Copolymer powder having polyamide and polyether blocks
The PEBA powder composition with controlled polyamide to polyether ratios and flow agent content, along with optimized milling, addresses the challenges of agglomeration and energy consumption, resulting in flexible and recyclable three-dimensional articles with enhanced mechanical properties.
Patent Information
- Application Number
- JP2021568100
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-05-16
- Filing Date
- 2020-05-15
- Publication Date
- 2024-10-09
- Estimated Expiration
- 2040-05-15
AI Technical Summary
Existing PEBA powders for three-dimensional article fabrication face challenges in achieving good mechanical properties, flexibility, and recyclability due to agglomeration and the need for high energy consumption, especially when using flow agents in excess.
A PEBA powder composition with a polyamide block to polyether block weight ratio of 0.7 or less, polyamide block molar mass of 1000 g/mol or less, and a flow agent content of 0.3% to 2% by weight, combined with specific milling and sieving processes, to enhance flowability and maintain mechanical properties.
The solution enables the production of three-dimensional articles with improved flexibility, high elongation at break, and impact strength, while allowing for efficient recycling and reduced energy consumption during the sintering process.
Smart Images

Figure 0007564827000001 
Figure 0007564827000002 
Figure 0007564827000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a powder composition of a copolymer comprising polyamide blocks and comprising polyether blocks, and to a method for its preparation.The invention also relates to the use of this powder and to the articles manufactured from said powder. [Background technology]
[0002] Copolymers containing polyamide blocks and containing polyether blocks, or "polyether block amides" (PEBA), are plasticizer-free thermoplastic elastomers belonging to the family of engineering polymers. They can be easily processed by injection molding and extrusion of profiles or films. They can also be used in the form of filaments, threads and fibers for woven and nonwoven fabrics. They are used in the sports field, in particular as components of sports footwear soles or golf balls, in the medical field, in particular for catheters, angioplasty balloons, peristaltic belts, or in automobiles, in particular as components of synthetic leather, leather, dashboards, airbags.
[0003] PEBAs, sold under the name Pebax® by Arkema, make it possible to combine in one and the same polymer unparalleled mechanical properties with low density in addition to very good resistance to thermal or UV aging. They therefore allow the manufacture of lightweight and flexible parts. In particular, at comparable hardness, they dissipate less energy than other materials, which gives them very good resistance to bending or tensile dynamic stresses and they show very good elastic recovery properties.
[0004] These polymers can also be used in the field of the shaping of three-dimensional articles by sintering. According to this process, a layer of polymer powder is selectively and briefly irradiated in a chamber with electromagnetic radiation (e.g. laser beam, infrared radiation, UV radiation), as a result of which the powder particles affected by the radiation melt. The molten particles rapidly fuse and solidify to form a solid mass. This process allows simple and rapid production of three-dimensional articles by repeatedly irradiating successive newly applied layers of powder. This technique is generally used to produce prototypes, models of parts ("rapid prototyping") or to produce finished parts in small series ("rapid manufacturing"), for example in the automotive, marine, aviation or aerospace sectors, in the medical sector (prostheses, hearing systems, tissues), textiles, clothing and fashion, decoration, housings for electronics, telephones, home automation, computers, lighting.
[0005] The layer-by-layer sintering process requires a prior conversion of the PEBA into a powder form, which must be suitable for use in the sintering equipment and allow the production of flexible parts with satisfactory mechanical properties.
[0006] The quality of the parts produced and also their mechanical properties depend on the properties of the PEBA powder. For example, powder agglomeration must be avoided, since it results in the production of three-dimensional objects with low definition. In addition, the powder must be conveyed to form a uniform bed without forming agglomerates or deposits or cracks, otherwise it cannot be converted correctly. The addition of additives such as flow agents can improve the flow properties to a certain extent. However, if a large amount of flow agents is used, a large amount of energy is required for the fusion of the powder, which makes it impossible to obtain parts with both good definition and good mechanical properties. In particular, they can reduce the breaking elongation of the material.
[0007] French Patent No. 2955330 relates to a thermoplastic powder composition having a D50 of less than 100 μm, comprising at least one block copolymer having a melting point of less than 180 ° C, 15% to 50% by weight of at least one powder filler having a Mohs hardness of less than 6 and a D50 of less than 20 μm, and 0.1% to 5% by weight of a powder flow agent having a D50 of less than 20 μm. This document relates in particular to the use of said composition for manufacturing flexible three-dimensional objects. The use of powder fillers facilitates the grinding and thus makes it possible to obtain the desired particle size. However, the presence of a high content of fillers in the manufactured parts has a negative effect on their mechanical properties.
[0008] EP 0 968 080 A1 relates to a thermoplastic powder comprising a mixture of a powdered flow agent and a powdered block copolymer thermoplastic resin having a glass transition temperature not exceeding 50° C. This powder can be used for the manufacture of flexible three-dimensional objects.
[0009] EP 1 845 129 A1 relates to a method for producing shaped articles from polymer powders by layer-by-layer sintering of the powder, the powder comprising at least one polyetheramide block prepared from an oligoamide-dicarboxylic acid and a polyetherdiamine.
[0010] Nevertheless, there remains a real need to provide PEBA powder compositions that allow the shaping of three-dimensional articles by sintering in an efficient manner, and in particular that allow working with a wider working window and at relatively low building temperatures, said articles being characterized by good mechanical properties, such as good flexibility. There is also a need to provide PEBA powder compositions that have good recyclability. Summary of the Invention
[0011] The present invention relates first to a composition comprising a powder of a copolymer comprising polyamide blocks and comprising polyether blocks, the copolymer being in the form of particles with a powder filler content of 0% to 10% by weight, the weight ratio of the polyamide blocks to the polyether blocks of the copolymer being less than or equal to 0.7, the number average molar mass of the polyamide blocks being less than or equal to 1000 g / mol, and the composition comprising a flow agent in a content of more than or equal to 0.3% by weight.
[0012] According to one particular embodiment, the polyamide blocks have a number average molar mass less than or equal to 900 g / mol.
[0013] According to one particular embodiment, the weight ratio of polyamide blocks to polyether blocks is less than or equal to 0.65.
[0014] According to a particular embodiment, the flow agent is present in a content of less than or equal to 2% by weight.
[0015] According to certain embodiments, the flow agent is selected from silica, in particular hydrated silica, pyrogenic silica, vitreous silica, or fumed silica; alumina, in particular amorphous alumina; glassy phosphates, glassy borates, glassy oxides, titanium dioxide, calcium silicate, magnesium silicate, talc, mica, kaolin, attapulgite, and mixtures thereof.
[0016] According to a particular embodiment, the particles of the powder have a size Dv10 greater than or equal to 30 μm, preferably greater than or equal to 35 μm.
[0017] According to a particular embodiment, the particles of the powder have a size Dv90 less than or equal to 250 μm, preferably less than or equal to 200 μm.
[0018] According to a particular embodiment, the particles of the powder have a size Dv50 of 80 to 150 μm, preferably 90 to 120 μm.
[0019] The sizes Dv10, Dv50 and Dv90 are measured, for example, by laser diffraction on a Malvern diffractometer by the dry route and by modelling the distribution of the particles according to ISO 9276, in accordance with ISO 13320:2009.
