Hot rolled steel plate
A hot-rolled steel sheet with controlled chemical composition and metallographic structure addresses the challenge of high strength and formability by enhancing hole expandability and shear workability, reducing manufacturing costs and improving end surface precision.
Patent Information
- Application Number
- JP2022545465
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2020-08-27
- Filing Date
- 2021-06-15
- Publication Date
- 2024-10-09
- Estimated Expiration
- 2041-06-15
AI Technical Summary
Existing high-strength steel plates face challenges in achieving both high strength and excellent formability, particularly in terms of hole expandability and shear workability, which are crucial for automobile parts, leading to increased manufacturing costs due to the need for post-processing to control fracture surface irregularities after shearing.
A hot-rolled steel sheet with a specific chemical composition and metallographic structure, characterized by a high fraction of martensite and tempered martensite, controlled Mn segregation, and fine austenite grain size, achieved through precise control of hot rolling and cooling processes, enhances tensile strength and improves hole expandability and shear workability.
The solution results in a steel sheet with excellent strength, hole expandability, and shear workability, reducing the likelihood of cracking during bending and enhancing the precision of end surface accuracy after shearing, thus lowering manufacturing costs and improving industrial applicability.
Smart Images

Figure 0007564463000013 
Figure 0007564463000001 
Figure 0007564463000002
Abstract
Description
[Technical field]
[0001] The present invention relates to a hot-rolled steel sheet. Specifically, the present invention relates to a hot-rolled steel sheet that is used by being formed into various shapes by press working or the like, and in particular to a hot-rolled steel sheet that has high strength and excellent hole expandability and shear workability. This application claims priority based on Japanese Patent Application No. 2020-143745, filed on August 27, 2020, the contents of which are incorporated herein by reference. [Background technology]
[0002] In recent years, from the viewpoint of protecting the global environment, efforts are being made in many fields to reduce carbon dioxide emissions. Automobile manufacturers are also actively developing technologies to reduce the weight of vehicles in order to improve fuel efficiency. However, reducing the weight of vehicles is not an easy task, as emphasis is also placed on improving crashworthiness to ensure the safety of passengers.
[0003] In order to achieve both weight reduction and crashworthiness, the use of high-strength steel sheets to thin components has been considered. For this reason, there is a strong demand for steel sheets that combine high strength with excellent formability, and several technologies have been proposed to meet these demands. Since there are various processing styles for automotive components, the required formability varies depending on the component to which it is applied, but among them, hole expandability is positioned as an important indicator of formability. In addition, automotive components are formed by press forming, and the blank sheets for press forming are often manufactured by shear processing, which has high productivity.
[0004] For example, Patent Document 1 discloses a high-strength steel sheet for automobiles with excellent crashworthiness and formability, in which retained austenite with an average grain size of 5 μm or less is dispersed in ferrite with an average grain size of 10 μm or less. In a steel sheet containing retained austenite in the metal structure, the austenite transforms into martensite during processing, and shows large elongation due to transformation-induced plasticity, but the formation of hard martensite impairs hole expandability. Patent Document 1 discloses that by refining the ferrite and retained austenite, not only ductility but also hole expandability is improved.
[0005] Patent Document 2 discloses a high-strength steel sheet having excellent elongation and hole expandability and a tensile strength of 980 MPa or more, in which a second phase consisting of retained austenite and / or martensite is finely dispersed within crystal grains.
[0006] Patent Documents 3 and 4 disclose a high-tensile hot-rolled steel sheet having excellent ductility and hole expandability and a manufacturing method thereof. Patent Document 3 discloses a manufacturing method of a high-strength hot-rolled steel sheet having excellent ductility and stretch flangeability, in which the sheet is cooled to a temperature range of 720°C or less within 1 second after completion of hot rolling, is allowed to stay in a temperature range of more than 500°C and less than 720°C for 1 to 20 seconds, and is then coiled in a temperature range of 350 to 500°C. Patent Document 4 also discloses a high-strength hot-rolled steel sheet having excellent ductility and stretch flangeability, which is mainly composed of bainite, has an appropriate amount of polygonal ferrite and retained austenite, and has an average grain size of 15 μm or less of grains surrounded by grain boundaries having a crystal orientation difference of 15° or more in the steel structure excluding the retained austenite. [Prior art documents] [Patent documents]
[0007] [Patent Document 1] Japanese Patent Application Publication No. 11-61326 [Patent Document 2] Japanese Patent Publication No. 2005-179703 [Patent Document 3] Japanese Patent Publication No. 2012-251200 [Patent Document 4] Japanese Patent Application Publication No. 2015-124410 [Non-patent literature]
[0008] [Non-Patent Document 1] J. Webel, J. Gola, D. Britz, F. Mucklich, Materials Characterization 144 (2018) 584-596 [Non-Patent Document 2] DL Naik, HU Sajid, R. Kiran, Metals 2019, 9, 546 [Non-Patent Document 3] K. Zuiderveld, Contrast Limited Adaptive Histogram Equalization, Chapter VIII.5, Graphics Gems IV. PS Heckbert (Eds.), Cambridge, MA, Academic Press, 1994, pp. 474-485 Summary of the Invention [Problem to be solved by the invention]
[0009] Since there are various processing styles for automotive parts, the required formability varies depending on the part to which it is applied, but among them, hole expandability is positioned as an important indicator of formability. In addition, automotive parts are formed by press forming, and the blank sheets for press forming are often manufactured by shear processing, which has high productivity, so the end surface accuracy after shear processing is required to be excellent. In particular, for high-strength steel plates of 980 MPa or more, the load required for post-processing such as coining after shear processing is large, so it is desired to control the unevenness of the fracture surface at the end surface after shear processing with particularly high precision.
[0010] The techniques disclosed in Patent Documents 1 to 4 are all techniques for improving strength and press formability during hole expansion, but there is no mention of a technique for improving shear workability. This means that post-processing will be required at the stage of press forming the part, which is presumably going to increase manufacturing costs.
[0011] The present invention has been made in consideration of the above problems of the conventional technology, and has an object to provide a hot-rolled steel sheet having high strength as well as excellent hole expandability and shear workability. [Means for solving the problem]
[0012] In view of the above-mentioned problems, the present inventors have conducted extensive research into the chemical composition and metal structure of a hot-rolled steel sheet and the relationship between the chemical composition and metal structure and the mechanical properties thereof, and have obtained the following findings (a) to (f) and completed the present invention. In addition, having excellent shear workability means that the boundary between the fracture surface and the shear surface at the end surface after shear processing has high linearity. This is because if the boundary between the fracture surface and the shear surface at the end surface after shear processing has high linearity, it can be considered that the end surface precision after shear processing is excellent. In addition, having excellent or high strength means that the tensile strength is 980 MPa or more.
[0013] (a) In order to obtain excellent tensile (maximum) strength and hole expandability, it is preferable that the matrix structure of the metal structure is hard. In other words, it is preferable that the fraction of soft structures such as ferrite and bainite is as small as possible.
[0014] (b) In order to form a large amount of martensite and tempered martensite, it is effective to quickly cool the austenite structure to a predetermined temperature. Therefore, it is effective to cool to a predetermined temperature without intermediate air cooling during the hot rolling process.
[0015] (c) In order to improve the linearity of the boundary between the fracture surface and the shear surface at the end face after shearing, it is important to have a metal structure with little Mn segregation, a non-periodic, random microstructure, and a non-uniform (low uniformity) structure.
[0016] (d) Specifically, it is effective to keep the standard deviation of the Mn concentration below a certain value and to control the periodicity and uniformity of the metallographic structure in order to improve the linearity of the boundary between the fracture surface and the shear surface at the end face after shearing.
[0017] (e) In order to keep the standard deviation of Mn concentration below a certain value, the slab heating process and the subsequent hot rolling process are important. For example, it is effective to hold the slab in the temperature range of 700 to 850°C for 900 seconds or more, then further heat it and hold it in the temperature range of 1100°C or higher for 6000 seconds or more, and to perform hot rolling in the temperature range of 850°C to 1100°C so that the sheet thickness is reduced by 90% or more in total.
