Thermal barrier coatings and thermal spray coating methods with CMAS resistance, high strain tolerance and low thermal conductivity
A multilayer ceramic coating with DVC and PVC layers made of rare earth-stabilized ZrO2 or HfO2 addresses CMAS degradation in TBCs, enhancing durability and reducing thermal conductivity for improved gas turbine engine performance.
Patent Information
- Application Number
- JP2020551460
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2018-04-09
- Filing Date
- 2019-04-08
- Publication Date
- 2024-10-09
- Estimated Expiration
- 2039-04-08
AI Technical Summary
Existing thermal barrier coatings (TBCs) used in high-temperature components of gas turbine engines are susceptible to degradation from calcium-magnesium-aluminum-silicate (CMAS) deposits, leading to reduced durability and toughness, while maintaining low thermal conductivity is crucial for engine performance.
A multilayer ceramic coating system comprising a dense vertical crack (DVC) top coat and a porous vertical crack (PVC) intermediate layer, made of rare earth-stabilized ZrO2 or HfO2, which provides erosion resistance and low thermal conductivity, respectively, applied through plasma spraying techniques.
The multilayer coating significantly enhances the durability and lifespan of TBCs by resisting CMAS degradation and reducing thermal conductivity, thereby improving the operating life of gas turbine engines.
Smart Images

Figure 0007564711000005 
Figure 0007564711000006 
Figure 0007564711000001
Abstract
Description
[Technical field]
[0001] (CROSS REFERENCE TO RELATED APPLICATIONS) This application claims priority under 35 U.S.C. § 119(e) to U.S. Provisional Patent Application No. 62 / 654,985, filed April 9, 2018, the disclosure of which is expressly incorporated herein by reference in its entirety.
[0002] (Statement regarding funded research and development) Not applicable
[0003] The present invention is an erosion-resistant, calcium-magnesium-aluminum-silicate (CMAS)-resistant multi-layer ceramic coating for ameliorating the CMAS degradation problem of thermal barrier coatings (TBCs) covering the surface of superalloy substrates. The multi-layer coating can include an erosion-resistant, CMAS-resistant, dense-vertical-crack (DVC) topcoat and a low thermal conductivity and strain-tolerant, porous-vertical-crack (PVC) intermediate coating. A coating method is also disclosed. [Background technology]
[0004] Hot section components of gas turbine engines are coated with thermal barrier coatings (TBCs) for protection at high temperatures. Eight weight percent (8 wt%) yttria-stabilized zirconia (8YSZ) has been the historical composition of the TBC due to its high toughness and low thermal conductivity up to high temperatures. Non-limiting examples include Metco 222A, 231A, 233A, 233B, 233C and 234A. However, as engine operating temperatures increase, molten siliceous deposits, commonly known as CMAS, attack the 8YSZ TBCs and have been recognized as a significant factor affecting TBC durability, representing a fundamental barrier to advancement in gas turbine technology. Various mitigation strategies for the problem of CMAS degradation have been attempted. The most promising strategy is to increase the reactivity between the coating and the CMAS melt. While these reactions consume the melt, the crystalline reaction products form a dense layer, blocking the path for further melt penetration. Most of these CMAS-reactive TBCs are based on rare earth zirconates. However, these compositions typically have lower toughness than 8YSZ coatings. Therefore, new strategies to increase the durability of CMAS-resistant TBCs while keeping the thermal conductivity of the TBC low and the toughness high are essential.
[0005] The use of yttria stabilized zirconia (YSZ) thermal barrier coatings is also known in the art and these have been used effectively in gas turbine engines for decades. Non-limiting examples include Metco 6608 and 6609.
[0006] The following documents, which are expressly incorporated herein by reference in their entireties, disclose various types of DVC coatings: Taylor, U.S. Pat. No. 8,197,950, issued June 12, 2012; Taylor, U.S. Pat. No. 5,073,433, issued December 17, 1991; Taylor, U.S. Pat. Publication No. 2014 / 0178632, issued June 26, 2014; Gray, U.S. Pat. No. 5,830,586, issued November 3, 1998; and Subramanian, U.S. Pat. No. 6,703,137, issued March 9, 2004.
[0007] The following documents, which are expressly incorporated herein by reference in their entireties, disclose various types of CMAS-resistant coatings: Maloney, U.S. Pat. No. 6,177,200, issued Jan. 23, 2001; Schlichting, U.S. Pat. No. 7,875,370, issued Jan. 25, 2011; Hongoh, U.S. Patent Publication No. 2012 / 0034491, issued Feb. 9, 2012; and Nagaraj, U.S. Pat. No. 9,023,486, issued May 5, 2015.
[0008] The following documents, which are expressly incorporated herein by reference in their entirety, disclose PVC coatings: Chen, U.S. Patent Publication No. 2016 / 0348226, published Dec. 1, 2016. Summary of the Invention
[0009] The present invention includes an erosion-resistant, CMAS-resistant multi-layer ceramic coating for ameliorating the CMAS degradation problem of TBCs. A coating method is also disclosed.
