Steel
A steel material with a tailored chemical composition and microstructure addresses the challenge of achieving high yield strength and low-temperature toughness in cryogenic environments, ensuring stability for carbon dioxide storage technology.
Patent Information
- Application Number
- JP2024529962
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2023-04-13
- Filing Date
- 2024-03-15
- Publication Date
- 2024-10-09
- Estimated Expiration
- 2044-03-15
AI Technical Summary
Existing steel materials used in carbon dioxide storage technology do not possess both high yield strength and excellent low-temperature toughness in cryogenic environments, particularly below -70°C, as they are not designed to handle sudden pressure and temperature changes associated with supercritical CO2 storage.
A steel material with a specific chemical composition and microstructural control, including elements like C, Si, Mn, Cr, Mo, and controlled carbide distribution, combined with a ratio of prior austenite grain size to block diameter (DA/DB) between 2.5 and 10.0, ensuring both high yield strength and low-temperature toughness.
The steel material achieves a yield strength of 552 to 655 MPa and excellent low-temperature toughness in cryogenic environments, maintaining stability under extreme conditions.
Smart Images

Figure 0007564499000001 
Figure 0007564499000002 
Figure 0007564499000003
Abstract
Description
[Technical field]
[0001] This disclosure relates to steel products, and more particularly to CO 2 This article relates to steel materials used in storage technology. [Background technology]
[0002] Currently, carbon dioxide (CO 2 ) is a global problem. 2 Efforts to reduce CO emissions are underway. 2 Among efforts to curb carbon emissions, CCUS in particular has been attracting attention.
[0003] CCUS is an abbreviation for Carbon dioxide Capture, Utilization and Storage. 2 The three technologies include CO capture, utilization, and storage. 2 As a technology to store CO emitted from industrial facilities such as power plants and factories, 2 CO2 is captured and pumped into depleted oil wells 2 Technology for injecting and storing gas has been attracting attention.
[0004] Such CO 2 Steel materials used in storage technology are required to have a yield strength of, for example, 80 ksi or more (552 MPa or more). Steel materials having a yield strength of 80 ksi or more have been proposed in JP 2002-115028 A (Patent Document 1) and WO 2017 / 149570 (Patent Document 2).
[0005] The steel material disclosed in Patent Document 1 is a steel pipe for oil wells, characterized in that it has a yield stress YS of 552 MPa (80 ksi) or more and an L-direction absorbed energy E (J) at 0°C that satisfies the formula (E≧-0.4169×YS+480). Patent Document 1 discloses that this steel material can withstand crushing caused by strong external pressure from the outside, which is required for casings.
[0006] The steel material disclosed in Patent Document 2 is a low-alloy, high-strength seamless steel pipe for oil wells, which contains, by mass%, C: 0.23 to 0.27%, Si: 0.01 to 0.35%, Mn: 0.45 to 0.70%, P: 0.010% or less, S: 0.001% or less, O: 0.0015% or less, Al: 0.015 to 0.080%, Cu: 0.02 to 0.09%, Cr: 0.8 to 1.5%, Mo: 0.5 to 1.0%, Nb: 0.02 to 0.05%, B: 0.0015 to 0.0030%, Ti: 0.005 to 0.020%, and N: 0.005% or less, with a ratio of the Ti content to the N content (Ti / N) of 3.0 to 4.0, and the balance being Fe and unavoidable impurities. This steel material also has a ratio of the stress at 0.7% strain to the stress at 0.4% strain in the stress-strain curve (σ 0.7 / σ 0.4 ) is 1.02 or less, and the yield strength is 655 MPa or more. This steel material has high strength equal to or higher than API T95 grade, while also having a stable high K ISSC Patent Document 2 discloses that it is possible to provide a low-alloy, high-strength seamless steel pipe for oil wells which exhibits high strength values. [Prior art documents] [Patent documents]
[0007] [Patent Document 1] JP 2002-115028 A [Patent Document 2] International Publication No. 2017 / 149570 Summary of the Invention [Problem to be solved by the invention]
[0008] By the way, CO 2 In order to increase the injection efficiency, 2 Gas may be compressed and pressurized to a supercritical state. 2 If CO leaks, it will go from a supercritical state to a gaseous form. 2The temperature of the gas drops suddenly due to a sudden drop in pressure. In this case, the environmental temperature may drop far below normal, even to -70°C or below. Therefore, steel materials intended for application to such carbon dioxide storage technology are required to have not only high strength but also low-temperature toughness in a cryogenic environment of -70°C or below. However, Patent Documents 1 and 2 do not consider low-temperature toughness in a cryogenic environment of -70°C or below.
[0009] An object of the present disclosure is to provide a steel material that combines a yield strength of 80 ksi or more (552 MPa or more) with excellent low-temperature toughness in an extremely low-temperature environment of -70°C or less. [Means for solving the problem]
[0010] The steel material according to the present disclosure is In mass%, C: 0.26-0.35%, Si: 0.10 to 1.00%, Mn: 1.00-1.40%, P: 0.015% or less, S: 0.0020% or less, Cr: 0.15~0.50%, Mo: 0.05-0.25%, sol.Al: 0.001~0.070%, N: 0.0010~0.0080%, V: 0~0.60%, Nb: 0-0.03%, Ti: 0 to 0.05%, W: 0 to 0.50%, Zr: 0 to 0.0050%, Co: 0-0.50%, Ni: 0-0.30%, Cu: 0-0.50%, Sn: 0~0.100%, Ca: 0 to 0.0035%, Mg: 0 to 0.0035%, B: 0~0.0010%, Rare earth elements: 0 to 0.0050%, and The balance is composed of Fe and impurities. The yield strength is less than 552 to 655 MPa, In the steel material, 10 carbides per mm with a circle equivalent diameter of 2 μm or more 2 is as follows: When the prior austenite grain size is defined as DA and the block diameter as DB, The DA and the DB satisfy the formula (1). 2.5≦DA / DB≦10.0 (1) Here, the prior austenite grain size (unit: μm) is substituted for DA in formula (1), and the block diameter (unit: μm) is substituted for DB in formula (1). Effect of the Invention
[0011] The steel material according to the present disclosure can achieve both a yield strength of 80 ksi or more (552 MPa or more) and excellent low-temperature toughness in an extremely low-temperature environment of -70°C or less. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0012] First, the inventors of the present invention investigated the possibility of obtaining a steel material having a yield strength of 552 to less than 655 MPa, assuming application to carbon dioxide storage technology. In other words, the inventors of the present invention investigated and examined a method of obtaining a yield strength of 552 to less than 655 MPa and excellent low-temperature toughness in an extremely low-temperature environment in a steel material assumed to be applied to carbon dioxide storage technology. As a result, the inventors of the present invention obtained the following findings.
[0013] First, the inventors focused on the chemical composition and investigated to obtain a steel material having a yield strength of 552 to less than 655 MPa and excellent low-temperature toughness in an extremely low-temperature environment. As a result, the steel material had the following composition by mass: C: 0.26 to 0.35%, Si: 0.10 to 1.00%, Mn: 1.00 to 1.40%, P: 0.015% or less, S: 0.0020% or less, Cr: 0.15 to 0.50%, Mo: 0.05 to 0.25%, sol.Al: 0.001 to 0.070%, N: 0.0010 to 0.0080%, V: 0 to 0.60%, Nb: 0 to 0.03%, Ti: 0 to 0.05%, W: 0 to 0.50%, Zr: It was believed that a steel material consisting of the following composition: 0~0.0050%, Co: 0~0.50%, Ni: 0~0.30%, Cu: 0~0.50%, Sn: 0~0.100%, Ca: 0~0.0035%, Mg: 0~0.0035%, B: 0~0.0010%, rare earth elements: 0~0.0050%, and the balance: Fe and impurities, could have a yield strength of 552~655 MPa and excellent low-temperature toughness in an extremely low-temperature environment.
[0014] Next, the inventors focused on fine particles in the steel material and tried to obtain a steel material that has both a yield strength of 552 to less than 655 MPa and excellent low-temperature toughness in a cryogenic environment. The inventors focused on relatively coarse particles in particular and tried to find a method for improving low-temperature toughness in a cryogenic environment while maintaining the yield strength. As a result, the inventors obtained the following findings.
[0015] In steel having the above-mentioned chemical composition, when attempting to obtain a yield strength of less than 552 to 655 MPa, coarse carbides may be formed. As a result of detailed studies by the present inventors, it has become clear that when a large number of carbides having an equivalent circle diameter of 2 μm or more are formed in the steel, the low-temperature toughness in an extremely low temperature environment decreases. Specifically, in steel having the above-mentioned chemical composition, carbides having an equivalent circle diameter of 2 μm or more are formed at a density of 10 carbides / mm 2By reducing the diameter to below 552 to 655 MPa, it is possible to achieve both a yield strength of 552 to 655 MPa and low-temperature toughness in an extremely low-temperature environment. Hereinafter, in this specification, carbides having an equivalent circle diameter of 2 μm or more are also referred to as "coarse carbides." In addition, in this specification, the equivalent circle diameter means the diameter of a circle when the area of an observed precipitate is replaced with a circle having the same area in a visual field in a structure observation.
[0016] On the other hand, the above-mentioned chemical composition and the yield strength of less than 552 to 655 MPa, and the number density of the coarse carbides is 10 / mm 2 Even if the content of the carbide was reduced to or below 552 to 655 MPa, there were cases in which low-temperature toughness in an extremely low-temperature environment could not be obtained. Therefore, the present inventors have developed a steel sheet having the above-mentioned chemical composition and a yield strength of less than 552 to 655 MPa, and a number density of coarse carbides having a circle equivalent diameter of 2 μm or more of 10 / mm 2 Various methods for improving the low-temperature toughness in cryogenic environments were investigated for the following steel materials.
