Ferritic Stainless Steel
By controlling the chemical composition and selectively removing the oxide film on ferritic stainless steel to form a pattern, the material achieves both design aesthetics and enhanced corrosion resistance through a high Cr fraction passive film on the exposed base.
Patent Information
- Application Number
- JP2020218545
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-12-28
- Publication Date
- 2024-10-09
- Estimated Expiration
- 2040-12-28
AI Technical Summary
The formation of patterns on stainless steel surfaces using black oxide films leads to reduced corrosion resistance due to exposure of the stainless steel base, which is prone to early rusting.
A ferritic stainless steel material with controlled chemical composition and selective removal of the black oxide film and internal oxide layer to expose the base, maintaining a specific difference in brightness and gloss, and forming a passive film with a high Cr fraction on the exposed part to enhance corrosion resistance.
The solution provides a stainless steel material with excellent design properties and improved corrosion resistance by ensuring the exposed base portion has a high Cr fraction passive film, preventing rusting and maintaining aesthetic appeal.
Smart Images

Figure 0007564707000003 
Figure 0007564707000004 
Figure 0007564707000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a ferritic stainless steel material having excellent designability and corrosion resistance, which has a black oxide film on its surface and a pattern formed by removing part of it to expose the stainless steel base material. [Background technology]
[0002] Stainless steel is not only a material with excellent corrosion resistance, but is also used as interior and exterior building materials, taking advantage of its shiny silver-white surface. In recent years, in order to enhance the design of stainless steel, it has become common to impart colors, typically black, to stainless steel using methods such as chemical coloring, painting, and oxidation treatment. Furthermore, colored stainless steel may be polished or etched to partially expose the stainless steel base material and impart a pattern.
[0003] Patent Document 1 describes a pattern forming method in which a stainless steel surface that has been colored by a chemical coloring method is mechanically polished to roughen the surface into a predetermined pattern, while Patent Document 2 describes a method for producing a plated steel sheet in which a pattern is imparted to the surface of a Zn-plated steel sheet that has been formed with a black oxide film by an oxidation treatment method by mechanically polishing the surface.
[0004] Furthermore, Patent Documents 3 and 4 describe black stainless steel sheets in which a black oxide film is formed on the surface of the stainless steel by an oxidation treatment method. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] Japanese Patent Application Publication No. 61-213380 [Patent Document 2] JP 2017-218647 A [Patent Document 3] JP 2019-178392 A [Patent Document 4] JP 2018-135591 A Summary of the Invention [Problem to be solved by the invention]
[0006] Incidentally, when a black oxide film is formed on the surface of a stainless steel base material and then part of it is polished to expose the base material to form a pattern, although the design is attractive, there is a problem in that the stainless steel base material exposed by polishing has lower corrosion resistance than the surrounding area covered with the black oxide film and often rusts early.
[0007] The present invention has been made to solve the above-mentioned problems, and aims to provide a ferritic stainless steel material with excellent designability and corrosion resistance, which has a black oxide film on its surface and a pattern formed by further removing part of the black oxide film to expose the base material of the stainless steel material. [Means for solving the problem]
[0008] The inventors conducted intensive research to solve the above-mentioned problems and discovered that the cause of the decrease in corrosion resistance that occurs when a stainless steel material having a black oxide film on its surface is polished to form a pattern is that part of the oxide film is removed by polishing, exposing a layer (internal oxide layer) containing a large number of internal oxides such as Ti oxide (TiO2) and Al oxide (Al2O3) directly below the oxide film, and that the composition of the passive film that is formed on the exposed base surface due to exposure to high temperatures during polishing is low in Cr and high in Fe.
[0009] That is, they found that it is possible to suppress a decrease in corrosion resistance of the exposed substrate by controlling the composition of the ferritic stainless steel, by removing the oxide film and the inner oxide layer when exposing the substrate by polishing, and by increasing the Cr fraction in the passive film formed on the exposed substrate. They further found that the removal state of the oxide film and the inner oxide layer can be confirmed by checking the difference in brightness and gloss between the oxide film and the exposed substrate within a specific range, which led to the present invention. The gist of the present invention, which was completed based on the above findings, is as follows.
[0010] (1) A ferritic stainless steel material according to one embodiment of the present invention has a composition, in mass%, of C: 0.050% or less, Si: 1.00% or less, Mn: 0.04 to 1.00%, P: 0.050% or less, S: 0.030% or less, Cr: 16.00 to 25.00%, Ni: 1.00% or less, Cu: 0.60% or less, Mo: 2.00% or less, N: 0.030% or less, Al: 0.500% or less, Ti: 0.080 to 0.500%, Nb: 0.500% or less, and the total content of Nb and Ti is 6 (C + N) or more (C and N represent the contents of C and N, respectively), with the balance being Fe and impurities, as a base material, and a surface of the base material has a lightness index L * ≦45.0, Chromathetics index -5.0≦a * ≦5.0, -5.0≦b * The present invention has an oxide film portion on which a black oxide film satisfying a gloss level GS(60°)≦5.0 and a gloss level GS(60°)≦40.0 is formed, and a base material exposed portion on which the oxide film is not formed, and a pattern is formed by the oxide film portion and the base material exposed portion, and a difference in brightness index ΔL between the oxide film portion and the base material exposed portion is * ≧30.0 and gloss difference ΔGS(60°) ≧130.0, and the passive film formed on the surface of the exposed substrate portion satisfies a Cr fraction ≧30%.
