Hot-rolled steel sheet
A hot-rolled steel sheet with a controlled chemical composition and metal structure addresses the challenge of achieving high strength and stable shear workability, ensuring consistent end face accuracy and reduced bending cracks, suitable for automotive and mechanical applications.
Patent Information
- Application Number
- JP2022545467
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2020-08-27
- Filing Date
- 2021-06-15
- Publication Date
- 2024-10-09
- Estimated Expiration
- 2041-06-15
AI Technical Summary
Existing high-strength steel sheets face challenges in achieving both high strength and stable shear workability, particularly when subjected to varying clearances during shearing, with existing technologies struggling to maintain consistent end face accuracy and sag ratios.
A hot-rolled steel sheet with a specific chemical composition and controlled metal structure, including controlled Mn segregation, periodic structure morphology, and recrystallization behavior during hot rolling, combined with accelerated cooling, to achieve tensile strengths of 780 MPa or more and stable sag ratios on sheared end faces.
The solution results in a steel sheet with enhanced strength, improved shear workability, and reduced cracking during bending, making it suitable for automotive and mechanical structural applications.
Smart Images

Figure 0007564464000009 
Figure 0007564464000001 
Figure 0007564464000002
Abstract
Description
[Technical field]
[0001] The present invention relates to a hot-rolled steel sheet. Specifically, the present invention relates to a hot-rolled steel sheet that is used by being formed into various shapes by press working or the like, and in particular to a hot-rolled steel sheet that has high strength and excellent shear workability. This application claims priority based on Japanese Patent Application No. 2020-143746, filed on August 27, 2020, the contents of which are incorporated herein by reference. [Background technology]
[0002] In recent years, from the viewpoint of protecting the global environment, efforts are being made in many fields to reduce carbon dioxide emissions. Automobile manufacturers are also actively developing technologies to reduce the weight of vehicles in order to improve fuel efficiency. However, reducing the weight of vehicles is not an easy task, as emphasis is also placed on improving crashworthiness to ensure the safety of passengers.
[0003] In order to achieve both weight reduction and crashworthiness of the vehicle body, it has been considered to use high-strength steel plates to make the components thinner. For this reason, there is a strong demand for steel plates that combine high strength with excellent formability, and several technologies have been proposed to meet these demands. Automotive components are formed by press molding, and blank plates for press molding are often manufactured by shear processing, which has high productivity. Since the clearance in blank processing is not necessarily constant, it is preferable that the end surface accuracy after shear processing is stable even with various clearances. For example, it is preferable that the ratio of sagging on the sheared end surface after shear processing is stable regardless of the clearance.
[0004] Regarding shear workability, for example, Patent Document 1 states that the ferrite grain size d s and the internal ferrite grains d b Relative to s / d b A technique is disclosed for controlling the burr height after punching by controlling the value of the square root of the square root to 0.95 or less. Patent Document 2 discloses a technique for improving peeling and curling at the sheet end surface by reducing the P content. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] Japanese Patent Publication No. 10-168544 [Patent Document 2] Japanese Patent Application Publication No. 2005-298924 [Non-patent literature]
[0006] [Non-Patent Document 1] J. Webel, J. Gola, D. Britz, F. Mucklich, Materials Characterization 144 (2018) 584-596 [Non-Patent Document 2] DL Naik, HU Sajid, R. Kiran, Metals 2019, 9, 546 [Non-Patent Document 3] K. Zuiderveld, Contrast Limited Adaptive Histogram Equalization, Chapter VIII.5, Graphics Gems IV. PS Heckbert (Eds.), Cambridge, MA, Academic Press, 1994, pp. 474-485 Summary of the Invention [Problem to be solved by the invention]
[0007] However, Patent Document 1 targets IF steel, and it may be difficult to apply it to high-strength components of 780 MPa or more. Patent Document 2 achieves a strength of 780 MPa or more, but does not consider the stability of sagging at the sheared end surface after shearing.
[0008] The present invention has been made in consideration of the above problems of the conventional technology, and has an object to provide a hot-rolled steel sheet having high strength and excellent shear workability. [Means for solving the problem]
[0009] In view of the above-mentioned problems, the present inventors have conducted extensive research into the chemical composition and metal structure of hot-rolled steel sheets and the relationship between the chemical composition and metal structure and the mechanical properties, and have obtained the following findings (a) to (f) and completed the present invention. The term "excellent shear workability" means that the ratio of sagging at the sheared end surface after shearing is stable regardless of the clearance during shearing. The term "excellent strength" or "high strength" means that the tensile strength is 780 MPa or more.
[0010] (a) In order to obtain excellent tensile (maximum) strength, it is preferable to utilize a hard structure, i.e., it is preferable to include martensite or bainite in the metal structure.
[0011] (b) In order to stabilize the ratio of sagging at the sheared end surface, it is important to have a metal structure with little Mn segregation, periodic structure morphology, and non-uniformity (low uniformity).
[0012] (c) Specifically, keeping the standard deviation of the Mn concentration below a certain value and controlling the periodicity and uniformity of the metal structure are effective in stabilizing the sagging ratio at the sheared edge.
[0013] (d) In order to keep the standard deviation of Mn concentration below a certain value, the slab heating process and the subsequent hot rolling process are important. For example, it is effective to hold the slab in the temperature range of 700 to 850°C for 900 seconds or more, then further heat it and hold it in the temperature range of 1100°C or higher for 6000 seconds or more, and to perform hot rolling in the temperature range of 850°C to 1100°C so that the sheet thickness is reduced by 90% or more in total.
[0014] (e) In order to improve the periodicity of the metal structure, it is important to control the recrystallization behavior of austenite during hot rolling. For example, it is effective to control the reduction rate and rolling temperature in the final stage of hot rolling within a predetermined range, to set the stress applied to the steel sheet after the rolling one stage before the final stage of hot rolling and before the rolling in the final stage to 170 kPa or more, and to set the stress applied to the steel sheet after the final stage of hot rolling and until the steel sheet is cooled to 750°C to 200 kPa or more. Such hot rolling conditions can create fine and flat austenite grains, and in combination with the subsequent cooling conditions, the periodicity of the metal structure can be improved as a result.
[0015] (f) In order to reduce the uniformity of the metal structure, it is effective to promote the precipitation of iron carbide by cooling to a temperature range of 400°C or more and less than 600°C before coiling.