[0017] Specifically, the inventors focused on the microstructure of the steel material. To date, a method of reducing the prior austenite grain size (hereinafter, the prior austenite grain size is also referred to as the "prior γ grain size DA") in the microstructure of the steel material has been known as a method for improving the low-temperature toughness of the steel material. On the other hand, a steel material having the above-mentioned chemical composition and a yield strength of less than 552 to 655 MPa and a number density of coarse carbides of 10 / mm 2 In the following steel materials, even if the prior γ grain size DA was small, low-temperature toughness in an extremely low temperature environment was not obtained in some cases. This point will be specifically explained using a table.
[0018] [Table 1]
[0019] Table 1 is an excerpt of some of the examples described later. Test numbers 13, 14, and 49 all had the above-mentioned chemical composition and a yield strength of less than 552 to 655 MPa, and the number density of coarse carbides was 10 pieces / mm 2The following was satisfied. Comparing test numbers 13 and 14 with test number 49 with reference to Table 1, test numbers 13 and 14 have a larger prior γ grain size DA than test number 49, but test numbers 13 and 14 have a lower fracture appearance transition temperature vTrs (℃), which is an index of low temperature toughness, than test number 49. Note that, as will be described in detail later, the lower the fracture appearance transition temperature vTrs, the better the low temperature toughness of the steel material. In other words, it can be confirmed that test numbers 13 and 14, which have a larger prior γ grain size DA, exhibit better low temperature toughness in an extremely low temperature environment than test number 49, which has a smaller prior γ grain size DA.
[0020] As a result of detailed investigations by the present inventors, it has been found that the carbide has the above-mentioned chemical composition, a yield strength of 552 to less than 655 MPa, and a number density of coarse carbides of 10 / mm 2 In the following steel materials, it has been revealed that not only the prior γ grain size DA but also the size of the block, which is the sub-structure, affects the low-temperature toughness in a cryogenic environment. Here, the microstructure of the steel material having the above-mentioned chemical composition and a yield strength of less than 552 to 655 MPa and excellent low-temperature toughness is mainly composed of tempered martensite and tempered bainite. Here, in the martensite sub-structure, a lath group having approximately the same orientation is called a martensite block. Similarly, in the bainite sub-structure, a bainite lath group having approximately the same orientation is called a bainite block. In this specification, the martensite block and the bainite block are also collectively referred to as blocks. In this specification, the average grain size of the martensite block and the average grain size of the bainite block are also collectively referred to as "block diameter DB".
[0021] As described above, generally, steel materials with fine prior gamma grain size DA tend to exhibit superior low-temperature toughness. Similarly, the inventors thought that steel materials with fine block diameter DB would exhibit superior low-temperature toughness. However, referring to Table 1, contrary to the inventors' expectation, it was confirmed that test numbers 13 and 14, which have a large prior gamma grain size DA as well as a large block diameter DB, exhibit superior low-temperature toughness in an extremely low temperature environment than test number 49, which has a small prior gamma grain size DA and a small block diameter DB.
[0022] As a result of further detailed studies by the present inventors based on the above findings, it was found that a carbide having the above-mentioned chemical composition and a yield strength of less than 552 to 655 MPa and a number density of coarse carbides of 10 particles / mm 2 It has become clear that the following steel materials can obtain excellent low-temperature toughness in cryogenic environments if the prior γ grain size DA and block diameter DB satisfy the following formula (1). 2.5≦DA / DB≦10.0 (1) Here, the prior austenite grain size (unit: μm) is substituted for DA in formula (1), and the block diameter (unit: μm) is substituted for DB in formula (1).
[0023] Fn1 is defined as Fn1=DA / DB. Fn1 has the above-mentioned chemical composition and a yield strength of less than 552 to 655 MPa, and the number density of coarse carbides is 10 / mm 2 It is an index of low temperature toughness in a cryogenic environment for the following steel material. When Fn1 exceeds 10.0 in the steel material, the prior γ grain size DA is too large relative to the block diameter DB. As a result, excellent low temperature toughness in a cryogenic environment cannot be obtained. Also, if Fn1 is 2.5 or more in the steel material, low temperature toughness in a cryogenic environment can be stably obtained. Therefore, it is preferable to use a steel material having the above-mentioned chemical composition and a yield strength of less than 552 to 655 MPa, and a number density of coarse carbides of 10 / mm 2 The following steel materials have excellent low-temperature toughness even in an extremely low-temperature environment when Fn1 satisfies 2.5 to 10.0.
[0024] The carbide has the above-mentioned chemical composition and a yield strength of less than 552 to 655 MPa, and the number density of the coarse carbides is 10 / mm 2 The details of the reason why the following steel material has excellent low-temperature toughness even in an extremely low-temperature environment as a result of satisfying Fn1 of 2.5 to 10.0 are not clear. However, it is possible that the steel material has the above-mentioned chemical composition, a yield strength of less than 552 to 655 MPa, and a number density of coarse carbides of 10 / mm 2 In the steel materials below, Fn1 satisfies 2.5 to 10.0, and as a result, they have excellent low-temperature toughness even in an extremely low-temperature environment, as is proven by the examples described later.
[0025] The gist of the steel material according to this embodiment, which was completed based on the above findings, is as follows.
[0026] [1] A steel material, In mass%, C: 0.26-0.35%, Si: 0.10 to 1.00%, Mn: 1.00-1.40%, P: 0.015% or less, S: 0.0020% or less, Cr: 0.15~0.50%, Mo: 0.05-0.25%, sol.Al: 0.001~0.070%, N: 0.0010~0.0080%, V: 0~0.60%, Nb: 0-0.03%, Ti: 0 to 0.05%, W: 0 to 0.50%, Zr: 0 to 0.0050%, Co: 0-0.50%, Ni: 0-0.30%, Cu: 0-0.50%, Sn: 0~0.100%, Ca: 0 to 0.0035%, Mg: 0 to 0.0035%, B: 0~0.0010%, Rare earth elements: 0 to 0.0050%, and The balance is composed of Fe and impurities. The yield strength is less than 552 to 655 MPa, In the steel material, 10 carbides per mm with a circle equivalent diameter of 2 μm or more 2 is as follows: When the prior austenite grain size is defined as DA and the block diameter as DB, The DA and the DB satisfy formula (1); Steel material. 2.5≦DA / DB≦10.0 (1) Here, the prior austenite grain size (unit: μm) is substituted for DA in formula (1), and the block diameter (unit: μm) is substituted for DB in formula (1).
[0027] [2] The steel material according to [1], V: 0.01 to 0.60%, Nb: 0.01 to 0.03%, Ti: 0.01 to 0.05%, W: 0.01 to 0.50%, Zr: 0.0001 to 0.0050%, Co: 0.01 to 0.50%, Ni: 0.01 to 0.30%, Cu: 0.01 to 0.50%, Sn: 0.001~0.100%, Ca: 0.0001 to 0.0035%, Mg: 0.0001 to 0.0035%, B: 0.0001 to 0.0010%, and Rare earth elements: 0.0001 to 0.0050%, containing one or more elements selected from the group consisting of Steel material.
[0028] [3] The steel material according to [1] or [2], The steel material is a steel pipe. Steel material.
[0029] The shape of the steel material according to this embodiment is not particularly limited. The steel material according to this embodiment may be a steel pipe, a round bar (solid material), or a steel plate. The round bar means a steel bar having a circular cross section perpendicular to the axial direction. The steel pipe may be a seamless steel pipe or a welded steel pipe.
[0030] The steel material according to this embodiment will be described in detail below. "%" for elements means mass % unless otherwise specified.
[0031] [Chemical composition] The chemical composition of the steel material according to this embodiment contains the following elements.
[0032] C: 0.26-0.35% Carbon (C) improves the hardenability of the steel material and increases its strength. C also refines the block diameter DB of the steel material. If the C content is too low, the above effects cannot be sufficiently obtained even if the contents of other elements are within the range of this embodiment. On the other hand, if the C content is too high, the strength of the steel material becomes too high even if the contents of other elements are within the range of this embodiment, and the low-temperature toughness of the steel material decreases. Therefore, the C content is 0.26 to 0.35%. The preferred lower limit of the C content is 0.27%, more preferably 0.28%, and even more preferably 0.29%. The preferred upper limit of the C content is 0.34%, more preferably 0.33%, and even more preferably 0.32%.
[0033] Silicon: 0.10 to 1.00% Silicon (Si) deoxidizes steel. If the Si content is too low, the above effect cannot be sufficiently obtained even if the contents of other elements are within the range of this embodiment. On the other hand, if the Si content is too high, the low-temperature toughness of the steel material decreases even if the contents of other elements are within the range of this embodiment. Therefore, the Si content is 0.10 to 1.00%. The preferred lower limit of the Si content is 0.12%, more preferably 0.14%, and even more preferably 0.15%. The preferred upper limit of the Si content is 0.95%, more preferably 0.90%, and even more preferably 0.80%.
[0034] Mn: 1.00-1.40% Manganese (Mn) improves the hardenability of steel material and increases its strength. If the Mn content is too low, the above effects cannot be sufficiently obtained even if the contents of other elements are within the ranges of this embodiment. On the other hand, if the Mn content is too high, Mn segregates to the grain boundaries together with impurities such as P and S, even if the contents of other elements are within the ranges of this embodiment, and the low-temperature toughness of the steel material decreases. Therefore, the Mn content is 1.00 to 1.40%. The lower limit of the Mn content is preferably 1.02%, more preferably 1.05%. The upper limit of the Mn content is preferably 1.35%, more preferably 1.30%.
