Pressure Sensitive Adhesive Tape
The pressure-sensitive adhesive tape with a specific resin and monomer composition shrinks after UV exposure, addressing the issue of adhesive residue and ensuring easy removal, thus enhancing its applicability in cutting processes.
Patent Information
- Application Number
- JP2023033562
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2022-11-28
- Filing Date
- 2023-03-06
- Publication Date
- 2024-10-09
- Estimated Expiration
- 2043-03-06
AI Technical Summary
Conventional pressure-sensitive adhesive tapes used in component cutting processes face issues with insufficient adhesive strength between the tape and the substrate, leading to difficulty in peeling off the tape and adhesive residue after exposure to ultraviolet light, limiting their application in cutting processes.
A pressure-sensitive adhesive tape comprising a release layer, an adhesive layer with a specific composition of 40% to 50% acrylic resin, 40% to 65% epoxy monomer, 0.05% to 0.5% curing agent, and 0.5% to 1.0% initiator, and a support layer, which shrinks after exposure to ultraviolet light, reducing adhesive strength and facilitating easy removal.
The adhesive tape achieves high initial adhesive strength for secure bonding during cutting and minimal adhesive residue after exposure to UV light, enabling effective use in cutting processes without leaving behind adhesive on the substrate.
Smart Images

Figure 0007564905000007 
Figure 0007564905000008 
Figure 0007564905000009
Abstract
Description
[Technical field]
[0001] The present invention relates to a tape, and more particularly to a pressure sensitive adhesive tape for use in part cutting processes. [Background technology]
[0002] In the prior art, pressure-sensitive adhesive tapes used in the cutting process of parts usually have an ultraviolet adhesive layer. The ultraviolet adhesive layer often uses only acrylic resin. However, the adhesive strength between the conventional pressure-sensitive adhesive tape and the substrate to be cut is insufficient. After exposure to ultraviolet light, the adhesive strength between the pressure-sensitive adhesive tape and the substrate to be cut is too high, making it difficult to peel the pressure-sensitive adhesive tape from the substrate to be cut, resulting in adhesive residue. Therefore, conventional pressure-sensitive adhesive tapes cannot be applied to various cutting processes of parts and are not widely used.
[0003] Therefore, in view of the fact that the above-mentioned problems can be improved, the inventors have conducted intensive research and applied scientific theory, resulting in the present invention as a method that is rational in design and can effectively improve the above-mentioned problems, thereby providing a pressure-sensitive adhesive tape that can be applied to the cutting processes of various parts. Summary of the Invention [Problem to be solved by the invention]
[0004] The technical problem to be solved by the present invention is to provide a pressure-sensitive adhesive tape suitable for cutting process of parts in response to the shortcomings of the prior art. [Means for solving the problem]
[0005] In order to solve the above technical problems, one technical means adopted by the present invention provides a pressure-sensitive adhesive tape applied to a cutting process of parts. The pressure-sensitive adhesive tape includes a release layer, an adhesive layer formed on one side of the release layer, and a support layer formed on the side of the adhesive layer away from the release layer, and the adhesive layer includes 40% to 50% by weight of an acrylic resin, 40% to 65% by weight of an epoxy monomer, 0.05% to 0.5% by weight of a curing agent, and 0.5% to 1.0% by weight of an initiator, with the total weight of the adhesive layer being 100% by weight, the adhesive layer has a first acid value before being exposed to ultraviolet light, and the adhesive layer shrinks and has a second acid value after being exposed to ultraviolet light, and the second acid value is smaller than the first acid value.
[0006] Preferably, the first acid value of the adhesive layer before exposure to the ultraviolet light is 5 mgKOH / g to 20 mgKOH / g, and the second acid value of the adhesive layer after exposure to the ultraviolet light is 1 mgKOH / g to 4 mgKOH / g.
[0007] Preferably, the first acid value of the adhesive layer before exposure to the ultraviolet light is 10 mgKOH / g to 15 mgKOH / g, and the second acid value of the adhesive layer after exposure to the ultraviolet light is 1 mgKOH / g to 3 mgKOH / g.
[0008] Preferably, the release layer has a first thickness of 25 μm to 45 μm, the adhesive layer has a second thickness of 3 μm to 30 μm, and the support layer has a third thickness of 50 μm to 180 μm, the release layer being mainly composed of a polyester material and the support layer being mainly composed of a polyolefin material.
[0009] Preferably, the epoxy monomer in the adhesive layer is a reactive epoxy monomer and has the following chemical structure: [ka]
[0010] Preferably, in the adhesive layer, the hardener is an isocyanate hardener and the initiator is a photoinitiator.
[0011] Preferably, the ultraviolet light has a wavelength of 300 nm to 380 nm, and the ultraviolet light exposure energy for the adhesive layer is 100 mJ / cm. 2 ~300mJ / cm 2 It is.
[0012] Preferably, in the cutting process of the part, the release layer is peeled off first, and the adhesive layer is bonded to a cutting substrate, the cutting substrate being a printed circuit board, a ceramic substrate, a glass substrate, or a wafer, and before the adhesive layer is exposed to the ultraviolet light, a first peel force between the adhesive layer and the cutting substrate is 10 N / inch or more.
