CATALYST SUPPORT MATERIAL, CATALYST SUPPORT, CATALYST, AND REACTION METHOD USING CATALYST

A composite catalyst structure with a SiC core protected by an alumina matrix and external layers addresses the instability of SiC in high-temperature, water vapor environments, enhancing durability and thermal conductivity for improved catalytic performance.

JP7564713B2Active Publication Date: 2024-10-09NEXCERIS INNOVATION HOLDINGS LLC
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2020568283
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2018-06-06
Filing Date
2019-06-06
Publication Date
2024-10-09
Estimated Expiration
2039-06-06

AI Technical Summary

Technical Problem

Silicon carbide (SiC) catalyst supports lack sufficient stability in high-temperature environments with the presence of oxygen or water vapor, leading to oxidation and corrosion, which reduces their effectiveness and lifespan in catalytic reactions.

Method used

A composite catalyst structure is developed, comprising a SiC core protected by an internal alumina matrix and external layers of alumina or barium strontium aluminosilicate (BSAS), enhancing oxidation resistance and maintaining thermal conductivity.

Benefits of technology

The composite catalyst structure significantly extends the lifespan of SiC-based catalysts in high-temperature, water vapor-containing environments, maintaining thermal conductivity and preventing oxidation, thereby improving the efficiency and durability of catalytic processes.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007564713000017
    Figure 0007564713000017
  • Figure 0007564713000018
    Figure 0007564713000018
  • Figure 0007564713000019
    Figure 0007564713000019
Patent Text Reader

Abstract

A catalyst having a core comprising a composite of SiC particles and a protective matrix of one or more metal oxides in the voids between the SiC particles, the core having a density of at least 60% of theoretical density, and having a catalytically active layer deposited on the core. A catalyst support comprising a composite of SiC particles and a protective matrix of one or more metal oxides in the voids between the SiC particles is also provided, along with a method for making the catalyst core.
Need to check novelty before this filing date? Find Prior Art

Description

[Background technology]

[0001] This invention was made in part with Government support under Grant No. DE-SC0013114 awarded by the U.S. Department of Energy. The Government has certain rights in the invention.

[0002] CROSS-REFERENCE TO RELATED APPLICATIONS This application claims priority to U.S. Provisional Patent Application No. 62 / 62 / 681,652, entitled "Catalyst Support Material, Catalyst Support, Catalyst, and Catalytic Reaction Method," filed June 6, 2019. The entire disclosure of the aforementioned provisional patent application is incorporated herein by reference.

[0003] Although there may be a variety of catalyst support materials, catalyst supports (also referred to herein as catalyst cores), catalysts, methods of making the above, and methods of reacting using the catalysts, it is believed that prior to the present inventors, no one has made or used the invention described herein. [Brief description of the drawings]

[0004] While the specification concludes with claims that particularly point out and distinctly claim the invention, it is believed that the invention will be better understood from the detailed description of specific embodiments thereof when read in conjunction with the accompanying drawings. Unless the context dictates otherwise, like reference numerals have been used in the drawings to identify similar elements therein. Also, some figures may be simplified by omitting certain elements to more clearly show other elements. Such omission does not necessarily indicate the presence or absence of a particular element in any of the illustrative embodiments, unless expressly described in the corresponding detailed description.

[0005] [Figure 1] Figure 1 shows cross-sectional SEM images of the inventive catalyst at low (left) and high (right) magnifications showing the interface between the core and the outer layer. This material was processed in air at 1250°C and contains an outer Al-Si layer. [Diagram 2]Figure 2 shows a cross-sectional SEM image of a material of the present invention that has been coated with BSAS (A), co-treated with BSAS (B), and heat treated at high temperature to convert the BSAS into a protective layer. BSAS is the white material. [Diagram 3] FIG. 3 shows a cross-sectional SEM image of inventive material coated with Al2O3 mixture introduced as a mixture of Al and Al2O3 in a slurry with volume ratios ranging from 25% to 75%. [Figure 4] Figure 4 shows cross-sectional SEM images of the adhesion-coated SiC / Al2O3 composite core pellets, where (A) refers to the layer containing Al2O3 mixed with CAS glass formers, (B) refers to the Al2O3 layer, and (C) is the core of the material. [Diagram 5] FIG. 5 shows a cross-sectional SEM image of a SiC / Al2O3 composite core pellet coated with a first interfacial layer of alumina and then an outer layer of Ni-containing catalytically active material. [Figure 6] Figure 6 shows photographs demonstrating the oxidation resistance of the inventive catalyst in a steam-containing and high temperature environment: Figure 6A shows a photograph of as-purchased commercial SiC pellets before (left) and after (right) exposure to 25% steam in air at 900°C for 44 hours, and Figure 6B shows a photograph of the inventive catalyst support before (left) and after (right) exposure to the same conditions and time. [Figure 7] FIG. 7 shows weight gain results of a representative sample of the inventive material over time under conditions of 50% water vapor in forming gas (3% hydrogen in nitrogen) at 900° C. [Figure 8] Figure 8 (A-D) shows plots of mass fraction of nth hydrocarbons versus carbon number of alpha ranging from 0.8 to 0.99. As alpha increases, the mass fraction of heavier hydrocarbons increases significantly. [Figure 9] FIG. 9 shows a plot of pellet void fraction and temperature effect on normalized radial conductivity of an inert packed bed. [Figure 10] FIG. 10 shows a plot of the effective packed bed thermal conductivity at 1970 hr (superficial velocity 0.52 m / s) for both the commercial SMR catalyst and the catalyst of the present invention. [Figure 11]FIG. 11 shows a comparative plot of experimental data for stagnation thermal conductivity (kr) of a commercial SMR catalyst (kr) and a catalyst support of the present invention (ks). [Figure 12] FIG. 12 shows a plot of reactor outer wall temperature versus axial distance with an average heat flux of 33.17 kW / m2, showing that the improved thermal conductivity from the inventive catalyst reduces the maximum wall temperature by 13° C. [Figure 13] FIG. 13 is a comparison of wall and gas temperatures versus axial distance for packed beds of commercial and inventive catalysts at a space velocity of 1970 hr −1 . [Figure 14] FIG. 14 shows the effect of increasing GHSV on dry methane slip for the catalyst of the present invention, showing that using the catalyst of the present invention as a support allows for a 36% higher GHSV for equivalent dry slip. [Figure 15] Figure 15 shows a plot of the heat flux profile of a comparable dry methane slip. For the same wall temperature and slip, the material of the present invention absorbs 33% more heat. [Figure 16] FIG. 16 shows a graph of the equilibrium conversion of methane over the temperature range of 650-900° C., pressures of 1-20 bara, and a steam to carbon (S / C) ratio of 3. [Figure 17] FIG. 17 shows the catalytic performance of the catalyst supports of the present invention in steam methane reforming conditions using option A, which has an outer porous layer impregnated with SMR active metal ions and then calcined, and option B, which has a layer of active catalyst deposited directly on the outside of the catalyst support material of the present invention. [Figure 18] FIG. 18 shows the results of space velocity studies for the inventive catalyst support materials under steam methane reforming conditions using option A, which has an outer porous layer impregnated with SMR active metal ions and then calcined, and option B, which has a layer of active catalyst deposited directly on the outside of the inventive catalyst support material. [Figure 19]FIG. 19 shows the performance stability under steam methane reforming conditions using option A, which has an outer porous layer impregnated with SMR active metal ions and then calcined, and option B, which has a layer of active catalyst deposited directly on the outside of the catalyst support material of the present invention. [Figure 20] FIG. 20 shows the packed bed thermal conductivity of commercial SMR material, different generations of the inventive catalyst, and dense SiC (normalized to dense SiC, which serves as a benchmark) at 530° C. and 830° C.

[0006] The drawings are intended to illustrate, rather than limit, the scope of the invention. Embodiments of the invention may be carried out in ways not necessarily depicted in the drawings. Thus, the drawings are intended merely to aid in the explanation of the invention. Thus, the invention is not limited to the precise arrangements shown in the drawings. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0007] Detailed Description The following detailed description describes example embodiments of the present disclosure solely for the purpose of enabling those skilled in the relevant art to make and use the same. As such, the detailed descriptions and illustrations of these embodiments are purely exemplary in nature and are not intended to limit the scope or protection of the present invention in any manner.

[0008] Embodiments of the present disclosure provide a catalyst comprising a silicon carbide (SiC)-based core (also referred to in the art as a catalyst support) and one or more catalytically active materials (e.g., one or more metals) attached thereto (e.g., a porous catalyst support layer forming a shell on the core). Embodiments of the present disclosure also provide a SiC-based core for use in the manufacture of catalysts, particularly core-shell catalysts. One or more protective materials are used in combination with the SiC-based core to protect the SiC-based core from oxidation and corrosion during subsequent use in catalytic reactions, particularly under high temperature conditions in the presence of H2O (e.g., as water vapor). Some In an embodiment, the catalytic core has a density of 60% or more of theoretical density and comprises a composite of SiC particles (or subparticles) and a protective matrix of one or more metal oxides (e.g., alumina) in the voids between the SiC particles. In another embodiment, the SiC-based core is protected by one or more interfacial layers located between the SiC core and the outer catalytically active layer. The interfacial layer can include, for example, high density alumina (e.g., ≧80%, ≧90%, or ≧95% of theoretical density) or another protective material such as barium strontium aluminosilicate ("BSAS"). In yet another embodiment, this interfacial layer (also referred to herein as a "third layer") can be applied over a composite SiC / oxide (e.g., SiC / Al2O3) core.

[0009] As is typical for achieving high surface area active catalysts comprising catalytic metals dispersed on an oxide support, the catalytically active material may be attached to the core in any of a variety of ways known to those skilled in the art or hereafter developed, such that it is disposed as spots, dots, nanoclusters, etc. on the surface (including the interior surface) of the porous catalyst support material. In some embodiments, one or more interfacial layers (e.g., a layer comprising α-alumina) are provided between the catalytically active material supported on the porous catalyst support and an inner moderately solid particle core comprised of silicon carbide (SiC). One embodiment of the interfacial layer is a substantially dense layer of A12O3 applied around the outside of the catalyst support (i.e., core), separating the SiC core from a porous catalyst layer comprised of a porous oxide with active catalytic metals dispersed therein.

[0010] Thus, the catalyst of the present disclosure is defined by a combination of at least two, three and possibly four (or more) layers. The first layer is defined by 60% or more of a theoretical density core consisting of SiC, which may contain other components such as Al and / or Si dispersed therein, as well as oxides of Al and Si (particularly alumina). The outer, second layer is catalytically active for the target reaction and typically consists of a porous oxide support with at least one active catalytic metal disposed therein, such as in the form of nanoclusters, spots, dots, etc. A third interfacial layer and, in some cases, a fourth non-porous, hermetic, protective coating layer ("fourth layer") are located between the first and second layers. The interfacial layer may be, for example, a substantially dense α-alumina layer that protects or passivates the first layer (i.e., the SiC surface) from corrosion by water vapor. The fourth layer may be a dense (90% or more, 95% or more, or about 100% of theoretical), non-porous, sealed coating that is airtight and prevents oxidation of the SiC in the core at high temperatures in environments containing water vapor. The third layer, and possibly the fourth layer, also act to secure or support the coated catalyst or second layer for a long operating life. It is undesirable for the second or outer layers of porous catalyst support with active metal disposed therein to peel, break, flake off, or disappear from the surface of the structure. Any or all layers may also be composed of, mixed with, coated, or doped with high emissivity materials or surface finish modified to increase the bulk emissivity of the support.

[0011] In yet another alternative embodiment, a porous interface layer can be provided between the first and second layers, particularly where the core includes a protective matrix such as alumina within the voids between the SiC particles. For example, as described further herein, a semi-transparent porous layer of alumina can be used to increase the emissivity of the catalyst.

[0012] In some embodiments, the catalyst core comprises a composite of SiC particles or subparticles with a protective matrix of metal oxide and, in some cases, residual metals around the SiC particles. Particles are defined as isolated crystallites of SiC and other components ranging in size from 0.01 to 100 microns. As further described herein, in the catalyst structures of the present invention, the first layer (i.e., core) of SiC particles are compressed during manufacture to produce a larger, compressed single pellet or other desired shape. Catalyst pellets are typically about 1 to 5 mm in size. The protective matrix acts to prevent water vapor, and possibly oxygen, from reaching the SiC in the core (i.e., first layer) of the pellet under reaction conditions. In one embodiment, the protective matrix is ​​comprised of alumina. In an alternative embodiment, the protective matrix barrier is comprised of alumina, titania, silica, zirconia, or a combination of two or more of the foregoing. The protective matrix not only protects the SiC particles from corrosive oxidation, but also acts as an intergranular phase that binds the SiC particles together to form the core. The result is a composite catalyst core with a theoretical density of 60% or more, rather than a traditional SiC catalyst core that is more porous (less than 60% theoretical density).

[0013] As discussed above, in some embodiments, the protective matrix comprises Al2O3. In yet other embodiments, the protective matrix comprises Al2O3 and silica and / or mullite (Al6SiO 13) in combination with one or more oxides of aluminum and silicon. Similarly, in other embodiments, the protective matrix comprises alumina and one or more oxides of titania, zirconia, and / or combined zirconia, aluminum, and / or titanium. Also as noted above, in some embodiments, the catalytic core (i.e., the first layer) is somewhat densified, such as, for example, an actual density of about 60% to about 100% of theoretical density, about 60% to about 95% of theoretical density, about 60% to about 90% of theoretical density, about 65% to about 90% of theoretical density, or about 65% to about 80% of theoretical density. Even at 60% of theoretical density, the cores of the present disclosure have a higher density than commercially available SiC catalytic cores, which are typically porous.

[0014] On the other hand, in the second layer, the active catalytic metal is dispersed within the porous support (i.e., the porous inner and outer surfaces) having a porosity (also referred to as void volume) ranging from about 40% to about 80%. A third optional interfacial layer that may be disposed between the first and second layers is made of a high density material, where the third layer has a density of about 80% to 100% of theoretical. The third layer, which serves as a protective layer to protect the underlying first layer of SiC, may be composed of, for example, alumina, silica, titania, zirconia or other material that can form a substantially high density layer on the core, is substantially inert to undesired reactions, and acts to help adhere the second layer of the porous support and the active catalytic metal disposed therein.

[0015] A fourth, gas-tight, protective coating layer, when utilized in combination with the third layer, provides a denser, more sealed protective coating for increased stability of the core material to corrosive gases, including water vapor and highly oxidizing environments at elevated temperatures. The fourth layer can be a gas-tight (90% or greater or 95% or greater of theoretical density) protective coating comprising Al2O3 in combination with glass formers such as alkaline earth aluminosilicate glasses, alkaline earth aluminoborosilicate glasses, and lanthanide aluminosilicate glasses.

[0016] Embodiments of the present disclosure also include methods of making catalyst cores (i.e., supports) by mixing SiC and Al (or Al-Si alloy) powders, along with one or more additives, such as binders, plasticizers, and / or lubricants. This mixture is then formed into pellets (or other desired shapes), such as by dry pressing or extrusion, and then calcined (e.g., in ambient air) to form dense catalyst cores comprising SiC in a protective matrix of Al2O3.

[0017] The catalyst supports and catalysts of the present disclosure can be made in any of a variety of shapes, including those known to those of skill in the art and those that will be developed in the future. Suitable shapes include, for example, spheres, cylinders, pellets, beads, lobed cylinders (e.g., bilobe, trilobe, tetralobe, etc.), and the like. Examples of suitable catalyst supports include pellets, such as tubular pellets, saddles, wheels, rings, pall rings, Raschig rings, ribbed or grooved cylinders, notched cubes, grooved pyramids, daisy-shaped, and star-shaped pellets. Alternatively, the catalysts of the present disclosure can be manufactured as monolithic structures. The catalyst supports can be formed into the desired shape and size, for example, by extrusion, pressing, or molding. Although some of the descriptions herein explicitly refer to pellets, it is understood that the descriptions apply equally to any other catalyst shape, unless the context dictates otherwise.

[0018] The catalyst of the present disclosure can be used in any of a wide variety of reactor types and configurations, including those known to those skilled in the art and those to be developed in the future. For example, the catalyst of the present disclosure can be used in fixed bed reactors (also referred to as packed bed reactors), fluidized bed reactors, mesochannel reactors, millichannel reactors, microchannel reactors, membrane reactors, ebullated bed reactors, chromatography reactors, and moving bed reactors. The catalyst of the present disclosure is particularly useful in fixed bed (i.e., packed bed) reactors, in which a free-flowing catalyst is loaded into a reaction chamber of various cross-sectional shapes, such as cylindrical, rectangular, square, or other shapes. The free-flowing catalyst conforms to the shape of the reaction chamber and is fixed in place for the reaction operation. During operation, the catalyst is substantially fixed in place in the reaction chamber, rather than moving as in the case of a fluidized bed reactor.

[0019] The catalytic cores of the present disclosure can be used with any of a wide variety of catalytically active materials attached (either directly or using one or more interfacial layers), including those known to those skilled in the art and those to be developed in the future. Suitable catalytically active materials include, for example, metals such as Ni, Co, Ru, Rh, Pd, Ir, Pt, Os, and Re. Further suitable catalytically active materials include Au, Ag, Cu, Fe, Mn, Mg, V, Mo, and Cr.

[0020] Further embodiments of the present disclosure include reaction methods using the catalysts described herein, such as, for example, steam methane reforming, acetylation, addition reactions, alkylation, dealkylation, hydrodealkylation, reductive alkylation, amination, aromatization, arylation, autothermal reforming, carbonylation, decarbonylation, reductive carbonylation, carboxylation, reductive carboxylation, reductive coupling, condensation, cracking, hydrocracking, cyclization, cyclo-oligomerization, dehalogenation, dimerization, epoxidation, esterification, Fischer-Tropsch synthesis, halogenation, hydrohalogenation, homologation, and the like. These include cation, hydration, dehydration, hydrogenation, dehydrogenation, hydrocarboxylation, hydroformylation, hydrocracking, hydrometallation, hydrosilylation, hydrotreatment, hydrodesulfurization / hydrodenitrogenation (HDS / HDN), isomerization, methanation, methanol synthesis, methylation, demethylation, metathesis, nitration, oxidation, partial oxidation, polymerization, reduction, steam and carbon dioxide reforming, sulfonation, telomerization, transesterification, trimerization, water gas shift (WGS), and reverse water gas shift (RWGS).

[0021] The catalytic cores and catalysts according to various embodiments of the present disclosure exhibit several advantageous properties and characteristics, as further described herein.

