Breathable and water-resistant member, and method for manufacturing breathable and water-resistant member

A breathable and water-resistant member with a micropore structure and water-repellent coating film addresses the lack of breathability and durability in existing waterproof members, ensuring high air permeability and water resistance with improved durability.

JP7565158B2Active Publication Date: 2024-10-10NIHON TOKUSHU TORYO CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2020021760
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-02-12
Publication Date
2024-10-10
Estimated Expiration
2040-02-12

AI Technical Summary

Technical Problem

Existing waterproof members lack both breathability and durability, with coating films having low hardness and durability issues.

Method used

A breathable and water-resistant member with micropores and a water-repellent coating film containing water-repellent particles and a binder resin, achieving a pencil hardness of 5B or more and a water contact angle of 90° or more, formed by applying a paint containing these components to a base material with micropores.

Benefits of technology

The member achieves good air permeability, water resistance, and enhanced durability, maintaining performance under high-pressure water washing.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 00000011_0000
    Figure 00000011_0000
  • Figure 00000012_0000
    Figure 00000012_0000
  • Figure 00000013_0000
    Figure 00000013_0000
Patent Text Reader

Abstract

To provide an air-permeable and water-resistant member having excellent air permeability and water resistance, and also having excellent durability, and provide a method for producing the air-permeable and water-resistant member.SOLUTION: An air-permeable and water-resistant member has an air-permeable part having micropores, and a water-repellent part having a coating comprising water-repellent particles and binder resin on its outermost surface layer. The coating has a pencil hardness of 5B or more at a load of 750±10 g, measured in accordance with JIS K 5600-5-4: 1999. There is also provided a method for producing the air-permeable and water-resistant member.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a breathable and water-resistant member and a method for manufacturing the breathable and water-resistant member. [Background technology]

[0002] 2. Description of the Related Art Conventionally, various waterproof members using water-repellent materials have been proposed for use in a wide range of fields, from fields requiring waterproofing for everyday life to the field of aircraft. In the aircraft field, for example, Patent Document 1 describes a mixed paint that can be suitably used in aircraft and is made by mixing a room-temperature reaction curing resin and a particulate fluororesin. Patent Document 2 describes an aircraft component that uses a mixed paint made by mixing a room-temperature reaction curing resin and a particulate fluororesin.

[0003] In recent years, there has been an increasing need for waterproof materials that are both waterproof and breathable, and the development of such materials is being promoted. For example, Patent Documents 3 and 4 disclose water-repellent net-like bodies that have been subjected to a water-repellent treatment using a water-repellent material that contains a fluorine-containing compound. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] Patent No. 5842023 [Patent Document 2] Patent No. 6170531 [Patent Document 3] JP 2000-290877 A [Patent Document 4] JP 2007-239109 A Summary of the Invention [Problem to be solved by the invention]

[0005] However, the inventors have found that the members described in Patent Documents 3 and 4 have problems in that the coating film obtained by the water-repellent treatment has low hardness and low durability. Moreover, Patent Documents 1 and 2 do not describe a member that is both waterproof and breathable.

[0006] Therefore, an object of the present invention is to provide a breathable and water-resistant member having good breathability and water resistance as well as excellent durability, and a method for manufacturing the breathable and water-resistant member. [Means for solving the problem]

[0007] The present inventors have found that the above problems can be solved by the following configuration. [1] A breathable and water-resistant member having a ventilation part having micropores and a water-repellent part having a coating film containing water-repellent particles and a binder resin as an outermost layer, The area of ​​the micropores is 1000 μm 2 ~25000μm 2 and The coating film has a pencil hardness of 5B or more under a load of 750±10 g as measured in accordance with JIS K 5600-5-4:1999; A breathable and waterproof member having a mesh shape. [2] before The breathable and water-resistant member according to [1], wherein the water contact angle of the coating surface in the water-repellent portion is 90° or more. [3] The method includes a step of applying a coating material containing water-repellent particles, a binder resin, and a solvent to a substrate having a ventilation portion with micropores, and forming a water-repellent portion having a coating film containing the water-repellent particles and the binder resin as an outermost layer, The area of ​​the micropores is 1000 μm 2 ~25000μm 2 and The method for producing a breathable and waterproof member according to [1] or [2], wherein the substrate has a mesh shape. [4] The method for producing a breathable and waterproof member according to [3], wherein the solvent is a fluorine-based solvent. Although the present invention relates to the above items [1] to [4], other items are also described for reference.