[0035] P:0.015% or less Phosphorus (P) is an impurity. That is, the lower limit of the P content is more than 0%. If the P content is too high, even if the contents of other elements are within the range of this embodiment, P segregates at the grain boundaries, and the low-temperature toughness of the steel material decreases. Therefore, the P content is 0.015% or less. A preferred upper limit of the P content is 0.014%, more preferably 0.013%. It is preferable that the P content is as low as possible. However, an extreme reduction in the P content significantly increases the manufacturing cost. Therefore, in consideration of industrial production, a preferred lower limit of the P content is 0.001%, more preferably 0.002%, and even more preferably 0.003%.
[0036] S: 0.0020% or less Sulfur (S) is an impurity. That is, the lower limit of the S content is more than 0%. If the S content is too high, even if the contents of other elements are within the range of this embodiment, S segregates at the grain boundaries, and the low-temperature toughness of the steel material decreases. Therefore, the S content is 0.0020% or less. A preferred upper limit of the S content is 0.0019%, more preferably 0.0018%, and even more preferably 0.0016%. The S content is preferably as low as possible. However, an extreme reduction in the S content significantly increases the manufacturing cost. Therefore, in consideration of industrial production, a preferred lower limit of the S content is 0.0001%, more preferably 0.0002%, and even more preferably 0.0003%.
[0037] Cr: 0.15~0.50% Chromium (Cr) improves the hardenability of steel material and increases the strength of the steel material. Cr is further concentrated in cementite in the steel material and suppresses the coarsening of cementite. As a result, the low-temperature toughness of the steel material is improved. If the Cr content is too low, the above effects cannot be sufficiently obtained even if the contents of other elements are within the range of this embodiment. On the other hand, if the Cr content is too high, the low-temperature toughness of the steel material decreases even if the contents of other elements are within the range of this embodiment. Therefore, the Cr content is 0.15 to 0.50%. The preferred lower limit of the Cr content is 0.18%, and more preferably 0.20%. The preferred upper limit of the Cr content is 0.45%, and more preferably 0.40%.
[0038] Mo: 0.05 to 0.25% Molybdenum (Mo) improves the hardenability of steel material and increases its strength. If the Mo content is too low, the above effects cannot be sufficiently obtained even if the contents of other elements are within the ranges of this embodiment. On the other hand, if the Mo content is too high, even if the contents of other elements are within the ranges of this embodiment, Mo carbides are excessively generated, and the low-temperature toughness of the steel material decreases. Therefore, the Mo content is 0.05 to 0.25%. The preferred lower limit of the Mo content is 0.06%, and more preferably 0.07%. The preferred upper limit of the Mo content is 0.24%, and more preferably 0.20%, and further preferably 0.18%.
[0039] Sol.Al: 0.001~0.070% Aluminum (Al) deoxidizes steel. If the Al content is too low, the above effect cannot be sufficiently obtained even if the contents of other elements are within the range of this embodiment. On the other hand, if the Al content is too high, coarse oxide-based inclusions are generated, and the low-temperature toughness of the steel material decreases, even if the contents of other elements are within the range of this embodiment. Therefore, the Al content is 0.001 to 0.070%. The preferred lower limit of the Al content is 0.005%, more preferably 0.010%. The preferred upper limit of the Al content is 0.065%, more preferably 0.060%. The "Al" content in this specification means the content of "acid-soluble Al", that is, "sol.Al".
[0040] N: 0.0010~0.0080% Nitrogen (N) forms nitrides and refines the prior γ grain size DA of the steel material by the pinning effect. As a result, the low-temperature toughness of the steel material is improved. If the N content is too low, the above effect cannot be sufficiently obtained even if the contents of other elements are within the range of this embodiment. On the other hand, if the N content is too high, coarse nitrides are generated even if the contents of other elements are within the range of this embodiment, and the low-temperature toughness of the steel material is reduced. Therefore, the N content is 0.0010 to 0.0080%. The preferable lower limit of the N content is 0.0015%, more preferably 0.0020%, and further preferably 0.0025%. The preferable upper limit of the N content is 0.0075%, more preferably 0.0070%.
[0041] The balance of the chemical composition of the steel material according to the present embodiment is composed of Fe and impurities. Here, the term "impurities" refers to substances that are mixed in from raw materials such as ore and scrap, or from the manufacturing environment, during industrial production of the steel material, and that are permissible within a range that does not adversely affect the steel material according to the present embodiment.
[0042] [Optional element] The chemical composition of the above-mentioned steel material may further contain one or more elements selected from the group consisting of V, Nb, Ti, W, and Zr in place of a portion of Fe. All of these elements are optional elements, and increase the temper softening resistance of the steel material and increase the strength of the steel material.
[0043] V: 0~0.60% Vanadium (V) is an optional element and may not be contained. That is, the V content may be 0%. When it is contained, V forms fine carbides during tempering, which increases the tempering softening resistance of the steel material and increases the strength of the steel material. If even a small amount of V is contained, the above effects can be obtained to a certain extent. However, if the V content is too high, the low-temperature toughness of the steel material decreases even if the contents of other elements are within the range of this embodiment. Therefore, the V content is 0 to 0.60%. The preferred lower limit of the V content is more than 0%, more preferably 0.01%, further preferably 0.02%, further preferably 0.04%, and further preferably 0.06%. The preferred upper limit of the V content is 0.40%, more preferably 0.30%, and further preferably 0.20%.
[0044] Nb: 0 to 0.03% Niobium (Nb) is an optional element and may not be contained. That is, the Nb content may be 0%. When Nb is contained, Nb forms fine carbides during tempering to increase the temper softening resistance of the steel material and increase the strength of the steel material. If even a small amount of Nb is contained, the above effects can be obtained to some extent. However, if the Nb content is too high, even if the contents of other elements are within the range of this embodiment, carbonitrides and the like are excessively generated, and the low-temperature toughness and SSC resistance of the steel material are reduced. Therefore, the Nb content is 0 to 0.03%. The preferable lower limit of the Nb content is more than 0%, more preferably 0.01%, and further preferably 0.02%. The preferable upper limit of the Nb content is less than 0.03%.
[0045] Ti: 0 to 0.05% Titanium (Ti) is an optional element and may not be contained. That is, the Ti content may be 0%. When contained, Ti forms fine carbides to increase the temper softening resistance of the steel material and increase the strength of the steel material. If even a small amount of Ti is contained, the above effects can be obtained to a certain extent. However, if the Ti content is too high, even if the contents of other elements are within the range of this embodiment, coarse nitrides are generated and the low-temperature toughness of the steel material decreases. Therefore, the Ti content is 0 to 0.05%. The preferred lower limit of the Ti content is more than 0%, more preferably 0.01%, and further preferably 0.02%. The preferred upper limit of the Ti content is less than 0.05%, and more preferably 0.04%.
[0046] W: 0~0.50% Tungsten (W) is an optional element and may not be contained. That is, the W content may be 0%. When W is contained, W forms fine carbides during tempering to increase the tempering softening resistance of the steel material and increase the strength of the steel material. If even a small amount of W is contained, the above effects can be obtained to a certain extent. However, if the W content is too high, even if the contents of other elements are within the range of this embodiment, coarse carbides are formed and the low-temperature toughness of the steel material decreases. Therefore, the W content is 0 to 0.50%. The preferred lower limit of the W content is more than 0%, more preferably 0.01%, and even more preferably 0.02%. The preferred upper limit of the W content is 0.45%, and more preferably 0.40%.
[0047] Zr: 0 to 0.0050% Zirconium (Zr) is an optional element and may not be contained. That is, the Zr content may be 0%. When contained, Zr forms fine carbides during tempering to increase the tempering softening resistance of the steel material and increase the strength of the steel material. If even a small amount of Zr is contained, the above effects can be obtained to a certain extent. However, if the Zr content is too high, even if the contents of other elements are within the range of this embodiment, coarse oxides are generated and the low-temperature toughness of the steel material decreases. Therefore, the Zr content is 0 to 0.0050%. The preferred lower limit of the Zr content is more than 0%, more preferably 0.0001%, even more preferably 0.0003%, even more preferably 0.0006%, and even more preferably 0.0010%. The preferred upper limit of the Zr content is 0.0045%, more preferably 0.0040%, and even more preferably 0.0035%.
[0048] The chemical composition of the steel material described above may further contain one or more elements selected from the group consisting of Co and Ni in place of a portion of Fe. All of these elements are optional elements, and improve the hardenability and strength of the steel material.
[0049] Co: 0 to 0.50% Cobalt (Co) is an optional element and may not be contained. That is, the Co content may be 0%. When contained, Co enhances the hardenability of the steel material and enhances the strength of the steel material. If even a small amount of Co is contained, the above effect can be obtained to some extent. However, if the Co content is too high, even if the contents of other elements are within the range of this embodiment, the hardenability of the steel material is rather reduced, and the strength of the steel material is reduced. Therefore, the Co content is 0 to 0.50%. The preferred lower limit of the Co content is more than 0%, more preferably 0.01%, further preferably 0.02%, further preferably 0.03%, and further preferably 0.05%. The preferred upper limit of the Co content is 0.45%, more preferably 0.40%.
[0050] Ni: 0 to 0.30% Nickel (Ni) is an optional element and may not be contained. That is, the Ni content may be 0%. When contained, Ni enhances the hardenability of the steel material and enhances the strength of the steel material. Even if even a small amount of Ni is contained, these effects can be obtained to a certain extent. However, if the Ni content is too high, even if the contents of other elements are within the range of this embodiment, local corrosion is promoted and the corrosion resistance of the steel material is reduced. Therefore, the Ni content is 0 to 0.30%. The preferred lower limit of the Ni content is more than 0%, more preferably 0.01%, and further preferably 0.02%. The preferred upper limit of the Ni content is 0.28%, and more preferably 0.25%.
