High strength superalloys for thermal power generating units and their processing processes

A high-strength superalloy with a tailored composition and processing method addresses the limitations of existing materials for thermal power generation units, achieving superior mechanical properties at high temperatures and cost-effectiveness.

JP7564238B2Active Publication Date: 2024-10-08HUANENG POWER INT INC +1
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
JP2022564104
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2020-05-08
Filing Date
2021-05-08
Publication Date
2024-10-08
Estimated Expiration
2041-05-08

AI Technical Summary

Technical Problem

Existing materials for large-diameter, thick-walled pipes in thermal power generation units, such as ferritic and austenitic heat-resistant steels, fail to meet the performance requirements at high temperatures exceeding 700°C, particularly in terms of strength, durability, and corrosion resistance, while nickel-based superalloys are expensive and have poor welding performance.

Method used

A high-strength superalloy with a specific composition (0.05% to 0.08% C, 14% to 17% Cr, 0.5% to 2.5% W, 0.3% to 2.0% Mo, 2.0% to 2.5% Ti, 1.0% to 1.5% Al, 0.003% to 0.03% Zr, 37% to 48% Fe, and the remainder Ni) is developed, processed through smelting, homogenization, forging, high-temperature rolling, and aging treatments to achieve optimal mechanical properties.

Benefits of technology

The superalloy exhibits excellent high-temperature strength with yield strength over 540 MPa and elongation ratio over 12% at 700°C, reducing material costs and simplifying the manufacturing process.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007564238000001
    Figure 0007564238000001
  • Figure 0007564238000002
    Figure 0007564238000002
  • Figure 0007564238000003
    Figure 0007564238000003
Patent Text Reader

Abstract

The present invention relates to a high-strength superalloy for thermal power generation units and its processing process. The superalloy contains, by mass, 0.05-0.08% C, 14-17% Cr, up to 0.5% Mn, up to 0.5% Si, 1.0-2.5% W, 0.3-2.0% Mo, 2.0-2.5% Ti, 1.0-1.5% Al, up to 0.003% B, up to 0.03% Zr, 37-48% Fe, and a margin of Ni. The pre-blended alloy furnace material is smelted in an electric arc furnace under a maximum vacuum of no more than 0.5 Pa. The alloy is billet-forged at a temperature 200-250°C above the Ni3Al (γ') precipitation temperature with a deformation of 70%, and hot-rolled at a temperature 150-200°C above the γ' precipitation temperature with a deformation of 80%. The alloy has excellent high-temperature mechanical properties above 650°C.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention belongs to the field of materials and material preparation, and specifically relates to a high-strength superalloy for thermal power generation units and its processing process, which can meet the processing and usage performance requirements of thick-walled parts such as main steam pipes and headers of advanced ultra-supercritical thermal power generation units at the 700°C level. [Background technology]

[0002] With the increasing demand for electricity in China, the problems of energy shortage and environmental pollution are becoming more and more evident, and there is an urgent need to develop a highly efficient, energy-saving and environmentally friendly power generation method. Thermal power generation has long been the most important power generation technology in China, and improving the steam parameters of the unit is considered to be the most effective way to solve the above problems. A large number of previous practices have shown that the service performance of key component materials is the most major cause of limiting the improvement of steam parameters of boiler units. In the boiler of a thermal power generation unit, as one of the key components with the most severe usage conditions, large-diameter thick-walled pipes such as main steam pipes and headers put forward very high requirements for the usage performance of materials. With the great improvement of the main steam parameters of thermal power generation units, the thermal power generation industry is urgently required to develop superalloy materials with excellent processing performance that can meet the performance requirements of large-diameter thick-walled pipes of 700℃-level units.

[0003] At present, ferritic heat-resistant steels (9~12wt.%Cr) and austenitic heat-resistant steels are mainly selected and used for large-diameter thick-walled pipes of thermal power generating units below 600℃ level in China and abroad. Commonly used ferritic heat-resistant steels are mainly TP91, NF616, E911, HCM12A, etc. These materials have excellent durability and corrosion resistance, so they are widely used for large-diameter thick-walled pipes of units below 600℃ level. Among them, TP91 has been fully domestically produced and widely applied in China's subcritical and supercritical thermal power generating units, and a large amount of performance data has been accumulated. All these data and practices show that ferritic heat-resistant steels are difficult to meet the performance requirements of high-temperature parameters for the performance of large-diameter thick-walled pipe materials. Compared to ferritic heat-resistant steels, austenitic heat-resistant steels such as coarse crystal (TP304H, TP347H), fine crystal (Super304H, TP347HFG) and high chromium (HR3C, NF709, SAVE25) are superior in durability, oxidation resistance and corrosion performance. However, they also have many problems in the application process, such as low heat transfer efficiency, high thermal expansion coefficient and high cost. In particular, when the main steam temperature exceeds 700℃, the strength of austenitic heat-resistant steels cannot meet the performance requirements for large diameter thick wall pipes.