[0011] (2) The ferritic stainless steel material described in (1) above may further contain, in the composition of the ferritic stainless steel, one or more elements selected from the group consisting of Zr: 1.00% or less, Co: 1.00% or less, V: 1.00% or less, and W: 1.00% or less, in mass percent.
[0012] (3) The ferritic stainless steel material described in (1) or (2) above may further contain, in mass %, one or more elements selected from the group consisting of REM: 0.100% or less and Ca: 0.100% or less in the composition of the ferritic stainless steel.
[0013] (4) The ferritic stainless steel material according to any one of (1) to (3) above may further contain, in mass %, one or more elements selected from the group consisting of Sn: 0.100% or less and B: 0.0100% or less in the composition of the stainless steel. Effect of the Invention
[0014] According to the above aspect of the present invention, a ferritic stainless steel material having excellent designability and corrosion resistance can be provided, which has a black oxide film on the surface and a pattern formed by removing part of the black oxide film to expose the base material. [Brief description of the drawings]
[0015] [Figure 1] FIG. 1 is a schematic diagram for explaining the process up to the formation of a pattern, where (a) is a cross-sectional view showing the vicinity of the surface layer of the base material before a black oxide film is formed, (b) is a cross-sectional view showing the vicinity of the surface layer of the base material after a black oxide film has been formed, and (c) is a cross-sectional view showing the vicinity of the surface layer of the stainless steel material after a pattern has been formed by polishing. [Diagram 2] FIG. 2 shows a top view and a side view of the bonded structure used in the corrosion resistance test. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0016] The following is a detailed description of the embodiments of the present invention. The present invention is not limited to the following embodiments, and it should be understood that modifications and improvements to the following embodiments, which are made based on the ordinary knowledge of those skilled in the art, fall within the scope of the present invention, without departing from the spirit of the present invention.
[0017] <1. Ferritic stainless steel material according to this embodiment> (1.1 Chemical composition) The base material of the ferritic stainless steel material according to this embodiment (hereinafter, sometimes simply referred to as "stainless steel material") has a composition of, in mass%, C: 0.050% or less, Si: 1.00% or less, Mn: 0.04 to 1.00%, P: 0.050% or less, S: 0.030% or less, Cr: 16.00 to 25.00%, Ni: 1.00% or less, Cu: 0.60% or less, Mo: 2.00% or less, N: 0.030% or less, Al: 0.500% or less, Ti: 0.080 to 0.500%, Nb: 0.500% or less, and the total content of Nb and Ti is 6 (C + N) or more (C and N represent the contents of C and N, respectively), with the balance being Fe and impurities. That is, the base material of the stainless steel material according to this embodiment has a chemical composition in which the metal structure at room temperature is mainly ferrite phase.
[0018] In this specification, the term "impurities" refers to components that are mixed in during industrial production of the base ferritic stainless steel due to various factors in the raw materials such as ores and scraps, and the manufacturing process, and are acceptable within a range that does not adversely affect the present invention. For example, impurities also include unavoidable impurities.
[0019] The base material of the stainless steel material according to the present embodiment may further contain, by mass%, one or more elements selected from the group consisting of Zr: 1.00% or less, Co: 1.00% or less, V: 1.00% or less, and W: 1.00% or less. The base material of the stainless steel material according to the present embodiment may further contain, by mass%, one or more elements selected from the group consisting of REM: 0.100% or less, and Ca: 0.100% or less. The base material of the stainless steel material according to the present embodiment may further contain, by mass%, one or more elements selected from the group consisting of Sn: 0.100% or less, and B: 0.0100% or less. The reasons for limiting the content of each element will be explained below.
[0020] (C: 0.050% by mass or less) C is an element that affects the properties of stainless steel materials, such as intergranular corrosion resistance (sensitization suppression effect) and workability. If the C content is too high, the workability and intergranular corrosion resistance of the stainless steel material will decrease. Therefore, the upper limit of the C content is 0.050 mass%, preferably 0.045 mass%, and more preferably 0.040 mass%. On the other hand, the lower limit of the C content is not particularly limited, but reducing the C content leads to an increase in refining costs. Therefore, the lower limit of the C content is preferably 0.0005 mass%, and preferably 0.001 mass%.
[0021] (Si: 1.00% by mass or less) Silicon is an element that improves the oxidation film peeling resistance and high-temperature oxidation resistance of stainless steel materials. If the Si content is too high, the workability and toughness decrease. Therefore, the upper limit of the Si content is 1.00 mass%, preferably 0.90 mass%, and more preferably 0.80 mass%. On the other hand, the lower limit of the Si content is not particularly limited, but is preferably 0.05 mass%, more preferably 0.10 mass%, and even more preferably 0.15 mass%, from the viewpoint of suppressing deterioration of surface quality due to oxide film peeling during the production of stainless steel materials.
[0022] (Mn:0.04~1.00% by mass) Mn is a useful element as a deoxidizing element and is also effective in improving oxidation film peeling resistance and high-temperature oxidation resistance. In addition, Mn is effective in forming a black color tone by forming a complex oxide with Cr. If the Mn content is too high, MnS, which is the starting point of corrosion, is easily generated and the ferrite phase is destabilized. Therefore, the upper limit of the Mn content is 1.00 mass%, preferably 0.95 mass%, and more preferably 0.90 mass%. On the other hand, if the Mn content is too low, the above effects may not be sufficiently obtained. Therefore, the lower limit of the Mn content is 0.04 mass%, and preferably 0.05 mass%.
