Manufacturing method of hot stamped parts
A steel plate composition and manufacturing process for hot-stamped parts with controlled elements and specific processing steps enhance deformability and fracture resistance, addressing the challenges of high-strength hot-stamped parts, achieving efficient production of high-strength parts with improved bendability and reduced manufacturing costs.
Patent Information
- Application Number
- JP2020055879
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-03-26
- Publication Date
- 2024-10-09
- Estimated Expiration
- 2040-03-26
AI Technical Summary
Existing hot-stamped parts with tensile strengths of 1.8 GPa or more face challenges in deformability and fracture resistance, leading to increased manufacturing costs and reduced efficiency.
A steel plate composition with controlled amounts of C, Si, Mn, P, S, Nb, Cr, Al, Ti, B, N, and other elements, combined with a manufacturing process involving specific heating, rolling, and annealing steps, results in a mixed structure of ferrite and pearlite with reduced MnS inclusions, enhancing deformability and fracture resistance.
The solution enables the production of hot-stamped parts with tensile strengths of 1.5 GPa or more without tempering, reducing thickness and weight while improving fracture resistance and maintaining bendability, thus lowering manufacturing costs.
Smart Images

Figure 0007564420000001 
Figure 0007564420000002 
Figure 0007564420000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a steel sheet for hot stamped parts and a method for producing the same. [Background technology]
[0002] In recent years, in order to improve the fuel efficiency of automobiles, there have been vigorous efforts to reduce the weight of automobiles by increasing the strength of the steel materials used. As a result, in the manufacture of parts (hereinafter referred to as "press-formed parts") manufactured by cold press forming thin steel sheets that are widely used in automobiles, it has become difficult to manufacture press-formed parts having complex shapes due to the decrease in press formability that accompanies the increase in the strength of the steel sheets.
[0003] Specifically, problems such as breakage at highly processed parts and deterioration of dimensional accuracy of press-formed parts due to increased springback and wall warpage caused by the decrease in ductility of steel sheets are frequently occurring. In particular, it is not easy to manufacture press-formed parts made of high-strength steel sheets having a tensile strength of 780 MPa or more.
[0004] Roll forming, rather than cold press forming, can easily produce roll-formed parts made of high strength steel sheets, but roll forming can only produce roll-formed parts with a constant cross section in the longitudinal direction, and cannot produce press-formed parts with complex cross-sectional shapes.
[0005] In contrast, in the hot stamping method (also known as hot press forming), in which heated steel sheet is press-formed, the hot steel sheet during forming is soft and highly ductile, making it possible to form press-formed parts having complex shapes with good dimensional accuracy without forming defects such as breakage, springback, and wall warping.
[0006] Moreover, according to the hot stamping method, the steel sheet is heated to a temperature in the austenite single phase region before being press-formed, and the formed product is rapidly cooled and quenched inside the die used for press forming, thereby simultaneously forming the steel sheet and increasing the strength of the press-formed part through martensitic transformation. Thus, the hot stamping method is an excellent technique suitable for manufacturing high-strength press-formed parts. In the following description, press-formed parts manufactured by the hot stamping method will be referred to as "hot stamped parts".
[0007] Currently, bumper reinforcement, which has a relatively simple shape, is known as an example of a hot stamped part. Hot stamped parts with a tensile strength of 1.5 GPa are already widely used in structural members (framework members) of body shells, such as bumper reinforcement, for example, B-pillar reinforcement.
[0008] In recent years, there has been research into the production of hot stamped parts with higher strength, particularly those with a tensile strength of 1.8 GPa or more. For example, there is consideration of using hot stamped parts with a tensile strength of 1.8 GPa or more for structural components (framework components) of the body shell, such as B-pillar reinforcements, which will bear the majority of the impact load in the event of a collision.
[0009] However, when the tensile strength of a hot stamped part reaches an ultra-high strength of 1.8 to 2.0 GPa, the deformability of the hot stamped part becomes insufficient, and the fracture resistance characteristics (e.g., bendability) of the hot stamped part decrease, and the hot stamped part itself is likely to break during a collision, or the absorbed energy of the hot stamped part decreases. For this reason, the only hot stamped parts with a tensile strength of 1.8 to 2.0 GPa that have been put into practical use are bumper reinforcements with a tensile strength of 1.8 GPa or more, and in fact, no examples of the manufacture of hot stamped parts with high deformability and a tensile strength of 1.8 GPa or more have been reported.
[0010] Therefore, in order to manufacture hot stamped parts with a tensile strength of 1.8 GPa or more, it is necessary to further temper the hot stamped parts to increase their deformability. However, adding a tempering process to the hot stamping process significantly increases the manufacturing costs of the hot stamped parts due to reduced work efficiency and increased equipment costs.