[0004] In response to the requirements for material performance of large diameter thick wall pipes of 700℃ level ultra supercritical unit boilers, currently overseas, a series of nickel-based irregular superalloy materials have been developed, such as Inconel74H developed by US Specialty Metals, Haynes282 developed by Hastelloy, US, CCA617 developed by ThyssenKrupp, Germany, Nimonic263 developed by Rolls-Royce, UK, and USC41 developed by Hitachi, Japan. These materials have excellent high temperature endurance strength and oxidation resistance, but are expensive, have poor welding performance, and have high technical requirements such as smelting and heat treatment, which restrict their rapid popularization and application. In addition, Sumitomo of Japan has also developed iron-nickel-based superalloys such as HR6W and HR35, and Santwick of Sweden has developed Sanicro25 iron-nickel-based alloy, and Shenyang Institute of Metallurgy and Institute of Steel Research of the Chinese Academy of Sciences in China have also developed iron-nickel-based irregular superalloys such as GH2984 and GH110. Although some of the above iron-nickel-based superalloys have advantages in terms of raw material cost compared with nickel-based special-shaped superalloys, they have low thermal strength, poor structural stability and corrosion resistance, and at the same time, they need to be deformed to obtain the structure and performance required for use, which makes the preparation and processing process complicated, the overall manufacturing cost high, and it is difficult to further improve the performance. Summary of the Invention [Problem to be solved by the invention]

[0005] The present invention aims to solve the problems of the prior art and to provide a high-strength superalloy for thermal power generation units and a processing process thereof. [Means for solving the problem]

[0006] In order to achieve the above objectives, the present invention adopts the following technical solutions: High strength superalloys for thermal power generation units contain, by mass%, 0.05% to 0.08% C, 14% to 17% Cr, 0.5% or less Mn, 0.5% or less Si, 1.0% to 2.5% W, 0.3% to 2.0% Mo, 2.0% to 2.5% Ti, 1.0% to 1.5% Al, 0.003% or less B, 0.03% or less Zr, 37% to 48% Fe, and remainder As Ni It consists of .

[0007] The preparation process of high strength superalloy for thermal power generation unit includes the following steps: Step (1)--Smelting and homogenization: In mass%, 0.05%-0.08% C, 14%-17% Cr, 0.5% Mn or less, 0.5% Si or less, 1.0%-2.5% W, 0.3%-2.0% Mo, 2.0%-2.5% Ti, 1.0%-1.5% Al, 0.003% B or less, 0.03% Zr or less, 37%-48% Fe, and remainder Ni is taken as the starting material, and Cr, Ni, W, Si, Mn, Mo, and Fe are melted and refined under vacuum. Then, Al, Ti, B, Zr, and C are added under the protection of argon gas, and the material is cast and solidified. Finally, a homogenization treatment is performed, and the material is air-cooled to room temperature.

[0008] Step (2)--Forging and billeting: The alloy refined and homogenized in step (1) is billeted and forged at a temperature 200°C to 250°C higher than the γ' precipitation temperature, with the deformation amount of each pass being 30% or more, and the final total deformation amount being 70% or more.

[0009] Step (3)--Hot rolling: The alloy forged and billeted in step (2) is hot rolled at a temperature 150°C to 200°C higher than the γ' precipitation temperature, with the deformation amount of each pass being 35% or more, and the final total deformation amount being 80% or more.

[0010] Step (4)--High temperature solubilization and aging treatment: The alloy hot-rolled in step (3) is subjected to high temperature solubilization and aging treatment.

[0011] A further improvement of the present invention is that the refining time in step (1) is 0.5-1 hour.