[0013] Preferably, after the adhesive layer is exposed to the ultraviolet light, the epoxy monomer in the adhesive layer undergoes a crosslinking reaction, and the adhesive layer is formed as an exposed adhesive layer, and the second peel force between the exposed adhesive layer and the cutting substrate is 0.2 N / inch or less.
[0014] Preferably, after the crosslinking reaction of the epoxy monomer occurs, the adhesive layer shrinks to reduce the contact area between the exposed adhesive layer and the cutting substrate. Effect of the Invention
[0015] As an advantageous effect of the present invention, the pressure-sensitive adhesive tape of the present invention has the following technical features: "the adhesive layer comprises 40% by weight to 50% by weight of acrylic resin, 40% by weight to 65% by weight of epoxy monomer, 0.05% by weight to 0.5% by weight of curing agent, and 0.5% by weight to 1.0% by weight of initiator, with the total weight of the adhesive layer being 100% by weight" and "the adhesive layer has a first acid value before being exposed to ultraviolet light, and the adhesive layer shrinks and has a second acid value after being exposed to ultraviolet light, and the second acid value is smaller than the first acid value", which improves the adhesive strength between the adhesive layer and the cutting substrate and prevents adhesive residue after removal. [Brief description of the drawings]
[0016] [Figure 1] 1 is a schematic diagram of a pressure-sensitive adhesive tape according to an embodiment of the present invention. [Figure 2A] 1 is a schematic diagram showing steps S110 to S160 of a method for using a pressure-sensitive adhesive tape according to an embodiment of the present invention. [Figure 2B] 1 is a schematic diagram showing steps S110 to S160 of a method for using a pressure-sensitive adhesive tape according to an embodiment of the present invention. [Figure 2C] 1 is a schematic diagram showing steps S110 to S160 of a method for using a pressure-sensitive adhesive tape according to an embodiment of the present invention. [Figure 2D] 1 is a schematic diagram showing steps S110 to S160 of a method for using a pressure-sensitive adhesive tape according to an embodiment of the present invention. [Figure 2E] 1 is a schematic diagram showing steps S110 to S160 of a method for using a pressure-sensitive adhesive tape according to an embodiment of the present invention. [Figure 2F] 1 is a schematic diagram showing steps S110 to S160 of a method for using a pressure-sensitive adhesive tape according to an embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0017] In order to better understand the features and technical contents of the present invention, please refer to the following detailed description of the present invention and the accompanying drawings, which are provided for reference and explanation only and are not intended to limit the scope of the present invention.
[0018] Hereinafter, the embodiments of the present invention will be described in accordance with certain specific embodiments, and those skilled in the art can understand the advantages and effects of the present invention based on the contents disclosed in this specification. The present invention can be implemented or applied in other different specific embodiments, and various modifications and changes can be made to each detail in this specification based on different perspectives and applications without departing from the concept of the present invention. In addition, as described in advance, the accompanying drawings of the present invention are simple schematic illustrations and are not drawn based on actual size. The technical contents of the present invention will be described in more detail based on the following embodiments, but the disclosed contents do not limit the protection scope of the present invention.
[0019] It should be understood that, although the present specification may use the terms "first", "second", "third" and the like to describe various elements or symbols, these elements or symbols are not limited by these terms. These terms are mainly used to distinguish one element from another element or one symbol from another symbol. In addition, the term "or" used in the present specification may include any one or more combinations of the associated listed items according to actual circumstances.
[0020] [Pressure-sensitive adhesive tape used in the part cutting process] As shown in FIG. 1, an embodiment of the present invention provides a pressure-sensitive adhesive tape 100, in particular a pressure-sensitive adhesive tape applied to a cutting process of a component. For example, the pressure-sensitive adhesive tape according to an embodiment of the present invention is applied to a cutting process of a semiconductor wafer or a cutting process of a packaged element, but the present invention is not limited thereto. In addition, in the cutting process, the substrate to be cut to which the pressure-sensitive adhesive tape is attached may be, for example, a printed circuit board, a ceramic substrate, a glass substrate, or a wafer (e.g., a substrate used as a carrier in an integrated circuit process).
[0021] As shown in FIG. 1, the pressure-sensitive adhesive tape 100 according to the embodiment of the present invention comprises a release layer 1, an adhesive layer 2, and a support layer 3, which are laminated from top to bottom. In other words, the adhesive layer 2 is formed on one side of the release layer 1 (for example, the lower surface of the release layer 1 in FIG. 1). The support layer 3 is formed on the side of the adhesive layer 2 that is away from the release layer 1 (for example, the lower surface of the adhesive layer 2 in FIG. 1), but the present invention is not limited thereto. In practical application, the installation direction of the pressure-sensitive adhesive tape 100 may be changed as necessary. For example, the support layer 3 may be the top layer, the release layer 1 may be the bottom layer, and the adhesive layer 2 may be between the support layer 3 and the release layer 1.