[0011] Patent Document 1 discloses a hot stamped part having a steel structure composed of automatically tempered martensite with an average prior austenite grain size of 10 μm or less and excellent toughness and a tensile strength of 1.8 GPa or more in an as-quenched state, and a steel sheet for this hot stamped part, which is obtained by holding a steel sheet containing one or more of C: 0.25 to 0.45% (in this specification, "%" related to a chemical composition or concentration means "mass %" unless otherwise specified), Mn + Cr: 0.5 to 3.0%, and further containing one or more of Si: 0.5% or less, Ni: 2% or less, Cu: 1% or less, V: 1% or less, and Al: 1% or less in a temperature range of Ac3 point or more (Ac3 point + 100°C) for 5 minutes or less, press forming, and then cooling at a cooling rate to the Ms point that is an upper critical cooling rate or more and at an average cooling rate from the Ms point to 150°C that is 10 to 500°C / s.
[0012] Patent Documents 2 and 3 disclose hot stamped parts having a fine structure including automatically tempered martensite with a prior austenite grain size of 10 μm or less and excellent toughness and a tensile strength of 1.8 GPa or more in an as-quenched state, which are obtained by holding a steel plate having a chemical composition containing 0.26 to 0.45% C, 0.5 to 3.0% Mn + Cr, 0.02 to 1.0% Nb, Ti in an amount satisfying 3.42N + 0.001 ≦ Ti ≦ 3.42N + 0.5, and one or more of 0.5% or less Si, 2% or less Ni, 1% or less Cu, 1% or less V, and 1% or less Al for 5 minutes or less in a temperature range of Ac3 point or more (Ac3 point + 100°C) and then press forming the steel plate, and then cooling the steel plate at a cooling rate to the Ms point at an upper critical cooling rate or more and at an average cooling rate from the Ms point to 150°C at a rate of 10 to 500°C / s. [Prior art documents] [Patent documents]
[0013] [Patent Document 1] JP 2006-152427 A [Patent Document 2] International Publication No. 2007 / 129676 [Patent Document 3] JP 2012-180594 A Summary of the Invention [Problem to be solved by the invention]
[0014] The inventions disclosed in Patent Documents 1 to 3 certainly provide hot stamped parts having a tensile strength of 1.8 GPa or more in the as-quenched state.
[0015] However, as described above, in order to use hot stamped parts with a tensile strength of 1.8 GPa or more for structural members (framework members) of a body shell, the hot stamped parts need not only to have high strength (tensile strength of 1.8 to 2.0 GPa) but also to have improved fracture resistance (e.g., bendability) by further improving deformability. From this perspective, there is still room for improvement in the deformability and fracture resistance of the hot stamped parts disclosed in Patent Documents 1 to 3.
[0016] In particular, in hot stamped parts with a tensile strength of 1.5 GPa or more, the improved deformability can be used to improve fracture resistance, thereby enabling reductions in plate thickness and weight.
[0017] The present invention has been made in view of the problems associated with the conventional techniques, and has an object to provide a technique for producing a hot stamped part that has excellent deformability and fracture resistance upon collision and has a tensile strength of, for example, 1.5 GPa or more, without tempering after quenching. [Means for solving the problem]
[0018] Generally, when the tensile strength of a hot stamped part is high, it becomes difficult to ensure the bendability of the hot stamped part. As a result of intensive research focusing on the improvement of the fracture resistance property of the hot stamped part during a collision, the inventors obtained the findings A and B listed below and completed the present invention.
[0019] (A) When the steel sheet for hot stamping parts was subjected to three-point bending, elongated MnS was present in the cracked area, and many dimples due to this MnS were confirmed on the fracture surface. In other words, the elongated MnS becomes the starting point of fracture. For this reason, it is necessary to reduce the amount of elongated MnS in the steel sheet for hot stamping parts.
[0020] (B) That is, in the manufacturing process of steel plate for hot stamped parts and hot stamped parts, impurities such as inclusions and carbides in the steel, which are the starting points for fracture of the hot stamped parts during a collision, can be reduced as much as possible, thereby making it possible to significantly improve the fracture resistance of the hot stamped parts. This makes it possible to use hot stamped parts with a tensile strength of 1.5 GPa or more, for example, in structural components (skeletal components) of a body shell.
[0021] The present invention is as follows:
[0022] (1) the chemical composition is, in mass%, C: 0.18% or more and less than 0.26%, Si: 0.001 to 2.00%, Mn: 0.001 to 3.00%, P: 0.1% or less, S: 0.0015% or less, Nb: less than 0.010%, Cr: 0.001 to 0.50%, Al: 0.0001 to 0.100%, Ti: 0.001 to 0.500%, O: less than 0.0030%, B: 0.0006 to 0.0030%, N: 0.0100% or less, the balance: Fe and impurities; The metal structure is a mixed structure of ferrite and pearlite, The number density of MnS particles with a length of 10 μm or more at a depth position of 1 / 4 to 3 / 4 of the plate thickness is 1.5 particles / 10,000 μm 2 and a tensile strength of 1.5 GPa or more.
[0023] (2) The steel sheet for hot stamped parts according to the above (1), wherein the chemical composition has, in mass%, one or more selected from V: 2.0% or less, Ta: 0.5% or less, and W: 3.0% or less.
