Austenitic stainless steel sheet and exhaust part using same

The austenitic stainless steel sheet with a controlled composition and manufacturing process addresses the challenge of high-temperature slidability and workability in turbocharger parts by forming a self-lubricating oxide scale, enhancing performance and processing efficiency.

JP7564656B2Active Publication Date: 2024-10-09NIPPON STEEL CORPORATION
View PDF 12 Cites 0 Cited by

Patent Information

Application Number
JP2020121415
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-07-15
Publication Date
2024-10-09
Estimated Expiration
2040-07-15

AI Technical Summary

Technical Problem

Austenitic stainless steel sheets used for turbocharger parts face challenges in achieving both high-temperature slidability and workability, with existing compositions exhibiting poor friction and wear resistance in high-temperature, non-lubricated environments, leading to potential adhesion and opening/closing issues.

Method used

Austenitic stainless steel with a controlled chemical composition, including specific ranges of elements such as Si, REM, and optimized manufacturing processes to form a self-lubricating oxide scale, ensuring good high-temperature slidability and workability, with a punching index of 0.2% or less and oxide scale roughness of 0.10 μm or less.

Benefits of technology

The solution provides an austenitic stainless steel sheet with improved high-temperature slidability and workability, suitable for turbocharger parts, reducing wear and improving processing efficiency while maintaining corrosion resistance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007564656000005
    Figure 0007564656000005
  • Figure 0007564656000006
    Figure 0007564656000006
  • Figure 0007564656000007
    Figure 0007564656000007
Patent Text Reader

Abstract

To provide an austenitic stainless steel sheet that has good high-temperature slidability and fabricability.SOLUTION: Provided is an austenitic stainless steel sheet that has a chemical composition, in mass%, of: C:0.005 to 0.30%, Si:0.010% or more and less than 3.00%, Mn:0.1 to 5.0%, P:0.010 to 0.050%, S:0.0001 to 0.010%, Ni:5.00 to 15.00%, Cr:15.00 to 30.00%, N:0.02 to 0.40%, Al:0.001 to 0.50%, REM:0.005 to 0.100%, optional elements, balance: Fe and impurities, and a die-stamping fabricability index of 0.2% or less.SELECTED DRAWING: Figure 2
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an austenitic stainless steel sheet and an exhaust part using the same. [Background technology]

[0002] An automobile is made up of a wide variety of parts, among which exhaust parts are required to stably ventilate high-temperature and corrosive exhaust gases, and therefore are required to be heat-resistant and corrosion-resistant.

[0003] Therefore, austenitic stainless steels, which have relatively good heat resistance and corrosion resistance, are sometimes used for exhaust parts. For example, Patent Documents 1 to 5 and Non-Patent Documents 1 and 2 disclose austenitic stainless steel sheets intended for use in exhaust parts. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] International Publication No. 2014 / 157655 [Patent Document 2] JP 2017-14538 A [Patent Document 3] JP 2017-160493 A [Patent Document 4] JP 2017-88928 A [Patent Document 5] JP 2019-143186 A [Non-patent literature]

[0005] [Non-Patent Document 1] Yushi Osako et al., Development of High Performance and High Reliability VG Turbocharger for Automobiles, Mitsubishi Heavy Industries Technical Review, 2006, Vol. 43, p. 31. [Non-Patent Document 2] Tomohiro Inoue et al., Development of RHV4 variable displacement (STEP4) turbocharger, IHI Technical Report, 2011, Vol. 51, p. 48. Summary of the Invention [Problem to be solved by the invention]

[0006] Incidentally, there are various types of exhaust parts, one example of which is turbocharger parts. Turbochargers are superchargers that are installed in automobiles in recent years based on the idea of ​​downsizing, which aims to improve fuel efficiency by reducing the weight of the vehicle body. Turbocharger parts can have complex shapes. For this reason, the austenitic stainless steel sheets used for these parts are required to have not only heat resistance but also good workability.

[0007] In addition, some turbocharger parts are used in a high-temperature, non-lubricated environment where friction occurs repeatedly. In this case, it is possible that parts in contact with each other will wear out and adhere to each other in the operating environment. As a result, for example, vanes and valves for adjusting the flow rate of exhaust gas inside the turbocharger may have problems opening and closing, resulting in poor gas flow. Therefore, turbocharger parts are also required to have high-temperature sliding properties, which are friction and wear resistance properties at high temperatures.

[0008] However, in austenitic stainless steel sheets having improved heat resistance, it is difficult to achieve both high-temperature sliding properties and workability at the same time.

[0009] Specifically, the austenitic stainless steel sheets disclosed in Patent Documents 1 and 2 have not been examined for high-temperature sliding properties, and there is room for further improvement in high-temperature sliding properties. Similarly, the high-temperature sliding properties of the austenitic stainless steel sheet disclosed in Patent Document 3 have not been fully examined. Although Patent Document 4 examines high-temperature sliding properties, there is room for further improvement in the high-temperature sliding properties of the austenitic stainless steel sheet disclosed in this document.

[0010] The austenitic stainless steel sheet disclosed in Patent Document 5 is thought to have a high Si content and poor workability. In addition, it is thought that the high-temperature sliding properties may be deteriorated under certain conditions. The austenitic stainless steel sheets disclosed in Non-Patent Documents 1 and 2 have good high-temperature sliding properties, but are thought to have a high Si content and poor workability.