[0016] The gist of the present invention made based on the above findings is as follows. (1) A hot-rolled steel sheet according to one aspect of the present invention has a chemical composition, in mass%, C: 0.050~0.250%, Si: 0.05 to 3.00%, Mn: 1.00-4.00%, One or more of Ti, Nb and V: 0.060 to 0.500% in total, Sol.Al: 0.001-2.000%, P: 0.100% or less, S: 0.0300% or less, N: 0.1000% or less, O: 0.0100% or less, Cu: 0-2.00%, Cr: 0-2.00%, Mo: 0-1.00%, Ni: 0-2.00%, B: 0~0.0100%, Ca: 0 to 0.0200%, Mg: 0 to 0.0200%, REM: 0~0.1000%, Bi: 0 to 0.020%, One or more of Zr, Co, Zn and W: 0 to 1.00% in total, and Sn: 0 to 0.05% the balance being Fe and impurities, The metal structure is In terms of area percentage, the retained austenite is less than 3.0%, the ferrite is less than 15.0%, and the pearlite is less than 5.0%; The remaining structure is one or more of bainite, martensite, and tempered martensite, The E value indicating the periodicity of the metal structure is less than 10.7, and the I value indicating the uniformity of the metal structure is less than 1.020, The standard deviation of the Mn concentration is 0.60 mass% or less; The tensile strength is 780 MPa or more. (2) The hot-rolled steel sheet according to the above (1) may have a ratio ds / dq of the average grain size ds of the surface layer to the average grain size dq at a depth position of ¼ of the sheet thickness from the surface, that is, 0.95 or less. (3) The hot-rolled steel sheet according to the above (1) or (2), wherein the chemical composition is, in mass%, Cu: 0.01-2.00%, Cr: 0.01-2.00%, Mo: 0.01 to 1.00%, Ni: 0.02 to 2.00%, B: 0.0001~0.0100%, Ca: 0.0005~0.0200%, Mg: 0.0005~0.0200%, REM: 0.0005 to 0.1000%, and Bi: 0.0005 to 0.020% The resin may contain one or more selected from the group consisting of: Effect of the Invention
[0017] According to the above-mentioned aspect of the present invention, it is possible to obtain a hot-rolled steel sheet having excellent strength and shear workability. Also, according to the above-mentioned preferred aspect of the present invention, it is possible to obtain a hot-rolled steel sheet having the above-mentioned properties and further suppressing the occurrence of internal cracks in bending, i.e., having excellent resistance to internal cracks in bending. The hot-rolled steel sheet according to the above aspect of the present invention is suitable as an industrial material used for automobile parts, machine structural parts, and further building parts. [Brief description of the drawings]
[0018] [Figure 1] FIG. 13 is a diagram for explaining a method for measuring the ratio of sagging on a sheared end surface after shearing. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0019] The chemical composition and metal structure of the hot-rolled steel sheet according to this embodiment (hereinafter, may be simply referred to as steel sheet) will be described in more detail below. However, the present invention is not limited to the configuration disclosed in this embodiment, and various modifications are possible without departing from the spirit of the present invention. In the following, the numerical ranges described with "~" include the lower and upper limits. Numerical values indicated as "less than" or "more than" are not included in the numerical range. In the following description, percentages related to the chemical composition of the steel sheet are mass% unless otherwise specified.
[0020] 1.Chemical composition The hot-rolled steel sheet according to the present embodiment contains, by mass%, C: 0.050-0.250%, Si: 0.05-3.00%, Mn: 1.00-4.00%, one or more of Ti, Nb and V: 0.060-0.500% in total, sol.Al: 0.001-2.000%, P: 0.100% or less, S: 0.0300% or less, N: 0.1000% or less, O: 0.0100% or less, and the balance: Fe and impurities. Each element will be described in detail below.
[0021] (1-1) C: 0.050-0.250% C increases the fraction of the hard phase and increases the strength of ferrite by combining with precipitation strengthening elements such as Ti, Nb, and V. If the C content is less than 0.050%, it is difficult to obtain the desired strength. Furthermore, the stability of sagging at the sheared end surface decreases. Therefore, the C content is set to 0.050% or more. The C content is preferably 0.060% or more, more preferably 0.070% or more, and even more preferably 0.080% or more. On the other hand, if the C content exceeds 0.250%, the weldability of the hot-rolled steel sheet decreases. Therefore, the C content is set to 0.250% or less. The C content is preferably 0.150% or less.
[0022] (1-2) Si: 0.05-3.00% Silicon has the effect of increasing the strength of hot-rolled steel sheet by solid solution strengthening. Silicon also has the effect of improving the soundness of steel by deoxidization (suppressing the occurrence of defects such as blowholes in steel). If the Si content is less than 0.05%, the above effects cannot be obtained. Therefore, the Si content is set to 0.05% or more. The Si content is preferably 0.50% or more, and more preferably 0.80% or more. However, if the Si content exceeds 3.00%, the surface properties and chemical conversion treatability of the hot-rolled steel sheet, as well as its ductility and weldability, are significantly deteriorated. 3 The transformation point increases significantly. This makes it difficult to perform stable hot rolling. Furthermore, the stability of sagging at the sheared edge decreases. Therefore, the Si content is set to 3.00% or less. The Si content is preferably 2.70% or less, and more preferably 2.50% or less.
[0023] (1-3) Mn: 1.00-4.00% Mn has the effect of suppressing ferrite transformation and increasing the strength of hot-rolled steel sheets. If the Mn content is less than 1.00%, a tensile strength of 780 MPa or more cannot be obtained. Furthermore, the stability of sagging at the sheared end surface decreases. Therefore, the Mn content is set to 1.00% or more. The Mn content is preferably 1.30% or more, and more preferably 1.50% or more. On the other hand, if the Mn content exceeds 4.00%, cracks occur near the center of the sheet thickness due to the central segregation of Mn, and the sheared edge properties after shearing deteriorate. Therefore, the Mn content is set to 4.00% or less. The Mn content is preferably 3.70% or less, and more preferably 3.50% or less.
[0024] (1-4) One or more of Ti, Nb and V: 0.060 to 0.500% in total Ti, Nb and V are elements that finely precipitate in steel as carbides and nitrides, improving the strength of steel through precipitation strengthening. They also form the above-mentioned carbides to fix C, suppressing the formation of cementite, which is harmful to shear workability. If the total content of Ti, Nb and V is less than 0.060%, these effects cannot be obtained. Therefore, the total content of Ti, Nb and V is set to 0.060% or more. It is not necessary to contain all of Ti, Nb and V, and it is sufficient that any one of them is contained in an amount of 0.060% or more. When two or more of Ti, Nb and V are contained, it is sufficient that the total content thereof is 0.060% or more. The total content of Ti, Nb and V is preferably 0.080% or more, more preferably 0.100% or more. On the other hand, if the total content of Ti, Nb and V exceeds 0.500%, the workability of the hot-rolled steel sheet deteriorates. Therefore, the total content of Ti, Nb and V is set to 0.500% or less, preferably 0.300% or less, more preferably 0.250% or less, and even more preferably 0.200% or less.
[0025] (1-5) sol.Al: 0.001-2.000% Like Si, Al has the effect of deoxidizing steel and improving the soundness of the steel. If the sol. Al content is less than 0.001%, the above effect cannot be obtained. Therefore, the sol. Al content is set to 0.001% or more. The sol. Al content is preferably 0.010% or more. On the other hand, if the sol.Al content exceeds 2.000%, the above effects are saturated and it is economically undesirable, so the sol.Al content is set to 2.000% or less. The sol.Al content is preferably 1.500% or less, more preferably 1.300% or less, and even more preferably 1.000% or less. Incidentally, sol. Al means acid-soluble Al, and indicates solute Al that is present in the steel in a solid solution state.