[0024] (3) The steel sheet for hot stamped parts according to the above (1) or (2), wherein the chemical composition has, in mass%, one or more selected from Ni: 5.0% or less, Cu: 3.0% or less, and Mo: 0.5% or less.
[0025] (4) The steel sheet for hot stamped part according to any one of (1) to (3) above, wherein the chemical composition has, in mass%, one or more elements selected from Mg: 0.003% or less, Ca: 0.003% or less, La: 0.03% or less, and Ce: 0.03% or less.
[0026] (5) A method for producing a steel sheet for hot stamped parts according to any one of (1) to (4) above, a rolling step of heating a steel ingot or billet having the above chemical composition at 1200 to 1350°C for 1 hour or more, completing rough rolling at 1000 to 1150°C, and completing finish rolling at Ae3+50°C or higher; A winding process at 600 to 750°C; A method for producing a steel sheet for hot stamped parts, comprising:
[0027] (6) The method for producing a steel sheet for hot stamped parts according to the above (5), further comprising a cold rolling step of carrying out descaling and cold rolling after the coiling step.
[0028] (7) The method for producing a steel sheet for hot stamped parts according to the above (6), further comprising an annealing step of performing annealing after the cold rolling step.
[0029] (8) The method for producing a steel sheet for hot stamped parts according to the above (5), further comprising, after the coiling step, an annealing step of carrying out descaling and annealing. Effect of the Invention
[0030] According to the present invention, it is possible to manufacture a hot stamped part having high strength (particularly a tensile strength of 1.5 GPa or more) and greatly improved fracture resistance by hot stamping and quenching without tempering. This makes it possible to reduce the thickness and weight of a hot stamped part having a tensile strength of 1.5 GPa or more, and to prevent an increase in the manufacturing cost of the hot stamped part having a tensile strength of 1.5 GPa or more. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0031] The present invention will now be described. 1. Steel sheet for hot stamped parts according to the present invention (1)Chemical composition
[0032] First, the essential elements will be described.
[0033] (1-1) C: 0.18% or more and less than 0.26% C is a very important element that improves the hardenability of steel sheets for hot stamped parts and mainly determines the tensile strength of the hot stamped parts after quenching. In particular, in order to ensure that the tensile strength of the hot stamped parts after quenching is 1.5 GPa or more, the C content is 0.18% or more, preferably 0.2% or more, and more preferably 0.21% or more. On the other hand, if the C content is 0.26% or more, the tensile strength of the hot stamped parts after quenching becomes too high, so that the deterioration of the bendability becomes significant. For this reason, the C content is less than 0.26%, preferably 0.24% or less, and more preferably 0.23% or less.
[0034] (1-2) Si: 0.001-2.00% Silicon is effective in improving the hardenability of steel sheets for hot stamped parts and stably achieving high strength of hot stamped parts after hardening. To achieve this effect, the silicon content is 0.001% or more, preferably 0.05% or more, and more preferably 0.1% or more. On the other hand, if the silicon content exceeds 2.00%, embrittlement occurs and bendability is significantly reduced. For this reason, the silicon content is 2.00% or less, preferably 1.5% or less, and more preferably 1.0% or less.
[0035] (1-3) Mn: 0.001-3.00% Mn is an element that is very effective in improving the hardenability of steel sheets for hot stamped parts and stably obtaining high strength of hot stamped parts after quenching. If the Mn content is less than 0.001%, this effect cannot be obtained sufficiently. Therefore, the Mn content is 0.001% or more, preferably 0.5% or more, and more preferably 1.0% or more. On the other hand, if the Mn content exceeds 3.00%, the number density of MnS increases and the bendability deteriorates. Therefore, the Mn content is 3.00% or less, preferably 2.5% or less, and more preferably 2.0% or less.
[0036] (1-4)P: 0.1% or less Since P significantly deteriorates the toughness of hot stamped parts after quenching, the lower the P content, the better, but a P content of 0.1% is permissible. Therefore, the P content is 0.1% or less. However, reducing the P content to less than 0.001% unavoidably increases the steelmaking cost. For this reason, the P content is preferably 0.001% or more.
[0037] (1-5)S: 0.0015% or less The lower the S content, the more improved the deformability and fracture resistance, so the S content is set to 0.0015% or less. It is preferably less than 0.001%. However, since reducing the S content requires high desulfurization costs, the S content is preferably set to 0.0001% or more. The S content is more preferably set to 0.0003% or more.
[0038] (1-6) Nb: less than 0.010% Nb is an impurity and is permitted to be present at less than 0.010%. Nb is mixed in through its inclusion in raw materials such as ore and scrap, or through its inclusion during the manufacturing process.
[0039] (1-7) Cr: 0.001-0.50% Cr is an element that is very effective in improving the hardenability of steel sheets for hot stamped parts and stably obtaining high strength of hot stamped parts after quenching. To obtain this effect, the Cr content is 0.001% or more, preferably 0.05% or more, and more preferably 0.1% or more. On the other hand, even if the Cr content exceeds 0.50%, the above effect saturates and it becomes difficult to ensure a stable tensile strength. For this reason, the Cr content is 0.50% or less, preferably 0.4% or less, and more preferably 0.3% or less.
