Dissolution-resistant tissue-adhesive chitosan materials.
Catechol-modified chitosan materials offer durable tissue adhesion and hemostasis in harsh biological environments, addressing limitations of current chitosan materials by providing effective bleeding control and promoting tissue healing.
Patent Information
- Application Number
- JP2020535507
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2018-02-15
- Filing Date
- 2018-12-28
- Publication Date
- 2024-10-10
- Estimated Expiration
- 2038-12-28
AI Technical Summary
Current chitosan materials used for medical applications are not effective in maintaining their structure and adhering to tissues in harsh biological environments such as the gastrointestinal tract and vasculature, limiting their use in procedures requiring prolonged tissue adhesion and hemostasis.
Development of catechol-modified chitosan materials that resist dissolution and maintain adhesion to tissues for up to 12 hours in the presence of biological fluids, allowing for effective hemostasis and tissue healing.
The catechol-modified chitosan materials provide reliable and durable tissue adhesion, enabling rapid bleeding control and promoting local clot formation, suitable for minimally invasive procedures and reducing hospital stays and complications.
Smart Images

Figure 0007565214000016 
Figure 0007565214000017 
Figure 0007565214000018
Abstract
Description
[Technical field]
[0001] Government Licensing Rights This invention was made with Government support under R42DK078400 and R44DK104564 awarded by the National Institute of Diabetes and Digestive and Kidney Diseases. The Government has certain rights in this invention.
[0002] background Technical Field Safe, reliable, and effective delivery of bioactive chitosan materials in the body remains a major challenge. In use, bioactive chitosan materials must remain unchanged for at least 12 hours in the presence of biological fluids such as gastric juice, blood, bile, and urine, and must be able to adhere to tissues such as the mucosa of the gastrointestinal tract and the internal elastic lamina of the vasculature for more than 24 hours. Bioactive chitosan has many applications in the body, including but not limited to drug delivery, hemostasis, wound healing, tissue regeneration, and embolization therapy. Current chitosan materials and compositions of chitosan materials used on or within the body are limited in their applications because they cannot withstand dissolution and rapid loss in harsh environments such as the stomach, and cannot be maintained in place by adhering to tissues.
[0003] FIELD OF THE DISCLOSURE The present disclosure relates to the field of chitosan materials, including catechol-modified chitosan, and uses thereof. [Background technology]
[0004] 2. Description of Related Art There are many surgeries on vascularized organs and tissues, such as the heart, liver, pancreas, stomach, intestines, colon, prostate, tonsils, ear, nose, throat, and brain, which often continue to bleed after injury and through wound healing. The initial injury may continue to bleed for days unless standard hemostasis is applied, and bleeding may recur at a later time. Standard of care initial hemostasis for the treatment of postoperative bleeding varies with the type of surgery. Ligatures, gauze packing, biological dressings, cautery, and banding may be applied to address the problem locally. In cases of prolonged bleeding, packing for up to 24 hours may be applied. If bleeding cannot be controlled after a period of conservative management, the patient must be immediately returned to the operating room for bleeding to be stopped by open or endoscopic techniques. Although there have been advances in bleeding control using advanced dressings, none of these advances have yet translated into reliable treatment options under specialized surgical conditions where continuous bleeding mixed with delivery, tissue adhesion, and other biological fluid considerations is highly challenging. Rapid control of bleeding in all situations is highly desirable.
[0005] Minimally invasive surgical procedures are becoming the preferred means of interventional access due to lower mortality rates, lower hospital costs, less patient discomfort, and the ability to access areas of the body with significantly reduced risk (compared to open surgery). Advanced biomaterials are at the forefront of addressing current limitations and enabling improvements in safety, reliability, and increased implementation and application of minimally invasive surgical procedures. Current limitations in the implementation of minimally invasive surgery include controlling bleeding (especially major bleeding), sutureless closure of sensitive soft tissue sites, local promotion of healing, local treatment of pathology, and local placement by anchoring or adhering to the surgical / intervention site. More recently, minimally invasive interventions have been used to address vascular etiologies such as vascular malformations, aneurysms, and vascular tumors. The preferred procedure for addressing vascular malformations, aneurysms, and vascular tumors is the use of embolic therapy to occlude abnormal blood vessels. Embolization therapy involves the local delivery of occlusive devices such as stents or coils of material or affixed biomaterials that promote the formation of massive thrombi that remain in place for an extended period of time and subsequently permanently block the blood vessel.
[0006] A biocompatible, tissue-adherent chitosan material that remains intact over time and promotes local thrombosis and normal tissue healing would provide an advanced material and allow for significant advances in surgical practice.
[0007] Furthermore, prolonged bleeding remains a significant problem in the gastrointestinal (GI) tract with attendant risks in mortality and morbidity. There is a need for techniques and devices that can provide rapid bleeding control of gastrointestinal bleeding (GIB) for upper gastrointestinal bleeding (UGIB) and lower gastrointestinal bleeding (LGIB). Current bleeding control during and after transurethral resection of the prostate (TURP) relies on cauterization for small vessel arterial bleeding and application of balloon pressure to address venous oozing. Both the bladder neck and prostate are highly vascularized tissues, and bleeding often continues after injury and during wound healing. Unless standard hemostasis is applied, the initial injury site may continue to bleed for several days, and bleeding may recur approximately one or two weeks after the TURP procedure, when the prostatic cavity scab sloughs. The current standard initial hemostasis for the treatment of bleeding after TURP is manual traction with a balloon catheter followed by continuous bladder irrigation with saline. Typically, balloon pressure can be applied for up to 24 hours in cases of prolonged bleeding. If bleeding cannot be controlled after a period of conservative management, the patient must be immediately returned to the operating room for open or endoscopic procedures to stop the bleeding.
[0008] Although there have been advances in bleeding control using advanced dressings for applications other than GIB or TURP bleeding control, none of these advances have yet translated to the special conditions of the gastrointestinal tract or bladder, particularly the upper gastrointestinal tract and prostate, where considerations related to delivery, adhesion, enzyme activity, continuous exudative bleeding, acidity, and urine are highly challenging. Rapid bleeding control in TURP, open prostatectomy, and cystectomy is highly desirable.
[0009] Gastrointestinal bleeding (GIB) is a common medical condition for emergency departments. According to the United States Department of Health and Human Services, from 2000 to 2014, there were an average of more than 350,000 hospital discharges from GI bleeding each year. In the United States, direct hospital costs from GIB exceeded $1.1 billion in 2010 [1]. Upper GIB (UGIB), defined as GI bleeding proximal to the Treitz ligature, is approximately five times more common than lower GIB (LGIB) [2]. Acute UGIB is a potentially fatal emergency that requires urgent evaluation, resuscitation, and appropriate medical and endoscopic management. Despite recent advances in the management of GIB in Western countries, mortality from acute UGIB has not improved markedly and remains high at 10–14% [3, 4]. The main cause of death after GIB is death secondary to cardiopulmonary complications, which is not surprising given the burden of comorbidities in such patients. Mortality from uncontrolled bleeding has been reported to account for 20%-25% of cases [5, 6]. Although little can be done to rapidly correct comorbid conditions, more effective and rapid bleeding control could significantly reduce the incidence of UGIB-related morbidity and mortality. In general, the most common causes of acute UGIB are gastrointestinal ulcers, gastroesophageal varices, Mallory-Weiss tears, and erosive esophagogastrointestinal bleeding [7]. Nonvariceal upper gastrointestinal bleeding (NVUGIB) encompasses all causes of UGIB except bleeding from esophageal or gastric varices. The incidence of gastrointestinal ulcer disease has decreased with the development and utilization of proton pump inhibitors, as well as the identification, treatment, and eradication of Helicobacter pylori in individual patients [8]. Despite the decrease in the incidence of gastrointestinal ulcers, the mortality rate in patients with NVUGIB ranges from 3-4% [9]. Although rarely fatal, gastric malignancies can result in fragile tissue with extensive bleeding that is difficult to manage by traditional physical hemostatic techniques (clips, bands, ligations) or cauterization
[10] .
[0010] Current endoscopic management of patients with acute UGIB includes thermal therapy (e.g., bipolar electrocoagulation, heater probe, monopolar electrocoagulation, argon plasma coagulation, and laser), injections (epinephrine, sclerosing agents (e.g., absolute ethanol, polidocanol, and ethanolamine), thrombin or fibrin glue (thrombin and fibrinogen), and clips [ 11 , 12 ].
[0011] In general, in the majority of patients with bleeding gastrointestinal ulcers, hemostasis is achieved by a combination of the above-mentioned endoscopic therapeutic procedures. However, there remains a subset of patients, approximately 5%, in whom endoscopic procedures are not sufficient for hemostasis and therefore require interventional radiotherapy or surgical intervention [13, 14].
[0012] Endoscopic therapy fails for a variety of reasons, including poor visualization of the lesion due to actively pulsating bleeding, difficulty in anatomical localization of the lesion with endoscopy, maximal therapy with currently available tools, and severe coagulopathy. Three different spray-based hemostatic powder devices, Ankeford Blood Stopper
[15] , EndoClot™
[16] , and HemoSpray™[17-19], available only outside the United States, are also believed to control NVUGIB. A potential concern with Hemospray is that it is a related product to WoundStat™, which was withdrawn in the United States in 2009 due to its thrombogenic nanoparticle bentonite, which promotes extensive microembolization
[20] that can cause tissue necrosis and organ failure.
[0013] Benign prostatic hyperplasia (BPH) and prostate cancer are two of the most common urological conditions treated by surgical intervention in older men. An estimated 50% of men will have histological evidence of BPH by age 50 years, and 75% will have such evidence by age 80 years. In 40-50% of these patients, BPH will become clinically significant. Although the incidence of uncontrolled bleeding from surgical interventions involving the prostate and urethra is relatively low, this remains a significant risk that must be addressed by a hospital stay of at least 2-3 nights. According to a statistical analysis from the U.S. Department of Health and Human Services from 2005 to 2010, there were an average of 150,000 hospital discharges from open or transurethral prostatectomy in the United States, with direct operative costs averaging more than $4.5 billion per year. In these patients, the average length of stay for open or transurethral prostatectomy was 3.1 and 2.4 days, respectively. In patients who required transfusions due to significant blood loss during surgery (4-5%), the average length of hospital stay increased to 5-6 days, which increased the average cost by $15,700 per case compared to the average cost for prostatectomy patients in 2010 ($29,300). The cost of the prostatectomy procedure is driven by operating room time, surgeon time, and length of hospital stay.
[0014] TURP is considered the benchmark therapy for BPH. Partial removal (resection) of the prostate is accomplished in TURP by minimally invasive surgery through the urethra using a cystoscope (transurethral cystoscope) and electrocautery. Although the thin-loop electrocautery used in TURP results in less tissue necrosis than other less common minimally invasive prostatectomy techniques, TURP results in more intraoperative bleeding. Adequate prostatectomy and control of bleeding in TURP are key challenges, as in other forms of prostatectomy. The amount of intraoperative bleeding in prostatectomy depends on the size of the prostate, the length of time to remove the prostate, and the skill of the surgeon. Significant or heavy bleeding after prostatectomy often leads to unwanted retention of blood clots (and therefore urine retention) in the bladder and urethra, which can increase hospital stays and even require reoperation. In general, arterial bleeding is easier to identify and controlled by electrocoagulation, whereas venous bleeding, which is more prevalent in TURP, is more difficult to control. Attempts to control venous bleeding by electrocautery and irrigation can result in undesirable outcomes such as TURP syndrome. In standard-of-care control, venous bleeding is controlled by filling the bladder with irrigating fluid and applying an inflated transurethral balloon catheter to compress the bleeding prostatic cavity. The postoperative morbidity associated with TURP is as high as 18%, with a reported operative mortality rate of 0.3%. In elderly patients, the risk of morbidity and mortality associated with blood loss is significantly increased in association with coagulopathy and cardiovascular abnormalities. Uncontrolled bleeding during TURP remains one of the major complications of prostatectomy, often resulting in conversion to the less desirable open surgery. Despite significant advances in the management of BPH, the incidence of uncontrolled heavy bleeding is still around 6%, with a transfusion rate to address this bleeding of 4%-5%.
[0015] A typical TURP involves a 2-4 day hospital stay, and the patient has an inflated urinary balloon catheter in place until bleeding has stopped and urine is clear. If postoperative bleeding after TURP can be significantly reduced, the time required for catheterization and hospital beds will be reduced. This will also reduce the incidence of ureteral infections, catheter-related patient discomfort, and associated complications. Significant hematuria (blood in the urine) resulting from transurethral or open surgery can cause hemodynamic instability and retention of blood clots, requiring urgent medical attention and medical treatment for hemostasis, removal of blood clots, transfusion, and evaluation of coagulation. Treating significant hematuria by a transurethral approach is cumbersome because the surgery is visually and spatially constrained. Patients often must be taken back to the operating room to perform open bladder surgery to achieve hemostasis and remove the bladder clot. A complicating factor for prostatectomy is that TURP patients are generally on anticoagulant therapy due to the presence of other chronic conditions, such as cardiovascular disease. Due to the risk of bleeding, it is preferable to wean these patients off anticoagulant medications such as Coumadin and Plavix prior to TURP surgery, but it is preferable to be able to perform the procedure while the patient remains on medication to reduce the chance of stroke or myocardial infarction during the procedure. There is an urgent need for a reliable and durable hemostatic approach for transurethral application to control significant bleeding after prostatectomy, preferably effective in individuals on anticoagulant therapy.
[0016] Chitosan materials have been used in the art to address hemorrhage in various applications with varying degrees of success. However, progress and improvements are desperately needed to unlock the potential of catechol-modified chitosan and provide alternative and better chitosan-based solutions for safe, reliable and effective delivery of bioactive chitosan materials within the body, especially in challenging in vivo biological environments. Summary of the Invention [Means for solving the problem]
[0017] A brief summary The present invention relates to dissolution-resistant tissue-adhesive chitosan materials. These chitosan materials include catechol-modified chitosans and are generally referred to herein as "dressings", a term used to refer to solid, dry materials formed from the chitosan materials of the present invention. The described chitosan materials may be suitable for and may be used in minimally invasive procedures.
[0018] It should be understood that the chitosan materials described herein have numerous beneficial properties attributable to the chitosan material itself, and that these chitosan materials can take a myriad of possible solid forms. Beneficial properties characteristic of and attributable to the chitosan materials described herein include, but are not limited to, the ability to tailor the material by controlling the degree of substitution and the level of oxidation. By tailoring the material by controlling the degree of substitution and the level of oxidation, the chitosan material can withstand rapid degradation in challenging biological environments such as the GI tract, urethra, lower GI tract, and internal body cavities such as the abdominal and thoracic cavities, and dissolve sufficiently to disappear in less than about 7 days. An additional beneficial property of the chitosan material is that it is also biocompatible, hemostatic, and tissue adhesive. Furthermore, the solid, dry chitosan material described herein can be delivered as a final form or a separate dry material construct that can displace interfering liquids due to its capillarity (the presence of holes or porosity) and / or pressurization, which in some cases may be at low pressure (e.g., about 1 atmosphere), or can be delivered at ventilation pressure in the case of a dry powder. The chitosan materials of the present invention produce final forms or discrete dry material constructs that are capable of rapid adhesion and resist dissolution.
[0019] The dressings described herein are provided as non-limiting examples of final forms made using the chitosan material of the present invention. The dressings described and illustrated herein provide examples of the conversion of catechol-modified chitosan materials into various test articles or final forms, demonstrating the solid attributes of the solid chitosan material. Additional dry, solid chitosan final forms include, but are not limited to, frozen phase-separated matrices and dressings formed therewith, fibers, powders, films, membranes, meshes, pledgets, and the like. The present disclosure generally relates to chitosan dressings that, in view of their characteristics, can be applied to stop bleeding in various physiological settings. Embodiments include, among others, chitosan gastrointestinal hemostatic dressings (CGHD) and chitosan intraluminal hemostatic dressings (CEHD).
[0020] The materials of the invention have one or more, or a combination of all of the following properties: (1) can be compressed for delivery without tearing or sacrificing mechanical performance; (2) can be applied in the presence of blood and other biological fluids at about 37° C. without significant dimensional change in length, width, and height or loss of mechanical properties; (3) can be delivered in the presence of biological fluids and blood; (4) can be delivered to a surgical site manually or by a minimally invasive delivery device; (5) can expand from a compressed state at the delivery site; (6) allows for capillarity, porosity, and absorbency to remove hydrophilic and hydrophobic biological fluids that may interfere with adhesion; (7) is activated by wetting and adheres to mucosa, excised mucosa, and excised tissue with the application of uniform pressure; (8) can contact itself and the packaging material when dry without adhering to itself or the packaging material; and (9) includes at least one tissue-adherent side of the material that can contact itself and the packaging material when wetted with urine or blood without adhering to itself or the packaging or delivery material if the wet contact does not exceed 300 seconds. (10) It can adhere uniformly to tissue and rapidly promote local thrombus formation. (11) It can be released from the delivery device and enable the delivery device to be retrieved from the surgical site. (12) Application ofAble to withstand dissolution when exposed to biological fluids ranging from about pH 3.0 to about pH 8 at about 37° C. for the first 12 hours. (13) Allows ostomy connection channels, such as those in the gastrointestinal tract and urethra (with or without a delivery device in place), to be unobstructed with existing material or material residue and to allow for an unobstructed excretory passage. (14) Provides protection to the injury site and promotes healing. (15) Provides controlled, slow degradation and / or dissolution from the attachment site such that removal without surgical assistance in less than seven days of ostomy use. (16) The material of the present invention may comprise one of a powder, film, matrix, membrane, thin foil, pledget, fiber, and coating. (17) The tissue adhesive materials of the present invention may include, but are not limited to, uses as adhesive dressings, adhesive hemostatic dressings, internal adhesive fixation materials, adhesive patches for localized controlled release of active agents, sutures, staples, orthopedic bone fixation materials, occlusive sutureless patches, and materials for promoting thrombus formation and sealing vascular malformations.
[0021] Although a significant portion of UGIB is easily controlled by existing tools in the United States, there is an unmet need for the low-risk devices of the present invention that provide rapid control of active arterial bleeding. Broad application of the present invention could allow for a significant reduction in morbidity and mortality in the treatment of gastrointestinal bleeding, with a concomitant reduction in associated health care costs.
[0022] The chitosan materials of the present invention are suitable for use in any gastrointestinal bleeding application and can be delivered, for example, as a chitosan gastrointestinal hemostatic dressing (CGHD) by wire through a standard endoscope working channel (diameter 3.2 mm or less) or by balloon catheter delivery. The subject materials of the present invention provide an opportunity to address or mitigate deficiencies associated with current procedures such as clipping, thermal coagulation, and injections, which require pinpoint accuracy and are difficult under conditions of active bleeding and impaired visibility.
[0023] The present invention provides such compositions, methods of using such compositions, and methods of making such compositions.
[0024] In a preferred embodiment, the chitosan material comprises a catechol-modified chitosan, and the CGHD dressing formed from the material is hemostatic and has a thickness of 500 microns or less. The CGHD dressing may have a dry dressing thickness that is one of: (i) about 200 microns or less, (ii) about 100 microns or less, or (iii) about 50 microns or less. The dressing has a dry dressing thickness of about 0.03 g / cm. 3 ~about 0.7g / cm 3 (i) about 0.3 g / cm 3 ~ approx. 0.4g / cm 3 (ii) in the range of about 0.4 g / cm 3 ~about 0.5g / cm 3 , or about 0.35 g / cm 3 ~about 0.55g / cm 3The dressing may have a density ranging from about 10 mm to about 50 mm. The dressing may be compressed. The dressing may be square, rectangular, circular, or circular petal shaped, with the measurements of each of the length and width of the square or rectangular shapes ranging from about 10 mm to about 50 mm, or the diameter of the circular or circular petal shapes ranging from about 10 mm to about 50 mm. In certain embodiments, the dressing measures one of: (i) 10 mm x 10 mm, (ii) 20 mm x 20 mm, or (iii) 25 mm x 25 mm. The dressing has a moisture content of (1) 15% by weight (w / w) or less, (2) 8% by weight (w / w) or less, or (3) 4% by weight (w / w) or less when dry. The dressing has an adhesive side and a non-adhesive side. The dressing may have an adhesive side provided on a first layer, and the non-adhesive side provided on a second layer. The adhesive side of the dressing adheres to the surface of the tissue when the dressing is wet. When the coating is wet, the non-adhesive side of the coating does not adhere to the delivery device. The coating can adhere to the gastrointestinal mucosa in one minute or less. The coating can form a quaternary ammonium cation with the C-2 amine of the glucosamine of the chitosan at the tissue site. The coating can include catechols oxidized to o-quinones and crosslinked in the chitosan coating. The chitosan coating can have a brown coloration, including a dark brown coloration. In one embodiment, the coating can include unoxidized catechols and the chitosan coating has a pink coloration. The coating can include lyophilized lamellae. The coating can include a lyophilized structure having a thickness of 50 microns or less. The coating can include a lyophilized structure including more than one lyophilized layer. The coating can include spun fibers. The coating can include a porous surface. The coating can include a porous surface, which provides one or more of (i) an absorbent surface and (ii) channels that redirect moisture away from the target tissue surface site. The dressing may adhere to moist tissue in moist conditions. The adhesive strength of the dressing may be greater than or equal to about 1 kPa. The dressing resists dissolution in water, saline solution, blood, or GI fluids for at least about 6 hours at about 37° C. The dressing may be folded or rolled without cracking or tearing.The dressing may have an outward facing surface area in an open, unrolled, or unfolded state that is one of about 6 times, about 5 times, or about 4 times the outward facing surface area of the same dressing in a closed, rolled, or folded state. The dressing may have a ratio of outward facing surface area in an open, unrolled, or unfolded state to that in a closed, rolled, or folded state of about 15:1, or about 14:1, or about 13:1, or about 12:1, or about 11:1, or about 10:1, or about 9:1, or about 8:1, or about 7:1, or about 6:1, or about 5:1, or about 4:1, or about 3:1, or about 2:1. The dressing may be punctured or sutured without cracking or tearing. The dressing may be crosslinked. The dressing can be delivered intact by a balloon device, a wire device, or an endoscopic device, the device including a working channel having a diameter of 3.2 mm or less, through which the dressing is delivered. The dressing can be moistened and adhered intact to the gastric mucosa in less than 30 seconds, for example, with application of light pressure of about 200-300 g. The dressing can remove hydrophilic and hydrophobic biological fluids that may interfere with adhesion. The dressing can remain intact in place and stop moderate to exudative bleeding at about 20 ml / min to about 150 ml / min. The dressing is easily removed from the delivery device after adhering to the target tissue site. After adhering to the injury site, the dressing can resist dissolution in the presence of erosive enzymes and an acidic environment of about pH 3 for at least 6 hours. The dressing can seal and protect the target tissue site for at least 12 hours. The dressing can achieve controlled slow dissolution from the attachment site over a period not exceeding 7 days. The dressing can be folded and unfolded. The dressing can be rolled or unrolled. The dressing does not readily dissolve in water, saline solution, blood, or GI fluids at about 37° C. for at least 12 hours after application. The dressing does not readily dissolve in water, saline solution, blood, or GI fluids at about 37° C. for at least 24 hours after application. The dressing does not adhere to the delivery device.The dressing does not increase or decrease in size by more than about 25% in length and width, or by more than about 50% in thickness, in the presence of water, saline solution, blood, or GI fluid at about 37° C. The dressing includes an adhesive side that interacts with the injury site, and the chitosan dressing includes a non-adhesive side that interacts with the delivery device or one of the adhesive sides when the dressing is in a dry folded or dry rolled state. The dressing can be terminally sterilized without affecting the characteristics of the dressing. The chitosan dressing can be stored under controlled conditions for extended periods of time without affecting the characteristics of the dressing.