[0022] In order to facilitate understanding of the present invention, other material properties of each layer in the pressure-sensitive adhesive tape 100 according to an embodiment of the present invention will be described below, and the connection relationship of each layer will be properly described.
[0023] The release layer 1 is peeled off from the adhesive layer 2 so that the adhesive layer is exposed when a cutting process of a part is performed. Regarding the thickness, the first thickness D1 of the release layer 1 is 25 μm to 45 μm, preferably 28 μm to 40 μm, and particularly preferably 30 μm to 38 μm, but the present invention is not limited thereto. The release layer 1 may be, for example, a polyester release layer (for example, a PET release film). In one embodiment of the present invention, the polyester release layer can achieve the effect of release by reducing the adhesive force of the polyester film surface by applying silicone oil to the surface of the polyester film or adding an inorganic material to the polyester film.
[0024] The adhesive layer 2 can be attached to the back surface of a substrate to be cut during a cutting process of a part. The solid content of the adhesive layer 2 includes an acrylic resin, an epoxy monomer, a hardener, and a photoinitiator.
[0025] With the total weight of the adhesive layer 2 being 100 weight % (wt%), the acrylic resin is 40 wt % to 50 wt %, the epoxy monomer is 40 wt % to 65 wt %, the curing agent is 0.05 wt % to 0.5 wt %, and the initiator is 0.5 wt % to 1.0 wt %.
[0026] Among them, the acrylic resin may be, for example, poly(methyl methacrylate) (PMMA) having a chemical structure represented by the following formula (I), in which n=3,000 to 5,000.
[0027] [ka] Formula (I)
[0028] Among them, the epoxy monomer is a reactive epoxy monomer for improving the adhesion of the adhesive layer 2, and the epoxy monomer undergoes a crosslinking reaction after being irradiated with ultraviolet light, thereby shrinking the adhesive layer 2 and reducing the adhesion of the adhesive layer 2. Among them, the epoxy monomer has a chemical structure represented by the following formula (II), but the present invention is not limited thereto.
[0029] [ka] Formula (II)
[0030] The curing agent increases the degree of polymerization of the acrylic resin in the adhesive layer 2, thereby increasing the molecular weight of the acrylic resin. The curing agent is an isocyanate curing agent. The isocyanate curing agent may be, for example, at least one of an aliphatic diisocyanate, an alicyclic diisocyanate, and an aromatic diisocyanate.
[0031] In some embodiments of the present invention, the aliphatic diisocyanate may be at least one selected from the group consisting of tetramethylene diisocyanate, hexamethylene diisocyanate, decamethylene diisocyanate, and lysine diisocyanate. The alicyclic diisocyanate may be at least one selected from the group consisting of isophorone diisocyanate, hydrogenated toluene diisocyanate, hydrogenated xylene diisocyanate, dicyclohexylmethane diisocyanate, and tetramethylxylene diisocyanate.
[0032] Examples of the aromatic diisocyanate include 2,4-tolylene diisocyanate, 2,6-tolylene diisocyanate, xylene-1,4-diisocyanate, xylene-1,3-diisocyanate, 4,4'-diphenylmethane diisocyanate, 2,4'-diphenylmethane diisocyanate, 4,4'-diphenylether diisocyanate, 2-nitrodiphenyl-4,4'-diisocyanate, 2,2'-diphenylpropane-4,4'-diisocyanate, 3,3' and aromatic diisocyanates such as 3,3'-dimethoxydiphenyl-4,4'-diisocyanate, 4,4'-diphenylpropane diisocyanate, m-phenylene diisocyanate, p-phenylene diisocyanate, naphthalene-1,4-diisocyanate, naphthalene-1,5-diisocyanate, and 3,3'-dimethoxydiphenyl-4,4'-diisocyanate, and polyphenylene polymethylene polyisocyanate.
[0033] In one specific embodiment of the present invention, the isocyanate curing agent is hexamethylene diisocyanate (HDI), but the present invention is not limited thereto.
[0034] The initiator is a photoinitiator for polymerizing the acrylic monomer in the adhesive layer 2 to form the acrylic resin. In a specific embodiment of the present invention, the initiator is diphenyl(2,4,6-trimethylbenzoyl) phosphine oxide, but the present invention is not limited thereto.
[0035] Regarding the thickness, the second thickness D2 of the adhesive layer 2 is 3 μm to 30 μm, preferably 5 μm to 25 μm, and particularly preferably 10 μm to 20 μm, although the present invention is not limited thereto.
[0036] In one embodiment of the present invention, the pressure-sensitive adhesive tape 100 has the following properties: (i) the first acid value of the adhesive layer 2 before exposure to ultraviolet rays is 5 mgKOH / g to 20 mgKOH / g, preferably 10 mgKOH / g to 15 mgKOH / g; (ii) the second acid value of the adhesive layer 2a after exposure to ultraviolet rays is 1 mgKOH / g to 4 mgKOH / g, preferably 1 mgKOH / g to 3 mgKOH / g. That is, it is preferable to take into consideration the control of the acid value before and after exposure of the adhesive layer 2 to ultraviolet rays.
