ADHESIVE FILM, OPTICAL MEMBER COMPRISING THE SAME, AND OPTICAL DISPLAY DEVICE COMPRISING THE SAME
A high-refractive-index adhesive film with aromatic rings in a (meth)acrylic copolymer addresses light loss in organic displays by enhancing light extraction and adhesion reliability, improving efficiency and reducing power consumption.
Patent Information
- Application Number
- JP2023063935
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2022-04-22
- Filing Date
- 2023-04-11
- Publication Date
- 2024-10-09
- Estimated Expiration
- 2043-04-11
AI Technical Summary
In organic light emitting device displays, a significant portion of light is lost due to reflection and absorption within the layered structures, leading to decreased light extraction efficiency and increased power consumption, necessitating the use of adhesive films that can minimize refractive index differences and enhance light path alteration.
An adhesive film with a high refractive index, achieved through a (meth)acrylic copolymer containing aromatic rings, is developed, which maintains excellent step followability, peel strength, and low haze, and has a controlled rate of change in peel strength over time.
The adhesive film effectively minimizes light reflection, enhances light extraction efficiency, and ensures reliable adhesion without bubbles or floating, even on high-refractive-index adherends, thereby reducing power consumption and extending device lifespan.
Smart Images

Figure 0007564909000011 
Figure 0007564909000001 
Figure 0007564909000002
Abstract
Description
[Technical field]
[0001] The present invention relates to an adhesive film, an optical member including the same, and an optical display device including the same. [Background technology]
[0002] In an organic light emitting diode display device, more than 80% of the light emitted from the light emitting layer is reflected or absorbed at the interface or inside of various layered structures of the light emitting device or the display device, and is lost without reaching the front of the display device. This reduces the light extraction efficiency, and it is difficult to avoid increasing power consumption in order to realize the desired brightness, which also shortens the life of the light emitting device.
[0003] The touch screen panel laminated on the light emitting element has a remarkably high refractive index compared to ordinary adhesive films because it is made of metal materials such as aluminum, titanium, etc. For this reason, in order to reduce the difference in refractive index between layers or to increase the light extraction efficiency by changing the path of light reflected at the interface, a method of further laminating a layer that can reduce the difference in refractive index or an adhesive film with a high refractive index is considered. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] Korean Patent No. 10-1189698 Summary of the Invention [Problem to be solved by the invention]
[0005] An object of the present invention is to provide a pressure-sensitive adhesive film which has a high refractive index, and is excellent in conformity to unevenness, peel strength, and appearance.
[0006] Another object of the present invention is to provide a pressure-sensitive adhesive film which has a high refractive index and a low rate of change in peel strength over time.
[0007] It is still another object of the present invention to provide a pressure-sensitive adhesive film having a high refractive index and low haze. [Means for solving the problem]
[0008] One aspect of the present invention relates to a pressure-sensitive adhesive film.
[0009] 1. The pressure-sensitive adhesive film of the present invention contains a (meth)acrylic copolymer having an aromatic ring, and the pressure-sensitive adhesive film has a refractive index of 1.55 or more. In the pressure-sensitive adhesive film, a ratio A represented by the following formula 1 is 1 to 8, and a ratio (B) represented by the following formula 2 is 1 to 15:
[0010]
number
[0011] In the above formula 1 and formula 2, G' 25 is the storage modulus of the adhesive film at 25°C (unit: kPa), G' 60 is the storage modulus of the adhesive film at 60°C (unit: kPa), G' 85 is the storage modulus (unit: kPa) of the adhesive film at 85°C.
[0012] 2. In the above 1, the adhesive film may have a rate of change in peel strength over time of 60% or less, as represented by the following formula 3:
[0013]
number
[0014] In the above formula 3, PS1 is the initial peel strength of the adhesive film against the substrate (unit: gf / inch), PS2 is the peel strength (unit: gf / inch) of the adhesive film to the above-mentioned adherend after it has been left to stand at 50° C. for 7 days.
[0015] 3. In the above 1. or 2., the pressure-sensitive adhesive film can have a peel strength from an adherend of 400 gf / inch (154.4 mN / mm) or more.
[0016] 4. In any one of the above 1. to 3., the pressure-sensitive adhesive film has a storage modulus (G' 60 ) can be between 5kPa and 70kPa.
[0017] 5. In any one of the above 1. to 4., the pressure-sensitive adhesive film has a storage modulus (G' 85 ) can be between 1kPa and 60kPa.
[0018] 6. In any one of the above 1. to 5., the pressure-sensitive adhesive film may further contain a photoinitiator and a thermosetting crosslinking agent.
[0019] 7. In any of the above 1. to 6., the pressure-sensitive adhesive film may be formed from a composition for pressure-sensitive adhesive films, which contains the above aromatic ring-containing (meth)acrylic copolymer, a photoinitiator, and a thermosetting crosslinking agent.
[0020] 8. In the above item 7, the (meth)acrylic copolymer having an aromatic ring is a copolymer of a monomer mixture containing a (meth)acrylic monomer having an aromatic ring, and the (meth)acrylic monomer having an aromatic ring may contain a (meth)acrylic monomer having two or more aromatic rings.
[0021] 9. In the above item 8, the (meth)acrylic monomer having two or more aromatic rings may be contained in an amount of 30% by mass or more based on the total mass of the monomer mixture.
[0022] 10. In the above item 8 or 9, the glass transition temperature of the homopolymer of the (meth)acrylic monomer having two or more aromatic rings can be 0° C. or higher.
[0023] 11. In any of the above 8. to 10., the (meth)acrylic monomer having two or more aromatic rings may include at least one selected from the group consisting of phenoxybenzyl (meth)acrylate, biphenylyl methyl (meth)acrylate, phenylphenoxyethyl (meth)acrylate, biphenylyl (meth)acrylate, and naphthyl (meth)acrylate.
[0024] 12. In any one of the above 8. to 11., the monomer mixture may further contain a hydroxyl group-containing (meth)acrylic monomer.
[0025] 13. In the above 12., the monomer mixture may have a content of the aromatic ring-containing (meth)acrylic monomer of 40% by mass to 95% by mass, and a content of the hydroxyl group-containing (meth)acrylic monomer of 5% by mass to 60% by mass, with the total mass of the monomer mixture being 100% by mass.
[0026] 14. In any of the above 7. to 13., the composition for adhesive films may contain 100 parts by mass of the (meth)acrylic copolymer having an aromatic ring, 0.005 to 5 parts by mass of the photoinitiator, and 0.05 or more parts by mass and less than 5 parts by mass of the thermosetting crosslinking agent.
[0027] 15. In any of the above 6. to 14., the pressure-sensitive adhesive film may further contain a leveling agent.
[0028] 16. In the above item 15, the leveling agent may include one or more types of silicon-modified polyacrylates.
[0029] In 17.1, the (meth)acrylic copolymer having an aromatic ring can be a random copolymer.
[0030] Another aspect of the present invention is an optical member.
[0031] The optical member includes the pressure-sensitive adhesive film of the present invention.
[0032] Yet another aspect of the present invention is an optical display device.
[0033] The optical display device includes the pressure-sensitive adhesive film of the present invention. Effect of the Invention
[0034] According to one aspect of the present invention, there is provided a pressure-sensitive adhesive film which has a high refractive index, and is excellent in conformability to unevenness, peel strength and appearance.
[0035] According to another aspect of the present invention, there is provided a pressure-sensitive adhesive film which has a high refractive index and a low rate of change in peel strength over time.
[0036] According to yet another aspect of the present invention, there is provided a pressure-sensitive adhesive film that has a high refractive index and low haze because it does not contain high refractive index inorganic particles. [Brief description of the drawings]
[0037] [Figure 1] 1 is a schematic cross-sectional view of an optical display device according to one embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0038] The present invention will now be described in detail with reference to the accompanying drawings, in which: FIG. 1 is a block diagram of a semiconductor device according to an embodiment of the present invention;
[0039] In order to clearly explain the present invention in the drawings, parts that are not relevant to the description are omitted, and the same names are used for the same or similar components throughout the specification. In the drawings, the length and size of each component are for explaining the present invention, and the present invention is not limited to the length and size of each component illustrated in the drawings.
