Duplex stainless steel with excellent diffusion bonding and weldability
A multi-phase stainless steel with controlled element composition and structure addresses the strength and corrosion issues of ferritic stainless steel, achieving high strength and improved bondability and weldability through a ferrite and martensitic phase structure.
Patent Information
- Application Number
- JP2020200882
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-12-03
- Publication Date
- 2024-10-09
- Estimated Expiration
- 2040-12-03
AI Technical Summary
Ferritic stainless steel, despite being cost-effective with lower Ni content, suffers from lower tensile strength and hardness, and when welded, forms Cr carbides leading to intergranular corrosion and poor corrosion resistance.
A multi-phase stainless steel with controlled composition and structure, comprising specific ranges of elements like C, Si, Mn, Ni, Cr, Cu, Sn, Nb, and others, ensuring a ferrite and martensitic phase structure with an M value between 35 and 65, enhancing diffusion bondability and weldability.
The multi-phase stainless steel achieves high strength with reduced Ni content, exhibiting excellent diffusion bondability and weldability, preventing Cr-deficient regions and intergranular corrosion.
Smart Images

Figure 0007564695000004 
Figure 0007564695000005 
Figure 0007564695000006
Abstract
Description
[Technical field]
[0001] The present invention relates to a duplex stainless steel having excellent diffusion bondability and weldability. [Background technology]
[0002] In recent years, due to the high cost of Ni, one of the essential metal components of stainless steel, a change from austenitic stainless steel with a high Ni content to ferritic stainless steel with a low Ni content has been increasingly considered in actual use in order to reduce product prices. However, ferritic stainless steel tends to have lower tensile strength and hardness than austenitic stainless steel. Therefore, in order to improve mechanical properties such as tensile strength, duplex stainless steels with a duplex structure of martensite and ferritic phases, which have high tensile strength, are being considered.
[0003] On the other hand, stainless steel is increasingly being used in various fields other than as a structural material. To be used in many fields, machining, joining, and other processes are sometimes combined to manufacture a final product of a desired shape. For example, duplex stainless steel having ferrite and martensite phases, which is suitable for use in machine parts, may be used by applying solid-state joining in addition to machining such as drawing. Furthermore, parts manufactured by solid-state joining may be stacked by welding to produce machine parts.
[0004] Patent Document 1 discloses a duplex stainless steel consisting of at least two phases, ferrite, martensite, and austenite, in which the grain size is controlled to be fine and suitable for diffusion bonding, which is a type of solid-state bonding method. It also discloses that a certain degree of bondability can be obtained under the diffusion bonding conditions of relatively low temperature and pressure, 1000°C and surface pressure of 0.1 MPa. However, when a welding method is performed in addition to diffusion bonding, there is a problem that Cr carbides precipitate in the heat-affected zone of a duplex stainless steel containing a ferrite phase, which makes intergranular corrosion and the like more likely to occur due to the Cr-deficient region, thereby reducing corrosion resistance. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] JP 2016-089223 A Summary of the Invention [Problem to be solved by the invention]
[0006] Therefore, the problem to be solved by the present invention is to provide a duplex stainless steel having a duplex structure of ferrite and martensite phases that has high strength while reducing the amount of Ni and has excellent diffusion bondability and weldability. [Means for solving the problem]
[0007] The present inventors have completed a duplex stainless steel having a multi-phase metal structure of ferrite and martensite phases, which has excellent diffusion bondability and weldability by controlling the component composition and metal structure.
[0008] Specifically, they are shown below. Below, elements are represented by symbols. [1] The present invention relates to a duplex stainless steel having excellent diffusion bondability and weldability, the duplex stainless steel containing, by mass%, C: 0.03% or less, Si: 0.01 to 1.00%, Mn: 0.01 to 2.50%, P: 0.04% or less, S: 0.015% or less, Ni: 1.5 to 5.5%, Cr: 17.5 to 22.0%, Cu: 0.01 to 2.0%, Sn: 0.001 to 0.1%, N: 0.03% or less, Nb: 7 × (C + N) to 0.70%, Ti: 0.1% or less, and Al: 0.1% or less, with the balance being Fe and unavoidable impurities, the M value represented by the following formula (1) being in the range of 35 to 65 when the T value is in the range of 950 to 1100, and the duplex stainless steel having a duplex structure of ferrite phase and martensite phase.