[0011] In view of the above, an object of the present invention is to solve the above problems and to provide an austenitic stainless steel sheet having good high-temperature sliding properties and workability. [Means for solving the problem]

[0012] The present invention has been made to solve the above problems, and the gist of the present invention is the following austenitic stainless steel sheet.

[0013] (1) Chemical composition, in mass%, C: 0.005-0.30%, Si: 0.010% or more and less than 3.00% Mn: 0.1-5.0%, P: 0.010~0.050%, S: 0.0001 to 0.010%, Ni: 5.00~15.00%, Cr: 15.00~30.00%, N: 0.02-0.40%, Al: 0.001 to 0.50%, REM: 0.005~0.100%, Cu: 0-4.0%, Mo: 0-2.0%, V: 0~1.0%, Ti: 0 to 0.30%, Nb: 0-0.30%, B: 0~0.0050%, Ca: 0 to 0.010%, W: 0-3.0%, Zr: 0-0.30%, Sn: 0-0.50%, Co: 0-0.30%, Mg: 0 to 0.010%, Sb: 0-0.50%, Ga: 0 to 0.30%, Ta: 0 to 1.0%, Hf: 0-1.0%, Bi: 0 to 0.020%, The balance is Fe and impurities. An austenitic stainless steel sheet having a punching index of 0.2% or less.

[0014] (2) The chemical composition is, in mass%, Cu: 0.1-4.0%, Mo: 0.1-2.0%, V: 0.05-1.0%, Ti: 0.005 to 0.30%, Nb: 0.005-0.30%, B: 0.0002~0.0050%, Ca: 0.0003~0.010%, W: 0.1-3.0%, Zr: 0.05-0.30%, Sn: 0.01 to 0.50%, Co: 0.03 to 0.30%, Mg: 0.0002~0.010%, Sb: 0.005 to 0.50%, Ga: 0.0002 to 0.30%, Ta: 0.001 to 1.0%, Hf: 0.001 to 1.0%, and Bi: 0.001 to 0.020%, Contains one or more selected from The austenitic stainless steel sheet according to (1) above.

[0015] (3) An austenitic stainless steel sheet according to (1) or (2) above, in which, after being held in air at 850°C for 1 hour, a pin-on-disk friction and wear test is carried out under conditions of a load of 0.5 N and a distance of 20 m, the depth of the wear mark is 7.0 μm or less.

[0016] (4) An austenitic stainless steel sheet according to any one of (1) to (3) above, in which, when the sheet is held at 850°C in air for 1 hour and then air-cooled, the arithmetic mean roughness Ra of the oxide scale formed on the surface is 0.10 µm or less.

[0017] (5) The austenitic stainless steel sheet according to any one of (1) to (4) above, which is used for turbocharger parts.

[0018] (6) An exhaust part using the austenitic stainless steel sheet according to any one of (1) to (5) above. Effect of the Invention

[0019] According to the present invention, an austenitic stainless steel sheet having good high-temperature sliding properties and workability can be obtained. [Brief description of the drawings]

[0020] [Figure 1] FIG. 1 is a graph showing the relationship between the Si content and the punching index. [Diagram 2] FIG. 2 is a diagram showing the relationship between the Si content and the REM content and each characteristic. [Diagram 3] FIG. 3 is a schematic diagram showing the shape of a punched hole made in a steel plate in a punching test. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0021] The present inventors have conducted research on austenitic stainless steel sheets in order to improve high-temperature sliding properties and workability, and have obtained the following findings (a) to (c).

[0022] (a) Turbocharger parts are used at high temperatures, and therefore a relatively thick oxide scale forms on the surface during use. The present inventors therefore focused on this oxide scale in order to improve high-temperature sliding properties. As a result, it was revealed that, depending on the oxide scale that is formed, when parts rub against each other, the scale transfers to the sliding surfaces and reduces the coefficient of friction, thereby acting as a so-called self-lubricating effect. When such a self-lubricating effect works, the high-temperature sliding properties are improved. Therefore, in order to form a scale with a self-lubricating effect, it is desirable to appropriately control the chemical composition of the steel and the manufacturing conditions.

[0023] (b) In order to provide the scale with a self-lubricating effect, it is preferable to include a large amount of Si and to include Si oxide in the scale. However, if the Si content is large, the workability decreases and it becomes difficult to process parts. Therefore, the present inventors have studied the Si content and the punching index, which is an index of workability. As shown in FIG. 1, it has been revealed that when the Si content is 3.0% or more, the punching index becomes 0.3% or more, and the workability decreases. Therefore, the Si content needs to be controlled to less than 3.0%.

[0024] (c) On the other hand, in order to ensure high-temperature sliding properties, it is necessary to form a sufficient amount of scale having a self-lubricating effect. The inventors have clarified that even if the Si content is not large, it is effective to add REM to the steel in order to improve the high-temperature sliding properties.

[0025] When the oxide scale of an austenitic stainless steel plate containing REM was compared with that of an austenitic stainless steel plate without REM in a high-temperature environment, it was found that the steel plate containing REM had a finer oxide scale on the surface. It is believed that such fine oxide scales rub against each other during high-temperature sliding, resulting in a self-lubricating effect and the formation of a denser oxide scale. As a result, it is believed that the oxide scale protects the sliding surface and improves high-temperature sliding performance.

[0026] The present invention has been made based on the above findings. Each of the features of the present invention will be described in detail below.

