Grain-finish artificial leather and its manufacturing method

The use of a water-based adhesive and buffing process to bond polyurethane layers in artificial leather addresses curling and VOC emissions, ensuring effective adhesion and environmental compliance.

JP7565200B2Active Publication Date: 2024-10-10KURARAY CO LTD
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
JP2020196791
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-11-27
Publication Date
2024-10-10
Estimated Expiration
2040-11-27

AI Technical Summary

Technical Problem

Silver-finished artificial leather experiences curling issues due to low adhesive strength in the polyurethane adhesive layer, leading to peeling and reduced workability, and the use of solvent-based adhesives contributes to VOC emissions and surface roughening, which are regulated and difficult to eliminate completely.

Method used

A manufacturing process that uses a water-based polyurethane adhesive to bond a polyurethane skin layer with a buffed wet polyurethane porous layer, ensuring no large pores remain on the surface to prevent curling and reduce VOC emissions, by roughening the porous layer through buffing and using a polyurethane association type thickener to maintain adhesive strength.

Benefits of technology

The process effectively prevents curling in silver-finished artificial leather and significantly reduces residual organic solvents, enhancing workability and compliance with environmental regulations.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007565200000001
    Figure 0007565200000001
  • Figure 0007565200000002
    Figure 0007565200000002
  • Figure 0007565200000003
    Figure 0007565200000003
Patent Text Reader

Abstract

To provide a grained tone artificial leather having a constitution in which a polyurethane skin layer is bonded on a wet-type porous polyurethane layer through a polyurethane adhesive layer, which can suppress curl generation immediately after production.MEANS: A grained tone artificial leather manufacturing method to be used comprises: a step to prepare a base material having a fiber entangled form and a wet-type porous polyurethane layer that is impregnated with and laminated on and integrated with the fiber entangled form; a step to buff a surface of the wet-type porous polyurethane layer so as not to expose open holes with average diameter of 15 μm or larger; a step to prepare a polyurethane skin layer; a step to form a polyurethane adhesive layer by applying an aqueous polyurethane adhesive containing aqueous polyurethane on a surface of the polyurethane skin layer or the wet-type porous polyurethane layer after buffing, and subsequently drying; and a press step to bond the wet-type porous polyurethane layer after buffing and the polyurethane skin layer to each other through the polyurethane adhesive layer.SELECTED DRAWING: Figure 2
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a grain-finished artificial leather comprising a fiber-entangled body, a wet-type polyurethane porous layer impregnated and laminated onto the fiber-entangled body to form an integrated body, and a polyurethane surface layer laminated onto the wet-type polyurethane porous layer via a polyurethane adhesive layer, and a method for producing the same. [Background technology]

[0002] There is known a grain-finished artificial leather having a grain-finished appearance similar to that of natural leather, which is used as a skin material for bags, clothing, shoes, etc. One such grain-finished artificial leather is one that includes a fiber entanglement body, a wet-type polyurethane porous layer laminated on the fiber entanglement body, and a polyurethane skin layer bonded to the wet-type polyurethane porous layer via a polyurethane adhesive layer.

[0003] For example, Patent Document 1 listed below discloses a grain-finished artificial leather having a grain surface layer formed from an aqueous polyurethane resin dispersion on at least one surface of a base layer made of a three-dimensionally entangled nonwoven fabric of staple fibers and a polymeric elastomer provided by an aqueous resin dispersion, in which the grain surface layer and the base layer are bonded together using a crosslinked polyurethane made from the aqueous polyurethane resin dispersion and a crosslinking agent, and the crosslinked polyurethane permeates into the base layer 150 to 400 μm below the surface of the base layer.

[0004] Also, for example, Patent Document 2 listed below discloses a method for producing a grain-finished artificial leather, which includes a step of applying a polyurethane solution to a fiber base layer, and wet-coagulating the solution to laminate a wet-type polyurethane porous layer on the surface of the fiber base layer, buffing the surface of the wet-type polyurethane porous layer, and then adhering a polyurethane skin layer to the surface via a polyurethane adhesive layer formed from a solvent-based adhesive.

[0005] Furthermore, for example, Patent Document 3 listed below discloses a two-component curing water-based adhesive used in the production of synthetic leather, which contains a base agent containing an aqueous polyurethane resin and a curing agent containing a polyisocyanate compound, in which the polyisocyanate compound has a biuret bond or is modified with trimethylolpropane. [Prior art documents] [Patent documents]

[0006] [Patent Document 1] JP 2003-155672 A [Patent Document 2] JP 2018-150649 A [Patent Document 3] JP 2010-229267 A Summary of the Invention [Problem to be solved by the invention]

[0007] A grain-finished artificial leather is known that has a structure in which a thin polyurethane skin layer having a thickness of about 10 to 50 μm is bonded to a wet polyurethane porous layer via a polyurethane adhesive layer. In such grain-finished artificial leather, since the thin polyurethane skin layer is bonded to the wet polyurethane porous layer, if the adhesive strength of the polyurethane adhesive layer is low, the polyurethane skin layer may easily peel off from the wet polyurethane porous layer due to aging. For this reason, a solvent-based adhesive containing an organic solvent that is likely to provide high adhesive strength has been widely used as the polyurethane adhesive layer. With a solvent-based adhesive, the organic solvent contained in the adhesive dissolves and roughens the surface layer of the wet polyurethane porous layer, so that high adhesiveness due to the anchor effect can be maintained.

[0008] However, when a solvent-based adhesive is used to form the polyurethane adhesive layer, the resulting grain-finished artificial leather has a problem of curling (inward curling). When the artificial leather is subjected to post-processing such as sewing in order to finish it into various products, the curl of the artificial leather must be straightened to make it flat, which reduces workability.

[0009] Another problem is that volatile organic compounds (VOCs) such as N,N-dimethylformamide (DMF) are used as solvents for polyurethane in the manufacturing process of artificial leather. In recent years, from the perspective of preventing air pollution, there have been increasingly strict demands for the reduction of VOC emissions through legal regulations and voluntary restrictions.