[0009] Formula (1): M value = -0.22T + 34.5Ni + 10.5Mn + 13.5Cu-17.3Cr-17.3Si-18Mo + 475.5 However, the content value of each element expressed in mass% is substituted for the element symbol on the right side of formula (1), and here, 0 (zero) is substituted for the element symbol for Mo.
[0010] [2] The present invention relates to a duplex stainless steel having excellent diffusion bondability and weldability as described in claim 1, further containing, by mass%, one or more of Mo: 2.0% or less, V: 0.5% or less, and B: 0.0001 to 0.01%. However, if Mo is not contained, 0 (zero) is substituted for the Mo element symbol. Effect of the Invention
[0011] According to the present invention, it is possible to provide a duplex stainless steel having a duplex structure of ferrite and martensite phases, which has high strength even with a small Ni content and is excellent in diffusion bondability and weldability. [Brief description of the drawings]
[0012] [Figure 1] FIG. 1 is a photograph showing a metal structure composed of martensite and ferrite phases. [Diagram 2] FIG. 2 is a diagram showing a measurement specimen used in the bondability test. [Diagram 3] FIG. 3 is a diagram explaining the weldability test, where (a) is a diagram showing the measurement specimen used in the weldability test, (b) is an example of corrosion resistance (◯), and (c) is an example of poor corrosion resistance (×). DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0013] Each metal element and the M value in formula (1) will be explained below. "%" in the content of a metal element means "mass %" unless otherwise specified.
[0014] (C: 0.03% or less) Carbon (C) is an austenite-forming element and has the effect of increasing the volume fraction of the austenite phase in the metal structure. It also increases the strength of the ferrite phase through solid solution strengthening, and has a large effect on the strength of the martensite phase. A certain amount of C content is preferable, but if the C content is too high, it will lead to the formation of Cr carbides, which will cause intergranular corrosion. Furthermore, if the C content is high, residual austenite may occur even after quenching. Therefore, in order to suppress the generation of residual austenite, the C content is set to 0.03% or less, preferably 0.02% or less. Carbide is formed by combining C with one or more other metal elements, and also includes carbonitrides in which C, N, and other elements are combined.
[0015] (N: 0.03% or less) Like C, N (nitrogen) is an austenite-forming element and has the effect of increasing the volume fraction of the austenite phase in the metal structure. In addition, N combines with Cr contained in duplex stainless steel to form Cr nitrides, which can form Cr-deficient regions and cause intergranular corrosion. Therefore, even if a certain amount of N is added, the volume fraction of the ferrite phase, martensite phase, etc., and the degree of contribution to mechanical strength are saturated, and the increase in the amount of Cr nitrides formed leads to a decrease in machinability. Therefore, the N content is set to 0.03% or less, preferably 0.02% or less.
[0016] (Ni: 1.5-5.5%) Ni (nickel) is an austenite-forming element, and forms an austenite phase in the temperature range where the diffusion bonding method is performed. It can also contribute to the corrosion resistance of the entire duplex stainless steel. The Ni content is preferably 1.5% or more, and more preferably 2.0% or more. On the other hand, Ni is an expensive element, and excessive addition leads to an increase in the product price. Therefore, from these points of view, the Ni content is set to 5.5% or less, and preferably 5.0% or less.
[0017] (Cr:17.5~22.0%) Cr (chromium) is a ferrite-forming element that forms a passive film on the surface of duplex stainless steel to provide corrosion resistance. It also increases resistance to localized corrosion such as pitting and crevice corrosion. To provide corrosion resistance to the martensite phase, the Cr content is preferably 17.5% or more, and more preferably 18.0% or more. On the other hand, if the Cr content is too high, it becomes difficult to reduce C and N, which impairs mechanical properties and toughness. Therefore, the Cr content is set to 22.0% or less, and preferably 20.5% or less.