[0025] UGIB bleeding rates, or blood flow rates, in ml / min suitable for treatment with the devices described herein may range from about 1 ml / min to about 200 ml / min. In a preferred embodiment, bleeding rates addressed by the device range from about 1 ml / min to about 150 ml / min. Forrest 1a UGIB is about 25 ml / min. Subjects experiencing bleeding rates greater than Forrest 1a are unlikely to survive unless they are already in the operating room. UGIB bleeding rates of about 20 ml / min to 25 ml / min are considered "active" bleeding. Exudative bleeding is generally greater than about 1 ml / min. This is because it has been noted that at low bleeding rates such as 1 ml / min, clots typically form and stop spontaneously unless the subject is on anticoagulant therapy or has a compromised clotting cascade for reasons other than taking anticoagulant medication. For such subjects who are receiving irreversible anticoagulant medication or have a bleeding disorder, exudative bleeding of 1 ml / min remains a concern and needs to be addressed, such as by devices formed from the materials of the present invention. In some embodiments, the devices described herein are used to address UGIB bleeding rates of about 1 ml / min to about 25 ml / min, or about 1 ml / min to about 20 ml / min, or about 1 ml / min to about 15 ml / min, or about 1 ml / min to about 10 ml / min, or about 1 ml / min to about 5 ml / min. In some embodiments, the dressings can be used to treat a disease, condition, disorder, trauma, or injury. For example, use of the dressings in treating a disease, condition, disorder, trauma, or injury includes adhering the dressing directly to the injury site upon wetting and applying pressure to the dressing for about 30 seconds. Dressings for use in treating a disease, condition, disorder, trauma, or injury can remove hydrophilic and hydrophobic biological fluids upon adhering. Dressings for use in treating a disease, condition, disorder, trauma, or injury can include leaving the dressing in place at the target tissue site, and the dressing can remain at the target tissue site for at least 24 hours. The dressings for use in treating a disease, condition, disorder, trauma, or injury can be slowly dissolving at the target tissue site, completely dissolving in seven days or less without human intervention.
[0026] In some embodiments, the invention disclosed herein includes a method for producing a chitosan coating. In one embodiment, the method includes the steps of carrying out synthesis with chitosan and catechol in an aqueous reaction solution, maintaining the pH of the reaction solution at or below pH 5.5, increasing the pH of the reaction solution and controlling the exposure of oxygen to the reaction solution to effect oxidation and crosslinking of the catechol, and drying the reaction solution. In certain embodiments, the method does not include an intermediate drying step between the steps. In certain embodiments, the method includes increasing the pH of the reaction solution to about 5.8 to about 6.2. Another embodiment of the method for producing a chitosan coating includes the steps of freeze-drying a first aqueous solution containing chitosan, freeze-drying a second aqueous solution containing chitosan, obtaining an interconnected porous structure low-density chitosan coating from each of the above steps, and compressing the low-density chitosan coating from each of the steps, and preparing a two-layer chitosan coating from the compressed low-density chitosan coating. In certain embodiments, the low density chitosan coating from each of the above freeze-drying steps are combined prior to compression. In certain embodiments, the compression step is carried out at a temperature ranging from about 20° C. to about 150° C. In certain embodiments, the coating is dried to a moisture content of less than about 15% (w / w).
[0027] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by those skilled in the art to which this invention belongs.Methods and materials are described herein for use in the present invention, and other suitable methods and materials known in the art can also be used.Materials, methods, and examples are for illustration only and are not intended to be limiting.All publications, patent applications, patents, sequences, database entries, and other references mentioned herein are incorporated by reference in their entirety.In case of discrepancies, the present specification, including definitions, will control.
[0028] Other features and advantages of the invention will become apparent from the following detailed description and drawings, and from the claims. In an embodiment of the present invention, for example, the following items are provided: (Item 1) A chitosan material comprising a catechol-modified chitosan, the chitosan material being in a dry solid form that resists dissolution. (Item 2) 2. The chitosan material of item 1 having a thickness of 500 microns or less. (Item 3) Approximately 0.03g / cm 3 ~about 0.7g / cm 3 3. The chitosan material according to item 1 or 2, having a density in the range of (Item 4) (i) Approx. 0.3g / cm 3 ~ approx. 0.4g / cm 3 , (ii) about 0.4 g / cm 3 ~about 0.5g / cm 3 3. The chitosan material according to item 1 or 2, having a density in the range of (Item 5) Approximately 0.35g / cm 3 ~about 0.55g / cm 3 3. The chitosan material according to item 1 or 2, having a density in the range of (Item 6) 4. The chitosan material according to any one of items 1 to 3, which is compressed. (Item 7) the material is in a square, rectangular, circular, or circular petal shape; The respective measurements of the length and width of the square or rectangle may range from 1) about 10 to about 50 mm, or 2) 30 mm to about 70 mm; The diameter of each of the circular or circular petal shapes is in the range of about 10 mm to about 50 mm, or 30 mm to about 70 mm; 4. The chitosan material according to any one of items 1 to 3. (Item 8) 8. The chitosan material according to item 7, wherein the dimensions of the material are one of: (i) 70 mm x 70 mm, (ii) 50 mm x 50 mm, (iii) 30 mm x 30 mm, (iv) 25 mm x 25 mm, (v) 20 mm x 20 mm, (vi) 10 mm x 10 mm. (Item 9) 4. The chitosan material according to any one of items 1 to 3, having a moisture content of (1) 15% by weight (w / w) or less, (2) 8% by weight (w / w) or less, or (3) 4% by weight (w / w) or less. (Item 10) 4. The chitosan material according to any one of the preceding claims, having an adhesive side and a non-adhesive side. (Item 11) 11. The chitosan material according to item 10, wherein the adhesive side is provided on a first layer and the non-adhesive side is provided on a second layer. (Item 12) 11. The chitosan material according to item 10, wherein the adhesive side adheres to a tissue surface when the material is wet. (Item 13) 11. The chitosan material of item 10, wherein the non-adhesive side does not adhere to a delivery device when the material is wet. (Item 14) 4. The chitosan material according to any one of items 1 to 3, which adheres to the gastrointestinal mucosa in 1 minute or less, or adheres to the bladder mucosa in 3 minutes or less, or both. (Item 15) 4. The chitosan material according to any one of the preceding claims, which forms a quaternary ammonium cation at the C-2 amine of the glucosamine of the chitosan at the tissue site. (Item 16) 4. The chitosan material according to any one of items 1 to 3, wherein the catechols in the chitosan material are oxidized to o-quinones to be crosslinked. (Item 17) 4. The chitosan material according to any one of items 1 to 3, having 1) a brown coloration, including a dark brown coloration, or 2) a pink to pinkish brown coloration. (Item 18) 4. The chitosan material according to any one of the preceding claims, wherein said catechol is not oxidized and said chitosan material has a pink coloration. (Item 19) 4. The chitosan material according to any one of the preceding claims, further comprising freeze-dried lamellae. (Item 20) 20. The chitosan material according to item 19, wherein the freeze-dried structure has a thickness of 50 microns or less, or 100 microns or less. (Item 21) 20. The chitosan material according to item 19, wherein the freeze-dried structure comprises more than one freeze-dried layer. (Item 22) 4. The chitosan material of any one of the preceding claims, further comprising spun fibers. (Item 23) 4. The chitosan material according to any one of the preceding claims, further comprising a porous surface. (Item 24) 24. The chitosan material of claim 23, wherein said porous surface provides one or more of: (i) an absorbent surface; and (ii) channels that redirect moisture away from the target tissue surface site. (Item 25) 4. The chitosan material according to any one of items 1 to 3, which adheres to wet tissue in wet conditions. (Item 26) 26. The chitosan material according to item 25, wherein the material adhesive strength is greater than or equal to about 1 kPa. (Item 27) 4. The chitosan material of any one of items 1 to 3, which resists dissolution in water, saline solution, blood, GI fluid, or urine at about 37° C. for at least about 6 hours. (Item 28) 4. The chitosan material according to any one of items 1 to 3, which can be folded or rolled without cracking or splitting. (Item 29) 4. The chitosan material of any one of the preceding claims, having an outwardly facing surface area in an open, unrolled or unfolded state that is one of about 8 times, about 7 times, about 6 times, about 5 times, or about 4 times the outwardly facing surface area of the same material when closed, rolled or folded. (Item 30) 4. The chitosan material according to any one of items 1 to 3, wherein the ratio of the outwardly facing surface area in the open, unrolled or unfolded state to the closed, rolled or folded state is about 15:1, or about 14:1, or about 13:1, or about 12:1, or about 11:1, or about 10:1, or about 9:1, or about 8:1, or about 7:1, or about 6:1, or about 5:1, or about 4:1, or about 3:1, or about 2:1. (Item 31) 4. The chitosan material according to any one of items 1 to 3, which can be drilled or sutured without cracking or splitting. (Item 32) 4. The chitosan material according to any one of items 1 to 3, which is crosslinked. (Item 33) 33. The chitosan material according to any one of the preceding claims, which is intact and can be delivered by a balloon device, a wire device or an endoscopic device. (Item 34) 34. The chitosan material according to item 33, wherein the balloon device or the wire device or the endoscopic device comprises a working channel having a diameter of 3.2 mm or less or 7.0 mm or less, through which the material is delivered. (Item 35) 33. The chitosan material according to any one of the preceding claims, which can be moistened and adhered intact to the gastric mucosa in less than 30 seconds with the application of light pressure, or can be moistened and adhered to the bladder mucosa in less than 3 minutes, or both. (Item 36) 36. The chitosan material according to item 35, wherein the light pressure is about 200-300 g, or the material adheres intact to the bladder mucosa in less than 2 minutes, or both. (Item 37) 33. The chitosan material according to any one of the preceding claims, which is capable of removing hydrophilic and hydrophobic biological fluids which may interfere with adhesion. (Item 38) 33. The chitosan material according to any one of the preceding claims, which remains intact in place and is capable of stopping moderate to exudative bleeding in the range of 1) about 20 ml / min to about 150 ml / min, or 2) about 1 ml / min to about 150 ml / min. (Item 39) 33. The chitosan material according to any one of the preceding claims, which is easily removed from the delivery device after adhering to the target tissue site. (Item 40) 33. The chitosan material according to any one of the preceding claims, which after being adhered to the injury site, can withstand dissolution in the presence of erosive enzymes and an acidic environment of about pH 3, or in the presence of urine, or both, for at least 6 hours. (Item 41) 33. The chitosan material according to any one of the preceding claims, which is capable of sealing and protecting the target tissue site for at least 12 hours. (Item 42) 33. The chitosan material according to any one of the preceding claims, which is capable of achieving controlled, slow dissolution from the site of attachment over a period not exceeding 7 days. (Item 43) 33. The chitosan material according to any one of the preceding claims, which can be folded and unfolded. (Item 44) 33. The chitosan material according to any one of the preceding claims, which can be rolled and unrolled. (Item 45) 33. The chitosan material according to any one of the preceding items, which is not readily soluble at about 37° C. and at about pH 4.5 to pH 8 for at least 12 hours after application. (Item 46) 33. The chitosan material according to any one of the preceding claims, which is not readily soluble in water, saline solution, blood, or GI or bladder fluids or urine at about 37°C for 1) at least 12 hours after application or 2) at least 24 hours after application or both 1) and 2). (Item 47) 33. The chitosan material according to any one of the preceding claims, which does not adhere to a delivery device. (Item 48) 33. The chitosan material according to any one of the preceding claims, which does not increase or decrease in size by more than about 25% in length and width, or by more than about 50% in thickness, in the presence of water, saline solution, blood, or GI or bladder fluid, or urine at about 37°C. (Item 49) 33. The chitosan material according to any one of the preceding claims, comprising an adhesive side that interacts with an injury site and a non-adhesive side that interacts with a delivery device or one of the adhesive sides when the material is in a dry folded or dry rolled state. (Item 50) 33. The chitosan material according to any one of the preceding claims, which can be terminally sterilized without affecting the characteristics of the material. (Item 51) 33. The chitosan material according to any of the preceding claims, which can be stored under controlled conditions for extended periods of time without affecting the characteristics of the material. (Item 52) 52. The chitosan material according to any one of the preceding items, for use in the treatment of a disease, condition, disorder, trauma or injury. (Item 53) 52. The chitosan material according to any one of the preceding claims for use in the treatment of a disease, condition, disorder, trauma or injury comprising adhering said material directly to the injury site upon wetting and applying pressure to said material for about 30 seconds. (Item 54) 52. The chitosan material according to any one of the preceding claims, for use in the treatment of a disease, condition, disorder, trauma or injury, wherein said material removes hydrophilic and hydrophobic biological fluids upon adhesion. (Item 55) 52. The chitosan material of any one of the preceding claims for use in the treatment of a disease, condition, disorder, trauma, or injury, further comprising leaving the material in place at the target tissue site. (Item 56) 56. The chitosan material according to item 55, for use in the treatment of a disease, condition, disorder, trauma, or injury, wherein said material remains at said target tissue site for at least 24 hours. (Item 57) 56. The chitosan material according to item 55, for use in the treatment of a disease, condition, disorder, trauma, or injury, wherein the dressing is capable of slowly dissolving at the target tissue site and dissolving completely in 7 days or less without human intervention. (Item 58) 52. The chitosan material according to any one of the preceding items, for use in combination with TURP. (Item 59) 59. The chitosan material according to item 58, which allows unimpeded passage of urine both in the presence and in the absence of a delivery device. (Item 60) 52. A method for producing a chitosan material according to any one of items 1 to 51. (Item 61) (a) carrying out the synthesis with chitosan and catechol in an aqueous reaction solution; (b) maintaining the reaction solution at or below pH 5.5; (c) increasing the pH of the reaction solution after step (b) and controlling the oxygen exposure of the reaction solution to effect oxidation and crosslinking of catechol; and (d) drying the reaction solution; does not include an intermediate drying step between steps (b) and (c); Methods for producing catechol-modified chitosan materials. (Item 62) Item 62. The method according to Item 61, wherein in step (c), the pH of the reaction solution is increased to a range of about 5.8 to about 6.2. (Item 63) (a) freeze-drying a first aqueous solution containing chitosan; (b) freeze-drying the second aqueous solution containing chitosan; (c) obtaining an interconnected porous low-density chitosan material from each of steps (a) and (b); and (d) compressing the low density chitosan material from each of steps (a) and (b); and (e) preparing a bilayer chitosan material from said compressed low density chitosan material from each of steps (a) and (b). 2. A method for producing a chitosan material comprising: (Item 64) Item 64. The method of item 63, wherein the low density chitosan material from each of steps (a) and (b) is combined prior to compression. (Item 65) Item 64. The method according to item 63, wherein the compressing in step (d) can be carried out at a temperature in the range of about 20°C to about 150°C. (Item 66) Item 64. The method of item 63, further comprising the step of drying the coating to a moisture content of less than about 15% (w / w). (Item 67) (a) controlling the degree of substitution; (b) controlling the level of oxidation; and (c) preparing a dry, solid catechol-modified chitosan material; 1. A method for producing a catechol-modified chitosan material comprising: The method, wherein the material resists dissolution in water, saline solution, blood, GI fluids, or urine at about 37° C. for at least about 6 hours. (Item 68) 60. The chitosan material according to any one of the preceding claims, wherein the dry solid form is a powder. (Item 69) 60. The chitosan material according to any one of the preceding claims, wherein the dry solid form is a matrix. (Item 70) 60. The chitosan material according to any one of the preceding claims, wherein the dry solid form is a film. (Item 71) 60. The chitosan material according to any one of the preceding claims, wherein the dry solid form is a thin foil. (Item 72) 60. The chitosan material of any one of the preceding claims, wherein the dry solid form is a pledget. (Item 73) 60. The chitosan material according to any one of the preceding claims, wherein the dry solid form is a fiber. (Item 74) 60. The chitosan material according to any one of the preceding claims, wherein the dry solid form is a coating. [Brief description of the drawings]
[0029] [Figure 1A] 1A, 1B, 1C, 1D, 1E, 1F, and 1G illustrate the introduction, installation, and use of coatings formed from materials of the present invention. [Figure 1B] 1A, 1B, 1C, 1D, 1E, 1F, and 1G illustrate the introduction, installation, and use of coatings formed from materials of the present invention. [Figure 1C] 1A, 1B, 1C, 1D, 1E, 1F, and 1G illustrate the introduction, installation, and use of coatings formed from materials of the present invention. [Figure 1D] 1A, 1B, 1C, 1D, 1E, 1F, and 1G illustrate the introduction, installation, and use of coatings formed from materials of the present invention. [Figure 1E] 1A, 1B, 1C, 1D, 1E, 1F, and 1G illustrate the introduction, installation, and use of coatings formed from materials of the present invention. [Figure 1F] 1A, 1B, 1C, 1D, 1E, 1F, and 1G illustrate the introduction, installation, and use of coatings formed from materials of the present invention. [Figure 1G] 1A, 1B, 1C, 1D, 1E, 1F, and 1G illustrate the introduction, installation, and use of coatings formed from materials of the present invention. [Diagram 2] Figure 2 illustrates a digital image of a gloved hand holding a folded, double-sided dressing formed from the material of the present invention. The dark side is the tissue-adherent catechol-modified chitosan side, and the light side and other edge area is the unmodified chitosan dressing side (the unmodified dressing surface is 2.5 inches in diameter, the modified catechol dressing surface is 2 inches in diameter). [Figure 3A] Figures 3A and 3B illustrate digital images of a double-sided catechol-modified chitosan coating formed from the material of the present invention that was adhered to the wall of a 250 ml graduated cylinder by application of a balloon catheter for 2 hours and immersed in 0.9% w / w saline solution at 25±3° C. for nearly 48 hours after initial attachment. Note that there is no trace of the original unmodified chitosan coating at 48 hours. Figure 3A is a side view and Figure 3B is a top view. [Figure 3B] Figures 3A and 3B illustrate digital images of a double-sided catechol-modified chitosan coating formed from the material of the present invention that was adhered to the wall of a 250 ml graduated cylinder by application of a balloon catheter for 2 hours and immersed in 0.9% w / w saline solution at 25±3° C. for nearly 48 hours after initial attachment. Note that there is no trace of the original unmodified chitosan coating at 48 hours. Figure 3A is a side view and Figure 3B is a top view. [Figure 4]FIG. 4 illustrates a digital endoscopic image of a catechol chitosan dressing formed from the material of the present invention within 30 minutes, uniformly attached to the bladder neck and urethral lumen of a nearly 100 pound sow. The bladder is swollen with urine and saline injected to aid in viewing. The image was acquired by trocar delivery of an endoscope through the pig's bladder wall and with the endoscope's perspective aimed at the pig's bladder neck and urethral entrance. The image shows a patent urethra, a faint unmodified chitosan lining that is rapidly degrading, and the modified catechol dressing in close contact with the bladder neck and urethral lumen. [Figure 5A]In Figures 5A and 5B, one image shows a plan view of the folded dressing, all other images show cross-sections / side views. Reference numbers, if included in the attached figures, correspond to the text as follows: 1 - prostate, 2 - bladder, 3 - urethral mucosa, 4 - catheter body tube, 5 - sheath, 6 - rolled CEHD on delivery balloon of delivery catheter, 7a - conically folded CEHD with attachment point (14) proximal (left) of delivery balloon catheter, 7b - conically folded CEHD with attachment point (14) distal (right) of delivery balloon catheter, 7c - CEHD with attachment point (14) distal. Plan view of conically folded CEHD. Note that there can be two dressings attached distally and proximally to one balloon or only one dressing attached proximally only. An alternative delivery is by a CEHD wrapped cylindrically around the delivery balloon, not shown. 8-Delivery balloon (shown is a less preferred single balloon catheter and a preferred double balloon). In a double balloon catheter the delivery balloon is also the proximal balloon. 9-Notches (9a: proximal, 9b: distal) for creating a circular window attachment point towards the tip of the conically folded covering, 10-Overlapping edges of the two faces of the conically folded covering facing each other, 11-Tip of the conically folded CEHD (11a: proximal, 11b: distal), 12-Perfusion port (12a: proximal, 12b: distal), 14-Attachment point of the tip of the conically folded CEHD to the balloon catheter where the body of the CEHD is folded over and wrapped around the delivery balloon. A simple double-sided pressure bond successfully attaches the CEHD tip to the catheter. This attachment aids in the application of the CEHD by allowing a fitted sheath to slide over the folded and rolled CEHD without the CEHD getting caught in the sheath. 