Photosensitive fiber-forming composition and method for forming fiber patterns

A photosensitive fiber forming composition using (meth)acrylic or polyvinylphenol resin enables the creation of flexible and conductive metal patterns, addressing the limitations of ITO films by providing a cost-effective and bendable alternative with high light transmittance and conductivity.

JP7564521B2Active Publication Date: 2024-10-09TOYAMA PREFECTURE +1
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2020571063
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-02-08
Filing Date
2020-01-16
Publication Date
2024-10-09
Estimated Expiration
2040-01-16

AI Technical Summary

Technical Problem

The need for alternative materials to Indium Tin Oxide (ITO) films in transparent conductive films and transparent wiring patterns due to the high cost, brittleness, and lack of bending resistance of indium, along with the challenge of forming flexible and conductive metal patterns using polymer nanofibers.

Method used

A photosensitive fiber forming composition is used to create a metal pattern by electrospinning a positive photosensitive material, such as a (meth)acrylic resin or polyvinylphenol resin, onto a metal thin film, patterning with light, and etching to form a flexible and conductive metal network.

Benefits of technology

The method produces a flexible and conductive metal pattern with high light transmittance and maintains conductivity through repeated bending, offering a cost-effective alternative to ITO films.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007564521000001
    Figure 0007564521000001
Patent Text Reader

Abstract

[Problem] The present invention addresses the problem of providing: a method for producing a metal pattern by processing a substrate having a metal layer at a surface thereof, using photosensitive fibers having a specific composition; a production method for a metal pattern; and a composition for producing the photosensitive fibers, and preferably providing a transparent interconnect pattern that is low-cost and is flexible. [Solution] The present invention provides a photosensitive fiber containing a positive photosensitive material. The positive photosensitive material may contain a novolac resin or the like. The production method for a metal pattern according to the present invention includes a first step for forming a fiber layer containing photosensitive fibers on a substrate having a metal layer at a surface thereof, a second step for exposing the fiber layer with light through a mask, a third step for developing the fiber layer using a developer liquid to form a photosensitive fiber pattern, and a fourth step for etching the metal layer using an etchant, and removing the photosensitive fibers, to form a reticulated metal pattern.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a photosensitive fiber-forming composition and a method for forming a fiber pattern. For example, a photosensitive fiber containing a photosensitive material is coated on a substrate having a metal layer on its surface, and then the metal is etched using the photosensitive fiber as a mask to obtain a substrate having a metal pattern. [Background technology]

[0002] In recent years, the market for transparent conductive films and transparent wiring patterns using ITO (Indium Tin Oxide) films has expanded along with the growing demand for solar cells and touch panels. However, indium, a rare metal, is expensive, brittle, and has poor bending resistance, so there is a strong demand for the development of alternative materials.

[0003] Recently, with the development of the electrospinning method, the use of polymer nanofibers has begun to progress in many fields, including clothing, batteries, and medicine. A new method is being researched to form a transparent conductive film with a metal network structure finer than the wavelength of visible light by etching a thin metal film using the fine mesh structure of polymer nanofibers as an etching mask (Non-Patent Documents 1 and 2).

[0004] Furthermore, Patent Documents 1 and 2 describe a technology (photosensitive nanofiber technology) in which photosensitivity is imparted to polymer nanofibers obtained by electrospinning and the deposited nanofiber sheet is patterned into any shape using light. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] International Publication No. 2015 / 056789 Brochure [Patent Document 2] International Publication No. 2016 / 171233 Brochure [Non-patent literature]

[0006] [Non-Patent Document 1] Keisuke Azuma, Koichi Sakajiri, Hidetoshi Matsumoto, Sungmin Kang, Junji Watanabe and Masatoshi Tokita, Mat.Lett.,115,187(2014) [Non-Patent Document 2] Tianda He, Aozhen Xie, Darrell H. Reneker and Yu Zhu, ACS Nano, 8(5), 4782(2014) Summary of the Invention [Problem to be solved by the invention]

[0007] The problem to be solved by the present invention is to provide a method for producing a metal pattern in which a substrate having a metal layer on its surface is processed using a photosensitive fiber having a specific composition, a method for producing a metal pattern, and a composition for producing the photosensitive fiber. As a specific example of the above problem, it is possible to provide an inexpensive and flexible transparent wiring pattern and a film with a transparent wiring pattern, which can replace ITO films, by using photosensitive nanofibers in a transparent conductive film. [Means for solving the problem]

[0008] The inventors have discovered that a wiring pattern consisting of a fine metal mesh structure that combines both flexibility and conductivity can be formed by using an electrospinning method to deposit a photosensitive polymer having a specific composition into nanofibers (fibers) on a thin metal film vapor-deposited on a film, irradiating the photosensitive fibers with light through a photomask to pattern them into wiring, and then etching the thin metal film using the photosensitive fibers as an etching mask, thereby completing the present invention.

[0009] That is, the present invention relates to the following. 1. A photosensitive fiber made of a positive-type photosensitive material, the positive-type photosensitive material containing a (meth)acrylic resin or a polyvinylphenol resin, and a dissolution inhibitor. 2. A composition for producing a photosensitive fiber, comprising a (meth)acrylic resin or a polyvinylphenol resin, a dissolution inhibitor and a solvent. 3. The composition according to claim 2, further comprising an electrolyte. 4. A method for producing a photosensitive fiber, comprising the step of spinning the composition described in 2 or 3 above. 5. A method for producing a photosensitive fiber pattern, comprising: a first step of spinning the composition described in 2 or 3 above onto a substrate to form a fiber layer composed of photosensitive fibers; a second step of exposing the fiber layer through a mask; and a third step of developing the fiber layer with a developer to form a photosensitive fiber pattern. 6. A method for producing a metal pattern, comprising: a first step of forming a fiber layer made of photosensitive fibers on a substrate having a metal layer on its surface; a second step of exposing the fiber layer through a mask; a third step of developing the fiber layer with a developer to form a photosensitive fiber pattern; and a fourth step of etching the metal layer with an etching solution, further removing the photosensitive fibers, and forming a mesh-like metal pattern. 7. The method for producing a metal pattern described in 6 above, wherein the photosensitive fiber comprises (i) a novolac resin and a dissolution inhibitor, (ii) a polyvinylphenol resin or a (meth)acrylic resin, and a photoacid generator, (iii) a polyvinylphenol resin or a (meth)acrylic resin containing a structural unit having a photoacid generating group in its side chain, or (iv) a polyvinylphenol resin or a (meth)acrylic resin, and a dissolution inhibitor. 8. The method for producing a metal pattern according to 6 or 7 above, wherein the mesh-like metal pattern has a light transmittance of 5% or more in the visible light wavelength region. 9. A method for producing a metal pattern according to any one of items 6 to 8 above, wherein the metal pattern can be bent 10 or more times while maintaining electrical conductivity in a repeated bending test. 10. A method for producing a substrate having a metal pattern, comprising: a first step of forming a fiber layer made of photosensitive fibers on a substrate having a metal layer on its surface; a second step of exposing the fiber layer through a mask; a third step of developing the fiber layer with a developer to form a photosensitive fiber pattern; and a fourth step of etching the metal layer with an etching solution, further removing the photosensitive fibers, and forming a mesh-like metal pattern. 11. A method for producing a substrate having a metal pattern according to claim 10, wherein the photosensitive fiber comprises (i) a novolac resin and a dissolution inhibitor, (ii) a polyvinylphenol resin or a (meth)acrylic resin, and a photoacid generator, (iii) a polyvinylphenol resin or a (meth)acrylic resin containing a structural unit having a photoacid generating group on its side chain, or (iv) a polyvinylphenol resin or a (meth)acrylic resin, and a dissolution inhibitor. 12. A substrate having a metal pattern produced by the method for producing a substrate having a metal pattern described in 10 or 11 above. 13. The substrate having a metal pattern according to the above item 12, wherein the mesh-like metal pattern has a light transmittance of 5% or more in the visible light wavelength region. 14. The substrate having a metal pattern according to 12 or 13 above, which can be bent 10 times or more while maintaining electrical conductivity in a repeated bending test. Effect of the Invention

[0010] According to the present invention, it is possible to provide a photosensitive fiber that can easily produce a complex and fine resist pattern, a fiber pattern formed using the photosensitive fiber, and methods for producing the same. Furthermore, according to the present invention, a composition for producing the above-mentioned photosensitive fiber (photosensitive fiber-forming composition) can be provided. Furthermore, according to the present invention, there can be provided a metal pattern formed from the above-mentioned fiber pattern, a substrate having a metal pattern, and methods for producing them. [Brief description of the drawings]

[0011] [Figure 1] 1A to 1C are schematic diagrams illustrating a method for forming a transparent wiring pattern using photosensitive fibers. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0012] 1. Photosensitive fiber and its manufacturing method The fiber of the present invention is mainly characterized by containing a positive-type photosensitive material. That is, the fiber of the present invention is preferably a fiber obtained by spinning (more preferably electrospinning) a raw material composition containing at least a positive-type photosensitive material. In the present invention, a fiber containing a positive-type photosensitive material may be referred to as a "positive-type photosensitive fiber."