[0010] In the manufacturing process of artificial leather, organic solvents such as DMF are used as a solvent for the polyurethane solution to be impregnated into the fiber substrate. In addition, in the manufacturing of grain-finished artificial leather, polyurethane-based adhesives containing organic solvents are often used to bond a grain-finish resin layer to the fiber substrate. In the manufacturing process of artificial leather, it is required to recover as much organic solvent generated in the process as possible in order to comply with various regulations.

[0011] However, a small amount of organic solvent may remain in the obtained artificial leather. Therefore, in the artificial leather manufacturing process, as a clean process that uses as little organic solvent as possible, the production process of the fiber base material is being made aqueous, and the process of impregnating the fiber base material with polyurethane is being made aqueous using an emulsion mainly made of water. However, it has not yet been realized at present that organic solvents can be completely eliminated from all the artificial leather manufacturing processes. Therefore, in the process using organic solvents, there is a demand for the development of a process that recovers as much of the organic solvent as possible within the process so that no organic solvent remains in the artificial leather product.

[0012] The present invention aims to solve such problems, that is, to provide a grain-finished artificial leather having a structure in which a polyurethane surface layer is bonded to a wet-type polyurethane porous layer via a polyurethane adhesive layer, which can suppress curling immediately after production, and a secondary object of the present invention is to reduce the amount of organic solvent remaining in the grain-finished artificial leather. [Means for solving the problem]

[0013] The present inventors have conducted research aimed at preventing curling immediately after the production of the above-mentioned grain-finished artificial leather, and as a result have found that when a thin polyurethane skin layer is bonded using a solvent-based adhesive, the solvent in the solvent-based adhesive is difficult to volatilize, dissolving the surface layer of the wet-type polyurethane porous layer too much, causing the porous structure to disappear and the volume of that portion to decrease, causing the polyurethane porous layer to shrink and curling the grain-finished artificial leather. In addition, in order to sufficiently bond the polyurethane skin layer while preventing curling, the inventors have found that curling is prevented by buffing the surface of the polyurethane porous layer to a degree that leaves a skin layer with almost no large pores, thereby making curling less likely to occur, and have arrived at the present invention.

[0014] That is, one aspect of the present invention is a fiber entanglement body and a fiber entanglement body impregnated and laminated therein to be integrated. In addition, the cross section of the surface layer in the thickness direction has a skin layer having a thickness of 10 to 20 μm, which contains many small voids having a diameter of 5 μm or less, but does not contain voids having a diameter of 10 μm or more, and an inner layer containing many large voids whose maximum width is 10 μm or more. a step of buffing the surface of the wet polyurethane porous layer so as not to expose open pores having an average diameter of 15 μm or more; a step of preparing a polyurethane surface layer having a thickness of 10 to 50 μm formed on release paper; a step of applying an aqueous polyurethane adhesive containing an aqueous polyurethane to the surface of the polyurethane surface layer or the wet polyurethane porous layer after buffing, and then drying to form a polyurethane adhesive layer; and a pressing step of bonding the wet polyurethane porous layer after buffing and the polyurethane surface layer via the polyurethane adhesive layer.

[0015] According to the above-mentioned manufacturing method, the surface of the wet polyurethane porous layer is buffed and roughened so as to leave a skin layer with almost no large pores, so that a strong skin layer remains on the wet polyurethane porous layer. Furthermore, when the wet polyurethane porous layer and the polyurethane surface layer are bonded together, the skin layer on the surface of the wet polyurethane porous layer is not dissolved by bonding the wet polyurethane porous layer and the polyurethane surface layer with an aqueous polyurethane adhesive. As a result, the grain-finished artificial leather is less likely to curl immediately after production. Moreover, as a secondary effect, according to this manufacturing method, the amount of residual VOCs derived from the polyurethane adhesive layer can be reduced.

[0016] In addition, the aqueous polyurethane adhesive preferably contains a polyurethane associative thickener, since this makes it easier to form a polyurethane adhesive layer having a thickness sufficient to sufficiently adhere the polyurethane surface layer.

[0017] Another aspect of the present invention is a polyurethane sheet comprising a fiber-entangled body, a wet-type polyurethane porous layer impregnated and laminated on the fiber-entangled body to be integrated, and a polyurethane surface layer having a thickness of 10 to 50 μm laminated on the wet-type polyurethane porous layer via a polyurethane adhesive layer. The wet-type polyurethane porous layer has a skin layer having a thickness of 10 to 20 μm, which contains many small pores having a diameter of 5 μm or less but does not contain pores having a diameter of 10 μm or more in a cross section in the thickness direction of the surface layer, and an inner layer containing many large pores whose maximum width is 10 μm or more. On the surface of the skin layer, open pores having an average pore diameter of less than 15 μm are present, and the porous layer has a thickness of 10 to 20 μm. Urethane Adhesive The layer is based on a water-based polyurethane adhesive, The grain-finished artificial leather is one in which the interface between the wet-type polyurethane porous layer and the polyurethane adhesive layer is not dissolved. In the wet-type polyurethane porous layer in which the interface between the wet-type polyurethane porous layer and the polyurethane adhesive layer is not dissolved, a skin layer not including large pores can be present on the surface. Specifically, for example, in the cross section in the thickness direction of the surface layer of the wet-type polyurethane porous layer, a skin layer having a thickness of 10 to 20 μm is present, in which no pores having a width of 10 μm or more exist. According to such grain-finished artificial leather, curling is unlikely to occur after production. In addition, as a secondary effect, the emission of VOCs originating from the polyurethane adhesive layer can be reduced.