[0023] (P: 0.050 mass% or less) P is an element that affects the properties of stainless steel materials, such as weldability and workability. If the P content is too high, the above properties may be degraded. Therefore, the upper limit of the P content is 0.050 mass%, preferably 0.045 mass%, and more preferably 0.040 mass%. On the other hand, the lower limit of the P content is not particularly limited, but reducing the P content leads to an increase in refining costs. Therefore, the lower limit of the P content is preferably 0.001 mass%, and more preferably 0.010 mass%.
[0024] (S: 0.030% by mass or less) S is an element that generates MnS, which is a corrosion starting point, and affects the properties of stainless steel materials, such as toughness. If the S content is too high, the above properties may be reduced. Therefore, the upper limit of the S content is 0.030 mass%, preferably 0.025 mass%, and more preferably 0.020 mass%. On the other hand, the lower limit of the S content is not particularly limited, but reducing the S content leads to an increase in refining costs. Therefore, the lower limit of the S content is preferably 0.0001 mass% or more, and more preferably 0.0005 mass% or more.
[0025] (Cr:16.00~25.00% by mass) Cr is an element effective in improving the corrosion resistance and oxidation resistance of stainless steel materials. If the Cr content is too high, the toughness of the stainless steel material decreases, and the growth of the oxide film is inhibited, making it impossible to form an oxide film having a black color tone. Therefore, the upper limit of the Cr content is 25.00 mass%, preferably 24.50 mass%, and more preferably 24.00 mass%. On the other hand, if the Cr content is too low, the above effects may not be sufficiently obtained. Therefore, the lower limit of the Cr content is 16.00 mass%, and preferably 16.50 mass%.
[0026] (Ni: 1.00% by mass or less) Ni is an element effective for improving the corrosion resistance and toughness of stainless steel materials. If the Ni content is too high, the ferrite phase becomes unstable and the manufacturing cost increases. Therefore, the upper limit of the Ni content is 1.00 mass%, preferably 0.90 mass%, and more preferably 0.80 mass%. On the other hand, the lower limit of the Ni content is not particularly limited, but is preferably 0.01 mass%, and more preferably 0.05 mass%, from the viewpoint of obtaining the above-mentioned effects.
[0027] (Cu: 0.60% by mass or less) Cu is an element effective for improving the corrosion resistance of stainless steel materials. If the Cu content is too high, the ferrite phase becomes unstable and the manufacturing cost increases. Therefore, the upper limit of the Cu content is 0.60 mass%, preferably 0.55 mass%, and more preferably 0.50 mass%. On the other hand, the lower limit of the Cu content is not particularly limited, but is preferably 0.001 mass%, and preferably 0.01 mass%.
[0028] (Mo: 2.00% by mass or less) Mo is an element effective for improving the corrosion resistance and oxidation resistance of stainless steel materials. If the Mo content is too high, the workability of the stainless steel material decreases, the manufacturing cost increases, and the oxidation resistance improves, making it difficult to form a black oxide film. Therefore, the upper limit of the Mo content is 2.00 mass%, preferably 1.90 mass%. On the other hand, the lower limit of the Mo content is not particularly limited, but is preferably 0.001 mass%, preferably 0.01 mass%.
[0029] (N: 0.030% by mass or less) N is an element that affects properties such as intergranular corrosion resistance (sensitization suppression effect) and workability. If the N content is too high, the intergranular corrosion resistance and workability of the stainless steel material will decrease. In addition, as described later, Ti is required for the formation of a black oxide film, but if the N content is high, TiN will precipitate, reducing the amount of solid-solubilized Ti in the steel, and the formation of the black oxide film will be inhibited. In addition, the formed nitrides are likely to become the starting point of corrosion, reducing the corrosion resistance, especially the pitting corrosion resistance. Therefore, the upper limit of the N content is 0.030 mass%, preferably 0.028 mass%, and more preferably 0.025 mass%. On the other hand, the lower limit of the N content is not particularly limited, but reducing the N content leads to an increase in refining costs. Therefore, the lower limit of the N content is preferably 0.0005 mass%, and preferably 0.001 mass%.
[0030] (Al: 0.500% by mass or less) Al is an element that effectively acts to suppress peeling of the oxide film by forming Al oxide on the surface of the stainless steel material when a black oxide film is formed. On the other hand, if the Al content is too high, the toughness of the stainless steel material decreases. Therefore, the upper limit of the Al content is 0.500 mass%, preferably 0.450 mass%, and more preferably 0.400 mass%. On the other hand, the lower limit of the Al content is not particularly limited, but is preferably 0.001 mass%, and preferably 0.010 mass%.
[0031] (Nb: 0.500 mass% or less, Ti: 0.080 to 0.500 mass%, total content of Nb and Ti: 6(C+N) or more) Nb and Ti are elements that affect properties such as intergranular corrosion resistance (sensitization suppression effect). Furthermore, Ti forms a complex oxide with Cr, giving the oxide film a black appearance.