[0040] In this specification, the terms "upper" and "lower" are defined based on the drawings, and depending on the viewing angle, the "upper" may become the "lower" and the "lower" may become the "upper".
[0041] In this specification, "(meth)acrylic" means acrylic and / or methacrylic.
[0042] In this specification, the "refractive index" is a value measured in the visible light region, for example, at a wavelength of 633 nm using a prism coupler.
[0043] In this specification, when describing a numerical range, "X to Y" means at least X and at most Y (X≦ and ≦Y).
[0044] The present invention relates to a pressure-sensitive adhesive film that exhibits a high refractive index, while at the same time being excellent in conformability to unevenness, peel strength and appearance, as well as a low rate of change in peel strength over time.
[0045] Because the pressure-sensitive adhesive film of the present invention has a high refractive index, even when it is laminated to an adherend having a high refractive index, the reflection of light incident on the pressure-sensitive adhesive film from the adherend can be minimized, thereby increasing the light extraction efficiency.
[0046] The adhesive film of the present invention has excellent conformability to unevenness, so even when it adheres to a patterned high refractive index substrate, spaces are unlikely to form between the adhesive film and the high refractive index substrate, and the adhesive film does not float, thereby improving the light extraction efficiency.
[0047] The pressure-sensitive adhesive film of the present invention has a low rate of change in peel strength over time. A low rate of change in peel strength over time means that the content of uncured components in the pressure-sensitive adhesive film is low, and there are no air bubbles or lifting when evaluating the reliability of the pressure-sensitive adhesive film.
[0048] Hereinafter, a pressure-sensitive adhesive film according to one embodiment of the present invention will be described.
[0049] The pressure-sensitive adhesive film according to the present invention has a refractive index of 1.55 or more. If the refractive index is within this range, even if the film is laminated on an adherend having a high refractive index, the reflection of light incident on the pressure-sensitive adhesive film from the adherend is minimized, thereby increasing the light extraction efficiency. For example, the pressure-sensitive adhesive film may have a refractive index of 1.55, 1.6, 1.65, 1.7, 1.75, or 1.8, preferably 1.55 to 1.8, and more preferably 1.55 to 1.65.
[0050] In the pressure-sensitive adhesive film according to the present invention, the ratio A represented by the following formula 1 is 1-8, and the ratio B represented by the following formula 2 is 1-15.
[0051]
number
[0052] In the above formula 1 and formula 2, G' 25 is the storage modulus of the adhesive film at 25°C (unit: kPa), G' 60 is the storage modulus of the adhesive film at 60°C (unit: kPa), G' 85 is the storage modulus (unit: kPa) of the adhesive film at 85°C.
[0053] The above formula 1 and formula 2 are relational expressions devised for evaluating whether a high refractive index adhesive film has excellent step conformability and a low rate of change in peel force over time.
[0054] The high refractive index of the adhesive film can be realized by a composition containing a (meth)acrylic copolymer having an aromatic ring obtained by complete or partial polymerization of a monomer mixture containing a (meth)acrylic monomer having an aromatic ring, or a polymer containing the same. The (meth)acrylic monomer having an aromatic ring has a higher glass transition temperature of a homopolymer than a normal (meth)acrylic monomer used in the manufacture of an adhesive film. The above formula 1 and the above formula 2 are relational expressions devised to ensure that an adhesive film manufactured by a composition containing a (meth)acrylic copolymer having an aromatic ring or a polymer containing the same obtained by complete or partial polymerization of a monomer mixture containing a (meth)acrylic monomer having an aromatic ring has excellent step conformability, excellent peel strength, and a low rate of change in peel strength over time. The step conformability is evaluated by aligning the adhesive film with a patterned adherend at room temperature (e.g., 23 to 25°C) and then treating it at a high temperature (e.g., 50 to 60°C) for a predetermined time, as shown below. The rate of change in peel strength over time is measured after leaving the adhesive film at high temperature for a long period of time, as represented by the following mathematical formula 3. A high rate of change in peel strength over time means that a large amount of unreacted components remain in the adhesive film, resulting in a significant increase in peel strength during the process of measuring the rate of change.
[0055] A PSA film in which the ratio A represented by the above formula 1 satisfies the range of the present invention, but the ratio B represented by the above formula 2 does not satisfy the range of the present invention, has poor step conformability, peeling force, and appearance. A PSA film in which the ratio B represented by the above formula 2 satisfies the range of the present invention, but the ratio A represented by the above formula 1 does not satisfy the range of the present invention, has poor peeling force, step conformability, and appearance.
[0056] For example, the ratio A represented by the above formula 1 can be 1, 1.5, 2, 2.5, 3, 3.5, 4, 4.5, 5, 5.5, 6, 6.5, 7, 7.5, 8, preferably 1 to 7, and more preferably 2 to 6.5. For example, the ratio B represented by the above formula 2 can be 1, 1.5, 2, 2.5, 3, 3.5, 4, 4.5, 5, 5.5, 6, 6.5, 7, 7.5, 8, 8.5, 9, 9.5, 10, 10.5, 11, 11.5, 12, 12.5, 13, 13.5, 14, 14.5, 15, preferably 1 to 13, and more preferably 2 to 12.
[0057] In some embodiments, the PSA film has a rate of change in peel strength over time represented by the following formula 3 of 60% or less, for example, 1%, 2%, 3%, 4%, 5%, 6%, 7%, 8%, 9%, 10%, 11%, 12%, 13%, 14%, 15%, 16%, 17%, 18%, 19%, 20%, 21%, 22%, 23%, 24%, 25%, 26%, 27% , 28%, 29%, 30%, 31%, 32%, 33%, 34%, 35%, 36%, 37%, 38%, 39%, 40%, 41%, 42%, 43%, 44%, 45%, 46%, 47%, 48%, 49%, 50%, 51%, 52%, 53%, 54%, 55%, 56%, 57%, 58%, 59%, 60%, specifically 5% to 50%. If the rate of change in peel force over time is within the above range, the reliability of the adhesive film is high, and bubbles and lifting after leaving the adhesive film at high temperature and / or high temperature and high humidity for a long period of time can be almost eliminated.
[0058]
number
[0059] In the above formula 3, PS1 is the initial peel strength of the adhesive film against the substrate (unit: gf / inch), PS2 is the peel strength (unit: gf / inch) of the adhesive film to the adherend after it has been left to stand at 50° C. for 7 days.
[0060] In the above formula 3, the initial peel strength means the peel strength measured before the PSA film was left at 50° C. for 7 days.
[0061] The "adherend" may include one or more of inorganic materials including glass, organic materials, and mixtures of organic and inorganic materials. The "adherend" may be in the form of a plate, a sheet, a film, or a display panel (touch panel layer). The "adherend" may be patterned. In one embodiment, the adherend may be a glass plate, preferably an alkali-free glass plate.
[0062] In some embodiments, the adhesive film has a peel strength to an adherend of 400 gf / inch (154.4 mN / mm) or more, for example, 400 gf / inch (154.4 mN / mm), 500 gf / inch (193.0 mN / mm), 600 gf / inch (231.6 mN / mm), 700 gf / inch (270.2 mN / mm), 800 gf / inch(308.8mN / mm), 900gf / inch(347.4mN / mm), 1000gf / inch(386.0mN / mm), 1100gf / inch(424.6mN / mm), 1200gf / inch(463.2mN / mm), 1300gf / inch(501.8mN / mm), 1400gf / inch(540.4mN / mm) , 1500gf / inch(579.0mN / mm), 1600gf / inch(617.6mN / mm), 1700gf / inch(656.2mN / mm), 1800gf / inch(694.8mN / mm), 1900gf / inch(733.4mN / mm), 2000gf / inch(772.0mN / mm), 2100gf / inch(810 .6mN / mm), 2200gf / inch (849.2mN / mm), 2300gf / inch (887.8mN / mm), 2400gf / inch (926.4mN / mm), 2500gf / inch (965.0mN / mm), for example, 400gf / inch (154.4mN / mm) to 2500gf / inch (965.0mN / mm). If the peeling force against the adherend is within the above range, the adhesive can be fixed to the adherend with high reliability, and further adherends can be easily laminated. Note that 1gf / inch=0.386mN / mm=0.386kg / s 2 It is.