[0010] The present invention also encompasses a coating system in which one or more TBC layers are first applied onto a superalloy substrate. Then, one or more low thermal conductivity strain tolerant layers are applied which are porous vertical crack (PVC) coating layers. Finally, one or more dense vertical crack (DVC) erosion resistant CMAS resistant coating layers are applied or deposited as the top layer.
[0011] In embodiments, the porosity of the DVC layer(s) may be 0% to 5% and the cracks may extend partially through the thickness of the layer(s), either less than 50% of the thickness, or about 50% of the thickness, or may extend through the entire thickness of the layer(s). In embodiments, the cracks may be substantially vertical and may range from 20 to 200 cracks per inch.
[0012] In embodiments, the porosity of the PVC layer(s) may be 5% to 25% and the cracks may extend partially through the thickness of the layer(s), either less than 50% of the thickness, or about 50% of the thickness, or may extend through the entire thickness of the layer(s). In embodiments, the cracks may be substantially vertical and may range from 20 to 200 cracks per inch.
[0013] The present invention allows for increased life of the TBC or coating, which in turn extends and improves the operating life of the engine.
[0014] In an embodiment of the present disclosure, a strain tolerant DVC coating top layer and an underlying PVC coating system are used to protect the TBC system. The DVC / PVC layers may be composed of tough rare earth (Re) stabilized ZrO2 or HfO2 mixed with a CMAS resistant chemical composition. As used herein, CMAS resistant chemical means any chemical composition that can react with CMAS dust to form a crystalline phase and prevent further penetration of CMAS into the coating or that can improve the CMAS melting temperature after reacting with CMAS. The DVC layer provides erosion resistance and the PVC layer reduces thermal conductivity.
[0015] The primary advantage of the present invention is that it includes tough Re stabilized ZrO2 or HfO2 mixed with CMAS resistant chemistries to improve the erosion resistance and CMAS resistance of the TBC system, and the PVC strain tolerant transition layer provides low thermal conductivity.
[0016] Non-limiting embodiments of DVC top layer(s) and / or PVC layer(s) where DVC is the erosion resistant CMAS resistant and PVC is the thermal barrier and CTE (coefficient of thermal expansion) mitigating layer include the following (examples of rare earth oxides include yttrium oxide, lanthanum oxide, cerium oxide, praseodymium oxide, neodymium oxide, samarium oxide, europium oxide, gadolinium oxide, terbium oxide, dysprosium oxide, holmium oxide, erbium oxide, ytterbium oxide, lutetium oxide, scandium oxide, thulium oxide): RE stabilized ZrO2 or HfO2 (RE=rare earth oxide) RE stabilized ZrO2 or HfO2 mixtures with rare earth oxides, or RE stabilized ZrO2 or HfO2 mixtures with rare earth silicates, or RE stabilized ZrO2 or HfO2 mixtures with rare earth aluminates, or RE stabilized ZrO2 or HfO2 mixtures with rare earth aluminate silicates, or RE stabilized ZrO2 or HfO2 mixtures with alkali oxides, or RE stabilized ZrO2 or HfO2 mixtures with gadolinium zirconate, or Any combination of the above is included.
[0017] The CTE of the DVC top layer or coating is approximately 9 x 10 -6 / ℃~13×10 -6 / °C, the thickness can be 2 mils (0.002 inches) to 40 mils (0.040 inches). As used herein, 1 mil equals 0.001 inches. This layer or coating can be applied by atmospheric plasma spray (APS), plasma spray-physical vapor deposition (PS-PVD), or suspension plasma spray (SPS).
[0018] The CTE of the PVC interlayer or coating, which may be multiple, is approximately 9 x 10 -6 / ℃~13×10 -6 / ° C. and can be from 1 mil to 40 mils in thickness. This layer or coating can be applied by atmospheric plasma spray (APS), plasma spray-physical vapor deposition (PS-PVD), or suspension plasma spray (SPS).
[0019] The bond coat layer or coating, which may be multiple, can be MCrAlY (M=Co, Ni) with a thickness between 2 mils and 13 mils, which can be applied by atmospheric plasma spray (APS), high velocity oxygen fuel spray (HVOF), high velocity air-fuel spray (HVAF), plasma spray-physical vapor deposition (PS-PVD) or suspension spray.
[0020] Non-limiting embodiments of the present invention include an erosion resistant CMAS-resistant coating disposed on a TBC coated substrate that provides low thermal conductivity and includes at least one porous longitudinally cracked (PVC) coating layer disposed on the TBC coated substrate and at least one dense longitudinally cracked (DVC) erosion resistant CMAS-resistant coating layer deposited on the at least one PVC coating layer.
[0021] In a non-limiting embodiment, the at least one DVC layer is a top layer. The coating layers can further include at least one bond coating layer disposed between the TBC and the substrate. The substrate can be a superalloy substrate.
