Method for producing catalysts with reduced attrition - Patent application
By producing hydrogenation catalysts with a higher nickel content and controlled size using an alkaline treatment, the method addresses high attrition rates, achieving reduced wear and improved activity in fixed bed reactors.
Patent Information
- Application Number
- JP2023012446
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2016-11-22
- Filing Date
- 2023-01-31
- Publication Date
- 2024-10-09
- Estimated Expiration
- 2037-11-20
AI Technical Summary
Existing hydrogenation catalysts based on porous nickel alloys suffer from high attrition rates due to mechanical forces during handling and use, leading to reduced catalyst life and productivity issues in fixed bed reactors.
A method is developed to produce catalysts with a higher nickel content (43% to 60% by weight) and controlled particle size (1 mm to 10 mm) using an alkaline treatment to reduce aluminum content, resulting in improved abrasion resistance and lower attrition rates.
The method achieves a significant reduction in catalyst wear (less than 7.0%) while maintaining high catalytic activity, enhancing the efficiency and longevity of fixed bed hydrogenation processes.
Smart Images

Figure 0007564900000003 
Figure 0007564900000001 
Figure 0007564900000002
Abstract
Description
Related Applications
[0001] CROSS-REFERENCE TO RELATED APPLICATIONS
[0001] This application claims the benefit of the filing date of U.S. Provisional Application No. 62 / 425,262, filed November 22, 2016, entitled “METHOD FOR MANUFACTURING CATALYSTS WITH REDUCED ATTRITION,” the disclosure of which is incorporated herein by reference. [Technical field]
[0002]
[0002] The present invention relates to catalysts, and more particularly to a method for producing catalysts having reduced attrition. [Background technology]
[0003]
[0003] Hydrogenation catalysts based on highly porous nickel materials are well known. Such materials are part of a family of metal alloy derived products sold under the trade name "RANEY®" by W.R. Grace & Co.-Conn. When viewed under a microscope, these porous materials have a sponge-like appearance with pore channels winding throughout the nickel metal particles. Thus, such materials are generally viewed as porous or sponge metal alloy products.
[0004]
[0004] The porous catalyst may be formed by first forming a precursor alloy of nickel and aluminum using conventional metallurgical techniques. The formed alloy is then crushed and / or ground and screened by passing through a sieve to provide material having the desired size. Larger particles that exit the crushing or grinding mechanism can be recycled for further size reduction.
[0005]
[0005] The formed alloy is then subjected to an aqueous alkaline (e.g., sodium hydroxide) solution to partially extract the aluminum metal from the alloy. The porous catalyst can be formed according to the processes described in U.S. Patent Nos. 1,628,190, 1,915,473, 2,139,602, 2,461,396, and 2,977,327, the teachings of which are incorporated herein by reference in their entireties.
[0006]
[0006] By conventional means of partial Al removal ("leaching") of large granular alloys, fixed bed catalysts may be made with an activity that correlates with the degree of leaching. All other things being equal, these catalysts generally have higher attrition as the degree of leaching (Al removal) increases. This means that there is a limit to the activity that can be achieved without the penalty of excessive attrition. Fixed bed catalysts also tend to have high attrition values due to their relatively large size.
[0007]
[0007] Usually, alloys with higher Al content (lower Ni) are preferred for use in making fixed bed catalysts due to the lower cost of these alloys. Kelley et al. (U.S. Pat. No. 4,247,722) also utilizes a catalyst comprising an alkali-activated 42% nickel-58% aluminum alloy, where at least 98% by weight of the nickel in the alloy is present as NiAl3 for the hydrogenation of butadiene peroxide to 1,2- and 1,4-butanediol.
