Photosensitive polyimide resin composition

The photosensitive polyimide resin composition addresses sensitivity and stability issues in FO-WLP by using a block copolymer with a benzophenone structure and diazide compound, ensuring solvent solubility during development and insolubility after photocrosslinking, enhancing sensitivity and reducing warpage.

JP7565088B2Active Publication Date: 2024-10-10PI R & D
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
JP2021524910
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-06-06
Filing Date
2020-06-05
Publication Date
2024-10-10
Estimated Expiration
2040-06-05

AI Technical Summary

Technical Problem

Current photosensitive polyimide compositions used in semiconductor package substrates face challenges with sensitivity, developability, and dimensional stability, particularly in Fan-out Wafer Level Packages (FO-WLP), leading to issues like warpage and film burrs due to high-temperature imidization and insufficient exposure and developability.

Method used

A photosensitive polyimide resin composition is developed using a block copolymer with an aromatic tetracarboxylic acid dihydride having a benzophenone structure and specific diamines, combined with a diazide compound, which allows for solvent solubility during development and insolubility after photocrosslinking, enhancing film properties and sensitivity.

Benefits of technology

The composition achieves improved sensitivity and dimensional stability, reducing warpage and film burrs, with good film properties and high sensitivity, suitable for large panel sizes and cost reduction in FO-WLP manufacturing.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007565088000001
    Figure 0007565088000001
  • Figure 0007565088000002
    Figure 0007565088000002
  • Figure 0007565088000003
    Figure 0007565088000003
Patent Text Reader

Abstract

The purpose of the present invention is to provide a photosensitive polyimide resin composition which has developer liquid solubility during development and developer liquid insolubility after photo-crosslinking, and which enables the achievement of good film properties and high sensitivity. The present invention provides a photosensitive polyimide resin composition which contains, as essential components, (A) a solvent-soluble polyimide and (B) a diazide compound, wherein: the solvent-soluble polyimide (A) is a block copolymer that comprises, in the main chain, (a) an aromatic tetracarboxylic acid dianhydride residue having a benzophenone structure and (b) a residue of at least one diamine that is selected from the group consisting of an aromatic diamine having an alkyl group at the ortho position of an amino group, an aromatic diamine having an indane structure, and a diamine having a polysiloxane structure; and the content of the diazide compound (B) is from 2.0 to 150 parts by weight relative to 100 parts by weight of the solvent-soluble polyimide (A).
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a photosensitive polyimide resin composition. [Background technology]

[0002] In recent years, in the field of semiconductor package substrates, there has been active consideration of a shift from FC-CSP and FC-BGA to Fan-out Wafer Level Package (FO-WLP), which allows for lower height, improved electrical properties (R, L, C), and reduced warpage, and some FO-WLPs have been mass-produced. The key organic materials used in FO-WLPs are the sealing material and various protective film materials, and photosensitive polyimide is used as the protective film material.

[0003] It is known that there are several methods for imparting photosensitivity to photosensitive polyimides (Patent Document 1), and they are broadly classified into positive-type and negative-type according to the image formation process. Positive-type polyimides are more sensitive than negative-type polyimides, but since they use a photodecomposition reaction, it is difficult to expect improvement in physical properties due to photoreaction. On the other hand, negative-type polyimides have the characteristic that their chemical resistance and heat resistance are easily improved because the exposed parts undergo a photocrosslinking reaction and remain after development processing. Therefore, although negative-type polyimides have some problems with sensitivity when used as permanent insulating films, they can provide products with excellent reliability.

[0004] Negative-type photosensitive polyimides are roughly divided into a method in which a photosensitive group is introduced into a precursor such as polyamic acid, and then the precursor is photoreacted and then heated to be imidized, and a method in which the ring-closed polyimide itself is made photosensitive. Representative methods that have been put to practical use in this field include a method in which a polyamic acid is ester-bonded with a hydroxyacrylate (Patent Document 2), and a method in which an aminoacrylate or the like is blended with a polyamic acid to introduce a photosensitive group through a salt bond (Patent Document 3).

[0005] As a method for imparting photosensitivity to a ring-closed polyimide itself, there have been reported a method using a polyimide copolymer obtained by a polycondensation reaction between a tetracarboxylic dianhydride having a benzophenone structure and a diamine (Patent Document 4), and a method in which an acryloyl group is added to the side chain of a solvent-soluble polyimide block copolymer synthesized by two-stage polycondensation (Patent Document 5). [Prior art documents] [Patent documents]

[0006] [Patent Document 1] Kenichi Fukuda, Mitsuru Ueda, Polymer Papers, vol63, No.9, pp.561-576 [Patent Document 2] Special Publication No. 55-41422 [Patent Document 3] Japanese Patent Application Publication No. 54-145794 [Patent Document 4] Japanese Patent Application Publication No. 5-39281 [Patent Document 5] JP 2000-147768 A Summary of the Invention [Problem to be solved by the invention]

[0007] Demands on semiconductor package substrates are becoming more stringent every year, and FO-WLP is no exception, with demands for thinner patterns, smaller diameter connection vias, multi-layering, etc. In order to meet these demands, photosensitive polyimides are also being required to not only improve their sensitivity and thin film reliability, but also to reduce warping and improve dimensional stability in large panel sizes, which are deeply related to cost reduction, the biggest challenge for FO-WLP.

[0008] However, the currently used method of using polyamic acid and performing thermal imidization after photoreaction requires high temperatures (e.g., 350 to 450°C) for imidization, during which dehydration shrinkage and elimination or volatilization of photosensitive groups occur, resulting in large film defects. This has a significant impact on warping and dimensional stability in the manufacturing process of semiconductor packages and electronic devices, and is also a factor in reducing storage stability.

[0009] Furthermore, even when a ring-closed polyimide is used, there is a problem in that it is necessary to have a structure in which the exposed area is soluble in a developer during development and is insoluble in the developer after exposure, and the previously reported methods have had the problem of insufficient exposure and developability.

[0010] Thus, as a protective film material for semiconductor package substrates and the like, there has been a demand for a photosensitive polyimide that is soluble in a developer during development and insoluble in a developer after photocrosslinking, and that can achieve good film properties and improved sensitivity.

[0011] An object of the present invention is to provide a photosensitive polyimide resin composition which is soluble in a developer during development and insoluble in a developer after photocrosslinking, and which can achieve good film properties and high sensitivity. [Means for solving the problem]

[0012] As a result of intensive research aimed at solving the above problems, the present inventors have found that by using a block copolymer having a structure in which an aromatic acid dianhydride having a benzophenone structure and a specific diamine are contained in the main chain as a ring-closed polyimide, and further combining this polyimide with a specific amount of a diazide compound, it is possible to provide a photosensitive polyimide resin composition which is soluble in a solvent during development and insoluble in a solvent after photocrosslinking, and which can achieve good film properties and high sensitivity, and have completed the present invention.

