Lens manufacturing method
A hydrophilic inorganic surface treatment film on lenses addresses abrasion and deterioration issues, ensuring durable optical performance by maintaining hydrophilicity and optical clarity under harsh outdoor conditions.
Patent Information
- Application Number
- JP2023186897
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2023-10-31
- Publication Date
- 2024-10-09
- Estimated Expiration
- 2039-03-12
AI Technical Summary
Conventional optical lenses used in outdoor environments, such as surveillance cameras, suffer from surface treatment films peeling off due to abrasion, trapping foreign matter, and deteriorating under harsh conditions, leading to impaired optical performance.
A hydrophilic surface treatment film made of inorganic materials, such as silica and titania compounds, is applied to the lens surface, ensuring a contact angle of less than 10° and a haze value of less than 1.0%, providing high abrasion resistance and maintaining hydrophilicity over time.
The lens maintains high hydrophilicity and optical properties, resisting damage from dust and water, even under prolonged exposure to sunlight, with the titania compound restoring surface conditions through photocatalytic action.
Smart Images

Figure 0007564928000002 
Figure 0007564928000001
Abstract
Description
[Technical field]
[0001] The present disclosure relates to a lens used in an imaging device such as a camera, a manufacturing method for the lens, and a lens unit equipped with the lens, and in particular to a lens that can maintain good optical properties even when used outdoors where the surface is exposed to water droplets such as rainwater, a manufacturing method thereof, and a lens unit. [Background technology]
[0002] 2. Description of the Related Art With the advancement of technological developments in image pickup elements such as charge-coupled devices (CCDs) and complementary metal oxide semiconductors (CMOSs), various cameras have been commercialized as imaging devices that use these image pickup elements to capture still images and moving images.
[0003] In recent years, imaging elements have become smaller, more sensitive, and less expensive, and lighter and less expensive plastic lens technology, data processing technology for compressing and recording imaging data, and memory element technology for recording large amounts of data at high speed have also developed, so it has become commonplace to capture still and moving images using so-called portable electronic information devices such as mobile phones, smartphones, tablet terminals, and portable game consoles, rather than using dedicated devices for recording still and moving images such as digital still cameras and digital video cameras. In addition, with the spread of imaging devices for capturing images, there are more opportunities to use cameras, which are precision products, in environments where they were not previously brought in, and there are also increasing applications such as cameras capable of underwater photography, information acquisition cameras for automatically controlling devices, monitor cameras mounted on robots, and surveillance cameras for fixed-point observation.
[0004] In particular, since monitor cameras and surveillance cameras are often used outdoors, raindrops and other water droplets and dust adhere to the lens located on the outermost surface of the camera lens, which is closest to the subject. In addition, fogging and condensation may occur on the surface of the optical element due to changes in the surrounding temperature environment. For this reason, in monitor cameras and surveillance cameras, the lens located on the outermost surface of the camera lens is subjected to a surface treatment to ensure a good field of view at all times regardless of the external environment.
[0005] As an optical lens with such a surface treatment film, an optical lens has been proposed in which a hard coat layer is disposed on the lens substrate side, an ultra-water-repellent layer is disposed on the outermost surface, and a scratch-resistant anti-reflection film having a multi-layer laminate structure including a high refractive index layer divided into multiple layers is formed in the intermediate portion between them (see Patent Document 1).An optical lens has also been proposed in which a coating that is an anti-reflection film and a surface protection film on the outer surface is formed by forming minute concave and convex portions using an inorganic-organic composite containing inorganic compound particles and a polymer bonded thereto (see Patent Document 2). [Prior art documents] [Patent documents]
[0006] [Patent Document 1] JP 2016-173613 A [Patent Document 2] JP 2015-091981 A Summary of the Invention [Problem to be solved by the invention]
[0007] The above conventional optical lenses have a surface treatment film formed on their surface that has anti-reflection and lens protection functions, and therefore, even when plastic lenses, which are easy to process, are used as the lenses, the optical properties can be improved and the problem specific to plastic lenses, that is, they are easily scratched, can be solved.
