpropyl, among others.
[0029] As used herein, "aryl" refers to an aryl group having 6 to 12 carbon atoms, optionally substituted with an alkyl group having 1 to 30 carbon atoms.
[0030] In one aspect, the present invention is a method for additively manufacturing a silicone elastomeric article, said method comprising the steps of: Steps below: 1) printing a first curable silicone composition onto a substrate using a 3D printer selected from an extrusion 3D printer or a material jetting 3D printer to form a first layer; 2) printing a second curable silicone composition onto the first layer or a previous layer with the 3D printer to form a subsequent layer; 3) optionally repeating step 2) for any additional layers desired, using independently selected curable silicone compositions; 4) Crosslinking the first and subsequent layers, optionally by heating, to obtain a cured silicone elastomeric article. Includes; At least one layer of the curable silicone composition is a curable silicone composition X, the curable silicone composition X comprising: (A) a silicone base containing an organosilicon component that cures via an addition cure, condensation cure, or peroxide cure reaction, respectively; (D) a curing agent capable of curing the silicone base, which is an addition catalyst, a condensation catalyst, or a peroxide curing compound, respectively; (C) at least one organopolysiloxane gum C having a consistency of 200 to 900 at 25° C., and at least one silicon-bonded C6-C 12 Organopolysiloxane gum C containing aryl groups and containing at least one functional group per molecule selected from the group consisting of silicon-bonded C2 to C 20 alkenyl groups, silicon-bonded hydrogen atoms, silicon-bonded hydroxyl groups, silicon-bonded alkoxy groups, silicon-bonded oxime groups, silicon-bonded amino groups, silicon-bonded amido groups, silicon-bonded aminoxy groups, silicon-bonded acyloxy groups, silicon-bonded ketiminoxy groups, and silicon-bonded enoxy groups; (E) at least one filler E Includes.
[0031] The inventors have surprisingly found that the use of the curable silicone composition X as defined herein provides an efficient additive manufacturing method for the production of 3D printed parts. In particular, the use of the curable silicone composition X of the present invention in 3D printing applications provides the following advantages: -Enabling a reduction in viscosity under high shear rates associated with extrusion and a high viscosity after extrusion to maintain shape; - Providing a stable composition whose rheology does not change over time (there is no accumulation of thixotropic effects due to hydrogen bonds created between polar additives and the silica surface). Providing the ability to not change the input 3D process parameters regardless of the age of the composition, -Enabling the 3D printing of silicone elastomer parts with great precision at room temperature without layer collapse or deformation before curing; - 3D elastomeric parts with improved mechanical properties, especially in the high durometer range, are obtained.
[0032] Curable silicone compositions are well known in the art and include silicone compositions that cure by three types of reactions: peroxide cure, addition cure, or condensation cure reactions.
[0033] In a preferred embodiment, the selection of the functional groups of the organopolysiloxane gum C can be carried out as follows: -Silicon bond C2~C 20 The alkenyl groups and silicon-bonded hydrogen atoms are preferably selected for compositions that cure by addition cure, -Silicon bond C2~C 20 is preferably selected for compositions that cure by peroxide cure, Silicon-bonded hydroxyl groups, silicon-bonded alkoxy groups, silicon-bonded oxime groups, silicon-bonded amino groups, silicon-bonded amide groups, silicon-bonded aminoxy groups, silicon-bonded acyloxy groups, silicon-bonded ketiminoxy groups and silicon-bonded enoxy groups are preferably selected for compositions that cure via a condensation cure reaction.
[0034] Curable silicone compositions are classified according to the curing method used, the curing temperature conditions, and the consistency or viscosity of the curable silicone composition, as follows: · HCR (High Consistency Silicone Rubbers) are heat curable silicone compositions (HTV, an acronym for High Temperature Vulcanizing silicone composition) whose components cure by addition cure or peroxide cure reactions. They are prepared from reactive silicone gums that contain high molecular weight polymers containing various reactive groups. · LSR (Liquid Silicone Rubbers) are heat cured silicone compositions (or high temperature vulcanization, HTV) that use an addition cure catalyst and are sold as two-part systems. The main difference between Liquid Silicone Rubber (LSR) and High Consistency Rubber (HCR) is the "flowable" or "liquid" nature of the LSR material. · RTV (Room Temperature Vulcanizing) are curable silicone compositions that use either an addition cure catalyst or a condensation cure catalyst. They are sold as single or two-component systems that cure from room temperature when using a condensation cure catalyst up to 200°C when using an addition cure catalyst.
[0035] Curable compositions that cure by peroxide cure are achieved by using organic peroxides that decompose at high temperatures to form highly peroxo-reactive radicals that react with silicone polymers containing alkenyl (e.g. vinyl) or alkyl groups. The organic peroxides used for curing are classified into alkenyl-specific peroxides (I) and non-alkenyl-specific peroxides (II). The first class cannot crosslink polydimethylsiloxanes (PDMS), which do not have alkenyl groups, while the second class can crosslink all types of PDMS. The following groups of peroxides are available: · Alkenyl group specific peroxides: diaroyl peroxides, · Non-specific peroxides of alkenyl groups: dialkyl peroxides, diaralkyl peroxides), alkylaroyl peroxides and alkylaryl peroxides, or mixtures of different groups. Useful peroxides are di(2,4-dichlorobenzoyl) peroxide (belonging to the group of diaroyl peroxides), dicumyl peroxide, 2,5-dimethyl-2,5-di-t-butylperoxyhexane and bis(dichlorobenzoyl) peroxide.
[0036] Curable compositions that cure by condensation cure reactions are referred to as curable silicone compositions. Here, cure is achieved by reaction between silanol groups (Si-OH) and / or hydrolyzable Si-X groups (X is a hydrolyzable group) of siloxane polymers or silanes in the presence of moisture, which leads to the formation of siloxane (Si-O-Si) bonds and hydrogen gas or water. Condensation cure silicone systems are usually cured with organotin compounds and / or titanates. Other catalysts may be mentioned, such as catalysts based on zinc, zirconium, aluminum, or amines such as guanidine derivatives. Classically, these formulations contain hydroxyl-terminated silicone oils, such as α,ω-(hydroxydimethylsilyl)-polydimethylsiloxanes (optionally pre-functionalized with silanes to have hydrolyzable and condensable ends), crosslinkers, polycondensation catalysts, classically tin salts or alkyl titanates, and optionally various fillers and additives depending on the intended end use.
[0037] These silicone compositions cure by polymerization and / or crosslinking at ambient temperature (which may vary between 5° and 30° C. depending on the region) and, as is well known to those skilled in the art, are classified into two distinct groups: Compositions packaged as "single-component" compositions (RTV-1), which are in the form of a single part (or component) in an airtight package; and Compositions packaged as "two-component" compositions (RTV-2), which are in the form of two separate parts (hence the name "two-component"), the packaging containing the catalyst being airtight.
[0038] The purpose of the airtight packaging is to prevent silicone compositions containing a catalyst from coming into contact with atmospheric moisture during storage prior to use. During the curing, which is accomplished by polymerization and / or crosslinking of these silicone compositions, in the case of RTV-1 compositions, water is provided by atmospheric moisture. In the case of RTV-2 compositions, dimethyltin dicarboxylate is commonly used as the catalyst, but it may be necessary to add some water to one of the parts to activate the catalyst and enable the polycondensation reaction when the contents of the two parts are mixed with the surrounding air to form the elastomeric network that leads to the curing of the composition.
[0039] For example, a single-component silicone composition (RTV-1) used as a mastic or adhesive undergoes low-temperature crosslinking by a mechanism involving two main reactions, which can be sequential or simultaneous: 1. Functionalization reactions resulting from contacting silicone oils having silanol functional groups, such as hydroxyl-terminated silicone oils (such as α,ω-(hydroxydimethylsilyl)-polydimethylsiloxanes), with crosslinkers (such as silanes of type SiX4) (for example silicates) or compounds having the following functional groups -SiX3 (X is most often an alkoxy, acyloxy, amino, amido, enoxy, aminoxy, ketiminoxy or oxime functional group). These functional groups are well known to react with silanol functional groups. The products obtained are most often called "functionalized oils". This reaction may be desired directly during the preparation of the composition (in situ functionalization) or, optionally, as a preliminary step before adding the other components of the composition. In this preliminary step, it is common to use functionalization catalysts such as lithia (or lithium hydroxide) or potash in order to give the single-component compositions good storage stability. For this purpose, the skilled person is able to select a specific functionalization catalyst and to adjust the amounts of reactants so as to have a molar excess of crosslinker relative to the silanol functional groups to be functionalized. 2. Crosslinking, generally by hydrolysis of the functionalized oil by water vapor diffusing into the material from the surface exposed to the atmosphere, and condensation between the silanol groups formed and other residual reactive functional groups.
[0040] For compositions packaged in the form of a two-component composition (RTV-2), the first component (or part) contains the polycondensable polyorganosiloxane and the second component (or part), which is airtight, contains the catalyst and one or more crosslinking agents. The two components (or parts) are mixed at the time of use and the mixture cures by crosslinking reaction in the form of a relatively hard elastomer, especially if the composition contains reinforcing fillers. These compositions packaged in two-component systems are well known and are described in particular in the work "Chemistry and Technology of Silicones" by Walter Noll (1968, 2nd edition, pages 395-398). These compositions most often contain the following components: reactive polyorganosiloxanes which contain silanol groups at the ends of the chain (e.g. α,ω-di(hydroxydimethylsilyl) (polydimethylsiloxane)), in the chain, or both at the ends and in the chain; · Crosslinking agents; Condensation catalysts; and Optionally, water is often present when a dialkyltin dicarboxylate is used as a catalyst, water acting as an activator for said catalyst.
[0041] Suitable catalysts are tin derivatives, such as alkyltin-based compounds, such as dibutyltin dilaurate (DBTDL). Alternative catalysts, in particular titanium-based catalysts, are known in the prior art (see, for example, WO 2013 / 036546). Other catalysts are mentioned, such as catalysts based on zinc, scandium, ytterbium, copper, silver, cerium, molybdenum, bismuth, hafnium or guanidine derivatives. The use of zirconium or titanium chelates is described in particular in WO 01 / 49789. Other alternatives that can be used as catalysts are described in French patent application 2856694 or US patent application 2017 / 022325.
[0042] A curable silicone composition that cures by an addition cure reaction refers to a composition in which the cure is achieved by a reaction called "addition reaction" (or hydrosilation reaction) between the silicon hydride group (Si-H) of the siloxane polymer and the silicon alkenyl (Si-alkenyl) or silicon alkynyl (Si-alkynyl) group of the siloxane polymer, forming an alkyl bridge between the two siloxane polymers. Metals belonging to the platinum group are suitable as catalysts for the addition cure reaction. Examples of suitable catalysts are platinum or rhodium compounds, germanium compounds, as described in WO 2016 / 075414, or nickel, cobalt or iron complexes, as described in WO 2016 / 071651, WO 2016 / 071652 and WO 2016 / 071654. The most commonly used catalysts are usually complexes of platinum in alcohols, xylenes, divinyl siloxanes, or cyclic vinyl siloxanes. One advantage of addition-curable silicone compositions is that the reaction is free of by-products and proceeds quickly.
[0043] All of the above standard curable compositions familiar to those skilled in the art are suitable according to the invention, taking into account the addition of: (A) at least one organopolysiloxane gum C having a consistency of 200 to 900 at 25° C., and at least one silicon-bonded C6-C 12 Organopolysiloxane gum C containing aryl groups and containing at least one functional group per molecule selected from the group consisting of silicon-bonded C2 to C 20 alkenyl groups, silicon-bonded hydrogen atoms, silicon-bonded hydroxyl groups, silicon-bonded alkoxy groups, silicon-bonded oxime groups, silicon-bonded amino groups, silicon-bonded amido groups, silicon-bonded aminoxy groups, silicon-bonded acyloxy groups, silicon-bonded ketiminoxy groups, and silicon-bonded enoxy groups; (E) at least one filler E, as defined below.
[0044] Examples of functional groups in condensation curable silicone compositions are as follows: Hydrolyzable and condensable groups of the alkoxy type can be used, such as groups having 1 to 8 carbon atoms, such as methoxy, ethoxy, n-propoxy, isopropoxy, n-butoxy, isobutoxy, sec-butoxy, tert-butoxy, 2-methoxyethoxy, hexyloxy or octyloxy groups. Hydrolyzable and condensable groups of the alkoxyalkyleneoxy type can be used, for example the methoxy-ethylene-oxy group. Hydrolysable and condensable groups of the amino type can be used, such as methylamino, dimethylamino, diethylamino, n-butylamino, sec-butylamino or cyclohexylamino groups. ·N-Methylacetamide group is a hydrolyzable and condensable group. Hydrolyzable and condensable groups of the acylamino type can be used, for example the benzoylamino group. Aminoxy-type hydrolyzable and condensable groups can be used, including, for example, dimethylaminooxy, diethylaminooxy, dioctylaminooxy or diphenylaminooxy groups. Hydrolyzable and condensable groups of the iminoxy and especially ketiminoxy type can be used. Examples include groups derived from the following oximes: acetophenone oxime, acetone oxime, benzophenone oxime, methyl ethyl ketoxime, diisopropyl ketoxime or methyl isobutyl ketoxime. Hydrolyzable and condensable groups of the acyloxy type can be used, for example the acetoxy group. Hydrolyzable and condensable groups of the enoxy type can be used, for example the 2-propenoxy group.