[0022] At least one dense crack (DVC) erosion-resistant CMAS-resistant coating layer may include RE-stabilized ZrO2 or HfO2. At least one dense crack (DVC) erosion-resistant CMAS-resistant coating layer may include RE-stabilized ZrO2 or HfO2 mixed with a rare earth silicate. At least one dense crack (DVC) erosion-resistant CMAS-resistant coating layer may include Re-stabilized ZrO2 or HfO2 mixed with a rare earth aluminate. At least one dense crack (DVC) erosion-resistant CMAS-resistant coating layer may include Re-stabilized ZrO2 or HfO2 mixed with a rare earth aluminate or silicate. At least one dense crack (DVC) erosion-resistant CMAS-resistant coating layer may include Re-stabilized ZrO2 or HfO2 mixed with an alkali oxide. At least one dense vertical crack (DVC) erosion resistant CMAS-resistant coating layer may comprise Re-stabilized ZrO2 or HfO2 mixed with gadolinium zirconate. At least one dense vertical crack (DVC) erosion resistant CMAS-resistant coating layer may comprise a mixture of one or more of the compositions described above.
[0023] At least one dense vertical crack (DVC) erosion resistant CMAS-resistant coating layer may include a full-thickness vertical crack. At least one porous vertical crack (PVC) coating layer may include a full-thickness vertical crack.
[0024] A non-limiting embodiment of the present invention provides a lower thermal conductivity and includes an erosion resistant CMAS-resistant coating disposed on a TBC coated substrate that includes at least one porous longitudinally cracked (PVC) thermal barrier coating layer disposed on an MCrAlY coated substrate and a top layer of a dense longitudinally cracked (DVC) erosion resistant CMAS-resistant coating material deposited on the at least one PVC thermal barrier coating layer.
[0025] In a non-limiting embodiment, the coating can further include at least one bond coating layer disposed between the TBC and the substrate. The substrate can be a superalloy substrate.
[0026] At least one dense crack (DVC) erosion-resistant CMAS-resistant coating layer may include Re-stabilized ZrO2 or HfO2 mixed with a rare earth oxide. At least one dense crack (DVC) erosion-resistant CMAS-resistant coating layer may include Re-stabilized ZrO2 or HfO2 mixed with a rare earth silicate. At least one dense crack (DVC) erosion-resistant CMAS-resistant coating layer may include Re-stabilized ZrO2 or HfO2 mixed with a rare earth aluminate. At least one dense crack (DVC) erosion-resistant CMAS-resistant coating layer may include Re-stabilized ZrO2 or HfO2 mixed with a rare earth aluminate or silicate. At least one dense crack (DVC) erosion-resistant CMAS-resistant coating layer may include Re-stabilized ZrO2 or HfO2 mixed with an alkali oxide. At least one dense vertical crack (DVC) erosion resistant CMAS-resistant coating layer may comprise Re-stabilized ZrO2 or HfO2 mixed with gadolinium zirconate. At least one dense vertical crack (DVC) erosion resistant CMAS-resistant coating layer may comprise a mixture of one or more of the compositions described above.
[0027] At least one dense vertical crack (DVC) erosion resistant CMAS-resistant coating layer may include a full-thickness vertical crack. At least one porous vertical crack (PVC) coating layer may include a full-thickness vertical crack.
[0028] A non-limiting embodiment of the present invention includes an erosion-resistant CMAS-resistant ceramic coating comprising a TBC coating layer disposed on and bonded to a superalloy substrate, a porous vertically cracked (PVC) ceramic coating layer providing a lower thermal conductivity deposited directly on the TBC coating layer, and a dense vertically cracked (DVC) erosion-resistant CMAS-resistant coating layer deposited directly on the PVC coating layer. In an embodiment, the TBC coating layer comprises a layer of MCrAlY, where M represents Ni, Co, or a combination thereof.
[0029] Non-limiting embodiments of the present invention include a method of plasma spraying an erosion resistant CMAS-resistant coating onto a TBC coated substrate comprising depositing at least one porous longitudinally cracked (PVC) thermal barrier coating layer providing a lower thermal conductivity onto the TBC coated substrate and depositing a dense longitudinally cracked (DVC) erosion resistant CMAS-resistant coating material onto the at least one PVC thermal barrier coating layer.
[0030] In embodiments, the TBC coated substrate may include at least one bond coating layer disposed between the TBC layer and the substrate. The plasma spraying may include one of atmospheric plasma spraying (APS), plasma spray-physical vapor deposition (PS-PVD), or suspension plasma spraying (SPS). [Brief description of the drawings]
[0031] The accompanying drawings are included to provide a further understanding of the invention, and are incorporated in and constitute a part of this specification. The accompanying drawings illustrate embodiments of the invention and, together with the description, serve to explain the principles of the invention. In the drawings: [Figure 1] FIG. 1 shows a schematic representation of a multi-layer coating according to the invention. [Diagram 2] FIG. 2 shows a scanning electron microscope (SEM) cross section of a multi-layer coating applied in accordance with the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0032] The following detailed description illustrates, by way of example and not by way of limitation, the principles of the present disclosure. This description clearly enables one skilled in the art to make and use the disclosure, and describes several embodiments, adaptations, variations, alternatives, and uses of the disclosure, including what is currently contemplated to be the best mode of carrying out the disclosure. It should be understood that the drawings are diagrammatic and schematic representations of illustrative embodiments of the disclosure, are not limiting of the disclosure, and are not necessarily drawn to scale.