[0037] The wavelength of the ultraviolet light is, for example, 300 nm to 380 nm, preferably 340 nm to 380 nm, and particularly preferably 360 nm to 375 nm, but the present invention is not limited thereto. The exposure energy of the ultraviolet light to the adhesive layer is, for example, 100 mJ / cm 2 ~300mJ / cm 2 and 150 mJ / cm 2 ~250mJ / cm 2 and preferably 175 mJ / cm 2 ~225mJ / cm 2 The exposure time of the adhesive layer to the ultraviolet light is, for example, 0.05 minutes to 5.0 minutes, preferably 0.10 minutes to 1.0 minutes, and particularly preferably 0.15 minutes to 0.5 minutes, but the present invention is not limited thereto.
[0038] In addition, the term "acid number" in this specification refers to the number of milligrams of potassium hydroxide (KOH) required to neutralize one gram of a chemical substance. "Acid number" is a metric standard for measuring the number of free fatty acids present in a compound (e.g., fatty acid) or mixture. For example, the acid number can be measured by dissolving a known amount of sample in an organic solvent, titrating with a potassium hydroxide solution of known concentration, and using a phenolphthalein solution as a color indicator. In an embodiment of the present invention, the acid number is measured according to ASTM D974, but the present invention is not limited thereto.
[0039] 2C, the adhesive layer 2 is arranged to match the substrate S to be cut in the cutting process of the part. Before the adhesive layer 2 is exposed to ultraviolet light, the first peel force between the adhesive layer 2 and the substrate S to be cut is 10 N / inch or more. That is, before the adhesive layer 2 is exposed to ultraviolet light, the adhesive strength between the adhesive layer 2 and the substrate S to be cut is high.
[0040] As shown in FIG. 2E, after the adhesive layer 2 is exposed to ultraviolet light, the epoxy monomer in the adhesive layer 2 undergoes self-crosslinking to form an exposed adhesive layer 2a. The second peel force between the exposed adhesive layer 2a and the cut substrate S' is less than 0.2 N / inch. That is, the adhesive strength between the exposed adhesive layer 2a and the cut substrate S' is greatly reduced after exposure. In this way, the exposed adhesive layer 2a can be easily peeled off from the cut substrate S' so that no residual adhesive layer remains on the cut substrate.
[0041] More specifically, the adhesive layer 2 shrinks after the cross-linking reaction of the epoxy monomer, reducing the contact area between the exposed adhesive layer 2a and the cut substrate S', thereby significantly reducing the adhesive strength between the exposed adhesive layer 2a and the cut substrate S'.
[0042] In some embodiments of the present invention, the substrate S to be cut may be, for example, a printed circuit board, a ceramic substrate, a glass substrate, or a wafer. For example, the substrate S to be cut is a glass substrate, but the present invention is not limited thereto.
[0043] The first peel strength and the second peel strength may be measured according to, for example, ASTM D3330.
[0044] For example, the following measurement method can be mentioned. The adhesive layer is attached to the substrate to be cut by rolling the roller back and forth once, and the measurement is performed after leaving it for a while. The substrate is fixed to the lower grip, and the sample is folded 180 degrees and fixed to the upper grip. The adhesive layer is peeled from the substrate at a specified speed (e.g., 300 mm / min) and the average value during peeling is measured. The unit is N / inch.
[0045] Generally speaking, an epoxy monomer (reactive monomer) is further added to the acrylic resin in the adhesive layer 2. The epoxy monomer can improve the adhesive strength of the adhesive layer, and after being exposed to ultraviolet light, the epoxy monomer undergoes a cross-linking curing reaction, causing the exposed adhesive layer 2a to shrink, reducing the contact area with the substrate and reducing the adhesive strength between the adhesive layer and the substrate.
[0046] To explain further, the support layer 3 may be, for example, a polyolefin film (PO film). Regarding the thickness, the third thickness D3 of the support layer 3 is 50 μm to 180 μm, preferably 80 μm to 150 μm, and particularly preferably 100 μm to 150 μm, but the present invention is not limited thereto. The material of the polyolefin is, for example, at least one selected from the group consisting of polyethylene (PE), polypropylene (PP), polymethylpentene (PMP), and polybutene-1 (PB-1). Preferably, the material of the polyolefin film may be, for example, polypropylene, but the present invention is not limited thereto.
[0047] [Pressure-sensitive adhesive tape manufacturing method] The above embodiment is a description of the materials and properties of the pressure-sensitive adhesive tape. The following is a description of a method for manufacturing a pressure-sensitive adhesive tape according to an embodiment of the present invention. The method for manufacturing a pressure-sensitive adhesive tape includes steps S110, S120, and S130. It should be noted that the order of each step and the actual operation method described in the embodiment of the present invention may be adjusted as necessary and are not limited to the description of the present embodiment. The method for manufacturing a pressure-sensitive adhesive tape according to the embodiment of the present invention may provide other operations before, between, or after each step, and some of the operations described may also be replaced, deleted, or rearranged to implement the manufacturing method.