[0008]
[0008] Fixed bed catalysts for hydrogenation, in addition to serving the primary function of promoting the conversion of organic compounds to higher values, must withstand handling and exposure to mechanical forces during use. The rate of attrition, i.e., the loss of some of the larger particles as they break down into smaller ones, is important to users. Higher attrition can lead to lower value catalysts due to reduced flow (pressure drop) of the reactant / product streams, as well as problems downstream caused by fine particles flowing out of the reactor. Commercial users of these catalysts prefer to avoid this breakage during the loading of large column reactors of hydrogenation processes, because it prevents problems of flow restrictions ("pressure drop") and fine particle losses that could in turn shorten catalyst bed life or worsen net productivity. Summary of the Invention
[0009]
[0009] Thus, one example of the present invention is an inventive method for producing a catalyst using a higher Ni content alloy, i.e., an alloy significantly richer in Ni compared to the conventional 42% Ni. The inventive method includes providing an alloy granule containing aluminum and nickel, and treating the alloy granule with an alkaline solution to form a catalyst. The nickel content in the alloy granule may be in the range of about 43% to about 60% by weight. The alloy granule may have an effective diameter in the range of about 1 mm to about 10 mm.
[0010]
[0010] Another example of the present invention is a catalyst comprising nickel and aluminum with reduced attrition. The nickel content in the catalyst may be in the range of about 57% to about 75% by weight. The catalyst may have an effective diameter in the range of about 1 mm to about 10 mm, and an attrition value of less than about 7.0%. [Brief description of the drawings]
[0011]
[0011] The subject matter which is regarded as the invention is particularly pointed out and distinctly claimed in the claims at the conclusion of this specification. The foregoing and other objects, features, and advantages of the invention will become apparent from the following detailed description taken in conjunction with the accompanying drawings.
[0012] [Figure 1]
[0012] Alloy granules having different ranges of effective diameters are shown: (a) about 3.3 to about 7 mm, (b) about 2.4 to about 3.3 mm, and (c) about 1.7 to about 2.4 mm. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0013]
[0013] The present invention has been described with respect to the embodiments thereof.
[0014] The following terms used in the specification and appended claims have the following definitions.
[0014]
[0015] The term "fixed bed" refers to a mass of catalyst that is packed into a confined, static bed within a catalytic reactor and through which the reaction mixture moves continuously, as opposed to a stirred bed or fluidized bed (a "slurry" system) that is constantly moving within the reactor with the reaction mixture.
[0015]
[0016] One example of the present invention is a method for producing a catalyst using a higher Ni content alloy, i.e., an alloy significantly richer in Ni than the conventional 42% Ni. In one embodiment, the method includes providing an alloy granule comprising aluminum and nickel. The nickel content in the alloy granule may be in the range of about 43% to about 60% by weight, preferably about 45% to about 58% by weight, more preferably about 50% to about 56% by weight, and most preferably about 50% to about 53% by weight.
[0016]
[0017] In one embodiment, these alloy granules may be obtained by reducing the size of larger alloy granules by crushing and / or grinding, and then classifying to provide alloy granules with a desired size. Crushing the alloy typically results in a wide distribution of particle sizes, which is narrowed in a classification step, usually by sieving, by removing granules that are too large or too small. The larger particles that exit the crushing or grinding mechanism can be recycled for further size reduction. These alloy granules may have irregular shapes. The term "effective diameter" of the granules formed by the crushing and / or grinding method refers to the size of a square opening in a standard sieve (US or Tyler notation) with the largest mesh number through which the granules can pass. The granules have a distribution of effective diameters, the range of which is determined by classifying through a sieving step. Specifically, the granules are first sieved and passed through a standard sieve with a lower mesh number. The passed granules are then sieved while being retained by a standard sieve with a higher mesh number. The effective diameter range of the retained granules is determined as the size of the higher mesh standard sieve to the size of the lower mesh standard sieve.
[0017]
[0018] In another embodiment, alloy granules of the desired size may be obtained by casting the molten alloy into a mold, pelletizing, or forming droplets directly from the molten alloy in a cooling medium (gas or liquid). The casting and pelletizing methods can produce uniform alloy granules with a cylindrical shape. The term "effective diameter" of a granule with a cylindrical shape refers to the diameter of the cross section (circular) of a cylinder. In one embodiment, spherical alloy granules may be formed by a "shot" of the molten alloy through rapid cooling. The term "effective diameter" of a granule with a spherical shape refers to the diameter of a sphere.