[0026] (1-6)P:0.100% or less P is an element that is generally contained as an impurity, but it also has the effect of increasing the strength of hot-rolled steel sheets by solid solution strengthening. Therefore, P may be actively contained, but P is an element that is easily segregated, and if the P content exceeds 0.100%, the decrease in ductility due to grain boundary segregation becomes significant. Therefore, the P content is set to 0.100% or less. The P content is preferably 0.030% or less. There is no need to specify a lower limit for the P content, but it is preferably set to 0.001% from the viewpoint of refining costs.
[0027] (1-7)S: 0.0300% or less S is an element contained as an impurity, and forms sulfide-based inclusions in steel, thereby reducing the ductility of the hot-rolled steel sheet. If the S content exceeds 0.0300%, the ductility of the hot-rolled steel sheet is significantly reduced. Therefore, the S content is set to 0.0300% or less. The S content is preferably set to 0.0050% or less. There is no particular need to specify a lower limit for the S content, but from the viewpoint of refining costs, it is preferably set to 0.0001%.
[0028] (1-8)N: 0.1000% or less N is an element contained in steel as an impurity, and has the effect of reducing the ductility of the hot-rolled steel sheet. If the N content exceeds 0.1000%, the ductility of the hot-rolled steel sheet is significantly reduced. Therefore, the N content is set to 0.1000% or less. The N content is preferably 0.0800% or less, more preferably 0.0700% or less, and even more preferably 0.0100% or less. There is no need to specify a lower limit for the N content, but when one or more of Ti, Nb, and V are contained to make the metal structure finer, the N content is preferably 0.0010% or more, and more preferably 0.0020% or more in order to promote the precipitation of carbonitrides.
[0029] (1-9)O: 0.0100% or less When O is contained in a large amount in steel, it forms coarse oxides that become the starting points of fracture, causing brittle fracture and hydrogen-induced cracking. Therefore, the O content is set to 0.0100% or less. The O content is preferably 0.0080% or less, and more preferably 0.0050% or less. In order to disperse a large number of fine oxides during deoxidation of molten steel, the O content may be set to 0.0005% or more, or 0.0010% or more.
[0030] The balance of the chemical composition of the hot-rolled steel sheet according to the present embodiment may be Fe and impurities. In the present embodiment, the term "impurities" refers to substances that are mixed in from raw materials such as ore, scrap, or the manufacturing environment, and / or substances that are allowed to be used within a range that does not adversely affect the hot-rolled steel sheet according to the present embodiment.
[0031] The hot-rolled steel sheet according to the present embodiment may contain Cu, Cr, Mo, Ni, B, Ca, Mg, REM, Bi, Zr, Co, Zn, W, and Sn as optional elements instead of a part of Fe. When the optional elements are not contained, the lower limit of the content is 0%. The optional elements will be described in detail below.
[0032] (1-10) Cu: 0.01-2.00%, Cr: 0.01-2.00%, Mo: 0.01-1.00%, Ni: 0.02-2.00% and B: 0.0001-0.0100% Cu, Cr, Mo, Ni and B all have the effect of increasing the hardenability of the hot-rolled steel sheet. Cu and Mo also have the effect of precipitating as carbides in the steel to increase the strength of the hot-rolled steel sheet. Furthermore, when Cu is contained, Ni has the effect of effectively suppressing grain boundary cracking of the slab caused by Cu. Therefore, one or more of these elements may be contained.
[0033] Cu has the effect of increasing the hardenability of hot-rolled steel sheets and the effect of precipitating as carbides in steel at low temperatures to increase the strength of hot-rolled steel sheets. In order to more reliably obtain the effects of the above-mentioned actions, the Cu content is preferably 0.01% or more, and more preferably 0.05% or more. However, if the Cu content exceeds 2.00%, grain boundary cracking of the slab may occur. Therefore, the Cu content is set to 2.00% or less. The Cu content is preferably 1.50% or less, more preferably 1.00% or less.
[0034] As described above, Cr has the effect of improving the hardenability of the hot-rolled steel sheet. In order to obtain the above-mentioned effect more reliably, the Cr content is preferably 0.01% or more, and more preferably 0.05% or more. However, if the Cr content exceeds 2.00%, the chemical conversion treatability of the hot-rolled steel sheet is significantly reduced. Therefore, the Cr content is set to 2.00% or less.
[0035] As described above, Mo has the effect of increasing the hardenability of a hot-rolled steel sheet and the effect of precipitating in the steel as carbides to increase the strength of the hot-rolled steel sheet. In order to obtain the above-mentioned effects more reliably, the Mo content is preferably 0.01% or more, and more preferably 0.02% or more. However, even if the Mo content exceeds 1.00%, the above-mentioned effects are saturated and it is not economically preferable. Therefore, the Mo content is set to 1.00% or less. The Mo content is preferably 0.50% or less, and more preferably 0.20% or less.
[0036] As described above, Ni has the effect of increasing the hardenability of hot-rolled steel sheet. Furthermore, when Cu is contained, Ni has the effect of effectively suppressing grain boundary cracking of slabs caused by Cu. In order to obtain the above-mentioned effect more reliably, the Ni content is preferably 0.02% or more. Since Ni is an expensive element, it is economically undesirable to contain a large amount of Ni. Therefore, the Ni content is set to 2.00% or less.
[0037] As described above, B has the effect of improving the hardenability of the hot-rolled steel sheet. In order to obtain the effect of this effect more reliably, the B content is preferably 0.0001% or more, and more preferably 0.0002% or more. However, if the B content exceeds 0.0100%, the formability of the hot-rolled steel sheet is significantly reduced, so the B content is set to 0.0100% or less. The B content is preferably set to 0.0050% or less.
[0038] (1-11) Ca: 0.0005-0.0200%, Mg: 0.0005-0.0200%, REM: 0.0005-0.1000%, and Bi: 0.0005-0.020% Ca, Mg and REM all have the effect of adjusting the shape of inclusions in steel to a preferred shape, thereby increasing the ductility of the hot-rolled steel sheet. Bi also has the effect of refining the solidification structure, thereby increasing the ductility of the hot-rolled steel sheet. Therefore, one or more of these elements may be contained. In order to obtain the effect of the above action more reliably, it is preferable that the content of one or more of Ca, Mg, REM and Bi is 0.0005% or more. However, if the Ca content or Mg content exceeds 0.0200%, or if the REM content exceeds 0.1000%, inclusions are excessively generated in the steel, which may actually reduce the ductility of the hot-rolled steel sheet. Also, even if the Bi content exceeds 0.020%, the effect of the above action is saturated, which is not economically preferable. Therefore, the Ca content and Mg content are each set to 0.0200% or less, the REM content to 0.1000% or less, and the Bi content to 0.020% or less. The Bi content is preferably 0.010% or less. Here, REM refers to a total of 17 elements consisting of Sc, Y and lanthanides, and the content of the above REM refers to the total content of these elements. In the case of lanthanides, they are added industrially in the form of misch metals.