[0018] (f) In order to reduce the periodicity of the microstructure, it is important to control the recrystallization behavior of austenite during hot rolling. For example, it is effective to control the reduction rate and rolling temperature in the final stage of hot rolling within a predetermined range, to set the stress applied to the steel sheet after the rolling one stage before the final stage of hot rolling and before the rolling in the final stage to 170 kPa or more, and to set the stress applied to the steel sheet after the rolling in the final stage of hot rolling and until the steel sheet is cooled to 800°C to less than 200 kPa. By using such hot rolling conditions, fine and equiaxed recrystallized austenite grains can be created, and by combining with the subsequent cooling conditions, the periodicity of the microstructure can be reduced.
[0019] The gist of the present invention made based on the above findings is as follows. (1) A hot-rolled steel sheet according to one aspect of the present invention has a chemical composition, in mass%, C: 0.040~0.250%, Si: 0.05 to 3.00%, Mn: 1.00-4.00%, Sol.Al: 0.001~0.500%, P: 0.100% or less, S: 0.0300% or less, N: 0.1000% or less, O: 0.0100% or less, Ti: 0 to 0.300%, Nb: 0 to 0.300%, V: 0 to 0.500%, Cu: 0-2.00%, Cr: 0-2.00%, Mo: 0-1.00%, Ni: 0-2.00%, B: 0~0.0100%, Ca: 0 to 0.0200%, Mg: 0 to 0.0200%, REM: 0~0.1000%, Bi: 0 to 0.020%, One or more of Zr, Co, Zn and W: 0 to 1.00% in total, and Sn: 0 to 0.05% the balance being Fe and impurities, The metal structure is In area%, The total content of martensite and tempered martensite is more than 92.0% and not more than 100.0%; The retained austenite is less than 3.0%. Ferrite is less than 5.0%; The E value indicating the periodicity of the metal structure is 11.0 or more, and the I value indicating the uniformity of the metal structure is less than 1.020, The standard deviation of the Mn concentration is 0.60 mass% or less; It is characterized by having a tensile strength of 980 MPa or more. (2) The hot-rolled steel sheet according to (1) above may have an average crystal grain size in the surface layer of less than 3.0 μm. (3) The hot-rolled steel sheet according to the above (1) or (2), wherein the chemical composition is, in mass%, Ti: 0.005 to 0.300%, Nb: 0.005 to 0.100%, V: 0.005~0.500%, Cu: 0.01-2.00%, Cr: 0.01-2.00%, Mo: 0.01 to 1.00%, Ni: 0.02 to 2.00%, B: 0.0001~0.0100%, Ca: 0.0005~0.0200%, Mg: 0.0005~0.0200%, REM: 0.0005 to 0.1000%, and Bi: 0.0005 to 0.020% The resin may contain one or more selected from the group consisting of: Effect of the Invention
[0020] According to the above-mentioned aspect of the present invention, it is possible to obtain a hot-rolled steel sheet having excellent strength, hole expandability and shear workability. Also, according to the above-mentioned preferred aspect of the present invention, it is possible to obtain a hot-rolled steel sheet having the above-mentioned properties and further suppressing the occurrence of internal cracks in bending, i.e., having excellent resistance to internal cracks in bending. The hot-rolled steel sheet according to the above aspect of the present invention is suitable as an industrial material used for automobile parts, machine structural parts, and further building parts. [Brief description of the drawings]
[0021] [Figure 1] FIG. 13 is a diagram for explaining a method for measuring the linearity of the boundary between the fracture surface and the shear surface at the end face after shearing. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0022] The chemical composition and metal structure of the hot-rolled steel sheet according to this embodiment will be described in more detail below. However, the present invention is not limited to the configuration disclosed in this embodiment, and various modifications are possible without departing from the spirit of the present invention. In the following, the numerical ranges described with "~" include the lower and upper limits. Numerical values indicated as "less than" or "more than" are not included in the numerical range. In the following description, percentages related to the chemical composition of the steel sheet are mass% unless otherwise specified.
[0023] 1.Chemical composition The hot-rolled steel sheet according to the present embodiment contains, by mass%, C: 0.040-0.250%, Si: 0.05-3.00%, Mn: 1.00-4.00%, sol.Al: 0.001-0.500%, P: 0.100% or less, S: 0.0300% or less, N: 0.1000% or less, O: 0.0100% or less, and the balance: Fe and impurities. Each element will be described in detail below.
[0024] (1-1) C: 0.040-0.250% C increases the area fraction of the hard phase. In addition, C increases the strength of martensite by combining with precipitation strengthening elements such as Ti, Nb, and V. If the C content is less than 0.040%, it is difficult to obtain the desired strength. If the C content is less than 0.040%, the ferrite fraction increases, and the I value also increases due to the influence of the flat ferrite structure. Therefore, the C content is set to 0.040% or more. The C content is preferably 0.060% or more, more preferably 0.070% or more. On the other hand, if the C content exceeds 0.250%, the formation of pearlite with low strength is promoted, and the area fraction of martensite and tempered martensite decreases, thereby decreasing the strength of the hot-rolled steel sheet. If the C content exceeds 0.250%, the flat cementite structure increases, and the E value decreases due to the influence of the formation of carbide regions with small brightness difference. Therefore, the C content is set to 0.250% or less. The C content is preferably 0.150% or less.
[0025] (1-2) Si: 0.05-3.00% Si has the effect of delaying the precipitation of cementite. This effect can increase the area fraction of martensite and tempered martensite, and can increase the strength of the steel sheet by solid solution strengthening. In addition, Si has the effect of making the steel sound by deoxidization (suppressing the occurrence of defects such as blowholes in the steel). If the Si content is less than 0.05%, the above effect cannot be obtained. If the Si content is less than 0.05%, the flat cementite structure increases, and the I value also increases due to the effect of the generation of carbide regions with small brightness differences. Therefore, the Si content is set to 0.05% or more. The Si content is preferably 0.50% or more, 1.00% or more. However, if the Si content exceeds 3.00%, the surface properties and chemical conversion treatability of the steel sheet, as well as the hole expandability and weldability, are significantly deteriorated, and the A3 transformation point is significantly increased. This makes it difficult to perform stable hot rolling. Furthermore, if the Si content exceeds 3.00%, the ferrite fraction increases and the E value decreases due to the influence of the flat ferrite structure. Therefore, the Si content is set to 3.00% or less. The Si content is preferably 2.70% or less, and more preferably 2.50% or less.
[0026] (1-3) Mn: 1.00-4.00% Mn has the effect of suppressing ferrite transformation and increasing the strength of the steel sheet. If the Mn content is less than 1.00%, a tensile strength of 980 MPa or more cannot be obtained. Therefore, the Mn content is set to 1.00% or more. The Mn content is preferably 1.50% or more, 2.00% or more, or 2.30% or more. On the other hand, if the Mn content exceeds 4.00%, the crystal orientation difference of the crystal grains in the hard phase becomes nonuniform due to the segregation of Mn, and the linearity of the boundary between the fracture surface and the shear surface at the end surface after shear processing decreases. Therefore, the Mn content is set to 4.00% or less. The Mn content is preferably 3.70% or less, 3.50% or less.
[0027] (1-4) sol.Al: 0.001-0.500% Like Si, Al has the effect of deoxidizing steel to improve the soundness of the steel sheet, and also has the effect of increasing the area fraction of martensite and tempered martensite by suppressing the precipitation of cementite from austenite. If the sol.Al content is less than 0.001%, the above-mentioned effect cannot be obtained. Therefore, the sol.Al content is set to 0.001% or more. The sol.Al content is preferably 0.010% or more. On the other hand, if the sol.Al content exceeds 0.500%, the above-mentioned effect saturates and is economically undesirable, so the sol.Al content is set to 0.500% or less. The sol.Al content is preferably 0.400% or less, 0.300% or less. In the present embodiment, sol. Al means acid-soluble Al, and indicates solute Al that is present in the steel in a solid solution state.