[0040] (1-8) Al: 0.0001-0.100% Al is an element that is effective in deoxidizing molten steel and improving the soundness of steel sheet. To obtain this effect, the Al content is 0.0001% or more, preferably 0.01% or more, and more preferably 0.02% or more. On the other hand, if the Al content exceeds 0.100%, alumina becomes coarse, and bendability may decrease. For this reason, the Al content is 0.100% or less, preferably 0.06% or less, and more preferably 0.04% or less.
[0041] (1-9) Ti: 0.001-0.500% Ti preferentially bonds with N to form TiN, suppressing the consumption of B due to the formation of BN, and has the effect of allowing B to function effectively. In order to reliably obtain this effect, the Ti content is 0.001% or more, preferably 0.005% or more, and more preferably 0.01% or more. On the other hand, even if the Ti content exceeds 0.500%, the above effect saturates and the cost only increases. For this reason, the Ti content is 0.500% or less, preferably 0.04% or less, and more preferably 0.03% or less.
[0042] (1-10) O: Less than 0.0030% O exists in steel as an impurity. If O is present, it forms oxides and reduces the fracture resistance properties, so a small O content is preferable, but a content of about 0.0030% is permissible. For this reason, the O content is less than 0.0030%.
[0043] (1-11) B: 0.0006~0.0030% B is effective in improving the hardenability of the steel sheet for hot stamped parts and in enhancing the effect of stably securing the tensile strength of the hot stamped parts after hardening. In addition, B is an important element in that it segregates at the grain boundaries to increase the grain boundary strength and improve the toughness of the hot stamped parts. Furthermore, B has a high effect of suppressing the growth of austenite grains during heating of the steel sheet for hot stamped parts. In order to obtain this effect, the B content is 0.0006% or more, preferably 0.0010% or more, and more preferably 0.0015% or more. On the other hand, if the B content exceeds 0.0030%, B carbonitrides are generated and the amount of solid-solubilized B decreases, thereby decreasing the hardenability and the strength. For this reason, the B content is 0.0030% or less, preferably 0.0025% or less, and more preferably 0.0020% or less.
[0044] (1-12)N: 0.0100% or less N exists in steel as an impurity. When N is present, it bonds with B to form BN, which reduces the effect of B, so a small N content is preferable, but a content of about 0.0100% is permissible. For this reason, the N content is 0.0100% or less, preferably 0.008% or less, and more preferably 0.006% or less.
[0045] Next, the optional elements will be described.
[0046] (1-13)V:2.0% or less V is an element that is effective in improving the hardenability of steel sheets for hot stamped parts and in stably ensuring the tensile strength of hot stamped parts after quenching. However, if the V content exceeds 2.0%, the above effects are saturated and the cost only increases. For this reason, the V content is 2.0% or less, preferably 1.5% or less, and more preferably 1.0% or less. In order to reliably obtain the above effects, the V content is 0.001% or more, preferably 0.1% or more, and more preferably 0.2% or more.
[0047] (1-14) Ta: 0.5% or less Ta is an element that is effective in improving the hardenability of steel sheets for hot stamped parts and in stably ensuring the tensile strength of hot stamped parts after quenching. However, if the Ta content exceeds 0.5%, the above effects are saturated and the cost only increases. For this reason, the Ta content is 0.5% or less, preferably 0.4% or less, and more preferably 0.3% or less. In order to reliably obtain the above effects, the Ta content is 0.001% or more, preferably 0.005% or more, and more preferably 0.1% or more.
[0048] (1-15)W:3.0% or less W is an element that is effective in improving the hardenability of steel sheets for hot stamped parts and stably ensuring the tensile strength of hot stamped parts after hardening. However, if the W content exceeds 3.0%, the above effects are saturated and the cost only increases. For this reason, the W content is 3.0% or less, preferably 2.0% or less, and more preferably 1.0% or less. In order to reliably obtain the above effects, the W content is 0.01% or more, preferably 0.05% or more, and more preferably 0.1% or more.
[0049] (1-16)Ni: 5.0% or less Ni is an element that is effective in improving the hardenability of steel sheets for hot stamped parts and in stably ensuring the tensile strength of hot stamped parts after quenching. However, when the Ni content exceeds 5.0%, the above effects are saturated and the cost only increases. For this reason, the Ni content is 5.0% or less, preferably 3.0% or less, and more preferably 2.0% or less. In order to reliably obtain the above effects, the Ni content is 0.01% or more, preferably 0.1% or more, and more preferably 0.2% or more.