[0020] According to a particular embodiment, the copolymer exhibits an instantaneous hardness of 20 to 75 Shore D, preferably 25 to 45 Shore D, measured according to ISO868:2003.
[0021] According to a particular embodiment, the polyamide block of the copolymer is a block of polyamide 11, or a block of polyamide 12, or a block of polyamide 6, or a block of polyamide 10.10, or a block of polyamide 10.12, or a block of polyamide 6.10, and / or the polyether block of the copolymer is a block of polyethylene glycol, a block of polypropylene glycol, or a block of polytetrahydrofuran.
[0022] According to a particular embodiment, the polyamide block of the copolymer is a block of polyamide 11 or a block of polyamide 12 or a block of polyamide 1010 or a block of polyamide 1012, and / or the polyether block of the copolymer is a block of polyethylene glycol, a block of polypropylene glycol or a block of polytetrahydrofuran.
[0023] According to a particular embodiment, the polyether blocks have a number average molar mass between 400 and 3000 g / mol, preferably between 800 and 2200 g / mol.
[0024] The present invention also provides a method for preparing the above composition, comprising the steps of: Providing a copolymer including polyamide blocks and including polyether blocks and grinding the copolymer; and contacting the copolymer with a flow agent; The present invention relates to an adjustment method including the steps of:
[0025] According to a particular embodiment, the copolymer is contacted with a flow agent prior to grinding.
[0026] According to a particular embodiment, the grinding is cryogenic grinding.
[0027] According to one particular embodiment, the copolymer is provided in the form of granules.
[0028] According to a particular embodiment, the particles resulting from the grinding are sieved and the sieve oversize is recycled to the grinding.
[0029] The invention also relates to the use of said composition for layer-by-layer fabrication of three-dimensional articles by electromagnetic radiation induced sintering.
[0030] The present invention also relates to three-dimensional articles produced from the above compositions, preferably by layer-by-layer fabrication by electromagnetic radiation induced sintering.
[0031] The present invention makes it possible to meet the above-mentioned needs. More particularly, it provides a PEBA powder composition that allows the shaping of three-dimensional articles by sintering in an efficient manner, in particular allowing to work with a wider working window and at relatively low shaping temperatures, said articles being characterized by good mechanical properties, such as good flexibility. The composition according to the invention furthermore exhibits good recyclability.
[0032] A powder filler content of 0% to 10% by weight in the PEBA particles allows to obtain three-dimensional articles with good mechanical properties, in particular high elongation at break. Furthermore, a powder filler content of 10% by weight or less allows to obtain three-dimensional articles with good impact strength. This is because the presence of powder fillers in the PEBA particles at a content of more than 10% by weight can lead to brittle three-dimensional articles, which can result in reduced impact strength.
[0033] In addition, a weight ratio of polyamide blocks to polyether blocks of less than or equal to 0.7 also makes it possible to obtain three-dimensional articles with the desired flexibility, and thus the three-dimensional articles produced from the composition according to the invention exhibit a relatively low modulus of elasticity.
[0034] The presence of the flow agent in an amount equal to or greater than 0.3% by weight makes it possible to further improve the flowability of the powder and its recyclability, while maintaining good mechanical properties of the three-dimensional article.
[0035] Finally, the fact that the polyamide blocks have a number-average molar mass of less than or equal to 1000 g / mol makes it possible to carry out the shaping process at relatively low working temperatures and to have a wide working window, in other words, it makes it possible to obtain powder compositions in which the PEBA copolymer has a relatively low melting point, well away from the crystallization temperature, and which then allows working with a wide range of shaping temperature values.
[0036] Furthermore, the fact that the PEBA copolymer is preferably contacted with a flow agent prior to the grinding step makes it possible to improve not only the efficiency (or yield) of grinding, but also the recycling of the polymer / flow agent mixture so as to increase the efficiency of the powder preparation process. More specifically, the better flowability of this mixture allows sieving to be performed so as to recycle the coarsest particles to the mill. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0037] The invention will now be explained in more detail, in a non-limiting manner, in the following description.
[0038] Copolymer The present invention uses copolymers containing polyamide (PA) blocks and containing polyether (PE) blocks, or "PEBA" copolymers.
[0039] PEBA is produced by the polycondensation of polyamide blocks containing reactive end groups with polyether blocks containing reactive end groups, inter alia: 1) polycondensation of a polyamide block containing a diamine chain end with a polyoxyalkylene block containing a dicarboxyl chain end; 2) polycondensation of polyamide blocks containing dicarboxyl chain ends with polyoxyalkylene blocks containing diamine chain ends, obtainable, for example, by cyanoethylation and hydrogenation of aliphatic α,ω-dihydroxylated polyoxyalkylene blocks known as polyether diols; 3) The product resulting from the polycondensation of a polyamide block containing dicarboxyl chain ends with a polyether diol is, in this particular case, a polyetheresteramide.
[0040] Preferably, the PEBA according to the invention is obtained by polycondensation 2) or 3), preferably by polycondensation 3).
[0041] Polyamide blocks containing dicarboxyl chain ends result, for example, from the condensation of polyamide precursors in the presence of dicarboxylic acid chain limiters, while polyamide blocks containing diamine chain ends result, for example, from the condensation of polyamide precursors in the presence of diamine chain limiters.
[0042] Three types of polyamide blocks can be advantageously used.
[0043] According to a first type, the polyamide blocks result from the condensation of dicarboxylic acids, in particular those having from 4 to 20 carbon atoms, preferably those having from 6 to 18 carbon atoms, and of aliphatic or aromatic diamines, in particular those having from 2 to 20 carbon atoms, preferably those having from 6 to 14 carbon atoms.
[0044] Examples of dicarboxylic acids include 1,4-cyclohexanedicarboxylic acid, butanedioic acid, adipic acid, azelaic acid, suberic acid, sebacic acid, dodecanedicarboxylic acid, and octadecanedicarboxylic acid, as well as terephthalic acid and isophthalic acid, and may also include dimerized fatty acids.
[0045] Examples of diamines include tetramethylenediamine, hexamethylenediamine, 1,10 decamethylenediamine, dodecamethylenediamine, trimethylhexamethylenediamine, bis(4-aminocyclohexyl)methane (BACM), bis(3-methyl-4-aminocyclohexyl)methane (BMACM), and 2,2-bis(3-methyl-4-aminocyclohexyl)propane (BMACP), paraaminodicyclohexylmethane (PACM), isophoronediamine (IPDA), 2,6-bis(aminomethyl)norbornane (BAMN), and isomers of piperazine (Pip).
[0046] Advantageously, the polyamide blocks PA412, PA414, PA418, PA610, PA612, PA614, PA618, PA912, PA1010, PA1012, PA1014 and PA1018 are used. In the notation of polyamides of the PA XY type, X represents, in the conventional manner, the number of carbon atoms originating from the diamine residue and Y represents the number of carbon atoms originating from the diacid residue.