[0027] 1.Chemical composition The reasons for limiting the content of each element are as follows. In the following description, "%" for the content means "mass %."

[0028] C: 0.005 to 0.30% C is an element that forms an austenite structure and improves high-temperature strength and high-temperature sliding properties. It is also an element necessary for ensuring high-temperature hardness. For this reason, the C content is set to 0.005% or more. However, if C is contained in excess, work hardening becomes more likely and workability decreases. In addition, Cr carbides are formed, which decreases corrosion resistance and intergranular corrosion properties. For this reason, the C content is set to 0.30% or less.

[0029] From the viewpoints of hot workability, high-temperature sliding properties, and manufacturing costs, the C content is preferably 0.03% or more and 0.20% or less, more preferably 0.05% or more and 0.19% or less.

[0030] Si: 0.010% or more and less than 3.00% Silicon is an element that has a deoxidizing effect. In addition, the internal oxidation of silicon improves scale spallation resistance and high-temperature sliding properties. In addition, the internal oxidation of silicon improves high-temperature strength and high-temperature hardness. For this reason, the silicon content is set to 0.010% or more.

[0031] However, if the Si content is 3.00% or more, the steel sheet becomes excessively hard, and part workability and manufacturability decrease. For this reason, the Si content is set to less than 3.00%. If it is desired to further improve high-temperature sliding properties, the Si content is preferably set to 1.50% or more. Also, from the viewpoints of manufacturing costs, pickling properties, and solidification cracking during welding, the Si content is preferably set to 2.80% or less.

[0032] Mn: 0.1-5.0% Mn is an element that has a deoxidizing effect. In addition, Mn has the effect of stabilizing austenite and improving scale adhesion. Furthermore, by including Mn, the scale is endowed with a self-lubricating effect and a self-repairing function, which leads to an improvement in high-temperature sliding properties. For this reason, the Mn content is set to 0.1% or more.

[0033] However, if the Mn content exceeds 5.0%, the scale becomes thick and peels off easily, and the high-temperature sliding properties are reduced. In addition, work hardening increases, and the part workability is reduced. In addition, the inclusion cleanability and pickling property are significantly reduced, and the surface roughness of the product becomes rough. For this reason, the Mn content is set to 5.0% or less. From the viewpoint of forming a scale with good adhesion and further improving the high-temperature sliding properties by utilizing the self-lubrication and self-repairing functions of the scale, the Mn content is preferably set to 0.2% or more, and more preferably set to 1.2% or more. From the viewpoint of pickling property and manufacturing cost, the Mn content is preferably set to 4.0% or less.

[0034] P: 0.010~0.050% P is an element that promotes hot workability and solidification cracking during manufacturing. For this reason, the P content is set to 0.050% or less. Although a lower P content is preferable, excessive reduction of P increases refining costs. For this reason, the P content is set to 0.010% or more. Furthermore, from the viewpoint of reducing manufacturing costs, the P content is preferably set to 0.020% or more and 0.040% or less.

[0035] S: 0.0001 to 0.010% S is an element that reduces hot workability and corrosion resistance. In addition, when coarse sulfides containing S (MnS) are formed, the inclusion cleanliness of the steel sheet is significantly reduced. For this reason, the S content is set to 0.010% or less. However, excessive reduction of S leads to an increase in refining costs. For this reason, the S content is set to 0.0001% or more. From the viewpoints of oxidation resistance and manufacturing costs, the S content is preferably set to 0.0005% or more, and preferably 0.005% or less.

[0036] Ni: 5.00~15.00% Ni is an austenite stabilizing element and also an element that improves corrosion resistance and oxidation resistance. For this reason, the Ni content is set to 5.00% or more. However, excessive Ni content increases the manufacturing cost and hardens the material. For this reason, the Ni content is set to 15.00% or less. From the viewpoints of high temperature strength, corrosion resistance, and manufacturability, the Ni content is preferably set to 9.00% or more. The Ni content is preferably set to 14.00% or less.

[0037] Cr: 15.00~30.00% Cr is an element that improves corrosion resistance, oxidation resistance, and high-temperature sliding properties. From the viewpoint of suppressing abnormal oxidation in the exhaust part environment, the Cr content is set to 15.00% or more. However, excessive Cr content hardens the material and increases manufacturing costs. For this reason, the Cr content is set to 30.00% or less. Furthermore, from the viewpoints of workability, manufacturability, and manufacturing costs, the Cr content is preferably set to 17.00% or more and 25.00% or less.

[0038] N: 0.02 to 0.40% Like C, N is an element that stabilizes austenite. It is also an element that is effective for improving high-temperature strength, high-temperature hardness, and high-temperature sliding properties. In particular, it acts as a solid-solution strengthening element to improve high-temperature strength. For this reason, the N content is set to 0.02% or more.

[0039] However, if the N content exceeds 0.40%, the room temperature material becomes significantly hard. As a result, the cold workability during steel plate manufacturing deteriorates, and part workability decreases. For this reason, the N content is set to 0.40% or less. In order to improve high-temperature sliding properties, the N content is preferably 0.03% or more, and more preferably more than 0.05%. On the other hand, from the viewpoint of suppressing pinholes and intergranular corrosion of welds during welding, the N content is preferably 0.30% or less.