[0012] A further improvement of the present invention is that in the specific process of step (1), when the vacuum degree reaches 0.3 Pa-0.5 Pa, Cr, Ni, W, Si, Mn, Mo and Fe are melted, coke is added for deoxidation, and the added mass of coke deoxidation does not exceed 25%-50% of the mass of C, then Ni-Mg alloy is added for secondary deoxidation, and finally Al, Ti, B, Zr and C are added, and after stirring for 5 minutes-10 minutes, it is taken out of the furnace for casting, the casting temperature is not less than 1600°C, and then solidified, and finally homogenized, and then air-cooled to room temperature.

[0013] A further improvement of the present invention is to use a mold during casting in step (1) and to coat the surface of the molten steel with an aluminum exothermic agent during solidification.

[0014] A further improvement of the present invention is that in step (1), the specific homogenization treatment is to increase the temperature from room temperature to 1050° C. to 1120° C. at a rate of 10° C. / min to 30° C. / min, and then maintain the temperature for 24 hours.

[0015] A further improvement of the present invention is that in step (1), after solidification, the mixture is kept at 900° C. to 980° C. for 1.0 to 1.5 hours, and then a homogenization treatment is performed.

[0016] A further improvement of the present invention is that in step (2), after each pass of forging and billet is completed, the billet is returned to the furnace for warming, and the warming time T and the out-furnace time t satisfy 5t≦T≦10t.

[0017] A further improvement of the present invention is that in step (3), after each pass of hot rolling is completed, the material is returned to the furnace for warming, and the warming time T and the out-furnace time t satisfy 5t≦T≦10t.

[0018] A further improvement of the present invention is that the specific process in step (4) is to first increase the temperature to 1100°C-1125°C, soak for 3-5 hours, and then air-cool to room temperature, then increase the temperature from room temperature to 630°C-680°C at a heating rate of 10°C / min-30°C / min, keep at that temperature for 7-10 hours, and then air-cool; finally, increase the temperature from room temperature to 740°C-800°C at a heating rate of 10°C / min-30°C / min, keep at that temperature for 1-3 hours, and then air-cool. Effect of the Invention

[0019] Compared with the prior art, the present invention has the following beneficial effects: The alloy of the present invention has a relatively high content of Fe element and a relatively low content of precious elements such as W and Nb, so that the raw material cost of the alloy is limited. At the same time, in the preparation process of the alloy, the traditional triple melting smelting process of superalloys is abandoned, and after electric arc melting smelting, direct billet rolling is adopted to reduce the preparation components of the alloy. Among them, secondary deoxidation is performed in the smelting process, and an exothermic agent is used to reduce the solidification speed of the molten metal after casting. Then, the alloy is subjected to multiple passes of large deformation processing, and the forging and rolling temperatures are controlled within the range of 200°C to 250°C and 150°C to 200°C higher than the γ' precipitation temperature, respectively. In addition, the deformation amount of the single pass is 30% and 35% or more, respectively, to ensure that the alloy stores sufficient strain storage energy during the supply period. Finally, the alloy after heat treatment has excellent high-temperature strength performance, with a yield strength of 540MPa or more at 700°C and an elongation of 12% or more. [Brief description of the drawings]

[0020] [Figure 1] 1 is a photograph of an ingot in Example 1 (with the surface oxide scale already removed). [Diagram 2] 1 is a photograph of a slab after forging in Example 1 is completed. [Diagram 3] 1 is a photograph of a plate material after single-pass rolling in Example 2. [Figure 4] 1 is a photograph of a plate material after rolling in Example 2. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0021] The present invention will now be described in more detail with reference to examples.

[0022] The high-strength superalloy for thermal power generation units of the present invention has alloy components in the following ranges (by mass%): 0.05% to 0.08% C, 14% to 17% Cr, 0.5% or less Mn, 0.5% or less Si, 1.0% to 2.5% W, 0.3% to 2.0% Mo, 2.0% to 2.5% Ti, 1.0% to 1.5% Al, 0.003% or less B, 0.03% or less Zr, 37% to 48% Fe, and remainder is compatible with Ni.