[0008] <1> A breathable and water-resistant member having a ventilation part having micropores and a water-repellent part having a coating film containing water-repellent particles and a binder resin as an outermost layer, The coating film has a pencil hardness of 5B or more under a load of 750±10 g, as measured in accordance with JIS K 5600-5-4:1999. <2> The area of ​​the micropores is 1 μm 2 ~1mm 2 and the water contact angle of the coating surface in the water-repellent portion is 90° or more. <1> The breathable and water-resistant member according to claim 1. <3> The method includes a step of applying a coating material containing water-repellent particles, a binder resin, and a solvent to a substrate having a ventilation portion with micropores, and forming a water-repellent portion having a coating film containing the water-repellent particles and the binder resin as an outermost layer. <1> or <2> A method for producing the breathable and waterproof member described in claim 1. <4> The solvent is a fluorine-containing solvent. <3> A method for producing the breathable and waterproof member described in claim 1. Effect of the Invention

[0009] According to the present invention, it is possible to provide a breathable and water-resistant member having good breathability and water resistance as well as excellent durability. Also, according to the present invention, it is possible to provide a method for producing the breathable and water-resistant member. [Brief description of the drawings]

[0010] [Figure 1] FIG. 2 is a schematic diagram showing an example of a breathable and water-resistant member. [Diagram 2] FIG. 2 is a schematic end view of an example of a breathable and waterproof member. [Diagram 3] FIG. 2 is a schematic diagram showing an example of a substrate. [Figure 4] FIG. 2 is a schematic diagram of an end surface of an example of a substrate. [Diagram 5] FIG. 2 is a diagram showing the appearance of the coating film of the breathable and waterproof member of Example 1 before a high-pressure water washing test was conducted. [Figure 6] 1 is a diagram showing the appearance of the coating film of the breathable and waterproof member of Example 1 after a high-pressure water washing test was carried out for 30 minutes. [Figure 7] FIG. 2 is a diagram showing the appearance of the coating film of the breathable and waterproof member of Example 2 before a high-pressure water washing test was conducted. [Figure 8] A figure showing the appearance of the coating film of the breathable and waterproof member of Example 2 after a high-pressure water washing test was conducted for 30 minutes. [Figure 9] FIG. 2 is a diagram showing the appearance of the coating film of the breathable and waterproof member of Comparative Example 1 before a high-pressure water washing test was performed. [Figure 10] FIG. 2 is a diagram showing the appearance of the coating film of the breathable and waterproof member of Comparative Example 1 after a high-pressure water washing test was carried out for 30 minutes. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] The breathable and water-resistant member of the present invention is a breathable and water-resistant member having a breathable portion with micropores and a water-repellent portion having a coating film containing water-repellent particles and a binder resin as an outermost layer, and the coating film has a pencil hardness of 5B or more under a 750±10 g load measured in accordance with JIS K 5600-5-4:1999.

[0012] DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS A breathable and water-resistant member and a method for manufacturing the same according to the present invention will be described below. Each configuration and combination thereof in the following embodiments are merely examples, and the present invention is not limited to the embodiments. In this specification, the symbol "to" is used to mean that the numerical values ​​before and after it are included as the lower limit and upper limit.

[0013] The breathable and water-resistant member of the present invention has a breathable portion and a water-repellent portion. The ventilation portion is a portion necessary for ensuring breathability, and can be formed, for example, by using a breathable base material (a base material having fine through holes). The water-repellent portion is a portion that has water repellency, and can be formed by a coating film that contains water-repellent particles and a binder resin.