[0013] That is, the present invention provides the following. (1) A photosensitive polyimide resin composition comprising (A) a solvent-soluble polyimide and (B) a diazide compound as essential components, wherein the (A) solvent-soluble polyimide is a block copolymer having, in its main chain, (a) an aromatic tetracarboxylic dianhydride residue having a benzophenone structure and (b) a residue of an aromatic diamine having a phenylindane structure, and the content of the (B) diazide compound is 2.0 to 150 parts by weight based on 100 parts by weight of the (A) solvent-soluble polyimide. (2) A photosensitive polyimide resin composition comprising (A) a solvent-soluble polyimide and (B) a diazide compound as essential components, wherein the (A) solvent-soluble polyimide is a block copolymer having, in its main chain, (a) an aromatic tetracarboxylic dianhydride residue having a benzophenone structure, and (b) a residue of at least one diamine selected from the group consisting of an aromatic diamine having an alkyl group at the ortho-position of an amino group, an aromatic diamine having an indane structure, and a diamine having a polysiloxane structure, the (B) diazide compound is 2,6-di(4'-azidobenzal)-4-ethylcyclohexanone, and the content of the (B) diazide compound is 2.0 to 150 parts by weight based on 100 parts by weight of the (A) solvent-soluble polyimide. (3) A photosensitive polyimide resin composition comprising (A) a solvent-soluble polyimide, (B) a diazide compound, (C) an epoxy resin, and (D) a photobase generator as essential components, wherein the (A) solvent-soluble polyimide is a block copolymer having, in its main chain, (a) an aromatic tetracarboxylic dianhydride residue having a benzophenone structure, and (b) a residue of at least one diamine selected from the group consisting of an aromatic diamine having an alkyl group at the ortho-position of an amino group, an aromatic diamine having an indane structure, and a diamine having a polysiloxane structure, and the content of the (B) diazide compound is 2.0 to 150 parts by weight based on 100 parts by weight of the (A) solvent-soluble polyimide. (4) The photosensitive polyimide resin composition according to any one of (1) to (3), characterized in that the photosensitive polyimide resin composition is a negative-tone solvent-developable composition. 3 ) The resin composition according to any one of claims 1 to 4. (5)(1)~( 4 2. A method for forming a pattern, comprising: exposing a substrate coated with the resin composition according to claim 1 to ultraviolet light; and developing and removing the unexposed areas. (6)(1)~( 4 2. A semiconductor package, an electronic element, a display element, or an organic multilayer wiring board having an interlayer insulating film, a passivation film, or a surface protective film formed using the resin composition according to any one of claims 1 to 11. Effect of the Invention

[0014] According to the present invention, by using a ring-closed photosensitive polyimide and a specific amount of a diazide compound, it is possible to provide a photosensitive polyimide resin composition that has both solvent solubility during development and solvent insolubility after photocrosslinking, and that can achieve excellent film properties and high sensitivity equal to or better than those of photosensitive polyimides using polyamic acids, without using a polyamic acid that requires imidization at high temperatures.

[0015] When a polyimide having a benzophenone skeleton, which has been conventionally used, is used, the quantum yield of hydrogen abstraction crosslinking between the benzophenone portion and the adjacent alkyl group is low, and a sufficient crosslinked structure cannot be obtained. However, in the present invention, by adding a diazide compound to the polyimide resin composition, a sufficient crosslinked structure of the polyimide can be realized.

[0016] Furthermore, when the thickness of a film formed using the polyimide resin composition is large, for example, 10 μm or more, a sufficient crosslinked structure can be realized by incorporating a photobase generator and an epoxy resin in the polyimide resin composition and photocrosslinking the epoxy resin with the photobase generator. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0017] The photosensitive polyimide resin composition of the present invention is a resin composition containing (A) a solvent-soluble polyimide and (B) a diazide compound as essential components.

[0018] (A) Solvent-soluble polyimide The (A) solvent-soluble polyimide of the present invention is a block copolymer having, in its main chain, (a) an aromatic acid dianhydride having a benzophenone structure, and at least one diamine (b) selected from the group consisting of (b-1) an aromatic diamine having an alkyl group at the ortho-position of an amino group, (b-2) an aromatic diamine having an indane structure, and (b-3) a diamine having a polysiloxane structure.

[0019] Specifically, the solvent-soluble polyimide (A) of the present invention is a block copolymer having at least one, and preferably two or more, of the repeating units represented by the following general formulas [I] to [III].

[0020] [ka] (In the formula, Z 1 is an aromatic tetracarboxylic dianhydride residue, and Ar 1 is an aromatic diamine residue having an alkyl group at the ortho position of the amino group.

[0021] [ka] (In the formula, Z 2 is an aromatic tetracarboxylic dianhydride residue, and Ar 2 is an aromatic diamine residue having an indane structure.

[0022] [ka] (In the formula, Z 3 is an aromatic tetracarboxylic dianhydride residue, and Ar 3 is a diamine residue having a polysiloxane structure)

[0023] In the present invention, Z in the above general formula [I] 1 Z in the above general formula [II] 2 Z in the above general formula [III] 3 At least one of the above is (a) an aromatic tetracarboxylic dianhydride residue having a benzophenone structure, and Z 1 , Z 2 and Z 3 is preferably (a) an aromatic tetracarboxylic dianhydride residue having a benzophenone structure.

[0024] Examples of the aromatic acid dianhydride that becomes the aromatic acid dianhydride residue having a benzophenone structure (a) in the present invention include 2,2',3,3'-benzophenonetetracarboxylic dianhydride (BTDA), 4,5,3',4'-benzophenonetetracarboxylic dianhydride (BTDA), and 3,3',4,4'-benzophenonetetracarboxylic dianhydride (BTDA). The morphology of BTDA-based polyimides also changes due to photocrosslinking. In other words, it is believed that the aggregated state becomes denser. This also contributes to improving chemical resistance and heat resistance.

[0025] The aromatic acid dianhydride having a benzophenone structure is preferably contained in an amount of 10 mol % or more, 45 mol % or more, or even 50 mol % or more of all aromatic acid dianhydrides constituting the solvent-soluble polyimide. If the content of the aromatic acid dianhydride having a benzophenone structure is less than 10 mol %, the solvent resistance of the polyimide resin composition after photocrosslinking tends to decrease, and the sensitivity tends to decrease.

[0026] Z in the above general formulas [I] to [III] 1 , Z 2 and Z 3Examples of the aromatic tetracarboxylic dianhydride residue having a benzophenone structure other than the above are not particularly limited, but include pyromellitic dianhydride, 3,4,3',4'-benzophenonetetracarboxylic dianhydride, 3,4,3',4'-diphenyltetracarboxylic dianhydride, bis-(3,4-dicarboxyphenyl)ether dianhydride, 2,2-bis-(3,4-dicarboxyphenyl)hexafluoropropane dianhydride, 4,4'-oxydiphthalic dianhydride, and the like.

[0027] The (A) solvent-soluble polyimide may have a repeating unit composed of an aromatic tetracarboxylic dianhydride residue and a diamine residue other than those of the above general formulas [I] to [III].

[0028] (b) Diamine (b-1) Aromatic diamines having an alkyl group at the ortho position of the amino group In the present invention, the aromatic diamine residue (Ar 1 ) includes aromatic diamine residues having a linear or branched alkyl group having 1 to 12 carbon atoms, preferably an alkyl group having 1 to 5 carbon atoms, and more preferably an alkyl group having 1 to 3 carbon atoms, at the ortho-position of the amino group, and specifically includes those having structures represented by the following formulas (1) to (3).