[0048] In the step S110, a release layer 1 is provided. The release layer 1 may be, for example, a polyester release layer (for example, a PET release film). The first thickness D1 of the release layer 1 is 25 μm to 45 μm, preferably 28 μm to 40 μm, and particularly preferably 30 μm to 38 μm, although the present invention is not limited thereto.
[0049] In the step S120, the adhesive coating liquid composition is applied to one side of the release layer 1 by an offline coater, and the solvent component in the adhesive coating liquid composition is removed to form an adhesive layer 2 on one side of the release layer 1. The second thickness of the adhesive layer 2 is 3 μm to 30 μm, preferably 5 μm to 25 μm, and particularly preferably 10 μm to 20 μm.
[0050] The adhesive coating liquid composition may include, for example, a solid component and a solvent component. The solid component includes an acrylic resin, an epoxy monomer, a hardener, and a photoinitiator. The material characteristics and composition of the solid component are similar to those of the above embodiment, so they will not be described here.
[0051] The solvent component dilutes the solid content so as to give a predetermined viscosity to the adhesive coating liquid composition, which makes it easier to apply the adhesive coating liquid composition to the release layer 1 and to mold it. The solvent component is, for example, at least one of ethyl acetate (EAC) and methyl ethyl ketone (MEK).
[0052] The predetermined viscosity of the adhesive coating liquid composition is, for example, 25 cps to 225 cps, and preferably 50 cps to 200 cps, but the present invention is not limited thereto. It should be noted that the predetermined viscosity of the adhesive coating liquid composition of this embodiment was measured at room temperature (25°C) and normal pressure (1 atm). The viscosity may be measured, for example, by a rotary viscometer, and the measurement method may be, for example, ASTM D2196.
[0053] The adhesive coating liquid composition is prepared, for example, by adding an acrylic monomer, a curing agent, and a solvent to a container in this order and stirring them to form a mixed solution, followed by adding a photoinitiator and an epoxy monomer in this order.
[0054] After the solvent in the adhesive coating liquid composition is removed, the adhesive layer 2 is formed. The adhesive layer 2 is cured after the solvent component is removed, so the viscosity cannot be measured. In the adhesive layer 2, the acrylic monomer first undergoes a curing crosslinking reaction (the molecular weight of acrylic is improved) by the action of a curing agent and a photoinitiator to form the acrylic resin. In addition, since the epoxy monomer does not undergo a crosslinking reaction before being exposed to ultraviolet light, the adhesive layer 2 has high adhesive strength and can be more appropriately adhered to the substrate to be cut. In addition, the epoxy monomer shrinks after being exposed to ultraviolet light, reducing the contact area with the substrate, reducing the adhesive strength and making it easier to separate from the substrate.
[0055] In step S130, the support layer 3 is attached to the surface of the adhesive layer 2 away from the release layer 1. The third thickness D3 of the support layer 3 is 50 μm to 180 μm, preferably 80 μm to 150 μm, and particularly preferably 100 μm to 150 μm, although the present invention is not limited thereto.
[0056] It should be noted that, in this embodiment, the adhesive layer 2 is formed on the release layer 1 first, and then the support layer 3 is bonded to the adhesive layer 2, but the present invention is not limited thereto. For example, the adhesive layer 2 may be formed on the support layer 3 first, and then the release layer 1 may be bonded to the adhesive layer 2.
[0057] [How to use pressure sensitive adhesive tape] The above embodiment is a description of the materials and properties of the pressure-sensitive adhesive tape. The following is a description of a method for manufacturing a pressure-sensitive adhesive tape according to an embodiment of the present invention. The method for manufacturing a pressure-sensitive adhesive tape includes steps S210, S220, S230, S240, S250, S260, and S170. It should be noted that the order of each step and the actual operation method described in the embodiment of the present invention may be adjusted as necessary and are not limited to the description of the present embodiment. The method for manufacturing a pressure-sensitive adhesive tape according to the embodiment of the present invention may provide other operations before, between, or after each step, and some of the operations described may also be replaced, deleted, or rearranged to implement the manufacturing method.
[0058] As shown in FIG. 2A, in step S210, the pressure-sensitive adhesive tape 100 according to the embodiment is provided, and the release layer 1 of the pressure-sensitive adhesive tape 100 is peeled off from the adhesive layer 2, thereby exposing the adhesive layer 2 to the external environment.
[0059] 2B, in step S220, a substrate S to be cut is provided, and the adhesive layer 2 of the pressure-sensitive adhesive tape 100 is placed facing the substrate S to be cut. The substrate S to be cut may be, for example, a printed circuit board, a ceramic substrate, a glass substrate, or a wafer.
[0060] 2C, in step 230, the pressure-sensitive adhesive tape 100 is attached to a substrate S to be cut via the adhesive layer 2. A first peel force between the adhesive layer 2 and the substrate S to be cut is 10 N / inch or more, and preferably 12 N / inch to 15 N / inch.
[0061] 2D, in step S240, a cutting step is performed on the substrate S to be cut, whereby the substrate S to be cut is cut from the surface away from the adhesive layer 2 to form a cut substrate S'. In this embodiment, cutting into three equal parts is described as an example, but the present invention is not limited thereto.