[0014] <Coating film> The breathable and water-resistant member of the present invention has a coating film containing water-repellent particles and a binder resin as the outermost layer of the water-repellent portion.

[0015] (Water-repellent particles) The water-repellent particles contained in the coating film are not particularly limited, but examples thereof include polytetrafluoroethylene resin (hereinafter referred to as "PTFE"), pitch fluoride, graphite fluoride, silicone powder, hydrophobic silica, methyl silicone powder, PTFE solvent dispersion, etc. As the water-repellent particles, particulate fluororesin is preferable, and as the particulate fluororesin, PTFE is particularly preferable. The method for preparing PTFE is not particularly limited. PTFE has a high water repellency effect and is easily mixed with a binder resin, so that PTFE having a low molecular weight, specifically, an average molecular weight of 500 to 5000, is preferred.

[0016] The average primary particle size of the water-repellent particles is preferably from 0.05 μm to 60 μm, and more preferably from 0.05 μm to 30 μm.

[0017] The average particle size of the water-repellent particles in the coating film is preferably 0.05 μm to 60 μm from the viewpoint of suppressing clogging of micropores and improving coating workability, and more preferably 0.05 μm to 30 μm. The average particle size here refers to the average particle size of particles including both primary particles and aggregated particles of the water-repellent particles.

[0018] The average primary particle size of the water-repellent particles and the average particle size of the water-repellent particles in the coating film can be measured by a laser diffraction particle size distribution measuring device (eg, SALD-2200 manufactured by Shimadzu Corporation).

[0019] The content of the water-repellent particles in the coating film is preferably 10 to 70% by mass from the viewpoint of water repellency and durability, more preferably 30 to 70% by mass, and even more preferably 50 to 70% by mass.

[0020] (binder resin) The binder resin is not particularly limited, but examples thereof include polyurethane resin, fluororesin, acrylic urethane resin, acrylic resin, and epoxy resin. From the viewpoint of durability, the binder resin is preferably a polyurethane resin. The binder resin may be any one of these resins or a mixture of two or more of them.

[0021] The content of the binder resin in the coating film is preferably 30 to 90% by mass from the viewpoints of water repellency and durability, more preferably 30 to 70% by mass, and even more preferably 30 to 50% by mass.

[0022] The coating film may contain other components in addition to the water-repellent particles and the binder resin, and examples of the other components include an antifoaming agent, a dispersant, a leveling agent, a catalyst, etc. When other components are contained, the content in the coating film is preferably 10% by mass or less.

[0023] The thickness of the coating film is not particularly limited, but is preferably 5 to 200 μm from the viewpoints of durability and breathability, and more preferably 10 to 60 μm.

[0024] <Base material> As described below, the breathable and waterproof member of the present invention is preferably obtained by applying a coating material containing water-repellent particles, a binder resin, and a solvent to a substrate having a ventilation portion with micropores to form a coating film. In the above-mentioned substrate, the shape of the micropores is not particularly limited and can be appropriately selected depending on the purpose. Examples of the shape include polygonal shapes such as triangles, rectangles, and pentagons, circles, ellipses, and stars. The area of ​​the micropores is 1 μm 2 ~1mm 2 From the viewpoint of water resistance, it is preferable that 2 ~25000μm 2 It is more preferable that:

[0025] The substrate used in the present invention preferably has a plurality of ventilation parts formed of fine holes, and specifically, the substrate is preferably in the form of a mesh.

[0026] The shape of the substrate is not particularly limited and can be appropriately selected depending on the purpose, and examples thereof include a flat, spherical, cylindrical, etc. shape.

[0027] The material of the substrate is not particularly limited and can be appropriately selected depending on the purpose. Examples of the material include metal substrates, glass substrates, wood substrates, ceramic substrates, plastic substrates, paper, and nylon fibers.

[0028] The substrate may be one that has been appropriately prepared, or a commercially available product may be used. The thickness of the substrate is not particularly limited and can be appropriately selected depending on the purpose, but is preferably 0.01 to 50 mm, and more preferably 0.1 to 20 mm.