[0008] However, for example, in the case of optical lenses used in imaging devices such as security cameras installed outdoors, it must be assumed that liquids such as rain or muddy water will adhere to the outer surface. In addition, it is also possible that minute foreign objects such as sand and dust will strongly strike the lens surface. Furthermore, when a user performs maintenance, it is assumed that a cloth or the like will be rubbed against the lens surface to remove any adhering dirt.
[0009] However, the surface treatment films used in the above conventional optical lenses are not designed for use under the harsh conditions associated with outdoor use, and problems have arisen such as the surface being peeled off when the surface is strongly rubbed, fine irregularities are generated on the surface of the surface treatment film, and foreign matter is trapped between the irregularities. In addition, when exposed to sunlight for a long period of time, deterioration of the surface treatment film due to ultraviolet rays has often become an issue.
[0010] Furthermore, there was also the problem that water droplets formed on the surface due to condensation or rain could prevent a normal image from being obtained.
[0011] The present disclosure is devised to solve the above-mentioned problems of the conventional art, and aims to provide a lens, a lens manufacturing method, and a lens unit that can maintain optical properties for a long period of time even when used under harsh conditions such as optical lenses intended for outdoor use, where foreign matter such as water and dust is likely to adhere and where the surface is subject to abrasion. [Means for solving the problem]
[0012] In order to solve the above problems, the present application discloses a lens manufacturing method for forming a hydrophilic surface treatment film on the surface of a lens used in an optical system, characterized in that a hydrophilic treatment liquid containing a silica compound as a filler in an inorganic binder is applied to the surface of the lens, and then dried to form the surface treatment film. Effect of the Invention
[0013] The lens disclosed in this application has a surface treatment film formed on the subject-side surface that is made of an inorganic material, a contact angle with water of less than 10°, and a lens haze value of less than 1.0%, which makes the surface highly resistant to abrasion and allows it to maintain high hydrophilicity and optical properties even over time.
[0014] In addition, the lens manufacturing method disclosed in the present application forms a surface treatment film by applying a hydrophilic treatment liquid containing a silica compound as a filler in an inorganic binder to the lens surface and drying it, which makes it possible to easily manufacture a surface treatment film made of a highly durable inorganic material.
[0015] Furthermore, in the lens unit disclosed in the present application, a lens disposed on the subject-side surface of the lens optical system is any of the lenses disclosed in the present application, or a lens manufactured by any of the manufacturing methods disclosed in the present application, thereby making it possible to realize a lens unit with high durability in actual use conditions. [Brief description of the drawings]
[0016] [Figure 1] 1 is a conceptual diagram illustrating a configuration of an imaging device including a lens according to an embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0017] The lens disclosed in the present application is used in an imaging device and is placed at the outermost surface of a lens optical system, wherein a surface treatment film formed on the subject-side surface of the lens is made of an inorganic material, the contact angle of the surface treatment film with water is less than 10°, and the haze value of the lens on which the surface treatment film is formed is less than 1.0%.
[0018] By doing this, the lens disclosed in the present application can be realized as a lens that is placed on the outermost surface facing the subject and has a surface that is resistant to damage even if dust or the like is blown onto it, and that can maintain high hydrophilicity and optical properties even when exposed to sunlight for long periods of time.
[0019] In the lens of the present disclosure, it is preferable that the surface treatment film further contains a titania compound, whereby the surface condition of the surface treatment film is restored by the photocatalytic action of the titania compound, and high hydrophilicity can be maintained for a long period of time.
[0020] The lens manufacturing method disclosed in the present application is a lens manufacturing method for forming a hydrophilic surface treatment film on the surface of a lens used in an optical system, in which a hydrophilic treatment liquid containing a silica compound as a filler in an inorganic binder is applied to the surface of the lens, and then dried to form the surface treatment film.
[0021] In this way, the lens manufacturing method disclosed in the present application can easily form a surface treatment film made of an inorganic material.
[0022] In the lens manufacturing method disclosed in the present application, it is preferable that the hydrophilic treatment liquid further contains a titania compound as a filler, which allows the photocatalytic action of the titania compound to restore the surface condition of the surface treatment film, making it possible to easily manufacture lenses that can maintain high hydrophilicity for a long period of time.