[0050] (1-17)Cu:3.0% or less Cu is an element that is effective in improving the hardenability of steel sheets for hot stamped parts and stably ensuring the tensile strength of hot stamped parts after hardening. However, even if the Cu content exceeds 3.0%, the above effects are saturated and the cost only increases. For this reason, the Cu content is 3.0% or less, preferably 2.0% or less, and more preferably 1.0% or less. In order to reliably obtain the above effects, the Cu content is 0.1% or more, preferably 0.2% or more, and more preferably 0.5% or more.
[0051] (1-18) Mo: 0.5% or less Mo is an element that is effective in improving the hardenability of steel sheets for hot stamped parts and in stably ensuring the tensile strength of hot stamped parts after quenching. However, even if the Mo content exceeds 0.5%, the above effects are saturated and the cost only increases. For this reason, the Mo content is 0.5% or less, preferably 0.4% or less, and more preferably 0.3% or less. In order to reliably obtain the above effects, the Mo content is 0.005% or more, preferably 0.1% or more, and more preferably 0.2% or more.
[0052] (1-19)Mg: 0.003% or less Mg has the effect of refining inclusions in steel and improving the toughness of hot stamped parts after quenching. However, when the Mg content exceeds 0.003%, this effect saturates and the cost increases. Therefore, the Mg content is 0.003% or less, preferably 0.0025% or less, and more preferably 0.002% or less. In order to reliably obtain the above effect, the Mg content is 0.0005% or more, preferably 0.001% or more, and more preferably 0.0015% or more.
[0053] (1-20)Ca: 0.003% or less Ca has the effect of refining inclusions in steel and improving the toughness of hot stamped parts after quenching. However, if the Ca content exceeds 0.003%, this effect saturates and the cost increases. Therefore, the Ca content is 0.003% or less, preferably 0.0025% or less, and more preferably 0.002% or less. In order to reliably obtain the above effect, the Ca content is 0.0005% or more, preferably 0.001% or more, and more preferably 0.0015% or more.
[0054] (1-21)La: 0.03% or less La has the effect of refining inclusions in steel and improving the toughness of hot stamped parts after quenching. However, when the La content exceeds 0.03%, this effect saturates and the cost increases. For this reason, the La content is 0.03% or less, preferably 0.02% or less, and more preferably 0.01% or less. In order to reliably obtain the above effect, the La content is 0.001% or more, preferably 0.003% or more, and more preferably 0.005% or more.
[0055] (1-22)Ce: 0.03% or less Ce has the effect of refining inclusions in steel and improving the toughness of hot stamped parts after quenching. However, when the Ce content exceeds 0.03%, this effect saturates and the cost increases. Therefore, the Ce content is 0.03% or less, preferably 0.025% or less, and more preferably 0.020% or less. In order to reliably obtain the above effect, the Ce content is 0.001% or more, preferably 0.005% or more, and more preferably 0.01% or more.
[0056] The balance other than the above is Fe and impurities. Examples of impurities include those contained in raw materials such as ores and scraps, and those contained in the manufacturing process.
[0057] (2) Metal structure (2-1) Mixed structure of ferrite and pearlite The steel sheet according to the present invention has a metal structure having a mixed structure of ferrite and pearlite from the viewpoint of workability of the blank for hot stamping, formability and hardenability during hot stamping, etc. The mixed structure of ferrite and pearlite preferably has a metal structure containing 10 to 80% ferrite and 20 to 90% pearlite in terms of area ratio, and the sum of the area ratios of ferrite and pearlite is 80 to 100%, and more preferably has a metal structure containing 30 to 75% ferrite and 15 to 70% pearlite, and the sum of the area ratios of ferrite and pearlite is 90 to 100%. Examples of the metal structure of the remainder other than ferrite and pearlite include bainite. The area ratio of the remainder structure is allowed to be up to 20%. The area ratio of the remainder structure is preferably 10% or less.
[0058] (2-2) Number density of MnS particles with a length of 10 μm or more at a depth position of 1 / 4 to 3 / 4 of the plate thickness: 1.5 particles / 10,000 μm 2 below
[0059] The center of a slab produced by continuous casting has a lot of segregation. Even when the slab is rolled into a thin plate, the segregation continues, and the center of the thin plate has a lot of segregation. For this reason, in the present invention, attention is paid to the position of the center of the plate thickness (1 / 4 to 3 / 4t).
[0060] It is known that MnS is the initiation point of cracks. In the present invention, the formation of MnS is suppressed by reducing the S content in the steel to 0.0015% or less, preferably to less than 0.001%.
[0061] However, it is still not possible to sufficiently suppress the formation of MnS, and the bending crack resistance is improved by preventing the formation of MnS. Specifically, the number density of MnS is set to 1.5 particles / 10,000 μm 2 However, extremely fine MnS with a length of less than 10 μm does not affect bending crack resistance. Therefore, the number density of elongated MnS with a length of 10 μm or more is 1.5 pieces / 10,000 μm. 2 or less, preferably 1.4 pieces / 10000 μm 2 More preferably, it is 1.1 particles / 10,000 μm or less. 2 The following is the result.
[0062] The area ratios of ferrite and pearlite, and the number density of MnS can be measured, for example, by the method described in the Examples.