[0039] (1-12) One or more of Zr, Co, Zn and W: 0 to 1.00% in total, and Sn: 0 to 0.05% The inventors have confirmed that the effect of the hot-rolled steel sheet according to the present embodiment is not impaired even if the total content of Zr, Co, Zn, and W is 1.00% or less. Therefore, one or more of Zr, Co, Zn, and W may be contained in a total content of 1.00% or less. The inventors have confirmed that the effect of the hot-rolled steel sheet according to the present embodiment is not impaired even if a small amount of Sn is contained. However, since a large amount of Sn may cause defects during hot rolling, the Sn content is set to 0.05% or less.
[0040] The chemical composition of the above-mentioned hot-rolled steel sheet may be measured by a general analytical method. For example, it may be measured by using ICP-AES (Inductively Coupled Plasma-Atomic Emission Spectrometry). Sol. Al may be measured by ICP-AES using the filtrate after thermally decomposing the sample with acid. C and S may be measured by the combustion-infrared absorption method, N by the inert gas fusion-thermal conductivity method, and O by the inert gas fusion-non-dispersive infrared absorption method.
[0041] 2. Metal structure of hot-rolled steel sheets Next, the metal structure of the hot-rolled steel sheet according to this embodiment will be described. The hot-rolled steel sheet according to the present embodiment has a metal structure in which, in terms of area%, the residual austenite is less than 3.0%, the ferrite is less than 15.0%, and the pearlite is less than 5.0%, the E value indicating the periodicity of the metal structure is less than 10.7, the I value indicating the uniformity of the metal structure is less than 1.020, and the standard deviation of the Mn concentration is 0.60 mass% or less. Therefore, the hot-rolled steel sheet according to the present embodiment can obtain high strength and excellent shear workability. In this embodiment, the structure fraction, E value, I value, and standard deviation of the Mn concentration in the metal structure at a depth position of 1 / 4 of the plate thickness from the surface in the plate thickness cross section parallel to the rolling direction are specified. The reason is that the metal structure at this position shows a typical metal structure of the steel sheet.
[0042] (2-1) Area fraction of retained austenite: less than 3.0% In the present invention, if the area fraction of the retained austenite is too high, the ratio of sagging at the sheared end surface may become unstable. It is presumed that the ratio of sagging at the sheared end surface becomes unstable because the retained austenite improves the work hardening ability of the hot-rolled steel sheet by transformation induced plasticity (TRIP). If the area fraction of the retained austenite is 3.0% or more, the shear workability of the hot-rolled steel sheet deteriorates. Therefore, the area fraction of the retained austenite is less than 3.0%. The area fraction of the retained austenite is preferably less than 1.5%, more preferably less than 1.0%. Since the amount of the retained austenite is preferably as small as possible, the area fraction of the retained austenite may be 0%.
[0043] Methods for measuring the area fraction of retained austenite include X-ray diffraction, EBSP (Electron Back Scattering Diffraction Pattern) analysis, magnetic measurement, etc., and the measured value may differ depending on the measurement method. In this embodiment, the area fraction of retained austenite is measured by X-ray diffraction. In the measurement of the area fraction of retained austenite by X-ray diffraction in this embodiment, the area fraction of retained austenite is obtained by obtaining the integrated intensities of a total of six peaks, α(110), α(200), α(211), γ(111), γ(200), and γ(220), using Co-Kα radiation at a depth position of 1 / 4 of the sheet thickness of the hot-rolled steel sheet (a region from 1 / 8 of the sheet thickness from the surface to 3 / 8 of the sheet thickness from the surface), and calculating the area fraction of retained austenite using an intensity averaging method.
[0044] (2-2) Area fraction of ferrite: less than 15.0% Ferrite is a structure that is generated when fcc transforms to bcc at a relatively high temperature. Since ferrite has a high work hardening ability, if the area fraction of ferrite is too high, the ratio of sagging at the sheared end surface becomes unstable. Therefore, the area fraction of ferrite is less than 15.0%. It is preferably 12.0% or less, more preferably 10.0% or less, and even more preferably 8.0% or less. The smaller the area fraction of ferrite, the more preferable it is, and the lower limit of the area fraction of ferrite may be 3.0%, 2.0%, or 0%.
[0045] (2-3) Pearlite area fraction: less than 5.0% Pearlite is a lamellar metal structure in which cementite is precipitated in layers between ferrite. Pearlite is also a soft metal structure compared to bainite and martensite. If the area fraction of pearlite is 5.0% or more, carbon is consumed by the cementite contained in pearlite, and the strength of the remaining structures, martensite and bainite, decreases, making it impossible to obtain a tensile strength of 780 MPa or more. Therefore, the area fraction of pearlite is less than 5.0%. The area fraction of pearlite is preferably 3.0% or less. In order to improve the stretch flangeability of the hot-rolled steel sheet, it is preferable to reduce the area fraction of pearlite as much as possible, and the lower limit of the area fraction of pearlite is preferably 2.0%, more preferably 1.0%, and even more preferably 0%.
[0046] The hot-rolled steel sheet according to this embodiment contains a hard structure consisting of one or more of bainite, martensite, and tempered martensite as a remaining structure other than the retained austenite, ferrite, and pearlite.
[0047] The area fraction of the metal structure is measured by the following method. A thickness cross section parallel to the rolling direction is mirror-finished and polished for 8 minutes at room temperature using colloidal silica that does not contain an alkaline solution to remove strain introduced into the surface layer of the sample. At any position in the longitudinal direction of the sample cross section, a region 50 μm long and 1 / 4 of the plate thickness from the surface (region from 1 / 8 of the plate thickness from the surface to 3 / 8 of the plate thickness from the surface) is measured by electron backscatter diffraction at measurement intervals of 0.1 μm to obtain crystal orientation information. For the measurement, an EBSD device consisting of a thermal field emission scanning electron microscope (JEOL JSM-7001F) and an EBSD detector (TSL DVC5 detector) is used. The degree of vacuum in the EBSD device was 9.6×10 -5 The EBSD spectrometer is equipped with a 300 MHz EBSD spectrometer, ...
[0048] Next, within the remaining region (region with a Grain Average Misorientation value of over 1.0°), under the condition that the 5° grain boundary is defined as the crystal grain boundary, when the maximum value of the "Grain Average IQ" of the ferrite region is defined as Iα, the region exceeding Iα / 2 is extracted as bainite, and the region below Iα / 2 is extracted as "pearlite, martensite, and tempered martensite." The area fraction of bainite is obtained by calculating the area fraction of the extracted bainite. In addition, the area fraction of the extracted "pearlite, martensite, and tempered martensite" is calculated, and the total area fraction of martensite and tempered martensite is obtained by subtracting the area fraction of pearlite obtained by the above-mentioned EBSD analysis.
[0049] (2-4) E value: less than 10.7, I value: less than 1.020 In order to stabilize the sagging ratio at the sheared end surface after shearing, it is important to have high periodicity of the metal structure and reduce the uniformity of the metal structure. In this embodiment, the sagging ratio at the sheared end surface is stabilized by controlling the E (Entropy) value, which indicates the periodicity of the metal structure, and the I (Inverse Differential Moment Norm) value, which indicates the uniformity of the metal structure.