[0023] The preparation process of the above alloy mainly includes the following three steps: alloy melting and refining, deformation and heat treatment. Step (1)--Smelting and homogenization: The above alloy is smelted in an induction electric arc furnace, which uses magnesium oxide alkali furnace lining, and before melting and smelting, a pure nickel cleaning furnace is adopted, and shot blasting is performed before adding the alloy raw materials. The vacuum degree is controlled within the range of 0.3 Pa to 0.5 Pa, and after Cr, Ni, W, Si, Mn, Mo and Fe in the alloy are completely melted, it is refined for 0.5 to 1 hour, and then Al, Ti, B, Zr and C are added and cast under the environment protected by high purity argon gas. After solidification, the ingot is homogenized for 24 to 72 hours at the range of 1050 ° C to 1120 ° C, and then air-cooled to room temperature.

[0024] Step (2)--Forging and billeting: The alloy refined and homogenized in step (1) is billeted and forged at a temperature 200°C to 250°C higher than the γ' precipitation temperature, with the deformation amount of each pass being 30% or more, and the final total deformation amount being 70% or more.

[0025] Step (3)--Hot rolling: The oxide scale on the surface of the ingot is removed from the alloy forged and billeted in step (2) to a depth of 0.5 mm to 1 mm. After the removal of the surface oxide scale is completed, the roll is heated to 500°C or higher and hot rolled at a temperature 150°C to 200°C higher than the γ' precipitation temperature, with the deformation amount of each pass being 35% or more and the final total deformation amount being 80% or more. After each pass of forging and rolling is completed, the ingot is returned to the furnace for warming, and the warming time T and the out-of-furnace time t satisfy 5t≦T≦10t.

[0026] Step (4)--High temperature sosolation and aging treatment: The alloy hot-rolled in step (3) is heated to 1100°C-1125°C and sosolated for 3-5 hours, then air-cooled to room temperature, then heated to 630°C-680°C and kept at that temperature for 7-10 hours, then air-cooled, and finally heated to 740°C-800°C and kept at that temperature for 1-3 hours, then air-cooled.

[0027] Preferably, after Cr, Ni, W, Si, Mn, Mo and Fe are completely melted, coke is added for deoxidation, the mass of coke deoxidation does not exceed 25% to 50% of the mass of C element in the alloy raw material, and after completion, Ni-Mg alloy is added for secondary deoxidation. Finally, elements that are easily burned such as Al, Ti, B, Zr and C are added, and the mixture is stirred for 5 to 10 minutes and then removed from the furnace, and the casting temperature when removed from the furnace is 1600°C or higher. In addition, a mold is used during casting, and an aluminum exothermic agent is used to cover the molten steel surface during solidification, thereby slowing down the solidification rate and promoting the shrinkage of the molten metal.

[0028] The heating rate of the alloy in the heating stages of the homogenization, sosoloid and aging treatments must be controlled within the range of 10°C / min to 30°C / min, and the ingot must be kept at 900°C to 980°C for 1.0 to 1.5 hours before being heated to the homogenization temperature. Next, the temperature is increased to 1050°C to 1120°C at a rate of 10°C / min to 30°C / min.

[0029] The heat-treated alloy has excellent high temperature strength performance, with a yield strength of 540 MPa or more at 700°C and an elongation of 12% or more.

[0030] Example 1 The high-strength superalloy for thermal power generation units in this embodiment contains, in mass%, 0.06% C, 16% Cr, 0.2% Mn, 0.15% Si, 1.6% W, 1.2% Mo, 2.2% Ti, 1.4% Al, 0.002% B, 0.02% Zr, 37% Fe, and remainder Contains Ni as a metal.

[0031] The alloy is smelted using magnesium oxide alkali furnace lining, and a pure nickel cleaning furnace is used before smelting, and shot blasting treatment is performed before adding the alloy raw material. The alloy is smelted using an induction electric arc furnace, the vacuum is controlled at 0.35 Pa, and after elements such as Cr, Ni and W are completely melted, it is refined for 40 minutes, and before adding Al, Ti, B, Zr and C, high purity argon gas is poured in for protection. After the alloy raw materials such as Cr, Ni and W are completely melted, coke is added for deoxidation, and its added mass should not exceed 50% of the C element mass in the alloy raw material. After completion, Ni-Mg alloy is added for secondary deoxidation, and finally, elements that are easy to burn such as Al, Ti, B, Zr and C are added, and the alloy is stirred for 5 minutes before being taken out of the furnace, and its casting temperature is 1630℃. The alloy casting is performed using a mold, and after casting, the molten steel surface is coated with sodium nitrate + aluminum oxide based heat generating agent to reduce the solidification speed and promote the candidate shrinkage of the molten metal.