[0063] (3)Applications The steel sheet according to the present invention is used for hot stamped parts, such as bumper reinforcement and structural members of automobile body shells (e.g., A-pillar reinforcement, B-pillar reinforcement, front side members, rear side members, roof rails, various cross members, etc.).
[0064] 2. Manufacturing method of hot stamped parts according to the present invention Next, a method for producing a hot stamping part having a tensile strength of 1.5 GPa or more according to the present invention will be described.
[0065] (1) Rolling process A steel ingot or billet having the above-mentioned chemical composition is heated at 1200 to 1350°C for at least one hour, and then rough rolling is completed at 1000 to 1150°C. MnS dissolves in the slab when it is heated. When it is cooled, it re-precipitates. However, if it is re-precipitated after dissolving in the slab, these inclusions are finely dispersed, and MnS with a length of 10 μm or more is unlikely to form.
[0066] MnS dissolves at about 1200 to 1250° C. Therefore, in order to dissolve MnS and cause it to finely precipitate, the heating temperature of the steel ingot or steel slab is 1200° C. or higher, and preferably 1250° C. or higher.
[0067] On the other hand, if the heating temperature of the steel ingot or billet is too high, the energy cost increases, so the heating temperature of the steel ingot or billet is 1350°C or lower, and preferably 1300°C or lower.
[0068] In order to sufficiently uniformly heat the steel ingot or slab, heating for 1 hour or more is effective, but since the energy cost increases when the heating time of the steel ingot or slab exceeds 2.0 hours, the heating time of the steel ingot or slab is preferably 2.0 hours or less.
[0069] After the steel ingot or steel slab is heated as described above, rough rolling is started and completed at 1000 to 1150°C. If the end temperature of rough rolling is less than 1000°C, the end temperature of finish rolling described below cannot be satisfied. On the other hand, if the end temperature of rough rolling exceeds 1150°C, recrystallization proceeds, but coarsening of crystal grains proceeds, leading to coarsening of crystal grains in finish rolling.
[0070] After this, finish rolling is completed at Ae3+50°C or higher. This is because if hot rolling is performed at a temperature lower than Ae3+50°C, the hardenability decreases and the tensile strength TS decreases. In the chemical composition system of the present invention, these problems do not occur if the hot rolling completion temperature is Ae3+50°C or higher. On the other hand, if the hot rolling completion temperature exceeds 1050°C, there is a risk of surface defects such as scale bite. Therefore, it is preferable that the hot rolling completion temperature is 1050°C or lower.
[0071] The Ae3 point is calculated according to the following formula. Ae3(℃)=937-477C+56Si-20Mn-16Cu-15Ni-5Cr+38Mo+136Ti-19Nb+198Al+3315B In the above formula, the element symbols represent the content (mass%) of each element contained in the steel sheet, and 0 is substituted when the element is not contained.
[0072] (2) Winding process After hot rolling, the steel is coiled at 600 to 750°C. By coiling in this temperature range, the structure can be made a mixed structure consisting of ferrite and pearlite. During cooling of the hot rolled coil, Cr and Mn are diffused and concentrated to Fe3C, which is stabilized. Therefore, in order to suppress the stabilization, it is effective to lower the coiling temperature and sufficiently reduce the diffusion rate of Cr and Mn. In addition, the tensile strength of the steel sheet is also reduced. For this reason, in the present invention, the coiling temperature is 750°C or less, and preferably 700°C or less.
[0073] On the other hand, if the coiling temperature is below 600°C, hard phases such as bainite may be generated, which increases the rolling load in the cold rolling that follows the hot rolling, impairing productivity. For this reason, the coiling temperature is 600°C or higher, and preferably 620°C or higher.
[0074] Thereafter, if necessary, the coil (steel strip) that has been wound into a coil may be unwound and then subjected to one or more treatments such as pickling, shot blasting, grinding, etc. to remove the scale formed on the surface (descaling).
[0075] (3) Cold rolling process After coiling, cold rolling is performed as necessary. Cold rolling is performed after the above-mentioned descaling is performed. Cold rolling may be performed under well-known and commonly used conditions, and the cold rolling temperature is preferably 10 to 60°C. Cold rolling has the effect of making the crystal grain size fine after hot stamping.
[0076] (4) Annealing process After cold rolling, annealing is performed as necessary. After coiling, pickling, etc., and descaling, annealing may be performed directly without performing the cold rolling process. Annealing should be performed at 600°C or higher, and 700°C or higher at which the austenite phase precipitates is preferable. On the other hand, if the annealing temperature exceeds 900°C, the combustion cost increases industrially.
[0077] The annealing may be continuous annealing performed in an uncoiled state, or box annealing performed after winding into a coil.
[0078] The annealing conditions may be any known or conventional condition. For example, when a cold-rolled steel strip is continuously annealed, it is annealed by heating it to 730 to 900°C, holding it at that temperature range for 10 seconds or more, cooling it to a temperature range of 300 to 500°C at an average cooling rate of 1 to 100°C / s, further holding it at the temperature range of 300 to 500°C for 30 seconds to 10 minutes, and then cooling it to room temperature at an average cooling rate of 1 to 50°C / s.