[0047] According to a second type, the polyamide blocks result from the condensation of one or more α,ω-aminocarboxylic acids and / or one or more lactams having 6 to 12 carbon atoms in the presence of dicarboxylic acids or diamines having 4 to 12 carbon atoms. Examples of lactams include caprolactam, oenantholactam, and lauryllactam. Examples of α,ω-aminocarboxylic acids include aminocaproic acid, 7-aminoheptanoic acid, 11-aminoundecanoic acid, and 12-aminododecanoic acid.
[0048] Advantageously, the second type of polyamide block is a PA11 (polyundecaneamide), PA12 (polydodecanamide) or PA6 (polycaprolactam) block. In the notation of a PA X type polyamide, X represents the number of carbon atoms originating from an amino acid (or lactam) residue.
[0049] According to a third type, the polyamide blocks result from the condensation of at least one α,ω-aminocarboxylic acid (or one lactam), at least one diamine and at least one dicarboxylic acid.
[0050] In this case, the polyamide PA block is - polycondensation of linear aliphatic or aromatic diamines having X carbon atoms, - polycondensation of a dicarboxylic acid having Y carbon atoms, and -prepared by polycondensation of comonomers {Z} selected from an equimolar mixture of lactams and an α,ω-aminocarboxylic acid having Z carbon atoms, and at least one diamine having X1 carbon atoms and at least one dicarboxylic acid having Y1 carbon atoms, (X1, Y1) being different from (X, Y), said comonomers {Z} in a weight proportion in the range advantageously up to 50%, preferably up to 20% and more advantageously even up to 10%, based on the combined polyamide precursor monomers, -dicarboxylic acids.
[0051] Advantageously, as chain limiter, a dicarboxylic acid having Y carbon atoms is used, which is introduced in excess with respect to the stoichiometry of the diamine.
[0052] According to this third type of alternative, the polyamide blocks result from the condensation, in the presence of an optional chain limiter, of at least two α,ω-amino carboxylic acids, or at least two lactams or one lactam having 6 to 12 carbon atoms, and an amino carboxylic acid not having the same number of carbon atoms. Examples of aliphatic α,ω-amino carboxylic acids include aminocaproic acid, 7-aminoheptanoic acid, 11-aminoundecanoic acid, and 12-aminododecanoic acid. Examples of lactams include caprolactam, oenantholactam, and lauryllactam. Examples of aliphatic diamines include hexamethylenediamine, dodecamethylenediamine, and trimethylhexamethylenediamine. Examples of cycloaliphatic diacids include 1,4-cyclohexanedicarboxylic acid. Examples of aliphatic diacids include butanedioic acid, adipic acid, azelaic acid, suberic acid, sebacic acid, and dodecanedicarboxylic acid, dimerized fatty acids. These dimerized fatty acids preferably have a dimer content of at least 98%, and preferably they are hydrogenated, such as the products sold by Croda under the brand Pripol, by BASF under the brand Empol, or by Oleon under the brand Radiacid, and polyoxyalkylene-α,ω-diacids. Examples of aromatic diacids include terephthalic acid (T), isophthalic acid (I). Examples of alicyclic diamines include bis(4-aminocyclohexyl)methane (BACM), bis(3-methyl-4-aminocyclohexyl)methane (BMACM) and 2,2-bis(3-methyl-4-aminocyclohexyl)propane (BMACP), and isomers of paraaminodicyclohexylmethane (PACM). Other commonly used diamines can be isophorone diamine (IPDA), 2,6-bis(aminomethyl)norbornane (BAMN), and piperazine.
[0053] As examples of polyamide blocks of the third type, mention may be made of: - PA66 / 6 (wherein 66 represents a hexamethylenediamine unit condensed with adipic acid and 6 represents a unit resulting from the condensation of caprolactam); PA66 / 610 / 11 / 12, in which 66 represents hexamethylenediamine condensed with adipic acid, 610 represents hexamethylenediamine condensed with sebacic acid, 11 represents units resulting from the condensation of aminoundecanoic acid, and 12 represents units resulting from the condensation of lauryllactam.
[0054] The designations PA X / Y, PA X / Y / Z etc. relate to copolyamides where X, Y, Z etc. represent homopolyamide units as defined above.
[0055] Advantageously, the polyamide blocks of the copolymers used according to the invention are selected from the group consisting of the polyamides PA6, PA11, PA12, PA54, PA59, PA510, PA512, PA513, PA514, PA516, PA518, PA536, PA64, PA69, PA610, PA612, PA613, PA614, PA616, PA618, PA636, PA104, PA109, PA1010, PA1012, PA1013, PA1014 , PA1016, PA1018, PA1036, PA10T, PA124, PA129, PA1210, PA1212, PA1213, PA1214, PA1216, PA1218, PA1236, PA12T, or mixtures or copolymers thereof, and preferably comprises blocks of polyamide PA6, PA11, PA12, PA610, PA1010, PA1012, or mixtures or copolymers thereof.
[0056] The polyether blocks consist of alkylene oxide units.
[0057] The polyether blocks may in particular be PEG (polyethylene glycol) blocks, i.e. consisting of ethylene oxide units, and / or PPG (propylene glycol) blocks, i.e. consisting of propylene oxide units, and / or PO3G (polytrimethylene glycol) blocks, i.e. consisting of polytrimethylene glycol ether units, and / or PTMG blocks, i.e. consisting of tetramethylene glycol (also called polytetrahydrofuran) units. PEBA copolymers may contain several types of polyethers in their chain, and the copolyethers can be block or random.
[0058] It is also possible to use blocks obtained by oxyethylation of bisphenols, such as, for example, bisphenol A. The latter products are described, inter alia, in EP 613 919.
[0059] The polyether blocks may also comprise ethoxylated primary amines. Examples of ethoxylated primary amines include those of the formula: Mention may be made of the products of formula TIFF0007564827000001.tif35170, where m and n are integers from 1 to 20, and x is an integer from 8 to 18. These products are commercially available, for example, under the Noramox® brand from CECA and the Genamin® brand from Clariant.
[0060] The polyether block may comprise a polyoxyalkylene block containing an NH2 chain end, such a block being obtainable by cyanoacetylation of an aliphatic α,ω-dihydroxylated polyoxyalkylene block known as a polyether diol. More specifically, a commercial product of Jeffamine or Elastamine (e.g., Jeffamine® D400, D2000, ED2003, or XTJ542, a commercial product from Huntsman, also described in JP 2004346274, JP 2004352794, and EP 1482011) may be used.
[0061] The polyether diol blocks are either used as is and co-condensed with polyamide blocks having carboxyl end groups, or converted to polyether diamines and aminated for condensation with polyamide blocks having carboxyl end groups.
[0062] The general method for the two-step preparation of PEBA copolymers with ester bonds between the PA and PE blocks is known and is described, for example, in FR 2846332. The general method for the preparation of PEBA copolymers with amide bonds between the PA and PE blocks is known and is described, for example, in EP 1482011. The polyether blocks can also be mixed with polyamide precursors and chain-limiting diacids to prepare polymers comprising polyamide blocks and polyether blocks with randomly distributed units (one-step process).
[0063] Of course, any reference to PEBA in this specification of the present invention may equally relate to PEBAX® products sold by Arkema, Vestamid® products sold by Evonik®, Grilamid® products sold by EMS, PEBA-type Pelestat® products sold by Sanyo, or any other PEBA from other suppliers.