[0062] As shown in FIG. 2E, in the step S250, the adhesive layer 2 of the pressure-sensitive adhesive tape 100 is exposed to ultraviolet light, thereby causing a crosslinking reaction of the epoxy monomer in the adhesive layer 2 and forming an exposed adhesive layer 2a. The second peeling force between the exposed adhesive layer 2a and the cut substrate S' is 0.2 N / inch or less, preferably 0.05 N / inch to 0.15 N / inch. The adhesive layer 2 shrinks after the crosslinking reaction of the epoxy monomer, reducing the contact area between the exposed adhesive layer 2a and the cut substrate S'. As a result, the adhesive strength between the exposed adhesive layer 2a and the cut substrate S' can be significantly reduced, making them easier to separate from each other.
[0063] In one embodiment of the present invention, the pressure-sensitive adhesive tape 100 has the following properties: (i) the first acid value of the adhesive layer 2 before exposure to ultraviolet rays is 5 mgKOH / g to 20 mgKOH / g, preferably 10 mgKOH / g to 15 mgKOH / g; (ii) the second acid value of the adhesive layer 2a after exposure to ultraviolet rays is 1 mgKOH / g to 4 mgKOH / g, preferably 1 mgKOH / g to 3 mgKOH / g. That is, it is preferable to take into consideration the control of the acid value before and after exposure of the adhesive layer to ultraviolet rays.
[0064] As shown in FIG. 2F, in step S260, the cut substrate S' is divided into a plurality of small sheet-like materials by separating the cut substrate S' from the exposed adhesive layer 2a.
[0065] Due to the above-mentioned configuration, the pressure-sensitive adhesive tape 100 according to the embodiment of the present invention has a high adhesive strength between the adhesive layer 2 and the substrate S to be cut (peel strength ≧10 N / inch), so that the adhesive layer 2 can be firmly attached to the substrate S to be cut so as not to fall off. When performing the cutting process, the adhesive layer 2 does not degumm or produce adhesive threads.
[0066] After being exposed to ultraviolet light, the adhesive strength between the exposed adhesive layer 2a and the cut substrate S' is significantly reduced (peel strength ≦2N / inch). The exposed adhesive layer 2a can be easily peeled off from the cut substrate S' without leaving any adhesive residue. The pressure-sensitive adhesive tape 100 according to the embodiment of the present invention can be applied to the cutting process of various parts.
[0067] [Experimental data and measurement results] In order to demonstrate the technical effects of the pressure-sensitive adhesive tape according to the embodiment of the present invention, experimental data and results are described below, however, the following examples and comparative examples are provided for the purpose of understanding the present invention, and the scope of protection of the present invention is not limited to these examples.
[0068] <Example 1> A pressure-sensitive adhesive tape was manufactured based on the manufacturing method of the pressure-sensitive adhesive tape. The pressure-sensitive adhesive tape includes a release layer, an adhesive layer, and a support layer, and the adhesive layer was manufactured based on the formulation in Table 1 below. The total weight of the adhesive layer was 100 wt%, and the adhesive layer contained 40 wt% acrylic, 0.2 wt% isocyanate curing agent, 0.8 wt% photoinitiator, and 59 wt% epoxy monomer. The viscosity of the paint formed on the release layer of the adhesive layer was about 150 cps, and the thickness of the adhesive layer was 20 μm. The release layer of Example 1 was a PET release film, and the support layer was a polyolefin film.
[0069] <Example 2> The results are almost the same as those of Example 1, except for the composition or thickness of the adhesive layer. The adhesive layer contained 40 wt% acrylic, 0.1 wt% isocyanate curing agent, 0.8 wt% photoinitiator, and 59.1 wt% epoxy monomer, with the total weight of the adhesive layer being 100 wt%. The viscosity of the paint formed on the release layer of the adhesive layer was about 153 cps, and the thickness of the adhesive layer was 20 μm.
[0070] <Example 3> The adhesive layer was almost the same as Example 1, except for the composition or thickness of the adhesive layer. The adhesive layer contained 40 wt% acrylic, 0.1 wt% isocyanate hardener, 0.8 wt% photoinitiator, and 59.1 wt% epoxy monomer, with the total weight of the adhesive layer being 100 wt%. The paint viscosity of the adhesive layer was about 153 cps, and the thickness of the adhesive layer was 10 μm.
[0071] <Example 4> The adhesive layer was almost the same as Example 1, except for the composition or thickness of the adhesive layer. The adhesive layer contained 45 wt% acrylic, 0.2 wt% isocyanate hardener, 0.8 wt% photoinitiator, and 54 wt% epoxy monomer, with the total weight of the adhesive layer being 100 wt%. The paint viscosity of the adhesive layer was about 121 cps, and the thickness of the adhesive layer was 20 μm.
[0072] <Example 5> The adhesive layer was almost the same as Example 1, except for the composition or thickness of the adhesive layer. The adhesive layer contained 50 wt% acrylic, 0.2 wt% isocyanate hardener, 0.8 wt% photoinitiator, and 49 wt% epoxy monomer, with the total weight of the adhesive layer being 100 wt%. The paint viscosity of the adhesive layer was about 106 cps, and the thickness of the adhesive layer was 20 μm.