[0040] Al: 0.001 to 0.50% Al acts as a deoxidizing element and improves inclusion cleanliness. In addition, Al suppresses the peeling of oxide scale and improves high-temperature sliding properties through slight internal oxidation. For this reason, the Al content is set to 0.001% or more. However, Al is a ferrite-forming element, and if it is contained in an amount exceeding 0.50%, it reduces the stability of the austenite structure. Furthermore, if Al is contained in excess, not only does it reduce pickling properties, but it also increases the amount of inclusions and increases surface roughness. As a result, the surface roughness of the oxide scale formed in the temperature range of 850°C becomes rough, and high-temperature sliding properties deteriorate. For this reason, the Al content is set to 0.50% or less.

[0041] From the viewpoints of refining costs and surface properties, the Al content is preferably 0.010% or more and 0.30% or less, and from the viewpoint of hot workability, the Al content is preferably 0.040% or more and 0.10% or less.

[0042] REM: 0.005~0.100% REM (rare earth elements) are effective in improving oxidation resistance and in improving high-temperature sliding properties by forming uniform and dense scale. For this reason, the REM content is set to 0.005% or more. However, if REM is contained in excess, oxides containing REM are formed in the nozzle through which molten steel flows during casting, causing nozzle clogging. In addition, sulfides containing REM are formed, reducing corrosion resistance. For this reason, the REM content is set to 0.100% or less. In order to further obtain the above effect, the REM content is preferably set to 0.010% or more, and more preferably set to 0.016% or more. On the other hand, from the viewpoint of manufacturing costs, the REM content is preferably set to 0.090% or less, and more preferably set to 0.070% or less.

[0043] Here, REM refers to a total of 17 elements, including Sc, Y and lanthanides, and the above REM content means the total content of these elements. In industry, REM is often added in the form of misch metal.

[0044] In addition to the above elements, the austenitic stainless steel sheet according to the present invention may contain one or more elements selected from Cu, Mo, V, Ti, Nb, B, Ca, W, Zr, Sn, Co, Mg, Sb, Ga, Ta, Hf, and Bi.

[0045] Cu: 0-4.0% Cu has the effect of stabilizing austenite and improving oxidation resistance and corrosion resistance. Cu also has the effect of imparting a self-lubricating action and a self-repairing function to the scale and improving high-temperature sliding properties. For this reason, Cu may be contained as necessary. However, excessive Cu content not only reduces oxidation resistance but also reduces manufacturability. Therefore, the Cu content is set to 4.0% or less. The Cu content is preferably set to 3.0% or less, and more preferably set to 2.8% or less. On the other hand, in order to obtain the above effect, the Cu content is preferably set to 0.1% or more, and more preferably set to 0.2% or more.

[0046] Mo: 0-2.0% Mo has the effect of improving corrosion resistance. Mo also has the effect of improving high-temperature strength and high-temperature hardness. This is because the inclusion of Mo leads to precipitation strengthening due to the precipitation of Mo carbides in addition to solid solution strengthening. Furthermore, the formation of precipitates can improve wear resistance properties. For this reason, Mo may be included as necessary. However, Mo is an expensive element, and if it is included in excess, the manufacturing cost increases. For this reason, the Mo content is set to 2.0% or less. The Mo content is preferably set to 1.7% or less. On the other hand, in order to obtain the above effects such as strengthening stability due to the precipitates and from the viewpoint of inclusion cleanliness, the Mo content is preferably set to 0.1% or more.

[0047] V: 0 to 1.0% V has the effect of improving corrosion resistance. It also forms carbides and has the effect of improving high-temperature strength and wear resistance at high temperatures. For this reason, V may be contained as necessary. However, excessive V content increases the manufacturing cost and decreases the abnormal oxidation limit temperature. For this reason, the V content is set to 1.0% or less. From the viewpoint of manufacturability and inclusion cleanliness, the V content is preferably set to 0.8% or less. On the other hand, in order to obtain the above effects, the V content is preferably set to 0.05% or more.

[0048] Ti: 0 to 0.30% Ti combines with C and N to improve corrosion resistance and intergranular corrosion resistance. Therefore, it may be contained as necessary. However, if Ti is contained in an amount exceeding 0.30%, nozzle clogging occurs easily during the casting stage, significantly reducing manufacturability. In addition, coarse Ti carbonitrides are formed, reducing part workability. For this reason, the Ti content is set to 0.30% or less. On the other hand, in order to obtain the above effects, the Ti content is preferably set to 0.005% or more. From the viewpoints of high-temperature strength, intergranular corrosion resistance of welds, and manufacturing costs, the Ti content is more preferably set to 0.010% or more, and more preferably set to 0.20% or less.

[0049] Nb: 0 to 0.30% Nb, like Ti, has the effect of improving corrosion resistance and intergranular corrosion resistance by combining with C and N. In addition, Nb is also an element that improves high-temperature strength. Therefore, it may be contained as necessary. However, if Nb is contained in an amount exceeding 0.30%, hot workability is significantly reduced. Furthermore, if coarse Nb carbonitrides are formed, part workability is reduced. For this reason, the Nb content is set to 0.30% or less. On the other hand, in order to obtain the above effect, the Nb content is preferably set to 0.005% or more. From the viewpoints of high-temperature strength, intergranular corrosion resistance of welded parts, and manufacturing costs, the Nb content is more preferably set to 0.010% or more, and preferably less than 0.15%.