[0045] The consistency of gum C is 200 to 900 at 25°C, preferably 300 to 900 at 25°C, or 450 to 750 at 25°C.
[0046] The consistency can be determined, for example, by measuring the penetration using a penetrometer according to one of the AFNOR standards NFT 60119 or NFT 60123. Standard NFT 60123 is particularly suitable for this description.
[0047] The term "gum" is usually used for organosilicate compounds with a viscosity above 600,000 mPa·s (which corresponds to a molecular weight of 200,000 g / mol or more). Gum hardness is measured at 25 °C by a penetrometer of PNR12 or equivalent model, which allows applying a cylindrical head to the sample under standardized conditions. The hardness of the gum is expressed as 10 times the depth (in mm) that the shape memory cylinder penetrates into the sample in 1 minute. To do this, the gum sample is placed in an aluminium container with a diameter of 40 mm and a height of 60 mm. A bronze or brass cylindrical head with a diameter of 6.35 mm and a height of 4.76 mm is attached to a metal rod with a length of 51 mm and a diameter of 3 mm suitable for the penetrometer. A load of 100 g is attached to this rod. The total weight of the assembly is 151.8 g. The gum sample container is placed in a bath set at 25 °C ± 0.5 °C for a minimum of 30 seconds. The measurement is carried out according to the manufacturer's instructions.
[0048] The viscosity of gum C is 0.01s at 25°C. -1 In some embodiments, the viscosity of Gum C is greater than 10 million mPa s at 25° C., as measured at a shear rate of 0.01 s. -1 In some embodiments, the viscosity of Gum C is greater than 0.01 s at 25° C. -1 In some embodiments, the viscosity of Gum C is greater than 0.01 s at 25° C. -1 is greater than 60 million mPa s, measured at a shear rate of
[0049] The viscosity of the gum was measured using an Anton Paar type rheometer or a zero gap set between two plateaus of 0.300 mm and a viscosity of 0.01 s at 25.0 °C. -1 ~100s -1The viscosity of the gum can be measured using an equivalent rheometer with a shear rate range between 0.01 s at 25° C. -1 The shear rate is measured.
[0050] In some embodiments, the at least one organopolysiloxane gum C comprises: At least one siloxy unit of formula (A-3): (Alk)(R) h SiO (3-h) / 2 (A-3) In the formula, the symbol "Alk" represents a C2-C alkyl group such as vinyl, allyl, hexenyl, decenyl, or tetradecenyl. 20 Represents an alkenyl group, and the symbol R is a C1-C alkyl group such as methyl, ethyl, propyl, or the like. 20 C6-C alkyl groups, such as xylyl, tolyl, or phenyl groups 12 represents an aryl group, in which "Alk" and R in each case may be the same or different, h=1 or 2; At least one siloxy unit of formula (A-4): (Ar) k (R 1 ) h SiO (4-h-k) / 2 (A-4) In the formula, the symbol "Ar" is C6-C 12 Aryl groups (optionally C2-C such as xylyl, tolyl, xylene, or phenyl groups) 20 substituted by an alkylene group), or C1-C 20 Aralkyl (optionally C2 to C 20 alkylene group), or naphthyl group (optionally C1-C 20 Alkyl group and / or C2-C 20 alkylene group), or anthracenyl group (optionally C1-C 20 Alkyl group and / or C2-C 20 substituted with an alkylene group), preferably a phenyl group, and the symbol R 1 is a C1-C group such as a methyl, ethyl, or propyl group. 20C2-C alkyl groups, such as vinyl, allyl, hexenyl, decenyl, or tetradecenyl groups 20 In each case, "Ar" and R represent an alkenyl group. 1 may be the same or different, h=0, 1 or 2; k=1 or 2 and h+k=1, 2, or 3; Other siloxy units of formula (A-2): (L) g SiO (4-g) / 2 (A-2) In the formula, the symbol L is a C1-C aryl such as methyl, ethyl, or propyl. 20 where the symbol g is equal to 0, 1, 2, or 3, and in each occurrence L may be the same or different.
[0051] In a preferred embodiment, the at least one organopolysiloxane gum C comprises: At least one siloxy unit of formula (A-3): (Alk)(R) h SiO (3-h) / 2 (A-3) In the formula, the symbol "Alk" represents a vinyl group, and the symbol R represents a C1-C alkyl group such as methyl, ethyl, or propyl. 20 represents an alkyl group, in which "Alk" and R in each case may be the same or different, h=1 or 2; At least one siloxy unit of formula (A-4): (Ar) k (R 1 ) h SiO (4-h-k) / 2 (A-4) In the formula, the symbol "Ar" represents a phenyl group, and the symbol R 1 is a C1-C group such as a methyl, ethyl, or propyl group. 20 C2-C alkyl groups, such as vinyl, allyl, hexenyl, decenyl, or tetradecenyl groups 20 In each case, "Ar" and R represent an alkenyl group. 1 may be the same or different, h=0 or 1, k=2; Other siloxy units of formula (A-2): (L) g SiO (4-g) / 2 (A-2) In the formula, the symbol L is a C1-C aryl such as methyl, ethyl, or propyl. 20 where the symbol g is equal to 0, 1, 2, or 3, and in each occurrence L may be the same or different.
[0052] In some embodiments, the at least one organopolysiloxane gum C is a diphenylsiloxane-dimethylsiloxane-vinylmethylsiloxane copolymer gum.
[0053] In some embodiments, at least one organopolysiloxane gum C is vinyl terminated.
[0054] In some embodiments, at least one organopolysiloxane gum C comprises less than 30 mol% aryl groups. For example, at least one organopolysiloxane gum C comprises less than 28 mol% aryl groups, less than 26 mol% aryl groups, less than 24 mol% aryl groups, less than 22 mol% aryl groups, less than 20 mol% aryl groups, less than 19 mol% aryl groups, less than 18 mol% aryl groups, less than 17 mol% aryl groups, less than 16 mol% aryl groups, less than 15 mol% aryl groups, less than 14 mol% aryl groups, less than 13 mol% aryl groups, less than 12 mol% aryl groups, less than 11 mol% aryl groups, less than 10 mol% aryl groups, less than 9 mol% aryl groups, less than 8 mol% aryl groups, less than 7 mol% aryl groups, less than 6 mol% aryl groups, less than 5 mol% aryl groups, less than 4 mol% aryl groups, less than 3 mol% aryl groups, less than 2 mol% aryl groups, or less than 1 mol% aryl groups.
[0055] In some embodiments, at least one organopolysiloxane gum C comprises about 1 mol % to about 28 mol % of aryl groups. In some embodiments, at least one organopolysiloxane gum C comprises about 2 mol % to about 28 mol % of aryl groups, about 3 mol % to about 28 mol % of aryl groups, about 4 mol % to about 28 mol % of aryl groups, about 5 mol % to about 28 mol % of aryl groups, about 6 mol % to about 28 mol % of aryl groups, about 7 mol % to about 28 mol % of aryl groups, about 8 mol % to about 28 mol % of aryl groups, about 9 mol % to about 28 mol % of aryl groups, about 10 mol % to about 28 mol % of aryl groups, about 11 mol % to about 28 mol % of aryl groups, about 12 mol % to about 28 mol % of aryl groups, about 13 mol % to about 28 mol % of aryl groups, about 14 mol % to about 28 mol % of aryl groups, about 15 mol % to about 28 mol % of aryl groups, about 16 mol % to about 28 mol % of aryl groups, about 17 mol % to about 28 mol % of aryl groups, about 18 mol % to about 28 mol % of aryl groups, about 19 mol % to about 28 mol % of aryl groups, about 20 mol % to about 28 mol % of aryl groups, about 21 mol % to about 28 mol % of aryl groups, about 22 mol % to about 28 mol % of aryl groups, about 23 28 mol % aryl groups, about 14 mol % to about 28 mol % aryl groups, about 15 mol % to about 28 mol % aryl groups, about 16 mol % to about 28 mol % aryl groups, about 17 mol % to about 28 mol % aryl groups, about 18 mol % to about 28 mol % aryl groups, about 19 mol % to about 28 mol % aryl groups, about 20 mol % to about 28 mol % aryl groups, about 21 mol % to about 28 mol % aryl groups, about 22 mol % to about 28 mol % aryl groups, about 23 mol % to about 28 mol % aryl groups, about 24 mol % to about 28 mol % aryl groups, or about 25 mol % to about 28 mol % aryl groups.
[0056] In some embodiments, at least one organopolysiloxane gum C comprises from about 1 mol % to about 26 mol % aryl groups, from about 1 mol % to about 24 mol % aryl groups, from about 1 mol % to about 22 mol % aryl groups, from about 1 mol % to about 20 mol % aryl groups, from about 1 mol % to about 19 mol % aryl groups, from about 1 mol % to about 18 mol % aryl groups, from about 1 mol % to about 17 mol % aryl groups, from about 1 mol % to about 16 mol % aryl groups, from about 1 mol % to about 15 mol % aryl groups, from about 1 mol % to about 14 mol % aryl groups, aryl groups, about 1 mol % to about 13 mol % aryl groups, about 1 mol % to about 12 mol % aryl groups, or about 1 mol % to about 11 mol % aryl groups, from about 1 mol % aryl groups, about 1 mol % to about 9 mol % aryl groups, about 1 mol % to about 8 mol % aryl groups, about 1 mol % to about 7 mol % aryl groups, about 1 mol % to about 6 mol % aryl groups, about 1 mol % to about 5 mol % aryl groups, about 1 mol % to about 4 mol % aryl groups, about 1 mol % to about 3 mol % aryl groups, or about 1 mol % to about 2 mol % aryl groups.
[0057] In some embodiments, at least one organopolysiloxane gum C contains about 10 mol % to about 20 mol % aryl groups, about 10 mol % to about 19 mol % aryl groups, about 10 mol % to about 18 mol % aryl groups, about 10 mol % to about 17 mol % aryl groups, about 10 mol % to about 16 mol % aryl groups, about 10 mol % to about 15 mol % aryl groups, about 10 mol % to about 14 mol % aryl groups, about 10 mol % to about 13 mol % aryl groups, or about 10 mol % to about 12 mol % aryl groups.
[0058] In some embodiments, at least one organopolysiloxane gum C contains about 2 mol % to about 14 mol % aryl groups, about 3 mol % to about 14 mol % aryl groups, about 4 mol % to about 14 mol % aryl groups, about 5 mol % to about 14 mol % aryl groups, about 6 mol % to about 14 mol % aryl groups, about 7 mol % to about 14 mol % aryl groups, about 8 mol % to about 14 mol % aryl groups, about 8 mol % to about 12 mol % aryl groups, or about 10 mol % to about 14 mol % aryl groups.
[0059] The at least one filler E may be one or more of reinforcing fillers, semi-reinforcing fillers, non-reinforcing fillers, filled mineral fillers, thermally conductive fillers, electrically conductive fillers, and mixtures thereof.
[0060] In some embodiments, the reinforcing filler is selected from silica and / or alumina, preferably silica.
[0061] As usable silicas, fillers are envisaged that are characterised by a fine particle size, often below 0.1 μm, and a high ratio of specific surface area to weight (generally within the range of about 50 square meters per gram to more than 300 square meters per gram). This type of silica is a commercially available product and is well known in the field of manufacturing adhesive silicone compositions. These silicas can be colloidal silicas, silicas prepared by pyrolysis (silicas called combustion or fumed silicas) or wet processes (precipitated silicas) of mixtures of these silicas.
[0062] The chemical nature and method of preparation of the silica that can form filler E is not critical for the purposes of the present invention, so long as the silica is capable of exerting a reinforcing effect on the final composition. Of course, various cuts of silica can also be used.
[0063] These silica powders generally have an average particle size close to or equal to 0.1 μm and a mean particle size of 50 μm. 2 / g, preferably 50 to 400m 2 / g, especially between 150 and 350m 2 / g.
[0064] These silicas are optional: It is pretreated with the aid of at least one compatibilizer selected from a group of molecules that meet at least two criteria: Has high interaction with silica in the area of hydrogen bonding with itself and with the surrounding silicone oil; As such, or their decomposition products, they are easily removed from the final mixture by heating under vacuum in a gas stream; low molecular weight compounds are preferred; and / or In a specific manner with the aid of at least one untreated silica, and / or in a complementary manner by using at least one compatibilizer of similar nature to those defined above, which can be used in the pretreatment, It is processed on site.
[0065] In-situ treatment of the silica filler is understood to mean placing the filler and the compatibilizer in the presence of at least a portion of the predominant silicone polymer referred to above.