[0028] (1-5)P:0.100% or less P is an element that is generally contained as an impurity, but it also has the effect of increasing strength by solid solution strengthening. Therefore, P may be actively contained, but P is an element that is easily segregated, and if the P content exceeds 0.100%, the hole expandability caused by grain boundary segregation will decrease significantly. Therefore, the P content is limited to 0.100% or less. The P content is preferably 0.030% or less. There is no need to specify the lower limit of the P content, but it is preferably 0.001% from the viewpoint of refining costs.
[0029] (1-6)S: 0.0300% or less S is an element contained as an impurity, and forms sulfide-based inclusions in steel, thereby reducing the hole expandability of hot-rolled steel sheets. If the S content exceeds 0.0300%, the hole expandability of the steel sheet is significantly reduced. Therefore, the S content is limited to 0.0300% or less. The S content is preferably 0.0050% or less. There is no need to specify a lower limit for the S content, but from the viewpoint of refining costs, it is preferably set to 0.0001%.
[0030] (1-7)N: 0.1000% or less N is an element contained in steel as an impurity, and has the effect of reducing the hole expandability of the steel sheet. If the N content exceeds 0.1000%, the hole expandability of the steel sheet is significantly reduced. Therefore, the N content is set to 0.1000% or less. The N content is preferably 0.0800% or less, and more preferably 0.0700% or less. There is no need to specify the lower limit of the N content, but it may be set to 0.0001%. As described later, when one or more of Ti, Nb, and V are contained to refine the metal structure, the N content is preferably 0.0010% or more, and more preferably 0.0020% or more, in order to promote the precipitation of carbonitrides.
[0031] (1-8)O: 0.0100% or less When O is contained in steel in a large amount, it forms coarse oxides that become the starting point of fracture, causing brittle fracture and hydrogen-induced cracking. Therefore, the O content is limited to 0.0100% or less. The O content is preferably 0.0080% or less, 0.0050% or less. In order to disperse a large number of fine oxides during deoxidation of molten steel, the O content may be 0.0005% or more, 0.0010% or more.
[0032] The balance of the chemical composition of the hot-rolled steel sheet according to the present embodiment may be Fe and impurities. In the present embodiment, the impurities refer to substances that are mixed in from raw materials such as ore, scrap, or the manufacturing environment, and are permissible within a range that does not adversely affect the hot-rolled steel sheet according to the present embodiment.
[0033] In addition to the above elements, the hot-rolled steel sheet according to the present embodiment may contain Ti, Nb, V, Cu, Cr, Mo, Ni, B, Ca, Mg, REM, Bi, Zr, Co, Zn, W, and Sn as optional elements. When the above optional elements are not contained, the lower limit of the content is 0%. The above optional elements will be described in detail below.
[0034] (1-9) Ti: 0.005-0.300%, Nb: 0.005-0.100%, and V: 0.005-0.500% Ti, Nb and V all precipitate as carbides or nitrides in steel and have the effect of refining the metal structure by the pinning effect, so one or more of these elements may be contained. In order to obtain the above-mentioned effect more reliably, it is preferable that the Ti content is 0.005% or more, the Nb content is 0.005% or more, or the V content is 0.005% or more. That is, it is preferable that the content of at least one of Ti, Nb and V is 0.005% or more. However, even if these elements are contained in excess, the effect of the above-mentioned action is saturated and is not economically preferable. Therefore, the Ti content is 0.300% or less, the Nb content is 0.100% or less, and the V content is 0.500% or less.
[0035] (1-10) Cu: 0.01-2.00%, Cr: 0.01-2.00%, Mo: 0.01-1.00%, Ni: 0.02-2.00% and B: 0.0001-0.0100% Cu, Cr, Mo, Ni and B all have the effect of increasing the hardenability of hot-rolled steel sheets. Cu and Mo also have the effect of precipitating carbides in steel at low temperatures to increase strength. Furthermore, when Cu is contained, Ni has the effect of effectively suppressing grain boundary cracking of slabs caused by Cu. Therefore, one or more of these elements may be contained.
[0036] As described above, Cu has the effect of increasing the hardenability of hot-rolled steel sheets and the effect of precipitating in steel as carbides at low temperatures to increase the strength of the steel sheets. In order to more reliably obtain the effects of the above-mentioned actions, the Cu content is preferably 0.01% or more, and more preferably 0.05% or more. However, if the Cu content exceeds 2.00%, grain boundary cracking of the slab may occur. Therefore, the Cu content is set to 2.00% or less. The Cu content is preferably 1.50% or less, 1.00% or less.
[0037] As described above, Cr has the effect of increasing the hardenability of hot-rolled steel sheets and the effect of precipitating carbides in steel at low temperatures to increase strength. In order to more reliably obtain the effects of the above-mentioned actions, the Cr content is preferably set to 0.01% or more, and more preferably 0.05% or more. However, if the Cr content exceeds 2.00%, the chemical conversion treatability of the steel sheet is significantly reduced. Therefore, the Cr content is set to 2.00% or less.
[0038] As described above, Mo has the effect of increasing the hardenability of hot-rolled steel sheets and the effect of precipitating carbides in steel to increase strength. In order to obtain the above-mentioned effects more reliably, the Mo content is preferably set to 0.01% or more, more preferably 0.02% or more. However, even if the Mo content exceeds 1.00%, the above-mentioned effects are saturated and it is not economically preferable. Therefore, the Mo content is set to 1.00% or less. The Mo content is preferably 0.50% or less, more preferably 0.20% or less.
[0039] As described above, Ni has the effect of increasing the hardenability of the hot-rolled steel sheet. Furthermore, when Cu is contained, Ni has the effect of effectively suppressing grain boundary cracking of the slab caused by Cu. In order to obtain the above-mentioned effect more reliably, it is preferable that the Ni content is 0.02% or more. Since Ni is an expensive element, it is economically undesirable to contain a large amount of Ni. Therefore, the Ni content is set to 2.00% or less.
[0040] As described above, B has the effect of improving the hardenability of hot-rolled steel sheet. In order to obtain the effect of this action more reliably, the B content is preferably 0.0001% or more, and more preferably 0.0002% or more. However, if the B content exceeds 0.0100%, the hole expandability of the steel sheet is significantly reduced, so the B content is set to 0.0100% or less. The B content is preferably set to 0.0050% or less.
[0041] (1-11) Ca: 0.0005-0.0200%, Mg: 0.0005-0.0200%, REM: 0.0005-0.1000%, and Bi: 0.0005-0.020% Ca, Mg and REM all have the effect of improving the hole expandability of the hot-rolled steel sheet by adjusting the shape of the inclusions to a preferred shape. Bi also has the effect of improving the formability of the hot-rolled steel sheet by refining the solidification structure. Therefore, one or more of these elements may be contained. In order to more reliably obtain the effect of the above action, it is preferable that any one or more of Ca, Mg, REM and Bi is 0.0005% or more. However, if the Ca content or Mg content exceeds 0.0200%, or if the REM content exceeds 0.1000%, inclusions are excessively generated in the steel, which may actually reduce the hole expandability of the steel sheet. Also, even if the Bi content exceeds 0.020%, the effect of the above action is saturated, which is not economically preferable. Therefore, the Ca content and Mg content are 0.0200% or less, the REM content is 0.1000% or less, and the Bi content is 0.020% or less. The Bi content is preferably 0.010% or less. Here, REM refers to a total of 17 elements consisting of Sc, Y and lanthanides, and the content of the above REM refers to the total content of these elements. In the case of lanthanides, they are added industrially in the form of misch metals.
[0042] (1-12) One or more of Zr, Co, Zn and W: 0 to 1.00% in total and Sn: 0 to 0.05% The inventors have confirmed that the effect of the hot-rolled steel sheet according to the present embodiment is not impaired even if the total content of Zr, Co, Zn, and W is 1.00% or less. Therefore, one or more of Zr, Co, Zn, and W may be contained in a total content of 1.00% or less. The inventors have confirmed that the effect of the hot-rolled steel sheet according to the present embodiment is not impaired even if a small amount of Sn is contained. However, since defects may occur during hot rolling, the Sn content is set to 0.05% or less.