[0023] Furthermore, it is preferable that the coating thickness of the hydrophilic treatment liquid is in the range of 2 to 10 times the average particle size of the particles contained in the hydrophilic treatment liquid, thereby forming a surface treatment film with small haze and little adverse effect on transmitted light.
[0024] In the lens manufacturing method disclosed in the present application, it is preferable to set the contact angle of the surface treatment film with water to less than 10°, and the haze value of the lens on which the surface treatment film is formed to less than 1.0%.
[0025] Furthermore, the lens unit disclosed in the present application includes a lens optical system, an image sensor, and a housing that houses the lens optical system and the image sensor, and the lens arranged on the subject-side surface of the lens optical system is any of the lenses disclosed in the present application or a lens manufactured by any of the manufacturing methods disclosed in the present application.
[0026] In this way, the lens placed on the subject-side surface can maintain high hydrophilicity and optical properties, and a lens unit that can withstand long-term use can be realized.
[0027] (Embodiment) DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS Hereinafter, embodiments of a lens, a manufacturing method thereof, and a lens unit according to the present disclosure will be described with reference to the drawings.
[0028] In the following, an imaging device used as an imaging unit of a surveillance camera will be described as an example of the lens unit disclosed in the present application, and the lens disposed closest to the subject of this imaging device will be described as an example of the lens disclosed in the present application.
[0029] FIG. 1 is a diagram illustrating a schematic configuration of an imaging device in which a lens disclosed in the present application is used.
[0030] As shown in FIG. 1, an imaging device 100 used as an imaging unit of a surveillance camera is made up of a lens optical system 10 made up of one or more lenses, and an imaging section 20 that captures an image.
[0031] The lens optical system 10, which irradiates light to be imaged by the imaging unit 20, is configured by arranging multiple lenses 12-16 (five in FIG. 1) inside a substantially cylindrical body 11. In the rest of this specification, a single lens will be referred to simply as a "lens," and the complex of lenses that irradiates a subject image onto the imaging element 21 of the imaging unit 20 as a whole will be referred to as the "lens optical system." For this reason, an arrangement of multiple single lenses within a housing as shown in FIG. 1 is a "lens optical system," and there is no restriction on the number of "lenses" that constitute the "lens optical system," and a system composed of only one lens is also included in the concept of the "lens optical system."
[0032] In the example of lens optical system 10 shown in Figure 1, five lenses are arranged, in order from the subject side (the camera's field of view) indicated by arrow A in Figure 1, namely, a first lens 12 that constitutes an objective lens group, a second lens 13, a third lens 14 as an intermediate lens, a fourth lens 15 that constitutes an eyepiece (image sensor side) lens group, and a fifth lens 16, at a predetermined interval and so that the optical axes of each of the lenses 12 to 16 are aligned.
[0033] In the lens optical system 10 of this embodiment, a surface treatment film 17, which is a hydrophilic film, is formed on the outer side of the first lens 12, which is the lens that is located closest to the subject among the multiple lenses, i.e., on the surface that is the surface on the subject side and is the outermost surface of the lens optical system 10.
[0034] In the lens optical system 10 of the imaging device shown in FIG. 1, a configuration of 3 groups and 5 lenses 12 to 16 is illustrated. In general, by increasing the number of lenses constituting the lens optical system and stacking different types of lenses such as convex lenses, concave lenses, and aspherical lenses, a lens optical system with higher optical properties can be realized, such as a wide-angle lens with a wide viewing angle and low image distortion, a high-magnification telephoto lens, and a zoom lens with an intermediate lens that can be moved back and forth. On the other hand, since an increase in the number of lenses leads to an increase in the cost of the lens optical system, a specific lens configuration is actually determined according to the optical properties required for the imaging device in which the lens optical system is used. For example, in the case of a camera that does not have a problem with images with a relatively low resolution or images with some distortion, the lens optical system may be configured with two lenses, or at most three lenses. On the other hand, a lens optical system with high resolution and high zoom magnification adopts a lens design having multiple lens groups combining a large number of lenses, such as a 4-group 7-element configuration.