[0018]
[0019] In one embodiment, the alloy granules may have an effective diameter within the range of about 1 mm to about 10 mm, preferably about 2 mm to about 6 mm, and more preferably about 2.5 mm to about 5 mm. In another embodiment, the overall range of granule sizes may extend from an upper limit of the sieve designation of about "4" (about 4.75 mm openings), which allows all of the utilized granules to pass through, to a lower limit of about "12" (about 1.7 mm openings), which does not allow substantially all of the utilized granules to pass through. In other words, the alloy granules have an effective diameter within the range of about 1.7 mm to about 4.75 mm. In another embodiment, the utilized granules may be within a range of effective diameters that is a subset of this widest overall range, for example, from an alloy designated as the "8-12 mesh" range, which has substantially all of the particles smaller than an 8 mesh (about 2.4 mm) square opening and larger than a 12 mesh (about 1.7 mm) opening. In other words, the alloy granules have an effective diameter within the range of about 1.7 mm to about 2.4 mm. In another embodiment, the granules utilized may be derived from alloy granules designated as the "4-8 mesh" range, having substantially all of the particles smaller than a 4 mesh (about 4.75 mm) square opening and larger than an 8 mesh (about 2.4 mm) opening. In other words, the alloy granules have an effective diameter within the range of about 2.4 mm to about 4.75 mm.
[0019]
[0020] The alloy granules may then be treated or activated with an alkaline solution to form the catalyst. During activation, aluminum may be partially leached from the alloy granules by the alkaline solution to the extent that at least 20%, preferably at least 30%, and more preferably at least 40% of the aluminum (Al) originally present is leached. The upper limit of the Al leaching range will vary for the particular use of the catalyst and depends on the balance of competing goals, i.e., higher activity (requiring higher leaching) versus minimized attrition. The alkaline solution may be derived from either inorganic or organic compounds. In one embodiment, the alkaline solution includes sodium hydroxide. The concentration of sodium hydroxide in the alkaline solution may be in the range of 1% to 20% by weight, preferably 1% to 15% by weight, and more preferably 1% to 10% by weight. The alloy granules may be treated with the alkaline solution at a temperature in the range of about 20°C to about 110°C, preferably about 30°C to about 90°C, and more preferably about 40°C to about 70°C.
[0020]
[0021] The process of treating the alloy granules with an alkaline solution is not limited. In one embodiment, the alloy granules being treated for fixed bed catalyst may be in a vessel into which the alkaline solution is pumped and / or recirculated. The aluminum contained in the alloy dissolves to form alkali metal aluminates (e.g., sodium aluminate) with vigorous evolution of hydrogen. The granules and the alkaline solution are typically kept in contact with each other at elevated temperatures (e.g., 40°C to 60°C) for up to several hours until the aluminum content is reduced to the desired level.
[0021]
[0022] The alkaline solution may be introduced as a single solution, as a series of solutions of increasing strength over time, or alternatively as solutions whose strength varies continuously over time by adding excess NaOH to an existing reservoir that contained the original weakest solution. In one embodiment, the alloy granules may be treated with a 3-10 wt. % excess NaOH solution that is continuously circulated through a bed of alloy granules while maintaining a temperature of 40-60°C.
[0022]
[0023] In another embodiment, the alloy granules are first treated with a low concentration, such as a 3-4 wt% NaOH solution, for about 10-20 minutes. Additional sodium hydroxide can then be slowly added to the solution to increase the concentration of the NaOH solution, for example, to 6-8 wt% over a period of 20-30 minutes. Finally, the alloy granules are treated with the increased concentration NaOH solution for another 20-30 minutes.
[0023]
[0024] After a specified time, the activation process is interrupted. The activated catalyst may be separated from the reaction solution and then washed with water until the wash water has a slightly alkaline pH value of about 8-9. The pore volume, pore size, and surface area of the catalyst depend on the amount of aluminum in the initial alloy and the degree of leaching.
[0024]
[0025] The method of making the catalyst may further include a step of promoting the catalyst. The catalyst may be promoted with about 0.1 wt. % to about 15 wt. % of a promoter transition metal, depending on the particular promoter metal. Such transition metals may include those that can promote the hydrogenation performance of the nickel catalyst, such as selectivity, conversion, and stability against deactivation. In one embodiment, the catalyst preferably has a promoter transition metal content in the range of about 0.1 to about 10 wt. %, preferably about 0.5 to about 5.0 wt. %.