[0022] Composition and fabrication of SiC-based catalytic cores with over 60% theoretical density Nickel-based catalysts have traditionally been used in steam methane reforming ("SMR") reactions, as well as other types of catalytic reforming processes. Typically, nickel (the catalytically active material) is used in high internal surface area (10-1500 m2) catalysts, including porous ceramics (e.g., alumina, ceria, titanium dioxide, magnesium oxide, silica, composites, mixtures, etc.). 2 The catalyst is arranged or dispersed as small nanoclusters (average diameter 5-100 nm) on a catalyst support of 0.1 g / g. This type of catalyst system is capable of performing catalytic dry reforming (DR) or combined steam and dry reforming (CSR), oxidative steam reforming (OSR), autothermal reforming (ATR), oxidative dehydrogenation (ODH) and other catalytic processes. R), and catalytic partial oxidation (CPOX), sometimes with the addition of other elements beneficial for suppressing coke formation and / or increasing the reaction rate and / or improving the thermal stability of the catalyst under high temperature operation with steam, have been used.

[0023] In addition to Ni, other metals such as Co, Ru, Rh, Pd, Ir, and Pt are utilized as either the primary active catalytic metal or as promoters or stabilizers when combined with Ni. High temperature processes (above 600° C.) are likely to include one or more platinum group metals (“PGM”: Ru, Rh, Pd, Ir, Os, and Pt) as the primary catalytically active material or as promoters or stabilizers used in combination with Ni. Industrially, Ni is the preferred active metal for the production of hydrogen via SMR of natural gas due to its sufficient activity, low cost, and availability. Although nickel is not the most active catalyst in SMR, industrial fixed bed reactors are usually equilibrium reaction limited. Also, the addition of heat required for endothermic reactions in industrial fixed-bed reactors (e.g., for SMRs) is slowed due to the relatively low effective thermal conductivity of commercially available fixed-bed catalysts.

[0024] For conventional SMR catalysts and catalysts used for other types of reforming, in most cases the active metal is disposed on a support or another material that functions as a high surface area support. Table 1 below provides a non-exhaustive summary of catalyst systems commonly used in some of the above technologies. As noted in Table 1, an alumina support is commonly used, but other compositions of porous supports with active metals disposed therein may also be used. For example, industrial SMRs using natural gas or biogas feedstocks are typically catalyzed using Ni supported on a porous alumina support. In some cases, small amounts of other components are added to improve the catalyst's resistance to coke formation and to enhance catalyst stability due to high temperature operation in a high steam environment, for example. In Table 1, ATR stands for autothermal reforming reaction. CPOX stands for catalytic partial oxidation reaction. DR stands for dry reforming reaction. OSR stands for oxidative steam reforming reaction. SMR stands for methane steam reforming reaction. [Table 1]

[0025] Silicon carbide (SiC) has been investigated as a catalyst support for use in reforming reactions. SiC is one type of material that is attractive because the base material exhibits high thermal conductivity, making it ideal for improving heat transfer within a reactor. For example, at room temperature, dense alumina has a thermal conductivity of about 25 W / m·K, decreasing to about 10 W / m·K at 530 °C and further decreasing to about 7 W / m·K at 830 °C. On the other hand, bulk (dense, not semiconductor grade) SiC has a thermal conductivity of about 130 W / m·K at room temperature (decreasing to about 60 W / m·K at 530 °C and further decreasing to about 38 W / m·K at 830 °C). The higher thermal conductivity of SiC compared to alumina is advantageous when used as a catalyst support. SiC also exhibits a high level of inertness with respect to side reactions, including carbon formation, resistance to acid and base environments, mechanical hardness, and other features that are advantageous for a catalyst support. However, SiC is not ideal as a catalyst support or core for applications requiring exposure to oxygen and / or water vapor at high reaction temperatures because the presence of water vapor degrades the material by forming SiO2, which forms volatile SiO-(OH) species.

[0026] Thus, despite having some advantageous properties, unprotected SiC lacks sufficient stability at high temperatures in oxygen (e.g., air) and / or H2O (e.g., water vapor) environments. Under these conditions, the surface of SiC is oxidized to SiO2 and further corrodes to form gaseous Si(OH)4 in the presence of water vapor or water vapor and oxygen. Over time, this phenomenon continues until all the SiC is oxidized. This leads to a degradation or weakening of the SiC structure, resulting in failure of the material or catalytic system. This is the main failure mechanism of SiC and the main reason why, despite its excellent thermal properties, it has not been industrially adopted as a catalyst support in reactions that require high temperatures and the presence of oxygen (e.g., air) or water (e.g., water vapor). Furthermore, when SiC is converted to SiO2, the thermal properties of the material are significantly altered. Silica has a much lower thermal conductivity than the SiC value, and therefore the formation of SiO2 also reduces the thermal conductivity of the material.

[0027] Due to these problems, applying catalytically active materials directly to unprotected SiC substrates (e.g., foams, monoliths, pellets, etc.) produces oxidation rates that cause unacceptably short catalyst life for steam methane reforming catalysts and many other reactions as well. The SiC surface needs to be protected or passivated when used in high temperature oxidation or hydrothermal reactions involving steam. Thus, the use of SiC as a catalyst support in reforming and related reactions has typically been limited to placing an outer porous layer such as alumina on commercially available SiC (either alpha or beta) and then impregnating the porous alumina layer with a catalytically active metal such as Ni. Alternatively, the addition of Ni and the porous layer (e.g., alumina) can be done in a single step. Coating the exterior surface of a SiC core with a porous ceramic catalyst support layer such as alumina slows the rate of ingress of water vapor and oxygen into the underlying SiC during catalyst use. However, the slight delay in corrosion does not provide a commercially acceptable life for industrial methane reforming catalysts.

[0028] The catalytic core of the present disclosure advantageously employs SiC to take advantage of its beneficial thermal properties while protecting the SiC core from oxidation and corrosion, significantly increasing the useful life of the catalyst. In one embodiment, the SiC core comprises a composite of SiC and alumina (and optionally silica). The alumina is present as a protective matrix around the SiC particles in the composite core. In an alternative embodiment (or in addition to the protective alumina matrix around the SiC particles in the core), a shell coating of dense alumina extends outside the SiC core. (It is understood that an outer coating of alumina, including, for example, porous alumina, may also be provided on a composite core of SiC / Al2O3 having a theoretical density of 60% or more, as further described herein.)

[0029] In a first embodiment, aluminum (e.g., as a powder, including powder of an Al-Si alloy) is combined with SiC (e.g., as a powder) before being formed, such as by pressing or extrusion, into a core pellet or other desired shape. Various additives such as additives, lubricants, processing aids, etc. may be included in the mixture. During pressing or extrusion (or other pellet / core forming process), the aluminum is plastically deformed to flow around the SiC particles. Then, during the subsequent heat treatment in the presence of oxygen (i.e., calcination), the aluminum melts, relocates into the voids between the SiC particles, and is converted to alumina with the oxygen at high temperatures (e.g., process temperatures of about 850°C or higher). The aluminum not only removes oxygen from the heat treatment atmosphere and prevents oxidation of the SiC particles, but also converts most of the aluminum to protective alumina. The alumina, and the unoxidized aluminum trapped in the matrix, provide a coating and protection for the SiC particles against water vapor and oxygen attack during use of the catalyst. At certain heat treatment temperatures, aluminum that is not alloyed with other materials in the system during high pressure pressing or high temperature heat treatment processes becomes liquid when the heat treatment temperature exceeds the melting point of aluminum (660°C). Portions of the raw aluminum may melt and flow into the gaps between and around the SiC particles, making the aluminum more accessible to oxygen and forming an alumina matrix. In the final structure, it is believed that the aluminum added to the SiC is converted to alumina and some of the aluminum is alloyed with other materials, providing a stable protective matrix around the SiC particles that does not form an internal liquid film within the core during use of the catalyst (e.g., during high temperature methane steam reforming). It is also believed that some of the alumina formed is exposed to the surface of the core, further protecting it. When Si is used in combination with Al (e.g., as an Al-Si alloy powder), some of the Si is trapped in the alumina matrix, and some of the Si oxidizes and reacts with the aluminum oxide during firing to form mullite (Al6SiO4O 13 ) is thought to form.

[0030] By providing an internal protective alumina matrix around the SiC particles of the catalyst core, embodiments of the present disclosure largely preserve the advantageous thermal properties of SiC while protecting the SiC from oxidation and corrosion. The addition of an internal protective (or barrier) matrix of alumina extends the commercial life of the catalyst by limiting oxidation and corrosion of the dense SiC core, thereby allowing a longer and more commercially acceptable catalyst life to be achieved. In one embodiment, the catalyst life ranges from 6 months to 5 years. In another embodiment, the catalyst life ranges from 6 months to 30 months before requiring replacement in an industrial reforming tube. Such extended catalyst life has been demonstrated at industrial pressures of 20 bar, S:C ratios of 3, and 2000 h. -1 and reaction temperatures in excess of 800°C.

[0031] In some cases, SiC powder is mixed with an Al-Si alloy (e.g., an alloy containing up to about 25% Si, about 5% to about 20% Si, about 10% to about 15% Si, or about 11% to 13% Si) and used in place of pure or substantially pure Al. Among other things, the Si in the alloy helps to lower the melting temperature of the metal components and / or improve wetting of the molten metal. In one embodiment, a eutectic or near-eutectic alloy of Al and Si having a melting point below 600° C. is used.

[0032] Alternatively, pure or substantially pure Al and Si powders can be combined with SiC rather than an Al-Si alloy. Similarly, it is contemplated that other aluminum alloys or even other metals or metal alloys having melting temperatures below 1400° C. could be used (with or in place of Al or Al-Si).

[0033] For reactions requiring high energy (e.g., strong endothermic or exothermic reaction heat), the high thermal conductivity of SiC, when arranged in a thermally efficient form as described herein for the pelletized or particulate catalyst structures of the present disclosure, is advantageous for radially pumping heat into an endothermic reaction chamber or radially removing heat from an exothermic reaction chamber. The catalysts described herein may also surprisingly provide advantages for autothermal reactions. The higher effective thermal conductivity of the catalyst of the present disclosure will reduce the local axial thermal gradient in the tubular reactor caused due to the strong exothermic part of the combined autothermal reaction by increasing the axial conduction and heat transfer. Heat is transferred more efficiently to the endothermic reaction in the combined autothermal reaction by axial conduction in the catalyst bed. Although the overall or global reaction energy or heat is balanced for the autothermal reaction, the local rate of the exothermic reaction and and their heat release usually exceeds the local reaction rate of the endothermic reaction. This results in the formation of local hot spots. The catalyst of the present disclosure improves the overall process efficiency by reducing the size of the hot spots at the front of the reaction channel and giving more time with more temperature for the slower endothermic reaction to reach a higher degree of reaction at the end of the reaction tube.

[0034] The alumina protective matrix of the catalyst core of the present disclosure can be made from a composition including aluminum dispersed in SiC, for example, by plastically deforming the aluminum to flow around the SiC particles (e.g., during pellet formation), followed by an oxidative heat treatment process to form an alumina protective barrier around the SiC particles. Optionally, silicon can be included by using an Al-Si alloy dispersed in the SiC powder and / or by adding Si powder together with the Al powder.

[0035] In one particular embodiment, SiC powder is mixed with aluminum and optionally silicon powder or subparticles (these terms are used interchangeably). This mixture is then pressed or extruded under high pressure or load into pellets (or other desired shapes) and then fired to form a bonded (i.e., fused) structure in which the particles stick together and do not easily fall apart. As a test of the bonded structure, if the pressed particles are dropped from a height of one meter, it does not break or shatter into the original arrangement of the particles. As described further herein, the pellets can be fired before or after being coated with catalytically active materials or other coatings (e.g., interfacial layers). The firing temperature of the pellets can vary, for example, between 850°C and 1450°C for between about 0.5 and 24 hours, or between about 900°C and about 1000°C for at least 2 hours in ambient air. As described further herein, in some embodiments, multiple heat treatment steps can be used at different temperatures and under different conditions. The result is a SiC / Al2O3 composite core (e.g., pellet) composed of angular SiC grains bound by an intergranular phase of Al2O3.

[0036] The pellets (or other shapes) before firing are composed of silicon carbide (SiC) powder and aluminum-silicon (Al-Si) powder, the latter as a mixture of Al and Si powders or as an alloy powder of Al and Si. In one particular embodiment, SiC powders of different particle sizes are blended with the Al-Si powder. To optimize particle packing within the green body (e.g., pellet), two or more different particle fractions of SiC powder can be used. For example, a coarse fraction of SiC (e.g., about 30 to about 70 microns average diameter) can be mixed with a small amount of a fine fraction of SiC (e.g., about 15 to about 30 microns average diameter), with the fine fraction used to fill the large gaps between the coarse fractions. The powder blend is further mixed with various additives such as one or more organic binders (such as polyvinyl alcohol, polyvinyl butyral ("PVB", ethyl or methyl cellulose, etc.), and / or one or more plasticizers (e.g., butyl benzyl phthalate "BBP", ethylene glycol, polyethyl glycol, etc.). These additives allow the fine powder to be processed (e.g., by pan drying, grinding and sieving, or by spray drying) to form larger agglomerated powders that can be more easily fed through a dry pressing operation (or other pellet forming equipment). Additionally, to aid in the pressing operation, lubricants such as zinc stearate, stearic acid, and / or carbon powders such as graphite may be added to the agglomerated powder to facilitate the dry pressing operation.

[0037] Dry pressing is used to form the catalyst cores (e.g., as pellets), however, various other methods can be used to form the cores, such as extrusion, wet pressing, slip casting, isostatic pressing, injection molding, and other common ceramic forming approaches, provided that the process compresses sufficiently to achieve the target density in the green state (60% or more of the theoretical density of the blended SiC / Al powders) and induces plastic deformation of the aluminum.

[0038] The pressed or extruded pellets may be subjected to sintering following pellet formation, but in alternative embodiments, the pellets may be subjected to a further pre-sintering high temperature heat treatment in a substantially oxygen-deficient environment before being subjected to sintering. If used, the pre-sintering heat treatment step may sinter the aluminum (or aluminum alloy) particles (e.g., at temperatures above 400° C.) and further melt and fuse (e.g., at temperatures above 550° C.), allowing for microstructural rearrangement. This liquid phase may also further slow or prevent oxidation of the SiC during a subsequent heat treatment at temperatures above 500° C. in air or oxygen-containing environments, by preventing the diffusion of oxygen or water vapor (gas) into the structure. Thus, the pre-sintering heat treatment may be carried out at the same or different temperatures, in particular lower temperatures, than the sintering temperature. Typically, however, the pellets are fired after pellet formation (i.e., without a pre-sintering heat treatment) at temperatures between 850-1450°C or 900-1000°C for a time sufficient to convert the aluminum to an alumina matrix around the SiC particles. The firing is carried out in an oxygen-containing environment, such as oxygen, air, water vapor, or the foregoing diluted with nitrogen, argon, hydrogen, and / or another carrier gas. In one embodiment, pellets containing SiC and Al (or Al-Si) are fired in ambient air without the need to control the amount of oxygen in the firing environment, thereby reducing costs.

[0039] Example of core formation - SiC particle in a protective matrix of metal oxide 180 grams of 400 grit SiC (average diameter about 40 microns), 45 grams of 1200 grit SiC (average diameter about 15 microns) and 21 grams of Al-Si alloy powder (Valimet eutectic alloy 4047 (11-13% Si), grade S-2, average diameter 2 microns) were combined and transferred to a powder mixer where mixing continued. Separately, 3.5 grams of PVB was dissolved in 50 grams of isopropyl alcohol by warming. The PVB in IPA solution was then sprayed onto the powder with continuous mixing. The evenly wet powder was then spread into a shallow bed and dried at 120°C until completely dry. To this powder, 4% by weight of stearic acid and 4% by weight of graphite carbon (KS-6) were added. These powders were added dry, but isopropyl alcohol was added to wet the mixture. The mixture was dried once more before pressing. The dry powder blend was then dry pressed into pellets in a laboratory scale press. Pressing can be done with a manual or automatic pellet press, and pressure can be applied uniaxially or isostatically.

[0040] The above examples can be modified by varying the type and amount of coarse and fine SiC fractions used. In some embodiments, the coarse SiC can be selected from SiC having a grit size of 230 (about 70 microns in average diameter) to 600 (about 30 microns in average diameter), while the fine SiC can be selected from SiC having a grit size of 600 (about 30 microns in average diameter) to 1200 (about 15 microns in average diameter). The weight percentage of coarse SiC in the mixed SiC powder can vary between 50% and 100%, and the weight percentage of fine SiC can vary between 0% and 50%. For Al-Si alloy powder, Barimet eutectic alloy 4047 (11-13% Si) can be used with various particle sizes, such as median particle sizes of 2-50 microns. Specific examples include Valimet's Al-Si eutectic alloy 4047 powder grades S-2, S-5, S-8, S-10, S-15, S-20, and S-25, including those having up to about 25% Si (on a molar basis). Alternatively, other Al-Si alloys can be used. The volume of Al-Si (or Al if no alloy is used) in the mixture can be varied from about 2.5% to about 80% of the volume of SiC, from about 5% to about 50% of the volume of SiC, from about 5% to about 30% of the volume of SiC, from about 10% to about 30% of the volume of SiC, or from about 10% to about 25% of the volume of SiC. If other oxide-forming metals are used instead of or in addition to Al or Al-Si alloys, a similar total amount of oxide-forming metal in the mixture is used (e.g., 2.5 to 80% of the volume of SiC, 5 to 50% of the volume of SiC, 5 to 30% of the volume of SiC, 10 to 30% of the volume of SiC, or 10 to 25% of the volume of SiC).

[0041] The volume of the combination of PVB and BBP can vary from 1% to 15% (based on the total formulation before pellet formation), while the weight percentages of stearic acid and carbon can vary from 0% to 15%, respectively. Finally, the volume ratio of BBP to PVB can vary from 0% to 50%. A summary of these variations is shown in Table 2 below, where the amounts of SiC and Al-Si are reported as volume % of the total amount of SiC and Al-Si powder, and the amounts of PVP, BBP, stearic acid and carbon are also reported as % of SiC and Al-Si powder. Figure 5 shows an SEM image of a catalyst particle having a SiC / Al2O3 core produced by the above method, together with an outer catalytically active layer and an additional interfacial (i.e., third) layer of alumina between the SiC / Al2O3 core and the outer catalytically active layer. [Table 2]

[0042] Example of alumina interface / third layer deposition with Al-coating deposition As previously mentioned, some embodiments of the catalyst of the present disclosure include one or more interfacial layers (i.e., third layers) coated on the core. The catalyst core, which includes SiC and Al2O3, is coated with one or more of these interfacial layers (i.e., third layers) to further protect the SiC component from oxidation when exposed to high temperature oxidizing environments. Under such conditions, unprotected SiC develops slow-growing, silica flakes. The flakes act as a barrier to further oxygen diffusion into the core of the granule, thus preventing further attack of the substratum. However, the main drawback of the resulting silica flakes is their susceptibility to volatilization (e.g., formation of Si(OH)4) and corrosion in the presence of alkaline salts (e.g., formation of Na2SO4), which limits their applicability for intended purposes. To mitigate this, a protective "third layer" coating is added between the atmosphere and the SiC surface. Acts as a barrier. In some embodiments, each of the one or more interfacial layers comprises alumina, silica, titania, zirconia, or a mixture or oxide compound of two or more of the foregoing (e.g., mullite).