[0013] The diameter of the fiber of the present invention can be appropriately adjusted depending on the application of the fiber and is not particularly limited, but from the viewpoint of application to etching masks when processing various substrates used in displays and semiconductors, medical materials, cosmetic materials, etc., the fiber of the present invention is preferably a fiber (nanofiber) having a diameter on the order of nanometers (e.g., 1 to 1000 nm) and / or a fiber (microfiber) having a diameter on the order of micrometers (e.g., 1 to 1000 μm). In the present invention, the fiber diameter is measured with a scanning electron microscope (SEM).

[0014] In the present invention, the term "positive photosensitive material" refers to a material that changes from poorly soluble or insoluble in alkali to easily soluble in alkali by the action of light (for example, a positive photoresist, a positive photosensitive resin composition, etc.).

[0015] The positive photosensitive material is not particularly limited as long as it can be made into a fiber form, and may be any known material that has been used conventionally as a positive photoresist or a positive photosensitive resin composition, etc. Examples of the material include (i) a novolac resin and a dissolution inhibitor, (ii) a polyvinylphenol resin or a (meth)acrylic resin, and a photoacid generator, and (iii) a polyvinylphenol resin or a (meth)acrylic resin containing a structural unit having a photoacid generating group in a side chain. Alternatively, (iv) the polyvinylphenol resin or the (meth)acrylic resin, and the dissolution inhibitor are also positive photosensitive materials used as a positive photosensitive resin composition or the like.

[0016] The positive-working photosensitive material used in the present invention may contain the above (i), the above (ii), the above (iii), or the above (iv).

[0017] As the novolak resin, any novolak resin that has been conventionally used in positive-type photosensitive materials can be used without any restrictions, and examples thereof include resins obtained by polymerizing phenols and aldehydes in the presence of an acid catalyst.

[0018] Examples of the phenols include cresols such as phenol, o-cresol, m-cresol, and p-cresol; xylenols such as 2,3-xylenol, 2,4-xylenol, 2,5-xylenol, 2,6-xylenol, 3,4-xylenol, and 3,5-xylenol; o-ethylphenol, m-ethylphenol, p-ethylphenol, 2-isopropylphenol, 3-isopropylphenol, 4-isopropylphenol, o-butylphenol, m-butylphenol, p-butylphenol, and p-tert Examples of the phenols include alkylphenols such as α-butylphenol, trialkylphenols such as 2,3,5-trimethylphenol and 3,4,5-trimethylphenol, polyhydric phenols such as resorcinol, catechol, hydroquinone, hydroquinone monomethyl ether, pyrogallol and phloroglucinol, alkyl polyhydric phenols such as alkylresorcinol, alkylcatechol and alkylhydroquinone (all alkyl groups have 1 to 4 carbon atoms), α-naphthol, β-naphthol, hydroxydiphenyl and bisphenol A. These phenols may be used alone or in combination of two or more.

[0019] Examples of the aldehydes include formaldehyde, paraformaldehyde, furfural, benzaldehyde, nitrobenzaldehyde, acetaldehyde, etc. These aldehydes may be used alone or in combination of two or more kinds.

[0020] Examples of the acid catalyst include inorganic acids such as hydrochloric acid, sulfuric acid, nitric acid, phosphoric acid, and phosphorous acid; organic acids such as formic acid, oxalic acid, acetic acid, diethylsulfuric acid, and paratoluenesulfonic acid; and metal salts such as zinc acetate.

[0021] The weight average molecular weight of the novolak resin is not particularly limited, but is preferably 500 to 50,000, and from the viewpoints of resolution and spinnability, is more preferably 1,500 to 15,000.

[0022] In the present invention, the "weight average molecular weight" refers to a molecular weight calculated in terms of polystyrene, measured by gel permeation chromatography (GPC).

[0023] The dissolution inhibitor may be any of those conventionally used as photosensitizers in positive-type photosensitive materials, without any restrictions. Examples of the dissolution inhibitor include naphthoquinone diazide compounds such as 1,2-naphthoquinone diazide-5-sulfonic acid ester and 1,2-naphthoquinone diazide-4-sulfonic acid ester, and preferably 1,2-naphthoquinone diazide-5-sulfonic acid ester.

[0024] The content of the dissolution inhibitor is usually 5 to 50 parts by weight, and preferably 10 to 40 parts by weight, based on 100 parts by weight of the novolak resin.

[0025] The polyvinylphenol resin may be any of those conventionally used in positive-type photosensitive materials without any restrictions, and examples thereof include resins obtained by polymerizing hydroxystyrenes in the presence of a radical polymerization initiator.

[0026] Examples of the hydroxystyrenes include o-hydroxystyrene, m-hydroxystyrene, p-hydroxystyrene, 2-(o-hydroxyphenyl)propylene, 2-(m-hydroxyphenyl)propylene, 2-(p-hydroxyphenyl)propylene, etc. These hydroxystyrenes may be used alone or in combination of two or more.

[0027] Examples of the radical polymerization initiator include organic peroxides such as benzoyl peroxide, dicumyl peroxide, and dibutyl peroxide; and azobis compounds such as azobisisobutyronitrile and azobisvaleronitrile.

[0028] The weight average molecular weight of the polyvinylphenol resin is not particularly limited, but is preferably 500 to 50,000, and from the viewpoints of resolution and spinnability, is more preferably 1,500 to 25,000.

[0029] The (meth)acrylic resin may be any resin that has been conventionally used in positive-type photosensitive materials without any restrictions, and examples thereof include resins obtained by polymerizing a polymerizable monomer having a (meth)acrylic group in the presence of a radical polymerization initiator. Examples of the polymerizable monomer having a (meth)acrylic group include methyl (meth)acrylic acid ester, ethyl (meth)acrylic acid ester, propyl (meth)acrylic acid ester, butyl (meth)acrylic acid ester, pentyl (meth)acrylic acid ester, hexyl (meth)acrylic acid ester, heptyl (meth)acrylic acid ester, octyl (meth)acrylic acid ester, 2-ethylhexyl (meth)acrylic acid ester, nonyl (meth)acrylic acid ester, decyl (meth)acrylic acid ester, undecyl (meth)acrylic acid ester, and the like. Examples of the (meth)acrylic acid alkyl esters include dodecyl acrylic acid, trifluoroethyl (meth)acrylic acid, and tetrafluoropropyl (meth)acrylic acid; acrylamides such as diacetone acrylamide; tetrahydrofurfuryl (meth)acrylic acid, dialkylaminoethyl (meth)acrylic acid, glycidyl (meth)acrylic acid, (meth)acrylic acid, α-bromo(meth)acrylic acid, α-chloro(meth)acrylic acid, β-furyl(meth)acrylic acid, and β-styryl(meth)acrylic acid. These polymerizable monomers having a (meth)acrylic group may be used alone or in combination of two or more.

[0030] Examples of the radical polymerization initiator include organic peroxides such as benzoyl peroxide, dicumyl peroxide, and dibutyl peroxide; and azobis compounds such as azobisisobutyronitrile and azobisvaleronitrile.