[0025]
[0026] The promoter transition metal may be added to the catalyst as a component in the nickel and aluminum base alloy, but may also be added in the leach solution used to remove the aluminum from the nickel aluminum alloy, or in the impregnation or coating bath after activation. In one embodiment, if added via the leach solution, it may contain an amount of promoter precursor, such as chromium chloride or other Cr compound, in a metal:catalyst ratio of about 0.2-2% by weight, preferably 0.5-1.5% by weight. In one embodiment, the catalyst may be promoted by treating it with a solution containing a soluble salt of a metal selected from the group consisting of Mo, Cr, W, Cu, and Fe, or mixtures thereof. In one embodiment, alkylheptamolybdate tetrahydrate (NH4)6Mo7O 24~4 H 20 The catalyst may be promoted with Mo using a soluble Mo salt such as MoCl4, MoO2, MoCl5, MoCl6, MoCl ...
[0026]
[0027] If the option of applying a promoter to the surface of the catalyst after activation is adopted, surface deposition may be performed during a post-activation wash step in which the catalyst is contacted with a (usually alkaline pH) salt solution to achieve the same approximate range of promoters mentioned above. This surface deposition may be performed at a selected pH, for example in the range of 8-12, preferably 9-11. The catalyst is stored in water at an alkaline pH, typically 9-11. In another post-leaching process, metals may be plated onto the catalyst utilizing coating or plating techniques described in U.S. Pat. No. 7,375,053, the contents of which are incorporated herein by reference.
[0027]
[0028] In one embodiment, the nickel content in the catalyst may be in the range of about 57% to about 75% by weight, preferably about 60% to about 70% by weight. In another embodiment, the catalyst may have an attrition value of less than about 7.0%, preferably less than about 5.0%, and more preferably less than about 3.0%.
[0028]
[0029] By using a higher Ni-containing Ni-Ai alloy, i.e., significantly richer than the conventional 42% Ni, the formed catalyst may be significantly less prone to attrition, i.e., the breakage of larger particles into smaller particles during handling and use. Without being bound to a particular theory, it is believed that compared to making catalysts by leaching conventional low Ni alloys, leaching from a more Ni-rich alloy may result in less disruption of the original structure and less internal restructuring of the alloy particles, thereby reducing their inherent vulnerability to impact, i.e., improving attrition resistance.
[0029]
[0030] Another example of the present invention is a catalyst formed by the method of the present invention, which includes treating a granular alloy having a high nickel content with an alkaline solution. The catalyst may be used partially or entirely as a fixed-bed sponge metal catalyst for hydrogenation processes. The catalyst may also be used in processes for hydrogenation, such as specifically a process for producing 1,4 butanediol by hydrogenation, or a process for producing sorbitol by hydrogenation of glucose.
[0030]
[0031] The catalyst can be utilized more efficiently in continuous processes, including those using fixed catalyst beds. Trickle bed processes can be used in conjunction with fixed catalyst beds. The catalysts utilized in conventional fixed bed processes can be in a variety of forms, including, but not limited to, granules, spheres, pressed cylinders, tablets, lozenges, wagon wheels, rings, stars, or extrudates such as solid extrudates, multi-lobe extrudates, hollow extrudates, and honeycomb bodies.
[0031]
[0032] The present invention will be described in more detail below with reference to examples, although the scope of the present invention is not limited to the following examples. EXAMPLES
[0032]
[0033] The methods for alloy formation and sizing, catalytic attrition testing, and catalytic activity testing are described first and apply uniformly to all subsequent examples.
[0033] Alloy particle formation and size determination
[0034] A nickel-aluminum alloy slab was formed by conventional melting and casting methods as described above. The cast alloy slab was then crushed into smaller granules (using a jaw crusher from Bico-Braun Intl. with about 1 / 4 jaw opening setting). The granules (particles) at this stage have an excessively broad distribution. In the subsequent sieving step, the granules are first sieved through a standard sieve with a lower mesh number. The passed granules are then sieved while being retained by a standard sieve with a higher mesh number. The effective diameter range of the retained granules is determined as the size of the standard sieve with the higher mesh number to the size of the standard sieve with the lower mesh number. Figure 1 shows alloy granules with different effective diameter ranges: (a) about 3.3 to about 7 mm, (b) about 2.4 to about 3.3 mm, and (c) about 1.7 to about 2.4 mm. These alloy granules were classified through standard sieves of (a) 3-6 mesh, (b) 6-8 mesh, and (c) 8-12 mesh, respectively.