[0063] In some embodiments, the adhesive film has a storage modulus (G' 25 The storage modulus (G') at 25°C may be 10 kPa to 100 kPa, for example, 10 kPa, 15 kPa, 20 kPa, 25 kPa, 30 kPa, 35 kPa, 40 kPa, 45 kPa, 50 kPa, 55 kPa, 60 kPa, 65 kPa, 70 kPa, 75 kPa, 80 kPa, 85 kPa, 90 kPa, 95 kPa, or 100 kPa, preferably 10 kPa to 80 kPa. 25 ) within the above range, excellent conformability to unevenness can be easily provided.
[0064] In some embodiments, the adhesive film has a storage modulus (G' 60 The storage modulus at 60° C. (G') can be 5 kPa to 70 kPa, for example, 5 kPa, 10 kPa, 15 kPa, 20 kPa, 25 kPa, 30 kPa, 35 kPa, 40 kPa, 45 kPa, 50 kPa, 60 kPa, 65 kPa, or 70 kPa, preferably 5 kPa to 50 kPa. 60 ) within the above range, excellent conformability to unevenness can be easily provided.
[0065] In some embodiments, the adhesive film has a storage modulus (G' 85 The storage modulus (G') at 85°C may be 1 kPa to 60 kPa, for example, 1 kPa, 5 kPa, 10 kPa, 15 kPa, 20 kPa, 25 kPa, 30 kPa, 35 kPa, 40 kPa, 45 kPa, 50 kPa, 55 kPa, or 60 kPa, and preferably 1 kPa to 40 kPa. 85 ) within the above range, it may be easy to prevent air bubbles and floating from occurring during reliability evaluation.
[0066] In some embodiments, the adhesive film may have a haze of 1% or less, for example, 0% to 0.5%, in the visible light region, for example, at a wavelength of 550 nm. If the haze of the adhesive film is within the above range, the adhesive film can transmit light incident from the adherend, thereby increasing the light extraction efficiency.
[0067] In some embodiments, the adhesive film may have a thickness of 50 μm or less, for example, more than 0 μm and less than 30 μm, or 1 μm to 25 μm. If the thickness of the adhesive film is within the above range, it can be used in an optical display device.
[0068] In some embodiments, the pressure-sensitive adhesive film includes a (meth)acrylic copolymer having an aromatic ring, a photoinitiator, and a thermosetting crosslinking agent. In some embodiments, the pressure-sensitive adhesive film is formed from a composition for pressure-sensitive adhesive films including a (meth)acrylic copolymer having an aromatic ring, a photoinitiator, and a thermosetting crosslinking agent. In some embodiments, the pressure-sensitive adhesive film can include a cured product of a composition for pressure-sensitive adhesive films including a (meth)acrylic copolymer having an aromatic ring, a photoinitiator, and a thermosetting crosslinking agent.
[0069] In some embodiments, the adhesive film may include a complete or partial polymer of a monomer mixture for an aromatic ring-containing (meth)acrylic copolymer, a photoinitiator, and a thermosetting crosslinking agent.
[0070] In some embodiments, the adhesive film may be formed from an adhesive film composition including a complete or partial polymer of a monomer mixture for an aromatic ring-containing (meth)acrylic copolymer, a photoinitiator, and a thermosetting crosslinking agent.
[0071] In some embodiments, the adhesive film may contain a portion of a monomer mixture for a (meth)acrylic copolymer having an aromatic ring.
[0072] The (meth)acrylic copolymer contains an aromatic group and a hydroxyl group, and can increase the peel strength and refractive index of the adhesive film.
[0073] The weight average molecular weight of the (meth)acrylic copolymer having an aromatic ring can be 200,000 g / mol to 3,000,000 g / mol, specifically 400,000 g / mol to 2,000,000 g / mol. If it is within the above range, the reliability of the adhesive film can be stably exhibited. The weight average molecular weight can be measured by a conventional method known to those skilled in the art, for example, by gel permeation chromatography using polystyrene as a standard sample.
[0074] The (meth)acrylic copolymer having an aromatic ring may include a (meth)acrylic copolymer of a monomer mixture including an aromatic ring-containing (meth)acrylic monomer and a hydroxyl group-containing (meth)acrylic monomer. The (meth)acrylic copolymer having an aromatic ring may be a random copolymer produced from the monomer mixture.
[0075] The monomer mixture essentially contains a (meth)acrylic monomer having two or more aromatic rings as an aromatic ring-containing (meth)acrylic monomer. This can easily ensure a refractive index of 1.55 or more even if the composition for adhesive film does not contain inorganic particles with a high refractive index. Here, the inorganic particles with a high refractive index have a refractive index of 1.55 or more, for example, inorganic particles with a refractive index of 1.55 to 3.0 can be, for example, zirconia, titania, zinc oxide, alumina, etc. When an adhesive film is produced from a composition containing inorganic particles with a high refractive index, the refractive index of the adhesive film can be easily increased, but there are problems such as the need to adjust the compatibility with the organic component in the composition, i.e., the (meth)acrylic copolymer, and an increase in haze of the adhesive film. The adhesive film of the present invention can have a refractive index of 1.55 or more even if it does not contain inorganic particles with a high refractive index.
[0076] The (meth)acrylic monomer having two or more aromatic rings also includes a (meth)acrylic monomer having a polycyclic group in which two or more aromatic monocyclic rings are bonded and / or condensed.
[0077] In one embodiment, the (meth)acrylic monomer having two or more aromatic rings may be contained in a content of 30% by mass or more, for example, 30% by mass, 35% by mass, 40% by mass, 45% by mass, 50% by mass, 55% by mass, 60% by mass, 65% by mass, 70% by mass, 75% by mass, 80% by mass, 85% by mass, 90% by mass, preferably 40% by mass to 95% by mass, more preferably 70% by mass to 90% by mass, based on the total mass of the monomer mixture being 100% by mass. If the content of the (meth)acrylic monomer having two or more aromatic rings is within the above range, it may be easy to make the refractive index of the adhesive film 1.55 or more, even without inorganic particles with a high refractive index.
[0078] In one embodiment, the (meth)acrylic monomer having two or more aromatic rings may have a homopolymer glass transition temperature of 0° C. or higher, for example, 0° C., 5° C., 10° C., 15° C., 20° C., 25° C., 30° C., 35° C., 40° C., 45° C., 50° C., 55° C., 60° C., preferably 0° C. to 60° C. The (meth)acrylic monomer having two or more aromatic rings has a homopolymer glass transition temperature that is much higher than that of a typical alkyl group-containing (meth)acrylic monomer or a hydroxyl group-containing (meth)acrylic monomer used in the manufacture of a (meth)acrylic binder contained in a typical (meth)acrylic adhesive film composition. This "homopolymer glass transition temperature" can be measured by a typical method known to those skilled in the art, or can be obtained by referring to a commercially available catalog or the like. For example, phenoxybenzyl (meth)acrylate may have a homopolymer glass transition temperature of 6°C, phenylphenoxyethyl (meth)acrylates including o-phenylphenoxyethyl acrylate and the like may have a homopolymer glass transition temperature of 33°C, biphenylylmethyl (meth)acrylates including 4-biphenylylmethyl (meth)acrylate and the like may have a homopolymer glass transition temperature of 6°C, and naphthyl acrylate may have a homopolymer glass transition temperature of 31°C.