[0031] The (meth)acrylic resin may be copolymerized with one or more of the following polymerizable monomers in addition to the polymerizable monomer having a (meth)acrylic group: polymerizable styrene derivatives substituted at the α-position or at the aromatic ring, such as styrene, vinyl toluene, and α-methyl styrene; esters of vinyl alcohol, such as acrylonitrile and vinyl-n-butyl ether; maleic acid monoesters, such as maleic acid, maleic anhydride, monomethyl maleate, monoethyl maleate, and monoisopropyl maleate; fumaric acid, cinnamic acid, α-cyanocinnamic acid, itaconic acid, and crotonic acid.

[0032] In this specification, "(meth)acrylic" means both "acrylic" and "methacrylic".

[0033] The weight average molecular weight of the (meth)acrylic resin is not particularly limited, but is preferably from 500 to 500,000, and from the viewpoints of resolution and spinnability, is more preferably from 1,500 to 100,000.

[0034] The polyvinylphenol resin or (meth)acrylic resin preferably contains a structural unit having, at the side chain, an alkali-soluble group protected by an acid labile protecting group.

[0035] Examples of the acid labile protecting group include a tert-butyl group, a tert-butoxycarbonyl group, a tert-butoxycarbonylmethyl group, a tert-amyloxycarbonyl group, a tert-amyloxycarbonylmethyl group, a 1,1-diethylpropyloxycarbonyl group, a 1,1-diethylpropyloxycarbonylmethyl group, a 1-ethylcyclopentyloxycarbonyl group, a 1-ethylcyclopentyloxycarbonylmethyl group, a 1-ethyl-2-cyclopentenyloxycarbonyl group, a 1-ethyl-2-cyclopentenyloxycarbonylmethyl group, a 1-ethoxyethoxycarbonylmethyl group, a 2-tetrahydropyranyloxycarbonylmethyl group, a 2-tetrahydrofuranyloxycarbonylmethyl group, a tetrahydrofuran-2-yl group, a 2-methyltetrahydrofuran-2-yl group, a tetrahydropyran-2-yl group, a 2-methyltetrahydropyran-2-yl group, and the like.

[0036] Examples of the alkali-soluble group include a phenolic hydroxy group and a carboxy group.

[0037] A polyvinylphenol resin or (meth)acrylic resin containing a structural unit having an alkali-soluble group protected by an acid labile protecting group in a side chain can be produced, for example, by introducing an acid labile protecting group into an alkali-soluble group of a polyvinylphenol resin or (meth)acrylic resin through a chemical reaction. Alternatively, the polyvinylphenol resin or (meth)acrylic resin can be produced by mixing a monomer corresponding to the structural unit having an alkali-soluble group protected by an acid labile protecting group in a side chain with a raw material monomer of the polyvinylphenol resin or (meth)acrylic resin, and copolymerizing the resulting monomer mixture.

[0038] The photoacid generator is not particularly limited as long as it is a compound that generates an acid directly or indirectly by the action of light, and examples thereof include diazomethane compounds, onium salt compounds, sulfonimide compounds, nitrobenzyl compounds, iron arene complexes, benzoin tosylate compounds, halogen-containing triazine compounds, cyano group-containing oxime sulfonate compounds, and naphthalimide compounds.

[0039] The content of the photoacid generator is usually 0.1 to 50 parts by weight, and preferably 3 to 30 parts by weight, based on 100 parts by weight of the polyvinylphenol resin or the (meth)acrylic resin.

[0040] A polyvinylphenol resin or (meth)acrylic resin containing a structural unit having a photoacid generating group in a side chain can be produced, for example, by mixing the above-mentioned photoacid generator as a monomer with raw material monomers for a polyvinylphenol resin or a (meth)acrylic resin, and copolymerizing the resulting monomer mixture.

[0041] The weight average molecular weight of the polyvinylphenol resin containing a structural unit having a photoacid generating group on the side chain is not particularly limited, but is preferably 500 to 50,000, and from the viewpoints of resolution and spinnability, is more preferably 1,500 to 25,000.

[0042] The weight average molecular weight of the (meth)acrylic resin containing a structural unit having a photoacid generating group on the side chain is not particularly limited, but is preferably 500 to 500,000, and from the viewpoints of resolution and spinnability, is more preferably 1,500 to 10,000.

[0043] The positive photosensitive material may be produced by a method known per se. For example, (i) a positive photosensitive material (positive photoresist) containing a novolak resin and a dissolution inhibitor can be produced by the method described in JP-B-7-66184 or the like. (ii) a positive photosensitive material (positive photoresist) containing a polyvinylphenol resin or an acrylic resin and a photoacid generator can be produced by the method described in JP-B-7-66184 and JP-A-2007-79589. (iii) a positive photosensitive material (positive photoresist) containing a polyvinylphenol resin or an acrylic resin containing a structural unit having a photoacid generating group in a side chain can be produced by the method described in JP-A-9-189998, JP-A-2002-72483, JP-A-2010-85971, JP-A-2010-256856, etc. Alternatively, a commercially available product may be used.

[0044] Regarding the production of the positive-working photosensitive material (iv), it can be produced by the method described in Japanese Patent No. 5093525 or the like.

[0045] The fibers of the present invention are preferably produced by spinning a photosensitive fiber-producing composition that contains a positive-type photosensitive material and a solvent.

[0046] The solvent is not particularly limited as long as it can uniformly dissolve or disperse the positive photosensitive material and does not react with each material, but a polar solvent is preferred. Examples of the polar solvent include water, methanol, ethanol, 2-propanol, propylene glycol monomethyl ether, propylene glycol monomethyl ether acetate, acetone, dimethylformamide, dimethylacetamide, N-methylpyrrolidone, and hexafluoroisopropanol. From the viewpoint of ease of spinning the composition for producing photosensitive fibers, preferred are propylene glycol monomethyl ether, propylene glycol monomethyl ether acetate, and hexafluoroisopropanol.

[0047] The solvents may be used alone or in combination of two or more kinds.

[0048] The fiber of the present invention is preferably produced by spinning a composition for producing a photosensitive fiber (hereinafter, also simply referred to as "the composition of the present invention") that contains a positive-type photosensitive material, a solvent, and an electrolyte.

[0049] The electrolyte may be, for example, tetrabutylammonium chloride.

[0050] The content of the positive photosensitive material in the composition of the present invention is preferably 60 to 100% by weight, more preferably 60 to 95% by weight, and particularly preferably 70 to 90% by weight, based on the solid content of the composition for manufacturing photosensitive fibers excluding the solvent, from the viewpoints of resolution and spinnability.

[0051] The composition of the present invention may contain, as necessary, additives that are usually used in compositions for fiber production other than the positive-type photosensitive material, so long as the additives do not significantly impair the object of the present invention. Examples of such additives include surfactants, rheology control agents, drugs, fine particles, etc.

[0052] The composition of the present invention is prepared by mixing a positive photosensitive material in a solvent, or by further mixing the above-mentioned additives therein. The mixing method is not particularly limited, and the mixing may be carried out by a method known per se or a method equivalent thereto.

[0053] The method for spinning the composition of the present invention is not particularly limited as long as it can form fibers. Examples of the method include melt-blowing, composite melt spinning, and electrospinning. From the viewpoint of the ability to form ultrafine fibers (nanofibers, microfibers), electrospinning is preferred.

[0054] The electrospinning method is a known spinning method and can be carried out using a known electrospinning device. Various conditions such as the speed at which the composition of the present invention is discharged from the tip of a nozzle (e.g., a needle, etc.) (discharge speed); applied voltage; and the distance from the tip of the nozzle discharging the composition of the present invention to the substrate receiving it (discharge distance) can be appropriately set according to the diameter of the fiber to be produced. The discharge speed is usually 0.1 to 100 μl / min, preferably 0.5 to 50 μl / min, and more preferably 1 to 20 μl / min. The applied voltage is usually 0.5 to 80 kV, preferably 1 to 60 kV, and more preferably 3 to 40 kV. The discharge distance is usually 1 to 60 cm, preferably 2 to 40 cm, and more preferably 3 to 30 cm.

[0055] The electrospinning method may also be carried out using a drum collector or the like. By using a drum collector or the like, the orientation of the fibers can be controlled. For example, when the drum is rotated at a low speed, a nonwoven fabric or the like can be obtained, and when the drum is rotated at a high speed, an oriented fiber sheet or the like can be obtained. This is effective when preparing an etching mask material or the like for processing semiconductor materials (e.g., substrates, etc.).