[0033] The novel features which are characteristic of the present disclosure, both as to its structure and method of operation, together with further objects and advantages thereof, will be understood from the following description considered in connection with the accompanying drawings, in which embodiments of the disclosure are shown by way of example, It is to be expressly understood, however, that the drawings are for the purpose of illustration and description only and are not intended as a definition of the limits of the disclosure.
[0034] In the following description, various embodiments of the present disclosure are described with reference to the accompanying drawings. If necessary, detailed embodiments of the present disclosure are discussed herein. However, it should be understood that the disclosed embodiments are merely illustrative of embodiments of the present disclosure that may be embodied in various alternative forms. The figures are not necessarily to scale, and some features may be exaggerated or minimized to show details of specific components. Therefore, specific structural and functional details disclosed herein should not be interpreted as limiting, but merely as a representative basis for teaching those skilled in the art to variously use the present disclosure.
[0035] The details shown in this specification are presented by way of example and for the sole purpose of specific discussion of embodiments of the present disclosure, and are presented for the reason of providing what is believed to be the most useful and easily understood explanation of the principles and conceptual aspects of the present disclosure. In this regard, no attempt has been made to show structural details of the present disclosure in more detail than is necessary for a fundamental understanding of the present disclosure, so that, taken together with the drawings, the present description will make apparent to those skilled in the art how forms of the present disclosure may be embodied in practice.
[0036] As used herein, the singular forms "a," "an," and "the" include plural references unless the context clearly dictates otherwise. For example, "powder material" means that there may be a mixture of one or more powder materials, unless specifically excluded. As used herein, the indefinite article "a" indicates the plural, not just one, and does not necessarily limit the referenced noun to the singular.
[0037] Unless otherwise noted, all numbers expressing quantities used in the specification and claims should be understood to be modified in all instances by the term "about." Accordingly, unless indicated to the contrary, the numerical parameters set forth in the specification and claims are approximations that may vary depending upon the desired properties sought to be obtained by the embodiments of the present disclosure. At the very least, and not as an attempt to limit the application of the doctrine of equivalents to the scope of the claims, each numerical parameter should be construed in light of the number of significant digits and ordinary rounding rules.
[0038] Additionally, the recitation of numerical ranges within this specification is considered to be a disclosure of all numerical values and ranges within that range (unless expressly stated otherwise). For example, if a range is from about 1 to about 50, it is considered to include, for example, 1, 7, 34, 46.1, 23.7, or any other value or range within that range.
[0039] As used herein, the terms "about" and "approximately" indicate that the amount or value in question may be the specified particular value or other values in its vicinity. In general, the terms "about" and "approximately" referring to a particular value shall indicate a range within ±5% of that value. As an example, the phrase "about 100" indicates a range of 100±5, i.e., a range of 95 to 105. In general, when the terms "about" and "approximately" are used, it can be expected that similar results or effects according to the present disclosure will be obtained within a range of ±5% of the indicated value.
[0040] As used herein, the term "and / or" indicates that all or only one of the elements of the group may be present. For example, "A and / or B" shall mean "A only, or B only, or both A and B." In the case of "A only," the term also encompasses the possibility that B is absent, i.e., "A only and no B."
[0041] The term "at least partially" is intended to indicate that the following characteristics are met to some extent or completely.
[0042] The terms "substantially" and "essentially" are used to indicate that the following feature, characteristic or parameter is realized or met completely (entirely) or to the extent that it has no adverse effect on the intended results.
[0043] The term "comprising" as used herein is intended to be non-exclusive and open-ended. Thus, for example, a composition comprising compound A may contain other compounds besides A. However, the term "comprising" also encompasses the more restrictive meanings of "consisting essentially of" and "consisting of," so that, for example, a "composition comprising compound A" may also consist (essentially) of compound A.
[0044] The various embodiments disclosed herein can be used separately and in various combinations, unless specifically stated to the contrary.
[0045] The present invention will be described with reference to FIG. 1, which shows a schematic of a multi-layer coating. As seen in FIG. 1, the multi-layer coating utilizes a top coating layer that is a strain tolerant DVC coating top layer. This layer is disposed over an underlying PVC coating system used to reduce the thermal conductivity of the layer. The DVC / PVC layer may be comprised of tough rare earth (Re) stabilized ZrO2 or HfO2 mixed with a CMAS resistant chemical composition. The one or more DVC layers provide erosion resistance and the one or more PVC layers provide CTE mitigation between the one or more high CTE top layers and the one or more low CTE bottom layers of the TBC. The DVC and PVC layers, which may be multiple, are disposed over a bond coating B and a substrate S.
[0046] The DVC layers may be composed of tough Re-stabilized ZrO2 or HfO2 mixed with CMAS-resistant chemistries to improve the erosion CMAS resistance of the TBC / CMC system. Additionally, the PVC strain-tolerant transition layers provide CTE relaxation between the high CTE top layers (DVC layers) and the low CTE bottom layers TBC. The PVC microstructure then further reduces the thermal conductivity of the TBC system.