[0079] In one embodiment, the (meth)acrylic monomer having two or more aromatic rings may have a surface tension of 40 mN / m or more at 25°C in the homopolymer state, for example, 40 mN / m or more, 45 mN / m or more, 50 mN / m or more, 55 mN / m or more, 60 mN / m, preferably 40 mN / m to 60 mN / m. In general, (meth)acrylic monomers having two or more aromatic rings tend to have a higher surface tension at 25°C than (meth)acrylic monomers having one aromatic ring, for example, benzyl (meth)acrylate. The "surface tension" can be measured by a conventional method known to those skilled in the art, or can be obtained by referring to a commercially available catalogue or the like. For example, phenoxybenzyl (meth)acrylate has a surface tension of 41 mN / m to 42 mN / m, phenylphenoxyethyl (meth)acrylate including o-phenylphenoxyethyl acrylate has a surface tension of 42 mN / m, biphenylylmethyl (meth)acrylate including 4-biphenylylmethyl (meth)acrylate has a surface tension of 42 mN / m to 43 mN / m, naphthyl acrylate has a surface tension of 44 mN / m to 45 mN / m, and benzyl acrylate may have a surface tension of 36 mN / m to 37 mN / m.
[0080] The adhesive film of the present invention, when produced from a composition containing a copolymer produced from a monomer mixture containing a large amount of a (meth)acrylic monomer having two or more aromatic rings, is characterized by simultaneously satisfying formula 1 and formula 2, providing excellent step conformability and excellent appearance, and reducing the rate of change in peel force over time.
[0081] In one embodiment, the (meth)acrylic monomer having two or more aromatic rings may include one or more of a (meth)acrylic monomer represented by the following chemical formula 1 and a (meth)acrylic monomer represented by the following chemical formula 2:
[0082] [ka]
[0083] In the above chemical formula 1, R 1 is a hydrogen atom or a methyl group, R 2 represents a single bond, a substituted or unsubstituted alkylene group having 1 to 10 carbon atoms, a substituted or unsubstituted monoalkyleneoxy group having 1 to 10 carbon atoms, or a substituted or unsubstituted polyalkyleneoxy group having 2 to 10 carbon atoms, R 3 represents a single bond, an oxygen atom, a substituted or unsubstituted alkylene group having 1 to 10 carbon atoms, a substituted or unsubstituted monoalkyleneoxy group having 1 to 10 carbon atoms, or a substituted or unsubstituted polyalkyleneoxy group having 2 to 10 carbon atoms, Ar 1 and Ar 2 are each independently a substituted or unsubstituted aryl group having 6 to 20 carbon atoms.
[0084] [ka]
[0085] In the above chemical formula 2, R 1 is a hydrogen atom or a methyl group, R 2 represents a single bond, a substituted or unsubstituted alkylene group having 1 to 10 carbon atoms, a substituted or unsubstituted monoalkyleneoxy group having 1 to 10 carbon atoms, or a substituted or unsubstituted polyalkyleneoxy group having 2 to 10 carbon atoms, Ar 3 is a substituted or unsubstituted aromatic fused ring group having 10 to 30 carbon atoms.
[0086] In the above Chemical Formula 1 and Chemical Formula 2, the alkyleneoxy group means "-RO-" (wherein R is an alkylene group having 1 to 10 carbon atoms).
[0087] In the present specification, in the term "substituted or unsubstituted," "substituted" means that one or more hydrogen atoms in the functional group are substituted with an aryl group having 6 to 10 carbon atoms, an arylalkyl group having 7 to 10 carbon atoms, an alkyl group having 1 to 5 carbon atoms, or the like.
[0088] For example, the (meth)acrylic monomer having two or more aromatic rings may include one or more, preferably two or more, of phenoxybenzyl (meth)acrylate, biphenylylmethyl (meth)acrylate including 4-biphenylylmethyl (meth)acrylate, phenylphenoxyethyl (meth)acrylate including o-phenylphenoxyethyl acrylate, biphenylyl (meth)acrylate including 4-biphenylyl (meth)acrylate, and naphthyl (meth)acrylate.
[0089] The monomer mixture may contain one or more (meth)acrylic monomers having two or more aromatic rings.
[0090] In some embodiments, the (meth)acrylic monomer having two or more aromatic rings may be contained in an amount of 80% by mass or more, for example, 80% by mass, 81% by mass, 82% by mass, 83% by mass, 84% by mass, 85% by mass, 86% by mass, 87% by mass, 88% by mass, 89% by mass, 90% by mass, 91% by mass, 92% by mass, 93% by mass, 94% by mass, 95% by mass, 96% by mass, 97% by mass, 98% by mass, 99% by mass, 100% by mass, for example, 90% by mass to 100% by mass.
[0091] The aromatic ring-containing (meth)acrylic monomer may further include a (meth)acrylic monomer having one aromatic ring. The (meth)acrylic monomer having one aromatic ring may include a common monomer known to those skilled in the art. For example, the monomer may include at least one selected from the group consisting of benzyl (meth)acrylate, phenoxyethyl (meth)acrylate, and (phenylthio)ethyl (meth)acrylate, but is not limited thereto.
[0092] The (meth)acrylic monomer having one aromatic ring may be contained in an amount of 30% by mass or less, for example, 0%, 5%, 10%, 15%, 20%, 25%, 30%, for example, 0% to 20% by mass, based on the total mass of the monomer mixture for producing the (meth)acrylic copolymer being 100% by mass. If the content of the (meth)acrylic monomer having one aromatic ring is within the above range, it will not affect the effects of the present invention and can help increase the refractive index.
[0093] The aromatic ring-containing (meth)acrylic monomer may be contained in a content of 30% by mass or more, for example, 30% by mass, 35% by mass, 40% by mass, 45% by mass, 50% by mass, 55% by mass, 60% by mass, 65% by mass, 70% by mass, 75% by mass, 80% by mass, 85% by mass, 90% by mass, preferably 40% by mass to 95% by mass, more preferably 50% by mass to 90% by mass, 70% by mass to 90% by mass, based on the total mass of the monomer mixture for producing the (meth)acrylic copolymer being 100% by mass. If the content of the aromatic ring-containing (meth)acrylic monomer is within the above range, it can help increase the refractive index of the adhesive film.
[0094] The hydroxyl group-containing (meth)acrylic monomer can provide the peeling force of the adhesive film.
[0095] The hydroxyl group-containing (meth)acrylic monomer may have a homopolymer glass transition temperature of −10° C. or lower, for example, −70° C., −65° C., −60° C., −55° C., −50° C., −45° C., −40° C., −35° C., −30° C., −25° C., −20° C., −15° C., or −10° C., for example, −70° C. to −10° C. If the glass transition temperature of the homopolymer of the hydroxyl group-containing (meth)acrylic monomer is within the above range, the peel strength of the pressure-sensitive adhesive film may be easily increased.
[0096] In some embodiments, the hydroxyl group-containing (meth)acrylic monomer may include one or more (meth)acrylates containing a linear or branched alkyl group having 1 to 10 carbon atoms containing one or more hydroxyl groups at the ester moiety. For example, the hydroxyl group-containing (meth)acrylic monomer may include at least one selected from the group consisting of 2-hydroxybutyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, and 6-hydroxyhexyl (meth)acrylate, but is not limited thereto.
[0097] The hydroxyl group-containing (meth)acrylic monomer may be contained in a content of 5% by mass to 70% by mass, for example, 5% by mass, 10% by mass, 15% by mass, 20% by mass, 25% by mass, 30% by mass, 35% by mass, 40% by mass, 45% by mass, 50% by mass, 55% by mass, 60% by mass, 65% by mass, 70% by mass, specifically 5% by mass to 60% by mass, 10% by mass to 50% by mass, 10% by mass to 30% by mass, based on the total mass of the monomer mixture for producing the (meth)acrylic copolymer being 100% by mass. If the content of the hydroxyl group-containing (meth)acrylic monomer is within the above range, the adhesive film can be provided with an effect of ensuring stability at high temperature and / or high humidity and enhancing peel strength.