[0029] [Ventilated and waterproof materials] The breathable and waterproof member of the present invention has a breathable part having fine pores and a water-repellent part having the above-mentioned coating film as the outermost layer. FIG. 1 shows a schematic diagram (plan view (viewed from a direction perpendicular to the coating surface)) of one example of the breathable and waterproof member of the present invention. The breathable and water-resistant member 1 shown in FIG. 1 has a breathable portion 2 (white portion) and a water-repellent portion 3 (hatched portion). Fig. 2 shows a schematic diagram of an end surface cut along dashed line AA' (schematic diagram of an end surface perpendicular to the coating surface) of the breathable and water-resistant member 1 in Fig. 1. The breathable and water-resistant member 1 in Fig. 2 is formed with a water-repellent portion 3 on the surface (outermost surface) of a substrate 4 (vertical line portion) having micropores. The water-repellent portion 3 is made of a coating film containing the water-repellent particles and binder resin described above. The coating film may be present on a part of the surface of the substrate, or on the entire surface of the substrate. For example, when the substrate is a flat substrate, the coating film may be present on one surface or on both surfaces. A preferred embodiment of the breathable and water-resistant member of the present invention is one in which a water-repellent portion 3 made of a coating film is provided not only on both surfaces of the substrate 4 but also on the surface of the inner wall 4a of the substrate 4, as shown in Figure 2, thereby achieving the effect of significantly improving water resistance.

[0030] FIG. 3 is a schematic diagram (plan view (viewed from a direction perpendicular to the surface of the substrate)) of one example of a substrate that can be used in the breathable and water-resistant member of the present invention. The substrate 4 shown in FIG. 3 has ventilation parts 2 consisting of micropores. Fig. 4 shows a schematic diagram of an end surface (schematic diagram of an end surface in a direction perpendicular to the surface of the substrate) taken along dashed line BB' of the substrate 4 in Fig. 3. The ventilation portion 2 of the substrate 4 is composed of fine holes passing through the substrate.

[0031] In the breathable and waterproof member of the present invention, the area of ​​the micropores of the ventilation part is 1 μm 2 ~1mm 2 From the viewpoint of breathability, it is preferable that the thickness is 1000 μm. 2 ~25000μm 2 It is more preferable that:

[0032] (water contact angle) In the breathable and waterproof member of the present invention, the water contact angle of the coating film surface is preferably 90° or more, more preferably 120° or more, and even more preferably 150° or more. By making the water contact angle 150° or more, particularly excellent water resistance can be achieved.

[0033] (Pencil hardness) In the breathable and water-resistant member of the present invention, the coating film has a pencil hardness of 5B or more under a load of 750±10 g measured according to JIS K 5600-5-4:1999. It is believed that by making the pencil hardness of the coating film surface 5B or more, it is possible to obtain a breathable and water-resistant member having high durability against high-pressure water washing, abrasion, and the like. The upper limit of the pencil hardness is preferably 3H or less. By making it 3H or less, it becomes easier to follow the flexibility of the substrate, and damage due to cracking or the like of the breathable and water-resistant member can be suppressed. Here, "5B or higher" means that the pencil hardness is 5B or harder than 5B. "3H or lower" means that the pencil hardness is 3H or softer than 3H. The pencil hardness of the coating film is preferably 5B to 3H.

[0034] (Surface roughness Ra) The arithmetic mean roughness (Ra) of the coating surface of the breathable and waterproof member of the present invention is not particularly limited, since it varies depending on the method for forming the coating (applying method). A preferred embodiment of the breathable and water-resistant member of the present invention is one in which the Ra of the coating film surface is 8 μm or less. By making the Ra of the coating film surface 8 μm or less, clogging in the ventilation part of the breathable and water-resistant member can be suppressed, and the breathability can be improved. However, it is believed that Ra does not affect other physical properties of the coating film. The means for making the coating surface Ra 8 μm or less is not particularly limited, but for example, it can be formed by a method of applying a paint containing water-repellent particles, a binder resin, and a solvent using a spray gun. In particular, it is preferable to use a fluorine-based solvent as the solvent, since the dispersibility of the water-repellent particles in the paint is improved, making it possible to reduce the Ra of the coating surface. The surface roughness index Ra can be measured by the JIS B0633 stylus method (for example, SURFCOM2900 SD3-12 manufactured by Tokyo Seimitsu).