[0064] Although the block copolymers described above generally comprise at least one polyamide block and at least one polyether block, the present invention also encompasses all copolymers comprising two, three, four (indeed even more) different blocks selected from those described herein, provided that these blocks comprise at least polyamide and polyether blocks.
[0065] For example, the copolymer according to the invention may comprise a segmented block copolymer (or "triblock" copolymer) comprising three different types of blocks, resulting from the condensation of several of the above blocks, said triblock being preferably selected from copolyetheresteramides and copolyetheramideurethanes.
[0066] Particularly preferred PEBA copolymers in the context of the present invention are -PA11 and PEG blocks, -PA11 and PTMG blocks, -PA12 and PEG blocks, -PA12 and PTMG blocks, -PA610 and PEG blocks, -PA610 and PTMG blocks, -PA1010 and PEG blocks, -PA1010 and PTMG blocks, -PA1012 and PEG block, -PA1012 and PTMG blocks, -PA6 and PEG blocks, -PA6 and PTMG blocks It is a copolymer comprising:
[0067] The number average molar mass of the polyamide blocks in the PEBA copolymer is less than or equal to 1000 g / mol, preferably less than or equal to 900 g / mol.
[0068] Thus, the polyamide blocks in the PEBA copolymer can have a number average molar mass of 100-200 g / mol, or 200-300 g / mol, or 300-400 g / mol, or 400-500 g / mol, or 500-600 g / mol, or 600-700 g / mol, or 700-800 g / mol, or 800-900 g / mol, or 900-1000 g / mol.
[0069] In a particular embodiment, the number average molar mass of the polyether blocks in the PEBA copolymer has a value of 250 to 2000 g / mol, preferably 400 to 2000 g / mol, for example, more preferably 800 to 1500 g / mol.
[0070] Thus, the polyether blocks in the PEBA copolymer can have a number average molar mass of 250-300 g / mol, or 300-400 g / mol, or 400-500 g / mol, or 500-600 g / mol, or 600-700 g / mol, or 700-800 g / mol, or 800-900 g / mol, or 900-1000 g / mol, or 1000-1500 g / mol, or 1500-2000 g / mol.
[0071] The number average molar mass is set by the content of chain limiter, which can be calculated according to the following relationship: M n =n モノマー ×MW 反復単位 / n 鎖制限剤 +MW 鎖制限剤
[0072] In this formula, n モノマー is the number of moles of monomer, n 鎖制限剤 is the number of moles of excess chain limiter (e.g., diacid), MW 反復単位 is the molar mass of the repeating unit, MW 鎖制限剤 is the molar mass of the excess chain limiter (e.g., diacid).
[0073] The number-average molar masses of the polyamide blocks and of the polyether blocks can be determined by gel permeation chromatography (GPC) before copolymerization of the blocks.
[0074] The weight ratio of the polyamide blocks to the polyether blocks of the PEBA copolymer is less than or equal to 0.7, preferably less than or equal to 0.65, which can be calculated by dividing the number average molar mass of the polyamide blocks by the number average molar mass of the polyether blocks.
[0075] Thus, the weight ratio of polyamide blocks to polyether blocks of the PEBA copolymer can be from 0.1 to 0.2, or from 0.2 to 0.3, or from 0.3 to 0.4, or from 0.4 to 0.5, or from 0.5 to 0.6, or from 0.6 to 0.7.
[0076] Preferably, the copolymers used in the present invention exhibit an instantaneous hardness of 20 Shore D to 75 Shore D, preferably 25 Shore D to 45 Shore D. Hardness measurements can be performed according to ISO standard 868:2003.
[0077] The practice of the present invention is particularly advantageous with particles of relatively flexible PEBA copolymers insofar as such copolymers have an increased tendency to agglomerate.
[0078] The PEBA copolymer may exhibit a glass transition temperature of 0° C. or less, preferably −20° C. or less, more preferably −40° C. or less, more preferably −50° C. or less, as measured by dynamic mechanical analysis (DMA) according to ISO standard 6721-11:2012.
[0079] Method for producing copolymer powder First, the method according to the present invention includes providing a PEBA copolymer as described above. According to certain embodiments, it is possible to use a mixture of two or more PEBA copolymers as described above. However, it is preferred to use a single PEBA copolymer as described above. The PEBA copolymer can be, for example, in the form of granules. Alternatively, the PEBA copolymer can be, for example, in the form of flakes or coarse powder having a size Dv50 of more than 250 μm.
[0080] The PEBA copolymer is then contacted with a flow agent, preferably prior to the grinding step, to form a mixture.
[0081] The term "flow agent" is understood to mean an agent that makes it possible to improve the flowability and leveling of the copolymer powder during the sintering process. The flow agent can be selected from those commonly used in the field of sintering of polymer powders. Preferably, this flow agent is substantially spherical. It is selected, for example, from silica, in particular hydrated silica, pyrogenic silica, vitreous silica or fumed silica; alumina, in particular amorphous alumina; glassy phosphates, glassy borates, glassy oxides, titanium dioxide, calcium silicate, magnesium silicate, talc, mica, kaolin, attapulgite, and mixtures thereof.
[0082] The flow agent is in the form of particles having an average size (Dv50) of 10 μm or less, more preferably 1 μm or less. For example, the size Dv50 of the particles of the flow agent can be 10 nm to 100 nm, 100 nm to 1 μm, 1 μm to 10 μm.
[0083] In the context of this patent application: - Dv10 corresponds to the particle size threshold at which 10% of the particles (by volume) have a size below the threshold and 90% of the particles (by volume) have a size above the threshold; - Dv50 corresponds to the particle size threshold at which 50% of the particles (by volume) have a size below the threshold and 50% of the particles (by volume) have a size above the threshold; - Dv90 corresponds to the particle size threshold for which 90% of the particles (by volume) have a size below the threshold and 10% of the particles (by volume) have a size above the threshold.
[0084] Dv10, Dv50 and Dv90 are measured according to ISO13320:2009, e.g. by laser diffraction using a Malvern diffractometer by the dry route, and the particle distribution is modelled according to ISO standard 9276-parts 1 to 6 "Presentation of the results of particle size analysis".
[0085] The flow agent is added to the PEBA copolymer in a proportion of at least 0.3% by weight, based on the total weight of the final composition.
[0086] The flow agent added to the copolymer may have a content of 3% by weight or less, preferably 2% by weight or less, relative to the total weight of the final composition, i.e., the flow agent may be added in a proportion of 0.3% to 0.4%, or 0.4% to 0.5%, or 0.5% to 0.6%, or 0.6% to 0.7%, or 0.7% to 0.8%, or 0.8% to 0.9%, or 0.9% to 1%, or 1% to 1.1%, or 1.1% to 1.2%, or 1.2% to 1.3%, or 1.3% to 1.4%, or 1.4% to 1.5%, or 1.5% to 1.6%, or 1.6% to 1.7%, or 1.7% to 1.8%, or 1.8% to 1.9%, or 1.9% to 2%, or 2% to 2.5%, or 2.5% to 3.0%.
[0087] The PEBA copolymer is preferably premixed with a flow agent and then undergoes a milling step to obtain a powder having the desired particle size.