[0018] In addition, it is preferable that the polyurethane adhesive layer contains a polyurethane associative thickener, since this makes it easier to form a polyurethane adhesive layer having a thickness sufficient to sufficiently adhere the polyurethane surface layer. Effect of the Invention

[0019] According to the present invention, a grain-finished artificial leather having a structure in which a thin polyurethane skin layer is bonded to a wet-type polyurethane porous layer via a polyurethane adhesive layer can be obtained, which can suppress curling immediately after production, and can also reduce the amount of organic solvent remaining in the grain-finished artificial leather. [Brief description of the drawings]

[0020] [Figure 1] FIG. 1 is a schematic cross-sectional view of a grain-finished artificial leather according to an embodiment. [Diagram 2] FIG. 2 shows five SEM images of the surface layer of the cross section in the thickness direction of the grain-finished artificial leather obtained in Example 1, observed at 800x magnification using a scanning electron microscope (SEM), with a total width of about 0.8 mm. [Diagram 3] FIG. 3 shows five SEM images of the surface layer of a cross section in the thickness direction of the grain-finished artificial leather obtained in Comparative Example 1, observed at 800x magnification using a scanning electron microscope (SEM), with a total width of about 0.8 mm. [Figure 4] FIG. 4 is a microscope image at 200x magnification of the surface of the wet-processed polyurethane porous layer used in the production of the grain-finished artificial leather obtained in Example 1 after buffing. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0021] One embodiment of the grain-finished artificial leather according to the present invention will be described with reference to the drawings. Fig. 1 shows a schematic cross-sectional view of grain-finished artificial leather 10. In Fig. 1, 1 is a fiber-entangled body, 2 is a wet-type polyurethane porous layer impregnated and laminated with the fiber-entangled body 1 to be integrated, 3 is a polyurethane adhesive layer adhered to the wet-type polyurethane porous layer 2, and 4 is a polyurethane skin layer laminated to the polyurethane adhesive layer 3.

[0022] Such a grain-finished artificial leather 10 is manufactured, for example, by the following process. One surface of the fiber entanglement body is impregnated with a polyurethane solution that is wet-coagulated, and the polyurethane solution is applied thereon, which is then immersed in a coagulating liquid for coagulating the polyurethane, so that a wet polyurethane porous layer is wet-coagulated from the polyurethane solution. The surface of the wet polyurethane porous layer is then buffed to a predetermined degree, which will be described later, to roughen the surface so that a skin layer that does not contain large pores remains on the surface layer. Meanwhile, a film of a polyurethane surface layer is formed on a release paper. Then, an aqueous polyurethane adhesive is applied to the polyurethane surface layer formed on the release paper or the wet polyurethane porous layer after buffing, and the water is completely or incompletely dried to a semi-cured state to form a polyurethane adhesive layer. Then, the wet polyurethane porous layer after buffing and the polyurethane surface layer are bonded together via the polyurethane adhesive layer and heat-pressed. Then, the polyurethane adhesive layer is cured by heating for a predetermined time, and the release paper is peeled off to obtain a grain-finished artificial leather.

[0023] The form of the entangled fiber body is not particularly limited, but a nonwoven fabric, a woven fabric, a knitted fabric, or a combination thereof is used, and preferably a nonwoven fabric is used. The thickness of the entangled fiber body is not particularly limited, but for example, it is preferably about 300 to 3000 μm, and further preferably about 500 to 1500 μm. The type of fiber forming the entangled fiber body is not particularly limited, and examples thereof include aromatic polyester-based resins such as polyethylene terephthalate (PET), modified polyethylene terephthalate, polybutylene terephthalate (PBT), polytrimethylene terephthalate (PTT), polytriethylene terephthalate, polyhexamethylene terephthalate, polypropylene terephthalate, and polyethylene naphthalate, and aliphatic polyester-based resins such as polylactic acid, polyethylene succinate, polybutylene succinate, polybutylene succinate adipate, and polyhydroxybutyrate-polyhydroxyvalerate copolymer. Examples of the resins include polyester fibers, polyamide resins such as polyamide 6, polyamide 66, polyamide 610, polyamide 10, polyamide 11, polyamide 12, and polyamide 6-12, polyolefin resins such as polypropylene, polyethylene, polybutene, polymethylpentene, chlorine-based polyolefins, ethylene-vinyl acetate copolymers, and styrene-ethylene copolymers, modified polyvinyl alcohol resins formed from modified polyvinyl alcohols containing 25 to 70 mol % of ethylene units, and crystalline elastomers such as polyurethane elastomers, polyamide elastomers, and polyester elastomers. Among these, polyamide resins and aromatic polyester resins are preferred because of their excellent balance of various properties.

[0024] The fineness and form of the fiber are not particularly limited. For example, the fineness may be a regular fiber having a fineness of more than 1 dtex, or an ultrafine fiber having a fineness of less than 1 dtex. The form of the fiber may be a solid fiber, or a fiber having voids such as a hollow fiber or a lotus root-like fiber.

[0025] The wet polyurethane porous layer is formed by impregnating the surface of the fiber-entangled body with a polyurethane solution that undergoes wet coagulation, applying a polyurethane solution thereon for forming a resin layer with a grained finish, and then coagulating the polyurethane solution in an aqueous coagulating liquid.

[0026] The polyurethane contained in the polyurethane solution is a polyurethane or polyurethane urea obtained by polymerizing a polyurethane raw material containing a polymer polyol having two or more hydroxyl groups at the molecular terminals, a polyisocyanate compound having two or more isocyanate groups in the molecule, and a short-chain polyol or a polyamine compound as a chain extender.

[0027] Specific examples of the polymer polyol include polycarbonate-based diols such as polyhexamethylene carbonate diol, poly(3-methyl-1,5-pentylene carbonate) diol, polypentamethylene carbonate diol, polytetramethylene carbonate diol, polyoctamethylene carbonate diol, polynonamethylene carbonate diol, polydecamethylene polycarbonate diol, and polydodecamethylene polycarbonate diol, and copolymers thereof; polyethylene glycol, polypropylene glycol, and the like. Examples of the diol include polyether diols such as lycol, polytetramethylene glycol, and polymethyltetramethylene glycol, and copolymers thereof; polyester diols such as polybutylene adipate diol, polybutylene sebacate diol, polyhexamethylene adipate diol, poly(3-methyl-1,5-pentylene adipate) diol, poly(3-methyl-1,5-pentylene sebacate) diol, and polycaprolactone diol, and copolymers thereof; and polymer diols such as polyester carbonate diol. These may be used alone or in combination of two or more.