[0051] The chemical composition of the steel material described above may further contain one or more elements selected from the group consisting of Cu and Sn in place of a portion of Fe. All of these elements are optional elements and increase the strength of the steel material.
[0052] Cu: 0-0.50% Copper (Cu) is an optional element and may not be contained. That is, the Cu content may be 0%. When contained, Cu increases the strength of the steel material. If even a small amount of Cu is contained, the above effect can be obtained to some extent. However, if the Cu content is too high, even if the contents of other elements are within the range of this embodiment, the strength of the steel material becomes too high, and the low-temperature toughness of the steel material decreases. Therefore, the Cu content is 0 to 0.50%. The preferred lower limit of the Cu content is more than 0%, more preferably 0.01%, further preferably 0.02%, and further preferably 0.05%. The preferred upper limit of the Cu content is 0.45%, more preferably 0.35%, and further preferably 0.25%.
[0053] Sn: 0 to 0.100% Tin (Sn) is an optional element and may not be contained. That is, the Sn content may be 0%. When contained, Sn increases the strength of the steel material. If even a small amount of Sn is contained, the above effect can be obtained to a certain extent. However, if the Sn content is too high, the hot workability of the steel material decreases even if the contents of other elements are within the range of this embodiment. Therefore, the Sn content is 0 to 0.100%. The preferred lower limit of the Sn content is more than 0%, more preferably 0.001%, further preferably 0.002%, and further preferably 0.003%. The preferred upper limit of the Sn content is 0.095%, more preferably 0.090%, further preferably 0.080%, and further preferably 0.070%.
[0054] The chemical composition of the above-mentioned steel material may further contain, instead of a part of Fe, one or more elements selected from the group consisting of Ca, Mg, B, and rare earth elements. All of these elements are optional elements, and improve the hot workability of the steel material.
[0055] Ca: 0 to 0.0035% Calcium (Ca) is an optional element and may not be contained. That is, the Ca content may be 0%. When contained, Ca renders S in the steel harmless as sulfides and improves the hot workability of the steel. If even a small amount of Ca is contained, the above effect can be obtained to some extent. However, if the Ca content is too high, even if the contents of other elements are within the range of this embodiment, coarse oxides are generated and the low-temperature toughness of the steel decreases. Therefore, the Ca content is 0 to 0.0035%. The preferred lower limit of the Ca content is more than 0%, more preferably 0.0001%, even more preferably 0.0003%, even more preferably 0.0006%, and even more preferably 0.0010%. The preferred upper limit of the Ca content is 0.0033%, and more preferably 0.0030%.
[0056] Magnesium: 0 to 0.0035% Magnesium (Mg) is an optional element and may not be contained. That is, the Mg content may be 0%. When contained, Mg renders S in the steel harmless as sulfide, and improves the hot workability of the steel. If even a small amount of Mg is contained, the above effect can be obtained to some extent. However, if the Mg content is too high, even if the contents of other elements are within the range of this embodiment, coarse oxides are generated, and the low-temperature toughness of the steel decreases. Therefore, the Mg content is 0 to 0.0035%. The preferable lower limit of the Mg content is more than 0%, more preferably 0.0001%, further preferably 0.0003%, further preferably 0.0006%, and further preferably 0.0010%. The preferable upper limit of the Mg content is 0.0033%, more preferably 0.0030%.
[0057] B: 0~0.0010% Boron (B) is an optional element and may not be contained. That is, the B content may be 0%. When contained, B suppresses segregation of S in the steel material to the grain boundaries, and improves the hot workability of the steel material. If even a small amount of B is contained, the above effect can be obtained to a certain degree. However, if the B content is too high, even if the contents of other elements are within the range of this embodiment, coarse nitrides are generated, and the low-temperature toughness of the steel material decreases. Therefore, the B content is 0 to 0.0010%. The preferred lower limit of the B content is more than 0%, more preferably 0.0001%, and further preferably 0.0002%. The preferred upper limit of the B content is 0.0009%, and more preferably 0.0008%.
[0058] Rare earth elements (REM): 0~0.0050% Rare earth elements (REM) are optional elements and may not be contained. That is, the REM content may be 0%. When contained, REM renders S in the steel harmless as sulfides and improves the hot workability of the steel. Even if even a small amount of REM is contained, the above effect can be obtained to some extent. However, if the REM content is too high, even if the contents of other elements are within the range of this embodiment, coarse oxides are formed and the low-temperature toughness of the steel decreases. Therefore, the REM content is 0 to 0.0050%. The preferred lower limit of the REM content is more than 0%, more preferably 0.0001%, even more preferably 0.0003%, and even more preferably 0.0006%. The preferred upper limit of the REM content is 0.0045%, more preferably 0.0040%.
[0059] In this specification, REM refers to one or more elements selected from the group consisting of scandium (Sc) with atomic number 21, yttrium (Y) with atomic number 39, and the lanthanides lanthanum (La) with atomic number 57 to lutetium (Lu) with atomic number 71. In addition, in this specification, the REM content refers to the total content of these elements.
[0060] [Yield strength] The yield strength of the steel material according to this embodiment is 552 to less than 655 MPa (80 to less than 95 ksi). The yield strength in this specification means the 0.2% offset yield strength (MPa) obtained by a tensile test at room temperature (24±3°C) in accordance with ASTM E8 / E8M(2021).
[0061] In this embodiment, the yield strength of the steel material can be determined by the following method. Specifically, a tensile test is performed by a method conforming to ASTM E8 / E8M (2021). A round bar test piece is prepared from the steel material according to this embodiment. When the steel material is a steel plate, the round bar test piece is prepared from the center of the plate thickness. In this case, the axial direction of the round bar test piece is parallel to the rolling direction of the steel plate. When the steel material is a steel pipe, the round bar test piece is prepared from the center of the wall thickness. In this case, the axial direction of the round bar test piece is parallel to the axial direction of the steel pipe. When the steel material is a round steel, the round bar test piece is prepared from the R / 2 position. In this case, the axial direction of the round bar test piece is parallel to the axial direction of the round steel. In this specification, the R / 2 position means the center position of the radius R in a cross section perpendicular to the axial direction of the round steel. The size of the round bar test piece is, for example, a parallel part diameter of 6 mm and a gauge length of 30 mm. A tensile test is performed using a round bar test piece at room temperature (24±3°C) in the air, and the obtained 0.2% offset proof stress (MPa) is defined as the yield strength (MPa). In this embodiment, the yield strength (MPa) is a value obtained by rounding off the obtained numerical value to the first decimal place.
[0062] [Number density of coarse carbides] The steel material according to the present embodiment has the above-mentioned chemical composition and a yield strength of less than 552 to 655 MPa, and further has a number density of coarse carbides (carbides having a circle equivalent diameter of 2 μm or more) of 10 particles / mm 2 As a result, the steel material according to this embodiment has excellent low-temperature toughness in a cryogenic environment, provided that the other configurations of this embodiment are satisfied. As described above, the circle equivalent diameter in this specification means the diameter of a circle when the area of an observed precipitate in a visual field in a structure observation is replaced with a circle having the same area.
[0063] In steel materials having the above-mentioned chemical composition, coarse carbides are easily formed. In particular, if the carbides remain without being dissolved in the quenching process described below, the remaining carbides tend to become coarse in the subsequent tempering process, and become coarse carbides. On the other hand, if the number of coarse carbides is less than 10 / mm 2If the precipitation exceeds 10 / mm, there is a concern that the low-temperature toughness of the steel material may be reduced. In particular, the effect is significant in an extremely low-temperature environment such as -70°C or lower. Therefore, the steel material according to this embodiment has the above-mentioned chemical composition and a yield strength of less than 552 to 655 MPa, and further has a number density of coarse carbides of 10 / mm 2 The following applies.
[0064] In this embodiment, the preferred upper limit of the number density of the coarse carbides is 9 pieces / mm 2 and more preferably 8 pieces / mm 2 and more preferably 7 pieces / mm 2 and more preferably 6 pieces / mm 2 and more preferably 5 pieces / mm 2 The lower limit of the number density of the coarse carbides is not particularly limited, and is 0 particles / mm 2 may be 1 piece / mm 2 may be also possible.
[0065] In this embodiment, the number density of coarse carbides in a steel material can be found by the following method. First, a test piece is prepared from the steel material according to this embodiment. Specifically, when the steel material is a steel plate, a test piece is prepared from the center of the plate thickness, with a surface including the rolling direction and the plate thickness direction as the observation surface. When the steel material is a steel pipe, a test piece is prepared from the center of the plate thickness, with a surface including the pipe axial direction and the pipe radial direction as the observation surface. When the steel material is a round bar, a test piece is prepared that includes the R / 2 position in the center, with a surface including the axial direction and the radial direction as the observation surface.
[0066] The observation surface of the prepared test piece is polished to a mirror finish before measurement. The area of the observation surface is not limited, but for example, 300 mm 2(20mm x 15mm). The number of carbides with a circle equivalent diameter of 2μm or more is obtained on the observation surface. Specifically, first, the particles on the observation surface are identified from the contrast. For each identified particle, element concentration analysis (EDS analysis) is performed by energy dispersive X-ray spectrometry (EDS). In the EDS analysis, the acceleration voltage is 20kV, and the target elements are quantified as C, N, O, Mg, Al, Si, P, S, Ca, Ti, Cr, Mn, Fe, Cu, Zr, and Nb. Based on the EDS analysis results of each particle, if C is detected and the Fe content is 50 mass% or more, the particle is identified as a "carbide". Here, in this specification, "C is detected" means that a characteristic X-ray peak identified as C is confirmed. Note that a person skilled in the art can naturally confirm a characteristic X-ray peak identified as C.