[0047] Non-limiting embodiments of the DVC top layers or layers and / or PVC layers or layers, where DVC is erosion and CMAS resistant and PVC is the thermal barrier and CTE (coefficient of thermal expansion) mitigating layer, include the following (examples of rare earth oxides include yttrium oxide, lanthanum oxide, cerium oxide, praseodymium oxide, neodymium oxide, samarium oxide, europium oxide, gadolinium oxide, terbium oxide, dysprosium oxide, holmium oxide, erbium oxide, ytterbium oxide, lutetium oxide, scandium oxide, thulium oxide): RE stabilized ZrO2 or HfO2 RE stabilized ZrO2 or HfO2 mixtures with rare earth oxides, or RE stabilized ZrO2 or HfO2 mixtures with rare earth silicates, or RE stabilized ZrO2 or HfO2 mixtures with rare earth aluminates, or RE stabilized ZrO2 or HfO2 mixtures with rare earth aluminate silicates, or RE stabilized ZrO2 or HfO2 mixtures with alkali oxides, or RE stabilized ZrO2 or HfO2 mixtures with gadolinium zirconate, or Any combination of the above is included.
[0048] The CTE of the DVC top layer or coating, which may be multiple layers, is approximately 9 x 10 -6 / ℃~13×10 -6 / ° C. and can be from 2 mils to 40 mils in thickness. This layer or coating can be applied by atmospheric plasma spray (APS), plasma spray-physical vapor deposition (PS-PVD), or suspension plasma spray (SPS).
[0049] The CTE of the PVC interlayer or coating, which may be multiple, is approximately 9 x 10 -6 / ℃~13×10 -6 / ° C. and can be from 1 mil to 40 mils in thickness. This layer or coating can be applied by atmospheric plasma spray (APS), plasma spray-physical vapor deposition (PS-PVD), or suspension plasma spray (SPS).
[0050] The bond coating layer or coating B, which may be multiple, may be MCrAlY (M=Ni, CO) and may have a thickness of 2 mils to 13 mils. This layer or coating may be applied by atmospheric plasma spray (APS), high velocity oxygen fuel spray (HVOF), high velocity air-fuel spray (HVAF), plasma spray-physical vapor deposition (PS-PVD) or suspension spray.
[0051] In embodiments, the porosity of the DVC layer(s) can be 0% to 5% and the cracks can extend partially through the thickness of the layer(s), i.e., either less than 50% of the thickness, or about 50% of the thickness, or can extend through the entire thickness of the layer(s). In embodiments, the cracks can be substantially vertical cracks and can range from 20 to 200 cracks per inch or linear inch. In non-limiting embodiments, the DVC layer(s) can also be of a type known in the art and described in one or more of the documents incorporated herein.
[0052] In embodiments, the porosity of the PVC layer(s) may be 5% to 25%, and the cracks may extend partially through the thickness of the layer(s), i.e., either less than 50% of the thickness, or about 50% of the thickness, or may extend through the entire thickness of the layer(s). In embodiments, the cracks may be substantially vertical cracks and may range from 20 to 200 cracks per inch or linear inch. In non-limiting embodiments, the PVC layers may also be of a type known in the art and described in one or more of the documents incorporated herein.
[0053] Non-limiting examples The following table contains a description of the coating system shown in Figures 1 and 2 and the parameters used to create it with the Sinplex plasma torch. [Table 1] [Table 2]
[0054] The following table contains a description of another coating system according to the present invention as well as the parameters used to form it with a Sinplex plasma torch. [Table 3] [Table 4]
[0055] Furthermore, because at least the invention is disclosed herein to enable the invention to be made and used, for example, for purposes of simplicity or efficiency, by disclosure of certain specific embodiments, the invention can be practiced in the absence of any additional elements or additional structure not specifically disclosed herein.