[0073] <Comparative Example 1> The examples are almost the same as those of Example 1, but the difference between them was the composition of the adhesive layer. The adhesive layer contained 20 wt% acrylic, 0.1 wt% isocyanate hardener, 0.8 wt% photoinitiator, and 79.1 wt% epoxy monomer, with the total weight of the adhesive layer being 100 wt%. The adhesive layer had a paint viscosity of about 485 cps and a thickness of 20 μm. The acrylic content of Comparative Example 1 was low (20 wt%) and the epoxy monomer content was high (79.1 wt%).
[0074] <Comparative Example 2> It is almost the same as Example 1, but the difference between them is the composition of the adhesive layer. The adhesive layer contained 80 wt% acrylic, 0.4 wt% isocyanate hardener, 0.8 wt% photoinitiator, and 18.8 wt% epoxy monomer, with the total weight of the adhesive layer being 100 wt%. The paint viscosity of the adhesive layer was about 86 cps, and the thickness of the adhesive layer was 20 μm. Comparative Example 2 had a high acrylic content (80 wt%) and a low epoxy monomer content (18.8 wt%).
[0075] <Comparative Example 3> It was almost the same as Example 1, but the difference was the composition of the adhesive layer. The adhesive layer contained 98.7 wt% acrylic, 0.5 wt% isocyanate hardener, and 0.8 wt% photoinitiator, with the total weight of the adhesive layer being 100 wt%. The paint viscosity of the adhesive layer was about 56 cps, and the thickness of the adhesive layer was 20 μm. Of these, Comparative Example 3 used almost acrylic (98.7 wt%) and did not use epoxy monomer.
[0076] In order to prove the technical effects of the embodiments of the present invention, in this experiment, the release layer was peeled off from the pressure-sensitive adhesive tape of any of the above-mentioned Examples 1 to 5 and Comparative Examples 1 to 3, and then the adhesive layer was attached to a substrate (e.g., a glass substrate) to be cut, and the physicochemical properties (e.g., acid value and peel strength) before and after exposure to ultraviolet light were measured.
[0077] <Acid value> A known amount of sample was dissolved in an organic solvent and titrated with a known concentration of potassium hydroxide solution, and phenolphthalein solution was used as a color indicator. In an embodiment of the present invention, the acid value was measured according to ASTM D974. The first acid value was the acid value before the adhesive layer was exposed to ultraviolet light, and the second acid value was the acid value after the adhesive layer was exposed to ultraviolet light.
[0078] <Peeling force> The adhesive layer was attached to the substrate to be cut by rolling the roller back and forth once, and the measurement was performed after leaving it for a while. The substrate was fixed to the lower grip, and the sample was folded 180° and fixed to the upper grip, after which the adhesive layer was peeled off from the substrate at a predetermined speed (e.g., 300 mm / min) and the average value during peeling was measured. The unit was N / inch. The first peel force was the peel force between the adhesive layer and the substrate before exposure to ultraviolet light, and the second peel force was the peel force between the adhesive layer and the substrate after exposure to ultraviolet light.
[0079] [Table 1]
[0080] [Results and Discussion] According to the experimental results, the pressure-sensitive adhesive tapes according to Examples 1 to 5 have a high adhesive strength between the adhesive and the substrate (first peeling force ≧10 N / inch), so the adhesive layer can be firmly attached without falling off. When cutting, the adhesive layer does not degumm or produce adhesive threads. After exposure to ultraviolet light, the adhesive strength between the exposed adhesive layer and the substrate is greatly reduced (second peeling force ≦0.5 N / inch). The exposed adhesive layer can be peeled off from the substrate without leaving any adhesive residue.
[0081] The adhesive layers of Comparative Examples 2 and 3 used a small amount of epoxy monomer or did not use any epoxy monomer. In the adhesive layers of Comparative Examples 2 and 3, significant adhesive residue was observed after the substrate was peeled off. The adhesive layer of Comparative Example 1 used a large amount of epoxy monomer. The peel strength and adhesive residue of Comparative Example 1 were similar to those of Examples 1 to 5, but the viscosity of the adhesive layer of Comparative Example 1 was too high when it was applied and molded, resulting in poor moldability.
[0082] More specifically, the viscosity of the adhesive layer in Comparative Example 1 was too high, making it difficult to control the thickness of the adhesive layer when it was applied, resulting in poor thickness uniformity and moldability. For these reasons, customers were unable to bond the adhesive layer firmly when using it to attach it to a package element or wafer, which resulted in problems such as water infiltration and contamination during cutting.
[0083] [Advantageous Effects of the Embodiments] The pressure-sensitive adhesive tape of the present invention has the following technical features: "The adhesive layer contains 40% by weight to 50% by weight of acrylic resin, 40% by weight to 65% by weight of epoxy monomer, 0.05% by weight to 0.5% by weight of curing agent, and 0.5% by weight to 1.0% by weight of initiator, with the total weight of the adhesive layer being 100% by weight" and "The adhesive layer has a first acid value before being exposed to ultraviolet light, and the adhesive layer shrinks after being exposed to ultraviolet light to have a second acid value, the second acid value being smaller than the first acid value". This improves the adhesive strength between the adhesive layer and the cutting substrate, and prevents adhesive residue after the adhesive layer is removed.