[0043] The chemical composition of the above-mentioned hot-rolled steel sheet may be measured by a general analytical method. For example, it may be measured by using ICP-AES (Inductively Coupled Plasma-Atomic Emission Spectrometry). Sol. Al may be measured by ICP-AES using the filtrate after thermally decomposing the sample with acid. C and S may be measured by the combustion-infrared absorption method, N by the inert gas fusion-thermal conductivity method, and O by the inert gas fusion-non-dispersive infrared absorption method.
[0044] 2. Metal structure of hot-rolled steel sheets Next, the metal structure of the hot-rolled steel sheet according to this embodiment will be described. In the hot-rolled steel sheet according to the present embodiment, the metal structure has, in terms of area%, a total of more than 92.0% and 100.0% or less of martensite and tempered martensite, less than 3.0% of retained austenite, less than 5.0% of ferrite, an E value indicating the periodicity of the metal structure of 11.0 or more, an I value indicating the uniformity of the metal structure of less than 1.020, and a standard deviation of the Mn concentration of 0.60 mass% or less. Therefore, the hot-rolled steel sheet according to the present embodiment can obtain excellent strength, hole expandability, and shear workability. In this embodiment, the metal structure at a ¼ depth position of the sheet thickness from the surface and at the center position in the sheet width direction of the cross section parallel to the rolling direction is specified. The reason is that the metal structure at this position shows a typical metal structure of the steel sheet.
[0045] (2-1) Area fraction of retained austenite: less than 3.0% The retained austenite is a metal structure that exists as a face-centered cubic lattice even at room temperature. The retained austenite has the effect of increasing the hole expandability of the hot-rolled steel sheet by transformation-induced plasticity (TRIP). On the other hand, the retained austenite is transformed into high-carbon martensite during shearing, which inhibits stable crack generation and causes a decrease in the linearity of the boundary between the fracture surface and the shear surface at the end surface after shearing. When the area fraction of the retained austenite is 3.0% or more, the above effect becomes apparent, and not only the shear workability of the hot-rolled steel sheet deteriorates (the linearity of the boundary between the fracture surface and the shear surface at the end surface after shearing decreases), but also the hole expandability decreases. Therefore, the area fraction of the retained austenite is less than 3.0%. The area fraction of the retained austenite is preferably 1.5% or less, and more preferably less than 1.0%. Since the smaller the amount of retained austenite, the more preferable it is, the area fraction of the retained austenite may be 0%.
[0046] (2-2) Area fraction of ferrite: less than 5.0% Ferrite is generally a soft metal structure. If the ferrite contains more than a certain amount, the desired strength may not be obtained, and the area of the sheared surface at the end face after shearing may increase. If the area of the sheared surface at the end face after shearing increases, the linearity of the boundary between the fracture surface and the sheared surface at the end face decreases, which is not preferable. If the area fraction of ferrite is 5.0% or more, the above-mentioned effect becomes apparent, and the shear workability of the hot-rolled steel sheet deteriorates. Therefore, the area fraction of ferrite is less than 5.0%. The area fraction of ferrite is preferably 3.0% or less, more preferably 2.0% or less, and even more preferably less than 1.0%. Since the less ferrite, the more preferable it is, the area fraction of ferrite may be 0%.
[0047] Methods for measuring the area fraction of retained austenite include X-ray diffraction, EBSP (Electron Back Scattering Diffraction Pattern) analysis, magnetic measurement, etc., and the measured value may differ depending on the measurement method. In this embodiment, the area fraction of retained austenite is measured by X-ray diffraction. In the measurement of the area fraction of retained austenite by X-ray diffraction in this embodiment, first, in a cross section parallel to the rolling direction at a depth position of 1 / 4 of the sheet thickness of the hot-rolled steel sheet (a region from 1 / 8 of the sheet thickness from the surface to 3 / 8 of the sheet thickness from the surface) and at the center position in the sheet width direction, Co-Kα radiation is used to determine the integrated intensities of a total of six peaks, α(110), α(200), α(211), γ(111), γ(200), and γ(220), and the area fraction of retained austenite is calculated using an intensity averaging method.
[0048] The area fraction of ferrite is measured by the following method. A cross section parallel to the rolling direction is mirror-finished and polished for 8 minutes at room temperature using colloidal silica that does not contain an alkaline solution to remove strain introduced into the surface layer of the sample. At any position in the longitudinal direction of the sample cross section, a region 50 μm long and from 1 / 8 of the plate thickness depth from the surface to 3 / 8 of the plate thickness depth from the surface is measured at measurement intervals of 0.1 μm using electron backscatter diffraction to obtain crystal orientation information. For the measurement, an EBSD analysis device consisting of a thermal field emission scanning electron microscope (JEOL JSM-7001F) and an EBSD detector (TSL DVC5 detector) is used. The degree of vacuum inside the EBSD analysis device was 9.6×10 -5 The irradiation current level is 13, and the electron beam irradiation level is 62.
[0049] Next, a backscattered electron image is taken in the same field of view. The backscattered electron image is used to identify crystal grains in which ferrite and cementite are precipitated in layers, and the area fraction of the crystal grains is calculated, thereby obtaining the area fraction of pearlite.
[0050] Then, for the crystal grains other than those determined to be pearlite, the obtained crystal orientation information is used to determine the areas with a Grain Average Misorientation value of 1.0° or less as ferrite using the "Grain Average Misorientation" function in the "OIM Analysis (registered trademark)" software that comes with the EBSD analyzer. The area fraction of the ferrite is obtained by calculating the area fraction of the areas determined to be ferrite.
[0051] Next, within the remaining region (region where the Grain Average Misorientation value exceeds 1.0°), under the condition that the 5° grain boundary is defined as the crystal grain boundary, when the maximum value of the "Grain Average IQ" of the ferrite region is Iα, the region where it exceeds Iα / 2 is extracted as bainite. The area fraction of bainite can be obtained by calculating the area ratio of the extracted bainite.
[0052] (2-3) Sum of area fractions of martensite and tempered martensite: more than 92.0% and less than or equal to 100.0% If the total area fraction of martensite and tempered martensite is 92.0% or less, the desired strength cannot be obtained. Therefore, the total area fraction of martensite and tempered martensite is set to be more than 92.0%. It is preferably 95.0% or more, 97.0% or more, or 99.0% or more. The total area fraction of martensite and tempered martensite is preferably as large as possible, so it may be set to 100.0%.
[0053] The method for measuring the area fraction of martensite and tempered martensite will be described below. First, in order to observe the same region as the EBSD measurement region where the area fraction of ferrite was measured with an SEM, a Vickers indentation is stamped near the observation position. After that, the surface contamination is polished away, leaving the structure of the observation surface, and the surface is etched with nital. Next, the same field of view as the EBSD observation surface is observed with an SEM at a magnification of 3000 times. Among the regions that are determined to have structures other than ferrite in the EBSD measurement, the regions that have a substructure within the grains and where cementite is precipitated with multiple variants are determined to be tempered martensite. Regions that have a high brightness and whose substructure is not revealed by etching are determined to be "martensite and retained austenite". The area fractions of tempered martensite and "martensite and retained austenite" are obtained by calculating the respective area fractions. The area fraction of martensite is obtained by subtracting the area fraction of retained austenite obtained by the above-mentioned X-ray diffraction from the obtained area fraction of "martensite and retained austenite". The sum of the area fractions of martensite and tempered martensite is calculated to obtain the sum of the area fractions of martensite and tempered martensite. Contamination on the surface of the observation surface can be removed by buffing using alumina particles with a particle size of 0.1 μm or less, or by Ar ion sputtering or other methods.
[0054] The heat-rolled steel sheet according to this embodiment may contain, as a remaining structure, one or both of bainite and pearlite, the total area fraction of which is 0% or more and less than 8.0%.