[0034]
[0035] In the subsequent examples and comparative examples, alloy granules (c) were used, which passed through a standard 8 mesh sieve but were retained (did not pass) by a 12 mesh sieve just below the 8 mesh sieve after treatment in a sieve shaker (Rotap®) for 1 minute.
[0035]
[0036] The relationship between sieve designations and nominal sieve openings is shown in Table 1 below, which is taken from the Aldrich 2003-2004 Catalog / Handbook of Fine Chemicals.
[0036]
[0037]
[0037] [Table 1]
[0038] Attrition testing of activated catalysts
[0038] The tendency of catalysts to break down into smaller particles under mechanical stress was measured with a simple roller mill apparatus consisting of a capped polyethylene bottle ("16 oz. Poly Jar with Baffles, FAB," available from Fisher Scientific) inside a cylindrical metal "mill jar" sleeve (part 000-264 from Advanced Ceramics Manufacturing) rotated at 100 RPM on the roller pair of a Paul O. Abbe, Inc. "Model JRM," a machine typically used as a ball mill. A 100 g catalyst sample was immersed in water in the capped bottle in each test. The residence time in this attrition test was 20 minutes. The amount of fines in the catalyst sample was determined by weighing both before and after the 20 minute roller mill process. Fine debris was separated from the main sample using a standard 12 mesh sieve that was mechanically shaken for 2 minutes on a Rotap® shaker. The fines separated by sieving before the attrition test were remixed with the main sample before continuing with the roller mill test and the second sieving. The attrition for each test was defined as the difference between the weighed fines content before and after, the fraction of catalyst passing through a 12 mesh sieve (approximately 1.7 mm openings) expressed as a percentage of the original sample weight.
[0039] Wear % = [% under 12 mesh after test] - [% under 12 mesh before test] Catalytic activity test
[0039] The catalytic activity was measured in a fixed-bed hydrogenation reactor using the conversion of dextrose (glucose) solution to sorbitol as the performance measure.
[0040]
[0040] A vertical column fixed bed reactor was used with an internal diameter of 1 / 2 inch and a working bed length of 6 inches, with a central 1 / 8 inch diameter thermocouple well. The working volume of the catalyst bed was 18 cc (mL). The catalyst was loaded into the column reactor in water and, after connecting the modular catalyst bed section to the main reactor piping system, was subsequently pushed out of the catalyst bed area by flowing nitrogen and then hydrogen.
[0041]
[0041] A 40% aqueous solution of crystalline dextrose in water was pumped from an external feed tank into the fixed bed reactor maintained at 120° C. Simultaneously, hydrogen gas was delivered through the catalyst bed at a flow rate of 500 mL / min and 1000 psig pressure (68 atm). The liquid flow rate was maintained continuously in multiple experimental runs at three different levels: 0.20, 0.23, and 0.25 mL / min. This is a means of distinguishing between catalysts of similar activity based on their ability to enhance the conversion of the feed to product at the highest possible flow rate.
[0042]
[0042] Product samples were collected over each 4 hour run period. Residual dextrose (unconverted feed) was determined by analysis with a "Hemocue Glucose 201 Analyzer" available from Fisher Scientific. Product samples were diluted with water to allow detection in the optimal instrument response range of the provided colorimetric slide. This provides the weight percent of dextrose in the product sample.
[0043]
[0043] The percent conversion of dextrose was defined as: 100%-2.5 * (dextrose weight %) where dextrose wt% is the residual amount in the product as determined above and the factor of 2.5 accounts for the 40% feed concentration. The conversion values obtained above were averaged for three segments of 4 hours each at a given liquid feed flow rate.