[0050] B: 0 to 0.0050% B is an element that improves hot workability. It may be contained as necessary to suppress work hardening at room temperature. However, excessive B content causes the formation of borocarbides. This reduces the inclusion cleanliness and intergranular corrosion resistance of the steel sheet. For this reason, the B content is set to 0.0050% or less. On the other hand, in order to obtain the above effects, the B content is preferably set to 0.0002% or more. From the viewpoints of refining costs and ductility, the B content is more preferably set to 0.0003% or more, and is preferably set to 0.0020% or less.

[0051] Ca: 0 to 0.010% Ca has a desulfurization effect, so it may be contained as necessary. However, if Ca is contained in an amount exceeding 0.010%, water-soluble inclusions such as CaS are formed. As a result, the inclusion cleanliness and corrosion resistance of the steel sheet are significantly reduced. For this reason, the Ca content is set to 0.010% or less. On the other hand, in order to obtain the above effects, the Ca content is preferably set to 0.0003% or more, and more preferably set to 0.0005% or more. Furthermore, from the viewpoints of manufacturability and surface properties, the Ca content is more preferably set to 0.0010% or more, and preferably set to 0.003% or less.

[0052] W: 0~3.0% W may be contained as necessary because it contributes to improving high-temperature strength and corrosion resistance. However, if W is contained in an amount exceeding 3.0%, it leads to hardening, deterioration of toughness during manufacturing, and increased manufacturing costs. For this reason, the W content is set to 3.0% or less. Furthermore, from the viewpoint of manufacturability and refining costs, the W content is preferably set to 2.0% or less. On the other hand, in order to obtain the above effects, the W content is preferably set to 0.1% or more.

[0053] Zr: 0 to 0.30% Zr combines with C or N to improve the intergranular corrosion resistance and oxidation resistance of the weld. Therefore, Zr may be contained as necessary. However, if Zr is contained in an amount exceeding 0.30%, it leads to a significant decrease in manufacturability and an increase in manufacturing costs. For this reason, the Zr content is set to 0.30% or less. From the viewpoint of manufacturability and refining costs, the Zr content is preferably set to 0.10% or less. On the other hand, in order to obtain the above effect, the Zr content is preferably set to 0.05% or more.

[0054] Sn: 0 to 0.50% Sn contributes to improving corrosion resistance and high-temperature strength, so it may be contained as necessary. However, if Sn is contained in an amount exceeding 0.50%, slab cracks may occur during production. For this reason, the Sn content is set to 0.50% or less. Furthermore, from the viewpoint of manufacturability and refining costs, the Sn content is preferably set to 0.30% or less. On the other hand, in order to obtain the above effects, the Sn content is preferably set to 0.01% or more, more preferably set to 0.03% or more, and even more preferably set to 0.05% or more.

[0055] Co: 0 to 0.30% Co contributes to improving high-temperature strength, so it may be contained as necessary. However, if Co is contained in an amount exceeding 0.30%, it leads to hardening of the steel plate, a decrease in toughness during manufacturing, and an increase in manufacturing costs. For this reason, the Co content is set to 0.30% or less. In consideration of manufacturability and refining costs, the Co content is preferably set to 0.20% or less. On the other hand, in order to obtain the above effects, the Co content is preferably set to 0.03% or more.

[0056] Magnesium: 0 to 0.010% Mg is an element having a deoxidizing effect. In addition, Mg has the effect of refining or dispersing the slab structure with its oxide, thereby refining the steel sheet structure and improving the inclusion cleanliness. For this reason, Mg may be contained as necessary. However, excessive Mg content reduces weldability and corrosion resistance. In addition, the formation of coarse Mg inclusions reduces part workability. For this reason, the Mg content is set to 0.010% or less. On the other hand, in order to obtain the above effect, the Mg content is preferably set to 0.0002% or more. In consideration of refining costs, the Mg content is preferably set to 0.0003% or more, and preferably 0.005% or less.

[0057] Sb: 0 to 0.50% Sb has the effect of improving high-temperature strength by segregating at grain boundaries, so it may be contained as necessary. However, if Sb is contained in an amount exceeding 0.50%, segregation occurs, and cracks occur during welding. For this reason, the Sb content is set to 0.50% or less. On the other hand, in order to obtain the above effect, the Sb content is preferably set to 0.005% or more. In consideration of high-temperature properties, toughness, and manufacturing costs, the Sb content is more preferably set to 0.030% or more, and preferably set to 0.30% or less. Moreover, the Sb content is further preferably set to 0.050% or more, and more preferably set to 0.20% or less.

[0058] Ga: 0 to 0.30% Ga has the effect of improving corrosion resistance and suppressing hydrogen embrittlement. Therefore, it may be contained as necessary. However, if Ga is contained in an amount exceeding 0.30%, coarse sulfides are generated and part workability is reduced. Therefore, the Ga content is set to 0.30% or less. On the other hand, in order to obtain the above effect, the Ga content is preferably set to 0.0002% or more. Furthermore, from the viewpoint of manufacturability and manufacturing costs, the Ga content is more preferably set to 0.0020% or more.

[0059] Ta: 0 to 1.0% Hf: 0~1.0% Bi: 0 to 0.020% Ta may be contained as necessary to improve high-temperature strength. However, excessive Ta content increases manufacturing costs, so the Ta content is set to 1.0% or less. On the other hand, in order to obtain the above effects, the Ta content is preferably 0.001% or more. In order to further increase the strength, the Ta content is more preferably 0.010% or more. For the same reason as Ta, the Hf content is also set to 1.0% or less. For the same reason as Ta, the Hf content is preferably 0.001% or more, more preferably 0.010% or more.