15- Distal or placement / positioning of the balloon in a double balloon delivery catheter. Double balloon catheters are preferred over single balloon catheters because the distal balloon can be used to rupture the sheath and initiate its removal, thus providing the ideal ability to position the delivery balloon.The distal balloon can be used to appose the CEHD to the bladder neck in cases of anastomosis and bladder neck injury. 16-Ports for balloon catheters (3 ports are typical for a 2-balloon catheter, but multi-lumen catheters with 2 balloons may have more ports). There is typically one port for each balloon, as well as at least one point for irrigation and drainage. The ports are typically connected to standard syringe luer connectors. [Figure 5B] Same as above. [Figure 6] Figure 6 illustrates the chemical structural representation of chitosan (R1 = H and acetyl groups) and catechol modified chitosan (R1 = H, acetyl, hydrocaffeic acid, caffeic acid, trans-caffeic acid, and homoprotocatechuic acid groups). For chitosan polymers, preferably n>60, more preferably n>300, and most preferably n>600. [Figure 7] FIG. 7 illustrates the N-acylation addition reaction in the presence of 1-ethyl-3-(-3-dimethylamino-propyl)-carbodiimide to covalently bond 3,4-dihydroxyhydrocinnamic acid to the C-2 amine of chitosan with a degree of substitution of 25% in aqueous solution at pH 5.5. [Figure 8] FIG. 8 illustrates the oxidation of catechol-modified chitosan to ortho-quinone-modified chitosan at high pH and in the presence of oxygen. [Figure 9] FIG. 9 illustrates the Schiff base (A) and Michael addition (B) reactions that lead to crosslinking between catechol-modified chitosan and chitosan. [Figure 10] FIG. 10 illustrates a 4 cm long and 1.5 cm internal diameter glass flow cell capable of supporting an elongated tube of porcine small intestinal submucosa 6 cm long and 1.5 cm diameter by applying pressure ties around both ends of the cell. [Figure 11]FIG. 11 illustrates a typical flow cell design (three cells mounted in parallel) for testing the adhesion and dissolution resistance under urine flow at 37° C. of the novel dressings adhered to cell-supported ex vivo tissue surfaces. [Figure 12A] 12A-12G show tables of various parameters of the batches used to prepare the chitosan coatings. [Figure 12B] Same as above. [Figure 12C] Same as above. [Figure 12D] Same as above. [Figure 12E] Same as above. [Figure 12F] Same as above. [Figure 12G] Same as above. [Figure 13A] 13A-13E show tables of various chitosan coating preparations including formulations, solubility, foldability, burst testing, ex vivo, accelerated stability, and in vivo characteristics. [Figure 13B] Same as above. [Figure 13C] Same as above. [Figure 13D] Same as above. [Figure 13E] Same as above. [Figure 14]FIG. 14 illustrates circular catechol modified chitosan dressings measuring 2.5 inches by 2 inches in diameter (before cutting) and compressed to approximately 50 microns. From left to right, the coloring of these catechol modified chitosan dressings ranges from a light pinkish brown (the first dressing), two dark pinkish brown dressings, two tan dressings (no pink), one brown dressing, and finally one dark brown dressing. Catechol chitosan dressings 5 and 6 were formed from 2.5 inch by 2 inch molds, both backed by unmodified chitosan dressings formed from a 2.5 inch mold. The unmodified chitosan is clearly visible as the white halo (no brown or pink) in dressing 6. The catechol chitosan and unmodified chitosan dressings adhere to each other during compression to a final covalent density of >0.4 g / cm3. Pink coloration is associated with unoxidized catechol, brown with oxidized catechol (o-quinone), light brown and light pink are associated with low degrees of substitution of chitosan with catechol (close to 10%), and darker coloration (pinkish brown and brown) is associated with high degrees of substitution of chitosan with catechol (close to 20%). [Figure 15] FIG. 15 illustrates a folded and unfolded catechol-modified chitosan dressing with the fold axis (crease) visible but intact. [Figure 16A] 16A-16C illustrate tables showing the results of the dissolution tests. [Figure 16B] Same as above. [Figure 16C] Same as above. [Figure 17A] 17A-17C illustrate tables showing the formulation approaches, hydrophilic polymers, and % w / w of hydrophilic polymer components in solution. [Figure 17B] Same as above. [Figure 17C] Same as above. [Figure 18]FIG. 18 illustrates a digital gastroscopic image of a modified catechol-chitosan dressing of the present invention in contact with the gastric mucosa, showing minimal swelling in the gastric environment and effective control of upper gastrointestinal bleeding (Forrest 1a) of an injured gastroepiploic artery inside a heparinized (ACT ≥ 250 seconds) porcine stomach 3 hours after application of the dressing to the arterial injury. [Figure 19] Figure 19 shows the presence of a strong, intact thrombus beneath the dressing of Figure 18 at the time of sacrifice of the animal, which occurred within 45 minutes of taking the image of Figure 18. The modified chitosan dressing was shown to be uniformly adherent to the injury and gastric mucosa at the time of sacrifice. [Figure 20] Figures 20-25 illustrate experiments using a peristaltic pump system circulating 0.9% saline through a 15 mm diameter glass cell containing the lumen of porcine small intestinal submucosa, pumped at a flow rate of 20 ml / min for 163 hours (close to 7 days (168 hours)) at a system temperature approaching 27°C. Small 10 mm x 10 mm patches of the modified catechol chitosan material of the present invention were hand applied to the small intestinal submucosa surface inside the glass cell and observed over time. Images show that the material remained firmly attached to the submucosal lumen over 7 days without loss of adhesion. When the lumen was removed from the cell on day 7, the material was found to have degraded and become extremely brittle. This system was used to screen formulations for transurethral development. Unmodified chitosan survived less than 2-3 hours in this model. [Figure 21] Same as above. [Figure 22] Same as above. [Figure 23] Same as above. [Figure 24] Same as above. [Diagram 25] Same as above. [Figure 26]FIG. 26 illustrates a digital gastroscopic image of a modified catechol chitosan coating formed from the material of the present invention in contact with the gastric mucosa, showing minimal swelling in the gastric environment and effective control of upper gastrointestinal bleeding (Forrest 1a) of an injured gastroepiploic artery inside a heparinized (ACT ≥ 250 seconds) porcine stomach 3 hours after application of the material to the arterial injury. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0030] Detailed Description In one aspect, the present invention relates to a biocompatible, foldable, thin profile chitosan-based dressing comprising catechol-modified chitosan and characterized by one or more or all of the following features: (1) Able to be delivered intact by balloon or through endoscopic devices; (2) Able to wet and adhere intact to gastric mucosa in less than 30 seconds with application of light pressure; (3) Able to have capillarity, porosity, and absorbency to remove hydrophilic and hydrophobic biological fluids that may interfere with adhesion; (4) Able to remain intact in place and stop moderate to exudative bleeding, e.g., bleeding rates of about 20 ml / min to about 100 ml / min or greater; (5) Able to release from a delivery device, allowing for retrieval of the delivery device from the GI environment; (6) Able to withstand adverse rapid degradation (less than 6 hours) in the aggressive enzymes and acidity (pH 3 or greater) of the GI environment. (7) It is capable of protecting the site of injury in the gastrointestinal tract for preferably up to 12 hours, more preferably up to 24 hours, and most preferably up to 96 hours, and subsequently assisting in rapid healing and closure, and (8) It is capable of achieving controlled, slow dissolution from the site of attachment, thereby allowing complete unassisted removal in less than 7 days, and allowing the dissolved residue to pass safely through the gastrointestinal tract.
[0031] The present invention addresses rapid bleeding control in transurethral resection of the prostate, open prostatectomy, and cystectomy using a foldable, thin (approximately 500 microns thick or less), tissue-adherent, chitosan-based hemostatic dressing. Dressings formed from the materials of the present invention have one or more, or all of the following characteristics: (1) They can be folded or rolled and unfolded without tearing or sacrificing mechanical performance; (2) They can be applied in the presence of blood and urine at approximately 37° C. without significant dimensional change in length, width, and height or loss of mechanical properties; (3) They can be delivered in the presence of urine and blood; (4) They can be delivered to the injury site by transluminal or transurethral delivery devices; (5) They can be unfolded or rolled at the delivery site; and (6) They are characterized by capillarity, porosity, and absorbency that can remove hydrophilic and hydrophobic biological fluids that may interfere with adhesion. (7) Activated by wetting and adheres to bladder mucosa, excised bladder mucosa, and excised prostate with application of uniform pressure. (8) Able to contact itself and the packaging material when dry without adhering to itself or the packaging material. (9) Includes a tissue-adherent side of the dressing that can contact itself and the packaging material when wetted with urine or blood without adhering to itself or the packaging material if the wetting contact is for about 300 seconds or less. (10) Able to uniformly adhere to tissue and rapidly stop moderate to exudative bleeding, or bleeding rates of, for example, about 20 ml / min to about 100 ml / min or more, with a pressure of about 50 mmHg or less, providing the opportunity to perform TURP as an outpatient procedure. (11) Able to release from the delivery device and allow for withdrawal of the delivery device from the urethra. (12) Application ofAble to withstand dissolution when exposed to urine at about pH 4.5 to about pH 8 at about 37° C. for about the first 12 hours; (13) Allows the urethra to be unobstructed and urine passage unimpeded with any dressing or dressing residue present (with or without a delivery device in situ); (14) Provides protection to the injury site and promotes healing; and (15) Provides controlled, slow degradation and / or dissolution from the attachment site (bladder neck, prostate, and / or urethra) allowing removal without surgical aid in less than about 7 days.
[0032] The present invention provides: (1) the ability to rapidly control bleeding in prostatectomy using a non-invasive technique; (2) the ability to control bleeding in patients receiving anticoagulant therapy; (3) significant reduction in patient pain and discomfort by controlling bleeding without the need for long-term catheter use; (4) significant reduction in hospital stays; (5) significant reduction in health care costs; (6) significant reduction in morbidity; and (7) a trend in outcomes toward reduced mortality.
[0033] As used herein, bladder mucosa is broadly defined to include any exposed tissue surface of the bladder, including any tissue surface exposed by an operation (e.g., a surgical procedure). Thus, bladder mucosa includes bladder mucosa naturally present in the bladder, excised bladder mucosa, and excised prostate, among others.
[0034] Chitosan intraluminal hemostatic dressing (CEHD), as used herein, refers to a chitosan dressing that is hemostatic and can be used in intraluminal areas, such as the inside of the bladder. CEHD is not limited to its location of application and includes chitosan dressings applied to any location inside the human body, including, but not limited to, the bladder mucosa.
[0035] Bleeding rates in ml / min, i.e. blood flow rates, suitable for treatment with the devices described herein may range from about 1 ml / min to about 200 ml / min. In a preferred embodiment, the bleeding rates addressed by the device range from about 1 ml / min to about 150 ml / min. Bleeding rates of about 20 ml / min to 25 ml / min are considered "active" bleeding. Exudative bleeding is generally greater than about 1 ml / min. This is because it has been noted that at low bleeding rates, such as 1 ml / min, clots typically form and stop spontaneously unless the subject is on anticoagulant therapy or has a disorder of the clotting cascade for reasons other than taking anticoagulant medication. For such subjects who are receiving irreversible anticoagulant medications or have bleeding disorders, exudative bleeding at 1 ml / min remains a concern and needs to be addressed, such as by devices formed from the materials of the present invention. In some embodiments, the devices described herein are used to address TURP bleeding rates of about 1 ml / min to about 25 ml / min, or about 1 ml / min to about 20 ml / min, or about 1 ml / min to about 15 ml / min, or about 1 ml / min to about 10 ml / min, or about 1 ml / min to about 5 ml / min.
[0036] A TURP delivery device can include any device used in or in connection with a TURP procedure.
[0037] Chitosan Dressing Chitosan dressings may refer to compositions containing various amounts of chitosan.The general content, general chemical composition, and various forms of chitosan dressings are described, for example, in U.S. Patent Nos. 7,820,872, 7,482,503, 7,371,403, 8,313,474, 7,897,832, 9,004,918, 8,920,514, 9,204,957, 8,741,335, 8,269,058, 9,205,170, and 10,086,105.Such chitosan dressings have been used to stop bleeding due to their chemical and physical properties as already described.
[0038] The chitosan used preferably comprises a non-mammalian material, poly[β-(1→4)-2-amino-2-deoxy-D-glucopyranose. Chitosan can be processed in a conventional manner from chitin obtained, for example, from the shells of animal crustaceans such as shrimp. Chitosan can be biocompatible and biodegradable in the body, and can break down into glucosamine, a harmless material. Catechol-modified chitosan as used herein can include reference to catechol-added chitosan.
[0039] Chitosan dressings may be dry or wet. A chitosan dressing is "dry" if it has a moisture content of less than about 15% by weight, preferably less than about 10% by weight, more preferably less than about 5% by weight. A chitosan dressing is "wet" if it has been in contact with a source of water, including water in physiological environments and biological fluids, or water in aqueous solutions. For example, a chitosan dressing described in this disclosure becomes wet if it is in contact with gastrointestinal fluids, urine, or blood, or with a tissue surface of the gastrointestinal tract or bladder (bladder mucosa or GI mucosa). A chitosan dressing that remains in a substantially solid form absorbs, replaces, redirects, or directs water / moisture in the physiological environment of the gastrointestinal tract or bladder mucosa in an amount sufficient to allow the chitosan dressing to adhere to the tissue surface. The adhered chitosan dressing can be used to seal wound surfaces and slow or stop further bleeding.
[0040] In a preferred embodiment, the chitosan gastrointestinal hemostatic dressing (CGHD) or chitosan intraluminal hemostatic dressing (CEHD) formed from the material of the present invention preferably comprises greater than or equal to 25% by weight of chitosan, more preferably greater than or equal to 50% by weight of chitosan, and most preferably greater than or equal to 75% by weight of chitosan. Chitosan is a common name used to describe linear polysaccharides (typically the number of glucosamines is equal to or greater than the number of N-acetylglucosamines) that are linked by β-(1-4) glycosidic linkages, the composition being soluble in dilute aqueous acid (Roberts 1991). The chitosan family includes poly-β-(1-4)-N-acetylglucosamine and poly-β-(1-4)-N-glucosamine with fractional acetyl residues, whose motif modification (random or block) affects the chemistry of chitosan. The C-2 amino group of the glucosamine ring of chitosan can be protonated, thus allowing the solubilization of chitosan in water (pKa approx. 6.5) (Roberts 1991).Other hydrophilic polymers such as guar, pectin, starch, and polyacrylic acid may also be used.
[0041] In preferred embodiments of CGHD, the dressings formed from the materials of the invention are polymeric, thin (preferably less than about 500 microns thick when dried, more preferably less than about 200 microns thick, and most preferably less than about 100 microns thick), flexible, porous, dry, biocompatible, tissue-adherent, and hemostatic.
[0042] In preferred embodiments of CEHD, the dressings formed from the materials of the invention are polymeric, thin (preferably having a dry dressing thickness of about 500 microns or less, more preferably about 200 microns or less or about 100 microns or less, and most preferably about 150 microns or less in thickness), flexible, porous, dry, biocompatible, tissue-adherent, and hemostatic.
[0043] In some embodiments, the dressing is about 100 microns thick and may include a two-layer dressing with two layers of about 70 microns (one adhesive, dissolution resistant layer and one layer of chitosan only) for a total thickness approaching 150 microns upon delivery.
[0044] The shape of the dressing is not limited, but a square, rectangular, circular, or circular petal shaped dressing is preferred. In one embodiment, the maximum size may be up to about 50mm x 50mm square or 50mm diameter. In another embodiment, the size of the dressing may be about 45mm x 45mm square or 45mm diameter, 40mm x 40mm square or 40mm diameter, 35mm x 35mm square or 35mm diameter, 30mm x 30mm square or 30mm diameter, 25mm x 25mm square or 25mm diameter, 15mm x 15mm square or 15mm diameter, 10mm x 10mm square or 10mm diameter, etc. In yet another embodiment, the length and width each may range from about 10mm to about 50mm, or from about 10mm to about 50mm diameter. Larger dressing sizes are more often subject to delivery limitations in confined cavities.
[0045] In another preferred embodiment, the coating is delivered by a balloon catheter, the coating having a diameter size of about 5 cm or up to 7 cm. The balloon catheter preferably passes through a small hole in the center of the coating (approximately the same diameter as the catheter balloon, which is generally about 4 mm to about 7 mm in diameter, or the hole can be larger, for example up to 12 mm), and the coating (30 mm to 70 mm in coating diameter) is attached to the catheter tube (same diameter as the catheter) on the other side of the balloon by small coating tabs on either side of the hole. In some embodiments, the change in surface area of the coating from a folded, rolled, or compressed state is about one-eighth of the surface area when the coating is in an unfolded, unrolled, or uncompressed state. The coatings described herein may provide a large coating surface area in an open, unrolled, or unfolded state. Alternatively, the coatings described herein may provide a small coating surface area in a closed, rolled, or folded state. The dressing can be folded, rolled, or closed so that it can be more compacted and protected for delivery, reducing the likelihood that the surface of the dressing will become prematurely wetted prior to delivery to the target tissue treatment site.
[0046] In a preferred embodiment of the CGHD, the dressing is about 50 microns thick, has a diameter of about 2.5 cm, and measures about 9.856 cm when unfolded, unrolled, or unfolded. 2 Inside the delivery device sheath (typical fluorinated ethylene propylene (FEP) delivery tubing has a wall thickness of about 150 microns), the closed, rolled, or folded dressing (within a 1.25 cm long cylinder) will have an outwardly facing surface area of about 2.07 cm inside the 0.45 cm diameter channel of the gastroscope. 2 or approximately 1.56 cm in the 0.32 cm diameter channel of a gastroscope. 2 or approximately 1.41 cm in the 0.28 cm diameter channel of a gastroscope. 2Thus, in one example, a dressing of the present invention may have an outward cylindrical surface area in an open, unrolled, or unfolded state that is about 6 times, about 5 times, or about 4 times the outward surface area of the same dressing when in a closed, rolled, or folded state. In some embodiments, the ratio of the outward surface area of the open, unrolled, or unfolded dressing to the closed, rolled, or folded dressing is about 15:1, or about 14:1, or about 13:1, or about 12:1, or about 11:1, or about 10:1, or about 9:1, or about 8:1, or about 7:1, or about 6:1, or about 5:1, or about 4:1, or about 3:1, or about 2:1.
[0047] In some CGHD embodiments, the most common gastroscope channel diameter is 0.28 cm (2.8 mm), and therefore this is the most preferred size for coating delivery. Alternatively, a more preferred size is 0.32 cm diameter, which is a standard gastroscope channel diameter, but is less common than the 0.28 cm channel. Another preferred gastroscope channel diameter size is 0.45 cm to 0.32 cm, which is a custom gastroscope channel size, and therefore is less common than the 0.32 cm or 0.28 cm gastroscope channel diameter sizes.
[0048] In a preferred embodiment of the CEHD, the dressing is about 100 microns thick, has a diameter of about 5.0 cm, and measures about 38.66 cm when unfolded, unrolled, or unfolded. 2 On a balloon delivery device, the closed, rolled, or folded covering (in a 2.5 cm long cylinder) will have an outward facing surface area of approximately 5.09 cm on a 7 mm diameter catheter balloon, assuming a covering diameter of 3.0 cm. 2 or approximately 14.0 cm when opened in a 4 mm diameter catheter balloon 2 , 1.85cm when closed 2Thus, in one example, a dressing of the present invention may have an outward cylindrical surface area in an open, unrolled, or unfolded state that is about 8 times the outward surface area of the same dressing when in a closed, rolled, or folded state. In some embodiments, the ratio of the outward surface area of the open, unrolled, or unfolded dressing to the closed, rolled, or folded dressing is about 15:1, or about 14:1, or about 13:1, or about 12:1, or about 11:1, or about 10:1, or about 9:1, or about 8:1, or about 7:1, or about 6:1, or about 5:1, or about 4:1, or about 3:1, or about 2:1.
[0049] In some CEHD embodiments, the most common catheter balloon diameter used with delivery devices in TURP is 0.4 cm (4.0 mm), and therefore this is the most preferred size for dressing delivery. Alternatively, a more preferred size is 0.5 cm in diameter, which is the standard catheter diameter for TURP delivery devices, but is less common than 0.4 cm catheters. Another preferred catheter diameter size for TURP delivery devices is 0.5 cm to 0.7 cm, which is a custom channel size, and therefore is less common than 0.4 or 0.5 cm catheter diameter sizes.
[0050] The dressings described herein can be folded and unfolded, and preferably are applied of More preferably, for the first 6 hours of application of First 12 hours, most preferably applied of It does not dissolve readily in body fluids such as blood or GI fluid or urine at about 37° C. within the first 24 hours, but degrades and / or dissolves completely within about 7 days upon contact with GI fluid or bladder fluid at about 37° C.