[0056] The foregoing examples are provided for illustrative purposes only and should not be construed as limiting the invention in any way. Although the invention has been described with reference to illustrative embodiments, it is understood that the words used herein are words of description and illustration, rather than words of limitation. Changes may be made, within the scope of the appended claims, without departing from the scope and spirit of the invention in its aspects, as presently stated and amended. Although the invention has been described herein with reference to particular means, materials and embodiments, the invention is not intended to be limited to the details disclosed herein. Rather, the invention extends to all functionally equivalent structures, methods and uses, as fall within the scope of the appended claims. Note that the following [1] to
[31] are all embodiments or aspects of the present invention. [1] At least one porous vertically cracked (PVC) coating layer providing low thermal conductivity disposed on a thermal barrier coating (TBC) comprising a layer of MCrAlY (M represents Ni, Co, or a combination thereof); and at least one dense longitudinal crack (DVC) erosion resistant CMAS resistant coating layer deposited on said at least one PVC coating layer; Erosion resistant CMAS resistant coating including. [2] 2. The coating of claim 1, wherein the at least one DVC layer is a top layer. [3] 13. The coating of claim 1, further comprising at least one bond coating layer disposed between the TBC and a substrate. [4] 2. The coating of claim 1, wherein the substrate is a superalloy substrate. [5] The at least one dense vertical crack (DVC) erosion resistant CMAS resistant coating layer is made of Re-stabilized ZrO mixed with rare earth oxides. 2 or HfO 2 The coating according to [1], [6] The at least one dense vertical crack (DVC) erosion resistant CMAS resistant coating layer is made of Re stabilized ZrO mixed with rare earth silicate. 2 or HfO 2 The coating according to [1], [7] The at least one dense vertical crack (DVC) erosion resistant CMAS resistant coating layer is made of Re stabilized ZrO mixed with rare earth aluminate. 2 or HfO 2 The coating according to [1], comprising: [8] The at least one dense vertical crack (DVC) erosion resistant CMAS resistant coating layer is preferably a Re stabilized ZrO mixed with a rare earth aluminate or silicate. 2 or HfO 2 The coating according to [1], [9] The at least one dense vertical crack (DVC) erosion resistant CMAS resistant coating layer is made of Re-stabilized ZrO mixed with an alkaline oxide. 2 or HfO 2 The coating according to [1], comprising:
[10] The at least one dense vertical crack (DVC) erosion resistant CMAS resistant coating layer is a Re-stabilized ZrO mixed with gadolinium zirconate. 2 or HfO 2 The coating according to [1],
[11] The at least one dense vertical crack (DVC) erosion resistant CMAS resistant coating layer is Re-stabilized ZrO mixed with rare earth oxides 2 or HfO 2 、 Re-stabilized ZrO mixed with rare earth silicates 2 or HfO 2 、 Re-stabilized ZrO mixed with rare earth aluminates 2 or HfO 2 、 Re-stabilized ZrO mixed with rare earth aluminates or silicates 2 or HfO 2 、 Re-stabilized ZrO mixed with alkali oxides 2 or HfO 2 , and Re-stabilized ZrO mixed with gadolinium zirconate 2 or HfO 2 The coating of [1], comprising a mixture of two or more of the following:
[12] 2. The coating of claim 1, wherein the at least one dense vertical crack (DVC) erosion resistant CMAS-resistant coating layer comprises a full-thickness vertical crack.
[13] 2. The coating of claim 1, wherein the at least one porous vertical crack (PVC) coating layer comprises a full-thickness vertical crack.
[14] at least one porous vertically split (PVC) thermal barrier coating layer providing a lower thermal conductivity disposed on the TBC coated substrate; and a top layer of a dense vertical crack (DVC) erosion resistant CMAS resistant coating material deposited on said at least one PVC thermal barrier coating layer; an erosion resistant CMAS resistant coating disposed on the TBC coated substrate.
[15] 14. The coating of claim 13, further comprising at least one bond coating layer disposed between the TBC and the substrate.
[16] 14. The coating of claim 13, wherein the TBC comprises at least one layer of MCrAlY, where M represents Ni, Co, or a combination thereof.
[17] The at least one dense vertical crack (DVC) erosion resistant CMAS resistant coating layer is made of Re-stabilized ZrO mixed with rare earth oxides. 2 or HfO 2 The coating according to
[14] , comprising:
[18] The at least one dense vertical crack (DVC) erosion resistant CMAS resistant coating layer is made of Re stabilized ZrO mixed with rare earth silicate. 2 or HfO 2 The coating according to
[14] , comprising:
[19] The at least one dense vertical crack (DVC) erosion resistant CMAS resistant coating layer is made of Re stabilized ZrO mixed with rare earth aluminate. 2 or HfO 2 The coating according to
[14] , comprising:
[20] The at least one dense vertical crack (DVC) erosion resistant CMAS resistant coating layer is preferably a Re stabilized ZrO mixed with a rare earth aluminate or silicate. 2 or HfO 2 The coating according to
[14] , comprising:
[21] The at least one dense vertical crack (DVC) erosion resistant CMAS resistant coating layer is made of Re-stabilized ZrO mixed with an alkaline oxide. 2 or HfO 2 The coating according to
[14] , comprising:
[22] The at least one dense vertical crack (DVC) erosion resistant CMAS resistant coating layer is a Re-stabilized ZrO mixed with gadolinium zirconate. 2 or HfO 2 The coating according to
[14] , comprising:
[23] The at least one dense vertical crack (DVC) erosion resistant CMAS resistant coating layer is Re-stabilized ZrO mixed with rare earth oxides 2 or HfO 2 、 Re-stabilized ZrO mixed with rare earth silicates 2 or HfO 2 、 Re-stabilized ZrO mixed with rare earth aluminates 2 or HfO 2 、 Re-stabilized ZrO mixed with rare earth aluminates or silicates 2 or HfO 2 、 Re-stabilized ZrO mixed with alkali oxides 2 or HfO 2 , and Re-stabilized ZrO mixed with gadolinium zirconate 2 or HfO 2
[14] The coating according to
[14] , comprising a mixture of two or more of:
[24] 14. The coating of claim 13, wherein a top layer of the dense vertical crack (DVC) erosion resistant CMAS-resistant coating layer comprises a full-thickness vertical crack.
[25] 14. The coating of claim 13, wherein the at least one porous vertical crack (PVC) coating layer comprises a full-thickness vertical crack.