[0055] (2-4) E value: 11.0 or more, I value: less than 1.020 In order to improve the linearity of the boundary between the fracture surface and the shear surface at the end face after shearing, it is important to reduce the periodicity of the metal structure and the uniformity of the metal structure. In this embodiment, the linearity of the boundary between the fracture surface and the shear surface at the end face after shearing is improved by controlling the E (Entropy) value, which indicates the periodicity of the metal structure, and the I (Inverse Differential Moment Norm) value, which indicates the uniformity of the metal structure.
[0056] The E value represents the periodicity of the metal structure. When the luminance is periodically arranged due to the effect of the formation of a band-shaped structure, that is, when the periodicity of the metal structure is high, the E value decreases. In this embodiment, since it is necessary to have a metal structure with low periodicity, it is necessary to increase the E value. If the E value is less than 11.0, the linearity of the boundary between the fracture surface and the shear surface at the end surface after shear processing is likely to decrease. In a metal structure with high periodicity, that is, a low E value, a crack is generated starting from the periodically arranged structure and running through multiple band-shaped structures present near the starting point to form a fracture surface. As a result, it is estimated that the linearity of the boundary between the fracture surface and the shear surface at the end surface after shear processing is likely to decrease. Therefore, the E value is set to 11.0 or more. It is preferably 11.1 or more, and more preferably 11.2 or more. The higher the E value, the better. There is no particular upper limit to the E value, but it may be 13.5 or less, 13.0 or less, 12.5 or less, or 12.0 or less.
[0057] The I value represents the uniformity of the metal structure, and increases as the area of the region having a certain brightness becomes larger. A high I value means that the uniformity of the metal structure is high. In this embodiment, it is necessary to make the metal structure mainly composed of martensite with low brightness uniformity, so it is necessary to reduce the I value. When the uniformity of the metal structure is high, that is, when the I value is high, cracks are likely to occur from the tip of the shear tool due to the effects of precipitates and element concentration differences in the crystal grains, and hardness differences caused by the soft ferrite phase. As a result, the linearity of the boundary between the fracture surface and the shear surface at the end surface after shear processing is likely to decrease. In other words, if the I value is 1.020 or more, it is estimated that the linearity of the boundary between the fracture surface and the shear surface at the end surface after shear processing cannot be improved. Therefore, the I value is less than 1.020. It is preferably 1.015 or less, and more preferably 1.010 or less. There is no particular restriction on the lower limit of the I value, but it may be 0.900 or more, 0.950 or more, or 1.000 or more.
[0058] The E and I values can be obtained by the following method. In this embodiment, the photographed region of the SEM image taken to calculate the E value and I value is a position at a depth of 1 / 4 of the sheet thickness from the surface of the steel sheet (a region from a depth of 1 / 8 of the sheet thickness from the surface to a depth of 3 / 8 of the sheet thickness from the surface) in a cross section parallel to the rolling direction, and at the center position in the sheet width direction. A SU-6600 Schottky electron gun manufactured by Hitachi High-Technologies Corporation is used to photograph the SEM image, with a tungsten emitter and an acceleration voltage of 1.5 kV. Under the above settings, the SEM image is output at a magnification of 1000 times and a gray scale of 256 gradations.
[0059] Next, the obtained SEM image is cut into an area of 880 x 880 pixels, and the image is subjected to smoothing processing with a tile grid size of 8 x 8 and a contrast enhancement limiting factor of 2.0 as described in Non-Patent Document 3. The smoothed SEM image is rotated counterclockwise in 1 degree increments from 0 to 179 degrees, excluding 90 degrees, and an image is created for each degree, resulting in a total of 179 images. Next, for each of these 179 images, the GLCM method described in Non-Patent Document 1 is used to collect the frequency value of the luminance between adjacent pixels in the form of a matrix.
[0060] The matrix of 179 frequency values collected by the above method is expressed as p k (k=0 89, 91, 179). For each image, the generated p k is summed for all k (k=0...89, 91...179), and then a 256 x 256 matrix P is calculated in which the sum of each component is normalized to be 1. Furthermore, the E value and I value are calculated using the following formulas (1) and (2) described in Non-Patent Document 2. In the following formulas (1) and (2), the value in the i-th row and j-th column of matrix P is taken as P ij It is written as follows.
[0061]
number
[0062]
number
[0063] (2-5) Standard deviation of Mn concentration: 0.60 mass% or less The standard deviation of the Mn concentration at a 1 / 4 depth position of the sheet thickness from the surface of the hot-rolled steel sheet according to this embodiment and at the center position in the sheet width direction is 0.60 mass% or less. This allows the hard phase to be uniformly dispersed, and prevents a decrease in the linearity of the boundary between the fracture surface and the shear surface at the end face. In other words, the shear workability can be improved. The standard deviation of the Mn concentration is preferably 0.50 mass% or less, and more preferably 0.47 mass% or less. From the viewpoint of suppressing excessive burrs, the smaller the lower limit of the standard deviation of the Mn concentration, the more desirable it is, but due to the constraints of the manufacturing process, the substantial lower limit is 0.10 mass%.
[0064] After mirror polishing a cross section (L cross section) parallel to the rolling direction of the hot-rolled steel sheet, the standard deviation of the Mn concentration is measured at a 1 / 4 depth position of the sheet thickness from the surface of the steel sheet (a region from 1 / 8 depth of the sheet thickness from the surface to 3 / 8 depth of the sheet thickness from the surface) and at the center position in the sheet width direction with an electron probe microanalyzer (EPMA). The measurement conditions are an acceleration voltage of 15 kV and a magnification of 5000 times, and a distribution image is measured in a range of 20 μm in the sample rolling direction and 20 μm in the sample sheet thickness direction. More specifically, the measurement interval is 0.1 μm, and the Mn concentration is measured at 40,000 or more points. Next, the standard deviation is calculated based on the Mn concentrations obtained from all measurement points to obtain the standard deviation of the Mn concentration.
[0065] (2-6) Average crystal grain size of the surface layer: less than 3.0 μm If the grain size of the surface layer is fine, it is possible to suppress cracks on the inside of the bend of hot-rolled steel sheets. The higher the strength of the steel sheet, the more likely it is that cracks will occur from the inside of the bend during bending (hereinafter referred to as cracks on the inside of the bend). The mechanism of cracks on the inside of the bend is presumed to be as follows. During bending, compressive stress is generated on the inside of the bend. At first, the entire inside of the bend is uniformly deformed as the bending proceeds, but as the amount of deformation increases, the deformation cannot be borne by the uniform deformation alone, and strain is concentrated locally, causing the deformation to proceed (generation of shear deformation bands). As this shear deformation band continues to grow, cracks are generated along the shear bands from the inside surface of the bend and grow. It is presumed that the reason why cracks on the inside of the bend tend to occur with increasing strength is that the decrease in work hardening ability associated with increasing strength makes it difficult for uniform deformation to proceed, making it easier for deformation bias to occur, which causes shear deformation bands to occur early in the bending process (or under loose processing conditions).
[0066] Research by the present inventors has revealed that internal cracks during bending are prominent in steel sheets with a tensile strength of 980 MPa or more. The present inventors have also found that the finer the crystal grain size in the surface layer of the hot-rolled steel sheet, the more localized strain concentration is suppressed, and the less likely internal cracks are to occur during bending. In order to achieve the above effect, the average crystal grain size in the surface layer of the hot-rolled steel sheet is preferably less than 3.0 μm, and more preferably 2.5 μm or less. In this embodiment, the surface layer refers to a region from the surface of the heat-rolled steel sheet to a depth of 50 μm from the surface.
[0067] The grain size of the surface layer is measured using the EBSP-OIM method described above. In a cross section parallel to the rolling direction, an analysis is performed in at least five fields of view in a region of 40 μm × 30 μm at a magnification of 1200 times in a region from the surface of the hot-rolled steel sheet to a depth of 50 μm from the surface and at the center position in the sheet width direction. A location where the angle difference between adjacent measurement points is 5° or more is defined as a grain boundary, and the area-average grain size is calculated. The obtained area-average grain size is regarded as the average grain size of the surface layer. In addition, since retained austenite is not a structure formed by phase transformation at 600℃ or less and does not have the effect of dislocation accumulation, this measurement method does not analyze retained austenite. With the EBSP-OIM method, retained austenite with an fcc crystal structure can be excluded from the analysis.