[0029] [ka]

[0030] In the above formula (1), the free bonds (the two bond positions to which the amino groups are attached) are in the meta or para positions relative to each other. In the above formula (2), the free bonds (the two bond positions to which the amino groups are attached) are preferably R 11 It is located in the meta or para position relative to R 5 and R 6 is attached to the two ortho positions of the free bond. R 11 -O-, -S-, -SS-, -SO-, -SO 2It represents -, -CO-, -COO-, -NH-, -CONH-, -CON-alkyl group- (the number of carbon atoms in the alkyl group, n, is 1 to 6), or -CON-benzyl group-. In the above formula (3), the free bonds (the two bond positions to which the amino groups are bonded) are present at the 2-, 3-, 6-, or 7-positions, and R 5 and R 6 is attached to the two ortho positions of the free bond. In the above formulas (1) to (3), R 5 and R 6 is a straight-chain or branched alkyl group having 1 to 12 carbon atoms, preferably an alkyl group having 1 to 5 carbon atoms, and more preferably an alkyl group having 1 to 3 carbon atoms.

[0031] In the present invention, the aromatic diamine residue (Ar 1 The content of diamine (A) in all diamines constituting the solvent-soluble polyimide is preferably 30 mol % or more, more preferably 50 mol % or more, and even more preferably 70 mol % or more. If it is less than 50 mol %, the crosslink density tends to decrease.

[0032] (b-2) Aromatic diamines having an indane structure In the present invention, the aromatic diamine residue having an indane structure (Ar 2 ) includes those having the following indane skeleton and a structure represented by the following formula (IV) or (V).

[0033] [ka]

[0034] In the above formula (IV), R 1 and R 2 represents an alkyl group having 1 to 12 carbon atoms, an alkoxy group having 1 to 12 carbon atoms, or an alkoxyalkyl group having 2 to 12 carbon atoms; R 1 and R 2 is preferably bonded to the two ortho positions of the free bonds (the two bond positions to which the amino groups are bonded).

[0035] [ka]

[0036] In the above formula (V), R 1 ,R 2 and R 3 each independently represents a hydrogen atom or an alkyl group having 1 to 5 carbon atoms; R 4 Each of and R 5 Each independently represents a hydrogen atom or an alkyl group having 1 to 5 carbon atoms. Specific examples include 5-amino-1-(4'-aminophenyl)-1,3,3-trimethylindan and 6-amino-1-(4'-aminophenyl)-1,3,3-trimethylindan. In the present invention, a solvent-soluble polyimide having an aromatic diamine residue having a phenylindane structure represented by the above formula (V) in the main chain is preferred.

[0037] In the present invention, the aromatic diamine residue having an indane structure (Ar 2 The content of diamine (A) in all diamines constituting the solvent-soluble polyimide is preferably 50 mol % or more, more preferably 60 mol % or more, and even more preferably 70 mol % or more. If it is less than 50 mol %, the crosslink density tends to decrease.

[0038] (b-3) Diamine residue having a polysiloxane structure (Ar 3 ) The diamine residue having a polysiloxane structure (Ar 3 ) include α,ω-bis(2-aminoethyl)polydimethylsiloxane, α,ω-bis(3-aminopropyl)polydimethylsiloxane, α,ω-bis(4-aminophenyl)polydimethylsiloxane, α,ω-bis(4-amino-3-methylphenyl)polydimethylsiloxane, α,ω-bis(3-aminopropyl)polydiphenylsiloxane, and α,ω-bis(4-aminobutyl)polydimethylsiloxane.

[0039] The diamine residue having a polysiloxane structure (Ar 3The content of the diamine having a polysiloxane structure in all the diamines constituting the solvent-soluble polyimide (A) is preferably 2.0 to 30 mol %, and more preferably 5.0 to 20 mol %. If the content of the diamine having a polysiloxane structure exceeds 30 mol %, the solvent solubility may become too high, and Tg also tends to decrease.

[0040] (A) Method for synthesizing solvent-soluble polyimide The method for synthesizing the solvent-soluble polyimide may be a known method and is not particularly limited, but the solvent-soluble polyimide can be synthesized by using approximately equal amounts of the above-mentioned tetracarboxylic dianhydride and aromatic diamine and reacting them in an organic polar solvent in the presence of a catalyst and a dehydrating agent at 160 to 200° C. for several hours. As the organic polar solvent, N-methylpyrrolidone (NMP), γ-butyrolactone, N,N'-dimethylacetamide, N,N'-dimethylformamide, dimethylsulfoxide, tetramethylurea, tetrahydrothiophene-1,1-oxide, etc. can be used.

[0041] The solvent-soluble polyimide (A) in the present invention is a block copolymer, and can be synthesized by carrying out a block copolymerization reaction as necessary. For example, it can be produced by a two-stage sequential addition reaction, in which a polyimide oligomer is synthesized from a tetracarboxylic dianhydride and an aromatic diamine in the first stage, and then a tetracarboxylic dianhydride and / or an aromatic diamine is further added in the second stage to carry out polycondensation to obtain a block copolymerized polyimide.

[0042] As a catalyst for block copolymerization, a two-component acid-base catalyst utilizing the equilibrium reaction of lactones can be used to promote the dehydration imidization reaction. Specifically, a two-component catalyst of γ-valerolactone and pyridine or N-methylmorpholine is used. As shown in the formula below, as the imidization proceeds, water is generated, and the generated water participates in the equilibrium of lactones, becoming an acid-base catalyst and exhibiting catalytic action.

[0043] [ka]

[0044] The water produced by the imidization reaction is removed from the system by azeotropy with a dehydrating agent such as toluene or xylene that coexists in the polar solvent. When the reaction is completed, the water in the solution is removed, and the acid-base catalyst becomes γ-valerolactone and pyridine or N-methylmorpholine, which are removed from the system. In this way, a high-purity polyimide solution can be obtained.

[0045] Other two-component catalysts include oxalic acid or malonic acid and pyridine or N-methylmorpholine. In a reaction solution at 160 to 200°C, oxalates or malonates act as acid catalysts to promote the imidization reaction. A catalytic amount of oxalic acid or malonic acid remains in the generated polyimide solvent. When this polyimide solution is applied to a substrate and then heated to 200°C or higher to remove the solvent and form a film, the oxalic acid or malonic acid remaining in the polyimide is thermally decomposed as shown in the following formula and removed from the system as a gas.

[0046] [ka]

[0047] By the above method, it is possible to obtain a high-purity solvent-soluble polyimide (A). The oxalic acid-pyridine catalyst is more active than the valerolactone-pyridine catalyst, and can produce a high-molecular-weight polyimide in a short period of time.

[0048] The term "solvent-soluble" in the present invention is used for the organic polar solvent used in the synthesis of polyimide and the solvent used in the film described below, and means that the polyimide is dissolved in an amount of 5 g or more in 100 g of solvent. Here, examples of the solvent include polar solvents such as N-methyl-2-pyrrolidone, γ-butyrolactone, dimethylformamide, dimethylacetamide, dimethylsulfoxide, sulfolane, and tetramethylurea.