[0043] In some embodiments, the interfacial layer has a density of 80% or more, 90% or more, or 95% or more of theoretical density. In some specific embodiments, the interfacial layer has a density higher than that of the core.

[0044] As another example, an outer layer of aluminum or an aluminum alloy, including a metal mixture with other transition metals or metal oxides, may be applied as a thin coating onto the surface of the support material to form an interfacial layer that converts substantially to a dense oxide layer upon firing.

[0045] The particle size of the metals and / or metal oxides used in the system to form the interfacial layer can be controlled to a particular range. For example, the particle size can be controlled so that substantially most of the granules are within the size of about 2 microns. The range of granule sizes can vary from less than 1 micron up to 20 microns.

[0046] One example of this approach is a thin coating of aluminum applied to the core surface. The coating can be applied by many methods, including but not limited to dip coating, spray coating, spin coating, or vacuum infiltration, and can be applied by either manual or automated processes. The coating slurry used can vary from a full organic solvent and binder system to an aqueous solvent system with a polymer binder, or a combination thereof. The coating material can vary from a pure alumina material to alumina mixed with other metals, metal oxides, or nonmetals. Also, the interfacial coating can be applied to a pre-fired support material, or to the as-formed core shape, as disclosed below. After firing, all of the metals (such as aluminum) in the coating are converted to alumina.

[0047] In this particular example, a completely organic based coating medium is employed. The composition of the coating slurry for the third layer coating is disclosed in Table 3. Examples of successful coating formulation ranges are listed but should not be considered limiting in terms of potential coating systems. [Table 3]

[0048] The slurry is deposited onto either the pre-calcined or non-pre-calcined material cores of the present disclosure. In this example, the coating is deposited onto the core by an organic-based aerosol spray method, either manually or alternatively using an automated spray device. In either method, depending on the thickness required for the final coating, the spraying is done in one step or by coatings being repeated several times with intermediate drying cycles. The drying cycles are The process can be carried out at various temperatures, between 60°C and 150°C. Once dried, the coated pellets are sintered at temperatures ranging from 800°C to 1500°C, preferentially between 1000°C and 1300°C, more preferentially between 1250°C and 1350°C. The result is a substantially dense (>80% of theoretical) alumina interfacial layer, which also contains a small amount of mullite (due to the use of an Al-Si alloy). An example of an aluminium-derived coating applied using a hand spray and converted to an alumina layer is shown in Figure 1.

[0049] Examples of BSAS "third layer" protective coatings by aerosol deposition of glass formers As previously mentioned, one method of protecting the core of the catalyst support material of the present disclosure involves treating the SiC in the presence of other elements, such as aluminum or mixtures or alloys of aluminum and silicon, as previously mentioned, which provides superior protection of the SiC against oxidation in high steam environments at high temperature conditions.

[0050] This example shows two other methods of protecting the SiC core from oxidation: one using barium strontium aluminosilicate (BSAS) as a second phase in a SiC-based composite core, and the other using a protective coating of BSAS around the Si-C core. Figure 2 shows examples of materials obtained with both methods. The white layer in these SEM images is BSAS.

[0051] While BSAS is used to demonstrate this concept, potential glass phase formers that could be used in these coatings as well are polycrystalline solids prepared by pre-reaction of glass-forming oxides such as CaO-SiO2-Al2O3, or MgO-SiO2-Al2O3, SrO-SiO2-Al2O3, or BaO-SiO2-Al2O3. Other suitable glasses could include binary mixtures of alkaline earth elements in the glass phase former (such as BSAS itself), adding rare earth elements in place of the alkaline earth elements in the formulation, or adding small amounts of B2O3 or TiO2 as glass modifiers. In general, alkaline earth aluminosilicates with rare earth modifications, borosilicate variants of the same, or titania modified variants of any of these formulations are sufficient to provide a hermetic, hermetic coating. In addition, such glass coatings may contain a second crystalline ceramic phase addition, such as alumina, titania, zirconia-mullite or other common oxide ceramics, to modify the thermal expansion of the layer and its densification behavior during heat treatment. In such composite coatings, the content of the crystalline oxide phase may reach 40 volume percent of the coating solids.

[0052] In the first example, BSAS is coated onto pelletized SiC either before or after sintering (i.e., heat treating) the pelletized Si. If applied after sintering the SiC, the BSAS coating is then heat treated. Heat treating of this coating leads to the formation of a substantially dense protective layer on the core material. The BSAS coating protects the SiC core from oxidation and corrosion during use.

[0053] Alternatively, BSAS is added to SiC powder and both powders are granulated together. This method is similar to that described above for the production of SiC / Al2O3 composite cores. The granulated powder is then heat treated in air (e.g., at temperatures above 1000 °C). During this treatment, the BSAS melts and forms a glassy composite that flows around the SiC coating during the process, encapsulating the SiC and preventing oxidation. The demonstrated SiC / BSAS composites, produced by dry pressing and heat treating a mixture of precursor powders, represent a unique and previously undisclosed approach to composites. Figure 2 shows examples of materials obtained with both methods. The white layer in these SEM images is the BSAS.

[0054] (Al+Al 2 O 3 ) derived alumina "third layer" interface coating In this example, a completely organic based process is utilized. The specific composition of the coating slurry is disclosed in Table 4, which provides the exact reagents used in the formulation, and the ranges these components may have. The slurry may optionally be formulated from an aqueous medium. In this example, a combination of aluminum metal and alumina is used in the coating slurry. Aluminum metal and alumina may be mixed in the predetermined ratios shown in Table 4, such that the ratio of Al to Al2O3 varies between 2.5% and 50% by volume.

[0055] As in the previous example, the slurry is deposited onto either a pre-calcined or non-pre-calcined core material of the present disclosure and dried. The coated core (such as a pellet) is then sintered at a temperature ranging from 800° C. to 1500° C., preferentially from 1000° C. to 1400° C., and more preferentially from 1250° C. to 1350° C. The resulting material is a core having a substantially uniform layer of dense alumina therearound, as shown in FIG. 3. [Table 4]

[0056] Examples of multi-layer protective coatings: In this example, the catalyst core of the present invention is coated with a multi-layer coating comprising a dense (sealing) protective coat (layer 4) and an underlying interfacial layer (layer 3). This method produces an interfacial layer that is 70-90% dense, followed by the deposition of an additional protective coating comprising an aluminum oxide powder coating with a small amount of a glass phase former, hereinafter referred to as (Al2O3 + glass formers). Upon firing at 1000-1400°C, the multi-layer structure creates a seal coating on the core.

[0057] For the interface layer, the process of "Example of Alumina "Third Layer" Deposition by Al Coating Deposition" is used to deposit a layer of aluminum metal powder 10-40 microns thick on the surface of the core. In one embodiment, this coating is heated at 1000-1400°C in air to produce an aluminum oxide coating of 70-90% density. After this heat treatment, a (Al2O3 + glass former) powder coating is applied by dip coating, spray deposition, etc. to a thickness of 20-80 microns. The deposited coating is then fired at 1000-1400°C in air to produce a hermetic protective coating.

[0058] In a second embodiment, the initial aluminum-derived layer is dried but not heat treated prior to deposition of a 20-80 micron thick (Al2O3 + glass formers) powder coating by dip coating, spray deposition, etc. Both deposited coatings are then fired at 1000-1400°C in air to produce a sealed coating.

[0059] The (Al2O3 + glass former) formulation consists of (75-99%) commercial alumina powder and (1-25% by weight) glass phase formers. The incorporation of glass formers effectively allows for enhanced densification of the coating, better adhesion to the underlying surface, and conformability of the coating during heat treatment, allowing a hermetic coating to be achieved.

[0060] Suitable candidates for glass formers include precursor blends prepared by pre-reaction of glass-forming oxides such as CaO-SiO2-Al2O3 ("CAS") or MgO-SiO2-Al2O3 ("MAS"), SrO-SiO2-Al2O3 or BaO-SiO2-Al2O3. Other suitable glasses include mixed alkaline earth aluminosilicates (e.g., BSAS), rare earth doped alkaline earth aluminosilicates, or B2O3 or TiO2 modified alkaline earth aluminosilicates.

[0061] In the present example, eutectic blends of the CaO-Al2O3-SiO2 and MgO-Al2O3-SiO2 families were added to the alumina coating in the form of pre-reacted oxide mixtures. A mixture of glass phase formers in the appropriate ratio to the Al2O3 powder was mixed in an aqueous solution.

[0062] To synthesize the glass phase former precursors (Table 5), eutectic CAS and MAS compositions (based on the individual oxides in the final formulation) are fused from calcium or magnesium nitrate in water, colloidal silica (SiO2), and boehmite (AlOOH), then dried at 150°C and ground to form a powder. The precursor powder is then calcined at 1000°C to pre-react the oxides and increase the surface area of ​​the powder to 8-12 m2. 2 Reduced to / g. [Table 5]

[0063] The glass former powders were then blended with alumina and appropriate polymer additives (dispersants, plasticizers, and binders) in an aqueous slurry as shown in Table 6. Commercially available alumina and synthetic CAS or MAS, or other glass formers, are mixed in various ratios. The aqueous slurries are shown in Table 6, although organic-based solvent systems can also be used.

[0064] The coating application process is preferentially via a dip coating process, but can also be via a spray deposition process and other coating processes known to those skilled in the art. The thickness of the coating is controlled by these processes and can vary from 20 to over 80 μm. The coated pellets are heat treated in air at temperatures between 1000 and 1500° C., preferentially between 1200 and 1400° C. A cross-sectional SEM micrograph of the sealed coated pellets is shown in FIG. [Table 6]

[0065] As described in more detail in the next section, catalytically active materials can be applied to the SiC / Al-Si cores produced by the above method either before or after heat treatment (i.e., calcination) of the composite core. The resulting core / shell catalysts are composed of at least two distinct layers and functions. The first layer is composed of a high thermal conductivity and high total normal emissivity SiC core that functions to improve radial or axial heat transfer within the reactor vessel. The optional third layer is a protective or barrier layer of alumina that functions to minimize access of corrosive water vapor to the underlying SiC core and thereby extend useful catalyst life. This optional layer may be desirable in addition to (or instead of) the alumina that forms around the grains in the core to completely passivate the underlying SiC. This optional third barrier layer preferentially consists of a continuous dense layer of alumina with a density between 80 and 100% of theoretical. This optional layer can be formed by applying a coating of aluminum (e.g., as a slurry) followed by heat treatment in an oxygen environment (e.g., ambient air) to convert the aluminum to a dense coating of alumina. The second layer is an outer layer of catalytically active material. In some embodiments, this second layer is composed of two sublayers: an inert but porous high surface area support, and a catalytically active metal disposed within the porous high surface area support to catalyze the desired reaction.

[0066] In some embodiments, the first layer is defined by an average pellet diameter of 50 to 50,000 microns, with a preferred range being 200 to 15,000 microns average diameter. The third zone is defined by an average thickness range of 0.3 to 50 microns having a density greater than 80% of theoretical. The second zone or active catalyst coating layer is defined by an average thickness range of 5 microns to 200 microns, preferably a thickness range of 10 to 100 microns.

[0067] Coating process for catalyst support material The nature of many industrial processes requires that powdered catalysts be replaced with pelletized forms, avoiding the problems associated with powders, such as handling, dosing, and accurate measurement. In some processes, such as SMR, the use of powdered catalysts is not possible due to the process conditions involved, i.e., high pressure, steam, and flow conditions, and the excessive and therefore uneconomical pressure drop of the flow through a small powder bed. Under these conditions, the powdered catalyst also has a tendency to be blown downstream of the reactor and into the product stream, which is undesirable.

[0068] The problem associated with the use of powders in industrial processes is the need to pelletize the powders and reduce the pressure drop. This is avoided by significantly improving handling and ease of use. Industrial processes such as SMR, catalytic partial oxidation, and dry reforming, among others, use pelletized catalysts in the reactor. For example, in SMR, the active metal (Ni) is impregnated into granular high surface area alumina.

[0069] In this disclosure, the catalyst includes a high thermal conductivity and emissivity support material (i.e., core) composed of either pre-sintered alpha and beta silicon carbide pellets with a protective outer coating (e.g., dense alumina or BSAS) or a SiC / Al2O3 (Si loaded) composite. The powder is first pelletized by either dry pressing or extrusion and then heat treated in an oxygen environment. The pellets are then coated with a catalytically active layer, thereby providing a core / shell catalyst. Coating methods and options are further described herein.

[0070] Several methods can be employed to protect the core SiC from oxidation under high water vapor and high temperature conditions. First, the SiC can be mixed with a protective metal, such as Al-Si powder, where the aluminum plastically deforms and flows around the SiC particles during pressing, forming an oxide phase around the SiC particles during the subsequent oxidation heat treatment. Second, a mixture of barium strontium aluminosilicate (BSAS) can be added to the SiC powder and granulated before dry pressing into pellets. The pellets are then heat treated in air at temperatures above 1000°C and up to 1500°C. During this treatment, the BSAS reacts, melts, and flows around the SiC particles, forming a glassy composite that coats the SiC particles. BSAS has excellent protective properties. Third, BSAS (or another protective layer, such as dense alumina) can be coated onto the pelletized SiC (either pure or as a SiC / Al2O3 composite) before or after sintering the core material. Heat treating this coating at 1000°C to 1500°C forms a protective coating of BSAS on the core material. The BSAS coating ensures that the core is protected from oxidation. Examples of the last two methods for protecting the core are shown in Figure 2.

[0071] In this disclosure, the high thermal conductivity material of the present invention is processed in various options as previously mentioned, such as (1) commercially available granular SiC material can be coated with a protective outer layer such as BSAS, (2) BSAS can be added to commercially available SiC and granulated prior to heat treatment, and (3) a mixture of Al and Si can be mixed into commercially available SiC powder, granulated, pelletized (or otherwise formed), and then heat treated. In these options, the resulting pellets are further coated with an outer layer of either catalytically active material or a support layer of catalytically active material (i.e., an interfacial layer), resulting in the formation of a core-shell catalyst. The outer layer can be applied either after the catalyst support (i.e., core) is heat treated, or prior to heat treatment (i.e., applied to the "green" core material). In either case, the deposited outer layer is typically heat treated at various temperatures to allow the deposited outer layer to adhere to the core support material. The deposited layers vary in size, with average layer thicknesses ranging from 10 μm to 200 μm. It is this layer that is impregnated with catalytic metals for various catalytic applications (unless catalytically active materials are incorporated in an outer layer deposited on the core).

[0072] In some embodiments, the outer layer is deposited onto a granulated, highly thermally conductive catalyst support material that has not been heat treated (i.e., is still green) from a slurry containing the selected material. In other embodiments, the deposition of the outer layer is performed on an already heat treated core. In both of these cases, the deposited outer layer is heat treated at various temperatures ranging from 600°C to 1500°C, or 850°C to 1450°C.

[0073] The catalytic outer layer of the present disclosure can be applied to the SiC / Al-Si composite core in a variety of ways, including spray coating or dip coating. In dip coating, the outer layer material is sprayed onto the pellets as an organic or aqueous slurry. In dip coating, granular particles are immersed in an organic or aqueous slurry containing the outer layer material. An example of a catalyst support core of the present invention is shown in the SEM image of Figure 5. Here, an outer layer of Ni-containing catalytically active layer (shown as C) is deposited on a SiC / Al2O3 composite core (A) with an intervening interfacial layer of alumina (B).

[0074] As mentioned above, the catalysts described herein are of the core-shell type, prepared by physically depositing an outer layer onto a SiC / Al-Si solid core. This outer shell can be an interfacial layer that is subsequently impregnated with catalytically active material, or a layer onto which catalytically active material has already been deposited (e.g., an oxide porous catalyst phase).

[0075] In one embodiment, the pressed pellets are coated with an organic or aqueous slurry containing secondary materials, either in the form of metal or oxide. The slurry is composed of known transition metal and metal oxide catalyst support materials. In one embodiment, the slurry contains a nanoscale slurry of Ni particles (or other PGM particles) synthesized by the polyol process. After coating, the slurry is dried so that the solid coating is retained on the surface. A calcination step is common in slurry-based catalyst coatings to oxidize the binder and other carbonaceous-based materials used in forming the slurry. The catalyst calcination step also serves to bond the catalyst coating layer to the surface. The materials are broadly classified into two types: (1) supported catalyst powders, and (2) catalyst support powders. The former refers to catalyst support powders that already contain active catalyst, while the latter refers to support powders that do not contain active metals, but are impregnated with active catalyst metals after the composite coating is formed. The active catalyst layer can be added to or coated onto the pressed pellets either as a complete catalyst with the active metal disposed throughout the high surface area support or just the high surface area support, without the active metal being added to or coated onto the pressed pellets, in which case the active metal is impregnated in a secondary step into a porous support layer already coated onto the pellets.

[0076] The coating slurry can be prepared by adding the desired powder materials to an organic solvent, such as, but not limited to, ethyl cellulose, polyvinyl alcohol, or alpha-terpineol. The powder materials can be selected from the following non-exhaustive list: aluminum-silicon, zirconia-ceria doped alumina, alumina, zirconia doped ceria, alumina-silica mixtures, gamma alumina, alpha alumina, magnesium promoted alumina, calcium promoted alumina, sodium promoted zirconium-cerium oxide, cerium oxide, titania promoted silica, and the like. These materials support the catalytically active material incorporated in the slurry or form a coating on a core that can be impregnated with catalytically active material after heat treatment. The above oxides can be applied with or without the following catalytically active metals disposed therein in the form of dispersed nanoclusters, spots, dots, and the like: nickel, platinum, rhodium, ruthenium, cobalt, rhenium, iridium, and the like. Elements known to play a role in promoting or inhibiting coke formation can be added optionally.

[0077] The as-dried coating is calcined on the pellets by slowly increasing the temperature to the target temperature and holding there for at least about 1 hour. The catalyst calcination temperature can range from about 300° C. to about 800° C. The oxygen environment (e.g., ambient air) of the calcination process would result in combustion of the binder used to form the catalyst slurry. After the catalyst calcination step, the catalyst coating layer is fused to the underlying SiC core at 60% or more of theoretical density, and the catalyst coating layer retains porosity and contains little to no organic binder.