[0066] The compatibilizer is selected according to the treatment method (pre-treatment or in situ) and may be selected, for example, from the group comprising: Chlorosilanes, Polyorganocyclosiloxanes such as octamethylcyclosiloxane (D4); Silazane, preferably disilazane, or mixtures thereof, hexamethyldisilazane (HMDZ) is a preferred silazane, which can be combined with divinyltetramethyldisilazane; a polyorganosiloxane having one or more silicon-bonded hydroxyl groups per molecule; an amine such as ammonia or a low molecular weight alkylamine such as diethylamine; low molecular weight organic acids such as formic acid and acetic acid, and mixtures thereof.
[0067] For in situ treatments, the compatibilizer is preferably used in the presence of water.
[0068] For further details in this respect, reference may be made, for example, to French Patent No. 2 764 894.
[0069] As a variant, it is possible to use prior art compatibilization methods which provide for early treatment with silazanes (for example FR 2 320 324) or delayed treatment (for example EP 462 032).
[0070] As reinforcing aluminas that can be used as filler E, highly dispersible aluminas are advantageously used, doped or not doped in a known manner. Of course, it is also possible to use different cuts of alumina. As non-limiting examples of such aluminas, reference can be made to aluminas A125, CR125, D65CR from the Baikowski Company. Preferably, the reinforcing filler used is fumed silica, alone or mixed with alumina.
[0071] Non-siliceous minerals that may be included as semi-reinforcing or reinforcing mineral fillers may be selected from the group consisting of: carbon black, titanium dioxide, aluminum oxide, alumina hydrate, calcium carbonate, finely divided quartz, diatomaceous earth, zinc oxide, mica, talc, iron oxide, barium sulfate, hydrated lime, gypsum, glass, hollow glass beads, hollow plastic beads, plastic powders, calcium silicate, cristobalite, zeolite, bentonite.
[0072] In terms of weight, it is preferred to use an amount of filler E of 5-40% by weight, preferably 10-35% by weight, more preferably 15-30% by weight, based on the total components of the composition.
[0073] In a preferred embodiment, the present invention is a method for additively manufacturing a silicone elastomeric article, comprising the steps of: 1) printing a first addition-curable liquid silicone composition onto a substrate using a 3D printer selected from an extrusion 3D printer or a material jetting 3D printer to form a first layer; 2) printing a second addition curable liquid silicone composition onto the first layer or a previous layer with the 3D printer to form a subsequent layer; 3) optionally repeating step 2) for any additional layers desired, using independently selected addition-curable liquid silicone compositions; 4) Crosslinking, optionally by heating, said first and subsequent layers to obtain a silicone elastomeric article. Here, at least one layer of the addition-curable liquid silicone composition is an addition-curable liquid silicone composition X of the present invention, as defined below.
[0074] In particular, the addition-curable liquid silicone composition X comprises: (A) At least two silicon bonds C2 to C per molecule 20 at least one organopolysiloxane A containing alkenyl groups; (B) at least one organosilicon crosslinker B containing at least three silicon-bonded hydrogen atoms per molecule; (C) at least one organopolysiloxane gum C having a consistency of 200 to 900 at 25 ° C., and at least one silicon bond C2 to C3 per molecule 20 Alkenyl group and at least one silicon bond C6-C per molecule 12 at least one organopolysiloxane gum C containing aryl groups; (D) at least one addition reaction catalyst D; (E) at least one filler E; (F) optionally, at least one diorganohydrogensiloxy-terminated diorganopolysiloxane chain extender F; (G) optionally, at least one cure rate modifier G; (H) optionally, at least one silicone resin H; and (I) Optionally, at least one additive I.
[0075] In particular, the addition-curable liquid silicone composition X of the present invention exhibits improved relaxation times compared to conventional compositions. The relaxation time (or recovery time) defined herein is the time required for a viscous material to recover from shear stress after the shear force is removed. One way to measure the relaxation time is to consider the intersection between the lines tangent to the initial and final parts of the storage modulus curve. Thus, the relaxation time provides an indication of how quickly the composition returns to its starting viscosity after shear, as experienced when the composition is extruded from the printing nozzle during 3D printing. The higher the relaxation time value, the slower the viscosity recovery. The lower the relaxation time value, the faster the relaxation. The faster the composition returns to its initial viscosity, the better the composition will hold its shape during 3D printing.
[0076] In some embodiments, the addition-curable liquid silicone composition X of the present invention has a viscosity of 1 rads. -1 In a preferred embodiment, the addition-curable liquid silicone composition X of the present invention exhibits a relaxation time of 100 seconds or less after a shear rate of 1 rads. -1 after exposure to an applied shear rate of ≦80 seconds, ≦70 seconds, ≦65 seconds, or ≦60 seconds.
[0077] In the first step of the method, a layer of a first addition curable liquid silicone composition is printed onto a substrate, forming a layer on the substrate. The substrate is not limited and may be any substrate. The substrate is selected to support the 3D article during its manufacturing process, for example, the substrate plate of a 3D printer. The substrate may be rigid or flexible, continuous or discontinuous. The substrate itself may be supported, for example, by a substrate table or plate, so that the substrate does not need to be rigid. It may also be removed from the 3D article. Alternatively, the substrate may be physically or chemically bonded to the 3D article. In one embodiment, the substrate may be silicone.
[0078] The layer formed by printing the first addition-curable liquid silicone composition can have any shape and any dimension. The layer can be continuous or discontinuous.
[0079] In the second step, a second addition-curing liquid silicone composition is printed on the previous layer formed in the first step with an extrusion 3D printer or a material 3D jet printer to form a subsequent layer. The extrusion 3D printer and the material 3D jet printer may be the same or different from the extrusion 3D printer or the material 3D jet printer used in step 1).
[0080] The second addition-curable liquid silicone composition may be the same as or different from the first addition-curable liquid silicone composition.
[0081] The subsequent layer formed by printing the second addition-curable liquid silicone composition can have any shape and any dimensions. The subsequent layer can be continuous or discontinuous.
[0082] In the third step, the second step is repeated to obtain the required number of layers.
[0083] In a fourth step, the layer is cured (optionally by heating) to obtain a silicone elastomer article. Curing or crosslinking can be completed at ambient temperature. Typically, ambient or room temperature refers to a temperature between 20°C and 25°C.
[0084] Heat can be used to accelerate crosslinking or curing of the layer. Heat curing after printing can be carried out at temperatures between 50°C and 200°C, preferably between 100°C and 150°C, to achieve complete curing or crosslinking more quickly.
[0085] As used herein, the term "layer" refers to a layer at any stage of the process (first layer, previous layer, or subsequent layer). Layers can be of various dimensions, such as thickness and width. The thickness of a layer can be uniform or can vary. The average thickness refers to the thickness of a layer immediately after printing.
[0086] In one embodiment, the layers independently have a thickness of 10 to 3000 μm, preferably 50 to 2000 μm, more preferably 100 to 800 μm, and most preferably 100 to 600 μm.
[0087] In certain embodiments, no energy source, such as heat or radiation, is applied during steps 1)-3) prior to printing of at least 10 layers, preferably 20 layers.
[0088] 3D printing is commonly associated with a number of related technologies used to manufacture physical objects from computer-generated, e.g., computer-aided design (CAD), data sources.
[0089] This disclosure generally incorporates ASTM designation F2792-12a, Standard Terminology for Additive Manufacturing Technologies. In this ASTM standard:
[0090] A "3D printer" is defined as "a machine used for three-dimensional printing" and "3D printing" is defined as "the production of objects by the deposition of material using a print head, nozzle, or another printer technology."
[0091] "Additive manufacturing (AM)" is defined as "a process of creating objects from 3D model data by combining materials, usually layer by layer, as opposed to subtractive manufacturing methodologies. Related and included synonyms for 3D printing include additive manufacturing, additive process, process technology, technology layer manufacturing, layer manufacturing, and freeform manufacturing." Additive manufacturing (AM) is also known as rapid prototyping (RP). As used herein, "3D printing" is generally interchangeable with "additive manufacturing" and vice versa.
[0092] "Printing" is defined as the deposition of a material, here a liquid silicone composition, using a print head, nozzle, or another printer technology.
[0093] In this disclosure, "3D or three-dimensional article, object, or part" refers to an article, object, or part obtained by additive manufacturing or 3D printing as disclosed herein.
[0094] In general, all 3D printing processes have a common starting point: a computer-generated data source or program that describes an object. The computer-generated data source or program can be based on a real object or a virtual object. For example, a 3D scanner can be used to scan a real object and the scan data can be used to create the computer-generated data source or program. Alternatively, the computer-generated data source or program can be designed from scratch.
[0095] The computer-generated data source or program is typically converted into the Standard Tessellation Language (STL) file format, although other file formats may also or additionally be used. The file is typically loaded into 3D printing software, which takes the file and any user input and slices it into individual "slices" of user-defined thickness. The 3D printing software typically outputs machine instructions, which may be in the form of G-code, that are read by the 3D printer to create each slice. The machine instructions are transferred to the 3D printer, which builds the object layer by layer based on this slice information in the form of machine instructions. The thickness of these slices may vary.
[0096] An extrusion 3D printer is a 3D printer in which material is extruded from a nozzle, syringe, or orifice during the additive manufacturing process. Material extrusion generally works by forcing material through a nozzle, syringe, or orifice to print one cross-section of an object. This can be repeated for each subsequent layer. The extruded material bonds to the layer below it during the material's hardening.
[0097] In a preferred embodiment, the method for additively manufacturing three-dimensional silicone elastomer articles uses an extrusion 3D printer. The addition curable liquid silicone composition is extruded through a nozzle. The nozzle can be heated to aid in dispensing the addition curable liquid silicone composition.
[0098] The average diameter of the nozzle defines the thickness of the layer, in one embodiment the diameter of the layer is between 50 μm and 3000 μm, preferably between 100 μm and 800 μm, most preferably between 100 μm and 500 μm.
[0099] The distance between the nozzle and the substrate is an important parameter to ensure the proper shape of the resulting silicone elastomer. Preferably, the distance between the nozzle and the substrate is 60-150% of the average diameter of the nozzle, more preferably 80-120%.
[0100] The addition-curable liquid silicone composition dispensed from the nozzle may be supplied from a cartridge-like system. The cartridge may contain a nozzle or nozzles with an associated fluid reservoir or reservoirs. A coaxial two-cartridge system with a static mixer and only one nozzle may also be used. The pressure is adapted to the fluid being dispensed, the average diameter of the associated nozzle, and the printing speed.
[0101] Due to the high shear rates generated during nozzle extrusion, the viscosity of the addition-curable liquid silicone composition is significantly reduced, allowing for the printing of finer layers.
[0102] The cartridge pressure can vary from 1 to 20 bar, preferably from 2 to 10 bar, most preferably from 4 to 8 bar. When using nozzle diameters less than 100 μm, the cartridge pressure needs to be higher than 20 bar to obtain good material extrusion. To withstand such pressures, adapted equipment using aluminum cartridges needs to be used.
[0103] The nozzle and / or build platform move in the X,Y (horizontal planes) to complete a cross section of the object, then move in the Z (vertical) plane once a layer is completed. The XYZ movement precision of the nozzle is high, on the order of 10μm. After each layer is printed on the (X,Y) work plane, the nozzle is moved in the Z direction a sufficient distance for the next layer to be applied to the (X,Y) work plane. In this way, the object that will become the three-dimensional article is built up layer by layer from bottom to top.
[0104] Advantageously, the printing speed is between 1 and 50 mm / s, preferably between 5 and 30 mm / s, in order to obtain the best balance between precision and production speed.
[0105] "Material jetting" is defined as "an additive manufacturing process in which droplets of a build material are selectively deposited". The material is applied (jetting) discontinuously in the form of individual droplets using a print head to the desired location of a working surface. 3D devices and processes for the stepwise production of 3D structures using a print head array comprising at least one, preferably 2 to 200 print head nozzles, allow for site-selective application of multiple materials, where appropriate. Application of materials by inkjet printing imposes certain requirements on the viscosity of the materials.
[0106] In a material 3D jetting printer, one or more reservoirs are under pressure and connected to a metering nozzle via a metering line. Upstream or downstream of the reservoirs there may be devices that allow the multi-component addition-curable liquid silicone composition to be mixed homogeneously and / or to expel dissolved gases. To build silicone elastomer articles from different addition-curable liquid silicone compositions or, for more complex structures, there may be one or more jetting devices operating independently of each other, thus allowing composite parts made from silicone elastomers and other plastics.
[0107] Due to the high shear rates that occur in the metering valve during the jetting and metering procedure, the viscosity of such addition-curing liquid silicone compositions is significantly reduced, allowing the jetting and metering of very fine droplets. After the fine droplets are deposited on the substrate, the viscosity increases again due to a rapid decrease in the shear rate. Thus, the deposited droplets quickly become highly viscous again, allowing the construction of precise shapes of three-dimensional structures.
[0108] Individual metering nozzles can be precisely positioned in the x, y, and z directions to allow for precisely targeted deposition of the addition-curable liquid silicone composition onto a substrate (or onto a previously deposited addition-curable liquid silicone composition, which may optionally have already been cured, during subsequent molding of a molded article).