[0032] If the Nb content is too high, the workability and toughness of the stainless steel material will decrease. Therefore, the upper limit of the Nb content is 0.500 mass%, preferably 0.480 mass%, and more preferably 0.450 mass%. If the Ti content is too high, the workability and surface quality of the stainless steel material will decrease. Therefore, the upper limit of the Ti content is 0.500 mass%, preferably 0.480 mass%, and more preferably 0.450 mass%.
[0033] On the other hand, the lower limit of the Nb and Ti content is controlled based on the relationship with the C and N content that reduces intergranular corrosion resistance. Specifically, the lower limit of the total content of Nb and Ti is 6 (C+N), preferably 7 (C+N), and more preferably 8 (C+N). Here, C and N represent the C and N contents, respectively. Also, if the Ti content is too low, the above-mentioned effects may not be sufficiently obtained. Therefore, the lower limit of the Ti content is 0.080 mass%, preferably 0.090 mass% or more, and more preferably 0.100 mass%.
[0034] (Zr: 1.00 mass% or less, Co: 1.00 mass% or less, V: 1.00 mass% or less, W: 1.00 mass% or less) Zr, Co, V and W are elements effective for improving the oxidation resistance of stainless steel materials. If the content of Zr, Co, V and W is too high, the workability and toughness of the stainless steel material will decrease, and the manufacturing cost will increase. Therefore, the upper limit of the content of Zr, Co, V and W is 1.0 mass%, preferably 0.8 mass%, and more preferably 0.5 mass%. On the other hand, the lower limit of the content of Zr, Co, V and W is not particularly limited, but is preferably 0.001 mass%, and more preferably 0.01 mass%.
[0035] (REM: 0.100 mass% or less, Ca: 0.100 mass% or less) REM and Ca are elements effective in improving the oxidation resistance of stainless steel materials. If the content of REM and Ca is too high, it leads to an increase in the manufacturing cost of stainless steel. Therefore, the upper limit of the content of REM and Ca is 0.100 mass%, preferably 0.080 mass%, and more preferably 0.05 mass%. On the other hand, the lower limit of REM and Ca is not particularly limited, but is preferably 0.0001 mass%, more preferably 0.003 mass%. REM is a collective term for 17 elements in total, including Sc, Y, and lanthanoids, and means rare earth metals. Specifically, La, Ce, Nd, etc. can be mentioned, and one of these can be contained alone, or two or more can be contained in combination. When two or more rare earth elements are contained, the above REM content means the total content of these rare earth elements. As a method of addition, for example, a misch metal (MM), which is a mixture of rare earth elements, may be used to contain the REM content in the above range.
[0036] (Sn: 0.100% by mass or less) Sn is an element effective for improving the corrosion resistance of stainless steel materials. If the Sn content is too high, Sn segregates and manufacturability decreases. Therefore, the upper limit of the Sn content is 0.100 mass%, preferably 0.080 mass%, and more preferably 0.050 mass%. On the other hand, the lower limit of the Sn content is not particularly limited, but is preferably 0.001 mass%, and more preferably 0.005 mass%.
[0037] (B: 0.0100% by mass or less) B is an element effective for improving the secondary workability of stainless steel materials. If the B content is too high, the fatigue strength of the stainless steel decreases. Therefore, the upper limit of the B content is 0.0100 mass%, preferably 0.0080 mass%, and more preferably 0.0050 mass%. On the other hand, the lower limit of the B content is not particularly limited, but is preferably 0.0001 mass%, and more preferably 0.0005 mass%.
[0038] (1.2 Composition of stainless steel materials) FIG. 1(c) is a cross-sectional view in the plate thickness direction, which is a schematic diagram showing the vicinity of the surface layer of the stainless steel material according to this embodiment, as described later. Referring to FIG. 1(c), the stainless steel material 1 according to this embodiment has an oxide film 4 having a black color tone on the surface, and has a design consisting of a pattern intentionally formed for decoration or other purposes by partially removing this black oxide film 4 by polishing. The stainless steel material according to this embodiment has a ferritic stainless steel base material 3 (hereinafter, simply referred to as "base material") and an oxide film 4 having a black color tone formed on the surface of the base material 3. The stainless steel material 1 according to this embodiment also has a base material exposed portion 7 in which a part of the black oxide film 4 and the internal oxide layer 5 immediately below it have been removed to partially expose the base material. A passive film 8 is formed on the base material exposed portion 7. A pattern is formed on the surface of the stainless steel material 1 according to this embodiment by an oxide film portion 41 on which the black oxide film 4 has been formed, and a base material exposed portion 7 in which the black oxide film 4 has been removed to expose the silver-white base material 3. The pattern may be, for example, a stripe or wave pattern with exposed base portion 7 having a width of 0.5 to 20 mm, a checkered pattern (lattice pattern) of similar width, or a polka dot pattern with exposed base portion having a diameter of 0.5 to 20 mm, or a combination of these.
[0039] (Oxide film color tone) The stainless steel material 1 according to this embodiment has a lightness index L * , Chromanetics Index a * , b * These values are in a specific range. Color measurements are performed at any five points according to JIS Z 8722:2009, and the average value is calculated by CIELAB (L) according to JIS Z 8781-4:2013. * a * b * The lightness index L * , Chromanetics Index a * , b * The oxide film 4 (oxide film portion 41) of the stainless steel material according to this embodiment has a surface of L * ≦45.0, -5.0≦a * ≦5.0, -5.0≦b* It has a range of ≦5.0.