[0060] For the same reason, Bi may be contained as necessary. However, excessive Bi content increases the manufacturing cost, so the Bi content is set to 0.020% or less. On the other hand, in order to obtain the same effect as above, the Bi content is preferably set to 0.001% or more. It is desirable to reduce the general harmful elements such as As and Pb, and impurity elements as much as possible.

[0061] In the chemical composition of the present invention, the balance is Fe and impurities. Here, "impurities" refer to components that are mixed in due to various factors in raw materials such as ores and scraps and in the manufacturing process during industrial production of austenitic stainless steel, and are permissible within a range that does not adversely affect the present invention.

[0062] 2.Punching processing index Some precision parts used in turbochargers are manufactured by punching. For example, if the Si content of the austenitic stainless steel sheet exceeds the above-mentioned range, the sheet is prone to work hardening, and the punch breaks frequently. As a result, the punch needs to be replaced more frequently, and the processing efficiency decreases. Therefore, for the austenitic stainless steel sheet according to the present invention, a punching index is defined as an index of the ease of punching.

[0063] The punching processing index is the number of times the punch is replaced per sheet, expressed as a percentage, when eight φ10 mm punched holes are made per steel plate, with a maximum of 1,000 steel plates being processed, and the above processing being performed with a maximum of two replacement punches. Punching index (%) = (number of punch replacements / number of punched steel sheets) × 100 (a)

[0064] In the austenitic stainless steel sheet according to the present invention, the punching index is set to 0.2% or less. If the punching index exceeds 0.2%, punching becomes difficult, and processing into turbocharger parts becomes difficult. The lower limit of the punching index is not particularly limited, but is usually 0.05% or more.

[0065] 3. Oxide scale formed in high temperature environments In the austenitic stainless steel sheet according to the present invention, the REM additive elements form a uniform and dense scale in a high-temperature operating environment, thereby providing the desired high-temperature sliding properties. For this reason, the arithmetic mean roughness Ra of the oxide scale formed in a high-temperature operating environment is specified.

[0066] Specifically, when the austenitic stainless steel sheet is held in air at 850°C for 1 hour and then air-cooled, the arithmetic mean roughness Ra of the oxide scale formed on the surface of the sheet is preferably 0.10 μm or less. In order to obtain better high-temperature sliding properties, the arithmetic mean roughness Ra of the oxide scale is more preferably 0.08 μm or less. The lower limit of the arithmetic mean roughness Ra of the oxide scale is not particularly limited, but is usually 0.01 μm or more.

[0067] 4. Evaluation of high-temperature sliding properties In the austenitic stainless steel sheet according to the present invention, the high-temperature sliding properties are evaluated by a pin-on-disk friction and wear test at high temperature. In the pin-on-disk friction and wear test, the test material is held in air at 850°C for 1 hour, and then a pin and a disk are brought into contact with each other at that temperature and atmosphere, and the test is performed by rotating the test material around a circumference with a rotation diameter of 20 mm for a test distance of 20 m at a load of 0.5 N and a sliding speed of 3.3 mm / s.

[0068] Thereafter, the wear mark depth of the sliding surface of the test material is measured using a laser microscope. If the wear mark depth is 7.0 μm or less, the high-temperature sliding property is judged to be good, and if the wear mark depth is more than 7.0 μm, the high-temperature sliding property is judged to be poor.

[0069] Here, the relationship between the Si and REM contents and each characteristic is shown. The values ​​in the squares in FIG. 2 are the values ​​of the wear scar depth measured after the pin-on-disk friction wear test under the above-mentioned conditions. From FIG. 2, even if the Si content is within the range of the present invention, when the REM content is less than 0.005% and is outside the range specified in the present invention, the wear scar depth is greater than 7.0 μm, and good high-temperature sliding properties cannot be obtained. Furthermore, when the Si content is 3.0% or more, the punching workability is reduced. Furthermore, when the REM content is 0.10% or more, nozzle clogging is likely to occur during casting.

[0070] 5.Applications The austenitic stainless steel sheet according to the present invention is suitable for use in turbocharger parts. Specifically, it is suitable for use in precision parts inside a nozzle vane type turbocharger and parts around the wastegate valve of a wastegate valve type turbocharger. More specifically, examples of precision parts for adjusting the flow velocity and flow rate of exhaust gas include a nozzle mount, a nozzle plate, a nozzle ring, a nozzle vane, a drive ring, a drive lever, a lever plate, a shroud, and a wastegate valve. It may also be used in exhaust parts other than the above-mentioned parts. Furthermore, it can also be applied to parts used in high-temperature environments, particularly high-temperature friction environments, such as various boilers and fuel cell systems.

[0071] 6. Manufacturing method A preferred method for producing the austenitic stainless steel sheet according to the present invention will now be described. The austenitic stainless steel sheet according to the present invention can obtain the effects described above regardless of the production method, but can be produced by the following production method.

[0072] The austenitic stainless steel sheet according to the present invention is preferably produced by the steps of steel making-hot rolling-annealing and pickling-cold rolling-annealing and pickling-temper rolling (polishing) as follows.