[0067] Among the carbides identified on the observation surface, carbides with a circle equivalent diameter of 2 μm or more (coarse carbides) are identified, and the total number of coarse carbides is calculated. The circle equivalent diameter of the carbides can be calculated by a well-known method, for example, by image analysis. Based on the total number of coarse carbides and the total area of the observation surface, the number density of the coarse carbides (pieces / mm 2 In this embodiment, the number density of coarse carbides (pieces / mm 2 ) is obtained by rounding off the obtained value to the first decimal place. The number density of the coarse carbides can be measured using a scanning electron microscope (SEM: Scanning Electron Microscope) equipped with a composition analysis function (SEM-EDS device). For example, an automatic analyzer manufactured by FEI (ASPEX) under the product name Metals Quality Analyzer can be used as the SEM-EDS device.
[0068] [Fn1(=DA / DB)] The steel material according to the present embodiment has the above-mentioned chemical composition, a yield strength of 552 to less than 655 MPa, and a number density of coarse carbides of 10 / mm 2Further, the prior austenite grain size DA and the block diameter DB satisfy the following formula (1): As a result, the steel material according to this embodiment can achieve both a yield strength of 552 to less than 655 MPa and excellent low-temperature toughness in an extremely low-temperature environment. 2.5≦DA / DB≦10.0 (1) Here, the prior austenite grain size (unit: μm) is substituted for DA in formula (1), and the block diameter (unit: μm) is substituted for DB in formula (1).
[0069] As described above, in this specification, the prior austenite grain size in the microstructure of the steel material is also referred to as the "prior γ grain size DA". Furthermore, in this specification, the average grain size of the martensite block and the average grain size of the bainite block are also collectively referred to as the "block diameter DB". As described above, the microstructure of the steel material according to this embodiment is mainly composed of tempered martensite and tempered bainite. Therefore, in this specification, the martensite block and the bainite block are also collectively referred to as the block.
[0070] Fn1 (=DA / DB) has the above-mentioned chemical composition and a yield strength of less than 552 to 655 MPa, and the number density of coarse carbides is 10 / mm 2 Fn1 is an index of low-temperature toughness in a cryogenic environment for the following steel material. If Fn1 exceeds 10.0, excellent low-temperature toughness in a cryogenic environment cannot be obtained. On the other hand, if the steel material has the above-mentioned chemical composition and a yield strength of less than 552 to 655 MPa, and the number density of coarse carbides is 10 / mm 2 In the steel material described below, if Fn1 is 2.5 or more, low-temperature toughness in an extremely low-temperature environment can be stably obtained. Therefore, the steel material according to this embodiment has the above-mentioned chemical composition and a yield strength of less than 552 to 655 MPa, and the number density of coarse carbides is 10 / mm 2 The following conditions must be met, and Fn1 must be between 2.5 and 10.0.
[0071] As described above, in a steel material having the above-mentioned chemical composition, if carbides remain without being solid-dissolved in the quenching process described later, the remaining carbides tend to coarsen in the subsequent tempering process to become coarse carbides. On the other hand, if the carbides are to be fully solid-dissolved in the quenching process, the prior γ grain size DA and / or the block diameter DB tend to become large. In this case, if either the prior γ grain size DA or the block diameter DB becomes too large, Fn1 becomes less than 2.5 or exceeds 10.0. As a result, excellent low-temperature toughness in an extremely low-temperature environment cannot be stably obtained. On the other hand, if the carbides are solid-dissolved in the quenching process described later and the number density of the coarse carbides becomes less than 10 / mm 2 If Fn1 satisfies the range of 2.5 to 10.0 after being reduced to the above value, excellent low-temperature toughness can be stably obtained even in an extremely low-temperature environment.
[0072] In the steel material according to the present embodiment, the prior γ grain size DA and block size DB are not particularly limited as long as Fn1 satisfies 2.5 to 10.0. However, as long as the steel material has the above-mentioned chemical composition and a yield strength of less than 552 to 655 MPa and the number density of coarse carbides is less than 10 pieces / mm 2 In the following steel materials, the prior γ grain size DA is, for example, 10.0 to 200.0 μm. In this embodiment, the preferred upper limit of the prior γ grain size DA is 180.0 μm, more preferably 160.0 μm, and even more preferably 150.0 μm. In the steel material according to this embodiment, even if the prior γ grain size DA is, for example, 15.0 μm or more, 20.0 μm or more, 30.0 μm or more, 40.0 μm or more, or even if it is coarse to 50.0 μm or more, the steel material according to this embodiment can achieve both a yield strength of 552 to less than 655 MPa and excellent low-temperature toughness in an extremely low-temperature environment by satisfying Fn1 of 2.5 to 10.0.
[0073] The above-mentioned chemical composition and yield strength of less than 552 to 655 MPa, and the number density of coarse carbides is 10 / mm 2In the steel material described below, the block diameter DB is, for example, 2.0 to 30.0 μm. In this embodiment, the upper limit of the block diameter DB is preferably 25.0 μm, more preferably 20.0 μm, and even more preferably 15.0 μm. In the steel material according to this embodiment, even if the block diameter DB is, for example, 5.0 μm or more, 7.0 μm or more, 8.0 μm or more, 10.0 μm or more, or even if it is coarse to 11.0 μm or more, by satisfying Fn1 of 2.5 to 10.0, it is possible to achieve both a yield strength of 552 to less than 655 MPa and excellent low-temperature toughness in an extremely low-temperature environment.
[0074] In this embodiment, the preferred lower limit of Fn1 is 3.0, more preferably 3.5, and even more preferably 4.0. In this embodiment, the preferred upper limit of Fn1 is 9.8, more preferably 9.5, and even more preferably 9.0.
[0075] In this embodiment, Fn1 can be obtained by the following method. First, the prior γ grain size DA of the steel material according to this embodiment is obtained. Specifically, a test piece for measuring the prior γ grain size DA is prepared from the steel material according to this embodiment. When the steel material is a steel plate, a test piece is prepared from the center of the plate thickness, with a surface including the rolling direction and the plate thickness direction as the observation surface. When the steel material is a steel pipe, a test piece is prepared from the center of the plate thickness, with a surface including the pipe axial direction and the pipe radial direction as the observation surface. When the steel material is a round bar, a test piece is prepared that includes the R / 2 position in the center and has a surface including the axial direction and the radial direction as the observation surface.
[0076] The test piece is embedded in resin, and the observation surface is polished to a mirror finish. It is then immersed for about 60 seconds in a solution of saturated aqueous picric acid mixed with an appropriate amount of surfactant, and the prior γ grain boundaries are revealed by etching. The area of the observation surface is not limited, but for example, 100 mm 2(10 mm x 10 mm). The grain size number G is obtained based on a cutting method in accordance with JIS G 0551 (2020) by optical microscope observation. The obtained grain size number G is converted to an average grain size M (μm) based on the following formulas (2) and (3). In this embodiment, the average grain size M obtained by the above method is defined as the prior γ grain size DA (μm). In other words, in this embodiment, the prior austenite grain size DA (μm) means the average grain size of the prior austenite grains obtained based on the cutting method in accordance with JIS G 0551 (2020). n=2 G+3 (2) M=1000 / n 1 / 2 (3)
[0077] Next, the block diameter DB of the steel material according to this embodiment is determined. Specifically, a test piece for measuring the block diameter DB is prepared from the steel material according to this embodiment. When the steel material is a steel plate, a test piece having an observation surface of 25 μm×25 μm is prepared from the center of the plate thickness. When the steel material is a steel pipe, a test piece having an observation surface of 25 μm×25 μm is prepared from the center of the wall thickness. When the steel material is a round bar, a test piece having an observation surface of 25 μm×25 μm that includes the R / 2 position in the center is prepared.
[0078] Measurements are performed on the observation surface of the test piece using electron backscatter diffraction (EBSD). EBSD measurements are performed at an acceleration voltage of 20 kV, with a field of view of 25 μm x 25 μm and a pitch of 0.1 μm. The orientation of the body-centered cubic structure (iron) is identified from the Kikuchi line pattern obtained by the EBSD measurement. A crystal orientation diagram is obtained from the orientation of the body-centered cubic structure (iron). From the crystal orientation diagram, areas surrounded by an orientation difference of 15° or more with adjacent crystals are identified, and a crystal orientation map is obtained. An area surrounded by an orientation difference of 15° or more is defined as one block.
[0079] For the defined blocks, the average grain size DB (μm) is calculated from the area of each block. Specifically, the total number of blocks in the crystal orientation map is k, and the area of each block is SBi (i is a natural number equal to or less than k) (μm 2), and the area of the crystal orientation map is ST (μm 2 In this case, the average grain size DB (μm) of the blocks is defined by the following formula (4).
number
[0080] Fn1 (=DA / DB) is calculated from the obtained prior gamma grain diameter DA (μm) and block diameter DB (μm). In this embodiment, the prior gamma grain diameter DA (μm) is a value obtained by rounding off the first decimal place of the obtained numerical value. In this embodiment, the block diameter DB (μm) is a value obtained by rounding off the first decimal place of the obtained numerical value. In this embodiment, Fn1 is a value obtained by rounding off the first decimal place of the obtained numerical value.
[0081] [Low temperature toughness] The steel material according to the present embodiment has the above-mentioned chemical composition and has a number density of coarse carbides of 10 / mm 2 or less, and Fn1 is 2.5 to 10.0. As a result, the steel material according to this embodiment has a yield strength of 552 to less than 655 MPa and excellent low-temperature toughness in a cryogenic environment. In this embodiment, excellent low-temperature toughness in a cryogenic environment is defined as follows.