[0040] (Oxide film gloss) Furthermore, the stainless steel material 1 according to this embodiment has a glossiness GS(60°) of the surface on which the black oxide film 4 is formed (surface other than the exposed substrate portion) within a specific range. This value is an average value obtained by performing glossiness measurements at any five points in accordance with JIS Z8741:1997. The glossiness GS(60°) indicates that it is measured by irradiating light at an incident angle (60°). The oxide film 4 (oxide film portion 41) of the stainless steel material according to this embodiment has a surface with a GS(60°)≦40.0 range. This allows for a black color that suppresses the generation of excessive reflected light.
[0041] (brightness difference and gloss difference) The stainless steel material 1 according to this embodiment is polished so that the oxide film 4 and the inner oxide layer 5 are removed from the exposed base portion 7. As a result, the lightness difference ΔL between the oxide film portion 41 and the exposed base portion 7 * and the gloss difference ΔGS(60°) falls within a specific range. The method for measuring the lightness and gloss of the exposed substrate portion 7 is the same as the method for measuring the color tone and gloss of the oxide film described above.
[0042] Difference in brightness index (hereinafter, simply referred to as "brightness difference") ΔL * is the lightness index L of the oxide film 4 (oxide film portion 41). * 1 and the lightness index L of the exposed substrate 7 * 2, and in this embodiment, it is usually L * 2 is L * Since the number is greater than 1, ΔL * =L * 2-L * 1 ≧ 30.0. Also preferably, ΔL * ≧32.0, more preferably ΔL *≧35.0. The color tone difference ΔGS(60°) is the difference between the glossiness GS(60°)1 of the oxide film 4 (oxide film portion 41) and the glossiness GS(60°)2 of the exposed substrate portion 7, and in this embodiment, since GS(60°)2 is usually a larger value than GS(60°)1, ΔGS(60°)=GS(60°)2-GS(60°)1≧130.0 is satisfied. Also, preferably, ΔGS(60°)≧135.0, and further preferably, ΔGS(60°)≧140.0 is satisfied. In other words, the lightness difference ΔL * If the gloss difference ΔGS(60°) is within the above-mentioned range, the oxide film 4 and the inner oxide layer 5 are sufficiently removed from the exposed base portion 7. * The inner oxide layer 5 is more reliably removed as the gloss difference ΔGS(60°) falls within the above-mentioned preferred range, and the more preferred range it is.
[0043] (Passive film composition on exposed substrate) On the surface of the substrate exposed portion 7 of the stainless steel material 1 according to this embodiment, the oxide film 4 and the internal oxide layer 5 immediately below the oxide film 4 are removed in a polishing process described later, and then a passive film 8 is formed by natural oxidation. Therefore, in the area where the oxide film 4 and the internal oxide layer 5 are removed and the oxide film 4 is not formed, the surface of the substrate 3 is not exposed, but the passive film 8 formed on the surface of the substrate 3 is exposed. However, the passive film 8 is extremely thin, having a thickness of about several nm, and when the surface is viewed from above, the silver-white color of the substrate 3 is seen almost as it is. Therefore, in this specification, the area where the oxide film 4 and the internal oxide layer 5 are removed by polishing and the passive film 8 is formed is referred to as the substrate exposed portion 7.
[0044] The passive film 8 formed on the surface of the exposed substrate 7 has a Cr fraction of 30% or more. When removing the oxide film 4 and the internal oxide layer 5 by polishing, the composition of the passive film 8 on the surface of the exposed substrate 7 can be made to have a Cr fraction of 30% or more by polishing so that the temperature of the stainless steel surface (temperature of the substrate surface) does not exceed 400°C. The composition of the passive film 8 on the surface of the exposed substrate 7 can be analyzed by glow discharge optical emission spectrometry (GDS), and is measured by glow discharge optical emission spectrometry (GD-OES) in accordance with JIS K0144:2018. At this time, the analysis range is limited so that it is included only in the exposed substrate 7. The Cr fraction (%) of the passive film 8 on the surface of the exposed substrate 7 is determined as the Cr concentration / (Fe concentration+Cr concentration+Mn concentration+Ti concentration)×100 at the point where O (oxygen) is three-quarters of the maximum value in the obtained surface profile. The stainless steel material 1 according to this embodiment has sufficient protective properties (corrosion resistance) because the Cr fraction of the passive film 8 on the surface of the exposed substrate portion 7 is 30% or more. This makes it possible to prevent the design from being impaired by corrosion, oxidation, and the like. The Cr fraction of the passive film 8 on the surface of the exposed substrate portion 7 is preferably 35% or more, and more preferably 40% or more. This makes it possible to provide a stainless steel material 1 that is more excellent in design and corrosion resistance.
[0045] The stainless steel material 1 according to this embodiment has a high designability while suppressing a decrease in corrosion resistance because the chemical composition of the substrate, the color tone of the oxide film, the difference in brightness and glossiness between the oxide film portion and the exposed substrate portion, and the passive film composition of the exposed substrate portion are all within a specified range. Therefore, this stainless steel material 1 is suitable for use as a design component. Design components include, but are not limited to, building materials (especially interior components such as decorative panels) and various components that require designability, such as piping.