[26] a TBC coating layer of MCrAlY disposed on and bonded to a superalloy substrate, wherein M represents Ni, Co, or a combination thereof; a porous vertically cracked (PVC) ceramic coating layer providing a CTE mitigation deposited directly on the TBC coating layer; and A dense longitudinal crack (DVC) erosion resistant CMAS resistant coating layer deposited directly onto the PVC coating layer Includes an erosion-resistant CMAS-resistant ceramic coating.
[27] 1. A method for plasma spraying an erosion resistant CMAS resistant coating onto a TBC coated substrate, comprising: depositing at least one porous vertically split (PVC) thermal barrier coating layer on the TBC coated substrate, the PVC thermal barrier coating layer providing a lower thermal conductivity; and depositing a dense vertical crack (DVC) erosion resistant CMAS resistant coating material over said at least one PVC thermal barrier coating layer; The method includes:
[28] 26. The method of claim 25, wherein the TBC coated substrate comprises at least one bond coating layer disposed between a TBC layer and the substrate.
[29] The plasma spraying Atmospheric Plasma Spraying (APS), Plasma Spray-Physical Vapor Deposition (PS-PVD) or Suspension Plasma Spray (SPS) The method according to
[27] , comprising one of the following:
[30] at least one porous vertically cracked (PVC) coating layer providing low thermal conductivity disposed on a thermal barrier coating (TBC) comprising a layer of NiCrAlY; and at least one dense longitudinal crack (DVC) erosion resistant CMAS resistant coating layer deposited on said at least one PVC coating layer; Erosion resistant CMAS resistant coating including.
[31] at least one porous vertically cracked (PVC) coating layer providing low thermal conductivity disposed on a thermal barrier coating (TBC) comprising a layer of CoCrAlY; and at least one dense longitudinal crack (DVC) erosion resistant CMAS resistant coating layer deposited on said at least one PVC coating layer; Erosion resistant CMAS resistant coating including.
Claims
1. At least one porous vertically cracked (PVC) coating layer providing low thermal conductivity disposed on a thermal barrier coating (TBC) comprising a layer of MCrAlY (M represents Ni, Co, or a combination thereof); and at least one dense longitudinal crack (DVC) erosion resistant CMAS resistant coating layer deposited on said at least one PVC coating layer; Including, The at least one dense vertical crack (DVC) erosion resistant CMAS resistant coating layer comprises: Rare Earth Oxide Stabilized ZrO Mixed with Rare Earth Silicates 2 or HfO 2 , Rare Earth Oxide Stabilized ZrO Mixed with Rare Earth Aluminate 2 or HfO 2 , and Rare Earth Oxide Stabilized ZrO Mixed with Gadolinium Zirconate 2 or HfO 2 1. An erosion resistant CMAS resistant coating comprising at least one of:
2. The coating of claim 1 , wherein the at least one DVC layer is a top layer.
3. The coating of claim 1 , further comprising: a coating formed on a substrate, the coating further comprising at least one bond coating layer disposed between the TBC and the substrate.
4. The coating of claim 1 , formed on a substrate, the substrate being a superalloy substrate.
5. The at least one dense vertical crack (DVC) erosion resistant CMAS resistant coating layer comprises: Rare Earth Oxide Stabilized ZrO Mixed with Rare Earth Oxides 2 or HfO 2 , Rare Earth Oxide Stabilized ZrO Mixed with Rare Earth Silicates 2 or HfO 2 , Rare Earth Oxide Stabilized ZrO Mixed with Rare Earth Aluminate 2 or HfO 2 , Rare Earth Oxide Stabilized ZrO Mixed with Rare Earth Aluminate or Silicate 2 or HfO 2 , Rare Earth Oxide Stabilized ZrO Mixed with Alkali Metal Oxides 2 or HfO 2 , and Rare Earth Oxide Stabilized ZrO Mixed with Gadolinium Zirconate 2 or HfO 2 The coating of claim 1 , comprising a mixture of two or more of the following:
6. 10. The coating of claim 1, wherein the at least one dense vertical crack (DVC) erosion resistant CMAS-resistant coating layer comprises a full thickness vertical crack.
7. 10. The coating of claim 1, wherein the at least one porous vertical cracked (PVC) coating layer comprises full thickness vertical cracks.
8. At least one porous vertically split (PVC) thermal barrier coating layer providing a lower thermal conductivity disposed on the TBC coated substrate; and a top layer of a dense vertical crack (DVC) erosion resistant CMAS resistant coating material deposited over the at least one PVC thermal barrier coating layer; an erosion resistant CMAS resistant coating disposed on the TBC coated substrate comprising: The dense vertical crack (DVC) erosion resistant CMAS resistant coating material comprises: Rare Earth Oxide Stabilized ZrO Mixed with Rare Earth Silicates 2 or HfO 2 , Rare Earth Oxide Stabilized ZrO Mixed with Rare Earth Aluminate 2 or HfO 2 , and Rare Earth Oxide Stabilized ZrO Mixed with Gadolinium Zirconate 2 or HfO 2 The erosion resistant CMAS resistant coating comprises at least one of:
9. The coating of claim 8 , further comprising at least one bond coating layer disposed between the TBC and the substrate.