[0084] Conventional UV adhesive layers use only a single resin, making it difficult to control the adhesive strength of the UV adhesive layer and prone to adhesive residue when the tape is peeled off, which makes it difficult to meet the requirements of the cutting process of various parts of customers. The present invention particularly improves the UV adhesive layer by introducing a reactive monomer into the UV adhesive layer to provide a better formulation, thereby improving the adhesive strength with the substrate and avoiding adhesive residue.
[0085] The above disclosure is merely a preferred embodiment of the present invention, and the scope of the claims of the present invention is not limited thereto. Therefore, all equivalent technical modifications made by utilizing the specification and drawings of the present invention are included in the scope of the claims of the present invention. [Explanation of symbols]
[0086] 100...Pressure-sensitive adhesive tape 1...Release layer 2...Adhesive layer 2a…Exposed adhesive layer 3…Support layer D1…First thickness D2: Second thickness D3…Third thickness S: Substrate to be cut S': Cut substrate
Claims
1. A pressure-sensitive adhesive tape for use in a cutting process of a part, comprising: The pressure-sensitive adhesive tape is A release layer; An adhesive layer formed on one surface of the release layer; a support layer formed on a surface of the adhesive layer away from the release layer, The adhesive layer includes 40% to 50% by weight of acrylic, 40% to 65% by weight of epoxy monomer, 0.05% to 0.5% by weight of isocyanate curing agent, and 0.5% to 1.0% by weight of photoinitiator, where the total weight of the adhesive layer is 100% by weight; The acrylic includes an acrylic monomer and an acrylic resin obtained by polymerizing the acrylic monomer, The acrylic resin obtained by polymerizing the acrylic monomer is poly(methyl methacrylate) (PMMA) having a chemical structure represented by the following formula (I), where n=3,000 to 5,000: 【Chemistry 1】 Formula (I) The epoxy monomer is a reactive epoxy monomer and has a chemical structure of the following formula (II): 【Chemistry 2】 Formula (II) the adhesive layer has a first acid number prior to exposure to ultraviolet light; The pressure sensitive adhesive tape, wherein the adhesive layer shrinks after exposure to ultraviolet light to have a second acid value, the second acid value being less than the first acid value.
2. 2. The pressure-sensitive adhesive tape of claim 1, wherein the first acid value of the adhesive layer before exposure to the ultraviolet light is from 5 mg KOH / g to 20 mg KOH / g, and the second acid value of the adhesive layer after exposure to the ultraviolet light is from 1 mg KOH / g to 4 mg KOH / g.
3. 3. The pressure-sensitive adhesive tape of claim 2, wherein the first acid value of the adhesive layer before exposure to the ultraviolet light is from 10 mg KOH / g to 15 mg KOH / g, and the second acid value of the adhesive layer after exposure to the ultraviolet light is from 1 mg KOH / g to 3 mg KOH / g.
4. 2. The pressure-sensitive adhesive tape of claim 1, wherein the release layer has a first thickness of 25 μm to 45 μm, the adhesive layer has a second thickness of 3 μm to 30 μm, and the support layer has a third thickness of 50 μm to 180 μm, the release layer being primarily composed of a polyester material and the support layer being primarily composed of a polyolefin material.
5. The wavelength of the ultraviolet light is 300 nm to 380 nm, and the exposure energy of the ultraviolet light to the adhesive layer is 100 mJ / cm 2 ~300 mJ / cm 2 2. The pressure-sensitive adhesive tape of claim 1, wherein
6. In the cutting step of the part, the release layer is peeled off first, and the adhesive layer is bonded to the cutting base material; The cutting substrate is a printed circuit board, a ceramic substrate, a glass substrate, or a wafer; 2. The pressure-sensitive adhesive tape of claim 1, wherein a first peel force between the adhesive layer and the cutting substrate is 10 N / inch or more before the adhesive layer is exposed to the ultraviolet light.
7. 7. The pressure-sensitive adhesive tape according to claim 6, wherein after the adhesive layer is exposed to the ultraviolet light, the epoxy monomer in the adhesive layer undergoes a crosslinking reaction, so that the adhesive layer is formed as an exposed adhesive layer, and a second peel force between the exposed adhesive layer and the cutting substrate is 0.2 N / inch or less.
8. 8. The pressure-sensitive adhesive tape of claim 7, wherein the adhesive layer shrinks after the crosslinking reaction of the epoxy monomer occurs, reducing the contact area between the exposed adhesive layer and the cutting substrate.
Citation Information
Patent Citations
Adhesive mass composition
JP1982155274A
Hardly stainable adhesive sheets and method for removing resist material
JP2001181585A
Adhesive sheet for optical use, optical member with adhesive and its manufacturing method
JP2009242633A
Adhesive composition, adhesive sheet, and method for producing semiconductor device