[0050] The E value represents the periodicity of the metal structure. When the luminance is periodically arranged due to the effect of the formation of a band-shaped structure, that is, when the periodicity of the metal structure is high, the E value decreases. In this embodiment, since it is necessary to have a metal structure with high periodicity, it is necessary to reduce the E value. If the E value is 10.7 or more, the ratio of sagging at the sheared end surface becomes more likely to fluctuate and is difficult to stabilize. It is estimated that by making the metal structure periodically arranged, the work hardening ability decreases, and the ratio of sagging at the sheared end surface becomes more likely to stabilize. Therefore, the E value is set to less than 10.7. It is preferably 10.6 or less, and more preferably 10.5 or less. The lower the E value, the more preferable it is. Although there is no particular lower limit, it may be 8.0 or more, 9.0 or more, or 10.0 or more.
[0051] The I value represents the uniformity of the metal structure, and increases as the area of the region having a certain brightness becomes larger. A low I value means that the uniformity of the metal structure is low. In this embodiment, it is necessary to make the metal structure have a low uniformity of the metal structure, so it is necessary to reduce the I value. If the I value is low and the uniformity of the metal structure is low, the work hardening ability decreases, so the ratio of sagging at the sheared end surface can be stabilized. If the I value is 1.020 or more, it is estimated that the ratio of sagging at the sheared end surface will not be stabilized. Therefore, the I value is less than 1.020. It is preferably 1.015 or less, and more preferably 1.010 or less. The lower limit of the I value is not particularly specified, but it may be 0.900 or more, 0.950 or more, or 1.000 or more.
[0052] The E and I values can be obtained by the following method. In this embodiment, the photographed region of the SEM image taken to calculate the E value and I value is a position at a 1 / 4 depth of the plate thickness from the surface of the steel plate in the plate thickness cross section parallel to the rolling direction (a region from 1 / 8 depth of the plate thickness from the surface to 3 / 8 depth of the plate thickness from the surface). A SU-6600 Schottky electron gun manufactured by Hitachi High-Technologies Corporation is used to photograph the SEM image, with a tungsten emitter and an acceleration voltage of 1.5 kV. Under the above settings, the SEM image is output at a magnification of 1000 times and a gray scale of 256 gradations.
[0053] Next, the obtained SEM image is cut into an area of 880 x 880 pixels, and the image is subjected to smoothing processing with a tile grid size of 8 x 8 and a contrast enhancement limiting factor of 2.0 as described in Non-Patent Document 3. The smoothed SEM image is rotated counterclockwise in 1 degree increments from 0 to 179 degrees, excluding 90 degrees, and an image is created for each degree, resulting in a total of 179 images. Next, for each of these 179 images, the GLCM method described in Non-Patent Document 1 is used to collect the frequency value of the luminance between adjacent pixels in the form of a matrix.
[0054] The matrix of 179 frequency values collected by the above method is expressed as p k(k=0 89, 91, 179). For each image, the generated p k is summed for all k (k=0...89, 91...179), and then a 256 x 256 matrix P is calculated in which the sum of each component is normalized to be 1. Furthermore, the E value and I value are calculated using the following formulas (1) and (2) described in Non-Patent Document 2. In the following formulas (1) and (2), the value in the i-th row and j-th column of matrix P is taken as P ij It is written as follows.
[0055]
number
[0056]
number
[0057] (2-5) Standard deviation of Mn concentration: 0.60 mass% or less The standard deviation of the Mn concentration at a depth of 1 / 4 of the sheet thickness from the surface of the hot-rolled steel sheet according to this embodiment is 0.60 mass% or less. This makes it possible to stabilize the ratio of sagging at the sheared end surface. It is presumed that this is because the work hardening ability can be reduced by uniformly dispersing the hard phase in a structure in which the metal structure is periodically arranged. The standard deviation of the Mn concentration is preferably 0.50 mass% or less, and more preferably 0.47 mass% or less. From the viewpoint of suppressing excessive burrs, the lower limit of the standard deviation of the Mn concentration is preferably as small as possible, but due to the constraints of the manufacturing process, the practical lower limit is 0.10 mass%.
[0058] After mirror polishing the thickness cross section (L cross section) parallel to the rolling direction of the hot-rolled steel sheet, the position at 1 / 4 depth of the sheet thickness from the surface of the steel sheet (the region from 1 / 8 depth of the sheet thickness from the surface to 3 / 8 depth of the sheet thickness from the surface) is measured with an electron probe microanalyzer (EPMA) to measure the standard deviation of the Mn concentration. The measurement conditions are an acceleration voltage of 15 kV and a magnification of 5000 times, and a distribution image is measured in a range of 20 μm in the rolling direction of the sample and 20 μm in the thickness direction and sheet direction of the sample. More specifically, the measurement interval is 0.1 μm, and the Mn concentration is measured at 40,000 or more points. Next, the standard deviation is calculated based on the Mn concentrations obtained from all the measurement points to obtain the standard deviation of the Mn concentration.
[0059] (2-6) The ratio of the average grain size ds of the surface layer to the average grain size dq at a depth of 1 / 4 of the plate thickness from the surface is 0.95 or less. By making the crystal grain size of the surface fine, it is possible to suppress cracks on the inside of the bend of hot-rolled steel sheets. The higher the strength of hot-rolled steel sheets, the more likely they are to crack from the inside of the bend during bending (hereinafter referred to as cracks on the inside of the bend). The mechanism of cracks on the inside of the bend is presumed to be as follows. During bending, compressive stress is generated on the inside of the bend. At first, the entire inside of the bend is uniformly deformed as the bending proceeds, but as the amount of deformation increases, the deformation cannot be borne by the uniform deformation alone, and strain is concentrated locally, causing the deformation to proceed (generation of shear deformation bands). As this shear deformation band continues to grow, cracks are generated along the shear bands from the inside surface of the bend and grow. It is presumed that the reason why cracks on the inside of the bend tend to occur with increasing strength is that the deformation proceeds non-uniformly due to the decrease in work hardening ability associated with increasing strength, causing shear deformation bands to occur early in the bending process (or under loose processing conditions).
[0060] The inventors have found that the finer the crystal grain size in the surface layer of the hot-rolled steel sheet, the more localized strain concentration is suppressed, and the less likely cracks are to occur inside bending. In order to achieve the above effect, it is preferable that ds / dq, which is the ratio of the average crystal grain size ds in the surface layer of the hot-rolled steel sheet to the average crystal grain size dq at a depth position of 1 / 4 of the sheet thickness from the surface, is 0.95 or less. ds / dq is more preferably 0.90 or less, and even more preferably 0.85 or less. There is no particular restriction on the lower limit of ds / dq, but it may be 0.50 or more. In this embodiment, the surface layer refers to a region from the surface of the heat-rolled steel sheet to a depth of 50 μm from the surface.
[0061] The crystal grain size of the surface layer is measured using EBSP-OIM (Electron Back Scatter Diffraction Pattern-Orientation Image Microscopy) method. EBSP-OIM method is performed using a device that combines a scanning electron microscope and an EBSP analysis device and OIM Analysis (registered trademark) manufactured by AMETEK. The analyzable area of EBSP-OIM method is the area that can be observed by SEM. Although it depends on the resolution of SEM, EBSP-OIM method can analyze with a minimum resolution of 20 nm.