[0032] After the molten steel solidifies, the ingot is heated to 1020°C at a rate of 10°C / min and held for 1.0 hour, then heated to within 1160°C and homogenized for 24 hours, then air-cooled to room temperature. After the surface oxide scale is removed, the alloy is billeted and forged at 220°C above the γ' precipitation temperature, with a deformation of 30% for each pass and a final total deformation of 70%. The alloy is then hot-rolled at 160°C above the γ' precipitation temperature, with a deformation of 35% for each pass and a final total deformation of 80%. The rolls are heated to above 500°C before rolling the alloy, and after each pass of forging and rolling is completed, the rolls are returned to the furnace and held for 30 minutes. After the rolling of the alloy is completed, the temperature is raised to 1120°C, sosoloided for 4 hours, and air-cooled to room temperature. Then, the alloy is heated to 650℃ and kept at that temperature for 8 hours, and then cooled in air. Finally, the alloy is heated to 760℃ and kept at that temperature for 2 hours, and then cooled in air. The heating rate of the alloy in the heating stages of the homogenization, sosoloid and aging treatments is 10℃ / min, and the ingot needs to be kept at 950℃ for 1.0 hour before it is heated to the homogenization temperature.

[0033] 1 and 2 are photographs of the ingot and the forged alloy slab in Example 1, and there is no obvious crack on the surface, which indicates that the smelting and processing method of the alloy is reasonable. The performance test results of the alloy show that the yield strength of the alloy at 700°C is 582 MPa and the elongation is 14.2%, which indicates that the alloy has good high temperature strength performance.

[0034] Example 2 The high strength superalloy in this embodiment contains, in mass%, 0.07% C, 15% Cr, 0.2% Mn, 0.15% Si, 2.2% W, 0.4% Mo, 2.2% Ti, 1.4% Al, 0.002% B, 0.02% Zr, 47% Fe, and remainderNi is included as the raw material. The alloy is melted and refined by using magnesium oxide alkali furnace lining, and a pure nickel cleaning furnace is used before melting and smelting, and shot blasting treatment is performed before adding the alloy raw material. The alloy is melted and refined in an induction electric arc furnace, the vacuum degree is controlled at 0.35 Pa, and after elements such as Cr, Ni and W are completely melted, it is refined for 40 minutes, and before adding Al, Ti, B, Zr and C, high purity argon gas is poured in for protection. After the alloy raw materials such as Cr, Ni and W are completely melted, coke is added for deoxidation, and its added mass should not exceed 40% of the C element mass in the alloy raw material. After completion, Ni-Mg alloy is added for secondary deoxidation, and finally elements such as Al, Ti, B, Zr and C that are easily burned are added, and the alloy is taken out of the furnace after stirring for 5 minutes, and its casting temperature is 1650℃. The alloy is cast using a mold, and after casting, the molten steel surface is coated with sodium nitrate + aluminum oxide heat generating agent to reduce the solidification speed and promote the candidate shrinkage of the molten metal. The ratio of sodium nitrate to aluminum oxide heat generating agent is well known to those skilled in the art.

[0035] After the molten steel solidifies, the ingot is heated to 1020°C at a rate of 10°C / min and held for 1.0 hour, then heated to within 1160°C and homogenized for 24 hours, then air-cooled to room temperature. After the surface oxide scale is removed, the alloy is billeted and forged at 240°C above the γ' precipitation temperature, with a deformation of 30% for each pass and a final total deformation of 70%. The alloy is then hot-rolled at 180°C above the γ' precipitation temperature, with a deformation of 35% for each pass and a final total deformation of 80%. The rolls are heated to above 500°C before rolling the alloy, and after each forging and rolling pass is completed, the rolls are returned to the furnace and held for 30 minutes. After the alloy is rolled, the temperature is raised to 1120°C, sosoloided for 4 hours, and air-cooled to room temperature. Then, it is heated to 650℃ and kept at that temperature for 8 hours, and then air-cooled, and finally, it is heated to 760℃ and kept at that temperature for 2 hours, and then air-cooled. Among them, the heating rate of the alloy in the heating stages of the homogenization treatment, sosoloid and aging treatment is 10℃ / min, and the ingot needs to be kept at 950℃ for 1.0 hour before it is heated to the homogenization treatment temperature.