[0088] Preferably, the grinding is cryogenic grinding. Thus, first, the mixture of the copolymer and the flow agent is cooled to a temperature lower than the glass transition temperature of the copolymer. This temperature can be 10 to 50°C lower than the glass transition temperature of the copolymer. That is, the mixture can be cooled to a temperature of -10°C or lower, preferably -50°C or lower, more preferably -80°C or lower. This temperature can be -10 to -20°C, or -20 to -30°C, or -30 to -40°C, or -40 to -50°C, or -50 to -60°C, or -60 to -70°C, or -70 to -80°C, or -80 to -90°C, or -90 to -100°C.
[0089] Cooling of the mixture of copolymer and flow agent can be carried out, for example, with liquid nitrogen, or with liquid carbon dioxide, or with dry ice, or with liquid helium.
[0090] Preferably, the grinding process is carried out in a mill with counter-rotating pins (pin mill), i.e. the mill has a first series of brushes rotating in one direction and a second series of brushes rotating in the opposite direction. This makes it possible to increase the speed and therefore the energy of the impact. Preferably, the pins can be grooved, which allows a greater impact on the particles to be ground.
[0091] Alternatively, the grinding step can be carried out in a hammer mill or whirlmill.
[0092] The mill used can be equipped with a sieve over which the ground particles are guided. The sieve exhibits pores (sieve openings) which, on the one hand, allow the retention of particles having a size larger than the sieve pores and, on the other hand, allow the passage of particles having a size smaller than the sieve pores. If the pores do not have circular openings, the term "diameter" of the pores is understood to mean the maximum distance between two points occurring in a plane parallel to the openings. For example, in the case of pores with rectangular or square openings, the diameter indicates the diagonal of each opening. The sieve can have pores with a diameter of, for example, 300 μm or less, or 250 μm or less, preferably 200 μm or less. The diameter of the pores can be, for example, 100 to 120 μm, 120 to 150 μm, or 150 to 200 μm, or 200 to 250 μm, or 250 to 300 μm.
[0093] Thus, particles larger than desired for powder preparation can be retained on the sieve while particles of the appropriate size can pass through the sieve.
[0094] The particles retained on the screen can then be recycled and directed to a mill for further comminution.
[0095] Preferably, the recycling of particles is continuous in the grinding process.
[0096] Preferably, a single grinding step is carried out.
[0097] After grinding, a specific particle size fraction of the powder can be selected in the present invention to obtain a desired particle size profile. The powder is thus dispersed by a selection wheel and conveyed by the classified air. The powder entrained in the air is conveyed through a support wheel and discharged from a first outlet. The crude product is rejected by a classifying wheel and conveyed to a second outlet. The selector can comprise several successive wheels operating in parallel.
[0098] PEBA powder composition The composition according to the present invention comprises particles of a PEBA copolymer and particles of a flow agent.
[0099] The particles of the composition according to the invention may have a size Dv10 of 30 μm or more, preferably 35 μm or more. For example, the size Dv10 of the particles of the composition may be 30-35 μm, or 35-40 μm, or 40-45 μm, or 45-50 μm.
[0100] A size Dv10 of 30 μm or more makes it possible to avoid problems related to the density and flowability of the powder. Advantageously, therefore, the use of powders with particles having a size Dv10 of 30 μm or more makes it possible to obtain a good quality powder bed and, as a result, to obtain articles with good definition of edges and contours.
[0101] The use of powders with a size Dv10 greater than 30 μm allows for less agglomeration of the powder in the three-dimensional printer and thus better recycling.
[0102] The amount of flow agent in the composition can be adapted as a function of the particle size of the powder. In general, the lower the Dv10 of the powder, the more flow agent is required in the powder to maintain its flowability and the mechanical properties of the manufactured parts.
[0103] The particles of the composition according to the invention may also have a size Dv90 of less than or equal to 250 μm, preferably less than or equal to 200 μm. For example, the size Dv90 of the particles of the composition may be 150-160 μm, or 160-170 μm, or 170-180 μm, or 180-190 μm, or 190-200 μm, or 200-210 μm, or 210-220 μm, or 220-230 μm, or 230-240 μm, or 240-250 μm.
[0104] A size Dv90 of less than or equal to 250 μm also makes it possible to obtain articles with good definition of edges and contours, since particles with a size Dv90 of more than 250 μm may result in articles exhibiting low definition due to the layer thickness used during the sintering process.
[0105] Furthermore, the particles of the composition according to the invention can have a size Dv50 of 80-150 μm, preferably 100-150 μm. For example, the size Dv50 of the particles of the composition can be 80-85 μm, or 85-90 μm, or 90-95 μm, or 95-100 μm, or 100-105 μm, or 105-110 μm, or 110-115 μm, or 115-120 μm, or 120-125 μm, or 125-130 μm, or 130-135 μm, or 135-140 μm, or 140-145 μm, or 145-150 μm.
[0106] The composition according to the invention preferably has a solubility of 80% or more, or 81% or more, or 82% or more, or 83% or more, or 84% or more, or 85% or more, or 86% or more, or 87% or more, or 88% or more, or 89% or more, or 90% or more, or 91% or more, or 92% or more, or 93% or more, or 94% or more, or 95% or more, or 96% or more, or 97% or more, or 98% or more, or 99% or more, or 99.1% or more, or 99.2% or more. , or 99.3% or more, or 99.4% or more, or 99.5% or more, or 99.6% or more, or 99.7% or more, or 99.8% or more, or 99.9% or more, or 99.91% or more, or 99.92% or more, or 99.93% or more, or 99.94% or more, or 99.95% or more, or 99.96% or more, or 99.97% or more, or 99.98% or more, or 99.99% or more by weight of PEBA copolymer.
[0107] The flow agent is present in the composition in a content of 0.3% by weight or more based on the weight of the composition. Preferably, the flow agent present in the composition can have a content of 2% by weight or less based on the weight of the composition. That is, the content can be 0.3% to 0.4%, or 0.4% to 0.5%, or 0.5% to 0.6%, or 0.6% to 0.7%, 0.7% to 0.8%, or 0.8% to 0.9%, or 0.9% to 1%, or 1% to 1.1%, or 1.1% to 1.2%, or 1.2% to 1.3%, or 1.3% to 1.4%, or 1.4% to 1.5%, or 1.5% to 1.6%, or 1.6% to 1.7%, or 1.7% to 1.8%, or 1.8% to 1.9%, or 1.9% to 2%.
[0108] The PEBA powder in this composition is 2m 2 / g.
[0109] The PEBA particles in the composition may contain powder fillers in a content of 0% to 10% by weight based on the weight of the composition. If they are present, these powder fillers may be incorporated into the PEBA particles by compounding, in particular during the manufacturing process of granules intended to be milled.
[0110] Thus, the composition may further comprise 0% to 10% by weight of a powder filler, based on the total weight of the composition.
[0111] The term "powder filler" refers to powders with an average size (Dv 50 ), which makes it possible to improve the mechanical properties (e.g. modulus of elasticity, elongation at break, impact strength) of the three-dimensional parts manufactured.