[0028] Examples of the polyisocyanate compound include aliphatic diisocyanates such as hexamethylene diisocyanate; alicyclic diisocyanates such as isophorone diisocyanate, norbornene diisocyanate, 4,4'-dicyclohexylmethane diisocyanate, 1,3-bis(isocyanatomethyl)cyclohexane, and 1,4-bis(isocyanatomethyl)cyclohexane; aromatic diisocyanates such as 2,4-tolylene diisocyanate, 2,6-tolylene diisocyanate, 4,4'-diphenylmethane diisocyanate, and xylylene diisocyanate; polyfunctional isocyanates that give branched structures such as isocyanurate-type, biuret-type, and adduct-type trifunctional and tetrafunctional isocyanates, and their isocyanate block products. These may be used alone or in combination of two or more.

[0029] Examples of the chain extender include hydrazine, ethylenediamine, propylenediamine, hexamethylenediamine, nonamethylenediamine, xylylenediamine, isophoronediamine, piperazine and derivatives thereof; diamines such as adipic acid dihydrazide and isophthalic acid dihydrazide; triamines such as diethylenetriamine; tetramines such as triethylenetetramine; diols such as ethylene glycol, propylene glycol, 1,4-butanediol, 1,6-hexanediol, 1,4-bis(β-hydroxyethoxy)benzene and 1,4-cyclohexanediol; aminoalcohols such as aminoethyl alcohol and aminopropyl alcohol, etc. These may be used alone or in combination of two or more.

[0030] Polyurethane is produced by a method of solution polymerization in the presence of a solvent using the polyurethane raw material described above. Examples of the solvent used in the solution polymerization include dimethylformamide (DMF), which is a hydrophilic solvent, dimethylformamide (MEK), which is a hydrophobic solvent, and a mixture of these solvents.

[0031] As the aqueous coagulation liquid, water or a mixture of water and an organic solvent such as DMF or dimethyl sulfoxide (DMSO) is used. By immersing the polyurethane solution in the coagulation liquid, the polyurethane coagulates due to the difference in solubility between the polyurethane in the solvent and the coagulation liquid. By adjusting the coagulation speed of the polyurethane, the pore size of the wet polyurethane porous layer can be adjusted.

[0032] During coagulation, the organic solvent such as DMF in the polyurethane solution is mixed into the water, and the concentration of the organic solvent in the water gradually increases, causing the coagulation rate to decrease. In order to suppress such a decrease in the coagulation rate and control the particle size, the pore size is adjusted by using a coagulation liquid containing a mixture of water and DMF, particularly a coagulation liquid with a water / DMF (mass ratio) of 90 / 10 to 70 / 30. The temperature of the coagulation bath is not particularly limited, but is preferably in the range of 20 to 50°C, since it is easy to form pores with an appropriate diameter.

[0033] In the formation of a wet-type porous polyurethane layer, when the polyurethane solution is solidified by a water-based coagulating liquid, the surface where the polyurethane solution first comes into contact with the coagulating liquid is instantaneously solidified by the polyurethane, forming a skin layer that contains a large number of very small pores, specifically, pores with a diameter of 5 μm or less, but does not contain large pores with a diameter of 10 μm or more. Then, the coagulating liquid gradually penetrates from the skin layer into the inside, and the coagulation of the layer inside the skin layer progresses. The surface of the skin layer thus formed is a glossy, substantially non-porous surface. Also, the diameter of the pores gradually increases toward the inner layer from the skin layer. Such an inner layer contains a large number of large pores with a teardrop-shaped cross section whose maximum width is 10 μm or more.

[0034] The solidification rate of polyurethane can also be affected by its chemical structure. Specifically, when the ratio of polyether polyol such as polytetramethylene glycol is high, the polyurethane becomes more hydrophilic and the solidification rate tends to decrease.

[0035] Furthermore, the polyurethane solution may contain, as necessary, colorants such as titanium oxide and carbon black, various stabilizers such as ultraviolet absorbers and antioxidants, fillers such as calcium carbonate, and known coagulation regulators.

[0036] The thickness of the wet polyurethane porous layer thus formed is, for example, preferably about 100 to 600 μm, and more preferably about 200 to 400 μm.

[0037] The wet polyurethane porous layer is buffed so as not to expose open pores having an average diameter of 15 μm or more, thereby roughening the surface so as to leave a skin layer that does not expose large open pores on the surface layer. Buffing is performed, for example, using fine sandpaper of no more than #200 to remove a thickness of preferably about 0.01 to 120 μm, more preferably about 0.05 to 30 μm, and particularly preferably about 0.5 to 15 μm, so as to leave the skin layer without opening large pores contained in the inner layer of the wet polyurethane porous layer.

[0038] The surface of the wet polyurethane porous layer formed by buffing is adjusted so as not to expose open pores having an average diameter of 15 μm or more, preferably 10 μm or more, when the surface of the wet polyurethane porous layer after buffing is observed under a microscope at 200 times. The diameter of the pores present on the surface of the wet polyurethane porous layer after buffing is in the range of 2 to 15 μm, preferably about 5 to 10 μm, and the average of these is preferably less than 15 μm. The density of the fine openings is preferably less than 1 mm 2 It is preferable that the number of particles per unit area is 125 or more, and more preferably about 150 to 250.

[0039] On the other hand, in the manufacturing method of the present embodiment, a polyurethane surface layer film to be adhered to the surface of the wet polyurethane porous layer is formed on a release paper. The polyurethane surface layer film is formed, for example, by dry surface forming as follows.