[0073] 6-1.Steelmaking process It is preferable to melt steel having the above chemical composition in an electric furnace or converter, followed by secondary refining. The REM contained in the steel according to the present invention forms oxides, which makes the nozzle more likely to become clogged when the molten steel is poured during casting. For this reason, as described above, the REM content is limited to 0.010% or less. In addition, in this process, it is preferable to provide stirring and settling time before casting to allow the REM oxides in the molten steel to float and be removed. The steel made may be made into a slab according to a known casting method (such as continuous casting). The thickness of the slab to be produced may be set appropriately depending on the subsequent rolling conditions, etc.

[0074] 6-2.Hot rolling process The slab is then heated at 1200 to 1300° C. and is preferably hot-rolled by continuous rolling until it has a predetermined thickness. The slab is hot-rolled to become a hot-rolled sheet. The reduction ratio during hot rolling may be appropriately selected.

[0075] The hot-rolled steel sheet is generally subjected to hot-rolled sheet annealing and pickling treatment, but the hot-rolled sheet annealing may be omitted. When hot-rolled sheet annealing is performed, the temperature condition is preferably in the range of 1100 to 1200°C, and the annealing time is preferably in the range of 10 to 60 seconds.

[0076] 6-3.Cold rolling process Next, the sheet is cold-rolled to a predetermined thickness to obtain a cold-rolled sheet. Here, the rolling reduction of the cold rolling is preferably in the range of 50 to 95%. If the rolling reduction of the cold rolling is less than 50%, a sufficient processing rate cannot be obtained, and recrystallization is not sufficiently promoted in the subsequent annealing. Also, if the rolling reduction of the cold rolling is more than 95%, the crystal grains become excessively fine in the subsequent annealing.

[0077] 6-4. Cold-rolled sheet annealing and pickling process After the cold rolling, the cold rolled sheet is annealed and pickled. Usually, the annealing temperature is preferably less than 1000 to 1200°C. The annealing time is preferably in the range of 10 to 60 seconds. This is because a good recrystallized structure can be obtained by setting the annealing temperature and annealing time in the above ranges. The annealing of the cold rolled sheet may be performed between passes of the cold rolling. The type of annealing may be either batch annealing or continuous annealing.

[0078] The subsequent pickling process is carried out to remove the scale formed on the steel surface by annealing. The pickling process may be any chemical descaling process using sulfuric acid, nitric hydrofluoric acid, nitric acid electrolysis, etc., and immersion in a molten alkali salt may be carried out as a pretreatment. The temperature and time conditions for immersion in a molten alkali salt can be appropriately changed depending on the desired properties of the steel sheet. The cold-rolled, annealed, pickled steel sheet may be appropriately subjected to temper rolling and polishing processes as necessary.

[0079] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples. EXAMPLES

[0080] After the steel having the chemical composition shown in Tables 1 and 2 was melted, the following steps were carried out to obtain a steel sheet. Specifically, a block of 90 mm length x 150 mm width x 40 mm thickness was cut out from an ingot cast in a 13 kg flat mold. This was hot rolled to 10 mm at 1250°C, hot-rolled sheet annealed at 1150°C for 60 seconds, and then pickled. The hot-rolled sheet obtained was then cold-rolled at a reduction rate of 50%, annealed at 1150°C for 60 seconds, and then pickled to obtain a steel sheet of 5.0 mm thickness.

[0081] [Table 1]

[0082] [Table 2]

[0083] (Roughness measurement) Samples were cut out from each of the obtained steel sheets, held in air at 850°C for 1 hour, and then air-cooled, and the arithmetic mean roughness Ra of the oxide scale formed on the surface was measured. The scale was measured in accordance with JIS B 0601:2013 at a length of 3.0 mm and a speed of 0.3 mm / s. The measurement was performed using a Surfcom 1400 made by Tokyo Seimitsu Co., Ltd.

[0084] When the measured arithmetic mean roughness Ra was 0.10 μm or less, the arithmetic mean roughness was evaluated as good, and marked with ◯ in the table. When the arithmetic mean roughness Ra was 0.08 μm or less, the arithmetic mean roughness was evaluated as even better, and marked with ◎ in the table. On the other hand, when the arithmetic mean roughness exceeded 0.10 μm, the arithmetic mean roughness was evaluated as poor, and marked with × in the table.

[0085] (Pin-on-disk friction and wear test) In the pin-on-disk friction and wear test, a circular disk was taken from each steel plate obtained, and a pin was placed so that the tip of the pin was in contact with the disk perpendicularly, and the pin was adjusted so that it would repeatedly undergo friction and wear as it rotated around the disk. The pin was made of the same material as the disk, and had a bullet-like shape with a base diameter of φ6 mm, a tip diameter of φ4 mm, and a total length of 10 mm. The disks were obtained by machining them to φ29 mm and a height of 5 mm.

[0086] In the above test, the pin and disk were initially placed without contact, then heated in a furnace in an air atmosphere, and after holding at 850°C for 1 hour, the pin and disk were brought into contact and the test was carried out. The test conditions were load 0.5N, test distance 20m, sliding speed 3.3mm / s, rotation diameter 20mm, and the rotating circle was rotated until the test distance was completed.