[0078] If the applied coating did not contain catalytically active material, the final step for producing a core-shell catalyst is to permeate (i.e., impregnate) this layer with active catalytic metal ions. The metal ions of interest are dissolved in a medium, preferably water but which may be organic. The pellets are immersed in the medium, where the ions impregnate the porous outer layer. After a defined period of time, for example ranging from about 5 minutes to about 4 hours, the metal ion-permeated support material is drained from the solution and dried, for example at 120° C., for a period of 30 to 60 minutes or more. Finally, the support material is calcined in air at various target temperatures, for example to remove binders (e.g. residual organics).

[0079] The catalyst structure of the invention and its support defined by its oxidation resistance Silicon carbide (SiC) and SiC-based composites require protective coatings when applications involve exposure to oxidizing environments and high temperatures typical of many chemical reactions, including but not limited to steam methane reforming. SiC simultaneously oxidizes and volatilizes in water vapor under these conditions. When exposed to oxygen at high temperatures, SiC: SiC + H2O (g) → SiO2+ CO (g) + 3H2(g) is oxidized via

[0080] The oxidation of SiC is limited by the mass transfer of oxygen to the core of the material. Thus, the oxidation becomes uneven and slows towards the core of the material. It has also been found that the undesirable oxidation of SiC is enhanced in the presence of water compared to the dry feed mixture at high temperatures. This oxidation is due to the significant solubility of SiO2 in water, which changes the rate to favor the formation of undesirable SiO2. In the presence of water, the reaction behind the volatilization of SiC is: SiO2+ H2O → Si(OH)4(g)

[0081] The underlying oxidation of SiC catalyst supports during catalytic chemical reactions is particularly problematic because it can weaken the base layer beneath the catalyst coating, resulting in loss of catalyst coated on top of the weak base layer through spallation or delamination. Catalyst loss manifests as catalyst deactivation during operation of the chemical reactor, which reduces efficiency. In addition, spallation can introduce fines into packed bed reactors, blocking some gas paths, increasing pressure losses, and reducing process or reaction efficiency.

[0082] As previously described herein, catalyst supports according to embodiments of the present disclosure may be fabricated by premixing SiC with Al (and optionally Si, particularly by using Al-Si alloys), pressing into dense pellets, and then further heating and melting at high temperatures in an oxygen environment. The resulting material (SiC / Al2O3) has a higher density and better oxidation resistance compared to conventional porous SiC. Experiments studying the oxidation behavior of SiC in the resulting composite of SiC and alumina pressed into pellets reveal a composite that is highly resistant to oxidation and subsequent volatilization, as evidenced by low mass gain under the following conditions, unlike bare SiC, which is easily oxidized in high temperature air and water vapor atmospheres:

[0083] The resistance of pellets with layers 1 and 2 to oxidation and volatilization was tested by heating the material at a temperature of 900°C in an environment of 25% water vapor in air. The material tested at 900°C in water vapor was first treated or heat treated at a temperature of 1250°C for 1 hour before performing the aging test. The heating rate to 1250°C in this test was 3°C / min and the cooling rate was 5°C / min. Similarly, the oxidation behavior of materials (coated or uncoated) treated at various temperatures from 1050°C to 1450°C was studied in an environment of 50% water vapor in forming gas (3% hydrogen, balance nitrogen). These reactions were studied for various periods of time. Figures 6A and 6B show the results from these studies. 6A and 6B are photographs showing sample results, and FIG. 7 is a plot of the mass gain of the samples under study. In the photograph of FIG. 6B, after 44 hours in 25% water vapor in air environment at 900° C., there is no visible change in the material (no mass gain or color change). In contrast, a commercial SiC pellet under the same conditions (FIG. 6A) is completely oxidized, as seen by the white color of the unprotected SiC pellet in FIG. 6A. FIG. 7 shows how a significant mass gain occurs over time when used in a high temperature environment with water vapor required for industrial methane reforming catalysts, and the importance of protecting the SiC.

[0084] To further quantify the mass gain, the pellets subject to this test are weighed and first dried at a temperature of 150°C. The dried pellets are loaded into an alumina ceramic boat and slid into the hot zone of a 1-inch nickel-Inconel tube. A flow of forming gas (3% H2 in N2) is passed over the pellets and the tube is heated to 900°C at a rate of 3°C / min. When the furnace temperature exceeds 300°C, water (pumped using an HPLC pump) is introduced into the tube. The water passes through a vaporization zone maintained at 500°C, converting the water to water vapor. Water is introduced such that the water vapor partial pressure is 50% of the total gaseous compounds. The test time begins when the furnace reaches 900°C. At the end of the timed test, the furnace is cooled at 5°C / min. When the furnace temperature reaches approximately 300°C, the water is turned off. The pellets are unloaded when the furnace has cooled substantially below 100°C and their mass is immediately recorded. The cumulative mass gain of the SiC and alumina composite pellets of the present invention is less than 1% mass gain over 300 hours, and more preferably, the protected pellets of the present invention have a mass gain of less than 0.1% over 300 hours when tested in a mixture of 50% water vapor in forming gas at 900° C. Similar results would be obtained from testing of catalytic particles (i.e., cores coated with a catalytically active layer).

[0085] As previously described herein, the pressed pellets are initially formed using a mixture of SiC and aluminum particles. The aluminum is dispersed within the pellet and plastically deformed around the SiC particles in a high pressure press operation. The particles are defined by substantially micron sized SiC particles (0.1 microns to 50 microns) that are mixed with the aluminum particles (0.1 microns to 50 microns) prior to densifying and forming the pellets created using a high pressure pelletizing press. When the pellets comprised of SiC and aluminum undergo an initial heat treatment process, the aluminum reacts preferentially with oxygen (in the form of air, oxygen, and / or water vapor) to form a protective flake comprised of aluminum oxide around the exposed or gas diffusion accessible (except solid diffusion) surfaces of the pellets' SiC particles. The most preferred form of the protective flake is the alpha-alumina phase. In one embodiment, the protective flake comprises a combination of alumina phases. The phase of alumina is controlled by the selection of heat treatment conditions, primarily temperature. Above about 900°C, alpha alumina predominates and the oxide formed at lower temperatures is further converted substantially to the dense alpha alumina phase. In some embodiments, the protective flakes are composed of alpha alumina and have an average thickness in the range of about 0.3 to 3 microns. Formation of the protective alumina flakes occurs at elevated temperatures above 850°C, such as by calcination at 900 to 1000°C for 2 to 20 hours.

[0086] The formation of a substantially dense alumina layer protecting the inner pressed SiC particles reduces oxidation or degradation of the SiC particles and extends catalyst life. The resulting catalytic core material exhibits less than 1% mass gain in 300 hours, and more preferably, the protected pellets of the present invention exhibit less than 0.1% mass gain in 300 hours when tested at 900° C. in a mixture of 50% water vapor in forming gas. Similar results would be obtained from testing of catalytic particles (i.e., cores coated with a catalytically active layer).

[0087] The resulting catalyst produced after formation of a protective alumina barrier and subsequent coating of active catalyst has been shown to be capable of withstanding 100 to 1000 hours of on-time during the conduct of a methane steam reforming reaction. The catalyst exhibits less than 1% activity loss between cycles. The catalyst is expected to have a catalytic life of at least 2 years before replacement due to a protective internal barrier against oxidative corrosion of the underlying high thermal conductivity SiC core. During the 2 year life, in situ regeneration cycles may be required to improve catalyst performance, but the catalyst will still be effective in operation and producing hydrogen. The operating conditions for the catalyst are 20 bar, steam to carbon ratio of at least 3, and a minimum of 2000 hr -1 and a tube wall temperature of at least 850°C, where methane conversion is greater than 50% and / or has an equilibrium approach temperature at least closer than 50°C.

[0088] In another embodiment, the catalyst according to the present disclosure will be consistent with an extended life of the steam methane reforming tubes. As the tube life is extended, the maintenance and plant downtime corresponding to tube replacement will be consistent with the catalyst life and catalyst replacement cycle. The end result is a methane steam reforming plant operating with increased uptime. In one embodiment using the catalyst of the present invention, the methane reforming plant has an uptime of greater than 0.95, more preferably greater than 0.98, and in the most preferred embodiment, the plant has an uptime of greater than 0.99. An uptime of greater than about 0.99 corresponds to a one week turnaround time or downtime when not producing hydrogen over an operating cycle of at least about two years. During the one week turnaround time, both the reaction tubes and the catalyst of the present invention housed therein are replaced to maximize the desired productivity or uptime (defined by the operating factor or the percentage of time the plant is producing product) of the methane steam reforming plant. For example, a commercial hydrogen plant producing at least 10 MM standard cubic feet of hydrogen per day using a catalyst of the present disclosure is operated continuously for 12 months, including the continued use of interrupted catalyst regeneration cycles lasting less than 48 hours, but not including complete shutdown of the plant (as may be required for tube replacement).

[0089] Improved selective oxidation reactions with the disclosed catalysts Selective or partial oxidation reactions combine a small molar volume of oxygen (added as pure oxygen, air, or some dilution with an inert gas) with a hydrocarbon reactant that may be in the gas or liquid phase. The oxygen reacts with the reactant hydrocarbons on the solid catalyst to preferentially produce high value products. Only a small amount of oxygen may combine with the reactants and / or desired products to form undesirable deep complete oxidation or combustion products. These reactions are exothermic to the desired partial or selective oxidation reactions, and the reaction energy is less than the heat released for oxygen molecules to form complete combustion products. The increase in temperature when heat is released from any of the series-parallel reactions increases the reaction rate to undesirable deep oxidation reactions. It is therefore advantageous to reduce the temperature rise of the catalyst during these reactions to produce higher selectivity to the target or desired partial or selective oxidation products.

[0090] An example of a selective oxidation reaction is the production of maleic anhydride from n-butane over a commercial VPO (vanadium-phosphorus-oxygen) catalyst. As described in Hoffman and Turek (2017), the gas-solid reaction mechanism is series-parallel, and the deep oxidation products can be formed in parallel and in series with the production of the desired product, maleic anhydride. The selectivity is very sensitive to the reactor temperature, and heat removal through the catalyst particle bed is a key parameter for efficient production.

[0091] Hoffman and Turek, 4800hr -1The performance is compared for catalyst bed thicknesses of 1.5 mm and 3 mm for a GHSV of 1000 MPa, a reaction temperature of 420° C., and an initial n-butane concentration of 1.4%. At a reaction diameter of 1.5 mm (tested as VPO catalyst particles packed in a microchannel slit or chamber) and an average catalyst particle diameter of about 400 microns, the selectivity to maleic anhydride was about 65% at about 60% n-butane conversion. At a higher n-butane conversion of about 95%, the selectivity to maleic anhydride drops to about 55%. The drop in selectivity with increasing conversion is due to a change in partial pressure within the catalyst bed that favors the deep oxidation reaction pathway. This is the result.

[0092] At the same catalyst particle size and reaction conditions, with a larger channel slit or gap or diameter of 3 mm, the selectivity drops to about 45% at about 95% conversion, while at equal conversion with the 1.5 mm slit, the selectivity was 55%. The lower selectivity at equal conversion and GHSV for the larger 3 mm slit compared to the 1.5 mm slit is a result of the increased temperature in the catalyst particle bed packed into the 3 mm reactor gap.

[0093] The measured reactor temperatures were essentially isothermal in the 1.5 mm slit reactor. The 3 mm slit reactor experimentally showed hot spots and temperature gradients of about 10° C. across the heat transfer distance of the 3 mm reactor for this case with an n-butane feed concentration of 1.4 vol.%. For a higher n-butane feed concentration of 4.5 vol.%, the hot spots rise to 15° C. in the 3 mm packed bed slit reactor. This type of hot spot formation and reduced product selectivity for selective oxidation reactions is common. GHSV is usually reduced to reduce the local heat release rate and maintain good selectivity.

[0094] In one embodiment, the use of the SiC-based catalyst of the present disclosure allows for an increase in GHSV of about 0.1 to 10% while maintaining comparable selectivity for comparable tube diameter, feed composition, temperature, pressure, catalyst composition and average catalyst particle size.

[0095] The catalysts of the present disclosure allow for higher effective thermal conductivity for fixed bed or particulate catalysts. When applied to selective oxidation reactions for the range of effective thermal conductivities measured, the expected increase in selectivity for the desired partial or selective oxidation reaction is about 0.1% to about 10% higher at equal WHSV, feed composition, temperature, pressure and active catalyst composition. WHSV (weight hourly space velocity) is defined as the weight of feed per hour divided by the weight of catalyst contained in the active layer or shell coated around the SiC core of the disclosed catalyst.

[0096] In another embodiment, the catalyst of the present disclosure can be applied to selective liquid-phase oxidation reactions. Liquid-phase reactions are usually carried out at very long residence times and very low WHSV of the catalyst. The mass diffusivity of reactants in liquid-phase reaction media is about three orders of magnitude lower than the gas-phase mass diffusivity, and therefore the eggshell (i.e., core-shell) morphology of the catalyst of the present disclosure provides advantages for effective catalyst use during liquid-phase selective oxidation reactions. Liquid-phase oxidation is also highly exothermic, and some reactions may operate at near-explosive conditions. Heat removal is essential for safe operation and maintaining high selectivity to the desired selective oxidation products. The catalyst of the present disclosure will remove heat more effectively than conventional fixed-bed pellets due to its higher effective thermal conductivity. When operated at the same WHSV, feed concentration, temperature, pressure, and catalyst composition, the selectivity to the high-value selective oxidation products is expected to increase by about 0.5 to 15 percent over conventional fixed-bed catalysts. The temperature of liquid phase selective oxidation over fixed bed particulate catalysts is often controlled by running at a low WHSV to minimize heat generation and thermal hot spots while maximizing the desired product selectivity. Because the WHSV is very low, the selectivity is often very high for liquid phase selective oxidation reactions. It is expected that the use of the catalysts of the present disclosure can increase the reaction WHSV without adversely affecting the product selectivity. In one embodiment, the WHSV of the productivity of the liquid phase selective oxidation reaction will increase by a factor of 1.2 while maintaining the same selectivity. In an alternative embodiment, the WHSV and reaction productivity will increase by 1.05 to 1.3 while maintaining the same selectivity for a catalyst of comparable composition when operated at similar hydrocarbon and oxidant feed rates, diluent composition, temperature, and pressure.

[0097] Catalysts including SiC-supported catalysts that can be loaded on-site without modification of the loading process or reactor Steam methane reforming (SMR) is used industrially to produce hydrogen and has a high It is an endothermic process (ΔHr=-206 kJ / mol). The process is operated at high pressure (up to 40 bar) and high temperature (reaching a reaction temperature of 950° C. or a tube temperature of 1050° C.) to ensure high methane conversion as a result of the thermodynamic equilibrium limit for this reaction at high temperature and pressure.

[0098] Heat is supplied around the outside of a series of parallel reaction tubes containing active catalyst to maintain high temperatures and provide the energy necessary to drive the powerful endothermic reactions. Several technologies have been designed to heat the reactor. Methods for supplying heat to the endothermic reactions include convective heat transfer, radiative heat transfer, and direct combustion or burners. Mini-reformers are also an active area of ​​development to enhance heat transfer and reduce the size and cost of industrial hydrogen production from methane reforming. Most industrial methane reformers supply heat from an integrated natural gas burner. The reactor includes a box-shaped radiant section that houses the burner, and a convective section that is intended to recover waste heat from the flue gas exiting the radiant section.

[0099] The catalysts used in steam methane reforming are typically made of Ni deposited on a high surface area support, primarily high surface area porous alumina. Alternative metals such as cobalt and noble metals also exhibit high activity but have not been widely adopted due to cost. Nickel surface area is the primary factor controlling catalytic activity, but overall hydrogen production is primarily limited by heat transfer, not catalytic activity.

[0100] For use in industrial reformers, a typical Ni / Al2O3 catalyst is formed into cylindrical pellets with a length of less than about 10 cm (usually 1-5 cm long) and a diameter of less than 10 cm (usually 0.5-3 cm diameter). Radial holes are formed throughout the cylindrical pellet to ensure maximum methane contact with the Ni particles and reduce the possibility of increased pressure drop. These catalyst pellets are typically packed into reaction tubes with a diameter of about 0.1 m and a length of up to about 10 meters.

[0101] Loading industrial SMR reactor tubes with catalyst pellets is not a simple process. A typical 10m tubular reactor is loaded with catalyst from above, and the pellets fall under gravity. Essentially, the pellets are subjected to significant shock as they tumble during loading from a high fixed height. Companies have designed loading methods aimed at minimizing this mechanical shock. These methods include (1) the use of Supersacks and attached sock, which allow the pellets to be loaded gradually, minimizing the maximum free fall distance; (2) the Unidense method, which loads the catalyst pellets using a proprietary Unidense device; and (3) the use of other vibration techniques, which allow the catalyst loading to be densified stepwise along the length of the tube, minimizing mechanical stress on the catalyst pellets. A dense loading is preferred to minimize non-uniformity in pressure drop between the many parallel tubes that make up an industrial methane reforming plant. Flow maldistribution between the tubes impacts performance and catalyst life, as these tubes with low flow cannot utilize the heat provided by the external burners, which in turn creates hot spots on the walls of the metal tubes. Hot spots serve to shorten the life of the reactor tubes.Finally, denser packing of the catalyst is required and preferred to reduce catalyst damage due to collision, friction, abrasion, and to minimize flow unevenness.

[0102] The catalysts of the present disclosure are designed to have advantageous thermal properties as well as be free-flowing, and therefore can be utilized in current SMR reactor tubes without modifying existing equipment or modifying existing catalyst loading and loading densification tools. The catalysts of the present disclosure can be loaded in-situ after installation of the original or replacement tubes. In an alternative embodiment, the catalysts of the present disclosure are loaded at a separate facility and then loaded onto the replacement reactor tubes during a factory turnaround. The catalyst may be shipped with the reaction tube. This embodiment minimizes the need for specialized catalyst loading equipment on-site and allows for high availability of catalyst loading equipment from specialized facilities.

[0103] Given the free-flowing nature of the catalyst of the present disclosure, it will follow conformal packing properties. If the catalyst needs to be replaced more frequently than the frequency of tube replacement, the catalyst can be packed more easily avoiding tube deformation. Industrial methane reforming tubes operated at high temperatures and pressures will deform over time during operation due to mechanical creep. Tubes that may no longer be perfectly symmetrical can still be reloaded relatively easily due to the conformal and free-flowing nature of the catalyst of the present disclosure. The conformal packing attributes of the catalyst of the present disclosure reduce the overall cost of plant operation by allowing catalyst replacement before the end of the useful life of the industrial reforming tube or to be replaced at the same time as a new reactor tube.