[0056] The method for producing the fiber of the present invention may further include a step of heating the spun fiber at a specific temperature in addition to the spinning step described above. The applied fiber needs to be in close contact with the conductive layer to function as a mask for the conductive layer. If the contact is insufficient, defects such as breaks may occur in the resulting fiber network structure, resulting in a decrease in conductivity. For example, heating at a temperature equal to or higher than the glass transition temperature of the fiber is effective as a method for increasing the adhesion of the applied fiber to the conductive layer.

[0057] The temperature to which the spun fibers are heated is usually in the range of 70 to 300°C, preferably 80 to 250°C, and more preferably 90 to 200°C.

[0058] The method for heating the spun fiber is not particularly limited as long as it can be heated at the above-mentioned heating temperature, and the fiber can be appropriately heated by a method known per se or a method equivalent thereto. Specific examples of the heating method include a method using a hot plate or an oven under air.

[0059] The time for heating the spun fiber can be appropriately set depending on the heating temperature, etc., but from the viewpoints of crosslinking reaction rate and production efficiency, it is preferably 1 minute to 48 hours, more preferably 5 minutes to 36 hours, and particularly preferably 10 minutes to 24 hours.

[0060] The fibers of the present invention have photosensitivity. Therefore, they can be used to prepare etching mask materials for processing semiconductor materials (e.g., substrates, etc.), medical materials, cosmetic materials, etc. In particular, nanofibers and microfibers can be suitably used to prepare etching masks with fine holes, cell culture substrates with patterns (biomimetic substrates, for example, substrates for co-culture with vascular cells, etc., to prevent deterioration of cultured cells, etc.), etc.

[0061] 2. Method for manufacturing photosensitive fiber pattern and substrate having photosensitive fiber pattern Since the fiber of the present invention has photosensitivity, a fiber layer is formed by assembling the fibers, and the fiber layer is directly subjected to lithography treatment, whereby the fibers in the exposed areas are solubilized and removed, and a fiber pattern is formed in which the unexposed areas remain, because the fiber of the present invention is a positive photosensitive fiber. By subjecting a fiber layer of nanofibers and / or microfibers to lithography treatment, it is possible to form a complex and fine fiber pattern.

[0062] The fibers in the fiber layer are assembled in a one-dimensional, two-dimensional, or three-dimensional state, and the assembly state may or may not have regularity. In addition, the "pattern" in the present invention refers to a shape that is recognized as a spatial object such as a design or a motif, which is mainly composed of straight lines, curves, and combinations of these. In addition, the pattern may have any shape, and the pattern itself may or may not have regularity.

[0063] The present invention provides a method for forming a photosensitive fiber pattern, comprising a first step of spinning the photosensitive fiber manufacturing composition on a substrate to form a fiber layer composed of photosensitive fibers (preferably the fibers of the present invention), a second step of exposing the fiber layer through a mask, and a third step of developing the fiber layer with a developer to form a photosensitive fiber pattern. This method can also be called a method for producing a fiber pattern. In addition, since this method can produce a substrate with a fiber pattern, this method can also be called a method for producing a substrate with a fiber pattern.

[0064] [1st step] The first step is a step of spinning the composition for producing a photosensitive fiber on a substrate to form a fiber layer made of a photosensitive fiber (preferably the fiber of the present invention). The method for forming a fiber layer made of photosensitive fibers (preferably the fibers of the present invention) on a substrate is not particularly limited, and for example, the composition of the present invention may be spun directly onto a substrate to form a fiber layer.

[0065] The substrate is not particularly limited as long as it is made of a material that does not deform or denature during lithography processing. For example, resin, glass, ceramics, plastic, semiconductors such as silicon, films, sheets, plates, fabrics (woven fabrics, knitted fabrics, nonwoven fabrics), threads, etc. can be used. Resins as the material of the substrate may be either natural or synthetic resins. Natural resins include cellulose, cellulose triacetate (CTA), cellulose immobilized with dextran sulfate, and synthetic resins include polyacrylonitrile (PAN), polyester polymer alloy (PEPA), polystyrene (PS), polysulfone (PSF), polymethyl methacrylate (PMMA), polyvinyl alcohol (PVA), polyurethane (PU), ethylene vinyl alcohol (EVAL), polyethylene (PE), polyester (PE) (e.g., polyethylene terephthalate (PET)), polypropylene (PP), polyvinylidene fluoride (PVDF), various ion exchange resins, and polyethersulfone (PES), but polyester (PE) is preferred in order to have the repeated bending property (bending resistance) described later, and among polyesters (PE), polyethylene terephthalate (PET) is particularly preferred.

[0066] The basis weight (amount supported per unit area on the substrate) of the fibers in the fiber layer after pattern formation is not particularly limited, but may be, for example, an amount sufficient to form a fiber layer with a thickness of about 5 μm to 50 μm.

[0067] [Second process] The second step is a step of exposing the fiber formed on the substrate in the first step through a mask. The exposure can be performed by, for example, g-line (wavelength 436 nm), h-line (wavelength 405 nm), i-line (wavelength 365 nm), a mercury lamp, various lasers (e.g., excimer lasers such as KrF excimer laser (wavelength 248 nm), ArF excimer laser (wavelength 193 nm), and F2 excimer laser (wavelength 157 nm)), EUV (extreme ultraviolet, wavelength 13 nm), LED, etc.

[0068] After the photosensitive fiber is exposed to light, the fiber may be baked (Post Exposure Bake: PEB) as necessary. The heating temperature can be appropriately set depending on the heating time, etc., but is usually 80 to 200° C. The heating time can be appropriately set depending on the heating temperature, etc., but is usually 1 to 20 minutes.

[0069] [3rd step] The third step is a step of developing the fiber exposed in the second step and heated as necessary with a developer. The developer may be a developer that is normally used for pattern formation of a photosensitive composition. The developer used in the third step more preferably contains water or an organic solvent.

[0070] The water may be water alone or various alkaline aqueous solutions (e.g., aqueous solutions of alkalis such as inorganic alkalis such as sodium hydroxide, potassium hydroxide, sodium carbonate, sodium silicate, sodium metasilicate, and ammonia water; primary amines such as ethylamine and N-propylamine; secondary amines such as diethylamine and di-N-butylamine; tertiary amines such as triethylamine and methyldiethylamine; alcohol amines such as dimethylethanolamine and triethanolamine; quaternary ammonium salts such as tetramethylammonium hydroxide, tetraethylammonium hydroxide, and choline; and cyclic amines such as pyrrole and piperidine).

[0071] Examples of the organic solvent include alcohols (e.g., 1-butanol, 2-butanol, isobutyl alcohol, tert-butyl alcohol, 1-pentanol, 2-pentanol, 3-pentanol, 1-heptanol, 2-heptanol, tert-amyl alcohol, neopentyl alcohol, 2-methyl-1-propanol, 2-methyl-1-butanol, 2-methyl-2-butanol, 3-methyl-1-butanol, 3-methyl-3-pentanol, cyclopentanol, 1-hexanol, 2 ... Sanol, 3-hexanol, 2,3-dimethyl-2-butanol, 3,3-dimethyl-1-butanol, 3,3-dimethyl-2-butanol, 2-diethyl-1-butanol, 2-methyl-1-pentanol, 2-methyl-2-pentanol, 2-methyl-3-pentanol, 3-methyl-1-pentanol, 3-methyl-2-pentanol, 3-methyl-3-pentanol, 4-methyl-1-pentanol, 4-methyl-2-pentanol, 4-methyl-3-pentanol, 1-butoxy-2-propanol and cyclohexanol, etc.) and solvents used in ordinary resist compositions and the like (e.g., ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, methyl cellosolve acetate, ethyl cellosolve acetate, diethylene glycol monomethyl ether, diethylene glycol monoethyl ether, propylene glycol, propylene glycol monomethyl ether, propylene glycol monomethyl ether acetate, propylene glycol propyl ether acetate, toluene, xylene, methyl ethyl ketone, cyclopentanone, cyclohexanone, ethyl 2-hydroxypropionate, ethyl 2-hydroxy-2-methylpropionate, ethyl ethoxyacetate, ethyl hydroxyacetate, methyl 2-hydroxy-3-methylbutanoate, methyl 3-methoxypropionate, ethyl 3-methoxypropionate, ethyl 3-ethoxypropionate, methyl 3-ethoxypropionate, methyl pyruvate, ethyl pyruvate, ethyl acetate, butyl acetate, ethyl lactate, butyl lactate, etc.).