[0109] In contrast to other additive manufacturing methods, it is not necessary to carry out the method of the present invention in an irradiated or heated environment to initiate curing after each layer is printed in order to avoid collapse of the structure. Thus, the irradiation and heating steps can be optional.
[0110] Typically, 3D printers utilize a dispenser, such as a nozzle or print head, to print a particular addition-curable liquid silicone composition. Optionally, the dispenser can be heated before, during, or after dispensing the addition-curable liquid silicone composition. Multiple dispensers can be utilized, each with independently selected properties.
[0111] In one embodiment, the method can use supports to build the object. If the object is printed using supports or rafts, they are typically removed after the printing process is complete, leaving the completed object.
[0112] Optionally, the resulting article can be subjected to a different post-treatment regimen. In one embodiment, the method further comprises heating the three-dimensional silicone article. Heating can hasten curing. In another embodiment, the method further comprises irradiating the three-dimensional silicone article. Further irradiation can be used to accelerate curing. In another embodiment, the method further comprises both heating and irradiating the three-dimensional silicone article.
[0113] Optionally, a post-processing step can significantly improve the surface quality of the print. Sanding is a common method to reduce or remove the visible layers of a model. Spraying or coating the surface of an elastomeric article can also be used to reduce the visible layers of a model and modify the appearance and properties of the surface.
[0114] Surface treatment using a laser is also possible.
[0115] For medical applications, sterilization of the final elastomeric article can be achieved by heating the object above 100° C. or in a UV oven.
[0116] The first and second addition curable liquid silicone compositions may be the same or different from each other, and when step 3) is repeated, independently selected addition curable liquid silicone compositions may be utilized. In the method of the present invention, at least one layer of the addition curable liquid silicone composition is the addition curable liquid silicone composition X of the present invention, which may be, for example, the first or second addition curable liquid silicone composition, or any other additional layer of addition curable liquid silicone composition. In one embodiment, all printed layers of the addition curable liquid silicone composition are the addition curable liquid silicone composition X of the present invention.
[0117] For brevity, the first and second addition-curable liquid silicone compositions, along with any other addition-curable liquid silicone compositions that are optionally utilized when step 3) is repeated, will be referred to collectively as simply the "addition-curable liquid silicone compositions" or "silicone compositions."
[0118] The addition-curable liquid silicone composition X of the present invention can be prepared by simply mixing the components in the desired ratio. However, for reasons of storage stability and bath life, it is advantageous to store the composition X in two parts A and B by separating the curing catalyst (D) from the organosilicon crosslinker (B) and / or diorganopolysiloxane (F) having hydrogen substituents before or during application of the composition to a substrate. The other components of the composition X are often dispersed in both parts in a ratio that allows the two parts to be easily mixed immediately before application. Such an easy mixing ratio can be, for example, a ratio of 1 / 10 or 1 / 1.
[0119] Preferably, the two-part addition-curable liquid silicone composition X of the present invention comprises a first liquid composition comprising components A and D, but not including B and F, and a second liquid composition comprising components A, B, C, and optionally F, but not including D.
[0120] The addition-curable liquid silicone composition X of the present invention comprises at least one organopolysiloxane gum C and at least one filler E, which are as described above.
[0121] The addition-curable liquid silicone composition X of the present invention comprises at least one alkenyl-containing organopolysiloxane A having two silicon-bonded alkenyl groups per molecule. In some embodiments, the addition-curable liquid silicone composition X of the present invention comprises more than one alkenyl-containing organopolysiloxane A having two silicon-bonded alkenyl groups per molecule. For example, the curable liquid silicone rubber composition of the present invention may comprise two or more alkenyl-containing organopolysiloxanes A (A1, A2, A3, etc.) having two silicon-bonded alkenyl groups per molecule.
[0122] In some embodiments, the at least one alkenyl-containing organopolysiloxane A comprises: Two siloxy units of formula (A-1): (Alk)(R)2SiO 1 / 2 (A-1) In the formula, the symbol "Alk" represents a C2-C alkyl group such as a vinyl group, an allyl group, a hexenyl group, a decenyl group, or a tetradecenyl group. 20 R represents an alkenyl group of the formula (I), preferably a hydrogen atom of a vinyl group, and R represents a C1-C alkyl group such as methyl, ethyl, propyl, trifluoropropyl, or an aryl group. 20 represents an alkyl group, preferably a methyl group; Other siloxy units of formula (A-2): (L) g SiO (4-g) / 2 (A-2) In the formula, the symbol L is a C1-C aryl group such as methyl, ethyl, propyl, or trifluoropropyl. 20 or an aryl group, preferably methyl, the symbol g is equal to 0, 1, 2 or 3, and in each case L may be the same or different.
[0123] In some preferred embodiments, at least one alkenyl-containing organopolysiloxane A has the following formula (1): [ka] (1) During the ceremony, n is an integer ranging from 1 to 1000, preferably from 50 to 1000; R is a C1-C aryl group such as methyl, ethyl, propyl, trifluoropropyl, or an aryl group. 20 an alkyl group, preferably a methyl group; R' is a C2-C alkyl group such as vinyl, allyl, hexenyl, decenyl, or tetradecenyl. 20 an alkenyl group, preferably a vinyl group; R″ is a C1-C aryl group such as methyl, ethyl, propyl, trifluoropropyl, or an aryl group. 20and preferably a methyl group.
[0124] In a preferred embodiment, the at least one alkenyl-containing organopolysiloxane A is one or more α,ω-vinylpolydimethylsiloxanes, more preferably one or more linear α,ω-vinylpolydimethylsiloxanes.
[0125] In some embodiments, the viscosity of the at least one alkenyl-containing organopolysiloxane A is about 50 to about 100,000 mPa·s, preferably about 100 to about 50,000 mPa·s, more preferably about 150 to about 25,000 mPa·s. In some embodiments, the curable liquid silicone rubber composition of the present invention comprises at least one alkenyl-containing organopolysiloxane A1 having a viscosity of about 50 to about 10,000 mPa·s and at least one alkenyl-containing organopolysiloxane A2 having a viscosity of about 5,000 to about 100,000 mPa·s. In a preferred embodiment, the viscosity of the at least one alkenyl-containing organopolysiloxane A1 is about 100 to about 7,500 mPa·s, more preferably about 150 to about 5,000 mPa·s. In a preferred embodiment, the viscosity of the at least one alkenyl-group-containing organopolysiloxane A2 is from about 7,500 to about 50,000 mPa·s, more preferably from about 10,000 to about 25,000 mPa·s.
[0126] The viscosity of the silicone compositions described herein and their individual components (except for organosiloxane gum C above) corresponds in magnitude to the "Newtonian" dynamic viscosity at 25°C (i.e. the dynamic viscosity measured in a manner known per se using a Brookfield viscometer at a shear rate gradient sufficiently low so that the measured viscosity is independent of the rate gradient).
[0127] In some embodiments, the molecular weight of at least one alkenyl-containing organopolysiloxane A is about 500 g / mol to about 90,000 g / mol, preferably about 1,000 g / mol to about 70,000 g / mol, more preferably about 5,000 g / mol to about 60,000 g / mol. In some embodiments, the curable liquid silicone rubber composition of the present invention comprises at least one alkenyl-containing organopolysiloxane A1 having a molecular weight of about 1,000 to about 50,000 g / mol and at least one alkenyl-containing organopolysiloxane A2 having a molecular weight of about 5,000 to about 80,000 g / mol. In a preferred embodiment, the molecular weight of at least one alkenyl-containing organopolysiloxane A1 is about 5,000 to about 40,000 g / mol, more preferably about 7,000 to about 30,000 g / mol. In a preferred embodiment, the molecular weight of the at least one alkenyl-group-containing organopolysiloxane A2 is from about 15,000 to about 75,000 g / mol, more preferably from about 30,000 to about 60,000 g / mol.
[0128] At least one alkenyl-containing organopolysiloxane A is preferably linear.
[0129] The addition-curable liquid silicone composition X of the present invention further comprises at least one organosilicon crosslinker B containing at least two, preferably at least three, silicon-bonded hydrogen atoms per molecule. In some embodiments, the organosilicon crosslinker B containing at least two silicon-bonded hydrogen atoms per molecule is an organohydrogenpolysiloxane containing from 10 to 500 silicon atoms in each molecule, preferably from 10 to 250 silicon atoms in each molecule.
[0130] Examples of suitable organosilicon crosslinkers B, which, if branched, contain at least two silicon-bonded hydrogen atoms per molecule, include the branched polymers of formula (I): (R2HSiO 1 / 2 ) x (R3SiO 1 / 2 ) y(RHSiO2 / 2) z (R2SiO 2 / 2 ) p (RSiO 3 / 2 ) q (HSiO 3 / 2 ) v (SiO 4 / 2 ) r (I) wherein H is hydrogen and R is a monovalent hydrocarbon radical of 1 to 40 carbon atoms, preferably a monovalent hydrocarbon radical of 1 to 20 carbon atoms, more preferably selected from the group consisting of methyl, ethyl, propyl, isopropyl, n-butyl, isobutyl, sec-butyl, tert-butyl, pentyl, hexyl, heptyl, phenyl, benzyl, and mesityl; most preferably selected from the group consisting of methyl and phenyl; In the formula, x≧2, y≧0, z≧0, p≧0, v≧0, and at least one of q and r is ≧1; alternatively, x≧2, y≧0, z≧0, p≧0, q≧0; v≧0, r≧1; alternatively, x≧2, y≧0, r≧1 (however, when r=1, x+y=4), and z, p, q, v=0. Alternatively, x>2, y>0, r>1, and z, p, q, v=0.
[0131] When branched polymers, specific crosslinkers B that contain at least two silicon-bonded hydrogen atoms per molecule include, but are not limited to, (H)(CH)SiO. 1 / 2 Siloxy unit (M H ) and SiO 4 / 2 Silicone resin M containing siloxy units (Q units) H Q, (CH3)3SiO 1 / 2 Siloxy unit (M), (CH3)2HSiO 1 / 2 Siloxy unit (M H ) and SiO 4 / 2 Silicone resin MM containing (Q) H Q, (CH3)2HSiO 1 / 2 Siloxy unit (M H ), (CH3)HSiO 2 / 2 (D H ) and SiO 4 / 2 Silicone resin M containing siloxy units (Q) H DH Q, (CH3)3SiO 1 / 2 Units (M units), (CH3)2HSiO 1 / 2 (M H ), (CH3)HSiO 2 / 2 (D H ) and SiO 4 / 2 Silicone resin containing unit (Q) MM H D H Q.
[0132] In some embodiments, the crosslinker B has the formula R2HSiO 1 / 2 and at least two M-H siloxy units of the formula SiO 4 / 2 where H is a hydrogen atom and R is a monovalent hydrocarbon radical of 1 to 40 carbon atoms, preferably 1 to 20 carbon atoms, more preferably selected from the group consisting of methyl, ethyl, propyl, isopropyl, n-butyl, isobutyl, sec-butyl, tert-butyl, pentyl, hexyl, heptyl, phenyl, benzyl, and mesityl; and most preferably selected from the group consisting of methyl and phenyl.
[0133] In a preferred embodiment, crosslinker B is a MHQ silicone resin having the formula: MH w Q z where Q is a group of formula SiO 4 / 2 and MH has the formula RHSiO 1 / 2 wherein H is a hydrogen atom, R is a monovalent hydrocarbon radical of 1 to 40 carbon atoms, preferably a monovalent hydrocarbon radical of 1 to 20 carbon atoms, more preferably selected from the group consisting of methyl, ethyl, propyl, isopropyl, n-butyl, isobutyl, sec-butyl, tert-butyl, pentyl, hexyl, heptyl, phenyl, benzyl, and mesityl; and most preferably selected from the group consisting of methyl and phenyl, and the subscripts w and z have a ratio of 0.5 to 4.0, preferably 0.6 to 3.5, more preferably 0.75 to 3.0, and most preferably 1.0 to 3.0, respectively.
[0134] In another preferred embodiment, the crosslinker B is a MHQ silicone resin having the formula: (MH w Q z ) j where Q is a group of formula SiO 4 / 2 and MH has the formula RHSiO 1 / 2 wherein R is a monovalent hydrocarbon radical of 1 to 40 carbon atoms, preferably a monovalent hydrocarbon radical of 1 to 20 carbon atoms, and more preferably selected from the group consisting of methyl, ethyl, propyl, isopropyl, n-butyl, isobutyl, sec-butyl, tert-butyl, pentyl, hexyl, heptyl, phenyl, benzyl, and mesityl; and most preferably selected from the group consisting of methyl and phenyl, the subscripts w and z each have a ratio of 0.5 to 4.0, preferably 0.6 to 3.5, more preferably 0.75 to 3.0, and most preferably 1.0 to 3.0, and the subscript j is in the range of about 2.0 to about 100, preferably about 2.0 to about 30, more preferably about 2.0 to about 10, and most preferably about 3.0 to about 5.0.