[0049] The (A) solvent-soluble polyimide synthesized as described above can be used in the form of a solution dissolved in the above organic polar solvent or a solvent used in the film described below so that the solid content is, for example, 10 to 30% by weight. The molecular weight of the (A) solvent-soluble polyimide is preferably 10,000 to 400,000 as a weight average molecular weight converted into polystyrene. Within this range, good solvent solubility, film properties, and insulating properties can be achieved. The appropriate viscosity of the (A) solvent-soluble polyimide is preferably 2 to 10 Pa·s / 25°C when the solid content is 20 to 40% by weight. The glass transition temperature (Tg) (measured by TMA measurement method) of the solvent-soluble polyimide is preferably 200°C or higher, more preferably 250°C or higher.

[0050] The concentration of the solvent-soluble polyimide (A) in the solution is preferably 5 to 50% by weight, more preferably 10 to 40% by weight. The polyimide obtained by the direct imidization reaction using the catalyst system consisting of the lactone and the base can be obtained in the form of a solution dissolved in a polar solvent, and the polyimide concentration can be set within the above-mentioned preferred range, so that the produced polyimide solution can be used as it is.

[0051] The produced polyimide solution can be further diluted, if desired, with a diluent, such as, but not limited to, a solvent that does not significantly impair the solubility, such as dioxane, dioxolane, N-methyl-2-pyrrolidone, γ-butyrolactone, cyclohexanone, cyclopentanone, propylene glycol monomethyl ether acetate, methyl lactate, anisole, methyl benzoate, ethyl acetate, etc.

[0052] (B) Diazide compounds In the present invention, by adding the diazide compound (B) to the photosensitive polyimide resin composition as another essential component, there is an effect that the exposure and developability are significantly improved.

[0053] (B) Examples of the diazide compound include 4,4'-diazidobenzalacetophenone, 2,6-di(4'-azidobenzal)cyclohexanone, 2,6-di(4'-azidobenzal)-4-methylcyclohexanone, 2,6-di(4'-azidobenzal)-4-ethylcyclohexanone, 2,6-di(4'-azidobenzal)-4-t-amylcyclohexanone, 4,4'-diazidodiphenylsulfone, 4,4'-diazidodiphenylether, 4,4'-diazidophenylsulfide, 4,4'-diazidodiphenylmethane, etc. Among these, those having an azidobenzalcyclohexanone structure are preferred, and from the viewpoint of crosslinking property and storage stability, 2,6-di(4'-azidobenzal)-4-ethylcyclohexanone is particularly excellent.

[0054] The (B) diazide compound is preferably contained in the photosensitive polyimide resin composition in an amount of 2.0 to 150 parts by weight, more preferably 5.0 to 100 parts by weight, and particularly preferably 10.0 to 80 parts by weight, per 100 parts by weight of the (A) solvent-soluble polyimide. If the amount is less than 2.0 parts by weight, the crosslink density tends to decrease, and if the amount is more than 150 parts by weight, the film properties tend to decrease. In order to complement the crosslinking property, a diazirine compound, a maleimide compound, or a bismaleimide compound may be used in combination.

[0055] The photosensitive polyimide resin composition of the present invention has poor light transmittance at low wavelengths, and therefore, in particular in the case of thick-film specifications, the pattern shape is prone to the reverse taper seen in negative solvent development. In order to improve this, it has been found that it is also effective to use photosensitive monomers or polymers with different photosensitive crosslinking length methods in combination. Among them, it has been found that the combination of (C) epoxy resin and (D) photobase generator, which have excellent compatibility with the photosensitive polyimide resin composition, is particularly effective as a component of the photosensitive polyimide resin composition of the present invention.

[0056] (C) Epoxy resin The epoxy resin (C) is not particularly limited and can be selected based on the reactivity with the photobase generator and the compatibility with the photosensitive polyimide resin composition. Examples of the epoxy resin include phenol novolac type epoxy resin, cresol novolac type epoxy resin, bisphenol A novolac type epoxy resin, triazine skeleton-containing epoxy resin, fluorene skeleton-containing epoxy resin, naphthalene type epoxy resin, biphenyl type epoxy resin, crystalline epoxy resin, bisphenol A type epoxy resin, etc., and these polymer epoxy resins can also be used. The content of the epoxy resin (C) in the photosensitive polyimide resin composition is preferably 2 to 50 parts by weight, and most preferably 2 to 20 parts by weight, based on 100 parts by weight of the solvent-soluble polyimide (A).

[0057] (D) Photobase generator (D) Photobase generators are components that generate anions (bases) when irradiated with ultraviolet light, and are broadly classified into non-ionic and ionic types. Non-ionic types include those that absorb light and generate primary amines, secondary amines, imidazoles, etc., while ionic types include those that generate strong organic bases such as amidines, guanidines, and phosphazenes. As the (D) photobase generator, those which generate a primary amine or a secondary amine in the reaction with the (C) epoxy resin are less likely to cause a chain reaction, and therefore, preferred are non-ionic ones which generate imidazole, and ionic ones which generate amidine, guanidine, or the like.

[0058] As the photobase generator (D) in the present invention, commercially available products can be used, such as WPBG-018, WPBG-140, WPBG-266, WPBG-300, WPBG-345, WPBG-027, and WPBG-165 (all manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.). The content of the photobase generator (D) in the photosensitive polyimide resin composition is preferably from 0.5 to 8% by weight, more preferably from 1 to 6% by weight, based on the epoxy resin (C).

[0059] (Photosensitizer) The photosensitive polyimide resin composition of the present invention can contain a photosensitizer to enhance the sensitivity of pattern resolution in order to adapt it to each final use. As the photosensitizer, one that acts on the long wavelength side (>350 nm) is preferable. As the photosensitizer, for example, an anthracene-based sensitizer, a thioxanthone-based sensitizer, etc. can be mentioned. The content of the photosensitizer is preferably about 0.3 to 2% by weight based on the photosensitive polyimide resin composition.

[0060] Specific examples of the anthracene-based sensitizer include 9,10-dimethoxyanthracene, 9,10-diethoxyanthracene, 9,10-dipropoxyanthracene, 9,10-diisopropoxyanthracene, 9,10-dibutoxyanthracene, 9,10-dipentyloxyanthracene, 9,10-dihexyloxyanthracene, 9,10-bis(2-methoxyethoxy)anthracene, 9,10-bis(2-ethoxyethoxy)anthracene, 9,10-bis(2-butoxyethoxy)anthracene, and 9,10-bis(3-butoxypropoxy). ) anthracene, 2-methyl- or 2-ethyl-9,10 dimethoxyanthracene, 2-methyl- or 2-ethyl-9,10-diethoxyanthracene, 2-methyl- or 2-ethyl-9,10-dipropoxyanthracene, 2-methyl- or 2-ethyl-9,10-diisopropoxyanthracene, 2-methyl- or 2-ethyl-9,10-dibutoxyanthracene, 2-methyl- or 2-ethyl-9,10-dipentyloxyanthracene, 2-methyl- or 2-ethyl-9,10-dihexyloxyanthracene, and the like. Commercially available anthracene sensitizers can be used, such as "Anthracure UVS-1331", "Anthracure UVS-1101" and "Anthracure UVS-1221" (all manufactured by Kawasaki Chemical Industries, Ltd.).

[0061] Examples of thioxanthone sensitizers include 2-isopropylthioxanthone, 4-isopropylthioxanthone, 2,4-diethylthioxanthone, and chloropropoxythioxanthone. Commercially available products can be used as the thioxanthone sensitizers. Examples of commercially available products include "KAYACURE DETX-S" (manufactured by Nippon Kayaku Co., Ltd.), "Speedcure ITX", "Speedcure DETX", and "Speedcure CPTX" (all manufactured by LAMBSON).