[0046] <2. Manufacturing method of ferritic stainless steel material> The stainless steel material 1 according to the present embodiment described above can be manufactured, for example, by the method described below. A preferred method for producing the stainless steel material 1 having the black oxide film 4 according to this embodiment is as follows: (1) an oxidation treatment step of heating a ferritic stainless steel material (base material 3) having the above-mentioned chemical composition in an oxidizing atmosphere at a temperature of 1000°C to 1100°C (e.g., 1050 to 1080°C) for 1 minute to 5 minutes (e.g., 2 to 3 minutes) to form an oxide film 4; (2) A polishing process is included in which the surface of the stainless steel material on which the oxide film 4 is formed is polished while maintaining the surface temperature at 400°C or less, thereby removing the oxide film 4 and the inner oxide layer 5 formed immediately below the oxide film 4 (on the substrate 3 side near the interface with the oxide film 4). Fig. 1 is a schematic diagram for explaining the flow up to the formation of a pattern. Each step will be explained below with reference to Fig. 1.
[0047] (Preparation of stainless steel material) FIG. 1(a) is a cross-sectional view showing the vicinity of the substrate surface before the black oxide film is formed. First, prior to each of the above-mentioned steps, a ferritic stainless steel material is prepared. The material may have a composition containing the above-mentioned elements and may be manufactured by a known method. For example, a cold-rolled sheet is produced by hot-rolling a ferritic stainless steel slab having the above-mentioned chemical composition, annealing and pickling the resulting hot-rolled coil, and then cold-rolling it at a rolling rate of 50% or more. Next, the surface of the resulting cold-rolled sheet is finish-polished with a polishing belt of #180 or more to obtain the base material 3 shown in Fig. 1(a). By using the base material 3 with the surface 2 polished in this manner, the appearance unevenness of the black oxide film 4 formed on the base material surface 2 in the subsequent process is suppressed.
[0048] (Oxidation treatment process) FIG. 1(b) is a cross-sectional view showing the vicinity of the surface layer of the substrate after the black oxide film has been formed. Referring to Fig. 1(b), this step is a step of forming a black oxide film 4 on the surface 2 of a base material 3 by heat treatment. The base material 3 is subjected to an oxidation treatment (annealing) in which the base material 3 is heated in an oxidizing atmosphere at a temperature of 1050 to 1080°C for 2 to 3 minutes, thereby forming the black oxide film 4 on the base material surface 2. The thickness of this oxide film 4 is 200 to 1000 nm, and preferably 250 to 900 nm. The thickness of the oxide film 4 can be adjusted by the annealing temperature and annealing time. An inner oxide layer 5 is formed on the inner surface side near the surface layer of the base material 3. The inner oxide layer 5 is a region in which a large number of inner oxides 6 such as TiO2 and Al2O3 exist. The thickness of the inner oxide layer 5 is about 400 to 1000 nm.
[0049] (polishing process) Fig. 1(c) is a cross-sectional view showing the vicinity of the surface layer of the stainless steel material after a pattern has been formed by polishing. In other words, Fig. 1(c) is a cross-sectional view that typically shows the vicinity of the surface layer in a cross section of the stainless steel material according to this embodiment cut in the plate thickness direction. Referring to FIG. 1(c), this step is a step of removing an arbitrary portion of the black oxide film 4 and the internal oxide layer 5 immediately below the oxide film 4 (on the substrate 3 side near the interface with the oxide film 4) by polishing. By removing the black oxide film 4 and the internal oxide layer 5 immediately below it at an arbitrary portion on the substrate surface 2 to expose the silver-white substrate 3, a pattern is formed on the surface of the stainless steel material 1 by forming a black oxide film portion 41 and a silver-white substrate exposed portion 7, and a design is imparted. The oxide film 4 and the internal oxide layer 5 can be removed by polishing. The surface 2 of the substrate 3 from which the oxide film 4 and the internal oxide layer 5 have been removed by polishing is exposed to the atmosphere after polishing is completed, and a thin passive film 8 of about several nm is formed by natural oxidation.
[0050] In the stainless steel material 1 according to the present embodiment, the oxide film 4 having a desired black color tone and the inner oxide layer 5 are removed from the exposed substrate portion 7, so that the brightness difference and gloss difference between the oxide film portion 41 and the exposed substrate portion 7 are within a predetermined range, and the stainless steel material 1 has excellent designability. Furthermore, the Cr fraction of the passive film 8 formed on the surface of the exposed substrate portion 7 is 30% or more, so that the stainless steel material 1 has excellent corrosion resistance. In order to make the composition of the passive film 8 have a Cr fraction of 30% or more, it is necessary to polish the steel sheet so that the surface temperature of the steel sheet (the temperature of the substrate surface 2) during polishing is kept at 400°C or less. For example, the steel sheet surface temperature during polishing can be kept at 400°C or less by polishing the steel sheet while cooling (water cooling, oil cooling, air cooling, etc.) without applying too much load. If the surface temperature of the steel sheet during polishing exceeds 400°C, a passive film 8 with a low Cr fraction and a high Fe fraction is formed, and the corrosion resistance of the exposed substrate portion 7 may deteriorate.
[0051] By the above steps, the stainless steel material 1 according to this embodiment, which has a pattern on its surface and is excellent in design and corrosion resistance, can be manufactured. Furthermore, the stainless steel material 1 according to this embodiment can be used not only as a decorative plate for wall materials, but also in bending, press forming, and welding, and therefore can be widely applied to steel pipes, processed products, and the like. EXAMPLES
[0052] The present invention will be described in detail below with reference to examples, but the present invention should not be construed as being limited to these.