[0035] Regardless of the number of lenses or the arrangement of the lens groups, the lens optical system 10 according to this embodiment only needs to have a surface treatment film 17 formed on the lens 12 located in the uppermost layer (outermost layer) of the lens 10 optical system, that is, on the subject-side surface of the lens 12 located closest to the subject among all the lenses, like the lens 12 in Fig. 1. For example, in order to prevent stray light from adversely affecting an image inside the lens housing, a surface treatment film may be formed on a surface other than the uppermost layer of the lenses constituting the lens optical system, but such a film is different from the surface treatment film 17 according to this embodiment.
[0036] 1, the imaging section 20 of the imaging device 100 used in a surveillance camera is disposed on the rear side of the lens optical system 10, indicated by the arrow B in Fig. 1, and is configured such that an imaging element 21, such as a CMOS or a CCD, is disposed on a circuit board 22. The circuit board 22 is equipped with a power supply line for driving the imaging element 21, a drive control circuit for controlling the imaging element 21 to obtain electrical signals from each pixel as image data, a signal line for transmitting captured image data to the outside, and the like, which are not shown in the figure.
[0037] 1, the imaging device 100 holds the lens optical system 10 and the imaging section 20, and regulates the imaging element 21 to be correctly positioned at the focal position of the lens optical system 10, and the lens optical system 10 and the imaging section 20 are integrated as a module by a unit housing that blocks stray light from the outside that becomes noise in the captured image. Therefore, a user can obtain an image captured by the imaging element 21 as an image signal from a signal output line by supplying power of a predetermined voltage value to the imaging unit.
[0038] On the surface of the lens according to this embodiment, a surface treatment film 17 is applied over the entire surface facing the subject, as shown in cross section in Fig. 1. Details of this surface treatment film 17 and a method for manufacturing a lens on which the surface treatment film is formed will be described below.
[0039] The surface treatment film 17 formed on the lens 12 according to this embodiment is a hydrophilic film (having a contact angle with water of less than 10°) composed of a binder made of an inorganic material and a filler made of a silica compound and / or a titania compound. That is, the surface treatment film 17 formed on the surface of the lens 12 according to this embodiment is entirely composed of inorganic materials, and in particular does not use an organic binder that has been generally used in the past as a surface treatment film for lenses.
[0040] In the present embodiment, the entire surface of the lens 12 is covered with a hydrophilic surface treatment film 17, so that even if raindrops fall on the surface of the lens 12, the raindrops cannot maintain their shape but spread out and become a film. Therefore, the subject photographed through the lens is not obstructed by waterdrops adhering to the lens surface, and a clear captured image can be obtained.
[0041] So-called water glass, that is, an aqueous solution of sodium silicate Na2SiO2 (sodium silicate: Na2·nSiO2·mH2O) can be suitably used as a binder for the inorganic material of the surface treatment film 17. The molar ratio of silicon to alkali (SiO2 / A2O+B; A=alkali metal, B=NH3) is preferably 4 to 30, and the silicon oxide equivalent concentration (SiO2 concentration) is preferably 6.8 to 30% by weight.
[0042] The surface treatment film 17 of the lens 12 in this embodiment can be formed by applying a hydrophilic treatment liquid containing an inorganic binder and, as a filler, silica, i.e., a silicon dioxide (SiO2) compound, or titania, i.e., a titanium oxide (TiO2) compound, or both a silica compound and a titania compound, to the surface of the lens 12 and drying it.
[0043] By setting the average particle size of the primary particles of the filler in the hydrophilic treatment liquid to 100 nm or less, it is possible to prevent the harmful effect that the transmitted light passing through the surface treatment film 17 is scattered, the optical image entering the imaging unit 20 through the lens is distorted, and the definition of the captured image is reduced. In order to minimize the deterioration of the optical characteristics of the lens, it is more preferable that the film thickness of the surface treatment film 17 is 100 nm or less, and even more preferable that it is 50 nm or less.
[0044] The inventors have confirmed that, from the viewpoint of preventing unevenness due to the filler from being formed on the surface of the surface treatment film 17 and preventing adverse effects such as distortion on an image through a lens, it is preferable that the ratio of the film thickness of the surface treatment film to the particle size of the filler (film thickness / average particle size) is 2 to 10, that is, the coating film thickness of the hydrophilic treatment liquid is in the range of 2 to 10 times the average particle size of the particles contained in the hydrophilic treatment liquid, and it is more preferable that the film thickness ratio (film thickness / average particle size) is about 5. For this reason, for example, when the film thickness of the surface treatment film 17 is set to 50 nm, it is preferable that the average particle size of the primary particles of the silica compound and / or titania compound, which are the filler, is 10 nm or less.