[0051] The coating described herein does not adhere to the delivery device and does not appreciably swell or shrink, i.e., it does not increase or decrease in size by more than about 25% in length and width, or more than about 50% in thickness, in the presence of blood and bodily fluids (GI fluids or urine or bladder fluids or mixtures thereof) at about 37°C.
[0052] In a preferred embodiment, the dressing may be heat sterilized without affecting the characteristics of the dressing, and when stored in its packaging under controlled conditions at room temperature of about 21° C. to about 25° C., its tissue adhesion, mechanical properties, solubility in GI or bladder fluids, swelling properties, and hemostatic properties are stable and do not appreciably change over time (e.g., up to about 2 years).
[0053] In a preferred embodiment, the dressing has a tissue-adherent side and a non-adherent side, in which the non-adherent side may provide a surface that, when moistened, easily slides off of itself and off the surface of any applicator or delivery device that pressurizes the dressing into the lumen and / or in the gastrointestinal tract or bladder.
[0054] A preferred embodiment of the coating is that it is formed from a substantially dry chitosan composition having a moisture content of about 15% or less, or about 8% or less. The dried chitosan composition is preferably formed using phase separation and drying of an aqueous solution of chitosan and water. The dried chitosan coating is preferably prepared in sheet form that can be cut to size.
[0055] Preferred embodiments of the biocompatible, biodissolvable, tissue-adherent chitosan dressings include materials and material structures that are capable of withstanding dissolution in gastrointestinal (GI) fluids and blood for at least about 6 hours at about 37° C. and promote resistance to rapid dissolution and degradation in the low pH and strong enzymatic digestive fluids of the upper GI tract. This is a significant advantage of the chitosan dressings disclosed herein, as the upper GI tract has evolved to rapidly digest most organic materials, such as chitosan, cellulose, and starch.
[0056] Preferred embodiments of the biocompatible, biodissolvable, tissue-adherent chitosan coating include materials and material structures that are capable of withstanding dissolution in bladder fluid and blood for at least about 6 hours at about 37° C. and promote resistance to rapid dissolution and degradation in urine within the bladder, which are significant advantages of the chitosan coatings disclosed herein.
[0057] The chitosan dressings provided herein can be applied with light pressure, i.e., pressures up to several hundred KPa, to mucosal surfaces, for example in the GI or bladder. As used herein, light pressure applied to a dressing on a tissue surface refers to a pressure that allows the chitosan dressing to adhere to and remain in contact with the injury site without significant deformation or movement of the tissue, thereby allowing the chitosan dressing, by virtue of its compositional structure and characteristics, to interact with the injury site to promote adhesion and stop bleeding. In some embodiments, light pressure is most preferably a pressure of about 10 kPa or less, more preferably 25 kPa or less, or preferably 50 kPa or less (100 g / cm 2 (Note that =9.8 kPa). Typically, soft tissues such as the stomach undergo significant deformation when loaded above 100 kPa, making it impossible to compress them without applying opposing pressure to support them. A review of the elastic modulus of the human stomach is provided in Saraf et al. 2007. Saraf, H. et al., Mechanical properties of soft human tissues under dynamic loading, J. OF BIOMECHANICS, 40(9), pp. 1960-1967 (2007).
[0058] Preparation of chitosan coating The chitosan coating of the present invention can be produced using various methods and processes. In some embodiments, the chitosan coating can be formed by freezing phase separation and drying. In an alternative embodiment, the coating is formed by the addition of a foaming agent to provide a low density foam prior to freezing and subsequent drying. Freezing phase separation followed by removal of the frozen solvent by sublimation is referred to as freeze-drying. Freezing phase separation is a process of solidification from a dilute solution in which the removal of heat through the surface of a container or mold holding the dilute solution and the resulting reduction in temperature results in localized solid crystal nucleation of the pure solvent and subsequent propagation and growth of the pure solvent crystals. Growth of pure solvent crystals in a dilute solution results in solute diffusing from the growing crystal front and solidifying in the interstices of the growing crystals. Freezing phase separation of a dilute aqueous polymer solution results in alternating layers of thin polymer lamellae between thick layers of ice. If the ice is removed by a method that does not destroy the polymer lamellae, a low density polymer coating with an interconnected porous structure is obtained. For example, in one embodiment, the low density polymer coating has a density of about 0.005 g / cm 3 ~about 0.05g / cm 3 The coating may have an initial coating density of
[0059] In an alternative embodiment, the frozen phase separated coating is formed by freezing a foamed dilute solution and subsequent drying. In an alternative embodiment, the coating is formed by a non-woven fiber spinning process such as centrifugal spinning, electrospinning, or solvent fiber extrusion into a coagulation bath. In yet another alternative embodiment, the dry coating formed from the material of the present invention can be formed from a woven fiber forming process. In yet another alternative embodiment, the dry coating formed from the material of the present invention can be formed by phase inversion and precipitation with a non-solvent (typically used to manufacture dialysis and filtration membranes). In yet another alternative embodiment, the coating formed from the material of the present invention can be formed by an additive 3D printing process.
[0060] In a preferred embodiment formed from the materials of the present invention, the coating preparation process results in an initial coating density in the initial preferred range of about 0.005 g / cm3 ~about 0.05g / cm 3 to the final preferred range of about 0.03 g / cm 3 ~about 0.7g / cm 3 However, the compression process may change the thickness to about 0.08 g / cm 3 ~Approx. 1.2g / cm 3 A range of about 1.5 g / cm is also contemplated. 3 It is noted that the density of is that of a non-porous chitosan dressing. The compression process may include application of a temperature ranging from about 20° C. to about 150° C. To avoid substantial dressing swelling upon contact of the compressed and dried dressing with biological fluids, the temperature of compression is preferably applied by methods that may include, but are not limited to, convection, conduction, and radiation, and the temperature of the compressed dressing should preferably be maintained at at least about 80° C. for at least about 15 seconds.
[0061] The heat during compression is a means that allows the chitosan to be plasticized and shaped without cracking or splitting (non-destructive shaping). The first glass transition temperature (Tg) of pure dry chitosan is around 80°C, which allows for the annealing of some of the crystallinity of its structure, which facilitates non-destructive shaping of chitosan when processing pure dry chitosan. It is possible to apply plasticizers such as water or glycerol to chitosan to lower the Tg, thereby achieving a similar level of non-destructive shaping at lower temperatures. It is noted here that chitosan can be non-destructively shaped in the range of 20°C to 150°C. Outside this range it is possible to shape chitosan non-destructively, but it becomes much more difficult. Above 150°C, thermal decomposition of chitosan begins, and below 20°C, the addition of plasticizers can cause an undesirable loss of the crystallinity of chitosan that provides resistance to dissolution as well as resistance to decomposition processes such as those that occur during sterilization.
[0062] Preferably, the compression prevents substantial swelling of the compressed and dried dressing upon contact with biological fluids and is performed such that the moisture content of the dried dressing during compression is about 15% w / w or less. Compression may be applied by double or multiple roller compression and / or uniaxially between adjacent platens.
[0063] Compression may be performed against a uniform flat or curved surface to provide a smooth finish to the compressed coating.
[0064] Alternatively, compression may be applied to surfaces that have been etched, machined, cut, or otherwise treated to provide missing or added surface texture. The surface texture may be random or in a regular repeating pattern. The surface pattern may aid in the folding and unfolding or rolling and unfolding of the dressing, giving it a hinge-like property. Such texture may be used as an aid to quickly lock the dressing in place and prevent it from moving when applied. Movement of the dressing surface during positioning on the target tissue surface may cause the formation of a film and therefore closure of open surface structures that may result in loss of ability to remove adhesion-inhibiting biological fluids at the surface and therefore loss of ability to adhere the dressing to the surface. The timescale of the changes that occur at the dressing surface is critical, and uptake of liquids at the surface with significant closure of surface dressing channels is highly undesirable. A good way to avoid such movement is to physically lock the dressing in place as soon as it contacts the tissue surface.
[0065] Prior to the present invention, thin, solid chitosan dressings were generally stiff and not flexible enough to bend, fold, or roll without breaking, shattering, or otherwise losing its original shape or otherwise becoming unsuitable for use. The chitosan dressings provided herein, due to their compositional structure and characteristics, can be folded and unfolded along the folding axis and still remain intact and suitable for use in stopping bleeding. Interestingly, and unexpectedly, it has been found that the chitosan dressings described herein, when folded, are less resistant to tearing or breaking along the folding lines. In some embodiments, the chitosan dressings provided herein, due to their compositional structure and characteristics, can be rolled without losing its compositional structure and characteristics and still remain intact and suitable for use in stopping bleeding.
[0066] In some embodiments of CGHD, the chitosan dressing provided herein, due to its compositional structure and characteristics, can be wrapped without losing its compositional structure and characteristics and still remain unchanged to stop bleeding.Thus, in some embodiments, the chitosan dressing provided herein can be delivered through a narrow working channel and still maintain its compositional structure and characteristics unchanged. Exemplary diameters of the narrow working channel through which the chitosan coatings provided herein can be delivered include diameters of about 3.2 mm or less, and such as, but not limited to, 0.1 mm, 0.2 mm, 0.3 mm, 0.4 mm, 0.5 mm, 0.6 mm, 0.7 mm, 0.8 mm, 0.9 mm, 1.0 mm, 1.1 mm, 1.2 mm, 1.3 mm, 1.4 mm, 1.5 mm, 1.6 mm, 1.7 mm, 1.8 mm, 1.9 mm, 2.0 mm, 2.1 mm, 2.2 mm, 2.3 mm, 2.4 mm, 2.5 mm, 2.6 mm, 2.7 mm, 2.8 mm, 2.9 mm, 3.0 mm, 3.1 mm, and 3.2 mm.
[0067] In some embodiments of CEHD, the chitosan dressing provided herein can be rolled without losing its compositional structure and characteristics and still stop bleeding unchanged due to its compositional structure and characteristics.Thus, in some embodiments, the chitosan dressing provided herein can be delivered by a balloon catheter along the urethra and still maintain its compositional structure and characteristics unchanged.Exemplary diameters of the balloon catheter supporting the chitosan dressing can include diameters of about 12mm or less, and include, but are not limited to, 3mm, 3.5mm, 4.0mm, 4.5mm, 5.0mm, 5.5mm, 6.0mm, 6.5mm, 7.0mm, 7.5mm, 8.0mm, 8.5mm, 9.0mm, 9.5mm, 10.0mm, 10.5mm, 11.0mm, 11.5mm, and 12.0mm.
[0068] Catechol-modified chitosan and its preparation The chitosan coatings described herein relate to chitosan coatings that include catechol-modified chitosan and / or hydrophilic polymers. Other aspects of chitosan coatings that include catechol-modified chitosan are described in more detail below.
[0069] Preferred embodiments of the CGHD or CEHD of the present disclosure include compositions comprising catechol-modified chitosan and / or other hydrophilic polymers as required. Preferably, the catechol-modified chitosan in the dressing adheres long term to wet tissue with a tissue adhesion of about 1 kPa or greater and resists dissolution in water, saline solution, blood and / or GI or bladder fluids at about 37° C. for about 6 hours or greater. Preferably, the catechol-modified chitosan is formed by N-acylation of the C-2 amine of the glucosamine of chitosan with 3,4-dihydroxyhydrocinnamic acid (also known as 3-(3,4-dihydroxyphenyl)propionic acid, hydrocaffeic acid). Alternatively, N-acylation of chitosan to produce catechol modified chitosan may include modification with one of, but not limited to, 3,4-dihydroxycinnamic acid (caffeic acid), trans-3,4-dihydroxycinnamic acid (trans-caffeic acid), and 3,4-dihydroxyphenylacetic acid (DOPAC, homoprotocatechuic acid).
[0070] The presence of catechol in the composition results in a polyconjugate structure, since catechol is oxidized to o-quinone. This results in a visible difference between the unmodified chitosan composition and the catechol-modified chitosan composition, which can be off-white or pink to dark brown in color, respectively. It is noted that the catechol-modified chitosan composition is pink to brown when oxidation of catechol occurs.
[0071] Pink coloring of the catechol modified chitosan, meaning substantially no crosslinking, is obtained in the aqueous synthesis by maintaining the pH of the reaction solution at or below 5.5. Pink coloring can also be obtained in the aqueous synthesis by performing the modification and subsequent process steps in the substantial absence of oxygen, such as by using an aqueous system purged with an inert gas, which may include, but is not limited to, argon or nitrogen. Although pink coloring is undesirable in the final solution or catechol modified product, it may be desirable in intermediate processing steps (such as immediately after derivatization of chitosan with catechol and / or subsequent dialysis and / or washing of the catechol chitosan solution to remove residual unreacted materials). This allows for the storage of a stable dry product polymer and the determination of the weight of the dry product with the subsequent ability to subsequently redissolve the pure dry catechol modified product in water to the desired dry weight. This water-soluble chitosan catechol material is then oxidized and crosslinked (brown coloring). However, catechol-modified chitosan dried prior to oxidation is not suitable for use in chitosan dressings formed from the materials of the present invention because dressings containing catechol-modified chitosan so treated do not readily redissolve and the final solution contains an undesirably large fraction (greater than 5% w / w) of insoluble particles (greater than 10 microns in diameter). Furthermore, catechol-chitosan prepared after an intermediate freeze-drying step is more prone to premature dissolution in gastrointestinal fluids or the bladder. Excessive cross-linking (i.e., brown color) in TURP is less desirable because it results in longer dissolution times in urine, e.g., greater than 168 hours when the target complete dissolution is from about 72 hours to about 168 hours.
[0072] In a preferred embodiment, the catechol modified chitosan is not removed from the solution with an intermediate drying step to allow storage, but rather is kept in the aqueous solution and oxidized in the aqueous solution by exposure to a pH above about pH 5.5 in the presence of atmospheric oxygen. A preferred pH control is achieved by adjusting the partial pressure of carbon dioxide dissolved in the water (increasing the partial pressure decreases the pH, decreasing the partial pressure increases the pH to near pH 7). An alternative preferred means of pH control is the incremental addition of a strong acid to decrease the pH, and a strong base to increase the pH. Examples of strong acids include, but are not limited to, hydrochloric acid, sulfuric acid, and nitric acid. Examples of strong bases include, but are not limited to, sodium hydroxide and potassium hydroxide. Subsequent drying of this aqueous, water-soluble oxidized catechol modified chitosan results in a preferred level of crosslinking of the catechol chitosan with good resistance to dissolution and degradation in the upper gastrointestinal tract and bladder. The catechol chitosan solution is diluted by the addition of water and concentrated by the removal of water. Water may be removed by techniques such as, but not limited to, ultrafiltration, reverse dialysis, and centrifugation. The solids fraction of a solution may be determined by sampling a known volume from the solution and performing analyses such as, but not limited to, gravimetry, Fourier transform infrared spectroscopy, UV-visible spectroscopy, refractive index methods, and pycnometer methods.
[0073] In a preferred embodiment, the catechol modified chitosan composition is brown due to oxidation of the catechol to o-quinone. The quinone is produced by autoxidation of the hydroxyl group of the catechol in the presence of oxygen and at a pH above about 5.5. Crosslinks are produced in the modified chitosan by a Schiff base reaction of the quinone with the C-2 amine of the chitosan. The color of the catechol modified chitosan composition is controlled by controlling the pH and exposure to oxygen during synthesis. By maintaining the pH at or below about pH 5.5, the production of o-quinone is inhibited. Subsequent conditioning of the dialysate, final washed or dialyzed catechol chitosan solution to a preferred pH range of 5.8 to 6.2 results in a darker, more oxidized catechol that is more resistant to dissolution. In some embodiments, the color of the catechol modified chitosan characterizes one aspect of the catechol modified chitosan coating. In some embodiments, the color reflects the degree of substitution of chitosan by catechol. In some embodiments, the pink to brown coloration correlates with the degree of substitution. Figure 15 shows an exemplary embodiment of different colorations reflecting and correlating with different degrees of substitution of chitosan with catechol.
[0074] To prepare a dried coating from catechol chitosan, a preferred light to dark brown aqueous catechol chitosan solution is prepared, which may be used by itself or mixed with other aqueous hydrophilic polymer solutions, including but not limited to chitosan and / or solutions of hydrophilic polymers as appropriate. Preferably, the dried phase separated catechol chitosan coating is prepared as a dried and densified frozen phase separated and fibrous coating structure.
[0075] Preferred crosslinked catechol-modified chitosan compositions of the present invention provide good tissue adhesion and increased resistance to dissolution in the upper gastrointestinal tract or bladder by 10-fold to 100-fold compared to coatings formed from substantially unmodified chitosan. For example, Figures 6A, 6B, and 6C show dissolution test results demonstrating that chitosan coatings disappear in 15 minutes, while some catechol coatings persist for over 24 hours. The catechol-modified chitosan compositions described herein provide a heretofore unknown durability, biocompatibility, and ultimately the ability to dissolve.
[0076] The preferred rapid adhesion (1 minute or less) of CGHD or CEHD formed from the material of the present invention to the gastrointestinal or bladder mucosa is achieved in the dry chitosan dressing by the presence of an acid in the dry dressing composition promoting the formation of a quaternary ammonium cation at the C-2 amine of the glucosamine of chitosan. Preferred acid salts of chitosan in the dressing may include salts of acetic acid, lactic acid, glycolic acid, citric acid, succinic acid, malic acid, hydrochloric acid, glutamic acid, ascorbic acid, malonic acid, glutaric acid, adipic acid, pimelic acid, and tartaric acid, and combinations thereof. Preferably, the weight percent of the acid salt of chitosan is greater than about 2% and less than about 15%. To achieve rapid adhesion (e.g., 1 minute or less) to wet tissue, the moisture in the dry gastrointestinal or bladder dressing is preferably less than about 15% by weight, more preferably less than about 10% by weight, and most preferably less than about 5% by weight.
[0077] In the case of frozen phase separated dried densified chitosan coatings, the chitosan solution is poured into a frozen phase separated mold (typically in the form of a horizontal flat bottom pan) preferably as about 0.1% w / w, more preferably about 0.5% w / w, and most preferably about 0.25% w / w of hydrophilic polymer chitosan solution. The hydrophilic polymer solution is preferably added to a horizontal flat pan to a vertical depth of preferably about 10 mm, more preferably 2.5 mm, and most preferably 5.0 mm deep in the mold. The solution in the mold is then frozen and dried to remove the water by sublimation or frozen phase displacement (solvent extraction of ice with a non-solvent for the polymer) to produce a low density (greater than 99% void volume), open or porous dry density of about 0.01 g / cm. 3 (or about 0.005 g / cm for uncompressed catechol chitosan coatings from e.g. a 0.5% solution) 3 This is about 0.025g / cm 3 Freeze drying is typically performed at pressures below 300 mTorr, whereas freeze substitution using anhydrous, chilled (e.g. below -20°C) solvents such as ethanol is performed at atmospheric pressure. The dried sponge is then preferably compressed to a density of about 0.4 g / cm 3 The mixture is compressed to a density of greater than about 100 microns and a thickness of less than about 100 microns. Preferred compression is not limited, but can include uniaxial compression between aligned flat platens. The platens are heated to 18° C. to 150° C., and pressures are up to 10,000 bar.
[0078] The preferred compression creates an exceptionally thin (e.g., in the range of about 50 microns or less to about 200 microns or less), strong (e.g., UTS of 5 MPa to 25 MPa), easily foldable chitosan dressing that can be minimally invasively placed anywhere in the body in a limited folded configuration that can be reformed for precise and effective large surface area placement and adhesion without sacrificing the performance of the original unfolded dressing configuration.
[0079] Foldability is addressed in the following examples. In one embodiment, folding testing involves first folding the final compressed circular dressing, flat on the horizontal, 180° counterclockwise edge-to-edge, holding the edges together and compressing tightly at the center of the dressing to create a single linear fold axis (i.e., crease) in the dressing. The folded dressing is then opened and the edge-to-edge fold is recreated along the new fold axis, but in the opposite clockwise direction. Successful folding can be ranked as no visible tears or cracks along the fold axis and no significant loss in the tensile properties of the dressing (determined by gently pulling the dressing across the fold). Figure 15 shows a catechol-modified chitosan dressing that has been folded and opened with no visible change in the fold axis (crease).
[0080] Freezing phase separation of dilute aqueous polymer solutions results in the phase separation of micron and submicron thin polymeric chitosan lamellae regularly sandwiched between sheets of ice crystals close to 200 microns wide. Removal of the ice by sublimation (freeze drying) or alternatively solvent extraction leaves a dry sponge consisting of roughly aligned, thin (1 micron or less) polymeric chitosan lamellae. Compression of the polymeric chitosan lamellae at temperatures close to or above their glass transition temperature (the Tg of dry chitosan is approximately 80° C.) allows compression into a thin (approximately 50 microns) dense polymer structure formed from hundreds of tough, compliant polymeric chitosan lamellae that do not readily propagate cracks and can be repeatedly folded without failure. Superior strength is achieved by stacking such multilayers. Prior to the present invention, high density, frozen phase separated chitosan coatings for manufacture and use as described herein have not previously been discussed that are intended to address the key challenges resolved by the present invention, such as removal of interfering liquids (by absorption, distribution, displacement, and / or redirection), adhesion by ability to form a fold axis, and ability to withstand mechanical disturbances from repeated folding and unfolding along the fold axis.
[0081] In one embodiment, the porosity (>99% pore space) is complete and uninterrupted in the uncompressed dressing with a pore size range of 20-300 microns with a substantial majority of the pores approximately 100-200 microns. The uninterrupted pore structure is demonstrated by the ability of the compressed dressing to absorb biological fluids such as blood.