[0062] (Other additives) The photosensitive polyimide resin composition of the present invention may contain modifiers that are typically added to photosensitive polyimide resin compositions, such as coupling agents, plasticizers, film-forming resins, surfactants, stabilizers, and spectral sensitivity regulators. In particular, when the adhesion of the polyimide to the substrate is poor, the adhesion to the substrate can be improved by adding a coupling agent, particularly a silane coupling agent such as vinyltrimethoxysilane, 3-glycidoxypropylmethyldimethoxysilane, p-styryltrimethoxysilane, 3-methacryloxypropyltrimethoxysilane, 3-aminopropyltrimethoxysilane, tris-(trimethoxysilylpropyl)isocyanurate, 3-ureidopropyltrialkoxysilane, 3-mercaptopropylmethyldimethoxysilane, 3-isocyanatepropyltriethoxysilane, 3-trimethoxysilylpropylsuccinic anhydride, hexamethyldisiloxane, hexamethyldisilazane, 1,3-bis(3-aminopropyl)tetramethyldisiloxane, or N-[3-(triethoxysilyl)propyl]phthalamic acid. In this case, the amount of the silane coupling agent added is preferably 0.1 to 5% by weight of the photosensitive polyimide resin composition.

[0063] In addition, when a substrate made of copper or a copper alloy is used, an azole compound can be added to the photosensitive polyimide resin composition in order to suppress discoloration of the substrate. Examples of the azole compound include 1H-benzotriazole, tolyltriazole, 5-methyl-1H-benzotrial, 4-methyl-1H-benzotrial, 5-carboxy-1H-benzotrial, and 4-carboxy-1H-benzotrial. In this case, the amount of the azole compound added is preferably 0.1 to 1% by weight of the photosensitive polyimide resin composition.

[0064] Furthermore, in order to suppress discoloration on copper, a hindered phenol compound can be blended into the photosensitive polyimide resin composition. Examples of the hindered phenol compound include 1,3,5-tris(4-t-butyl-3-hydroxy-2,6-dimethylbenzyl)-1,3,5-triazine-2,4,6-(1H,3H,5H)-trione, 1,3,5-tris(4-t-butyl-5-ethyl-3-hydroxy-2,6-dimethylbenzyl)-1,3,5-triazine-2,4,6-(1H,3H,5H)-trione, and 1,3,5-tris(4-triethylmethyl-3-hydroxy-2,6-dimethylbenzyl)-1,3,5-triazine-2,4,6-(1H,3H,5H)-trione. In this case, the amount of the hindered phenol compound added is preferably 0.1 to 2% by weight of the photosensitive polyimide resin composition. Other resins that can be used in combination include polyarylate resins and polyethersulfone resins.

[0065] The photosensitive polyimide resin composition of the present invention can be in the form of a solution suitable for application onto a substrate, in which case the solvent can be a polar solvent such as N-methyl-2-pyrrolidone, γ-butyrolactone, dimethylformamide, dimethylacetamide, dimethylsulfoxide, sulfolane, or tetramethylurea, which is used as a solvent for imidization reactions.

[0066] Method for manufacturing photosensitive polyimide patterns A photosensitive polyimide pattern can be produced on a substrate by using the photosensitive polyimide resin composition containing the above-mentioned components. Specifically, the photosensitive polyimide pattern can be produced by a method including the steps of: (1) forming a resin layer on a substrate by applying the above-mentioned photosensitive polyimide resin composition of the present invention on the substrate; (2) exposing the resin layer; (3) developing the exposed resin layer to form a photosensitive polyimide pattern for an insulating material of an electronic component, and a passivation film, a buffer coat film, an interlayer insulating film, etc. in a semiconductor package; and (4) completing the photosensitive polyimide pattern as a permanent insulating film by heat treatment.

[0067] A typical embodiment of each step will be described below. (1) forming a resin layer on a substrate by applying a photosensitive resin composition onto the substrate; In this step, the photosensitive resin composition of the present invention is applied onto a substrate such as a silicon wafer, a metal substrate, a ceramic substrate, an organic substrate, etc., and then dried as necessary to form a resin layer. As the application method, a method that has been conventionally used for applying a photosensitive resin composition, such as a method of applying with a spin coater, a bar coater, a blade coater, a curtain coater, a screen printer, etc., or a method of spray application with a spray coater, etc. can be used.

[0068] If necessary, the coating film made of the photosensitive resin composition can be dried. As the drying method, air drying, heat drying with an oven or a hot plate, vacuum drying, etc. can be used. Specifically, when air drying or heat drying is performed, drying can be performed under conditions of 20 to 140°C for 1 to 30 minutes. There is no limitation to this range as long as it does not impair the various properties of the photosensitive resin composition of the present invention.

[0069] (2) Step of exposing the resin layer to light: In this step, the resin layer formed in the above step (1) is exposed to an ultraviolet light source or the like through a photomask or reticle having a pattern, or directly, using an exposure device such as a contact aligner, mirror projection, or stepper. Thereafter, for the purpose of improving photosensitivity, etc., post-exposure baking and / or pre-development baking may be performed at any combination of temperature and time, as necessary. The range of baking conditions is preferably a temperature of 40 to 120° C. and a time of 10 to 240 seconds, but is not limited to this range as long as it does not impair the various properties of the photosensitive resin composition of the present invention.

[0070] (3) A process of developing the exposed resin layer to form a photosensitive polyimide pattern: In this step, the unexposed portion of the photosensitive resin layer after exposure is developed and removed. As the development method, any method can be selected from conventionally known photoresist development methods, such as the rotary spray method, the paddle method, and the immersion method accompanied by ultrasonic treatment. After development, post-development baking may be performed at any combination of temperature and time as necessary for the purpose of adjusting the shape of the photosensitive polyimide pattern.

[0071] The developer used for development is preferably a good solvent for the photosensitive resin composition, or a combination of the good solvent and a poor solvent. For example, the good solvent is preferably N-methylpyrrolidone, N-cyclohexyl-2-pyrrolidone, N,N-dimethylacetamide, cyclopentanone, cyclohexanone, γ-butyrolactone, α-acetyl-γ-butyrolactone, etc. The poor solvent is preferably toluene, xylene, methanol, ethanol, isopropyl alcohol, ethyl lactate, propylene glycol methyl ether acetate, etc. When a good solvent and a poor solvent are used in combination, it is preferable to adjust the ratio of the poor solvent to the good solvent according to the solubility of the polymer in the photosensitive resin composition. In addition, two or more solvents, for example, several types, can be used in combination for each of the good solvent and the poor solvent.

[0072] (4) A process of completing the photosensitive polyimide pattern as a permanent insulating film by heat treatment: In this process, the photosensitive polyimide pattern obtained by the above development is heated to complete it as a permanent insulating film. That is, unlike the polyamic acid type, since imidization has already been completed, it can be completed as a permanent insulating film by removing the residues such as the solvent. As the method of heat curing, various methods can be selected, such as using a hot plate, an oven, or a temperature-elevating oven that can set a temperature program. Heating is performed under conditions sufficient to evaporate the contained solvent, for example, at 150 to 250°C for about 30 minutes to 2 hours. The atmospheric gas during heating may be air, or an inert gas such as nitrogen or argon may be used.