[0044]
[0044] HPLC analysis of product samples was performed separately to confirm the accuracy of the Hemocue instrument for dextrose content. The conditions used for the HPLC were: Rezex RCM Monosaccharide Ca+2 column (serial number 735463-1) with dimensions 300 x 7.8 mm, Rezex RCM Monosaccharide Ca+2 column guard (serial number 728606-3) with dimensions 50 x 7.8 mm, flow rate 0.7 mL / min, deionized water for effluent, gradient: isocratic, 10 μL injection, RI detector, run time 35 min.
[0045]
[0045] The main by-product, mannitol, was found to be in the range of 0.4–0.7 wt % for all subsequent experimental catalysts.
[0046] Comparative Example 1
[0046] catalyst activation
[0047] A 42%Ni-58%Al alloy produced by conventional melting and mixing techniques was crushed and sieved to the 8-12 mesh size range (approximately 2-3 mm particle size). To activate this alloy into a catalyst by Al leaching, 680 g of this 8-12 mesh alloy was placed into a 4 liter beaker, and then 8.1 liters of 3% aqueous NaOH solution was recycled using a pump between the beaker and an external reservoir holding the excess NaOH solution. This first condition (stage 1) was continued for 10 minutes, maintaining the temperature in the leaching beaker at 45°C by using a cooling coil in the beaker. For the next 20 minutes (stage 2), a solution containing an additional 288 g (pure solid) NaOH and 462 g water was steadily and continuously added to the reservoir to eventually increase the NaOH input from the initial 3% concentration to the equivalent of the initial 6% NaOH (i.e., ignoring the amount consumed by the Al leaching reaction). After the NaOH addition, the system was held at the same temperature and liquid flow conditions for 20 minutes (Step 3).
[0047]
[0048] The catalyst was then washed with 5 liters of 2% NaOH solution for 10 minutes, followed by water at 45°C until the effluent wash water reached a tentative pH of 10. Molybdenum promoter was added to the catalyst using 20.5 g of ammonium heptamolybdate (NH4)6Mo7O24-4H2O in 70 g of water. The MO-containing solution was then stirred to distribute through the catalyst bed for 60 minutes. The catalyst was then further washed with water to bring the pH to 9.
[0048]
[0049] The final composition of the catalyst, as determined by ICP chemical analysis, was 54.9% Ni, 43.3% Al and 1.6% Mo, corresponding to a leaching (removal) of 43% of the initial aluminum in the alloy.
[0049]
[0050] The catalyst of Comparative Example 1 had an attrition rate of 10.2%, which represents the baseline range of fracture for conventional catalysts. The % dextrose conversion for this catalyst at the three programmed feed flow rates was: 99.9% conversion at a flow rate of 0.20 mL / min 99.9% conversion at a flow rate of 0.23 mL / min There was a 99.3% conversion at a flow rate of 0.25 mL / min.
[0050]
[0051] The combination of high activity but with excess breakage (approximately 10%) represents an improvement over existing catalysts.
[0051] Comparative Example 2
[0052] A catalyst was prepared from a 58% Al, 42% Ni alloy in a manner similar to that of Comparative Example 1 above, with these differences:
[0052] a) The NaOH added in stage 2 amounted to 465 g solid NaOH dissolved in 285 g water, increasing the total NaOH input to the equivalent of a starting concentration of 8% (vs. 6% in Comparative Example 1).
[0053] b) After the 20 minute addition time in step 2, the mixture was held with the liquid circulating for 10 minutes, a shorter duration than the 20 minutes in Comparative Example 1.
[0053] Catalyst analysis obtained by ICP showed 49.8% Ni, 49.0% Al, and 1.1% Mo, corresponding to leaching of only 29% of the initial Al versus 45% for Comparative Example 1. Attrition levels from the method described above were only an 8.6% improvement over the 10.2% baseline.
[0054]
[0054] The % dextrose conversion for the catalyst of Comparative Example 2 is: 99.5% conversion at a flow rate of 0.20 mL / min, 96.5% conversion at a flow rate of 0.23 mL / min. There was a 96.3% conversion at a flow rate of 0.25 mL / min.
[0055]
[0055] Although both activity and wear were reduced as a result of the lower levels of Al leaching compared to the baseline of Comparative Example 1, this tradeoff is still undesirable in that activity was significantly affected without significantly improving wear.