[0098] The total content of the aromatic ring-containing (meth)acrylic monomer and the hydroxyl group-containing (meth)acrylic monomer may be 90% by mass or more, for example, 90% by mass, 91% by mass, 92% by mass, 93% by mass, 94% by mass, 95% by mass, 96% by mass, 97% by mass, 98% by mass, 99% by mass, 100% by mass, for example, 95% by mass to 100% by mass, based on the total mass of the monomer mixture for producing the (meth)acrylic copolymer. If the total content of the aromatic ring-containing (meth)acrylic monomer and the hydroxyl group-containing (meth)acrylic monomer is within the above range, the effect of the present invention may be easily realized.
[0099] The monomer mixture may not contain one or more of the following monomers: (meth)acrylic monomer having an alkyl group, (meth)acrylic monomer having an amide group, (meth)acrylic monomer having an alicyclic group, (meth)acrylic monomer having a heteroalicyclic group, (meth)acrylic monomer having a carboxylic acid group, (meth)acrylic monomer having an alkylene oxide group. However, the monomer mixture may contain a small amount of the above monomer within a range that does not interfere with the effects of the present invention, that is, a refractive index of 1.55 or more, excellent step followability, and low rate of change in peel force over time, thereby obtaining the effects of the addition of the above monomer. In some embodiments, the content of the above monomer may be 0% by mass to 5% by mass, for example, more than 0% by mass and 3% by mass or less, with the total mass of the monomer mixture for producing the (meth)acrylic copolymer being 100% by mass.
[0100] Specific compounds of the (meth)acrylic monomer having an alkyl group, the (meth)acrylic monomer having an amide group, the (meth)acrylic monomer having an alicyclic group, the (meth)acrylic monomer having a heteroalicyclic group, the (meth)acrylic monomer having a carboxylic acid group, and the (meth)acrylic monomer having an alkylene oxide group may include ordinary compounds known to those skilled in the art.
[0101] The (meth)acrylic monomer having an alkyl group may include a (meth)acrylic acid ester having a linear or branched alkyl group having 1 to 20 carbon atoms (preferably 2 to 20 carbon atoms). The (meth)acrylic acid ester having an alkyl group having 1 to 20 carbon atoms may include at least one selected from the group consisting of methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, n-butyl (meth)acrylate, iso-butyl (meth)acrylate, pentyl (meth)acrylate, hexyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, heptyl (meth)acrylate, octyl (meth)acrylate, iso-octyl (meth)acrylate, nonyl (meth)acrylate, decyl (meth)acrylate, and dodecyl (meth)acrylate, but is not limited thereto.
[0102] The (meth)acrylic copolymer can be produced by a conventional method known to those skilled in the art, for example, by adding a thermal polymerization initiator to the monomer mixture, polymerizing the mixture at a predetermined polymerization temperature for a predetermined polymerization time, and then purifying the resulting mixture.
[0103] In some embodiments, the (meth)acrylic copolymer is a random copolymer. The random copolymer can be produced by adding a monomer mixture for the (meth)acrylic copolymer to a reactor at once, then adding a polymerization initiator and carrying out a polymerization reaction.
[0104] The photoinitiator can be used when the adhesive film composition is applied to a substrate film or the like, dried to produce a coating film, and then photocured. The photoinitiator helps the adhesive film reach the ratio A represented by the above formula 1 and the ratio B represented by the above formula 2.
[0105] The photoinitiator may include a photoradical initiator that generates photoradicals by light such as UV light.
[0106] The photoinitiator may include a long-wavelength absorbing photoinitiator having a maximum absorption wavelength of 250 nm or more, for example, 300 nm to 400 nm. When UV is irradiated through the substrate film in the above maximum absorption wavelength range, a significant reduction in adhesive strength due to UV irradiation can be obtained, so the effect of the present invention can be obtained even with weak UV irradiation. Note that the "maximum absorption wavelength" refers to the wavelength at which the maximum absorbance appears when the photoinitiator is dissolved in cyclohexane to a concentration of 1 mg / ml and then the absorbance is measured.
[0107] Specifically, the photoinitiator may be a phosphine oxide-based, benzoin-based, hydroxyketone-based or aminoketone-based photoinitiator. For example, the photoinitiator may be an acetophenone compound such as benzoin, benzoin methyl ether, benzoin ethyl ether, benzoin isopropyl ether, benzoin n-butyl ether, benzoin isobutyl ether, 2,2-dimethoxy-2-phenylacetophenone, 2,2'-diethoxyacetophenone, 2,2'-dibutoxyacetophenone, 2-hydroxy-2-methylpropiophenone, pt-butyltrichloroacetophenone, pt-butyldichloroacetophenone, 4-chloroacetophenone, or 2,2'-dichloro-4-phenoxyacetophenone; 2-(4-(methylthio)phenyl)-2-morpholino-propan-1-one, 4-(2-hydroxyethoxy)phenyl-2-(hydroxy-2-propyl)ketone, benzophenone, p-phenylbenzophenone, 4,4- Examples of suitable benzoyl compounds include, but are not limited to, diethylaminobenzophenone, dichlorobenzophenone, 2-methylanthraquinone, 2-ethylanthraquinone, 2-t-butylanthraquinone, 2-aminoanthraquinone, 2-methylthioxanthone, 2-ethylthioxanthone, 2-chlorothioxanthone, 2,4-dimethylthioxanthone, 2,4-diethylthioxanthone, benzyl dimethyl ketal, acetophenone dimethyl ketal, p-dimethylaminobenzoic acid ester, oligo[2-hydroxy-2-methyl-1-[4-(1-methylvinyl)phenyl]propanone], and 2,4,6-trimethylbenzoyl-diphenyl-phosphine oxide.
[0108] The photoinitiator is used in an amount of 0.005 to 5 parts by mass, for example, 0.005 parts by mass, 0.01 parts by mass, 0.015 parts by mass, 0.02 parts by mass, 0.025 parts by mass, 0.03 parts by mass, 0.035 parts by mass, 0.04 parts by mass, 0.045 parts by mass, 0.05 parts by mass, 0.055 parts by mass, 0.06 parts by mass, 0.065 parts by mass, 0.07 parts by mass, 0. It may be included in the amount of 0.075 parts by weight, 0.08 parts by weight, 0.085 parts by weight, 0.09 parts by weight, 0.095 parts by weight, 0.1 parts by weight, 0.2 parts by weight, 0.3 parts by weight, 0.4 parts by weight, 0.5 parts by weight, 0.6 parts by weight, 0.7 parts by weight, 0.8 parts by weight, 0.9 parts by weight, 1 part by weight, 2 parts by weight, 3 parts by weight, 4.5 parts by weight, specifically 0.01 parts by weight to 3 parts by weight, more specifically 0.01 parts by weight to 0.1 parts by weight. If the content of the photoinitiator is within the above range, it helps to reach the ratio A represented by the above formula 1 and the ratio B represented by the above formula 2, and can prevent the generation of bubbles at high temperature reliability by controlling the peeling force and cohesive force.
[0109] The thermosetting crosslinking agent thermally cures the (meth)acrylic copolymer to form a matrix of the adhesive film, helping the adhesive film to reach the ratio A represented by the above formula 1 and the ratio B represented by the above formula 2.
[0110] The thermosetting crosslinking agent may be contained in an amount of 0.05 parts by mass or more and less than 5 parts by mass, for example, 0.05 parts by mass, 0.1 parts by mass, 0.15 parts by mass, 0.2 parts by mass, 0.25 parts by mass, 0.3 parts by mass, 0.35 parts by mass, 0.4 parts by mass, 0.45 parts by mass, 0.5 parts by mass, 0.55 parts by mass, 0.6 parts by mass, 0.65 parts by mass, 0.7 parts by mass, 0.75 parts by mass, 0.8 parts by mass, 0.85 parts by mass, 0.9 parts by mass, 1 part by mass, 2 parts by mass, 3 parts by mass, 4 parts by mass, specifically, 0.1 parts by mass to 2 parts by mass, more specifically, 0.1 parts by mass to 0.8 parts by mass, relative to 100 parts by mass of the (meth)acrylic polymer or monomer mixture. If the content of the thermosetting crosslinking agent is within the above range, the matrix of the adhesive film is well formed, helping to reach the ratio A represented by the above formula 1 and the ratio represented by the above formula 2.