[0068] 3. Tensile strength properties The hot-rolled steel sheet according to this embodiment has a tensile (maximum) strength of 980 MPa or more. If the tensile strength is less than 980 MPa, the applicable parts are limited, and the contribution to the weight reduction of the vehicle body is small. The upper limit does not need to be particularly set, but may be 1780 MPa from the viewpoint of suppressing die wear. The tensile strength is measured in accordance with JIS Z 2241: 2011 using a No. 5 test piece of JIS Z 2241: 2011. The tensile test piece is taken from a quarter part from the end in the plate width direction, and the direction perpendicular to the rolling direction is the longitudinal direction.
[0069] 4.Hole expansion characteristics The hot-rolled steel sheet according to the present embodiment preferably has a hole expansion ratio λ of 55% or more. When the hole expansion ratio λ is 55% or more, a hot-rolled steel sheet that contributes greatly to reducing the weight of a vehicle body can be obtained without being limited to applicable parts. There is no need to particularly limit the upper limit. The hole expansion ratio λ is measured in accordance with JIS Z 2256: 2010 using a No. 5 test piece of JIS Z 2241: 2011. The hole expansion test piece may be taken from a 1 / 4 portion from the end in the sheet width direction of the hot-rolled steel sheet.
[0070] 5. Plate thickness The thickness of the hot-rolled steel sheet according to this embodiment is not particularly limited, but may be 0.5 to 8.0 mm. By making the thickness of the hot-rolled steel sheet 0.5 mm or more, it is easy to ensure the rolling completion temperature and the rolling load can be reduced, and hot rolling can be easily performed. Therefore, the thickness of the hot-rolled steel sheet according to this embodiment may be 0.5 mm or more. It is preferably 1.2 mm or more, 1.4 mm or more. Moreover, by making the thickness 8.0 mm or less, it is easy to make the metal structure fine, and the above-mentioned metal structure can be easily ensured. Therefore, the thickness may be 8.0 mm or less. It is preferably 6.0 mm or less.
[0071] 6.Other (6-1) Plating layer The hot-rolled steel sheet according to the present embodiment having the above-mentioned chemical composition and metal structure may be provided with a plating layer on the surface for the purpose of improving corrosion resistance, etc., to form a surface-treated steel sheet. The plating layer may be an electroplating layer or a hot-dip plating layer. Examples of the electroplating layer include electrogalvanizing and electrogalvanizing Zn-Ni alloy plating. Examples of the hot-dip plating layer include hot-dip galvanizing, alloyed hot-dip galvanizing, hot-dip aluminum plating, hot-dip Zn-Al alloy plating, hot-dip Zn-Al-Mg alloy plating, and hot-dip Zn-Al-Mg-Si alloy plating. The coating weight is not particularly limited and may be the same as in the past. In addition, it is also possible to further improve the corrosion resistance by performing an appropriate chemical conversion treatment (for example, application of a silicate-based chromium-free chemical conversion treatment liquid and drying) after plating.
[0072] 7.Manufacturing conditions A suitable method for producing the hot-rolled steel sheet according to this embodiment having the above-mentioned chemical composition and metal structure is as follows.
[0073] In order to obtain the hot-rolled steel sheet according to this embodiment, it is important to heat the slab under prescribed conditions, then perform hot rolling, accelerate cooling to a prescribed temperature range, and control the cooling history after coiling.
[0074] In a preferred method for producing a hot-rolled steel sheet according to this embodiment, the following steps (1) to (8) are carried out in sequence. Note that the temperature of the slab and the temperature of the steel sheet in this embodiment refer to the surface temperature of the slab and the surface temperature of the steel sheet. (1) The slab is held in the temperature range of 700°C to 850°C for 900 seconds or more, and then further heated and held in the temperature range of 1100°C or higher for 6000 seconds or more. (2) Hot rolling is performed in the temperature range of 850 to 1100°C to reduce the plate thickness by a total of 90% or more. (3) After the rolling stage before the final stage of hot rolling and before the final stage of rolling, a stress of 170 kPa or more is applied to the steel plate. (4) The reduction rate in the final stage of hot rolling is 8% or more, and the hot rolling is completed so that the rolling completion temperature Tf is 900°C or more and less than 960°C. (5) The stress applied to the steel plate after the final stage of hot rolling and before the steel plate is cooled to 800°C is less than 200 kPa. (6) Within 1 second after the completion of hot rolling, the material is cooled to a temperature range below the hot rolling completion temperature Tf-50°C, and then cooled at an average cooling rate of 50°C / sec or more according to the following formula: <1> However, it is more preferable to cool the material to a temperature range of the hot rolling completion temperature Tf-50°C or lower within 1 second after the completion of hot rolling. (7) Cool from T1 (°C) to the coiling temperature at an average cooling rate of 50°C / sec or more. (8) The winding temperature is 350°C or less.
[0075] T1(℃)=770-270×[C]-90×[Mn]-37×[Ni]-70×[Cr]-83×[Mo]… <1> In the formulas, the [element symbol] indicates the content (mass%) of each element in the steel. If the element is not contained, 0 is substituted.
[0076] By adopting the above manufacturing method, it is possible to stably manufacture a hot-rolled steel sheet having a metal structure excellent in strength, hole expandability, and shear workability. That is, by appropriately controlling the slab heating conditions and hot rolling conditions, Mn segregation is reduced and the pre-transformation austenite is made equiaxed, and in combination with the cooling conditions after hot rolling described later, a hot-rolled steel sheet having a desired metal structure can be stably manufactured.
[0077] (7-1) Slab, slab temperature when subjected to hot rolling, and holding time The slab to be subjected to hot rolling may be a slab obtained by continuous casting or a slab obtained by casting and blooming, and may be one that has been subjected to hot or cold working, if necessary. The slab to be subjected to hot rolling is preferably held in a temperature range of 700°C to 850°C during heating for 900 seconds or more, and then further heated and held in a temperature range of 1100°C or higher for 6000 seconds or more. When held in a temperature range of 700°C to 850°C, the steel sheet temperature may be varied within this temperature range or may be constant. When held in a temperature range of 1100°C or higher, the steel sheet temperature may be varied within a temperature range of 1100°C or higher or may be constant.
[0078] During the austenite transformation at 700°C to 850°C, Mn is distributed between ferrite and austenite, and by extending the transformation time, Mn can diffuse into the ferrite region. This eliminates Mn microsegregation unevenly distributed in the slab and significantly reduces the standard deviation of Mn concentration. By reducing the standard deviation of Mn concentration, the linearity of the fracture surface and shear surface at the end surface after shear processing can be improved. In order to reduce the standard deviation of the Mn concentration, the holding time in the temperature range of 1100° C. or higher is preferably 6000 seconds or more. In order to obtain the desired amount of martensite and tempered martensite, the temperature at which the material is held for 6000 seconds or more is preferably 1100° C. or higher.
[0079] The hot rolling is preferably performed using a reverse mill or a tandem mill as multi-pass rolling. From the viewpoint of industrial productivity, it is more preferable to perform hot rolling using a tandem mill for at least the final several stages.
[0080] (7-2) Reduction rate of hot rolling: Total thickness reduction of 90% or more in the temperature range of 850 to 1100°C By performing hot rolling to reduce the sheet thickness by 90% or more in total in the temperature range of 850 to 1100°C, mainly recrystallized austenite grains are refined, the accumulation of strain energy in the unrecrystallized austenite grains is promoted, the recrystallization of austenite is promoted, and the atomic diffusion of Mn is promoted, thereby making it possible to reduce the standard deviation of the Mn concentration. Therefore, hot rolling is performed to reduce the sheet thickness by 90% or more in total in the temperature range of 850 to 1100°C. The thickness reduction in the temperature range of 850 to 1100°C can be expressed as (t0-t1) / t0×100(%), where t0 is the entrance thickness before the first pass in rolling in this temperature range, and t1 is the exit thickness after the final pass in rolling in this temperature range.