[0056] Example 1
[0056] The catalyst was prepared by a process similar to that of Comparative Example 1, but with modifications and details as described below.
[0057] a) Derived from an alloy having 53% Ni and 47% Al. The alloy weight used was 500 g. b) The initial 3% leach solution had a volume of approximately 6 liters.
[0058] c) The timing of steps 1, 2, and 3 were 10 minutes, 20 minutes, and 20 minutes, respectively, as in Comparative Example 1. The temperature was 45° C., as in Comparative Examples 1 and 2. d) The amount of NaOH used to increase the input concentration to approximately 6% equivalent in step 2 was 212 g solid NaOH dissolved in 340 g water.
[0059] e) Molybdate addition: 15.1 g ammonium heptamolybdate.
[0057] The resulting catalyst had the following content by ICP analysis: 68.5% Ni, 28.8% Al, and 1.6% Mo, corresponding to 53% Al removal. Attrition testing showed much lower results at 2.7%, about a quarter of the baseline Comparative Example 1.
[0060]
[0058] The activity test of the catalyst of Example 1 showed that 96.4% conversion at a flow rate of 0.20 mL / min. 93.6% conversion at a flow rate of 0.23 mL / min. A flow rate of 0.25 mL / min gave a conversion of 95.4%.
[0061] Example 2
[0059] Compared to Example 1, the changes made in this catalyst preparation were as follows:
[0062] a) The activation temperature was increased from 45°C and maintained at 60°C. b) In stage 2, the input % of NaOH was increased from the initial 3% to 8% by adding a mixture of 342 g solid NaOH and 209 g water.
[0063] c) The durations of stages 1, 2, and 3 were 10, 12, and 17 minutes, respectively. d) At the end of stage 3, the spent leach solution was removed from the reactor + reservoir and replaced with 6.5 litres of 10% NaOH solution which was recirculated through the catalyst bed at 60°C for a further 12 minutes.
[0064]
[0060] Catalyst analysis obtained by ICP gave 65.4% Ni, 32.5% Al, and 1.5% Mo. This represents a leaching of 44% of the original Al. Attrition testing showed an improvement of 2.6% compared to Comparative Example 1.
[0065]
[0061] The activity test of the catalyst of Example 2 showed that 99.4% conversion at a flow rate of 0.20 mL / min 99.0% conversion at a flow rate of 0.23 mL / min. A flow rate of 0.25 mL / min gave a conversion of 98.8%.
[0066] Example 3
[0062] This catalyst preparation included only one change from Example 2, namely the substitution of a 50% Ni, 50% Al alloy for the 53% Ni, 47% Al alloy.
[0067]
[0063] Catalyst analysis obtained by ICP gave 61.1% Ni, 37.2% Al, and 1.4% Mo. This represents a leaching of 39% of the original Al.
[0068]
[0064] The selective removal of 39% of the original aluminum reduces the weight of the alloy overall by 0.391 x 50% or 19.56% (i.e., 19.56 g out of 100 g, for example). The addition of Mo promoter increases the weight by 1.15 g per 100 g of original alloy. Normalizing the catalyst quantification is equivalent to dividing the weight of each component by 1.15 + (100 - 19.44), or 81.71, of the new total catalyst weight.
[0069] Therefore, the final Al% is (100%) * (50-19.44) / 81.71=37.3%. Final Ni% is (100%) * 50 / 81.71=61.2%. And Final Mo% is (100%) * 1.15 / 81.71=1.4%.
[0070]
[0065] Abrasion testing showed results of 5.4% or approximately half the prior art baseline of Comparative Example 1.
[0071]
[0066] The activity test of the catalyst of Example 3 showed that 99.8% conversion at a flow rate of 0.20 mL / min 99.5% conversion at a flow rate of 0.23 mL / min A flow rate of 0.25 mL / min gave a conversion of 99.6%.
[0072]
[0067] Examples 2 and 3 achieved the best balance of high activity (dextrose conversion) and low attrition.
[0073] The complete results are shown in Table 2 below.