[0053] A ferritic stainless steel having the chemical composition shown in Table 1 was hot-rolled to produce a hot-rolled sheet having a thickness of 3.0 mm. The hot-rolled sheet was annealed at 1050°C for 3 minutes, and then the oxide scale on the surface was removed by dry honing. The sheet was then cold-rolled to a thickness of 1.0 mm, and finish-annealed at 1000°C for 1 minute. The sheet was then hand-polished using dry polishing papers of No. 120 and No. 240 in sequence to remove the oxide scale on the steel sheet surface. The chemical composition in Table 1 is shown in mass%, with the remainder being Fe and impurities. In addition, REM in the table means rare earth elements, and here, misch metal (MM) containing La, Ce, and Nd was used.
[0054] [Table 1]
[0055] Thereafter, in order to blacken the surface of the above obtained stainless steel sheet (to form a black oxide film on the surface of the stainless steel sheet), heat treatment was performed in an air atmosphere at the temperature and time shown in Table 2. Thereafter, a test piece 50 mm wide and 100 mm long was cut out, and the central 10 mm wide portion was mechanically polished while cooling to remove the black oxide film and form an exposed base material portion, which was used as the test piece. In Comparative Example 3, mechanical polishing was performed without cooling. The polishing time in Comparative Example 2 was shorter than that in Example 1, and the polishing time in Comparative Example 1 was even shorter than that in Comparative Example 2.
[0056] (Color and gloss) At five points on the oxide film part where a black oxide film is formed on the surface of the test piece, color tone measurements were performed in accordance with JIS Z 8722:2009 using a spectrophotometer with a measurement diameter of 3 mm, and the average value was calculated as CIELAB(L) in accordance with JIS Z 8781-4:2013. * a * b * The lightness index L * , Chromanetics Index a * , b * Similarly, the gloss of five arbitrary points on the oxide film part where the black oxide film was formed on the surface of the test piece was measured using a gloss meter in accordance with JIS Z 8741, and the average value was expressed as GS (60°). Similarly, the color tone and gloss were measured at five arbitrary points on the exposed base material, and the brightness difference ΔL from the oxide film (oxide film part) was calculated. * And the gloss difference ΔGS(60°) was derived. * When the gloss difference ΔGS(60°) was 30 or more, it was evaluated as passing (excellent brightness difference), and when it was 30 or less, it was evaluated as failing (insufficient brightness difference). In addition, when the gloss difference ΔGS(60°) was 130 or more, it was evaluated as passing (excellent gloss difference), and when it was 130 or less, it was evaluated as failing (insufficient gloss difference).
[0057] The conditions for measuring the color tone are as follows. Equipment: Konica Minolta Spectrophotometer CM-700d Light source: Pulsed xenon lamp Photodetector: Dual 36-element silicon photodiode array Target mask: Φ3mm Measurement: 10° field of view Auxiliary Illuminant: D65 daylight, color temperature 6504K Specular reflection processing mode: SCI
[0058] The gloss measurement conditions are as follows. Equipment: Nippon Denshoku Co., Ltd. Handy gloss meter PG1M Light source: Tungsten lamp Detector: Photodiode Incident angle: 60°
[0059] (Passive film composition) Using the above test pieces, the composition of the passive film on the exposed substrate was analyzed by Glow Discharge Optical Emission Spectroscopy (GD-OES) in accordance with JIS K 0144:2018, and the Cr fraction (%) of the passive film on the exposed substrate was measured. In the GDS analysis (GD-OES), the Cr fraction (%) of the passive film on the exposed substrate was determined as the Cr concentration / (Fe concentration + Cr concentration + Mn concentration + Ti concentration) x 100 at the point where the O peak intensity was 3 / 4 of the maximum value.
[0060] The measurement conditions for GDS are as follows. Equipment: Rigaku Corporation GDA750 Analysis diameter (anode diameter): Φ4mm Voltage: 650V Ar pressure: 2.8hPa
[0061] (Corrosion resistance) The bonded body 11 shown in FIG. 2 was prepared using the above test piece as follows. FIG. 2(a) is a top view of the bonded body, and FIG. 2(b) is a side view. First, the cut end faces of three sides of the four cut end faces of the test piece 12 for measurement, except for one short side, were covered with rubber 13 (one-liquid condensation type RTV rubber KE44 manufactured by Shin-Etsu Silicone Co., Ltd.). Next, two polyethylene tubes 15 of 20 mmφ×10 mm were placed and bonded on a Bakelite plate 14 of 70 mm×150 mm, and the test piece 12 for measurement covered with rubber 13 was bonded on the two polyethylene tubes. The bonded body 11 obtained in this manner was used to evaluate corrosion resistance in accordance with the salt spray test specified in JIS Z2371:2015. Specifically, the bonded body 11 was placed in a combined cycle tester so that the test piece 12 for measurement was at an angle of 75 degrees to the horizontal plane and the uncoated short side was on the lower side, and then 5% salt spray was performed for 48 hours. After the salt spray test, the adhesive 11 was washed with water and dried, and the rust rate of the surface of the adhesive 11 was evaluated in accordance with JIS G0595:2004. When the rating number (RN) of the exposed base material was 8 or more (rust area rate ≦0.062%), the corrosion resistance was evaluated as excellent (○), and when the rating number (RN) was less than 8 (rust area rate >0.062%), the corrosion resistance was evaluated as insufficient (×).