[0036] 3 and 4 are photographs of the single-pass rolling and rolling completed in Example 2, and there is no obvious crack on the surface, which indicates that the processing process of the alloy is reasonable. The alloy performance test results show that the yield strength of the alloy at 700°C is 543MPa and the elongation is 16.1%, which indicates that the alloy has good high temperature strength performance.

[0037] Example 3 Step (1)--Smelting and homogenization: 0.05% C, 14% Cr, 0.5% Mn, 0.1% Si, 1.0% W, 2.0% Mo, 2.0% Ti, 1.0% Al, 0.003% B, 0.01% Zr, 37% Fe, and remainder Take Ni as an example.

[0038] When the vacuum reaches 0.3 Pa to 0.5 Pa, Cr, Ni, W, Si, Mn, Mo and Fe are melted, and then coke is added for deoxidation, and the added mass of coke deoxidation should not exceed 25% of the mass of C. Next, Ni-Mg alloy is added for secondary deoxidation, and finally, Al, Ti, B, Zr and C are added, and after stirring for 5 minutes, it is removed from the furnace and cast. A mold is used for casting, and the casting temperature is 1600°C or higher, and then it is solidified and the molten steel surface is covered with an aluminum exothermic agent. Next, it is kept at 900°C for 1.5 hours, and finally, it is heated from room temperature to 1120°C at a heating rate of 10°C / min, and homogenized for 24 hours, and then air-cooled to room temperature.

[0039] Step (2)--Forging and billeting: The alloy smelted and homogenized in step (1) is billeted and forged at a temperature 200°C higher than the γ' precipitation temperature, with the deformation amount of each pass being 30% or more, and the final total deformation amount being 70% or more. After each pass of forging and billeting is completed, it is returned to the furnace for warming, and the warming time T and the out-furnace time t satisfy 5t≦T≦10t.

[0040] Step (3)--Hot rolling: The alloy forged and billeted in step (2) is hot rolled at a temperature 150°C higher than the γ' precipitation temperature, with the deformation amount of each pass being 35% or more, and the final total deformation amount being 80% or more. After each pass of hot rolling is completed, it is returned to the furnace for warming, and the warming time T and the out-furnace time t satisfy 5t≦T≦10t.

[0041] Step (4)-High temperature solubilization and aging treatment: First, heat the material to 1100℃, solubilize for 5 hours, and then air-cool to room temperature. Then, heat the material from room temperature to 630℃ at a rate of 10℃ / min, keep the material at that temperature for 10 hours, and then air-cool. Finally, heat the material from room temperature to 740℃ at a rate of 10℃ / min, keep the material at that temperature for 3 hours, and then air-cool.

[0042] Example 4 Step (1)--Smelting and homogenization: 0.08% C, 15% Cr, 0.2% Mn, 0.5% Si, 2.5% W, 1.0% Mo, 2.0% Ti, 1.5% Al, 0.001% B, 0.02% Zr, 48% Fe, and remainder Take Ni as an example.

[0043] When the vacuum reaches 0.3 Pa to 0.5 Pa, after Cr, Ni, W, Si, Mn, Mo and Fe are melted, coke is added for deoxidation, and the added mass of coke deoxidation should not exceed 35% of the mass of C. Next, Ni-Mg alloy is added for secondary deoxidation, and finally, Al, Ti, B, Zr and C are added, and after stirring for 7 minutes, it is removed from the furnace and cast. A mold is used for casting, and the casting temperature is 1600°C or higher. Then, it is solidified, and the molten steel surface is covered with an aluminum heat generating agent, and then it is kept at 980°C for 1 hour. Finally, the temperature is increased from room temperature to 1100°C at a heating rate of 20°C / min, and homogenized for 24 hours, and then air-cooled to room temperature.

[0044] Step (2)--Forging and billeting: The alloy smelted and homogenized in step (1) is billeted and forged at a temperature 220°C higher than the γ' precipitation temperature, with the deformation amount of each pass being 30% or more, and the final total deformation amount being 70% or more. After each pass of forging and billeting is completed, it is returned to the furnace for warming, and the warming time T and the out-furnace time t satisfy 5t≦T≦10t.