[0074] [Table 2]
[0075] [Mode of the invention] [1] A method for producing a catalyst, comprising the steps of: Providing alloy granules comprising aluminum and nickel; and treating the alloy granules with an alkaline solution to form the catalyst. The content of the nickel in the alloy granules is in the range of 43% by weight to 60% by weight. How to do it. [2] 1. The alloy granules have an effective diameter in the range of 1 mm to 10 mm. How to. [3] The content of the nickel in the alloy granules is within a range of 45% by weight to 58% by weight. 2. The method according to claim 1. [4] The content of the nickel in the alloy granules is within a range of 50% by weight to 56% by weight. 2. The method according to claim 1. [5] The content of the nickel in the alloy granules is within a range of 50% by weight to 53% by weight. 2. The method according to claim 1. [6] 1. The alloy granules according to claim 1, wherein the alloy granules have an effective diameter in the range of 2 mm to 6 mm. method. [7] 2. The method of claim 1, wherein the alkaline solution comprises sodium hydroxide. [8] The concentration of the sodium hydroxide in the alkaline solution is within the range of 1% by weight to 20% by weight. 8. The method according to claim 7, [9] The concentration of the sodium hydroxide in the alkaline solution is within the range of 1% by weight to 15% by weight. 8. The method according to claim 7,
[10] The concentration of the sodium hydroxide in the alkaline solution is within the range of 1% by weight to 10% by weight. 8. The method according to claim 7,
[11] The alloy granules are treated with the alkaline solution at a temperature in the range of 20°C to 110°C. 2. The method according to claim 1.
[12] a. Mo, Cr, W, Cu, and Fe, or a mixture thereof; treating the catalyst with a solution containing a soluble salt of the metal to be treated; or b. Mo, Cr, W, Cu, and Fe, or a mixture thereof. and forming said alloy granules using an additional process step selected from: 2. The method of claim 1, further comprising promoting the catalyst.
[13] The content of the nickel in the catalyst is within a range of 57% by weight to 75% by weight. 1. The method according to claim 1.
[14] The content of the nickel in the catalyst is within a range of 60% by weight to 70% by weight. 1. The method according to claim 1.
[15] 2. The method of claim 1, wherein the catalyst has an attrition value of less than 7.0%.
[16] 2. The method of claim 1, wherein the catalyst has an attrition value of less than 5.0%.
[17] 2. The method of claim 1, wherein the catalyst has an attrition value of less than 3.0%.
[18] 1. A catalyst formed by the method according to claim 1.
[19] Catalyst formed by the method according to claim 2.
[20] 19. A fixed bed sponge metal catalyst comprising the catalyst according to 18 for a hydrogenation process. [twenty one] 20. A fixed bed sponge metal catalyst comprising the catalyst according to 19 for a hydrogenation process. [twenty two] 19. A process for hydrogenation using the catalyst according to 19. [twenty three] 19 to produce 1,4 butanediol by hydrogenation using the catalyst described in process. [twenty four] 19. A process for producing sorbitol by hydrogenation using a catalyst as described in vinegar.
Claims
1. A hydrogenation catalyst, the nickel content in said catalyst being between 65.4% and 68.5% by weight, said catalyst having an attrition value of less than 5.0%, The aluminum content in the catalyst is 28.8 to 32.5 wt. %, and the catalyst has pores resulting from leaching of 44 to 53 wt. % of the aluminum from a nickel-aluminum alloy containing 53 wt. % nickel and 47 wt. % aluminum. Hydrogenation catalyst.
2. A fixed bed sponge metal catalyst comprising the hydrogenation catalyst of claim 1.
3. A process for hydrogenation using the hydrogenation catalyst of claim 1.
4. A process for producing 1,4 butanediol by hydrogenation using the hydrogenation catalyst of claim 1.
5. 2. A process for producing sorbitol by hydrogenation using the hydrogenation catalyst of claim 1.
Citation Information
Patent Citations
Method for removing trace aldehydes by alcohol hydrogenation
CN104945226A
JP1974034964A
Material composition useful for raney catalyst for hydrogenating halonitroaromatic compound into haloaminoaromatic compound and its application
JP1995165682A
Preparation of substituted amines by hydrogenation of substituted organic nitro compounds
JP2004517137A
Method for producing alcohol by hydrogenation of carbonyl compounds
JP2004526686A