[0112] Examples of powder fillers are carbonate-containing inorganic fillers, in particular calcium carbonate, magnesium carbonate, dolomite or calcite, barium sulfate, calcium sulfate, dolomite, alumina hydrate, wollastonite, montmorillonite, zeolite or perlite, organic fillers, for example polymer powders having a melting point higher than the maximum temperature that the composition will withstand during the layer-by-layer modeling process, in particular such polymer powders having an elastic modulus of more than 1000 MPa.
[0113] According to one preferred embodiment, the PEBA particles of the composition of the present invention are free of powder fillers.
[0114] According to certain preferred embodiments, the composition according to the invention does not contain powder fillers.
[0115] Alternatively, when a powder filler is present in the PEBA particles, the powder filler is present in a weight content of 10 wt% or less, preferably 5 wt% or less, more preferably 1 wt% or less. For example, the powder filler can be present in the PEBA particles in a weight content of 0.05-1 wt%, or 1-2 wt%, or 2-3 wt%, or 3-4 wt%, or 4-5 wt%, or 5-6 wt%, or 6-7 wt%, or 7-8 wt%, or 8-9 wt%, or 9-10 wt%.
[0116] The total weight content of powder filler (if present) in the composition (including those present in the PEBA particles, if applicable) is preferably not more than 10%, preferably not more than 5%, more preferably not more than 1%.
[0117] In addition to the flow agents and powder fillers already mentioned, the compositions according to the invention can contain any kind of other additives suitable for polymer powders used for sintering, in particular additives (in powder or non-powder form) that contribute to improving the properties of the powder for use in agglomeration techniques and / or additives that make it possible to improve the properties of the object obtained by fusion, for example the aesthetic (color) properties. The compositions according to the invention can in particular contain dyes, pigments for coloring, TiO2, pigments for infrared absorption, carbon black, fire additives, glass fibers, carbon fibers, etc. The compositions according to the invention can further contain at least one additive selected from stabilizers, antioxidants, light stabilizers, impact modifiers, antistatic agents, flame retardants, and mixtures thereof. These additives are preferably in the form of a powder with a Dv50 of less than 20 μm, in particular less than 10 μm. Advantageously, the additives in powder form have a Dv of more than 100 nm, very particularly more than 1 μm.
[0118] These additives may be present in the composition in a weight content ranging from 0.05% to 5% by weight.
[0119] Preferably, the additive comprises one or more pigments.
[0120] The additives may be mixed with the PEBA copolymer before and / or after the grinding step described above.
[0121] In a particular embodiment, the powder composition may have a crystallization temperature of the polyamide blocks of 40-160° C., preferably 50-100° C. The composition may in particular have a crystallization temperature of the polyamide blocks of 40-50° C., or 50-60° C., or 60-70° C., or 70-80° C., or 80-90° C., or 90-100° C., or 100-110° C., or 110-120° C., or 120-130° C., or 130-140° C., or 140-150° C., or 150-160° C. The crystallization temperature can be measured by differential scanning calorimetry according to ISO standard 11357-3.
[0122] The PEBA copolymer may have a melting point of 150° C. or less, preferably 140° C. or less. The PEBA copolymer may in particular have a melting point of 100-105° C., or 105-110° C., or 110-115° C., or 115-120° C., or 120-125° C., or 125-130° C., or 130-135° C., or 135-140° C., or 140-145° C., or 145-150° C. The melting point can be measured by differential scanning calorimetry according to ISO standard 11357-3.
[0123] A melting point of 150° C. or less makes it possible to reduce the heating time and energy consumption during the process for layer-by-layer fabrication of three-dimensional articles by sintering, thus improving the efficiency of the process for the preparation of such articles.
[0124] The difference between the crystallization temperature and the melting point is preferably 30°C or more, more preferably 40°C or more, or 50°C or more, or 60°C or more, or 70°C or more, or 80°C or more.
[0125] The powder composition according to the invention may have a flowability of 2 to 10 seconds. The flowability may be measured according to method A (25 mm hole at 23° C.) of ISO standard 6186:1998(E).
[0126] Process for sintering powders The PEBA powder is used in a process for layer-by-layer fabrication of three-dimensional articles by electromagnetic radiation induced sintering, as described above.
[0127] The electromagnetic radiation may for example be infrared radiation, ultraviolet radiation or, preferably, laser radiation.
[0128] According to this process, a thin layer of powder is deposited on a horizontal plate maintained in a chamber heated to a temperature called the build temperature. The term "build temperature" denotes the temperature to which the powder bed of the constituent layers of the three-dimensional object being built is heated during the process for layer-by-layer sintering of the powder. This temperature can be 100°C below the melting point of the PEBA copolymer, preferably below 40°C, more preferably about 20°C below. The electromagnetic radiation then provides the energy necessary to sinter the powder particles at various positions of the powder layer according to the geometric shape corresponding to the object (for example, using a computer that has the shape of the object in memory and reproduces the latter in the form of a cross section).
[0129] The horizontal plate is then lowered by a value corresponding to the thickness of the powder layer and a new layer is deposited. The electromagnetic radiation provides the energy necessary to sinter the powder particles according to the geometric shape corresponding to this new cross section of the object, and so on. This procedure is repeated until the object is produced.
[0130] Preferably, the powder layer deposited on the horizontal plate (before sintering) may have a thickness of 20-200 μm, preferably 50-150 μm. The layer of agglomerated material may have a thickness of 10-150 μm, preferably 30-100 μm, after sintering.
[0131] The powder composition can be recycled and reused in several successive layers, as described above, for example, as is or as a mixture with other powders, recycled or not recycled.
[0132] That is, the powder composition can be recycled (ie, used in two or more stacks) one, or two, or three, or four, or five, or six or more times.
[0133] The three-dimensional article produced may exhibit an elongation at break of 200% or more, preferably 400% or more, more preferably 500% or more. The term "elongation at break" is understood to mean the ability of a material to elongate before breaking when placed under tensile stress. Elongation at break can be measured according to ISO standard 527 1A.
[0134] The three-dimensional article produced can advantageously exhibit an elastic modulus of less than or equal to 100 MPa, more preferably less than or equal to 70 MPa, or less than or equal to 50 MPa, which can be, for example, between 1 and 100 MPa, preferably between 10 and 70 MPa. The elastic modulus can be measured according to ISO standard 527 1:2019.
[0135] Thus, the powder composition according to the invention makes it possible to produce good quality three-dimensional articles having good mechanical properties and precise and well-defined dimensions and contours. EXAMPLES
[0136] The following examples illustrate the invention without limiting it. Unless otherwise indicated, the percentages indicated refer to percentages by weight based on the complete formulation.