[0040] A polyurethane solution or molten resin for forming a polyurethane skin layer is applied onto a release paper and then solidified to form a film of the polyurethane skin layer.

[0041] The type of polyurethane used to form the polyurethane surface layer is the same as the polyurethane described above, but it is particularly preferable to use a polycarbonate-based polyurethane to form the surface layer because it has excellent scratch resistance. The polyurethane surface layer may be non-porous or porous. The polyurethane surface layer may be a single layer or may have a multi-layer structure consisting of an intermediate layer and a top layer. The polyurethane surface layer may contain a colorant or other additives as necessary. The release paper is not particularly limited, but it is preferable to use one that has irregularities to impart a grain pattern to the surface.

[0042] The thickness of the polyurethane skin layer is 10 to 50 μm, preferably 15 to 50 μm, and more preferably 20 to 40 μm. If the polyurethane skin layer is less than 10 μm, the abrasion resistance of the surface is reduced. If the polyurethane skin layer is more than 50 μm, the rigidity of the polyurethane skin layer becomes too high, which makes the polyurethane skin layer more likely to curl and peel over time.

[0043] Then, after applying an aqueous polyurethane adhesive to the surface of the polyurethane skin layer on the release paper, the water is completely or partially removed and the layer is dried. In this manner, a polyurethane adhesive layer is formed on the surface of the polyurethane skin layer on the release paper. The polyurethane adhesive layer may be formed on the surface side of the buffed wet polyurethane porous layer instead of on the film of the polyurethane skin layer on the release paper.

[0044] The aqueous polyurethane adhesive is an emulsion or dispersion in which aqueous polyurethane particles are dispersed in an aqueous medium, and may contain a crosslinking agent, a colorant such as a pigment, a thickener, an antifoaming agent, etc., as necessary.

[0045] The aqueous medium contained in the aqueous polyurethane adhesive includes a mixed solvent containing 90 to 100% by mass of water and, if necessary, a small amount of glycols or alcohols.

[0046] In addition, the type of water-based polyurethane contained in the water-based polyurethane adhesive is not particularly limited, and examples include polycarbonate-based polyurethanes such as aromatic polycarbonate-based polyurethanes, polycarbonate-polytetramethylene glycol copolymer-based polyurethanes, polyester glycol-based polyurethanes, polypropylene glycol-based polyurethanes, polytetramethylene glycol-based polyurethanes, etc. Among these, aromatic polycarbonate-based polyurethanes are particularly preferred because of their excellent abrasion resistance.

[0047] In addition, water-based polyurethane is preferable because it has crosslinking properties and can form a polyurethane adhesive layer with excellent peel resistance and solvent resistance. Examples of polyurethanes having such crosslinking properties include polyurethanes having reactive groups such as hydroxyl groups, carboxyl groups, and isocyanate groups at the ends or side chains. When using water-based polyurethanes having such crosslinking properties, a crosslinking agent is blended into the water-based polyurethane adhesive.

[0048] Examples of crosslinking agents that can be incorporated into the aqueous polyurethane adhesive include isocyanate-based crosslinking agents, carbodiimide-based crosslinking agents, aziridine-based crosslinking agents, etc. Among these, isocyanate-based crosslinking agents are particularly preferred from the viewpoint of improving adhesive strength and water resistance.

[0049] In addition, the aqueous polyurethane adhesive preferably contains a thickener to facilitate adjustment of the thickness of the coating film of the aqueous polyurethane adhesive to be applied. As such a thickener, a polyurethane association type thickener is particularly preferable because a high viscosity can be obtained with a small amount and the viscosity stability is excellent. Specific examples of polyurethane association type thickeners include polymers generated by reacting alcohol alkoxylate and / or polyether polyol with isocyanate or polyisocyanate. The amount of polyurethane association type thickener added is preferably 0.1 to 1 mass% based on polyurethane.

[0050] The solution viscosity of the aqueous polyurethane adhesive, measured at 20° C. using a Brookfield viscometer, is preferably 3 to 10 Pa·s.

[0051] The thickness of the polyurethane adhesive layer thus formed is preferably 5 to 200 μm, more preferably 30 to 70 μm. If the polyurethane adhesive layer is too thick, the bending resistance tends to decrease, resulting in a decrease in adhesive strength.

[0052] Then, the polyurethane adhesive layer laminated on the film of the polyurethane surface layer formed on the release paper is attached to the surface of the wet polyurethane porous layer after buffing, and pressed, and the polyurethane adhesive layer is cured to bond the wet polyurethane porous layer and the polyurethane surface layer via the polyurethane adhesive layer. The pressing temperature is not particularly limited, but the surface temperature is set to 70 to 100° C. In addition, in order to completely cure the polyurethane adhesive layer, it is preferable to provide an aging period in which the polyurethane adhesive layer is left in an environment of 30 to 70 RH% at a temperature of 45 to 65° C. for several hours to several days.

[0053] The total thickness of the bonded polyurethane surface layer and polyurethane adhesive layer is preferably about 10 to 300 μm, more preferably 30 to 200 μm, and even more preferably about 50 to 100 μm, in order to maintain a balance between mechanical properties and texture.

[0054] The release paper is then peeled off from the surface of the polyurethane skin layer to obtain grain-finished artificial leather having a polyurethane skin layer.

[0055] In the thus obtained grain-finished artificial leather, the wet-type polyurethane porous layer and the polyurethane skin layer are bonded with an aqueous polyurethane adhesive, so that the interface between the wet-type polyurethane porous layer and the polyurethane adhesive layer is not dissolved by a solvent, and therefore, a wet-type polyurethane porous layer having a skin layer with a thickness of 10 to 20 μm can be formed, in which no pores having a width of 10 μm or more cross the cross section of the surface layer in the thickness direction.

[0056] Here, a wet-type polyurethane porous layer having a skin layer with a thickness of 10 to 20 μm in which no pores having a width of 10 μm or more cross the cross section of the surface layer in the thickness direction is described with reference to FIG. 2.