[0082] In some embodiments, holes approximately 500 microns in diameter, free of cracks and clean edges, can be formed in the dressing by compression by applying a fine gauge (approximately 500 microns in diameter) sharp-tipped needle locally through the dressing to a flat, hard, resilient surface applied directly against the dressing that can receive and release the tip of the needle. Preferred flat surfaces of receiving supports include, but are not limited to, clean, dry thermoplastic elastomers with a Shore hardness of 55D to 90D. Alternative methods of forming holes can include, but are not limited to, small diameter hole punches (approximately 500 microns) or laser cut holes.
[0083] In some embodiments, the chitosan dressings provided herein have holes in the dressing. In some embodiments, these holes receive fibers or other reinforcing attachment elements. Such reinforcing elements can be formed by simple local application of a reinforcing liquid that bonds locally to the edges of the holes. Reinforcing liquids used in the development of the present invention include cyanoacrylate glues that bind the compressed chitosan lamellae of the dressing together and prevent local delamination and fibrillation of the chitosan at the stress points of the holes. Another embodiment of the reinforcing elements of the holes are plastic or metal micromolded interlocking pieces (soluble in the upper gastrointestinal tract or bladder or alternative areas of internal application) that are placed on one side of the hole and on the other side of the hole and are permanently aligned to support a load through the hole without delamination, fibrillation, or other stress-related failure of the dressing at the hole when a load is applied. In some embodiments, the micromolded pieces may include a part on the delivery device that allows the dressing to be conveniently snap-on attached to the delivery device and snap-off detached from the delivery device.
[0084] As used herein, the term fold axis refers to a portion of a sheet of covering material that represents bending stress and / or memory of a fold in the material, typically localized in a narrow area of high bending stress and shear. A crease in a folded piece of paper is an example of a fold axis.
[0085] In a preferred embodiment, the tissue adhesive component of the dressing is formed from a freeze-phase separated dried chitosan sheet that includes a composition that includes catechol chitosan. In a preferred embodiment, the non-tissue adhesive component of the dressing is formed from a freeze-phase separated dried chitosan sheet that does not include modified chitosan. In a preferred embodiment, both the tissue adhesive and non-tissue adhesive dried sheets have a density of about 0.03 g / cm before compression. 3 The density is approximately 0.4g / cm 3 The final density is equal to or greater than 100 μm.
[0086] To prepare a dressing from both sheets, with the dressing having a tissue-adhesive surface layer and a non-adhesive surface layer, the two sheets are bonded together, for example, by placing one sheet on top of the other and applying sufficient uniform pressure onto the dressings to compress them to a higher density. In a preferred process, the sheet is pressed against the dressing at a density of about 0.03 g / cm of each sheet. 3 The original densities below are approximately 0.30 g / cm of the final density of the coating. 3 In a more preferred process, the density of each sheet mold is increased to about 0.015 g / cm 3 The original densities below are approximately 0.4 g / cm of the final density of the coating. 3 In the most preferred process, the density of each sheet mold is increased to about 0.01 g / cm 3 The original densities below are approximately 0.5 g / cm of the final density of the coating. 3 Once compression is complete, the two compressed sheets are bonded together and cannot be easily peeled one from the other, and the dressing can be handled by folding and rolling without delamination.
[0087] This physical bonding of materials by compressing two or more low density porous materials together to form a final high density two or more layer porous material solves the difficult problem of how to bond such materials together without physical or chemical changes to the individual materials and without the addition of additional binders or adhesives. It is believed that the bonding can be attributed to micro surface collisions and penetration of the coating material through the pores and physical interlocking due to compression of the pores. This physical interlocking of low density frozen phase separated dried sheets is not limited to only two materials or two layers of the same thickness because the interlocking effect is not dependent on laterality or thickness. Thus, a multilayer construction of individual frozen phase separated dried sheets of the same or different materials of the same or different thicknesses can be achieved by combining low density sheets (preferably with a density of 0.05 g / cm3 or less) with low density sheets (preferably with a density of 0.05 g / cm3 or less). 3 (below) and stack the assembly together, density 0.3g / cm 3 Such a final physically bonded assembly is expected to offer the advantages of thin top and bottom surface layers including, but not limited to, adhesive or non-adhesive materials with layers therein providing structural, physical, and chemical elements, etc.
[0088] In some embodiments, the chitosan coating has an adhesive side and a non-adhesive side. In some embodiments, the adhesive side of the chitosan adheres to tissue and absorbs and / or redirects surface moisture. In some embodiments, the non-adhesive side detaches from the delivery device when the chitosan coating is applied to the injury site, and the chitosan coating is moistened. This is in part because the adhesive strength of the chitosan coating to the tissue surface controls the position of the coating upon removal of the coating from the delivery device. Detachment or "easily detached" in a double-sided chitosan coating, as used herein, indicates that the adhesive side is applied to a tissue surface or injury site, and the adhered chitosan coating remains on the tissue surface or injury site upon absorption of moisture, while the non-adhesive side is released from the delivery device, thereby allowing the delivery device to be withdrawn from the injury site without disturbing the position of the chitosan coating on the tissue surface or injury site. In some embodiments, the chitosan coating adheres to the delivery device when dry, thereby allowing the chitosan coating to be delivered to the injury site with the device.
[0089] In one embodiment, the dressing needs to be locally attached to the delivery device. Typically, these local attachment areas are at the tip of the dressing. For example, one design is to provide localized pinpoint attachment to tabs at the tip of the dressing around the periphery of the dressing and no other locations to avoid the risk of the dressing sticking to the delivery sheath, the delivery device, or itself (when rolling / folding). The attachment locations may be designed to weaken when moistened or activated for release by some type of physical release mechanism.
[0090] In one mechanism, the chitosan dressing provided herein can stop bleeding by absorbing, conducting, and / or redirecting hydrophilic and hydrophobic liquids at the injury site. Absorption sufficiently removes water from the injury site, thereby allowing a subsequent hemostatic reaction between the chitosan dressing and tissue at the injury site, which stops bleeding and allows the chitosan dressing to remain attached, thereby sealing the injury site. The porous and dense multi-layer structure of the chitosan dressing provided herein facilitates the absorption, conducting, and / or redirection of water at the injury site, as well as the attachment or adhesion of the chitosan dressing to the injury site.
[0091] The chitosan dressings disclosed herein are biocompatible, and in some embodiments, dissolved residues from a chitosan dressing applied to an injury site in vivo can safely pass through the feeding tube or urethra and be excreted along with other bodily wastes.
[0092] More than one or multiple chitosan dressings may be used or applied sequentially to a tissue treatment or injury site. When more than one chitosan dressing is placed, such dressings may be individually attached to adjacent tissue or injury site areas or may overlap each other to various degrees. Because the chitosan dressings described herein are thin, it is contemplated that multiple chitosan dressings may be used as needed to promote or achieve hemostasis at the injury site, depending on the application.
[0093] In one embodiment, the chitosan coatings overlap one another during application. In such cases, ideally the wet adhesive side of the subsequent coating will adhere to some degree to the wet coating backing of the previous coating. Thus, in one embodiment, the chitosan coating does not have a non-adhesive backing, but rather a weakly wet adhesive backing that provides sufficient adhesion for subsequent placement of overlapping chitosan coatings.
[0094] Delivery Device A delivery device, as used herein, is a device for delivering a chitosan dressing. The delivery device delivers the chitosan dressing to an injury site at various locations within the body of an animal, including humans, pigs, dogs, and others.
[0095] In some embodiments, the delivery device is a minimally invasive device capable of delivering a coating, such as a chitosan coating, in a non-invasive or minimally invasive manner to a physiological site within an animal's body. In some embodiments, the delivery device is a balloon device. In some embodiments, the delivery device is a wire device or a device laser cut from a small diameter cylinder of Nitinol or stainless steel. In some embodiments, the non-invasive or minimally invasive feature of the delivery device is achieved by delivery of the coating, such as a chitosan coating, through a thin catheter or equivalent working channel. In some embodiments of the CGHD, the catheter or equivalent working channel has a diameter of less than 3.2 mm. In other embodiments of the CGHD, the channel of the gastroscope may range in diameter size from 2.8 mm to 4.5 mm. In some embodiments of the CEHD, the balloon catheter or equivalent working channel has a diameter of less than about 7 mm. In other embodiments of the CEHD, the channel of the TURP delivery device may range in diameter size from 5 mm to 7 mm.
[0096] In some CGHD embodiments, the working channel of the catheter or balloon catheter or equivalent has a diameter of less than 3.2 mm. In other CGHD embodiments, the channel of the gastroscope may range in diameter size from 2.8 mm to 4.5 mm.
[0097] In some CEHD embodiments, the working channel of the catheter or balloon catheter or equivalent has a diameter of less than about 7 mm. In other embodiments, the channel of the TURP delivery device may range in size from 5 mm to 7 mm in diameter.
[0098] Exemplary delivery devices include, but are not limited to, balloon devices, balloon catheters, wire devices, cylindrical devices with laser cut ends, indwelling catheters, urethral or suprapubic catheters, external catheters, short-term catheters, and intermittent catheters.
[0099] The delivery device may be an endoscopic device used in various aspects of medical procedures, in some embodiments, the endoscopic device is non-invasive or minimally invasive with a thin catheter or tube or similarly small diameter section of the device.
[0100] The delivery device may be a transluminal or transurethral delivery device, hi some embodiments, the transurethral delivery device is non-invasive or minimally invasive by means of a thin catheter or tube / tube or similarly small diameter section of the device.
[0101] Delivery devices include thin tubes or catheters, or other devices having a similar structure.
[0102] Attaching the Dressing to the Delivery Device CGHD Frozen phase separation coatings are composed of compressed layers of fragile and easily peeled lamellae, requiring special attachment of the coating to wire and laser cut cylindrical delivery devices. Each attachment point of the coating to the delivery device must be able to withstand up to 50-100 g of load when rolling and unrolling the coating. Direct adhesion of the coating to the delivery device (e.g. by cyanoacrylate glue) is not an option for frozen phase separation coatings formed from well dissolved solutions, since the cohesive strength of the surface lamellae is low. One embodiment where this is less of an issue is where catechol chitosan is formed from chitosan dissolved in carbonic acid. In this case, the pure chitosan aqueous gel, precipitated with base prior to dissolving into carbonated chitosan and subsequently washed with water, contains a dispersion of solid chitosan fibers insoluble in carbonic acid (0.2% w / w or more of chitosan), which reinforces the subsequent catechol modified chitosan from the carbonated solution. In addition to this example of chitosan carbonate, where the bulk and surface structure of the frozen phase separated dressing is reinforced with a low fraction of chitosan fibers (0.2%-5% w / w of chitosan), the preferred mode of localized reinforcement and attachment of the dressing to the delivery device in the case of wire delivery is to provide small diameter (approximately 500 micron) through-holes with reinforcing elements in the dressing at the point of attachment to the delivery device.
[0103] Preforming holes in frozen phase separated and dried Dressing sponge is the preferred method of creating receiving holes in uncompressed Dressing sponge. 3Since uncompressed sponges (less than 100 mm thick) peel easily and are extremely fragile and therefore cannot accept the usual drilling approach of applying any load to the sponge, the preferred method of creating holes in these sponges without any damage to the lamellar structure of the sponge is to apply insulating hydrophobic (non-adhesive) rod mandrels to the forming solution (from the top of the solution, through the solution to the other side, in contact with the bottom surface of the mold, preferably through the bottom surface to the bottom of the mold) just before the solution is frozen phase separated. These mandrels are tapered so that they can be easily removed after the frozen phase separated sponge is dried. It is envisioned that such mandrels are made of hard or semi-hard hydrophobic materials that can be machined or shaped. Suitable mandrel materials include, but are not limited to, fluorinated materials, Teflon™ and Kel-F™, and high density polyethylene (HDPE). The diameter of the holes created after removal of the mandrel is designed to allow easy placement of threads in the fragile uncompressed sponge without damaging the sponge. The mandrel may be supported on the mold by being inserted into a suitably sized receiving hole in the bottom surface of the mold. Alternatively, the mandrel may be supported by a sheet of releasable hydrophobic film placed directly on the top surface of the frozen phase separation mold and the casting solution. This film is removed from the frozen phase separation surface leaving the mandrel in place prior to drying when the frozen phase separation solution is dried. Thus, after drying, the preformed hole is ready to receive a tie thread for attaching the dressing to a delivery / placement device. The tie thread is positioned on the sponge prior to compression in a suitable arrangement to take all the forces of rolling, unrolling and delivering the dressing. Low density (0.05 g / cm 3 less than 0.4g / cm 3Compression of the sponge to a depth of 10 mm (exceeding 10 mm) secures the tie threads and any other reinforcing / attachment elements in place. The threads may be glued in place before or after compression of the dressing, or the threads may be used to locally apply a liquid reinforcing element, such as a cyanoacrylate glue, through the holes where the threads were removed after application. An alternative embodiment of forming suitable holes in the uncompressed sponge to take support threads or other types of support elements is by laser hole cutting.
[0104] Holes approximately 500 microns in diameter, free of cracks and with clean edges, can be formed in the dressing by compression by applying a fine gauge (approximately 500 microns in diameter) sharp-tipped needle locally through the dressing to a flat, hard, resilient surface applied directly against the dressing that can receive and release the tip of the needle. Preferred flat surfaces of receiving supports include, but are not limited to, clean, dry thermoplastic elastomers with a Shore hardness of 55D to 90D. Alternative methods of forming holes can include, but are not limited to, small diameter hole punches (approximately 500 microns) or laser cut holes.
[0105] The holes in the dressing can receive fibers or other reinforcing attachment elements. Such reinforcing elements can be formed by simple local application of a reinforcing liquid that bonds locally to the edges of the holes. Reinforcing liquids used in the development of the present invention include cyanoacrylate glues that bind the compressed chitosan lamellae of the dressing together and prevent local delamination and fibrillation of the chitosan at the stress points of the holes. Another embodiment of the reinforcing elements of the holes are micromolded interlocking pieces of plastic or metal (soluble in the upper gastrointestinal tract or alternative areas of internal application) that are placed on one side of the hole and on the other side of the hole and are permanently aligned to support a load through the hole without delamination, fibrillation, or other stress-related failure of the dressing at the hole when a load is applied. It is envisioned that such micromolded pieces may include parts on the delivery device attachment side that allow the dressing to be conveniently snap-on attached to the delivery device and snap-off detached from the delivery device.
[0106] General release of the dressing from the delivery device can be accomplished by several methods, including snap-off detachment. A preferred method of dressing release is by using the delivery device to attach the dressing to fibers that are strong when dry and weak when wet. Such fibers include, but are not limited to, chitosan fibers that have been treated to make them rapidly water soluble. A preferred chitosan fiber is a water soluble multifilament fiber with a strength of over 30 MPa when dry and less than 0.1 MPa when wet.
[0107] CEHD (Attachment of TURP covering material to balloon) In one embodiment, the circular covering is folded once on itself edge-to-edge, then the folded covering (now in half) is folded once more on itself edge-to-edge (now in quarters). When the covering is opened, there are two fold lines passing through the center of the covering. A trace of the catheter's perimeter is drawn in the center of the covering (small center circle). Using the tip of a pair of scissors or other sharp cutting instrument, cut along the intersecting fold lines in the center of the covering to the perimeter drawn on the catheter. Once the fold lines are cut, there are four triangular windows in the center of the covering, i.e., tabs for catheter connection. The catheter can be sewn through the opening in the center of the covering, and the covering tabs can be attached by double-sided adhesive tape or other adhesive method for application, fixing the tabs in the desired position on the catheter, and the entire covering can be set over and against the catheter balloon. The covering tabs are preferably placed on the side of the covering facing away from the catheter balloon over which the covering is folded. Preferably, the adhesive used to attach the tabs to the catheter is water soluble, allowing the covering to be slid off the catheter after pressurization with the balloon catheter (and, if desired, removing the catheter) and left in place.
[0108] Methods of application and treatment The embodiments of the chitosan dressings formed from the materials of the present invention provided in this disclosure can be used to stop bleeding in suitable diseases, conditions, disorders, or acute trauma or injury. In some embodiments, the dry, solid chitosan materials of the present invention can be used to stop bleeding from any wet physiological surface, such as mucous membranes. Exemplary applications include, but are not limited to, gastrointestinal or bladder bleeding, vascular applications, bleeding from internal surgery, bleeding from internal biopsies, other intraluminal applications including internal bleeding after removal of solid organs, and oral, ophthalmic, auditory, or nasal bleeding. Additional applications that may require the addition of water or liquid to promote adhesion of the chitosan dressing to tissue surfaces or injury sites are also contemplated, such as the use of the chitosan dressing on external surfaces.
[0109] The dry, solid chitosan material of the present invention can be used to treat gastrointestinal bleeding, which may include, but is not limited to, bleeding in esophageal varices, bleeding from digestive ulcers, bleeding from duodenal ulcers, bleeding associated with biopsies of the upper and lower gastrointestinal tract, resections of the upper and lower gastrointestinal tract, and lacerations or ruptures in the upper and lower gastrointestinal tract. Other diseases, conditions, disorders, or acute trauma or injuries may include, but are not limited to, internal arterial injuries, internal bleeding from the liver, internal bleeding from the vena cava, injuries to the thoracic cavity, including perforation of the heart and lungs and their blood vessels, and injuries to the abdominal cavity.
[0110] The chitosan materials of the present invention may also be used for the treatment of transurethral prostate resection and / or bladder neck bleeding, which may include, but is not limited to, the treatment of bleeding.
[0111] The chitosan material of the present invention can also be used to protect the injury site following acute internal injury (e.g., occurring during UGIB, TURP, or other minimally invasive procedures, or open surgery) by providing an environment conducive to cellular regeneration before closing the injury site and dissolving or degrading within seven days.
[0112] The chitosan material of the present invention can also be used to deliver and locally adhere to specific target sites for general therapeutic purposes, including delivery of active pharmaceutical and / or biological agents. Such target sites may include, but are not limited to, vascular anastomoses, esophageal varices, digestive ulcers, resected prostate fissures, liver resection and biopsy, kidney resection and biopsy, bladder resection and biopsy, throat resection and biopsy, pancreas resection and biopsy, stomach resection and biopsy, lower gastrointestinal tract resection and biopsy, lung resection and biopsy, and heart resection and biopsy.
[0113] The above various embodiments can be combined to provide further embodiments. All U.S. patents, U.S. patent application publications, U.S. patent applications, foreign patents, foreign patent applications, and non-patent publications mentioned herein and / or listed in the Application Data Sheet, including but not limited to U.S. Provisional Patent Application Nos. 62 / 612,013 and 62 / 631,290, are incorporated herein by reference in their entirety. Aspects of the present embodiment can be modified as necessary to employ concepts from various patents, applications, and publications to provide further embodiments.
[0114] These and other changes can be made to the present embodiments in light of the above detailed description. Generally, in the following claims, the terms used should not be construed to limit the claims to the specific embodiments disclosed in the specification and claims, but rather to include all possible embodiments along with the full scope of equivalents to which such claims are entitled. Accordingly, the claims are not limited by this disclosure. EXAMPLES
[0115] Examples 1-6 represent CEHD chitosan dressings.