[0111] The thermosetting crosslinking agent may include a typical thermosetting agent used when thermally curing a (meth)acrylic copolymer. For example, the crosslinking agent may include at least one selected from the group consisting of an isocyanate crosslinking agent, a carbodiimide crosslinking agent, an aziridine crosslinking agent, and an epoxy crosslinking agent. Preferably, the crosslinking agent includes an isocyanate crosslinking agent.
[0112] The isocyanate-based crosslinking agent may include a difunctional or higher, for example, a difunctional to hexafunctional isocyanate-type crosslinking agent. In one embodiment, the isocyanate-based crosslinking agent may include one or more of xylene diisocyanate (XDI) including m-xylene diisocyanate, methylene bis(phenylisocyanate) (MDI) including 4,4'-methylene bis(phenylisocyanate), naphthalene diisocyanate, tolylene diisocyanate, hexamethylene diisocyanate, isophorone diisocyanate, their adducts, or their isocyanurates. Examples of the adduct or isocyanurate include a trimethylolpropane adduct of tolylene diisocyanate, a trimethylolpropane adduct of hexamethylene diisocyanate, a trimethylolpropane adduct of isophorone diisocyanate, a trimethylolpropane adduct of xylylene diisocyanate, an isocyanurate of tolylene diisocyanate, an isocyanurate of hexamethylene diisocyanate, and an isocyanurate of isophorone diisocyanate.
[0113] In one embodiment, the adhesive film or the composition for an adhesive film may further include a leveling agent.
[0114] The leveling agent can be contained in a larger amount per 100 parts by mass of the (meth)acrylic polymer as compared to the thermosetting crosslinking agent.
[0115] The leveling agent is contained in an amount of more than 0.01 parts by mass and not more than 2 parts by mass, for example, 0.02 parts by mass, 0.03 parts by mass, 0.04 parts by mass, 0.05 parts by mass, 0.06 parts by mass, 0.07 parts by mass, 0.08 parts by mass, 0.09 parts by mass, 0.1 parts by mass, 0.2 parts by mass, 0.3 parts by mass, 0.4 parts by mass, 0.5 parts by mass, 0.6 parts by mass, 0.7 parts by mass, 0.8 parts by mass, 0.9 parts by mass, 1.0 parts by mass, 1.1 parts by mass, 1.2 parts by mass, 1.3 parts by mass, 1.4 parts by mass, 1.5 parts by mass, 1.6 parts by mass, 1.7 parts by mass, 1.8 parts by mass, 1.9 parts by mass, or 2 parts by mass, specifically, 0.05 parts by mass to 1.0 parts by mass, and more specifically, 0.1 parts by mass to 1.0 parts by mass. When the content of the leveling agent is within the above range, the surface energy of the PSA film can be reduced, thereby improving poor appearance.
[0116] The leveling agent may include at least one type of silicone-modified polyacrylate. The leveling agent may have a hydroxyl group (OH), which may facilitate the realization of the effects of the present invention.
[0117] The composition for a pressure-sensitive adhesive film according to the present invention may further contain a silane coupling agent.
[0118] The silane coupling agent plays a role in further increasing the peeling force of the adhesive film against the adherend. The silane coupling agent may include ordinary types known to those skilled in the art. For example, the silane coupling agent may include at least one selected from the group consisting of acetylacetone-based silane coupling agents; silicon compounds having an epoxy structure such as 3-glycidoxypropyltrimethoxysilane, 3-glycidoxypropylmethyldimethoxysilane, 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane; polymerizable unsaturated group-containing silicon compounds such as vinyltrimethoxysilane, vinyltriethoxysilane, (meth)acryloxypropyltrimethoxysilane; amino group-containing silicon compounds such as 3-aminopropyltrimethoxysilane, N-(2-aminoethyl)-3-aminopropyltrimethoxysilane, N-(2-aminoethyl)-3-aminopropylmethyldimethoxysilane; and 3-chloropropyltrimethoxysilane, but is not limited thereto. Preferably, the silane coupling agent may be an acetylacetone-based silane coupling agent.
[0119] The silane coupling agent is used in an amount of 0.01 to 2 parts by mass, for example, 0.05 parts by mass, 0.1 parts by mass, 0.15 parts by mass, 0.2 parts by mass, 0.25 parts by mass, 0.3 parts by mass, 0.35 parts by mass, 0.4 parts by mass, 0.45 parts by mass, 0.5 parts by mass, 0.55 parts by mass, 0.6 parts by mass, 0.65 parts by mass, 0.7 parts by mass, 0.75 parts by mass, 0.8 parts by mass, 0.85 parts by mass, 0.9 parts by mass, or the like, relative to 100 parts by mass of the (meth)acrylic polymer or the monomer mixture. Parts, 0.95 parts by mass, 1 part by mass, 1 part by mass, 1.05 parts by mass, 1.1 parts by mass, 1.15 parts by mass, 1.2 parts by mass, 1.25 parts by mass, 1.3 parts by mass, 1.35 parts by mass, 1.4 parts by mass, 1.45 parts by mass, 1.5 parts by mass, 1.55 parts by mass, 1.6 parts by mass, 1.65 parts by mass, 1.7 parts by mass, 1.75 parts by mass, 1.8 parts by mass, 1.85 parts by mass, 1.9 parts by mass, 1.95 parts by mass, or 2 parts by mass, specifically 0.05 parts by mass to 1 part by mass. If the content of the silane coupling agent is within the above range, it is possible to increase the peeling force of the adhesive film against the adherend while not affecting other physical properties of the adhesive film.
[0120] The adhesive film may further include an additive.
[0121] The additives may include conventional additives such as UV absorbers, antistatic agents, surfactants, curing accelerators, ionic liquids, lithium salts, softeners, molecular weight regulators, antioxidants, antiaging agents, stabilizers, tackifier resins, modifying resins (polyol resins, phenolic resins, acrylic resins, polyester resins, polyolefin resins, epoxy resins, epoxidized polybutadiene resins, etc.), defoamers, plasticizers, dyes, pigments (coloring pigments, extender pigments, etc.), treatment agents, fluorescent brighteners, dispersants, heat stabilizers, light stabilizers, flocculants, and lubricants, but are not limited to these.
[0122] The additive may be contained in an amount of 10% by mass or less, specifically 0.01% by mass to 10% by mass, specifically 0.01% by mass to 1% by mass, based on the total mass of the adhesive film. If the amount of the additive is within the above range, the adhesive strength and reliability of the adhesive film are not affected, and the additive effect can be exerted.
[0123] The adhesive film according to the present invention can be produced by coating one surface of a substrate film with the above-mentioned adhesive film composition to form a coating layer, drying the coating layer to form a coating film for an adhesive film, and then curing the coating film. After or before curing the coating film, a release film can be further laminated to one surface of the coating layer or the adhesive film in order to prevent foreign matter from adhering to the adhesive film. The substrate film is as described above. The release film is preferably a polymer film that has been subjected to a release treatment (e.g., silicon treatment or fluorine treatment), and may be a polyester film including a polyethylene terephthalate film, etc.
[0124] Drying may include, but is not limited to, a step of treating the coating layer at 100°C to 150°C for 0.5 to 5 minutes. Curing includes photocuring and thermal curing. Photocuring is a process in which the coating film is exposed to light such as UV at 200 mJ / cm2. 2~500mJ / cm 2 The heat curing (aging) may include a step of treating the coating film at 40° C. to 80° C. for 0.5 to 3 days, but is not limited thereto.
[0125] An optical member according to one embodiment of the present invention will be described below.
[0126] The optical member according to this embodiment includes the pressure-sensitive adhesive film of the present invention.