[0057] FIG. 2 shows five images of five randomly selected locations near the surface layer of a cross section in the thickness direction of the grain-finished artificial leather obtained in Example 1 described later, which were observed at 800x magnification using a scanning electron microscope (SEM).

[0058] In Fig. 2, a curve L1 is shown which indicates the interface between the wet-type polyurethane porous layer and the polyurethane adhesive layer in a cross section in the thickness direction of the grain-finished artificial leather, and a curve L2 which is 20 μm away from the curve L1 is also shown.

[0059] As shown in FIG. 2, in the grain-finished artificial leather of this embodiment, numerous small pores having a diameter of 5 μm or less are observed in the region of interface L2, which is 20 μm away from interface L1 of the wet-type polyurethane porous layer with the polyurethane adhesive layer, but no large pores having a diameter of 10 μm or more are present.

[0060] On the other hand, Fig. 3 shows five images of five randomly selected points near the surface layer of the cross section in the thickness direction of the grain-finished artificial leather obtained in Comparative Example 1 described later, observed at 800 times with a scanning electron microscope (SEM). Similarly, in Fig. 3, a curve L1 is drawn at the interface between the wet polyurethane porous layer and the polyurethane adhesive layer. As shown in Fig. 3, in the cross section in the thickness direction of the grain-finished artificial leather obtained in Comparative Example 1 using a solvent-based adhesive to form the polyurethane adhesive layer, a large number of large pores V having a diameter of 10 μm or more are present across the interface L1 with the polyurethane adhesive layer of the wet polyurethane porous layer. In addition, since the surface layer of the polyurethane adhesive layer of such a wet polyurethane porous layer is dissolved with a solvent, an interface with large undulations is formed. In the part dissolved with a solvent, the polyurethane adhesive layer is bonded while the polyurethane is dissolved and reduced in volume, so that internal stress is likely to concentrate. Therefore, in the pressing step for bonding the polyurethane surface layer to the wet polyurethane porous layer after buffing via the polyurethane adhesive layer, or in the subsequent treatment for maturing the adhesion, the internal stress is gradually released, and the obtained grain-finished artificial leather is likely to curl. Note that the surface of the polyurethane surface layer bonded to such a wet polyurethane porous layer having large waviness is likely to form a wavy surface with low smoothness that reflects the waviness.

[0061] In such a grain-finished artificial leather, the interface between the polyurethane adhesive layer and the wet-type polyurethane porous layer is not dissolved. Preferably, in an image of the vicinity of the surface layer of a cross section in the thickness direction of the grain-finished artificial leather observed at 800 times with a scanning electron microscope (SEM), when a virtual line is drawn 20 μm away from the interface between the wet-type polyurethane porous layer and the polyurethane adhesive layer, a skin layer not including large pores is present without being dissolved. Preferably, in a cross section in the thickness direction of the surface layer of the wet-type polyurethane porous layer, a skin layer having a thickness of 10 to 20 μm is present, which is not crossed by large pores having a width of 10 μm or more.

[0062] Here, a skin layer having a thickness of 10 to 20 μm, which is not crossed by pores having a width of 10 μm or more in a cross section in the thickness direction of the surface layer of the wet polyurethane porous layer, is described. With reference to Fig. 2, such a skin layer means a layer in which, when a virtual line L2 is drawn parallel to the interface L1 between the wet polyurethane porous layer and the polyurethane adhesive layer, the virtual line L2, which is not crossed by pores having a width of 10 μm or more, is 10 to 20 μm away from the interface L1. The judgment is made based on five images obtained by photographing the cross sections at five evenly selected locations.

[0063] When the imaginary line L2 crossed by the pores V having a width of 10 μm or more is within a range of less than 10 μm from the interface L1, the skin layer on the surface of the wet polyurethane porous layer is dissolved, and there is no skin layer having a thickness of 10 to 20 μm that is not crossed by the pores having a width of 10 μm or more. In such a case, internal stress remains in the polyurethane adhesive layer adhered to the surface of the wet polyurethane porous layer, and the residual internal stress is released by the heat applied during the manufacturing process, making the obtained grain-finished artificial leather prone to curling.

[0064] When the grain-finished artificial leather of the present embodiment described above is used as a skin material to manufacture bags, clothes, shoes, etc., it can be directly subjected to processing such as sewing without correcting curls of the grain-finished artificial leather. In addition, as a secondary effect, the amount of residual organic solvents in the grain-finished artificial leather contained in such products can be reduced. EXAMPLES

[0065] The present invention will be described in more detail below with reference to examples, although the scope of the present invention is not limited to these examples in any way.

[0066] (Measurement of the average diameter of open pores on the surface of a wet polyurethane porous layer after buffing) The surface of the wet polyurethane porous layer after buffing was observed under a microscope at 200 times magnification, and the image was saved. The saved image was then printed, and the average diameter of the open pores present in a randomly selected 200 μm square was determined from the printed image. When the open pores were elliptical, the average values ​​of the major and minor diameters were measured. FIG. 4 shows an example of an image of the surface of the wet polyurethane porous layer after buffing used in Example 1.

[0067] (Observation of a cross section in the thickness direction of the surface layer of a wet polyurethane porous layer) The cross section of the grain-finished artificial leather in the thickness direction was observed at 800 times magnification with a scanning electron microscope, and the images were saved. The photographs were taken at five randomly selected locations. Then, for the five images obtained, a virtual line was drawn on the wet polyurethane porous layer at a location 10 μm away from the interface with the polyurethane adhesive layer. Specifically, a curve L1 showing the interface was drawn along the interface between the polyurethane adhesive layer and the wet polyurethane porous layer. Then, a curve L2 was drawn parallel to this curve at a distance of 10 to 20 μm. Then, the presence or absence of voids crossing the virtual line L2 by a width of 10 μm or more was confirmed. The measurement was performed using five images. If there are no voids crossing the curve L2 by a width of 10 μm or more at a distance of 10 μm, it can be said that a skin layer having a thickness of 10 μm is formed.