[0062] In the thickness section of the hot-rolled steel sheet parallel to the rolling direction, analysis is performed at least five fields of view in the surface layer of the hot-rolled steel sheet (the region from the surface of the hot-rolled steel sheet to a depth of 50 μm from the surface) and at 1 / 4 depth from the surface (the region from 1 / 8 depth of the sheet thickness from the surface to 3 / 8 depth of the sheet thickness from the surface) at a magnification of 1200 times and an area of 40 μm x 30 μm, and the location where the angle difference between adjacent measurement points is 5° or more is defined as a grain boundary, and the area-average grain size is calculated. The area-average grain size obtained at each measurement position is the average grain size of the surface layer and the average grain size at 1 / 4 depth from the surface.
[0063] 3. Tensile strength properties The tensile strength characteristics (tensile strength) of the mechanical properties of the hot-rolled steel sheet are evaluated in accordance with JIS Z 2241: 2011. The test specimen is the No. 5 test specimen of JIS Z 2241: 2011, and the test direction is perpendicular to the rolling direction.
[0064] The hot-rolled steel sheet according to this embodiment has a tensile (maximum) strength of 780 MPa or more. It is preferably 980 MPa or more. If the tensile strength is less than 780 MPa, the applicable parts are limited, and the contribution to the weight reduction of the vehicle body is small. There is no need to set the upper limit in particular, but it may be set to 1780 MPa from the viewpoint of suppressing die wear.
[0065] 4. Plate thickness The thickness of the hot-rolled steel sheet according to the present embodiment is not particularly limited, but may be 1.2 to 8.0 mm. If the thickness of the hot-rolled steel sheet is less than 1.2 mm, it may be difficult to ensure the rolling completion temperature and the rolling load may become excessive, making hot rolling difficult. Therefore, the thickness of the hot-rolled steel sheet according to the present embodiment may be 1.2 mm or more. It is preferably 1.4 mm or more. On the other hand, if the thickness exceeds 8.0 mm, it may be difficult to refine the metal structure, and it may be difficult to obtain the above-mentioned metal structure. Therefore, the thickness may be 8.0 mm or less. It is preferably 6.0 mm or less.
[0066] 5.Other (5-1) Plating layer The hot-rolled steel sheet according to the present embodiment having the above-mentioned chemical composition and metal structure may be provided with a plating layer on the surface for the purpose of improving corrosion resistance, etc., to form a surface-treated steel sheet. The plating layer may be an electroplating layer or a hot-dip plating layer. Examples of the electroplating layer include electrogalvanizing and electrogalvanizing Zn-Ni alloy plating. Examples of the hot-dip plating layer include hot-dip galvanizing, alloyed hot-dip galvanizing, hot-dip aluminum plating, hot-dip Zn-Al alloy plating, hot-dip Zn-Al-Mg alloy plating, and hot-dip Zn-Al-Mg-Si alloy plating. The coating weight is not particularly limited and may be the same as in the past. In addition, it is also possible to further improve the corrosion resistance by performing an appropriate chemical conversion treatment (for example, application of a silicate-based chromium-free chemical conversion treatment liquid and drying) after plating.
[0067] 6.Manufacturing conditions A suitable method for producing the hot-rolled steel sheet according to this embodiment having the above-mentioned chemical composition and metal structure is as follows.
[0068] In order to obtain the hot-rolled steel sheet according to this embodiment, it is effective to heat the slab under predetermined conditions, then perform hot rolling, accelerate cooling to a predetermined temperature range, and then slowly cool the slab, and control the cooling history until coiling.
[0069] In a preferred method for producing a hot-rolled steel sheet according to this embodiment, the following steps (1) to (6) are performed in sequence. Note that the temperature of the slab and the temperature of the steel sheet in this embodiment refer to the surface temperature of the slab and the surface temperature of the steel sheet. Also, the stress refers to the stress applied in the rolling direction of the steel sheet. (1) The slab is held in the temperature range of 700 to 850°C for 900 seconds or more, and then further heated and held in the temperature range of 1100°C or higher for 6000 seconds or more. (2) Hot rolling is performed in the temperature range of 850 to 1100°C to reduce the plate thickness by a total of 90% or more. (3) After the rolling stage before the final stage of hot rolling and before the final stage of rolling, a stress of 170 kPa or more is applied to the steel plate. (4) The reduction rate in the final stage of hot rolling is set to 8% or more, and the hot rolling is completed so that the rolling completion temperature Tf is equal to or higher than the temperature T1 (°C) represented by the following formula (A) and lower than 900°C. (5) The stress applied to the steel plate after the final stage of hot rolling and before the steel plate is cooled to 750°C is 200 kPa or more. (6) After completion of hot rolling, accelerated cooling is performed at an average cooling rate of 50°C / sec or more to a temperature range of 600°C or less. More preferably, cooling is performed within 1 second after completion of hot rolling to a temperature range of the hot rolling completion temperature Tf-50°C or less. (7) The residence time in the temperature range of 600 to 730°C is 3.0 seconds or less. (8) Coiling is performed at a temperature range of 400°C or higher and lower than 600°C.
[0070] T1(℃)=868-396×[C]-68.1×[Mn]+24.6×[Si]-36.1×[Ni]-24.8×[Cr]-20.7×[Cu]+250×[sol.Al]…(A) In the above formula (A), the [element symbol] indicates the content (mass%) of each element in the steel. If the element is not contained, 0 is substituted.
[0071] By adopting the above-mentioned manufacturing method, it is possible to stably manufacture a hot-rolled steel sheet having a metal structure excellent in strength and shear workability. That is, by appropriately controlling the slab heating conditions and the hot rolling conditions, Mn segregation is reduced and pre-transformation austenite is flattened, and in combination with the cooling conditions after hot rolling described below, it is possible to stably manufacture a hot-rolled steel sheet having a metal structure excellent in strength and shear workability.
[0072] (1) Slab, slab temperature and holding time when subjected to hot rolling The slab to be subjected to hot rolling may be a slab obtained by continuous casting or a slab obtained by casting and blooming, and may be one that has been subjected to hot working or cold working as necessary. The slab to be subjected to hot rolling is preferably held in a temperature range of 700 to 850°C for 900 seconds or more during slab heating, and then further heated and held in a temperature range of 1100°C or higher for 6000 seconds or more. When held in a temperature range of 700 to 850°C, the steel sheet temperature may be fluctuated within this temperature range or may be constant. When held at 1100°C or higher, the steel sheet temperature may be fluctuated within a temperature range of 1100°C or higher or may be constant. In the austenite transformation in the temperature range of 700 to 850°C, Mn is distributed between ferrite and austenite, and by lengthening the transformation time, Mn can diffuse within the ferrite region. This eliminates the Mn microsegregation that is unevenly distributed in the slab and significantly reduces the standard deviation of the Mn concentration. Also, by holding the slab at a temperature of 1100°C or higher for 6000 seconds or more, the austenite grains can be made uniform during slab heating.