[0073] The photosensitive polyimide pattern thus formed can be used as an interlayer insulating film, a passivation film or a surface protective film for a semiconductor package, an electronic element, a display element or an organic multilayer wiring board. EXAMPLES

[0074] The present invention will be described in detail below using examples, but the present invention is not limited to these.

[0075] (Synthesis of block copolymer polyimide) Synthesis Example 1 A three-necked separable glass flask was fitted with a stirrer, a nitrogen inlet tube, and a cooling tube equipped with a water receiver. 64.45 g (0.2 mol) of 3,4,3',4'-benzophenonetetracarboxylic dianhydride (hereinafter referred to as BTDA), 29.23 g (0.1 mol) of 1,3-bis(3-aminophenoxy)benzene, 1.5 g (0.015 mol) of valerolactone, 2.4 g (0.03 mol) of pyridine, 200 g of NMP, and 30 g of toluene were charged and stirred at room temperature under a nitrogen atmosphere at 200 rpm for 30 minutes, and then heated to 180°C and stirred for 1 hour. During the reaction, the toluene-water azeotrope was removed. After cooling to room temperature, 48.33g (0.15 mol) of BTDA, 44.57g (0.25 mol) of 2,4-diethyl-6-methyl-1,3-benzenediamine (an aromatic diamine having an alkyl group at the ortho position relative to the N-), 360g of NMP, and 90g of toluene were added and stirred at room temperature for 30 minutes, and then the temperature was raised to 180°C and heated and stirred for 1 hour. The reaction was terminated by heating and stirring at 180°C for 2 hours and 30 minutes while removing the water-toluene azeotropic reflux from the system. The obtained product was diluted with NMP to obtain a block copolymer polyimide solution with a solid content of 20% by weight.

[0076] Synthesis Example 2 A glass separable three-neck flask was equipped with a stirrer, a nitrogen inlet tube, and a cooling tube equipped with a water receiver. 64.45g (0.2 mol) of 3,4,3',4'-benzophenonetetracarboxylic dianhydride (hereinafter referred to as BTDA), 29.23g (0.1 mol) of 1,3-bis(3-aminophenoxy)benzene, 1.5g (0.015 mol) of valerolactone, 2.4g (0.03 mol) of pyridine, 200g of NMP, and 30g of toluene were charged and stirred at room temperature under a nitrogen atmosphere at 200 rpm for 30 minutes, and then heated to 180°C and stirred for 1 hour. During the reaction, the toluene-water azeotrope was removed. After cooling to room temperature, 48.33g (0.15 mol) of BTDA, 51.08g (0.25 mol) of 5,7-diamino-1,1,4,6-tetramethylindane (aromatic diamine having an alkyl group at the ortho position relative to N-), 360g of NMP, and 90g of toluene were added, and the mixture was stirred at room temperature for 30 minutes, and then heated to 180°C and stirred for 1 hour. The reaction was terminated by heating and stirring at 180°C for 2 hours and 30 minutes while removing the water-toluene azeotropic reflux from the system. The obtained product was diluted with NMP to obtain a block copolymer polyimide solution with a solid content of 20% by weight.

[0077] Synthesis Example 3 A glass separable three-neck flask was equipped with a stirrer, a nitrogen inlet tube, and a cooling tube equipped with a water receiver. 64.45g (0.2 mol) of 3,4,3',4'-benzophenonetetracarboxylic dianhydride (hereinafter referred to as BTDA), 29.23g (0.1 mol) of 1,3-bis(3-aminophenoxy)benzene, 1.5g (0.015 mol) of valerolactone, 2.4g (0.03 mol) of pyridine, 200g of NMP, and 30g of toluene were charged and stirred at room temperature under a nitrogen atmosphere at 200 rpm for 30 minutes, and then heated to 180°C and stirred for 1 hour. During the reaction, the toluene-water azeotrope was removed. After cooling to room temperature, 44.13g (0.15mol) of 3,4,3',4'-biphenyltetracarboxylic dianhydride, 44.57g (0.25mol) of 2,4-diethyl-6-methyl-1,3-benzenediamine (aromatic diamine having an alkyl group at the ortho position relative to N-), 360g of NMP, and 90g of toluene were added and stirred at room temperature for 30 minutes, then heated to 180°C and stirred for 1 hour. The reaction was terminated by heating and stirring at 180°C for 2 hours and 30 minutes while removing the water-toluene azeotropic reflux from the system. The obtained product was diluted with NMP to obtain a block copolymer polyimide solution with a solid content of 20% by weight.

[0078] Synthesis Example 4 A three-necked separable glass flask was fitted with a stirrer, a nitrogen inlet tube, and a cooling tube equipped with a water receiver. 64.45 g (0.2 mol) of 3,4,3',4'-benzophenonetetracarboxylic dianhydride (hereinafter referred to as BTDA), 26.64 g (0.1 mol) of 5-amino-1-(4'-aminophenyl)-1,3,3-trimethylindane (aromatic diamine containing a phenylindane structure), 1.5 g (0.015 mol) of valerolactone, 2.4 g (0.03 mol) of pyridine, 200 g of NMP, and 30 g of toluene were charged and stirred at room temperature under a nitrogen atmosphere at 200 rpm for 30 minutes, and then heated to 180°C and stirred for 1 hour. During the reaction, the toluene-water azeotrope was removed. After cooling to room temperature, 48.33g (0.15 mol) of BTDA, 66.60g (0.25 mol) of 5-amino-1-(4'-aminophenyl)-1,3,3-trimethylindane, 360g of NMP, and 90g of toluene were added, and the mixture was stirred at room temperature for 30 minutes, and then heated to 180°C and stirred for 1 hour. The reaction was terminated by heating and stirring at 180°C for 2 hours and 30 minutes while removing the water-toluene azeotropic reflux from the system. The obtained product was diluted with NMP to obtain a block copolymer polyimide solution with a solid content of 20% by weight.

[0079] Synthesis Example 5 A three-necked separable glass flask was fitted with a stirrer, a nitrogen inlet tube, and a cooling tube equipped with a water receiver. 64.45 g (0.2 mol) of 3,4,3',4'-benzophenonetetracarboxylic dianhydride (hereinafter referred to as BTDA), 12.22 g (0.1 mol) of 2,4-diaminotoluene (an aromatic diamine having an alkyl group at the ortho position relative to the N-), 1.5 g (0.015 mol) of valerolactone, 2.4 g (0.03 mol) of pyridine, 200 g of NMP, and 30 g of toluene were charged and stirred at room temperature under a nitrogen atmosphere at 200 rpm for 30 minutes, and then heated to 180°C and stirred for 1 hour. During the reaction, the toluene-water azeotrope was removed. After cooling to room temperature, 48.33g (0.15mol) of BTDA, 66.60g (0.25mol) of 5-amino-1-(4'-aminophenyl)-1,3,3-trimethylindane, 360g of NMP, and 90g of toluene were added, and the mixture was stirred at room temperature for 30 minutes, and then heated to 180°C and stirred for 1 hour. The reaction was terminated by heating and stirring at 180°C for 2 hours and 30 minutes while removing the water-toluene azeotropic reflux from the system. The obtained product was diluted with NMP to obtain a block copolymer polyimide solution with a solid content of 20% by weight.