[0087] After that, the wear mark depth of each disk was measured from the surface using a laser microscope. When the wear mark depth was 7.0 μm or less, the high-temperature sliding property was evaluated as good, and was marked with ◎ in the table. On the other hand, when the wear mark depth was more than 7.0 μm, the high-temperature sliding property was evaluated as poor, and was marked with × in the table. In addition, a High-Temperature Tribometer manufactured by CSM Instruments was used for the pin-on-disk method friction and wear test. In addition, a VF-8500 manufactured by Keyence Corporation was used for measuring the wear mark depth.

[0088] (Punching test) In the punching test, a 100 mm square sample was cut from each steel plate, and eight φ10 mm punched holes were made in each sample at 30 mm intervals as shown in Figure 3. This process was carried out for up to 1000 sheets. If the punching punch was chipped or broken during the test, the punch was replaced. The percentage of the number of times the punch was replaced per sheet during the punching test up to 1000 sheets was defined as the punching index, and when the punching index was 0.2% or less, the punching workability was evaluated as good and marked with ◎. On the other hand, when the punching index exceeded 0.2%, the punching workability was evaluated as poor and marked with ×.

[0089] (Nozzle clogging) Regarding nozzle clogging that occurs during casting, because the amount of REM added has an effect, steel with an REM content of 0.1% or less was evaluated as being less susceptible to nozzle clogging and marked with ◎. On the other hand, steel with an REM content of more than 0.1% was evaluated as being more susceptible to nozzle clogging and marked with ×. The results are summarized below in Tables 3 and 4.

[0090] [Table 3]

[0091] [Table 4]

[0092] Nos. 1 to 11, which satisfy the requirements of the present invention, were excellent in high-temperature sliding properties and punching workability, and satisfied the performance required for turbocharger parts. On the other hand, Nos. 12 to 15, which do not satisfy the requirements of the present invention, were inferior in at least one of high-temperature sliding properties and punching workability. [Industrial Applicability]

[0093] According to the present invention, it is possible to provide an austenitic stainless steel sheet having excellent properties for exhaust parts that require high-temperature sliding properties and workability. In particular, by using it as a turbocharger part among exhaust parts, it is possible to provide a part that satisfies automobile exhaust gas regulations, is lightweight, and improves fuel efficiency.

Claims

1. The chemical composition, in mass%, is C: 0.005-0.30%, Si: 0.010% or more and less than 3.00%; Mn: 0.1 to 5.0%, P: 0.010-0.050%, S: 0.0001-0.010%, Ni: 5.00 to 15.00%, Cr: 15.00-30.00%, N: 0.02-0.40%, Al: 0.001-0.50%, REM: 0.005-0.100%, Cu: 0-4.0%, Mo: 0-2.0%, V: 0 to 1.0%, Ti: 0 to 0.30%, Nb: 0 to 0.30%, B: 0 to 0.0050%, Ca: 0-0.010%, W: 0 to 3.0%, Zr: 0 to 0.30%, Sn: 0 to 0.50%, Co: 0 to 0.30%, Mg: 0 to 0.010%, Sb: 0 to 0.50%, Ga: 0-0.30%, Ta: 0 to 1.0%, Hf: 0-1.0%, Bi: 0 to 0.020%, The balance is Fe and impurities. The punching index defined below is 0.2% or less, When the sample is held in air at 850° C. for 1 hour and then air-cooled, the arithmetic mean roughness Ra of the oxide scale formed on the surface is 0.10 μm or less. Austenitic stainless steel plate. (Punching processing index) The punching process index is the number of times, expressed as a percentage, that the punch was replaced per steel plate in a test in which a punch was used to create eight φ10 mm punched holes per steel plate and the punch was replaced if it was chipped or broken (however, the upper limit of the number of steel plates was 1,000, and the upper limit of the number of replacements was two times).

2. The chemical composition, in mass%, Cu: 0.1 to 4.0%, Mo: 0.1-2.0%, V: 0.05-1.0%, Ti: 0.005-0.30%, Nb: 0.005-0.30%, B: 0.0002 to 0.0050%, Ca: 0.0003-0.010%, W: 0.1-3.0%, Zr: 0.05-0.30%, Sn: 0.01-0.50%, Co: 0.03 to 0.30%, Mg: 0.0002 to 0.010%, Sb: 0.005 to 0.50%, Ga: 0.0002-0.30%, Ta: 0.001 to 1.0%, Hf: 0.001 to 1.0%, and Bi: 0.001-0.020%, Contains one or more selected from The austenitic stainless steel sheet according to claim 1.

3. 3. The austenitic stainless steel sheet according to claim 1, wherein when the sheet is held in air at 850° C. for 1 hour and then subjected to a pin-on-disk friction and wear test at said temperature and atmosphere under conditions of a load of 0.5 N and a distance of 20 m, the depth of the wear mark is 7.0 μm or less.

4. The austenitic stainless steel sheet according to any one of claims 1 to 3, which is used for turbocharger parts.

5. An exhaust part using an austenitic stainless steel sheet according to any one of claims 1 to 4.

Citation Information

Patent Citations

  • Austenitic stainless cold rolled steel sheet excellent in bulging formability and its production

    JP1998036946A

  • Cold rolled austenitic stainless steel sheet reduced in amount of springback, and its production

    JP1998072644A

  • Austenitic stainless steel and automotive exhaust system paprts

    JP2001059141A

  • Method for manufacturing austenitic stainless steel plate having excellent precision punching property

    JP2005220443A

  • Steel sheet for valve seat of four-way valve in air conditioner

    JP2006257536A