[0135] In another preferred embodiment, crosslinker B has 0.10 wt. % to 2.00 wt. % H as SiH and has the formula RHSiO 1 / 2 MH siloxy units of the formula SiO 4 / 2 where H is a hydrogen atom and R is a monovalent hydrocarbon radical of 1 to 40 carbon atoms, preferably 1 to 20 carbon atoms, more preferably selected from the group consisting of methyl, ethyl, propyl, isopropyl, n-butyl, isobutyl, sec-butyl, tert-butyl, pentyl, hexyl, heptyl, phenyl, benzyl, and mesityl; most preferably selected from the group consisting of methyl and phenyl.
[0136] At least one organosilicon crosslinker B may be included in the addition-curable liquid silicone composition X in an amount of from about 0.01% to about 5%, preferably from about 0.05% to about 2%, and preferably from about 0.1% to about 1% by weight of the total composition.
[0137] Organosilicon crosslinking agent B preferably contains 0.45% to 50% by weight SiH, more preferably 1% to 35% by weight SiH, more preferably 5% to 30% by weight SiH, or 15% to 25% by weight SiH.
[0138] In some embodiments, the organosilicon crosslinker B comprises: (i) at least two, preferably three, siloxy units of the same or different formula (XL-1): (H)(Z) e SiO (3-e) / 2 (XL-1) During the ceremony, - The symbol H represents a hydrogen atom, the symbol Z represents an alkyl group containing 1 to 8 carbon atoms; - the symbol e is equal to 0, 1 or 2; and / or (ii) at least one, preferably 1 to 550, siloxy units of formula (XL-2): (Z) g SiO (4-g) / 2 (XL-2) During the ceremony, The symbol Z represents an alkyl group having 1 to 8 carbon atoms; The symbol g is equal to 0, 1, 2, or 3.
[0139] In some embodiments, Z in XL-1 and / or XL-2 is selected from methyl, ethyl, propyl, and 3,3,3-trifluoropropyl groups, cycloalkyl groups (such as cyclohexyl, cycloheptyl, or cyclooctyl groups), and aryl groups (such as xylyl, tolyl, and phenyl groups).
[0140] Preferably, Z is a methyl group, provided that Z in XL-1 and XL-2 may be the same or different.
[0141] In a preferred embodiment, e in XL-1 is 1 or 2.
[0142] In a preferred embodiment, g in XL-2 is 2.
[0143] In a preferred embodiment, organosilicon crosslinker B contains 3 to 60 siloxy units of formula (XL-1) and 1 to 250 siloxy units of formula (XL-2).
[0144] The addition-curable liquid silicone composition X of the present invention has at least one silicon-bonded C2-C 20 Alkenyl group and at least one silicon bond C6-C per molecule 12 It further comprises at least one organopolysiloxane gum C as described above, which comprises aryl groups.
[0145] In some embodiments, the at least one organopolysiloxane gum C may be contained in the addition-curable liquid silicone composition X in an amount of about 0.1 to about 40%, preferably about 1% to about 40%, preferably about 3% to about 30%, preferably about 5% to about 25%, based on the weight of the total composition.
[0146] In some embodiments, the at least one organopolysiloxane gum C may be present in the addition-curable liquid silicone composition X in an amount of at least 5 parts by weight, at least 8 parts by weight, at least 10 parts by weight, at least 15 parts by weight, or at least 20 parts by weight, based on the weight of the total addition-curable liquid silicone composition X.
[0147] In some embodiments, the at least one organopolysiloxane gum C can be included in the addition-curable liquid silicone composition X in an amount such that the total aryl group content in mole percent is at least 0.5 mole percent. For example, the at least one organopolysiloxane gum C can be included in the addition-curable liquid silicone composition X in an amount such that the total aryl group content in mole percent is at least 0.6 mole percent, at least 0.7 mole percent, at least 0.8 mole percent, at least 0.9 mole percent, at least 1.0 mole percent, at least 1.1 mole percent, at least 1.2 mole percent, at least 1.3 mole percent, at least 1.4 mole percent, at least 1.5 mole percent, at least 1.6 mole percent, at least 1.7 mole percent, at least 1.8 mole percent, at least 1.9 mole percent, or at least 2.0 mole percent.
[0148] In some embodiments, the at least one organopolysiloxane gum C has a total aryl group content in mole percent in the addition-curable liquid silicone composition X of from about 0.5 mol % to about 10 mol %, from about 0.5 mol % to about 9 mol %, from about 0.5 mol % to about 8 mol %, from about 0.5 mol % to about 7 mol %, from about 0.5 mol % to about 6 mol %, from about 0.5 mol % to about 5.5 mol %, from about 0.5 mol % to about 5 mol %, from about 0.5 mol % to about 4.5 mol %, from about 0.5 mol % to about 4 mol %, from about 0.5 mol % to about 3.5 mol%, about 0.5 mol% to about 3 mol%, about 0.5 mol% to about 2.5 mol%, about 0.5 mol% to about 2 mol%, about 0.5 mol% to about 1.5 mol%, about 0.5 mol% to about 1.4 mol%, about 0.5 mol% to about 1.3 mol%, about 0.5 mol% to about 1.2 mol%, about 0.5 mol% to about 1.1 mol%, 0.5 mol% to about 1.0 mol%, about 0.5 mol% to about 0.9 mol%, about 0.5 mol% to about 0.8 mol%, or about 0.5 mol% to about 0.7 mol%.
[0149] In some embodiments, the at least one organopolysiloxane gum C is present in the addition-curable liquid silicone composition X in an amount having a total aryl group content in mole percent of from about 1 mol % to about 10 mol %, from about 1.2 mol % to about 10 mol %, from about 1.4 mol % to about 10 mol %, from about 1.6 mol % to about 10 mol %, from about 1.8 mol % to about 10 mol %, from about 2 mol % to about 10 mol %, from about 2.2 mol % to about 10 mol %, %, about 2.4 mol% to about 10 mol%, about 2.6 mol% to about 10 mol%, about 2.8 mol% to about 10 mol%, about 3 mol% to about 10 mol%, about 3.5 mol% to about 10 mol%, about 4 mol% to about 10 mol%, about 5 mol% to about 10 mol%, about 6 mol% to about 10 mol%, about 7 mol% to about 10 mol%, about 8 mol% to about 10 mol%, or about 9 mol% to about 10 mol%.
[0150] In some embodiments, the at least one organopolysiloxane gum C has a total aryl group content in mole percent in the addition-curable liquid silicone composition X of from about 1.2 mol % to about 7 mol %, from about 1.4 mol % to about 6 mol %, from about 1.6 mol % to about 6 mol %, from about 1.8 mol % to about 6 mol %, from about 2 mol % to about 6 mol %, from about 2.2 mol % to about 6 mol %, from about 2.4 mol % to about 6 mol %, from about 2.6 mol % to about 6 mol %, from about 2.8 mol % to about 6 mol %, from about 3 mol % to about 6 mol %, or from about 4 mol % to about 6 mol %, from about 1.2 mol % to about 5 mol %, from about 1.2 mol % to about 4 mol %, from about 1.2 mol % to about 3 mol %, from about 1.2 mol % to about 2.8 mol % , about 1.2 mol% to about 2.6 mol%, about 1.2 mol% to about 2.4 mol%, about 1.4 mol% to about 4 mol%, about 1.4 mol% to about 3 mol%, about 1.4 mol% to about 2.8 mol%, about 1.4 mol% to about 2.6 mol%, about 1.4 mol% to about 2.4 mol%, about 1.6 mol% to about 4 mol%, about 1.6 mol% to about 3 mol%, about 1.6 mol% to about 2.8 mol%, about 1.6 mol% to about 2.6 mol%, about 1.6 mol% to about 2.4 mol%, about 1.8 mol% to about 4 mol%, about 1.8 mol% to about 3 mol%, about 1.8 mol% to about 2.8 mol%, about 1.8 mol% to about 2.6 mol%, or about 1.8 mol% to about 2.4 mol%.
[0151] The addition-curable liquid silicone composition X of the present invention further contains at least one type of addition reaction catalyst D. The addition reaction catalyst D can be contained in any amount that can cure the composition. For example, the addition reaction catalyst D can be contained in an amount such that the amount of platinum group metal in the catalyst D is 0.01 to 500 parts by weight per 1 million parts by weight of the alkenyl group-containing organopolysiloxane A.
[0152] Catalyst D can be selected from platinum and rhodium compounds in particular.In particular, it is possible to use platinum complexes and organic products (described in US Pat. No. 3,159,601, US Pat. No. 3,159,602, US Pat. No. 3,220,972, and European Patent Application Publication Nos. 0057459, 0118978, 0190530), platinum and vinylorganosiloxane complexes (described in US Pat. No. 3,419,593, US Pat. No. 3,715,334, US Pat. No. 3,377,432, and US Pat. No. 3,814,730).In a preferred embodiment, addition reaction catalyst D is a platinum group metal-containing catalyst.
[0153] The addition-curable liquid silicone composition X further comprises at least one filler E as defined above.
[0154] The addition-curable liquid silicone composition X of the present invention may also contain at least one diorganohydrogensiloxy-terminated diorganopolysiloxane chain extender F. The at least one diorganohydrogensiloxy-terminated diorganopolysiloxane chain extender F may be contained in the addition-curable liquid silicone composition X in an amount of 0% to about 20%, preferably about 0.5% to about 15%, and preferably about 0.5% to about 10%, based on the weight of the total composition.
[0155] In some embodiments, the diorganohydrogensiloxy-terminated diorganopolysiloxane F has the following formula (2): [ka] wherein: R is independent, C1~C 20 or C6-C alkyl groups such as xylyl, tolyl, or phenyl groups. 12 R is independently selected from the group consisting of methyl, ethyl, propyl, and aryl, and most preferably, R is methyl; n is an integer ranging from 1 to 500, preferably from 2 to 100, and more preferably from 3 to 50.
[0156] In some embodiments, the viscosity of the at least one diorganohydrogensiloxy-terminated diorganopolysiloxane F is from about 1 to about 500 mPa·s, preferably from about 2 to about 100 mPa·s, and more preferably from about 4 to about 50 mPa·s or from about 5 to about 20 mPa·s.
[0157] In some embodiments, the molecular weight of the at least one diorganohydrogensiloxy-terminated diorganopolysiloxane F is from about 100 to about 5,000 g / mol, preferably from about 250 to about 2,500 g / mol, and more preferably from about 500 to about 1,000 g / mol.
[0158] The addition-curable liquid silicone composition X of the present invention may also contain at least one cure rate modifier G. The cure rate modifier G may be, for example, a crosslinking inhibitor G1 and / or a crosslinking retarder G2.
[0159] Crosslinking inhibitors are also well known. Examples of crosslinking inhibitors G1 that can be used as cure rate regulators G include: Polyorganosiloxanes, advantageously cyclic and substituted with at least one alkenyl group, tetramethylvinyltetrasiloxane being particularly preferred; Pyridine, Phosphines and organic phosphites, Unsaturated amides, Alkylated maleates, Acetylenic alcohol.
[0160] These acetylenic alcohols (see French Patent No. 1528464 and French Patent Application No. 2372874) form part of the preferred thermal blockers for the hydrosilylation reaction and have the formula: (R)(R')C(OH)-C≡CH During the ceremony: R is a linear or branched alkyl radical, or a phenyl radical; R' is H or a linear or branched alkyl radical, or a phenyl radical; The radicals R, R' and the carbon atom alpha to the triple bond may form a ring; The total number of carbon atoms contained in R and R' is at least 5, and preferably 9-20.
[0161] The alcohols are preferably chosen with a boiling point of about 250° C. By way of example, the following may be mentioned: 1-ethynyl-1-cyclohexanol (ECH); Methyl-3 dodecyn-1ol-3; Trimethyl-3,7,11-dodecyn-1-ol-3; Diphenyl-1,1-propyn-2-ol-1 Ethyl-3 ethyl-6 nonynoyl-3; Methyl-3-pentadecyn-1-ol-3.
[0162] These α-acetylenic alcohols are commercially available.
[0163] Such modifiers are present in an amount up to 2,000 ppm, preferably 20 to 50 ppm, based on the total weight of organopolysiloxanes A, B, C, and optionally F.
[0164] Examples of crosslinking retarders G2 that can be used as curing rate regulator G include so-called inhibitors for controlling the crosslinking reaction and extending the pot life of the silicone composition. Examples of advantageous crosslinking retarders G2 that can be used as curing rate regulator G include, for example, vinyl siloxane, 1,3-divinyltetramethyldisiloxane, or tetravinyl-tetramethyl-tetracyclosiloxane. It is also possible to use other known inhibitors, such as ethynylcyclohexanol, 3-methylbutynol, or dimethyl maleate.