[0068] (Evaluation of curl occurrence) A test piece measuring 20 cm in length and 10 cm in width was cut out from the grain-finish artificial leather. The test piece was then left in an environment of 20°C and 45% RH for 24 hours. After leaving it for 24 hours, the distance between both ends in the width direction was measured in three places and the average value was calculated. If curling had occurred, the ends would come closer together due to the curling. The ratio of the distance between both ends after leaving it for 24 hours to a width of 10 cm was then calculated. The greater the curling, the smaller the ratio of the distance between both ends.

[0069] [Example 1] An islands-in-sea composite fiber consisting of 45 parts by mass of 6-nylon (sea component) and 55 parts by mass of polystyrene (island component) was obtained by melt spinning. This was stretched three times, a fiber oil was added, mechanically crimped, and then dried. The crimped fiber obtained was cut to 51 mm and made into 3 dtex staples, which were then formed into a web, and then alternately combined from both sides to obtain approximately 500 punches / cm. 2 The nonwoven fabric had a basis weight of 350 g / m 2 The apparent specific gravity was 0.17. The nonwoven fabric was treated with a 4% aqueous solution of polyvinyl alcohol, compressed and fixed to a thickness of about 1.3 mm, and the surface was buffed to make it smooth.

[0070] Meanwhile, a polyurethane solution was prepared as follows. 1000 parts by mass of polybutylene adipate with a number average molecular weight of 2000, 249 parts by mass of polyhexylene carbonate with a number average molecular weight of 2000, and 70.4 parts by mass of ethylene glycol were added and dissolved in 5650 parts by mass of N,N-dimethylformamide, and 415 parts by mass of diphenylmethane-4,4'-diisocyanate were gradually added while stirring so that NCO / OH=0.94, and the reaction was carried out at 80°C for 3 hours to obtain an intermediate with essentially OH terminals. Next, 125 parts by mass of polyethylene glycol with a number average molecular weight of 20,000 were added, and diphenylmethane-4,4'-diisocyanate was gradually added and the reaction was carried out. When NCO / OH=1.05 and the solution viscosity (30°C) became 40 Pa·s, the solution was cooled to obtain a polycarbonate / polyester polyurethane solution.

[0071] The obtained polyurethane solution was then prepared into a 13% dimethylformamide solution, and the nonwoven fabric was impregnated with the solution. The surface of the nonwoven fabric was then impregnated with a 25% dimethylformamide solution of the same polyurethane at a solid content of 80 g / m. 2After applying the amount of the wet polyurethane to the fiber using a bar coater, the fiber was immersed in a mixture of water / DMF=75 / 25 by mass at 30°C to wet-solidify the polyurethane into a porous form. The island components were then dissolved and removed in hot toluene to convert the composite fiber into a hollow fiber, thereby obtaining a fiber-entangled body with a laminated wet polyurethane porous layer. Microscopic observation showed that the wet polyurethane porous layer had a thickness of 300 μm.

[0072] The surface of the wet-type polyurethane porous layer was then buffed with sandpaper no. 180 so as to leave the skin layer. Figure 4 shows a photograph of the surface of the wet-type polyurethane porous layer observed under a microscope at 200x magnification. The average diameter of the open pores was 8.3 μm.

[0073] Next, a solution containing 100 parts by mass of non-yellowing polycarbonate-based polyurethane solution (resin content 25%), 20 parts by mass of Seika Seven BS780 Black (Dainichi Seika Chemicals Co., Ltd.), 30 parts by mass of DMF, and 30 parts by mass of methyl ethyl ketone was applied onto a release paper (DE-125 manufactured by Dai Nippon Printing Co., Ltd.) so as to have a thickness of 15 μm after drying, and was dried to form a top layer constituting a polyurethane skin layer. Then, a DMF solution containing 100 parts by mass of one-liquid type polyether-based polyurethane (Rezamin ME8116 manufactured by Dainichi Seika Chemicals Co., Ltd.) and 20 parts by mass of Rezamin DUT4790 Black was applied onto the top layer so as to have a thickness of 20 μm after drying, and was dried to form a polyurethane intermediate layer constituting a polyurethane skin layer. In this way, a polyurethane skin layer was formed. The thickness of the obtained polyurethane skin layer was 35 μm.

[0074] Then, an aqueous polyurethane adhesive, which is an aqueous polyurethane resin dispersion blend, is applied to the surface of the polyurethane skin layer at a rate of 150 g / m 2The aqueous polyurethane adhesive was a 45% by mass aqueous adhesive containing 100 parts by mass of a crosslinkable aromatic polycarbonate polyurethane (HYDRAN WLA-515AR manufactured by DIC Corporation), 8 parts by mass of an isocyanate crosslinking agent (Bayhydur XP2655 manufactured by Covestro), and 1 part by mass of a polyurethane association type thickener (Borch Gel 0626 manufactured by Borchers) as active ingredients.

[0075] The polyurethane surface layer coated with the aqueous polyurethane adhesive was dried at 110°C for 2 minutes, and then dried at 130°C for 2 minutes to evaporate most of the water, forming a tacky semi-dried polyurethane adhesive layer. The polyurethane surface layer was then bonded to the surface of the wet polyurethane porous layer by the semi-dried polyurethane adhesive layer, passed through a roll press with a surface temperature of 80°C, and contacted with a drum cylinder heated to 110°C for 10 seconds to form a laminated intermediate. The laminated intermediate was then aged at 45°C for 3 days to mature the adhesion between the polyurethane surface layer and the wet polyurethane porous layer. The release paper was then peeled off to obtain a grained artificial leather. Figure 2 shows five images of the surface layer of the cross section of the grained artificial leather obtained in Example 1 in the thickness direction, observed at 800 times using a scanning electron microscope (SEM). Evaluation was then performed according to the above-mentioned evaluation method.