[0045] As a method for forming the surface treatment film 17 on the surface of the lens 12, since water glass having a relatively high viscosity is used as an inorganic binder of the hydrophilic treatment liquid as described above, various coating methods suitable for coating a highly viscous liquid, such as a so-called brush coating method using a coater having a dedicated coating member or a dip coating method using a dip coater, can be used. After coating the lens surface to a predetermined thickness, the surface treatment film 17 is formed by drying at a temperature of, for example, about 100°C. The lens 12 on which the surface treatment film 17 is formed can be either a so-called plastic lens made of resin or a glass lens, and there is no particular restriction on the lens material.
[0046] [Example] Below, a surface treatment film was applied to the lens according to this embodiment under various conditions, and the hydrophilicity and optical properties were confirmed.
[0047] In Example 1, a hydrophilic treatment liquid "Cleanfast MS" (product name: manufactured by Toso Sangyo Co., Ltd.) containing water glass as a binder and a silica compound (content 5%) as a filler was applied to one surface of a glass lens (diameter 10 mm) whose surface had been cleaned using a dip coater, and then dried at 100°C for 3 minutes to produce a glass lens on which a surface treatment film was formed. The average particle size of the hydrophilic treatment liquid was 10 nm, the film thickness of the surface treatment film was 50 nm, and the ratio of the film thickness of the surface treatment film to the average particle size was 5.
[0048] Furthermore, using the same hydrophilic treatment liquid, a glass lens of Example 2 in which the surface treatment film on the lens surface was made to a thickness of 20 nm, and a glass lens of Example 3 in which the surface treatment film was made to a thickness of 100 nm were produced.
[0049] As Example 4, a glass lens on which a surface treatment film was formed was obtained by the same method as in Example 1, using a hydrophilic treatment liquid "Cleanfast MT-01" (product name: manufactured by Toso Sangyo Co., Ltd.) containing 5% of a titania compound as a filler relative to the content of the silica compound. The average particle size of the hydrophilic treatment liquid was 10 nm, the same as in Example 1, and the film thickness of the surface treatment film was 50 nm. The ratio of the average particle size to the film thickness of the surface treatment film was 5, the same as in Example 1.
[0050] As Example 5, a hydrophilic treatment liquid "CLEANFAST MT-03" (product name: manufactured by Toso Sangyo Co., Ltd.) containing 15% of a titania compound as a filler relative to the content of a silica compound was used to obtain a glass lens on which a surface treatment film was formed in the same manner as in Example 1. The average particle size of the hydrophilic treatment liquid was 10 nm, the film thickness of the surface treatment film was 50 nm, and the value of the ratio of film thickness to average particle size was 5, similar to Examples 1 and 4.
[0051] Next, as Comparative Example 1, a surface treatment film having a coating thickness of 10 nm (ratio of film thickness / average particle diameter=1) was formed using the same hydrophilic treatment liquid as used in Example 1. Furthermore, as Comparative Example 2, a glass lens having a surface treatment film having a coating thickness of 150 nm (ratio of film thickness / average particle diameter=15) was formed using the same hydrophilic treatment liquid as used in Example 1.
[0052] Furthermore, a hydrophilic treatment liquid "Cleanfast FA" (product name: manufactured by Toso Sangyo Co., Ltd.) having a filler of a silica compound in a binder containing an organic material (urethane) and an inorganic material (water glass) was used to produce a glass lens of Comparative Example 3. The average particle size of the hydrophilic treatment liquid was 150 nm, and the coating thickness of the surface treatment film was 200 nm (film thickness / average particle size=1.3).
[0053] Furthermore, as the glass lens having the surface treatment film of Comparative Example 4, a lens having a surface treatment film with a thickness of 150 nm was produced using a hydrophilic treatment liquid "Cleanfast CMT-2" (product name: manufactured by Toso Sangyo Co., Ltd.) having an average particle size of 150 nm and containing a silica compound filler in an inorganic material (water glass) binder.