[0116] The following materials and preparations were considered in the chitosan intraluminal hemostatic dressing invention process. Chitosan A: Primex, ChitoClear 65010, TM 4375, MW=250-300kDa, Brookfield Chitosan B: Primex, ChitoClear 43000, TM 4167, MW = 110-150 kDa, Brookfield viscosity of 1.0% w / w chitosan solution in 1.0% acetic acid at 25°C and spindle LV1 = 9 cPs, DDA = 95% (by colloid titration) Glacial Acetic Acid: Fisher Scientific, Catalog No. A38-212 Hydrochloric acid: 1.0 M in water, Sigma Aldrich, Catalog No. H9892 L-Lactic Acid: JT Baker, Catalog No. 0196-01 Glycolic Acid: JT Baker, Catalog No. M821-05 Sodium hydroxide: 5.0M NaOH in water, Sigma Aldrich, Catalog No. S8263-150ml Potassium hydroxide: 0.1 M KOH in methanol (BDH) Ethanol: 200° proof Sigma Aldrich, Catalog No. 459844-1L Acetic anhydride: Obtained from Sigman Aldrich, ACS reagent grade, catalog number 320102-1L 3,4-Dihydroxyhydrocinnamic acid (hydrocaffeic acid): 98% Sigma Aldrich, Cat. No. 102601 3,4-Dihydroxycinnamic acid (caffeic acid): 98% Sigma Aldrich, Cat. No. C0625 trans-3,4-Dihydroxycinnamic acid (trans-caffeic acid): Sigma Aldrich, Cat. No. 51868 3,4-Dihydroxyphenylacetic acid (DOPAC, homoprotocatechuic acid): 98% Sigma Aldrich, Cat. No. 850217 1-Ethyl-3-(-3-dimethylamino-propyl)-carbodiimide: (alternatively N-(3-dimethylaminopropyl)-N'-ethylcarbodiimide hydrochloride, commonly acronym EDC) Sigma Aldrich, catalog # E7750 N-Acetyl-L-Cysteine: Sigma Aldrich, Catalog No. A7250 Sodium chloride: Sigma Aldrich, Cat. No. 793566-500g Glycerol: Sigma Aldrich, Cat. No. G-8773 Polyethylene glycol: Spectrum, Catalog No. PO108 Polyethylene oxide: Mw 400,000 da, Sigma Aldrich, Catalog No. 372773-500G Poloxamer 407: Spectrum, Catalog No. P1166 Sucrose: Sigma, Cat. No. S3929 D-Sorbitol: Sigma, catalog S1876 Hydroxypropyl cellulose (HPC): Aldrich, Catalog No. 191892 Hydroxyethyl cellulose (HEC): Aldrich, Catalog No. 308633 Synthetic urine formulation: Calcium chloride dihydrate Sigma, Catalog No. C5080 (1.30 g); Magnesium chloride hexahydrate Sigma, Catalog No. M2670 (1.30 g); Sodium chloride Sigma, Catalog No. 793566 (9.20 g); Sodium sulfate Aldrich, Catalog No. 238597 (4.60 g); Sodium citrate dihydrate Sigma, Catalog No. S4641 (1.30 g); Sodium oxalate Sigma, Catalog No. 71800 (0. Add 0.04 g); Potassium dihydrogen orthophosphate Sigma, Catalog No. P5655 (5.60 g); Potassium chloride Fisher, Catalog No. BP366 (3.20 g); Ammonium chloride Sigma, Catalog No. 09718 (2.00 g); Urea Sigma, Catalog No. U1250 (50.00 g); Creatinine Acros, Catalog No. 228940500 (2.20 g) to a 2.0 L volumetric flask and add 1.5 L of deionized water to dissolve. After the ingredients have dissolved in the water and the temperature of the solution has equilibrated to room temperature, add deionized water up to the 2.0 L mark. Pig bladder with urethra: Animal Biotech Industries Inc. (Danboro, PA 18916) Pig small intestine casing: Butcher and Packer (29 / 32mm) (Madison Heights, MI 48071) Citrated bovine whole blood: Lampire Biological Laboratory Bovine CPD, Catalog No. 7720010 Cyanoacrylate A: Permabond 910 Tissue Adhesive, Catalog No. 72590 Cyanoacrylate B: Loctite 4902 instant adhesive, catalog no. 1875841 Dialysis tubing: 3,500Da MWCO Snakeskin dialysis tubing (Fisher Scientific), catalog no. PI88244 Parafilm: "M" Laboratory film, Pechiney plastic packaging (Chicago, IL 60631) Adhesive: Double-sided 3M, Catalog No. 21200-46144-6 (St Paul, MN 55144) Scotch Fine Line Tape 218:3M, Catalog No. 70-0060-4397-3 (St Paul, MN 55144)
[0117] Example 1 Preparation and characterization of catechol chitosan The synthesis of catechol chitosan is the N-acylation reaction of a catechol molecule containing a terminal carboxylic acid with the C-2 amine of the glucosamine mer of chitosan (see FIG. 7). The reaction is carried out in dilute aqueous solution at room temperature with pH control. Figures 12A and 12B show some examples of catechol modified formulations used in the preparation of the present invention. Column 1 of FIG. 12B shows a list of the formulations of the dressings. The formulations of the formulations are shown in column 2 of FIG. 12B. The formulations of catechol chitosan have the acronym "Cs-Cat". The formulation number of Cs-Cat is shown immediately after "Cs-Cat" and written as "Cs-Cat,XX", where XX is the numerical designation of the formulation number of catechol chitosan. Chitosan solutions are prepared and typically written as "chitosan" or "Cs" along with the acid (lactic or acetic acid) used to obtain the aqueous solution. HPMC is hydroxypropyl methylcellulose. HPC is hydroxypropyl cellulose and HEC is hydroxyethyl cellulose. The chitosan lots are listed in column 3. The degree of catechol substitution of chitosan (column 4 of Figure 12B) was determined as follows. A quartz UV test cell (path length 1 cm, ×2 (HACH Co., Cat. No. 48228-00) was used to obtain the UV / Vis spectrum. The UV / Vis spectrometer was a Varian Cary Bio100. Standard solutions of 3,4-dihydroxyhydrocinnamic acid in water were prepared and the absorbance at 280 nm was plotted against the concentration. The extinction coefficient ε in the Beer Lambert relationship for absorbance in dilute solutions is given below: A = ε c l (A is the absorbance (dimensionless) and l is the optical path length.)
[0118] (absorbance < 0.5) was determined as 2,540 ± 50 liters / (mol·cm). This value was used to determine the degree of substitution in dilute aqueous solutions of modified chitosan with known amounts, known volumes of solution, and the peak absorbance measured at 280 nm.
[0119] The chitosan catechol solution is diluted (usually about 50 or 100 times) so that its absorbance at 280 nm is less than 0.5. Using the absorbance, the weight of the solution used for dilution, and the percent solids (CS-catechol), the formula
number
[0120] The percentage of solute (primarily hydrophilic polymer) in solution is shown in column 5 of FIG. 12B. The depth of the solution poured into the flat well mold for freezing phase separation is shown in column 6 of FIG. 12B. Since the pour depth remains substantially unchanged upon freezing, after freeze drying the pour depth provides a useful indication of the amount of change due to compression when referenced to the final set of compressed dressings (shown in column 7 of FIG. 12B). The final density of the compressed and dried dressings is shown in column 8 of FIG. 12B. Column 9 of FIG. 12B provides additional information regarding the dressing preparations, if any. It is interesting to note that dressing preparations 71, 79, 80, 83, 84, and 85 were all performed with co-compression of a non-catechol chitosan dressing, whereas dressing 17 preparation was highly dried. All of these non-catechol chitosan dressings used as backings were formed from a 5 mm pour of 43000 0.5% w / w chitosan acetate solution.
[0121] Examples of catechol chitosan synthesis are illustrated in the six approach variations provided below.
[0122] Approach 1 CS-Catechol, batch 15: Chitosan (1.51 g) was dissolved in deionized water (140 g) with 1.0 M HCl (5 mL). A 1:1 v / v solution of deionized water and ethanol (145 mL) was prepared. 3,4-Dihydroxyhydrocinnamic acid (HCA, 10.5 mmol) and N-(3-dimethylaminopropyl)-N'-ethylcarbodiimide hydrochloride (EDC, 13.0 mmol) were dissolved in the water / alcohol solution. The water / alcohol solution was then slowly added to the chitosan solution prepared above and the reaction mixture was stirred. The pH of the reaction mixture was maintained at 5.5 using 5.0 M NaOH solution and allowed to react overnight. After overnight reaction, the solution was dialyzed against 5 L of deionized water acidified with one drop of 1.0 M HCl solution for 3 days and against deionized water for 4 hours. The dialysate was changed periodically (at least every 24-48 hours) during dialysis.
[0123] Approach 2 CS-Catechol, batch 22-1: Chitosan (9.03 g) was dissolved in deionized water (126 g) with 1.0 M HCl (30 mL). The pH of the solution was then adjusted to 5.1 using 1.0 M NaOH solution. A 1:1 v / v solution of deionized water and ethanol (150 mL) was prepared and N-(3-dimethylaminopropyl)-N'-ethylcarbodiimide hydrochloride (EDC, 31.3 mmol) was dissolved in the water / alcohol solution. 3,4-Dihydroxyhydrocinnamic acid (HCA, 15.7 mmol) was dissolved in deionized water (15 mL). The HCA solution was then slowly added to the chitosan solution prepared above and the reaction mixture was stirred from above. The EDC solution was then slowly added to the HCA / chitosan solution. The pH of the reaction mixture was maintained at 4.9 using 0.1 N KOH methanol solution. After overnight reaction, the solution was dialyzed against 5 L of deionized water acidified with one drop of 1.0 M HCl solution for 4 days. During dialysis, the dialysate was changed regularly (at least every 24–48 h).
[0124] A portion of the solution isolated after dialysis from CS-catechol, batch 22 was placed in an oven to concentrate the solution. The solution was heated at 80° C. to reduce the volume by approximately one third.
[0125] Approach 3 CS-Catechol, Batch 32 (Prototype A, Acute in vivo I): Chitosan (1.504 g) was dissolved in deionized water (143.5 g) along with 1.0 M HCl solution (5.0 mL). The pH of the solution was then raised to 5.5 with 1.0 M NaOH solution. A 1:1 v / v solution of deionized water and ethanol (150 mL) was prepared and N-(3-dimethylaminopropyl)-N'-ethylcarbodiimide hydrochloride (EDC, 2.93 mmol) and 3,4-dihydroxyhydrocinnamic acid (HCA, 10.41 mmol) were dissolved in the water / alcohol solution. The water / alcohol reactant solution was then added slowly to the chitosan chloride solution. During the addition of the reactants to the chitosan solution, the pH was controlled between 4.9 and 5.5 using 1.0 M NaOH solution. After the addition of the reactants, the reaction mixture was monitored for 2-4 hours and the pH was controlled between 5.4 and 5.7 using drops of 1.0 M HCl and 1.0 M NaOH as needed. The pH was then controlled at 5.5 and allowed to react overnight. After overnight (approximately 18-24 hours) reaction, the pH of the chitosan catechol solution was controlled back to 5.5. The chitosan catechol solution was then dialyzed against 5 L of deionized water at approximately pH 5.8 for 5 days and against deionized water at approximately pH 6.1 for 4-24 hours. The dialysate was changed periodically (at least every 24-48 hours) during the dialysis procedure.
[0126] Approach 4 CS-Catechol, Batch 33 Chitosan (0.507 g) was dissolved in deionized water (47.5 g) along with 1.0 M HCl solution (2.0 mL). The pH of the solution was raised to 5.5 using 5.0 M NaOH solution. A 1:1 v / v solution of deionized water and ethanol (50 mL) was prepared and N-(3-dimethylaminopropyl)-N'-ethylcarbodiimide hydrochloride (EDC, 2.94 mmol) and 3,4-dihydroxyhydrocinnamic acid (HCA, 1.49 mmol) were dissolved in the water / alcohol solution (reactant solution). The reactant solution was then slowly added to the chitosan chloride solution. The pH was controlled at 5.4-5.6 for 2.5 hours. The pH was then controlled and lowered to 5.4 and allowed to react overnight (approximately 18-24 hours). The pH of the resulting chitosan catechol solution was controlled at approximately 5.5, and then dialyzed against deionized water at approximately pH 5.8 for 3 days. The dialysate was replaced periodically during the dialysis procedure. After dialysis, the solution in the dialysis tubing was hung in a fume hood overnight to allow excess water that had increased during dialysis to evaporate from the solution. The solution was left to return to its pre-dialysis weight.
[0127] Approach 5 CS-Catechol, Batch 35 Chitosan (1.681 g + 10.6% w / w moisture) was dissolved in deionized water (143.5 g) with 1.0 M HCl solution (11 mL). The pH of the chitosan chloride solution was then raised to approximately 5.5 with 1.0 M NaOH solution. A 1:1 v / v solution of deionized water and ethanol (150 mL) was prepared and N-(3-dimethylaminopropyl)-N'-ethylcarbodiimide hydrochloride (EDC, 8.76 mmol), 3,4-dihydroxyhydrocinnamic acid (HCA, 2.39 mmol), and N-acetyl-L-cysteine (NAC, 2.36 mmol) were dissolved in the water / alcohol solution (reactant solution). The reactant solution was then added to the chitosan chloride solution. During the addition of the reactant solution, the pH of the reaction mixture was controlled at 5.2-5.3. After 2 h, the pH of the reaction mixture was raised to approximately 5.4. The solution was then allowed to react overnight (approximately 18-24 hours). After overnight reaction, the pH of the solution was controlled to approximately 5.5. The solution was dialyzed against 5 L of deionized water for 6 days. The dialysate was changed periodically (at least every 24-48 hours) during the dialysis procedure.
[0128] Approach 6 CS-Catechol, Batch 38 Chitosan (1.678 g + 10.6% w / w moisture) was dissolved in deionized water (143.3 g) with 1.0 M HCl solution (8 g). The pH of the chitosan chloride solution was then raised to approximately 5.5 with 1.0 M NaOH solution. A 1:1 v / v solution of deionized water and ethanol (150 mL) was prepared and N-(3-dimethylaminopropyl)-N'-ethylcarbodiimide hydrochloride (EDC, 2.95 mmol), 3,4-dihydroxyhydrocinnamic acid (HCA, 1.475 mmol) were dissolved in the water / alcohol solution (reactant solution). The reactant solution was then added to the chitosan chloride solution. The reaction mixture was controlled at around pH 5.5 during the addition of the reactant solution. After 2 hours, the pH of the reaction mixture was adjusted to 5.51. The solution was then allowed to react in a covered beaker at room temperature for 20 hours. After 20 hours, the pH of the solution was 5.54. The solution was divided into three lots of approximately 100 g of solution in dialysis tubing and dialyzed against 5 L of deionized water for 5 days at pH 5.8-5.9 for the first 3 days and pH 6.2 for day 4. The dialysate was changed periodically (every 24 hours) during the dialysis procedure.
[0129] Example 2 Freeze-phase separation hydrophilic polymer coating material Aqueous solutions of hydrophilic polymers were prepared in 500 ml, 1000 ml, or 2000 ml Nalgene LDPE bottles or polypropylene beakers by adding ingredients including, but not limited to, pre-prepared solutions, hydrophilic polymers, water, acid, and additional ingredients. Figure 12B shows the 85 formulation types studied.
[0130] The main problems experienced in formulating for transurethral prostate resection applications with dressings in direct contact with urine were 1) the rapid dissolution of chitosan (generally less than 30 minutes) promoted by urine, 2) blood interference in achieving rapid adhesion of pure catechol-modified chitosan, and 3) susceptibility of the dressing to crack and tear when the formulation was modified to address issues in dissolution and adhesion. The %w / w of the final hydrophilic polymer solution was 0.1% to 4% polymer by weight. The capped bottle and its contents were mixed continuously at room temperature for 12-24 hours using an IKA KS260 orbital shaker or a Wheaton benchtop bottle roller to achieve complete solution homogeneity. The solution in the beaker was mixed with magnetic stirring beads on a magnetic stirrer plate for 12-24 hours at room temperature to achieve solution homogeneity. The beaker was closed from the external environment using parafilm during mixing. The solutions prepared for freeze phase separation were substantially homogenous and clear in the absence of suspending conditions. The catechol chitosan solution had some haze and milky appearance, indicating the presence of some dispersed fine spherical particles of catechol chitosan.
[0131] Chitosan solutions were prepared as frozen phase separation coatings with the weight percent of the final solution of hydrophilic polymer ranging from 0.25% to 4% w / w in water. Frozen phase separation was performed in Teflon coated aluminum mold wells with a horizontal flat bottom. The solution was poured into the well to a height from the bottom of the mold of preferably about 10 mm, more preferably 2.5 mm, and most preferably 5.0 mm or less. The solution, which was initially at a temperature in the mold of 15°C to 30°C before freezing, was then frozen by cooling through the bottom of the mold. The shelf cooling temperature applied was preferably -40°C, more preferably the cooling temperature was -55°C, and most preferably the cooling temperature was -45°C, although other cooling temperatures can be applied to achieve a suitable frozen phase separation structure. After the solution reached frozen phase separation and the temperature of the frozen solution reached equilibrium with the freezing temperature, the system was further frozen phase separated and equilibrated for at least another hour before drying. In a modified freezing and mold-filling method to provide layers of various frozen phase-separated solutions, the first layer was added to the mold to a desired depth and frozen, and then the second layer was added and frozen, thus preparing a multi-layer frozen phase-separated coating. Care had to be taken to ensure that frost would not form between the (n-1)th frozen solution and the nth poured solution, causing cracking due to differences in the frozen structure of the layers. Layering of separate frozen layers that would bond together and not crack is a major challenge. During this investigation, it was an unexpected and significant finding to discover that a method of bonding single layers of pre-dried hydrophilic polymer matrix over and over to a single co-bonded compressed multi-layer composite sheet works well.
[0132] A Virtis Benchmark 2000 pilot scale freeze dryer with a 24 ft2 shelf was used to sublimation freeze dry the frozen phase separated plaques of the frozen solution. In the first freeze drying (removal of ice not hydrogen bonded to the hydrophilic polymer), the equilibrated frozen plaques in the mold were subjected to a vacuum of 300 mTorr or less in the freeze dryer, the freeze dryer condenser was set at or below -65°C, and the freeze dryer shelf was heated to promote sublimation of ice from the freeze separated plaques without the temperature of the plaques exceeding -15°C. After substantially all of the unbonded ice was removed, the shelf temperature was increased to approximately 25°C to remove the hydrogen bonded ice and reduce the moisture content in the dried coating matrix so that the residual moisture in the dried coating matrix was 4% or less. The final dried matrix conformed to the original shape of the filled mold, shrank approximately 5% in length and width, and had a density of 0.005 g / cm3. 3 ~0.04g / cm 3 These contained more than 95% void space and were interconnected porous structures with fine polymer lamellae (submicron to 5 microns thick) and pores separating adjacent lamellae of 100 to 300 microns.
[0133] After freezing phase separation and drying, the dried matrix was compressed from its original thickness (10 mm to 2.5 mm) to a final thickness, preferably close to 50 microns. If two uncompressed sheets of dressing are compressed together on top of each other, they will be permanently bonded together at the end of the compression process. In compression, a thin shim of calibrated uniform thickness can be used to obtain a compressed dressing of the desired thickness, substantially the same thickness as the shim. There are several methods to achieve this compression, with the desired compression set near 50 microns. The preferred compression method used in this study was to compress the entire dry uncompressed dressing (dimensions typically close to 100 mm length x 100 mm width x 2.5 mm height or 50 mm diameter x 2.5 mm height) between aligned platens to a thickness of 100 microns or less, at a uniaxial compression speed of 0.5 mm / min or less. Platens (diamond sprayed or Teflon coated Mic 6 aluminum 300mm x 300mm x 90mm) were machined to a flat planar surface (less than 5 microns at 300mm) with no or some controlled texture machined on its surface. The temperature of the platen during compression was preferably maintained near 80°C for 3-5 minutes of uniaxial compression. Compression was achieved by screw loading at the four corners of the platen applying up to 4 tonnes of load per corner. Compression was maintained for at least 2 minutes before releasing the load. The compressed thickness and weight of the novel compressed hydrophilic polymer matrix were measured. Final density was 0.25-0.9 g / cm 3 After compression, the dressings were further processed. This additional processing included die cutting into 2.5 cm diameter test specimens and in some cases thermal annealing heat treatment (heating in a convection oven at 60°C to 150°C for 5 to 30 minutes). Once processed, the dressings were placed into Ziploc® or foil pouches with heat seals. Packaged dressings intended for animal and biocompatibility testing were gamma irradiated at 25 kGy.
[0134] Example 3 In vitro and ex vivo testing of a prototype chitosan intraluminal hemostatic dressing In vitro beaker test The dissolution behavior of CEHD was studied under conditions similar to those that would be experienced during in vivo use of TURP. Dissolution was monitored for periods up to 7 days to establish that CEHD tolerated early dissolution (first 24 hours), followed by later dissolution to meet the goal of no residual CEHD after 168 hours (7 days).
[0135] A section of porcine bladder tissue (25 mm x 25 mm x 3 mm) with the mucosal surface facing outward was fixed with cyanoacrylate cement to the bottom of a 200 milliliter polystyrene beaker. A drop of a 1:250 v / v solution of blood in normal saline was placed on top of the ex vivo sectioned bladder tissue. A piece of CEHD dressing (1.3 cm x 1.9 cm) was applied to the wetted tissue surface with a pressure of 9.7 kPa (73 mmHg) by applying a 500 gram standard weight (Troemner, Thorofare, NJ 08086) to a 2.54 cm diameter probe for 5 minutes. Sufficient synthetic urine (50 ml) was added to the beaker at room temperature to immerse the CEHD piece. The beaker was covered with parafilm, incubated at 37°C (Fisher Scientific, Model 146E, CAT.97-990E), and placed on a shaker (IKA AS260.1, KS260) at 120 rpm. The synthetic urine solution was replaced every 24 hours, and dissolution behavior was recorded by visual inspection of the amount of dressing present at regular intervals until complete dissolution or up to 168 hours. In some tests, adhesion of the CEHD specimens to tissue was evaluated by measuring resistance to shear forces using a horizontal scratching motion of tweezers. Tissue adhesion testing of the CEHD was performed on a pass or fail basis during the in vitro dissolution test and was recorded as low, moderate, and high.
[0136] The in vitro solubility and adhesion to porcine bladder mucosa results are shown in Figure 15. The in vitro solubility and adhesion to porcine bladder mucosa results, along with the folding and device placement test results, were used to select three preferred dressing types for biocompatibility and in vivo testing. These dressing types included a catechol-modified chitosan preparation and both catechol and thiol-modified chitosan preparations. The preferred ex-in vivo dressing types were labeled Type A, B, and C. Dressing lots 71 and 81 represent Type A dressings, lots 78 and 83 represent Type B dressings, and lots 75, 80, and 84 represent Type C dressings.
[0137] In vitro simulated venous wound sealing (SVWS) test A laboratory simulated venous wound sealing (SVWS) device was constructed to test the sealing ability of a CEHD adhered by a drop of dilute blood, i.e., blood in normal saline at 1:250 v / v, with a load of 9.7 kPa for 5 minutes across a 1.5 mm diameter "injury" opening in the center of a standard PVC plate with a surface previously shown to mimic dermis for binding of mucoadhesive chitosan to the dermis. Silastic laboratory tubing (Dow Corning Corporation, Midland, MI 48686), with an inner diameter of 0.250 inches and an outer diameter of 0.375 inches, connected an open container of citrated whole bovine blood to an opening with a stopper valve just prior to the opening. The vertical height of the blood level in the container relative to the opening was adjustable between 0.0 and 50 cm. After installing the CEHD test dressing centered over the opening in the standard PVC face, the stopper valve was opened and the dressing was observed for 15 minutes to assess (pass / fail) the dressing's ability to maintain a seal (no blood leaking through or under the installed dressing). The pressure head was recorded for each test. This test provided a rapid simulated bleeding control test of the prototype CEHD at venous output pressure.
[0138] The simulated bleeding rate (g / min) was determined by the weight difference between a pre-weighed absorbent sheet and the same absorbent sheet placed over the "injury" and collecting flowing blood for 15 seconds and multiplied by 4.