[0035] [Method of manufacturing breathable and waterproof member] The present invention also relates to a method for producing a breathable and waterproof member, which includes a step of applying a coating material containing water-repellent particles, a binder resin, and a solvent to a substrate having a ventilation part with micropores, and forming a water-repellent part having a coating film containing the water-repellent particles and the binder resin as the outermost layer.

[0036] <Paint> The coating material used in the manufacturing method of the breathable and waterproof member of the present invention (hereinafter also referred to as the manufacturing method of the present invention) contains water-repellent particles, a binder resin, and a solvent.

[0037] The water-repellent particles and the binder resin are as described above. The coating material may contain other components as solids other than the water-repellent particles and the binder resin, and the above-mentioned other components can be used. The binder resin may be contained in the coating material as a raw material monomer, and may be formed into the binder resin by a polymerization reaction after coating.

[0038] (solvent) The solvent used in the coating material is not particularly limited, and examples thereof include fluorine-based solvents, aliphatic and aromatic hydrocarbon solvents, ketone-based solvents, carboxylate-based solvents, alcohol-based solvents, ether-based solvents, amide-based solvents, etc. From the viewpoint of improving the dispersibility of the water-repellent particles, fluorine-based solvents are preferable. In addition, when a fluorine-based solvent is used as the solvent, the viscosity of the coating material decreases, and the discharge amount increases when the coating material is sprayed, which has the effect of improving productivity. Examples of fluorine-based solvents include perfluorocarbons (PFCs), hydrochlorofluorocarbons (HCFCs), hydrofluorocarbons (HFCs), and hydrofluoroethers (HFEs). The content of the fluorine-based solvent in the paint is not particularly limited, but from the viewpoints of the coatability of the paint and the dispersibility of the water-repellent particles, it is preferably 0.1% by mass to 50% by mass, and more preferably 5% by mass to 40% by mass, of the total solid content in the paint.

[0039] The average particle size of the water-repellent particles in the coating material is not particularly limited, but is preferably 0.05 μm to 100 μm from the viewpoint of suppressing clogging of micropores and improving breathability, more preferably 0.05 μm to 50 μm, and even more preferably 0.05 μm to 20 μm. The average particle size here refers to the average particle size of particles including both primary particles and aggregated particles of the water-repellent particles.

[0040] <Water-repellent part formation process> The manufacturing method of the present invention includes a step of applying the above-mentioned coating material to a substrate having a ventilation portion with micropores, and forming a water-repellent portion having a coating film containing the above-mentioned water-repellent particles and the above-mentioned binder resin as the outermost layer.

[0041] As the substrate having a ventilation portion having micropores, the substrates mentioned above in the description of the breathable and water-resistant member can be used.

[0042] The coating method is not particularly limited, but examples thereof include spray coating, dip coating, spin coating, brush coating, roller coating, and the like.

[0043] After application of the coating material, it is preferable to remove the solvent by drying to form a coating film.

[0044] The thickness of the coating film is preferably 5 to 200 μm from the viewpoint of durability, and more preferably 10 to 60 μm.

[0045] The coating film may be formed on a part of the surface of the substrate, or on the entire surface. For example, when the substrate is a flat substrate, the coating film may be formed on one surface, or on both surfaces. From the viewpoint of water resistance, it is more preferable that the coating film is applied to the inner surface of the pores.

[0046] The breathable and waterproof member of the present invention has breathability, water resistance, and durability, and can therefore be suitably used for audio equipment, screen doors, umbrellas, clothing, shoes, bags, packaging materials, agricultural sheets, and the like. EXAMPLES

[0047] The present invention will be described in more detail with reference to the following examples. The materials, amounts, ratios, processing contents, processing procedures, etc. shown in the following examples can be changed as appropriate without departing from the spirit of the present invention.