[0082] A Charpy impact test in accordance with ASTM E23 (2018) is carried out on the steel material according to this embodiment. First, a V-notch test piece is prepared from the steel material according to this embodiment in accordance with ASTM E23 (2018). Specifically, when the steel material is a steel plate, a V-notch test piece is prepared from the center of the plate thickness, having a notch surface perpendicular to the plate thickness direction and a longitudinal direction parallel to the plate width direction. When the steel material is a steel pipe, a V-notch test piece is prepared from the center of the plate thickness, having a notch surface perpendicular to the pipe axial direction and a longitudinal direction perpendicular to the pipe axial direction and the pipe radial direction. When the steel material is a round steel, a V-notch test piece is prepared from the R / 2 position in a cross section perpendicular to the axial direction, having a notch surface perpendicular to the axial direction and a longitudinal direction perpendicular to the axial direction and the cross-sectional radial direction.
[0083] The prepared V-notch test specimen is subjected to a Charpy impact test in accordance with ASTM E23 (2018). Specifically, the test temperature is set to eight levels (-120°C, -100°C, -80°C, -60°C, -40°C, -20°C, 0°C, and 20°C) in which the test temperature is changed by 20°C in the range of -120 to 20°C. The Charpy impact test is performed using two test specimens for each test temperature. Under the above conditions, the brittle fracture rate (%) of the test specimen after the test at each temperature is obtained. The test temperature (°C) and the obtained brittle fracture rate (%) are plotted to obtain an approximation curve. From the obtained approximation curve, the temperature (°C) at which the brittle fracture rate becomes 50% is obtained and defined as the fracture transition temperature vTrs (°C). In this embodiment, when the fracture transition temperature vTrs is -70°C or less, it is determined that the specimen has excellent low-temperature toughness in an extremely low-temperature environment.
[0084] [Microstructure] As described above, the microstructure of the steel material according to this embodiment is mainly composed of tempered martensite and tempered bainite. Specifically, the microstructure of the steel material according to this embodiment has a total volume ratio of tempered martensite and tempered bainite of 90% or more. The remainder of the microstructure is, for example, ferrite or pearlite. The above-mentioned chemical composition, a yield strength of less than 552 to 655 MPa, and a number of pieces / mm 2In the case of a steel material satisfying the following number density of coarse carbides and Fn1 of 2.5 to 10.0, when the steel material has a microstructure in which the total volume fraction of tempered martensite and tempered bainite is 90% or more, the steel material has excellent low-temperature toughness in an extremely low-temperature environment. Therefore, in this embodiment, the steel material has the above-mentioned chemical composition, a yield strength of less than 552 to 655 MPa, and a coarse carbide density of 10 carbides / mm 2 If a steel material that satisfies the number density of coarse carbides below and Fn1 of 2.5 to 10.0 has excellent low-temperature toughness in an extremely low temperature environment, the microstructure of the steel material is determined to have a total volume fraction of tempered martensite and tempered bainite of 90% or more.
[0085] When the volume fractions of tempered martensite and tempered bainite are determined by observation, they can be determined by the following method. First, a test piece having a specific observation surface is prepared from the steel material according to this embodiment. When the steel material is a steel plate, a test piece is prepared from the center of the plate thickness, with a surface including the rolling direction and the plate thickness direction as the observation surface. When the steel material is a steel pipe, a test piece is prepared from the center of the plate thickness, with a surface including the pipe axial direction and the pipe radial direction as the observation surface. When the steel material is a round bar, a test piece is prepared that includes the R / 2 position in the center, with a surface including the axial direction and the radial direction as the observation surface.
[0086] After polishing the observation surface of the test piece to a mirror finish, it is immersed in a nital etching solution for about 10 seconds to reveal the structure by etching. The etched observation surface is observed in 10 fields of view using a SEM with secondary electron images. The field area is, for example, 0.01 mm 2 (magnification 1000x). In each field of view, tempered martensite and tempered bainite are identified from the contrast. The area ratios of the identified tempered martensite and tempered bainite are determined. The method for determining the area ratios is not particularly limited, and any known method may be used. For example, the area ratios of tempered martensite and tempered bainite can be determined by image analysis. In this embodiment, the arithmetic average value of the area ratios of tempered martensite and tempered bainite determined in all fields of view is defined as the volume ratios of tempered martensite and tempered bainite.
[0087] [Manufacturing method] A method for manufacturing a steel material according to this embodiment will be described below. A method for manufacturing a seamless steel pipe will be described below as an example of the steel material according to this embodiment. The method for manufacturing a seamless steel pipe includes a step of preparing a mother pipe (preparation step), and a step of quenching and tempering the mother pipe to produce a seamless steel pipe (quenching step and tempering step). Note that the manufacturing method according to this embodiment is not limited to the manufacturing method described below. Each step will be described in detail below.
[0088] [Preparation process] In the preparation step, an intermediate steel material having the above-mentioned chemical composition is prepared. As long as the intermediate steel material has the above-mentioned chemical composition, the manufacturing method of the intermediate steel material is not particularly limited. The intermediate steel material referred to here is a plate-shaped steel material when the final product is a steel plate, a blank pipe when the final product is a steel pipe, and a steel material having a circular cross section perpendicular to the axial direction when the final product is a round steel.
[0089] The preparation step may include a step of preparing a material (material preparation step) and a step of hot working the material to produce an intermediate steel material (hot working step). Hereinafter, the case including the material preparation step and the hot working step will be described in detail.
[0090] [Material preparation process] In the material preparation step, a material is manufactured using molten steel having the above-mentioned chemical composition. The method for manufacturing the material is not particularly limited and may be a well-known method. Specifically, a cast piece (slab, bloom, or billet) may be manufactured using the molten steel by a continuous casting method. An ingot may be manufactured using the molten steel by an ingot casting method. If necessary, the slab, bloom, or ingot may be rolled to manufacture a billet. The material (slab, bloom, or billet) is manufactured by the above steps.
[0091] [Hot processing process] In the hot working process, the prepared material is hot worked to produce an intermediate steel material. When the steel material is a seamless steel pipe, the intermediate steel material corresponds to a mother pipe. First, the billet is heated in a heating furnace. The heating temperature is not particularly limited, but is, for example, 1100 to 1300°C. The billet extracted from the heating furnace is hot worked to produce a mother pipe (seamless steel pipe). The method of hot working is not particularly limited, and may be a well-known method.
[0092] For example, the Mannesmann process may be carried out as the hot working to produce a mother pipe. In this case, a round billet is pierced and rolled using a piercing machine. When piercing and rolling is performed, the piercing ratio is not particularly limited, but is, for example, 1.0 to 4.0. The pierced and rolled round billet is further hot rolled using a mandrel mill, a reducer, a sizing mill, or the like to produce a mother pipe. The cumulative reduction in area in the hot working process is, for example, 20 to 70%.
[0093] Other hot working methods may be used to manufacture a mother pipe from the billet. For example, in the case of a short, thick-walled steel material such as a coupling, the mother pipe may be manufactured by forging such as the Erhardt process. The mother pipe is manufactured by the above steps. The thickness of the mother pipe is not particularly limited, but is, for example, 9 to 60 mm.
[0094] When the steel material is round steel, the material is first heated in a heating furnace. The heating temperature is not particularly limited, but is, for example, 1100 to 1300°C. The material extracted from the heating furnace is subjected to hot processing to produce an intermediate steel material having a circular cross section perpendicular to the axial direction. The hot processing is, for example, blooming rolling by a blooming mill, or hot rolling by a continuous rolling mill. In the continuous rolling mill, a horizontal stand having a pair of grooved rolls arranged side by side in the vertical direction and a vertical stand having a pair of grooved rolls arranged side by side in the horizontal direction are alternately arranged.
[0095] When the steel material is a steel plate, the material is first heated in a heating furnace. The heating temperature is not particularly limited, but is, for example, 1100 to 1300° C. The material removed from the heating furnace is subjected to hot rolling using a blooming mill and a continuous rolling mill to produce an intermediate steel material in the shape of a steel plate.
[0096] The mother pipe produced by hot working may be air-cooled (as-rolled). The mother pipe produced by hot working may be quenched directly after the hot working without being cooled to room temperature, or may be quenched after being reheated after the hot working.
[0097] When quenching is performed directly after hot working, or after reheating, cooling may be stopped or slow cooling may be performed during quenching. In this case, it is possible to prevent quench cracks from occurring in the mother pipe. When quenching is performed directly after hot working, or after reheating, stress relief annealing (SR) may be performed after quenching and before the next heat treatment. In this case, residual stress in the mother pipe is removed.
[0098] As described above, in the preparation step, an intermediate steel material is prepared. The intermediate steel material may be manufactured by the above-mentioned preferred step, or an intermediate steel material manufactured by a third party, or an intermediate steel material manufactured in a factory or business establishment other than the factory where the quenching step and tempering step described below are performed, may be prepared. The quenching step will be described in detail below.
[0099] [Quenching process] In the quenching process, quenching is performed on the prepared intermediate steel material (blank pipe). 3 This means that the intermediate steel material is quenched at a temperature equal to or higher than the quenching temperature. In this specification, the temperature of the intermediate steel material immediately before quenching when quenching is performed is also referred to as the quenching temperature. Preferably, in the quenching process according to this embodiment, heating is performed in two stages, followed by quenching. That is, the quenching process according to this embodiment includes a first heating process, a second heating process, and a quenching process. Each process will be described in detail below.