[0139] A head height difference of 20 cm to 42 cm at 23° C. is equivalent to a pressure of 14.7 mmHg to 30.9 mmHg (typical of venous pressure in prostatic bleeding). The bleeding rates for head height differences of 20 cm and 42 cm were determined to be 4.7 and 8.0 g / min, respectively.
[0140] The results of the in vitro simulated venous wound sealing (SVWS) test are shown in Table 1 (along with the shelf life, stored in foil packaging at 25°C for 0–6 months) for dressing lots B and C that were gamma irradiated at 25 kGy. [Table 1]
[0141] Ex vivo flow testing of 10mm x 10mm dressings bonded over 3mm diameter perforations in SIS Test dressings that performed well in vitro (10 of each dressing types B and C; see Figures 12A, 12B, and 15) were bonded to porcine small intestinal submucosa (SIS) at the center of a 3 mm diameter hole in the SIS supported in a custom-made Adams and Chittenden glass test cell at a balloon pressure of near 7 psi for approximately 3 minutes (see Figure 10). The test cell, containing the dressing bonded to the SIS and sealing the defect, was connected to a flow system as shown in Figure 11. A Fisher Scientific FH100M multichannel peristaltic pump with a 13-310-911 flow cassette was used to control the flow rate at near 20 ml / min. Synthetic urine, which completely filled the cell volume at near 34°C to 37°C, was flowed through the cell at near 20 ml / min for 6 to 20 hours. The objective of the test was to demonstrate the ability of the dressing to remain adherent to the mucosa during urinary flow without tearing or loss of particles or large pieces from the dressing.
[0142] In the case of dressing type C (dressing lots 75 and 80), one test was performed for 20 hours. At the end of the test, an external pressure approximating 20 mmHg of 1:250 v / v blood in normal saline was applied through the jacketed circuit of the glass test cell to test the adhesion of the test dressing to the tissue. Pressurization was performed four times, and the dressing successfully remained adhered over the 3 mm diameter hole to the inner SIS surface, resistant to the external application of liquid pressure in all four pressurizations. The dressings tested for 20 hours were also examined for mass loss (by gravimetric comparison of the dry weight before and after testing). Gravimetric testing of the dressing type C after 20 hours showed that the catechol modified chitosan had lost less than 15% of the dry weight of the original dressing (most likely due to dissolution). All other tests on the dressing type C were performed for 6 hours without the application of external pressure stress. In the case of the dressing type C, there was no significant visible dissolution of the dressing or loss of material from the dressing. All dressings remained adherent to the SIS at the end of the study. Adhesion and cohesion of the dressings (to the SIS mucosa) were rated as moderate.
[0143] In the case of dressing lots Type B (dressing lots 78 and 83), one test was performed for 24 hours. The dressings tested for 24 hours were examined for mass loss (by gravimetric comparison of dry weight before and after testing). Gravimetric testing of the Type B dressings after 24 hours showed significant material loss of the catechol modified chitosan (most likely due to dissolution) at 39.4% of the dry weight of the original dressing. All other tests on Type B dressings were performed for 6 hours. In the case of Type B dressings, there were visible signs of significant dissolution (gelling) of the dressing and loss of material (release of visible flakes from the dressing). Adhesion (to the SIS mucosa) and cohesion of the dressings were rated as moderate to low.
[0144] Example 4 Testing the foldability and placement of the covering All dressing lots (N3 and above) were tested for foldability, as this is a key feature for the ability to attach, wrap, and place dressings formed from the materials of the present invention at the prostate and bladder neck injury sites. The fold test involved first folding the final compressed circular dressing, flat on the horizontal, 180° counterclockwise, edge-to-edge, and then holding the edges together and compressing tightly at the center of the dressing to create a single linear fold axis (i.e., crease) in the dressing. The folded dressing is then unfolded and the edge-to-edge fold is recreated along the new fold axis, but in the opposite clockwise direction. Successful folding is ranked by the absence of visible tears or cracks along the fold axis and no significant loss in the tensile properties of the dressing (determined by gently pulling the dressing across the fold). The results of the fold test are shown in column 4 of FIG. 15.
[0145] A placement test (N=5) was conducted for the preferred chitosan-backed dressings types A, B, and C using a 250 milliliter volumetric flask filled with normal saline as a model of a urine-filled bladder neck. The fully assembled device with CEHD dressing, sheath cover, and balloon catheter (distal and proximal balloons) was immersed in normal saline up to below the neck of the volumetric flask. The application of the CEHD was initiated by inflating the distal balloon to break the protective water-resistant sheath at its end, then manually removing the broken sheath completely and intact by pulling the dry free end of the sheath outside the flask, quickly positioning the distal balloon at the bladder neck, and immediately thereafter smoothly and rapidly inflating and opening the proximal balloon to adhere the dressing to the neck of the flask. All dressing types (A, B, and C) adhered well to the neck of the glass vessel and delivery was successful.
[0146] Example 5 Biocompatibility of the coating type The finished, packaged, sterile (final gamma irradiation 25 kGy) device was subjected to ISO 10993-1 biocompatibility testing in accordance with the testing requirements for extracorporeal devices with indirect blood flow path contact for limited access. Testing included cytotoxicity, skin irritation, and acute systemic toxicity (triplicates for each test).
[0147] Coatings A and C passed all biocompatibility tests, but coating B failed the acute systemic toxicity test, likely due to the generation of cytotoxic thiol residues in coating B after gamma irradiation.
[0148] Example 6 An acute in vivo bladder neck and porcine splenic capsule avulsion model of hemostasis Acute in vivo studies were performed in six acclimatized Yorkshire sows (Oak Hill Genetics, CA) weighing 40-50 kg, in which delivery devices were assembled with three CEHD prototypes (Dressing A: n=6, Dressing B: n=9, Dressing C: n=10). The experiment was designed as a randomized, blinded study of the efficacy of individual prototypes versus controls in an acute porcine bladder neck and splenic parenchymal bleeding injury model. [Table 2] *Dressing material C was selected to proceed to the 7-day survival study. ‡0, 1, 2, 3, and 4 = none (material does not adhere), low (adheres but can be easily removed), medium (edge can be removed by probe), medium-strong (resists edge removal by probe), and strong (edge cannot be removed by probe) adhesion, respectively. †Surgical gauze was used as a negative control for the spleen injury model.
[0149] (Examples 7 to 11) Examples 7-11 represent CGHD chitosan dressings. The following materials were used in the development of CGHD:
[0150] Chitosan A: Primex, ChitoClear 65010, TM 4375, MW = 250-300 kDa, Brookfield viscosity of 1.0% w / w chitosan solution in 1.0% acetic acid at 25°C and spindle LV1 = 390 cPs, DDA = 80% (by colloid titration) Chitosan B: Primex, ChitoClear 43000, TM 4167, MW = 110-150 kDa, Brookfield viscosity of 1.0% w / w chitosan solution in 1.0% acetic acid at 25°C and spindle LV1 = 9 cPs, DDA = 95% (by colloid titration) Glacial Acetic Acid: Fisher Scientific, Catalog No. A38-212 Hydrochloric acid: 1.0 M in water, Sigma Aldrich, Catalog No. H9892 L-Lactic Acid: JT Baker, Catalog No. 0196-01 Glycolic Acid: JT Baker, Catalog No. M821-05 Sodium hydroxide: 5.0M NaOH in water, Sigma Aldrich, Catalog No. S8263-150ml Potassium hydroxide: 0.1 M KOH in methanol (BDH) Ethanol: 200° proof Sigma Aldrich, Catalog No. 459844-1L Fine fiber chitin: diameter about 10 microns, aspect ratio about 100 / 1, 100% acetylated, Weifang Centrifugal spun chitosan nanofiber: Lot G01, basis weight 12g / m 2 Tricol Medical Grade Non-Woven Microfiber Deionized water: Ricca ACS Reagent Grade Deionized Water, Catalog No. 9152-5 Acetic anhydride: Obtained from Sigman Aldrich, ACS reagent grade, catalog number 320102-1L 3,4-Dihydroxyhydrocinnamic acid (Mw=182.17g / mol): 98% Sigma Aldrich, Cat. No. 102601 1-Ethyl-3-(-3-dimethylamino-propyl)carbodiimide: (alternatively N-(3-dimethylaminopropyl)-N'-ethylcarbodiimide hydrochloride, commonly acronym EDC) Sigma Aldrich, catalog # E7750 Sodium chloride: Sigma Aldrich, Cat. No. 793566-500g Synthetic gastric juice: Pepsin - Sigma Aldrich, P7000-25G, NaCl - Sigma Aldrich, 793566-500G, H2O ACS Reagent Grade, NaOH - Sigma Aldrich, Cat. No. S8263-150ml Tissues: Fresh porcine bladder mucosa, fresh porcine gastric mucosa, obtained from Animal Biotech Industries Inc. Citrated bovine whole blood: Lampire Biological Laboratory Bovine CPD, Catalog No. 7720010 Cyanoacrylate: Permabond 910 Tissue Adhesive, Catalog No. 72590 Dialysis tubing: 3,500Da MWCO Snakeskin dialysis tubing (Fisher Scientific), catalog #PI88244 Pectin: MP Biomedicals LLC, Catalog No. 102587 Glycerol: Sigma Aldrich, Cat. No. G-8773 Polyethylene glycol: Spectrum, Catalog No. PO108 Polyethylene oxide: Mw 400,000 da, Sigma Aldrich, Catalog No. 372773-500G Poloxamer 407: Spectrum, Catalog No. P1166 Guar: Sigma Aldrich, Cat. No. G4129 Cellulose (microcrystalline powder): Sigma Aldrich, Cat. No. 435236 Polyacrylic acid: Mv 1,250,000 Sigma Aldrich, Catalog No. 306215-100G HemCon Patch® Pro, a commercially available highly efficient chitosan hemostatic dressing, was used as a positive control dressing in the acute hemostatic study.
[0151] Standard surgical gauze was used as a negative control for acute hemostasis studies.
[0152] Example 7 Preparation and characterization of catechol chitosan
[0153] Approach 1 Chitosan A (9.0 g) was dissolved in deionized water (148 g) and HCl (28 ml, 1.0 M HCl). A 1:1 (150 ml) solution of water:ethanol was prepared. 3,4-Dihydroxyhydrocinnamic acid (25.9 mmol) and N-(3-dimethylaminopropyl)-N'-ethylcarbodiimide hydrochloride (51.8 mmol) were dissolved in the water / alcohol solution. The water / alcohol solution was added to the chitosan solution. The solution was mixed vigorously. The reaction mixture was controlled at pH 5.4 using dropwise addition of 0.1 M HCl and 0.1 M NaOH solutions and allowed to react for at least 12 hours by stirring from above. The chitosan solution (approximately 300 ml) was then dialyzed against 5 liters of water acidified with one drop of 1.0 M HCl solution for 6 days and against non-acidified water for at least 3 hours. During dialysis, the water was replaced and the dialysate was changed at least five times at intervals of approximately 24 hours.
[0154] Approach 2 Chitosan A (1.5 g) was dissolved in water (140 g) and HCl (5 ml, 1.0 M HCl). A 1:1 solution of water:ethanol (145 ml) was prepared. 3,4-Dihydroxyhydrocinnamic acid (10.5 mmol) and N-(3-dimethylaminopropyl)-N'-ethylcarbodiimide hydrochloride (13.0 mmol) were dissolved in the water / alcohol solution. The water / alcohol solution was slowly added to the chitosan solution and the reaction mixture was stirred at a low stirring speed by an overhead mechanical stirrer. The reaction mixture was controlled at pH 5.5 using dropwise addition of 0.1 M NaOH and 0.1 M NaOH solutions and allowed to react for about 12 hours under stirring. After the reaction process, the solution was dialyzed as described in approach 1.
[0155] Approach 3 Chitosan A (9.0 g) was dissolved in water (126 g) acidified with HCl (30 ml, 1.0 M). A 1:1 solution of water:ethanol (150 ml) was prepared and N-(3-dimethylaminopropyl)-N'-ethylcarbodiimide hydrochloride (31.3 mmol) was dissolved in the water / alcohol solution. Then, 3,4-dihydroxyhydrocinnamic acid (15.7 mmol) was dissolved in 15 ml of water and this solution was slowly added to the chitosan solution under moderate mechanical stirring from above. The water / alcohol solution containing N-(3-dimethylaminopropyl)-N'-ethylcarbodiimide hydrochloride was slowly added to the chitosan solution and the reaction mixture was stirred at low stirring speed by a mechanical stirrer from above. The reaction mixture was controlled at pH 5.5 using dropwise addition of 0.1 M KOH (in methanol) and 0.1 M HCl solutions and allowed to react for about 12 hours under stirring. After the reaction process, the solution was dialyzed as described in approach 1.
[0156] Approach 4 Chitosan A (9.0 g) was dissolved in water (126 g) acidified with HCl (30 ml, 1.0 M). The solution was then adjusted to approximately pH 5.1 using 0.1 M HCl and 0.1 M aqueous NaOH. A 1:1 solution of water:ethanol (150 ml) was prepared and N-(3-dimethylaminopropyl)-N'-ethylcarbodiimide hydrochloride (31.3 mmol) was dissolved in the water / alcohol solution. Then 3,4-dihydroxyhydrocinnamic acid (15.7 mmol) was dissolved in 15 ml water and this solution was added slowly to the chitosan solution under moderate overhead mechanical stirring. The water / alcohol solution containing N-(3-dimethylaminopropyl)-N'-ethylcarbodiimide hydrochloride was added slowly to the chitosan solution and the reaction mixture was stirred at a low stirring speed by an overhead mechanical stirrer. The reaction mixture was controlled at pH 5.0 using dropwise addition of 0.1 M KOH (in methanol) and 0.1 M HCl solutions and reacted under stirring for about 12 hours. After the reaction process, the solution was dialyzed as described in Approach 1.
[0157] Degree of substitution of catechol chitosan A quartz UV test cell (path length 1 cm, ×2 (HACH Co., Cat. No. 48228-00) was used to obtain the UV / visible spectra.
[0158] The UV / Vis spectrometer was a Varian Cary Bio100. Standard solutions of 3,4-dihydroxyhydrocinnamic acid were prepared in water and the absorbance at 280 nm was plotted against the concentration. The extinction coefficient ε in the Beer Lambert relationship for absorbance in dilute solutions is given below:
number
[0159] (absorbance < 0.5) was determined as 2,540 ± 50 liters / (mol·cm). This value was used to determine the degree of substitution in dilute aqueous solutions of modified chitosan with known amounts, known volumes of solution, and the peak absorbance measured at 280 nm.
[0160] The chitosan catechol solution is diluted (usually about 50 or 100 times) so that its absorbance at 280 nm is less than 0.5. Using the absorbance, the weight of the solution used for dilution, and the percent solids (CS-catechol), the formula
number
[0161] result Chitosan-catechol synthesis yielded 50-300 mL of chitosan-catechol solutions ranging from milky to clear, light pink to brown, and with viscosities ranging from thin liquid-like consistency (e.g., the viscosity of water is around 1 cps) to thick liquid-like consistency (e.g., the viscosity of honey is over 100,000 cps). The synthesis results (see Table 1) depended on the initial concentration of chitosan, prevention of chitosan precipitation during the pH adjustment step from approximately pH 2 to pH 5, maintenance of a pH of approximately 5.0-5.5 during the reaction, and complete removal of low molecular weight components during the dialysis washing step. [Table 3] ¶ The percentage of dry solids in the solution was determined gravimetrically. *Synthesis via approach 2 resulted in excess UV / Vis absorbance in determining the degree of substitution †Catechol chitosan was concentrated by removing water from the solution suspended in a dialysis membrane with heat-assisted drying.
[0162] Example 8 Freeze-phase separation hydrophilic polymer coating material Aqueous solutions of hydrophilic polymers were prepared in 500 ml, 1000 ml, or 2000 ml Nalgene LDPE bottles or polypropylene beakers by adding ingredients including, but not limited to, pre-prepared solution, hydrophilic polymer, water, acid, and additional ingredients. Figures 17A-17C list the formulation approaches, hydrophilic polymers, and % w / w of hydrophilic polymer components in the solution. Some of the formulations in Figures 17A-17C do not contain chitosan. The formulation strategies are listed in Figures 17A-17C as A, B, C, D, E, F, and G. Strategy A was primarily a control for materials such as chitosan that were tested with simulated gastrointestinal fluid in vitro and predicted not to survive dissolution in the stomach. Reacetylation (Strategy B) was one of the proposed strategies to reduce the rate of dissolution / degradation until in vitro simulated gastrointestinal fluid testing in the presence of pepsin, which demonstrated that a lower degree of deacetylation resulted in a faster rate of chitosan degradation and dissolution. Strategy C examined compositions of known polysaccharides (guar, pectin, and starch) without chitosan, which are resistant to digestion by simulated gastrointestinal fluid in vitro. Strategy D was Strategy C plus chitosan and possibly other hydrophilic polymers. Strategy E used catechol-modified chitosan as the only hydrophilic polymer. Strategy F used catechol-modified chitosan and other hydrophilic polymers. Strategy G used centrifugally spun chitosan fibers.
[0163] The major problems experienced in formulating the hemostatic dressing for application in the gastrointestinal tract were (1) the unexpected rapid (<10 min) pepsin-promoted degradation of chitin and chitosan in synthetic gastric fluid (pepsin accelerates the rate of chitosan degradation at a rate that increases with decreasing degree of deacetylation), (2) the unexpected interference by blood in achieving adhesion of pure catechol-modified chitosan, and (3) the susceptibility of the dressing to crack and tear when the formulation was modified to address other problems.
[0164] The %w / w of the final hydrophilic polymer solutions ranged from 0.1% to 4% polymer. The capped bottles and their contents were mixed continuously at room temperature for 12-24 hours using an IKA KS260 orbital shaker or a Wheaton benchtop bottle roller to achieve complete solution homogeneity. The solutions in the beakers were mixed at room temperature for 12-24 hours using magnetic stirring beads on a magnetic stirrer plate to achieve solution homogeneity. The beakers were closed from the outside environment using parafilm during mixing. The solutions prepared for freeze phase separation were substantially homogenous and clear in the absence of suspending conditions (except for A06, B02, B04, and C05). The catechol chitosan solutions exhibited some haze and milky appearance and showed the presence of some dispersed fine catechol chitosan spherical particles.
[0165] Except for strategy G, chitosan solutions were prepared as frozen phase separation coatings with the weight % of the final solution of hydrophilic polymer ranging from 0.25% to 4% w / w in water. Frozen phase separation was performed in Teflon coated aluminum mold wells with a horizontal flat bottom. The solution was poured into the well to a height from the bottom of the mold of preferably about 10 mm, more preferably 2.5 mm, and most preferably 5.0 mm or less. The solution, which was initially at a temperature in the mold of 15°C to 30°C before freezing, was then frozen by cooling through the bottom of the mold. The shelf cooling temperature applied was preferably -40°C, more preferably the cooling temperature was -55°C, and most preferably the cooling temperature was -45°C, although other cooling temperatures can be applied to achieve a suitable frozen phase separation structure. After the solution reached frozen phase separation and the temperature of the frozen solution reached equilibrium with the freezing temperature, the system was further frozen phase separated and equilibrated for at least another hour before drying. In a modified freezing and mold-filling method to provide layers of various frozen phase-separated solutions, a first layer was added to the mold to a desired depth and frozen, and then a second layer was added and frozen, thus preparing a multi-layer frozen phase-separated coating. Care had to be taken to ensure that frost would not form between the (n-1)th frozen solution and the nth poured solution, causing cracks due to differences in the frozen structure of the layers. During this investigation, an unexpected and significant finding was the successful superposition and bonding of a single layer of a previously freeze-dried hydrophilic polymer matrix to a single co-bonded compressed multi-layer composite sheet. Separately prepared freeze-dried compositions can also be combined using compression.
[0166] A Virtis Benchmark 2000 pilot scale freeze dryer with a 24 ft2 shelf was used to sublimation freeze dry the frozen phase separated plaques of the frozen solution. In the first freeze drying (removal of ice not hydrogen bonded to the hydrophilic polymer), the equilibrated frozen plaques in the mold were subjected to a vacuum of 300 mTorr or less in the freeze dryer, the freeze dryer condenser was set at or below -65°C, and the freeze dryer shelf was heated to promote sublimation of ice from the freeze separated plaques without the temperature of the plaques exceeding -15°C. After substantially all of the unbonded ice was removed, the shelf temperature was increased to approximately 25°C to remove the hydrogen bonded ice and reduce the moisture content in the dried coating to less than 4% residual moisture in the dried coating. The final dried matrix conformed to the original shape of the filled mold, shrank approximately 5% in length and width, and had a density of 0.005 g / cm3. 3 ~0.04g / cm 3 These had greater than 95% void space and were interconnected porous structures (e.g., 20-300 microns) with fine polymer lamellae (e.g., submicron to 5 microns thick) and pores separating adjacent lamellae of, e.g., 20 microns to 300 microns.