[0079] In this manner, the steel sheet for hot stamped parts according to the present invention having a tensile strength of 1.5 GPa or more is manufactured. EXAMPLES
[0080] The present invention will now be described in detail with reference to examples.
[0081] A slab having the chemical composition shown in Tables 1 and 2 (the balance other than those shown in Tables 1 and 2 is Fe and impurities) was heated at the slab heating temperature and slab heating time shown in Table 3, and then rough rolling was started and completed at the rough rolling end temperature shown in Table 3. Furthermore, finish rolling was completed at the finish rolling end temperature shown in Table 3 to give a plate thickness of 3.2 mm, and the plate was wound into a coil at the coiling temperature shown in Table 3.
[0082] Some of the coils were recoiled, descaled, and annealed, while others were recoiled, pickled, descaled, and then cold rolled to a thickness of 1.6 mm.
[0083] Some of the cold-rolled pieces were further annealed. For the pieces that were cold-rolled and annealed, the cold-rolling temperature and annealing temperature are shown in Table 3. In Table 3, RT stands for room temperature. The underlines in Tables 2 and 3 indicate that the items are outside the scope of the present invention.
[0084] [Table 1]
[0085] [Table 2]
[0086] [Table 3]
[0087] Regarding the manufactured coils ,set We also conducted weaving observations. Hot stamping process, The steel sheets were evaluated for their properties as hot stamped parts. Specifically, the steel sheets Nos. 1 to 34 and x1 to x14 for hot stamped parts were manufactured and the microstructures were observed as shown in (1) and (2) below.
[0088] (1) Area ratio of ferrite and pearlite A sample piece was cut out from a part of the steel plate, the L-section of the sample was mirror-polished, and the metal structure was corroded using a nital solution.Then, a 1 / 4t region of the plate thickness was observed under an optical microscope at 500x magnification, and the area ratio of each structure was measured.
[0089] (2) Number density of MnS particles with lengths of 10 μm or more at a depth of 1 / 4 to 3 / 4 of the plate thickness A sample piece was cut out from a part of the steel sheet, and the L-section of the sample was mirror-polished to measure the size and number density of MnS using an optical microscope. 2 ) was used as the measurement area.
[0090] on the other hand, Hot stamping parts The characteristics were evaluated by the methods shown in (3) and (4) below.
[0091] (3) Strength (TS,YS) Test piece No. 5 specified in JIS Z 2201 Hot stamping parts The specimens were taken from the test pieces and subjected to tensile tests in accordance with JIS Z 2241 to evaluate their strength (TS, YS).
[0092] (4) Limit bending radius Regarding bendability evaluation, Hot stamping parts A 30mm x 100mm test piece was taken from the specimen and a 90 degree bending test was performed using a punch with a tip R of 2.0 to 5.0 to determine the maximum R at which cracks do not occur in the bent portion. Since the maximum R at which cracks occur also depends on the plate thickness t, the obtained maximum R was divided by the plate thickness t to determine the limit R / t, and those with an R / t of less than 2.0 were evaluated as having good bendability. Note that those in which cracks occurred even when the tip R was 5.0 are indicated with a "-" in Table 5.
[0093] Table 4 shows the results of the structure observation. Hot stamping partsThe results of the plate thickness and mechanical properties are shown in Table 4. The underlined values in Table 4 indicate values outside the range of the present invention, and the underlined values in Table 5 indicate values where the mechanical properties are not satisfactory.
[0094] [Table 4]
[0095] [Table 5]
[0096] Nos. 1 to 34 in Table 5 are examples of the present invention that satisfy all of the requirements of the present invention, and Nos. x1 to x14 are comparative examples that do not satisfy the requirements of the present invention.
[0097] As shown in Table 5, in the examples of the present invention, No. 1 to No. 34, the number density of MnS particles having a length of 10 μm or more at a depth position of 1 / 4 to 3 / 4 of the plate thickness: 0.10 to 1.33 (particles / 10,000 μm 2 ) can be obtained by hot stamping and quenching without tempering, and the mechanical properties are TS: 1530-1696 (MPa), YS: 1020-1204 (MPa), and limit R / t: 0.8-1.6. It is clear that it is possible to manufacture hot stamped parts that have ultra-high strength (particularly tensile strength of 1.5-1.7 GPa) and significantly improved fracture resistance.
[0098] In contrast, in No. x1, the S content exceeded the upper limit of the range of the present invention, and therefore the number density of MnS exceeded the upper limit of the range of the present invention, and the critical R / t was an unsatisfactory value.
[0099] In No. x2, the S content exceeded the upper limit of the range of the present invention, and therefore the number density of MnS exceeded the upper limit of the range of the present invention, and the critical R / t was an unsatisfactory value.