[0045] Step (3)--Hot rolling: The alloy forged and billeted in step (2) is hot rolled at a temperature 200°C higher than the γ' precipitation temperature, with the deformation amount of each pass being 35% or more, and the final total deformation amount being 80% or more. After each pass of hot rolling is completed, it is returned to the furnace for warming, and the warming time T and the out-furnace time t satisfy 5t≦T≦10t.

[0046] Step (4)-High temperature solubilization and aging treatment: First, heat the material to 1120℃, solubilize for 3 hours, and then air-cool to room temperature. Then, heat the material from room temperature to 650℃ at a rate of 20℃ / min, keep the material at that temperature for 8 hours, and then air-cool. Finally, heat the material from room temperature to 800℃ at a rate of 20℃ / min, keep the material at that temperature for 1 hour, and then air-cool.

[0047] Example 5 Step (1)--Smelting and homogenization: 0.06% C, 17% Cr, 0.1% Mn, 0.3% Si, 2.0% W, 0.3% Mo, 2.1% Ti, 1.3% Al, 0.01% Zr, 42% Fe, and remainder Take Ni as an example.

[0048] When the vacuum reaches 0.3 Pa to 0.5 Pa, Cr, Ni, W, Si, Mn, Mo and Fe are melted, and then coke is added for deoxidation, and the mass of coke deoxidation added should not exceed 50% of the mass of C. Next, Ni-Mg alloy is added for secondary deoxidation. Finally, Al, Ti, B, Zr and C are added, and the mixture is stirred for 10 minutes, and then removed from the furnace and cast. A mold is used for casting, and the casting temperature is 1600°C or higher. Then, the mixture is solidified, and the molten steel surface is covered with an aluminum heat generating agent, and then the mixture is kept at 950°C for 1 hour. Finally, the mixture is heated from room temperature to 1050°C at a heating rate of 30°C / min, homogenized for 24 hours, and then air-cooled to room temperature.

[0049] Step (2)--Forging and billeting: The alloy smelted and homogenized in step (1) is billeted and forged at a temperature 250°C higher than the γ' precipitation temperature, with the deformation amount of each pass being 30% or more, and the final total deformation amount being 70% or more. After each pass of forging and billeting is completed, it is returned to the furnace for warming, and the warming time T and the out-furnace time t satisfy 5t≦T≦10t.

[0050] Step (3)--Hot rolling: The alloy forged and billeted in step (2) is hot rolled at a temperature 170°C higher than the γ' precipitation temperature, with the deformation amount of each pass being 35% or more, and the final total deformation amount being 80% or more. After each pass of hot rolling is completed, it is returned to the furnace for warming, and the warming time T and the out-furnace time t satisfy 5t≦T≦10t.

[0051] Step (4)-High temperature solubilization and aging treatment: First, heat the material to 1115℃, solubilize for 4 hours, and then air-cool to room temperature. Then, heat the material from room temperature to 680℃ at a rate of 30℃ / min, keep the material at that temperature for 7 hours, and then air-cool. Finally, heat the material from room temperature to 770℃ at a rate of 30℃ / min, keep the material at that temperature for 2 hours, and then air-cool.

[0052] The components of the superalloy of the present invention are, in mass%, 0.05% to 0.08% C, 14% to 17% Cr, 0.5% or less Mn, 0.5% or less Si, 1.0% to 2.5% W, 0.3% to 2.0% Mo, 2.0% to 2.5% Ti, 1.0% to 1.5% Al, 0.003% or less B, 0.03% or less Zr, 37% to 48% Fe, and remainder The alloy is processed by an electric arc furnace at a vacuum not exceeding 0.3 Pa to smelt the premixed alloy furnace material. The alloy is billeted and forged at a temperature range of 200°C to 250°C higher than the precipitation temperature of Ni3Al(γ') with a deformation of 70%. The alloy is hot rolled at a temperature range of 150°C to 200°C higher than the precipitation temperature of γ' with a deformation of 80%. The processing process of the alloy of the present invention has low preparation cost, and the alloy prepared by the method of the present invention has excellent high temperature mechanical performance at a temperature of 650°C or higher.

Claims

1. 1. A high-strength superalloy for a thermal power generating unit, comprising, by mass%, 0.05% to 0.08% C, 14% to 17% Cr, 0.5% or less Mn, 0.5% or less Si, 1.0% to 2.5% W, 0.3% to 2.0% Mo, 2.0% to 2.5% Ti, 1.0% to 1.5% Al, 0.003% or less B, 0.03% or less Zr, 37% to 48% Fe, and the balance Ni.