[0072] The developer used in the third step is preferably water, an aqueous solution of ethyl lactate or tetramethylammonium hydroxide, particularly preferably water or ethyl lactate. The pH of the developer is preferably near neutral or basic, and the developer may contain additives such as a surfactant.

[0073] The photosensitive fiber pattern of the present invention formed on a substrate through the above-mentioned steps may be used together with the substrate or may be used separately from the substrate.

[0074] When the photosensitive fiber pattern of the present invention is used together with a substrate, the substrate (i.e., a substrate having the photosensitive fiber pattern of the present invention on its surface) can be suitably used as an etching mask used in processing substrates such as semiconductors, a cell culture scaffold material, etc., so long as the photosensitive fiber pattern of the present invention is formed of nanofibers and / or microfibers. When the substrate having the photosensitive fiber pattern of the present invention on its surface is used as a cell culture scaffold material, the substrate is preferably glass or plastic.

[0075] 3. Method for manufacturing metal pattern and substrate with metal pattern The present invention can provide a method for producing a metal pattern, comprising: a first step of forming a fiber layer consisting of photosensitive fibers (preferably the fibers of the present invention) on a substrate having a metal layer on its surface; a second step of exposing the fiber layer through a mask; a third step of developing the fiber layer with a developer to form a photosensitive fiber pattern; and a fourth step of etching the metal layer with an etching solution, further removing the photosensitive fibers, and forming a metal pattern.

[0076] The difference between the first step of the method for producing a metal pattern and the first step of the method for producing a photosensitive fiber pattern is the part having a metal layer on the surface of the substrate.

[0077] [1st step] The first step is a step of forming a fiber layer made of photosensitive fibers on a substrate having a metal layer on its surface. The metal may be cobalt, nickel, copper, zinc, chromium, molybdenum, ruthenium, rhodium, palladium, silver, cadmium, osmium, titanium, iridium, platinum, gold, aluminum, or an alloy of these metals, but the metal pattern of the present invention is not limited to these and can be applied to any conductive metal. In providing a transparent conductive film using the metal pattern of the present invention, copper, silver, and aluminum are preferred from the viewpoint of conductivity, and in providing a flexible transparent electrode (transparent conductive film), metals such as aluminum and copper or alloys are preferred, and aluminum is more preferred from the viewpoint of light weight and low cost.

[0078] [Second process] The second step is a step of exposing the fibers formed on the substrate having a metal layer on its surface in the first step to light through a mask. Regarding the light to be exposed and the heating of the fiber after exposure in the second step, please refer to the contents described in the second step of "2" above.

[0079] [3rd step] The third step is a step of developing the fibers that have been exposed and, if necessary, heated in the second step, with a developer. Regarding the developer used in the third step, the contents described in the third step of "2" above can be referred to.

[0080] [4th step] The fourth step is a step of etching the metal layer corresponding to the fiber layer portion developed in the third step with an etching solution, and further removing the photosensitive fiber to form a metal pattern. Regarding etching, the method of removing the metal layer area not covered with fibers depends on the characteristics of the metal forming the metal layer, but examples of the method include a wet method in which the metal is immersed in an acidic aqueous solution such as hydrochloric acid or nitric acid, or an aqueous solution of sodium hydroxide or potassium hydroxide, and the metal is dissolved in the aqueous solution by ionizing or complex ionizing. The immersion time and temperature can be appropriately selected depending on the type and concentration of the aqueous solution used and the type and thickness of the metal layer to be dissolved, and can be replaced by a dry method using an organic gas or a halogen gas, if necessary. After removing the metal layer area not covered with the photosensitive fiber, it is preferable to thoroughly wash the substrate including the metal pattern covered with the photosensitive fiber with water or the like in order to remove impurities such as compounds in which the metal is ionized or complexed and solutes contained in the aqueous solution. Then, the photosensitive fiber covering the metal pattern is removed. The photosensitive fiber can usually be completely removed with an organic solvent. For example, it can be removed with acetone. This makes it possible to form a metal pattern consisting of a fine metal mesh structure, that is, a mesh-like metal pattern, or a wiring pattern using a mesh-like metal pattern as wiring, on the substrate.

[0081] After the photosensitive fiber is removed, the light transmittance of the mesh metal pattern in the visible light wavelength range is, for example, 5% or more, for example, 8% or more, for example, 10% or more, for example, 15% or more, for example, 20% or more, for example, 30% or more, for example, 40% or more, for example, 50% or more, for example, 60% or more.

[0082] The metal pattern of the present invention formed on a substrate through the above steps can be used together with the substrate or can be used separately from the substrate. When used together with the substrate, the substrate becomes a substrate with a metal pattern.

[0083] <Repeated bending resistance (flexibility)> The metal pattern of the present application and the substrate with the metal pattern have resistance to repeated bending. Specifically, as described in the examples, even if bending with a bending radius of 2 mm is performed, for example, 2 or more times, 5 or more times, 10 or more times, 50 or more times, 100 or more times, or 200 or more times, the change rate of the sheet resistance of the metal pattern is small (for example, the change rate of the sheet resistance compared to before bending is within 10%).

[0084] As an example of the relationship between the light transmittance, sheet resistance value, and fiber coating rate, the following combinations can be mentioned, but are not limited thereto. When the light transmittance of the above-mentioned mesh-shaped metal pattern in the visible light wavelength region is 5 to 11%, the sheet resistance value is 5 to 9 Ω / □, and the fiber coating rate is 75% to 90%. When the light transmittance of the above-mentioned mesh-shaped metal pattern in the visible light wavelength region is 12% or more (for example, 15% or more, for example, 20% or more, for example, 30% or more, for example, 40% or more, for example, 50% or more, for example, 60% or more), the sheet resistance value is 10 to 500 Ω / □, and the fiber coating rate is 1 to 70%.

Examples

[0085] Hereinafter, specific examples according to the present invention will be described, but the present invention is not limited thereby.

[0086] [Measurement of weight average molecular weight] In this example, the weight average molecular weight of the polymer was measured by gel permeation chromatography (GPC). The apparatus and measurement conditions used for the measurement are as follows. Apparatus: TOSOH HLC-8320GPC system Columns: Shodex (registered trademark) KF-803L, KF-802, and KF-801 Column temperature: 40 °C Eluent: DMF Flow rate: 0.6 ml / min Detector: RI Standard sample: Polystyrene

[0087] 「Example 1」 <a. Production of copolymer> 10 g of benzyl acrylate and 1.12 g of acrylic acid were dissolved in 50 ml of tetrahydrofuran, and nitrogen bubbling was carried out for 10 minutes. Subsequently, 0.018 g of 2,2'-azobis(isobutyric acid) dimethyl was added as a polymerization initiator, and polymerization was carried out at 70 °C under a nitrogen atmosphere by heating to reflux for 6 hours. After polymerization, the solution was poured into 1 L of n-hexane to precipitate the polymer, which was then separated by filtration and dried to obtain a white polymer. The structure of the obtained polymer was found to be a polymer with a molar fraction of benzyl acrylate structure of 80% and a molar fraction of acrylic acid structure of 20% from various analytical methods. When the molecular weight of this polymer in terms of polystyrene was examined by gel permeation chromatography (GPC) in tetrahydrofuran, the weight average molecular weight (Mw) was 25,900.

[0088] <b. Preparation of Composition for Manufacturing Photosensitive Fiber> 10 g of the above copolymer, 3 g of a dissolution inhibitor (naphthoquinonediazosulfonic acid ester compound), and 0.1 g of an electrolyte (tetrabutylammonium chloride) were dissolved in 40 g of an organic solvent (hexafluoroisopropanol) to prepare a positive-type composition for manufacturing photosensitive fiber. Also, when the glass transition temperature of the solid component after drying and removing the solvent component from this composition was examined by a differential scanning calorimeter (DSC), the glass transition temperature was 28.5 °C.