[0104] The disclosed catalysts are made from densified (>60% of theoretical density) SiC cores with superior mechanical properties. The crush strength and vibration resistance of SiC-based catalyst pellets are improved over those of conventional porous alumina pellets. The disclosed catalysts provide closer to expected initial performance and longer catalyst life after catalyst loading by reducing crack formation, catalyst fracture, and fines formation after the catalyst loading process.

[0105] The disclosed catalyst support materials have been subjected to mechanical studies aimed at determining how they would withstand typical packing processes used in industrial reforming tubes. These mechanical studies were developed using standard ASTM methods and include radial crushing tests that involve placing pellets under radial packing to study how much force is required to crush the pellets. Table 7 summarizes the mechanical properties of the catalyst cores of the disclosed supports compared to commercial catalysts. The results show that the materials are superior and that no special changes to current reactor packing methods are required. [Table 7]

[0106] The crush strength of the disclosed catalyst supports is at least 2 times, and in one embodiment 2 to 5 times, greater than the commercially available catalysts. The crush strength of the disclosed catalysts is greater than 50 N / mm and has a range of 50 to 150 N / mm, whereas the crush strength of the commercially available reforming catalyst is 44 N / mm. The crush strength of the disclosed and commercially available catalysts was performed according to the prescribed ASTM international test protocol (ASTM D6175-03(2013)).

[0107] In Table 7, "Gen1" is a commercially available porous SiC catalyst support coated with BSAS. The porous SiC catalyst support is not dense enough (i.e., less than 60% of theoretical density). "Gen2 and 3" are composite cores containing SiC / BSAS, and "Gen4" and "Gen5" are composite cores containing SiC / Al2O3 with slightly different amounts of lubricant added during processing.

[0108] Fischer-Tropsch reaction catalyst Fischer-Tropsch synthesis (FTS) (see Equations 1 and 2 below) is a method for converting non-petroleum carbon sources, including coal, coal seam gas, and biomass, into liquid fuels and chemicals. These sources are converted to fuels and chemicals via FTS by producing synthesis gas, also known as syngas (CO and H2), through techniques such as steam reforming or gasification. Two categories of products are obtained from FTS: non-oxygenated products such as gasoline, diesel, and light olefins, and oxygenated hydrocarbons such as methanol, ethanol, and mixed higher alcohols. (2n+1) H2+ nCO = C n H 2n + 2+nH2O (Formula 1) 2nH2+ nCO = C n H 2n + nH2O (Equation 2)

[0109] Due to the role of FTS in converting non-petroleum carbon sources via syngas, FTS have seen renewed interest in recent years due to dwindling crude oil reserves and rapidly increasing global demand for liquid fuels.

[0110] Critical to the success of FTS is the catalyst, which plays an active role in the conversion of syngas to products. Catalysts with higher activity, selectivity, and stability are the main drivers of current work in FTS research. Typical active metals used in FTS are Fe, Co, Ru. Usually, these metals are deposited on supports such as Al2O3, SiO2, TiO2, among others. FTS is an exothermic reaction that releases heat to the surroundings. As a result, excessive heat on the catalyst surface can lead to hot spots, compromising the performance (activity and selectivity) of the catalyst. To be effective, this heat must be dispersed faster away from the surface of the catalyst. Therefore, a catalyst support system that can remove heat from the reaction surface to the outside of the tube is highly desirable. Thus, apart from a catalyst being active, selective, and stable, its ability to efficiently remove heat from the reaction surface, thus preventing the development of hot spots, makes it a more efficient catalyst. An increase in efficiency can lead to an increase in activity or selectivity.

[0111] The catalyst supports (i.e., cores) of the present disclosure (high effective thermal conductivity support materials) provide improved support for FTS catalysts. High thermal conductivity compared to the low thermal conductivity of current FTS supports enhances the removal of heat from the reaction surfaces. This leads to the avoidance of thermal hot spots and thus efficient FTS catalysts.

[0112] The Fischer-Tropsch reaction combines carbon monoxide and hydrogen (syngas) over a cobalt or iron-based catalyst at high pressure and temperature to enable the chain-forming reaction that produces synthetic crude oil. The product mixture is a mixture of C1 (methane gas) to C2 (synthetic crude oil). 100 and beyond (solid waxes). Synthetic crude is then refined and upgraded to create different product mixes: gasoline, diesel, jet fuel, and waxes.

[0113] It is desirable to convert as much of the syngas as possible to carbon fractions greater than 5 carbon atoms in order to minimize the amount of undesirable light gases, primarily methane. High carbon efficiency is desired and is characterized by the chain propagation, alpha. Alpha is the chain growth parameter of the Anderson-Schultz-Flory distribution (see Equation 3 below), where F n is the mass fraction of hydrocarbons with n carbon atoms (e.g., octane, CH 18 (n=8) [ka]

[0114] 8A-D show the nth carbon number for alpha ranging from 0.8 to 0.99. As alpha increases, the mass fraction of heavier hydrocarbons increases significantly. As alpha approaches a value of 1, the resulting hydrocarbon product consists of very long chain hydrocarbons that are essentially solid wax. In practical systems, an alpha value of 0.95 is very good and minimizes the amount of methane slip or light gas produced at selectivities below 5 mole percent. Alpha values ​​below 0.8 are not considered adequate and represent methane slip of more than 10 mole percent. Note that the composition of light gases (less than 5 carbons) may deviate (exceed) the weight fraction predicted by the traditional Anderson-Schultz-Flory distribution.

[0115] The chain formation reactions (equation 4 below) are favored at low temperatures, while higher temperatures favor the production of light gases, primarily methane (equation 5 below). The Fischer-Tropsch reaction is highly exothermic and heat must be removed from the chemical reactor during operation to avoid thermal runaway and to control the selectivity to the desired products. CO + 2 H2 = (-CH2-) + H2O ΔH r_298K = -152 kJ / mol (Equation 4) CO + 3 H2 = CH4 + H2O ΔH r_298K = -206 kJ / mol (Equation 5)

[0116] The chain formation reaction is slightly less exothermic than methane formation, so hot spots within the catalyst tend to further enhance unwanted methane formation in a negative feedback loop. In some cases, thermal runaway can occur, where insufficient heat removal and high internal temperatures promote a high rate of methanation reactions.

[0117] Fixed catalyst bed designs are common for cobalt-based catalysts. Typical operating conditions range from 190°C to 240°C, with pressures ranging from 10 to 40 bar. The reaction tubes are usually cooled by steam generation as water flows around and between the tubes, removing the reaction energy at the end of each catalyst-filled tube. A temperature increase of 10°C or more within the catalyst bed or particles increases the molar selectivity for methane production by 5% or more and reduces the alpha by 0.05 or more. It is desirable to minimize heat generation or hot spots within the catalyst bed to less than 10°C, more preferably less than 5°C.

[0118] One option to reduce catalyst hot spots is to reduce the diameter of the tubes housing the particulate or fixed bed catalyst. The practical tube diameter of about 1-2.5 inches can be reduced to about 0.5-0.75 inches, but this adversely affects the economics of the overall process. More tubes to achieve a given capacity or production rate requires more metal (higher cost) and more complexity to manifold more tubes in a larger vessel. It would be desirable to reduce hot spots in fixed bed catalysts without reducing the diameter of the reactor tubes.

[0119] The catalyst of the present disclosure has two features that actively reduce hot spots and provide better reaction performance in a reactor filled with Fischer-Tropsch catalyst. The first advantage is a higher effective heat transfer rate within the fixed bed. Improved radial heat transfer removes more heat generation and reduces hot spots within the catalyst bed. Improved axial and radial heat transfer reduces or smooths out large temperature gradients and reduces the overall magnitude of hot spots. This results in lower hot spots, which increases reaction alpha and reduces the amount of unwanted methane. A higher reaction alpha is preferred because the value of the wax produced is high and, depending on current market drivers, the wax can be hydrocracked into valuable jet fuel or different fuel blends.

[0120] A Fischer-Tropsch catalyst made with the disclosed thin catalyst layer on a SiC-based core is expected to result in a 2° C. to 8° C. reduction in exotherms or hot spots compared to conventional Fischer-Tropsch catalysts when operated under comparable conditions. The molar selectivity to methane produced by the catalyst is reduced by more than 2%, and perhaps 2-5%, from the corresponding conventional catalyst when operated under similar conditions. -1 At an onset temperature of about 200-240° C. for the cobalt-based catalyst and about 300-350° C. for the iron-based catalyst, a pressure of about 10-40 bara, and a hydrogen to carbon monoxide feed ratio of about 1.9-2.5, the product alpha is at least 0.02 higher and in the range of 0.02-0.08 higher.

[0121] A second advantageous feature of the disclosed catalyst for the Fischer-Tropsch reaction is the local control of the hydrogen to carbon monoxide ratio. From the reaction equation, a syngas feed ratio (H2 / CO ratio) close to 2 favors the desired chain-forming reactions, while a syngas ratio close to 3 favors undesirable methane formation. Within the catalyst pores, hydrogen diffuses much more easily and quickly to the internal active catalyst sites than carbon monoxide. As the hydrogen to carbon monoxide ratio approaches 3, methane formation within the catalyst is promoted. Increased methane formation within the catalyst particle has two negative attributes - more undesirable methane is formed, and more heat is released within the particle, which serves to shift reactions further away from the desired chain-forming reactions, resulting in even more methane formation.

[0122] The use of eggshell catalysts, in which the active catalyst is impregnated in a thin ring or shell around the outside of a porous catalyst pellet, has been described in the Fischer-Tropsch prior art. Eggshell catalysts act to reduce the number of active catalyst sites where the local syngas ratio is greater than 2, typically greater than about 2.5 to 3.

[0123] The catalyst structure of the present disclosure uses a densified (60% or more of theoretical density) catalyst core rather than a porous core, so the center of the catalyst pellet cannot fill with unconverted hydrogen and remain a reservoir of liquid or wax products formed. An internal reservoir of liquid or wax inside the catalyst particle makes catalyst regeneration more difficult. Unconverted hydrogen remaining in the porous core of the catalyst particle can back-diffuse to the inner edge of the eggshell catalyst, thereby increasing the local ratio of hydrogen to carbon monoxide, which in turn increases the undesirable methane selectivity.

[0124] The catalysts disclosed herein have hydrogen and carbon monoxide diffusing only from the exterior of the catalyst particle surface due to the solid core, and diffusion distances are kept short, i.e., 10-100 microns, within the exterior catalyst coating of the dense pellet. When operated under similar conditions, selectivity to the desired chain-forming reaction is increased with the disclosed catalyst, and alpha values ​​are expected to be 0.02-0.08 higher than conventional catalyst pellets, and methane selectivity is expected to be 2-5% lower than conventional catalysts. The expected performance improvements of lower methane selectivity and higher alpha represent a significant improvement in the overall process economics of the Fischer-Tropsch process.

[0125] The disclosed Fischer-Tropsch catalysts according to the present disclosure can be used in conventional gas to liquids plants. Methane or natural gas is steam reformed to produce syngas before undergoing process steps to reduce the temperature and remove some hydrogen (to approach a syngas ratio of 2 to 3) before being introduced into a fixed bed Fischer-Tropsch reactor. The disclosed Fischer-Tropsch catalysts can also be used in non-traditional gas to liquids plants, including the use of biogas or bio-derived syngas formed from a gasification process using waste or biomass feedstocks. The syngas production process can include partial oxidation, autothermal reforming or conventional reforming to form a carbon monoxide and hydrogen syngas feed mixture prior to the Fischer-Tropsch process utilizing the disclosed catalyst.

[0126] Catalyst for the production of benzene, toluene and xylene (BTX) Benzene, toluene and xylenes (commonly referred to as "BTX") are important petrochemical compounds and are among the most abundantly produced chemicals in the world. BTX is defined by a product mixture that contains benzene, toluene, and / or xylene. BTX chemicals are essential feedstocks for the manufacture of automotive products, fibers, plastics, solvents, and many other common industrial products. BTX is primarily produced by endothermic catalytic reforming of naphtha refined from petroleum, particularly naphtha obtained from the distillation of crude oil. Bio-based processes for producing BTX chemicals are under development but face similar challenges as seen in conventional naphtha reforming, including thermally limited production rates and strong catalyst deactivation exacerbated by cold spots. Catalysts produced according to the present disclosure are effective for use in bio-based processes as well as conventional BTX production using naphtha feedstocks.

[0127] As an example, a typical catalytic reforming system for producing BTX from naphtha includes multiple reactors (e.g., 3 or 4) operating in series. Because the catalytic reaction is endothermic, heaters are usually provided upstream of the first reactor and between the reactors to heat (and reheat) the gas mixture. Electrical heaters are also provided along the reaction tubes to provide the additional energy required for the endothermic reaction. The reactors are usually packed with a catalyst made of Pt deposited on chlorinated Al2O3. The base catalyst has been modified over the years by adding various elements that extend the catalyst's life and reduce deactivation. The reaction is carried out at temperatures up to 550 °C and pressure levels up to 40 bar.

[0128] There are various reactions that take place in catalytic reforming reactors. In the production of BTX, the dehydrocyclization of paraffins to aromatics and aromatization of paraffins lead to the formation of BTX compounds. These reactions are endothermic and characterized by consuming heat as heat is supplied to the catalyst from the outside. For this reason, heaters on the outside of the reactor tube walls are required to maintain a high heat generation rate to maintain sufficient heat flux across the reactor walls to drive the reactions. Heat is also added to the cooled effluent gas mixture from the primary reactor stage using gas-gas heat exchangers placed between the reactors to preheat the reactants before introducing them to the next reactor in the series. The thermal conductivity properties of porous alumina catalyst pellets are poor and therefore the heat transfer efficiency from radial heat transfer is limited by current catalyst technology.

[0129] The disclosed catalyst cores having high effective thermal conductivity are advantageous for use as naphtha reforming catalysts for producing BTX. Use of the disclosed catalyst support technology will result in improved heat transfer from the reactor tube wall to the active catalyst sites across the reactor radius, thus resulting in higher BTX productivity.

[0130] Fixed-bed reactors used in semi-regenerative reactor designs for catalytic reforming of naphthalene to form BTX typically contain additional reactor beds (e.g., three initial reactors plus a spare used during regeneration) to maintain continuous and steady production. The reaction is prone to coke formation, requiring a regeneration cycle for each fixed bed every 6 to 24 months. Performance slowly declines as carbon accumulates during the regeneration cycle. The catalyst can only be regenerated three to four times before needing replacement.

[0131] The disclosed catalysts of the present disclosure will improve the radial heat addition from the tube walls to the endothermic reactions occurring within the catalyst. With more heat added to the reactor, BTX manufacturability can be increased by reducing cold spots. The reduction in cold spots (higher temperature gradient) within the reactor also reduces the rate of deactivation, including carbon formation. Lower deactivation rates increase production capacity between reactor regeneration cycles and increase the time between regeneration cycles, thereby extending the total catalyst life. Turaga and Ramanathan reported that manufacturability or best catalyst activity for naphtha reforming to BTX is in the temperature range of 733-798 K (460-525 °C), with deactivation increasing in the temperature range of 755-773 K (482-500 °C). Thus, the disclosed catalysts of the present disclosure having a higher effective thermal conductivity will result in smaller cold spots and therefore lower deactivation rates.

[0132] Maintaining temperatures over 500°C throughout the reactor radius can be possible with reduced deactivation rates and with the use of the disclosed high effective thermal conductivity catalysts. In one embodiment, the disclosed catalysts can enable simplified construction of naphtha reforming plants. Existing naphtha reforming plants can be retrofitted to increase capacity and the inventive process based on the use of the disclosed catalysts can be based on two fixed bed reactors instead of three or four. The first primary fixed bed reactor operates with improved radial heat addition to enable the disclosed catalyst to reduce internal catalyst temperature gradients to maintain manufacturability and minimize deactivation, including coking. Reactor operation can be switched between two reactors to enable regeneration of one fixed bed reactor while maintaining production capacity in the second fixed bed reactor. In one embodiment, a four-reactor bed naphtha reforming plant can be retrofitted as two two-reactor naphtha plants, thereby increasing the overall plant production capacity of BTX.

[0133] The other major type of naphtha reforming to BTX is the continuous catalytic reformer, where a portion of the catalyst is removed from the reactor bed during operation and flows to a regeneration reactor before returning to the top of the original catalyst bed. For this type of process, the free flowing nature of the catalyst of the present disclosure, along with its improved effective thermal conductivity, acts to reduce deactivation and increase the time between regeneration cycles.

[0134] Examples of several types of naphtha reformers have been described in the prior art and include the continuous catalytic reforming reactor (CCR) or continuous circulating process used by manufacturers or support catalyst suppliers such as Accens, Criterion Catalyst Company, ExxonMobile, Indian Petrochemicals Corporation, IMP (Instituto Mexicano del Petróleo) and UOP. Examples of semi-regenerative reactors for naphtha reformers used by manufacturers or support catalyst suppliers include (Axens, Criterion Catalyst Company, Exxon Mobile (Powerforming process), BP (Ultraforming process), Chevron (Reniforming process), BASF (Magnaforming process developed by Engelhardt), Air Products and Chemicals (Aldrichforming process), Indian Petrochemicals Corporation, IMP (Instituto Mexicano del Petroleo), and U.O.P.).

[0135] BTX can also be produced from biomass rather than crude oil. One process under development by Anellotech uses biomass-derived fast pyrolysis oil to produce BTX over a zeolite catalyst in a single-stage catalytic fluidized bed reactor. The catalyst slipstream is continuously regenerated. Virent has also developed a bioforming process to produce BTX from biomass feedstocks to co-produce jet fuel and gasoline. Other researchers [5] have developed a production process for bio-feedstocks, including crude glycerol, to produce Bio-BTX. The reaction remains endothermic, and improved heat addition, made available by the catalyst of this disclosure, would improve efficiency. Bio-BTX production remains a challenge due to the co-production of carbon or solid coke, which coats the catalyst and limits production efficiency.

[0136] It is contemplated that use of the catalysts of the present disclosure can extend the catalyst regeneration interval by 1 to 12 months compared to conventional catalysts defined by catalyst composition, feed WHSV (grams feed per gram catalyst per hour), and comparable feed composition.

[0137] Catalysts including SiC supported catalysts that can provide longer tube life The highly thermally conductive catalyst supports created by the disclosed catalyst systems described herein allow for significant energy savings for strongly endothermic reactions (such as steam reforming of methane or dry or CO2 reforming of methane). The disclosed catalysts also reduce wall temperatures, allowing for simplified metallurgy or extended tube life. Alternatively and in addition, such catalysts can increase the production capacity or throughput of the reactor.