[0062] The results of each of the above evaluations are shown in Table 2.
[0063] [Table 2]
[0064] As shown in Table 2, the stainless steel sheets of Examples 1 to 7 within the scope of the present invention met the chemical composition of the substrate and the color tone standard of the oxide film portion. * and gloss difference ΔGS (60°) met the criteria (i.e., the oxide film and inner oxide layer were sufficiently removed), and furthermore the Cr fraction of the passive film on the exposed substrate was 30% or more. Therefore, no rust was observed in the corrosion resistance test, and good corrosion resistance was demonstrated.
[0065] In contrast, the stainless steel sheets of Comparative Examples 1 to 7 were inferior to the Examples in either color tone or the corrosion resistance of the passive film at the exposed base. Comparative Example 1 met the color tone standard for the oxide film, but polishing was insufficient, and the oxide film was not sufficiently removed, resulting in a lightness difference ΔL * and gloss difference ΔGS(60°) did not meet the criteria. Comparative Example 2 met the color tone of the oxide film, but polishing was insufficient and the inner oxide layer was not sufficiently removed, so the gloss difference ΔGS(60°) did not meet the criteria and the corrosion resistance was also insufficient. The fact that the inner oxide layer was not sufficiently removed and remained was confirmed by the appearance of a Ti peak in the GDS analysis. Comparative Example 3 was polished without cooling, so the substrate surface temperature during polishing exceeded 400°C, and therefore the Cr fraction of the passive film in the exposed substrate was low, and the corrosion resistance was insufficient. Comparative Example 4 had a low Cr content, so the brightness difference ΔL * Although the gloss difference ΔGS(60°) and the Cr fraction of the passive film met the standards, the corrosion resistance was insufficient. Comparative Example 5 had a high Cr content, Comparative Example 6 had a low Ti content, and Comparative Example 7 had a low Mn content, so the color tone standards for the oxide film were not met.
[0066] As can be seen from the above results, according to the present invention, it is possible to provide a ferritic stainless steel material having excellent designability and corrosion resistance, which has a black oxide film on the surface and a pattern formed by removing part of the oxide film to expose the base material. [Explanation of symbols]
[0067] 1 Ferritic stainless steel 2. Base surface 3. Base 4. Oxide film 41 Oxide film part 5. Inner oxide layer 6. Inner oxide 7 Exposed base material 8 Passive Film 11 Adhesive body 12 Test piece for measurement 13. Rubber 14 Bakelite plate 15 Polyethylene tube
Claims
1. a ferritic stainless steel substrate having a composition, in mass%, of C: 0.050% or less, Si: 1.00% or less, Mn: 0.04 to 1.00%, P: 0.050% or less, S: 0.030% or less, Cr: 16.00 to 25.00%, Ni: 1.00% or less, Cu: 0.60% or less, Mo: 2.00% or less, N: 0.030% or less, Al: 0.500% or less, Ti: 0.080 to 0.500%, Nb: 0.500% or less, and a total content of Nb and Ti of 6(C+N) or more (C and N represent the contents of C and N, respectively), with the balance being Fe and impurities; The surface of the base material has a brightness index L * ≦45.0, Chromathetics index -5.0≦a * ≦5.0, −5.0≦b * and a black oxide film portion on which a black oxide film satisfying a gloss level GS(60°)≦5.0 and a gloss level GS(60°)≦40.0 is formed, and a base material exposed portion on which the oxide film is not formed, and a pattern is formed by the oxide film portion and the base material exposed portion, The difference in brightness index ΔL between the oxide film portion and the exposed base material portion * ≧30.0 and gloss difference ΔGS(60°)≧130.0, and The passive film formed on the surface of the exposed substrate satisfies a Cr fraction of 30% or more. Here, the Cr fraction (%) is expressed as the Cr concentration at the point where O (oxygen) is three-quarters of the maximum value in a surface profile obtained by measurement using glow discharge optical emission spectrometry (GD-OES) in accordance with JIS K0144:2018 / (Fe concentration+Cr concentration+Mn concentration+Ti concentration)×100, which is a ferritic stainless steel material.
2. The ferritic stainless steel material according to claim 1, further comprising, in mass%, one or more elements selected from the group consisting of Zr: 1.00% or less, Co: 1.00% or less, V: 1.00% or less, and W: 1.00% or less.
3. The ferritic stainless steel material according to claim 1 or 2, further comprising, by mass%, one or more elements selected from the group consisting of REM: 0.100% or less and Ca: 0.100% or less.
4. The ferritic stainless steel material according to any one of claims 1 to 3, further comprising, by mass%, one or more elements selected from the group consisting of Sn: 0.100% or less and B: 0.0100% or less.
Citation Information
Patent Citations
Formation of pattern on surface of metallic plate
JP1986213380A
Designed stainless steel sheet and production thereof
JP1990133581A
Production of polished ferritic stainless steel sheet excellent in oxidation resistance
JP1993195053A
MOLTEN Zn-BASED PLATED STEEL SHEET HAVING LINEAR PATTERN
JP2017218647A
Black ferritic stainless steel sheet
JP2018135591A