[0167] After freezing phase separation and drying, the dried matrix was compressed from its original thickness (10 mm to 2.5 mm) to a final thickness, preferably close to 50 microns. If two uncompressed sheets of dressing are compressed together on top of each other, they will be permanently bonded together at the end of the compression process. In compression, a thin shim of calibrated uniform thickness can be used to obtain a compressed dressing of the desired thickness, substantially the same thickness as the shim. There are several methods to achieve this compression, with the desired compression set near 50 microns. The preferred compression method used in this study was to compress the entire dry uncompressed dressing (dimensions typically close to 100 mm length x 100 mm width x 2.5 mm height or 50 mm diameter x 2.5 mm height) between aligned platens to a thickness of 100 microns or less at a uniaxial compression speed of 10 mm / min or less or about 0.5 mm / min or less. The slower the compression speed, the better the mechanical properties of the final dressing, e.g. dressings prepared at initial compression speeds close to about 10 mm / min are acceptable. Platens (Teflon coated Mic 6 aluminum 300mm x 300mm x 90mm) were machined to a flat planar surface (less than 5 microns at 300mm). The temperature of the platens during compression was preferably maintained near 80°C for 3-5 minutes of uniaxial compression. Compression was achieved by a screw load on the four corners of the platen applying up to 4 tonnes (a tonne means 1000 kilograms) of load per corner. Compression was maintained for at least 2 minutes before the load was released. The compressed thickness and weight of the novel compressed hydrophilic polymer matrix were measured. The final density was 0.35-0.55 g / cm. 3 After compression, the dressings were further processed. This additional processing included die cutting into 2.5 cm diameter test specimens and in some cases thermal annealing heat treatment (heating in a convection oven at 60°C to 150°C for 5 to 30 minutes). Once processing was complete, the dressings were placed into foil pouches with heat seals. Packaged dressings intended for animal and biocompatibility testing were gamma irradiated at 25 kGy.
[0168] Example 9 In vitro testing of prototype gastrointestinal hemostatic dressings. Preparation of synthetic gastric fluid: Pepsin (1.6 g), NaCl (1 g), and water (500 ml) were added to a Nalgene LDPE 1000 ml bottle and mixed. Acidity was adjusted to pH 3-4 using Millipore pH 0-14 Universal Indicator Strips and the dropwise addition of 3.0 M HCl. If necessary, the pH was increased using the dropwise addition of 1.0 M NaOH.
[0169] 1. Test tube method To rapidly screen the resistance of test articles to dissolution / fragmentation in synthetic gastric fluid, a 0.5 cm x 0.5 cm piece of test article sheet was added to the bottom of a labeled 15 ml Falcon tube, 5 ml of gastric fluid was added to the tube, which was then stoppered and placed upright in a 37°C incubator with gentle shaking. The tubes were monitored until demonstrable sample dissolution / fragmentation was observed, and the time to dissolution / fragmentation was recorded. The results of the test tube studies are shown in Figures 16A-16C.
[0170] 2.Beaker method For materials showing resistance in the test tube test, a modified test method was developed. A 38 mm x 38 mm piece of fresh gastric mucosa was glued to the inside bottom of a polystyrene beaker (250 ml, Fisher, Cat. No. 08-732-124) using a thin layer of cyanoacrylate adhesive applied using a cotton swab. The mucosal surface prior to gluing was patted dry using a Texwipe tissue. The adhesive was allowed to dry for 2-5 minutes. After complete adhesion to the beaker, the exposed tissue surface was moistened with a drop (typically 2 drops) of citrated whole bovine blood, and a 20 mm x 20 mm piece of the test article sheet was adhered to the blood-covered mucosal surface by applying a 500 g load perpendicular to the mucosal surface through a 25 mm diameter PVC flat-tipped probe for 1 minute. A volume of synthetic gastric juice (approximately 90 ml) was added to the beaker. The beaker was sealed using parafilm and placed upright in an IKA KS260 orbital shaker in a 37° C. incubator with gentle shaking (130 rpm). The interior of the beaker was monitored for several minutes and then hourly until demonstrable detachment from the mucosa and / or lysis / fragmentation of the sample was observed, and the time to detachment / lysis / fragmentation was recorded.
[0171] During the development of the test method, the applied load (up to 5 kg) and application time for adhesion were up to 5 minutes. In comparison to the minimally invasive in vivo application, the Gastrointestinal Surgery Team advised applying a load of not more than 30 seconds uniformly and not more than 300 g for a 2.5 cm diameter dressing. The original conditions of 5 kg and 120 seconds were modified to 500 g, 1 minute. Here, a load of 300 g and 30 seconds of application are applied. The results of the beaker test are shown in Figures 16A-16C.
[0172] 3. Mechanical folding test The sample sheet was folded 180° along the length and width axes and the crease lines were compressed. The dried test sheets (25 mm x 25 mm) were folded and unfolded and observations of resistance to tears and cracks were recorded. The results of the folding tests are shown in Figures 16A-16C.
[0173] 4. Mechanical tissue adhesion Wet adhesion to mucosa was studied using a uniaxial mechanical tester (Instron, Model 5844) equipped with a 10 N load cell. Adhesion testing was performed using ASTM F2258-03 "Standard Test Method for Strength: Properties of Tissue Adhesives in Tension". Testing was performed in a test configuration with the lower and upper PVC probes aligned in a single axis in the z-vertical direction such that the edges of the xy-horizontal 15.2 mm diameter faces of these probes were precisely aligned (±0.2 mm) with each other with the uniaxial descent of the upper probe supported on the upper movable crosshead of the Instron chuck fixture. The lower PVC probe was supported by the stationary bottom chuck fixture. The bottom PVC horizontal surface was used to support a 10 mm × 10 mm mucosal tissue sample that had been adhered to the PVC surface with cyanoacrylate glue for at least 5 minutes prior to testing. An upper PVC horizontal surface was used to support a 10 mm x 10 mm CGHD specimen that was adhered with 3M double-sided tape for at least 5 minutes prior to testing. The square tissue specimen was wetted with 0.25 ml of decitrated whole bovine blood CPD before lowering the probe onto the test surface. The probe was lowered at 10 mm / min until a maximum load of 0.98 N was reached. Upon contact, the specimen and tissue specimen were in precise (±0.2 mm) contact and coplanar with each other. The 0.98 N uniaxial probe load was maintained for 30 seconds, after which the probe was removed at 10 mm / min to record the maximum failure stress. The results of the adhesion test are shown in Table 4.
[0174] [Table 4]
[0175] Example 10 In vivo (pig model of upper gastrointestinal bleeding) screening study
[0176] animal A total of four outbred adult habituated pigs (weight range 40-50 kg) were used in this study.
[0177] All experiments were performed in accordance with the 2011 National Research Council, "Guide for the Care and Use of Laboratory Animals" and applicable federal regulations. Animal protocols followed the NIH Guidelines for the Care and Use of Laboratory Animals and were approved by the Institutional Animal Care and Use Committee. All procedures and animal care were performed in an approved animal research facility.
[0178] Veterinary staff examined all animals to ensure baseline health. Animals were removed from all bedding 72 hours prior to the procedure and fasted 24 hours prior to surgery. Animals were allowed to drink water ad libitum. 20 minutes prior to the procedure, animals received a liquid bolus of 500 mg intravenous cefotetan and 250 ml Ringer's lactate. After premedication with glycopyrrolate and a combination of tiletamine HCl and zolazepam HCl (Telazol®, Fort Dodge Laboratories, Fort Dodge, IA), anesthesia was induced by mask using 5% isoflurane. The pigs were intubated, placed on a ventilator, and maintained with 2-3% isoflurane via endotracheal intubation. The right femoral artery was surgically isolated and a 6Fr catheter was inserted to facilitate continuous blood pressure monitoring and blood withdrawal for laboratory studies. 5000 units of heparin were administered intravenously (IV) to induce a state of coagulopathy. A continuous infusion of heparin at 50 units / kg was used throughout the procedure to maintain anticoagulation. After 10 minutes, and then every 20 minutes throughout the procedure, activated clotting time (ACT) levels were tested and additional heparin (50% of original dose, 2500 units) was administered IV as needed to maintain anticoagulation with an ACT of >250 seconds. ECG, blood pressure, and oxygen saturation were monitored throughout surgery and recovery. Vital signs were recorded every 15 minutes, including blood pressure, % isoflurane, O2 flow, respiratory rate, heart rate, SpO2, capillary refill time, blood pressure and mean arterial pressure, and temperature.
[0179] At the completion of the experiment, animals were euthanized by IV administration of Eutazol (1 mg / 10 lbs) while under anesthesia. Death was confirmed by a flat ECG and absence of pulsation by stethoscope.
[0180] Gastric bleeding model The pig was prepped with chlorhexadine and draped aseptically. A midline laparotomy was performed to expose the stomach. A 5 cm segment of the gastroepiploic vessels was dissected free from the stomach wall. For each segment, a 1 cm gastroincision was made adjacent to the free but intact vessels. The artery was then pushed and positioned towards the gastroincision so that it was exposed to the gastric lumen. The gastric incision was then closed in the usual manner along with the abdominal wall. An upper endoscopy (GIF Type Q180, Olympus) was performed to identify the gastric wound site within the stomach. The wound site and gastric vessels were then located and dissected with endoscopic biopsy forceps to create pulsatile bleeding.
[0181] Chitosan gastrointestinal hemostatic dressings (CGHD) identified in Table 5 below were applied by manual application by hand. Briefly, an incision of approximately 12 cm was made in the anterior stomach wall, exposing the gastric cavity, and a CGHD prototype dressing (20 mm x 20 mm) was applied to the bleeding site in the stomach. Prior to application of the dressing, a dry, pre-weighed, folded gauze sponge was used to absorb any blood from the wound for 15 seconds, weighed, multiplied by 4, and the bleeding rate (blood weight) was determined by calculating the bleeding rate per minute. The CGHD dressing was placed over the wound with the gauze sponge on top. Light pressure of around 200-300 g was applied evenly by hand over the patch for 30 seconds. At 30 seconds, the gauze was removed and the area was observed for initial hemostasis and followed for signs of rebleeding up to 10 minutes. Upon completion of application, the CGHD dressings were removed and the adhesion of the dressing to the tissue was graded using an adhesion scoring system (Table 5) with an adhesion score according to how well the dressing adhered to the tissue surface. [Table 5-1]
[0182] result [Table 5-2]
[0183] Three CGHD family prototypes (D24, F11, and G01) demonstrated good hemostatic properties in terms of rapid hemostasis and acceptable adhesion scores in a gastric vascular injury model. The slow wound tissue adhesion of pure catechol-modified chitosan was addressed by a combination of unmodified chitosan and catechol-chitosan. These compressed frozen phase-separated dressings were finally heat-treated at around 80°C for 15-30 min to obtain dressings with good rapid tissue adhesion and therefore promising hemostatic performance that rapidly controlled pulsatile hemorrhagic gastrointestinal bleeding by short (30 s) low applied pressure. It is noted that Patch Pro cannot be folded as required and is too thick, making it unsuitable for use in gastroscopic delivery. Also, Patch Pro is formed from standard chitosan that degrades in the upper GI in about 15 min or less.
[0184] Example 11 In vivo (porcine model of upper gastrointestinal bleeding) 3-hour study
[0185] animal A total of four outbred adult habituated pigs (weight range 40-50 kg) were used in this study.
[0186] Animal preparation, surgical preparation, animal anesthesia, and animal sacrifice were the same as presented in Example 4.
[0187] Gastric bleeding model The pig was prepped with chlorhexadine and draped aseptically. A midline laparotomy was performed to expose the stomach. Two 5 cm segments of the gastroepiploic vessels were dissected free from the stomach wall. For each segment, a 1 cm gastroincision was made adjacent to the free but intact vessels. The artery was then pushed towards the gastroincision and positioned so that it was exposed to the gastric lumen. The gastric incision was then closed in the usual manner along with the abdominal wall (Figure 2). An approximately 12 cm incision was made in the anterior wall of the stomach to expose the gastric cavity. The wound site and gastric vessels were then located and dissected with forceps to create pulsatile bleeding. Prior to application, the bleeding rate was determined by absorbing any blood from the wound using a pre-measured folded gauze sponge for 15 seconds, weighing, multiplying by 4, and calculating the bleeding rate. The CGHD dressing was then placed over the bleeding wound with the gauze sponge placed over it. Manual pressure was applied evenly over the patch for 30 seconds. At 30 seconds, the gauze was removed and the area was observed initially and up to 10 minutes for hemostasis. After 10 minutes of observation, if hemostasis was achieved, the gastric incision was closed in a layered fashion, i.e., the layers incised by the surgeon were continuously sutured together. The abdominal wall was then closed and observed for 3 hours. Upon completion of the 3-hour application, an upper endoscopy (GIF Type Q180, Olympus) was performed to identify and visually inspect the wound dressing. The abdominal and gastric incisions were then reopened for a gross observation of the dressing. The CGHD dressing was removed and an adhesion score was given according to how well the dressing adhered to the tissue surface using the adhesion score system (Table 5).
[0188] Once these procedures were completed, the wound sites were reprepared by removing the old clot and residual wound dressing for reapplication of the second set of dressings as described above. Each wound site was used to test two dressings in this phase of the study.
[0189] bleeding rate Metzenbaum scissors were used to create a hemisect vascular injury to the gastric vessels, creating pulsatile bleeding. The bleeding rate was measured with pre-weighed gauze and recorded in g / min. The bleeding rate was determined and recorded for each injury before applying the dressing.
[0190] The test specimen was 20 mm x 20 mm. Eight coatings from each type of nanospun chitosan (G01) and chitosan catechol blend (F11) were tested.
[0191] Application of test specimen The test strip was applied centrally over the injury with sufficient finger pressure to stop the bleeding and a 30 second timer was started. A 50mm x 50mm piece of gauze was folded in two and applied over the 20mm x 20mm test strip. Any pooled blood was then aspirated from the site. After applying light finger pressure (approximately 300g load) for 30 seconds, the finger was removed and the test dressing was observed for signs of bleeding. If bleeding was observed, pressure was applied again for 30 seconds. If hemostasis was achieved when pressure was removed, the dressing was observed for 10 minutes. If there was no recurrence of bleeding, the stomach wall was closed and observed with a GI endoscope for 3 hours. If there was no recurrence of bleeding after 3 hours, the dressing strip was considered successful. If bleeding recurred within 5 minutes, the dressing was removed and a new dressing was applied. Up to two reapplications were utilized. [Table 6] *One dressing in each group had an extra dressing to stop exudation after the third compression. **One coating was held for an additional 30 seconds
[0192] The nanospun chitosan dressing (G01) had 4 successful applications out of 12 dressing applications, while the 25% catechol / 75% 2% chitosan dressing (F11) had 6 successful applications out of 13 dressings tested. Two deviations in dressing application were noted. One dressing in each group had extra dressing to stop exudation that did not stop in pig #4. One of the nanospun chitosan dressings was held on for an additional 30 seconds.
[0193] In all applications, an endoscope was inserted to assess whether the dressings were still present and hemostatic. In all cases, all dressings were confirmed to be present, hemostatic, and visible through the endoscope. After more than 3 hours of dressing application, the stomach was opened to allow inspection of the injury site and dressings. All dressings were unchanged. Thrombus formation was observed in all wounds. It was noted that in all cases of initial dressing success, no subsequent bleeding from the wound was observed at the 3 hour time point.
[0194] The final best dressing prototypes identified by testing in Examples 3, 4, and 5 demonstrated sustained efficacy once adhered with the brief light hand pressure hold required for delivery through the delivery port of a standard gastroscope. The best dressings developed were suitable for a folded (or rolled) configuration for delivery through the standard 2.8 mm diameter delivery channel of a standard gastroscope.
[0195] All CGHD dressings that achieved hemostasis (complete cessation of bleeding) within the first 10 minutes of application with three or fewer 30 second retention applications maintained complete hemostasis throughout the 3 hour test period in the closed porcine stomach. Success was achieved in 31% of G01 prototype applications and 46% of F11 prototype applications. The challenging nature of this study resulted in nearly 50% success (i.e., F11 prototype) for clinical application, especially noting that all initial mucoadhesive application successes resulted in 100% success in the long term. Chitosan and catechol-chitosan blend dressings are substantially resistant to digestion by digestive fluids, can be folded / rolled into the most complex and compact configurations, and can provide good adhesive properties in combination with blends with unmodified chitosan.
[0196] References Below is a list of references, listed in numerical order, corresponding to the bracketed numbers noted throughout the specification. [ka] [ka] [ka]
Claims
1. A chitosan material comprising a catechol-modified chitosan, wherein the catechol-modified chitosan is a chitosan modified with a chemical selected from the group consisting of at least one of 3,4-dihydroxyhydrocinnamic acid (hydrocaffeic acid), 3,4-dihydroxycinnamic acid (caffeic acid), trans-3,4-dihydroxycinnamic acid (trans-caffeic acid), and 3,4-dihydroxyphenylacetic acid (DOPAC, homoprotocatechuic acid), wherein the catechol-modified chitosan further comprises catechol oxidized to an o-quinone and a crosslinked material, which is selected from the group consisting of compound (A). [Case 1A] Or (B) [chemical 1B] At least one of wherein said material is in a dry solid form that resists dissolution in the form of visible signs of gelling or fragmentation when exposed to biological fluids ranging from pH 3.0 to pH 8.0 at 37° C. within the first 6 hours of application, and dissolves from the application site within 7 days, and wherein said material adheres to the surface of tissue when wet, and has an adhesive strength greater than or equal to 1 kPa. Chitosan material.
2. 10. The chitosan material of claim 1 having a thickness of 500 microns or less.
3. 0.03 g / cm 3 ~0.7g / cm 3 3. The chitosan material according to claim 1 or 2, having a density in the range of
4. (i) 0.3g / cm 3 ~0.4g / cm 3 or (ii) 0.4 g / cm 3 ~0.5g / cm 3 3. The chitosan material according to claim 1 or 2, having a density in the range of
5. 0.35 g / cm 3 ~0.55g / cm 3 3. The chitosan material according to claim 1 or 2, having a density in the range of
6. 4. The chitosan material according to claim 1, which is compressed.
7. 4. The chitosan material of claim 1, wherein the material is square, rectangular, circular, or circular petal shaped.
8. 4. The chitosan material of claim 1, having a moisture content of (1) 15% by weight (w / w) or less, (2) 8% by weight (w / w) or less, or (3) 4% by weight (w / w) or less.
9. 4. The chitosan material according to claim 1, having an adhesive side and a non-adhesive side.
10. 10. The chitosan material of claim 9, wherein the adhesive side is provided on a first layer and the non-adhesive side is provided on a second layer.
11. The chitosan material of claim 9 , wherein the adhesive side adheres to a tissue surface when the material is wet.
12. The chitosan material of claim 9 , wherein the non-adhesive side does not adhere to a delivery device.
13. 4. The chitosan material of claim 1, wherein the material adheres to the gastrointestinal mucosa in 1 minute or less, or adheres to the bladder mucosa in 3 minutes or less, or both, when wet, and has an adhesive strength greater than or equal to 1 kPa.
14. 4. The chitosan material of claim 1, which forms a quaternary ammonium cation at the C-2 amine of the glucosamine of the chitosan at the tissue site.
15. 4. The chitosan material according to any one of claims 1 to 3, having 1) a brown colouration, including a dark brown colouration, or 2) a pink to pinkish brown colouration.
16. 4. The chitosan material according to claim 1, wherein the catechol is not oxidized and the chitosan material has a pink coloration.
17. 4. The chitosan material of claim 1, further comprising freeze-dried lamellae.
18. 18. The chitosan material of claim 17, wherein the freeze-dried lamellae form a structure comprising more than one freeze-dried layer.
19. 4. The chitosan material of claim 1 further comprising spun fibers.
20. The chitosan material of claim 1 , further comprising a porous surface.
21. 21. The chitosan material of claim 20, wherein the porous surface provides one or more of: (i) an absorbent surface; and (ii) channels that redirect moisture away from the target tissue surface site.
22. 4. The chitosan material of claim 1, which is resistant to dissolution in water, saline solution, blood, GI fluids, or urine.
23. 4. The chitosan material of claim 1, which can be folded or rolled without cracking or splitting.
24. 4. The chitosan material of claim 1, having an outward surface area in an open, unrolled or unfolded state that is one of 8, 7, 6, 5 or 4 times the outward surface area of the same material when closed, rolled or folded.
25. 25. The chitosan material of any one of claims 1 to 24, which is intact and capable of being delivered by a balloon device, a wire device, or an endoscopic device.
26. 26. The chitosan material of claim 25, wherein the balloon device or the wire device or the endoscopic device comprises a working channel having a diameter of 3.2 mm or less or 7.0 mm or less, through which the material is delivered.
27. 25. The chitosan material of any one of claims 1 to 24, capable of removing hydrophilic and hydrophobic biological fluids that may interfere with adhesion.
28. After attachment of the chitosan material to the target tissue site, the chitosan material is removed from the delivery device.
25. The chitosan material of claim 1 , wherein the chitosan material is released from the
29. 25. The chitosan material of any one of claims 1 to 24, which after being adhered to an injury site, is capable of resisting dissolution in the presence of erosive enzymes and an acidic environment of pH 3, or in the presence of urine, or both, for at least 6 hours.
30. 25. The chitosan material of any one of claims 1 to 24, capable of achieving controlled slow dissolution from the attachment site.
31. 25. The chitosan material according to any one of claims 1 to 24, which can be folded and unfolded.
32. A chitosan material described in any one of claims 1 to 24, which does not readily dissolve in water, saline solution, blood, or GI fluid or bladder fluid or urine at 37°C for (1) at least 12 hours after application, or (2) at least 24 hours after application, or both (1) and (2).
33. 25. The chitosan material of any one of claims 1 to 24, which can be terminally sterilized without affecting the characteristics of the material.
34. 34. The chitosan material of any one of claims 1 to 33 for use in the treatment of a disease, condition, disorder, trauma, or injury.
Citation Information
Patent Citations
N-phenylpropenoyl chitosan oligosaccharide and preparation thereof
CN101289477A
Self-assembled short-peptide hydrogel and application thereof
CN111632026A
Adhesive and hemostatic injectable chitosan gel, and preparation method and applications thereof
CN113209363A
Easily reworked rubber surface treating agent and preparation method thereof
CN115895440A
5G communication module detection device and use method thereof
CN116540072A