[0081] (7-3) Stress after the rolling stage before the final stage of hot rolling and before the final stage of rolling: 170 kPa or more It is preferable that the stress applied to the steel sheet after the rolling one stage before the final stage of hot rolling and before the final stage of rolling is 170 kPa or more. <001> The number of grains having a crystal orientation of {110} can be reduced. <001> Since this is a crystal orientation that is difficult to recrystallize, suppressing the formation of this crystal orientation can effectively promote recrystallization by reduction in the final stage. As a result, the band-shaped structure of the hot-rolled steel sheet is improved, the periodicity of the metal structure is reduced, and the E value increases. If the stress applied to the steel sheet is less than 170 kPa, it may not be possible to achieve an E value of 11.0 or more. The stress applied to the steel sheet is more preferably 190 kPa or more. The stress applied to the steel sheet can be controlled by adjusting the roll rotation speed during tandem rolling.
[0082] (7-4) Reduction rate in the final stage of hot rolling: 8% or more, hot rolling completion temperature Tf: 900°C or more, less than 960°C It is preferable that the reduction rate in the final stage of hot rolling is 8% or more, and the hot rolling completion temperature Tf is 900°C or more. By setting the reduction rate in the final stage of hot rolling to 8% or more, recrystallization due to the reduction in the final stage can be promoted. As a result, the band-shaped structure of the hot-rolled steel sheet is improved, the periodicity of the metal structure is reduced, and the E value is increased. By setting the hot-rolling completion temperature Tf to 900°C or more, an excessive increase in the number of ferrite nucleation sites in austenite can be suppressed. As a result, the generation of ferrite in the final structure (metal structure of the hot-rolled steel sheet after production) can be suppressed, and a high-strength hot-rolled steel sheet can be obtained. In addition, by setting Tf to less than 960°C, the coarsening of the austenite grain size can be suppressed, the periodicity of the metal structure can be reduced, and the E value can be made 11.0 or more.
[0083] (7-5) Stress after the final stage of hot rolling and until the steel plate is cooled to 800°C: Less than 200 kPa The stress applied to the steel sheet after the final stage of hot rolling and before the steel sheet is cooled to 800°C is preferably less than 200 kPa. By applying a stress of less than 200 kPa to the steel sheet, austenite recrystallization proceeds preferentially in the rolling direction, and an increase in the periodicity of the metal structure can be suppressed. As a result, the E value can be made 11.0 or more. The stress applied to the steel sheet is more preferably 180 MPa or less.
[0084] (7-6) After cooling to a temperature range below the hot rolling completion temperature Tf-50℃, cool to T1 (℃) at an average cooling rate of 50℃ / sec or more. After the hot rolling is completed and the steel sheet is cooled to a temperature range below the hot rolling completion temperature Tf-50°C, the formation of ferrite, bainite and pearlite can be suppressed by performing accelerated cooling to T1 (°C) or less at an average cooling rate of 50°C / s or more. This improves the strength of the hot-rolled steel sheet. The average cooling rate here refers to the value obtained by dividing the temperature drop of the steel sheet from the start of accelerated cooling (the time when the steel sheet is introduced into the cooling equipment) to T1 (°C) by the time required from the start of accelerated cooling until the steel sheet temperature reaches T1 (°C). By setting the average cooling rate to 50°C / s or more until T1 (°C) after cooling to a temperature range below the hot rolling completion temperature Tf-50°C, the ferrite transformation, bainite transformation and / or pearlite transformation inside the steel sheet can be suppressed, and TS≧980MPa can be obtained. If air cooling or the like is performed during accelerated cooling to T1 (°C) after the completion of hot rolling, an average cooling rate of 50°C / sec or more cannot be achieved, and the above-mentioned effects cannot be obtained. Although the upper limit of the average cooling rate is not particularly specified, a faster cooling rate requires larger cooling equipment and higher equipment costs. Therefore, in consideration of equipment costs, the average cooling rate of the accelerated cooling is preferably 300° C. / sec or less.
[0085] In the cooling after the completion of hot rolling, it is more preferable to cool to a temperature range of the hot rolling completion temperature Tf-50 ° C. within 1.0 second after the completion of hot rolling. That is, it is more preferable to set the cooling amount for 1 second after the completion of hot rolling to 50 ° C. or more. This is because the growth of austenite grains refined by hot rolling can be suppressed. In order to cool to a temperature range of the hot rolling completion temperature Tf-50 ° C. or less within 1.0 second after the completion of hot rolling, cooling with a large average cooling rate may be performed immediately after the completion of hot rolling, for example, by spraying cooling water on the steel sheet surface. By cooling to a temperature range of Tf-50 ° C. or less within 1.0 second after the completion of hot rolling, the crystal grain size of the surface layer can be refined, and the bending internal crack resistance of the hot-rolled steel sheet can be improved. After cooling to the temperature range of the hot rolling completion temperature Tf-50°C within 1.0 second after the completion of hot rolling, accelerated cooling may be performed to a temperature below T1 (°C) at an average cooling rate of 50°C / second or more, as described above.
[0086] (7-7) The average cooling rate from T1 (℃) to the coiling temperature is 50℃ / sec or more In order to suppress the area fractions of ferrite, bainite, and pearlite and obtain a strength of TS≧980MPa, it is preferable to set the average cooling rate from T1 (°C) to the coiling temperature to 50°C / s or more. This makes it possible to harden the matrix structure. The average cooling rate here means the value obtained by dividing the temperature drop of the steel sheet from T1 (°C) to the coiling temperature by the time required from when the steel sheet temperature reaches T1 (°C) until coiling. By setting the average cooling rate to 50°C / s or more, it is possible to suppress the area fractions of ferrite, bainite, and pearlite and ensure strength and shear workability. Therefore, the average cooling rate from T1 (°C) to the coiling temperature is set to 50°C / s or more.
[0087] (7-8) Winding temperature: 350℃ or less The coiling temperature is preferably 350°C or less. By setting the coiling temperature to 350°C or less, the driving force for transformation from austenite to bcc can be increased, and the deformation strength of austenite can be increased. Therefore, when transforming from austenite to martensite, the hard phase is uniformly distributed, and the variation can be improved. As a result, the I value can be reduced, and the linearity of the boundary between the fracture surface and the shear surface at the end surface after shear processing can be improved. That is, excellent shear processing can be obtained. In addition, the decrease in hole expandability due to the influence of residual austenite can be suppressed. Therefore, the coiling temperature is preferably 350°C or less. EXAMPLES
[0088] Next, the effect of one embodiment of the present invention will be described in more detail with reference to an example, but the conditions in the example are merely an example of conditions adopted to confirm the feasibility and effect of the present invention, and the present invention is not limited to this example of conditions. Various conditions may be adopted in the present invention as long as they do not deviate from the gist of the present invention and the object of the present invention is achieved.
[0089] Steels having the chemical compositions shown in Tables 1 and 2 were melted and continuously cast into slabs having thicknesses of 240 to 300 mm. The resulting slabs were used to obtain hot-rolled steel sheets shown in Tables 5A to 6B under the manufacturing conditions shown in Tables 3A to 4B. For Production No. 11 in Table 3A, the hot-rolled steel sheet was produced by holding the steel in a temperature range of 700 to 850°C, then further heating and holding at 1036°C for 9366 seconds.
[0090] For the obtained hot-rolled steel sheets, the area fraction of the metal structure, the E value, the I value, the standard deviation of the Mn concentration, and the average crystal grain size of the surface layer were measured by the above-mentioned methods. The obtained measurement results are shown in Tables 5A to 6B. The remaining structure was one or two of bainite and pearlite.