[0080] Synthesis Example 6 A three-necked separable glass flask was fitted with a stirrer, a nitrogen inlet tube, and a cooling tube equipped with a water receiver. 64.45g (0.2 mol) of 3,4,3',4'-benzophenonetetracarboxylic dianhydride (hereinafter referred to as BTDA), 15.98g (0.06 mol) of 5-amino-1-(4'-aminophenyl)-1,3,3-trimethylindane, 9.94g (0.04 mol) of 1,3-bis(3-aminopropyl)tetramethyldisiloxane, 1.5g (0.015 mol) of valerolactone, 2.4g (0.03 mol) of pyridine, 200g of NMP, and 30g of toluene were charged and stirred at room temperature for 30 minutes, then heated to 180°C and stirred for 1 hour. During the reaction, the toluene-water azeotrope was removed. After cooling to room temperature, 48.33g (0.15mol) of BTDA, 66.60g (0.25mol) of 5-amino-1-(4'-aminophenyl)-1,3,3-trimethylindane, 360g of NMP, and 90g of toluene were added, and the mixture was stirred at room temperature for 30 minutes, and then heated to 180°C and stirred for 1 hour. The reaction was terminated by heating and stirring at 180°C for 2 hours and 30 minutes while removing the water-toluene azeotropic reflux from the system. The obtained product was diluted with NMP to obtain a block copolymer polyimide solution with a solid content of 20% by weight.

[0081] Comparative Synthesis Example 1 A separable three-necked glass flask was equipped with a stirrer, a nitrogen inlet tube, and a cooling tube equipped with a water receiver. 29.23g (0.1 mol) of 1,3-bis(3-aminophenoxy)benzene, 1.5g (0.015 mol) of valerolactone, 2.4g (0.03 mol) of pyridine, 200g of NMP, and 30g of toluene were charged and stirred at 200 rpm for 30 minutes at room temperature under a nitrogen atmosphere, and then heated to 180°C and stirred for 1 hour. During the reaction, the toluene-water azeotrope was removed. After cooling to room temperature, 48.33g (0.15 mol) of 3,4,3',4'-benzophenonetetracarboxylic dianhydride, 44.57g (0.25 mol) of 2,4-diethyl-6-methyl-1,3-benzenediamine (an aromatic diamine having an alkyl group at the ortho position relative to N-), 360g of NMP, and 90g of toluene were added, and the mixture was stirred at room temperature for 30 minutes, then heated to 180°C and stirred for 1 hour. The reaction was terminated by heating and stirring at 180°C for 2 hours and 30 minutes while removing the water-toluene azeotropic reflux from the system. The obtained product was diluted with NMP to obtain a block copolymer polyimide solution with a solid content of 20% by weight.

[0082] Comparative Synthesis Example 2 A three-necked separable glass flask was fitted with a stirrer, a nitrogen inlet tube, and a cooling tube equipped with a water receiver. 64.45 g (0.2 mol) of 3,4,3',4'-benzophenonetetracarboxylic dianhydride (hereinafter referred to as BTDA), 12.22 g (0.1 mol) of 2,4-diaminotoluene (an aromatic diamine having an alkyl group at the ortho position relative to the N-), 1.5 g (0.015 mol) of valerolactone, 2.4 g (0.03 mol) of pyridine, 200 g of NMP, and 30 g of toluene were charged and stirred at room temperature under a nitrogen atmosphere at 200 rpm for 30 minutes, and then heated to 180°C and stirred for 1 hour. During the reaction, the toluene-water azeotrope was removed. After cooling in the air, 48.33 g (0.15 mol) of BTDA, 73.08 g (0.25 mol) of 1,3-bis(3-aminophenoxy)benzene (aromatic ether bond-containing aromatic diamine), 360 g of NMP, and 90 g of toluene were added and stirred at room temperature for 30 minutes, then the temperature was raised to 180°C and heated and stirred for 1 hour. The reaction was terminated by heating and stirring at 180°C for 2 hours and 30 minutes while removing the water-toluene azeotropic reflux from the system. The obtained product was diluted with NMP to obtain a block copolymer polyimide solution with a solid content of 20% by weight.

[0083] (Preparation of Photosensitive Polyimide Resin Composition) In the following examples and comparative examples, "parts" means "parts by weight". Examples 1 to 6 20 parts of 2,6-di(4'-azidobenzal)-4-ethylcyclohexanone, 1 part of 9,10-dibutoxyanthracene, 1 part of 3-glycidoxypropylmethyldimethoxysilane, 0.1 parts of 5-methyl-1H-benzotrial, and 1 part of 1,3,5-tris(4-triethylmethyl-3-hydroxy-2,6-dimethylbenzyl)-1,3,5-triazine-2,4,6-(1H,3H,5H)-trione were added to 500 parts of the block copolymer polyimide solution (solid content 20% by weight) of Synthesis Examples 1 to 6, and the mixture was dissolved in methyl benzoate to obtain a photosensitive resin composition having a solid content of 20%.

[0084] Example 7 A photosensitive resin composition was prepared in the same manner as in Example 1 (using the polyimide solution of Synthesis Example 1), except that 2,6-di(4'-azidobenzal)-4-methylcyclohexanone was used instead of 2,6-di(4'-azidobenzal)-4-ethylcyclohexanone.

[0085] Example 8 A photosensitive resin composition was prepared in the same manner as in Example 1 (using the polyimide solution of Synthesis Example 1), except that 4,4'-diazidobenzalacetophenone was used instead of 2,6-di(4'-azidobenzal)-4-ethylcyclohexanone.

[0086] Example 9 A photosensitive resin composition was prepared in the same manner as in Example 1 (using the polyimide solution of Synthesis Example 1), except that 16.7 parts of YX-6954BH30 (polymer epoxy; manufactured by Mitsubishi Chemical Corporation) and 0.25 parts of WPBG-300 (photobase generator; manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) were further added.

[0087] Example 10 A photosensitive resin composition was prepared in the same manner as in Example 1 (using the polyimide solution of Synthesis Example 1), except that 5 parts of TEPIC-VL (trifunctional epoxy: manufactured by Nissan Chemical Industries, Ltd.) and 0.25 parts of WPBG-300 (photobase generator: manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) were further added.

[0088] Comparative Example 1 A photosensitive resin composition was prepared in the same manner as in Example 7 (using the polyimide solution of Synthesis Example 1), except that 2,6-di(4'-azidobenzal)-4-methylcyclohexanone was not used.

[0089] Comparative Example 2 A photosensitive resin composition was prepared in the same manner as in Example 7 (using the polyimide solution of Synthesis Example 1), except that 1.5 parts of 2,6-di(4'-azidobenzal)-4-methylcyclohexanone was used instead of 20 parts.

[0090] (Performance evaluation of polyimide resin composition) 1. Mechanical strength, thermal expansion coefficient and 5% thermal weight loss temperature The resin compositions obtained in Examples 1 to 10 and Comparative Examples 1 and 2 were spin-coated onto a 6-inch silicon wafer so that the film thickness after final drying would be 15 to 17 μm, and the wafer was pre-baked at 90° C. for 360 seconds. After that, the wafer was exposed to a high-pressure mercury lamp with an i-line equivalent of 2,500 mJ / cm 2 After exposure to light of all wavelengths, the film was immersed in a cyclopentanone solution for 120 seconds, and then dried by heating at 200° C. (or 180° C.) for 90 minutes to prepare a dried resin film. This dried resin film was peeled off from the wafer with hydrofluoric acid to prepare a test sample for measuring mechanical strength, thermal expansion coefficient, and 5% thermal weight loss temperature.