[0018] (Si: 0.01 to 1.00%) Silicon (Si) is a ferrite-forming element and is an effective deoxidizing agent in the manufacturing process of duplex stainless steel. It also dissolves in large amounts in the ferrite phase and has the effect of increasing the strength of the ferrite phase. To obtain these effects, the Si content is preferably 0.01% or more. On the other hand, excessive Si content may form a Si oxide film during the diffusion bonding or welding process, resulting in a decrease in diffusion bonding and weldability. Therefore, the Si content is set to 1.00% or less, preferably 0.80% or less.
[0019] (Mn: 0.01 to 2.50%) Mn (manganese) is an austenite-forming element and is effective in making the austenite phase coexist with the ferrite phase at the diffusion bonding temperature. The Mn content is set to 0.01% or more. However, excessive addition of Mn causes a decrease in corrosion resistance and forms a Mn oxide film during the diffusion bonding or welding process, which leads to a decrease in diffusion bondability and weldability, so the Mn content is set to 2.50% or less, preferably 1.50% or less.
[0020] (Cu: 0.01 to 2.0%) Cu (copper) is an austenite generating element and ensures the volume fraction of the austenite phase at the diffusion bonding temperature. Furthermore, when added in combination with Sn, it has the effect of improving diffusion bonding. This is because, during the diffusion bonding process, the CuSn phase, which is a low melting point compound, temporarily precipitates finely and becomes a liquid phase, improving diffusion bonding. The CuSn phase then diffuses and does not affect the metal structure or mechanical properties after bonding. To obtain these effects, a Cu content of 0.01% or more is ensured. However, if the Cu content is too high, it will lead to the precipitation of the εCu phase, which will cause a decrease in corrosion resistance. Therefore, the Cu content is set to 2.0% or less, preferably 1.5% or less.
[0021] (Sn: 0.001~0.1%) Sn (tin) has the effect of improving diffusion bonding when added in combination with Cu. This is because the CuSn phase, a low melting point compound, temporarily precipitates finely during the diffusion bonding process, becoming liquid and improving diffusion bonding. The CuSn phase then diffuses and does not affect the structure or characteristics after bonding. In order to achieve these effects, Sn is an essential metallic element, and the Sn content must be at least 0.001%. However, if the Sn content is too high, it will cause a decrease in the hot workability of duplex stainless steel, so it should be 0.1% or less, preferably 0.05% or less.
[0022] (Nb: 7×(C+N)~0.70%) Nb (niobium) is an element that fixes C and N in duplex stainless steel and is effective in preventing intergranular corrosion in duplex stainless steel. Nb does not precipitate in molten steel, and most of it is finely dispersed and precipitated in duplex stainless steel as Nb carbide or nitride during the cooling process after solidification is complete, and functions as a precipitation nucleus for Cr carbide that is formed at a lower temperature. If the Nb content is less than 7 × (C + N), Cr is consumed by precipitation as Cr carbide or nitride, which generates a Cr-deficient region, causing intergranular corrosion and deteriorating weldability. For this reason, the Nb content is set to 7 × (C + N) or more to prevent intergranular corrosion. Note that C and N represent the contents (mass%) in duplex stainless steel. However, excessive addition of Nb hardens duplex stainless steel and causes a decrease in machinability. Therefore, the Nb content is set to 0.70% or less, preferably 0.45% or less.
[0023] (Ti: 0.1% or less) Like Nb, Ti (titanium) has the effect of fixing C and N, so it can be added as necessary. However, since Ti forms a Ti oxide film on the surface of duplex stainless steel during diffusion bonding and welding, which leads to a decrease in diffusion bondability and weldability, the Ti content should be 0.1% or less, preferably 0.03% or less.
[0024] (Al: 0.1% or less) Al (aluminum) is an effective element as a deoxidizer and can be added as necessary. However, since an Al oxide film is formed on the surface of duplex stainless steel during diffusion bonding and welding, resulting in reduced diffusion bonding and weldability, the Al content should be 0.1% or less, preferably 0.03% or less.