2. A process for preparing a high strength superalloy for a thermal power generating unit, comprising the steps of: Smelting and homogenization: Step (1) of taking a material consisting of, by mass%, 0.05% to 0.08% C, 14% to 17% Cr, 0.5% or less Mn, 0.5% or less Si, 1.0% to 2.5% W, 0.3% to 2.0% Mo, 2.0% to 2.5% Ti, 1.0% to 1.5% Al, 0.003% or less B, 0.03% or less Zr, 37% to 48% Fe, and the balance Ni, melting and refining Cr, Ni, W, Si, Mn, Mo, and Fe under vacuum, and then adding Al, Ti, B, Zr, and C under the protection of argon gas, casting, solidifying, and finally performing homogenization treatment, followed by air cooling to room temperature; Step (2): forging and billeting the alloy smelted and homogenized in step (1) at a temperature 200°C to 250°C higher than the γ' precipitation temperature, the deformation amount of each pass is 30% or more, and the final total deformation amount is 70% or more; Step (3), in which the forged and billeted alloy in step (2) is hot-rolled at a temperature 150°C to 200°C higher than the γ' precipitation temperature, with the deformation amount of each pass being 35% or more and the final total deformation amount being 80% or more; and High temperature sothroid and aging treatment: A process for preparing a high strength superalloy for thermal power generation units, comprising step (4) of high temperature sothroid and aging treatment of the alloy hot rolled in step (3).

3. The preparation process of high strength superalloy for thermal power generating unit according to claim 2, characterized in that in step (1), the refining time is 0.5-1 hour.

4. The specific process of step (1) is characterized in that: when the vacuum degree reaches 0.3 Pa-0.5 Pa, Cr, Ni, W, Si, Mn, Mo and Fe are melted, and then coke is added for deoxidation, and the added mass of coke deoxidation does not exceed 25%-50% of the mass of C; then Ni-Mg alloy is added for secondary deoxidation; finally Al, Ti, B, Zr and C are added; and the mixture is stirred for 5 minutes-10 minutes, and then removed from the furnace for casting, the casting temperature is above 1600°C; then solidified; and finally homogenized and cooled to room temperature.

5. 3. The preparation process of high strength superalloy for thermal power generating unit according to claim 2, characterized in that in step (1), a mold is used during casting, and an aluminum exothermic agent is used to coat the molten steel surface during solidification.

6. The preparation process of high strength superalloy for thermal power generating unit according to claim 2, characterized in that in step (1), the homogenization treatment is carried out by increasing the temperature from room temperature to 1050°C-1120°C at a heating rate of 10°C / min-30°C / min, and then keeping the temperature for 24 hours.

7. The preparation process of high strength superalloy for thermal power generation unit according to claim 2, characterized in that in step (1), after solidification, the alloy is kept at 900°C-980°C for 1.0-1.5 hours, and then homogenized.

8. 3. The process for preparing high strength superalloy for thermal power generating unit according to claim 2, characterized in that in step (2), after each pass of forging and billet is completed, the billet is returned to the furnace for warming, and the warming time T and the out-furnace time t satisfy 5t≦T≦10t.

9. 3. The process for preparing high strength superalloy for thermal power generating units as claimed in claim 2, characterized in that in step (3), after each pass of hot rolling is completed, the steel is returned to the furnace for warming, and the warming time T and the out-furnace time t satisfy 5t≦T≦10t.

10. The specific process of step (4) is characterized in that: first, the temperature is increased from room temperature to 1100°C-1125°C, soaked for 3-5 hours, and then air-cooled to room temperature; then, the temperature is increased from room temperature to 630°C-680°C at a heating rate of 10°C / min-30°C / min, kept at this temperature for 7-10 hours, and then air-cooled; finally, the temperature is increased from room temperature to 740°C-800°C at a heating rate of 10°C / min-30°C / min, kept at this temperature for 1-3 hours, and then air-cooled.

Citation Information

Patent Citations

  • High-temperature alloy cast tube material for 700 DEG C level ultra-supercritical thermal power generating unit reheater and preparation method of high-temperature alloy cast tube material

    CN103556073A

  • High-strength high-toughness antioxidant iron-nickel-based high-temperature alloy and preparation method thereof