[0091] Method for evaluating the properties of hot-rolled steel sheets (1) Tensile strength and hole expansion ratio The tensile strength was evaluated in accordance with JIS Z 2241:2011. The test pieces were No. 5 test pieces of JIS Z 2241:2011. The tensile test pieces were taken from a quarter part from the end in the plate width direction, and the direction perpendicular to the rolling direction was the longitudinal direction. The hole expansion ratio was measured in accordance with JIS Z 2256: 2010 using a No. 5 test piece of JIS Z 2241: 2011. The hole expansion test piece was taken from a 1 / 4 portion from the end in the sheet width direction of the hot-rolled steel sheet.
[0092] When the tensile strength TS was 980 MPa or more, the specimen was judged to have excellent strength and passed the test, whereas when the tensile strength TS was less than 980 MPa, the specimen was judged to have poor strength and failed the test. When the hole expanding ratio was ≥ 55%, the specimen was judged as having excellent hole expandability and thus passed the test. On the other hand, when the hole expanding ratio was < 55%, the specimen was judged as having poor hole expandability and thus failed the test.
[0093] (2) Shear workability The shear workability of the hot-rolled steel sheet was evaluated by determining the linearity at the boundary between the fracture surface and the shear in a punching test. Five punched holes were made at the center of the sheet width with a hole diameter of 10 mm, a clearance of 15%, and a punching speed of 3 m / s. Next, the appearance of 10 end faces parallel to the rolling direction (two end faces per punched hole) of the five punched holes was photographed using an optical microscope. In the obtained observation photograph, the end faces shown in Figure 1(a) can be observed. As shown in Figures 1(a) and (b), sagging, shear surfaces, fracture surfaces, and burrs are observed on the end faces after punching. Note that Figure 1(a) is a schematic diagram of the end faces parallel to the rolling direction of the punched holes, and Figure 1(b) is a schematic diagram of the side of the punched holes. A sag is a smooth, R-shaped surface, a shear surface is a punched end surface that is separated by shear deformation, a fracture surface is a punched end surface that is separated by a crack that occurs near the cutting edge after the end of shear deformation, and a burr is a surface with a protrusion protruding from the underside of the hot-rolled steel plate.
[0094] In the observation photographs of 10 end faces obtained from 5 end faces, the linearity at the boundary between the fracture surface and the shear was measured by the method described below, and the maximum linearity was calculated. If the maximum linearity was less than 1.045, the boundary between the fracture surface and the shear surface at the end face after shear processing was high, i.e., the hot-rolled steel sheet had excellent shear workability, and was judged to be acceptable. On the other hand, if the maximum linearity was 1.045 or more, the boundary between the fracture surface and the shear surface at the end face after shear processing was low, i.e., the hot-rolled steel sheet had poor shear workability, and was judged to be unacceptable.
[0095] The linearity at the boundary between the fracture surface and the shear was obtained by the following method. As shown in Figure 1(b), the boundary points between the shear plane and the fracture plane (points A and B in Figure 1(b)) were determined for the end face. The length of the distance x connecting points A and B with a straight line was measured. Next, the length y of the curve along the boundary between the fracture plane and the shear plane was measured. The value obtained by dividing the obtained y by x was taken as the straightness at the boundary between the fracture plane and the shear plane.
[0096] (3) Resistance to internal cracking during bending The bending test pieces were cut out from the hot-rolled steel sheets at half the width of the sheets, into rectangular test pieces measuring 100 mm x 30 mm, and the resistance to internal bending cracks was evaluated by the following bending test. The resistance to internal cracking was investigated in accordance with JIS Z 2248:2014 (V-block 90° bending test) for both bending in which the bending ridgeline is parallel to the rolling direction (L direction) (L-axis bending) and bending in which the bending ridgeline is parallel to the direction perpendicular to the rolling direction (C direction) (C-axis bending), and the minimum bending radius at which cracks do not occur was determined. The average of the minimum bending radii in the L and C axes divided by the plate thickness was used as the limit bending R / t, which was used as an index value for bendability. If R / t was ≦ 3.0, it was determined that the hot-rolled steel sheet had excellent resistance to internal cracking in bending. However, to determine the presence or absence of cracks, after the V-block 90° bending test, the test piece was cut in a plane parallel to the bending direction and perpendicular to the plate surface, and the cross section was mirror-polished to a polished finish, after which cracks were observed under an optical microscope.If the length of the crack observed on the inside of the bent test piece exceeded 30 μm, it was determined that a crack was present. The measurement results obtained are shown in Tables 6A and 6B.
[0097] [Table 1]
[0098] [Table 2]
[0099] [Table 3A]
[0100] [Table 3B]
[0101] [Table 4A]
[0102] [Table 4B]
[0103] [Table 5A]
[0104] [Table 5B]
[0105] [Table 6A]
[0106] [Table 6B]
[0107] As can be seen from Tables 6A and 6B, the examples of the present invention provided hot-rolled steel sheets with excellent strength, hole expandability, and shear workability. Furthermore, the examples of the present invention, in which the average grain size of the surface layer was less than 3.0 μm, provided hot-rolled steel sheets with excellent resistance to internal bending cracking in addition to the above-mentioned properties. On the other hand, the comparative examples, whose chemical compositions and metal structures were outside the ranges specified by the present invention, were inferior in at least one of the properties (tensile strength TS, hole expandability, shear workability). [Industrial Applicability]
[0108] According to the above-mentioned aspect of the present invention, it is possible to provide a hot-rolled steel sheet having excellent strength, hole expandability and shear workability. Also, according to the above-mentioned preferred aspect of the present invention, it is possible to obtain a hot-rolled steel sheet having the above-mentioned properties and further suppressing the occurrence of internal cracks during bending, i.e., having excellent resistance to internal cracks during bending. The hot-rolled steel sheet according to the present invention is suitable as an industrial material used for automobile parts, machine structural parts, and further building parts.
Claims
1. The chemical composition, in mass%, is C: 0.040-0.250%, Si: 0.05-3.00%, Mn: 1.00-4.00%, sol. Al: 0.001 to 0.500%, P: 0.100% or less, S: 0.0300% or less, N: 0.1000% or less, O: 0.0100% or less, Ti: 0-0.300%, Nb: 0 to 0.300%, V: 0 to 0.500%, Cu: 0-2.00%, Cr: 0-2.00%, Mo: 0-1.00%, Ni: 0-2.00%, B: 0 to 0.0100%, Ca: 0-0.0200%, Mg: 0 to 0.0200%, REM: 0-0.1000%, Bi: 0 to 0.020%, One or more of Zr, Co, Zn, and W: 0 to 1.00% in total; and Sn: 0 to 0.05%; The balance is Fe and impurities, The metal structure is In area %, The total content of martensite and tempered martensite is more than 92.0% and is not more than 100.0%; The retained austenite is less than 3.0%; Ferrite is less than 5.0%; an E value indicating the periodicity of the metal structure is 11.0 or more, and an I value indicating the uniformity of the metal structure is less than 1.020; The standard deviation of the Mn concentration is 0.60 mass% or less; A hot-rolled steel sheet having a tensile strength of 980 MPa or more.
2. The hot-rolled steel sheet according to claim 1, characterized in that the average crystal grain size in the surface layer is less than 3.0 µm.
3. The chemical composition, in mass%, Ti: 0.005-0.300%, Nb: 0.005-0.100%, V: 0.005-0.500%, Cu: 0.01-2.00%, Cr: 0.01-2.00%, Mo: 0.01-1.00%, Ni: 0.02-2.00%, B: 0.0001 to 0.0100%, Ca: 0.0005-0.0200%, Mg: 0.0005-0.0200%, REM: 0.0005 to 0.1000%, and Bi: 0.0005-0.020% The hot-rolled steel sheet according to claim 1 or 2, further comprising one or more selected from the group consisting of:
Citation Information
Patent Citations
High strength automobile steel plate superior in collision safety and formability, and its manufacture
JP1999061326A
High strength steel sheet having excellent elongation and stretch-flange formability
JP2005179703A
High strength thin steel sheet having excellent elongation and hole expandability, and method for producing the same
JP2007070661A
Method for manufacturing hot rolled steel sheet
JP2012251200A
Hot rolled steel sheet
JP2015124410A