[0138] A well-established problem in steam methane reforming is the need for high operating temperatures (800-950°C) and high operating pressures (up to about 40 atm) to overcome fundamental thermodynamic limitations on reaction conversion and selectivity of hydrogen production from methane. These conditions are also necessary to enable downstream synthesis gas purification by other reactors such as pressure swing adsorption or Fischer-Tropsch synthesis. To channel heat to the endothermic reactions, the metal walls housing conventional particulate or fixed-bed catalysts must operate at very high temperatures, generated by external burners. Combustion near the exterior surface of the tubes creates the high wall temperatures required to drive sufficient energy within the tubes and through the particulate catalyst to match the energy consumption demand from the strongly endothermic reactions.

[0139] The highly endothermic methane reforming reaction is shown below in Equation 6. The highly endothermic dry reforming reaction is shown in Equation 7. The water gas shift reaction, which occurs in parallel and is fully reversible according to the thermodynamic limit as a function of temperature, is shown in Equation 8. Combustion of the methane reaction provides energy for the endothermic reaction and is shown in Equation 9. CH4+ H2O = CO + 3 H2ΔHr_0 = 206 kJ / mol (Equation 6) CH4+ CO2= 2 CO + 2 H2ΔHr_0 = 247 kJ / mol (Equation 7) CO + H2O = CO2+ H2ΔHr_0 = -41 kJ / mol (Equation 8) CH4+ 2O2= CO2+ 2 H2O ΔHr_0 = -803 kJ / mol (Equation 9)

[0140] High wall temperatures coupled with high internal pressures generate tremendous thermomechanical stresses in the reactor tubes. Very expensive high chromium and high nickel alloys are centrifugally cast to meet the design requirements of the operation. However, even these tubes are taxed by the combination of heat and pressure, which accelerates grain growth, precipitation, and grain boundary void formation (due to microstructural coarsening). The operating conditions of the tubes are squarely in the metallurgical creep regime limiting the practical life of these expensive components. Tube lifespans of as little as one year in industrial use are not uncommon.

[0141] Tube failure is highly dependent on operating temperature through the Larson-Miller relationship (Ref API 530). Tube life is very sensitive to the absolute operating temperature of the tube, so operation at tube wall temperatures significantly above design can rapidly increase the number of tube failures. A 20°C increase in tube metal temperature can reduce tube life by more than 50% (Ref. Bou Matha, World Academy of Science, Engineering and Technology International Journal of Chemical and Molecular Engineering, Vol. 4, No. 11, 2010).

[0142] As described herein, catalysts and catalyst supports constructed from high thermal conductivity support materials improve the effective thermal conductivity of the catalyst particle bed. As the effective thermal conductivity of the catalyst bed is increased by the disclosed catalyst system, the wall temperature required to achieve comparable performance is reduced. More heat is drawn away from the tube walls and into the catalyst bed and reactant gases. This effect reduces the required heat generated by the reactor burner, resulting in a significant reduction in maximum operating temperature while also reducing fuel consumption. Lower fuel feed rates improve carbon efficiency for hydrogen production, thus reducing production costs. By reducing the operating temperature of the metal reactor walls, the tube life can be significantly extended, resulting in less tube maintenance, higher plant uptime, and longer change intervals during reactor operation. Use of the disclosed catalyst is expected to extend tube life by 3 to 18 months over the existing tube life of approximately 12 months when operated with conventional reforming catalysts. The expected tube life of a steam methane reforming plant when operated with the disclosed high effective thermal conductivity catalyst system is in the range of 15 to 30 months.

[0143] Additionally, lower operating temperatures may provide other advantages in system design, allowing for thinner walled tubes, tubes of less expensive alloys, or more conventional manufacturing processes, which may also contribute to reduced capital costs.

[0144] Catalysts containing SiC-supported catalysts capable of lowering metal wall temperatures As described herein, catalysts and catalyst supports constructed from high thermal conductivity supports (i.e., cores) provide improved heat transfer in packed beds, even while maintaining similar geometry and bed packing density as conventional materials. Effective bed thermal conductivities were experimentally determined using the experimental procedures and apparatus described in the Example entitled "Reduced Wall Temperatures and Increased Hydrogen Production for Steam Methane Reforming Using Disclosed Catalysts" later in this specification. As described in that Example, the expected wall temperatures using the disclosed catalyst systems can be 10-30°C lower compared to the required wall temperatures of conventional methane reforming catalysts while providing comparable hydrogen production rates.

[0145] The relationship between the thermal conductivity of the material and the conductivity of the bed is a function of several non-trivial non-linear relationships. [ka] where T is the pellet and gas temperature, P is the gas pressure, and ρ p is the density of the catalyst pellet, and φ p is the pellet porosity, k p is the thermal conductivity of the catalyst pellet, and ε n、p is the total normal emissivity of the catalyst pellet surface, and d p is the diameter of the pellet, and h p is the pellet height, and d tubeis the diameter of the reactor bed, U is the superficial gas velocity (in Darcy), and k g is the thermal conductivity of the void gas, and ε b means bed porosity, and R e d p is the Reynolds number of the surface gas for e d p is the Peclet number of the surface gas relative to the

[0146] Although highly complex, these relationships can be broken down into core components. k effective = k p,o + k convective + k radiation where k p、o is the static pellet conductivity including the effects of porosity and grain boundary interactions. k convective is the result of convection effects, heat dispersion, turbulent conduction, and other gas and pellet interactions in the porous bed. radiation is directly related to the emissivity of the pellet surface and the pellet temperature. For the same pellet and reactor geometry, the convection effects are approximately the same. Radiation effects deviate from the change in material emissivity, but can be largely neglected for comparative reasons. Furthermore, for the materials investigated, the surface emissivity is within 10-15%. Thus, the increase in conductivity is directly related to the stationary pellet conductivity. This is evident from Figure 11, as described further in the relevant text herein. Over a wide range of temperatures, the total effective radial conductivity is approximately 1 / k, which is the stationary pellet conductivity. r、o are consistently separated by the same value.

[0147] Calculations of stationary radiative bed conductivity for representative geometries were performed using simplified models, numerical simulations, and experimental methods. The effect of pellet porosity and temperature on a stationary packed bed is shown in Figure 9. A decrease in thermal conductivity is caused by pellet porosity until the porosity reaches 40%. At this porosity level, the internal pellet thermal conduction losses are overridden by gas conduction and the emissivity of the pellet's surface. In this model, the highly porous surface effect on emissivity was ignored. Add 1 to the porosity and density factors. Thus, material composition, porosity, grain boundaries, and surface emissivity are important measures to control the bed conductivity.

[0148] Therefore, by increasing the thermal conductivity of the catalyst by using a high thermal conductivity material instead of the conventional catalyst (i.e., by replacing the porous Ni-Al2O3 composite with a catalyst coating on a densified support comprising SiC), the heat transfer capacity of the bed is improved by about 4 times at stagnant conditions, with a further increase from about 1.5 to 3.5 at expected system flows of 2000 to 5000 GHSV, which represent methane reforming reactions at high temperatures (see Figures 10, 11 and Table 8), due to the effects of heat dispersion and pressure turbulence conduction. [Table 8]

[0149] Increasing the effective radial thermal conductivity transfers heat more efficiently from the hot reactor tube walls to the catalyst bed and reactant gases, driving endothermic reactions more efficiently. Although the heat required to complete the reaction remains unchanged, lower peak temperatures reduce heat losses and allow for reduced energy input in the form of fuel and oxygen (or air) feed rates.

[0150] The temperature gradient between the tube wall and the center of the catalyst particle bed is reduced, which allows for lower tube wall temperatures and equivalent hydrogen production. Alternatively, the tube walls can be maintained at the same temperature with similar tube life as conventional catalysts, while increasing hydrogen throughput or productivity by 5-40% compared to conventional catalysts. Tube life can be significantly increased, and thinner walled tubes, tubes with cheaper alloys, or more conventional manufacturing processes can be used, all of which would provide significant capital cost savings for the system.

[0151] Examples demonstrating SMR improvements using catalysts of the present disclosure Reduced wall temperature and increased hydrogen production for steam methane reforming using the catalyst of the present invention Steam methane reforming (SMR), or reforming, is an important industrial reaction for producing hydrogen. Hydrogen is commonly used in refinery applications for upgrading crude oil into commodity fuels, metal processing, hydrogenation of lipids, and many other diverse areas. Hydrogen is produced by adding steam to methane (the main component of natural gas) and reacting it over a nickel-based catalyst at high temperature and pressure. The SMR reaction is highly endothermic, and a significant amount of energy (e.g., heat) must be added to drive the reaction for hydrogen production. CH4 + H2O = CO + 3 H2(ΔHr 298K = 206 kJ / mol) CO + H2O = CO2 + H2(ΔHr 298K = -41 kJ / mol)

[0152] Industrial methane reformers utilize burner technology to burn natural gas outside a parallel arrangement of tubes (typically 100 cm in diameter) filled with catalyst pellets or particles. Heat or energy released by the exothermic combustion reaction is conducted through the tube walls and then into and through the packed or fixed bed reactor. This radial heat conduction through the catalyst particles drives the endothermic reforming reaction. Energy is also added and dispersed via gas convection: the gas thickens when it contacts the inner surface of the tube walls, then diffuses heat as it flows in a tortuous path around the catalyst particles.

[0153] Improving heat transfer through a fixed bed using the inventive higher effective thermal conductivity catalysts of the present disclosure This drives more energy into the reforming reaction and therefore requires a lower wall temperature for comparable performance. Reducing the peak wall temperature of the reforming tubes increases their lifespan and reduces failure rates, resulting in higher availability of the hydrogen plant. A 20°C reduction in wall temperature doubled the expected tube lifespan, according to a 2016 report by Rao et al. The replacement costs of high-nickel alloy SMR tubes and associated plant downtime increase the capital and operational costs of hydrogen production. Lower wall temperatures in industrial burners also reduce operational costs because less fuel is required.

[0154] At an equal wall temperature, the use of the inventive higher effective thermal conductivity catalyst of the present disclosure increases the overall reactor manufacturability since more hydrogen is produced per equal reactor volume compared to conventional commercial SMR catalysts.

[0155] As described herein above, the catalysts of the present disclosure rely on a central core of high thermal conductivity SiC passivated with an inner matrix of alumina and / or an outer coating of dense alumina, BSAS or other protective material, and coated with an effective layer of high surface area catalyst support with catalytically active metal (e.g., Ni) for methane reforming.

[0156] Data was collected to measure the effective thermal conductivity of the catalysts of the present invention and compared to conventional methane reforming catalysts. Specifically, the data was collected as follows: GHSV (hr -1 ) at 500 and 800 °C. Under stagnant conditions, the effective thermal conductivity of the catalyst of the present invention is about five times that of the conventional SMR catalyst (4.8 W / m K vs. 1.0 W / m K at 800 °C). As the GHSV increases (higher flow rate), the total effective thermal conductivity of the catalyst increases further due to heat dispersion and convective heat transfer.

[0157] FIG. 10 provides a comparison of experimental data for the effective thermal conductivity of a commercial SMR catalyst and the catalyst of the present invention, both with and without an active catalyst layer, as a function of temperature. -1 At a temperature of 800°C, the total effective thermal conductivity of the catalyst of the present invention is 13.1 W / m·K, while the conventional reforming catalyst is 9.6 W / m·K, an increase of up to about 36% in effective thermal conductivity due to the catalyst of the present invention. These respective values ​​of effective thermal conductivity are used to evaluate the reactor performance of the catalyst system of the present invention compared to the conventional industrial reforming catalyst. The addition of the catalyst support coating layer and its active metal made little difference to the effective thermal conductivity of the entire catalyst system of the present invention. Figure 11 shows a comparison of experimental data of the effective thermal conductivity of the commercial SMR catalyst and the catalyst of the present invention under stagnant conditions at 500°C and 800°C.

[0158] Modeling results supporting the high thermal conductivity properties of the inventive support material As shown in FIG. 11 (catalyst of the present invention (circles) compared to commercial catalyst (squares)), the catalyst support of the present invention has been experimentally shown to have superior pellet thermal conductivity compared to commercial alumina-based steam methane reforming catalyst. The thermal conductivity (k s The catalytic converter (catalyst of the present invention) changes from 6.3 W / m K at 500 °C to 4.5 W / m K at 900 °C, whereas the commercial SMR catalyst (k s The thermal conductivity of SiO2 (commercially available) remains almost unchanged at 1.0 W / m K in the temperature range.

[0159] With these experimentally determined values, the thermal properties of the stagnant packed bed can be determined using the modified Zener, Bauer, and Schlunder (ZBS) model shown in Figure 11 (k r,o : HP, solid line of the catalyst of the present invention and k r,o :Com, commercial dashed line). The catalyst of the present invention maintains the advantage of a consistent packed bed thermal conductivity of 1.25-2.00 W / m K over the commercial catalyst.

[0160] Using commercial geometry and reactor operating conditions for comparison, the effective radial thermal conductivity properties of the catalyst of the present invention under flow conditions are also enhanced over those of the commercial material. FIG. 10 shows a plot of the packed bed thermal conductivity of the commercial and inventive catalysts. Gas flow conditions 1970 hr -1 (superficial velocity 0.52 m / s), steam to carbon (S / C) ratio 2.7, inlet gas temperature 580° C., pressure 30.65 bar(a), and reactor diameter 152.4 mm (outer, inner 127 mm) and length 10.0 meters, there is an increase of more than 35% in effective radial thermal conductivity using the catalyst of the present invention compared to a commercial SMR catalyst.

[0161] The enhanced thermal conductivity of the catalyst of the present invention influences other reactor properties such as tube wall temperature. 2 1 shows plots of reactor wall temperature and reactor internal temperature versus axial distance for an applied average heat flux of 0.01 mm. For a fixed reactor heat flux, the improvement in bed conductivity with the catalyst of the present invention is 1.13°C increased tube wall temperature, 2. Reduced equilibrium distance, i.e., 4.0 meters (using the catalyst of the present invention) compared to 9.0 meters for the commercial SMR catalyst. Leads to.

[0162] Literature suggests that a 20° C. reduction in tube wall temperature doubles the life of the reactor tube. The catalyst of the present invention offers a tube wall temperature advantage of 13° C. compared to the commercial SMR catalyst, which would extend tube life by 65% ​​compared to the commercial SMR catalyst.

[0163] The tube wall temperature profile obtained from commercial operation was adapted to the catalyst fixed bed of the present invention, and the results are shown in Table 1. -1 % methane slip when the catalyst of the present invention is substituted (FIG. 14), confirming the superior properties introduced by the catalyst of the present invention.

[0164] The data presented in Figure 15 shows that at a constant tube wall temperature profile, increasing the gas hourly space velocity (GHSV) of the reactants leads to an increase in throughput with the catalyst of the present invention. -1 Only after the increase does it result in a methane slip of 8.0 vol.%. This increase in GHSV represents a 36% increase over the commercial catalyst. For the same wall temperature and slip, the catalyst of the present invention absorbs 33% more heat.

[0165] Table 9 summarizes the additional enhancements provided by using the catalyst of the present invention compared to commercial SMR technology. [Table 9]

[0166] Core-shell SMR catalysts defined by catalytic utilization The main catalyst used in methane steam reforming is Ni metal deposited on alumina (Ni / Al2O3). Current industrial catalysts are prepared by impregnating porous alumina with Ni ions in solution or by related processes. A typical industrial catalyst is a cylindrical pellet of approximately 0.5×0.5 in. (L×OD) dimensions with up to four (or more) internal holes. The composition of Ni in this catalyst is anywhere between about 10% and 20% by weight (average is about 12% by weight). The catalyst also contains small amounts of other elements compared to Ni. This is a single pellet catalyst with no outer or inner shell, but the Ni is dispersed throughout the pellet structure. A typical weight for this cylindrical pellet is 2.9 grams, but it depends on the size of the pellet used. Using the average value of about 12% and the above weight of the cylinder, the amount of Ni averages about 0.35 grams per pellet. However, due to mass and heat transfer limitations, this total weight of Ni per pellet is not active.

[0167] Core-shell materials consist of a core material on which another material is deposited to form an outer shell. These materials are usually designed to achieve a specific purpose. There are various purposes for the design of core-shell materials. One reason for forming a shell is to combine two materials to create two different properties within the same material, another reason is to take advantage of the properties of the materials that are brought about by a specific design and geometry, and finally to generate an entirely new set of properties that the individual materials do not possess. For example, Fe3O4 / SiO2 core-shell In core-shell materials, the properties of the core, such as magnetic susceptibility, can be properties of systems where magnetic separation is desired while utilizing the intrinsic luminescent optical properties of SiO2. The properties of the core and shell can be engineered such that the best synergy is realized. Core-shell materials have opened up research opportunities in almost every field of science, including nanotechnology, catalysis, optics, electronics, medicine, catalysis, materials, biotechnology, and energy storage.

[0168] Most of the core-shell materials have been synthesized at the nanoscale or microscale level. The synthesis process for creating these structures includes chemical or physical methods. Chemical methods include chemical synthesis or cation exchange processes. Chemical synthesis involves first synthesizing the core material and then growing the shell on top of the core. Cation exchange relies on synthesizing the core and subsequently generating the shell from the core itself via cation exchange of ions in solution with lattice elements. Physical methods are few and most of the reported methods involve deposition of gaseous components on the substrate. For reforming applications, Ni / SiO2, Ni / Al2O3, Ni / CeO2, and Ni / TiO2 catalysts have been designed and their activity has been studied in acetic acid reforming. Among the catalysts studied, Ni / Al2O3 showed the highest activity due to the small and narrow Ni nanoparticle size of the core. Core-shell Ni / SiO2 catalysts have also been used in biogas reforming.

[0169] The inventive catalysts of the present disclosure have a core-shell structure prepared by physical deposition of an oxide porous catalytic phase onto a composite solid core. In some embodiments, the core comprises a protective matrix of SiC and alumina. The catalytically active shell can be deposited, for example, via spray deposition of a selected metal or metal oxide from an aqueous or organic medium. In alternative embodiments, the catalytic shell or coating can be deposited by other means known in the art in addition to spray coating or deposition.

[0170] In a typical process, the pressed pellets of the present disclosure are coated with a slurry of catalyst support powder with or without active catalyst material in the slurry. If the slurry does not contain active catalyst material, the catalyst support layer is later impregnated with active catalyst material after the coating is formed.

[0171] The coating slurry is prepared by adding powdered materials in an organic medium, such as, but not limited to, ethyl cellulose, and alpha-terpineol. The powdered materials for supporting the active catalyst on the pellet core may be selected from the following non-exhaustive list: aluminum-silicon, zirconia-ceria doped alumina, alumina, zirconia doped ceria, alumina-silica mixtures, gamma alumina, alpha alumina, magnesium promoted alumina, calcium promoted alumina, sodium promoted zirconium-cerium oxide, cerium oxide, titania promoted silica, etc. The above oxides may be applied with or without one or more of the following metals (or other catalytically active materials): nickel, platinum, rhodium, ruthenium, cobalt, rhenium, iridium, among others. Elements known to play a role in coke formation or promote inhibition may be added optionally.