[0137] Example 1 In this example, powders of PEBA copolymer (without filler) (600 g / mol of PA11 block, 1000 g / mol of PTMG block, weight ratio PA11 / PTMG=0.6, Tm=135° C., formulated with 0.8 wt. % of stabilizing additive) having size Dv10 of 21 μm, size Dv50 of 48 μm, and size Dv90 of 100 μm were mixed in a high-speed mixer with different weight contents of the following flow agents: Agent 1: Average size 0.1 to less than 0.3 μm, specific surface area 50 m 2 / g pyrogenic silica, treated with dimethyldichlorosilane, TS610 sold by Cabot Corporation) Agent 2: Average size less than 1 μm, specific surface area 220 m 2 / g pyrogenic silica (CT1221 sold by Cabot Corporation) Agent 3: Average size 7-40 nm, specific surface area 50 m 2 Calcined alumina (Alumina C sold by Evonik) with > 1.0 g (BET)
[0138] The flowability of these mixtures with holes of diameter 25 mm and 15 mm is also measured, as well as the apparent density and tamped density (flowability according to method A of ISO standard 6186:1998(E), 23°C, tamping volume meter according to DIN ISO standard 787 part 11:1981, 2500 taps on a graduated cylinder with graduations for tamped density). TIFF0007564827000002.tif85170
[0139] It is observed that mixtures with a flow agent content of 0.3% by weight or more give better results. More specifically, a good flowability can be characterized in particular by the flowability through a 15 mm diameter funnel and a 25 mm diameter funnel, which makes it possible to obtain a good supply of powder. This also makes it possible to obtain sufficient diffusion to obtain a good powder bed before and during sintering, as well as sufficient flow to fill the cavities of the part after the laser pass. Mixtures with a flow agent content of 0.3% by weight or more also make it possible to improve the apparent density and the tamping density compared to PEBA powder alone.
[0140] Example 2 In this example, PEBA powders (with the same characteristics as in Example 1) having a size Dv10 of 42 μm, a size Dv50 of 106 μm, and a size Dv90 of 178 μm (without filler) are mixed in a high-speed mixer with different weight contents of flow agent (TS610 sold by Cabot Corporation). TIFF0007564827000003.tif32170
[0141] As in this example, when the PEBA copolymer powder has a size Dv10 greater than 30 μm, a size Dv50 between 50 and 150 μm, and a size Dv90 less than 250 μm, it is observed that the flowability, and also the apparent density and tamped density, are improved compared to the PEBA powder alone.
[0142] Example 3 In this example, PEBA powder (same characteristics as in Example 1) is mixed with 0.3% by weight of a flow agent (TS610 sold by Cabot Corporation). The flow agent is added to the PEBA granules before grinding to obtain a powder. The resulting powder has a Dv10 of 24 μm, a Dv50 of 73 μm and a Dv90 of 217 μm (composition A). Selection is then performed using a CFS 5 HD-S selector (Netzsch) by setting the rotation speed so as to obtain a powder with a Dv10 of 38 μm, a Dv50 of 88 μm and a Dv90 of 231 μm at an inlet flow rate of 2 kg / h (composition B).
[0143] The following tests were carried out on the two compositions, and the results are shown in Table 3 below. The two compositions are poured into two metal cylinders of 5 cm diameter and 3 cm height in the same way. The cylinders containing the compositions are then placed in an oven at a temperature 20° C. below the melting point of the PEBA copolymer (115° C.) for 4 hours. The cylinders are removed from the oven and allowed to cool to room temperature (23° C.) for 4 hours.
[0144] A needle with a diameter of 1 mm, ballasted with a 500 g weight, is then dropped onto various locations on the surface of the powder. By measuring the depth to which the needle sinks, it is possible to evaluate the cohesion of the powder after 4 hours at 20° C. below the melting point of the PEBA copolymer and 4 hours of cooling down to room temperature. The less the needle sinks and the more the powder sticks to itself in the oven, the more difficult it will be to reuse it. TIFF0007564827000004.tif20170
[0145] It is observed that the needles sink deeper in composition B, which has a Dv10 of more than 30 μm, meaning that this powder is less sticky and therefore easier to recycle.
[0146] Example 4 Filler-free PEBA granules (850 g / mol PA12 block, 2000 g / mol PTMG block, weight ratio PA12 / PTMG=0.425, compounded with 0.2 wt.% stabilizing additive) are ground under cryogenic conditions using a Mikropul 2DH hammer mill. This powder composition (C) obtained after grinding has a size Dv10 of 66 μm, a size Dv50 of 157 μm and a size Dv90 of 292 μm.
[0147] Similarly, the same PEBA granules premixed with 1.0% by weight of flow agent (TS610 sold by Cabot Corporation) are introduced into the mill under the same conditions. This powder composition (D) obtained after grinding has a size Dv10 of 60 μm, a size Dv50 of 137 μm and a size Dv90 of 247 μm. It can be seen that powder composition D has a reduced Dv90 compared to powder composition C.
[0148] Example 5 The following powders are tested: -EC1 (comparison): PA12 powder (PEBA 2301 Primepart ST sold by EOS) -EC2 (comparison): PA12 / PPG PEBA powder with a PA12 block size of 1068 g / mol, a PPG block size of 2000 g / mol, and a PA12 / PPG ratio of approximately 0.53 -EC3 (comparison): PA12 / PEG PEBA powder with PA12 block size of 1500g / mol, PEG block size of 1500g / mol, and PA12 / PEG ratio of 1 -EC4 (comparison): PA12 / PTMG PEBA powder with PA12 block size of 1000g / mol, PTMG block size of 1000g / mol, and PA12 / PTMG ratio of 1 -EC5 (comparison): PA11 / PTMG PEBA powder with PA11 block size of 1000g / mol, PTMG block size of 1000g / mol, and PA11 / PTMG ratio of 1 -E1 (invention): PA12 / PTMG PEBA powder with a PA12 block size of 850 g / mol, a PTMG block size of 2000 g / mol, and a PA12 / PTMG ratio of 0.43 -E2 (invention): PA11 / PTMG PEBA powder with a PA11 block size of 600 g / mol, a PTMG block size of 1000 g / mol, and a PA11 / PTMG ratio of 0.6 -E3 (invention): PA12 / PTMG PEBA powder with a PA12 block size of 600 g / mol, a PTMG block size of 2000 g / mol, and a PA12 / PTMG ratio of 0.3 -E4 (invention): PA11 / PTMG PEBA powder with a PA11 block size of 600 g / mol, a PTMG block size of 2000 g / mol, and a PA11 / PTMG ratio of 0.3
[0149] The PA12 based PEBA is compounded with 0.2 wt% stabilizing additive, and the PA11 based PEBA is compounded with 0.8 wt% stabilizing additive. All of these powders are filler-free.
[0150] Differential scanning calorimetry (DSC) analysis of these powders at 20° C. / min (standard conditions) and also measurement of the elastic moduli of parts produced by injection molding starting from these powders gave the following results: TIFF0007564827000005.tif61170
[0151] When the weight ratio of polyamide blocks to polyether blocks in the PEBA is less than or equal to 0.7 and when the polyamide blocks have a number average molar mass less than or equal to 1000 g / mol (E1 to E4), the melting points of the PEBA copolymers are observed to be lower (with respect to EC1 to EC5) and sufficiently far from the crystallization temperature, which subsequently makes it possible to work with a wide range of build temperature values in the layer-by-layer build process.
[0152] It was also observed that the tensile modulus measured on the resulting injection molded parts was less than 50 MPa, which means that the powders of the invention impart good mechanical properties, in particular good flexibility.
[0153] The elastic modulus is measured according to ISO standard 527-1 / 2.