[0073] In the hot rolling, a reverse mill or a tandem mill is preferably used as a multi-pass rolling mill. In particular, from the viewpoint of industrial productivity and the stress load on the steel sheet during rolling, it is more preferable to use a tandem mill for at least the final two stages of hot rolling.
[0074] (2) Reduction rate of hot rolling: Total thickness reduction of 90% or more in the temperature range of 850 to 1100°C By performing hot rolling so as to reduce the sheet thickness by 90% or more in total in the temperature range of 850 to 1100°C, mainly recrystallized austenite grains are refined and the accumulation of strain energy in the unrecrystallized austenite grains is promoted. In addition, the recrystallization of austenite is promoted and the atomic diffusion of Mn is promoted, so that the standard deviation of the Mn concentration can be reduced. Therefore, it is preferable to perform hot rolling so as to reduce the sheet thickness by 90% or more in total in the temperature range of 850 to 1100°C. In addition, the thickness reduction in the temperature range of 850 to 1100°C is the thickness at the entrance of the rolling process before the first rolling in this temperature range. 0 The exit thickness after the final rolling stage in this temperature range is t 1 Then, {(t 0 -t 1 ) / t 0}×100(%).
[0075] (3) Load stress after the rolling stage before the final stage of hot rolling and before the final stage of rolling: 170 kPa or more It is preferable that the stress applied to the steel sheet after the rolling one stage before the final stage of hot rolling and before the final stage of rolling is 170 kPa or more. <001> The number of grains with the crystal orientation of {110} increases. <001> Since this is a crystal orientation that is difficult to recrystallize, promoting the formation of this crystal orientation can effectively suppress recrystallization due to the reduction in the final stage. As a result, a metal structure with a favorably controlled E value can be obtained. The stress applied to the steel sheet is more preferably 190 kPa or more. The stress applied to the steel sheet can be controlled by adjusting the roll rotation speed during tandem rolling.
[0076] (4) Reduction rate in the final stage of hot rolling: 8% or more, hot rolling completion temperature Tf: T1 (℃) or more, less than 900℃ It is preferable that the reduction rate in the final stage of hot rolling is 8% or more, and the hot rolling completion temperature Tf is T1 (°C) or more. By setting the reduction rate in the final stage of hot rolling to 8% or more, the austenite grains due to the reduction in the final stage are flattened, a band-shaped structure is formed in the hot rolled steel sheet, the periodicity of the metal structure is increased, and the E value is reduced. By setting the hot rolling completion temperature Tf to T1 (°C) or more, an excessive increase in the number of ferrite nucleation sites in austenite can be suppressed. As a result, the generation of ferrite in the final structure (metal structure of the hot rolled steel sheet after production) can be suppressed, and a high-strength hot rolled steel sheet can be obtained. In addition, by setting Tf to less than 900°C, recrystallization and coarsening of austenite can be suppressed, the periodicity of the metal structure is increased, and a metal structure with a favorably controlled E value can be obtained.
[0077] (5) Load stress after the final stage of hot rolling and until the steel plate is cooled to 750°C: 200 kPa or more The stress applied to the steel sheet after the final stage of hot rolling and until the steel sheet is cooled to 750°C is preferably 200 kPa or more. By applying a stress of 200 kPa or more to the steel sheet, flattening of austenite is promoted and the periodicity of the metal structure can be improved. As a result, a metal structure with a favorably controlled E value can be obtained.
[0078] (6) After completion of hot rolling, accelerate cooling is performed at an average cooling rate of 50°C / sec or more to a temperature range of 600°C or less, and more preferably, within 1 second after completion of hot rolling, to a temperature range of the hot rolling completion temperature Tf-50°C or less. In order to suppress the growth of austenite grains refined by hot rolling, it is more preferable to cool the steel sheet by 50°C or more within 1 second after the completion of hot rolling. In order to cool the steel sheet to a temperature range of the hot rolling completion temperature Tf-50°C or less within 1 second after the completion of hot rolling, the steel sheet is cooled at a high average cooling rate immediately after the completion of hot rolling, for example, by spraying cooling water on the steel sheet surface. By cooling the steel sheet to a temperature range of Tf-50°C or less within 1 second after the completion of hot rolling, the grain size of the surface layer can be refined and the resistance to internal bending cracks can be improved.
[0079] In addition, by performing accelerated cooling to a temperature range of 600°C or less at an average cooling rate of 50°C / sec or more after the completion of hot rolling, the formation of ferrite and pearlite, which have a small amount of precipitation strengthening, can be suppressed. This improves the strength of the hot-rolled steel sheet. The average cooling rate here refers to the temperature drop of the steel sheet from the start of accelerated cooling (when the steel sheet is introduced into the cooling equipment) to the end of accelerated cooling (when the steel sheet is removed from the cooling equipment) divided by the time required from the start of accelerated cooling to the end of accelerated cooling. Although the upper limit of the cooling rate is not particularly specified, a faster cooling rate requires a larger cooling facility, which increases the facility cost. Therefore, in consideration of the facility cost, a cooling rate of 300°C / sec or less is preferable. In addition, the cooling stop temperature of the accelerated cooling is preferably set to 400°C or more in relation to the coiling temperature.
[0080] (7) Residence time in the temperature range of 600 to 730°C: 3.0 seconds or less In order to suppress the formation of ferrite and pearlite and harden the matrix structure to obtain a tensile strength of 780 MPa or more, the residence time in the ferrite transformation temperature range of 600 to 730°C is preferably 3.0 seconds or less, and more preferably 2.0 seconds or less.
[0081] (7) Winding temperature: 400°C or higher, less than 600°C The coiling temperature is set to a temperature range of 400°C or higher and lower than 600°C. By setting the coiling temperature in this temperature range, the amount of iron carbide precipitated can be increased and the variation in hardness distribution within the hard phase can be improved. As a result, the I value can be reduced and excellent shear workability can be obtained. EXAMPLES
[0082] Next, the effect of one embodiment of the present invention will be described in more detail with reference to an example, but the conditions in the example are merely an example of conditions adopted to confirm the feasibility and effect of the present invention, and the present invention is not limited to this example of conditions. Various conditions may be adopted in the present invention as long as they do not deviate from the gist of the present invention and the object of the present invention is achieved.
[0083] Steels having the chemical compositions shown in Tables 1 and 2 were melted and continuously cast into slabs having thicknesses of 240 to 300 mm. The resulting slabs were used to obtain hot-rolled steel sheets shown in Tables 4A and 4B under the manufacturing conditions shown in Tables 3A and 3B.
[0084] The area fraction of the metal structure, the E value, the I value, the standard deviation of the Mn concentration, the ratio ds / dq of the average grain size ds in the surface layer to the average grain size dq at a depth of 1 / 4 of the sheet thickness from the surface, and the tensile strength TS were determined for the obtained hot-rolled steel sheets by the above-mentioned methods. The measurement results are shown in Tables 4A and 4B. The remaining structure was one or more of bainite, martensite, and tempered martensite.