[0127] In one embodiment, the optical member includes an adhesive film and an adherend laminated on at least one surface of the adhesive film. In one embodiment, the adherend may have a higher refractive index than the adhesive film. A light emitting element panel is located on the lower surface of the adherend, and light incident from the light emitting element panel may be transmitted through the adherend, the adhesive film, etc. in order. The adhesive film of the present invention can increase the light extraction efficiency by lowering the difference in refractive index with the adherend compared to conventional adhesive films. For example, the adherend may have a refractive index of 1.5 or more, specifically 1.5 to 2.0, more specifically 1.7 to 2.0.
[0128] The optical display device of the present invention includes the pressure-sensitive adhesive film of the present invention or the optical member of the present invention. The optical display device may include a light-emitting display device including an organic light-emitting display device, a liquid crystal display device, or the like.
[0129] In one embodiment, the optical display device includes a display panel including one or more functional layers having a refractive index of 1.5 to 2, a first adhesive film, and an optical film, where the first adhesive film includes the adhesive film of the present invention.
[0130] According to one embodiment, in an optical display device, a display panel including a functional layer having a refractive index of 1.5 to 2, an adhesive film, and an optical film may be laminated in this order.
[0131] The display panel includes light emitting elements and emits light to drive the display device. The light emitting elements in the display panel may include, but are not limited to, organic light emitting diode (OLED), quantum dot display (QD), quantum dot organic light emitting diode (QD-OLED), etc.
[0132] The functional layer preferably has a refractive index of 1.5 to 2, and can provide an additional function when the optical display device or display panel is driven. The functional layer may have a single-layer structure or a multi-layer structure of two or more layers.
[0133] In one embodiment, the functional layer may include a touch screen panel, a passivation layer, etc. The touch screen panel receives input data on the screen so that the display device can perform a specific process by grasping the position of the touch on the screen of the optical display device with a hand or a pen. The touch screen panel may be made of a metal material such as aluminum or titanium. The passivation layer is an insulating layer, and may be composed of multiple layers made of one or more organic and inorganic materials.
[0134] The optical film may include a window film, a window, a polarizing plate, a color filter, a retardation film, an elliptical polarizing film, a reflective polarizing film, an anti-reflection film, a compensation film, a brightness enhancement film, an alignment film, a light diffusion film, a glass shatterproof film, etc. Preferably, the optical film may be a polarizing plate including a polarizer and a protective layer (e.g., a protective film or a protective coating layer) formed on at least one surface of the polarizer.
[0135] The above-mentioned base film may not be included between the optical film and the first adhesive film. This is because the base film is easily removed from the adhesive film by UV irradiation. This will be described in detail with reference to FIG. 1 below.
[0136] A second adhesive film may be further included between the optical film and the first adhesive film. The second adhesive film is not limited in type as long as it can provide high adhesion to the optical film. For example, the second adhesive film may be a pressure sensitive adhesive (PSA).
[0137] FIG. 1 is a schematic cross-sectional view of an optical display device according to one embodiment of the present invention.
[0138] 1, the optical display device may include a display panel 110, a touch screen panel 120, an adhesive film 140, and an optical film 150, which are sequentially laminated on an upper surface of the display panel 110. A passivation layer 130 is patterned and formed on an upper surface of the touch screen panel 120. The display panel, the touch screen panel, the adhesive film, the optical film, and the passivation layer are as described above. EXAMPLES
[0139] The present invention will be described in more detail with reference to the following preferred embodiments, which are merely illustrative of the present invention and should not be construed as limiting the present invention in any way.
[0140] Example 1 Eighty parts by mass of ethyl acetate was added to a 1 L reactor equipped with a cooling device for easy temperature control by refluxing nitrogen gas. 85 parts by mass of a mixture of 70 parts by mass of 4-biphenylylmethyl acrylate (Tg of homopolymer: 6°C) and 15 parts by mass of 2-phenylphenoxyethyl acrylate (Tg of homopolymer: 33°C) and 100 parts by mass of a monomer mixture containing 15 parts by mass of 4-hydroxybutyl acrylate (Tg of homopolymer: -30°C) were added to the reactor. Nitrogen gas was introduced into the reactor for 1 hour to remove oxygen from the monomer mixture, and the internal temperature of the reactor was maintained at 70°C. After the monomer mixture was stirred uniformly, 0.05 parts by mass of azobisisobutyronitrile, a polymerization initiator, was added and reacted for 4 hours to produce a solution containing a (meth)acrylic random copolymer (weight average molecular weight: 550,000 g / mol) containing aromatic groups (4-biphenyl groups and 2-phenylphenoxy groups) and hydroxyl groups. Ethyl acetate was then added to produce a solution with a solid content of 35% by mass.
[0141] On a solids basis, 100 parts by mass of the (meth)acrylic copolymer produced above, 0.04 parts by mass of a phosphorus-based initiator (Omnirad (registered trademark) TPO H, manufactured by IGM Resins BV) as a photoinitiator, 0.4 parts by mass of an isocyanate-based crosslinking agent (hexamethylene diisocyanate-based crosslinking agent, CK-164, manufactured by NCI) as a thermosetting crosslinking agent, 0.25 parts by mass of an acetylacetone-based silane coupling agent (A-50, manufactured by Soken Chemical & Engineering Co., Ltd.) as a silane coupling agent, and 0.8 parts by mass of a silane-based leveling agent (BYK (registered trademark)-Silclean 3700, manufactured by BYK) as a leveling agent were added, and the mixture was diluted with 10 parts by mass of toluene and stirred for 30 minutes to produce a composition.
[0142] The composition prepared above was applied to one side of a polyethylene terephthalate film (thickness: 75 μm, not release-treated) as a base film in a predetermined thickness and dried at 120° C. for 2 minutes to form a coating film for adhesive film with a thickness of 20 μm. The obtained coating film was covered with a polyethylene terephthalate film (thickness: 38 μm, release-treated) as a release film, and then 300 mJ / cm 2 was applied using a metal halide lamp. 2 The laminate was irradiated with UV light at an integrated light amount of 100000000000000000000000000 and cured (aged) at 50°C for 2 days to produce a laminate of the base film, adhesive film (thickness: 20 µm), and release film.
[0143] (Example 2, Example 3, Comparative Example 1 and Comparative Example 2) A laminate of a base film, an adhesive film, and a release film was produced in the same manner as in Example 1, except that the content of each component was changed as shown in Table 1 below (unit: parts by mass).
[0144] [Table 1]
[0145] The laminates produced in the examples and comparative examples were evaluated for the following physical properties, and the results are shown in Table 2 below.
[0146] (1) Storage modulus (unit: kPa): The storage modulus was measured for the adhesive film obtained by peeling off all the base film and release film from the laminate. The storage modulus was evaluated under temperature sweep conditions using a dynamic viscoelasticity measuring device ARES (manufactured by Anton Parr, MCR-501). A plurality of the above adhesive films were laminated to prepare a sample with a thickness of 600 μm. The laminate was perforated with a punching machine with a diameter of 8 mm to be used as a test piece. The storage modulus was obtained at the temperatures shown in Table 2 below while applying a normal force of 1.0 N to the test piece using an 8 mm jig, at a frequency of 1 Hz, strain: 1%, and at a temperature of -30°C to 100°C, while increasing the temperature at a rate of 10°C / min.
[0147] (2) Refractive index: The refractive index of an adhesive film obtained by separating the base film and the release film from the laminate was measured at a wavelength of 633 nm using a refractive index measuring instrument, Prism Coupler.
[0148] (3) Peeling force (unit: gf / inch, mN / mm): The release film was peeled off from the laminate (horizontal x vertical, 2.5 cm x 10 cm) of base film / adhesive film / release film produced in the examples and comparative examples. Then, the laminate of adhesive film / base film was attached to an alkali-free glass plate (horizontal x vertical, 3 cm x 10 cm) via the adhesive film to produce a test piece. The produced test piece was fixed to a peeling force measuring device manufactured by TA Instrument, and the peeling force was measured when peeling the adhesive film from the alkali-free glass plate at 25°C, a peeling speed of 300 mm / min, and a peeling angle of 180°. The peeling force values in units of mN / mm are also shown in Table 2 below.