[0100] In No. x3, the rough rolling end temperature was below the lower limit of the range of the present invention, and as a result, the finish rolling end temperature was also below the lower limit of the range of the present invention, so that the hardenability was reduced and the tensile strength TS was insufficient.
[0101] In No. x4, the coiling temperature exceeded the upper limit of the range of the present invention, so that the hardenability decreased and the tensile strength TS was insufficient.
[0102] In No. x5, the slab heating temperature was below the lower limit of the range of the present invention, so the number density of MnS exceeded the upper limit of the range of the present invention, and the limit R / t was an unsatisfactory value.
[0103] In No. x6, the slab heating time was below the lower limit of the range of the present invention, so the number density of MnS exceeded the upper limit of the range of the present invention, and the limit R / t was an unsatisfactory value.
[0104] In No. x7, the C content exceeded the upper limit of the range of the present invention, and therefore the critical R / t was an unsatisfactory value.
[0105] In No. x8, the Si content exceeded the upper limit of the range of the present invention, and therefore cracks occurred even when a 90-degree bending test was performed using a punch with a tip R of 5.0.
[0106] In No. x9, the Mn content exceeded the upper limit of the range of the present invention, and therefore the number density of MnS exceeded the upper limit of the range of the present invention, and the limit R / t was an unsatisfactory value.
[0107] In No. x10, the Cr content exceeded the upper limit of the range of the present invention, and therefore the tensile strength TS was insufficient.
[0108] In No. x11, the B content exceeded the upper limit of the range of the present invention, and therefore the tensile strength TS was insufficient.
[0109] In No. x12, the Al content exceeded the upper limit of the range of the present invention, and therefore cracks occurred even when a 90-degree bending test was performed using a punch with a tip R of 5.0.
[0110] In No. x13, the N content exceeded the upper limit of the range of the present invention, and therefore the tensile strength TS was insufficient.
[0111] Furthermore, in No. x14, the O content exceeded the upper limit of the range of the present invention, and therefore the limit R / t was an unsatisfactory value.
Claims
1. The chemical composition, in mass percent, is C: 0.18% or more and less than 0.26%; Si: 0.001 to 2.00%, Mn: 0.001 to 3.00%, P: 0.1% or less, S: 0.0015% or less, Nb: less than 0.010%; Cr: 0.001-0.50%, Al: 0.0001-0.100% Ti: 0.001 to 0.500%, O: less than 0.0030%, B: 0.0006 to 0.0030%, N: 0.0100% or less, The balance is Fe and impurities. The steel ingot or billet is heated at 1200 to 1350°C for at least one hour, then roughly rolled at 1000 to 1150°C. 3 A rolling step of completing finish rolling at +50°C or higher; A winding process at 600 to 750°C; By carrying out a process including The metal structure is a mixed structure of ferrite and pearlite, The area ratio is 10 to 80% ferrite and 20 to 90% pearlite, and the sum of the area ratios of ferrite and pearlite is 80 to 100%, After obtaining a steel sheet having a number density of MnS particles having a length of 10 μm or more at a depth position of 1 / 4 to 3 / 4 of the sheet thickness of 1.5 particles / 10,000 μm or less, The method for producing a hot stamped part includes subjecting the steel plate to a hot stamping process to obtain a hot stamped part having a tensile strength of 1.5 GPa or more.
2. The method for producing a hot stamped part according to claim 1 , further comprising the steps of: after the coiling step, carrying out descaling and a cold rolling step of carrying out cold rolling to obtain the steel plate.
3. The method for producing a hot stamped part according to claim 2, further comprising the steps of: after the cold rolling step, performing an annealing step to obtain the steel sheet.
4. The method for producing a hot stamped part according to claim 1 , further comprising the steps of: performing descaling after the coiling step; and performing an annealing step to obtain the steel sheet.
5. The chemical composition, in mass%, V: 2.0% or less, Ta: 0.5% or less, and W: 3.0% or less The method for producing a hot stamped part according to claim 1 , further comprising:
6. The chemical composition, in mass%, Ni: 5.0% or less, Cu: 3.0% or less, and Mo: 0.5% or less The method for producing a hot stamped part according to claim 1 or claim 5, further comprising one or more selected from the group consisting of:
7. The chemical composition, in mass%, Mg: 0.003% or less, Ca: 0.003% or less, La: 0.03% or less, and Ce: 0.03% or less The method for producing a hot stamped part according to claim 1 , claim 5 , or claim 6 , further comprising one or more selected from the group consisting of:
Citation Information
Patent Citations
Hot-pressed steel sheet member, manufacturing method therefor and steel sheet to be hot-pressed
JP2006152427A
Hot rolled steel sheet for hot press, method for producing the same and method for producing hot press formed member
JP2006265583A
Steel sheet to be hot-pressed, hot-pressed steel sheet member, and method for manufacturing them
JP2007314817A
Steel sheet for hot pressing and method for producing the same, and method for producing hot-pressed steel sheet member
JP2010047786A
Steel sheet for quenching and high strength member
JP2010121209A