[0085] Method for evaluating the properties of hot-rolled steel sheets (1) Tensile strength properties When the tensile strength TS was 780 MPa or more, the hot-rolled steel sheet was judged to have excellent strength and to pass the test, whereas when the tensile strength TS was less than 780 MPa, the hot-rolled steel sheet was judged to have poor strength and to fail the test.
[0086] (2) Shear workability The shear workability of the hot-rolled steel sheet was evaluated by determining the sagging ratio (sagging ratio) at the end face after punching in a punching test. Three punched holes with a hole diameter of 10 mm and a punching speed of 3 m / s and a clearance of 10% and 20% were made. Next, the state of the end face parallel to the rolling direction (two end faces per punched hole) of each punched hole was photographed with an optical microscope. In the obtained observation photograph, the end face shown in Figure 1(a) can be observed. As shown in Figures 1(a) and (b), sagging, shear surfaces, fracture surfaces, and burrs are observed at the end face after punching. Note that Figure 1(a) is a schematic diagram of the end face parallel to the rolling direction of the punched hole, and Figure 1(b) is a schematic diagram of the side of the punched hole. The sagging is a smooth surface with an R shape, the shear surface is a punched end surface separated by shear deformation, the fracture surface is a punched end surface separated by a crack generated near the cutting edge after the shear deformation is completed, and the burr is a surface having a protrusion protruding from the lower surface of the hot-rolled steel sheet. The sagging ratio at the end surface was measured using the method described below in the observation photograph of the obtained end surface. The sagging ratio at the clearance of 20% was divided by the sagging ratio at the clearance of 10% to calculate the value. If this value was 1.70 or less, the sagging ratio at the sheared end surface after shear processing was stable, that is, the hot-rolled steel sheet had excellent shear workability, and was judged to be acceptable. On the other hand, if the above value was more than 1.70, the hot-rolled steel sheet had poor shear workability, and was judged to be unacceptable.
[0087] The sagging ratio at the end face can be obtained by drawing a straight line 1 perpendicular to the top and bottom surfaces of the hot-rolled steel plate in the observation photograph of the end face, as shown in Figure 1(a), and calculating the ratio of the sagging length d1 to the sum of the sagging length d1, the shear surface length d2, the fracture surface length d3, and the burr length d4 on that straight line 1 (=d1 / (d1+d2+d3+d4)×100).
[0088] (3) Resistance to internal cracking during bending The resistance to internal cracking due to bending was evaluated by the following bending test. A rectangular test piece measuring 100 mm x 30 mm was cut out from the hot-rolled steel sheet to obtain a bending test piece. The resistance to internal cracking was investigated in accordance with JIS Z 2248:2014 (V-block 90° bending test) for both bending in which the bending ridgeline is parallel to the rolling direction (L direction) (L-axis bending) and bending in which the bending ridgeline is parallel to the direction perpendicular to the rolling direction (C direction) (C-axis bending), and the minimum bending radius at which cracks do not occur was obtained. The average value of the minimum bending radius in the L axis and C axis divided by the sheet thickness was used as the limit bending R / t, which was used as an index value for resistance to internal cracking in bending. When R / t was 2.5 or less, the hot-rolled steel sheet was judged to have excellent resistance to internal cracking in bending.
[0089] However, to determine the presence or absence of cracks, after the V-block 90° bending test, the test piece was cut in a plane parallel to the bending direction and perpendicular to the plate surface, and the cross section was mirror-polished to a polished finish, after which cracks were observed under an optical microscope.If the length of the crack observed on the inside of the bent test piece exceeded 30 μm, it was determined that a crack was present. The results obtained are shown in Tables 4A and 4B.
[0090] [Table 1]
[0091] [Table 2]
[0092] [Table 3A]
[0093] [Table 3B]
[0094] [Table 4A]
[0095] [Table 4B]
[0096] From Tables 4A and 4B, it can be seen that the hot-rolled steel sheets according to the examples of the present invention have excellent strength and shear workability. In addition, it can be seen that the hot-rolled steel sheets according to the examples of the present invention having a ds / dq ratio of 0.95 or less have excellent resistance to internal bending cracking in addition to the above-mentioned properties. On the other hand, it is found that the hot-rolled steel sheets according to the comparative examples do not have at least one of excellent strength and shear workability. [Industrial Applicability]
[0097] According to the above-mentioned aspect of the present invention, it is possible to provide a hot-rolled steel sheet having excellent strength and shear workability. Also, according to the above-mentioned preferred aspect of the present invention, it is possible to obtain a hot-rolled steel sheet having the above-mentioned properties and further suppressing the occurrence of internal cracks in bending, i.e., having excellent resistance to internal cracks in bending. The hot-rolled steel sheet according to the present invention is suitable as an industrial material used for automobile parts, machine structural parts, and further building parts.
Claims
1. The chemical composition, in mass%, is C: 0.050-0.250%, Si: 0.05-3.00%, Mn: 1.00-4.00%, One or more of Ti, Nb, and V: 0.060 to 0.500% in total, sol. Al: 0.001 to 2.000%, P: 0.100% or less, S: 0.0300% or less, N: 0.1000% or less, O: 0.0100% or less, Cu: 0-2.00%, Cr: 0-2.00%, Mo: 0-1.00%, Ni: 0-2.00%, B: 0 to 0.0100%, Ca: 0-0.0200%, Mg: 0 to 0.0200%, REM: 0-0.1000%, Bi: 0 to 0.020%, One or more of Zr, Co, Zn, and W: 0 to 1.00% in total; and Sn: 0 to 0.05%; The balance is Fe and impurities, The metal structure is In terms of area percentage, the retained austenite is less than 3.0%, the ferrite is less than 15.0%, the pearlite is less than 5.0%, and the remaining structure is one or more of bainite, martensite, and tempered martensite, an E value indicating the periodicity of the metal structure is less than 10.7, and an I value indicating the uniformity of the metal structure is less than 1.020; The standard deviation of the Mn concentration is 0.60 mass% or less; Tensile strength is 780 MPa or more A hot-rolled steel sheet characterized by:
2. The hot-rolled steel sheet according to claim 1, characterized in that the ratio ds / dq of the average grain size ds of the surface layer to the average grain size dq at a depth position of 1 / 4 of the sheet thickness from the surface is 0.95 or less.
3. The chemical composition, in mass%, Cu: 0.01-2.00%, Cr: 0.01-2.00%, Mo: 0.01-1.00%, Ni: 0.02-2.00%, B: 0.0001 to 0.0100%, Ca: 0.0005-0.0200%, Mg: 0.0005-0.0200%, REM: 0.0005 to 0.1000%, and Bi: 0.0005-0.020% Contains one or more selected from the group consisting of The hot-rolled steel sheet according to claim 1 or 2.
Citation Information
Patent Citations
Cold rolled steel sheet excellent in blanking property and its production
JP1998168544A
High strength hot rolled steel sheet having excellent stamping workability and its production method
JP2005298924A
High strength thin steel sheet having excellent elongation and hole expandability, and method for producing the same
JP2007070661A
High strength hot rolled steel sheet and manufacturing method therefor
JP2015160984A
High strength steel sheet excellent in flexure property and manufacturing method therefor
JP2017150051A