[0089] <c. Method for Manufacturing Fiber by Electrospinning Method> In this example, the manufacturing of fiber by the electrospinning method was carried out using an electrosprayer ES-2000 (manufactured by Fluence Co., Ltd.). The composition for manufacturing fiber was injected into a 1-ml lock-type glass syringe (manufactured by AS ONE Corporation), and a 24G lock-type metal needle with a needle length of 13 mm (manufactured by Musashi Engineering, Inc.) was attached. The distance from the needle tip to the substrate for receiving the fiber (discharge distance) was 10 cm, the applied voltage was 5 kV, the discharge rate was 10 μl / min, and the discharge time was 5 seconds. Also, the temperature in the laboratory during electrospinning was 23 °C.

[0090] <d. Patterning of Photosensitive Fiber> A composition for manufacturing photosensitive fibers was electrospun onto the aluminum vapor-deposited film surface of a static aluminum vapor-deposited PET film (PET film thickness: 12 μm, aluminum vapor-deposited film thickness: 50 nm) to form a fiber layer composed of intertwined fibers with a diameter of approximately 300 nm. At this time, the coverage rate (the ratio of the aluminum vapor-deposited PET film covered by the fibers of the fiber layer) was approximately 40%. Subsequently, heating was performed in an oven at 40 °C for 5 minutes to remove the residual solvent in the fiber layer and to adhere the fiber layer to the aluminum vapor-deposited PET film by utilizing the thermal sag of the fibers. Next, using an ultra-high-pressure mercury lamp as a light source, the fiber layer was contact-exposed through a photomask on which a circuit pattern including a wiring pattern with a minimum line width of 50 μm was drawn. The exposure wavelength was broad-band exposure from 350 nm to 450 nm, and the exposure dose was measured at the i-line wavelength and was 2 set to 1000 mJ / cm

[0091] <e. Etching of the aluminum vapor-deposited PET film> The aluminum vapor-deposited PET film on which the fiber layer with the above-mentioned wiring pattern with a line width of 50 μm was formed was immersed in an aluminum etchant Pure Etch AS1 (phosphoric acid-nitric acid-acetic acid type, manufactured by Hayashi Junyaku Kogyo Co., Ltd.), and wet etching of aluminum was performed using the fiber layer as an etching mask (25 °C, 5 minutes). Then, when the fiber layer was completely removed with an organic solvent (acetone), a circuit pattern including a wiring pattern with a minimum line width of 50 μm composed of a fine aluminum network structure with a line width of approximately 300 nm could be formed on the PET film.

[0092] <f. Electrical, optical, and mechanical properties of the wiring pattern) The electrical properties of the circuit pattern portion composed of a fine aluminum network structure with a line width of about 300 nm were measured by the four-terminal resistance measurement method. As a result, it was confirmed that conductivity was exhibited, and the sheet resistance was about 10 Ω / □. At this time, no anisotropy in conductivity was observed. Next, the optical properties were measured and observed by an ultraviolet-visible spectrophotometer and visually. As a result, the network pattern portion of the wiring pattern formed by the network-shaped metal pattern showed a light transmittance of about 60% in the wavelength region of visible light from 380 nm to 780 nm, and it was confirmed that it was also transparent visually. Next, a bending test with a bending radius of 2 mm was performed. Even after 100 bends, no change was observed in the sheet resistance, and high conductivity could be maintained.

[0093] "Example 2" <a. Production of copolymer> 10 g of 4-hydroxyphenyl methacrylate, 20.04 g of benzyl acrylate, and 7.92 g of benzyl methacrylate were dissolved in 120 ml of tetrahydrofuran, and nitrogen bubbling was performed for 10 minutes. Subsequently, 0.26 g of 2,2'-azobis(isobutyric acid) dimethyl was added as a polymerization initiator, and polymerization was carried out at 70 °C under a nitrogen atmosphere with reflux by heating for 6 hours. After polymerization, the solution was poured into 2 l of n-hexane to precipitate the polymer, which was then filtered off and dried to obtain a white polymer. The structure of the obtained polymer was found to be a polymer with a molar fraction of 4-hydroxyphenyl methacrylate structure of 25%, a molar fraction of benzyl acrylate structure of 55%, and a molar fraction of benzyl methacrylate structure of 20% from various analytical methods. When the molecular weight of this polymer in terms of polystyrene was examined by gel permeation chromatography (GPC) in tetrahydrofuran, the weight average molecular weight (Mw) was 31,000.

[0094] <b. Preparation of photosensitive fiber production composition> 10 g of the above copolymer, 3 g of a dissolution inhibitor (naphthoquinonediazosulfonic acid ester compound), and 0.5 g of an electrolyte (tetrabutylammonium chloride) were dissolved in 90 g of an organic solvent (hexafluoroisopropanol) to prepare a positive-type photosensitive fiber manufacturing composition. Further, when the glass transition temperature of the solid component after drying and removing the solvent component from this composition was examined using a differential scanning calorimeter (DSC), the glass transition temperature was 85.6 °C.

[0095] <c. Method for manufacturing fibers by electrospinning method> In this example, the manufacturing of fibers by the electrospinning method was carried out using an electrosprayer ES-2000 (manufactured by Fluence Co., Ltd.). The fiber manufacturing composition was injected into a 1-ml lock-type glass syringe (manufactured by AS ONE Corporation), and a lock-type metal needle 24G with a needle length of 13 mm (manufactured by Musashi Engineering Co., Ltd.) was attached. The distance from the needle tip to the substrate for receiving the fibers (discharge distance) was 20 cm, the applied voltage was 5 kV, the discharge speed was 10 μl / min, and the discharge time was 5 seconds. Also, the temperature in the laboratory during electrospinning was 23 °C.

[0096] <d. Patterning of photosensitive fibers> The photosensitive fiber manufacturing composition was electrospun onto the aluminum vapor-deposited film surface of a static aluminum vapor-deposited PET film (PET film thickness: 12 μm, aluminum vapor-deposited film thickness: 50 nm) to form a fiber layer composed of intertwined fibers with a diameter of approximately 500 nm. At this time, the coverage rate (the ratio of the aluminum vapor-deposited PET film covered by the fibers of the fiber layer) was approximately 20%. Next, heating was performed in an oven at 90 °C for 5 minutes to remove the residual solvent in the fiber layer and to adhere the fiber layer to the aluminum vapor-deposited PET film using the heat sag of the fibers. Next, using an ultra-high pressure mercury lamp as a light source, the fiber layer was contact-exposed through a photomask on which a circuit pattern including a wiring pattern with a minimum line width of 50 μm was drawn. The exposure wavelength was broad-band exposure from 350 nm to 450 nm, and the exposure amount was measured at the i-line wavelength and was 280 mJ / cm 2It was set as such. After the fiber layer was exposed, it was exposed to a developer (an alkaline aqueous solution containing a metal corrosion inhibitor (3.3% tetramethylammonium hydroxide)) for 2 minutes, and then rinsed with pure water for 5 minutes. Thereafter, it was dried by heating in an oven at 40 °C for 5 minutes, and a fiber layer having a wiring pattern with a line width of 50 μm was obtained on the aluminum vapor-deposited PET film.

[0097] <e. Etching of Aluminum Vapor-Deposited PET Film> The aluminum vapor-deposited PET film on which the fiber layer having the above wiring pattern with a line width of 50 μm was formed was immersed in an aluminum etchant Pure Etch AS1 (phosphoric acid-nitric acid-acetic acid type, manufactured by Hayashi Junyaku Kogyo Co., Ltd.), and wet etching of aluminum was performed using the fiber layer as an etching mask (25 °C, 1 minute). Thereafter, when the fiber layer was completely removed with an organic solvent (acetone), a circuit pattern including a wiring pattern with a minimum line width of 50 μm composed of a fine aluminum network structure with a line width of about 500 nm was formed on the PET film.