[0054] Furthermore, a hydrophilic treatment liquid "Cleanfast MK-01" (product name: manufactured by Toso Sangyo Co., Ltd.) having a binder containing an organic material (urethane) and an inorganic material (water glass) and 1% filler of a titania compound and a silica compound was used to produce a glass lens of Comparative Example 5. The average particle size of the hydrophilic treatment liquid was 150 nm, and the coating thickness of the surface treatment film was 200 nm (film thickness / average particle size=1.3).
[0055] In each of the above examples and comparative examples, the particle size of the hydrophilic treatment liquid was measured using a particle size distribution measuring device "Multisizer 4e" (product name) manufactured by Beckman Coulter, Inc. The thickness of the surface treatment film was obtained by simulating the reflectance of the lens formed with the obtained surface treatment film using "Multichannel Spectrometer MCPD-3000" (product name) manufactured by Otsuka Electronics Co., Ltd.
[0056] For the glass lenses of Examples 1 to 5 and Comparative Examples 1 to 5 thus prepared, the water contact angle of the surface treatment film in the initial state was measured 10 seconds after 1 μL of water was dropped using a wettability evaluation device (contact angle meter) "LSE-B100TW" (product name) manufactured by NIC Co., Ltd. In addition, the haze value was measured as an optical characteristic in the initial state using a haze meter "NDH 2000" (product name) manufactured by Nippon Denshoku Industries Co., Ltd.
[0057] After measuring the initial water contact angle and haze value, an abrasion test was conducted, simulating the situation in which fine foreign matter is sprayed onto the lens surface during actual use, or the user wipes off dust from the surface. Specifically, a hand-washing brush called "Nylon Soft" (product name: AS ONE Corporation), which is made of nylon bristles with a diameter of 0.2 mm and a length of 20 mm, was used and swept back and forth 100 times with a load of 1 kg.
[0058] After the abrasion test, the contact angle and haze value of the surface treatment film were measured again for each of the glass lenses of Examples 1 to 5 and Comparative Examples 1 to 5 in the same manner as in the initial state.
[0059] In addition, for the glass lenses of Examples 4 and 5, which contain a titania compound in the binder, and Comparative Example 5, after the contact angle and haze value were measured after the abrasion test, UV light was further irradiated. Specifically, using a handy UV lamp "LUV-16" (product name) manufactured by AS ONE Corporation, ultraviolet light with a wavelength of 365 nm was irradiated from two 8 W discharge tubes for 5 hours, and the degree of recovery of the characteristic values due to the so-called photocatalytic action of the titania compound, which repaired the surface treatment film that had been scratched in the abrasion test, was measured.
[0060] For Examples 1 to 5 and Comparative Examples 1 to 5, the state of the surface treatment film, the contact angle with water, and the haze value were measured, and the results are shown in Table 1 below.
[0061] In addition, the surface treatment film of Comparative Example 2, which was prepared using the same hydrophilic treatment liquid as in Examples 1 to 3 to give a thickness of 150 nm, had many cracks when dried after application and could not be formed as a coating film, so the contact angle with water and the haze value were not measured.
[0062] [Table 1]
[0063] As shown in Table 1, the glass lens of Example 1, which was formed from a hydrophilic treatment liquid containing a silica compound filler with an average particle size of 10 nm in a water glass binder and was coated with a surface treatment film having a thickness of 50 nm and a ratio of film thickness to average particle size of 5, showed high hydrophilicity with an initial contact angle with water of 4° and a haze value of 0.5%, indicating very good optical properties. Even after the abrasion test, the glass lens of Example 1 maintained high hydrophilicity with a contact angle of 8°, and although the haze value increased slightly to 0.6%, no significant change occurred in the optical properties, indicating high abrasion resistance.
[0064] When the thickness of the same hydrophilic treatment film as in Example 1 was changed, the glass lens of Example 2, in which the surface treatment film had a thickness of 20 nm, and the glass lens of Example 3, in which the surface treatment film had a thickness of 100 nm, both showed the same initial contact angle and haze value as the glass lens of Example 1.