[0100] [First heating step] Preferably, in the first heating step according to this embodiment, the prepared intermediate steel material (blank pipe) is heated to a heating temperature T1 (°C) and held for a heating time t1 (min). If the heating temperature T1 is too low, the austenite transformation may not be completed. In this case, the produced steel material does not have a yield strength of less than 552 to 655 MPa. On the other hand, if the heating temperature T1 is too high, the prior γ grain size DA may become coarse and Fn1 may become too large. In this case, the produced steel material does not exhibit excellent low-temperature toughness in an extremely low-temperature environment. Therefore, the heating temperature T1 (°C) in the first heating step is preferably set to 900 to 980°C.
[0101] Furthermore, if the heating time t1 is too short, the austenite transformation may not be completed. In this case, the produced steel material does not have a yield strength of less than 552 to 655 MPa. On the other hand, if the heating time t1 is too long, the prior γ grain size DA may become coarse and Fn1 may become too large. In this case, the produced steel material does not exhibit excellent low-temperature toughness in an extremely low-temperature environment. Therefore, the heating time t1 (min) of the first heating step is preferably set to 5 to 15 min.
[0102] [Second heating process] Preferably, in the second heating step according to the present embodiment, the intermediate steel material (blank pipe) heated in the first heating step is heated to a heating temperature T2 (°C) and held for a heating time t2 (min). If the heating temperature T2 is too low, the carbides may not be sufficiently dissolved. In this case, the number density of the coarse carbides may be too high in the manufactured steel material, and the manufactured steel material does not exhibit excellent low-temperature toughness in a cryogenic environment. On the other hand, if the heating temperature T2 is too high, the prior γ grain size DA may become coarse, and Fn1 may become too large. In this case, the manufactured steel material does not exhibit excellent low-temperature toughness in a cryogenic environment. Therefore, the heating temperature T2 (°C) in the second heating step is preferably set to 1000 to 1100°C.
[0103] Furthermore, if the heating time t2 is too short, the carbides may not be sufficiently dissolved. In this case, the number density of coarse carbides in the produced steel material becomes too high, and the steel material does not exhibit excellent low-temperature toughness in a cryogenic environment. On the other hand, if the heating time t2 is too long, the prior γ grain size DA may become coarse, and Fn1 may become too large. In this case, the produced steel material does not exhibit excellent low-temperature toughness in a cryogenic environment. Therefore, the heating time t2 (min) of the second heating step is preferably set to 3 to 10 min.
[0104] [Quenching process] In the quenching process, the intermediate steel material (blank tube) heated in the second heating process is quenched. In the quenching process, the intermediate steel material (blank tube) is continuously cooled to continuously lower the surface temperature of the blank tube. The method of the continuous cooling treatment is not particularly limited, and may be a well-known method. For example, the continuous cooling treatment method is a method of immersing the blank tube in a water tank for cooling, or a method of accelerating cooling the blank tube by shower water cooling or mist cooling.
[0105] If the cooling rate during quenching is too slow, the microstructure will not be mainly composed of tempered martensite and tempered bainite after the tempering process described below, and the mechanical properties specified in this embodiment will not be obtained. Here, in the rapid cooling process according to this embodiment, the average cooling rate in the range of the surface temperature of the intermediate steel material (blank pipe) during quenching from 800 to 500°C is defined as the cooling rate during quenching CR 800-500 Specifically, the cooling rate during quenching, CR 800-500 is determined from the temperature measured at the slowest cooling location in the cross section of the intermediate steel being quenched (e.g., the center of the intermediate steel thickness when both surfaces are forced cooled).
[0106] In the quenching step according to the present embodiment, the preferred cooling rate during quenching is CR 800-500 The cooling rate during quenching is preferably 60°C / min or more. 800-500 The lower limit of the cooling rate during quenching is 300° C. / min, and more preferably 600° C. / min. 800-500The upper limit of the quenching rate is not particularly specified, but is, for example, 6000° C. / min. Through the above steps, the quenching process according to this embodiment can be carried out. The tempering process will be described in detail below.
[0107] [Tempering process] In the tempering process, tempering is performed after the above-mentioned quenching. In this specification, "tempering" refers to the process of tempering the intermediate steel material after quenching. c1 This means that the steel is reheated to a temperature below the predetermined holding temperature and held therein. The holding temperature in the tempering process is adjusted as appropriate according to the chemical composition of the steel and the yield strength to be obtained. That is, the holding temperature is adjusted for an intermediate steel (blank pipe) having the chemical composition of this embodiment, so that the yield strength of the steel is adjusted to 80 to less than 95 ksi (552 to less than 655 MPa). Here, the holding temperature corresponds to the temperature of the furnace when the intermediate steel after quenching is heated and held therein. The holding time refers to the time from when the temperature of the intermediate steel reaches a predetermined holding temperature to when it is extracted from the heat treatment furnace.
[0108] The holding temperature is appropriately adjusted depending on the chemical composition of the steel material and the yield strength to be obtained. That is, the holding temperature is adjusted for an intermediate steel material (blank pipe) having the chemical composition of this embodiment, so that the yield strength of the steel material is adjusted to 552 to less than 655 MPa. In the tempering process according to this embodiment, the preferred holding temperature is 640 to 720°C.
[0109] If the holding time is too short, a microstructure mainly composed of tempered martensite and tempered bainite may not be obtained. On the other hand, if the holding time is too long, the above effects are saturated. Therefore, in the tempering process of this embodiment, the holding time is preferably 20 to 180 minutes. A more preferable lower limit of the holding time is 30 minutes. A more preferable upper limit of the holding time is 150 minutes, and further preferably 120 minutes.
[0110] The steel material according to this embodiment can be manufactured by the above manufacturing method. In the above manufacturing method, a method for manufacturing a steel pipe has been described as one example. However, the steel material according to this embodiment may be a steel plate or other shape. Similar to the above manufacturing method, a manufacturing method for a steel plate or other shape also includes, for example, a preparation step, a quenching step, and a tempering step. Furthermore, the above manufacturing method is one example, and the steel material may be manufactured by other manufacturing methods.
[0111] The present invention will be described in more detail below with reference to examples. Note that the examples described below are examples of conditions adopted to confirm the feasibility and effects of the steel material according to this embodiment. In other words, the steel material according to this embodiment is not limited to the examples described below. EXAMPLES
[0112] 180 kg of molten steel having the chemical composition shown in Tables 2-1 and 2-2 was produced. In Tables 2-1 and 2-2, "-" means that the content of the corresponding element was at the impurity level. Specifically, the V content, Nb content, Ti content, W content, Co content, Ni content, and Cu content of Test No. 1 were 0% when rounded off to the second decimal place. The Sn content of Test No. 1 was 0% when rounded off to the fourth decimal place. The Zr content, Ca content, Mg content, B content, and REM content of Test No. 1 were 0% when rounded off to the fifth decimal place.
[0113] [Table 2-1]
[0114] [Table 2-2]
[0115] A round billet was produced by continuous casting using the molten steel of each test number. The produced round billet of each test number was heated and hot worked. Specifically, the round billet of each test number was subjected to hot rolling by the Mannesmann-mandrel method as hot working to produce a blank pipe (seamless steel pipe) of each test number.
[0116] The obtained blank tubes of each test number were subjected to quenching and tempering. At this time, the heating in the quenching process was performed in two stages, a first heating process and a second heating process. Specifically, the blank tubes of each test number were heated in the first heating process at the heating temperature T1 (°C) for the heating time t1 (min) shown in the "Quenching process" column of Table 3, and then in the second heating process at the heating temperature T2 (°C) for the heating time t2 (min). The heated blank tubes of each test number were water-cooled to perform quenching. At this time, the cooling rate during quenching of the blank tubes of each test number was CR 800-500 was in the range of 60 to 6000℃ / min.
[0117] [Table 3]
[0118] Furthermore, the obtained blank pipes of each test number were tempered. Specifically, the blank pipes of each test number were tempered by holding them at the holding temperature (°C) for the holding time (minutes) shown in the "Tempering step" column in Table 3. Through the above manufacturing process, seamless steel pipes of each test number were obtained.
[0119] [Evaluation test] The seamless steel pipes having the respective test numbers after tempering were subjected to a tensile test, a coarse carbide number density measurement test, an Fn1 measurement test, and a Charpy impact test, which will be described below.
[0120] [Tensile test] A tensile test was performed on the seamless steel pipe of each test number in accordance with ASTM E8 / E8M (2021). Specifically, a round bar test piece with a parallel part diameter of 6 mm and a gauge length of 30 mm was prepared from the center of the wall thickness of the seamless steel pipe of each test number. The axial direction of the round bar test piece was parallel to the pipe axial direction of the seamless steel pipe. Using the prepared round bar tensile test piece, a tensile test was performed at room temperature (25 ° C) in air to obtain the yield strength (MPa) of the seamless steel pipe of each test number. In this embodiment, the 0.2% offset proof stress (MPa) obtained in the tensile test was defined as the yield strength. The obtained yield strength of each test number is shown in Table 4 as "YS (MPa)".
[0121] [Table 4]
[0122] [Measurement test for number and density of coarse carbides] A coarse carbide number density measurement test was carried out for each seamless steel pipe of test number by the above-mentioned method. Specifically, a test piece was prepared from the center of the wall thickness of each seamless steel pipe of test number, with the surface including the pipe axis direction and the pipe diameter direction as the observation surface. The observation surface of the prepared test piece was polished to a mirror finish, and then cut into 300 mm pieces. 2 In the observation surface (20 mm × 15 mm), the particles identified from the contrast by the above-mentioned method were subjected to EDS analysis by the above-mentioned method to identify carbides. In this example, as in the above-mentioned method, particles in which C was detected and the Fe content was 50 mass% or more were identified as carbides.
[0123] Among the identified carbides, carbides with a circle equivalent diameter of 2 μm or more were identified using image analysis. The number density of the coarse carbides (pieces / mm 2 The density of coarse carbides (pieces / mm 2 ) are shown in Table 4.