[0149] (4) Step conformability: A plurality of patterns (width x length x height, 25 μm x 25 μm x 3 μm) spaced apart from each other were made on a glass plate using photoresist. The release film was removed from the laminates made in the examples and comparative examples, and the laminates were attached to the above-made patterns via an adhesive film at 25°C, and then autoclaved (50°C and 5.5 bar for 1000 seconds). The presence of air bubbles in the step portions of the pattern was confirmed with an optical microscope. If no air bubbles were generated, it was evaluated as OK, and if even a small amount of air bubbles were generated, it was evaluated as NG.
[0150] (5) Appearance: The adhesive film compositions obtained in the Examples and Comparative Examples were applied in one direction, and the surface of the adhesive film coating obtained by drying was rated as NG if it had straight lines (unevenness) in the direction of application, and OK if it had no lines. If there were lines, they would remain on the final adhesive film surface, degrading the appearance of the adhesive film.
[0151] (6) Change in peel strength over time (unit: %): After the release film was peeled off from the base film / adhesive film / release film laminate (horizontal x vertical, 2.5 cm x 10 cm) produced in the examples and comparative examples, the adhesive film / base film laminate was attached to an alkali-free glass plate (horizontal x vertical, 3 cm x 10 cm) via the adhesive film to produce a test specimen. The produced test specimen was fixed to a peel strength measuring device manufactured by TA Instrument, and the peel strength (PS1) was measured when peeling the adhesive film from the alkali-free glass plate at 25°C, a peel speed of 300 mm / min, and a peel angle of 180°.
[0152] The laminate was left in a constant temperature and humidity chamber at 50°C and 50% RH for 7 days, and then the peel strength (PS2) was measured in the same manner as above. The rate of change in peel strength over time was calculated using PS1, PS2, and the above formula 3.
[0153] (7) Reliability: The release film was peeled off from the laminates in the examples and comparative examples, and the laminates were attached to a glass plate via an adhesive film, then cut into a horizontal x vertical size (100 mm x 100 mm) and left in a chamber at 60°C and a relative humidity of 95% RH for 500 hours. If air bubbles or lifting occurred, it was rated as ×, and if air bubbles or lifting did not occur, it was rated as ○.
[0154] [Table 2]
[0155] As is clear from Table 2 above, the pressure-sensitive adhesive film of the present invention had a high refractive index, excellent step conformability and appearance, and high peel strength. In addition, the pressure-sensitive adhesive film of the present invention had a low rate of change in peel strength over time and was highly reliable.
[0156] On the other hand, the adhesive film of Comparative Example 1, in which the ratio A represented by the mathematical formula 1 according to the present invention does not satisfy the range of the present invention, had poor step conformability, appearance, and peel strength. The adhesive film of Comparative Example 2, in which the ratio A represented by the mathematical formula 1 according to the present invention and the ratio B represented by the mathematical formula 2 according to the present invention do not both satisfy the range of the present invention, had a too high rate of change in peel strength over time, and therefore had poor reliability.
[0157] Simple modifications or alterations of the present invention can be easily implemented by a person having ordinary skill in the art, and all such modifications and alterations can be considered to be included within the scope of the present invention. [Explanation of symbols]
[0158] 110 display panel, 120 touch screen panel, 130 passivation layer, 140 Adhesive film, 150 Optical Film.
Claims
1. An adhesive film comprising a (meth)acrylic copolymer having an aromatic ring, The pressure-sensitive adhesive film has a refractive index of 1.55 or more, The pressure-sensitive adhesive film has a ratio A represented by the following formula 1 of 1 to 8, and a ratio B represented by the following formula 2 of 1 to 15, The pressure-sensitive adhesive film has a storage modulus (G' 60 ) at 60° C. of 5 kPa to 70 kPa; The pressure-sensitive adhesive film has a storage modulus (G' 85 ) at 85° C. of 1 kPa to 60 kPa; The (meth)acrylic copolymer having an aromatic ring is a copolymer of a monomer mixture containing a (meth)acrylic monomer having an aromatic ring and a hydroxyl group-containing (meth)acrylic monomer, The (meth)acrylic monomer having an aromatic ring includes a (meth)acrylic monomer having two or more aromatic rings, the (meth)acrylic monomer having two or more aromatic rings is contained in an amount of 30% by mass to 95% by mass, with the total mass of the monomer mixture being 100% by mass; The hydroxyl group-containing (meth)acrylic monomer is contained in an amount of 5% by mass to 70% by mass, with the total mass of the monomer mixture being 100% by mass. [0010] In the above formula 1 and formula 2, G' 25 is the storage modulus of the adhesive film at 25 ° C. (unit: kPa), G' 60 is the storage modulus of the adhesive film at 60 ° C. (unit: kPa), G' 85 is the storage modulus (unit: kPa) of the adhesive film at 85°C.
2. The pressure-sensitive adhesive film according to claim 1, wherein the rate of change in peel strength over time, represented by the following formula 3, is 60% or less: [0025] In the above formula 3, PS1 is the initial peel strength of the adhesive film against the adherend (unit: gf / inch), PS2 is the peel strength (unit: gf / inch) of the pressure-sensitive adhesive film to the adherend after it has been left standing at 50° C. for 7 days.
3. The pressure-sensitive adhesive film according to claim 1 , wherein the pressure-sensitive adhesive film has a peel strength from an adherend of 400 gf / inch (154.4 mN / mm) or more.
4. The pressure-sensitive adhesive film according to claim 1 , further comprising a photoinitiator and a thermosetting crosslinking agent.
5. The pressure-sensitive adhesive film according to claim 1 , which is formed from a composition for pressure-sensitive adhesive films, the composition comprising the (meth)acrylic copolymer having an aromatic ring, a photoinitiator, and a thermosetting crosslinking agent.
6. The pressure-sensitive adhesive film according to claim 1 , wherein the (meth)acrylic monomer having two or more aromatic rings has a glass transition temperature of a homopolymer of 0° C. or higher.
7. The (meth)acrylic monomer having two or more aromatic rings includes at least one selected from the group consisting of phenoxybenzyl (meth)acrylate, biphenylyl methyl (meth)acrylate, phenylphenoxyethyl (meth)acrylate, biphenylyl (meth)acrylate, and naphthyl (meth)acrylate. The pressure-sensitive adhesive film according to claim 1.
8. The pressure-sensitive adhesive film according to claim 1, wherein the monomer mixture has a content of the (meth)acrylic monomer having two or more aromatic rings of 40% by mass to 95% by mass and a content of the hydroxyl group-containing (meth)acrylic monomer of 5% by mass to 60% by mass, where the total mass of the monomer mixture is 100% by mass.
9. The pressure-sensitive adhesive film composition comprises 100 parts by mass of the (meth)acrylic copolymer having an aromatic ring, 0.005 parts by mass to 5 parts by mass of the photoinitiator, and 0.05 parts by mass or more and less than 5 parts by mass of the thermosetting crosslinking agent. The pressure-sensitive adhesive film according to claim 5.
10. The pressure-sensitive adhesive film according to claim 4 , further comprising a leveling agent.
11. The pressure-sensitive adhesive film according to claim 10, wherein the leveling agent comprises one or more silicone-modified polyacrylates.
12. The pressure-sensitive adhesive film according to claim 1 , wherein the (meth)acrylic copolymer having an aromatic group is a random copolymer.
13. An optical member comprising the pressure-sensitive adhesive film according to any one of claims 1 to 12.
14. An optical display device comprising the pressure-sensitive adhesive film according to any one of claims 1 to 12.
Citation Information
Patent Citations
Pressure-sensitive adhesive composition for sticking / fixing of optical film to liquid crystal panel, pressure-sensitive adhesive sheet, and optical film
JP2010196064A
Optically compensated acrylic adhesive composition, polarizing plate and liquid crystal display element containing the same
JP2010516855A
Acrylic adhesive composition
JP2011510114A
Optical components, adhesive compositions, and liquid crystal display devices
JP2015525368A
Adhesive sheet
JP2019065113A