[0065] It was also confirmed that the values after the abrasion test also had high properties, with a contact angle of less than 10° and a haze value of less than 1.0%. It was also confirmed from the measurement results of the glass lenses of the three examples with different film thicknesses that the contact angle and haze value after the abrasion test both tended to be higher as the film thickness increased.
[0066] In contrast, in the glass lens of Comparative Example 1, which has a thin film thickness of 10 nm, the initial contact angle and haze value are similar to those of the glass lenses of Examples 1 to 3, but after the abrasion test, the water contact angle was 15° and the haze value was 1.2%, and it was not possible to maintain the water contact angle of less than 10° and the haze value of less than 1.0%, which were assumed to be in a good range. At this time, when the upper surface of the surface treatment film was observed, many fine sliding scratches were confirmed. This is thought to be because the surface treatment film was peeled off during the abrasion test due to the thin film thickness of 10 nm, and the surface of the glass lens was damaged. In addition, as described above, if the coating thickness of the hydrophilic treatment liquid applied to the front surface of the glass lens is 150 nm, a good surface treatment film is not formed due to cracks during drying. For this reason, it was found that the suitable film thickness range of the surface treatment film is about 20 nm to 100 nm.
[0067] In addition, in the glass lens of Example 4 having a surface treatment film formed by a hydrophilic treatment film containing 5% titania compound in silica compound as a binder filler, the initial contact angle was 5° and the haze value was 0.7, which is as good as the case of only silica compound as a filler, but it was confirmed that the contact angle after the abrasion test was large at 12°, and the hydrophilicity was reduced. On the other hand, it was found that the contact angle was restored to 6°, a value almost close to the initial state, by irradiating the glass lens after the abrasion test with UV light. This is thought to be because the photocatalytic action of the titania compound repaired the fine unevenness on the surface of the surface treatment film, removing dirt, and thus restoring the hydrophilicity of the surface treatment film.
[0068] In the case of the glass lens of Example 5, in which the ratio of the titania compound in the filler of the hydrophilic treatment liquid was 15%, the contact angle after the abrasion test increased significantly to 14°, but it was confirmed that the contact angle recovered to 5°, the same as the initial contact angle, by irradiation with UV light.
[0069] In this way, when the binder of the hydrophilic treatment liquid forming the surface treatment film contains a titania compound as a filler, the initial hydrophilicity can be realized at almost the same level as when the filler does not contain a titania compound and only contains a silica compound, and although the contact angle increases and the hydrophilicity decreases as the surface is worn, it was confirmed that the hydrophilicity is restored by the photocatalytic action of the titania compound when irradiated with UV light. In the case of a surface treatment film formed by a hydrophilic treatment liquid containing only a silica compound and not a titania compound as a filler, the hydrophilicity of the surface, which gradually decreases over a long period of time, is not restored, but by containing a titania compound, it is expected that the hydrophilicity will be restored to a state close to the initial state, so for example, in the case of a lens used in a lens unit used in a surveillance camera installed outdoors where sunlight is exposed, it is preferable to include a titania compound in the filler of the binder of the hydrophilic treatment liquid.
[0070] In addition, in the case of a lens module placed in a place exposed to sunlight in an actual usage state, the surface of the surface treatment film is continuously irradiated with UV light immediately after the start of use. Therefore, as shown in the experimental results in Table 1, it is expected that the photocatalytic action of the titania compound will work at any time before the surface treatment film is worn away and the hydrophilicity is significantly reduced, and the state of the surface treatment film will continue to be maintained in a good state. Therefore, it is considered that during actual use, the lens of Example 4 and the lens of Example 5 will both maintain a contact angle with water of less than 10°.
[0071] In the case of the glass lens of Comparative Example 3 having a surface treatment film formed by a hydrophilic treatment liquid containing an inorganic material and an organic material in the binder, the initial hydrophilicity and haze value were good, but after the abrasion test, the contact angle was 30° and the haze value was 2%, both of which were significantly deteriorated. In addition, many sliding scratches were confirmed on the surface treatment film. In this way, it was confirmed that the abrasion resistance of the surface treatment film was significantly reduced by the inclusion of an organic material (urethane) that is softer than inorganic materials in the binder of the hydrophilic treatment liquid.