[0098] <f. Electrical, Optical, and Mechanical Characteristics of Wiring Pattern) The electrical characteristics of the circuit pattern portion composed of a fine aluminum network structure with a line width of about 500 nm were measured by the four-terminal resistance measurement method. As a result, it was confirmed that it exhibited conductivity, and the sheet resistance was about 20 Ω / □. At this time, no anisotropy in conductivity was observed. Next, the optical characteristics were measured and observed by an ultraviolet-visible spectrophotometer and visually. As a result, the network pattern portion of the wiring pattern formed by the network-shaped metal pattern showed a light transmittance of about 65% in the wavelength region of visible light of 380 nm to 780 nm, and it was confirmed that it was also transparent visually. Next, a bending test with a bending radius of 2 mm was performed. Even after 100 bends, no change was observed in the sheet resistance, and high conductivity could be maintained.

[0099] "Example 3" (when the ratio (coverage rate) of the aluminum vapor-deposited PET film covered by the fibers of the fiber layer is low) <a. Method for Manufacturing Fibers by Electrospinning Method> In this example, the production of fibers by the electrospinning method was carried out using an electrosprayer ES-2000 (manufactured by Fluence Co., Ltd.). The composition for fiber production was injected into a 1-ml lock-type glass syringe (manufactured by AS ONE Corporation), and a 24G lock-type metal needle with a needle length of 13 mm (manufactured by Musashi Engineering Co., Ltd.) was attached. The distance from the needle tip to the substrate for receiving the fibers (discharge distance) was 20 cm, the applied voltage was 5 kV, the discharge speed was 10 μl / min, and the discharge time was 1 second. Also, the temperature in the laboratory during electrospinning was set to 23°C.

[0100] <b. Patterning of photosensitive fibers> In Example 2 The composition for producing photosensitive fibers adjusted as described above was electrospun onto the aluminum vapor-deposited film surface of a static aluminum vapor-deposited PET film (PET film thickness: 12 μm, aluminum vapor-deposited film thickness: 50 nm) to form a fiber layer composed of entangled fibers with a diameter of approximately 500 nm. At this time, the coverage rate (the ratio of the aluminum vapor-deposited PET film covered by the fibers of the fiber layer) was approximately 3%. Subsequently, heating was performed in an oven at 90 °C for 5 minutes to remove the residual solvent in the fiber layer and to adhere the fiber layer to the aluminum vapor-deposited PET film by utilizing the thermal sag of the fibers. Next, using an ultra-high pressure mercury lamp as a light source, the fiber layer was contact-exposed through a photomask on which a circuit pattern including a wiring pattern with a minimum line width of 50 μm was drawn. The exposure wavelength was broad-band exposure from 350 nm to 450 nm, and the exposure dose was measured at the i-line wavelength and set to 280 mJ / cm 2 ². After the exposure of the fiber layer, it was exposed to a developer (an alkaline aqueous solution containing a metal corrosion inhibitor (tetramethylammonium hydroxide 3.3%)) for 2 minutes, and then rinsed with pure water for 5 minutes. Thereafter, it was heated and dried in an oven at 40 °C for 5 minutes to obtain a fiber layer having a wiring pattern with a line width of 50 μm on the aluminum vapor-deposited PET film.

[0101] <c. Etching of Aluminum Vapor-Deposited PET Film> The aluminum vapor-deposited PET film on which the fiber layer having the above-mentioned wiring pattern with a line width of 50 μm was formed was immersed in an aluminum etchant Pure Etch AS1 (phosphoric acid·nitric acid·acetic acid type, manufactured by Hayashi Junyaku Kogyo Co., Ltd.), and wet etching of aluminum was performed using the fiber layer as an etching mask (25 °C, 1 minute). Thereafter, the fiber layer was completely removed with an organic solvent (acetone) to form a circuit pattern including a wiring pattern with a minimum line width of 50 μm composed of a fine aluminum network structure with a line width of approximately 500 nm on the PET film.

[0102] <d. Electrical, Optical, and Mechanical Characteristics of Wiring Pattern) The electrical properties of the circuit pattern portion composed of a fine aluminum network structure with a line width of about 500 nm were measured by the four-terminal resistance measurement method. As a result, it was confirmed that the conductivity was exhibited, and the sheet resistance was about 250 Ω / □. Next, the optical properties were measured and observed by an ultraviolet-visible spectrophotometer and visually. As a result, the mesh-like metal pattern portion of the wiring pattern formed by the mesh-like metal pattern showed a light transmittance of about 87% in the wavelength region of visible light of 380 nm to 780 nm. Next, a bending test with a bending radius of 2 mm was performed. Even after 100 bendings, no change was observed in the sheet resistance, and high conductivity was maintained.

[0103] "Example 4" (when the ratio (coverage rate) of the aluminum-deposited PET film covered by the fibers of the fiber layer is high) <a. Method for manufacturing fibers by electrospinning method> In this example, the production of fibers by the electrospinning method was carried out using an electrosprayer ES-2000 (manufactured by Fluence Co., Ltd.). The fiber production composition was injected into a 1 ml lock-type glass syringe (manufactured by AS ONE Corporation), and a 24G lock-type metal needle with a needle length of 13 mm (manufactured by Musashi Engineering Co., Ltd.) was attached. The distance from the needle tip to the substrate for receiving the fibers (discharge distance) was 20 cm, the applied voltage was 5 kV, the discharge speed was 10 μl / min, and the discharge time was 20 seconds. Also, the temperature in the laboratory during electrospinning was 23 °C. <b. Patterning of photosensitive fibers> of Example 2 The photosensitive fiber manufacturing composition adjusted as described above was electrospun onto the aluminum vapor-deposited film surface of a static aluminum vapor-deposited PET film (PET film thickness: 12 μm, aluminum vapor-deposited film thickness: 50 nm) to form a fiber layer composed of intertwined fibers with a diameter of approximately 500 nm. At this time, the coverage rate (the ratio of the aluminum vapor-deposited PET film covered by the fibers of the fiber layer) was approximately 80%. Next, heating was performed in an oven at 90 °C for 5 minutes to remove the residual solvent in the fiber layer and to adhere the fiber layer to the aluminum vapor-deposited PET film by utilizing the thermal sag of the fibers. Next, using an ultra-high pressure mercury lamp as the light source, the fiber layer was contact-exposed through a photomask on which a circuit pattern including a wiring pattern with a minimum line width of 50 μm was drawn. The exposure wavelength was broad-band exposure from 350 nm to 450 nm, and the exposure dose was measured at the i-line wavelength and was 280 mJ / cm 2 ². After exposure of the fiber layer, it was exposed to a developer (an alkaline aqueous solution containing a metal corrosion inhibitor (tetramethylammonium hydroxide 3.3%)) for 2 minutes and then rinsed with pure water for 5 minutes. Thereafter, it was heated and dried in an oven at 40 °C for 5 minutes to obtain a fiber layer having a wiring pattern with a line width of 50 μm on the aluminum vapor-deposited PET film. <c. Etching of the aluminum vapor-deposited PET film> The aluminum vapor-deposited PET film on which the fiber layer having the above-described wiring pattern with a line width of 50 μm was formed was immersed in an aluminum etchant Pure Etch AS1 (phosphoric acid / nitric acid / acetic acid type, manufactured by Hayashi Junyaku Kogyo Co., Ltd.), and wet etching of aluminum was performed (25 °C, 1 minute) using the fiber layer as an etching mask. Thereafter, when the fiber layer was completely removed with an organic solvent (acetone), a circuit pattern including a wiring pattern with a minimum line width of 50 μm composed of a fine aluminum network structure with a line width of approximately 500 nm was formed on the PET film. <d. Electrical, optical, and mechanical properties of the wiring pattern) The electrical properties of the circuit pattern portion composed of a fine aluminum network structure with a line width of about 500 nm were measured by the four-terminal resistance measurement method. As a result, it was confirmed that conductivity was exhibited, and the sheet resistance was about 8 Ω / □. Next, the optical properties were measured and observed by an ultraviolet-visible spectrophotometer and visually. As a result, the mesh-like metal pattern portion of the wiring pattern formed by the mesh-like metal pattern showed a light transmittance of about 10% in the wavelength region of visible light of 380 nm to 780 nm. Next, a bending test with a bending radius of 2 mm was performed. Even after 100 bends, no change was observed in the sheet resistance, and high conductivity was maintained.