[0025] (P:0.04% or less) P (phosphorus) is an element that contributes to solid solution strengthening, but also reduces corrosion resistance. Therefore, the lower the P content, the better. Therefore, the P content is set to 0.04% or less, preferably 0.035% or less.
[0026] (S:0.015% or less) S (sulfur) is an element that forms MnS, which is likely to be the starting point of pitting corrosion, and impairs corrosion resistance. In addition, when S segregates at the grain boundaries of the austenite phase, hot workability is reduced. Therefore, the lower the S content, the better. Therefore, the S content is set to 0.015% or less, and preferably 0.010% or less.
[0027] (Mo: 2.0% or less) Mo (molybdenum) is a ferrite forming element, and together with Cr, it acts to improve corrosion resistance without reducing tensile strength. On the other hand, excessive Mo can lead to a decrease in machinability. Therefore, the Mo content is set to 2.0% or less, preferably 1.0% or less.
[0028] (V:0.5% or less) Vanadium (V) works with Cr to improve corrosion resistance without reducing tensile strength and machinability. It also fixes solute carbon as carbides, which contributes to improving machinability. On the other hand, if the amount is too high, it can harden the duplex stainless steel, resulting in reduced manufacturability. Therefore, the V content is set to 0.5% or less, and preferably 0.35% or less.
[0029] (B: 0.0001~0.01%) The addition of a small amount of B (boron) improves the strength of the grain boundaries at high temperatures, and is effective in improving machinability. For this reason, in the present invention, B can be added as necessary. To fully obtain this effect, it is effective to ensure a B content of 0.0001% or more. However, the addition of excessive B leads to the formation of borides, which in turn reduces deformability at high temperatures. The B content should be 0.01% or less, and preferably 0.006% or less.
[0030] (Ca, Mg, Y, REM, etc.) Other elements such as Ca (calcium), Mg (magnesium), Y (yttrium), and REM (rare earth metal elements) are likely to be mixed into duplex stainless steel from the scrap raw materials, refractories in the smelting equipment, deposits on the furnace walls, slag, etc., but the unavoidable impurities of Ca, Mg, Y, and REM are permitted to be mixed in up to a total of 0.01%. The remainder is Fe.
[0031] (M value) In the duplex stainless steel of the present invention, the austenite phase formed in the high temperature region is converted to martensite phase at room temperature, and a duplex structure of ferrite phase and martensite phase is formed at room temperature. The volume fraction of the austenite phase in the metal structure is controlled in the temperature range where the diffusion bonding method and the welding method can be carried out, and the volume fraction of the martensite phase and the coexisting ferrite phase at room temperature is also controlled.
[0032] The inventors produced duplex stainless steels with varying contents of Ni, Mn, Cu, Cr, Si, and Mo, which are metal elements that have a large influence on the volume fraction of the austenite phase, and further, taking into account the melting temperature, created the following equation (1) for deriving the M value, which is an index representing the volume fraction of the austenite phase. Formula (1): M value = -0.22T + 34.5Ni + 10.5Mn + 13.5Cu-17.3Cr-17.3Si-18Mo + 475.5
[0033] In formula (1), the T value represents the temperature (°C) in the range of 950 to 1100. In the diffusion bonding method, pressure is applied at a temperature below the melting point of the base material to minimize plastic deformation, the surface film of the joint is removed, and the joint surfaces are bonded together. Therefore, the applicable temperature range is set to 950 to 1100°C because evaluation at this temperature makes it possible to obtain duplex stainless steel with excellent diffusion bonding properties.
[0034] Among the metal elements contained, Ni, Mn, and Cu are elements that are included in Fe and form the austenite phase in the temperature range of the diffusion bonding method. On the other hand, Cr, Si, and Mo are elements that form the ferrite phase. The other elements also have some effect, but their influence is smaller than that of Ni, Cr, etc. Therefore, the M value can be controlled by controlling the content of the metal elements such as Ni and Cr listed in this formula (1).