[0165] The addition-curable liquid silicone composition X of the present invention may also contain a silicone resin H. Silicone resins are well-known and commercially available branched organopolysiloxane oligomers or polymers. They have the structure of the formula RSiO 1 / 2 (unit: M), R2SiO 2 / 2 (unit D), RSiO 3 / 2 (unit T) and SiO 4 / 2 (unit Q), at least one of these units being a unit T or Q. The radicals R are identical or different and are selected from linear or branched C1-C8 alkyl, hydroxyl, aryl or alkylaryl radicals. For example, the alkyl radicals may be methyl, ethyl, isopropyl, tert-butyl and n-hexyl groups. Examples of branched organopolysiloxane oligomers or polymers may include MQ, MDQ, TD and MDT resins, in which the hydroxyl functional groups may be carried by the units M, D and / or T.
[0166] The addition-curable liquid silicone composition X of the present invention may also contain at least one blowing agent J, preferably said blowing agent J is a chemical blowing agent, most preferably said blowing agent J is selected from the group consisting of ammonium bicarbonate, ammonium hydrogen carbonate, alkali metal hydrogen carbonates and mixtures thereof. For ease of application and manufacture, the blowing agent J is preferably a polydimethylsiloxane or a mixture of at least two silicon-bonded C2-C20 It can be pre-dispersed in organopolysiloxane A having alkenyl groups, for example at a level of 30% to 60% by weight. Certain optional additives that may help to stabilize the shelf life of the resulting composition are finally incorporated. In another preferred embodiment, blowing agent J can be selected from the group consisting of ammonium bicarbonate, ammonium hydrogen carbonate, alkali metal hydrogen carbonates and mixtures thereof, wherein said blowing agent J has a median particle size (D50) of ≦50 μm, even more preferably ≦10 μm.
[0167] The addition-curable liquid silicone composition X of the present invention may also contain at least one additive I commonly used in the field of the present invention.
[0168] A rheology modifier can be optionally added to improve the rheological properties and provide higher flowability and a smooth surface of the molded article. Such a rheology modifier can be a flow additive such as PTFE powder, boron oxide derivatives, fatty acid fatty alcohol derivatives or derivatives, esters and their salts, or fluoroalkyl surfactants. Examples of rheology modifiers that can be used include, for example, epoxy-functional silanes, poly(aryl)siloxanes, polyalkylene glycols, polyester polyols, polyhydric alcohols, dicarboxylic acids, polyester diols, and silicone polyethers such as silicone-polyether block copolymers, free polyethers, and mixtures thereof, for example, BLUESIL SP-3300 (siloxane and silicone, di-Me, 3-hydroxypropyl Me, ethoxylated propoxylated; Elkem Silicones).
[0169] Examples of additives I that can be used include, but are not limited to: organic dyes or pigments, stabilizers introduced into silicone rubber to improve thermal stability, resistance to hot air, reversion, depolymerization under attack by traces of acid or water at high temperatures; plasticizers, release oils, or hydrophobizing oils without reactive alkenyl or SiH groups, such as polydimethylsiloxane oils; release agents such as fatty acid derivatives, fatty alcohol derivatives, fluoroalkyls; compatibilizers such as hydroxylated silicone oils; adhesion promoters and adhesion modifiers such as organosilanes.
[0170] In some embodiments, at least one additive I is an additive, such as a colorant or functional additive approved for use in the medical field, such as, for example, Mevopur® or Remafin® concentrate (Clariant).
[0171] It is believed that the cured silicone elastomer obtained by curing the addition curable liquid silicone composition X of the present invention can be used in medical applications such as long-term implantable / drug delivery device systems. In such systems, at least one additive I can be an active pharmaceutical ingredient, such as an active pharmaceutical ingredient having a terminal alkene, alkyne, or carbonyl functional group. Non-limiting examples of active pharmaceutical ingredients are hormones such as levonorgestrel, ethinyl estradiol, norethisterone, ethynodiol diacetate, desogestrel, lynestrenol, progesterone and mixtures thereof, synthetic hormones such as bimatoprost, corticosteroids such as dexamethasone, antiviral compounds such as pritelivir, fungicides such as dapiribine, and any combination thereof.
[0172] The present invention also relates to cured silicone elastomers obtainable by curing the addition-curable liquid silicone composition X as defined herein.
[0173] It has been advantageously demonstrated that the cured silicone elastomers obtained by curing the addition-curable liquid silicone composition X of the present invention exhibit improved mechanical properties.
[0174] In some embodiments, the tensile strength of the cured silicone elastomer obtained by curing the addition-curable liquid silicone composition X is increased compared to the cured silicone elastomer in the absence of organosiloxane gum C. For example, the tensile strength of the cured silicone elastomer obtained by curing the addition-curable liquid silicone composition X is at least 5% greater, at least 10% greater, at least 15% greater, or at least 20% greater than the tensile strength of the cured silicone elastomer in the absence of organosiloxane gum C. In some embodiments, the tensile strength of the cured silicone elastomer obtained by curing the addition-curable liquid silicone composition X is increased by at least 21% compared to the tensile strength of the cured silicone elastomer in the absence of organosiloxane gum C.
[0175] In some embodiments, the elongation at break of the cured silicone elastomer obtained by curing the addition-curable liquid silicone composition X is increased compared to the cured silicone elastomer in the absence of organosiloxane gum C. For example, the elongation at break of the cured silicone elastomer obtained by curing the addition-curable liquid silicone composition X is at least 5% greater, at least 10% greater, at least 15% greater, at least 20% greater, at least 25% greater, at least 30% greater, at least 35% greater, at least 40% greater, at least 45% greater, at least 50% greater, at least 55% greater, at least 60% greater, at least 65% greater, at least 70% greater, at least 75% greater, at least 80% greater, or at least 85% greater than the elongation at break of the cured silicone elastomer in the absence of organosiloxane gum C. In some embodiments, the elongation at break of the cured silicone elastomer obtained by curing the addition-curable liquid silicone composition X is increased by at least 87% compared to the elongation at break of the cured silicone elastomer in the absence of organosiloxane gum C.
[0176] In some embodiments, the tear strength of the cured silicone elastomer obtained by curing the addition-curable liquid silicone composition X is increased compared to the cured silicone elastomer in the absence of organosiloxane gum C. For example, the tear strength of the cured silicone elastomer obtained by curing the addition-curable liquid silicone composition X is at least 5% greater, at least 10% greater, at least 15% greater, at least 20% greater, at least 25% greater, at least 30% greater, at least 35% greater, at least 40% greater, at least 45% greater, at least 50% greater, at least 55% greater, at least 60% greater, at least 65% greater, at least 70% greater, or at least 75% greater than the tear strength of the cured silicone elastomer in the absence of organosiloxane gum C. In some embodiments, the tear strength of the cured silicone elastomer obtained by curing the addition-curable liquid silicone composition X is increased by at least 79% compared to the tear strength of the cured silicone elastomer in the absence of organosiloxane gum C.
[0177] The use of the addition-curable liquid silicone composition X according to the present invention in a 3D printer, such as an extrusion 3D printer or a material jetting 3D printer, is also provided herein.
[0178] In some embodiments, the addition-curable liquid silicone composition X according to the present invention can be used in the field of medical materials and / or devices. For example, a cured product comprising the addition-curable liquid silicone composition X according to the present invention is also provided, which may be suitable for use in a variety of applications, such as drug delivery devices, implant devices, medical tubes, gastric catheters, medical balloons, catheter balloons, artificial dialysis machines, hemodialysis machines, implant parts, chemical stoppers, O-rings, tubes of peristaltic drug delivery pumps, check valves, resuscitator valves, diaphragms for attaching limbs and suction cups of prostheses.
[0179] Also provided is the use of the cured silicone elastomers of the present invention in articles and / or products such as the medical or electronic devices described herein.
[0180] Other advantages provided by the present invention will become apparent from the following illustrative examples. EXAMPLES
[0181] Materials and Methods Preparation of Silicone Composition In the examples below, the following ingredients were used: A1: Linear α,ω-vinyl polydimethylsiloxane (average viscosity 20,000 mPa·s; Mn≒49,000 g / mol) A2: Linear α,ω-vinyl polydimethylsiloxane (average viscosity 4000 mPa s; Mn ≒ 31,000 g / mol) A3: Linear α,ω-vinyl polydimethylsiloxane (average viscosity 1000 mPa s; Mn ≒ 18,000 g / mol) A4: Linear α,ω-vinyl polydimethylsiloxane (average viscosity 200 mPa s; Mn ≒ 7,500 g / mol) B1: Trimethyl-terminated (dimethylsiloxane-methylhydrogensiloxane)-dimethylsiloxane copolymer (viscosity 18-26 mPa·s; SiH 17-23% by weight) B2: MH4Q silicone resin PH gum 1: Diphenylsiloxane-dimethylsiloxane-vinylmethylsiloxane copolymer gum (total phenyl content ≒ 12 mol%; total vinyl content ≒ 0.072 wt%; 0.01s -1 Viscosity at 63,578,000 mPa·s; Mn≒180,000 g / mol; consistency=540 (range 450-750) PH gum 2: vinyldimethyl terminated diphenylsiloxane-dimethylsiloxane copolymer gum (total phenyl content ≒ 10 mol%; total vinyl content ≒ 0.015 wt%; viscosity ≒ 64,000,000 mPa·s; Mn ≒ 180,000 g / mol); viscosity (consistency) = range 450-750 PH gum 3: vinyldimethyl terminated diphenylsiloxane-dimethylsiloxane copolymer gum (total phenyl content ≒ 30 mol%; total vinyl content ≒ 0.015 wt%; viscosity ≒ 64,000,000 mPa·s; Mn ≒ 180,000 g / mol); viscosity (consistency) = range 450-750 PH gum 4: Diphenylsiloxane-dimethylsiloxane-vinylmethylsiloxane copolymer gum (total phenyl content ≒ 12 mol%; total vinyl content ≒ 0.036 wt%; 0.01s -1 Viscosity at 59,700,000 mPa·s; Mn≒180,000 g / mol; consistency=672 (range 450-750) Ph oil: Vinyldimethyl-terminated diphenylsiloxane-dimethylsiloxane copolymer oil (total phenyl content ≒ 39 mol%; total vinyl content ≒ 0.70 wt%; viscosity 800 mPa s; Mn ≒ 7,400 g / mol) Gum 1: Terminal vinyldimethyl (vinylmethylsiloxane)-dimethylsiloxane copolymer gum (total vinyl content 0.04-0.06 wt%, viscosity >10,000,000 mPa·s, Mn ≒ 220,000 g / mol) Viscosity=648 (range 600~900) Gum 2: Trimethyl-terminated (vinylmethylsiloxane)-dimethylsiloxane copolymer gum (total vinyl content 0.0675-0.0825 wt%, viscosity at 0.01 s-1 19,290,000 mPa·s, Mn ≒ 220,000 g / mol) Viscosity = 692 (range 600-900) OH gum: hydroxy-terminated polydimethylsiloxane gum (total hydroxy content ≒ 0.01 wt%; viscosity > 10,000,000 mPa·s; Mn ≒ 220,000 g / mol) D1: Platinum catalyst solution: Platinum metal diluted in short linear α,ω-vinylpolydimethylsiloxane oil (wt% in platinum = 3.38) D2: Platinum catalyst solution: Platinum metal diluted in short linear α,ω-vinyl polydimethylsiloxane oil (wt% in platinum=10) E1: In situ treated hydrophilic fumed silica (AEROSIL® 300 treated with hexamethyldisilazane) E2: In-situ treated hydrophilic fumed silica (AEROSIL® 300 treated with hexamethyldisilazane and divinyltetramethyldisilazane) F: α,ω-hydridopolydimethylsiloxane (H-PDMS-H) (viscosity 7-10 mPa.s; Mn ≒ 750 g / mol) G1: ECH (1-ethynyl-1-cyclohexanol) G2: Tetramethyltetravinylcyclotetrasiloxane
[0182] method 1) 3D geometry and STL files - A 50% filled cubic grid with dimensions 20mm x 20mm x 20mm. STL file created in Cura 2.0, sliced and saved to SD card. -Printing parameters (unchanged throughout) are built in: speed, extrusion rate, layer height, etc.
[0183] 2) Printers and dispensers -Ultimaker2+ 3D printer combined with Structur3d's Discov3ry Paste Extruder - 60cc PE Luer Lock Syringe with Standard Plunger from Genesis Instruments, Luer Lock connection and .41mm diameter conical nozzle (both from Nordson EFD).
[0184] 3) 3D printing suitability test After curing, the 3D printed silicone elastomers were visually inspected and characterized according to the following criteria: - Excellent: The 3D printed article maintains all structural integrity and high fidelity with respect to the CAD file rendering, in both the uncured and cured states. - "Good": The 3D printed article maintains most of its structural integrity, but may have lost some fidelity with respect to the CAD file's rendering due to slumping, crumbling, or warping in both the uncured and cured states. - "Fair": The 3D printed article maintains some structural integrity but may have lost some fidelity with respect to the CAD file's rendering due to slumping, crumbling, or warping in both the uncured and cured states. - "No Good": The 3D printed article maintains little or no structural integrity and shows little or no fidelity to the rendering in the CAD file.