[0154] The elastic modulus of a sintered part may differ with respect to that of an injection-molded part. This is due to the more crystallized sintered three-dimensional object, which remains longer between Tm and Tc than injection-molded. However, the relative comparison of the elastic modulus obtained with injection molding represents the relative comparison of the elastic modulus obtained with sintering. Thus, according to the invention, it is possible to obtain three-dimensional articles exhibiting an elastic modulus of less than or equal to 70 MPa, preferably less than or equal to 50 MPa.
[0155] Example 6 PEBA powders (PA11 block size 600 g / mol, PTMG block size 1000 g / mol, weight ratio of PA11 / PTMG block 0.6) with size Dv10 of 42 μm, size Dv50 of 106 μm, and size Dv90 of 178 μm, without fillers and with added flow agent (TS610 sold by Cabot Corporation) are sieved at 160 μm by passing through an EOS Formiga P100 machine before undergoing the sintering process. The specimens are sieved at 350 mJ / mm at a build temperature of 103.5 °C. 31000μm, which makes it possible to obtain good fineness and optimal mechanical properties. The powder from the bed not touched by the electromagnetic radiation is sieved again at 160μm after cooling.
[0156] The results are shown below. TIFF0007564827000006.tif33170
[0157] It is observed that the addition of 0.2% by weight of flow agent does not allow to obtain good recyclability of the powder. However, the addition of flow agent at a content of 0.3% by weight or more reduces the agglomeration of the powder, and as a result the recyclability of the powder is significantly improved. The addition of 1% by weight of flow agent makes it possible to achieve the full maximum recyclability of the powder.
[0158] Example 7 Using the PEBA powder of Example 6, an EOS Formiga P100 machine (printing temperature 103.5°C, laser energy 350 mJ / mm 3 ) to carry out the laser sintering process. 1BA test specimens for tensile testing and test specimens (notched after sintering) for measuring the Charpy impact strength at room temperature and at -30°C are obtained.
[0159] The results are shown below. TIFF0007564827000007.tif35170
[0160] The elongation at break was measured according to ISO standard 527-2 1BA.
[0161] The measurements of the Charpy impact strength were carried out according to ISO standard 179 / 1eA (at 23° C. and −30° C.).
[0162] It is observed that the presence of flow agents in amounts of 0.3% to 1.0% by weight does not impair the mechanical properties of the parts obtained by laser sintering.
[0163] Example 8 PEBA granules (same characteristics as in Example 1) are mixed with 20% by weight of dolomite, a powder filler, then ground in a Mikropul 2DH hammer mill, and the powder is subsequently sieved at 160 μm. The powder has a size Dv10 of 33 μm, a size Dv50 of 62 μm, and a size Dv90 of 111 μm.
[0164] A similar powder is prepared without the incorporation of any filler.
[0165] Subsequently, 0.3% by weight of a flow agent (TS610) is added to the two resulting powders.
[0166] Starting from these powders, the sintering process was carried out using a Formiga P100 machine (sold by EOS) under optimized conditions (build temperature 105 °C, laser energy 350 mJ / mm 3 ) was used.
[0167] The results are shown below. TIFF0007564827000008.tif29170
[0168] When powder filler is present in a significant content in the PEBA particles, it is observed that three-dimensional articles are obtained that have impaired mechanical properties, in particular reduced elongation at break, compared to three-dimensional articles obtained from compositions that do not contain powder filler in the PEBA particles.
Claims
1. 1. A composition comprising a powder of a copolymer comprising polyamide blocks and comprising polyether blocks, the copolymer being in the form of particles having a powder filler content of 0% to 10% by weight, the copolymer having a weight ratio of polyamide blocks to polyether blocks of less than or equal to 0.7, the polyamide blocks having a number average molar mass of less than or equal to 1000 g / mol; the composition comprising a flow agent in a content of more than or equal to 0.3% by weight.
2. 2. The composition according to claim 1, wherein the polyamide blocks have a number-average molar mass of less than or equal to 900 g / mol.
3. 3. The composition according to claim 1, wherein the weight ratio of polyamide blocks to polyether blocks is less than or equal to 0.
65.
4. 4. The composition according to claim 1, wherein the flow agent is present in a content of less than or equal to 2% by weight.
5. 5. The composition of claim 1, wherein the flow agent is selected from silica, alumina, glassy phosphates, glassy borates, glassy oxides, titanium dioxide, calcium silicate, magnesium silicate, talc, mica, kaolin, attapulgite, and mixtures thereof.
6. 6. The composition according to claim 1, wherein the particles of the powder have a size Dv10 of 30 μm or more.
7. 7. The composition according to claim 1, wherein the particles of the powder have a size Dv90 of less than or equal to 250 μm.
8. 8. The composition according to claim 1, wherein the particles of the powder have a size Dv50 of 80 to 150 μm.
9. The composition according to any one of claims 1 to 8, wherein the copolymer exhibits an instantaneous hardness of from 20 to 75 Shore D.
10. 10. The composition according to claim 1, wherein the polyamide block of the copolymer is a block of polyamide 11, or polyamide 12, or polyamide 6, or polyamide 1010, or polyamide 1012, or polyamide 610; and / or the polyether block of the copolymer is a block of polyethylene glycol, polypropylene glycol, or polytetrahydrofuran.
11. 11. The composition according to claim 1, wherein the polyamide block of the copolymer is a block of polyamide 11, or polyamide 12, or polyamide 1010, or polyamide 1012; and / or the polyether block of the copolymer is a block of polyethylene glycol, polypropylene glycol, or polytetrahydrofuran.
12. 12. The composition according to claim 1, wherein the polyether blocks have a number-average molar mass of from 400 to 3000 g / mol.
13. A method for preparing a composition according to any one of claims 1 to 12, comprising: Providing and grinding a copolymer including polyamide blocks and including polyether blocks; and contacting the copolymer with a flow agent; The method includes:
14. 14. The method of claim 13, wherein the copolymer is contacted with a flow agent prior to grinding.
15. 15. The method according to claim 13 or 14, wherein the grinding is carried out on the mixture cooled to a temperature of -10°C or lower.
16. 16. The method according to any one of claims 13 to 15, wherein the copolymer is provided in the form of granules.
17. 17. The method according to any one of claims 13 to 16, wherein the particles resulting from the grinding are sieved and the sieve oversize is recycled to the grinding.
18. 13. Use of a composition according to any one of claims 1 to 12 for layer-by-layer fabrication of three-dimensional articles by sintering of the composition induced by electromagnetic radiation.
19. 13. A three-dimensional article produced from the composition of any one of claims 1 to 12 by layer-by-layer fabrication with electromagnetic radiation induced sintering.
Citation Information
Patent Citations
Laser-sinterable thermoplastic powder
JP2002512645A
Polymer powder containing block polyether amide, its use in molding method and molded article produced from the polymer powder
JP2006225664A
Thermoplastic powder composition and a three-dimensional object obtained by sintering this composition
JP2013517344A
Precipitation of polyether block amide and thermoplastic polyethylene to enhance operational window for three dimensional printing
US20190264047A1
Thermoplastic powder composition and reinforced three-dimensional object produced by 3D printing of such a composition
WO2019069032A1