[0035] When duplex stainless steel is a single phase austenite, the M value is 100, and when it is a single phase ferrite, the M value is 0. However, when the M value exceeds 100 according to calculations, it is set to 100, and when it is 0 or less, it is set to 0. Furthermore, in duplex stainless steel, the C and N contents are both kept low at 0.03% or less so that retained austenite phase does not form when the austenite phase that exists at high temperatures is rapidly cooled to form martensite phase.
[0036] (multiphase structure) The duplex stainless steel of the present invention has a duplex structure of ferrite and martensite phases at room temperature. In the duplex stainless steel of the present invention, the temperature range to which the diffusion bonding method is applied is 950 to 1100°C, and the M value is in the range of 35 to 65. The range is preferably 37.5 to 62.5, and more preferably 40 to 60. At the interface between the ferrite phase and the martensite phase, which have different compositions or crystal structures, the ferrite phase and the martensite phase are less likely to move than at the interface between the phases having the same composition or crystal structure. Therefore, when the ratio of the ferrite phase and the austenite phase is equal, the ratio of the interface between the phases is the highest, the movement is restricted, and coarsening is suppressed. For this reason, the closer the phase ratio of the ferrite phase and the martensite phase is to 50:50, the more grain growth is suppressed.
[0037] If the M value is less than 35, the austenite phase is small, the pinning effect is insufficient, the grain size of the ferrite phase becomes coarse, grain boundary sliding is suppressed, and diffusion bondability is reduced. If the M value exceeds 65, the ferrite phase is small, the pinning effect is insufficient, the austenite phase becomes coarse, grain boundary sliding is suppressed, and diffusion bondability is reduced.
[0038] In Patent Document 1, it is considered that the grain size can be finely controlled if the second phase is present at 10%. However, in the duplex stainless steel of the present invention, the ferrite phase and the austenite phase check each other, forming a second phase with a ratio of 35 to 65. This allows each phase to exert a pinning effect on the other phase, preventing the grain size of the other phase from becoming coarse, while causing a certain degree of grain boundary sliding, thereby achieving diffusion bondability.
[0039] The duplex stainless steel of the present invention is used in a diffusion bonding method by a direct method without using an insert welding material. In the temperature range where diffusion bonding proceeds, this duplex stainless steel maintains a fine structure by suppressing the grain growth that occurs between the ferrite phase and the austenite phase at high temperatures, and easily causes creep deformation caused by grain boundary sliding. As a result, deformation is easily promoted at the uneven parts of the bonding surface, making diffusion bonding possible. Furthermore, by containing Cu and Sn, the slipperiness of the grain boundaries is improved and excessive grain boundary sliding is suppressed, preventing deformation of the material by the diffusion bonding method and obtaining excellent strength when bonded.
[0040] In the duplex stainless steel of the present invention, a specific diffusion bonding method is, for example, a direct contact state with a contact surface pressure of 0.1 to 1.0 MPa, and a pressure of 1.0 × 10 -2 Pa or less, preferably 1.0×10 -3 Diffusion bonding is carried out by heating and holding the material in a furnace with a temperature of 950 to 1100°C and a dew point of -40°C or less for a period of 0.5 to 3 hours.
[0041] In addition to the diffusion bonding method, the duplex stainless steel of the present invention can also be used in welding methods that melt the base metal itself and then cool it to bond it, without using an insert rod, welding rod, brazing material, etc. For example, it can be used in the TIG method, the MiG method, the laser method, the high-frequency method, etc.
[0042] In duplex stainless steel, the austenite phase formed during melting is rapidly cooled to form a hard martensite phase in the heat-affected zone, and carbides are formed locally, reducing the toughness of the weld. In duplex stainless steel, Cr carbides are more likely to precipitate at the grain boundaries than within the grains, and after welding, Cr carbides are preferentially precipitated at the grain boundaries. When Cr carbides are preferentially precipitated at the grain boundaries, the amount of solute Cr decreases, Cr-depleted areas are formed along the grain boundaries, and corrosion resistance is reduced.
[0043] Therefore, the duplex stainless steel of the present invention can obtain excellent weldability by suppressing the formation of Cr-depleted regions by adding Nb. Nb fixes C and N and prevents intergranular corrosion. Therefore, the duplex stainless steel of the present invention has a low C and N content and specifies the Nb content corresponding to the C and N content.