10. The coating of claim 8 , wherein the TBC comprises at least one layer of MCrAlY, where M represents Ni, Co, or a combination thereof.
11. The at least one dense longitudinal crack (DVC) erosion resistant CMAS resistant coating material is Rare Earth Oxide Stabilized ZrO Mixed with Rare Earth Oxides 2 or HfO 2 , Rare Earth Oxide Stabilized ZrO Mixed with Rare Earth Silicates 2 or HfO 2 , Rare Earth Oxide Stabilized ZrO Mixed with Rare Earth Aluminate 2 or HfO 2 , Rare Earth Oxide Stabilized ZrO Mixed with Rare Earth Aluminate or Silicate 2 or HfO 2 , Rare Earth Oxide Stabilized ZrO Mixed with Alkali Metal Oxides 2 or HfO 2 , and Rare Earth Oxide Stabilized ZrO Mixed with Gadolinium Zirconate 2 or HfO 2 The coating of claim 8 comprising a mixture of two or more of:
12. 10. The coating of claim 8, wherein the top layer of the dense vertical crack (DVC) erosion resistant CMAS resistant coating material comprises a full thickness vertical crack.
13. 10. The coating of claim 8, wherein the at least one porous vertical cracked (PVC) coating layer comprises full thickness vertical cracks.
14. a TBC coating layer of MCrAlY disposed on a superalloy substrate and bonded to said substrate, where M represents Ni, Co, or a combination thereof; a porous vertically cracked (PVC) ceramic coating layer providing CTE mitigation deposited directly on the TBC coating layer; and A dense vertical crack (DVC) erosion resistant CMAS resistant coating layer deposited directly onto the PVC coating layer Including, The dense vertical crack (DVC) erosion resistant CMAS resistant coating layer comprises: Rare Earth Oxide Stabilized ZrO Mixed with Rare Earth Silicates 2 or HfO 2 , Rare Earth Oxide Stabilized ZrO Mixed with Rare Earth Aluminate 2 or HfO 2 , and Rare Earth Oxide Stabilized ZrO Mixed with Gadolinium Zirconate 2 or HfO 2 1. An erosion resistant CMAS-resistant ceramic coating comprising at least one of:
15. 10. A method for plasma spraying the erosion resistant CMAS resistant coating of claim 8 onto a TBC coated substrate, comprising the steps of: depositing at least one porous vertically-cracked (PVC) thermal barrier coating layer on the TBC coated substrate, the PVC thermal barrier coating layer providing a lower thermal conductivity; and depositing a dense vertical crack (DVC) erosion resistant CMAS resistant coating material over said at least one PVC thermal barrier coating layer; The method includes:
16. The method of claim 15 , wherein the TBC coated substrate comprises at least one bond coating layer disposed between a TBC layer and the substrate.
17. The plasma spraying Atmospheric Plasma Spraying (APS), Plasma Spray-Physical Vapor Deposition (PS-PVD) or Suspension Plasma Spray (SPS) 16. The method of claim 15, comprising one of:
18. At least one porous vertically cracked (PVC) coating layer providing low thermal conductivity disposed on a thermal barrier coating (TBC) including a layer of NiCrAlY; and at least one dense longitudinal crack (DVC) erosion resistant CMAS resistant coating layer deposited on said at least one PVC coating layer; Including, The at least one dense vertical crack (DVC) erosion resistant CMAS resistant coating layer comprises: Rare Earth Oxide Stabilized ZrO Mixed with Rare Earth Silicates 2 or HfO 2 , Rare Earth Oxide Stabilized ZrO Mixed with Rare Earth Aluminate 2 or HfO 2 , and Rare Earth Oxide Stabilized ZrO Mixed with Gadolinium Zirconate 2 or HfO 2 1. An erosion resistant CMAS resistant coating comprising at least one of:
19. At least one porous vertically cracked (PVC) coating layer providing low thermal conductivity disposed on a thermal barrier coating (TBC) including a layer of CoCrAlY; and at least one dense longitudinal crack (DVC) erosion resistant CMAS resistant coating layer deposited on said at least one PVC coating layer; Including, The at least one dense vertical crack (DVC) erosion resistant CMAS resistant coating layer comprises: Rare Earth Oxide Stabilized ZrO Mixed with Rare Earth Silicates 2 or HfO 2 , Rare Earth Oxide Stabilized ZrO Mixed with Rare Earth Aluminate 2 or HfO 2 , and Rare Earth Oxide Stabilized ZrO Mixed with Gadolinium Zirconate 2 or HfO 2 1. An erosion resistant CMAS resistant coating comprising at least one of:
Citation Information
Patent Citations
Heat-shielding coating system and covering articles containing a rare earth aluminate layer for improving CMAS penetration resistance
JP2011508092A
Heat-shielding coating including CMAS-resistant heat-shielding coating layer
JP2013540887A
Heat-shielding coating system and method thereof
JP2015501375A
Thermal barrier coating and coating method
JP2017515968A
Article for high temperature service
US20150159507A1