[0172] At laboratory scale, the as-pressed (green) catalyst pellets are weighed and placed on a stainless steel strainer. The coating slurry is transferred to a specially made glass container connected to a slurry spray system for manual deposition. The porous outer layer coating is applied manually by manually spraying the above slurry onto the pellets. The pellets are constantly stirred on the strainer for uniform coating. The coated pellets are then dried at a temperature of 70°C to 120°C for 30 to 60 minutes. After drying, the final weight is measured to determine how much porous material in the form of a coating has been deposited on the pellets. The uncalcined coated pellets are calcined by slowly increasing the temperature to the target temperature and held there for at least about 1 hour. Another method of applying the outer coating is by dip coating. The calcination temperature of the active catalyst layer can range from about 300°C to about 800°C.

[0173] The final step of the core-shell catalytic material of the present invention, which comprises only a support material shell without active catalyst, is to impregnate this layer with active catalytic metal ions. The metal ions of interest are dissolved in a solvent, preferably water but which may be organic. The pellets are immersed in the medium so that the metal ions impregnate the porous layer. After a sufficient time for the desired loading has elapsed, the metal ion-impregnated support material is drained from the solution and dried at 70°C to 120°C (e.g., for 30 to 60 minutes, or sometimes longer). Finally, the coated and impregnated pellets are calcined in air.

[0174] For the intended application of steam reforming, this approach of coating a high thermal conductivity core with a porous outer layer (also called a shell or eggshell) is unique compared to the current practice of methane steam reforming as described above. In some embodiments, the shell has a controllable thickness ranging from about 10 microns to about 200 microns, or from about 50 to about 100 microns. The amount of material required to achieve a 50 micron thickness is about 0.05 grams per gram of catalyst. If a conventional steam reforming catalyst is replaced with the disclosed catalyst and the weight of each pellet of the disclosed catalyst is the same as a typical industrial SMR catalyst (e.g., 2.9 grams), a 50 micron shell on this pellet would utilize about 0.145 grams of material to form the outer shell. Depositing about 12% Ni active metal on an already formed catalyst, or impregnating the shell with a target Ni weight of about 12%, adds about 0.02 grams of Ni per pellet of catalyst. This represents an absolute reduction in Ni metal weight per pellet of about 94%, or in the range of about an 80-95% reduction. If the reaction was not mass or heat transfer limited, a 94% reduction in the absolute amount of catalyst metal would reduce the overall reaction rate or manufacturability. However, because conventional methane reforming pellets are strongly mass and heat transfer limited, only a small portion of Ni (on the order of 10% or less) effectively contributes to the overall reaction rate of conventional reforming catalyst pellets.

[0175] The porosity of the outer layer is also important and has been studied as a design principle. The addition of a porous support element in the slurry results in a layer with improved porosity. The increased porosity is important in the application of the material of the invention in catalysis and also acts to increase reactant diffusion within the coating layer, thereby further enhancing the effective use of the active catalyst contained therein. Additives that lead to improved porosity of the outer layer may include lanthanum carbonate, magnesium carbonate, graphitic carbon, among others. Figure 5 shows a cross-sectional SEM image of a catalyst according to the present disclosure, including an outer layer deposited on a core. The image on the left shows the unmodified outer layer, while the image on the right shows the effect of modifying the composition to increase the porosity of the outer layer.

[0176] Although the amount of active nickel on an absolute basis is reduced in the inventive catalyst pellets of the present disclosure, the effectiveness factor associated with the eggshell coating of the present disclosure is significantly higher than that of conventional methane reforming pellets. With a much higher effectiveness factor, the net activity of the catalyst of the present disclosure will be comparable to that of conventional catalysts, even though the absolute mass of catalytically active material is reduced. In one embodiment, the volumetric activity of a fixed bed reactor comprised of the catalyst of the present invention is within 80% of the activity of a conventional methane reforming catalyst. In an alternative embodiment, the activity of the catalyst of the present invention on a reactor load basis will be comparable to that of a conventional methane reforming catalyst. In a preferred embodiment, the catalyst of the present invention will have a volumetric activity in the range of about 1.0 to 1.3 times the volumetric activity of a conventional methane reforming catalyst.

[0177] The reaction takes place inside the catalyst pellet and is limited by both mass and heat transfer. As an endothermic reaction proceeds inside the pellet, the pellet cools and the net catalytic activity of this thermodynamically limited reaction decreases. The transfer of heat deep inside the cold pellet It is preferred to have the catalyst in the eggshell layer for the methane steam reforming reaction in order to allow for efficient use of the active metal catalyst while at the same time efficiently transporting heat into the catalytic shell coating rather than requiring a catalyst in the eggshell layer.

[0178] A classical effectiveness factor analysis was performed to evaluate the effectiveness of the catalysts according to the present disclosure, where the relationship between effectiveness factor and Thiele number is known in the art. Effectiveness factors for conventional methane steam reforming reactions have been reported to be about 1-10%. That is, more than 90% of the active catalyst metal is ineffective for the desired methane steam reforming reaction in conventional methane reforming pellets.

[0179] The effectiveness factor (ratio of actual or apparent reaction rate to intrinsic reaction rate) of conventional SMR catalysts is low due to mass diffusion limitations and poor internal heat transfer within conventional catalyst pellets. The internal volume of the catalyst pellet cools as the reaction proceeds, further slowing the apparent reaction rate beyond the mass transfer limitations. Adolis reports a commercial effectiveness factor of ~0.008 for methane consumption. Rao also reports an effectiveness factor of 0.1 for a commercial steam methane reformer, where the effectiveness factor is increased due to the use of internal pellet holes and other shape modifications to reduce the internal pellet mass transfer resistance.

[0180] The Thiele number (Φ) is shown in the following Equation 10. The effectiveness factor (ε) is shown in the following Equation 11. [ka] where R represents the radius of the pellet or the diffusion distance for mass transfer within the catalyst coating. The reaction rate constant is k1. The effective diffusion coefficient (D eff ) is the gas diffusion in the porous catalyst divided by the tortuosity factor, which is typically around 3 for most catalytic systems. The analytical expression for the effectiveness factor shown in Equation 11 is for first-order reactions, but the expression has been readily shown in the literature to be robust and reasonably well behaved for zero to second-order rate expressions.

[0181] For a methane reforming reaction operated at about 20 bara and about 850° C., the molecular diffusion coefficient can be calculated using the Chapman-Enskog theory of mass diffusion to be about 0.143 cm for water (steam); 2 / sec, about 0.495 cm for methane 2 / sec. Molecular diffusion collapses when the mean free path of the molecules is within three times the pore diameter for diffusion to occur. The mean free paths of water vapor and methane under reaction conditions are 0.03 and 0.01 microns, respectively. For catalysts with pore sizes less than about 0.1 micron, Knudsen diffusion, rather than molecular diffusion, is considered the predominant mode of mass transfer in the catalyst pores. The Knudsen diffusion coefficient for both reactants is about 0.05 cm 2 / sec, or about 2-3 times slower than molecular diffusion.

[0182] As shown in the SEM photographs of the catalyst and its manufacturing method according to the present disclosure, the voids (i.e., pores) in the catalyst coating layer are larger than about 1 micron, and diffusion occurs easily by molecular mechanisms therein. To consider the effectiveness factor of the catalyst of the present invention, the diffusion coefficient of the slowest reactant (water vapor) was used in molecular diffusion state, which is 0.143 cm. 2 / sec is an estimate.

[0183] Conventional methane reforming catalyst pellets are compressed to form a desired shape, and the reactant zone is considered to be the Knudsen zone. The diffusion coefficient of gas phase reactants through a conventional methane reforming pellet is approximately 0.05 cm 2 / second.

[0184] When adding in the effects of tortuous, i.e., circuitous paths for mass transport through a catalyst bed or pellet for reactants to reach active catalytic sites disposed therein, rather than a straight diffusion path, the actual or effective diffusion coefficient for the catalyst of the present invention is 0.0477 cm 2 / sec, and the effective diffusion coefficient for a commercial SMR catalyst is estimated to be 0.0167 cm 2 / sec.

[0185] By using the selected catalyst coating for the inventive catalyst of this disclosure with engineered larger pores, diffusion of reactants through the thickness of the catalyst occurs primarily with more favorable molecules rather than the slower Knudsen diffusion as seen in conventional methane reforming pellets.

[0186] The value of k1 or the reaction rate constant (sec -1 (unit: 0.01) is approximately 34.3 sec using Hoang's 2005 reaction kinetics. -1 It has been estimated that the effective distance or R of the Thiele number equation is evaluated for the catalysts of the present disclosure and compared to conventional SMR catalysts. Table 10 calculates the effectiveness factor for the catalysts of the present disclosure having coating thicknesses up to about 200 microns. In all cases, the effectiveness factor is very high indicating that the actual reaction rate is very close to the intrinsic reaction rate of methane steam reforming. The effectiveness factor is about 0.98 for a 200 micron coating and about 0.999 for a 50 micron coating thickness. Thus, the effectiveness factor for the catalysts of the present invention is greater than about 0.90 for the methane steam reforming reaction, greater than about 0.95 in a preferred embodiment, and about 0.99 to 0.9999 in a most preferred embodiment. [Table 10]

[0187] Using the same calculation methodology and conditions as for a conventional methane steam reformer, the calculated effectiveness factors are shown in Table 11 over a practical range of catalyst pellet sizes. As suggested in the literature, conventional catalyst effectiveness factors are very low. For a 1 / 2 inch catalyst pellet (no internal holes), the effectiveness factor is about 0.051. For an effective diffusion distance of about 1 / 4 inch, the effectiveness factor for a conventional methane reforming catalyst is about 0.1. Even for very small catalyst pellets, such as those about 1 mm in diameter, the effectiveness factor only rises to about 0.5. These very small pellets, about 1 mm in diameter, exhibit very high pressure drop in the full length reactor and are not commercially considered. [Table 11]

[0188] Thus, the catalysts described herein provide a significantly higher effectiveness factor than conventional methane steam reforming catalysts. The catalysts of the present invention have an effectiveness factor of greater than about 0.9, while commercially available methane reforming catalysts operate at effectiveness factors of less than about 0.1 to about 0.2. That is, the catalysts of the present invention have an effectiveness factor that is 9 to 10 times greater than the effectiveness factor of conventional methane steam reforming pellets. The amount of active nickel (or other metal) sites can be reduced per volume by a similar factor of 9 to 10 in the catalysts of the present invention while maintaining the same or similar volumetric reactor activity as conventional methane steam reforming catalysts.

[0189] Performance-defined core-shell SMR catalysts The industrial production of hydrogen is achieved through steam methane reforming (SMR), a process in which methane, a major component of natural gas, reacts with hot steam in the presence of a catalyst to produce hydrogen and carbon monoxide, which then reacts with steam to produce more hydrogen and carbon dioxide. CH4 + H2O = CO + 3 H2(ΔHr 298K = +206 kJ / mol) (1) CO + H2O = CO2 + H2(ΔHr 298K = -41 kJ / mol) (2) The overall reaction is given below. CH4 + 2 H2O = CO2 + 4 H2(ΔHr 298K = +165 kJ / mol) (3) This reaction is catalyzed by certain catalysts. In the absence of a catalyst, the reaction requires very high temperatures. Methane steam reforming is catalyzed by metals such as nickel (Ni), cobalt (Co), ruthenium (Ru), rhodium (Rh), palladium (Pd), iridium (Ir), and platinum (Pt). Ni is the most widely used catalyst for SMR.

[0190] An embodiment of the catalyst core of the present disclosure includes a high thermal conductivity composite of SiC / Al2O3. These materials are mixed, pressed into pellets, and optionally coated in a subsequent step, then calcined in an oxygen environment (e.g., ambient air). The resulting material, which has been confirmed to have high thermal properties, is then impregnated with SMR active metal ions or coated with an active metal-containing slurry and calcined. The impregnated metal or coated catalyst slurries are cited from the SMR active metals above. These metals are supported on a variety of supports drawn from the following non-exclusive list: aluminum-silicon, zirconia-ceria doped alumina, alumina, zirconia doped ceria, alumina-silica mixtures, gamma alumina, alpha alumina, magnesium promoted alumina, calcium promoted alumina, sodium promoted zirconium oxide-cerium oxide, cerium oxide, titania promoted silica, among others.

[0191] The coated catalyst operates at a high effectiveness factor, for example greater than 0.9, but Meanwhile, conventional modified pellets operate at low effectiveness factors, typically less than about 0.2, and in some embodiments from about 0.05 to about 0.1. The net activity of the coated catalyst with reduced net mass of nickel remains similar to conventional pellets with nickel dispersed throughout, due to the much higher effectiveness factor of the support material of the present invention.

[0192] SMR is an endothermic equilibrium controlled reaction that expands in volume with increasing moles as the reaction proceeds. This means that the temperature needs to be increased, especially as pressure increases, for the reaction to proceed to a level of meaningful hydrogen production. Figure 16 shows that as temperature increases, conversion increases in a monotonically increasing function. Conversion decreases as pressure increases. Industrial reactors operate at temperatures between 850°C and 950°C and pressures between 20 and 40 bara. High pressure conditions are necessary to meet downstream processing requirements, such as avoiding costly and risky hydrogen compression while at the same time achieving high conversion to overcome equilibrium constraints. To keep methane conversion above 80%, the average catalyst bed temperature needs to be kept high (above about 850°C at about 20 bar). Also, due to the equilibrium nature of SMR, comparisons of catalyst performance versus activity are meaningfully made at 1 bara and low temperatures, where reaction rate plays a larger role than at high pressures and temperatures.

[0193] The catalytic performance of the inventive catalyst support material of the present disclosure, with the SMR catalyst deposited as an outer coating (i.e., shell) around a SiC core, was experimentally evaluated in both laboratory and pilot plant scale reaction tests. In the laboratory, the reaction was carried out by loading a specific amount of pellets into a hot ½ inch Inconel Ni alloy tube. Heat was provided in the laboratory using an electrically heated furnace. The reaction conditions for the laboratory scale tests are shown in Table 12. The temperatures recorded are the tube surface temperatures outside the catalyst bed. Prior to entering the reactor, the methane is contacted with vaporized water vapor in a vaporization chamber maintained at 500°C. [Table 12]

[0194] The catalyst coated pellets are weighed and loaded into a 1 inch nickel-Inconel tube reactor supported on inert alumina media at both ends. The inlet side of the reactant contains substantially more inert material than the outlet side. The reactor is placed in an electrically heated furnace. A flow of reducing gas (hydrogen or a mixture of hydrogen and nitrogen) is introduced into the reactor and heated at 3°C / min to 650°C where the reduction is carried out for a minimum of 2 hours. The reaction is initiated by flowing a flow of 100 sccm pure hydrogen followed by water. The water passes through the heating zone and vaporizes to steam. After another 15 minutes, methane is introduced and after another 15 minutes the hydrogen is removed. The steam to methane content is controlled at 3 and the progress of the reaction is monitored using gas chromatography (GC) throughout the temperature range of 650°C to 850°C. At 850°C, the catalyst life performance is monitored by periodic sampling using GC. 100% conversion of methane is achieved when no methane signal can be detected by GC, but when the methane signal is recorded at 1% by a calibrated GC, there is a 1% drop due to loss of activity. Even this can be realized.

[0195] The catalysts tested were prepared by coating the SMR catalyst onto the inventive high thermal conductivity cores of this disclosure. Similarly, a porous support material was coated onto the inventive catalyst cores, and then the SMR active metals were impregnated onto the porous support layer. For example, catalyst A was prepared by spraying 0.21 g of a catalyst containing 1.5% precious metals supported on a ceria-zirconia support onto 10 grams of the disclosed catalyst support. In this study, 10.2 grams of catalyst A (or about 7.5 cm 3 Catalyst B contained 0.8 grams of outer layer deposited on 20 grams of disclosed core, which was converted to 0.46 grams of Ni metal, corresponding to 36.5% Ni in the outer layer. 2+ It was prepared by infiltrating Mg ions. 2+ ions (equivalent to 0.05 grams of MgO) were added to this outer layer. In this example, 17.3 grams of catalyst B (or approximately 15 cm 3) was loaded into the reactor. These catalysts had coating thicknesses ranging anywhere from 25 to 100 μm.

[0196] Figure 17 shows the graphical results of low pressure testing of the above catalysts. All of these catalysts show equilibrium conversion at the temperatures and conditions tested. For example, the equilibrium performance is 3000 to 9000 hr -1 These catalysts were tested at various space velocities as shown in FIG.

[0197] Industrially, commercial hydrogen production by SMR takes approximately 2,000 to 3,000 hours. -1 The lifetime activity of some of these materials has been evaluated for a period of 600 hours without evidence of degradation, carbon formation, pressure rise, or metal dust. The catalyst lifetimes are shown in FIG. 19. These results demonstrate that catalysts supported on the catalyst support materials of the present invention are capable of supporting an outer layer of reforming catalyst, either deposited as a catalyst slurry or impregnated into a pre-deposited porous coating, and maintaining high activity for at least 600 hours.

[0198] As shown in FIG. 18, catalyst A (1.5% PGM-coated catalyst) was subjected to 650° C., 1 bara, 3:1 steam:carbon, and 3,000 hr -1 GHSV and 1.5hr -1 The results show that the catalyst B (1.5% PGM impregnated catalyst) approaches equilibrium at a WHSV of 3,000 hr. -1 GHSV and 0.1hr -1 It is shown that the equilibrium is approached by 92% at a WHSV of .

[0199] Catalyst A (1.5% PGM catalyst) is 9000hr -1 GHSV and 1,787,000hr -1 WHSV of 850° C. as well as a temperature of 850° C., which approach equilibrium by more than 95%, whereas catalyst B under the same conditions approaches equilibrium by more than 90%.

[0200] The disclosed SiC-based catalyst support cores provide: (1) lower OPEX reactor costs and (2) higher manufacturability. SMR is the main route for industrial hydrogen production and is an equilibrium-controlled, highly endothermic reaction. Industrially, SMR reactors are operated at high temperature (850-950° C.) and pressure conditions (20-40 bar). The high operating pressure is usually a result of pressure requirements from downstream processes, and high temperatures are required to overcome thermodynamic limitations and achieve high methane conversion (>70%).

[0201] The SMR reaction is typically carried out over a catalyst arranged as a bed of tightly packed or otherwise loose particles in a fixed-bed tubular reactor, which is placed inside a reactor box. The tubes are arranged in an array at a fixed distance from each other, with natural gas burners interspersed between them to provide heat. The heat from the burners (temperatures of over 1100°C) is passed through the reactor tube walls and the fixed bed to the catalyst chamber where endothermic reforming of methane with steam takes place. The heat generated by the endothermic reaction is radiated to the surface of the reactor. The endothermic nature of the reaction means that the temperature of the catalyst surface continually decreases, which can lead to cold spots. The drop in heat as a result of the endothermic reaction is countered by an increase in heat flux from the reactor walls. The increased heat flux increases the energy demand of the burner. The effect of this increased availability is increased natural gas usage and operating costs.