[0044] The duplex stainless steel of the present invention can be applied to parts manufactured by welding after diffusion bonding. The duplex stainless steel can be used for diffusion bonding by specifying the composition of metal elements such as Cu and Sn and the M value of the ferrite phase and the martensite phase, and can also be used for welding by specifying Nb in the composition.
[0045] (Average grain size before bonding) As a duplex stainless steel, high strength is achieved by grain refinement. In the case of a duplex phase of ferrite and martensite, in addition to grain refinement, a hard martensite phase is included, so that even higher strength can be obtained. In addition, the finer the grain size, the better the diffusion bonding. The finer the grain structure of the duplex stainless steel of the present invention, the smaller the unevenness on the bonding surface and the larger the bonding area, so that the diffusion bonding process can proceed quickly. Therefore, the average grain size before bonding is preferably 20 μm or less, more preferably 10 μm or less.
[0046] The grain size is the average grain size of the duplex stainless steel before diffusion bonding, and is calculated by dividing the metal structure of the plate thickness cross section parallel to the cold rolling direction by 1 mm. 2Based on the above observations, the number of crystal grains contained within a unit area is calculated using the quadrature method, and the value calculated by multiplying the average area per crystal grain by the power of 1 / 2 is used.
[0047] (Manufacturing of duplex stainless steel) First, the raw material of the duplex stainless steel is melted, and oxygen is blown into the molten steel to decarburize it, and Si is added to react with the oxygen in the molten steel to reduce the oxygen concentration. Next, the melted molten steel is made into a slab by continuous casting, and the slab is heated to 1100 to 1300 ° C and hot rolled to make a hot rolled steel strip. The hot rolled steel strip is annealed and then pickled, or pickled without annealing. When annealing is performed, continuous annealing at about 900 to 1150 ° C or batch annealing at 600 to 900 ° C is preferred. After pickling, the strip is cold rolled to a predetermined thickness, and then finish annealing is performed. The finish annealing temperature is in the range of 700 to 1150 ° C, preferably 850 to 1100 ° C. In addition, intermediate annealing and intermediate rolling may be performed before finish annealing as necessary, for example, when the final thickness is thin. EXAMPLES
[0048] Examples will be described below, but the present invention is not limited to the following examples.
[0049] The duplex stainless steels of Examples 1 to 5 and Comparative Examples 1 to 7 having the composition shown in Table 1 were melted and hot rolled to produce hot-rolled sheets with a thickness of 3 mm. Then, the sheets were cold rolled to a thickness of 1.0 mm, finish annealed at 1000 to 1070°C, and pickled to obtain test materials.
[0050] Figure 1 is a photograph showing the metal structure composed of martensite and ferrite phases. It can be seen that the alloy exhibits a fine structure composed of martensite and ferrite phases with a grain size of 10 μm or less.
[0051] The amounts of addition in Table 1 are all in mass%, with the remainder being Fe and unavoidable impurities. Additionally, (-) indicates that no addition was made, and underlining indicates that the composition is outside the range of the present invention. Additionally, in Comparative Example 5, the amount of Nb can be calculated from the amounts of C and N to be 7×(C+N)=0.469, but the composition is 0.10%, which is outside the range of the present invention. Similarly, in Comparative Example 6, the amount of Nb can be calculated to be 7×(C+N)=0.149, but the composition is 0.03%, which is outside the range of the present invention.
[0052] [Table 1]
[0053] Table 2 also shows the M values in formula (1) at temperatures of 950, 1000, 1050 and 1100° C. The underlines indicate that the M values are outside the range of the present invention.