[0185] 4) Rheological behavior - relaxation time - Rheological measurements were performed at Anton Paar using a sweep analysis gap = 0.300 mm, temperature = 25.0 °C, applied shear rate = 1 rads-1, and displacement profile = viscoelastic. -Storage modulus is a measure of the energy stored in a material when deformation is applied ("applied shear rate"). -The thixotropic behavior of the formulations was characterized by determining the recovery or relaxation time. This was obtained from the measurement of the evolution of the storage modulus over time after a shear pretreatment. The purpose of this shear pretreatment is to simulate the effect of the flow in a printer nozzle. The recovery time was then defined by the intersection point between the lines tangent to the initial and final parts of the storage modulus curve.
[0186] 5) Mechanical properties The following mechanical properties were evaluated according to the method described in standard ASTM D412: durometer Shore A / Shore OO, tensile strength, elongation at break, tear strength, hardness, and modulus of elasticity.
[0187] Example 1 - Exemplary compositions of the present invention. Silicone compositions defined in Table 1 below were 3D printed at room temperature as described above, followed by heating for 30 minutes to 150° C. Rheological measurements were performed separately as described above.
[0188] [Table 1]
[0189] The introduction of a phenyl-containing gum (Ph Gum 1) significantly improved the 3D printability of the liquid silicone composition and maintained the liquid silicone composition's ability to cure under heat, as shown in Table 1 and Figure 1. The presence of phenyl groups in the backbone induces thixotropic behavior as indicated by rapid relaxation times (Table 1).
[0190] Substitution of the phenyl-containing gums with gums containing other functional groups such as hydroxyl (OH gum) or vinyl functional groups (Gum 1 and Gum 2) did not result in the same thixotropic effect, as shown by the comparative examples Comparatives 2-4 in Table 1 above and Figure 2.
[0191] Representative photographs of the 3D printed compositions are provided in FIG. 1 for Comparative Example 1 (Comp1, no gum, FIG. 1A), Exemplary Composition 1 (Ex. 1, phenyl gum (Ph Gum 1), FIG. 1B), and Comparative Composition 2 (Comp. 2, vinyl gum (Gum 2), FIG. 1E). Only Ex. 1 (FIG. 1B) held its shape without collapsing.
[0192] Example 2 - Effects of various amounts of phenyl-containing gum Low durometer silicone compositions were formulated and evaluated containing different amounts of Ph Gum 1. To make up for the loss of Ph Gum 1, Gum 2 was added to make up for the loss of Ph Gum 1 to make up for the final 100%.
[0193] Silicone compositions defined in Table 2 below were 3D printed at room temperature as described above, followed by heating to 150°C for 30 minutes. Rheological measurements were performed separately as described above. After curing at 150°C for 30 minutes followed by 115°C for 30 minutes, mechanical properties were measured as described above. Results are shown in Table 2. Thixotropic properties are shown in Figure 3.
[0194] [Table 2]
[0195] As shown in Table 2, Figure 1, and Figure 3, the 3D printability and thixotropic behavior of the liquid silicone compositions deteriorated as the percentage of phenyl-containing gum in the composition decreased. In particular, Figure 1B shows a representative photograph of the 3D printed composition of Example 1, Figure 1C shows a representative photograph of the 3D printed composition of Example 2, Figure 1D shows a representative photograph of the 3D printed composition of Example 3, Figure 1E shows a representative photograph of the 3D printed composition of Example 4, and Figure 1F shows a representative photograph of the 3D printed composition of Comparative 2.
[0196] Example 3 – Effects of various phenyl-containing gums and oils Silicone compositions defined in Table 3 below were 3D printed at room temperature as described above, followed by heating for 30 minutes to 150° C. Rheological measurements were performed separately as described above.
[0197] [Table 3]
[0198] As shown in Table 3 and Figure 4, liquid silicone compositions containing organosiloxanes with low phenyl content (less than 30 mol%) performed better than liquid silicone compositions containing organosiloxanes with high phenyl content (greater than 30 mol%), even though the total mole percent of phenyl in the composition was maintained at 2.4%. Specifically, Examples 1 and 5, which contain gums with phenyl content of 12 mol% (Ph Gum 1) or 10 mol% (Ph Gum 2), respectively, exhibited favorable relaxation times and Log 10 In contrast, Example 6, which includes a gum with a phenyl content of 30 mol % (Ph Gum 3), exhibited a longer relaxation time and a lower Log (storage modulus) even though the total mol % of phenyl in the composition was maintained at 2.4%. 10(storage modulus). This does not appear to be due to a change in viscosity, as the addition of Gum 2 (a vinyl gum) maintained the total gum % at 20%. Increasing the amount of Ph Gum 3 to 20% (Example 7) improved the results, suggesting that both the amount of phenyl gum in the composition and the phenyl content of the gum are important to the overall properties of the composition.
[0199] The use of a phenyl-containing organosiloxane oil having a higher phenyl content (Comparative 5) also resulted in longer relaxation times and lower Log 10 (storage modulus).
[0200] Example 4 - High hardness silicone elastomer Silicone compositions, defined in Table 4 below, were 3D printed at room temperature as described above, followed by heating to 150° C. for 30 minutes. Rheological measurements were performed separately as described above. Mechanical properties were measured as described above after curing at 150° C. for 30 minutes and at 115° C. for a further 30 minutes.
[0201] [Table 4]
[0202] As shown in Table 4 and Figure 5, the use of phenyl-containing organosiloxane gum (Ph Gum 1) in place of phenyl-containing organosiloxane oil (Ph Oil 3) improved the 3D printability of the resulting liquid silicone composition. Figure 5A shows a representative photograph of the 3D printed composition of Comparative 6, Figure 5B shows a representative photograph of the 3D printed composition of Example 8, and Figure 5C shows a representative photograph of the 3D printed composition of Example 9. Example 8 exhibited some internal collapse that was not evident from Figure 5B, and therefore is characterized in Table 4 as having a 3D printability of "Fair."
[0203] Furthermore, the cured silicone elastomers containing the phenyl-containing organosiloxane gums exhibited superior mechanical properties (e.g., higher tensile strength, elongation at break, and tear strength) compared to the cured silicone elastomers containing the phenyl-containing organosiloxane oils. In particular, the cured silicone elastomers containing the phenyl-containing organosiloxane gums of the present invention exhibited at least a 21% increase in tensile strength, at least an 87% increase in elongation at break, and at least a 79% increase in tear strength compared to the cured silicone elastomers containing the phenyl-containing organosiloxane oils.
[0204] Example 5 - Comparison of thixotropic properties of Ph Gum 1 and Gum 2 As shown in the above examples, both low and high durometer silicone compositions containing phenyl-containing gums outperformed silicone compositions containing similar gums without phenyl groups. Therefore, three of the gums used in the above examples (Ph Gum 1, Gum 1, and Gum 2) were compared to determine whether their thixotropic properties could contribute to this effect. An additional phenyl gum with similar properties to Ph Gum 1 was also studied (Ph Gum 4; vinyl dimethyl terminated diphenylsiloxane-dimethylsiloxane copolymer gum (total phenyl content ≈ 30 mol %; total vinyl content ≈ 0.036 wt %; viscosity ≈ 64,000,000 mPa·s; Mn ≈ 180,000 g / mol)).
[0205] The consistency is measured at 25 °C by a penetrometer of PNR12 or an equivalent model that allows applying a cylindrical head to the sample under standardized conditions. The gum hardness is expressed as 10 times the depth (in mm) that the shape memory cylinder penetrates into the sample in 1 minute. To do this, the gum sample is placed in an aluminium container with a diameter of 40 mm and a height of 60 mm. A bronze or brass cylindrical head with a diameter of 6.35 mm and a height of 4.76 mm is attached to a metal rod with a length of 51 mm and a diameter of 3 mm suitable for the penetrometer. A load of 100 g is attached to this rod. The total weight of the assembly is 151.8 g. The gum sample container is placed in a bath set at 25 °C ± 0.5 °C for a minimum of 30 seconds. The measurement is carried out according to the manufacturer's instructions.
[0206] The viscosity of the gum was measured using an Anton Paar type rheometer or a zero gap set between two plateaus of 0.300 mm and a viscosity of 0.01 s at 25.0 °C. -1 ~100s -1 The shear rate range was measured using an equivalent rheometer with a shear rate range between
[0207] Table 5 shows the viscosity and consistency values for each of these gums. Figure 6 provides the thixotropic properties on both linear (Figure 6A) and logarithmic (Figure 6B) scales. Both phenyl gums (Ph Gum 1 and Ph Gum 4) were more viscous than the vinyl gums (Gum 1 and Gum 2) at low shear rates (e.g., 0.01 s-1). However, at higher shear rates (e.g., 0.3 s-1 and above), the viscosities of all four gums were similar.
[0208] [Table 5]
[0209] Example 6 - Effect of fillers A series of samples containing phenyl gum (Ph gum 1), filler (HMDZ treated silica (E1)), and linear α,ω-vinyl polydimethylsiloxane (average viscosity 60000; PDMS fluid) were made in four combinations (no phenyl gum / no filler, no phenyl gum / no filler, phenyl gum / no filler, phenyl gum / no filler). 20% phenyl gum and 1% filler were added. The aim was to determine where the thixotropic effect came from, rather than simply an increase in viscosity. It was found that all four samples showed a significant increase in viscosity but did not exhibit thixotropic properties. A filler content of 1 wt% was insufficient. Further samples of 50% phenyl gum and 50% PDMS fluid were made, again increasing the viscosity but not the thixotropic properties. Given that typical combinations of PDMS fluids and concentrated fillers (>25%) also do not exhibit thixotropic properties, these factors alone cannot render a composition 3D printable, but rather a synergistic effect between the phenyl content of the gum and the filler is necessary.
[0210] All references cited herein are incorporated by reference as if each reference was specifically and individually indicated to be incorporated by reference. The citation of a reference is for its disclosure prior to the filing date and should not be construed as an admission that the present disclosure is not entitled to antedate such reference by virtue of prior invention.
[0211] It is understood that each of the above elements, or a collection of two or more, may also find useful application in other types of methods different from the types described above. Without further analysis, the foregoing fully reveals the gist of the present disclosure, so that others can easily adapt it to various applications by applying their current knowledge, without omitting features that, in the light of the prior art, fairly constitute essential features of the general or specific aspects of the present disclosure as set forth in the appended claims. The above-described embodiments are presented only as examples. The scope of the present disclosure should be limited only by the scope of the claims.
Claims
1. 1. A method for additively manufacturing a silicone elastomeric article, comprising the steps of: 1) printing a first addition curable liquid silicone composition onto a substrate using a 3D printer selected from an extrusion 3D printer or a material jetting 3D printer to form a first layer; 2) printing a second curable silicone composition onto the first layer or a previous layer with the 3D printer to form a subsequent layer; 3) optionally repeating step 2) for any additional layers desired, using independently selected addition-curable liquid silicone compositions; 4) Crosslinking said first and subsequent layers, optionally by heating, to obtain a cured silicone elastomeric article. Including; At least one layer of the addition-curable liquid silicone composition is an addition-curable liquid silicone composition X, the curable silicone composition X comprising: (A) at least two silicon bonds C per molecule 2 ~C 20 At least one organopolysiloxane A containing alkenyl groups; (B) at least one organosilicon crosslinker B containing at least two silicon-bonded hydrogen atoms per molecule; (C) at least one organopolysiloxane gum C having a consistency of 200 to 900 at 25° C., and containing at least one silicon-bonded C per molecule; 2 ~C 20 Alkenyl group and at least one silicon bond C per molecule 6 ~C 12 at least one organopolysiloxane gum C containing aryl groups; (D) at least one addition reaction catalyst D; (E) at least one filler E; (F) optionally, at least one diorganohydrogensiloxy-terminated diorganopolysiloxane chain extender F; (G) optionally at least one cure rate modifier G; (H) optionally at least one silicone resin H; and (I) Optionally, at least one additive I A method comprising:
2. At least two silicon bonds C per molecule 2 ~C 20 2. The method according to claim 1, wherein the at least one organopolysiloxane A containing alkenyl groups is of the following formula (1): [Formula 1] During the ceremony, -n is an integer ranging from 1 to 1000, -R is independently C 1 ~C 20 Alkyl group, or C 6 ~C 12 Aryl group, or C 2 ~C 20 alkenyl groups, -R' is independently C 2 ~C 20 alkenyl groups, -R" is C 1 ~C 20 Alkyl group, or C 6 ~C 12 aryl groups.
3. At least two silicon bonds C per molecule 2 ~C 20 3. The method according to claim 1 or 2, wherein the at least one organopolysiloxane A containing alkenyl groups is of the following formula (1): [chemical 2] During the ceremony, -n is an integer ranging from 1 to 1000, -R is a methyl group; -R' is a vinyl group, -R" is a methyl group.