[0076] In the obtained grain-finished artificial leather, the interface between the wet polyurethane porous layer and the polyurethane adhesive layer was not dissolved, and a skin layer having a thickness of 10 to 20 μm was formed in the cross section of the surface layer of the wet polyurethane porous layer in the thickness direction, in which no pores having a width of 10 μm or more were crossing.Furthermore, the flatness was evaluated to be 97%.

[0077] [Comparative Example 1] The same fiber-entangled body having a wet-type polyurethane porous layer laminated thereon and a polyurethane surface layer formed on a release paper as those produced in Example 1 were prepared.

[0078] Then, a solvent-based polyurethane adhesive was applied to the surface of the polyurethane skin layer at 130 g / m2 After coating and drying at 120°C for 15 seconds to evaporate the solvent, a laminate intermediate was obtained by bonding to a wet polyurethane porous layer. The solvent-based polyurethane adhesive was a 50% by mass solvent-based adhesive containing a composition obtained by adding a crosslinking agent and a crosslinking accelerator to 100 parts by mass of crosslinked polyurethane (TA205FT, Dainichiseika Color & Chemicals Mfg. Co., Ltd.) as an adhesive component, and containing 40 parts by mass of DMF as a solvent.

[0079] The obtained laminated intermediate was passed through a roll press having a surface temperature of 80°C to press and bond the laminated intermediate, while the polyurethane adhesive was allowed to penetrate into the wet polyurethane porous layer. The laminate was then dried at 130°C for 3 minutes, and then aged at 50°C for 3 days. The release paper was then peeled off to obtain a grain-finished artificial leather. Figure 3 shows five images of the vicinity of the surface layer of the cross section in the thickness direction of the grain-finished artificial leather obtained in Comparative Example 1, observed at 800 times with a scanning electron microscope (SEM). The grain-finished artificial leather was evaluated according to the evaluation method described above.

[0080] In the obtained grain-finished artificial leather, the interface between the wet-type polyurethane porous layer and the polyurethane adhesive layer was dissolved to have a large undulation. In addition, in three of the five images, in the cross section of the surface layer of the wet-type polyurethane porous layer in the thickness direction, many pores having a width of 10 μm or more crossed the imaginary line L2 drawn 10 μm away from the interface, and a skin layer exceeding 10 μm was not formed continuously. In addition, the flatness was evaluated as 70%.

[0081] [Comparative Example 2] In Example 1, instead of using #180 sandpaper to buff the leather so as to leave the skin layer and form open pores having an average diameter of 8.3 μm, #120 sandpaper was used and the buffing time was extended to form open pores having an average diameter of 25 μm. In the same manner as in Example 1, except that, a grain-finished artificial leather was obtained and evaluated.

[0082] The obtained grain-finished artificial leather had many pores with a width of 10 μm or more across the imaginary line L2 drawn 10 μm away from the interface, and no continuous skin layer with a thickness of more than 10 μm was formed. In addition, because a large amount of the skin layer was removed, the adhesive penetrated excessively into the wet polyurethane porous layer, and less adhesive remained on the surface of the wet polyurethane porous layer, resulting in a decrease in peel strength. The flatness was evaluated as 95%. [Explanation of symbols]

[0083] 1 Fiber entanglement 2. Wet polyurethane porous layer 3 Polyurethane adhesive layer 4 Polyurethane skin layer 10 Silver-tone artificial leather V pores L1 interface L2 Virtual Line

Claims

1. preparing a substrate including a fiber-entangled body and a wet-type polyurethane porous layer, the wet-type polyurethane porous layer having a skin layer having a thickness of 10 to 20 μm and including a large number of small pores having a diameter of 5 μm or less but no pores having a diameter of 10 μm or more in a cross section in the thickness direction of a surface layer, the skin layer being impregnated with and laminated on the fiber-entangled body to be integrated, and an inner layer including a large number of large pores having a maximum width of 10 μm or more; buffing the surface of the wet-type polyurethane porous layer so as not to expose open pores having an average diameter of 15 μm or more; providing a polyurethane skin layer having a thickness of 10 to 50 μm formed on a release liner; a step of applying an aqueous polyurethane adhesive to the surface of the polyurethane surface layer or the wet polyurethane porous layer after buffing, and then drying the applied adhesive to form a polyurethane adhesive layer; and a pressing step for bonding the wet polyurethane porous layer and the polyurethane skin layer together via the polyurethane adhesive layer after buffing.

2. 2. The method for producing a grain-finished artificial leather according to claim 1, wherein the aqueous polyurethane adhesive contains a polyurethane associative thickener.

3. a fiber-entangled body; a wet-type polyurethane porous layer impregnated with and laminated on the fiber-entangled body to be integrated; and a polyurethane surface layer having a thickness of 10 to 50 μm laminated on the wet-type polyurethane porous layer via a polyurethane adhesive layer, The wet polyurethane porous layer has a surface layer having a thickness of 10 to 20 μm, the surface layer including a large number of small pores having a diameter of 5 μm or less but no pores having a diameter of 10 μm or more in a cross section in the thickness direction, and an inner layer including a large number of large pores having a maximum width of 10 μm or more; The grain-finished artificial leather is characterized in that open pores having an average pore size of less than 15 μm are present on the surface of the skin layer, and the polyurethane adhesive layer is derived from an aqueous polyurethane adhesive, so that the interface between the wet polyurethane porous layer and the polyurethane adhesive layer is not dissolved.

4. A silver-finished artificial leather as described in claim 3, wherein the polyurethane adhesive layer contains a polyurethane associative thickener.

Citation Information

Patent Citations

  • Production of leathery sheet-like product

    JP1990242979A

  • Synthetic leather

    JP1993044173A

  • Grain artificial leather and method for producing the same

    JP2003155672A

  • Aqueous dispersion of polyurethane resin and water-base adhesive

    JP2004051778A

  • Leathery, sheet-like product and method for producing the same

    JP2008057062A