[0104] "Example 5" (when the fiber diameter is thick) <a. Preparation of Composition for Producing Photosensitive Fiber> of Example 2 10 g of the copolymer synthesized, 3 g of a dissolution inhibitor (naphthoquinonediazosulfonic acid ester compound), and 0.5 g of an electrolyte (tetrabutylammonium chloride) were dissolved in 40 g of an organic solvent (hexafluoroisopropanol) to prepare a positive-type photosensitive fiber manufacturing composition.

[0105] <b. Method for manufacturing fibers by electrospinning method> In this example, the manufacturing of fibers by the electrospinning method was carried out using an electrosprayer ES-2000 (manufactured by Fluence Co., Ltd.). The fiber manufacturing composition was injected into a 1 ml lock-type glass syringe (manufactured by AS ONE Corporation), and a lock-type metal needle 24G with a needle length of 13 mm (manufactured by Musashi Engineering Co., Ltd.) was attached. The distance from the needle tip to the substrate for receiving the fibers (discharge distance) was 20 cm, the applied voltage was 5 kV, the discharge speed was 10 μl / min, and the discharge time was 5 seconds. Also, the temperature in the laboratory during electrospinning was 23°C.

[0106] <c. Patterning of photosensitive fibers> The photosensitive fiber manufacturing composition was electrospun onto the aluminum vapor-deposited film surface of a static aluminum vapor-deposited PET film (PET film thickness 12 μm, aluminum vapor-deposited film thickness 50 nm) to form a fiber layer composed of intertwined fibers with a diameter of approximately 2 μm. At this time, the coverage rate (the ratio of the aluminum vapor-deposited PET film covered by the fibers of the fiber layer) was approximately 20%. Next, heating was performed in an oven at 90°C for 5 minutes to remove the residual solvent in the fiber layer and to adhere the fiber layer to the aluminum vapor-deposited PET film by utilizing the thermal sag of the fibers. Next, using an ultra-high pressure mercury lamp as a light source, the fiber layer was contact-exposed through a photomask on which a circuit pattern including a wiring pattern with a minimum line width of 50 μm was drawn. The exposure wavelength was broad-band exposure from 350 nm to 450 nm, and the exposure dose was measured at the i-line wavelength and was 280 mJ / cm 2 It was set as such. After the exposure of the fiber layer, it was exposed to a developer (an alkaline aqueous solution containing a metal corrosion inhibitor (3.3% tetramethylammonium hydroxide)) for 2 minutes, and then rinsed with pure water for 5 minutes. Thereafter, it was heated in an oven at 40 °C for 5 minutes to dry, and a fiber layer having a wiring pattern with a line width of 50 μm was obtained on the aluminum-deposited PET film.

[0107] <d. Etching of Aluminum-Deposited PET Film> The aluminum-deposited PET film on which the fiber layer having the above wiring pattern with a line width of 50 μm was formed was immersed in an aluminum etchant Pure Etch AS1 (phosphoric acid-nitric acid-acetic acid type, manufactured by Hayashi Junyaku Kogyo Co., Ltd.), and wet etching of aluminum was performed using the fiber layer as an etching mask (25 °C, 1 minute). Thereafter, when the fiber layer was completely removed with an organic solvent (acetone), a circuit pattern including a wiring pattern with a minimum line width of 50 μm composed of a mesh-like network structure of aluminum with a line width of about 2 μm could be formed on the PET film.

[0108] <e. Electrical, Optical, and Mechanical Characteristics of Wiring Pattern) The electrical characteristics of the circuit pattern portion composed of the mesh-like network structure of aluminum with a line width of about 2 μm were measured by the four-terminal resistance measurement method. As a result, it was confirmed that it exhibited conductivity, and the sheet resistance was about 25 Ω / □. Next, the optical characteristics were measured and observed by an ultraviolet-visible spectrophotometer and visually. As a result, the mesh-like metal pattern portion of the wiring pattern formed by the mesh-like metal pattern showed a light transmittance of about 60% in the wavelength region of visible light from 380 nm to 780 nm. It was also confirmed visually that it was transparent. Next, a bending test with a bending radius of 2 mm was performed. Even after 100 bends, no change was observed in the sheet resistance, and high conductivity was maintained.

[0109] 「Comparative Example 1」(Flexural Resistance of ITO Film) <Electrical, Optical, and Mechanical Characteristics of ITO Transparent Conductive Film> The electrical properties of the ITO transparent conductive film (ITO film thickness approximately 75 nm) formed on the PET film were measured using a four-terminal resistance measurement method. As a result, the sheet resistance was approximately 100 Ω / □. At this time, no anisotropy in the conductivity was observed. Next, the optical properties were measured and observed using a UV-Visible spectrophotometer and visually. As a result, a light transmittance of approximately 78% was observed in the visible light wavelength range of 550 nm, and it was confirmed to be transparent by visual observation. Next, a bending test was performed with a bending radius of 2 mm. After one bending, the sheet resistance increased to approximately 4 kΩ / □, and a significant decrease in conductivity was observed.

Claims

1. A photosensitive fiber made of a positive-type photosensitive material, the positive-type photosensitive material containing a (meth)acrylic resin, a dissolution inhibitor and an electrolyte, and the (meth)acrylic resin containing benzyl (meth)acrylate.

2. A composition for producing a photosensitive fiber made of a positive-type photosensitive material, comprising: The composition comprises a (meth)acrylic resin, a dissolution inhibitor, an electrolyte, and a solvent, wherein the (meth)acrylic resin comprises benzyl (meth)acrylate.

3. A method for producing a photosensitive fiber comprising the step of spinning the composition of claim 2.

4. A first step of spinning the composition according to claim 2 on a substrate to form a fiber layer comprising photosensitive fibers; A second step of exposing the fiber layer to light through a mask; and The fiber layer is developed with a developer to form a photosensitive fiber pattern. A method for producing a photosensitive fiber pattern comprising:

5. A first step of forming a fiber layer made of a photosensitive fiber on a substrate having a metal layer on its surface; A second step of exposing the fiber layer to light through a mask; A third step of developing the fiber layer with a developer to form a photosensitive fiber pattern; and A fourth step of etching the metal layer with an etching solution to further remove the photosensitive fibers and form a mesh-like metal pattern. A method for producing a metal pattern, comprising: the photosensitive fiber is made of a positive photosensitive material, The positive-type photosensitive material contains a (meth)acrylic resin, a dissolution inhibitor, and an electrolyte, The (meth)acrylic resin contains benzyl (meth)acrylate. Manufacturing method.

6. The method for producing a metal pattern according to claim 5 , wherein the mesh-like metal pattern has a light transmittance of 5% or more in the visible light wavelength region.

7. 7. The method for producing a metal pattern according to claim 5, wherein the metal pattern can be bent 10 or more times in a repeated bending test while maintaining electrical conductivity.

8. A first step of forming a fiber layer made of a photosensitive fiber on a substrate having a metal layer on its surface; A second step of exposing the fiber layer to light through a mask; A third step of developing the fiber layer with a developer to form a photosensitive fiber pattern; and A fourth step of etching the metal layer with an etching solution to further remove the photosensitive fibers and form a mesh-like metal pattern. A method for producing a substrate having a metal pattern, comprising: the photosensitive fiber is made of a positive photosensitive material, The positive-type photosensitive material contains a (meth)acrylic resin, a dissolution inhibitor and an electrolyte, and the (meth)acrylic resin contains benzyl (meth)acrylate.

9. A substrate having a metal pattern, produced by the method for producing a substrate having a metal pattern according to claim 8.

10. The substrate having a metal pattern according to claim 9 , wherein the mesh-like metal pattern has a light transmittance of 5% or more in the visible light wavelength region.

11. The substrate with a metal pattern according to claim 9 or 10, which can be bent 10 or more times while maintaining electrical conductivity in a repeated bending test.

Citation Information

Patent Citations

  • Positive type photosensitive resin composition

    JP2001281853A

  • Pattern forming method

    JP2011248147A

  • Method of manufacturing patterned conductor

    JP2017098237A

  • Method for manufacturing dry film photoresist and dry film photoresist manufactured by the same

    KR1020150043997A

  • Photosensitive fiber and method for manufacturing same

    WO2015056789A1