[0048] [Paint used] Paint a: Skyhalo HAS (PTFE-containing two-component solvent-based paint (containing fluorine-based solvent, polyurethane), manufactured by Nippon Tokushu Toryo Co., Ltd.) Paint B: Paint according to Example 2 of Japanese Patent No. 5842023 (PTFE-containing two-component solvent-based paint (no fluorine-based solvent, polyurethane-containing) Paint c: HIREC100 (PTFE-containing one-component solvent-based paint) manufactured by NTT Advanced Technology Corporation)

[0049] The average particle size of the particulate fluororesin in each paint was measured using an SALD-2200 (manufactured by Shimadzu Corporation). The results are shown in Table 1.

[0050] [Manufacturing of breathable and waterproof members] <Example 1> Paint a was applied to a stainless steel substrate, a φ130 mm circular 100 mesh (mesh size 154 μm), using an air spray gun LPH-101-164LVG (manufactured by Anest Iwata Corporation), and cured at room temperature to form a coating film, thereby obtaining a breathable and waterproof component sample (test piece) of Example 1. The application conditions for the air spray gun were as follows: LPH-101-164LVG: diameter 1.6 mm (manufactured by Anest Iwata), hand pressure 1.0 kg / cm 2 The pattern width was expanded to its full width using the attached screw, the discharge volume adjustment screw was adjusted to three turns, the distance from the substrate was fixed at 15 cm, and then coating was performed. The dry thickness of the coating film was set to 15 μm to 20 μm.

[0051] <Example 2, Comparative Example 1> Except for changing the paint a to the paint shown in Table 1, the same method as in Example 1 was used to obtain breathable and waterproof member samples of Example 2 and Comparative Example 1.

[0052] (Paint discharge amount) The amount of each paint dispensed when applied with an air spray gun was measured, and the results are shown in Table 1.

[0053] (Pencil hardness) The outermost coating film of each of the obtained breathable and waterproof member samples was subjected to pencil hardness evaluation according to JIS K 5600-5-4:1999 under a load of 750±10 g. The results are shown in Table 1.

[0054] (Surface roughness) The arithmetic mean surface roughness Ra of the water-repellent portion on the coating side of each of the obtained breathable and water-resistant member samples was measured using SURFCOM2900 SD3-12 (manufactured by Tokyo Seimitsu) according to the method described in JIS B0633: 2001. The results are shown in Table 1.

[0055] (Water droplet contact angle) The water droplet contact angle of each of the obtained breathable and water-resistant member samples was measured using DMs-601 (manufactured by Kyowa Interface Science Co., Ltd.) according to the method described in JIS R 3257 6.3:1999 Wettability test. The results are shown in Table 1.

[0056] (micropore area ratio) For each of the obtained breathable and waterproof member samples, the micropore area ratio was measured using the automatic area calculation of a digital microscope VHX-2000 (manufactured by Keyence). The measurement was performed at a magnification of 100 times, and a certain area (8.8 mm 2 ) was calculated as the ratio of the total area of ​​micropores to the total area of ​​micropores.

[0057] (micropore unit area) For each of the obtained breathable and waterproof member samples, the micropore unit area was measured using the automatic area calculation of a digital microscope VHX-2000 (manufactured by Keyence Corporation). The measurement was performed at a magnification of 300 times, and the average value of eight micropores was calculated.

[0058] The following performance evaluations were carried out for each of the obtained breathable and waterproof member samples.

[0059] <Breathability> The air permeability of each of the obtained breathable and water-resistant member samples was measured according to JIS L 1096 8.26:2010 Air Permeability Method A, Frazier type method. The measurement was performed using a Frazier type air permeability tester (FP2, manufactured by Toyo Seiki Seisakusho Co., Ltd.) with a measurement area of ​​5 cm 2 The evaluation was performed based on the air flow rate when a suction pressure (differential pressure) of 125 Pa was applied to the test piece. The results are shown in Table 1 for the case where the high-pressure water washing time was 0 minutes.