[0072] In addition, in the glass lens of Comparative Example 4, in which the particle diameter in the hydrophilic treatment liquid forming the surface treatment film is as large as 150 nm, the initial contact angle and haze value were at a good level, but after the abrasion test, the contact angle increased to 20°, the hydrophilicity was lost, and the haze value after the abrasion test also increased to 1.5%. In addition, a large number of sliding scratches were confirmed on the upper surface of the surface treatment film. This is thought to be because, in the surface treatment film formed by large particles whose ratio to the film thickness is 1, the shape of the surface treatment film changed due to peeling of some particles caused by rubbing the surface, and both the hydrophilicity and optical properties were deteriorated.
[0073] In the glass lens of Comparative Example 5, which has a surface treatment film formed by a hydrophilic treatment liquid containing an inorganic material and an organic material as a binder and containing a silica compound and 1% titania compound as a filler, the initial contact angle is relatively large at 6°, and the haze value is also 2%, which is inferior in optical properties compared to other comparative examples. Furthermore, the contact angle after the abrasion test is large at 20°, and even when irradiated with UV light, it only recovers to 12°. Furthermore, a large number of sliding scratches were confirmed on the surface after the abrasion test. This is thought to be because the surface hardness of the surface treatment film is low because the binder contains an organic material (urethane), and the restoration action of the surface treatment film by the photocatalytic action of the titania compound is limited.
[0074] From the above measurement results, it can be seen that the surface treatment film of this embodiment is composed only of inorganic materials without containing any organic materials in the binder, and contains a silica compound or a titania compound, or both, as a filler, and thus has good hydrophilicity with a contact angle with water of less than 10° and good optical properties with a haze value of less than 1.0%, both in the initial state immediately after the formation of the surface treatment film and when the surface of the surface treatment film is worn down during actual use.
[0075] Furthermore, by setting the ratio of the thickness of the surface treatment film to the particle diameter of the primary particles in the hydrophilic treatment liquid that forms the surface treatment film, that is, [film thickness / particle diameter], in the range of 2 to 10, it is possible to obtain good protective properties for the lens surface by the surface treatment film and high hydrophilicity.
[0076] Furthermore, it was confirmed that by including a titania compound as a filler in the surface treatment film, the contact angle of the surface treatment film with water is restored by the photocatalytic action when irradiated with ultraviolet light, and high hydrophilicity can be maintained for a long period of time. [Industrial Applicability]
[0077] The lenses, lens manufacturing methods, and lens units disclosed herein have a surface treatment film formed on the lens surface that is made of a highly durable inorganic material, and therefore it is possible to realize lenses and lens units that can maintain high hydrophilicity and optical properties for long periods of time even when used in an environment where rain or sand grains are present, or when dust and the like is removed from the lens surface by the user with a cloth during maintenance. [Explanation of symbols]
[0078] 10 Lens optical system 12 (Outermost) Lens 17 Surface treatment film 20 Imaging unit 21 Image sensor 100 Imaging device
Claims
1. A method for manufacturing a lens for forming a hydrophilic surface treatment film on a surface of a lens used in an optical system, comprising the steps of: A hydrophilic treatment liquid containing a silica compound as a filler in an inorganic binder is directly applied to the surface of the lens, and the surface treatment film is formed by drying the hydrophilic treatment liquid. the contact angle of the surface treatment film with water is less than 10°, and the haze value of the lens on which the surface treatment film is formed is less than 1.0%, A method for manufacturing a lens, wherein the thickness of the surface treatment film is 2 to 10 times the average particle size of a filler contained in the surface treatment film.
2. The method for manufacturing a lens according to claim 1 , wherein the hydrophilic treatment liquid further contains a titania compound as a filler.
Citation Information
Patent Citations
Anticlouding coating film and its production
JP1998101374A
Photocatalytic membrane and its production
JP2000271491A
On-vehicle camera
JP2015049281A
Organic inorganic composite and manufacturing method therefor, organic inorganic composite film and manufacturing method therefor, photonic crystal, coating material, thermoplastic composition, fine structure doby, optical material, antireflection member and optical lens
JP2015091981A
Optical lens with scratch-resistant antireflection layer
JP2016173613A