[0202] The catalyst of the present disclosure is shown to have enhanced heat transfer properties compared to current SMR catalysts (see FIG. 20). Table 13 shows a performance comparison at 20 bara feed pressure for a packed bed of the present disclosure showing the effect of effective thermal conductivity and wall temperature of a conventional packed bed. When the thermal conductivity of the presently disclosed inventive catalyst and commercial SMR catalyst materials are used in a reactor performance prediction model (as previously described herein), the results show an increase in the thermal conductivity of the inventive material leading to a reduction in tube wall temperature by up to 30° C., with a representative case of a 13° C. reduction for similar methane conversion / hydrogen yields, compared to the commercial catalyst. This phenomenon (purely due to increased thermal conductivity) has several advantages, two of which are: [Table 13]

[0203] First, if the tube wall temperature is not decreased but maintained at a set constant temperature, the catalyst support material of the present invention results in a higher outlet temperature and a higher methane conversion / hydrogen yield. This improved performance is the margin to increase the feed flow rate without decreasing the baseline conversion (conversion of a commercial catalyst at similar conditions). The increased feed flow rate leads to improved manufacturability, which is attractive for hydrogen producers with limited plant capacity.

[0204] Second, the increase in reactor tube exit temperature as a result of the use of the material of the present invention suggests that the reactor tube wall temperature can be reduced by a similar margin and still maintain the original heat flux across the reactor tube without losing methane conversion. The 30°C tube wall temperature reduction is the result of a 125°C reduction in the natural gas burner temperature. Burning at a lower burner temperature has the effect of consuming less natural gas, thus reducing the operating expenses (OPEX) associated with natural gas burner fuel. The burner temperature is reduced by 30°C to 1100°C.

[0205] The main advantages of the catalyst according to the present disclosure are summarized based on the detailed description herein.

[0206] Tube wall metal temperature reduction of 5-30°C at comparable GHSV, temperature, pressure, and feed composition compared to commercial SMR catalyst

[0207] Increased feed rate at equal conversion compared to a commercial SMR catalyst at equal temperature, pressure, and feed composition. 1-30% increase in feed flow rate and corresponding hydrogen production

[0208] The lower operating costs of hydrogen production are due to the lower tube wall temperatures. As reported by Zolotek, a 30-50°F (16-28°C) reduction in tube wall temperature results in a fuel savings of 1.5-2.5 BTU / scf, which translates to annual OPEX savings of $200,000-$350,000 for a 100 million SCFD reformer. The catalysts of the present disclosure will reduce SMR OPEX by at least 2.5 BTU / scf and in the range of 1 to about 3 BTU / scf when compared to conventional methane reforming catalysts in similar plant designs.

[0209] The reduced tube wall temperature of 30°C used in combination with conformal catalyst loading, as enabled by the catalyst of the present disclosure, facilitates catalyst integration within existing reactor tubes or existing tube and plant designs. This technology is different from structured catalysts, which are difficult to integrate into existing plant tube and reactor designs. In 2015, Kumar et al. reported that a 20°C reduction in tube wall temperature increases tube life by 50%. They also reported that a 1% reduction in the energy cost portion of plant OPEX would result in annual savings of $600,000 for a 100 million SCFD hydrogen plant. A 30°C reduction in tube wall temperature reduces the energy cost of hydrogen production by about 0.25 to about 1%.

[0210] In 2003, Rostrup-Nielsen and Sehestedt reported that without steam export, the energy consumption for hydrogen production from SMR is 300 BTU / scf. The reduction in tube wall temperature thereby reduces OPEX by up to about 1% or in the range of about 0.1 to about 1% for hydrogen production from methane reforming using the disclosed catalyst. The overall thermal efficiency of the methane reforming plant, including waste heat recovery, is about 95%. The reduction in operating costs of about 1% is significant for hydrogen production, and represents an additional savings in addition to the reduction in costs for tube replacement and associated plant downtime during tube turnaround, e.g., maintenance and tube replacement cycles.

[0211] As described in the John Zink Combustion Handbook, SMR tubes operating at high temperatures and pressures are in the creep region and approaching the mechanical limits of their material properties. Tube failure can cause safety hazards or plant fires and can also result in reduced uptime. The catalysts of the present disclosure allow for lower wall temperatures and therefore operate at tube wall operating temperatures that are farther away from the mechanical limits of performance to reduce tube cracks, bursts, and plant shutdowns. The catalysts of the present disclosure can extend tube life by 3 to 12 months and allow plants to operate safely with fewer tube bursts and plant fires.

[0212] Enhancement of effective packed bed conductivity with SiC-containing catalysts and catalyst cores through changes in solids loading, thermal conductivity, and emissivity. As previously described herein, the catalysts and catalyst cores (i.e., catalyst supports) of the present disclosure are comprised of high thermal conductivity SiC / Al2O3 composites that provide improved heat transfer in packed beds. Additionally, these catalysts and catalyst cores provide higher total normal emissivity compared to conventional commercial catalysts, and therefore improved heat transfer in packed beds when operating in high temperature environments. Improved effective packed bed thermal conductivity due to the conductivity and emissivity of the catalysts and catalyst cores is achieved even while maintaining a similar geometry and bed packing density as conventional catalysts.

[0213] The effective bed thermal conductivity was experimentally determined using the experimental procedures and apparatus previously described herein. As previously described, the expected reactor tube wall temperatures when using the catalyst system of the present disclosure are approximately 100% lower than those required when using conventional methane reforming catalysts while providing comparable hydrogen production rates. The wall temperature can be reduced by 10 to 30°C compared to the conventional method.

[0214] One basis for calculating the effective packed-bed thermal conductivity from the individual geometric and bed properties is the ZBS (Zener, Bauer, and Schröder) model. The ZBS model includes a representative cylindrical unit cell consisting of catalyst pellets and fluid media, and considers the geometric interactions between other pellets and solid / fluid domains. The model adjusts the effective conductivity based on the fluid and pellet solid conductivities, pellet solid emissivity, packed bed porosity (i.e., void fraction) (geometric effect), shape corrections, deformation parameters, pressure, and gas dynamics, which vary based on the mean free path of the gas molecules.

[0215] In the previous examples herein, the effect of increasing the thermal conductivity of the pellets was investigated alone. At low temperatures, the effect of radiative heat transfer is minimal or negligible. However, at temperatures utilized during steam methane reforming and other catalytic reactions, radiative heat transfer is the dominant means. Radiation plays a major role since it scales with the cube of temperature. The ZBS model can resolve the effects of emissivity and conductivity.

[0216] Using the measured and calculated parameters, the effective packed bed thermal conductivity was determined for various ranges of total normal emissivity and pellet thermal conductivity. A fixed packed bed geometry was used that corresponds to the experimental measurements discussed in the above example entitled "Reduced Wall Temperature and Increased Hydrogen Production for Steam Methane Reforming Using the Catalyst of the Invention". The packed bed model was maintained at a fixed temperature of 800°C and ambient pressure with a bed porosity of 0.40 in nitrogen gas.

[0217] The effect of total normal emissivity varies exponentially with low pellet thermal conductivity and linearly with high pellet conductivity. For reference, measured and calculated parameters for the catalyst core of the present disclosure and a commercial catalyst are provided. The novel core of the present disclosure achieves its enhanced effective packed bed thermal conductivity through its improved pellet thermal conductivity as well as its increased total normal emissivity. However, an increase in either parameter both increases the overall effective conductivity.

[0218] In one embodiment of the catalyst of the present disclosure, a SiC-based core (e.g., SiC in a protective alumina matrix) is coated with a thin translucent coating of porous alumina to increase the emissivity of the catalyst produced therefrom. The total normal emissivity of SiC at high temperatures is very high, but can be increased with the use of other types of coatings, dopants, or base metals. These base metals are usually lightly to heavily oxidized and include, but are not limited to, iron, steel, stainless steel, nickel, titanium, nichrome, and the like. SiC is not the only ceramic that can be used to increase emissivity. Other ceramics include carbide coatings, iron oxide, silicon nitride, zirconia, MgO, ZrC, and the like. Additionally, high emissivity glasses can be used. BSAS can also be used to increase the emissivity of the support while simultaneously protecting the core SiC material from its environment (as described further herein). Other glass, base, or ceramic coatings may be used, such as aluminum silicate, borosilicate, Vycor, Pyrex, various carbide materials, CaO stabilized with Zr / Fe / Cr oxides, carbon random, and unstabilized zirconia.

[0219] Thus, by increasing the thermal conductivity of the catalyst by using a high thermal conductivity and high total normal emissivity material in place of a conventional catalyst (i.e., replacing a porous Ni-Al2O3 composite catalyst with one containing a catalyst coating on a dense core containing SiC), the heat transfer capacity of the bed is improved by about 5 times under stagnant conditions and a constant offset of about 1.5 to 3.5 is achieved at expected system flows of 2000 to 5000 GHSV (see Figures 10 and 11), representative of methane reforming reactions at high temperatures, due to the effects of heat dispersion and turbulent conduction of pressure. This can be improved by improving the model.

[0220] Increasing the effective radial thermal conductivity transfers heat more efficiently from the hot reactor tube walls to the catalyst bed and reactant gases, thereby driving the endothermic reactions more efficiently. Although the heat required to complete the reaction remains unchanged, heat losses are reduced due to lower peak temperatures, allowing for reduced energy input in the form of fuel and oxygen (or air) feed rates.

[0221] The temperature gradient between the tube walls and the center of the catalyst particle bed is reduced, thereby allowing for lower tube wall temperatures to produce equivalent amounts of hydrogen. Alternatively, the tube walls can be maintained at the same temperature with similar tube life as conventional catalysts, while increasing hydrogen throughput or manufacturability in the range of 5-30% compared to conventional catalysts. Tube life can be significantly improved and tubes with thinner walls, cheaper alloys, or more conventional manufacturing processes can be used, all achieving significant capital cost reductions for the system.

[0222] Various embodiments of the catalytic cores (i.e., catalytic supports) and catalysts according to the present disclosure have been described in detail above, as have the various types and classes of reactions for which the catalysts of the present disclosure can be used. However, it is understood that the components, features and configurations, as well as the methods of making and using the catalytic cores and catalysts, are not limited to the specific embodiments described herein.

[0223] By way of example, any of the various catalytic cores and catalysts using the cores described herein may be used in the preparation of a wide variety of catalytic reactions, including acetylation, addition reactions, alkylation, dealkylation, hydrodealkylation, reductive alkylation, amination, aromatization, arylation, autothermal reforming, carbonylation, decarbonylation, reductive carbonylation, carboxylation, reductive carboxylation, reductive coupling, condensation, cracking, hydrocracking, cyclization, cyclo-oligomerization, dehalogenation, dimerization, epoxidation, esterification, Fischer-Tropsch reactions, halogenation, hydrohalogenation, homologation, hydration, dehydration, hydrogen ... The catalytic reactions and processes may be used in any of a wide variety of catalytic reactions and processes, including, but not limited to, dehydrogenation, hydrocarbonylation, hydroformylation, hydrocracking, hydrometallation, hydrosilation, hydrotreatment, hydrodesulfurization / hydrodenitrogenation (HDS / HDN), isomerization, methanation, methanol synthesis, methylation, demethylation, metathesis, nitration, oxidation, partial oxidation, polymerization, reduction, steam and carbon dioxide reforming, sulfonation, telomerization, transesterification, trimerization, water gas shift (WGS), and reverse water gas shift (RWGS).

Claims

1. a) a core comprising a composite of SiC particles and a protective matrix of one or more metal oxides in the voids between the SiC particles, the protective matrix binding the SiC particles together, the core having a density of 60% or greater than theoretical density; and b) a catalytically active layer attached to said core; Including, wherein the one or more metal oxides are selected from the group consisting of alumina, titania and silica. catalyst.

2. The protective matrix is ​​Al 2 O 3 The catalyst of claim 1 , comprising:

3. The protective matrix is (a) Silica, mixed oxides of aluminum and silicon, and Al 6 S 2 O 13 or one or more further metal oxides selected from the group consisting of (b) one or more additional metal oxides selected from the group consisting of titania and mixed oxides of aluminum and titanium. The catalyst of claim 2 further comprising:

4. 4. The catalyst of claim 1, wherein the volume ratio of metal in the metal oxide protective matrix to SiC in the core is from 0.05 to 0.50, from 0.05 to 0.30, or from 0.10 to 0.

25.

5. 5. The catalyst of claim 4, wherein the volume ratio of aluminum to SiC in the core is from 0.05 to 0.50, from 0.05 to 0.30, or from 0.10 to 0.

25.

6. The core has a density of 60% to 95%, 60% to 90%, 65% to 90%, or 6. The catalyst of any one of claims 1 to 5, having a density of 65% to 80%.

7. 7. The catalyst according to any one of claims 1 to 6, wherein the catalytically active layer comprises one or more catalytically active metals.

8. 8. The catalyst of claim 7, wherein the one or more catalytically active metals are selected from the group consisting of Ni, Co, Ru, Rh, Pd, Ir, Pt, Os, Re, Au, Ag, Cu, Fe, Mn, Mg, V, Mo and Cr.

9. 7. The catalyst of claim 1, wherein the catalytically active layer comprises a porous coating overlying a core and catalytically active material disposed on inner and outer surfaces of the porous coating.

10. 9. The catalyst of claim 7 or claim 8, wherein the catalytically active layer further comprises a porous coating overlying the core, wherein the one or more catalytically active metals are disposed on the inner and outer surfaces of the porous coating.

11. 11. The catalyst of claim 9 or claim 10, wherein the porous coating comprises a porous oxide shell surrounding a core.

12. 11. The catalyst of claim 9 or claim 10, wherein the porous coating comprises a porous alumina shell.

13. The catalyst of claim 1 further comprising an interfacial layer disposed between said core and said catalytically active layer.

14. 14. The catalyst of claim 13, wherein the interfacial layer comprises a dense coating over the core, wherein the interfacial layer has a density of 80% to 100%, 90% or more, or 95% or more of theoretical density, and further wherein the interfacial layer comprises alumina, alpha-alumina, silica, titania, or barium strontium aluminosilicate ("BSAS").

15. 15. The catalyst of claim 1, further comprising an interfacial layer disposed between the core and the catalytically active layer, the interfacial layer comprising a high density alumina coating over the core, wherein the interfacial layer has a density of 70% to 90%, 80% to 100%, 90% or more, or 95% or more of theoretical density.

16. 16. The catalyst of any one of claims 13 to 15, further comprising a gas impermeable protective coating disposed between the catalytically active layer and the core or between the catalytically active layer and the interfacial layer.

17. The gas impermeable protective coating may be made of alkaline earth aluminosilicate glass, alkaline earth aluminoborosilicate glass, lanthanide aluminosilicate glass, CaO-SiO 2 -Al 2 O 3 ("CAS"), MgO-SiO 2 -Al 2 O 3 ("MAS"), SrO-SiO 2 -Al 2 O 3 , BaO-SiO 2 -Al 2 O 3 , mixed alkaline earth aluminosilicate, rare earth doped alkaline earth aluminosilicate 、 B 2 O 3 Modified alkaline earth aluminosilicate and / or TiO 2 Al in combination with at least one glass former selected from the group consisting of modified alkaline earth aluminosilicates 2 O 3 The catalyst of claim 16 comprising:

18. A protective matrix of one or more metal oxides in the voids between the SiC particles. The present invention relates to a composite core having a density of 60% or more of theoretical density, and a porous coating covering the core, wherein the protective matrix is ​​Al. 2 O 3 A catalyst support comprising:

19. 20. The catalyst support of claim 18, wherein said one or more metal oxides are selected from the group consisting of alumina, titania, and silica.

20. The catalyst support of claim 18 further comprising an interfacial layer disposed between said core and said porous coating.

21. The catalyst support of claim 20 further comprising a gas impermeable protective coating disposed between said porous coating and said interfacial layer.

22. 1. A method for making a catalytic core comprising a composite of SiC particles and a protective matrix of one or more metal oxides in the voids between the SiC particles, comprising: (a) combining SiC powder and one or more metal powders to form a mixture; (b) forming the mixture into a predetermined shape under compression, wherein the compression applies sufficient pressure to the mixture to provide a density in the green state that is 60% or greater than theoretical density, thereby causing plastic deformation of the metal powder such that the metal flows around the SiC particles; and (c) heating the predetermined shape in an oxygen-containing atmosphere such that at least a portion of the metal is converted to the corresponding metal oxide, thereby forming a metal oxide protective barrier around the SiC particles that binds the SiC particles together; Including, A method according to claim 1, wherein the catalyst core has a density of 60% or more of theoretical density, and the one or more metal powders comprise Al and / or Al-Si alloys.

23. 23. The method of claim 22, wherein in step (a) the SiC powder is combined with an Al-Si alloy containing up to 25% Si in the alloy, 5% to 20% Si in the alloy, 10% to 15% Si in the alloy, or 11% to 13% Si in the alloy.

24. (a) CO and H from the raw material 2 generating a synthesis gas comprising (b) supplying synthesis gas to a fixed bed reactor having a reactor volume comprising a catalyst according to any one of claims 1 to 17, wherein the catalytically active bed comprises one or more catalytically active metals suitable for Fischer-Tropsch synthesis; and (c) reacting the synthesis gas in a fixed bed reactor over a catalyst to produce a hydrocarbon product mixture.

1. A method for carrying out a Fischer-Tropsch synthesis of hydrocarbons, comprising:

25. (a) feeding methane and steam into a plurality of fixed bed reactor tubes filled with the catalyst of any one of claims 1 to 17, wherein the catalytically active layer comprises one or more catalytically active metals suitable for steam methane reforming; and (c) reacting methane and steam in said reactor tubes over a catalyst to produce hydrogen.

26. (a) feeding one or more reactants into a reactor containing the catalyst of any one of claims 1 to 17, wherein the catalytically active layer comprises one or more catalytically active metals suitable for catalyzing a reaction; and (b) reacting one or more reactants in a reactor over the catalyst to produce a product; A method for carrying out a catalytic reaction comprising:

Citation Information

Patent Citations

  • Silicon carbide supported catalyst for partial oxidation of natural gas to syngas

    JP2006517176A

  • Hydrogen manufacturing apparatus and hydrogen manufacturing method

    JP2015020929A

  • Catalyst supports made from silicon carbide covered with tio2 for fischer-tropsch synthesis

    US20150191401A1

  • Supported rhodium-lanthanide based catalysts and process for producing synthesis gas

    WO2002098557A1

  • Honeycomb structure, method for production thereof and exhaust gas purification device

    WO2006025498A1