[0060] <Water resistance> The water resistance of each of the obtained breathable and water-resistant members was measured according to JIS L 1092 7.1:2009 Water resistance test (hydrostatic pressure method). For the measurement, a high water pressure water resistance tester (WP-1000K, manufactured by Daiei Scientific Instruments Co., Ltd.) was used to gradually pressurize the test piece, and the test piece was evaluated based on the pressure when water passed through three points. The results are shown in Table 1 as the results for a high-pressure water washing time of 0 minutes. Note that 1 mmAq = 9.80665 Pa.

[0061] <Durability: High pressure water washing test> Water was sprayed at 15 MPa from a distance of 50 cm from the coating film of each of the obtained breathable and waterproof members, and a high-pressure water washing test was performed. The high-pressure water washing time was 5 minutes, 15 minutes, and 30 minutes. For each test piece after high-pressure water washing, the breathability, water resistance, and coating appearance were evaluated in the same manner as described above. The evaluation results are shown in Table 1. The coating appearance was observed after the test using an image magnified 100 times with a digital microscope VHX-2000 (manufactured by Keyence). Figure 5 shows the coating appearance of Example 1 before the high-pressure water washing test, Figure 6 shows the coating appearance of Example 1 after the high-pressure water washing test for 30 minutes, Figure 7 shows the coating appearance of Example 2 before the high-pressure water washing test, Figure 8 shows the coating appearance of Example 2 after the high-pressure water washing test for 30 minutes, Figure 9 shows the coating appearance of Comparative Example 1 before the high-pressure water washing test, and Figure 10 shows the coating appearance of Comparative Example 1 after the high-pressure water washing test for 30 minutes.

[0062] [Table 1]

[0063] From the results in Table 1, the breathable and waterproof member of the present invention had good breathability and water resistance. In addition, the change in breathability and water resistance before and after the durability test using high-pressure water washing was small, indicating that the member had excellent durability. In particular, in Example 1, in which a fluorine-based solvent was used as the solvent in the paint, the particulate fluororesin was present on the member surface in a more dispersed state, so that clogging of the micropores was less likely to occur, and it is believed that the breathability before the durability test was improved. In addition, the paint of Example 1, which used a fluorine-based solvent, had a large discharge amount and was highly productive. On the other hand, in Comparative Example 1, the hardness of the coating film was low and the coating film peeled off due to high-pressure water washing, which is thought to be the reason for the decrease in water resistance. [Explanation of symbols]

[0064] 1. Ventilated and waterproof materials 2 Ventilation section 3 Water-repellent section 4 Base material 4a Inner wall of substrate

Claims

1. A breathable and water-resistant member having a ventilation part having micropores and a water-repellent part having a coating film containing water-repellent particles and a binder resin as an outermost layer, The area of ​​the micropores is 1000 μm 2 to 25000 μm 2 , The coating film has a pencil hardness of 5B or more under a load of 750±10 g as measured in accordance with JIS K 5600-5-4:1999; A breathable and waterproof member having a mesh shape.

2. A breathable and water-resistant member as described in claim 1, wherein the water contact angle of the coating surface in the water-repellent portion is 90° or more.

3. The method includes a step of applying a coating material containing water-repellent particles, a binder resin, and a solvent to a substrate having a ventilation portion with micropores, and forming a water-repellent portion having a coating film containing the water-repellent particles and the binder resin as an outermost layer, The area of ​​the micropores is 1000 μm 2 to 25000 μm 2 , The method for producing a breathable and waterproof member according to claim 1 or 2, wherein the substrate has a mesh shape.

4. The method for producing a breathable and waterproof member according to claim 3, wherein the solvent is a fluorine-based solvent.

Citation Information

Patent Citations

  • Endoscope provided with solid-state image pickup element

    JP1983042023A

  • Driving method of liquid crystal element

    JP1986070531A

  • Water repellent reticulate material and its production

    JP2000290877A

  • Impermeable opening member

    JP2007239109A