4. The at least one organosilicon crosslinker B, containing at least two silicon-bonded hydrogen atoms per molecule, is (i) at least two siloxy units of the same or different formula (XL-1): (H) (Z) e SiO (3-e) / 2 (XL-1) During the ceremony, The symbol H represents a hydrogen atom, the symbol Z represents an alkyl group containing 1 to 8 carbon atoms, the symbol e is equal to 0, 1 or 2; and (ii) at least one siloxy unit of formula (XL-2): (Z) g SiO (4-g) / 2 (XL-2) During the ceremony, The symbol Z is an alkyl group having 1 to 8 carbon atoms or 6 ~C 12 represents an aryl group, the symbol g is equal to 0, 1, 2 or 3; Including, The method according to any one of claims 1 to 3, wherein Z in XL-1 and XL-2 may be the same or different.
5. 5. The method of claim 4, wherein said at least one organosilicon crosslinker B comprises from 3 to 60 siloxy units of formula (XL-1) and from 1 to 250 siloxy units of formula (XL-2).
6. At least one silicon bond C per molecule 2 ~C 20 Alkenyl group and at least one silicon bond C per molecule 6 ~C 12 The method according to any one of claims 1 to 5, wherein the at least one organopolysiloxane gum C containing aryl groups comprises: At least one siloxy unit of formula (A-3): (Alk) (R) h SiO (3-h) / 2 (A-3) In the formula, the symbol "Alk" is C 2 ~C 20 represents an alkenyl group, and the symbol R is C 1 ~C 20 Alkyl, or C 6 ~C 12 represents an aryl group, in which "Alk" and R in each occurrence may be the same or different; h=1 or 2; At least one siloxy unit of formula (A-4): (Ar) k (R 1 ) h SiO (4-h-k) / 2 (A-4) In the formula, the symbol "Ar" is C 6 ~C 12 An aryl group (optionally C 2 ~C 20 substituted by an alkylene group), or C 1 ~C 20 Aralkyl (optionally C 2 ~C 20 substituted by an alkylene group), or a naphthyl group (optionally 1 ~C 20 Alkyl group and / or C 2 ~C 20 alkylene group), or anthracenyl group (optionally C 1 ~C 20 Alkyl group and / or C 2 ~C 20 substituted with an alkylene group; 1 is C 1 ~C 20 Alkyl group, or C 2 ~C 20 alkenyl group, and in each case "Ar" and R 1 may be the same or different, h=0, 1 or 2; k=1 or 2 and h+k=1, 2, or 3; Other siloxy units of formula (A-2): (L) g SiO (4-g) / 2 (A-2) In the formula, the symbol L is C 1 ~C 20 where the symbol g is equal to 0, 1, 2, or 3, and in each occurrence L may be the same or different.
7. At least one silicon bond C per molecule 2 ~C 20 Alkenyl group and at least one silicon bond C per molecule 6 ~C 12 The method according to any one of claims 1 to 6, wherein the at least one organopolysiloxane gum C containing aryl groups comprises: At least one siloxy unit of formula (A-3): (Alk) (R) h SiO (3-h) / 2 (A-3) In the formula, the symbol "Alk" represents a vinyl group, and the symbol R represents C 1 ~C 20 represents an alkyl group, in which "Alk" and R in each occurrence may be the same or different; h=1 or 2; At least one siloxy unit of formula (A-4): (Ar) k (R 1 ) h SiO (4-h-k) / 2 (A-4) In the formula, the symbol "Ar" represents a phenyl group, and the symbol R 1 is C 1 ~C 20 Alkyl group, or C 2 ~C 20 alkenyl group, and in each case "Ar" and R 1 may be the same or different, h=0 or 1; k=2; Other siloxy units of formula (A-2): (L) g SiO (4-g) / 2 (A-2) In the formula, the symbol L is C 1 ~C 20where the symbol g is equal to 0, 1, 2, or 3, and in each occurrence L may be the same or different.
8. At least one silicon bond C per molecule 2 ~C 20 Alkenyl group and at least one silicon bond C per molecule 6 ~C 12 8. The method according to claim 1, wherein the at least one organopolysiloxane gum C containing aryl groups is a diphenylsiloxane-dimethylsiloxane-vinylmethylsiloxane copolymer gum.
9. At least one silicon bond C per molecule 2 ~C 20 Alkenyl group and at least one silicon bond C per molecule 6 ~C 12 9. The method according to claim 1, wherein the at least one organopolysiloxane gum C containing aryl groups is vinyl terminated.
10. At least one silicon bond C per molecule 2 ~C 20 Alkenyl group and at least one silicon bond C per molecule 6 ~C 12 10. The method according to claim 1, wherein the at least one organopolysiloxane gum C containing aryl groups contains less than 30 mol % of aryl groups.
11. At least one silicon bond C per molecule 2 ~C 20 Alkenyl group and at least one silicon bond C per molecule 6 ~C 12 11. The method according to claim 1, wherein the at least one organopolysiloxane gum C containing aryl groups comprises from about 10 mol % to about 20 mol % of aryl groups.
12. The method according to any one of claims 1 to 11, wherein said catalyst D is a platinum group metal-containing catalyst.
13. 13. The method according to claim 1, wherein the at least one filler E is a fumed silica treated with at least one compatibilizer in the presence of at least a portion of the at least one organopolysiloxane A carrying alkenyl groups.
14. The method according to any one of claims 1 to 13, wherein the 3D printer is an extrusion 3D printer.
15. An addition-curable liquid silicone composition X for additively manufacturing silicone elastomer articles, comprising: (A) at least two silicon bonds C per molecule 2 ~C 20 At least one organopolysiloxane A containing alkenyl groups; (B) at least one organosilicon crosslinker B containing at least two silicon-bonded hydrogen atoms per molecule; (C) at least one organopolysiloxane gum C having a consistency of 200 to 900 at 25° C., and containing at least one silicon-bonded C per molecule; 2 ~C 20 Alkenyl group and at least one silicon bond C per molecule 6 ~C 12 at least one organopolysiloxane gum C containing aryl groups; (D) at least one addition reaction catalyst D; (E) at least one filler E; (F) optionally, at least one diorganohydrogensiloxy-terminated diorganopolysiloxane chain extender F; (G) optionally at least one cure rate modifier G; (H) optionally at least one silicone resin H; and (I) Optionally, at least one additive I.
16. At least two silicon bonds C per molecule 2 ~C 20 The addition-curable liquid silicone composition X according to claim 15, wherein the at least one organopolysiloxane A having an alkenyl group is represented by the following formula (1): [C3] During the ceremony, -n is an integer ranging from 1 to 1000, -R is independently C 1 ~C 20 Alkyl group, or C 6 ~C 12 Aryl group, or C 2 ~C 20 alkenyl groups, -R' is independently C 2 ~C 20 alkenyl groups, -R" is independently C 1 ~C 20 Alkyl group, or C 6 ~C 12 aryl groups.
17. At least two silicon bonds C per molecule 2 ~C 20 The addition-curable liquid silicone composition X according to claim 15 or 16, wherein the at least one organopolysiloxane A having an alkenyl group is represented by the following formula (1): [C4] During the ceremony, -n is an integer ranging from 1 to 1000, -R is a methyl group; -R' is a vinyl group, -R" is a methyl group.
18. The at least one organosilicon crosslinker B, containing at least two silicon-bonded hydrogen atoms per molecule, is (i) at least two siloxy units of the same or different formula (XL-1): (H) (Z) e SiO (3-e) / 2 (XL-1) During the ceremony, The symbol H represents a hydrogen atom, the symbol Z represents an alkyl group containing 1 to 8 carbon atoms, the symbol e is equal to 0, 1 or 2; and (ii) at least one siloxy unit of formula (XL-2): (Z) g SiO (4-g) / 2 (XL-2) During the ceremony, The symbol Z is an alkyl group having 1 to 8 carbon atoms or 6 ~C 12 represents an aryl group, the symbol g is equal to 0, 1, 2 or 3; Including, The addition-curable liquid silicone composition X according to any one of claims 15 to 17, wherein Z in XL-1 and XL-2 may be the same or different.
19. 19. The addition-curable liquid silicone composition X of claim 18, wherein the at least one organosilicon crosslinker B comprises 3 to 60 siloxy units of formula (XL-1) and 1 to 250 siloxy units of formula (XL-2).
20. At least one silicon bond C per molecule 2 ~C 20 Alkenyl group and at least one silicon bond C per molecule 6 ~C 12 The addition-curable liquid silicone composition X according to any one of claims 15 to 19, wherein the at least one organopolysiloxane gum C containing aryl groups comprises: At least one siloxy unit of formula (A-3): (Alk) (R) h SiO (3-h) / 2 (A-3) In the formula, the symbol "Alk" is C 2 ~C 20 represents an alkenyl group, and the symbol R is C 1 ~C 20 Alkyl group, or C 6 ~C 12 represents an aryl group, in which "Alk" and R in each occurrence may be the same or different; h=1 or 2; At least one siloxy unit of formula (A-4): (Ar) k (R 1 ) h SiO (4-h-k) / 2 (A-4) In the formula, the symbol "Ar" is C 6 ~C 12 An aryl group (optionally C 2 ~C 20 substituted by an alkylene group), or C 1 ~C 20 Aralkyl (optionally C 2 ~C 20 substituted by an alkylene group), or a naphthyl group (optionally 1 ~C 20 Alkyl group and / or C 2 ~C 20 alkylene group), or anthracenyl group (optionally C 1 ~C 20 Alkyl group and / or C 2 ~C 20 substituted with an alkylene group; 1 is C 1 ~C 20 Alkyl group, or C 2 ~C 20 alkenyl group, and in each case "Ar" and R 1 may be the same or different, h=0, 1 or 2; k=1 or 2 and h+k=1, 2, or 3; Other siloxy units of formula (A-2): (L) g SiO (4-g) / 2 (A-2) In the formula, the symbol L is C 1 ~C 20where the symbol g is equal to 0, 1, 2, or 3, and in each occurrence L may be the same or different.
21. At least one silicon bond C per molecule 2 ~C 20 Alkenyl group and at least one silicon bond C per molecule 6 ~C 12 The addition-curable liquid silicone composition X according to any one of claims 15 to 20, wherein the at least one organopolysiloxane gum C containing aryl groups comprises: At least one siloxy unit of formula (A-3): (Alk) (R) h SiO (3-h) / 2 (A-3) In the formula, the symbol "Alk" represents a vinyl group, and the symbol R represents C 1 ~C 20 Alkyl group or C 6 ~C 12 represents an aryl group, in which "Alk" and R in each occurrence may be the same or different; h=1 or 2; At least one siloxy unit of formula (A-4): (Ar) k (R 1 ) h SiO (4-h-k) / 2 (A-4) In the formula, the symbol "Ar" represents a phenyl group, and the symbol R 1 is C 1 ~C 20 Alkyl group, or C 2 ~C 20 alkenyl group, and in each case "Ar" and R 1 may be the same or different, h=0 or 1; k=2; Other siloxy units of formula (A-2): (L) g SiO (4-g) / 2 (A-2) In the formula, the symbol L is C 1 ~C 20where the symbol g is equal to 0, 1, 2, or 3, and in each occurrence L may be the same or different.
22. At least one silicon bond C per molecule 2 ~C 20 Alkenyl group and at least one silicon bond C per molecule 6 ~C 12 The addition-curable liquid silicone composition X according to any one of claims 15 to 21, wherein the at least one organopolysiloxane gum C containing aryl groups is a diphenylsiloxane-dimethylsiloxane-vinylmethylsiloxane copolymer gum.
23. At least one silicon bond C per molecule 2 ~C 20 Alkenyl group and at least one silicon bond C per molecule 6 ~C 12 The addition-curable liquid silicone composition X according to any one of claims 15 to 22, wherein the at least one organopolysiloxane gum C containing aryl groups has a vinyl end.
24. At least one silicon bond C per molecule 2 ~C 20 Alkenyl group and at least one silicon bond C per molecule 6 ~C 12 The addition-curable liquid silicone composition X according to any one of claims 15 to 23, wherein the at least one organopolysiloxane gum C containing aryl groups contains less than 30 mol % of aryl groups.
25. At least one silicon bond C per molecule 2 ~C 20 Alkenyl group and at least one silicon bond C per molecule 6 ~C 12 The addition-curable liquid silicone composition X according to any one of claims 15 to 24, wherein the at least one organopolysiloxane gum C containing aryl groups comprises from about 10 mol % to about 20 mol % of aryl groups.
26. The addition-curable liquid silicone composition X according to any one of claims 15 to 25, wherein the catalyst D is a platinum group metal-containing catalyst.
27. The addition-curable liquid silicone composition X according to any one of claims 15 to 26, wherein the at least one filler E is a fumed silica that has been treated with at least one compatibilizer in the presence of at least a portion of the at least one organopolysiloxane A having alkenyl groups.
28. Use of the addition-curable liquid silicone composition X according to any one of claims 15 to 27 in a 3D printer.
29. 29. The use according to claim 28, wherein the 3D printer is selected from an extrusion 3D printer or a material jetting 3D printer.
Citation Information
Patent Citations
Dual component liquid silica gel for 3D printing and printing method thereof
CN110128833A
Heattcurable silicone rubber composition
JP1981041252A
Polyorganosiloxane composition
JP1985088069A
Low-temperature curing silicone elastomer
JP2019504919A
Silicone formulations for 3D printing
US20190100626A1