[0091] 2. Adhesion strength The dried resin film formed on the silicon wafer prepared above is used. (1) Using a cutter knife, make 11 cuts reaching down to the base material on the test surface to create 100 grids. Use a cutter guide to make the cuts 1 mm apart. (2) Firmly press cellophane tape (registered trademark) onto the grid, then pull off the end of the tape at a 45° angle in one go, and evaluate the state of the grid by comparing it with the standard diagram. Determine the adhesion strength after 240 hours under normal conditions and HAST (80℃ x 85% RH).

[0092] 3. Film Remaining Rate The resin compositions obtained in Examples 1 to 10 and Comparative Examples 1 and 2 were spin-coated onto 6-inch silicon wafers so that the film thickness after final drying would be 5 to 7 μm and 10 to 12 μm, respectively, and the wafers were pre-baked at 90° C. for 240 seconds and 90° C. for 300 seconds. The thicknesses (t 1 ) is then measured using a high-pressure mercury lamp, with the i-line equivalent being 1,000 (or 2,500) mJ / cm 2 After exposure to all wavelengths, the film was immersed in a cyclopentanone solution for 120 seconds and then measured for thickness (t 2 ) is measured. Then, the film is dried by heating at 200℃ (or 180℃) for 90 minutes, and the thickness (t 3 ) are measured. From these measurements, t 2 / t 1、 t 3 / t 1 and t 3 / t 2 was calculated as the remaining film rate.

[0093] 4. Exposure and development properties The pattern evaluation was carried out by the following method. (1) Resolution The resin compositions obtained in Examples 1 to 10 and Comparative Examples 1 and 2 were dropped onto a 6-inch silicon wafer and spin-coated for 30 seconds, then pre-baked on a hot plate at 90°C for 240 seconds. At this time, the coating spin was adjusted so that the film thickness after baking would be approximately 6 to 8 μm. Next, exposure was performed using a high-pressure mercury lamp. The exposure dose measured with i-line was 1,000 mJ / cm. 2 Then, the pattern was developed with cyclopentanone, rinsed, and dried at 200°C (or 180°C) for 90 minutes. The resolution was determined as the smallest resolution among L / S=5 / 5, 10 / 10, 15 / 15, 20 / 20, 30 / 30, 50 / 50μm and square via hole patterns of 10, 15, 20, 30, 40, and 50μm.

[0094] (2) Pattern edge residue, cracks Pattern processing was performed in the same manner as in (1) above, and first, the film surface after development was visually observed for abnormalities. Next, a 15 μm square via hole pattern was observed with an optical microscope, and if there was a crack at the corner of the pattern, it was judged to have a crack. Furthermore, the pattern edge of L / S=15 / 15 was observed, and if there was a development residue, it was judged to have a residue.

[0095] The evaluation results of the resin compositions obtained in Examples 1 to 10 and Comparative Examples 1 to 2 are shown in Tables 1 and 2 below. In the evaluation of the residual film rate and exposure developability of the resin compositions obtained in Comparative Examples 1 to 2, the film was dissolved when immersed in a cyclopentanone solution after exposure. This result indicates that the resin compositions obtained in Comparative Examples 1 to 2 did not have good solvent insolubility after photocrosslinking. Therefore, the Tg, thermal expansion coefficient, 5% thermal weight loss temperature, mechanical strength, and adhesion strength of the resin compositions obtained in Comparative Examples 1 to 2 were evaluated by preparing samples without immersing the resin compositions in a cyclopentanone solution. On the other hand, it can be seen that the resin compositions obtained in Examples 1 to 10 have both solvent solubility during development and solvent insolubility after photocrosslinking, and also achieve good film properties and high sensitivity.

[0096] [Table 1]

[0097] [Table 2] [Industrial Applicability]

[0098] The negative type photosensitive polyimide resin composition of the present invention is useful for producing, for example, electronic elements such as semiconductor packages such as FO-WLP and WLP, thin film magnetic elements such as thin film magnetic heads, thin film inductors, and common mode choke coils, display elements such as TFT liquid crystal elements, color filter elements, and organic EL elements, and organic multilayer wiring boards, and can be suitably used in the field of photosensitive materials.

Claims

1. A photosensitive polyimide resin composition comprising (A) a solvent-soluble polyimide and (B) a diazide compound as essential components, the (A) solvent-soluble polyimide is a block copolymer having, in its main chain, (a) an aromatic tetracarboxylic dianhydride residue having a benzophenone structure and (b) an aromatic diamine residue having a phenylindane structure, The photosensitive polyimide resin composition has a content of the diazide compound (B) of 2.0 to 150 parts by weight based on 100 parts by weight of the solvent-soluble polyimide (A).

2. A photosensitive polyimide resin composition comprising (A) a solvent-soluble polyimide and (B) a diazide compound as essential components, the (A) solvent-soluble polyimide is a block copolymer having, in its main chain, (a) an aromatic tetracarboxylic dianhydride residue having a benzophenone structure, and (b) a residue of at least one diamine selected from the group consisting of an aromatic diamine having an alkyl group at the ortho-position of an amino group, an aromatic diamine having an indane structure, and a diamine having a polysiloxane structure; The (B) diazide compound is 2,6-di(4'-azidobenzal)-4-ethylcyclohexanone, The photosensitive polyimide resin composition has a content of the diazide compound (B) of 2.0 to 150 parts by weight based on 100 parts by weight of the solvent-soluble polyimide (A).

3. A photosensitive polyimide resin composition comprising, as essential components, (A) a solvent-soluble polyimide, (B) a diazide compound, (C) an epoxy resin, and (D) a photobase generator, the (A) solvent-soluble polyimide is a block copolymer having, in its main chain, (a) an aromatic tetracarboxylic dianhydride residue having a benzophenone structure, and (b) a residue of at least one diamine selected from the group consisting of an aromatic diamine having an alkyl group at the ortho-position of an amino group, an aromatic diamine having an indane structure, and a diamine having a polysiloxane structure; The photosensitive polyimide resin composition has a content of the diazide compound (B) of 2.0 to 150 parts by weight based on 100 parts by weight of the solvent-soluble polyimide (A).

4. The resin composition according to any one of claims 1 to 3, wherein the photosensitive polyimide resin composition is a negative-tone solvent-developable composition.

5. A method for forming a pattern, comprising exposing a substrate coated with the resin composition according to any one of claims 1 to 4 to ultraviolet light and developing and removing unexposed areas.

6. A semiconductor package, an electronic element, a display element, or an organic multilayer wiring board having an interlayer insulating film, a passivation film, or a surface protective film formed using the resin composition according to any one of claims 1 to 4.

Citation Information

Patent Citations

  • Producing method and producing device of semiconductor device

    JP1977016179A

  • Heattresistant photosensitive material

    JP1979145794A

  • Encipherment treatment system

    JP1980041422A

  • Cover material

    JP1987056948A

  • Photosensitive polymer composition

    JP1987179563A