[0124] [Fn1 measurement test] For each seamless steel pipe of each test number, the prior gamma grain size DA (μm), block diameter DB (μm), and Fn1 (=DA / DB) were determined using the method described above. Specifically, a test piece for measuring the prior gamma grain size DA was prepared from the center of the wall thickness of each seamless steel pipe of each test number, with the surface including the pipe axis direction and the pipe diameter direction as the observation surface. The prepared test piece was embedded in resin, and the observation surface was polished to a mirror finish. After that, it was immersed for about 60 seconds in a solution of a saturated aqueous solution of picric acid mixed with an appropriate amount of surfactant, and the prior gamma grain boundaries were revealed by etching. The etched 100 mm 2 The observation surface (10 mm × 10 mm) was observed with an optical microscope, and the grain size number was determined based on the cutting method in accordance with JIS G 0551 (2020). Using the obtained grain size number, the prior austenite grain size (prior γ grain size DA) was determined by the above-mentioned method.
[0125] Next, a test piece for measuring the block diameter DB, with an observation surface of 25 μm × 25 μm, was prepared from the center of the wall thickness of each seamless steel pipe with each test number. EBSD measurement was performed on the observation surface of the test piece. The EBSD measurement was performed with an acceleration voltage of 20 kV, a field of view of 25 μm × 25 μm, and a pitch of 0.1 μm. A crystal orientation diagram was obtained from the obtained Kikuchi line pattern, and an area surrounded by an orientation difference of 15° or more with adjacent crystals was identified to obtain a crystal orientation map. An area surrounded by an orientation difference of 15° or more was defined as one block. For the defined blocks, the average grain size of the block (block diameter DB) was obtained using the method described above.
[0126] The prior gamma grain size DA (μm) obtained for each test number is shown in the "DA (μm)" column of Table 4. The block diameter DB (μm) obtained for each test number is shown in the "DB (μm)" column of Table 4. Fn1 (= DA / DB) was calculated from the prior gamma grain size DA (μm) and block diameter DB (μm) obtained for each test number. Table 4 shows the Fn1 obtained for each test number.
[0127] [Charpy impact test] A Charpy impact test in accordance with ASTM E23 (2018) was carried out on the seamless steel pipes of each test number. Specifically, a V-notch test piece having a notch surface perpendicular to the pipe axis direction and a longitudinal direction perpendicular to the pipe axis direction and the pipe diameter direction was prepared from the center of the wall thickness of the seamless steel pipes of each test number. A Charpy impact test was carried out on the prepared V-notch test piece in accordance with ASTM E23 (2018). The test temperature was set to eight levels (-120°C, -100°C, -80°C, -60°C, -40°C, -20°C, 0°C, and 20°C) that were changed by 20°C in the range of -120 to 20°C. The Charpy impact test was carried out using two test pieces for each test temperature. The brittle fracture rate (%) of the test piece after the test at each temperature was calculated. The temperature (°C) at which the brittle fracture rate becomes 50% was calculated from the approximate curve obtained by plotting the test temperature (°C) and the brittle fracture rate (%), and the fracture transition temperature vTrs (°C) was obtained. The fracture transition temperature vTrs (°C) for each test number is shown in the "vTrs (°C)" column in Table 4.
[0128] [Evaluation Results] With reference to Tables 2-1, 2-2, 3, and 4, the seamless steel pipes of test numbers 1 to 38 had appropriate chemical compositions and the manufacturing methods also satisfied the preferred conditions described in the specification. As a result, these seamless steel pipes had a yield strength of 552 to less than 655 MPa and a coarse carbide number density of 10 pieces / mm 2 or less, and Fn1 was 2.5 to 10.0. As a result, these seamless steel pipes had a fracture appearance transition temperature vTrs of -70°C or less, and had excellent low-temperature toughness even in an extremely low-temperature environment. It was also determined that the total volume fraction of tempered martensite and tempered bainite in all of these seamless steel pipes was 90% or more.
[0129] On the other hand, the seamless steel pipe of test number 39 had too low a C content and too low a Fn1. As a result, the seamless steel pipe had a fracture transition temperature vTrs exceeding -70°C and did not have excellent low-temperature toughness in an extremely low-temperature environment.
[0130] The seamless steel pipe of test number 40 had too high a Mn content. As a result, the seamless steel pipe had a fracture transition temperature vTrs exceeding -70°C and did not have excellent low-temperature toughness in an extremely low-temperature environment.
[0131] The seamless steel pipe of test number 41 had too high a P content. As a result, the fracture transition temperature vTrs of this seamless steel pipe exceeded -70°C, and it did not have excellent low-temperature toughness in an extremely low-temperature environment.
[0132] The seamless steel pipe of test number 42 had too high a S content. As a result, the fracture transition temperature vTrs of this seamless steel pipe exceeded -70°C, and it did not have excellent low-temperature toughness in an extremely low-temperature environment.
[0133] The seamless steel pipe of test number 43 had too low a Cr content, and as a result, the fracture transition temperature vTrs of this seamless steel pipe exceeded -70°C, and it did not have excellent low-temperature toughness in an extremely low-temperature environment.
[0134] The seamless steel pipe of test number 44 had too high a Cr content. As a result, the seamless steel pipe had a yield strength of 655 MPa or more, which was not the desired yield strength. As a result, the seamless steel pipe had a fracture transition temperature vTrs of over -70°C, and did not have excellent low-temperature toughness in an extremely low-temperature environment.
[0135] The seamless steel pipe of test number 45 had too high a Mo content. As a result, the fracture transition temperature vTrs of this seamless steel pipe exceeded -70°C, and it did not have excellent low-temperature toughness in an extremely low-temperature environment.
[0136] The seamless steel pipe of test number 46 had a too low holding temperature in the tempering process. As a result, the seamless steel pipe had a yield strength of 655 MPa or more, which was not the desired yield strength. As a result, the seamless steel pipe had a fracture transition temperature vTrs of over -70°C, and did not have excellent low-temperature toughness in an extremely low-temperature environment.
[0137] For the seamless steel pipe of test number 47, the second heating step was not performed in the quenching process. As a result, the number density of coarse carbides in this seamless steel pipe was 10 pieces / mm 2 As a result, the fracture appearance transition temperature vTrs of this seamless steel pipe exceeded -70°C, and it did not have excellent low-temperature toughness in an extremely low-temperature environment.
[0138] The seamless steel pipe of test number 48 had a heating temperature T2 in the second heating step of the quenching process that was too high. As a result, the seamless steel pipe had an Fn1 value of more than 10.0. As a result, the seamless steel pipe had a fracture transition temperature vTrs of more than -70°C and did not have excellent low-temperature toughness in an extremely low-temperature environment.
[0139] The seamless steel pipe of test number 49 had a heating time t2 in the second heating step of the quenching process that was too long. As a result, the seamless steel pipe had an Fn1 value of more than 10.0. As a result, the seamless steel pipe had a fracture transition temperature vTrs of more than -70°C and did not have excellent low-temperature toughness in an extremely low-temperature environment.
[0140] The embodiments of the present disclosure have been described above. However, the above-described embodiments are merely examples for implementing the present disclosure. Therefore, the present disclosure is not limited to the above-described embodiments, and can be implemented by appropriately modifying the above-described embodiments without departing from the spirit of the present disclosure.
Claims
1. A steel material, In mass percent, C: 0.26-0.35%, Si: 0.10-1.00%, Mn: 1.00-1.40%, P: 0.015% or less, S: 0.0020% or less, Cr: 0.15-0.50%, Mo: 0.05-0.25%, sol. Al: 0.001 to 0.070%, N: 0.0010-0.0080%, V: 0-0.60%, Nb: 0 to 0.03%, Ti: 0 to 0.05%, W: 0-0.50%, Zr: 0 to 0.0050%, Co: 0 to 0.50%, Ni: 0 to 0.30%, Cu: 0 to 0.50%, Sn: 0-0.100%, Ca: 0-0.0035%, Mg: 0 to 0.0035%, B: 0 to 0.0010%, Rare earth elements: 0 to 0.0050%, and The balance is composed of Fe and impurities. The yield strength is less than 552 to 655 MPa; In the microstructure of the steel material, the total volume fraction of tempered martensite and tempered bainite is 90% or more, In the steel material, 10 carbides per mm with a circle equivalent diameter of 2 μm or more 2 is as follows: When the prior austenite grain size is defined as DA and the block diameter as DB, The DA and the DB satisfy formula (1), Steel material. 2.5≦DA / DB≦10.0 (1) Here, the prior austenite grain size (unit: μm) is substituted for DA in formula (1), and the block diameter (unit: μm) is substituted for DB in formula (1).
2. The steel material according to claim 1, V: 0.01-0.60%, Nb: 0.01-0.03%, Ti: 0.01-0.05%, W: 0.01-0.50%, Zr: 0.0001 to 0.0050%, Co: 0.01 to 0.50%, Ni: 0.01 to 0.30%, Cu: 0.01 to 0.50%, Sn: 0.001 to 0.100%, Ca: 0.0001-0.0035%, Mg: 0.0001 to 0.0035%, B: 0.0001 to 0.0010%, and Rare earth elements: 0.0001 to 0.0050%; containing one or more elements selected from the group consisting of Steel material.
3. The steel material according to claim 1 or 2, The steel material is a steel pipe. Steel material.
Citation Information
Patent Citations
CO2 corrosion resistant steel tube and preparation method thereof
CN112921250A
Seamless steel tube with high toughness and high corrosion resistance
JP2001073086A
Steel material with high toughness and method for manufacturing steel pipe thereof
JP2003041341A
Seamless steel tube and method for producing the same
JP2007031769A
Oil well steel pipe to be placed under ground and be expanded
WO2004106572A1