[0054] [Table 2]
[0055] (Diffusion bonding test) A flat test piece of 20 mm × 20 mm was taken from each steel plate and diffusion-bonded in the following manner. Two test pieces of the same steel material were stacked together so that their surfaces were in contact with each other, and pressure was applied to the contact surfaces of the two test pieces so that the surface pressure was 0.1 MPa. The initial vacuum was 1.0 × 10 -3 ~1.0×10 -4 The temperature was raised to 1000°C at 90 kPa in about 1 h, and the sample was held at that temperature for 2 h before being transferred to a cooling chamber and cooled. The above degree of vacuum was maintained until the sample was cooled to 900°C, after which Ar gas was introduced and the sample was cooled to below about 100°C in an Ar gas atmosphere at 90 kPa.
[0056] FIG. 2 shows the test specimens used in the bondability test. The laminated body after the above heat treatment was measured for thickness at 49 measurement points set at 3 mm pitch on the surface of the laminated body of 20 mm × 20 mm as shown in Figure 2 using an ultrasonic thickness gauge (Olympus; Model 35DL). The probe diameter was 1.5 mm. When the measured thickness at a certain measurement point indicates the total thickness of two steel sheets, it can be considered that the two steel sheets are integrated at the interface position of the two steel sheets corresponding to that measurement point by atomic diffusion. On the other hand, when the measured thickness is less than the total thickness of both steel sheets, there is an unjoined part (defect) at the interface position of the two steel sheets corresponding to that measurement point. When the correspondence relationship between the cross-sectional structure of the laminated body after the heat treatment and the measurement results obtained by this measurement method was examined, it was confirmed that the area ratio of the joint part in the contact area can be accurately evaluated by the value obtained by dividing the number of measurement points where the measurement result is the total thickness of both steel sheets by the total number of measurements, 49, and rounding off the decimal point (hereinafter referred to as the "joining ratio"). Therefore, the diffusion bonding was evaluated using the following evaluation criteria. Furthermore, a similar evaluation was performed when the diffusion bonding temperature was set to 950°C, 1050°C, and 1100°C.
[0057] The evaluation criteria are as follows: ◎: Bonding rate 100% (excellent) ○: Bonding rate 90~99% (good) △: Bonding rate 60-89% (slightly poor) ×: Bonding rate 0~59% (defective) When the bonding rate is 90% or more, which is evaluated as (◎) or (◯), the sealing property between the two components (the property of preventing gas leakage through communicating defects) is good and the strength of the diffusion bond is sufficiently secured, so the diffusion bond is judged to be acceptable.
[0058] (Corrosion resistance test) The corrosion resistance of the welds was evaluated by performing an appearance evaluation in a corrosion resistance test using a salt-dry-wet cyclic test in which cold-rolled annealed sheets were welded by the TIG method and subjected to repeated "salt spray, drying, and wetting." The test pieces were cut into rectangles measuring 25 mm (width direction) x 100 mm (rolling direction) by machining, butted together, and welded by the TIG method. The end faces used for corrosion resistance evaluation (hereinafter referred to as "evaluation faces") were wet-polished to #600, then covered with silicone sealant and fixed to a Bakelite base to prepare test pieces for corrosion resistance testing. The test pieces were subjected to a salt-dry-wet cycle test. The corrosion resistance test consisted of spraying 5% NaCl for 15 minutes in a 35°C atmosphere, then holding for 1 hour in a 60°C, 30% relative humidity atmosphere to dry, and then holding for 3 hours in a 50°C, 95% relative humidity, wet environment, and repeating this cycle for 50 cycles. The amount of salt spray was adjusted to 1.5 ml / cm2·h. The corrosion resistance was judged by visually inspecting the appearance of the weld and the degree of corrosion of the base material. FIG. 3 is a diagram for explaining the weldability test, in which (a) is a diagram showing the measurement specimen used in the weldability test, (b) is an example with corrosion resistance, and (c) is an example with poor corrosion resistance.
[0059] The evaluation criteria are as follows: ○: Corrosion resistant ×: No corrosion resistance If there is no difference in the level of corrosion between the weld and the base material upon appearance, it is judged to have corrosion resistance (O); if there is a difference in the level of corrosion between the weld and the base material upon appearance, it is judged to have no corrosion resistance (X).
[0060] (Evaluation Results) Table 3 shows the evaluation results of the diffusion bondability test and the weld corrosion resistance test for Examples 1-5 and Comparative Examples 1-7. [Table 3]
[0061] In the invention examples 1 to 5, the M value is in the range of 35 to 65 in the temperature range of 950 to 1100°C, and all metal elements including Cu and Sn are within the appropriate range. Therefore, the diffusion bondability is excellent (◎) or good (◯), indicating excellent diffusion bondability. In addition, since all metal elements including Nb are within the appropriate range, the weld corrosion resistance is all good (◯). Therefore, it is understood that Examples 1 to 5 can be practically used without any problems in either the diffusion bonding method or the welding method.
[0062] On the other hand, in Comparative Examples 1 and 2, since the M value is outside the range of 35 to 65 within the temperature range of 950 to 1100°C, even though the composition of the metal elements is within the range of the present invention, the diffusion bondability is low and the bond rate is poor (×).
[0063] In Comparative Example 3, the M value is in the range of 35 to 65 in the temperature range of 950 to 1100°C. However, the Al content in the composition is higher than the range of the present invention, and therefore, when the temperature becomes high during diffusion bonding, an Al oxide film is formed, which inhibits bonding, resulting in low diffusion bondability and a slightly poor bonding rate (△). In Comparative Example 4, the M value is in the range of 35 to 65 in the temperature range of 950 to 1100°C. However, the Ti content in the composition is higher than the range of the present invention, and therefore, when the temperature becomes high during diffusion bonding, a Ti oxide film is formed, which inhibits bonding, resulting in low diffusion bondability and a poor bonding rate (×).
[0064] In Comparative Example 5, the M value is in the range of 35 to 65 in the temperature range of 950 to 1100°C, and the diffusion bondability is high and the bond rate is excellent (◎). However, the C content is high in the composition, and the Cr and Nb contents are low, so the weld corrosion resistance is poor (×). In Comparative Example 6, the M value is in the range of 35 to 65 in the temperature range of 950 to 1100°C, and the diffusion bondability is high and the bond rate is excellent (◎). However, the Nb content is low in the composition, and therefore the formation of Nb carbide is low, and as a result, the formation of Cr carbide causes intergranular corrosion, and the weld corrosion resistance is poor (×).
[0065] Comparative Example 7 contains Nb and thus has good weld corrosion resistance (◯), but does not contain Cu or Sn and thus has low diffusion bondability and a somewhat poor bond rate (Δ).
Claims
1. A duplex stainless steel having excellent diffusion bondability and weldability, containing, by mass%, C: 0.03% or less, Si: 0.01 to 1.00%, Mn: 0.01 to 2.50%, P: 0.04% or less, S: 0.015% or less, Ni: 1.5 to 5.5%, Cr: 17.5 to 22.0%, Cu: 0.01 to 2.0%, Sn: 0.001 to 0.1%, N: 0.03% or less, Nb: 7 × (C + N) to 0.70%, Ti: 0.1% or less, and Al: 0.1% or less, with the balance being Fe and unavoidable impurities, and having an M value represented by the following formula (1) in the range of 35 to 65 in any temperature range when the T value is 950 to 1100 (°C), and having a duplex structure of ferrite phase and martensite phase. Formula (1): M value = -0.22T + 34.5Ni + 10.5Mn + 13.5Cu - 17.3Cr - 17.3Si - 18Mo + 475.5 However, the content value of the element expressed in mass% is substituted into the element symbol on the right side of formula (1), and here, 0 (zero) is substituted into the element symbol for Mo.
2. The duplex stainless steel according to claim 1, further comprising, by mass%, one or more of Mo: 2.0% or less, V: 0.5% or less, and B: 0.0001 to 0.01%. However, when Mo is not contained, 0 (zero) is substituted for the Mo element symbol.
Citation Information
Patent Citations
Stainless steel for brazing and brazing method
JP2010065278A
Dual phase structure stainless steel sheet and steel strip, and methods for manufacturing the same
JP2011225970A
Ferritic stainless steel plate excellent in heat resistance
JP2013204136A
Stainless steel material for diffusion junction
JP2016089223A
Dual-phase structure stainless steel sheet, member, and method for manufacturing brake disc